Manufacturing method of rough wire for diamond wire
The production method for rough drawing wire with specific chemical compositions and controlled processes addresses the challenge of producing 5000 MPa class diamond wire by ensuring high cleanliness, uniform structure, and optimal mechanical properties, achieving low breakage and high strength for diamond wire applications.
Patent Information
- Application Number
- JP2023521827
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-10-22
- Filing Date
- 2020-11-12
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-11-12
AI Technical Summary
Existing methods cannot produce rough drawn wire capable of manufacturing 5000 MPa class diamond wire, which is essential for cutting materials like silicon wafers and quartz, due to issues with diameter, breakage, and strength requirements.
A production method involving vacuum melting, electroslag or vacuum self-consuming remelting, billet manufacturing, high-speed wire rolling, and controlled cooling to achieve a rough drawing wire with specific chemical compositions (C: 1.01~1.10%, Si: 0.15~0.40%, Mn: 0.30~0.60%, Cr: 0.01~0.40%, B: 0.0005~0.0020%, V: 0.01~0.09%, and controlled impurities) to ensure high cleanliness, uniform structure, and optimal mechanical properties.
The method produces a rough drawing wire with a tensile strength of ≥1320 MPa, area reduction rate of ≥30%, and a breakage rate of ≤2 times/1,000 km, suitable for manufacturing ultra-fine, high-strength diamond wires with a diameter of 40~46 μm, meeting market demands for high drawing performance and low breakage.
Smart Images

Figure 0007583157000001 
Figure 0007583157000002 
Figure 0007583157000003
Abstract
Description
[Technical field]
[0001] The present invention belongs to the technical field of material manufacturing. , Da How to produce diamond wire rods By law Regarding. [Background technology]
[0002] Cutting steel wire, also called cutting wire, cutting steel wire, or cutting wire, is a special wire material for splitting, and is also a special steel wire with a diameter of less than 0.20 mm and a zinc-copper plated surface. It is widely used as a consumer material in the fields of energy, aviation, equipment, and public facilities. Diamond wire is a high-carbon cutting steel wire with diamond particles embedded on the surface, and is mainly used for cutting and shaping solar cell silicon wafers, quartz materials, single crystal silicon, polycrystalline silicon, diamond, and other materials.
[0003] In order to reduce the loss of materials to be cut, such as silicon materials, during the cutting process, diamond wires are developed in the direction of smaller diameter, longer mileage without breakage, and higher strength. Therefore, the requirements for raw materials for producing cutting steel wire, such as high carbon steel wire rods, are becoming more and more stringent, that is, higher requirements are required for the cleanliness, structure uniformity, mechanical performance, and drawing performance of the wire rods. Specifically, it is necessary to control the size of inclusions to be smaller and the structure to be more uniform, and not to form abnormal structures such as martensite, bainite, and mesh-like carbide that affect drawing, and at the same time, it is necessary to increase the strength as much as possible and ensure the plasticity of the wire rods.
[0004] However, currently, there is still a lack of wire rods capable of producing 5000 MPa class diamond wire by drawing. In other words, it is practically impossible for existing wire rods to produce 5000 MPa class diamond wire while satisfying the basic requirements of diameter and mileage without breakage. Summary of the Invention
[0005] In order to solve the above technical problems, the present invention provides a rough drawing method which can be used to manufacture a 5000 MPa class diamond wire busbar by deep drawing and which satisfies the high market requirements for the diameter and breakage rate of diamond wire. Line The present invention aims to provide a production method.
[0006] In order to achieve the object of the invention, one embodiment of the present invention provides a method for producing a wire rod for deep drawing, in particular, a method for producing a wire rod for drawing into a 5000 MPa class diamond wire, wherein the chemical components of the wire rod include, in mass percent, C: 1.01-1.10%, Si: 0.15-0.40%, Mn: 0.30-0.60%, Cr: 0.01-0.40%, and either or both of B: 0.0005-0.0020% and V: 0.01-0.09%, with the balance being Fe and unavoidable impurities, with the proviso that the impurities include Al≦0.003%, Ti≦0.0008%, S≦0.005%, P≦0.008%, O≦0.0010%, and N≦0.0020%, and the production method includes: A vacuum melting process in which molten steel is smelted in a vacuum melting furnace under an atmosphere with an internal pressure of 10 Pa or less and cast into steel ingots; a steel ingot remelting process for treating a steel ingot by either or both of electroslag remelting and vacuum autogenous remelting to obtain a remelted ingot, wherein the electroslag remelting is performed under a protective atmosphere, and the remelting rate of the vacuum autogenous remelting is 3.0-3.5 kg / min; a billet making and grinding process, which comprises blooming or forging the remelted ingot into a steel billet and grinding the steel billet; a high-speed wire rolling process in which the steel billet is rolled into a wire rod, the rolling start temperature being 1030-1060°C and the rolling end temperature being 950-1020°C; and a cooling step in which the wire rod is cooled at a controlled temperature on the Stelmor, with the first to fourth fans turned on and the airflow is 80% to 100%, and the remaining fans turned off.
[0007] In order to achieve the above object of the present invention, one embodiment of the present invention provides a method for producing a wire rod for deep drawing, in particular, a method for producing a wire rod for drawing into a 5000 MPa class diamond wire, the method comprising the steps of: a vacuum melting process in which alloy elements are blended in molten iron according to a composition design of C: 1.01-1.10%, Si: 0.15-0.40%, Mn: 0.30-0.60%, Cr: 0.01-0.40%, and either or both of B: 0.0005-0.0020% and V: 0.01-0.09%, and the molten steel is smelted in a vacuum melting furnace under an atmosphere with an internal pressure of 10 Pa or less, and cast into a steel ingot; a steel ingot remelting process, which comprises treating a steel ingot with either or both of electroslag remelting and vacuum self-consumption remelting to obtain a remelted ingot, the chemical composition of which is C, Si, Mn, Cr, and either or both of B and V, with the balance being Fe and unavoidable impurities, and impurity elements being Al≦0.003%, Ti≦0.0008%, S≦0.005%, P≦0.008%, O≦0.0010% and N≦0.0020%, wherein the electroslag remelting is carried out under a protective atmosphere, and the remelting rate of the vacuum self-consumption remelting is 3.0-3.5 kg / min; a billet making and grinding process, which comprises blooming or forging the remelted ingot into a steel billet and grinding the steel billet; a high-speed wire rolling process in which the steel billet is rolled into a wire rod, the rolling start temperature being 1030-1060°C and the rolling end temperature being 950-1020°C; and a cooling step in which the wire rod is cooled at a controlled temperature on the Stelmor, with the first to fourth fans turned on and the airflow is 80% to 100%, and the remaining fans turned off.
[0008] More preferably, in the case of a vacuum melting process, the pressure inside the furnace is 5 Pa or less.
[0009] More preferably, in the case of a vacuum smelting process, industrially pure iron containing Al≦0.001%, Ti≦0.0005%, Cu≦0.001% and Ni≦0.001% is used as a raw material, alloy elements are mixed according to a composition design, and molten steel is smelted using a vacuum smelting furnace.
[0010] More preferably, in the case of a vacuum melting process, the casting temperature is 1580 to 1620°C.
[0011] More preferably, in the case of the steel ingot remelting process, after the remelted ingot is obtained by vacuum self-consumption remelting, the obtained remelted ingot is kept warm for 48 hours or more.
[0012] More preferably, in the case of the billet production process, the remelted ingot is bloomed or forged into a square billet having a length of 9 to 16 m and a size of 145 mm×145 mm.
[0013] More preferably, in the case of the billet manufacturing process, the remelted ingot is bloomed or forged at a temperature of 1130 to 1160°C.
[0014] More preferably, in the case of the grinding step, the total grinding depth relative to the steel billet surface is ≧1.5 mm.
[0015] More preferably, in the grinding process, the surface of the steel billet is ground using 16 mesh, 24 mesh, and 30 mesh grinding wheels in sequence, with the grinding depth of each pass being ≧0.9 mm, ≧0.5 mm, and ≧0.1 mm, respectively, and the corner grinding width being ≧5 mm.
[0016] More preferably, in the case of a high speed wire rolling process, the steel billet is rolled into a roughly drawn wire having a diameter of Φ4.5 to Φ5.5 mm.
[0017] More preferably, in the case of a high speed wire rolling process, the rolling end speed is 100 to 110 m / s.
[0018] More preferably, the laying temperature is 890 to 920°C in the case of a high speed wire rolling process.
[0019] More preferably, in the cooling step, the operating speed of the roller conveyor at the inlet portion before the first blower is 0.9 to 1.0 m / s.
[0020] More preferably, in the cooling step, all the heat-retaining covers are opened, and the operating speed ratio of the roller conveyors corresponding to the first to fourth blowers is 1.10:1.05:1.02:1.00.
[0021] More preferably, in the cooling step, the wind speed in the overlapping portion is adjusted to 1.1 to 1.4 times the wind speed in the non-overlapping portion using an air flow regulator (Optiflex).
[0022] More preferably, the production method further includes a heat treatment step of subjecting the rough wire after Stelmor cooling to a salt bath heat treatment or a lead bath heat treatment, in which the temperature of the isothermal phase change step is 520 to 560°C and the time is 20 to 80 s.
[0023] More preferably, when the wire rod produced by the above production method is packed with a packing wire, the packing wire and the wire rod are separated by a flexible wear-resistant material, and then aging treatment is performed, in which when the room temperature is ≧15° C., the aging treatment time is ≧10 days, and when the room temperature is <15° C., the aging treatment time is ≧20 days.
[0024] In order to achieve the above object of the invention, one embodiment of the present invention provides a wire rod for deep drawing, particularly a wire rod for drawing into a 5000 MPa class diamond wire, manufactured by the production method provided in any of the above embodiments. The chemical composition of the wire rod is, in mass percent, C: 1.01-1.10%, Si: 0.15-0.40%, Mn: 0.30-0.60%, Cr: 0.01-0.40%, and either or both of B: 0.0005-0.0020% and V: 0.01-0.09%, with the balance being Fe and unavoidable impurities, with the proviso that the impurities include Al≦0.003%, Ti≦0.0008%, S≦0.005%, P≦0.008%, O≦0.0010%, and N≦0.0020%.
[0025] Furthermore, the diameter of the roughly drawn wire is Φ4.5 to Φ5.5 mm.
[0026] Furthermore, the roughly drawn wire has a tensile strength of ≧1320 MPa and a cross-sectional area reduction of ≧30%.
[0027] Furthermore, the maximum inclusion size of the roughly drawn wire is ≦4 μm, and the mesh-like carbide is ≦1.0 grade.
[0028] Furthermore, the maximum inclusion size being ≦4 μm includes the maximum lateral inclusion size being ≦4 μm and the maximum longitudinal inclusion size being ≦4 μm.
[0029] Furthermore, the detection rate of mesh-like carbide is ≦30%, and the central carbon segregation ratio is ≦1.03.
[0030] Furthermore, the rough wire has a surface crack depth of ≦30 μm, a decarburized layer depth of ≦40 μm, a ratio of the decarburized layer to the entire circumference of ≦15%, and a surface scale thickness of 7 to 15 μm.
[0031] In order to achieve the above object of the invention, one embodiment of the present invention provides a wire rod for deep drawing, in particular a wire rod for drawing into a 5000 MPa class diamond wire, whose chemical composition, in mass percent, includes C: 1.01-1.10%, Si: 0.15-0.40%, Mn: 0.30-0.60%, Cr: 0.01-0.40%, and either or both of B: 0.0005-0.0020% and V: 0.01-0.09%, with the balance being Fe and unavoidable impurities, with the proviso that the impurities include Al≦0.003%, Ti≦0.0008%, S≦0.005%, P≦0.008%, O≦0.0010%, and N≦0.0020%; The tensile strength of the roughly drawn wire is ≧1320 MPa, the reduction in area is ≧30%, the maximum size of inclusions is ≦4 μm, and the mesh-like carbide is ≦1.0 grade. Effect of the Invention
[0032] Compared with the prior art, the beneficial effects of the present invention include the following (1), (2) and (3).
[0033] (1) By increasing the content of pearlite strengthening elements, especially the content of C element, in combination with the addition of B and / or V, and strictly controlling the content of impurity elements, the uniform structure is ensured, the formation of high melting point inclusions is avoided, and the cleanliness, tensile strength and drawability are improved.
[0034] (2) By controlling the furnace pressure in the vacuum melting process, and performing the electroslag remelting process under a protective atmosphere, and / or controlling the remelting speed in the vacuum self-consumption remelting process, the chemical components in the material are precisely controlled, the cleanliness is high, the occurrence of inclusions is greatly reduced, and the size of inclusions is small. In addition, by grinding the steel billet, the surface quality of the steel billet is optimized, and defects such as surface pits and decarburized layers of the steel billet are eliminated. In addition, by controlling the rolling start temperature in the high-speed wire rolling process, the steel billet is kept in the recrystallization region and rolled, and in combination with the temperature-controlled cooling in the cooling process, the cooling rate during and after the pearlite phase transformation process is avoided to be too fast, and the formation of martensite structure due to insufficient phase transformation time is prevented. At the same time, the internal stress is reduced, the structure performance is optimized, and the tensile strength and drawing performance of the rough wire are enhanced.
[0035] (3) The wire rod is applicable to the production of ultra-fine, high-strength diamond wire mother bar with low breakage rate, and can be produced by drawing diamond wire having a diameter of 40-46 μm, a breakage rate of ≦2 times / 1000 kilometers, and a tensile strength of ≧5000 MPa. The wire rod is suitable for producing diamond wire for cutting silicon wafers, and fully meets the market demand for steel wire with high drawing performance, low breakage rate and high strength, thereby filling the technical gap for wire rod for diamond wire of 5000 MPa or above at home and abroad. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0036] As mentioned in the background art, the conventional wire-drawing technique for high-strength diamond wire still has room for improvement, and cannot meet the increasingly high requirements for diameter, mileage without breakage, and strength of diamond wire, and in particular, there is still a blank state for wire-drawing suitable for industrialized production of 5000MPa-class diamond wire. Therefore, the present invention aims to provide a wire-drawing technique for deep drawing and a method for producing the same, in particular, a hypereutectoid steel wire-drawing technique that can be produced by drawing diamond wire and a method for producing the same, and the wire-drawing technique has the advantages of high cleanliness, high structure uniformity, and ultra-high strength, and can be used for producing 5000MPa-class diamond wire that is ultra-fine and has a low wire-breaking rate.
[0037] Hereinafter, the technical solutions of the present invention will be further described with reference to specific embodiments, but the scope of the claimed invention is not limited to the description provided.
[0038] First Embodiment This embodiment provides a wire rod for deep drawing, particularly a wire rod for drawing into a 5000MPa diamond wire. Of course, the wire rod can be used to draw into a 5000MPa diamond wire base wire, but is not limited thereto, and can be understood to be, for example, drawn into other steel wire products according to the actual production needs of enterprises.
[0039] The chemical components of the rough wire rod include, in mass percent, C: 1.01-1.10%, Si: 0.15-0.40%, Mn: 0.30-0.60%, Cr: 0.01-0.40%, and either or both of B: 0.0005-0.0020% and V: 0.01-0.09%, with the balance being Fe and unavoidable impurities, with the proviso that the impurities include Al≦0.003%, Ti≦0.0008%, S≦0.005%, P≦0.008%, O≦0.0010%, and N≦0.0020%.
[0040] The key idea in designing the chemical components of the wire rod in the present invention is to increase the content of pearlite strengthening elements, especially the content of C element, while ensuring the controllability of the structure and avoiding the formation of high melting point inclusions.
[0041] Specifically, the design principle of the chemical components of the wire rod will be described below.
[0042] C is the most important composition element, and the C content can significantly affect the strength of steel and directly affect the structure of steel. In detail, on the one hand, an increase in the C content can significantly increase the strength of steel, and on the other hand, in a general steel structure, the eutectoid structure in which C is involved in the formation can increase the strength and strain hardening rate of steel, but if the C content is too high, a pro-eutectoid network cementite structure can be formed, which destroys the continuity of the eutectoid structure and causes the formation of microcracks in the drawing process in which the steel wire is processed by rough drawing, and ultimately causes wire breakage. Therefore, in the chemical composition design of the present invention, the carbon content is increased as much as possible to increase the strength and strain hardening rate of the steel, and in combination with the content design of B or V, the occurrence of local network cementite structure is avoided, and based on this, the C content is 1.01 to 1.10%.
[0043] Although Si is a solid solution strengthening element, it can also be used to reduce the oxygen content in steel. However, if the Si content is too high, the plasticity of the steel material decreases, the tendency of the steel billet to decarbonize increases, and this is disadvantageous in controlling the surface quality of the wire rod. In the present invention, the Si content is 0.15 to 0.40%.
[0044] Mn is a solid solution strengthening element, which can increase the strength of the roughly drawn wire and also can reduce the thermal brittleness of the roughly drawn wire by combining with the harmful element S. However, if the Mn content is too high, the hardenability becomes strong, and bainite or martensite that affects drawing is likely to occur after the high-speed wire rolling process, and further, the plasticity and drawability of the roughly drawn wire are deteriorated. In the present invention, the Mn content is 0.30 to 0.60%.
[0045] Cr can increase the strength of the roughly drawn wire by refining the pearlite structure (i.e., eutectoid structure) and reducing the lamellar spacing of the pearlite structure. However, similar to Mn, if the Cr content is too high, the hardenability improves, and bainite or martensite that affects drawing is likely to occur after the high-speed wire rolling process, and further, the plasticity and drawability of the roughly drawn wire deteriorates. In the present invention, the Cr content is 0.01 to 0.40%.
[0046] Regarding B and V, The element B is involved in the formation of fine carbonitrides in high carbon steels, and is preferentially distributed at the austenite grain boundaries, which is advantageous in inhibiting the formation of a network-like cementite structure. However, if the B content is too high, it may embrittle the grain boundaries and reduce the drawability of the roughly drawn wire.
[0047] The V element is favorable for forming VC particles at the austenite grain boundaries at the beginning of the phase transition, suppressing the growth of austenite crystal grains during high-speed wire rolling, reducing the C content at the grain boundaries, and suppressing the formation of a network-like cementite structure. The V element is also favorable for increasing the strength of the wire-drawn by precipitating carbonitrides during the phase transition process. However, if the V content is too high, a hardened structure is easily generated, which is unfavorable for controlling the wire-drawn structure.
[0048] Both B and V elements can be used to inhibit the formation of a mesh-like cementite structure and are useful for increasing the upper limit of the C content, so as described above, the chemical composition of the wire rod contains either or both of B: 0.0005-0.0020% and V: 0.01-0.09%, i.e., the following three embodiments are included. The first embodiment is that the chemical composition of the wire rod contains B: 0.0005-0.0020% and does not contain V, and uses the B element to form fine carbonitrides at the austenite grain boundaries and inhibit the formation of a mesh-like cementite structure. The second embodiment is that the chemical composition of the wire rod does not contain B and contains V: 0.01-0.09%, and uses the V element to form VC particles at the early stage of phase transition and reduce the C content at the grain boundaries, inhibiting the formation of a mesh-like cementite structure. Thirdly, more preferably, the chemical components of the rough wire contain simultaneously 0.0005 to 0.0020% B and 0.01 to 0.09% V, on the one hand, the V element forms VC particles at the early stage of phase transition and reduces the C content at the grain boundaries, thereby inhibiting the formation of a mesh-like cementite structure, and on the other hand, the B element simultaneously forms fine carbonitrides at the austenite grain boundaries, thereby inhibiting the formation of a mesh-like cementite structure.
[0049] Al is a harmful element in deep drawing wire. Al combines with O in steel to form Al2O3 inclusions which are large in size, prone to agglomeration, have a high melting point and low plasticity. This is one of the main causes of breakage of thin wires during the production of steel wire by rough wire drawing. In the present invention, the Al content is within 0.003%.
[0050] Ti is a harmful element in deep drawing wire rods. Together with C and N, Ti is very likely to form large angular Ti(C,N) inclusions, which further cause stress concentration and microcracks. In the present invention, the Ti content is within 0.0008%.
[0051] S, P, O, and N are harmful impurity elements, with the contents of S≦0.005%, P≦0.008%, O≦0.0010%, and N≦0.0020%, respectively.
[0052] Furthermore, the diameter of the wire rod is Φ4.5-5.5mm, which can meet the requirements for producing steel wire by subsequent drawing.
[0053] Furthermore, since the tensile strength of the roughly drawn wire is ≧1320 MPa, the tensile strength of the produced steel wire is ≧5000 MPa. The roughly drawn wire has excellent drawing performance, and its cross-sectional reduction rate is ≧30%, which ensures a low wire breakage rate during the drawing process.
[0054] Furthermore, the rough wire has excellent internal quality and uniform structure, the maximum inclusion size is ≦4 μm, and the mesh-like carbide is ≦1.0 grade, where the maximum inclusion size ≦4 μm includes the maximum transverse inclusion size ≦4 μm and the maximum longitudinal inclusion size ≦4 μm, and further, the detection rate of mesh-like carbide is ≦30%, and the central carbon segregation ratio is ≦1.03, where the central carbon segregation ratio means the carbon content ratio between the region with the most severe segregation and the substrate position.
[0055] Furthermore, the rough wire has a surface crack depth of ≦30 μm, a decarburized layer depth of ≦40 μm, a ratio of the decarburized layer to the entire circumference of ≦15%, and a surface scale thickness of 7 to 15 μm.
[0056] From the above, the wire rod of this embodiment has high cleanliness, uniform structure, high mechanical performance and high drawing performance, and can satisfy the production of diamond wire. Furthermore, compared with the conventional technology of manufacturing diamond wire using wire rod, the wire rod of the present invention can be used to manufacture steel wire having a diameter of 40 to 46 μm, a wire breakage rate of ≦2 times / 1000 kilometers, and a tensile strength of ≧5000 MPa, fully meeting the market demand for steel wire with high drawing performance, low wire breakage rate, and high strength.
[0057] In one embodiment, a method for producing the wire rod is provided, in which the wire rod is produced by the steps of vacuum melting, remelting a steel ingot, making a billet and grinding, high speed wire rolling and cooling, which are carried out in sequence. a vacuum melting process in which alloy elements are blended in molten iron according to a composition design such as C: 1.01-1.10%, Si: 0.15-0.40%, Mn: 0.30-0.60%, Cr: 0.01-0.40%, and either or both of B: 0.0005-0.0020% and V: 0.01-0.09%, and the molten steel is smelted in a vacuum melting furnace under an atmosphere with an internal pressure of 10 Pa or less, and cast into a steel ingot; a steel ingot remelting process in a protective atmosphere by electroslag remelting to obtain a remelted ingot, the chemical composition of which is C, Si, Mn, Cr, and either or both of B and V, with the balance being Fe and unavoidable impurities, and the impurity elements are Al≦0.003%, Ti≦0.0008%, S≦0.005%, P≦0.008%, O≦0.0010%, and N≦0.0020%; a billet making and grinding process, which comprises blooming or forging the remelted ingot into a steel billet and grinding the steel billet; a high-speed wire rolling process in which the steel billet is rolled into a wire rod, the rolling start temperature being 1030-1060°C and the rolling end temperature being 950-1020°C; and a cooling step in which the wire rod is cooled at a controlled temperature on the Stelmor, with the first to fourth fans turned on and the airflow is 80% to 100%, and the remaining fans turned off.
[0058] Thus, by controlling the furnace pressure in the vacuum melting process and carrying out the electroslag remelting process under a protective atmosphere, the chemical components in the material are precisely controlled, the cleanliness is high, the occurrence of inclusions is greatly reduced, and the size of the inclusions is small. In addition, by grinding the steel billet, the surface quality of the steel billet is optimized, and defects such as surface pits and decarburized layers of the steel billet are eliminated. In addition, by controlling the rolling start temperature in the high-speed wire rolling process, the steel billet is kept in the recrystallization region and rolled, and combined with the temperature-controlled cooling in the cooling process, the cooling rate during and after the pearlite phase transformation process is avoided to be too fast, and the formation of martensite structure due to insufficient phase transformation time is prevented, and at the same time, the internal stress is reduced, the structure performance is optimized, and the tensile strength and drawing performance of the rough wire are enhanced.
[0059] A preferred implementation of each step is described in detail below.
[0060] (1) Vacuum melting process In the vacuum smelting process, based on the design concept of the chemical components of the rough wire described above, alloy elements are blended in molten iron in accordance with a composition design such as 1.01-1.10% C, 0.15-0.40% Si, 0.30-0.60% Mn, 0.01-0.40% Cr, and either or both of 0.0005-0.0020% B and 0.01-0.09% V, to produce molten steel.
[0061] Preferably, the raw materials and auxiliary materials used in the vacuum smelting process are high quality raw materials and auxiliary materials with low impurity element contents. For example, the raw material is industrial pure iron with Al≦0.001%, Ti≦0.0005%, Cu≦0.001% and Ni≦0.001%, and alloy elements are mixed according to the composition design. That is, the above-mentioned molten iron is made by melting industrial pure iron with Al≦0.001%, Ti≦0.0005%, Cu≦0.001% and Ni≦0.001%. Naturally, the impurity elements in the industrial pure iron, which is the raw material of the molten iron, are preferably, but not necessarily limited to, the above-mentioned contents. In this way, the harmful elements can be reduced and the cleanliness can be increased from the early stage of smelting the molten steel, which is also advantageous for the subsequent precise control of inclusions.
[0062] In the vacuum melting process, molten steel is smelted in a vacuum melting furnace under an atmosphere with an internal pressure of 10 Pa or less, and cast into a steel ingot. Here, controlling the internal pressure of the furnace to 10 Pa or less maintains the inside of the furnace at a high vacuum, which is advantageous in preventing the effects of the O and N elements in the air on the molten steel and controlling the contents of the harmful elements O and N in the molten steel to low levels. More preferably, the internal pressure of the furnace is controlled to 5 Pa or less.
[0063] Preferably, in the vacuum melting process, in the process of casting the molten steel into a steel ingot, the casting temperature is 1580-1620°C, that is, the molten steel is cast into an ingot when the temperature is heated to 1580-1620°C, and the casting speed is 300-400 kg / min, which on the one hand can further ensure the cleanliness of the molten steel, and on the other hand can ensure that the core solute of the steel ingot can be sufficiently diffused, and the center segregation of the steel ingot can be reduced.
[0064] (2) Steel ingot remelting process In the steel ingot remelting process, the steel ingot obtained in the vacuum melting process is subjected to electroslag remelting treatment under a protective atmosphere to obtain a remelted ingot, the chemical composition of which is C, Si, Mn, Cr, and either or both of B and V, with the balance being Fe and unavoidable impurities, and the impurity elements are Al≦0.003%, Ti≦0.0008%, S≦0.005%, P≦0.008%, O≦0.0010%, and N≦0.0020%.
[0065] That is, the steel ingot remelting process, combined with the precise control of the vacuum melting process, achieves strict control over impurity elements (i.e., harmful elements) in the material, thereby ensuring high cleanliness, greatly reducing the occurrence of inclusions, reducing the size of inclusions, and ensuring uniform chemical composition.
[0066] Here, if electroslag remelting is performed under the protective atmosphere, it is possible to ensure that the molten steel is not oxidized and to reduce the occurrence of inclusions. Specifically, the protective atmosphere may be an atmosphere consisting of an inert gas. For example, air is discharged from within the electroslag furnace and replaced with an inert gas, and then the steel ingot is subjected to the remelting process.
[0067] (3) Billet manufacturing process and grinding process In the billet manufacturing process, the remelted ingot obtained in the steel ingot remelting process is bloomed or forged into a steel billet. Preferably, the steel billet is a square billet having a length of 9 to 16 m and a size of 145 mm x 145 mm, although the dimensions of the steel billet are not limited to these and may be any industrially feasible size.
[0068] More preferably, in the billet manufacturing process, the remelted ingot is bloomed or forged at a temperature of 1130 to 1160°C, which further ensures temperature uniformity between the core and surface of the steel billet, and is advantageous in improving structural uniformity.
[0069] In the grinding process, the steel billet obtained in the billet making process is ground to optimize the surface quality of the steel billet, remove defects such as surface pits and decarburized layers of the steel billet, and further lay a good foundation for the subsequent high-speed wire rolling.
[0070] Preferably, in the grinding process, the total grinding depth of the steel billet surface is ≧1.5mm. Specifically, the surface of the steel billet is ground by successively using 16 mesh, 24 mesh, and 30 mesh grindstones, and the grinding depth of each pass is ≧0.9mm, ≧0.5mm, and ≧0.1mm, respectively, that is, the surface grinding depth of the steel billet by the 16 mesh grindstone is ≧0.9mm, the surface grinding depth of the steel billet by the 24 mesh grindstone is ≧0.5mm, and the surface grinding depth of the steel billet by the 30 mesh grindstone is ≧0.1mm. In addition, the grinding width for the corner of the steel billet is ≧5mm, specifically, the corner of the steel billet is bevel-ground, and the width of the slope formed at the corner after completion is the corner grinding width. Thus, the grinding process finally ensures that the surface of the steel billet is smooth and burr-free.
[0071] (4) High-speed wire rolling process In the high-speed wire rolling process, the steel billet is rolled into a roughly drawn wire, and the soaking temperature during heating before rolling is adjusted to set the rolling start temperature to 1030-1060°C, and the rolling end temperature is set to 950-1020°C by temperature control means such as water cooling during the rolling process, thereby ensuring that the steel billet is basically kept within the recrystallization region during rolling, and precisely controlling the structure of the roughly drawn wire to avoid the generation of bainite, martensite, and network cementite structures.
[0072] Preferably, in the high speed wire rolling process, the steel billet is rolled into a wire rod having a diameter of Φ4.5-5.5 mm, i.e., the diameter of the wire rod finally produced by the production method of this embodiment is Φ4.5-5.5 mm, so as to meet the requirements of steel wire production by subsequent drawing.
[0073] Preferably, in the high-speed wire rolling process, the rolling end speed is 100 to 110 m / s, which further ensures that the steel billet is essentially kept within the recrystallization region during rolling, and the laying temperature is 890 to 920°C, which more precisely controls the structure of the roughly drawn wire and is advantageous for temperature control during subsequent air cooling.
[0074] (5) Cooling process In the cooling process, the wire rod is cooled at a controlled temperature on a Stelmor, the first to fourth fans are turned on and the air volume is 80% to 100%, and the remaining fans are turned off, that is, the temperature controlled cooling process is performed using the Stelmor air cooling technology. The cooling method of the present invention can avoid the cooling rate during and after the pearlite phase transformation process being too fast, and prevent the formation of martensite structure due to insufficient phase transformation time, while at the same time reducing internal stress, optimizing the structure performance, and further enhancing the tensile strength and drawability of the wire rod.
[0075] Preferably, during the cooling process, all the thermal insulation covers on the stelmor are opened, i.e., air cooling is performed on the roller conveyor segments corresponding to the first four blowers, and natural cooling is performed on all roller conveyor segments corresponding to the remaining blowers.
[0076] Preferably, before the first blower, the operating speed of the roller conveyor inlet portion is 0.9-1.0 m / s, the operating speed ratio of the roller conveyors corresponding to the first to fourth blowers is 1.10:1.05:1.02:1.00, and the operating speed ratio of the roller conveyors corresponding to the remaining blowers is 0.8:1.00-1.05:1.00.
[0077] In addition, in the cooling process, an air flow regulator is used to adjust the air speed in the overlapping areas to 1.1 to 1.4 times that in the non-overlapping areas, thereby ensuring a balance in the cooling rates of the overlapping and non-overlapping areas and making it easier to obtain more uniform structural performance.
[0078] More preferably, the wire rod produced by the above production method can be packed in a packing wire, and a flexible wear-resistant material is interposed between the packing wire and the wire rod so that the packing wire does not scratch the wire rod during transportation, transfer, and storage. Then, an aging treatment is performed, in which the aging treatment time is ≥ 10 days when the room temperature is ≥ 15°C, and the aging treatment time is ≥ 20 days when the room temperature is < 15°C.
[0079] Compared with the prior art, the beneficial effects of one embodiment of the present invention are as follows:
[0080] (1) By increasing the content of pearlite strengthening elements, especially the content of C element, in combination with the addition of B and / or V, and strictly controlling the content of impurity elements, the structure is ensured to be uniform, the formation of high melting point inclusions is avoided, and the cleanliness, tensile strength and drawability are improved.
[0081] (2) By controlling the furnace pressure in the vacuum melting process and carrying out the electroslag remelting process under a protective atmosphere, the chemical components in the material are precisely controlled, the cleanliness is high, the occurrence of inclusions is greatly reduced, and the size of the inclusions is small. In addition, by grinding the steel billet, the surface quality of the steel billet is optimized, and defects such as surface pits and decarburized layers of the steel billet are eliminated. In addition, by controlling the rolling start temperature in the high-speed wire rolling process, the steel billet is kept in the recrystallization region and rolled, and combined with the temperature-controlled cooling in the cooling process, the cooling rate during and after the pearlite phase transformation process is avoided to be too fast, and the formation of martensite structure due to insufficient phase transformation time is prevented. At the same time, the internal stress is reduced, the structure performance is optimized, and the tensile strength and drawing performance of the rough wire are enhanced.
[0082] (3) The above-mentioned wire rod is applicable to the production of ultra-fine, high-strength diamond wire steel wire with low breakage rate, and can be produced by drawing diamond wire having a diameter of 40-46 μm, a breakage rate of ≦2 times / 1000 kilometers, and a tensile strength of ≧5000 MPa. The wire rod is suitable for producing diamond wire for cutting silicon wafers, fully meeting the market demand for steel wire with high drawing performance, low breakage rate and high strength, and filling the technical gap for wire rod for diamond wire of 5000 MPa or above at home and abroad.
[0083] <Second embodiment> The present embodiment also provides a wire rod for deep drawing, particularly a wire rod for drawing as a 5000 MPa-class diamond wire, and a method for producing the wire rod. The difference between the present embodiment and the first embodiment is the steel ingot remelting step in the production method, and all other techniques are the same as those in the first embodiment. Hereinafter, only the differences between the present embodiment and the first embodiment will be described, and the remaining similar parts will not be described any further.
[0084] In this embodiment, step (2) of the production method, the steel ingot remelting step, is specifically as follows.
[0085] In the steel ingot remelting process, the steel ingot is treated by vacuum self-consumption remelting, and the remelting rate is 3.0-3.5 kg / min to obtain a remelted ingot, the chemical composition of which is C, Si, Mn, Cr, and either or both of B and V, with the balance being Fe and unavoidable impurities, and the impurity elements are Al≦0.003%, Ti≦0.0008%, S≦0.005%, P≦0.008%, O≦0.0010%, and N≦0.0020%.
[0086] That is, the steel ingot remelting process, combined with the precise control of the vacuum melting process, provides strict control over impurity elements (i.e., harmful elements) in the material, thereby ensuring high cleanliness, greatly reducing the occurrence of inclusions, reducing inclusion size, controlling inclusion type, and providing uniform chemical composition.
[0087] Specifically, in the steel ingot remelting process, vacuum self-consumption remelting is performed using the steel ingot obtained in the vacuum melting process as an electrode.
[0088] In addition, in the steel ingot remelting process, after obtaining the remelted ingot through vacuum self-consumption remelting, the obtained remelted ingot is kept warm for more than 48 hours, thereby further reducing the stress cracks on the surface and core of the remelted ingot.
[0089] In summary, in the steel ingot remelting process of this embodiment, vacuum self-consumption remelting is adopted instead of electroslag remelting in the first embodiment, and everything else is the same as in the first embodiment. Therefore, this embodiment has the same beneficial effects as the first embodiment, and detailed description will be omitted.
[0090] <Third embodiment> The present embodiment also provides a wire rod for deep drawing, particularly a wire rod for drawing as a 5000 MPa-class diamond wire, and a method for producing the wire rod. The difference between the present embodiment and the first embodiment is the steel ingot remelting step in the production method, and all other techniques are the same as those in the first embodiment. Hereinafter, only the differences between the present embodiment and the first embodiment will be described, and the remaining similar parts will not be described any further.
[0091] In this embodiment, step (2) of the production method, the steel ingot remelting step, is specifically as follows.
[0092] In the steel ingot remelting process, first, the steel ingot obtained in the vacuum melting process is subjected to electroslag remelting treatment under a protective atmosphere, and then the remelted ingot obtained by electroslag remelting is used as an electrode and processed by vacuum self-consumption remelting, with a remelting rate of 3.0-3.5 kg / min, to obtain a remelted ingot, whose chemical composition is C, Si, Mn, Cr, and either or both of B and V, with the balance being Fe and unavoidable impurities, and the impurity elements are Al≦0.003%, Ti≦0.0008%, S≦0.005%, P≦0.008%, O≦0.0010%, and N≦0.0020%.
[0093] Furthermore, in the present embodiment, in the steel ingot remelting process, after the remelted ingot is obtained by vacuum self-consumption remelting, the obtained remelted ingot is kept warm for 48 hours or more, thereby further reducing stress cracks on the surface and core of the remelted ingot.
[0094] In summary, the electroslag remelting process in this embodiment is the same as that in the first embodiment, and the vacuum self-consumption remelting is further added to the first embodiment, which can more precisely control the impurity elements (i.e., harmful elements) and further guarantee the cleanliness and inclusions. Other than that, this embodiment also has the beneficial effects of the first embodiment, and a detailed description is omitted.
[0095] Of course, in an alternative embodiment, the order of performing vacuum autogenous remelting and electroslag remelting may be reversed, i.e., vacuum autogenous remelting may be performed first, followed by electroslag remelting.
[0096] <Fourth embodiment> This embodiment also provides a wire rod for deep drawing, particularly a wire rod for drawing as a 5000 MPa-class diamond wire, and a method for producing the wire rod. The only difference between this embodiment and the first, second, and third embodiments is that the production method further includes a heat treatment step added after the cooling step, and all other techniques are the same as those of the first, second, and third embodiments. Hereinafter, only the above differences will be described, and the remaining same parts will not be described any further.
[0097] In this embodiment, the production method further includes the following step (6).
[0098] (6) Heat treatment process The wire rod after Stelmor cooling is subjected to salt bath heat treatment or lead bath heat treatment, in which the temperature of the isothermal phase change step is 520-560° C. and the time is 20-80 s.
[0099] As a result, in this embodiment, the rough wire rod obtained has more uniform texture, and has stronger drawability and tensile strength than the first, second, and third embodiments.
[0100] The technical solutions of the present invention are further illustrated below through several embodiments of the present invention.
[0101] Example 1 Example 1 provides a wire rod having a diameter of Φ5.5 mm, whose chemical composition, in mass percent, includes C: 1.01%, Si: 0.30%, Mn: 0.60%, Cr: 0.40%, B: 0.0013%, V: 0.09%, and the balance is Fe and unavoidable impurities, with the proviso that the impurities include Al: 0.001%, Ti: 0.0006%, S: 0.003%, P: 0.006%, O: 0.0008%, and N: 0.0012%.
[0102] The structural performance of the wire rod of this embodiment is detected so as to include the following first and second cases.
[0103] In the first case, 12 samples were taken per wire rod and each was inspected. The tensile strength was 1320-1350 MPa and the reduction in area was 35-40%.
[0104] In the second case, 12 samples are taken per rough wire, including 6 longitudinal section samples and 6 transverse section samples. After polishing, the maximum surface crack depth, scale thickness, maximum transverse inclusion dimension (abbreviated as transverse inclusion dimension in the table), maximum longitudinal inclusion dimension (abbreviated as longitudinal inclusion dimension in the table) and mesh-like carbide level (abbreviated as mesh carbon level in the table) of each sample are observed and measured using a metallographic microscope, the central carbon segregation ratio is detected and analyzed using an electron probe, and each sample is corroded and then the maximum decarburized layer depth and the percentage of the decarburized layer to the entire circumference (abbreviated as decarburization percentage in the table) are observed.
[0105] [Table 1]
[0106] As can be seen from this, the wire rod of this embodiment has high cleanliness, uniform structure, high tensile strength and high drawing performance, and can meet the high market demand for wire rods for deep drawing. Furthermore, when the wire rod of this embodiment is used as a base material and a conventional diamond wire manufacturing process is used to manufacture a diamond wire mother wire for cutting silicon wafers, the resulting diamond wire has a tensile strength of 5300 MPa, a diameter of 46 μm, and a wire breakage rate of approximately 1.2 times / 1000 kilometers, which is far superior to the conventional technology.
[0107] Example 2 Example 2 provides a wire rod having a diameter of Φ5.0 mm, whose chemical composition, in mass percent, includes C: 1.03%, Si: 0.18%, Mn: 0.58%, Cr: 0.36%, B: 0.002%, and the balance is Fe and unavoidable impurities, with the proviso that the impurities include Al: 0.001%, Ti: 0.0005%, S: 0.002%, P: 0.004%, O: 0.001%, and N: 0.0013%.
[0108] The structural performance of the wire rod of this embodiment is detected so as to include the following first and second cases.
[0109] In the first case, 12 samples were taken per wire rod and each was inspected. The tensile strength was 1330-1360 MPa and the reduction in area was 33-40%.
[0110] In the second case, 12 samples were taken per wire rod, including 6 longitudinal section samples and 6 transverse section samples. After polishing, the maximum surface crack depth, scale thickness, maximum transverse inclusion dimension (abbreviated as transverse inclusion dimension in the table), maximum longitudinal inclusion dimension (abbreviated as longitudinal inclusion dimension in the table) and mesh-like carbide level (abbreviated as mesh carbon level in the table) of each sample were observed and measured using a metallographic microscope, the central carbon segregation ratio was detected and analyzed using an electron probe, and each sample was corroded and then the maximum decarburized layer depth and the percentage of the decarburized layer to the entire circumference (abbreviated as decarburization percentage in the table) were observed.
[0111] [Table 2]
[0112] As can be seen from this, the wire rod of this embodiment has high cleanliness, uniform structure, high tensile strength and high drawing performance, and can meet the high market requirements for wire rods for deep drawing. Furthermore, when the wire rod of this embodiment is used as a base material and a conventional diamond wire manufacturing process is adopted to manufacture a diamond wire mother wire for cutting silicon wafers, the resulting diamond wire has a tensile strength of 5500 MPa, a diameter of 45 μm, and a wire breakage rate of approximately 1.5 times / 1000 kilometers, which is far superior to the conventional technology.
[0113] Example 3 Example 3 provides a wire rod having a diameter of Φ5.5 mm, whose chemical composition, in mass percent, includes C: 1.03%, Si: 0.20%, Mn: 0.55%, Cr: 0.22%, V: 0.06%, and the balance is Fe and unavoidable impurities, with the proviso that the impurities include Al: 0.002%, Ti: 0.0006%, S: 0.002%, P: 0.006%, O: 0.0006%, and N: 0.0008%.
[0114] The structural performance of the wire rod of this embodiment is detected so as to include the following first and second cases.
[0115] In the first case, 12 samples were taken per wire rod and each was inspected. The tensile strength was 1320-1350 MPa and the reduction in area was 33-39%.
[0116] In the second case, 12 samples are taken per wire rod, including 6 longitudinal section samples and 6 transverse section samples. After polishing, the maximum surface crack depth, scale thickness, maximum transverse inclusion dimension (abbreviated as transverse inclusion dimension in the table), maximum longitudinal inclusion dimension (abbreviated as longitudinal inclusion dimension in the table) and mesh-like carbide level (abbreviated as mesh carbon level in the table) of each sample are observed and measured using a metallographic microscope, an electron probe is used to detect and analyze the central carbon segregation ratio, and each sample is corroded and then the maximum decarburized layer depth and the percentage of the decarburized layer to the entire circumference (abbreviated as decarburization percentage in the table) are observed.
[0117] [Table 3]
[0118] As can be seen from this, the wire rod of this embodiment has high cleanliness, uniform structure, high tensile strength and high drawing performance, and can meet the high market requirements for wire rods for deep drawing. Furthermore, when the wire rod of this embodiment is used as a base material and a conventional diamond wire manufacturing process is adopted to manufacture a diamond wire mother wire for cutting silicon wafers, the resulting diamond wire has a tensile strength of 5500 MPa, a diameter of 45 μm, and a wire breakage rate of approximately 1.6 times / 1000 kilometers, which is far superior to the conventional technology.
[0119] Example 4 Example 4 provides a wire rod having a diameter of Φ4.5 mm, whose chemical composition, in mass percent, includes C: 1.05%, Si: 0.16%, Mn: 0.55%, Cr: 0.01%, B: 0.0005%, V: 0.04%, and the balance is Fe and unavoidable impurities, with the proviso that the impurities include Al: 0.002%, Ti: 0.0003%, S: 0.001%, P: 0.003%, O: 0.0003%, and N: 0.0009%.
[0120] The structural performance of the wire rod of this embodiment is detected so as to include the following first and second cases.
[0121] In the first case, 12 samples were taken per wire rod and each was inspected. The tensile strength was 1320-1360 MPa and the reduction in area was 32-38%.
[0122] In the second case, 12 samples were taken per wire rod, including 6 longitudinal section samples and 6 transverse section samples. After polishing, the maximum surface crack depth, scale thickness, maximum transverse inclusion dimension (abbreviated as transverse inclusion dimension in the table), maximum longitudinal inclusion dimension (abbreviated as longitudinal inclusion dimension in the table) and mesh-like carbide level (abbreviated as mesh carbon level in the table) of each sample were observed and measured using a metallographic microscope, and the central carbon segregation ratio was detected and analyzed using an electron probe. After etching each sample, the maximum decarburized layer depth and the percentage of the decarburized layer to the entire circumference (abbreviated as decarburization percentage in the table) were observed.
[0123] [Table 4]
[0124] As can be seen from this, the wire rod of this embodiment has high cleanliness, uniform structure, high tensile strength and high drawing performance, and can meet the high market requirements for wire rods for deep drawing. Furthermore, when the wire rod of this embodiment is used as a base material and a conventional diamond wire manufacturing process is adopted to manufacture a diamond wire mother wire for cutting silicon wafers, the resulting diamond wire has a tensile strength of 5500 MPa, a diameter of 40 μm, and a wire breakage rate of approximately 1.8 times / 1000 kilometers, which is far superior to the conventional technology.
[0125] Example 5 Example 5 provides a wire rod having a diameter of Φ5.5 mm, whose chemical composition, in mass percent, includes C: 1.05%, Si: 0.22%, Mn: 0.45%, Cr: 0.19%, B: 0.001%, and the balance is Fe and unavoidable impurities, with the proviso that the impurities include Al: 0.001%, Ti: 0.0002%, S: 0.003%, P: 0.004%, O: 0.0005%, and N: 0.001%.
[0126] The structural performance of the wire rod of this embodiment is detected so as to include the following first and second cases.
[0127] In the first case, 12 samples were taken per wire rod and each was inspected. The tensile strength was 1340-1380 MPa and the reduction in area was 30-38%.
[0128] In the second case, 12 samples were taken per wire rod, including 6 longitudinal section samples and 6 transverse section samples. After polishing, the maximum surface crack depth, scale thickness, maximum transverse inclusion dimension (abbreviated as transverse inclusion dimension in the table), maximum longitudinal inclusion dimension (abbreviated as longitudinal inclusion dimension in the table) and mesh-like carbide level (abbreviated as mesh carbon level in the table) of each sample were observed and measured using a metallographic microscope, an electron probe was used to detect and analyze the central carbon segregation ratio, and each sample was corroded and then the maximum decarburized layer depth and the percentage of the decarburized layer to the entire circumference (abbreviated as decarburization percentage in the table) were observed.
[0129] [Table 5]
[0130] As can be seen from this, the wire rod of this embodiment has high cleanliness, uniform structure, high tensile strength and high drawing performance, and can meet the high market demand for wire rods for deep drawing. Furthermore, when the wire rod of this embodiment is used as a base material and a conventional diamond wire manufacturing process is adopted to manufacture a diamond wire mother wire for cutting silicon wafers, the resulting diamond wire has a tensile strength of 6100 MPa, a diameter of 40 μm, and a wire breakage rate of approximately 1.9 times / 1000 kilometers, which is far superior to the conventional technology.
[0131] Example 6 Example 6 provides a wire rod having a diameter of Φ5.0 mm, whose chemical composition, in mass percent, includes C: 1.08%, Si: 0.25%, Mn: 0.32%, Cr: 0.18%, V: 0.01%, and the balance is Fe and unavoidable impurities, with the proviso that the impurities include Al: 0.001%, Ti: 0.0005%, S: 0.001%, P: 0.003%, O: 0.0004%, and N: 0.0006%.
[0132] The structural performance of the wire rod of this embodiment is detected so as to include the following first and second cases.
[0133] In the first case, 12 samples were taken per wire rod and each was inspected. The tensile strength was 1350-1400 MPa and the reduction in area was 30-38%.
[0134] In the second case, 12 samples are taken per wire rod, including 6 longitudinal section samples and 6 transverse section samples. After polishing, the maximum surface crack depth, scale thickness, maximum transverse inclusion dimension (abbreviated as transverse inclusion dimension in the table), maximum longitudinal inclusion dimension (abbreviated as longitudinal inclusion dimension in the table) and mesh-like carbide level (abbreviated as mesh carbon level in the table) of each sample are observed and measured using a metallographic microscope, an electron probe is used to detect and analyze the central carbon segregation ratio, and each sample is corroded and then the maximum decarburized layer depth and the percentage of the decarburized layer to the entire circumference (abbreviated as decarburization percentage in the table) are observed.
[0135] [Table 6]
[0136] As can be seen from this, the wire rod of this embodiment has high cleanliness, uniform structure, high tensile strength and high drawing performance, and can meet the high market requirements for wire rods for deep drawing. Furthermore, when the wire rod of this embodiment is used as a base material and a conventional diamond wire manufacturing process is adopted to manufacture a diamond wire mother wire for cutting silicon wafers, the resulting diamond wire has a tensile strength of 6400 MPa, a diameter of 45 μm, and a wire breakage rate of approximately 1.9 times / 1000 kilometers, which is far superior to the conventional technology.
[0137] Example 7 Example 7 provides a wire rod having a diameter of Φ5.5 mm, whose chemical composition, in mass percent, includes C: 1.10%, Si: 0.16%, Mn: 0.30%, Cr: 0.15%, V: 0.05%, and the balance is Fe and unavoidable impurities, with the proviso that the impurities include Al: 0.001%, Ti: 0.0002%, S: 0.002%, P: 0.003%, O: 0.0002%, and N: 0.0009%.
[0138] The structural performance of the wire rod of this embodiment is detected so as to include the following first and second cases.
[0139] In the first case, 12 samples were taken per wire rod and each was inspected. The tensile strength was 1340-1390 MPa and the reduction in area was 32-38%.
[0140] In the second case, 12 samples are taken per wire rod, including 6 longitudinal section samples and 6 transverse section samples. After polishing, the maximum surface crack depth, scale thickness, maximum transverse inclusion dimension (abbreviated as transverse inclusion dimension in the table), maximum longitudinal inclusion dimension (abbreviated as longitudinal inclusion dimension in the table) and mesh-like carbide level (abbreviated as mesh carbon level in the table) of each sample are observed and measured using a metallographic microscope, and the central carbon segregation ratio is detected and analyzed using an electronic probe. After etching each sample, the maximum decarburized layer depth and the percentage of the decarburized layer to the entire circumference (abbreviated as decarburization percentage in the table) are observed.
[0141] [Table 7]
[0142] As can be seen from this, the wire rod of this embodiment has high cleanliness, uniform structure, high tensile strength and high drawing performance, and can meet the high market demand for wire rods for deep drawing. Furthermore, when the wire rod of this embodiment is used as a base material and a conventional diamond wire manufacturing process is used to manufacture a diamond wire mother wire for cutting silicon wafers, the resulting cutting diamond wire has a tensile strength of 6000 MPa, a diameter of 46 μm, and a wire breakage rate of approximately 2.0 times / 1000 kilometers, which is far superior to the conventional technology.
[0143] Example 8 Example 8 provides a method for producing the wire rod of Example 1. The method specifically includes the following steps (1), (2), (3), (4), and (5).
[0144] (1) Vacuum melting process Using industrially pure iron with Al≦0.001%, Ti≦0.0005%, Cu≦0.001% and Ni≦0.001% as the raw material, alloy elements are blended into molten iron in accordance with a composition design of C: 1.01-1.10%, Si: 0.15-0.40%, Mn: 0.30-0.60%, Cr: 0.01-0.40%, B: 0.0005-0.0020%, and V: 0.01-0.09%, and the pressure inside the vacuum smelting furnace is maintained at 5 Pa, thereby smelting molten steel.
[0145] When the temperature of the smelted molten steel is heated to 1580-1600°C, it is protected under an inert gas atmosphere and cast into an ingot at a casting speed of 370 kg / min.
[0146] (2) Steel ingot remelting process First, the steel ingot obtained in the vacuum melting process is subjected to electroslag remelting treatment under an inert gas atmosphere, and then the remelted ingot obtained by electroslag remelting is used as an electrode to be processed by vacuum self-consumption remelting, with a remelting rate of 3.2 kg / min to obtain a remelted ingot, which is then kept warm for 60 hours.
[0147] The chemical composition of the remelted ingot was found to be, in mass percent, C: 1.01%, Si: 0.30%, Mn: 0.60%, Cr: 0.40%, B: 0.0013%, V: 0.09%, and the remainder Fe and unavoidable impurities, with the proviso that the impurities included Al: 0.001%, Ti: 0.0006%, S: 0.003%, P: 0.006%, O: 0.0008%, and N: 0.0012%.
[0148] (3) Billet manufacturing process and grinding process The remelted ingot obtained in the steel ingot remelting process is forged at a temperature of 1150°C into a steel billet, which is a square billet with a length of 12 m and a size of 145 mm x 145 mm, and then the surface of the steel billet is ground using 16 mesh, 24 mesh, and 30 mesh grinding wheels in sequence, the surface grinding depth of the steel billet by the 16 mesh grinding wheel is approximately 1 mm, the surface grinding depth of the steel billet by the 24 mesh grinding wheel is approximately 0.6 mm, the surface grinding depth of the steel billet by the 30 mesh grinding wheel is approximately 0.2 mm, the total grinding depth on one side is approximately 1.8 mm (correspondingly, the total grinding depth on both sides is approximately 3.6 mm), the corner grinding width is 6 mm, and the steel billet surface after grinding is smooth and burr-free.
[0149] (4) High-speed wire rolling process The ground steel billet is sent to a high-speed wire rolling machine and rolled into a rough wire with a diameter of Φ5.5 mm. The soaking temperature during heating before rolling is adjusted to set the rolling start temperature to 1030-1050°C, and the rolling end temperature is set to 980-1020°C by temperature control means such as water cooling during the rolling process, thereby ensuring that the steel billet is essentially kept within the recrystallization region during rolling.
[0150] The rolling end speed is 105 m / s, and the laying temperature is 890 to 910°C.
[0151] (5) Cooling process The wire rod is cooled at a controlled temperature on the Stelmor, the first to fourth fans are turned on and the airflow is 100%, 100%, 100%, 90% in sequence, the remaining fans are turned off, and all the thermal covers on the Stelmor are opened.
[0152] Before the first blower, the operating speed of the roller conveyor inlet part is 0.9m / s, the operating speed ratio of the roller conveyors corresponding to the first to fourth blowers is 1.10:1.05:1.02:1.00, and the operating speed ratio of the roller conveyors corresponding to the remaining blowers is 0.8:1.00~1.05:1.00. In addition, the wind speed of the overlapping part is adjusted to 1.25 times that of the non-overlapping part using an air volume adjustment device to ensure the cooling speed balance between the overlapping part and the non-overlapping part.
[0153] According to the production method of the present embodiment, the roughly drawn wire of the first embodiment can be obtained.
[0154] The wire rod is wrapped in a packing wire, and the wire rod is separated from the packing wire by linen cloth, and then wrapped and fixed. The room temperature during high-speed wire rolling is 25°C, and the natural aging treatment time is 12 days, after which the wire rod is transported to the user for drawing. Here, during transportation and transfer, a rubber pad is laid to avoid scratches on the wire rod.
[0155] Example 9 Example 9 provides a method for producing the wire rod of Example 2. The method specifically includes the following steps (1), (2), (3), (4), and (5).
[0156] (1) Vacuum melting process Using industrially pure iron with low impurity element content as the raw material, alloy elements are blended into the molten iron according to a composition design of C: 1.01-1.10%, Si: 0.15-0.40%, Mn: 0.30-0.60%, Cr: 0.01-0.40%, and B: 0.0005-0.0020%. The pressure inside the vacuum smelting furnace is maintained at 6 Pa, and molten steel is produced.
[0157] When the temperature of the smelted molten steel is heated to 1600-1620°C, it is protected under an inert gas atmosphere and cast into an ingot at a casting speed of 360 kg / min.
[0158] (2) Steel ingot remelting process The steel ingot obtained in the vacuum melting process is used as an electrode, and processed by vacuum self-consumption remelting, the remelting speed is 3.5 kg / min, and the remelted ingot is obtained. The remelted ingot is then kept warm for 72 hours, and then stacked in a wind-proof place to allow it to cool naturally.
[0159] The chemical composition of the remelted ingot was found to be, in mass percent, C: 1.03%, Si: 0.18%, Mn: 0.58%, Cr: 0.36%, B: 0.002%, with the remainder being Fe and unavoidable impurities, with the proviso that the impurities included Al: 0.001%, Ti: 0.0005%, S: 0.002%, P: 0.004%, O: 0.001%, and N: 0.0013%.
[0160] (3) Billet manufacturing process and grinding process The remelted ingot obtained in the steel ingot remelting process is forged at a temperature of 1130°C into a steel billet, which is a square billet with a length of 13 m and a size of 145 mm x 145 mm, and then the surface of the steel billet is ground using 16 mesh, 24 mesh, and 30 mesh grinding wheels in sequence, the surface grinding depth of the steel billet by the 16 mesh grinding wheel is approximately 1.2 mm, the surface grinding depth of the steel billet by the 24 mesh grinding wheel is approximately 0.5 mm, the surface grinding depth of the steel billet by the 30 mesh grinding wheel is approximately 0.3 mm, the total grinding depth on one side is approximately 2 mm (correspondingly, the total grinding depth on both sides is approximately 4 mm), the corner grinding width is 9 mm, and the steel billet surface after grinding is smooth and burr-free.
[0161] (4) High-speed wire rolling process The ground steel billet is sent to a high-speed wire rolling machine and rolled into a rough wire with a diameter of Φ5.0 mm. The soaking temperature during heating before rolling is adjusted to set the rolling start temperature to 1040-1060°C, and the rolling end temperature is set to 960-1010°C by temperature control means such as water cooling during the rolling process, thereby ensuring that the steel billet is essentially kept within the recrystallization region during rolling.
[0162] The rolling end speed is 103 m / s, and the laying temperature is 900 to 920°C.
[0163] (5) Cooling process The wire rod is cooled at a controlled temperature on the Stelmor, the first to fourth fans are turned on and the airflow is 100%, 100%, 90%, 90% in sequence, the remaining fans are turned off, and all the thermal covers on the Stelmor are opened.
[0164] Before the first blower, the operating speed of the roller conveyor inlet part is 0.85m / s, the operating speed ratio of the roller conveyors corresponding to the first to fourth blowers is 1.10:1.05:1.02:1.00, and the operating speed ratio of the roller conveyors corresponding to the remaining blowers is 0.8:1.00~1.05:1.00. In addition, the wind speed of the overlapping part is adjusted to 1.3 times that of the non-overlapping part using an air volume adjustment device to ensure the cooling speed balance between the overlapping part and the non-overlapping part.
[0165] According to the production method of this embodiment, the roughly drawn wire of Example 2 can be obtained.
[0166] The wire rod obtained is wrapped in a packing wire after winding, and the packing wire and the wire rod are separated by linen cloth, and then wrapped and fixed for packaging. The room temperature during high-speed wire rolling is 30°C, and the natural aging treatment time is 10 days, after which the steel wire is transported to the user for production by drawing. Here, during transportation and transfer, a rubber pad is laid to avoid scratches on the wire rod.
[0167] Example 10 Example 10 provides a method for producing the wire rod of Example 3. The method specifically includes the following steps (1), (2), (3), (4), and (5).
[0168] (1) Vacuum melting process Using industrially pure iron with Al≦0.001%, Ti≦0.0005%, Cu≦0.001% and Ni≦0.001% as the raw material, alloy elements are blended into molten iron in accordance with a composition design of C: 1.01-1.10%, Si: 0.15-0.40%, Mn: 0.30-0.60%, Cr: 0.01-0.40%, and V: 0.01-0.09%, and the pressure inside the vacuum smelting furnace is maintained at 5 Pa, thereby smelting molten steel.
[0169] When the temperature of the smelted molten steel is heated to 1600-1620°C, it is protected under an inert gas atmosphere and cast into an ingot at a casting speed of 330 kg / min.
[0170] (2) Steel ingot remelting process The steel ingot obtained in the vacuum melting process is used as an electrode, and processed by vacuum self-consumption remelting, the remelting speed is 3.0 kg / min, and the remelted ingot is obtained. The remelted ingot is then kept warm for 72 hours, and then stacked in a wind-proof place to allow it to cool naturally.
[0171] The chemical composition of the remelted ingot was found to be, in mass percent, C: 1.03%, Si: 0.20%, Mn: 0.55%, Cr: 0.22%, V: 0.06%, with the remainder being Fe and unavoidable impurities, with the proviso that the impurities included Al: 0.002%, Ti: 0.0006%, S: 0.002%, P: 0.006%, O: 0.0006%, and N: 0.0008%.
[0172] (3) Billet manufacturing process and grinding process The remelted ingot obtained in the steel ingot remelting process is bloomed by continuous rolling at a temperature of 1130°C to obtain a steel billet which is a square billet with a length of 15 m and a size of 145 mm x 145 mm. Then, the surface of the steel billet is ground using 16 mesh, 24 mesh, and 30 mesh grinding wheels in sequence, the surface grinding depth of the steel billet by the 16 mesh grinding wheel is approximately 1.1 mm, the surface grinding depth of the steel billet by the 24 mesh grinding wheel is approximately 0.7 mm, the surface grinding depth of the steel billet by the 30 mesh grinding wheel is approximately 0.2 mm, the total grinding depth on one side is approximately 2 mm (correspondingly, the total grinding depth on both sides is approximately 4 mm), the corner grinding width is 6 mm, and the surface of the steel billet after grinding is smooth and burr-free.
[0173] (4) High-speed wire rolling process The ground steel billet is sent to a high-speed wire rolling machine and rolled into a rough wire with a diameter of Φ5.5 mm. The soaking temperature during heating before rolling is adjusted to set the rolling start temperature to 1040-1060°C, and the rolling end temperature is set to 1000-1020°C by temperature control means such as water cooling during the rolling process, thereby ensuring that the steel billet is essentially kept within the recrystallization region during rolling.
[0174] The rolling end speed is 108 m / s, and the laying temperature is 890 to 910°C.
[0175] (5) Cooling process The wire rod is cooled at a controlled temperature on the Stelmor, the first through fourth fans are turned on and the airflow is 100%, 100%, 95%, 95% in sequence, the remaining fans are turned off, and all the thermal covers on the Stelmor are opened.
[0176] Before the first blower, the operating speed of the roller conveyor inlet part is 1.0m / s, the operating speed ratio of the roller conveyors corresponding to the first to fourth blowers is 1.10:1.05:1.02:1.00, and the operating speed ratio of the roller conveyors corresponding to the remaining blowers is 0.8:1.00~1.05:1.00. In addition, the wind speed of the overlapping part is adjusted to 1.3 times that of the non-overlapping part using an air volume adjustment device to ensure the cooling speed balance between the overlapping part and the non-overlapping part.
[0177] According to the production method of this embodiment, the roughly drawn wire of Example 3 can be obtained.
[0178] The wire rod obtained is wrapped in a packing wire, and the wire rod is separated from the packing wire by linen cloth, and then wrapped and fixed. The room temperature during high-speed wire rolling is 10°C, and the natural aging treatment time is 21 days, after which the wire rod is transported to the user for production by drawing. Here, during transportation and transfer, a rubber pad is laid to avoid scratches on the wire rod.
[0179] Example 11 Example 11 provides a method for producing the wire rod of Example 4. The method specifically includes the following steps (1), (2), (3), (4), and (5).
[0180] (1) Vacuum melting process Using industrially pure iron with Al≦0.001%, Ti≦0.0005%, Cu≦0.001% and Ni≦0.001% as the raw material, alloy elements are blended into molten iron in accordance with a composition design of C: 1.01-1.10%, Si: 0.15-0.40%, Mn: 0.30-0.60%, Cr: 0.01-0.40%, B: 0.0005-0.0020%, and V: 0.01-0.09%, and the pressure inside the vacuum smelting furnace is maintained at 6 Pa to smelt molten steel.
[0181] When the temperature of the smelted molten steel is heated to 1600-1620°C, it is protected under an inert gas atmosphere and cast into an ingot at a casting speed of 350 kg / min.
[0182] (2) Steel ingot remelting process The steel ingot obtained in the vacuum melting process is used as an electrode, and processed by vacuum self-consumption remelting, the remelting speed is 3.3 kg / min, and the remelted ingot is obtained. The remelted ingot is then kept warm for 72 hours, and then stacked in a wind-proof place to allow it to cool naturally.
[0183] The chemical composition of the remelted ingot was found to be, in mass percent, C: 1.05%, Si: 0.16%, Mn: 0.55%, Cr: 0.01%, B: 0.0005%, V: 0.04%, with the remainder being Fe and unavoidable impurities, with the proviso that the impurities included Al: 0.002%, Ti: 0.0003%, S: 0.001%, P: 0.003%, O: 0.0003%, and N: 0.0009%.
[0184] (3) Billet manufacturing process and grinding process The remelted ingot obtained in the steel ingot remelting process is forged at a temperature of 1130°C into a steel billet, which is a square billet with a length of 14 m and a size of 145 mm x 145 mm, and then the surface of the steel billet is ground using 16 mesh, 24 mesh, and 30 mesh grinding wheels in sequence, the surface grinding depth of the steel billet by the 16 mesh grinding wheel is approximately 1.2 mm, the surface grinding depth of the steel billet by the 24 mesh grinding wheel is approximately 0.5 mm, the surface grinding depth of the steel billet by the 30 mesh grinding wheel is approximately 0.2 mm, the total grinding depth on one side is approximately 1.9 mm (correspondingly, the total grinding depth on both sides is approximately 3.8 mm), the corner grinding width is 8 mm, and the steel billet surface after grinding is smooth and burr-free.
[0185] (4) High-speed wire rolling process The ground steel billet is sent to a high-speed wire rolling machine and rolled into a rough wire with a diameter of Φ4.5 mm. The soaking temperature during heating before rolling is adjusted to set the rolling start temperature to 1050-1060°C, and the rolling end temperature is set to 980-1010°C by temperature control means such as water cooling during the rolling process, thereby ensuring that the steel billet is essentially kept within the recrystallization region during rolling.
[0186] The rolling end speed is 110 m / s, and the laying temperature is 900 to 920°C.
[0187] (5) Cooling process The wire rod is cooled at a controlled temperature on the Stelmor, the first to fourth fans are turned on and the airflow is 100%, 100%, 85%, 80% in sequence, the remaining fans are turned off, and all the thermal covers on the Stelmor are opened.
[0188] Before the first blower, the operating speed of the roller conveyor inlet part is 0.93m / s, the operating speed ratio of the roller conveyors corresponding to the first to fourth blowers is 1.10:1.05:1.02:1.00, and the operating speed ratio of the roller conveyors corresponding to the remaining blowers is 0.8:1.00~1.05:1.00. In addition, the wind speed of the overlapping part is adjusted to 1.25 times that of the non-overlapping part using an air volume adjustment device to ensure the cooling speed balance between the overlapping part and the non-overlapping part.
[0189] According to the production method of this embodiment, the roughly drawn wire of Example 4 can be obtained.
[0190] The wire rod is wrapped in a packing wire, and the wire rod is separated from the packing wire by linen cloth, and then wrapped and fixed. The room temperature during high-speed wire rolling is 32°C, and the natural aging treatment time is 11 days, after which the wire rod is transported to the user for drawing. Here, during transportation and transfer, a rubber pad is laid to avoid scratches on the wire rod.
[0191] Example 12 Example 12 provides a method for producing the wire rod of Example 5. The method specifically includes the following steps (1), (2), (3), (4), and (5).
[0192] (1) Vacuum melting process Using industrially pure iron as the raw material, alloy elements are blended into molten iron according to a composition design of C: 1.01-1.10%, Si: 0.15-0.40%, Mn: 0.30-0.60%, Cr: 0.01-0.40%, and B: 0.0005-0.0020%. The pressure inside the vacuum smelting furnace is maintained at 8 Pa, and molten steel is thereby smelted.
[0193] When the temperature of the smelted molten steel is heated to 1580-1600°C, it is protected under an inert gas atmosphere and cast into an ingot at a casting speed of 320 kg / min.
[0194] (2) Steel ingot remelting process First, the steel ingot obtained in the vacuum melting process is subjected to electroslag remelting treatment under an inert gas atmosphere, and then the remelted ingot obtained by electroslag remelting is used as an electrode to be processed by vacuum self-consumption remelting, with a remelting rate of 3.3 kg / min to obtain a remelted ingot, which is then kept warm for 72 hours.
[0195] The chemical composition of the remelted ingot was found to be, in mass percent, C: 1.05%, Si: 0.22%, Mn: 0.45%, Cr: 0.19%, B: 0.001%, with the remainder being Fe and unavoidable impurities, with the proviso that the impurities included Al: 0.001%, Ti: 0.0002%, S: 0.003%, P: 0.004%, O: 0.0005%, and N: 0.001%.
[0196] (3) Billet manufacturing process and grinding process The remelted ingot obtained in the steel ingot remelting process is forged at a temperature of 1140°C into a steel billet, which is a square billet with a length of 10 m and a size of 145 mm x 145 mm, and then the surface of the steel billet is ground using 16 mesh, 24 mesh, and 30 mesh grinding wheels in sequence, the surface grinding depth of the steel billet by the 16 mesh grinding wheel is approximately 1.4 mm, the surface grinding depth of the steel billet by the 24 mesh grinding wheel is approximately 0.5 mm, the surface grinding depth of the steel billet by the 30 mesh grinding wheel is approximately 0.1 mm, the total grinding depth on one side is approximately 2.0 mm (correspondingly, the total grinding depth on both sides is approximately 4.0 mm), the corner grinding width is 8 mm, and the steel billet surface after grinding is smooth and burr-free.
[0197] (4) High-speed wire rolling process The ground steel billet is sent to a high-speed wire rolling machine and rolled into a rough wire with a diameter of Φ5.5 mm. The soaking temperature during heating before rolling is adjusted to set the rolling start temperature to 1040-1060°C, and the rolling end temperature is set to 980-1020°C by temperature control means such as water cooling during the rolling process, thereby ensuring that the steel billet is essentially kept within the recrystallization region during rolling.
[0198] The rolling end speed is 110 m / s, and the laying temperature is 890 to 910°C.
[0199] (5) Cooling process The wire rod is cooled at a controlled temperature on the Stelmor, the first through fourth fans are turned on and the airflow is 100%, 100%, 100%, 100% in sequence, the remaining fans are turned off, and all the thermal covers on the Stelmor are opened.
[0200] Before the first blower, the operating speed of the roller conveyor inlet part is 1.0m / s, the operating speed ratio of the roller conveyors corresponding to the first to fourth blowers is 1.10:1.05:1.02:1.00, and the operating speed ratio of the roller conveyors corresponding to the remaining blowers is 0.8:1.00~1.05:1.00. In addition, the wind speed of the overlapping part is adjusted to 1.28 times that of the non-overlapping part using an air volume adjustment device to ensure the cooling speed balance between the overlapping part and the non-overlapping part.
[0201] According to the production method of this embodiment, the roughly drawn wire of Example 5 can be obtained.
[0202] The wire rod is wrapped in a packing wire, and the wire rod is separated from the packing wire by linen cloth, and then wrapped and fixed. The room temperature during high-speed wire rolling is 28°C, and the natural aging treatment time is 11 days, after which the wire rod is transported to the user for production by drawing. Here, during transportation and transfer, a rubber pad is laid to avoid scratches on the wire rod.
[0203] Example 13 Example 13 provides a method for producing the wire rod of Example 6. The method specifically includes the following steps (1), (2), (3), (4), (5), and (6).
[0204] (1) Vacuum melting process Using industrially pure iron with low contents of impurity elements such as Al, Ti, Cu and Ni as the raw material, alloy elements are blended into molten iron according to a composition design of C: 1.01-1.10%, Si: 0.15-0.40%, Mn: 0.30-0.60%, Cr: 0.01-0.40%, and V: 0.01-0.09%, the pressure inside the vacuum smelting furnace is maintained at 8 Pa, and molten steel is thereby smelted.
[0205] When the temperature of the smelted molten steel is heated to 1600-1610°C, it is protected under an inert gas atmosphere and cast into an ingot at a casting speed of 350 kg / min.
[0206] (2) Steel ingot remelting process The steel ingot obtained in the vacuum melting process is used as an electrode, and processed by vacuum self-consumption remelting, the remelting speed is 3.4 kg / min, and the remelted ingot is obtained. The remelted ingot is then kept warm for 72 hours, and then stacked in a wind-proof place to allow it to cool naturally.
[0207] The chemical composition of the remelted ingot was found to be, in mass percent, C: 1.08%, Si: 0.25%, Mn: 0.32%, Cr: 0.18%, V: 0.01%, with the remainder being Fe and unavoidable impurities, with the proviso that the impurities included Al: 0.001%, Ti: 0.0005%, S: 0.001%, P: 0.003%, O: 0.0004%, and N: 0.0006%.
[0208] (3) Billet manufacturing process and grinding process The remelted ingot obtained in the steel ingot remelting process is bloomed by continuous rolling at a temperature of 1130°C to obtain a steel billet, which is a square billet with a length of 14 m and a size of 145 mm x 145 mm. Then, the surface of the steel billet is ground using 16 mesh, 24 mesh, and 30 mesh grinding wheels in sequence, the surface grinding depth of the steel billet by the 16 mesh grinding wheel is approximately 1.1 mm, the surface grinding depth of the steel billet by the 24 mesh grinding wheel is approximately 0.7 mm, the surface grinding depth of the steel billet by the 30 mesh grinding wheel is approximately 0.2 mm, the total grinding depth on one side is approximately 2 mm (correspondingly, the total grinding depth on both sides is approximately 4 mm), the corner grinding width is 6 mm, and the surface of the steel billet after grinding is smooth and burr-free.
[0209] (4) High-speed wire rolling process The ground steel billet is sent to a high-speed wire rolling machine and rolled into a rough wire with a diameter of Φ5.0 mm. The soaking temperature during heating before rolling is adjusted to set the rolling start temperature to 1040-1060°C, and the rolling end temperature is set to 1000-1020°C by temperature control means such as water cooling during the rolling process, thereby ensuring that the steel billet is essentially kept within the recrystallization region during rolling.
[0210] The rolling end speed is 110 m / s, and the laying temperature is 890 to 910°C.
[0211] (5) Cooling process The wire rod is cooled at a controlled temperature on the Stelmor, the first through fourth fans are turned on and the airflow is 100%, 100%, 95%, 95% in sequence, the remaining fans are turned off, and all the thermal covers on the Stelmor are opened.
[0212] Before the first blower, the operating speed of the roller conveyor inlet part is 1.0m / s, the operating speed ratio of the roller conveyors corresponding to the first to fourth blowers is 1.10:1.05:1.02:1.00, and the operating speed ratio of the roller conveyors corresponding to the remaining blowers is 0.8:1.00~1.05:1.00. In addition, the wind speed of the overlapping part is adjusted to 1.2 times that of the non-overlapping part using an air volume adjustment device to ensure the cooling speed balance between the overlapping part and the non-overlapping part.
[0213] (6) Heat treatment process The wire rod after Stelmor cooling is subjected to offline salt bath heat treatment (can be replaced by lead bath heat treatment), in which the temperature of the isothermal phase change step is 540-560°C and the time is 70s.
[0214] According to the production method of this embodiment, the roughly drawn wire of Example 6 can be obtained.
[0215] The wire rod obtained is wrapped in a packing wire after winding, and the packing wire and the wire rod are separated by linen cloth, and then wrapped and fixed for packaging. The room temperature during high-speed wire rolling is 5°C, and the natural aging treatment time is 23 days, after which the steel wire is transported to the user for production by drawing. Here, during transportation and transfer, a rubber pad is laid to avoid scratches on the wire rod.
[0216] Example 14 Example 14 provides a method for producing the wire rod of Example 7. The method specifically includes the following steps (1), (2), (3), (4), (5), and (6).
[0217] (1) Vacuum melting process Using industrially pure iron with Al≦0.001%, Ti≦0.0005%, Cu≦0.001% and Ni≦0.001% as the raw material, alloy elements are blended into molten iron in accordance with a composition design of C: 1.01-1.10%, Si: 0.15-0.40%, Mn: 0.30-0.60%, Cr: 0.01-0.40%, and V: 0.01-0.09%, and the pressure inside the vacuum smelting furnace is maintained at 6 Pa to produce molten steel.
[0218] When the temperature of the smelted molten steel is heated to 1590-1600°C, it is protected under an inert gas atmosphere and cast into an ingot at a casting speed of 330 kg / min.
[0219] (2) Steel ingot remelting process The steel ingot obtained in the vacuum melting process is used as an electrode, and processed by vacuum self-consumption remelting, the remelting speed is 3.5 kg / min, and the remelted ingot is obtained. The remelted ingot is then kept warm for 72 hours, and then stacked in a wind-proof place to allow it to cool naturally.
[0220] The chemical composition of the remelted ingot was found to be, in mass percent, C: 1.10%, Si: 0.16%, Mn: 0.30%, Cr: 0.15%, V: 0.05%, with the remainder being Fe and unavoidable impurities, with the proviso that the impurities included Al: 0.001%, Ti: 0.0002%, S: 0.002%, P: 0.003%, O: 0.0002%, and N: 0.0009%.
[0221] (3) Billet manufacturing process and grinding process The remelted ingot obtained in the steel ingot remelting process is forged at a temperature of 1150°C into a steel billet, which is a square billet with a length of 10 m and a size of 145 mm x 145 mm, and then the surface of the steel billet is ground using 16 mesh, 24 mesh, and 30 mesh grinding wheels in sequence, the surface grinding depth of the steel billet by the 16 mesh grinding wheel is approximately 1.1 mm, the surface grinding depth of the steel billet by the 24 mesh grinding wheel is approximately 0.7 mm, the surface grinding depth of the steel billet by the 30 mesh grinding wheel is approximately 0.2 mm, the total grinding depth on one side is approximately 2 mm (correspondingly, the total grinding depth on both sides is approximately 4 mm), the corner grinding width is 8 mm, and the steel billet surface after grinding is smooth and burr-free.
[0222] (4) High-speed wire rolling process The ground steel billet is sent to a high-speed wire rolling machine and rolled into a rough wire with a diameter of Φ5.5 mm. The soaking temperature during heating before rolling is adjusted to set the rolling start temperature to 1030-1050°C, and the rolling end temperature is set to 950-990°C by temperature control means such as water cooling during the rolling process, thereby ensuring that the steel billet is essentially kept within the recrystallization region during rolling.
[0223] The rolling end speed is 108 m / s, and the laying temperature is 890 to 910°C.
[0224] (5) Cooling process The wire rod is cooled at a controlled temperature on the Stelmor, the first to fourth fans are turned on and the airflow is 100%, 100%, 99%, 95% in sequence, the remaining fans are turned off, and all the thermal covers on the Stelmor are opened.
[0225] Before the first blower, the operating speed of the roller conveyor inlet part is 1.0m / s, the operating speed ratio of the roller conveyors corresponding to the first to fourth blowers is 1.10:1.05:1.02:1.00, and the operating speed ratio of the roller conveyors corresponding to the remaining blowers is 0.8:1.00~1.05:1.00. In addition, the wind speed of the overlapping part is adjusted to 1.18 times that of the non-overlapping part using an air volume adjustment device to ensure the cooling speed balance between the overlapping part and the non-overlapping part.
[0226] (6) Heat treatment process The wire rod after Stelmor cooling is subjected to offline salt bath heat treatment, in which the temperature of the isothermal phase change step is 520-540°C and the time is 80s.
[0227] According to the production method of this embodiment, the roughly drawn wire of Example 7 can be obtained.
[0228] The wire rod is wrapped in a packing wire, and the wire rod is separated from the packing wire by linen cloth, and then wrapped and fixed. The room temperature during high-speed wire rolling is 25°C, and the natural aging treatment time is 13 days, after which the wire rod is transported to the user for production by drawing. Here, during transportation and transfer, a rubber pad is laid to avoid scratches on the wire rod.
[0229] In general, the present invention has the following beneficial effects compared with the prior art: by designing chemical components and improving the process technology of the production method, the size and type of impurities are strictly controlled, high cleanliness and uniform structure are ensured, and the tensile strength and drawing performance of the wire rod are improved. The wire rod can be applied to the production of high-strength diamond wire with ultra-fine and low breakage rate, and can be produced by drawing a diamond wire mother wire with a diameter of 40-46 μm, a breakage rate of ≦2 times / 1000 km, and a tensile strength of ≧5000 MPa, which is suitable for producing diamond wire for cutting silicon wafers, fully meeting the market demand for steel wire with high drawing performance, low breakage rate, and high strength, and filling the technical gap of 5000 MPa-class or higher wire rod for diamond wire at home and abroad.
Claims
1. A method for producing a rough wire for diamond wire, the method comprising the steps of: chemical components, in mass percent, including C: 1.01-1.10%, Si: 0.15-0.40%, Mn: 0.30-0.60%, Cr: 0.01-0.40%, and either or both of B: 0.0005-0.0020% and V: 0.01-0.09%, with the balance being Fe and unavoidable impurities, with the proviso that the impurities include Al≦0.003%, Ti≦0.0008%, S≦0.005%, P≦0.008%, O≦0.0010%, and N≦0.0020%, a vacuum smelting process in which molten steel is smelted in a vacuum smelting furnace under an atmosphere with an internal pressure of 10 Pa or less, and the molten steel is cast into a steel ingot; a steel ingot remelting process for treating a steel ingot by either or both of electroslag remelting and vacuum autogenous remelting to obtain a remelted ingot, wherein the electroslag remelting is performed under a protective atmosphere and the remelting rate of the vacuum autogenous remelting is 3.0-3.5 kg / min; a billet making and grinding process, which comprises blooming or forging the remelted ingot into a steel billet and grinding the steel billet; a high speed wire rolling step of rolling the steel billet into a wire rod, the rolling start temperature being 1030-1060°C and the rolling end temperature being 950-1020°C; and a cooling step in which the wire rod is cooled on a Stelmor at a controlled temperature, with the first to fourth blowers being turned on and the airflow being 80% to 100%, and the remaining blowers being turned off.
2. 2. The method for producing a rough wire for diamond wire according to claim 1, wherein in the vacuum melting step, a furnace pressure is 5 Pa or less.
3. 2. The method for producing a rough wire for diamond wire according to claim 1, characterized in that in the vacuum smelting process, industrial pure iron containing Al≦0.001%, Ti≦0.0005%, Cu≦0.001% and Ni≦0.001% is used as a raw material, alloy elements are blended according to a composition design, and molten steel is smelted using the vacuum smelting furnace.
4. The method for producing a rough wire for diamond wire according to claim 1, wherein the casting temperature is 1580 to 1620° C. in the vacuum melting process.
5. 2. The method for producing a rough wire for diamond wire according to claim 1, wherein in the steel ingot remelting step, after obtaining a remelted ingot by the vacuum self-consumption remelting, the obtained remelted ingot is kept at a temperature for 48 hours or more.
6. The method for producing a rough wire for diamond wire according to claim 1, characterized in that in the billet production step, the remelted ingot is bloomed or forged into a square billet having a length of 9 to 16 m and a size of 145 mm x 145 mm.
7. 2. The method for producing a rough wire rod for diamond wire according to claim 1, wherein in the billet production step, the remelted ingot is bloomed or forged at a temperature of 1130 to 1160°C.
8. 2. The method for producing a rough wire for diamond wire according to claim 1, characterized in that in the grinding step, the total grinding depth on the steel billet surface is ≧1.5 mm.
9. 9. The method for producing a rough wire for diamond wire according to claim 8, characterized in that in the grinding step, the surface of the steel billet is ground using grindstones of 16 mesh, 24 mesh, and 30 mesh in sequence, the grinding depth of each pass is ≧0.9 mm, ≧0.5 mm, and ≧0.1 mm, respectively, and the corner grinding width is ≧5 mm.
10. 2. The method for producing a rough wire rod for diamond wire according to claim 1, wherein in the high-speed wire rolling step, the steel billet is rolled into a rough wire rod having a diameter of Φ4.5 to Φ5.5 mm.
11. 2. The method for producing a rough wire for diamond wire according to claim 1, wherein in the high-speed wire rolling process, a rolling end speed is 100 to 110 m / s.
12. 2. The method for producing a rough wire for diamond wire according to claim 1, wherein in the high speed wire rolling process, a laying temperature is 890 to 920° C.
13. 2. The method for producing a rough wire for diamond wire according to claim 1, wherein in the cooling step, an operating speed of an inlet portion of a roller conveyor before the first blower is 0.9 to 1.0 m / s.
14. The method for producing a rough wire for diamond wire according to claim 13, characterized in that in the cooling step, all of the thermal insulation covers are opened, and an operating speed ratio of roller conveyors corresponding to the first to fourth blowers is 1.10:1.05:1.02:1.
00.
15. 2. The method for producing a rough wire for diamond wire according to claim 1, wherein in the cooling step, an air flow rate adjusting device is used to adjust an air flow rate at the overlapping portion to 1.1 to 1.4 times that at the non-overlapping portion.
16. 2. The method for producing a rough wire for diamond wire according to claim 1, further comprising a heat treatment process for subjecting the rough wire after the Stelmor cooling to a salt bath heat treatment or a lead bath heat treatment, in which the temperature of an isothermal phase change step is 520 to 560° C. and the time is 20 to 80 s.
Citation Information
Patent Citations
Control method of plasticization of inclusion in steel for hyperfine cutting wire
CN108456819A
Production of clean steel
JP1989319623A
High strength spring steel and its production
JP1993214484A
Steel wire rod, and method of producing steel wire
JP2005002413A
Methods of melting and refining alloys
JP2018525518A