Silicone elastomer composition

A curable silicone elastomer composition with unsaturated groups and anhydride functional groups addresses the adhesion issues of silicone elastomers to plastics and thermoplastics, providing reliable and durable bonding without primers or surface treatments.

JP7583180B2Active Publication Date: 2024-11-13DOW SILICONES CORP +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023547436
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-02-10
Filing Date
2022-02-08
Publication Date
2024-11-13
Estimated Expiration
2042-02-08

AI Technical Summary

Technical Problem

Existing silicone elastomers exhibit poor adhesion to plastics and thermoplastics, and conventional methods like surface priming and plasma treatment are unreliable and environmentally harmful.

Method used

A curable silicone elastomer composition containing unsaturated groups, organopolysiloxanes, and a curing agent with anhydride functional groups, which allows for primerless adhesion to various substrates through hydrosilylation, enhancing bonding strength.

Benefits of technology

The composition achieves strong and durable adhesion to a wide range of substrates without the need for surface treatments, improving productivity and reliability in manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583180000001
    Figure 0007583180000001
  • Figure 0007583180000002
    Figure 0007583180000002
  • Figure 0007583180000003
    Figure 0007583180000003
Patent Text Reader

Abstract

The present disclosure relates to a curable silicone elastomer composition (hereinafter referred to as "curable silicone elastomer composition") having enhanced adhesive properties to a wide variety of substrates. The elastomer produced by curing the aforementioned composition can be adhered to a wide variety of substrates to form a composite comprising the elastomer produced from the curable silicone elastomer composition and the substrate. A method of adhering the elastomer curable silicone elastomer composition to the substrate is also provided. Component (D), an adhesion promoter, is provided to enhance adhesion. Component (D) is a polyorganosiloxane having (i) at least one unsaturated group per molecule selected from an alkenyl group and an alkynyl group, and (ii) anhydride and aromatic functional groups, where the carbon of the aromatic functional group is separated from the carbon of the carbonyl group of the anhydride by a carbon chain containing 1 to 3 non-aromatic carbon atoms.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a curable silicone elastomer composition (hereinafter referred to as "curable silicone elastomer composition") that has improved adhesion properties to a wide variety of substrates. The elastomers produced by curing the aforementioned compositions can be adhered to a wide variety of substrates to form composites comprising the elastomers produced from the curable silicone elastomer composition and the substrate. A method of adhering the elastomers produced from the curable silicone elastomer composition to a substrate is also provided.

[0002] The curable silicone elastomer composition cures to provide a silicone elastomer material (alternatively called a silicone rubber). One suitable curing process is via an addition cure mechanism; another is described as a hydrosilylation process using a platinum group catalyst.

[0003] The adhesion of addition curable silicone elastomers is generally poor on plastics. Traditionally, the adhesion of silicone elastomers can be increased by modifying the silicone matrix or the substrate surface, for example, by priming and forms of surface activation, such as plasma treatment, among others. To overcome this problem, the application of a primer to the substrate surface was first utilized. However, some problems have been encountered using methods that require a primer and / or high energy surface pretreatment, such as irradiation by exposure to plasma, corona, flame, UV, or UV-ozone sources, to activate the surface for adhesion. Primer methods are troublesome because they can result in unreliable productivity, quality control issues, and actual reliability issues, especially for the parts / articles being manufactured. Primers also have the disadvantage that they often contain volatile organic solvents.

[0004] It is therefore desirable to avoid the use of primers if possible, and this is achieved by using self-adhesive silicone elastomeric materials that have sufficient adhesion without the need for a subsequently primed surface, i.e., they can adhere during cure to substrates made from, for example, thermoplastic materials, organic resin-based materials, or both thermoplastic and organic resin-based materials, that are placed in direct contact with them before or during the curing process.

[0005] It is known that the adhesion of addition curable silicone elastomers can be improved by incorporating adhesive additives containing reactive functional groups, including but not limited to alkoxysilane, epoxy and carboxyl groups.However, their use has been limited in various applications due to their inability to form sufficiently strong adhesive bonds with plastic and thermoplastic substrates, such as polycarbonate.For example, alkoxysilane coupling agents are sometimes used to achieve adhesion to plastics, but they are prone to side reactions, such as self-reaction, and release volatile alcohols during reaction, which can reduce their effectiveness.

[0006] Further alternative proposals suggest incorporating hydrosilylation curable silicone elastomer crosslinkers, such as organohydrogenpolysiloxanes, into polycarbonate substrates.However, such processes have been found to adversely affect the physical properties of the polycarbonate itself, preventing the resin from exerting its own properties.The physical engagement method leaves open the possibility that the two segments can be disengaged by physical forces.

[0007] The use of silicone elastomers, such as self-adhesive silicone elastomers, is a preferred alternative because it can improve manufacturability, quality control, and reliability of parts / articles, at least in part, by eliminating the need for the use of primers or surface pretreatments.

[0008] The durability of the adhesion between the self-adhesive silicone material and a wide variety of non-silicone substrates, such as thermoplastic substrates, organic resin substrates, or thermoplastic and organic resin substrates, is very important for the successful use of the combination, but providing such composite materials with good adhesion to a variety of substrates remains a technical challenge.

[0009] The present disclosure relates to (A) one or more organopolysiloxanes containing at least two unsaturated groups per molecule selected from alkenyl and alkynyl groups and having a viscosity in the range of 1000 mPa.s to 500,000 mPa.s at 25°C, but no anhydride functionality; (B) a curing agent, (B)(i) an organic peroxide radical initiator, or (B)(ii) a hydrosilylation curing catalyst package comprising: a. an organosilicon compound having at least two or at least three Si-H groups per molecule; and b. a curing agent comprising a hydrosilylation curing catalyst package comprising a hydrosilylation catalyst; (C) at least one reinforcing filler and optionally one or more non-reinforcing fillers; (D) a polyorganosiloxane, (i) at least one unsaturated group per molecule selected from an alkenyl group and an alkynyl group, and and (ii) a polyorganosiloxane having an anhydride functionality and an aromatic functionality, where the carbon of the aromatic functionality is separated from the carbon of the carbonyl group of the anhydride by a carbon chain containing 1-3 non-aromatic carbon atoms.

[0010] This composition as described above is capable of achieving primerless adhesion to plastics with addition curable silicone elastomers, where component D is an adhesion promoter that contains neither Si-H nor alkoxysilane groups that provide primerless adhesion to commercially important engineering thermoplastics.

[0011] Component (A) is one or more organopolysiloxanes containing at least two unsaturated groups per molecule selected from alkenyl and alkynyl groups and having a viscosity in the range of 1000 mPa.s to 500,000 mPa.s at 25°C, but no anhydride functionality.

[0012] In one embodiment, each of the one or more organopolysiloxanes (A) contains at least two alkenyl and / or alkynyl groups bonded to silicon atoms per molecule and, unless otherwise specified, has a viscosity of from 1000 mPa.s to 500,000 mPa.s at 25° C., alternatively from 1000 mPa.s to 150,000 mPa.s at 25° C., alternatively from 1000 mPa.s to 100,000 mPa.s at 25° C., alternatively from 1000 mPa.s to 75,000 mPa.s at 25° C., using a rheometer such as an Anton-Paar MCR-301 rheometer equipped with a 25 mm cone and plate fixture and operated at 25° C. Unless otherwise specified, viscosity is reported as zero shear viscosity, which means the value extrapolated to zero shear rate from the statistically significant rate-independent Newtonian region of the viscosity versus shear rate sweep. Alternatively, if desired, viscosity can be measured using a Brookfield™ rotational viscometer using spindles (LV1-LV-4) and adjusting the speed depending on the viscosity of the polymer; all viscosity measurements were taken at 25° C. unless otherwise specified.

[0013] Each of the at least two unsaturated groups per molecule may be the same or different and is selected from alkenyl and alkynyl groups, or alkenyl and alkynyl groups having 2 to 12 carbons, or alkenyl and alkynyl groups having 2 to 6 carbons. Examples of alkenyl groups include vinyl, allyl, butenyl, pentenyl, cyclohexenyl, and hexenyl groups. Examples of alkynyl groups include ethynyl, propynyl, butynyl, pentynyl, cyclohexynyl, and hexynyl groups. The unsaturated groups may be pendant or terminal, or both, i.e., such groups may be present on any of the siloxy units of the organopolysiloxane (A).

[0014] Component (A) may be a linear and / or branched organopolysiloxane containing a plurality of units of formula (1), [ka] In the formula, each R' may be the same or different and represents a hydrocarbon group having 1 to 18 carbon atoms, a substituted hydrocarbon group having 1 to 18 carbon atoms, or a hydrocarbonoxy group having up to 18 carbon atoms, and has an average a value of 1 to 3, preferably 1.8 to 2.2.

[0015] For the purposes of this application, "substitution" means that one or more hydrogen atoms in a hydrocarbon group are replaced with another substituent. Examples of such substituents include, but are not limited to, halogen atoms such as chlorine, fluorine, bromine and iodine; halogen atom-containing groups such as chloromethyl, perfluorobutyl, trifluoroethyl, trifluoropropyl and nonafluorohexyl; oxygen atoms; oxygen atom-containing groups such as (meth)acrylic and carboxyl groups; nitrogen atoms; nitrogen atom-containing groups such as amino, amide and cyano functional groups; sulfur atoms; and sulfur atom-containing groups such as mercapto groups.

[0016] Siloxy units may be described in contractions (abbreviations), i.e., "M", "D", "T", and "Q", where R is usually an alkyl group, e.g., a methyl group, unless otherwise specified. (Further teachings on silicone nomenclature can be found in Walter Noll, Chemistry and Technology of Silicones, dated 1962, Chapter I, pages 1-9.) M units are siloxy units where a=3, i.e., RSiO 1 / 2 and D units are siloxy units where a=2, i.e., RSiO 2 / 2 where T units are siloxy units where a=1, i.e., RSiO 3 / 2 and Q units are siloxy units where a=0, i.e., SiO 4 / 2 is equivalent to.

[0017] Examples of raw material (A) are polydiorganosiloxanes containing alkenyl or alkynyl groups at two termini, but typically containing alkenyl groups, and can be represented by the general formula (I): [ka]

[0018] In formula (I), each R' is an alkenyl or alkynyl group, typically containing from 2 to 10 carbon atoms, such as vinyl, allyl, and 5-hexenyl, but is typically an alkenyl group.

[0019] R" does not contain ethylenic unsaturation. Each R" may be the same or different and is independently selected from monovalent saturated hydrocarbon groups generally containing from 1 to 10 carbon atoms and monovalent aromatic hydrocarbon groups generally containing from 6 to 12 carbon atoms. R" may be unsubstituted or substituted with one or more groups that do not interfere with the cure of the compositions of the present invention, such as halogen atoms. R''' is R' or R", and m represents a suitable degree of polymerization for raw material (A) to have a viscosity within the ranges discussed below.

[0020] Typically, all R" and R''' groups contained in the compound according to formula (I) are methyl groups. Alternatively, at least one R" and / or R''' group in the compound according to formula (I) is a methyl group and the others are phenyl or 3,3,3-trifluoropropyl groups. This preference is based on the availability of reactants typically used to prepare the polydiorganosiloxanes (feedstock (A)) and the desirable properties of the cured elastomers prepared from compositions containing such polydiorganosiloxanes.

[0021] Particularly preferred examples of the radical R' include methyl, ethyl, propyl, butyl, vinyl, cyclohexyl, phenyl, tolyl, propyl groups substituted with chlorine or fluorine, such as 3,3,3-trifluoropropyl, chlorophenyl, β-(perfluorobutyl)ethyl or chlorocyclohexyl. ’ At least some, more preferably substantially all, of the R' groups are methyl. Some R' groups may be phenyl or fluoro. In one alternative, the polydiorganosiloxanes are predominantly polydialkylsiloxanes and / or polydialkylalkylphenylsiloxanes having at least two alkenyl groups per molecule. In a further alternative, the polydiorganosiloxanes are predominantly polydimethylsiloxanes having at least two alkenyl groups per molecule. These are preferably of the formula R"3SiO 1 / 2 where each R″ is the same or different. It is understood that the cure rate and physical properties of the curable composition are affected by the structure and degree of functionality of component (A). For example, in some embodiments, it may be advantageous to utilize a branched, resinous, or cyclic-containing organopolysiloxane having pendant alkenyl or alkynyl groups as part or all of component (A).

[0022] The viscosity of organopolysiloxane (A) at 25° C. is typically measured using a rheometer or a Brookfield™ rotational viscometer as described above using a spindle (LV-4) and adjusting the speed depending on the viscosity of the polymer; all viscosity measurements were taken at 25° C. unless otherwise specified.

[0023] Examples of organopolysiloxanes (A) that can be used include vinyldimethylsiloxy endblocked dimethylsiloxane-vinylmethylsiloxane copolymers, vinyldimethylsiloxy endblocked polydimethylsiloxanes, vinylmethylhydroxysiloxy endblocked dimethylsiloxane-vinylmethylsiloxane copolymers, and mixtures thereof.

[0024] The organopolysiloxane (A) may be either a single polymer or a combination of two or more different polymers. Alternatively or additionally, the organopolysiloxane (A) may be a silicone resin containing [T] units and / or [Q] units as defined above. For example, the siloxane resin of component (A) may be characterized as a DT resin, an MQ resin, an MDQ resin, etc., but in each case must contain at least two unsaturated groups, typically alkenyl groups as described above.

[0025] The organopolysiloxane (A) is present in the composition in a concentration from 10 to 85% by weight, based on the total weight of the composition, alternatively from 20 to 80% by weight, based on the total weight of the composition, alternatively from 20 to 75% by weight, based on the total weight of the composition, alternatively from 30 to 65% by weight, based on the total weight of the composition.

[0026] B) Hardener The compositions described herein may be cured with an organic peroxide radical initiator (catalyst) (B)(i) or a mixture of different types of peroxides (radical initiators / catalysts).

[0027] The peroxide catalyst / radical initiator may be any commercially available peroxide known for use in curing silicone and / or fluorosilicone elastomer compositions. The amount of organic peroxide used is determined by the nature of the curing process, the organic peroxide used, and the composition used. In general, the amount of organic peroxide used in the compositions described herein is 0.2 to 3 wt%, alternatively 0.2 to 2 wt%, in each case based on the weight of the composition.

[0028] Suitable organic peroxides are substituted or unsubstituted dialkyl-, alkylaroyl-, diaroyl-peroxides, such as benzoyl peroxide and 2,4-dichlorobenzoyl peroxide, ditertiarybutyl peroxide, dicumyl peroxide, lauroyl peroxide, t-butylcumyl peroxide, bis(t-butylperoxyisopropyl)benzene, cyclohexanone peroxide, cumene hydroperoxide, tert-butyl hydroperoxide bis(t-butylperoxy)-2,5-dimethylhexyne, 2,4-dimethyl-2,5-di(t-butylperoxy)hexane, di-t-butyl peroxide, and 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane.

[0029] Alternatively, the composition comprises: (B)(ii)(a) an organosilicon compound having at least two, or alternatively at least three, Si-H groups per molecule; and (B)(ii)(b) may be cured using a hydrosilylation catalyst package (B)(ii) in the form of a hydrosilylation catalyst.

[0030] Component (B)(ii)(a) is a crosslinker in the form of an organosilicon compound containing at least two or three silicon-bonded hydrogen atoms per molecule. Typically, component (B)(ii)(a) contains three or more silicon-bonded hydrogen atoms, which hydrogen atoms are capable of reacting with unsaturated alkenyl or alkynyl groups in polymer (A) to form a network structure therewith, thereby curing the composition. Alternatively, when polymer (A) has more than two (>2) alkenyl or alkynyl groups per molecule, some or all of component (B)(ii)(a) may have two silicon-bonded hydrogen atoms per molecule.

[0031] The structure of the organosilicon compound can be linear, branched, cyclic, or resinous. The cyclosilanes and cyclosiloxanes can have 3 to 12 silicon atoms, alternatively 3 to 10 silicon atoms, alternatively 3 to 4 silicon atoms. In the acyclic polysilanes and polysiloxanes, the silicon-bonded hydrogen atoms can be located at terminal, pendant, or both terminal and pendant positions.

[0032] Examples of suitable organohydrogensilanes that may be used as crosslinkers include diphenylsilane, 2-chloroethylsilane, bis[(p-dimethylsilyl)phenyl]ether, 1,4-dimethyldisilylethane, 1,3,5-tris(dimethylsilyl)benzene, 1,3,5-trimethyl-1,3,5-trisilane, poly(methylsilylene)phenylene, and poly(methylsilylene)methylene. In some examples, the organohydrogensilane can be represented by the formula HR 1 2Si-R 2 -SiR 1 2H, where R 1 is C1~C 10 Hydrocarbyl or C1-C 10 halogen-substituted hydrocarbyls, both of which are free of aliphatic unsaturation, R 2 is 1,4- or 1,3-disubstituted phenyl, 4,4'- or 3,3'-disubstituted-1,1'-biphenyl, or para- or meta-disubstituted Ph(C g H2g ) Ph,

[0033] The molecular architecture of organopolysiloxane (B)(ii)(a), which contains at least 2 or 3 silicon-bonded hydrogen atoms per molecule, is not particularly limited and can be linear, linear with some branching, cyclic, or silicone resin-based. The molecular weight of this component is not particularly limited, but the viscosity is generally 0.001 to 50 Pa.s at 25°C using the rheometer described above or the cup / spindle method of ASTM D1084 Method B, using the Brookfield™ RV or LV range spindle most appropriate for the viscosity range, to obtain good miscibility with polymer (A). The silicon-bonded organic groups used in component (B)(ii)(a) may be exemplified by methyl, ethyl, propyl, butenyl, pentenyl, hexyl, or similar alkyl groups; phenyl, tolyl, xylyl, or similar aryl groups; 3-chloropropyl, 3,3,3-trifluoropropyl, or similar halogenated alkyl groups, of which methyl and phenyl groups are preferred.

[0034] Organopolysiloxane (B)(ii)(a) containing at least 2 or 3 silicon-bonded hydrogen atoms per molecule is typically added in an amount such that the molar ratio of the total number of silicon-bonded hydrogen atoms in component (B)(ii)(a) to the total number of alkenyl and / or alkynyl groups in polymer (A) is 0.5:1 to 20:1. If this ratio is less than 0.5:1, a sufficiently cured composition is not obtained. If this ratio is greater than 20:1, the hardness of the cured composition tends to increase when heated.

[0035] Examples of organopolysiloxanes (B)(ii)(a) containing at least 2 or 3 silicon-bonded hydrogen atoms per molecule include, but are not limited to, the following: (a') trimethylsiloxy-terminated methylhydrogenpolysiloxane, (b') trimethylsiloxy-terminated polydimethylsiloxane-methylhydrogensiloxane; (c') dimethylhydrogensiloxy-terminated dimethylsiloxane-methylhydrogensiloxane copolymer; (d') cyclic copolymer of dimethylsiloxane-methylhydrogensiloxane; (e')(CH3)2HSiO 1 / 2 Unit: (CH3)3SiO 1 / 2 Units, and SiO 4 / 2 copolymers and / or silicone resins consisting of units; (f')(CH3)2HSiO 1 / 2 Units and SiO 4 / 2 copolymers and / or silicone resins consisting of units; (g')(CH3)2HSiO 1 / 2 Units, SiO 4 / 2 Units and (C6H5)3SiO 1 / 2 Copolymers of units and / or silicone resins, as well as alternatives in which the methyl is replaced by a phenyl group or other alkyl group. Alternatively, component (B)(ii)(a) the crosslinker may be a filler, such as a silica that has been treated with one of the above.

[0036] Component (B)(ii)(a) may be exemplified by the following compounds: methylhydrogenpolysiloxanes terminally terminated with trimethylsiloxy groups; copolymers of methylhydrogensiloxane and dimethylsiloxane terminally terminated with trimethylsiloxy groups; dimethylsiloxane terminally terminated with dimethylhydrogensiloxy groups; copolymers of methylhydrogensiloxane and dimethylsiloxane terminally terminated with dimethylhydrogensiloxy groups; copolymers of methylhydrogensiloxane and methylphenylsiloxane terminally terminated with dimethylphenylsiloxy groups; cyclic methylhydrogenpolysiloxanes; (CH3)2HSiO 1 / 2 Siloxane unit and SiO 4 / 2 A copolymer consisting of (CH3)2HSiO units. 1 / 2Siloxane unit, (CH3)3SiO 1 / 2 Siloxane units, and SiO 4 / 2 units in which some or all of the methyl groups of the above organopolysiloxanes have been replaced with ethyl, propyl, or similar alkyl groups; phenyl, tolyl, or similar aryl groups; 3,3,3-trifluoropropyl, or similar halogenated alkyl groups; or mixtures of two or more of the above organopolysiloxanes.

[0037] The organosilicon compound crosslinker (B)(ii)(a) is present in the curable silicone elastomer composition in an amount such that the ratio of the moles of silicon-bonded hydrogen atoms in component (B)(ii)(a) to the moles of alkenyl groups in component (A) is generally in the range of from (0.7:1.0) to (5.0:1.0), preferably from (0.9:1.0) to (2.5:1.0), and most preferably from (0.9:1.0) to (2.0:1.0).

[0038] The silicon-bonded hydrogen (Si-H) content of component (B)(ii)(a) and the unsaturated group content of component (a) are determined using quantitative infrared analysis according to ASTM E168. In the present invention, the ratio of silicon-bonded hydrogen to alkenyl (vinyl) and / or alkynyl is important when relying on a hydrosilylation cure process. Generally, this is determined by calculating the total weight percent of alkenyl groups in the composition, e.g., vinyl [V], and the total weight percent of silicon-bonded hydrogen [H] in the composition, where the molecular weight of hydrogen is 1 and the molecular weight of vinyl is 27, resulting in a molar ratio of silicon-bonded hydrogen to vinyl of 27 [H] / [V].

[0039] Typically, depending on the number of unsaturated groups in component (A) and the number of Si-H groups in component (B)(ii)(a), component (B)(ii)(a) will be present in an amount from 0.1 to 40% by weight of the total composition, alternatively from 0.5 to 20% by weight of the total composition, alternatively from 0.5 to 10% by weight of the total composition, and further alternatively from 1% to 5% by weight of the total composition.

[0040] Component (B)(ii)(b) is at least one hydrosilylation (addition) reaction catalyst. Usually, these are selected from catalysts of the platinum metal group (platinum, ruthenium, osmium, rhodium, iridium, and palladium) or one or more compounds of such metals. Platinum and rhodium compounds are preferred due to the high activity level of these catalysts in hydrosilylation reactions. Component (B)(ii)(b) catalyzes the reaction between the alkenyl group (e.g., vinyl group) of component (A) and the Si-H group of component (B)(ii)(a), resulting in a crosslinked network when the curable silicone elastomer composition cures to its corresponding elastomer.

[0041] Catalyst (B)(ii)(b) may be a platinum group metal, a platinum group metal deposited on a support such as activated carbon, a metal oxide (such as aluminum oxide or silicon dioxide), silica gel or powdered charcoal, or a compound or complex of a platinum group metal.

[0042] Examples of preferred hydrosilylation catalysts (B)(ii)(b) are platinum-based catalysts, such as platinum black, platinum on various solid supports, chloroplatinic acid, alcoholic solutions of chloroplatinic acid, and complexes of chloroplatinic acid with ethylenically unsaturated compounds such as olefins and organosiloxanes containing ethylenically unsaturated hydrocarbon groups bonded to silicon. Usable soluble platinum compounds include, for example, platinum-olefin complexes of the formulae (PtCl2(olefin)2 and H(PtCl3.olefin), where preference is given in this context to the use of alkenes having 2 to 8 carbon atoms, such as ethylene, propylene, the isomers of butene and octene, or cycloalkanes having 5 to 7 carbon atoms, such as cyclopentene, cyclohexene, and cycloheptene. Other soluble platinum catalysts are, for example, platinum complexes of the formula (PtCl2C3H6)2. Gold-cyclopropane complexes, reaction products of hexachloroplatinic acid with alcohols, ethers, and aldehydes or mixtures thereof, or reaction products of hexachloroplatinic acid with methylvinylcyclotetrasiloxane in the presence of sodium bicarbonate in ethanolic solution. Platinum catalysts with phosphorus, sulfur, and amine ligands, for example (Ph3P)2PtCl2, and complexes of platinum with vinylsiloxanes such as sym-divinyltetramethyldisiloxane, can also be used.

[0043] Therefore, specific examples of suitable platinum-based catalysts include: (i) Complexes of chloroplatinic acid with organosiloxanes containing ethylenically unsaturated hydrocarbon groups, as described in U.S. Pat. No. 3,419,593; (ii) Chloroplatinic acid in either the hexahydrate or anhydrous form; (iii) a platinum-containing catalyst obtained by a process comprising reacting chloroplatinic acid with an aliphatically unsaturated organosilicon compound, such as divinyltetramethyldisiloxane; (iv) alkene-platinum-silyl complexes as described in U.S. Pat. No. 6,605,734, such as (COD)Pt(SiMeCl2)2, where "COD" is 1,5-cyclooctadiene; and / or (v) Karstedt's catalysts, i.e. platinum divinyltetramethyldisiloxane complexes containing about 1% by weight of platinum in a solvent such as toluene, which may typically be used. These are described in U.S. Patent Nos. 3,715,334 and 3,814,730.

[0044] The hydrosilylation catalyst (B)(ii)(b) of the hydrosilylation-curable silicone elastomer composition is present in the overall composition in a catalytic amount, i.e., an amount or quantity sufficient to catalyze the addition / hydrosilylation reaction and cure the composition into an elastomeric material under desired conditions. Varying levels of the hydrosilylation catalyst (B)(ii)(b) can be used to adjust the reaction rate and cure reaction rate. The catalytic amount of the hydrosilylation catalyst (B)(ii)(b) is generally from 0.01 ppm to 10,000 ppm, alternatively from 0.01 to 5000 ppm, alternatively from 0.01 to 3,000 ppm, alternatively from 0.01 to 1,000 ppm, by weight of platinum group metal per million parts (ppm) based on the weight of the polymer (A) and filler (C) of the composition. In certain embodiments, the catalytic amount of catalyst may range from 0.01 to 1,000 ppm, alternatively 0.01 to 750 ppm, alternatively 0.01 to 500 ppm, alternatively 0.01 to 100 ppm, based on the weight of the composition. The ranges may relate to only the metal content in the catalyst, or to the entire catalyst (including its ligands), as specified, but typically these ranges relate to only the metal content in the catalyst. The catalyst may be added as a single species or as a mixture of two or more different species. Typically, the amount of catalyst present is in the range of 0.001 to 3.0 wt% of the composition, depending on the form / concentration in which the catalyst package is provided.

[0045] Component (C) is one or more reinforcing fillers, preferably provided in finely divided form, optionally in combination with one or more and / or non-reinforcing fillers. The reinforcing fillers of component (C) may be exemplified by fumed silica, preferably in finely divided form, and / or precipitated silica, preferably in finely divided form, and / or colloidal silica, and / or a suitable silicone resin.

[0046] Precipitated silica, fumed silica and / or colloidal silica are generally at least 50m 2 They are particularly preferred due to their relatively high surface area of ​​50 to 450 m / g (BET method according to ISO 9277:2010). 2 / g (BET method according to ISO9277:2010), or 50-300m 2 Use fillers with a surface area of ​​0.1 μm / g (BET method according to ISO 9277:2010). All these types of silica are commercially available.

[0047] If the reinforcing filler (C) is naturally hydrophilic (e.g., untreated silica filler), it is typically treated with a treating agent to render it hydrophobic. The resulting surface-modified reinforcing filler (C) does not agglomerate and can be homogeneously incorporated into the organopolysiloxane / polydiorganosiloxane polymer (A) described below, since the surface treatment allows the filler to be easily wetted by the organopolysiloxane / polydiorganosiloxane polymer (A).

[0048] Typically, the reinforcing filler (C) can be surface-treated with any low molecular weight organosilicon compound disclosed in the art that can be applied to prevent creping of the organosiloxane composition during processing.For example, organosilanes, polydiorganosiloxanes, or organosilazanes, such as hexaalkyldisilazanes, short chain siloxanediols, that make the filler hydrophobic and thus easier to handle and to obtain a homogeneous mixture with other raw materials. Specific examples include, but are not limited to, silanol-terminated trifluoropropylmethylsiloxane, silanol-terminated vinylmethyl (ViMe) siloxane, silanol-terminated MePh siloxane, liquid hydroxyldimethyl-terminated polydiorganosiloxanes containing an average of 2 to 20 repeating units of diorganosiloxane in each molecule, hydroxyldimethyl-terminated phenylmethylsiloxane, hexamethyldisiloxane, divinyltetramethyldisiloxane and other hexamethyldisilazane ( hexaorganodisilazanes, such as HMDZ, divinyltetramethyldisilazane, and tetramethyldi(trifluoropropyl)disilazane; hydroxyldimethyl-terminated polydimethylmethylvinylsiloxane, octamethylcyclotetrasiloxane, and silanes, including but not limited to methyltrimethoxysilane, dimethyldimethoxysilane, vinyltrimethoxysilane, methyltriethoxysilane, vinyltriethoxysilane, chlorotrimethylsilane, dichlorodimethylsilane, trichloromethylsilane. A small amount of water can be added with the silica treating agent as a processing aid.

[0049] The surface treatment can be carried out prior to introduction into the composition or in situ (i.e., by mixing these components together at room temperature in the presence of at least a portion of the other ingredients of the compositions herein until the filler is completely treated). Typically, untreated reinforcing filler (C) is treated with a treating agent in situ in the presence of polydiorganosiloxane polymer (A), thereby preparing a silicone elastomer base material that can then be mixed with other ingredients.

[0050] The reinforcing filler (C) is present in an amount of 5.0-40 wt% of the solids content of the composition, alternatively 7.5-35 wt% of the solids content of the composition, alternatively 10.0-35 wt% based on the weight percent of the solids content of the composition. From this, the amount of reinforcing filler (C) herein, such as micronized silica and / or silicone resin, can therefore be, for example, 2.0-20 wt% of the total composition, alternatively 2.5-15 wt% of the total composition. In some cases, the amount of reinforcing filler can be 5.0-15 wt% based on the weight of the total composition.

[0051] Non-reinforcing fillers may optionally be included in component (C) herein. These may include, for example, crushed quartz, calcium carbonate, diatomaceous earth, barium sulfate, iron oxide, titanium dioxide and carbon black, talc, wollastonite, aluminite, calcium sulfate (anhydrite), gypsum, calcium sulfate, magnesium carbonate, clays such as kaolin, aluminum trihydroxide, magnesium hydroxide (hydrotalcite), graphite, copper carbonates such as malachite, nickel carbonates such as zarachite, barium carbonates such as witherite, and / or strontium carbonates such as strontianite.

[0052] Other non-reinforcing fillers may include aluminum oxide, silicates from the group consisting of the olivine family, the garnet family, aluminosilicates, cyclic silicates, chain silicates, and layered silicates. The olivine family includes silicate minerals such as, but not limited to, forsterite and Mg2SiO4. The garnet family includes red garnet; Mg3Al2Si3O 12 ; green garnet; and Ca2Al2Si3O 12 The aluminosilicates include, but are not limited to, ground silicate minerals such as sillimanite, Al2SiO5, mullite, 3Al2O32SiO2, kyanite, and Al2SiO5. Cyclic silicates may also be utilized as non-reinforcing fillers, such as cordierite and Al3(Mg,Fe)2[Si4AlO 18The chain silicate family includes ground silicate minerals such as, but not limited to, wollastonite and Ca[SiO3]. Layered silicates may alternatively or additionally be used as non-reinforcing fillers, suitable groups include silicate minerals such as, but not limited to, mica; K2Al 14 [Si6Al2O 20 ](OH)4;phyllite;Al4[Si8O 20 ](OH)4;Talc;Mg6[SiO 20 ](OH)4; serpentine, e.g. asbestos; kaolinite; Al4[Si4O 10

[0036] (OH)8; and vermiculite. In one alternative, the filler is selected from one or more of fumed silica, precipitated silica, calcium carbonate, talc, mica, quartz, and aluminum oxide.

[0053] As previously indicated, component (D) above is (i) at least one unsaturated group per molecule selected from an alkenyl group and an alkynyl group, and (ii) Polyorganosiloxanes having anhydride and aromatic functionality, where the carbon of the aromatic functionality is separated from the carbon of the carbonyl group of the anhydride by a carbon chain containing 1 to 3 non-aromatic carbon atoms. Component (D) may be prepared as described in International PCT Application No. 20 / 044709, published by the applicant as WO 2021 / 0260055, the contents of which are incorporated herein by reference.

[0054] Component (D) may have the same general structure as the linear or branched organopolysiloxane component (A), i.e., it may be a linear or branched organopolysiloxane, and the unsaturated groups of component (D)(i) are the same as the unsaturated groups in component (A), with the proviso that: Except that component (D) may have a viscosity of from 5 to over 100,000 MPa.s at 25°C. A portion of the unsaturated groups in component (A) are replaced by anhydride functional groups in (D)(ii), resulting in the existence of components (D)(i) and (D)(ii). This is accomplished using a functionalization reaction, described below, which introduces anhydride functionality onto the polyorganosiloxane by radical grafting.

[0055] Anhydride functionality can be added onto the polysiloxane by radical grafting. For example, an alkenyl-functional polysiloxane (e.g., a vinyl-functional polyorganosiloxane) can be combined with an unsaturated anhydride (e.g., maleic anhydride) in the presence of a radical initiator, allowing a free radical grafting reaction to occur between the alkenyl group of the polysiloxane and the unsaturated portion of the anhydride to graft the anhydride onto the polyorganosiloxane. The reaction is often carried out with an aromatic initiator and / or in an aromatic solvent, so that the radicals of the initiator and / or solvent are also grafted onto the anhydride. In this application, it is necessary to have both the unsaturated and anhydride groups on the same molecule. To ensure that this occurs, i.e., a partial conversion approaching 50% occurs to obtain an average of one anhydride and one vinyl on the end-functional siloxane, the process is controlled by using a stoichiometric deficiency of the anhydride reagent relative to the vinyl on the siloxane.

[0056] As an example, R 4 and R 5 where V is an alkyl group and Vi refers to a vinyl group, the vinyl-functional polyorganosiloxane can be combined with maleic anhydride in an aromatic solvent (such as xylene or toluene) along with a radical initiator such as dibenzoyl peroxide and then heated to initiate the free radical reaction: [ka] When a substoichiometric amount of anhydride is utilized, the primary reaction product obtained is (a) below, although some (b) and (c) may also be present, depending on the molar ratio of the reactants. (a) Monofunctional polyorganosiloxane: ViR 4 2SiO-(R 5 2SiO) m -SiR 4 2A' (b) Bifunctional polyorganosiloxane: A'R 4 2SiO-(R 5 2SiO) m -SiR 4 2A'; (c) Unreacted vinyl-functional polyorganosiloxane: ViR 4 2SiO-(R 5 2SiO) m -SiR 4 2Vi; [ka] And A' is where X is an aromatic group that is the remainder of a solvent (e.g., a tolyl or xylyl group) or an initiator (e.g., a benzoyl group).

[0057] In a preferred embodiment, the polymer backbone of the siloxane starting material may be a dimethylmethylalkenyl copolymer backbone, typically a dimethylmethylvinyl copolymer backbone, in which case the pendant groups A' may be designed to partially replace the pendant alkenyl (vinyl) groups of the starting material. Thus, component (D) may be represented by the formula [ka] wherein Each R 4 is an alkyl group, and each R 5 is an alkyl group, an alkenyl group, an alkynyl group, or A', and A' is [ka] where X is an aromatic group and each molecule contains at least one alkenyl or alkynyl group. In one embodiment, X can be any suitable aromatic group, such as, but not limited to, a benzoyl group, a tolyl group, or a xylyl group.

[0058] The average concentration of anhydride functional groups (D)(ii) on the second polyorganosiloxane, component (D), can be determined based on the number of reactive sites (e.g., alkenyl groups) in the polyorganosiloxane prior to functionalization with anhydride and then determining the ratio of anhydride groups to the number of reactive sites in component (D). This can be done by dividing the number of reactive sites and anhydride groups by: 1 This can be accomplished by measuring the number of reactive sites and anhydride groups using H nuclear magnetic resonance (NMR) spectroscopy, or alternatively Fourier Transform Infrared (FTIR) spectroscopy. For example, the number of reactive sites and anhydride groups can be measured using 1,4-dioxane as an internal standard. 1 H NMR spectroscopy is used to measure. The concentrations of functional groups such as alkenyl and anhydride can be calculated using the following calculations:

number

[0059] Depending on the intended use of the curable silicone elastomer composition, optional additives may be present in the composition, including one or more cure inhibitors, mold release agents, peroxides and / or pigments, conductive fillers, thermally conductive fillers, pot life extenders, flame retardants, lubricants, UV light stabilizers, germicides, wetting agents, heat stabilizers, chain extenders, compression set additives, and plasticizers.

[0060] Cure inhibitors are used as necessary to prevent or slow down the addition reaction cure process, especially during storage. Optional cure (addition reaction) inhibitors for platinum-based catalysts are well known in the art, and include hydrazines, triazoles, phosphines, mercaptans, organic nitrogen compounds, acetylene alcohols, silylated acetylene alcohols, maleates, fumarates, ethylenically or aromatically unsaturated amides, ethylenically unsaturated isocyanates, olefinic siloxanes, unsaturated hydrocarbon monoesters and diesters, conjugated ene-ynes, hydroperoxides, nitriles, and diaziridines. Alkenyl-substituted siloxanes, such as those described in US Pat. No. 3,989,667, may also be used, of which cyclic methylvinylsiloxanes are preferred.

[0061] One class of known hydrosilylation reaction inhibitors includes the acetylenic compounds disclosed in U.S. Patent No. 3,445,420. Acetylenic alcohols such as 2-methyl-3-butyn-2-ol constitute a preferred class of inhibitors which suppress the activity of platinum-containing catalysts at 25° C. Typically, compositions containing these inhibitors must be heated to temperatures of 70° C. or above in order to cure at a practical rate.

[0062] Examples of acetylene alcohols and their derivatives include 1-ethynyl-1-cyclohexanol (ETCH), 2-methyl-3-butyn-2-ol, 3-butyn-1-ol, 3-butyn-2-ol, propargyl alcohol, 1-phenyl-2-propyn-1-ol, 3,5-dimethyl-1-hexyn-3-ol, 1-ethynylcyclopentanol, 3-methyl-1-penten-4-yn-3-ol, and mixtures thereof. Derivatives of acetylene alcohols may include those compounds having at least one silicon atom.

[0063] In some cases, inhibitor concentrations as low as 1 mole of inhibitor per mole of catalyst metal, if present, will impart satisfactory storage stability and cure rates. In other cases, inhibitor concentrations of up to 500 moles of inhibitor per mole of catalyst metal are necessary. The optimum concentration for a given inhibitor in a given composition is readily determined by routine experimentation. Depending on the concentration and form in which the selected inhibitor is commercially provided / marketed, if present in the composition, the inhibitor is generally present in an amount of 0.0125-10% by weight of the composition.

[0064] There may further be present dimethylvinyl polydiorganosiloxanes having a viscosity of 10 to 750 mPa.s at 25°C. Such dimethylvinyl polydiorganosiloxanes typically have a similar structure to component (A), polydimethylsiloxane polymer chains with dimethylvinyl end groups, but potentially some combination of vinylmethyl groups along the length of the polymer chain. For these polymers, the main difference is the chain length and the resulting viscosity, in contrast to component (A), this type of polymer has a zero shear viscosity of 10 to 750 mPa.s at 25°C. The zero shear viscosity is obtained by fitting to zero the values ​​obtained at low shear rates where the viscosity-shear rate curve is rate independent, which is a value independent of the test method. The zero shear viscosity of a material at 25° C. is typically obtained using a rheometer such as an Anton-Paar MCR-301 rheometer equipped with a 25 mm cone-plate fixture, or a viscometer such as a Brookfield™ rotational viscometer using spindles (LV-1-LV-4) and adapting the speed according to the polymer viscosity.

[0065] Examples of conductive fillers include metal particles, metal oxide particles, metal coated metal particles (such as silver plated nickel), metal coated non-metallic core particles (such as silver coated talc, or mica, or quartz), and combinations thereof. The metal particles may be in the form of powders, flakes, or filaments, and mixtures or derivatives thereof.

[0066] Examples of thermally conductive fillers include boron nitride, alumina, metal oxides (such as zinc oxide, magnesium oxide, and aluminum oxide), graphite, diamond, and mixtures or derivatives thereof.

[0067] Examples of chain extenders include linear organopolysiloxanes containing two silicon-bonded hydrogen groups at terminal positions. Such chain extenders are different from component (B)(ii)(a), which is a crosslinker in the form of an organosilicon compound containing at least two or three silicon-bonded hydrogen atoms per molecule. Typically, the chain extender will have two Si-H groups and the crosslinker will have at least three Si-H groups. Examples of chain extenders include, but are not limited to, disiloxanes or low molecular weight polyorganosiloxanes containing two silicon-bonded hydrogen atoms at terminal positions. Chain extenders generally react with the alkenyl groups of polymers (i) and (ii) to link two or more molecules of polymers (i) and (ii) together, increasing the effective molecular weight and the distance between potential crosslinking sites.

[0068] Disiloxanes are typically represented by the general formula (HR a 2Si)2O. When the chain extender is a polyorganosiloxane, it has the general formula HR a 2SiO 1 / 2 and the terminal units of formula R b 2SiO. In these formulas, R a and R b independently represent an unsubstituted or substituted monovalent hydrocarbon group having no ethylenic unsaturation and no fluorine content, including, but not limited to, alkyl groups containing 1 to 10 carbon atoms, substituted alkyl groups containing 1 to 10 carbon atoms such as chloromethyl, cycloalkyl groups containing 3 to 10 carbon atoms, aryl groups containing 6 to 10 carbon atoms, alkaryl groups containing 7 to 10 carbon atoms such as tolyl and xylyl, and aralkyl groups containing 7 to 10 carbon atoms such as benzyl groups.

[0069] Further examples of chain extenders include tetramethyldihydrogendisiloxane or dimethylhydrogen terminated polydimethylsiloxane.

[0070] The chain extender may be added in an amount of 1 to 10 parts by weight based on the weight of polymers (i) and (ii), typically 1 to 10 parts per 100 parts of the total of polymers (i) and (ii).

[0071] Examples of flame retardants include aluminum trihydrate, magnesium hydroxide, magnesium silicate, chlorinated paraffins, chlorinated paraffins, hexabromocyclododecane, triphenyl phosphate, dimethylmethylphosphonate, tris(2,3-dibromopropyl)phosphate (tris)brominated, and mixtures or derivatives thereof.

[0072] Examples of pigments include iron oxide, carbon black, and mixtures or derivatives thereof.

[0073] Examples of the lubricant include tetrafluoroethylene, resin powder, graphite, fluorinated graphite, talc, boron nitride, fluorine oil, silicone oil, molybdenum disulfide, and mixtures or derivatives thereof.

[0074] Further additives include silicone fluids such as trimethylsilyl or OH terminated siloxanes. Such trimethylsiloxy or OH terminated polydimethylsiloxanes typically have a viscosity of less than 150 mPa.s at 25° C. Such silicone fluids, when present, may be present in the curable silicone elastomer composition in an amount ranging from 0.1 to 5 wt %, based on the total weight of the composition.

[0075] The curable silicone elastomer composition comprises The present invention may include a curable silicone elastomer composition capable of achieving significant adhesion on a thermoplastic substrate, on an organic resin substrate, or on both a thermoplastic and an organic resin substrate surface, which comprises the following components: Ingredient A one or more organopolysiloxanes containing at least two alkenyl groups per molecule and having a viscosity in the range of 1000 mPa.s to 500,000 mPa.s at 25° C., in an amount of 10 to 85% by weight based on the total weight of the composition, alternatively 20 to 80% by weight based on the total weight of the composition, alternatively 20 to 75% by weight based on the total weight of the composition, alternatively 30 to 65% by weight based on the total weight of the composition, Component B When component (B) is (B)(i), the organic peroxide may be present in an amount of from 0.2 to 3 weight percent, alternatively from 0.2 to 2 weight percent, in each case based on the weight of the composition. or if component (B)(ii)(a), an organopolysiloxane containing at least 2 or 3 silicon-bonded hydrogen atoms per molecule in an amount of 0.1 to 40% by weight of the total composition, alternatively 0.5 to 20% by weight of the total composition, alternatively 0.5 to 10% by weight of the total composition, and further alternatively 1% to 5% by weight of the total composition; at least one hydrosilylation catalyst, if component (B)(ii)(b), in an amount of from 0.01 to 10% by weight of the total composition, alternatively from 0.01% to 5% by weight of the total composition, further alternatively from 0.05% to 2% by weight of the total composition; Component (C), at least one reinforcing filler and optionally one or more non-reinforcing fillers, in an amount of 1 to 80% by weight based on the total weight of the composition, alternatively 1 to 50% by weight based on the total weight of the composition, alternatively 5 to 50% by weight based on the total weight of the composition, and further alternatively 8 to 30% by weight based on the total weight of the composition; Component (D) is also included.

[0076] The present disclosure is intended to include any of the above combinations providing that the total composition % of components (A)-(D) and optional additives constitutes 100% by weight of the composition.

[0077] When cured by hydrosilylation, it is important that the catalyst (B)(ii)(b) is stored separately from the crosslinker (B)(ii)(a) to prevent premature curing during storage. Typically, the catalyst (B)(ii)(b) is included in the Part A composition, and the crosslinker (B)(ii)(a) and optional inhibitor are stored in the Part B composition.

[0078] Optional additives (except inhibitors) can be in either part (A) or part (B), or in both parts. They can also be added to the final mixture after parts (A) or (B) are combined.

[0079] In one embodiment, a) forming a mixture of a curable silicone elastomer composition as described herein; b) optionally applying the mixture onto a surface of a substrate after the substrate has been surface treated, for example by plasma, corona and / or UV-C; c) curing the mixture at a temperature of 80-250°C.

[0080] In step (a), if the composition is stored in multiple parts prior to use, the different parts are combined together and mixed homogeneously, with an optional subsequent step of adding any additional additives that may be required for the end use of the composition.

[0081] The substrate can be any suitable thermoplastic or organic resin substrate. Examples of substrates include acrylonitrile-butadiene-styrene, polyphenylene / styrene blends, polystyrene, polycarbonate (PC), polyurethane, styrene resin, polyethylene, polypropylene, acrylic, polyacrylate, polymethacrylate, polyacrylamide, polyester, polyethylene terephthalate, polybutylene terephthalate (PBT), polyphenylene oxide, polyphenylene sulfide, polysulfone, nylon, polyamide (PA), blends of polyamide resin with syndiotactic polystyrene, polyimide, fluoropolymer, and liquid crystal resin, non-resin-containing polyetherimide; phenolic resin, epoxy resin, epoxy molding compound, urea resin, melamine resin, alkyd resin, acrylonitrile-butadiene-styrene, styrene-modified poly(phenylene oxide), poly(phenylene sulfide), vinyl ester, or polyphthalamide, and combinations thereof. Other substrates may include, for example, metals, cellulose, and fabrics / textiles, for example, on cotton or other natural and synthetic fiber garments. Any of the above may be activated, for example, plasma, corona, or UV-C activated, if desired. Typically, if the composition is not self-adhesive, the compositions herein may be applied to metal substrates, for example, silicon, aluminum, stainless steel alloys, titanium, copper, nickel, silver, gold, and combinations thereof.

[0082] The intimate mixing of the components of the curable silicone elastomer composition can be carried out using any suitable mixing means, such as a kneader mixer, a Z-blade mixer, a two-roll mill (open mill), a three-roll mill, a Haake® Rheomix OS Lab mixer, a screw extruder or a twin-screw extruder, etc. Alternatively, speed mixers such as those sold by Hauscheric, such as DC150.1FV, DAC400FVZ, or DAC600FVZ, can be used.

[0083] The curable silicone elastomer composition may be processed (or cured) by injection molding, press molding, extrusion molding, transfer molding, press vulcanization, or calendaring.

[0084] Curing can be carried out, for example, in a mold to form a molded silicone article, for example, attached to a polycarbonate substrate. The curable silicone elastomer composition can be injection molded to form an article, for example, attached to a polycarbonate material, or the composition can be overmolded by injection molding around or on a thermoplastic substrate, an organic resin substrate, or a thermoplastic and organic resin substrate or article. When cured in the presence of a heat-sensitive substrate, the curable silicone elastomer composition as described herein above is cured under conditions that allow the development of mechanical adhesion with the heat-sensitive substrate, more specifically, using a temperature and cure time that does not cause the heat-sensitive substrate to deform, melt, or be modified.

[0085] The curable silicone elastomer composition can be cured into thermoplastic substrates, organic resin substrates, or silicone elastomer articles applied to thermoplastic and organic resin substrates, such as tubes, strips, solid cords, or custom profiles, according to manufacturer size specifications.

[0086] The curable silicone elastomer composition as described herein above can be applied to the surface of a substrate by any suitable means, such as rolling, spreading, 3D printing, etc., and cured as described above. After the curable silicone elastomer composition is applied onto the substrate, the composition is cured at a curing temperature ranging from 80° C. to 250° C. Such temperatures are generally determined by the materials involved. In the case of 3D printing, the 3D printer may be selected from a fused filament fabrication printer, a selective laser sintering printer, a selective laser melting printer, a stereolithography printer, a powder bed (binder jet) printer, a material jet printer, a direct metal laser sintering printer, an electron beam melting printer, a laminated object manufacturing deposition printer, a directed energy deposition printer, a laser powder forming printer, a polyjet printer, an ink-jetting printer, a material jetting printer, and a syringe extrusion printer.

[0087] In one embodiment herein, there is provided an article comprising a silicone elastomer cured from a curable silicone elastomer composition as described herein above, or an article comprising a silicone elastomer cured from a curable silicone elastomer composition on a rigid or flexible substrate such as the type described above.

[0088] In another embodiment, a composite part is provided, comprising a silicone elastomer cured from the curable silicone elastomer composition as described herein above on a rigid or flexible substrate. It should be understood that such composite parts include structures in which either the substrate and the silicone elastomer are used as integral components in the article. Examples of substrates as described above.

[0089] In one embodiment, an article or composite part is provided that includes an elastomeric material produced from the above curable silicone elastomer composition deposited on a thermoplastic substrate, an organic resin substrate, or a thermoplastic and organic resin substrate such as those described above.

[0090] In another embodiment, the curable silicone elastomer composition as described herein above can be applied to the surface of a substrate to be processed using a 3D printing method. A typical method for forming a three-dimensional (3D) article may include multiple steps. For example, the method may include (i) providing a thermoplastic substrate, an organic resin substrate, or a thermoplastic and organic resin substrate. The method may further include (ii) heating the substrate. The method may also include (iii) printing the curable silicone elastomer composition as described herein above on the substrate with a 3D printer to form a subsequent layer. Optionally, the latter step may be repeated as necessary to apply one or more additional layers.

[0091] Examples of such articles or composite parts can be found in various industries, including but not limited to automotive applications, medical applications, consumer and industrial applications, electronic applications, in all the above cases. In automotive applications, this may include housings with silicone seals or gaskets, plugs and connectors, components of various sensors, membranes, bulkheads, climate ventilation components, etc. Electronic applications may include mobile phone cover seals, mobile phone accessories, precision electronics, electrical switches and switch covers, watches and wristbands, wearable appliances, such as face masks, wearable electronic devices, etc.; communication equipment, game consoles, watches, image receivers, DVD equipment, MD equipment, CD equipment, and other precision electronics, microwave ovens, refrigerators, electric rice cookers, televisions, LCD televisions and plasma televisions flat screen displays, various home appliances, copiers, printers, facsimile machines, and other office automation (OA) equipment, connector seals, spark plug caps, components of various sensors, and other parts of automotive components. EXAMPLES

[0092] All viscosities in the following examples were measured using a rheometer such as an Anton-Paar MCR-301 rheometer equipped with a 25 mm cone-plate fixture and operated at 25° C., unless otherwise stated. Viscosity is reported as zero shear viscosity, meaning the value extrapolated from the statistically significant rate-independent Newtonian region of the viscosity versus shear rate sweep to zero shear rate, unless otherwise stated. Vinyl and Si-H weight percentages were determined using quantitative infrared analysis according to ASTM E168. In the first series of examples, a reference example and three examples were provided with compositions containing the following components: [Table 1]

[0093] The treated filler was a fumed silica sold under the trade name CAB-O-SIL™ S-17D by Cabot Corporation that had been treated with hexamethyldisilazane (HMDZ) and tetramethyldivinyldisilazane.

[0094] In the first series of examples below, four alternative adhesion promoters were utilized, which were prepared according to the methods described in International PCT Application No. / US20 / 044709, published as WO 2021 / 0260055. Adhesion promoter 1: ViR 4 2SiO-(R 5 2SiO) m -SiR 4 2Vi [wherein, R 4 and R 5 is methyl, and the average value of m is 177] with maleic anhydride (MAH) and AH and benzoyl peroxide (BPO) in m-xylene, the resulting product having a vinyl equivalent weight (g / mol Vi) of 9600 and an anhydride equivalent weight (g / mol anhydride) of 22,000. Adhesion promoter 2 ViR 4 2SiO-(R 5 2SiO) m -SiR 4 2Vi [wherein, R 4 and R 5 is methyl, and the average value of m is 46] with maleic anhydride and benzoyl peroxide (BPO) in m-xylene; the resulting product had a vinyl equivalent weight (g / mol Vi) of 3700 and an anhydride equivalent weight (g / mol anhydride) of 3900. Adhesion promoter 3 ViR 4 2SiO-(R 5 2SiO) m -SiR 4 2Vi [wherein, R 4 and R 5is methyl, and the average value of m is 7] with maleic anhydride and benzoyl peroxide (BPO) in m-xylene, the resulting product having a vinyl equivalent weight (g / mol Vi) of 1000 and an anhydride equivalent weight (g / mol anhydride) of 860. Adhesion Promoter 4 is a further example using the starting components identified for Adhesion Promoter 3, but using a reduced MAH:Vi ratio than that used for Additive 3, resulting in a vinyl equivalent weight (g / mol Vi) of 590 and an anhydride equivalent weight (g / mol anhydride) of 1400. In the above, estimates of the average value of m were determined from the number average molecular weight (Mn) of the polymer peak obtained by GPC in a solvent such as toluene calibrated with polystyrene standards by using the following formula:

number

number

number

[0095] The seven different compositions evaluated were prepared by making a Part A composition, then a Part B composition, and then mixing the Part A and Part B compositions in a 1:1 ratio by weight. [Table 2]

[0096] Adhesion promoters 1 and 2 were added directly to Part A. Adhesion promoters 3 and 4 were found to be solids and were solubilized in one equivalent of acetone, which was then mixed into the Part A composition. The acetone was then allowed to evaporate.

[0097] Part A composition was prepared using a Flacktek speedmixer®, the ingredients were added to a polypropylene dental cup, the mixture was then mixed at 2000 rpm for 20 seconds, followed by hand scraping to mix. The sample was mixed at 2000 rpm for an additional 20 seconds, followed by hand scraping to mix, then mixed at 2000 rpm for 20 seconds for the final mix. [Table 3]

[0098] A similar mixing protocol was used to mix Part B as was used for the Part A composition. Parts A and B were then mixed together in a 1:1 weight ratio.

[0099] Different compositions prepared by mixing the Part A composition and the Part B composition together were applied onto the two substrates. Substrate 1 (S.1) was polybutylene terephthalate (PBT) sold by BASF under the trade name Ultradur™ B4300G4 (20% glass fibre).

[0100] In each case, each substrate was wiped with isopropyl alcohol (IPA) and air-dried before applying the prepared composition. In each case, the prepared composition was then applied to the substrate at a thickness of 25 mils (0.0635 cm). The silicone composition was then cured in a forced air oven at 150°C for 1 hour. Using a razor blade, two perpendicular lines separated by approximately the width of the spatula blade were etched across the width of the substrate and through the depth of the cured material to the substrate surface. Manual pressure was applied to the material between the cuts with the spatula held down at an angle of approximately 30° from the substrate surface. The adhesion (or lack of adhesion) was then subjectively evaluated. [Table 4]

[0101] For the avoidance of doubt, above and in the tables below etc., when we refer to the total composition, this is to everything shown in the ingredients list. When we refer to the matrix, we are discussing the unfilled composition (total composition minus any processed fillers).

[0102] In Table 4, the designation is (-) poor adhesion = adhesive failure (separation from the substrate), and +) fair to good adhesion = mixed mode failure [cohesive failure (tear in the elastomer) and adhesive failure].

[0103] The above table shows the remarkable effect of anhydride-grafted additives in the compositions of the present invention compared to those without adequate levels of anhydride functionality. Note that additives with lower anhydride content (or higher equivalents of anhydride EWanh) require proportionally higher concentrations, by weight %, to be effective. For example, adhesion promoter 1 (EWanh=22000 g / mol) requires a much higher concentration (above the concentrations tested) in the LSR formulation than adhesion promoter 2 (EWanh=3900 g / mol) and adhesion promoter 3 (EWanh=860 g / mol) to be effective as an adhesion promoter in this formulation.

[0104] A second series of examples was prepared using alternative compositions. The previously unidentified components are set forth below in Table 5, and the compositions themselves are set forth in Table 6. [Table 5]

[0105] In this case, adhesion promoter 1 as described above is utilized as the adhesion promoter, and the corresponding polymer starting material for making adhesion promoter 1, i.e., ViMe2SiO[Me2SiO] having a viscosity of about 443 mPa.s, is used. 177 Comparison was made with SiMe2Vi (hereafter referred to as the anhydride-free additive). Particle size information for fillers 1, 2 and 3 is taken from the supplier's data sheets.

[0106] The following table lists the sample formulations from Part I showing the grams (g) of each component (Table 3), as well as the calculated anhydrous mmol concentration per 100 g of total formulation and matrix components (Table 4). [Table 6]

[0107] Sample preparation: In a dental cup, prepare "Inhibitor solution 1" and "Catalyst solution 1" as shown below.

[0108] Inhibitor solution 1 A sample of Inhibitor Solution 1 is prepared in a dental cup by first adding 2.00 g of Inhibitor 1, followed by 18.00 g of Polymer 2. The added components are then mixed at 2000 revolutions per minute (rpm) for 30 seconds.

[0109] Catalyst solution 1 A sample of catalyst solution 1 is prepared in a dental cup by first adding 2.00 g of platinum catalyst 1, followed by 18.00 g of polymer 2. The added components are then mixed at 200 revolutions per minute (rpm) for 30 seconds.

[0110] Preparation of Formulations In a dental cup, add the desired amount of Polymer 1, Polymer 2, Additive 1 or 2 (if applicable), Silane 1, Silane 2, and Filler 1. Hand mix gently and dental mix once at 1600 rpm for 30 seconds. Add Filler 2. Hand mix gently and dental mix once at 1600 rpm for 30 seconds. Add Filler 3. Hand mix gently and dental mix twice at 1600 rpm for 30 seconds. Add the desired amount of Inhibitor solution 1 and Crosslinker 1. Hand mix gently and dental mix once at 1600 rpm for 30 seconds. Add the desired amount of Catalyst solution 1. Hand mix gently and dental mix once at 1600 rpm for 30 seconds to obtain the final sample. [Table 7]

[0111] Explanation for calculation of mmol anhydride: mmol anhydride was calculated by dividing the number of grams of anhydride-grafted additive (e.g., maleic anhydride-grafted additive) in 100 g of the formulation or in 100 g of the matrix component (unfilled) itself (as shown in the table) by 22000 g / mol (for additive 1) and then multiplying by 1000.

[0112] A film-like polyester release liner (3M™ 9956 Medical Release Liner, polyester, fluoropolymer) with a fluorinated coating on one side was used as the substrate for curing the samples between the two sheets, with the polyester side of the substrate exposed to the sample. Each composition from Table 6 above was applied to the substrate surface and the sandwiched materials were cured at 150° C. for 1 hour and then evaluated for relative adhesive strength by determining whether cohesive failure resulted from a peel test. The results show that a control formulation without Additive 1 (Reference Example 1), a formulation with an additive that does not contain an anhydride functional group (Additive 2, Comparative Example 1), and a formulation containing 0.1 wt. % Additive 1 (Comparative Example 22) show adhesive failure. Formulations containing 0.5-2 wt. % Additive 1 show cohesive failure indicating improved relative adhesion to the substrate. This surprising result prompted previous examples using LSR demonstrating that adhesion to plastics and other substrates can be improved using component (D) described herein. These examples demonstrate that this is also achievable using filled siloxane systems, e.g., conductive composites.

[0113] To determine if cohesive failure had occurred, peel tests were performed at room temperature on the cured samples by manually peeling the two sheets apart.

Claims

1. 1. A curable silicone elastomer composition capable of achieving adhesion to a suitable material substrate, comprising: (A) one or more organopolysiloxanes containing at least two unsaturated groups per molecule selected from alkenyl and alkynyl groups, but containing no anhydride functionality, and having a viscosity in the range of 1000 mPa.s to 500,000 mPa.s at 25°C; (B) a curing agent, (B)(i) an organic peroxide radical initiator, or (B)(ii) a hydrosilylation curing catalyst package comprising: a. an organosilicon compound having at least two, or at least three, Si—H groups per molecule; and b. a curing agent comprising a hydrosilylation curing catalyst package comprising a hydrosilylation catalyst; (C) at least one reinforcing filler and optionally one or more non-reinforcing fillers; (D) a polyorganosiloxane, (i) at least one unsaturated group per molecule selected from an alkenyl group and an alkynyl group; and (ii) a polyorganosiloxane having an anhydride functional group and an aromatic functional group, where the carbon of the aromatic functional group is separated from the carbon of the carbonyl group of the anhydride by a carbon chain containing 1 to 3 non-aromatic carbon atoms; Component (D) is represented by the formula 【Chemistry 1】 wherein m is a number from 7 to 177, and each R 4 is an alkyl group, and each R 5 is an alkyl group, an alkenyl group, an alkynyl group, or A', and A' is 【Chemistry 2】 where X is a benzoyl, tolyl or xylyl group, and each molecule contains at least one alkenyl or alkynyl group; The component (D) is contained in an amount of 0.5 to 5% by weight based on the total amount of the composition. A curable silicone elastomer composition.

2. The curable silicone elastomer composition of claim 1 , wherein the composition comprises a cure inhibitor.

3. 10. The curable silicone elastomer composition of claim 1, stored in at least two separate parts prior to use.

4. 1. A process for preparing an article or a composite part of an article, comprising: a) forming a mixture of the curable silicone elastomer composition of claim 1; b) applying the mixture onto a surface of a substrate; c) curing the mixture at a temperature of 80-250°C.

5. The process of claim 4 , wherein the substrate is polycarbonate.

6. 10. An article cured from the curable silicone elastomer composition of claim 1.

7. 10. An article comprising a silicone elastomer cured from the curable silicone elastomer composition according to claim 1 applied to a plastic substrate.

8. 13. An article in which a silicone elastomer cured from the curable silicone elastomer composition according to claim 1 is applied to a thermoplastic substrate, an organic resin substrate, or both a thermoplastic substrate and an organic resin substrate.

9. Housings having silicone seals, gaskets, plugs, connectors, sensor components, membranes, bulkheads, or climate ventilation components; and personal electronic devices selected from mobile phone cover seals, mobile phone accessories, precision electronic equipment, electrical switches, switch covers, watches, wristbands, and wearable electronic devices; The article according to claim 6 or 7, wherein the article is selected from the group consisting of

10. 13. A composite comprising a silicone elastomer cured from the curable silicone elastomer composition of claim 1 on a substrate of a plastic, thermoplastic, or resinous material.

11. Housings with silicone seals, gaskets, plugs, connectors, sensor components, membranes, bulkheads, or climate ventilation components; A personal electronic device selected from a mobile phone cover seal, a mobile phone accessory, a precision electronic device, an electrical switch, a switch cover, a watch, a wristband, a wearable appliance, and a wearable electronic device; and Parts of components for mobile phones, mobile communication devices, game machines, watches, image receivers, DVD devices, MD devices, CD devices, microwave ovens, refrigerators, electric rice cookers, cathode ray televisions, LCD televisions and plasma televisions, copy machines, printers, facsimile machines, connector seals, spark plug caps or sensors; The compound of claim 10, wherein the compound is selected from the group consisting of

Citation Information

Patent Citations

  • Anhydride and aromatic functionalized polyorganosiloxanes

    WO2021026055A1

  • Silicone elastomer compositions

    WO2021262832A1