Coated Cutting Tools
The coated cutting tool with a Ti compound lower layer, α-type Al2O3 intermediate layer, and TiCN upper layer addresses the issue of chipping and wear resistance, enhancing tool life under high-speed and deep-cut conditions.
Patent Information
- Application Number
- JP2022195751
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-12-07
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2042-12-07
AI Technical Summary
Conventional coated cutting tools lack sufficient chipping resistance and wear resistance under high-speed and deep-cut conditions, leading to reduced tool life.
A coated cutting tool with a specific layer configuration comprising a lower layer of Ti compound, an intermediate layer of α-type Al2O3, and an upper layer of Ti compound, particularly TiCN, with controlled misorientation angles and thicknesses to enhance adhesion and wear resistance.
The tool exhibits improved chipping resistance and wear resistance, extending tool life significantly.
Smart Images

Figure 0007583376000016 
Figure 0007583376000001 
Figure 0007583376000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a coated cutting tool. [Background technology]
[0002] It is well known that coated cutting tools, which are formed by depositing a coating layer with a total thickness of 3 to 20 μm on the surface of a substrate made of cemented carbide by a chemical vapor deposition method, are used for cutting steel, cast iron, etc. As the coating layer, for example, a coating layer consisting of a single layer or a multilayer of two or more types selected from the group consisting of Ti carbides, nitrides, carbonitrides, carbonates, and carbonitrides, and aluminum oxide (Al2O3) is known.
[0003] Patent Document 1 describes a coated hard alloy having a coating layer on the surface of the hard alloy, the coating layer comprising an inner layer, an intermediate layer and an outer layer in that order from the hard alloy side, the inner layer including one or more layers selected from carbides, nitrides, borides, oxides and solid solutions thereof of Groups IVa, Va and VIa of the periodic table, the intermediate layer including one or more layers selected from aluminum oxide, zirconium oxide and solid solutions thereof, the outer layer including one or more layers selected from carbides, nitrides, borides, oxides and solid solutions thereof of Groups IVa, Va and VIa of the periodic table and aluminum oxide, including a titanium carbonitride layer having a columnar structure, and the coated hard alloy is characterized in that the relationship between the maximum roughness Amax of the surface layer portion of the intermediate layer and the maximum roughness Bmax of the surface layer portion of the titanium carbonitride layer having a columnar structure in the outer layer in the cross-sectional structure of the coated hard alloy satisfies Formula 1. (Bmax / Amax)<1 …Equation 1 (However, 0.5 μm <Amax<4.5μm 0.5μm≦Bmax≦4.5μm) Patent Document 1 also describes that the orientation index TC, as shown in Equation 3, of the titanium carbonitride layer having a columnar structure in the outer layer is largest in any one of the (220), (311), (331) and (422) planes, and that the maximum value is 1.3 or more and 3.5 or less.
number
[0004] [Patent Document 1] International Publication No. 2000 / 079022 Summary of the Invention [Problem to be solved by the invention]
[0005] In recent cutting processes, the trend toward higher speeds, higher feed rates, and deeper cuts has become more prominent, and there is a demand for tools with improved chipping resistance and wear resistance. In particular, cutting processes that impose loads on coated cutting tools, such as high-speed cutting of steel, have become more common in recent years, and under such severe cutting conditions, conventional tools do not have sufficient chipping resistance and wear resistance, making it difficult to extend the tool life. The coated hard alloy described in Patent Document 1 has excellent adhesion between the intermediate layer and the outer layer, but is insufficient in wear resistance and has room for improvement.
[0006] The present invention has been made in view of the above circumstances, and has an object to provide a coated cutting tool that has excellent chipping resistance and wear resistance, thereby enabling an extension of the tool life. [Means for solving the problem]
[0007] From the above viewpoints, the inventors have conducted extensive research into extending the tool life of coated cutting tools, and as a result have discovered that a specific configuration can improve chipping resistance and wear resistance, thereby making it possible to extend the tool life, which has led to the completion of the present invention.
[0008] That is, the present invention is as follows. [1] A coated cutting tool comprising a substrate and a coating layer formed on a surface of the substrate, The coating layer includes a lower layer, an intermediate layer, and an upper layer in this order from the substrate side toward the surface side of the coating layer, the lower layer includes one or more Ti compound layers each comprising a Ti compound of Ti and at least one element selected from the group consisting of C, N, O, and B; the intermediate layer includes an α-Al2O3 layer made of α-Al2O3, the upper layer includes one or more Ti compound layers each composed of a Ti compound of Ti and at least one element selected from the group consisting of C, N, and O, and at least one of the Ti compound layers in the upper layer is a TiCN layer; The average thickness of the upper layer is 1.00 μm or more and 6.50 μm or less, A coated cutting tool, wherein the upper layer satisfies the conditions represented by the following formulas (i) and (ii): 25≦RSA1<70 (i) (In formula (i), RSA1 is the ratio (unit: area %) of the cross-sectional area of a region in a cross-section of the upper layer perpendicular to the surface of the base material, where the misorientation A, which is the angle (unit: degree) between the normal to the (220) plane of each particle having a cubic crystal structure and the normal to the surface of the base material, is 0 degrees or more and less than 10 degrees, when the total area of the entire cross-section is taken as 100 area %).) 25≦RSA2<70 (ii) (In formula (ii), RSA2 is the ratio (unit: area %) of the cross-sectional area of a region in a cross-section of the upper layer perpendicular to the surface of the base material, where the misorientation A, which is the angle (unit: degree) between the normal to the (220) plane of each particle having a cubic crystal structure and the normal to the surface of the base material, is 20 degrees or more and less than 30 degrees, when the total area of the entire cross-section is taken as 100 area %).) [2] The coated cutting tool according to [1], wherein the sum of the RSA1 and RSA2 is 60 area % or more and 90 area % or less in the upper layer. [3] The coated cutting tool according to [1] or [2], wherein the upper layer is in contact with the intermediate layer, and the upper layer includes at least one layer selected from the group consisting of a layer of TiCO, a layer of TiON, and a layer of TiCNO as an adhesion layer on a side in contact with the intermediate layer, and the adhesion layer has an average thickness of 0.05 μm or more and 1.50 μm or less. [4] The coated cutting tool according to any one of [1] to [3], wherein in the intermediate layer, a texture coefficient TC(0,0,12) of the (0,0,12) plane of the α-type Al2O3 layer, represented by the following formula (1), is 5.9 or more and 8.9 or less.
number
[0009] The coated cutting tool of the present invention has excellent chipping resistance and wear resistance, thereby enabling an extended tool life. [Brief description of the drawings]
[0010] [Figure 1] 1 is a schematic cross-sectional view showing an example of a coated cutting tool of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, a mode for carrying out the present invention (hereinafter simply referred to as "the present embodiment") will be described in detail with reference to the drawings as necessary, but the present invention is not limited to the present embodiment described below. The present invention can be modified in various ways without departing from the gist of the invention. In addition, positional relationships such as up, down, left, and right in the drawings are based on the positional relationships shown in the drawings unless otherwise specified. Furthermore, the dimensional ratios of the drawings are not limited to the ratios shown in the drawings.
[0012] The coated cutting tool of this embodiment is a coated cutting tool including a substrate and a coating layer formed on a surface of the substrate. The coating layer includes a lower layer, an intermediate layer, and an upper layer, in this order from the substrate side toward the surface side of the coating layer. The lower layer includes one or more Ti compound layers made of a Ti compound with at least one element selected from the group consisting of Ti and C, N, O, and B. The intermediate layer includes an α-Al2O3 layer made of α-Al2O3. The upper layer includes one or more Ti compound layers made of a Ti compound with at least one element selected from the group consisting of Ti and C, N, and O. At least one of the Ti compound layers in the upper layer is a TiCN layer. The upper layer has an average thickness of 1.00 μm or more and 6.50 μm or less. The upper layer satisfies the conditions represented by the following formulas (i) and (ii). 25≦RSA1<70 (i) (In formula (i), RSA1 is the ratio (unit: area %) of the cross-sectional area of a region in a cross-section of the upper layer perpendicular to the surface of the substrate, where the misorientation A, which is the angle (unit: degree) between the normal to the (220) plane of each particle having a cubic crystal structure and the normal to the surface of the substrate, is 0 degrees or more and less than 10 degrees, when the total area of the entire cross-section is taken as 100 area %).) 25≦RSA2<70 (ii) (In formula (ii), RSA2 is the ratio (unit: area %) of the cross-sectional area of a region in a cross-section of the upper layer perpendicular to the surface of the substrate, where the misorientation A, which is the angle (unit: degree) between the normal to the (220) plane of each particle having a cubic crystal structure and the normal to the surface of the substrate, is 20 degrees or more and less than 30 degrees, when the total area of the entire cross-section is taken as 100 area %).)
[0013] The coated cutting tool of this embodiment has the above-mentioned configuration, and thus can improve chipping resistance and wear resistance, and as a result, can extend the tool life. The factors that improve the chipping resistance and wear resistance of the coated cutting tool of this embodiment are considered to be as follows. However, the present invention is not limited by the following factors. That is, first, the coated cutting tool of this embodiment has improved wear resistance because the average thickness of the upper layer is 1.00 μm or more. On the other hand, the coated cutting tool of this embodiment has improved adhesion between the upper layer and the intermediate layer because the average thickness of the upper layer is 6.50 μm or less, and thus has excellent chipping resistance. In addition, the coated cutting tool of this embodiment has excellent adhesion between the upper layer and the intermediate layer and excellent chipping resistance because RSA1 is 25 area % or more. On the other hand, the coated cutting tool of this embodiment has excellent wear resistance because RSA1 is less than 70 area %. In addition, the coated cutting tool of this embodiment has excellent wear resistance because RSA2 is 25 area % or more. On the other hand, the coated cutting tool of this embodiment is easy to manufacture because the RSA2 accounts for less than 70% by area. By combining these configurations, the coated cutting tool of this embodiment is improved in chipping resistance and wear resistance, and as a result, it is believed that the tool life can be extended.
[0014] 1 is a schematic cross-sectional view showing an example of a coated cutting tool according to the present embodiment. The coated cutting tool 6 includes a substrate 1 and a coating layer 5 formed on the surface of the substrate 1. In the coating layer 5, a lower layer 2, an intermediate layer 3, and an upper layer 4 are laminated in this order from the substrate side upward.
[0015] The coated cutting tool of the present embodiment includes a substrate and a coating layer formed on the substrate. Specific examples of the coated cutting tool include indexable cutting inserts for milling or turning, drills, and end mills.
[0016] The substrate used in this embodiment is not particularly limited as long as it can be used as the substrate of coated cutting tool.Such substrate can be, for example, cemented carbide, cermet, ceramics, cubic boron nitride sintered body, diamond sintered body and high speed steel.Among them, if the substrate is any of cemented carbide, cermet, ceramics and cubic boron nitride sintered body, it is preferable because it has better wear resistance and chipping resistance, and from the same viewpoint, it is more preferable that the substrate is cemented carbide.
[0017] The substrate may have a surface modified. For example, when the substrate is made of cemented carbide, a de-β layer may be formed on the substrate. When the substrate is made of cermet, a hard layer may be formed on the substrate. Even when the substrate is surface modified in this manner, the effects of the present invention can be achieved.
[0018] The coating layer used in this embodiment preferably has an overall average thickness of 10.00 μm or more and 30.00 μm or less. When the average thickness of the entire coating layer of the coated cutting tool of this embodiment is 10.00 μm or more, the wear resistance tends to be improved, and when the average thickness of the entire coating layer is 30.00 μm or less, the chipping resistance and fracture resistance tend to be excellent. From the same viewpoint, the average thickness of the entire coating layer is more preferably 13.50 μm or more and 26.45 μm or less, and even more preferably 14.70 μm or more and 25.05 μm or less. The average thickness of each layer and of the entire coating layer in the coated cutting tool of this embodiment can be determined by measuring the thickness of each layer or the thickness of the entire coating layer from three or more cross sections in each layer or the entire coating layer, and calculating the arithmetic mean value.
[0019] Bottom Layer The lower layer used in this embodiment includes one or more Ti compound layers made of a Ti compound of Ti and at least one element selected from the group consisting of C, N, O, and B. When the coated cutting tool includes the lower layer between the substrate and the intermediate layer including the α-Al2O3 layer, the wear resistance and adhesion are improved.
[0020] The Ti compound layer in the lower layer is not particularly limited, but examples thereof include a TiC layer made of TiC, a TiN layer made of TiN, a TiCN layer made of TiCN, a TiCO layer made of TiCO, a TiCNO layer made of TiCNO, a TiON layer made of TiON, and a TiB2 layer made of TiB2.
[0021] The lower layer may be composed of one layer or multiple layers (e.g., two or three layers), but is preferably composed of multiple layers, more preferably composed of two or three layers, and even more preferably composed of three layers. The Ti compound constituting the Ti compound layer contained in the lower layer is preferably at least one selected from the group consisting of TiN, TiC, TiCN, TiCNO, TiON and TiB2, from the viewpoint of further improving wear resistance and adhesion. In addition, in the coated cutting tool of this embodiment, it is preferable that at least one layer of the lower layer is a TiCN layer, since wear resistance is further improved. When the lower layer is composed of three layers, a TiC layer or a TiN layer may be formed as a first layer on the surface of the base material, a TiCN layer may be formed as a second layer on the surface of the first layer, and a TiCNO layer or a TiCO layer may be formed as a third layer on the surface of the second layer. Among them, the lower layer may form a TiN layer as a first layer on the surface of the substrate, a TiCN layer as a second layer on the surface of the first layer, and a TiCNO layer as a third layer on the surface of the second layer.
[0022] The average thickness of the lower layer used in this embodiment is preferably 3.00 μm or more and 15.00 μm or less. The coated cutting tool of this embodiment has a tendency to have improved wear resistance because the average thickness of the lower layer is 3.00 μm or more. On the other hand, the coated cutting tool of this embodiment has a tendency to have improved chipping resistance and fracture resistance because the average thickness of the lower layer is 15.00 μm or less. From the same viewpoint, the average thickness of the lower layer is more preferably 3.50 μm or more and 12.50 μm or less, and even more preferably 4.50 μm or more and 10.30 μm or less.
[0023] From the viewpoint of further improving wear resistance and chipping resistance, the average thickness of the TiC layer or TiN layer in the lower layer is preferably 0.05 μm or more and 2.00 μm or less. From the same viewpoint, the average thickness of the TiC layer or TiN layer in the lower layer is more preferably 0.10 μm or more and 1.80 μm or less, and further preferably 0.20 μm or more and 1.50 μm or less.
[0024] From the viewpoint of further improving the wear resistance and chipping resistance, the average thickness of the TiCN layer in the lower layer is preferably 2.00 μm or more and 15.00 μm or less. From the same viewpoint, the average thickness of the TiCN layer in the lower layer is more preferably 2.50 μm or more and 14.50 μm or less, and further preferably 3.00 μm or more and 12.00 μm or less.
[0025] From the viewpoint of further improving the wear resistance and chipping resistance, the average thickness of the TiCNO layer or TiCO layer in the lower layer is preferably 0.10 μm or more and 1.00 μm or less. From the same viewpoint, the average thickness of the TiCNO layer or TiCO layer in the lower layer is more preferably 0.20 μm or more and 0.50 μm or less.
[0026] The Ti compound layer in the lower layer is a layer consisting of a Ti compound of Ti and at least one element selected from the group consisting of C, N, O, and B, but may contain trace amounts of components other than the above elements as long as the effect of the lower layer is exhibited.
[0027] [Middle layer] The intermediate layer used in this embodiment includes an α-type Al2O3 layer made of α-type Al2O3.
[0028] The average thickness of the intermediate layer used in this embodiment is preferably 3.00 μm or more and 15.00 μm or less. When the average thickness of the intermediate layer is 3.00 μm or more, the wear resistance tends to be improved, and the control of TC (0,0,12) described later becomes easier. When the average thickness of the intermediate layer is 15.00 μm or less, the adhesion between the upper layer and the intermediate layer tends to be excellent, and the chipping resistance tends to be excellent. From the same viewpoint, the average thickness of the intermediate layer is more preferably 3.20 μm or more and 14.60 μm or less, and further preferably 4.00 μm or more and 13.00 μm or less.
[0029] In the coated cutting tool of this embodiment, the texture coefficient TC(0,0,12) of the (0,0,12) plane of the α-type Al2O3 layer, represented by the following formula (1), is preferably 5.9 or more and 8.9 or less in the intermediate layer.
number
[0030] The coated cutting tool of this embodiment tends to have excellent wear resistance and can increase the RSA2 value because the texture coefficient TC(0,0,12) of the (0,0,12) plane of the α-Al2O3 layer expressed by the above formula (1) is 5.9 or more in the intermediate layer. On the other hand, the coated cutting tool of this embodiment can be easily manufactured when the texture coefficient TC(0,0,12) of the (0,0,12) plane of the α-Al2O3 layer expressed by the above formula (1) is 8.9 or less in the intermediate layer. From the same viewpoint, the texture coefficient TC(0,0,12) of the (0,0,12) plane of the α-Al2O3 layer expressed by the above formula (1) is more preferably 6.3 to 8.9, and even more preferably 7.0 to 8.9. In this embodiment, the texture coefficient TC(0,0,12) of the (0,0,12) plane of the α-Al2O3 layer can be determined by the method described in the Examples below.
[0031] The intermediate layer only needs to have a layer made of α-type aluminum oxide (α-type Al2O3), and may or may not contain components other than α-type aluminum oxide (α-type Al2O3) as long as the effects of the present invention are achieved.
[0032] [Top layer] The upper layer used in this embodiment includes one or more Ti compound layers made of a Ti compound of Ti and at least one element selected from the group consisting of C, N, and O, and at least one of the Ti compound layers in the upper layer is a TiCN layer. In addition, the upper layer used in this embodiment satisfies the conditions represented by the following formulas (i) and (ii). 25≦RSA1<70 (i) (In formula (i), RSA1 is the ratio (unit: area %) of the cross-sectional area of a region in a cross-section of the upper layer perpendicular to the surface of the base material, where the misorientation A, which is the angle (unit: degree) between the normal to the (220) plane of each particle having a cubic crystal structure and the normal to the surface of the base material, is 0 degrees or more and less than 10 degrees, when the total area of the entire cross-section is taken as 100 area %).) 25≦RSA2<70 (ii) (In formula (ii), RSA2 is the ratio (unit: area %) of the cross-sectional area of a region in a cross-section of the upper layer perpendicular to the surface of the base material, where the misorientation A, which is the angle (unit: degree) between the normal to the (220) plane of each particle having a cubic crystal structure and the normal to the surface of the base material, is 20 degrees or more and less than 30 degrees, when the total area of the entire cross-section is taken as 100 area %).)
[0033] The coated cutting tool of this embodiment has excellent adhesion between the upper layer and the intermediate layer and excellent chipping resistance because RSA1 is 25 area % or more. On the other hand, the coated cutting tool of this embodiment has excellent wear resistance because RSA1 is less than 70 area %. From the same viewpoint, RSA1 is more preferably 27 area % or more and 61 area % or less, and further preferably 30 area % or more and 48 area % or less. Furthermore, the coated cutting tool of this embodiment has excellent wear resistance because RSA2 is 25 area % or more. On the other hand, the coated cutting tool of this embodiment has easy manufacturing because RSA2 is less than 70 area %. From the same viewpoint, RSA2 is more preferably 26 area % or more and 65 area % or less, and further preferably 28 area % or more and 53 area % or less.
[0034] In addition, in the coated cutting tool of this embodiment, the total of RSA1 and RSA2 is preferably 60 area % or more and 90 area % or less in the upper layer. When the total of RSA1 and RSA2 is 60 area % or more in the upper layer, the coated cutting tool of this embodiment tends to have excellent chipping resistance and wear resistance. On the other hand, when the total of RSA1 and RSA2 is 90 area % or less in the upper layer, the coated cutting tool of this embodiment is easy to manufacture. From the same viewpoint, the total of RSA1 and RSA2 is more preferably 62 area % or more and 90 area % or less, and further preferably 64 area % or more and 90 area % or less. In this embodiment, RSA1 and RSA2 can be determined by the method described in the Examples below.
[0035] The upper layer used in this embodiment includes one or more Ti compound layers made of a Ti compound of Ti and at least one element selected from the group consisting of C, N, and O. In addition, at least one of the Ti compound layers in the upper layer is a TiCN layer made of TiCN. At least one of the Ti compound layers in the upper layer is preferably a TiCN layer, since it improves wear resistance. Other Ti compound layers in the upper layer are not particularly limited, but include, for example, a TiC layer made of TiC, a TiN layer made of TiN, a TiCO layer made of TiCO, a TiCNO layer made of TiCNO, and a TiON layer made of TiON.
[0036] The upper layer may be composed of one layer or may be composed of multiple layers (for example, two or three layers). When the upper layer is composed of multiple layers, it is preferable to form an adhesion layer, which will be described later, as the layer on the side in contact with the intermediate layer, and another layer may be formed on the surface of the TiCN layer opposite to the substrate. When the upper layer is composed of two layers, the TiCN layer may be formed as the first layer, and a TiN layer may be formed as the second layer on the surface of the first layer. When the upper layer is composed of three layers, a TiCNO layer or a TiCO layer may be formed as the adhesion layer on the side in contact with the intermediate layer, a TiCN layer may be formed as the second layer on the surface of the adhesion layer, and a TiN layer may be formed as the third layer on the surface of the second layer.
[0037] The average thickness of the upper layer used in this embodiment is 1.00 μm or more and 6.50 μm or less. In the coated cutting tool of this embodiment, the average thickness of the upper layer is 1.00 μm or more, so that the wear resistance is improved. On the other hand, in the coated cutting tool of this embodiment, the average thickness of the upper layer is 6.50 μm or less, so that the adhesion between the upper layer and the intermediate layer is improved and the chipping resistance is excellent. From the same viewpoint, the average thickness of the upper layer is preferably 1.20 μm or more and 5.00 μm or less, and more preferably 1.55 μm or more and 4.80 μm or less.
[0038] The average thickness of the TiCN layer in the upper layer is preferably 1.00 μm or more and 6.50 μm or less. The coated cutting tool of this embodiment has a tendency to have improved wear resistance because the average thickness of the TiCN layer in the upper layer is 1.00 μm or more. In addition, the coated cutting tool of this embodiment has a tendency to have improved adhesion between the upper layer and the intermediate layer and excellent chipping resistance because the average thickness of the TiCN layer in the upper layer is 6.50 μm or less. From the same viewpoint, the average thickness of the TiCN layer in the upper layer is more preferably 1.50 μm or more and 5.00 μm or less, and even more preferably 2.00 μm or more and 4.80 μm or less.
[0039] When the upper layer used in this embodiment is in contact with the intermediate layer, the upper layer preferably includes at least one layer selected from the group consisting of a layer made of TiCO, a layer made of TiON, and a layer made of TiCNO as an adhesive layer (hereinafter, also simply referred to as "adhesive layer") on the side in contact with the intermediate layer. When the upper layer used in this embodiment is provided with such an adhesive layer, the adhesiveness with the intermediate layer tends to be improved, and the RSA1 can be easily controlled. From the same viewpoint, the adhesive layer is more preferably a TiCO layer or a TiCNO layer.
[0040] In the upper layer used in this embodiment, the average thickness of the adhesion layer is preferably 0.05 μm or more and 1.50 μm or less. In the coated cutting tool of this embodiment, when the average thickness of the adhesion layer is 0.05 μm or more, the adhesion between the upper layer and the intermediate layer is excellent, the chipping resistance tends to be improved, and RSA1 tends to be easily increased. On the other hand, in the coated cutting tool of this embodiment, when the average thickness of the adhesion layer is 1.50 μm or less, the decrease in RSA2 can be suppressed, so that the wear resistance tends to be improved. From the same viewpoint, the average thickness of the adhesion layer is more preferably 0.05 μm or more and 1.00 μm or less, and further preferably 0.05 μm or more and 0.30 μm or less.
[0041] The Ti compound layer in the upper layer is a Ti compound layer consisting of a Ti compound of Ti and at least one element selected from the group consisting of C, N, and O, but may contain trace amounts of components other than the above elements as long as the upper layer exerts its functional effects.
[0042] [Method of forming coating layer] The layers constituting the coating layer in the coated cutting tool of this embodiment can be formed, for example, by the following method, although the method for forming each layer is not limited thereto.
[0043] First, a lower layer consisting of one or more Ti compound layers is formed on the surface of the substrate. Next, the surface of the layer furthest from the substrate is oxidized. After that, a nucleus of an α-Al2O3 layer is formed on the surface of the layer furthest from the substrate, and with the nucleus formed, an α-Al2O3 layer is formed. Furthermore, an upper layer consisting of one or more Ti compound layers is formed on the surface of the α-Al2O3 layer.
[0044] The method for forming the Ti compound layer in the lower layer is not particularly limited, but the following method can be mentioned, for example. For example, a Ti compound layer consisting of a Ti nitride layer (hereinafter also referred to as a "TiN layer") can be formed by a chemical vapor deposition method using a raw material composition of TiCl4: 5.0 to 10.0 mol%, N2: 20 to 60 mol%, H2: balance, at a temperature of 850 to 950°C and a pressure of 350 to 450 hPa.
[0045] The Ti compound layer consisting of a Ti carbide layer (hereinafter also referred to as a "TiC layer") can be formed by a chemical vapor deposition method using a raw material composition of TiCl4: 1.5 to 3.5 mol%, CH4: 3.5 to 5.5 mol%, H2: balance, at a temperature of 950 to 1050°C and a pressure of 70 to 80 hPa.
[0046] The Ti compound layer consisting of a Ti carbonitride layer (hereinafter also referred to as a "TiCN layer") can be formed by a chemical vapor deposition method using a raw material composition of TiCl4: 5.0 to 7.0 mol%, CH3CN: 0.5 to 1.5 mol%, H2: balance, at a temperature of 800 to 900°C and a pressure of 70 to 90 hPa.
[0047] The Ti compound layer consisting of a Ti oxycarbonitride layer (hereinafter also referred to as the "TiCNO layer") in the lower layer can be formed by a chemical vapor deposition method with a raw material composition of TiCl4: 3.0-4.0 mol%, CO: 0.5-1.0 mol%, N2: 30-40 mol%, H2: balance, at a temperature of 950-1050°C and a pressure of 50-150 hPa.
[0048] The Ti compound layer consisting of a Ti carbonate layer (hereinafter also referred to as a "TiCO layer") can be formed by a chemical vapor deposition method using a raw material composition of TiCl4: 1.0 to 2.0 mol%, CO: 2.0 to 3.0 mol%, H2: balance, at a temperature of 950 to 1050°C and a pressure of 50 to 150 hPa.
[0049] Moreover, the intermediate layer made of an α-type Al2O3 layer (hereinafter, simply referred to as an "Al2O3 layer") is formed, for example, by the following method.
[0050] First, the surface of the lower layer that is the furthest from the substrate is oxidized under conditions of a raw material composition of CO2: 0.1-0.5 mol%, H2S: 0.05-0.15 mol%, H2: balance, a temperature of 900-950°C, and a pressure of 60-80 hPa (oxidation step). The oxidation treatment time at this time is preferably 1-3 minutes.
[0051] Thereafter, the nuclei of the α-type Al2O3 layer are formed by chemical vapor deposition at a temperature of 900-950°C and a pressure of 60-80hPa using a raw material composition of AlCl3: 1.0-4.0mol%, CO: 0.05-2.0mol%, CO2: 1.0-3.0mol%, HCl: 2.0-3.0mol%, and H2: balance (nucleation step). The preferred time for the nucleation step is 3-30 minutes.
[0052] The α-type Al2O3 layer is formed by chemical vapor deposition (CVD) at a temperature of 980-1020°C and a pressure of 60-80hPa using a raw material composition of AlCl3: 2.0-5.0mol%, CO2: 2.5-4.0mol%, HCl: 2.0-3.0mol%, H2S: 0.6-1.0mol%, and H2: balance (film formation process).
[0053] In order to set the texture coefficient TC(0,0,12) of the (0,0,12) plane of the α-Al2O3 layer expressed by formula (1) in the intermediate layer to the above-mentioned specific range, for example, the ratio of H2S in the gas composition in the film formation process or the average thickness of the intermediate layer may be controlled. More specifically, for example, by increasing the ratio of H2S in the gas composition in the film formation process or increasing the average thickness of the intermediate layer, the texture coefficient TC(0,0,12) of the (0,0,12) plane of the α-Al2O3 layer expressed by formula (1) tends to be increased.
[0054] Furthermore, the method for forming the Ti compound layer in the upper layer is not particularly limited, but may be, for example, the following method. First, when forming an adhesive layer on the side in contact with the intermediate layer (α-type Al2O3 layer), a Ti compound layer is formed on the surface of the α-type Al2O3 layer in the first step of forming the upper layer. Next, a TiCN layer is formed on the surface of the adhesive layer in the second step of forming the upper layer. Furthermore, a Ti compound layer may be formed on the surface of the TiCN layer.
[0055] In the first step of forming the upper layer, for example, when a TiCNO layer is formed on the surface of the α-Al2O3 layer, the upper layer can be formed by a chemical vapor deposition method with a raw material composition of TiCl4: 9.0-11.0 mol%, C2H4: 0.5-1.0 mol%, CH3CN: 1.5-2.0 mol%, CO: 2.0-8.0 mol%, N2: 15-25 mol%, H2: balance, at a temperature of 980-1020°C and a pressure of 80-100 hPa.
[0056] In the first step of forming the upper layer, for example, a TiCN layer is formed on the surface of the α-Al2O3 layer, and the composition of the raw materials is TiCl4: 10.0-12.0 mol%, C2H4: 0.5-1.5 mol%, CH3CN: 1.5-2.5 mol%, N2: 20-30 mol%, H2: balance, and the temperature is 980-1020°C and the pressure is 100-140 hPa by chemical vapor deposition. Here, the time for forming the TiCN layer is preferably 2-8 minutes.
[0057] In the first step of forming the upper layer, for example, when a TiCO layer is formed on the surface of the α-Al2O3 layer, the upper layer can be formed by a chemical vapor deposition method with a raw material composition of TiCl4: 8.0-10.0 mol%, C2H4: 0.3-0.7 mol%, CO: 4.0-10.0 mol%, H2: balance, at a temperature of 980-1020°C and a pressure of 60-80 hPa.
[0058] In the second step of forming the upper layer, when a TiCN layer is formed, the raw material composition is TiCl4: 9.0-11.0 mol%, CH4: 0.5-1.5 mol%, CH3CN: 1.5-2.5 mol%, N2: 15-25 mol%, H2: balance, and the layer can be formed by chemical vapor deposition at a temperature of 930-970°C and a pressure of 70-120 hPa.
[0059] Furthermore, when a TiN layer is formed on the surface of a TiCN layer, it can be formed by a chemical vapor deposition method with a raw material composition of TiCl4: 5.0 to 10.0 mol%, N2: 20 to 60 mol%, H2: balance, at a temperature of 950 to 1050°C and a pressure of 300 to 400 hPa.
[0060] In order to set RSA1 in the above-mentioned specific range in the upper layer, for example, the ratio of C2H4 or the ratio of CO in the gas composition in the first step of forming the upper layer may be controlled, or, if the upper layer includes an adhesive layer, the average thickness of the adhesive layer may be controlled. More specifically, for example, RSA1 tends to be increased by increasing the ratio of C2H4 or the ratio of CO in the gas composition in the first step of forming the upper layer. Also, for example, if the upper layer includes an adhesive layer, RSA1 tends to be increased by increasing the average thickness of the adhesive layer.
[0061] In order to set RSA2 in the upper layer within the above-mentioned specific range, for example, the ratio of CH4 or the ratio of CH3CN in the gas composition in the second step of forming the upper layer may be controlled. More specifically, RSA2 tends to be increased by increasing the ratio of CH4 or the ratio of CH3CN in the gas composition in the second step of forming the upper layer. Furthermore, if the first step of forming the upper layer is not performed, or if the various conditions in the first step of forming the upper layer are outside the above-mentioned ranges, performing the second step of forming the upper layer under the above-mentioned conditions tends to increase RSA2 and also tends to increase the proportion of those with an orientation difference A of 30 degrees or more and 45 degrees or less.
[0062] The thickness of each layer in the coating layer of the coated cutting tool of this embodiment can be measured by observing the cross-sectional structure of the coated cutting tool using an optical microscope, a scanning electron microscope (SEM), a FE-SEM, or the like. The average thickness of each layer in the coated cutting tool of this embodiment can be calculated as the arithmetic mean value of the thicknesses of each layer measured at three or more locations in the vicinity of a position 50 μm from the cutting edge toward the center of the rake face of the coated cutting tool. The composition of each layer can be measured from the cross-sectional structure of the coated cutting tool of this embodiment using an energy dispersive X-ray spectrometer (EDS), a wavelength dispersive X-ray spectrometer (WDS), or the like. EXAMPLES
[0063] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0064] A cutting insert made of cemented carbide having a CNMG120408 shape and a composition of 88.9% WC-7.9% Co-1.5 TiN-1.4% NbC-0.3% Cr3C2 (all mass%) was prepared as the substrate. After performing round honing on the cutting edge of this substrate with a SiC brush, the surface of the substrate was cleaned.
[0065] [Invention products 1-25 and comparison products 1-13] After cleaning the surface of the substrate, the coating layer was formed by chemical vapor deposition. First, a lower layer was formed on the surface of the substrate. Specifically, the substrate was loaded into an external heat type chemical vapor deposition apparatus, and under the conditions of the raw material composition, temperature and pressure shown in Table 1, an A layer having a composition shown in Table 6 was formed on the surface of the substrate to have an average thickness shown in Table 6. Next, under the conditions of the raw material composition, temperature and pressure shown in Table 1, a B layer having a composition shown in Table 6 was formed on the surface of the A layer to have an average thickness shown in Table 6. Next, for the invention products 1 to 22 and 25 and the comparative products 1 to 13, a C layer having a composition shown in Table 6 was further formed on the surface of the B layer to have an average thickness shown in Table 6 under the conditions of the raw material composition, temperature and pressure shown in Table 1. This formed a lower layer consisting of two or three layers. Then, under the conditions of the composition, temperature and pressure shown in Table 2, an oxidation treatment was performed on the surface of the lower layer for the time shown in Table 2. Next, under the conditions of the raw material composition, temperature and pressure shown in Table 2, α-type aluminum oxide (α-type Al2O3) cores were formed on the surface of the lower layer that had been subjected to oxidation treatment for the time shown in Table 2. Furthermore, under the conditions of the raw material composition, temperature and pressure shown in Table 3, an intermediate layer (α-type Al2O3 layer) with the composition shown in Table 6 was formed on the surface of the lower layer and the α-type aluminum oxide (α-type Al2O3) core to have the average thickness shown in Table 6. Next, an upper layer was formed on the surface of the intermediate layer (α-type Al2O3 layer). Specifically, first, as the first step of forming the upper layer, for the invention products 1 to 7 and 12 to 25 and the comparative products 1 to 5, 7 to 10, 12 and 13, an X layer (adhesion layer) with the composition shown in Table 7 was formed on the surface of the α-type Al2O3 layer to have the average thickness shown in Table 7 under the conditions of the raw material composition, temperature and pressure shown in Table 4. For the invention products 8 to 11 and the comparative product 6, the first step of forming the upper layer was carried out for 5 minutes under the conditions of the raw material composition, temperature and pressure shown in Table 4, and a part (average thickness: about 0.05 μm) of the Y layer (TiCN layer) whose composition is shown in Table 7 was formed on the surface of the intermediate layer (α-type Al2O3 layer). Next, as the second step of forming the upper layer, the Y layer whose composition is shown in Table 7 was formed on the surface of the X layer or the surface of the intermediate layer (α-type Al2O3 layer) under the conditions of the raw material composition, temperature and pressure shown in Table 5, so as to have the average thickness shown in Table 7.For invention products 8-11 and comparative product 6, a Y layer (TiCN layer) with the composition shown in Table 7 was formed on the surface of the intermediate layer (α-type Al2O3 layer) so that the combined average thickness of the first and second steps for forming the upper layer was shown in Table 7. Furthermore, for invention products 1-7, 9, 10, 12, 14, and 16-25 and comparative products 1-3, and 6-13, a Z layer with the composition shown in Table 7 was formed on the surface of the Y layer with the average thickness shown in Table 7 under the conditions of the raw material composition, temperature, and pressure shown in Table 1. In this way, the coated cutting tools of invention products 1-25 and comparative products 1-13 were obtained.
[0066] The thickness of each layer of the sample was determined as follows. That is, using FE-SEM, the thickness was measured at three locations on the cross section in the vicinity of a position 50 μm from the cutting edge of the coated cutting tool toward the center of the rake face, and the arithmetic mean value was determined as the average thickness. The composition of each layer of the obtained sample was measured using EDS in the cross section in the vicinity of a position 50 μm from the cutting edge of the coated cutting tool toward the center of the rake face.
[0067] [Table 1]
[0068] [Table 2]
[0069] [Table 3]
[0070] [Table 4]
[0071] [Table 5]
[0072] [Table 6]
[0073] [Table 7]
[0074] [RSA1 and RSA2] In the obtained sample, the cross section of the upper layer was exposed in a direction perpendicular to the surface of the substrate. The obtained cross section was mirror-polished, and the mirror-polished surface was observed with a field emission scanning electron microscope (FE-SEM). Using an electron backscattering diffraction (EBSD) device attached to the FE-SEM, the misorientation A between the normal to the (220) plane of each particle having a cubic crystal structure and the normal to the substrate surface was measured. The sum of the cross-sectional areas of the analyzed upper layers in the region where the misorientation A was 0 degrees or more and less than 10 degrees (the sum of the cross-sectional areas of the particles in the upper layer where the misorientation A is in the range of 0 degrees or more and 45 degrees or less: RSA) was calculated. Total ) to 100% area, was defined as RSA1 (unit: area%). The ratio of the cross-sectional area of the region where the misorientation A is 20 degrees or more and less than 30 degrees to the total cross-sectional area of the analyzed upper layer, 100% area, was defined as RSA2 (unit: area%). Specifically, the cross-sectional area of the particles in the range of misorientation A of 0 degrees or more and less than 45 degrees was divided into sections at intervals of 5 degrees, and the area of the particle cross section for each section was calculated. Next, the total area of the particle cross section in each section where the misorientation A is 0 degrees or more and less than 10 degrees, 10 degrees or more and less than 20 degrees, 20 degrees or more and less than 30 degrees, and 30 degrees or more and less than 45 degrees was calculated. The total area of the particle cross section in each of these sections where the misorientation A is 0 degrees or more and less than 45 degrees was calculated. Total The ratio of the cross-sectional area of the grains with misorientation A between 20 degrees and 30 degrees is RSA1. TotalThe ratio of the RSA2 to the RSA1 was defined as RSA2. The above measurement results are shown in Table 8 below. The EBSD measurements were performed as follows. The sample was set in the FE-SEM. The sample was irradiated with an electron beam at an incident angle of 70 degrees, an acceleration voltage of 15 kV, and an irradiation current of 1.0 nA. The orientation error and cross-sectional area of each particle were measured with an EBSD setting of a measurement range of 10 μm × 50 μm and a step size of 0.1 μm. The area of the particle cross-section of the upper layer within the measurement range was the sum of the pixels corresponding to that area. In other words, the total area of the particle cross-sections in each section of the particles in each layer at a pitch of 10 degrees or 15 degrees based on the orientation error A was calculated by tallying up the pixels occupied by the particle cross-sections corresponding to each section and converting them into areas.
[0075] [Table 8]
[0076] [Texture coefficient TC(0,0,12) of the (0,0,12) plane of the α-type Al2O3 layer] The obtained sample was subjected to X-ray diffraction measurement of the 2θ / θ focusing optical system using Cu-Kα radiation under the following conditions: output: 45 kV, 200 mA, incident side Soller slit: 5°, divergence vertical slit: 2 / 3°, divergence vertical limiting slit: 5 mm, scattering slit: 8 mm, light receiving side Soller slit: 5°, light receiving slit: 10 mm, detector: D / tex ultra, scan mode: continuous, sampling width: 0.01°, scan speed: 12° / min, 2θ measurement range: 25° to 140°. The apparatus used was an X-ray diffraction apparatus (model "SmartLab") manufactured by Rigaku Corporation. The peak intensity of each crystal plane of the α-type Al2O3 layer in the intermediate layer was obtained from the X-ray diffraction pattern. The texture coefficient TC(0,0,12) of the (0,0,12) plane of the α-type Al2O3 layer, expressed by the following formula (1), was obtained from the peak intensity of each obtained crystal plane. The results are shown in Table 9.
number
[0077] [Table 9]
[0078] Using the obtained invention products 1 to 25 and comparison products 1 to 13, cutting test 1 and cutting test 2 were performed under the following conditions. Cutting test 1 is a chipping test to evaluate chipping resistance, and cutting test 2 is a wear test to evaluate wear resistance. The results of each cutting test are shown in Table 10.
[0079] [Cutting test 1] Work material: SCM415, Workpiece shape: Round bar with two equally spaced grooves on the outer surface. Cutting speed: 200m / min, Cutting depth: 1.5mm, Feed: 0.3mm / rev, Coolant: Water-soluble coolant, Evaluation item: After starting cutting, the cutting was stopped every 500 impacts and the cutting edge of the cutting tool was observed under a stereo microscope (100x magnification). The same procedure was repeated until chipping was confirmed on the cutting edge. The cumulative number of impacts up to the point where chipping occurred was regarded as the tool life.
[0080] [Cutting test 2] Work material: S45C, Workpiece shape: round bar, Cutting speed: 250m / min, Cutting depth: 2.0mm, Feed: 0.3mm / rev, Coolant: Water-soluble coolant, Evaluation item: The machining time until the flank wear width of the cutting tool exceeded 0.3 mm was defined as the tool life, and the machining time until the tool life was measured.
[0081] The cumulative impact counts until the tool life in cutting test 1 (chipping test) were evaluated as "A" for 12,000 or more, "B" for 8,000 or more and less than 12,000, and "C" for less than 8,000. In addition, the processing time until the tool life in cutting test 2 (wear test) was evaluated as "A" for 35 minutes or more, "B" for 25 minutes or more and less than 35 minutes, and "C" for less than 25 minutes. In this evaluation, "A" means the best, followed by "B" and "C" means the worst, and the more A or B there are, the better the cutting performance. The evaluation results obtained are shown in Table 10.
[0082] [Table 10]
[0083] From the results shown in Table 10, the chipping test and abrasion test of the inventive product were both rated "A" or "B". On the other hand, the comparative product was rated "C" in both or either the chipping test and the abrasion test. Therefore, it can be seen that the chipping resistance and abrasion resistance of the inventive product are generally superior to those of the comparative product.
[0084] From the above results, it is clear that the inventive product has excellent chipping resistance and wear resistance, resulting in a long tool life. [Industrial Applicability]
[0085] INDUSTRIAL APPLICABILITY The coated cutting tool of the present invention has excellent chipping resistance and wear resistance, and therefore can extend the tool life as compared with conventional ones. From this viewpoint, the coated cutting tool has industrial applicability. [Explanation of symbols]
[0086] 1...substrate, 2...lower layer, 3...middle layer, 4...upper layer, 5...coating layer, 6...coated cutting tool.
Claims
1. A coated cutting tool comprising a substrate and a coating layer formed on a surface of the substrate, The coating layer includes a lower layer, an intermediate layer, and an upper layer in this order from the substrate side toward the surface side of the coating layer, the lower layer includes one or more Ti compound layers each comprising a Ti compound of Ti and at least one element selected from the group consisting of C, N, O, and B; The intermediate layer is made of α-type Al 2 O 3 α-type Al consisting of 2 O 3 layer, the upper layer includes one or more Ti compound layers each composed of a Ti compound of Ti and at least one element selected from the group consisting of C, N, and O, and at least one of the Ti compound layers in the upper layer is a TiCN layer; The average thickness of the upper layer is 1.00 μm or more and 6.50 μm or less, A coated cutting tool, wherein the upper layer satisfies the conditions represented by the following formulas (i) and (ii): 25≦RSA1<70 (i) (In formula (i), RSA1 is the ratio (unit: area %) of the cross-sectional area of a region in a cross-section of the upper layer perpendicular to the surface of the base material, in which the misorientation A, which is the angle (unit: degree) between the normal to the (220) plane of each particle having a cubic crystal structure and the normal to the surface of the base material, is 0 degrees or more and less than 10 degrees, when the total area of the entire cross-section is taken as 100 area %).) 25≦RSA2<70 (ii) (In formula (ii), RSA2 is the ratio (unit: area %) of the cross-sectional area of a region in a cross-section of the upper layer perpendicular to the surface of the base material, in which the misorientation A, which is the angle (unit: degree) between the normal to the (220) plane of each particle having a cubic crystal structure and the normal to the surface of the base material, is 20 degrees or more and less than 30 degrees, when the total area of the entire cross-section is taken as 100 area %).)
2. The coated cutting tool according to claim 1 , wherein in the upper layer, the sum of RSA1 and RSA2 is 60 area % or more and 90 area % or less.
3. 3. The coated cutting tool according to claim 1, wherein the upper layer is in contact with the intermediate layer, and the upper layer includes at least one layer selected from the group consisting of a layer of TiCO, a layer of TiON, and a layer of TiCNO as an adhesion layer on a side in contact with the intermediate layer, and the average thickness of the adhesion layer is 0.05 μm or more and 1.50 μm or less.
4. In the intermediate layer, α-type Al represented by the following formula (1) 2 O 3 3. The coated cutting tool according to claim 1, wherein a texture coefficient TC(0,0,12) of a (0,0,12) plane of the layer is 5.9 or more and 8.9 or less. [0010] (In formula (1), I(h, k, l) is α-type Al 2 O 3 is the peak intensity by X-ray diffraction measured on the (h, k, l) plane of the layer, and I 0 (h, k, l) are α-type Al according to JCPDS card number 10-0173 2 O 3 The standard diffraction intensities of the (h, k, l) planes of the crystal are (0, 1, 2), (1, 0, 4), (1, 1, 3), (0, 2, 4), (1, 1, 6), (2, 1, 4), (3, 0, 0), (0, 2, 10), and (0, 0, 12).
5. The coated cutting tool according to claim 1 or 2, wherein the intermediate layer has an average thickness of 3.00 μm or more and 15.00 μm or less.
6. The coated cutting tool according to claim 1 or 2, wherein the lower layer has an average thickness of 3.00 μm or more and 15.00 μm or less.
7. 3. The coated cutting tool according to claim 1, wherein the coating layer has an average thickness of 10.00 μm or more and 30.00 μm or less.
Citation Information
Patent Citations
Coated cutting tool
JP2019098430A
Coated cutting tool
JP2020116645A
Coated cutting tool
JP2020116646A
Coated cutting tool
JP2020185642A
Coated hard alloy
WO2000079022A1