Catalyst for purifying exhaust gas containing sulfur compounds and method for purifying exhaust gas containing sulfur compounds
A catalyst with a γ-alumina carrier layer and platinum-palladium support addresses the issue of heat and sulfur poisoning resistance, ensuring effective purification of sulfur compounds in exhaust gas.
Patent Information
- Application Number
- JP2021005850
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-18
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2041-01-18
AI Technical Summary
Existing catalysts for purifying exhaust gas containing sulfur compounds lack sufficient heat resistance and resistance to sulfur poisoning, leading to performance deterioration at high temperatures.
A catalyst comprising a base material with a carrier layer of γ-alumina supporting platinum and palladium, with specific ratios and particle sizes, and a BET specific surface area of 150 m²/g or more, designed to maintain catalytic activity and resistance to sulfur poisoning.
The catalyst provides effective purification of sulfur compound-containing exhaust gas, maintaining high catalytic activity and resistance to sulfur poisoning even at high temperatures.
Smart Images

Figure 0007583441000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a catalyst for purifying an exhaust gas containing sulfur compounds and a method for purifying an exhaust gas containing sulfur compounds. [Background technology]
[0002] Gases emitted from petrochemical plants and the like contain flammable and harmful odorous components. In order to treat such exhaust gases, the components are oxidized and decomposed using a catalyst. Since the oxidative decomposition using a catalyst is an exothermic reaction, the catalyst is required to have heat resistance. In addition, the exhaust gas may contain sulfur compounds that act as catalyst poisons. Since sulfur compounds reduce the catalyst's lifespan, the catalyst is also required to have resistance to sulfur poisoning. Patent Document 1 discloses a catalyst for purifying exhaust gases containing sulfur compounds, characterized in that a platinum group element is supported on a titanium dioxide-alumina mixed molded support. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Publication No. 55-064839 Summary of the Invention [Problem to be solved by the invention]
[0004] Although the invention described in Patent Document 1 is said to be resistant to sulfur compounds, there is a risk that the performance may decrease at high temperatures.
[0005] The present disclosure has been made in view of the above circumstances, and aims to provide a catalyst for purifying exhaust gas containing sulfur compounds, which has heat resistance and resistance to sulfur poisoning, and a method for purifying exhaust gas containing sulfur compounds using the catalyst. [Means for solving the problem]
[0006] The present disclosure provides a catalyst for purifying exhaust gas containing sulfur compounds, comprising a substrate, a support layer containing γ-alumina supported on the substrate, and precious metals containing platinum and palladium supported on the support layer, wherein the amount of γ-alumina supported is 22 g / L or more per unit volume of the substrate, the amount of palladium supported is 0.55 g / L or more per unit volume of the substrate, and the mass ratio of the amount of platinum supported to the amount of palladium supported (Pt / Pd) is 0.55 to 4.0.
[0007] In the present disclosure, the BET specific surface area of the support layer is 150 m 2 / g or more.
[0008] In the present disclosure, the catalyst may be substantially free of chlorine atoms.
[0009] In the present disclosure, the average particle size of platinum may be smaller than the average particle size of palladium.
[0010] In the present disclosure, the average particle size of platinum may be 6 nm or less, and the average particle size of palladium may be 15 nm or less.
[0011] The present disclosure provides a method for purifying an exhaust gas containing sulfur compounds, comprising a step of contacting the above catalyst with an exhaust gas containing sulfur compounds.
[0012] In the present disclosure, the above step may be a step of oxidizing hydrocarbons contained in exhaust gas.
[0013] In the present disclosure, the hydrocarbon may include propane. Effect of the Invention
[0014] According to the present disclosure, it is possible to provide a catalyst for purifying exhaust gas containing sulfur compounds, which has heat resistance and resistance to sulfur poisoning. Also, according to the present disclosure, it is possible to provide a method for purifying exhaust gas containing sulfur compounds using the catalyst. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Preferred embodiments of the present disclosure will be described in detail below, but the present disclosure is not limited to the following embodiments.
[0016] <Sulfur compound-containing exhaust gas purification catalyst> The catalyst for purifying exhaust gas containing sulfur compounds (hereinafter, sometimes simply referred to as "catalyst") includes a substrate, a carrier layer containing γ-alumina supported on the substrate, and a precious metal containing platinum and palladium supported on the carrier layer. The precious metal may be precious metal particles.
[0017] (base material) The shape of the substrate is not particularly limited, but may be a shape that generates a small differential pressure during gas flow and has a large contact area with the gas. Examples of the shape of the substrate include honeycomb, sphere, sheet, mesh, foam, fiber, pipe, filter, etc. Examples of the material of the substrate are not particularly limited, but include known catalyst carriers such as cordierite and alumina, carbon fiber, metal fiber, glass fiber, ceramic fiber, and metals such as titanium, aluminum, and stainless steel. In the case of a substrate having pores such as a honeycomb or foam, the volume of the substrate is the total volume including the pores, and is the volume of the portion surrounded by the outer periphery. For example, in the case of a honeycomb or foam having a rectangular parallelepiped shape, the volume of the substrate can be calculated from the lengths of the three sides of the rectangular parallelepiped (length x width x height).
[0018] (Carrier layer) Unlike titania, γ-alumina is less likely to experience a decrease in specific surface area at high temperatures. Therefore, by using a carrier layer containing γ-alumina, a catalyst with excellent heat resistance and activity that is less likely to decrease even at high temperatures can be obtained. From this perspective, the amount of γ-alumina supported is 22 g / L or more per unit volume of the substrate, may be 30 g / L or more, or may be 40 g / L or more. The upper limit of the amount of γ-alumina supported is not particularly limited from the viewpoint of activity, but since an excessively large amount of support may reduce production efficiency in production, it may be set to 200 g / L.
[0019] From the viewpoints of heat resistance and maintaining activity at high temperatures, the content of γ-alumina in the support layer may be 25 mass% or more, 30 mass% or more, or may be 100 mass% (the support layer is substantially composed of γ-alumina).
[0020] The carrier layer may contain other components other than γ-alumina. Examples of other components include various inorganic oxides intended to reinforce the properties of γ-alumina or to impart properties not found in γ-alumina to the carrier layer. For example, from the viewpoint of further improving heat resistance, oxides of rare earth elements such as lanthanum and yttrium, oxides of alkaline earth metal elements such as calcium and barium, and oxides of other transition metal elements may be blended into the carrier layer. In addition, from the viewpoint of imparting oxygen storage performance, oxides of cerium may be blended into the carrier layer. In addition, oxides of zirconium, silicon, iron, copper, and the like, which are generally used as carriers, or composite oxides thereof may be blended into the carrier layer. In addition, examples of other components include binder components used to coat the carrier layer on the substrate, such as colloidal silica, silica sol, alumina sol, silicic acid sol, titania sol, boehmite, clay, kaolin, and sepiolite. The binder components listed here are inorganic binders, and the heat resistance of the carrier layer is easily maintained.
[0021] The specific surface area of the support layer measured by the BET method (BET specific surface area) is set to 150 m from the viewpoint of increasing the catalytic activity. 2 / g or more, 2 / g or more.
[0022] The average pore size of the support layer (on the adsorption side by the BJH method) may be 5 to 40 nm or 6 to 20 nm from the viewpoint of further enhancing the catalytic activity. From the same viewpoint, the volume of pores in the range of 1.7 to 300 nm in the support layer is 0.1 to 2.0 cm 3 / g, and 0.5 to 1.0 cm 3 The average pore diameter and pore volume can be determined by a nitrogen adsorption method.
[0023] (Precious metals) The carrier layer supports both platinum and palladium as precious metals, resulting in a catalyst with high activity. The mass ratio (Pt / Pd) of the amount of platinum supported to the amount of palladium supported is 0.55 to 4.0, and may be 0.6 to 3.5. When Pt / Pd is 0.55 or more, sufficient sulfur poisoning resistance can be maintained before (fresh state) and when exposed to high temperatures (650°C or higher). When Pt / Pd is 4.0 or less, excellent heat resistance is obtained, so sufficient catalytic activity can be maintained when exposed to high temperatures.
[0024] The amount of palladium supported is 0.55 g / L or more per unit volume of the substrate, and may be 0.6 g / L or more. This provides excellent heat resistance and allows sufficient catalytic activity to be maintained when exposed to high temperatures. The amount of platinum supported may be adjusted so that the above ratio Pt / Pd is satisfied.
[0025] The upper limit of the supported amount of platinum and palladium is not particularly limited from the viewpoint of catalytic performance, but can be set to 10 g / L from the viewpoint of suppressing the amount of precious metal used.
[0026] The catalyst may contain precious metals other than platinum and palladium (e.g., gold, silver, copper, rhodium, ruthenium, etc.) within the range in which the catalytic activity is appropriately maintained. The total amount of platinum and palladium contained in the precious metals may be 90 mass% or more, or may be 100 mass% (the precious metals substantially contain only platinum and palladium).
[0027] The amounts of platinum and palladium supported can be determined by dissolving the catalyst in aqua regia and then performing ICP analysis.
[0028] The average particle size of platinum may be smaller than that of palladium. This allows both catalytic activity and sulfur poisoning resistance to be achieved at a higher level. From this viewpoint, the average particle size of platinum may be 6 nm or less, or 4 nm or less, and the average particle size of palladium may be 15 nm or less, or 10 nm or less. The lower limit of the average particle size of both particles is not particularly limited, but can be 0.5 nm or more from the viewpoint of manufacturing technology. The average particle size can be confirmed by a scanning electron microscope (SEM), a transmission electron microscope (TEM), a scanning transmission electron microscope (STEM), or the like. Here, the particle size refers to the diameter of the smallest circumscribing circle of the particle in the obtained image. The average particle size can be obtained by averaging the diameters of 20 particles obtained in this manner.
[0029] The catalyst preferably does not substantially contain chlorine atoms. The catalyst preferably does not contain chlorine atoms other than chlorine atoms that may be contained due to inevitable impurities. The catalyst does not contain chlorine atoms, so that the catalytic activity is further increased. In order to make the catalyst substantially free of chlorine atoms, it is possible to not use a precursor containing chlorine atoms when forming a support layer, or not use a precursor containing chlorine atoms when supporting a precious metal.
[0030] <Method of manufacturing a catalyst for purifying exhaust gas containing sulfur compounds> The method for producing the catalyst for purifying exhaust gas containing sulfur compounds is not particularly limited, but the following method can be mentioned, for example.
[0031] A slurry containing γ-alumina or boehmite, which is a precursor of γ-alumina, is prepared. The slurry may contain other components as exemplified above.
[0032] The prepared slurry is coated on a substrate and dried. The coating method is not particularly limited, and known methods such as wash coating and dipping can be used. When boehmite is used, the boehmite is converted to γ-alumina by baking at 400 to 700°C after drying. The thickness of the carrier layer and the amount of γ-alumina supported can be adjusted by adjusting the solid concentration in the slurry or by repeating the coating-drying process. As a result, a carrier layer containing γ-alumina is formed on the substrate.
[0033] Next, the precious metal is supported on the carrier layer by the impregnation method. In the impregnation method, the carrier layer is impregnated with a precious metal precursor solution. The platinum precursor is not particularly limited, and a commonly used platinum salt can be used. Examples of platinum salts include dinitrodiamine platinum, chloroplatinic acid, and tetraammine platinum. From the viewpoint of further increasing activity, a platinum salt that does not contain a chlorine atom is preferable. The palladium precursor is not particularly limited, and a commonly used palladium salt can be used. Examples of palladium salts include palladium nitrate, palladium chloride, and tetraammine palladium. From the viewpoint of further increasing activity, a palladium salt that does not contain a chlorine atom is preferable.
[0034] After impregnation with the precious metal precursor solution, the support layer is dried at 80° C. to 200° C. After drying the support layer, the whole is fired at 250° C. to 600° C. In this manner, a catalyst is obtained that includes a substrate, a support layer containing γ-alumina supported on the substrate, and precious metals containing platinum and palladium supported on the support layer.
[0035] <Method for purifying exhaust gas containing sulfur compounds> The method for purifying an exhaust gas containing sulfur compounds includes a step of contacting the catalyst with an exhaust gas containing sulfur compounds. The step decomposes the substances to be treated in the exhaust gas. For example, the step may be a step of oxidizing hydrocarbons contained in the exhaust gas. The catalyst is effective for hydrocarbons containing propane. By using the catalyst, the decomposition activity can be maintained for a long period of time even if the exhaust gas contains sulfur compounds or even if high temperatures are generated by the catalytic decomposition of the substances to be treated.
[0036] Examples of sulfur compounds include sulfur dioxide, sulfur trioxide, hydrogen sulfide, methyl mercaptan, dimethyl sulfide, and dimethyl disulfide. The catalyst can effectively exhibit catalytic activity even when the concentration of sulfur compounds contained in exhaust gas is 0.1 ppm by volume or more. The upper limit of the concentration of sulfur compounds can be set to 50 ppm by volume or less from the viewpoint of effectively exhibiting catalytic activity.
[0037] The space velocity (SV) of the exhaust gas to be treated against the catalyst is determined appropriately taking into consideration the characteristics of the exhaust gas and the target decomposition rate, etc., but is generally in the range of 100 to 100,000 h -1 The temperature of the decomposition reaction is appropriately determined depending on the properties of the exhaust gas (water vapor concentration and ammonia concentration), the reaction conditions (space velocity, etc.), the degree of catalyst deterioration, etc., and may be 200 to 500°C, or 250 to 450°C. EXAMPLES
[0038] The present disclosure will be described in more detail with reference to the following examples, but the present disclosure is not limited to these examples.
[0039] <Catalyst Preparation> Example 1 A slurry was prepared by mixing 100 g of γ-alumina powder (manufactured by JGC-Universal Co., Ltd.) and 25 g of boehmite (manufactured by UOP Co., Ltd.) as a binder with 350 g of an acidic aqueous solution of nitric acid. This slurry was applied to a cordierite honeycomb substrate (manufactured by Nippon Insulators Co., Ltd., 200 cells / square inch) by a wash coat method so that the weight of the carrier layer per liter of honeycomb (weight after the carrier layer was formed) was 40 g, and excess slurry was blown off with compressed air. Thereafter, the honeycomb substrate coated with the slurry was dried in a dryer at 150° C. for 3 hours and further fired in air at 500° C. for 2 hours, thereby forming a γ-alumina (γ-Al 2 O 3 The BET specific surface area of the support layer was 223 m 2 / g, the average pore diameter (on the adsorption side of the BJH method) was 10.9 nm, and the pore volume in the range of 1.7 to 300 nm was 0.70 cm 3 / g.
[0040] Then, a mixed solution (impregnation liquid) of dinitrodiamine platinum aqueous solution (Tanaka Kikinzoku Kogyo Co., Ltd.) and palladium nitrate (Tanaka Kikinzoku Kogyo Co., Ltd.) was prepared. The mixed amount was adjusted so that the amount of platinum supported was 1.0 g / L and the amount of palladium supported was 1.5 g / L. The honeycomb substrate with the carrier layer obtained above was impregnated with this impregnation liquid. This was dried at 150°C for 3 hours, and then heated at 500°C for 1 hour in an air atmosphere. As a result, a honeycomb-type catalyst was obtained in which 1.0 g / L of platinum and 1.5 g / L of palladium were supported on the γ-alumina carrier layer. The average particle diameter of platinum was 1.0 nm, and the average particle diameter of palladium was 5.1 nm.
[0041] Example 2 A catalyst was obtained in the same manner as in Example 1, except that the composition of the impregnation solution was changed so that the amount of supported platinum was 1.5 g / L and the amount of supported palladium was 1.5 g / L. The average particle size of platinum was 1.2 nm, and the average particle size of palladium was 5.0 nm.
[0042] Example 3 A catalyst was obtained in the same manner as in Example 1, except that the composition of the impregnation solution was changed so that the amount of supported platinum was 2.0 g / L and the amount of supported palladium was 1.5 g / L. The average particle size of platinum was 1.2 nm, and the average particle size of palladium was 5.1 nm.
[0043] Example 4 A catalyst was obtained in the same manner as in Example 1, except that the composition of the impregnation solution was changed so that the amount of supported platinum was 3.0 g / L and the amount of supported palladium was 1.5 g / L. The average particle size of platinum was 1.7 nm, and the average particle size of palladium was 5.1 nm.
[0044] Example 5 A catalyst was obtained in the same manner as in Example 1, except that the composition of the impregnation solution was changed so that the amount of supported platinum was 1.0 g / L and the amount of supported palladium was 0.75 g / L. The average particle size of platinum was 1.1 nm, and the average particle size of palladium was 4.7 nm.
[0045] Example 6 A catalyst was obtained in the same manner as in Example 1, except that the composition of the impregnation solution was changed so that the amount of supported platinum was 2.0 g / L and the amount of supported palladium was 0.75 g / L. The average particle size of platinum was 1.5 nm, and the average particle size of palladium was 4.6 nm.
[0046] Example 7 A catalyst was obtained in the same manner as in Example 1, except that the composition of the impregnation solution was changed so that the amount of supported platinum was 1.0 g / L and the amount of supported palladium was 0.6 g / L. The average particle size of platinum was 1.0 nm, and the average particle size of palladium was 4.5 nm.
[0047] Example 8 A catalyst was obtained in the same manner as in Example 1, except that the composition of the impregnation solution was changed so that the amount of supported platinum was 2.0 g / L and the amount of supported palladium was 0.6 g / L. The average particle size of platinum was 1.2 nm, and the average particle size of palladium was 4.5 nm.
[0048] Example 9 A catalyst was obtained in the same manner as in Example 3, except that the amount of the γ-alumina support layer was changed to 80 g / L.
[0049] Example 10 A slurry was prepared by mixing 38 g of γ-alumina powder (manufactured by JGC Universal Co., Ltd.), 50 g of zirconium oxide powder (manufactured by Daiichi Kigenso Kagaku Kogyo Co., Ltd., RC-100), and 49 g of boehmite (manufactured by UOP Co., Ltd.) as a binder with 350 g of nitric acid acidic aqueous solution. This slurry was applied to a cordierite honeycomb substrate (manufactured by Nippon Gaishi Co., Ltd., 200 cells / square inch) by wash coating so that the weight of the carrier layer per liter of honeycomb (weight after the carrier layer was formed) was 80 g, and excess slurry was blown off with compressed air. Thereafter, the honeycomb substrate coated with the slurry was dried in a dryer at 150° C. for 3 hours, and further fired in air at 500° C. for 2 hours, thereby supporting a carrier layer containing γ-alumina (60% by mass) and zirconium oxide (40% by mass) on the cordierite honeycomb substrate. The BET specific surface area of the carrier layer was 199 m 2 / g, the average pore diameter is 8.2 nm, and the pore volume in the range of 1.7–300 nm is 0.62 cm 3 Thereafter, platinum and palladium were supported on the carrier layer in the same manner as in Example 3 to obtain a catalyst.
[0050] Example 11 A slurry was prepared by mixing 89 g of zirconium oxide powder (RC-100, manufactured by Daiichi Kigenso Kagaku Kogyo Co., Ltd.) and 49 g of boehmite (manufactured by UOP Co., Ltd.) as a binder with 350 g of an acidic aqueous solution of nitric acid. Except for this, a carrier layer containing γ-alumina (30 mass%) and zirconium oxide (70 mass%) was supported on a cordierite honeycomb substrate in the same manner as in Example 10. The BET specific surface area of the carrier layer was 224 m 2 / g, the average pore diameter is 6.2 nm, and the pore volume in the range of 1.7–300 nm is 0.55 cm 3 Thereafter, platinum and palladium were supported on the carrier layer in the same manner as in Example 3 to obtain a catalyst.
[0051] Comparative Example 1 A slurry was prepared by mixing 100 g of titanium oxide powder (manufactured by Ishihara Sangyo Kaisha, Ltd.) and 25 g (solid content) of colloidal silica (manufactured by Nissan Chemical Industries, Ltd., Snowtex OUP) as a binder with 350 g of nitric acid acidic aqueous solution. This slurry was applied to a cordierite honeycomb substrate (manufactured by Nippon Gaishi Co., Ltd., 200 cells / square inch) by washcoat method so that the weight of the carrier layer per liter of honeycomb (weight after carrier layer formation) was 40 g, and excess slurry was blown off with compressed air. Thereafter, the honeycomb substrate coated with the slurry was dried in a dryer at 150° C. for 3 hours, and further calcined in air at 500° C. for 2 hours, thereby supporting a carrier layer containing titania (80% by mass) and silica (20% by mass, binder) on the cordierite honeycomb substrate. Thereafter, platinum and palladium were supported on the carrier layer in the same manner as in Example 3 to obtain a catalyst.
[0052] Comparative Example 2 A catalyst was obtained in the same manner as in Example 1, except that the composition of the impregnation solution was changed so that the amount of supported platinum was 1.0 g / L and the amount of supported palladium was 2.0 g / L. The average particle size of platinum was 1.1 nm, and the average particle size of palladium was 5.3 nm.
[0053] Comparative Example 3 A catalyst was obtained in the same manner as in Example 3, except that the amount of the γ-alumina support layer was changed to 20 g / L.
[0054] As described above, in each example, a precursor containing chlorine atoms was not used to form the support layer, and a precursor containing chlorine atoms was not used to support the precious metal. It can be said that the catalyst obtained in each example does not substantially contain chlorine atoms.
[0055] <Various evaluations> (Method for evaluating propane cracking activity) A cylindrical honeycomb catalyst (diameter 21 mm, length 50 mm) was collected from the honeycomb catalyst obtained in each example, and this was packed into a flow-type reactor. The flow rate was controlled by a mass flow controller to allow a predetermined amount of gas to flow through the catalyst. The catalyst was heated in an electric furnace, and the temperature at the catalyst inlet (inlet temperature) was set to a predetermined temperature, and the propane decomposition activity (decomposition rate) was evaluated. For each example, two types of catalyst were used for the evaluation: an untreated product (the catalyst as prepared) and a heat-treated product (catalyst that had been heat-treated at 650°C for 50 hours). The gas conditions were as follows: Gas Conditions: SV=30000h -1 , catalyst temperature (inlet temperature) = 400°C, propane concentration 200 ppm by volume, SO 2 = 10 ppm by volume, moisture = 20% by volume, oxygen = 4% by volume, nitrogen balance.
[0056] The propane gas concentration at the catalyst outlet side was analyzed by gas chromatography (GC4000, manufactured by GL Sciences Inc.), and the propane decomposition rate was calculated.
[0057] The evaluation results are shown in Table 1. The catalysts of the examples met the following pass criteria. Passing criteria: Fresh: Initial activity is 80% or more and SO 2 Activity was over 80% after 120 hours of poisoning. Heat-treated product: initial activity is 30% or more and SO 2 Activity is over 50% after 120 hours of poisoning.
[0058] [Table 1] [Industrial Applicability]
[0059] The catalyst of the present disclosure can suitably purify exhaust gas containing sulfur compounds. The catalyst of the present disclosure is suitable for purifying industrial exhaust gas containing sulfur compounds, and is particularly suitable for purifying exhaust gas containing propane discharged from an acrylic acid manufacturing plant or the like.
Claims
1. A catalyst catalyst comprising: a substrate; a carrier layer including γ-alumina supported on the substrate; and a precious metal including platinum and palladium supported on the carrier layer; The amount of the γ-alumina supported per unit volume of the substrate is 22 g / L or more, the amount of palladium supported per unit volume of the substrate is 0.55 g / L or more; a mass ratio (Pt / Pd) of the amount of the supported platinum to the amount of the supported palladium is 0.55 to 4.0; A catalyst for purifying exhaust gases containing sulfur compounds, wherein the average particle size of the platinum is smaller than the average particle size of the palladium.
2. The BET specific surface area of the carrier layer is 150 m 2 The catalyst according to claim 1, wherein the Mo is 0.01 to 0.
15.
3. The catalyst according to claim 1 or 2, which is substantially free of chlorine atoms.
4. The catalyst according to any one of claims 1 to 3, wherein the average particle size of the platinum is 6 nm or less, and the average particle size of the palladium is 15 nm or less.
5. A method for purifying an exhaust gas containing sulfur compounds, comprising a step of contacting the catalyst according to any one of claims 1 to 4 with an exhaust gas containing sulfur compounds.
6. The purification method according to claim 5 , wherein the step comprises oxidizing hydrocarbons contained in the exhaust gas.
7. The method of claim 6 , wherein the hydrocarbon comprises propane.
Citation Information
Patent Citations
Catalyst for cleaning exhaust gas containing sulfureous compound
JP1980064839A
Preparation of catalyst for removing hydrocarbon in methane-containing exhaust gas
JP2000225343A
Catalyst for oxidation of hydrocarbon with low concentration in exhaust gas and method for preparing it
JP2001129400A
Exhaust gas purifying catalyst
JP2012217933A
Exhaust gas purifying catalyst
JP2012217938A