MEMS Piezoelectric Actuator Manufacturing Method

The method addresses dielectric breakdown and electric field concentration in MEMS piezoelectric actuators by detecting and removing foreign matter through photoetching with a tapered peripheral wall, ensuring robust actuator performance.

JP7583532B2Active Publication Date: 2024-11-14STANLEY ELECTRIC CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020067307
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-04-03
Publication Date
2024-11-14
Estimated Expiration
2040-04-03

AI Technical Summary

Technical Problem

Existing MEMS piezoelectric actuator manufacturing methods face issues with foreign matter causing dielectric breakdown due to laser alteration of non-target areas and electrode layer burrs leading to electric field concentration.

Method used

A method involving lamination of a lower electrode and piezoelectric film, detection of foreign matter, and selective removal of the upper electrode layer using photoetching with a tapered peripheral wall to avoid dielectric breakdown and electrode layer scattering.

Benefits of technology

Prevents dielectric breakdown and electric field concentration by precisely removing foreign matter areas without altering surrounding structures, enhancing actuator performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583532000001
    Figure 0007583532000001
  • Figure 0007583532000002
    Figure 0007583532000002
  • Figure 0007583532000003
    Figure 0007583532000003
Patent Text Reader

Abstract

To provide a MEMS manufacturing piezoelectric actuator method capable of performing a contamination foreign material measurement without a side effect problem.SOLUTION: A manufacturing method comprises: a STEP 1 of laminating a lower electrode layer 31 and a piezoelectric film layer 32 in order from a lower side on a front face side of a wafer 30; a STEP 2 of detecting each region of a foreign material 36 as a detection region; a STEP 3 of forming an upper electrode layer 40; and a STEP 4-6 of forming a removal region 53 onto the upper electrode layer 40 in the size corresponded to the detection region by a photo-etching by an exposure pattern on the basis of the detection of the detection region of the foreign material 36 and exposing the front face of the piezoelectric film layer 32.SELECTED DRAWING: Figure 2B
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a MEMS (Micro Electro Mechanical Systems) piezoelectric actuator. [Background technology]

[0002] In the manufacturing method of the MEMS piezoelectric actuator, foreign matter may get mixed in the piezoelectric film layer. This can easily cause (electrical) insulation breakdown in the piezoelectric film layer when the MEMS piezoelectric actuator is in use, so measures to prevent this are required.

[0003] Patent Documents 1 and 2 disclose a method for manufacturing a MEMS piezoelectric actuator that addresses dielectric breakdown caused by foreign matter.

[0004] In the MEMS piezoelectric actuator manufacturing method of Patent Document 1, focusing on the fact that when the top end of a foreign object protrudes from the piezoelectric film layer, the corresponding portion of the surface of the upper electrode layer also protrudes, laser light is irradiated from the surface side of the upper electrode layer to the area including the protrusion inside. This removes the upper electrode layer in that area, so that when the MEMS piezoelectric actuator is used, no voltage is applied from the upper electrode to the foreign object in the removed area, suppressing dielectric breakdown caused by the foreign object.

[0005] In the MEMS piezoelectric actuator manufacturing method of Patent Document 2, a predetermined voltage is applied between the upper electrode layer and the lower electrode layer in a process before a conductive diaphragm layer is additionally formed on the surface side of the upper electrode layer after the upper electrode layer is formed. This removes the area of ​​the upper electrode layer directly above the foreign object, so that the MEMS piezoelectric actuator after manufacture is prevented from being subjected to dielectric breakdown due to the foreign object. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2015 / 182228 [Patent Document 2] Patent No. 3843004 Summary of the Invention [Problem to be solved by the invention]

[0007] In the MEMS piezoelectric actuator manufacturing method of Patent Document 1, when the upper electrode layer is removed with a laser beam, the laser beam is not directly irradiated, but a large area near the directly irradiated area is affected by the laser beam and altered. Such alteration weakens the actuator force. Burrs are generated along the upper edge of the peripheral wall of the removed area in the upper electrode layer, which causes a side effect problem of electric field concentration.

[0008] In the MEMS piezoelectric actuator manufacturing method of Patent Document 2, after the upper electrode layer is formed, a predetermined voltage is applied between the upper electrode layer and the lower electrode layer in advance to pre-destroy the upper electrode layer directly above the foreign object, and then another coating such as a conductive diaphragm layer is laminated on the surface of the upper electrode layer. However, during the pre-destruction, the debris from the upper electrode layer scatters on the surface of the non-destroyed area of ​​the upper electrode layer, making it necessary to perform a process of removing the debris before additionally forming another coating.

[0009] An object of the present invention is to provide a method for manufacturing a MEMS piezoelectric actuator that can take measures against foreign matter being mixed in without causing side effects. [Means for solving the problem]

[0010] The method for manufacturing a MEMS piezoelectric actuator of the present invention includes the steps of: A first step of laminating a lower electrode layer and a piezoelectric film layer in this order from the bottom on a surface of a wafer; a second step of detecting and storing each area of ​​the foreign matter mixed in the piezoelectric film layer as a detection area on the surface of the piezoelectric film layer; a third step of laminating an upper electrode layer on a surface of the piezoelectric film layer; a fourth step of removing a removal area from the upper electrode layer by photoetching based on an exposure pattern created based on the detection area detected in the second step, the removal area being a size corresponding to the detection area and including the detection area therein, and exposing a surface of the piezoelectric film layer in the removal area; Equipped with.

[0011] According to the method for manufacturing the MEMS piezoelectric actuator of the present invention, the removal area including the detection area for foreign matter is removed from the upper electrode layer by photoetching. As a result, it is possible to remove the removal area from the upper electrode layer while avoiding problems such as the piezoelectric film layer outside the area including directly below the removal area being altered by the influence of the laser light during manufacturing, and the scattering of broken material when the removal area is destroyed.

[0012] Preferably, in the method for producing a MEMS piezoelectric actuator of the present invention, The photoetching in the fourth step includes underetching, which is performed by dry etching before the resist layer is peeled off, to form the peripheral wall of the removed region into a tapered shape whose inner diameter decreases toward the piezoelectric film layer.

[0013] According to this configuration, by tapering the peripheral wall of the removed region, electric field concentration on the peripheral wall of the removed region can be prevented, and dielectric breakdown caused by foreign matter can be further suppressed.

[0014] Preferably, in the method for producing a MEMS piezoelectric actuator of the present invention, In the photoetching of the fourth step, the peripheral contour of the removed region is formed into a circle or a polygon in which all interior angles are obtuse.

[0015] This configuration makes it possible to prevent a large electric field concentration from occurring at the apex of the peripheral contour of the removed region.

[0016] Preferably, in the method for producing a MEMS piezoelectric actuator of the present invention, For each foreign particle, on the surface of the piezoelectric film layer, the diameter of the circumscribing circle of the detection area of ​​the foreign particle is ΦUo, the diameter of the inscribing circle of the removal area that includes the circumscribing circle is ΦUi, and the distance between the center of the circumscribing circle and the center of the inscribing circle is Da. The center of the inscribed circle is located inside the circumscribed circle, And ΦUi-ΦUo>Da.

[0017] According to this configuration, even when the center of the foreign matter is unclear, an appropriate removal area can be set.

[0018] Preferably, in the method for producing a MEMS piezoelectric actuator of the present invention, For ΦUo of 3 to 10 μm, ΦUi is almost 2.2 times ΦUo.

[0019] According to this configuration, it is possible to appropriately set the removal region so that it is not unnecessarily large.

[0020] Preferably, in the method for producing a MEMS piezoelectric actuator of the present invention, The MEMS piezoelectric actuator is mounted on a MEMS optical deflector.

[0021] The MEMS piezoelectric actuator of a MEMS optical deflector has a larger electric field difference per unit thickness in the piezoelectric film layer than the MEMS piezoelectric actuators installed in inkjet printers and other devices, and is more susceptible to dielectric breakdown due to foreign matter. This configuration is particularly suitable as a manufacturing method for the MEMS piezoelectric actuator of a MEMS optical deflector. [Brief description of the drawings]

[0022] [Figure 1] 1 is a schematic diagram showing an optical deflector equipped with a MEMS piezoelectric actuator according to an embodiment of the present invention, as viewed from the front. [Figure 2A] 1A to 1C are diagrams showing a method of manufacturing a MEMS piezoelectric actuator for an optical deflector in the order of steps. [Figure 2B] The steps are shown in the order following those of FIG. 2A. [Diagram 3] 11 is an explanatory diagram of the inclination angle of a tapered portion formed on a wall portion of the upper electrode layer surrounding a recess. FIG. [Figure 4] 5A to 5C are diagrams illustrating examples of the shape of a recess. [Diagram 5] FIG. 11 is an explanatory diagram of the dimensional relationship of a removal region. [Figure 6] 13 is a graph showing the relationship between test time and failure rate for the embodiment and the comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Preferred embodiments of the present invention will be described below. It goes without saying that the present invention is not limited to the following embodiments. The present invention can be implemented in various forms within the scope of the technical ideas disclosed in the specification. Note that components common to the embodiments are given the same reference numerals.

[0024] (light deflector) 1 is a schematic diagram showing an optical deflector 10 equipped with a MEMS piezoelectric actuator according to an embodiment of the present invention, viewed from the front. The MEMS optical deflector 10 includes, as its main components, a mirror unit 11, torsion bars 12a and 12b, inner piezoelectric actuators 13a and 13b, a movable frame unit 14, an outer piezoelectric actuator 15, and a fixed frame unit 16.

[0025] For ease of explanation of the configuration, a three-axis coordinate system is defined. The origin O is set at the center of the mirror section 11. The Z axis is an axis parallel to the thickness direction of the optical deflector 10. The mirror section 11 reciprocates around two axes, a non-resonant rotation axis Lx and a resonant rotation axis Ly. The X and Y axes are defined as directions that coincide with the non-resonant rotation axis Lx and the resonant rotation axis Ly when the normal to the mirror surface of the plane of the mirror section 11 erected at the origin O becomes parallel to the Z axis.

[0026] The torsion bar 12 (a collective term for the upper and lower torsion bars 12a, 12b) extends along the Y axis and is interposed between the mirror portion 11 and the movable frame portion .

[0027] The inner piezoelectric actuator 13 (a collective term for the left and right inner piezoelectric actuators 13a and 13b) has an elliptical peripheral contour that is elongated in the Y-axis direction and surrounds the circular mirror portion 11. The torsion bar 12 is connected to the inner piezoelectric actuator 13 at its middle portion.

[0028] The movable frame portion 14 has the same shape as the inner piezoelectric actuator 13 and surrounds the inner piezoelectric actuator 13. The midpoints of the inner piezoelectric actuators 13a, 13b are located on the X-axis and are coupled to the inner periphery of the movable frame portion 14.

[0029] The outer piezoelectric actuator 15 (a collective term for the left and right outer piezoelectric actuators 15a and 15b) is composed of multiple cantilevers 20 connected in series in a meandering arrangement. Both ends of the outer piezoelectric actuator 15 are located on the X-axis and connected to the outer periphery of the movable frame 14 and the inner periphery of the rectangular fixed frame 16.

[0030] A plurality of electrode pads 17 (a collective term for the left and right electrode pads 17a and 17b) are formed on the left and right sides of the fixed frame portion 16. When the optical deflector 10 is sealed in a package, each electrode pad 17 is connected to a corresponding terminal on the package side by a bonding wire. Each electrode pad 17 is connected to electrodes (not shown) of the inner piezoelectric actuator 13 and the outer piezoelectric actuator 15 via internal wiring (not shown) of the optical deflector 10.

[0031] (Manufacturing method) 2A and 2B show, in order of steps, a method for manufacturing the MEMS piezoelectric actuators of the optical deflector 10. In the optical deflector 10, the MEMS piezoelectric actuators are an inner piezoelectric actuator 13 and an outer piezoelectric actuator 15.

[0032] STEP 1 corresponds to the first step of the present invention. A lower electrode layer 31 and a piezoelectric film layer 32 are laminated in this order from the bottom on the front surface side of a wafer 30. The piezoelectric film layer 32 is made of, for example, a PZT (lead zirconate of titanium) film.

[0033] The piezoelectric film layer 32 may be formed by, for example, magnetron sputtering, a sol-gel method, an MOCVD method, or an ion plating method.

[0034] Foreign matter 36 may be mixed into the piezoelectric film layer 32. The foreign matter 36 has a protruding portion 37 above the surface of the piezoelectric film layer 32 and a buried portion 38 below the surface of the piezoelectric film layer 32.

[0035] STEP 2 corresponds to the second step of the present invention. The wafer 30 has an orientation flat 39. A large number of chips of the optical deflector 10 are manufactured from one wafer 30. STEP 1 to STEP 7 are processes that are performed simultaneously on the entire wafer 30, not on each chip of the optical deflector 10.

[0036] The diagram in STEP 2 shows the piezoelectric film layer 32 and the foreign object 36 viewed from above the piezoelectric film layer 32 in a direction perpendicular to the surface of the piezoelectric film layer 32 (=thickness direction of the wafer 30). The piezoelectric film layer 32 of a PZT film is transparent, whereas the foreign object 36 has a color (e.g., black). Therefore, by photographing the piezoelectric film layer 32 from above the surface with an RGB camera and analyzing the color of the photographed image, it is possible to detect the area of ​​the foreign object 36 parallel to the surface of the piezoelectric film layer 32 (hereinafter referred to as the "detection area").

[0037] Furthermore, the foreign matter 36 usually has a maximum diameter in a direction parallel to the surface of the piezoelectric film layer 32, which is greater in the buried portion 38 than in the protruding portion 37. Based on this, the buried portion 38 is illustrated in the diagram of STEP 2.

[0038] The position of this detection area is stored in a storage device attached to the RGB camera and is used as exposure pattern data in STEP 5, which will be described later.

[0039] In STEP 2, when the foreign object 36 is detected by, for example, a tactile sensor rather than an RGB camera, only the raised portion 37 is detected as the portion exposed from the piezoelectric film layer 32. In this case, the maximum diameter part of the raised portion 37 (usually the base region of the raised portion 37) becomes the detection area. Even when the maximum diameter part of the raised portion 37 becomes the detection area, data of the detection area is stored in a storage device (not shown) and used as data of the exposure pattern.

[0040] STEP 3 corresponds to the third step of the present invention. An upper electrode layer 40 is formed on the surface side of the piezoelectric film layer 32. Furthermore, a resist layer 41 is formed on the surface side of the upper electrode layer 40. This resist layer 41 is assumed to be a positive type.

[0041] Examples of the dimensions are as follows: Thickness of the lower electrode layer 31: 200 nm Thickness of the piezoelectric film layer 32: 5 μm Thickness of the upper electrode layer 40: 100 nm

[0042] STEP 4-6 corresponds to the fourth step of the present invention.

[0043] In STEP 4, the resist layer 41 is exposed to light based on the position of the detection area stored in STEP 2. Since this resist layer 41 is a positive type, the ultraviolet light Lv is irradiated to an area including the position directly above the foreign object 36. The ultraviolet light Lv is a laser beam that can expose the resist layer 41 and has an intensity that does not affect the upper electrode layer 40, and is selectively irradiated to the position of the detection area.

[0044] In STEP 5, by dry etching included in the photoetching, a removal area 53 is formed on the surface side of the piezoelectric film layer 32 and inside the upper electrode layer 40 and the resist layer 41. The illustrated removal area 53 includes not only the removal area of ​​the upper electrode layer 40 but also the removal area of ​​the resist layer 41. The removal area of ​​the upper electrode layer 40 and the removal area of ​​the resist layer 41 coincide with the position of the area projected from the upper side of the resist layer 41 onto the surface of the piezoelectric film layer 32 in parallel to the thickness direction of the wafer 30.

[0045] The exposure pattern of the laser light is set so that the foreign matter 36 is located approximately at the center of the removal region 53. A tapered portion 58 (STEP 6) is formed by under-etching 54 in the upper electrode layer 40 on the lower surface side of the edge of the resist layer 41 surrounding the removal region 53.

[0046] The photoetching in STEPs 4 and 5 will be described in more detail. The resist layer 41 is made of AZ6130 manufactured by Merck Ltd. and has a thickness of 2 μm. After pattern exposure by irradiation with ultraviolet light Lv (laser light), development is performed to wash away the portions of the resist layer 41 that correspond to the removal regions 53. Post-baking after development is performed at 110° C. for 1 minute to round the edges of the resist layer 41.

[0047] The subsequent dry etching was performed by RF (radio frequency) discharge using etching gases Ar+Cl at a pressure of 1 Pa. The structure shown in STEP 5 is the structure after this dry etching.

[0048] STEP 6 is a step of removing the resist layer 41. By this removal step, the resist layer 41 is removed from the surface of the upper electrode layer 40. The tapered portion 58 is formed by under-etching 54 in STEP 6, and is inclined toward the center of the removal region 53 toward the surface side of the piezoelectric film layer 32. The specific structures of the removal region 53 and the under-etching 54 will be described with reference to FIG. 3.

[0049] After STEP 6, the optical deflector 10 is completed through a well-known MEMS manufacturing process.

[0050] (Detailed explanation of the removal area) FIG. 3 is an explanatory diagram of the inclination angle α of the tapered portion 58 formed in the wall portion of the upper electrode layer 40 surrounding the removed region 53. As shown in FIG.

[0051] As explained in STEP 5 of FIG. 2B, the surrounding wall surrounding the removed region 53 in the upper electrode layer 40 becomes a tapered portion 58 by under-etching 54. In FIG. 3, a lower end 61 and an upper end 62 are the upper and lower ends of the tapered portion 58, respectively, and their heights coincide with the lower and upper surfaces of the upper electrode layer 40. Reference numeral 65 denotes a normal line to the surface of the piezoelectric film layer 32 where the lower end 61 stands. An inclined line 66 is a straight line connecting the lower end 61 and the upper end 62.

[0052] In FIG. 3, the definitions of the symbols are as follows: Hs: Direction of a plane parallel to the surface of the piezoelectric film layer 32 α: Angle of inclination of the inclined line 66 from the lower end 61 to the upper end 62 with respect to the normal line 65 Wa: Distance in the Hs direction between the base of the raised portion 37 (the point where the raised portion 37 starts to rise from the surface of the piezoelectric film layer 32) and the bottom end 61 Wb: the shortest distance between the foreign object 36 and the lower end 61. In the illustrated example, the point where the foreign object 36 protrudes most toward the lower end 61 in the parallel direction is in the buried portion 38, so the shortest distance is the distance in the Hs direction between the buried portion 38 and the lower end 61. Wc: Distance in the Hs direction between the lower end 61 and the upper end 62

[0053] The under-etching 54 varies depending on the circumferential position of the removed region 53. Therefore, the inclination angle α is not uniform over the entire circumference of the tapered portion 58 but varies. The average inclination angle α over the entire circumference of the tapered portion 58 is defined as αavr. It is preferable to set αavr as follows. 0°<αavr≦75°...(Formula 1)

[0054] 2A and 2B, removal region 53 is formed by photoetching rather than by irradiation with laser light, so that it is possible to eliminate side effects such as burrs continuously lining up on the surface of upper electrode layer 40, particularly along upper end 62 of removal region 53. As a result, no burrs are present on the surface of upper electrode layer 40 in the range from raised portion 37 to 2·Wa+Wc or from buried portion 38 to 2·Wb+Wc in the Hs direction. This means that removal region 53 can be removed without side effects such as burrs being generated to generate removal region 53, which then cause electric field concentration and result in insulation breakdown separate from foreign matter 36.

[0055] In addition, in Fig. 3, the difference in length between Wa and Wb is exaggerated, but in reality it is a small difference, and either Wa or Wb can be used. When detecting the detection area of ​​foreign body 36 with an RGB camera that can detect the area of ​​buried portion 38, Wa is used, and when detecting the detection area of ​​foreign body 36 with a tactile sensor that can only detect raised portion 37, Wb is used.

[0056] 4 shows the shapes (circumferential contours) of removal regions 53a and 53b as examples of the shape of removal region 53. The shape of removal region 53 (collectively referring to removal regions 53a and 53b) is determined by the irradiation pattern (circumferential contour) of the laser light in STEP 4 of FIG. 2B.

[0057] In FIG. 4, the reason for describing "raised portion 37 or buried portion 38" is that, as described above, when detecting the maximum diameter portion of foreign body 36, which determines the size of upper electrode layer 40, there are cases where buried portion 38 is included in the detection ("38": for example, when an RGB camera is used) and cases where buried portion 38 is excluded and only raised portion 37 is detected ("37": for example, when a tactile sensor is used).

[0058] The shape of the foreign object 36 when viewed from above the piezoelectric film layer 32 in the thickness direction of the wafer 30 is not circular, but is illustrated as a circle for convenience of illustration. The shape of the removal area 53a is circular. The shape of the removal area 53b is a polygon with all interior angles being obtuse. This makes it possible to avoid electric field concentration, which is likely to cause dielectric breakdown of the piezoelectric film layer 32, occurring at some points around the entire periphery of the removal area 53.

[0059] In Fig. 4(b), Co is the circumscribing circle of raised portion 37 when raised portion 37 has a non-circular shape when viewed from above, and Ci is the inscribing circle of removed area 53b. Note that the periphery of both removed areas 53a and 53b is tapered portion 58, and the circumferential outline of removed area 53 in Fig. 4 corresponds to the position of lower end 61 of tapered portion 58.

[0060] Fig. 5 is an explanatory diagram of the dimensional relationship of the removed region 53b. In order to explain the dimensional relationship, Fig. 5 is an enlarged view of Fig. 4(b). In Fig. 5, the definitions of the respective symbols are as follows:

[0061] Oi: Center of inscribed circle Ci Oo: Center of circumscribing circle Co ΦUi: Diameter of the inscribed circle Ci ΦUo: Diameter of circumscribing circle Co Da: Distance between Oi and Oo

[0062] The center Oi is set inside the circumscribing circle Co. In addition, the following relationship is set: ΦUi-ΦUo>Da (Eq. 2)

[0063] (Confirmation test) 6 is a graph showing the test time and failure rate for the embodiment and the comparative example. In both the embodiment and the comparative example, the test subject was a MEMS piezoelectric actuator assumed to be used as the outer piezoelectric actuator 15 of the optical deflector 10. However, the outer piezoelectric actuator 15 of the optical deflector 10 of the comparative example did not have a removed region 53, whereas the outer piezoelectric actuator 15 of the optical deflector 10 of the embodiment had a removed region 53. In the optical deflector 10, the voltage per unit length in the thickness direction during operation is greater for the outer piezoelectric actuator 15 than for the inner piezoelectric actuator 13, so that the outer piezoelectric actuator 15 is more likely to suffer dielectric breakdown than the inner piezoelectric actuator 13.

[0064] From the results of FIG. 6, it was found that the failure rate (time until dielectric breakdown) was significantly increased by forming removed region 53.

[0065] (Modification) In STEP 5 of FIG. 2B, the resist layer 41 is a positive type, but in the method for producing the MEMS piezoelectric actuator of the present invention, a negative type resist can also be used.

[0066] In the embodiment, the inner piezoelectric actuator 13 and the outer piezoelectric actuator 15 of the optical deflector 10 are shown as the MEMS piezoelectric actuator of the present invention. However, the MEMS piezoelectric actuator manufacturing method to which the present invention is applied may also be a MEMS piezoelectric actuator manufacturing method and a MEMS piezoelectric actuator provided in something other than an optical deflector. Also, the optical deflector may be a uniaxial scanning type instead of a biaxial scanning type like the optical deflector 10.

[0067] In the embodiment, the etching for achieving the under-etching 54 in STEPs 4 and 5 has been described as dry etching. In the present invention, it is also possible to form the tapered portion 58 by wet etching or ion milling instead of dry etching.

[0068] The optical deflector 10 of the embodiment is assumed to be mounted on a vehicle headlight or the like. In the optical deflector 10 for the headlight, the outer piezoelectric actuator 15 as the MEMS piezoelectric actuator must be guaranteed to operate in the range of, for example, -40 to 125°C. That is, while the MEMS piezoelectric actuator of an inkjet printer is normally used in an environment of 60°C, the MEMS piezoelectric actuator of the headlight is exposed to a severe high-temperature environment of 125°C. For this reason, the MEMS piezoelectric actuator of the headlight is susceptible to the problem of dielectric breakdown when a foreign object 36 is mixed into the piezoelectric film layer 32. Therefore, the MEMS piezoelectric actuator of the present invention is particularly advantageous when applied to the MEMS piezoelectric actuator of the optical deflector mounted on the vehicle headlight and used to generate scanning light. [Explanation of symbols]

[0069] 10···optical deflector, 15···outer piezoelectric actuator (MEMS piezoelectric actuator), 30···wafer, 31···lower electrode layer, 32···piezoelectric film layer, 33···upper electrode layer, 36···foreign matter, 40···upper electrode layer, 41···resist layer, 53···removed area, 54···underetching, 58···tapered portion.

Claims

1. A first step of laminating a lower electrode layer and a piezoelectric film layer in this order from the bottom on a surface of a wafer; a second step of detecting and storing each area of ​​the foreign matter mixed in the piezoelectric film layer as a detection area on the surface of the piezoelectric film layer; a third step of laminating an upper electrode layer on a surface of the piezoelectric film layer; a fourth step of removing the upper electrode layer by photoetching while leaving the foreign object embedded in the piezoelectric film layer in a removal area that includes the foreign object and has a size corresponding to the detection area, based on an exposure pattern created based on the detection area stored in the second step, thereby exposing a raised portion of the foreign object on the surface of the piezoelectric film layer in the removal area; A method for manufacturing a MEMS piezoelectric actuator, comprising:

2. 2. The method for manufacturing a MEMS piezoelectric actuator according to claim 1, The method for manufacturing a MEMS piezoelectric actuator, characterized in that the photoetching in the fourth step includes underetching, which is a dry etching step performed before the resist layer is peeled off, to form a peripheral wall of the upper electrode layer around the removal area into a tapered shape whose inner diameter decreases toward the piezoelectric film layer.

3. 3. The method for manufacturing a MEMS piezoelectric actuator according to claim 1, further comprising the steps of: In the fourth step of photoetching, the peripheral contour of the removal region is formed into a circle or a polygon all of whose interior angles are obtuse.

4. The method for manufacturing a MEMS piezoelectric actuator according to any one of claims 1 to 3, For each foreign particle, on the surface of the piezoelectric film layer, the diameter of the circumscribing circle of the detection region of the foreign particle is ΦUo, the diameter of the inscribing circle of the removal region that includes the circumscribing circle is ΦUi, and the distance between the center of the circumscribing circle and the center of the inscribing circle is Da. The center of the inscribed circle is located inside the circumscribed circle, and ΦUi-ΦUo>Da.

5. 5. The method for manufacturing a MEMS piezoelectric actuator according to claim 4, A method for manufacturing a MEMS piezoelectric actuator, characterized in that ΦUo is 3 to 10 μm, and ΦUi is approximately 2.2 times ΦUo.

6. The method for manufacturing a MEMS piezoelectric actuator according to any one of claims 1 to 5, The method for manufacturing a MEMS piezoelectric actuator is characterized in that the MEMS piezoelectric actuator is provided in a MEMS optical deflector.

Citation Information

Patent Citations

  • Ink jet head, its manufacturing method, and ink jet recording device

    JP2003159799A

  • Piezoelectric element, piezoelectric actuator, and manufacturing method of the piezoelectric element

    JP2019207938A

  • Inkjet head, manufacturing method thereof, and inkjet recording apparatus

    JP3843004B2

  • Process for fabricating piezoelectric element

    WO2006090618A1

  • Capacitor fabrication method, capacitor fabricating device, capacitor fabricating program, and recording medium