Gas barrier coating agent, gas barrier coating layer, and laminate
A gas barrier coating agent using polysaccharides and alkoxysilane compounds with amino groups addresses thickening and gelation issues, enabling higher solid content concentrations and improved water resistance and barrier properties.
Patent Information
- Application Number
- JP2020178585
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-06-15
- Filing Date
- 2020-10-26
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2040-10-26
AI Technical Summary
Coating agents using natural resources (biomass) for gas barrier properties face issues such as thickening and gelation when the solid content concentration is increased.
A gas barrier coating agent comprising polysaccharides with carboxyl groups, alkoxysilane compounds with amino groups and/or their hydrolyzed condensates, alcohol, and water, which improve solubility and prevent gelation, allowing for higher solid content concentrations.
The solution enhances the solid content concentration of the coating agent, improving its water resistance and barrier properties while maintaining stability and preventing gelation.
Smart Images

Figure 0007583573000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a gas barrier coating agent, a gas barrier coating layer, and a laminate. [Background technology]
[0002] In packaging materials used for food, medicine, electronic parts, etc., coating agents with gas barrier properties that block gases such as oxygen and water vapor are used to protect the contents. From the viewpoint of environmental conservation, coating agents with gas barrier properties that utilize natural resources (biomass) are also known (Patent Documents 1-3). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2001-334600 A [Patent Document 2] JP 2008-49606 A [Patent Document 3] International Publication No. 2011 / 118520 Summary of the Invention [Problem to be solved by the invention]
[0004] It has been found that the above-mentioned coating agents having gas barrier properties that utilize natural resources (biomass) have problems such as thickening and gelling of the coating agent when the solid content concentration is increased.
[0005] The present invention has been made in view of the above circumstances, and has an object to provide a gas barrier coating agent that utilizes biomass and is capable of increasing the solid content concentration.
[0006] Another object of the present invention is to provide a gas barrier coating layer formed from the gas barrier coating agent, and a laminate having the coating layer. [Means for solving the problem]
[0007] That is, the present invention relates to a gas barrier coating agent containing a polysaccharide having a carboxyl group, an alkoxysilane compound having an amino group and / or a hydrolysis condensate thereof, an alcohol, and water.
[0008] The present invention also relates to a gas barrier coating layer formed from the gas barrier coating agent.
[0009] The present invention also relates to a laminate having a substrate and the gas barrier coating layer. Effect of the Invention
[0010] Although the details of the mechanism of action of the gas barrier coating agent of the present invention are unclear, it is presumed as follows, however, the present invention is not limited to this mechanism of action.
[0011] The gas barrier coating agent of the present invention contains a polysaccharide having a carboxyl group, an alkoxysilane compound having an amino group and / or its hydrolysis condensate, an alcohol, and water. The alkoxysilane compound having an amino group and / or its hydrolysis condensate has excellent gas barrier properties, and the polysaccharide having a carboxyl group is neutralized by the alkoxysilane compound and / or its hydrolysis condensate, thereby improving its solubility in alcohol and suppressing gelation, and it is presumed that the solid content concentration of the gas barrier coating agent can be increased. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The gas barrier coating agent of the present invention contains a polysaccharide having a carboxyl group, an alkoxysilane compound having an amino group and / or a hydrolysis condensate thereof, an alcohol, and water.
[0013] <Polysaccharides with carboxyl groups> The polysaccharide having a carboxyl group may be a known one, and examples thereof include polysaccharides (natural polysaccharides) that originally have a carboxyl group, such as pectin, alginic acid, and hyaluronic acid. The polysaccharide having a carboxyl group may be one in which at least a part of the functional groups (e.g., hydroxyl group, amino group, etc.) in the molecule of a polysaccharide such as starch, amylose, amylopectin, dextrin, glycogen, cyclodextrin, cellulose, agarose, inulin, glucomannan, chitin, or chitosan is chemically modified to introduce a carboxyl group. Among these, polysaccharides that originally have a carboxyl group are preferred from the viewpoint of increasing the biomass degree of the solid content contained in the gas barrier coating agent, and pectin is more preferred from the viewpoint of increasing the coating film strength such as water resistance. The polysaccharide having a carboxyl group may be used alone or in combination of two or more kinds.
[0014] <Alkoxysilane Compound Having Amino Group and / or Hydrolysis Condensate thereof> The alkoxysilane compound having an amino group and / or its hydrolysis condensate may be an alkoxysilane compound having an amino group and / or its hydrolysis condensation reaction product, and examples of the alkoxysilane compound having an amino group include 3-aminopropyltrimethoxysilane, 3-(2-aminoethylamino)propyltriethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, N-phenyl-γ-aminopropyltrimethoxysilane, etc. The alkoxysilane compound having an amino group and / or its hydrolysis condensate may be used alone or in combination of two or more.
[0015] <Alcohol> The alcohol may be any known alcohol, for example, an alcohol having about 1 to 10 carbon atoms, but from the viewpoint of improving the drying property of the coating agent and the stability of the hydrolysis condensate of the alkoxysilane compound, it is preferable to include a lower alcohol having 2 to 4 carbon atoms, such as ethyl alcohol, n-propyl alcohol, iso-propyl alcohol, n-butyl alcohol, iso-butyl alcohol, sec-butyl alcohol, tert-butyl alcohol, etc. The alcohol may be used alone or in combination of two or more kinds.
[0016] In the gas barrier coating agent, the total ratio of the polysaccharide having a carboxyl group and the alkoxysilane compound having an amino group and / or its hydrolysis condensate can be 3% by mass or more by including at least an alkoxysilane compound having an amino group and / or its hydrolysis condensate in the gas barrier coating agent. In the gas barrier coating agent, the total ratio of the polysaccharide having a carboxyl group and the alkoxysilane compound having an amino group and / or its hydrolysis condensate is preferably 4% by mass or more, more preferably 5% by mass or more, from the viewpoint of improving the water resistance and barrier properties of the gas barrier coating layer, and is preferably 15% by mass or less, more preferably 10% by mass or less, and even more preferably 8% by mass or less, from the viewpoint of improving the water resistance and barrier properties of the gas barrier coating layer.
[0017] The mass ratio of the polysaccharide having a carboxyl group to the alkoxysilane compound having an amino group and / or its hydrolysis condensate (polysaccharide having a carboxyl group / alkoxysilane compound having an amino group and / or its hydrolysis condensate) is preferably 0.2 or more, and more preferably 0.4 or more, from the viewpoint of improving the water resistance and barrier properties of the gas barrier coating layer, and is preferably 1.2 or less, more preferably 0.9 or less, and even more preferably 0.7 or less, from the viewpoint of improving the water resistance and barrier properties of the gas barrier coating layer.
[0018] The proportion of the alcohol in the gas barrier coating agent is preferably 15% by mass or more, more preferably 20% by mass or more, and even more preferably 25% by mass or more, from the viewpoint of improving the coatability and storage stability of the gas barrier coating agent and preventing the precipitation of the hydrolysis condensation product of the alkoxysilane compound having an amino group, and is preferably 60% by mass or less, more preferably 50% by mass or less, and even more preferably 40% by mass or less, from the viewpoint of improving the coatability and storage stability of the gas barrier coating agent and preventing the gelation of the polysaccharide having a carboxyl group. The alcohol also includes alcohol generated by the hydrolysis condensation product of the alkoxysilane compound having an amino group.
[0019] The proportion of water in the gas barrier coating agent is preferably 45% by mass or more, more preferably 50% by mass or more, from the viewpoint of adjusting the viscosity so that the gas barrier coating agent has good handleability, and is preferably 75% by mass or less, more preferably 70% by mass or less, from the viewpoint of preventing gelation of polysaccharides having carboxyl groups and preventing precipitation of hydrolysis condensation products of alkoxysilane compounds having amino groups. The water also includes water used in the hydrolysis condensation reaction of alkoxysilane compounds.
[0020] The gas barrier coating agent may contain a basic compound (excluding the alkoxysilane compound having an amino group and / or its hydrolysis condensate) from the viewpoint of improving the water resistance and barrier properties of the gas barrier coating layer. The basic compound may be a known one, and examples thereof include inorganic basic compounds such as sodium hydroxide and potassium hydroxide; and organic basic compounds such as ammonia, methylamine, ethylamine, monoethanolamine, N,N-dimethylethanolamine, N,N-diethylethanolamine, N,N-dibutylethanolamine, diethanolamine, N-methyldiethanolamine, triethanolamine, morpholine, N-methylmorpholine, and N-ethylmorpholine. Among these, ammonia is preferred from the viewpoint of improving the water resistance of the gas barrier coating layer. The basic compounds may be used alone or in combination of two or more kinds.
[0021] The gas barrier coating agent may contain additives such as disaccharides such as sucrose; polysaccharides other than polysaccharides having a carboxyl group, such as starch, amylose, amylopectin, dextrin, glycogen, cyclodextrin, cellulose, agarose, inulin, glucomannan, chitin, and chitosan; gas barrier resins such as polyvinyl alcohol resins and ethylene-vinyl alcohol resins; ultraviolet absorbers, antistatic agents, leveling agents, defoamers, preservatives, and fillers, as necessary.
[0022] In the solid content of the gas barrier coating agent (excluding the basic compound), the total proportion of the polysaccharide having a carboxyl group and the alkoxysilane compound having an amino group and / or its hydrolysis condensate is preferably 50 mass% or more, more preferably 60 mass% or more, and even more preferably 70 mass% or more.
[0023] The gas barrier coating agent preferably has a biomass ratio of 25% or more, more preferably 30% or more, and even more preferably 40% or more, in the solid content contained in the gas barrier coating agent (excluding the basic compound).
[0024] The gas barrier coating agent contains the alkoxysilane compound having an amino group and / or its hydrolysis condensate, and from the viewpoint of suppressing gelation of the polysaccharide having a carboxyl group, the pH is preferably 2.0 or higher, and more preferably 2.5 or higher, and from the viewpoint of improving the storage stability of the gas barrier coating agent, the pH is preferably 8.0 or lower, and more preferably 7.0 or lower.
[0025] From the viewpoint of coatability, the gas barrier coating agent preferably has a viscosity (initial viscosity after production) of 1 to 1000 mPa·s, more preferably 5 to 500 mPa·s, and even more preferably 10 to 200 mPa·s.
[0026] The method for preparing the gas barrier coating agent is not particularly limited. For example, the above-mentioned components may be added in order or simultaneously and mixed with a stirrer or disperser.
[0027] <Gas barrier coating layer, laminate> The gas barrier coating layer of the present invention is a dry film formed from the gas barrier coating agent. The laminate of the present invention has a substrate and the gas barrier coating layer. The laminate is usually obtained by applying the gas barrier coating agent to the substrate. The method of applying the gas barrier coating agent is not particularly limited, and examples of the method include coating methods using various coating devices such as a blade coater, an air knife coater, a roll coater, a bar coater, a gravure coater, a rod blade coater, a lip coater, a curtain coater, a die coater, and a spray coater.
[0028] The coating amount (dry film thickness) of the gas barrier coating layer is usually 0.1 g / m 2 It is preferable that the content is 0.5 g / m or more. 2 More preferably, it is 10 g / m or more. 2 It is preferable that the thickness is less than 5 g / m 2 It is more preferable that:
[0029] Examples of the substrate include base paper such as pulp that has been conventionally used in paper barrier materials, various plastic films made of polyolefin, modified polyolefin, polyester, nylon, polystyrene, etc. that have been conventionally used in flexible packaging, and composite films made of two or more of these. The substrate may be subjected to metal vapor deposition treatment, corona discharge treatment, surface coating treatment, etc.
[0030] In addition to the above-mentioned substrate and gas barrier coating layer, the laminate may further include a thermoplastic resin layer that enables heat sealing, a printed layer, a protective layer, etc. In this case, each layer may be laminated by melt extrusion or by using an adhesive. EXAMPLES
[0031] The present invention will be described below with reference to examples, but the present invention is not limited to these.
[0032] <Preparation Example 1> <Preparation of an aqueous solution of polysaccharides having carboxyl groups> 90 parts of ion-exchanged water was added to 10 parts by mass of a pectin mixture (product name "LM-100AS-HP", manufactured by Sansho Co., Ltd.), and the mixture was stirred at 90°C for 1 hour to obtain an aqueous pectin solution (pectin concentration 5.5% by mass, sucrose concentration 4.5% by mass).
[0033] <Preparation of aqueous solution of polyvinyl alcohol> 90 parts by mass of ion-exchanged water was added to 10 parts by mass of polyvinyl alcohol (trade name "PVA-105", manufactured by Kuraray), and the mixture was stirred at 95°C for 1 hour to obtain an aqueous PVA solution (solid content 10% by mass).
[0034] <Preparation of hydrolysis condensation product of alkoxysilane compound having amino group (1)> 64.6 parts by mass of ion-exchanged water was added to 20.4 parts by mass of 3-aminopropyltrimethoxysilane, and 14.7 parts by mass of ethanol and 0.3 parts by mass of 1 N hydrochloric acid as a hydrolysis catalyst were added with stirring, and the mixture was heated at 50°C for 1 hour to obtain an aqueous solution of 3-aminopropyltrimethoxysilane (APTMS) hydrolysis condensate (solid content 12.5% by mass).
[0035] <Preparation of hydrolysis condensation product of alkoxysilane compound having amino group (2)> 66.8 parts by mass of ion-exchanged water was added to 18.2 parts by mass of 3-(2-aminoethylamino)propyltriethoxysilane, and 14.7 parts by mass of ethanol and 0.3 parts by mass of 1 N hydrochloric acid as a hydrolysis catalyst were added with stirring, and the mixture was heated at 50°C for 1 hour to obtain an aqueous solution of 3-(2-aminoethylamino)propyltriethoxysilane (AEAPTES) hydrolysis condensate (solids content 12.5% by mass).
[0036] <Preparation of hydrolysis condensation product of alkoxysilane compound> 41.7 parts by mass of ion-exchanged water was added to 43.3 parts by mass of tetraethoxysilane (product name "High-purity ethyl orthosilicate", manufactured by Tama Chemical Industry Co., Ltd.), and 14.7 parts by mass of ethanol and 0.3 parts by mass of 1 N hydrochloric acid as a hydrolysis catalyst were added with stirring, followed by heating at 50°C for 1 hour to obtain an aqueous solution of tetraethoxysilane (TEOS) hydrolysis condensate (solid content 12.5% by mass).
[0037] <Example 1> <Production of gas barrier coating agent> 30 parts by mass of the above pectin aqueous solution, 32 parts by mass of the above APTMS hydrolysis condensate aqueous solution, 20 parts by mass of ethanol, and 18 parts by mass of ion-exchanged water were mixed and stirred at room temperature for 10 minutes to produce the gas barrier coating agent of Example 1. The pH of the gas barrier coating agent was 5.0.
[0038] <Preparation of Laminate Having Gas Barrier Coating Layer> The gas barrier coating agent obtained above was applied to a polypropylene film (product name "P-2161", manufactured by Toyobo Co., Ltd.) using a No. 6 wire bar, dried using a dryer, and then aged at 60°C for one day to form a gas barrier coating layer (coating amount of about 0.6 g / m 2 ) was formed to prepare a laminate having a gas barrier coating layer.
[0039] <Examples 2-8, Comparative Examples 1-3> According to the formulations in Table 1, the gas barrier coating agents of the Examples and Comparative Examples were produced and laminates having a gas barrier coating layer were prepared by the same operations as in Example 1. However, the gas barrier coating agent of Comparative Example 1 gelled, so that a laminate having a gas barrier coating layer could not be produced.
[0040] The laminates having the gas barrier coating layer obtained in the above Examples and Comparative Examples were evaluated as follows. The evaluation results are shown in Table 1.
[0041] <Evaluation of gas barrier properties under high humidity conditions> The laminate having the gas barrier coating layer obtained above was left for 72 hours in an atmosphere of 25°C and 90% RH, and then the oxygen transmission rate (OTR value) (unit: (cc / m)) was measured using an oxygen transmission rate measuring device (manufactured by Mocon, product name "OX-TRAN1 / 50") in accordance with JIS 7126 B method. 2 The measurements were performed at 25°C and in an atmosphere of 90% RH. 2 The passing criteria was 100 / day·atm or less.
[0042] <Water resistance evaluation> The coating layer surface of the laminate having the gas barrier coating layer obtained above was rubbed with a cotton swab moistened with water, and evaluated according to the following evaluation criteria. ○: It takes 4 or more strokes for the coating to melt or peel off. ×: The coating film melts or peels off within 3 strokes.
[0043] [Table 1]
[0044] In Table 1, the APTMS ethanol solution (solid content: 12.5% by mass) indicates a solution in which 3-aminopropyltrimethoxysilane (APTMS) is mixed in ethanol.
Claims
1. A gas barrier coating agent comprising a polysaccharide having a carboxyl group, an alkoxysilane compound having an amino group and / or a hydrolysis condensate thereof, an alcohol, and water, The gas barrier coating agent has a solid content of 5% by mass or more, A gas barrier coating agent, characterized in that the solid content contained in the gas barrier coating agent has a biomass ratio of 25% or more.
2. 2. The gas barrier coating agent according to claim 1, characterized in that the total ratio of the polysaccharide having a carboxyl group and the alkoxysilane compound having an amino group and / or its hydrolysis condensate in the gas barrier coating agent is 5 mass% or more.
3. 3. The gas barrier coating agent according to claim 1, wherein the alcohol content in the gas barrier coating agent is 15% by mass or more and 60% by mass or less.
4. 4. The gas barrier coating agent according to claim 1, wherein the polysaccharide having a carboxyl group is pectin.
5. A gas barrier coating layer formed from the gas barrier coating agent according to any one of claims 1 to 4.
6. A laminate comprising a substrate and the gas barrier coating layer according to claim 5.
7. 7. The laminate according to claim 6, wherein the substrate is a base paper or a plastic film.
Citation Information
Patent Citations
Gas barrier material
JP2001334600A
Biodegradable gas-barrier material
JP2008049606A
Polysaccharide composite material
JP2008189692A
Gas barrier molded body, coating liquid and method for manufacturing gas barrier molded body using coating liquid
JP2008238475A
Alkoxysilane coating
JP2009506218A