Adhesive compositions, adhesive films, films for touch panels, films for electronic paper, films for organic electroluminescence

A copolymerization method using nitrogen-containing vinyl monomers and specific monomer ratios in adhesive films addresses the challenge of maintaining transparency and preventing clouding under high temperature and humidity, ensuring durability and low haze values.

JP7583872B2Active Publication Date: 2024-11-14ZACROS CORP
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2023127211
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-08-03
Publication Date
2024-11-14
Estimated Expiration
2031-09-20

AI Technical Summary

Technical Problem

Optical adhesive films applied with thick layers face challenges in maintaining transparency and preventing clouding under high temperature and high humidity conditions, often compromising durability when attempts to improve clouding prevention performance.

Method used

A copolymerization method using nitrogen-containing vinyl monomers without hydroxyl groups and alkyl (meth)acrylate monomers with alkoxy groups, combined with a copolymer lacking carboxyl groups but containing hydroxyl groups, along with specific monomer ratios and crosslinking agents, forms an adhesive composition that maintains transparency and prevents clouding.

Benefits of technology

The adhesive composition achieves excellent transparency and clouding prevention even under high temperature and high humidity, with a haze value of 4.0% or less after 240 hours, and maintains durability without peeling or foaming.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583872000004
    Figure 0007583872000004
  • Figure 0007583872000001
    Figure 0007583872000001
  • Figure 0007583872000002
    Figure 0007583872000002
Patent Text Reader

Abstract

To provide an adhesive composition having turbidity prevention performance without causing turbidity even if an adhesive film on which an adhesive layer is thickly coated is left stand in an atmosphere of high temperature and high humidity for a long period of time.SOLUTION: There is provided an adhesive composition in which an acrylic polymer is a copolymer having a weight average molecular weight of 200000 to 2000000 comprising (A) a total 50 to 95 pts.wt. of an alkyl (meth)acrylate monomer having an alkyl group having 1 to 14 carbon atoms and a phenoxy group-containing alkyl(meth)acrylate monomer, (B) 5 to 50 pts.wt. of at least one of a nitrogen-containing vinyl monomer containing no hydroxy group and carboxyl group or an alkoxy group-containing alkyl (meth)acrylate monomer, (C) a total of 0.5 to 10 pts.wt. of at least one hydroxyl group-containing (meth)acrylic acid ester, which is a copolymerizable vinyl monomer containing a hydroxyl group without containing a carboxyl group in the functional group, and (D) 0.01 to 5 pts.wt. of the crosslinking agent.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pressure-sensitive adhesive composition and a pressure-sensitive adhesive film having a clouding prevention performance, which prevents clouding even when a pressure-sensitive adhesive layer is applied to the pressure-sensitive adhesive film and the pressure-sensitive adhesive film is left in a high-temperature and high-humidity atmosphere for a long period of time. More specifically, the present invention relates to a pressure-sensitive adhesive composition containing a nitrogen-containing vinyl monomer or an alkoxy group-containing (meth)acrylic acid ester monomer that does not contain a hydroxyl group, and relates to providing a pressure-sensitive adhesive composition that does not lose transparency even when the pressure-sensitive adhesive layer is applied to a thick thickness, and further has excellent clouding prevention performance even after being left in a high-temperature and high-humidity atmosphere for a long period of time, and a pressure-sensitive adhesive film using the same. [Background technology]

[0002] 2. Description of the Related Art In recent years, in various displays such as PDPs (plasma displays), liquid crystal panels, and organic EL panels, various optical films and protective plates are attached to the front surface of the display. For example, in a PDP, in addition to electromagnetic wave shielding films, near-infrared absorbing films to prevent malfunction of various remote control switches that use the near-infrared wavelength region, ultraviolet absorbing films to prevent deterioration over time of the near-infrared absorbing agent used in the near-infrared absorbing films, neon light blocking films to adjust the color tone in the visible light region, anti-reflection films to prevent external light from being reflected on the surface of the optical filter, etc. are attached to the front of the display. By using these films as optical filters for displays, the quality of image reflection is improved.

[0003] In addition, in mobile phones in which a liquid crystal panel is used as a display, a shock-absorbing protective plate is attached to the front of the liquid crystal panel via an air gap to prevent the liquid crystal panel from cracking. However, in recent years, in order to reduce weight and thickness and improve visibility, a thin protective plate is directly attached to the front of the liquid crystal panel of a mobile phone using an adhesive layer without providing an air gap. Also, in the case of PDPs, in order to reduce weight and thickness and improve visibility, a direct color filter method is being considered in which an optical filter film is directly attached to the PDP panel.

[0004] The above optical films and protective plates are attached to the front surface of a display using an adhesive layer. However, when various optical films are attached to a display using the adhesive layer, there is a problem that air bubbles are entrapped, resulting in the formation of microbubbles in the adhesive layer. In addition, display performance tests conducted before shipment of display devices require the display to pass a durability test under environmental conditions of high temperature and high humidity using an oven. However, in the case of optical films using adhesive layers with unimproved anti-clouding performance, the adhesive layer becomes cloudy after removal from the oven, which reduces the commercial value of the display.

[0005] Thus, there is the problem of microscopic air bubbles forming in the adhesive layer when adhesive tape is used to bond an optical film to a display, and there is also the problem of the adhesive layer becoming cloudy when a durability test is performed on a display in an oven under high temperature and high humidity environmental conditions, and after the display is removed from the oven. To solve this problem, various efforts have been made in the past.

[0006] For example, Patent Document 1 discloses an adhesive optical film using an adhesive layer that improves the repair performance when a depression occurs on the surface of the adhesive layer and prevents the entrapment of air bubbles. Specifically, the adhesive layer is formed of a crosslinked product of a composition containing a polymer containing an alkyl (meth)acrylate with an alkyl group having 7 to 18 carbon atoms and a hydroxyl group-containing monomer in a weight ratio of 100:0.01 to 5, and a compound having two or more functional groups that react with hydroxyl groups. After laminating an optical film using this adhesive layer (thickness 20 μm) to glass, it is left in an atmosphere of 50°C x 0.05 MPa for 5 minutes, and the presence or absence of air bubbles is inspected by a method of visually checking the presence or absence of microbubbles in the adhesive layer, and it is stated that the generation of microbubbles is prevented.

[0007] Patent Document 2 discloses a resin composition containing an acrylic acid derivative, an acrylic acid derivative polymer, and a high molecular weight crosslinking agent for shock absorption necessary for protecting image display devices, etc. The resin composition is said to be useful for preventing cracking of image display panels or mitigating stress and shock, and has excellent transparency. Moisture absorption tests were conducted by placing a resin sheet molded in a frame 0.5 mm deep in a high temperature, high humidity test chamber at 60°C and 90% RH for 50 hours, and the results were evaluated by visual observation. As a result, it was found that this resin composition had little foaming and excellent transparency.

[0008] Patent Document 3 discloses an adhesive layer for electronic displays having excellent wet heat resistance. Specifically, the adhesive composition for electronic displays contains a copolymer and / or a mixture of a (meth)acrylic acid alkyl ester monomer and a carboxyl group-containing monomer, and further contains a monomer having an alkyleneoxy group and a hydroxyl group-containing (meth)acrylic acid ester monomer. In a moisture absorption test, a laminate made by attaching a pressure-sensitive adhesive layer (200 μm thick) laminated on a resin film to a glass plate is left in an environment of 60°C and 90% RH for 120 hours, and then left at room temperature (25°C) for 30 minutes, after which the haze value is measured to determine the transparency of the laminate. It is said that this pressure-sensitive adhesive composition maintains high transparency with little foaming even after being left at high temperature and high humidity. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2003-262729 A [Patent Document 2] JP 2008-248221 A [Patent Document 3] JP 2008-001739 A Summary of the Invention [Problem to be solved by the invention]

[0010] In recent years, the requirements for optical pressure sensitive adhesive films have been that they must maintain high transparency even when the pressure sensitive adhesive layer is applied thickly, and that they do not become cloudy when left in a high temperature and high humidity environment for an extended period of time and then taken out into a room temperature environment. However, even if high transparency can be achieved by applying a thick adhesive layer, it is often difficult to achieve anti-clouding performance at high temperatures and high humidity. In addition, attempts have been made to improve the anti-clouding performance by increasing the amount of hydroxyl group-containing monomers added, and although the anti-clouding performance has been improved, in exchange, there are many drawbacks such as the inability to maintain performance such as durability. There is a need for an adhesive that can overcome these drawbacks at the same time.

[0011] In other words, an object of the present invention is to provide an adhesive composition and an adhesive film that have anti-clouding properties and that do not become cloudy even when an adhesive film having a thick adhesive layer applied thereto is left in a high-temperature, high-humidity atmosphere for a long period of time. [Means for solving the problem]

[0012] In order to solve the above problems, the present invention provides a pressure-sensitive adhesive composition comprising at least one of a nitrogen-containing vinyl monomer not containing a hydroxyl group or an alkoxy group-containing alkyl (meth)acrylate monomer, and at least one copolymerizable vinyl monomer not containing a carboxyl group but containing a hydroxyl group as a functional group. The pressure-sensitive adhesive composition of the present invention preferably contains (A) 50 to 95 parts by weight of at least one of an alkyl (meth)acrylate monomer having an alkyl group with a carbon number of C1 to C14 or a phenoxy group-containing alkyl (meth)acrylate monomer, (B) 5 to 50 parts by weight of at least one of the nitrogen-containing vinyl monomer not containing a hydroxyl group or an alkoxy group-containing alkyl (meth)acrylate monomer, and (C) 0.5 to 10 parts by weight of at least one of the copolymerizable vinyl monomers having a hydroxyl group but not a carboxyl group in the functional group, and having a weight average molecular weight of 200,000 to 2,000,000, and (D) 0.01 to 5 parts by weight of a crosslinking agent, in a ratio such that the sum of (A) and (B) is 100 parts by weight. It is preferable that a pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition and having a coating thickness of 250 μm has a total light transmittance of 90% or more and a haze value of 1.0% or less. It is preferable that a pressure-sensitive adhesive layer having a coating thickness of 250 μm formed from the pressure-sensitive adhesive composition has a haze value of 4.0% or less when left for 240 hours in an atmosphere of 60° C. and 90% RH and then removed to a room temperature environment. The present invention also provides a pressure-sensitive adhesive film comprising a substrate and a pressure-sensitive adhesive layer formed of the pressure-sensitive adhesive composition laminated on one surface of the substrate. The present invention also provides a film for a touch panel, which uses the pressure-sensitive adhesive film. The present invention also provides a film for electronic paper, which uses the pressure-sensitive adhesive film. The present invention also provides a film for organic electroluminescence (EL) display, which uses the pressure-sensitive adhesive film. The present invention also provides an optical film with a pressure-sensitive adhesive, comprising an optical film and a pressure-sensitive adhesive layer made of the pressure-sensitive adhesive composition laminated on at least one surface of the optical film. Effect of the Invention

[0013] According to the present invention, when the pressure-sensitive adhesive layer is applied in a thick coating having a thickness of 250 μm or more, not only is the transparency excellent, but also the ability to prevent clouding under high temperature and high humidity conditions can be improved. [Brief description of the drawings]

[0014] [Figure 1] 1 is a graph showing the change in haze value immediately after removal from a high-temperature and high-humidity environment for Example 1 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present invention will be described below based on preferred embodiments. The pressure-sensitive adhesive composition of the present invention contains (B) at least one of a nitrogen-containing vinyl monomer or an alkoxy group-containing alkyl (meth)acrylate monomer, and (C) a copolymerizable vinyl monomer that does not contain a carboxyl group but does contain a hydroxyl group as a functional group.

[0016] The adhesive polymer used in the present invention is preferably an acrylic polymer, and in particular, a copolymer composition containing as a main component at least one kind of (A) alkyl (meth)acrylate monomer having an alkyl group with a carbon number of C1 to C14.

[0017] (A) Examples of alkyl (meth)acrylate monomers having an alkyl group with a carbon number of C1 to C14 include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, etc. The alkyl group of the alkyl (meth)acrylate monomer may be linear, branched, or cyclic. In place of a portion of the (A) alkyl (meth)acrylate monomer having an alkyl group with a carbon number of C1 to C14, a phenoxy group-containing alkyl (meth)acrylate monomer such as 2-phenoxyethyl (meth)acrylate can also be used in combination.

[0018] Among (B), examples of the nitrogen-containing vinyl monomer include cyclic nitrogen-containing vinyl compounds such as N-vinyl-2-pyrrolidone, N-vinylcaprolactam, and N-acryloylmorpholine; dialkyl-substituted (meth)acrylamides such as N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropylacrylamide, N,N-diisopropyl(meth)acrylamide, N,N-dibutyl(meth)acrylamide, N-ethyl-N-methyl(meth)acrylamide, N-methyl-N-propyl(meth)acrylamide, and N-methyl-N-isopropyl(meth)acrylamide; N,N-dimethylaminomethyl(meth)acrylate, N,N-dimethylaminoethyl(meth)acrylate, N,N-dimethylaminopropyl(meth)acrylate, N,N-dimethylaminoisopropyl(meth)acrylate, and N,N-dimethylaminobutyl(meth)acrylamide. dialkylamino(meth)acrylates such as N-ethyl-N-methylaminoethyl(meth)acrylate, N-methyl-N-propylaminoethyl(meth)acrylate, N-methyl-N-isopropylaminoethyl(meth)acrylate, and N,N-dibutylaminoethyl(meth)acrylate; and N,N-dialkyl-substituted aminopropyl(meth)acrylamides such as N,N-dimethylaminopropyl(meth)acrylamide, N,N-diethylaminopropyl(meth)acrylamide, N,N-dipropylaminopropyl(meth)acrylamide, N,N-diisopropylaminopropyl(meth)acrylamide, N-ethyl-N-methylaminopropyl(meth)acrylamide, N-methyl-N-propylaminopropyl(meth)acrylamide, and N-methyl-N-isopropylaminopropyl(meth)acrylamide. The nitrogen-containing vinyl monomer (B) is preferably one that does not contain a hydroxyl group, more preferably one that does not contain a hydroxyl group or a carboxyl group. As such a monomer, the above-mentioned monomers are preferable, for example, acrylic monomers containing N,N-dialkyl-substituted amino groups or N,N-dialkyl-substituted amide groups; N-vinyl-2-pyrrolidone, N-vinylcaprolactam, N-vinyl-2-piperidone, and other N-vinyl-substituted lactams; N-(meth)acryloylmorpholine, N-(meth)acryloylpyrrolidine, and other N-(meth)acryloyl-substituted cyclic amines.

[0019] Among (B), examples of the alkoxy group-containing alkyl (meth)acrylate monomer include 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-propoxyethyl (meth)acrylate, 2-isopropoxyethyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, 2-methoxypropyl (meth)acrylate, 2-ethoxypropyl (meth)acrylate, 2-propoxypropyl (meth)acrylate, 2-isopropoxypropyl (meth)acrylate, 2-butoxypropyl (meth)acrylate, Propyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 3-ethoxypropyl (meth)acrylate, 3-propoxypropyl (meth)acrylate, 3-isopropoxypropyl (meth)acrylate, 3-butoxypropyl (meth)acrylate, 4-methoxybutyl (meth)acrylate, 4-ethoxybutyl (meth)acrylate, 4-propoxybutyl (meth)acrylate, 4-isopropoxybutyl (meth)acrylate, 4-butoxybutyl (meth)acrylate, and the like. These alkoxy group-containing alkyl(meth)acrylate monomers have a structure in which an atom of an alkyl group in an alkyl(meth)acrylate is substituted with an alkoxy group.

[0020] (C) Examples of copolymerizable vinyl monomers having a hydroxyl group but not a carboxyl group in the functional group include hydroxyl group-containing (meth)acrylic acid esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 8-hydroxyoctyl (meth)acrylate, and hydroxyl group-containing (meth)acrylamides such as N-hydroxy(meth)acrylamide, N-hydroxymethyl (meth)acrylamide, and N-hydroxyethyl (meth)acrylamide. At least one selected from these compound groups is preferable. Although the hydroxyl group-containing (meth)acrylamides contain nitrogen, in the present invention they belong to group (C) rather than group (B).

[0021] Examples of copolymerizable vinyl monomers other than those mentioned above include copolymerizable vinyl monomers containing a carboxyl group, such as (meth)acrylic acid, itaconic acid, crotonic acid, maleic acid, fumaric acid, carboxyethyl (meth)acrylate, and carboxypentyl (meth)acrylate; aromatic group-containing (meth)acrylic acid esters, such as benzyl (meth)acrylate; and various vinyl monomers, such as styrene, acrylamide, acrylonitrile, methyl vinyl ether, ethyl vinyl ether, vinyl acetate, and vinyl chloride.

[0022] The above monomers (A), (B) and (C) constitute an adhesive polymer as an acrylic copolymer, which is the main component of the adhesive. The polymerization method for the copolymer is not particularly limited, and any appropriate polymerization method such as solution polymerization, bulk polymerization, suspension polymerization, emulsion polymerization, etc. can be used. The average molecular weight of the adhesive polymer is not particularly limited, but may be, for example, within a weight average molecular weight range of 200,000 to 2,000,000.

[0023] The adhesive polymer used in the present invention is preferably a copolymer consisting of (A) 50-95 parts by weight of at least one of an alkyl (meth)acrylate monomer having an alkyl group with carbon number of C1-C14 or an alkyl (meth)acrylate monomer containing a phenoxy group, (B) 5-50 parts by weight of at least one of a nitrogen-containing vinyl monomer not containing a hydroxyl group or an alkyl (meth)acrylate monomer containing an alkoxy group, and (C) 0.5-10 parts by weight of at least one of a copolymerizable vinyl monomer containing a hydroxyl group but not a carboxyl group in the functional group. Here, the parts by weight of (A) to (C) are specified so that the sum of (A) and (B) is 100 parts by weight.

[0024] In the pressure-sensitive adhesive composition of the present invention, it is preferable to crosslink the pressure-sensitive adhesive polymer when forming the pressure-sensitive adhesive layer. To achieve crosslinking, the pressure-sensitive adhesive composition may contain a known crosslinking agent, or may be crosslinked by photocrosslinking such as ultraviolet (UV) light. Examples of the crosslinking agent include difunctional or higher isocyanate compounds, difunctional or higher epoxy compounds, difunctional or higher acrylate compounds, and metal chelate compounds. The content of the crosslinking agent is not particularly limited, but may be 0.01 to 5 parts by weight.

[0025] As the (D) crosslinking agent, one that can crosslink the acrylic copolymer by reacting with the hydroxyl group contained in the (C) monomer is preferred. Examples of such crosslinking agents include biuret modified or isocyanurate modified diisocyanates (compounds having two NCO groups in one molecule) such as hexamethylene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, tolylene diisocyanate, and xylylene diisocyanate, and polyisocyanate compounds such as adducts (polyol modified) with trivalent or higher polyols (compounds having at least three or more OH groups in one molecule) such as trimethylolpropane and glycerin. Crosslinking may also be performed by photocrosslinking such as ultraviolet light (UV). The copolymer used in the present invention contains the hydroxyl group-containing vinyl monomer (C) as a functional group monomer that reacts with a crosslinking agent, and therefore may not contain a carboxyl group-containing vinyl monomer.

[0026] The pressure-sensitive adhesive composition of the present invention preferably contains (A) 50 to 95 parts by weight of at least one of an alkyl (meth)acrylate monomer having an alkyl group with a carbon number of C1 to C14 or a phenoxy group-containing alkyl (meth)acrylate monomer, (B) 5 to 50 parts by weight of at least one of a nitrogen-containing vinyl monomer not containing a hydroxyl group or an alkoxy group-containing alkyl (meth)acrylate monomer, and (C) 0.5 to 10 parts by weight of at least one copolymerizable vinyl monomer which does not contain a carboxyl group in its functional group and contains a hydroxyl group, and has a weight average molecular weight of 200,000 to 2,000,000, and (D) 0.01 to 5 parts by weight of a crosslinking agent, in a ratio such that the sum of (A) and (B) is 100 parts by weight.

[0027] The pressure-sensitive adhesive composition of the present invention may further contain, as other components, known additives such as silane coupling agents, antioxidants, surfactants, curing accelerators, plasticizers, fillers, curing retarders, processing aids, and antioxidants. These may be used alone or in combination of two or more.

[0028] According to the pressure-sensitive adhesive composition of the present invention, when the pressure-sensitive adhesive layer is thickly coated, it is possible to improve the anti-clouding performance at high temperature and high humidity as well as to obtain excellent transparency. It is preferable that the pressure-sensitive adhesive layer having a coating thickness of 250 μm formed from the pressure-sensitive adhesive composition has a total light transmittance of 90% or more and a haze value of 1.0% or less. It is also preferable that the pressure-sensitive adhesive layer having a coating thickness of 250 μm formed from the pressure-sensitive adhesive composition has a haze value of 4.0% or less when it is left in an atmosphere of 60° C. and 90% RH for 240 hours and then taken out into a room temperature environment.

[0029] The adhesive film of the present invention is obtained by laminating an adhesive layer made of the adhesive composition of the present invention on one side of a substrate film. The adhesive film of the present invention can be used for various applications such as touch panels, electronic paper, organic EL, optical members, and surface protection. The thickness of the adhesive layer is not particularly limited, but is, for example, 100 to 2000 μm. If the adhesive layer is too thin, the impact absorption performance is deteriorated, but if the adhesive layer is too thick, it is disadvantageous in that the cost increases. In particular, it is preferable that the adhesive layer is thick-coated to a thickness of 250 μm or more, since the effect of the present invention is high.

[0030] As the base film of the pressure-sensitive adhesive layer and the release film (separator) that protects the pressure-sensitive adhesive surface, a resin film such as a polyester film can be used. The substrate film may be subjected to an antifouling treatment using a silicone-based or fluorine-based release agent or coating agent, or silica microparticles or the like, or an antistatic treatment by coating or kneading an antistatic agent, on the side opposite to the side on which the pressure-sensitive adhesive layer of the resin film is formed. The release film is subjected to a release treatment with a silicone-based or fluorine-based release agent on the surface thereof that is to be joined to the adhesive surface of the adhesive layer. In the case of an optical surface protection film such as a surface protection film for a polarizing plate, the base film and the pressure-sensitive adhesive layer preferably have sufficient transparency. In addition, the adhesive layer may be used for a laminated film in which various films are laminated with each other via the adhesive layer, such as a film for a touch panel, a film for electronic paper, a film for an organic electroluminescence (EL) display, or an optical film.

[0031] The pressure-sensitive adhesive composition of the present invention can also be used for a pressure-sensitive adhesive-attached optical film in which a pressure-sensitive adhesive layer is laminated on at least one surface of an optical film. In the pressure-sensitive adhesive optical film, an optical film such as a polarizing plate film, a retardation plate film, a lens film, a polarizing plate film also serving as a retardation plate, or a polarizing plate film also serving as a lens film can be used as the base film. The optical film with adhesive is formed by laminating an adhesive layer on one or both sides of an optical film, and can be used for bonding to a glass plate or the like of an image display device. These optical films with adhesive can be bonded to a glass substrate or the like via the adhesive layer, and incorporated into an image display device or the like. The adhesive layer used in the optical film with adhesive, such as an adhesive polarizing plate, preferably has sufficient transparency. Moreover, the polarizing plate used as the substrate film generally has a three-layer structure in which a polyvinyl alcohol-based polarizer is sandwiched between triacetyl cellulose-based protective films on both sides. The polarizing plate has a structure in which a discotic liquid crystal is coated on the surface of a protective film, or a stretched triacetyl cellulose film, a stretched polycycloolefin film, a stretched cellulose acetate propionate film, or the like is laminated instead of a triacetyl cellulose film. Furthermore, these polarizing plate films are laminated to a glass substrate, which is a surface base material of a liquid crystal display panel, via an adhesive layer. EXAMPLES

[0032] The present invention will be specifically described below with reference to examples.

[0033] <Production of Acrylic Copolymer> [Example 1] Nitrogen gas was introduced into a reactor equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen inlet tube, and the air in the reactor was replaced with nitrogen gas. Then, 95 parts by weight of 2-ethylhexyl acrylate, 5 parts by weight of N-vinyl-2-pyrrolidone, 1.0 parts by weight of 6-hydroxyhexyl acrylate, and 100 parts of a solvent (ethyl acetate) were added to the reactor. Then, 0.1 parts by weight of azobisisobutyronitrile was dropped as a polymerization initiator over 2 hours, and the mixture was reacted at 65°C for 8 hours to obtain an acrylic copolymer solution 1 of Example 1 having a weight average molecular weight of 800,000. [Examples 2 to 7 and Comparative Examples 1 to 2] Acrylic copolymer solutions used in Examples 2 to 7 and Comparative Examples 1 and 2 were obtained in the same manner as in the acrylic copolymer solution 1 used in Example 1 above, except that the monomer compositions were as shown in Table 1.

[0034] <Production of Pressure-Sensitive Adhesive Composition and Pressure-Sensitive Adhesive Film> [Example 1] 0.5 parts by weight of Coronate HX (an isocyanurate of a hexamethylene diisocyanate compound) was added to the acrylic copolymer solution 1 (100 parts by weight of group (A) + group (B)) produced as described above, and the mixture was stirred and mixed to obtain an adhesive composition of Example 1. This adhesive composition was applied onto a release film made of a silicone resin-coated polyethylene terephthalate (PET) film, and then dried at 90°C to remove the solvent, thereby obtaining an adhesive film with an adhesive layer thickness of 250 μm. Thereafter, the adhesive sheet was transferred onto a polyethylene terephthalate (PET) film to obtain the adhesive film of Example 1 having a laminated structure of "PET film / adhesive layer / release film (silicone resin-coated PET film)". [Examples 2 to 7 and Comparative Examples 1 to 2] Pressure-sensitive adhesive films of Examples 2 to 7 and Comparative Examples 1 and 2 were obtained in the same manner as for the surface protection film of Example 1 above, except that the composition of the crosslinking agent was as shown in Table 1 (D).

[0035] In Table 1, the blending ratio of each component is shown in parentheses in parts by weight, calculated with the total of group (A) + group (B) being 100 parts by weight. Mw in Table 1 means weight average molecular weight. Table 2 shows the compound names of the abbreviations of each component used in Table 1. In addition, in group (D) of Table 2, HDI means hexamethylene diisocyanate, and XDI means xylylene diisocyanate. Coronate (registered trademark) HX, Coronate (registered trademark) HL, and Coronate (registered trademark) L-45 are trade names of Nippon Polyurethane Industry Co., Ltd., Duranate (registered trademark) 24A-100 is a trade name of Asahi Kasei Chemicals Corporation, and Takenate (registered trademark) D-110N is a trade name of Mitsui Chemicals, Inc.

[0036] [Table 1]

[0037] [Table 2]

[0038] <Test methods and evaluation> The adhesive films of Examples 1 to 7 and Comparative Examples 1 and 2 were aged for 7 days under an atmosphere of 23°C and 50% RH, and then the release film (a silicone resin-coated PET film) was peeled off to expose the adhesive layer, which was used as a sample for measuring total light transmittance. In addition, the adhesive films of Examples 1 to 7 and Comparative Examples 1 and 2 were aged for 7 days under an atmosphere of 23°C and 50% RH, and then the films with both sides of the adhesive layer still covered with release films (silicone resin-coated PET films) were used as samples for measuring the haze value. In addition, the adhesive films of Examples 1 to 7 and Comparative Examples 1 and 2 were aged for 7 days in an atmosphere of 23°C and 50% RH, and then left in an oven in an atmosphere of 60°C and 90% RH for 240 hours, and then removed from the oven to a room temperature environment (23°C, 50% RH). The adhesive films, with both sides of the adhesive layer still covered with release films (PET films coated with silicone resin), were used as samples for measuring the haze value after wet heat. In addition, the adhesive film with the adhesive layer exposed was attached to the surface of a non-alkali glass plate via the adhesive layer, and after leaving it for one day, it was autoclaved at 50°C and 5 atmospheres for 20 minutes and then left at room temperature for a further 12 hours to prepare a sample for measuring adhesive strength. Furthermore, the pressure-sensitive adhesive film with the pressure-sensitive adhesive layer exposed was attached to the surface of a non-alkali glass plate via the pressure-sensitive adhesive layer to prepare a sample for measuring durability.

[0039] <Total light transmittance> For the sample for measuring the total light transmittance obtained above, the total light transmittance of the pressure-sensitive adhesive layer was measured in accordance with JISK7105 using a haze meter (manufacturer: Nippon Denshoku Co., Ltd., model: Haze Meter, NDH2000).

[0040] <Haze value and haze value after wet heat treatment> For the samples for measuring the haze value and the haze value after wet heat obtained above, the haze value of the pressure-sensitive adhesive layer was measured using a haze meter (manufacturer: Nippon Denshoku Co., Ltd., model: Haze Meter, NDH2000). In the above measurement samples, the adhesive layer was covered on both sides with a release film (a silicone resin-coated PET film) and the haze value and the haze value after wet heat were measured. It was confirmed that the haze value of the release film itself was negligibly small.

[0041] <Adhesive strength to glass plate> The adhesive strength measurement sample obtained above (a 25 mm wide adhesive film attached to the surface of an alkali-free glass plate) was peeled off in a 180° direction at a tensile speed of 0.3 m / min using a tensile tester, and the measured peel strength was taken as the adhesive strength.

[0042] <Durability> The durability measurement samples obtained above were left in an atmosphere of 80℃ (dry) for 250 hours, then removed to room temperature and visually inspected for peeling from the adherend, foaming, etc. The evaluation criteria were "○" when no peeling or foaming was observed, "△" when slight peeling or foaming was observed, and "×" when peeling or foaming was clearly observed.

[0043] Table 3 shows the measurement and evaluation results.

[0044] [Table 3]

[0045] The pressure-sensitive adhesive films of Examples 1 to 7 not only had transparency (total light transmittance of 90% or more, haze value of 1.0% or less) when the pressure-sensitive adhesive layer was applied thickly (250 μm), but also had anti-clouding performance with little clouding even when left in a high-temperature, high-humidity atmosphere for a long period of time (haze value of 4.0% or less after leaving at 60° C., 90% RH for 240 hours), and were able to improve the anti-clouding performance. Furthermore, there was no peeling or foaming even when left in a high-temperature atmosphere for a long period of time. The adhesive films of Comparative Examples 1 and 2 showed an increase in haze value when left in a high-temperature, high-humidity atmosphere for a long period of time, and showed problems with the anti-clouding performance. In addition, peeling and foaming were observed when left in a high-temperature atmosphere for a long period of time, and showed problems with durability. Furthermore, in Comparative Example 1, the measurement results of transparency (total light transmittance, haze value) were poor even before being left in a high-temperature, high-humidity atmosphere.

[0046] <Change in haze value after removal from high temperature and high humidity environment> In addition, the pressure-sensitive adhesive films of Example 1 and Comparative Example 1 were aged for 7 days in an atmosphere of 23°C and 50% RH, and then left in an oven in an atmosphere of 60°C and 90% RH for 240 hours, and then taken out of the oven to a room temperature environment (23°C, 50% RH), and the haze value was measured from immediately after taking out until 60 minutes had elapsed. The obtained change in haze value after taking out from the high temperature and high humidity environment is shown in FIG. 1, it can be seen that in Example 1 according to the present invention, the haze value reaches a maximum value (3.5%) about one minute after removal from the oven, but the haze value does not exceed 4.0% even one hour after removal from the oven, demonstrating excellent anti-clouding performance. On the other hand, in Comparative Example 1, the haze value increases to a maximum value of about 25% within a few minutes after removal from the oven, and then tends to gradually decrease as the time passes, but the significant clouding state continues for more than 60 minutes. In both Example 1 and Comparative Example 1, the above-mentioned cloudiness that occurred in a high temperature and high humidity environment gradually disappeared when left at room temperature for several hours, and the adhesive film eventually became transparent (haze value of 1.0% or less). This evaluation is the change that occurs when both sides of the adhesive layer are covered between release films, and the time it takes for the cloudiness to disappear is relatively short. However, in the case of samples bonded to glass plates with poor gas permeability or acrylic plates and glass, the timing at which the cloudiness appears is the same, but it may take several days for the cloudiness to disappear.

Claims

1. A pressure-sensitive adhesive composition comprising an acrylic polymer and a crosslinking agent, The acrylic polymer is a total of 50 to 95 parts by weight of at least one alkyl (meth)acrylate monomer having an alkyl group with a carbon number of C1 to C14 and at least one phenoxy group-containing alkyl (meth)acrylate monomer; 5 to 50 parts by weight of at least one of a nitrogen-containing vinyl monomer not containing a hydroxyl group or a carboxyl group, or an alkoxy group-containing alkyl (meth)acrylate monomer, 0.5 to 10 parts by weight of at least one hydroxyl group-containing (meth)acrylic acid ester, which is a copolymerizable vinyl monomer that does not contain a carboxyl group but contains a hydroxyl group as a functional group; A copolymer having a weight average molecular weight of 200,000 to 2,000,000, The alkoxy group-containing alkyl (meth)acrylate monomer is 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-propoxyethyl (meth)acrylate, 2-isopropoxyethyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, 2-methoxypropyl (meth)acrylate, 2-ethoxypropyl (meth)acrylate, 2-propoxypropyl (meth)acrylate, 2-isopropoxypropyl (meth)acrylate, 2-butoxypropyl (meth)acrylate. at least one selected from the group consisting of butyl acrylate, 3-methoxypropyl (meth)acrylate, 3-ethoxypropyl (meth)acrylate, 3-propoxypropyl (meth)acrylate, 3-isopropoxypropyl (meth)acrylate, 3-butoxypropyl (meth)acrylate, 4-methoxybutyl (meth)acrylate, 4-ethoxybutyl (meth)acrylate, 4-propoxybutyl (meth)acrylate, 4-isopropoxybutyl (meth)acrylate, and 4-butoxybutyl (meth)acrylate; the total of at least one alkyl (meth)acrylate monomer having an alkyl group with a carbon number of C1 to C14 and at least one phenoxy group-containing alkyl (meth)acrylate monomer is 50 to 95 parts by weight, and the total of at least one nitrogen-containing vinyl monomer or alkoxy group-containing alkyl (meth)acrylate monomer not containing a hydroxyl group or a carboxyl group is 5 to 50 parts by weight, so that the total of the at least one alkyl (meth)acrylate monomer is 100 parts by weight; the pressure-sensitive adhesive composition comprises 50 to 95 parts by weight of the total of at least one alkyl (meth)acrylate monomer having a carbon number of C1 to C14 in the alkyl group and at least one phenoxy group-containing alkyl (meth)acrylate monomer, and 5 to 50 parts by weight of the at least one nitrogen-containing vinyl monomer or alkoxy group-containing alkyl (meth)acrylate monomer not containing a hydroxyl group or a carboxyl group, and the crosslinking agent is contained in an amount of 0.01 to 5 parts by weight per 100 parts by weight of the total of at least one alkyl (meth)acrylate monomer having a carbon number of C1 to C14 in the alkyl group and at least one phenoxy group-containing alkyl (meth)acrylate monomer; a pressure-sensitive adhesive layer having a coating thickness of 250 μm formed from the pressure-sensitive adhesive composition has a total light transmittance of 90% or more and a haze value of 1.0% or less; A pressure-sensitive adhesive composition, characterized in that a pressure-sensitive adhesive layer having a coating thickness of 250 μm formed from the pressure-sensitive adhesive composition has a haze value of 4.0% or less when left for 240 hours in an atmosphere of 60° C. and 90% RH and then removed to a room temperature environment.

2. 13. A pressure-sensitive adhesive film comprising a substrate and a pressure-sensitive adhesive layer comprising the pressure-sensitive adhesive composition according to claim 1 laminated on one surface of the substrate.

3. A film for a touch panel, comprising the adhesive film according to claim 2 .

4. A film for electronic paper, comprising the adhesive film according to claim 2 .

5. A film for organic electroluminescence (EL), comprising the pressure-sensitive adhesive film according to claim 2 .

Citation Information

Patent Citations

  • Moisture-resistant adhesive sheet and its use

    JP2001123136A

  • Adhesive optical film and image display device

    JP2003262729A

  • Pressure-sensitive adhesive optical film, pressure- sensitive adhesive composition for optical film and image display device

    JP2003329838A

  • Adhesive composition for optical film and adhesive sheet, and optical member using the same

    JP2007138057A

  • Adhesive composition for electronic display, adhesive layer for electronic display and adhesive filter for electronic display