Resin composition for moldings coated with water-based paint and moldings thereof
A resin composition with a specific ratio of thermoplastic resin and natural fillers like eggshell powder and used tea leaves enhances paintability with water-based paints, addressing environmental sustainability in molded products.
Patent Information
- Application Number
- JP2023517067
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-04-27
- Filing Date
- 2022-02-09
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2042-02-09
AI Technical Summary
Existing resin compositions for molded products face challenges in achieving good paintability with water-based paints while reducing the use of fossil resource-derived materials, which is necessary for environmental sustainability.
A resin composition combining a thermoplastic resin with a specific mass ratio of biomineral-derived inorganic and plant-derived organic fillers, such as eggshell powder and used tea leaves or coffee grounds, enhances wettability and paintability with water-based paints.
The composition improves wettability and paintability with water-based paints, reducing the use of fossil resource-derived materials and minimizing environmental impact.
Smart Images

Figure 0007583920000001 
Figure 0007583920000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition for a molded article to be coated with a water-based paint, and to a molded article made thereof. [Background technology]
[0002] Conventionally, resin products used in home appliances, automobile interior materials, toys, etc. are molded by injection molding or the like. Among these products, those for which the surface appearance is important may have their surfaces painted. In addition, there are also known resin toys and the like that allow consumers to paint them as they like (for example, Patent Document 1, etc.).
[0003] Incidentally, in recent years, environmental issues such as global warming have come to be emphasized, and there is a demand for reducing the amount of resin materials derived from fossil resources such as petroleum. In response to such demands, for example, studies are being conducted on blending biomass raw materials with thermoplastic resins to reduce the amount of resin materials used. Meanwhile, in the field of painting, there is an increasing demand for water-based paints that have a low environmental impact (Patent Document 2, etc.). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Publication No. 106646 / 1983 [Patent Document 2] JP 2016-188338 A Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention has been made in consideration of the above circumstances, and has an object to provide a resin composition that contains a small amount of resin material derived from fossil resources and can provide a molded article that has good paintability with water-based paints, and a molded article made from the resin composition. [Means for solving the problem]
[0006] In order to solve the above problems, the inventors of the present application conducted extensive research and found that a molded article obtained from a resin composition in which a filler derived from a natural material and a thermoplastic resin are combined in a specific mass ratio has improved wettability with water and good paintability with water-based paints. They also found that such a resin composition can reduce the amount of thermoplastic resin derived from fossil resources, and can provide a molded article with less environmental impact, leading to the completion of the present invention. That is, the present invention has the following aspects. [1] A resin composition for use in molded products to be coated with an aqueous paint, comprising a thermoplastic resin (A) and a filler (B) derived from natural materials in a mass ratio ((A) / (B)) of 50 / 50 to 30 / 70, wherein the filler (B) comprises at least one selected from an inorganic filler (B1) derived from biominerals and an organic filler (B2) derived from plants. [2] A resin composition for molded products to be coated with the aqueous paint according to [1], wherein the thermoplastic resin (A) comprises a polystyrene-based resin (A1), and the filler (B) comprises the inorganic filler (B1) or the organic filler (B2). [3] A resin composition for molded products to be coated with the aqueous paint according to [1], wherein the thermoplastic resin (A) comprises a polyolefin resin (A2), and the filler (B) comprises the organic filler (B2). [4] The resin composition for molded products to be coated with the aqueous paint according to [1] or [2], wherein the inorganic filler (B1) comprises at least one selected from eggshell powder and seashell powder. [5] A resin composition for moldings that is coated with the aqueous paint according to any one of [1] to [3], wherein the organic filler (B2) comprises ground wood. [6] A resin composition for moldings to be painted with the water-based paint according to [5], wherein the ground wood material comprises at least one ground wood material selected from tree leaves, stems, buds, and seeds. [7] A resin composition for moldings that is coated with the aqueous paint according to any one of [1] to [6], wherein the filler (B) is a filler derived from food waste. [8] The resin composition for molded products to be coated with the water-based paint according to [7], wherein the organic filler (B2) comprises at least one selected from the group consisting of used tea leaves and coffee grounds. [9] A molded article comprising the resin composition for molded articles that is coated with the water-based paint according to any one of [1] to [8]. Effect of the Invention
[0007] According to the present invention, it is possible to provide a resin composition which contains a small amount of resin material derived from fossil resources and which can provide a molded article having good paintability with water-based paints, and a molded article made from the resin composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The present invention will be described in detail below, but the present invention is not limited to the following embodiments. In this specification, the symbol "~" means "at least one or less than one." In other words, "3 to 50" means "at least one or more than 3 and at most 50." [Resin composition for moldings to be painted with water-based paint] The resin composition for molded products to be coated with the water-based paint according to the present invention contains a thermoplastic resin (A) and a filler (B) derived from natural materials in a mass ratio ((A) / (B)) of 50 / 50 to 30 / 70, and the filler (B) contains at least one selected from an inorganic filler (B1) derived from biominerals and an organic filler (B2) derived from plants. The resin composition for molded products to be coated with the water-based paint according to the present invention (hereinafter, sometimes referred to as "resin composition") has improved wettability with water, and can provide molded products having good coatability with water-based paint. In addition, the proportion of the thermoplastic resin (A) in the resin composition can be reduced, which reduces the burden on the environment.
[0009] The mass ratio ((A) / (B)) of the thermoplastic resin (A) to the filler (B) derived from a natural material (hereinafter referred to as "filler (B)") in the resin composition is 50 / 50 to 30 / 70, preferably 45 / 55 to 30 / 70, and more preferably 40 / 60 to 30 / 70. When the mass ratio ((A) / (B)) is 50 / 50 to 30 / 70, the wettability with water is improved, and a molded article having good paintability with water-based paint can be provided. The mass ratio ((A) / (B)) means the ratio when the total amount of the thermoplastic resin (A) and the filler (B) is 100. In other words, when the combined amount of thermoplastic resin (A) and filler (B) relative to the total amount of the resin composition is 80 mass%, "the mass ratio of thermoplastic resin (A) to filler (B) ((A) / (B)) is 50 / 50" means that the proportion of thermoplastic resin (A) in the resin composition is 40 mass%, and the proportion of filler (B) in the resin composition is 40 mass%.
[0010] In this specification, the "wettability to water" may be evaluated by the contact angle of the resin composition to water measured by the θ / 2 method. Specifically, the resin composition is press-molded in a pressure molding machine (Shoji Co., Ltd., 50t heating molding machine) at a heating temperature of 200°C, a pressure of 5 MPa, a preheating time of 3 minutes, and a pressurizing time of 3 minutes to obtain a molded product of 150 mm x 150 mm x thickness of 1.0 mm. The contact angle of the molded product surface to water is measured at 25°C using a contact angle measuring device (Kyowa Interface Science Co., Ltd., product name "Automatic Contact Angle Meter DM-500"), and the wettability to water is evaluated based on the value of the contact angle obtained. In this specification, "improved wettability to water" means that the contact angle θ2 of the molded product surface obtained from the resin composition according to the present invention, measured by the θ / 2 method, is smaller than the contact angle θ1 of the molded product surface obtained from only the thermoplastic resin (A). In other words, the relationship is θ1>θ2.
[0011] In one embodiment of the resin composition for molded products to be coated with the aqueous paint according to the present invention, the composition contains a thermoplastic resin (A) and a filler (B) derived from natural materials in a mass ratio ((A) / (B)) of 50 / 50 to 30 / 70, and the filler (B) contains at least one selected from an inorganic filler (B1) derived from biominerals and an organic filler (B2) derived from plants, and the contact angle at 25°C measured by the θ / 2 method is preferably 90° or less. It is more preferable that the aforementioned θ1 and θ2 satisfy the following conditions (1) and (2). θ1-θ2≧3° (1) θ2≦90° (2) If θ2 is 90° or less and θ1 is at least 3° larger than θ2, the wettability with water becomes better, and the coatability with a water-based paint tends to improve. The thermoplastic resin (A) preferably contains a polystyrene-based resin (A1) or a polyolefin-based resin (A2) described below. The inorganic filler (B1) derived from biominerals preferably contains eggshell powder described below. The organic filler (B2) derived from plants preferably contains used tea leaves or coffee grounds described below.
[0012] The proportion of the filler (B) in the resin composition is preferably more than 20% by mass, more preferably 30% by mass or more, and even more preferably 40% by mass or more, based on the total mass of the resin composition. If the proportion of the filler (B) in the resin composition is more than 20% by mass, the above θ2 is likely to be 90° or less, and the wettability of the resulting molded product to water is likely to be improved. In addition, from the viewpoint of reducing the blending amount of the thermoplastic resin (A) in the resin composition to obtain a resin composition with less environmental load, the proportion of the filler (B) in the resin composition may be 50% by mass or more. In addition, from the viewpoint of the moldability of the resin composition, the upper limit of the filler (B) is preferably less than 80% by mass, and more preferably 70% by mass or less. That is, the proportion of the filler (B) in the resin composition can be adjusted in the range of more than 20% by mass and less than 80% by mass. From the viewpoint of the moldability and the wettability to water being more likely to be improved, the proportion of the filler (B) is particularly preferably 50 to 70% by mass, based on the total mass of the resin composition.
[0013] The proportion of the thermoplastic resin (A) in the resin composition is preferably more than 20% by mass from the viewpoint of molding processability. From the viewpoint of obtaining a molded product with better coatability with water-based paints and from the viewpoint of further reducing the amount of resin material derived from fossil resources, the proportion of the thermoplastic resin (A) in the resin composition is preferably in the range of 30 to 50% by mass based on the total mass of the resin composition.
[0014] <Thermoplastic resin (A)> The resin composition according to the present invention contains a thermoplastic resin (A). Examples of the thermoplastic resin (A) include polystyrene-based resins, polyolefin-based resins, polyester-based resins, and polycarbonate-based resins.
[0015] (Polystyrene resin (A1)) The polystyrene resin according to the present invention is a polymer containing a monomer unit derived from an aromatic vinyl compound, and examples thereof include polystyrene (GPPS, homopolymer of styrene), high impact polystyrene (HIPS), copolymers of aromatic vinyl compounds and conjugated dienes or hydrogenated products thereof, graft copolymers of aromatic compounds and ethylene, copolymers of compounds copolymerizable with aromatic vinyl compounds and aromatic vinyl compounds, and other polymers containing 50 mol% or more of monomer units derived from aromatic compounds in the molecular chain. These may be used alone or in combination of two or more. That is, the polystyrene resin (A1) may be a mixture.
[0016] Examples of aromatic vinyl compounds include styrene, α-methylstyrene, p-methylstyrene, o-methylstyrene, m-methylstyrene, ethylstyrene, and pt-butylstyrene. These aromatic vinyl compounds may be used alone or in combination of two or more. Among these, it is preferable to use styrene.
[0017] Examples of compounds copolymerizable with aromatic vinyl compounds include methacrylic acid esters such as methyl methacrylate and ethyl methacrylate, unsaturated nitrile compounds such as acrylonitrile and methacrylonitrile, acid anhydrides such as maleic anhydride, etc. Examples of copolymers of these compounds with aromatic vinyl compounds include acrylonitrile-butadiene-styrene copolymer (ABS), methyl methacrylate-butadiene-styrene copolymer (MBS), acrylonitrile-styrene copolymer (AS), etc.
[0018] Examples of copolymers of aromatic compounds and conjugated dienes include block copolymers such as styrene-butadiene (SB), styrene-isoprene (SI), styrene-butadiene-butylene (SBB), styrene-butadiene-isoprene (SBI), styrene-butadiene-styrene (SBS), styrene-butadiene-butylene-styrene (SBBS), styrene-isoprene-styrene (SIS), and styrene-butadiene-isoprene-styrene (SBIS), as well as hydrogenated block copolymers thereof. These may be used alone or in combination of two or more.
[0019] Among the above, the polystyrene resin (A1) is preferably GPPS, ABS, AS, or MBS, more preferably GPPS or ABS, from the viewpoint of high versatility. The polystyrene resin preferably has an MFR (200° C., 5 kg load) value measured according to the JIS K 7260 standard of 1 to 50 g / 10 min, more preferably 3 to 30 g / 10 min.
[0020] (Polyolefin resin (A2)) Examples of polyolefin resins include homopolymers of aliphatic olefin compounds such as high density polyethylene, low density polyethylene, linear low density polyethylene, polypropylene resins, and poly-1-butene, and copolymers thereof. Examples of copolymers include ethylene-propylene copolymers, ethylene-1-butene copolymers, and ethylene-methylpentene copolymers. The polypropylene resins include polypropylene homopolymers and polyolefin copolymers containing 50 mol% or more of propylene monomer units. The polyolefin resins may be used alone or in combination of two or more. Among these, from the viewpoint of high versatility, polypropylene, high density polyethylene, and low density polyethylene are preferred as the polyolefin resin (A2), and polypropylene is more preferred.
[0021] (Polyester resin) Examples of polyester resins include resins obtained by copolymerizing a diol component such as diethylene glycol, neopentyl glycol, or polyalkylene glycol with a dicarboxylic acid component such as adipic acid, sebacic acid, phthalic acid, isophthalic acid, or 2,6-naphthalenedicarboxylic acid. Specific examples include polyethylene terephthalate, polybutylene terephthalate, polyethylene-2,6-naphthalate, and polymethylene terephthalate. These may be used alone or in combination of two or more.
[0022] (Polycarbonate resin) Polycarbonate resins are resins in which the bonds between monomers are mainly carried out by carbonate groups. Examples of polycarbonate resins include those obtained by reacting one or more bisphenols with phosgene or carbonic acid diesters, or those obtained by reacting one or more bisphenols with diphenyl carbonates by transesterification. Examples of the bisphenols include bis-(4-hydroxyphenyl)-alkanes such as bisphenol A, bis-(4-hydroxyphenyl)-cycloalkanes, bis-(4-hydroxyphenyl)-sulfides, bis-(4-hydroxyphenyl)-ethers, bis-(4-hydroxyphenyl)-ketones, bis-(4-hydroxyphenyl)-sulfones, and bisphenol fluorene. In addition, for the purpose of improving processing characteristics, a copolymer obtained by copolymerizing a compound such as hydroquinone or 4,4-dihydroxybiphenyl as a dihydric phenol other than bisphenols may be used. The polycarbonate resins may be used alone or in combination of two or more kinds.
[0023] In the resin composition according to the present invention, the thermoplastic resin (A) preferably contains a polystyrene-based resin (A1) or a polyolefin-based resin (A2) from the viewpoint of easily improving moldability, and more preferably contains polystyrene (GPPS) or polypropylene.
[0024] <Filling material derived from natural materials (B)> The resin composition according to the present invention contains a filler (B). In this specification, "derived from natural materials" means derived from materials or ingredients other than fossil resources. The filler (B) according to the present invention contains at least one selected from an inorganic filler (B1) derived from biominerals and an organic filler (B2) derived from plants.
[0025] (Inorganic filler derived from biominerals (B1)) The filler (B) according to the present invention includes an inorganic filler (B1) derived from a biomineral (hereinafter referred to as "inorganic filler (B1)"). "Biominerals" refer to minerals produced by living organisms, and examples thereof include pearls, shells, eggshells, bones, and exoskeletons of crustaceans. As the inorganic filler (B1) according to the present invention, animal bones, eggshells, and the like processed into particles or powder can be used. The type of animal is not particularly limited as long as it has the effect of the present invention. Specific examples of the inorganic filler (B1) include bone powder of livestock such as chickens, cows, pigs, and sheep, eggshell powder of poultry, bone powder of fish and shellfish, and shellfish powder (shell powder). These may be used alone or in combination of two or more. Among these, from the viewpoint of ease of availability and ease of pulverization, the inorganic filler (B1) preferably includes at least one powder selected from eggshell powder and shell powder, and more preferably includes eggshell powder. In addition, from the viewpoint of further reducing the burden on the environment, the eggshell powder and shell powder are preferably powders derived from food waste. In this specification, "derived from food waste" may refer to materials derived from food waste such as unsold or leftover food generated during the distribution or consumption of food, in addition to processing residues generated during the production or cooking of food.
[0026] The eggshell powder is preferably made from chicken eggshells. More than 200,000 tons of chicken eggshells are disposed of annually, and it is desirable to make effective use of them. Chicken eggshells generally contain 95% by mass or more of calcium carbonate. The eggshell powder contained in the inorganic filler (B1) according to the present invention preferably contains chicken eggshell powder.
[0027] When eggshell powder is used as the inorganic filler (B1), its average particle size (D50) is preferably 1 to 500 μm, more preferably 1 to 100 μm, and even more preferably 1 to 50 μm. If the average particle size (D50) of the eggshell powder is within the above range, it is easy to obtain a resin composition that can give a molded product with better coatability with water-based paint. The average particle size (D50) refers to the particle size at which the cumulative value corresponds to 50% in the volume-based cumulative particle size distribution measured by a laser diffraction / scattering method (refractive index: 1.50). The cumulative particle size distribution is represented by a distribution curve with the particle size (μm) on the horizontal axis and the cumulative value (%) on the vertical axis. The volume-based cumulative particle size distribution measured by the laser diffraction scattering method (refractive index: 1.50) is measured using a laser diffraction scattering particle size distribution analyzer (manufactured by Beckman Coulter, product name: LS 13 320) and water (refractive index: 1.3) as the solvent, after dispersion treatment using a homogenizer (manufactured by Branson Ultrasonics Corporation, model: DIGITAL SONIFIER 450) for 1 minute as pretreatment.
[0028] The specific gravity of the eggshell powder is preferably 2.0 to 3.0, more preferably 2.0 to 2.8, and even more preferably 2.3 to 2.7. The specific gravity of the eggshell powder is a true specific gravity value measured at 25°C using a dry automatic densitometer (product name: Accupyc II1345, manufactured by Micrometrics Corporation).
[0029] When the inorganic filler (B1) is an eggshell powder or shell powder, a conventionally known method can be used for its production. That is, after washing the shells, the eggshells are pulverized by a known method, and then classified to obtain an eggshell powder or shell powder having a desired average particle size (D50). In a more specific method for obtaining eggshell powder, the eggshell membrane is removed from the washed eggshell, and then the eggshell is dried. The eggshell is then pulverized in a pulverizer or the like to obtain eggshell powder. The eggshell powder can then be obtained by classifying the eggshell powder using a sieve with an appropriate mesh size. Commercially available eggshell powders and shell powders can also be used. Examples of commercially available eggshell powders include GT-26 (manufactured by Green Techno 21 Co., Ltd.) and Calhope (registered trademark) (manufactured by Kewpie Egg Co., Ltd.). Examples of commercially available shell powders include Scallop Shell Baked Powder (manufactured by Unicera Co., Ltd.) and Scallop Power 12 (manufactured by Omi Co., Ltd.).
[0030] (Plant-derived organic filler (B2)) The filler (B) according to the present invention includes an organic filler (B2) derived from plants (hereinafter, referred to as "organic filler (B2)"). The organic filler (B2) is a filler obtained from a general plant material, and may be in any form of fiber, particles, or powder. The organic filler (B2) preferably includes ground wood. Examples of ground wood include wood powder, bamboo powder, and at least one ground material selected from plant leaves, stems, buds, and seeds. Among these, from the viewpoint of further reducing the burden on the environment, it is more preferable to include wood powder or bamboo powder made from thinned wood, waste wood, sawdust discharged from a lumber factory, or an organic filler derived from food waste. Examples of organic fillers derived from food waste include used tea leaves and coffee grounds. In one embodiment, the organic filler (B2) preferably includes an organic filler derived from food waste, and more preferably includes at least one selected from used tea leaves and coffee grounds.
[0031] Used tea leaves are the residue left after tea ingredients are extracted, and contain tea plant leaves, stems, buds, etc. Coffee grounds are the residue left after coffee ingredients are extracted, and are porous particles made by crushing coffee plant seeds. The amount of such residues left after extracting beverage ingredients has been steadily increasing in recent years, and although they were previously treated as food waste (or food waste), their reuse is being considered. By blending used tea leaves or coffee grounds as the organic filler (B2), a resin composition with less environmental impact can be obtained. In addition, by combining used tea leaves or coffee grounds with the thermoplastic resin (A), wettability with water is easily improved, and a molded product with better coatability with water-based paints can be easily obtained.
[0032] The type of used tea leaves is not particularly limited as long as it is the residue after extracting the tea components as described above, and green tea, black tea, etc. can be used. When used tea leaves are used as the organic filler (B2), used tea leaves can be crushed into fibers, particles, or powder. When using particles of used tea leaves, the average particle size is preferably 0.001 to 5.0 mm, more preferably 0.001 to 2.0 mm, from the viewpoint of moldability and kneadability of the resin composition. The average particle size of used tea leaves means the average value of the particle sizes (diameter or major axis) of 20 crushed used tea leaves measured with a vernier caliper.
[0033] Since the coffee grounds are processed into particles, they may be blended directly into the thermoplastic resin (A), or may be crushed and further pulverized as necessary. From the viewpoint of the moldability and kneadability of the resin composition, the average particle size of the coffee grounds is preferably 0.001 to 5.0 mm, and more preferably 0.001 to 2.0 mm. The average particle size of used tea leaves refers to the average value of the particle sizes (diameter or major axis) of 20 coffee grounds measured with a vernier caliper.
[0034] When using the residues of tea leaves and coffee grounds, which are left over after extracting beverage components, as the organic filler (B2), it is preferable to use dried ones. The moisture content of the tea leaves and coffee grounds is preferably 5% or less, more preferably 4% or less, and even more preferably 3% or less.
[0035] In the first embodiment of the resin composition for molded products to be coated with the water-based paint according to the present invention, it is preferable that the thermoplastic resin (A) comprises a polystyrene-based resin (A1), and the filler (B) comprises the inorganic filler (B1) or the organic filler (B2). The resin composition according to the first embodiment more preferably contains a polystyrene resin (A1) and an inorganic filler (B1) or an organic filler (B2) in a mass ratio ((A1) / (B1) or (A1) / (B2)) of 50 / 50 to 30 / 70. The inorganic filler (B1) is preferably eggshell powder. The organic filler (B2) is preferably tea leaves. By combining the eggshell powder or tea leaves with the polystyrene resin (A1) in the above mass ratio, the wettability of the obtained molded article with water is more easily improved, and a molded article having better coatability with water-based paints is more easily obtained.
[0036] In the first embodiment, the proportion of the inorganic filler (B1) or the organic filler (B2) in the resin composition is preferably more than 20% by mass and less than 80% by mass, more preferably 30 to 70% by mass, and even more preferably 50 to 70% by mass, based on the total mass of the resin composition. If the proportion of the inorganic filler (B1) or the organic filler (B2) is within the above range, it is easy to obtain a molded product that is less likely to deteriorate in moldability and has better coatability with water-based paints. The proportion of the polystyrene resin (A1) in the resin composition is preferably more than 20% by mass and less than 80% by mass, more preferably 30 to 70% by mass, and even more preferably 30 to 50% by mass, based on the total mass of the resin composition. If the proportion of the polystyrene resin (A1) is within the above range, it is easy to obtain a molded product in which the molding processability is not easily deteriorated and which has better coatability with water-based paints. In the first embodiment, the polystyrene resin (A1) preferably contains GPPS.
[0037] In a second embodiment of the resin composition for molded products to be painted with the water-based paint of the present invention, it is preferable that the thermoplastic resin (A) contains a polyolefin resin (A2) and the filler (B) contains the organic filler (B2). The resin composition according to the second embodiment more preferably contains a polyolefin resin (A2) and an organic filler (B2) in a mass ratio ((A2) / (B2)) of 50 / 50 to 30 / 70. The organic filler (B2) is preferably coffee grounds. By combining the polyolefin resin (A2) and the organic filler (B2) in a specific mass ratio, the wettability of the resulting molded article with water is more easily improved, and a molded article having better coatability with water-based paint is more easily obtained.
[0038] In the second embodiment, the proportion of the organic filler (B2) in the resin composition is preferably more than 20% by mass and less than 80% by mass, more preferably 30 to 70% by mass, and even more preferably 50 to 70% by mass, based on the total mass of the resin composition. If the proportion of the organic filler (B2) is within the above range, it is easy to obtain a molded product that is less likely to deteriorate in moldability and has better coatability with water-based paints. The proportion of the polyolefin resin (A2) in the resin composition is preferably more than 20% by mass and less than 80% by mass, more preferably 30 to 70% by mass, and even more preferably 30 to 50% by mass, based on the total mass of the resin composition. If the proportion of the polyolefin resin (A2) is within the above range, it is easy to obtain a molded product that is less likely to deteriorate in moldability and has better coatability with water-based paints. In the second embodiment, the polyolefin resin (A2) preferably contains a polypropylene resin.
[0039] The resin composition according to the present invention may contain, as necessary, other additives such as ultraviolet absorbers, light stabilizers, antioxidants, lubricants, plasticizers, colorants, antistatic agents, flame retardants, and mineral oils, and reinforcing fibers such as glass fibers, carbon fibers, and aramid fibers. These may be used alone or in combination of two or more.
[0040] Examples of the ultraviolet absorber include 2-(5'-methyl-2'-hydroxyphenyl)benzotriazole, 2-(5'-t-butyl-2'-hydroxyphenyl)benzotriazole, 2-[2'-hydroxy-3',5'-bis(α,α-dimethylbenzyl)phenyl]benzotriazole, 2-(3',5'-di-t-butyl-2'-hydroxyphenyl)benzotriazole, 2-(3'-t-butyl-5'-methyl-2'-hydroxyphenyl)-5-chlorobenzotriazole, 2-(3',5'-di-t-butyl-2'-hydroxyphenyl)benzotriazole, 2-(3',5'-di-t-amyl-2'-hydroxyphenyl)benzotriazole, 2-[3'-(3”,4”,5”,6”-tetrahydrophthalimidomethyl)-5'-methyl-2'-hydroxyphenyl]benzotriazole, 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazole-2-yl)phenol] and other benzotriazole-based ultraviolet absorbers; 2-ethoxy-2'-ethyl oxalic acid bisanilide, 2-ethoxy-5-t-butyl oxalic acid anilide ultraviolet absorbers such as 2-ethyl-2'-ethyl oxalic acid bisanilide and 2-ethoxy-4'-isodecylphenyl oxalic acid bisanilide; 2-hydroxy-4-n-octoxybenzophenone, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxy-5-sulfobenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, and 2-hydroxy-4-methoxy-2'-carboxybenzophenone; Examples of the ultraviolet absorbing agent include benzophenone-based ultraviolet absorbers; salicylic acid-based ultraviolet absorbers such as phenyl salicylate, pt-butylphenyl salicylate, and p-octylphenyl salicylate; cyanoacrylate-based ultraviolet absorbers such as 2-ethylhexyl-2-cyano-3,3'-diphenylacrylate and ethyl-2-cyano-3,3'-diphenylacrylate; and titanium oxide-based ultraviolet stabilizers such as rutile titanium oxide, anatase titanium oxide, alumina, silica, titanium oxide treated with a surface treatment agent such as a silane coupling agent or a titanium-based coupling agent.These may be used alone or in combination of two or more.
[0041] Examples of light stabilizers include bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidyl) sebacate, dimethyl succinate·1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine polycondensate, and poly[[6,(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl] [(2,2,6,6-tetramethyl-4-piperidyl)imino]-hexamethylene-[(2,2,6,6-tetramethyl-4-piperidyl)imino]], 1-[2-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionyloxy]ethyl]-4-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionyloxy]-2,2,6,6-tetramethylpiperidine, etc. These may be used alone or in combination of two or more.
[0042] Examples of the antioxidant include triethylene glycol bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate], 2,4-bis(n-octylthio)-6-(4-hydroxy-3,5-di-t-butylanilino)-1,3,5-triazine, pentaerythrityl tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-t-butyl phenol-based antioxidants such as 2,2-thiobis(4-methyl-6-t-butylphenol) and 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene; ditridecyl-3,3'-thiodipropionate, dilauryl-3,3'-thiodipropionate, ditetradecyl-3,3'-thiodipropionate, distearyl-3,3' -thiodipropionate, dioctyl-3,3'-thiodipropionate and other sulfur-based antioxidants; trisnonylphenyl phosphite, 4,4'-butylidene-bis(3-methyl-6-t-butylphenyl-di-tridecyl)phosphite, (tridecyl)pentaerythritol diphosphite, bis(octadecyl)pentaerythritol diphosphite, bis(di-t-butylphenyl)pentaerythritol diphosphite, bis Examples of the phosphorus-based antioxidants include (di-t-butyl-4-methylphenyl)pentaerythritol diphosphite, dinonylphenyl octyl phosphonite, tetrakis(2,4-di-t-butylphenyl)1,4-phenylene diphosphonite, tetrakis(2,4-di-t-butylphenyl)4,4'-biphenylene diphosphonite, and 10-decyloxy-9,10-dihydro-9-oxa-10-phosphaphenanthrene. These may be used alone or in combination of two or more.
[0043] Examples of lubricants include magnesium stearate, zinc stearate, zinc 1,2-hydroxystearate, calcium stearate, lithium stearate, lithium 1,2-hydroxystearate, sodium stearate, erucic acid amide, etc. These may be used alone or in combination of two or more.
[0044] [Method of producing resin composition] The resin composition according to the present invention can be produced by melt-kneading the thermoplastic resin (A), the filler (B), and other components as necessary. Specifically, the thermoplastic resin (A) and the filler (B) are each charged into a twin-screw extruder in a mass ratio ((A) / (B)) of 50 / 50 to 30 / 70, and other components are further added as necessary. The mixture is melt-kneaded at a temperature of 180 to 250°C, and then extruded in the form of strands to prepare a pellet-shaped resin composition.
[0045] [Application] As described above, the resin composition according to the present invention can provide a molded article having good paintability with respect to water-based paint. Therefore, it is suitable for use in molded articles to be painted with water-based paint, such as home appliances, automobile interior materials, toys, etc. However, the use of the resin composition according to the present invention is not limited to the above-mentioned uses.
[0046] [Molded products] The molded article according to the present invention can be painted with a water-based paint to form a painted molded article. The molded article according to the present invention contains the resin composition described above. Preferably, the molded article is obtained only from the resin composition according to the present invention. The molded article according to the present invention has improved wettability with water and good paintability with water-based paints. In addition, the molded article according to the present invention is molded from a resin composition containing a filler derived from natural materials and a small amount of resin material derived from fossil resources, thereby reducing the burden on the environment.
[0047] The method for producing the molded product is not particularly limited, and a conventionally known method can be used. Specifically, a molded product having a desired shape can be obtained by injection molding using pellets obtained from the resin composition according to the present invention. Then, the molded product can be painted with a water-based paint to obtain a painted molded product.
[0048] More preferred embodiments of the resin composition according to the present invention are as follows. <1> A resin composition for molded products to be coated with a water-based paint, comprising a polystyrene-based resin (A1) and eggshell powder (B1), wherein the proportion of the eggshell powder (B1) is 50 mass% or more relative to the total mass of the resin composition. <2> The average particle size (D50) of the eggshell powder is 1 to 50 μm. <1> A resin composition for moldings which is coated with the aqueous paint according to claim 1. <3> The polystyrene-based resin (A1) contains polystyrene (GPPS), <1> or <2> A resin composition for moldings which is coated with the aqueous paint according to claim 1. <4> Satisfying the following formulas (1) and (2), <1> from <3> 13. A resin composition for molded products, which is coated with the aqueous paint according to claim 12. θ1-θ2≧3° (1) θ2≦90° (2) (In the formulas (1) and (2), θ1 is the contact angle of water of a molded article obtained from the polystyrene resin (A1) measured by the θ / 2 method, and θ2 is the contact angle of water of a molded article obtained from the resin composition measured by the θ / 2 method.) <5> A resin composition for molded products to be coated with a water-based paint, comprising a polyolefin resin (A2) and at least one organic filler (B2) selected from used tea leaves and coffee grounds, wherein the proportion of the organic filler (B1) is 50 mass% or more relative to the total mass of the resin composition. <6> The polyolefin resin (A2) contains polypropylene. <5> A resin composition for moldings which is coated with the aqueous paint according to claim 1. <7> Satisfying the following formulas (3) to (4), <5> or <6> A resin composition for moldings which is coated with the aqueous paint according to claim 1. θ3-θ4≧3° (3) θ4≦90° (4) (In the formulas (3) and (4), θ3 is the contact angle of water of a molded article obtained from the polyolefin resin (A2) measured by the θ / 2 method, and θ4 is the contact angle of water of a molded article obtained from the resin composition measured by the θ / 2 method.) <8> <1> from <7> 2. A molded article comprising the resin composition for molded articles which is coated with the water-based paint according to claim 1 . EXAMPLES
[0049] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the following description.
[0050] [Example 1] As the inorganic filler (B1), 60 parts by mass of eggshell powder (manufactured by Green Techno 21 Co., Ltd., product name "GT-26", average particle size (D50) 30 μm) and as the thermoplastic resin (A), 40 parts by mass of polystyrene resin (manufactured by Toyo Styrene Co., Ltd., product name "Toyo Styrol (registered trademark) GP-HRM61C", GPPS, Mw 245000) were weighed and mixed. The mixture was then placed in a twin-screw kneader (manufactured by Brabender Technology, product name "Plasticorder (registered trademark) W50EHT") and kneaded for 10 minutes at a kneading temperature of 200°C and a rotation speed of 100 rpm to obtain a resin composition. The obtained resin composition was press-molded in a pressure molding machine (manufactured by Shoji, 50t heating molding machine) at a heating temperature of 200°C, a pressure of 5 MPa, a preheating time of 3 minutes, and a pressurizing time of 3 minutes to obtain a molded product of 150 mm x 150 mm x 1.0 mm in thickness. As a comparative sample, only the above polystyrene resin was press-molded under the same conditions to produce a comparative molded product of 150 mm x 1500 mm x 1.0 mm in thickness.
[0051] The average particle size (D50) of the eggshell powder was measured under the following conditions. Using a laser diffraction / scattering particle size analyzer (manufactured by Beckman Coulter, product name: LS 13 320), eggshell powder was dispersed using water (refractive index: 1.3) as the solvent for 1 minute using a homogenizer (manufactured by Branson Ultrasonics Corporation, model: DIGITAL SONIFIER 450) as a pretreatment, and the D50 particle size was measured.
[0052] <Paintability evaluation> The paintability of the molded article obtained in Example 1 with respect to a water-based paint was evaluated based on the wettability (contact angle) with water. 1 μL of distilled water was dropped onto the surface of the molded product, and the contact angle θ2 with water was measured at 25°C using a contact angle measuring device (manufactured by Kyowa Interface Science Co., Ltd., product name "Automatic Contact Angle Meter DM-500"). Next, the contact angle θ1 with water of the comparative molded product was measured under the same conditions. If the contact angle θ1 with water of the comparative molded product is 3° or more larger than the contact angle θ2 with water of the molded product, it can be determined that the wettability of the molded product with water has improved. It is believed that improved wettability with water will also improve the paintability with water-based paints. Therefore, the wettability with water was evaluated according to the following evaluation criteria. The results are shown in Table 1. (Evaluation Criteria) Good: θ1-θ2 is 3° or more Not possible: θ1-θ2 is less than 3°
[0053] <Evaluation of processability> The processability of the resin composition was evaluated based on the dispersibility of the filler (B) during kneading. When the thermoplastic resin (A) and the filler (B) were kneaded, the filler (B) was not aggregated and was dispersed in the thermoplastic resin (A) as "good", and the filler (B) was aggregated or was not dispersed in the thermoplastic resin (A) as "poor". The processability was evaluated visually. The results are shown in Table 1.
[0054] [Example 2] Instead of the inorganic filler (B1) (eggshell powder), an organic filler (B2) was used to obtain a resin composition with the composition shown in Table 1. As the organic filler (B2), used were used used tea leaves (ground Japanese tea leaves, moisture content 2%, average particle size 1.5 mm). A molded product was prepared in the same manner as in Example 1. Thereafter, the paintability and processability were evaluated in the same manner as in Example 1. The results are shown in Table 1. The average particle size of the used tea leaves was determined by measuring the maximum particle size (long axis or diameter) of 20 pieces of used tea leaves using a caliper, and the average value was used. The moisture content of the used tea leaves was measured using a Karl Fischer moisture meter (manufactured by Kyoto Electronics Manufacturing Co., Ltd., product name: MKC-510).
[0055] [Example 3] A resin composition was obtained with the composition shown in Table 1 using coffee grounds (moisture content 2%, average particle size 1.5 mm) as the organic filler (B2) and polypropylene (polyolefin resin (A2)) (manufactured by Japan Polypropylene Corporation, product name "Novatec (registered trademark) PP-BC03B", MFR: 30 g / 10 min) as the thermoplastic resin (A). A molded product and a comparative molded product (Reference Example 2) were prepared in the same manner as in Example 1. Then, the paintability and processability were evaluated in the same manner as in Example 1. The results are shown in Table 1. The average particle size of the coffee grounds was determined by measuring the maximum particle size (long axis or diameter) of 20 coffee grounds using a caliper and using the average value. The moisture content of the coffee grounds was measured using a Karl Fischer moisture meter (manufactured by Kyoto Electronics Manufacturing Co., Ltd., product name: MKC-510).
[0056] [Examples 4 to 9 and Comparative Examples 1 to 6] A resin composition was prepared and a molded article was obtained in the same manner as in Example 1, except that the components of the resin composition were as shown in Tables 1 and 2. In addition, the coatability and processability were evaluated in the same manner as in Example 1. The results are shown in Tables 1 and 2.
[0057] Details of the raw materials shown in Tables 1 and 2 are as follows. (Thermoplastic resin (A)) Polystyrene resin (A1): GPPS (manufactured by Toyo Styrene Co., Ltd., product name "Toyo Styrol GP-HRM61C", Mw: 245,000). Polyolefin resin (A2): Polypropylene (manufactured by Japan Polypropylene Corporation, product name "Novatec PP-BC03B", MFR: 30g / 10min). (Filling material (B)) Inorganic filler (B1-1): Eggshell powder (manufactured by Green Techno 21 Co., Ltd., product name "GT-26", average particle size (D50) 30 μm). Organic filler (B2-1): Tea leaves (moisture content 2%, average particle size 1.5 mm). Organic filler (B2-2): Coffee grounds (moisture content 2%, average particle size 1.5 mm).
[0058] [Table 1]
[0059] [Table 2]
[0060] In Table 1, Reference Examples 1 and 2 are evaluations of the coatability and processability of resins consisting of only polystyrene-based resin (A1) or polyolefin-based resin (A2). The coatability of the resin compositions of the Examples and Comparative Examples was evaluated based on the contact angle value of Reference Example 1 or Reference Example 2. Of these, the resin compositions of Examples 1 to 9, which satisfy the configuration of the present invention, had a contact angle with water that was changed by 3° or more from the value of Reference Example 1 or Reference Example 2, and had improved wettability. In contrast, the resin compositions of Comparative Examples 1 to 6, which do not satisfy the configuration of the present invention, did not change in wettability with water, and the problem could not be solved. In addition, the resin compositions of Comparative Examples 2, 4, and 6 had poor processability, and the wettability of the molded product could not be evaluated. From the above results, it was found that the resin composition according to the present invention can provide a molded product having good coatability with water-based paint. In addition, the resin composition according to the present invention contains a filler (B) derived from a natural material at a certain ratio to the thermoplastic resin (A), so that the amount of thermoplastic resin (A) in the resin composition can be reduced, and a molded product with less environmental impact can be provided.
Claims
1. A resin composition for use in molded products to be coated with a water-based paint, comprising a thermoplastic resin (A) including a polystyrene-based resin or a polyolefin-based resin, and at least one inorganic filler (B1) selected from eggshell powder and seashell powder, in a mass ratio ((A) / (B1)) of 50 / 50 to 30 / 70.
2. The resin composition for moldings to be coated with an aqueous paint according to claim 1, wherein the inorganic filler (B1) is a filler derived from food waste.
3. A resin composition for molded products to be painted with the aqueous paint described in claim 1 or 2, wherein the inorganic filler (B1) comprises eggshell powder having an average particle diameter (D50) of 1 to 50 μm.
4. A resin composition for molded products that is painted with an aqueous paint described in any one of claims 1 to 3, wherein the polystyrene-based resin contains polystyrene (GPPS).
5. A molded article comprising a resin composition for molded articles, which is coated with the water-based paint according to any one of claims 1 to 4.
Citation Information
Patent Citations
Resin composition and molded article
EP4328250A1
Resin composition for engraving by cutting
JP1986106646A
Additive for water-based coating, and water-based coating composition
JP2016188338A
JPP6764210B
Woody resin molding, polished woody resin, and processes for producing the same