Rust prevention treatment method and rust prevention treated article

The rust prevention treatment using inorganic acids and salts at elevated temperatures addresses inefficiencies in existing methods, providing enhanced rust prevention for metals and alloys without requiring additional high-temperature processing.

JP7584149B2Active Publication Date: 2024-11-15NOF METAL COATINGS ASIA PACIFIC CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2021548942
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-26
Filing Date
2020-09-23
Publication Date
2024-11-15
Estimated Expiration
2040-09-23

AI Technical Summary

Technical Problem

Existing rust prevention methods for metal surfaces, such as those involving metal or alloy films, are not efficient in providing high rust prevention performance and often require complex processes or high-temperature treatments.

Method used

A rust prevention treatment method using an aqueous solution of inorganic acids or salts, such as silicic acid, silicate, phosphoric acid, and zirconium salts, applied at temperatures exceeding 180°C, which can be done without subsequent high-temperature heating, to enhance rust prevention performance on metal or alloy surfaces.

Benefits of technology

The method effectively imparts superior rust prevention performance to metal and alloy materials, reducing rust formation significantly even at elevated temperatures, and can be applied without additional high-temperature processing steps.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584149000001
    Figure 0007584149000001
  • Figure 0007584149000002
    Figure 0007584149000002
  • Figure 0007584149000003
    Figure 0007584149000003
Patent Text Reader

Abstract

The present invention relates to: a rust-proofing treatment method comprising the step of treating an object that comprises a metal or an alloy and is heated to a temperature higher than 180℃ or an object that has, formed on the surface thereof, a film or layer comprising a metal or an alloy and is heated to a temperature higher than 180℃ with an aqueous solution containing an inorganic acid or an inorganic salt, or comprising the step of treating an object comprising a metal or an alloy or an object having, formed on the surface thereof, a film or layer comprising a metal or an alloy with an aqueous solution containing at least one component selected from silicic acid, a silicic acid salt, phosphoric acid, a phosphoric acid salt, a monohydrogen phosphate salt, a dihydrogen phosphate salt and a zirconium salt; and an article characterized by being rust-proofing-treated by the rust-proofing treatment method.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a rust prevention method and an article that has been treated with a rust prevention treatment. [Background technology]

[0002] BACKGROUND ART Conventionally, a common rust prevention treatment method involves forming an anti-rust film or anti-rust layer containing a metal such as zinc or an alloy on the surface of a metal or alloy.

[0003] For example, Patent Document 1 discloses an anticorrosion paint composition containing metal particles (specifically, metal particles based on zinc or a zinc alloy) having an inorganic modification (specifically, silicon dioxide) on the surface thereof, and an anticorrosion coating obtained from this composition.

[0004] Patent Document 2 discloses a curable coating composition for metal substrates that inhibits or prevents corrosion, which comprises a resin binder and nanoparticles (specifically, ZnO, Al2O3, Al(O)OH, etc.) whose surfaces are treated with at least one surface-modifying group (specifically, polydialkylsiloxane, etc.).

[0005] Patent Document 3 discloses a method for producing a deformable anticorrosion layer on a metal surface, which comprises the steps of mixing metallic magnesium, zinc, aluminum or titanium particles, or a mixture or alloy containing at least one of these metals, with at least one metal compound (specifically, titanium alkoxide, zirconium alkoxide, etc.), and a reaction between the metal particles and the metal compound results in surface-modified metal particles; applying the resulting surface-modified metal particles to the metal surface; hardening the layer produced from the surface-modified metal particles at a temperature between room temperature and 500°C; and a tempering step carried out at a temperature in the range of 250°C to approximately 700°C and lasting from a few seconds to a few hours. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Laid-Open No. 2018-70999 [Patent Document 2] Special Publication No. 2013-510932 [Patent Document 3] Special Publication No. 2012-505963 Summary of the Invention [Problem to be solved by the invention]

[0007] However, the higher the rust-preventing performance, the more desirable it is, and it is also desirable to be able to impart excellent rust-preventing performance in a simple manner.

[0008] An object of the present invention is to provide a rust prevention treatment method that can easily impart superior rust prevention performance to metal or alloy materials, and also to provide an article having superior rust prevention performance. [Means for solving the problem]

[0009] The present invention relates to the following items. [1] A rust prevention method comprising the step of treating a workpiece containing a metal or alloy that has been heated to a temperature exceeding 180°C, or a workpiece having a film or layer containing a metal or alloy on its surface that has been heated to a temperature exceeding 180°C, with an aqueous solution containing an inorganic acid or an inorganic salt. [2] The rust prevention treatment method according to [1] above, wherein the temperature of the object to be treated when treated with the aqueous solution is above 220°C. [3] The rust prevention treatment method according to [1] or [2] above, wherein the aqueous solution containing an inorganic acid or an inorganic salt is an aqueous solution containing at least one selected from silicic acid, silicates, phosphoric acid, phosphates, monohydrogen phosphates, dihydrogen phosphates, sulfuric acid, sulfates, nitric acid, nitrates, molybdic acid, molybdates, and zirconium salts. [4] The rust prevention treatment method according to any one of [1] to [3] above, wherein the content of the inorganic acid and / or inorganic salt in the aqueous solution containing the inorganic acid or inorganic salt is 0.1 mass % or more. [5] The rust prevention treatment method according to any one of the above [1] to [4], wherein the aqueous solution containing the inorganic acid or inorganic salt further contains a lubricant. [6] The rust prevention treatment method according to any one of the above [1] to [5], wherein the aqueous solution containing the inorganic acid or inorganic salt has a pH of 4 or higher. [7] The rust prevention treatment method according to any one of [1] to [6] above, characterized in that it does not include a step of heating the object to 200° C. or higher after the treatment with the aqueous solution.

[0010] [8] A rust prevention method comprising a step of treating a workpiece containing a metal or alloy, or a workpiece having a film or layer containing a metal or alloy on its surface, with an aqueous solution containing at least one selected from silicic acid, silicates, phosphoric acid, phosphates, monohydrogen phosphates, dihydrogen phosphates, and zirconium salts. [9] The rust prevention treatment method according to the above item [8], wherein the aqueous solution containing the inorganic acid or inorganic salt further contains a lubricant.

[10] The rust prevention treatment method according to [8] or [9] above, characterized in that it does not include a step of heating the object to be treated to 200°C or higher after treatment with the aqueous solution.

[0011]

[11] The rust prevention treatment method according to any one of the above items [1] to

[10] , characterized in that the object to be treated contains at least one selected from zinc, zinc alloys, aluminum, aluminum alloys, iron, and iron alloys, or has on its surface a film or layer containing at least one selected from zinc, zinc alloys, aluminum, aluminum alloys, iron, and iron alloys.

[12] The rust prevention treatment method according to any one of [1] to

[10] above, wherein the object to be treated has a rust prevention film on its surface, the rust prevention film containing at least one selected from zinc, a zinc alloy, aluminum, and an aluminum alloy.

[0012]

[13] An article that has been subjected to a rust prevention treatment by the rust prevention treatment method according to any one of [1] to

[12] above. [Effects of the Invention]

[0013] According to the present invention, it is possible to provide a rust prevention treatment method that can easily impart superior rust prevention performance to metal materials or alloy materials, and also to provide an article having superior rust prevention performance. [Brief explanation of the drawings]

[0014] [Figure 1A] FIG. 1A is a photograph of the cold-rolled steel sheet of Example 58 that had been immersed in an aqueous sodium silicate solution, taken one hour after the start of the salt spray test. [Figure 1B] FIG. 1B is a photograph of the cold-rolled steel sheet of Example 58 that had been immersed in an aqueous sodium silicate solution, taken 5 hours after the start of the salt spray test. [Figure 2A] FIG. 2A is a photograph of the cold-rolled steel sheet of Comparative Example 14 that was not subjected to immersion treatment in an aqueous sodium silicate solution, taken one hour after the start of the salt spray test. [Figure 2B] FIG. 2B is a photograph of the cold-rolled steel sheet of Comparative Example 14 that was not subjected to immersion treatment in an aqueous sodium silicate solution, taken 5 hours after the start of the salt spray test. DETAILED DESCRIPTION OF THE INVENTION

[0015] A first aspect of the rust prevention treatment method of the present invention includes a step of treating a metal- or alloy-containing object heated to a temperature exceeding 180°C, or an object having a metal- or alloy-containing film or layer on its surface heated to a temperature exceeding 180°C, with an aqueous solution containing an inorganic acid or inorganic salt (hereinafter also referred to as an "inorganic acid treatment agent"). A second aspect of the rust prevention treatment method of the present invention includes a step of treating a metal- or alloy-containing object or an object having a metal- or alloy-containing film or layer on its surface with an aqueous solution containing at least one selected from silicic acid, silicates, phosphoric acid, phosphates, monohydrogen phosphates, dihydrogen phosphates, and zirconium salts. Hereinafter, the first aspect of the rust prevention treatment method of the present invention and the second aspect of the rust prevention treatment method of the present invention may be collectively referred to as the "rust prevention treatment method of the present invention."

[0016] In the rust prevention treatment method of the present invention, a workpiece containing a metal or alloy, or a workpiece having a film or layer containing a metal or alloy on its surface, is treated with an inorganic acid treatment agent. Here, by setting the temperature of the workpiece during treatment with the inorganic acid treatment agent to a temperature exceeding 180°C, preferably exceeding 220°C, the rust prevention performance of the workpiece can be improved. Furthermore, when the workpiece is treated with an aqueous solution containing at least one inorganic acid treatment agent selected from silicic acid, silicates, phosphoric acid, phosphates, monohydrogen phosphates, dihydrogen phosphates, and zirconium salts, the rust prevention performance of the workpiece can be sufficiently improved even if the temperature of the workpiece is 180°C or lower.

[0017] That is, according to the rust prevention treatment method of the first aspect of the present invention, in which an object to be treated that has been heated to a temperature exceeding 180°C is treated with an inorganic acid-based treatment agent, it is possible to easily impart superior rust prevention performance to a metal material or an alloy material. Also, according to the rust prevention treatment method of the second aspect of the present invention, in which an object to be treated is treated with an aqueous solution containing at least one selected from silicic acid, silicates, phosphoric acid, phosphates, monohydrogen phosphates, dihydrogen phosphates, and zirconium salts, it is possible to easily impart superior rust prevention performance to a metal material or an alloy material, whether the object to be treated is heated to a temperature exceeding 180°C or is not heated to a temperature exceeding 180°C, such as at room temperature.

[0018] The inorganic acid treatment agent used in the present invention is an aqueous solution containing an inorganic acid and / or an inorganic salt. Examples of inorganic acids and inorganic salts include silicic acid, silicates, phosphoric acid, phosphates, monohydrogenphosphate, dihydrogenphosphate, sulfuric acid, sulfates, nitric acid, nitrates, molybdic acid, molybdates, and zirconium salts. Examples of silicic acid and silicates that can be used include orthosilicic acid and orthosilicates, pyrosilicate and pyrosilicates, and metasilicic acid and metasilicates. Examples of phosphoric acid and phosphates that can be used include orthophosphoric acid and orthophosphates, pyrophosphoric acid and pyrophosphates, and metaphosphoric acid and metaphosphates.

[0019] Among inorganic acids and inorganic salts, silicic acid, silicates, phosphoric acid, phosphates, monohydrogen phosphates, dihydrogen phosphates, and zirconium salts are preferred. The inorganic salts silicates, phosphates, monohydrogen phosphates, dihydrogen phosphates, sulfates, nitrates, and molybdates are all preferably metal salts, particularly monovalent metal salts such as lithium salts, sodium salts, and potassium salts, and divalent metal salts such as magnesium salts and calcium salts. Preferred zirconium salts include, for example, ammonium zirconium carbonate, potassium zirconium carbonate, and sodium zirconium carbonate. The inorganic acids and inorganic salts may be used alone or in combination of two or more.

[0020] The concentration of the inorganic acid treatment agent (aqueous solution containing an inorganic acid or an inorganic salt), i.e., the content of the inorganic acid and / or inorganic salt in the aqueous solution, is not particularly limited, but is usually preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more. The upper limit of the concentration of the inorganic acid treatment agent, i.e., the content of the inorganic acid and / or inorganic salt in the aqueous solution, is not particularly limited and may be a saturated solution, but is usually preferably 15% by mass or less, more preferably 5% by mass or less.

[0021] The inorganic acid-based treatment agent may contain additives or additional components such as pH adjusters, water-soluble crosslinkers, water-soluble resins, lubricants, pigments, antifoaming agents, dispersants, antisettling agents, leveling agents, thickeners, matting agents, antifouling agents, preservatives, UV absorbers, and dyes, as long as the desired effects are not impaired. It may be preferable to add additives or additional components such as lubricants to the inorganic acid-based treatment agent for the purpose of improving or changing the physical properties of the article to be treated with rust prevention. On the other hand, if there is no need to improve or change the physical properties of the article to be treated with rust prevention, it is usually preferable that the inorganic acid-based treatment agent contain no additional components other than the pH adjuster. Furthermore, it is usually preferable that the inorganic acid-based treatment agent contain only water as a solvent, i.e., no organic solvent. However, from the viewpoint of dispersibility, it may be preferable to add a small amount (e.g., 10% by mass or less, preferably 5% by mass or less) of an organic solvent.

[0022] In one embodiment, the inorganic acid treatment agent used in the present invention preferably contains a lubricant. By containing a lubricant in the inorganic acid treatment agent, the coefficient of friction of the surface of the article that has been subjected to the rust prevention treatment of the present invention can be reduced, and the coefficient of friction of the surface of the article that has been subjected to the rust prevention treatment of the present invention can be easily controlled.

[0023] The lubricant is not particularly limited, but examples thereof include waxes such as polyolefin and modified polyolefin (polyethylene, modified polyethylene, polypropylene, modified polypropylene, etc.), paraffin, carnauba wax, fluororesin, melamine cyanurate, hexagonal boron nitride, etc. Waxes are usually preferably added and mixed in the form of an emulsion to prepare an inorganic acid-based treatment agent. Lubricants are commercially available, and examples thereof include BYK's "CERAFLOUR 913" (trade name), "CERAFLOUR 914" (trade name), "CERAFLOUR 915" (trade name), "CERAFLOUR 916" (trade name), "CERAFLOUR 917" (trade name), "CERAFLOUR 925" (trade name), "CERAFLOUR 927" (trade name), "CERAFLOUR 929" (trade name), "CERAFLOUR 950" (trade name), "CERAFLOUR 988" (trade name), "CERAFLOUR 1000" (trade name), E497 (trade name), "AQUACER 507" (trade name), "AQUACER 515" (trade name), "AQUACER 526" (trade name), "AQUACER 531" (trade name), "AQUACER 537" (trade name), "AQUACER 539" (trade name), "AQUACER 552" (trade name), and "AQUACER 553" (trade name). 593" (product name), "AQUACER 840" (product name), "AQUACER 1547" (product name), "AQUAMAT 208" (product name), "AQUAMAT 263" (product name), "AQUAMAT 272" (product name), "AQUAMAT 8421" (product name), "HARDAMER PE02" (product name), "HARDAMER PE03" (product name), "HARDAMER PE04" (product name), "CERACOL 79" (product name), Sanyo Chemical Industries, Ltd.'s "Sunwax 161-P" (product name), "Sunwax 131-P" (product name), "Sunwax 151-P" (product name), "Sunwax 171-P" (product name), "Viscol 330-P" (product name), "Viscol 440-P" (product name), "Viscol 550-P" (product name), "Viscol 660-P" (product name), Mitsui Chemicals, Inc.'s "Hiwax 100P" (product name), "Hiwax400P" (product name), "Hiwax 800P" (product name), "Hiwax 1105A" (product name), "Hiwax 2203A" (product name), "Hiwax 1120H" (product name), "Hiwax 4202E" (product name), "Hiwax 405MP" (product name), "Hiwax 4051E" (product name), "Hiwax 410P" (product name), CLARIANT's "LICOWAX PE 520" (product name), "LICOWAX PE 130" (product name), "LICOWAX PE 190" (product name), "LICOWAX PED 521" (product name), "LICOWAX PED 522" (product name), "LICOWAX PED 153" (product name), "LICOWAX PED 191" (product name), "LICOWAX PED 192" (product name), "LICOWAX 371 FP" (product name), "LICOCENE PP 6102" (product name), "LICOCENE PP 6502" (product name), "LICOCENE PP 7502" (product name), "LICOCENE PP 1302" (product name), "LICOCENE PP 1502" (product name), "LICOCENE PP 1602" (product name), "LICOCENE PP 2602" (product name), "LICOCENE PP 3602" (product name), "LICOCENE PE 4201" (product name), "LICOCENE PE 5301" (product name), "LICOCENE PP MA 1332" (product name), "LICOCENE PP MA 6252" (product name), "LICOCENE PP MA 6452" (product name), "LICOCENE PP MA 7452” (product name), “LICOCENE PE MA 4221” (product name), “LICOCENE PE MA 4351” (product name), “CERIDUST 3620” (product name), “CERIDUST 3610" (product name), "CERIDUST 3715" (product name), "CERIDUST 6050 M" (product name), "CERIDUST 9610 F" (product name), "CERIDUST 9630 F" (product name), "CERIDUST 3920 F" (product name), "CERIDUST 3940 F" (product name), "CERIDUST 9202 F" (product name), "CERIDUST 9205F" (product name), Westlake "Epolene E-10" (product name), "Epolene E-10P" (product name), "Epolene E-14" (product name), "Epolene E-14E" (product name), "Epolene E-14EP" (product name), "Epolene E-14P" (product name), "Epolene E-16" (product name), "Epolene "E-20" (product name), "Epolene E-20P" (product name), "Epolene EE-2" (product name), "Epolene E-43" (product name), "Epolene E-43P" (product name), "Hi-Disper A-113" (product name), "Hi-Disper A-375" (product name), "Hi-Disper" manufactured by Gifu Seratsuku Manufacturing Co., Ltd. AB-50” (product name), “Hi-Disper AF-41” (product name), “Hi-Disper AG-73” (product name), “Hi-Disper A-110” (product name), “Hi-Disper Suitable lubricants include "Hi-Disper A-512" (trade name), "Hi-Disper A-348" (trade name), "Hi-Disper A-332" (trade name), "Hi-Disper A-206N" (trade name), "Hi-Disper AD-62" (trade name), "nanoFLONE PTFE AQ-60" (trade name) and "nanoFLONE PTFE AQ 50 SM" (trade name) manufactured by Shamrock Technologies, "Poligen WE 1" (trade name), "Poligen WE 3" (trade name), "Poligen WE 4" (trade name), "Poligen WE 6" (trade name), and "Poligen Wax V Flakes" (trade name) manufactured by BASF, and "Lubron LDW-410" (trade name) manufactured by Daikin Corporation. One type of lubricant may be used alone, or two or more types may be used in combination.

[0024] The content of the lubricant in the inorganic acid-based treatment agent (aqueous solution containing an inorganic acid or an inorganic salt) is not particularly limited and can be selected appropriately so as to obtain the desired coefficient of friction on the surface of the article, but it is usually preferable that it be 10 mass % or less.

[0025] The inorganic acid treatment agent used in the present invention can be prepared by a known method by mixing and dissolving a predetermined amount of inorganic acid and / or inorganic salt, and, if necessary, additives or additional components, in an aqueous solvent.

[0026] In one embodiment, the pH of the inorganic acid treatment agent (aqueous solution containing an inorganic acid or an inorganic salt) used in the present invention is preferably 4 or higher, and more preferably 4 to 12. If the pH is less than 4, the surface containing a metal or alloy may be more susceptible to the effects of the acid. On the other hand, if the pH is high, caution may be required in handling for safety reasons. Note that the pH in the present invention refers to the pH at 20°C.

[0027] In the present invention, the pH of the inorganic acid treatment agent varies depending on the type and concentration of the inorganic acid and inorganic salt used, and therefore, in order to adjust the pH to a predetermined level, sodium hydroxide, potassium hydroxide, lithium hydroxide, nitric acid, etc. can be used as a pH adjuster.

[0028] The object to be treated to which the rust prevention treatment method of the present invention is applied is an object having a metal material or an alloy material on its surface, that is, an object to be treated containing a metal or alloy, or an object to be treated having a film or layer containing a metal or alloy on its surface. The film or layer containing a metal or alloy may be formed on the entire surface of the object to be treated, or on only a part of the surface.

[0029] Metal or alloy materials to which the rust prevention treatment method of the present invention can be applied are not particularly limited, but examples include zinc and zinc alloys such as Zn-Al alloys, aluminum and aluminum alloys such as Al-Mg alloys, iron alloys such as iron and carbon steel, and magnesium alloys such as Mg-Zn alloys.

[0030] In particular, the rust prevention treatment method of the present invention can be suitably applied to a substrate containing at least one selected from zinc, zinc alloy, aluminum, aluminum alloy, iron, and iron alloy, or a substrate having a film or layer on its surface containing at least one selected from zinc, zinc alloy, aluminum, aluminum alloy, iron, and iron alloy. Here, the zinc alloy (or aluminum alloy) may be a zinc-aluminum alloy. Furthermore, rust prevention treatment of metal or alloy materials typically involves forming a rust prevention film on the surface containing zinc, zinc alloy, aluminum, or aluminum alloy. The rust prevention treatment method of the present invention can also be suitably applied to a substrate having a rust prevention film on its surface containing at least one selected from zinc, zinc alloy, aluminum, and aluminum alloy, thereby further improving the rust prevention performance of the substrate.

[0031] In the rust prevention treatment method of the present invention, a substrate containing a metal or alloy, or a substrate having a film or layer containing a metal or alloy on its surface, is treated with the inorganic acid treatment agent (an aqueous solution containing an inorganic acid or an inorganic salt) as described above, preferably with or without heating to a temperature above 180°C. The inorganic acid treatment agent may also be heated or unheated, or may be cooled to a temperature at which it does not solidify. Treatment with this inorganic acid treatment agent can be carried out, for example, by immersion, i.e., by immersing the substrate in the inorganic acid treatment agent, or by spraying, i.e., by spraying the inorganic acid treatment agent onto the substrate.

[0032] In the rust prevention treatment method of the first aspect of the present invention, the temperature of the treated object when treated with the inorganic acid treatment agent is above 180°C, preferably above 220°C. In the rust prevention treatment method of the second aspect of the present invention, the temperature of the treated object when treated with the inorganic acid treatment agent (an aqueous solution containing at least one selected from silicic acid, silicates, phosphoric acid, phosphates, monohydrogen phosphates, dihydrogen phosphates, and zirconium salts) is not particularly limited and may be 180°C or lower. However, in this case, the temperature of the treated object when treated with the inorganic acid treatment agent is preferably above 180°C, more preferably above 220°C, in order to further improve the rust prevention performance. Note that, depending on the type of lubricant added, when the temperature of the treated object is high, for example, above 180°C, or even higher, the coefficient of friction of the surface of the article may become lower.

[0033] In both the rust prevention treatment method of the first aspect of the present invention and the rust prevention treatment method of the second aspect of the present invention, the upper limit of the temperature of the object to be treated when treated with the inorganic acid-based treatment agent is not particularly limited, but is usually preferably 350°C or lower, and more preferably 320°C or lower.

[0034] On the other hand, the temperature of the inorganic acid-based treatment agent used when treating the object to be treated is not particularly limited as long as it is above the freezing point and below the boiling point of the inorganic acid-based treatment agent (an aqueous solution containing an inorganic acid or an inorganic salt). However, from the viewpoints of cost and ease of operation, a temperature of about 15 to 50°C is usually preferred.

[0035] The time for treating the object to be treated with an inorganic acid-based treating agent (an aqueous solution containing an inorganic acid or an inorganic salt) (in the case of an immersion treatment, the time for immersing the object in the inorganic acid-based treating agent; in the case of a spray treatment, the time for spraying the object with the inorganic acid-based treating agent) is not particularly limited and depends on the concentration of the inorganic acid-based treating agent, but is usually preferably 1 second or more, more preferably 5 seconds or more. Furthermore, the object to be treated may be treated with the inorganic acid-based treating agent for a long period of time, but from the standpoint of productivity and efficiency, it is usually preferably 15 minutes or less, more preferably 10 minutes or less.

[0036] In addition, the treatment with an inorganic acid-based treatment agent only requires that at least a portion, preferably the entire surface of the metal or alloy-containing object be treated with the inorganic acid-based treatment agent, and it is not necessary to treat the entire surface of the object with the inorganic acid-based treatment agent. For example, in the case of immersion treatment, the entire object may be immersed in the inorganic acid-based treatment agent, or only the metal or alloy-containing surface of the object may be immersed in the inorganic acid-based treatment agent. In the case of spray treatment, the inorganic acid-based treatment agent may be sprayed on the entire surface of the object, including the surface not containing the metal or alloy, or it is sufficient to spray the inorganic acid-based treatment agent on the metal or alloy-containing surface of the object.

[0037] The treatment with the inorganic acid-based treatment agent can be performed on the entire surface of the object to be treated simultaneously or on each surface at a time. Furthermore, the entire surface of the object to be treated can be treated with the same inorganic acid-based treatment agent (aqueous solution containing an inorganic acid or an inorganic salt), or with different agents.

[0038] Heating of the workpiece and heating or cooling of the inorganic acid treatment agent can be carried out by known means, and treatment with the inorganic acid treatment agent, specifically, immersion treatment and spray treatment, can also be carried out by known means. Furthermore, treatment conditions other than the temperature of the workpiece, the temperature of the inorganic acid treatment agent, and the treatment time are not particularly limited and can be selected appropriately. In both immersion treatment and spray treatment, it is preferable to treat the entire surface containing the metal or alloy uniformly.

[0039] After treating the object to be treated with an inorganic acid-based treatment agent (an aqueous solution containing an inorganic acid or an inorganic salt), it can be washed with water as needed and dried to obtain an article that has been subjected to the rust prevention treatment of the present invention.

[0040] The object to be treated with the inorganic acid-based treatment agent can be dried by known means, and the drying conditions are not particularly limited and can be selected appropriately. For example, the object can be naturally dried or air-dried at room temperature, or centrifugal dried. The drying can be carried out in the air, in an inert gas such as nitrogen gas, or under reduced pressure.

[0041] Although the object to be treated can be dried by heating, in the present invention, it is not necessary to heat the object to a high temperature as long as the aqueous solvent is removed. From the viewpoints of cost and ease of operation, it is usually preferable not to heat the object to a high temperature. Specifically, it is preferable not to include a step of heating the object to 200°C or higher after treatment with an inorganic acid-based treatment agent, and it is more preferable not to include a step of heating the object to 150°C or higher.

[0042] In one embodiment, the substrate to which the rust prevention treatment method of the present invention is applied has a film or layer containing a metal or alloy on its surface, for example, a rust prevention film containing zinc, zinc alloy, aluminum, or aluminum alloy. Such a film or layer containing a metal such as zinc or aluminum, or an alloy thereof, can be formed by a known method. For example, a solution or dispersion containing metal particles or alloy particles and a binder resin or a binder resin precursor (such as a monomer or oligomer that polymerizes or hardens to form a binder resin) can be applied to the surface of the substrate, followed by heating to a high temperature to remove the solvent and, in the case of a binder resin precursor, to polymerize or harden it. The heat treatment temperature when forming this metal or alloy-containing film or layer is often above 250°C, or even above 300°C.

[0043] When the article to be treated has a film or layer containing a metal or alloy on its surface, it can be heated to a temperature exceeding 250°C, or even exceeding 300°C, as described above, to form a film or layer containing a metal or alloy on the surface of the article to be treated, and then, without cooling, the article can be treated with an inorganic acid-based treatment agent (an aqueous solution containing an inorganic acid or an inorganic salt) while still at a temperature exceeding 250°C, or while slightly cooled naturally to a temperature exceeding 180°C. Carrying out the rust prevention treatment method of the present invention in this manner is preferable because it eliminates the need to cool or reheat the article to be treated after forming a film or layer containing a metal or alloy on its surface, thereby shortening the process.

[0044] The method for forming an anti-corrosion film containing zinc, a zinc alloy, aluminum, or an aluminum alloy on the surface of the article to be treated is not particularly limited, but it can be suitably formed, for example, by the methods described in JP-A-2005-200678 and JP-A-2006-52361. [Example]

[0045] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0046] Example 1 A zinc flake-based basecoat treatment was prepared by uniformly mixing the following ingredients: Deionized water 39.06% by mass Zinc flakes 32.12% by mass Aluminum flakes 5.08% by mass DPG (dipropylene glycol) 10.29% by mass Synperonic® 13 / 6.5 3.15% by weight Silquest® A187 8.66% by weight Schwego foam (registered trademark) 0.40% by mass Nipar® S10 0.71% by weight Aerosol® TR70 0.53% by weight

[0047] The products listed above are listed under the following trade names: Synperonic® 13 / 6.5: Polyoxyethylene (6.5) Isotridecanol Surfactant Silquest® A187: gamma-glycidoxypropyltrimethoxysilane Schwego foam®: Defoamer Nipar® S10: 1-Nitropropane Aerosol® TR70: Anionic surfactant (bistridecylsodium sulfosuccinate)

[0048] Furthermore, sodium silicate was dissolved in deionized water to prepare 150 ml of a 3% by mass aqueous solution of sodium silicate as an immersion treatment agent. The pH of the prepared immersion treatment agent was 11.4.

[0049] Next, five M6 hex flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method (dip spin method) with centrifugal shake-off. After that, they were preheated in an electric furnace at 100°C for 10 minutes, and then baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum. The coating weight was 6 g / m 2 Hereinafter, the treatment for forming the coating containing zinc and aluminum will be referred to as the "base treatment."

[0050] The five bolts were removed from the electric furnace and their surface temperatures were confirmed to be between 265°C and 300°C using an infrared radiation thermometer. They were then immersed in 150 ml of the prepared 3% by mass sodium silicate aqueous solution at a liquid temperature of 20°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0051] The base treatment (coating weight 6 g / m) prepared in this way 2) and immersion treatment (sodium silicate aqueous solution; bolt surface temperature 265°C-300°C), five bolts were subjected to a salt spray test in accordance with JIS Z-2371, and the bolts were checked for rust every 168 hours from the start of the test to evaluate their corrosion resistance. As a result, at 840 hours after the start of the salt spray test, no rust was found on any of the five bolts, but at 1008 hours after the start of the test, rust was found on only one bolt.

[0052] <Comparative Example 1> Five bolts that had been subjected to only the base treatment were produced in the same manner as in Example 1, except that after the base treatment, the bolts were not immersed in a 3 mass % sodium silicate aqueous solution, but were simply cooled to room temperature.

[0053] The base treatment (coating weight 6 g / m) prepared in this way 2 ) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and corrosion resistance was evaluated. As a result, rust was confirmed in two of the five bolts 168 hours after the start of the salt spray test. Rust was confirmed in three or more bolts, more than half of the bolts, 336 hours after the start of the test.

[0054] <Example 2> During base treatment, the coating weight of the zinc and aluminum-containing coating was increased to 8 g / m by changing the rotation speed when applying and centrifuging the coating using the dip spin method. 2 Five bolts were produced by the base treatment and immersion treatment in the same manner as in Example 1, except that the above-mentioned was changed to the above.

[0055] The base treatment (coating weight 8g / m) prepared in this way 2 Five bolts that had been subjected to the immersion treatment (sodium silicate aqueous solution; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, no rust was found on any of the five bolts even 1008 hours after the start of the salt spray test.

[0056] <Comparative Example 2> Five bolts that had been subjected to only the base treatment were produced in the same manner as in Example 2, except that after the base treatment, the bolts were not immersed in a 3 mass % sodium silicate aqueous solution, but were simply cooled to room temperature.

[0057] The base treatment (coating weight 8g / m) prepared in this way 2 ) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and corrosion resistance was evaluated. As a result, rust was confirmed in two of the five bolts 168 hours after the start of the salt spray test. Rust was confirmed in three or more bolts, more than half of the bolts, 336 hours after the start of the test.

[0058] Example 3 During base treatment, the coating weight of the zinc and aluminum-containing coating was increased to 10 g / m by changing the rotation speed when applying and centrifuging the coating using the dip spin method. 2 Five bolts were produced by the base treatment and immersion treatment in the same manner as in Example 1, except that the above-mentioned was changed to the above.

[0059] The base treatment (coating weight 10 g / m) prepared in this way 2 Five bolts that had been subjected to the immersion treatment (sodium silicate aqueous solution; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, no rust was found on any of the five bolts even 1008 hours after the start of the salt spray test.

[0060] <Comparative Example 3> Five bolts that had been subjected to only the base treatment were produced in the same manner as in Example 3, except that after the base treatment, the bolts were not immersed in a 3 mass % sodium silicate aqueous solution, but were simply cooled to room temperature.

[0061] The base treatment (coating weight 10 g / m) prepared in this way2 ) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1 to evaluate corrosion resistance. As a result, no rust was observed in any of the five bolts 168 hours after the start of the salt spray test, but rust was observed in more than half of the bolts (three or more bolts) 336 hours after the start of the test.

[0062] Example 4 During base treatment, the coating weight of the zinc and aluminum-containing coating was increased to 12 g / m by changing the rotation speed when applying and centrifuging the coating using the dip spin method. 2 Five bolts were produced by the base treatment and immersion treatment in the same manner as in Example 1, except that the above-mentioned was changed to the above.

[0063] The base treatment (coating weight 12 g / m) prepared in this way 2 Five bolts that had been subjected to a salt spray test in accordance with JIS Z-2371 and immersion treatment (sodium silicate aqueous solution; bolt surface temperature 265°C to 300°C) were subjected to the same salt spray test as in Example 1, and their corrosion resistance was evaluated. As a result, even at 1008 hours after the start of the salt spray test, no rust was observed on any of the five bolts. Even at 1176 hours after the start of the test, no rust was observed on any of the five bolts, and at 1344 hours after the start of the test, rust was observed on only one bolt. Even at 2016 hours after the start of the test, rust was observed on only one bolt.

[0064] <Comparative Example 4> Five bolts that had been subjected to only the base treatment were produced in the same manner as in Example 4, except that after the base treatment, the bolts were not immersed in a 3 mass % sodium silicate aqueous solution, but were simply cooled to room temperature.

[0065] The base treatment (coating weight 12 g / m) prepared in this way 2) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1 to evaluate corrosion resistance. As a result, no rust was observed in any of the five bolts 168 hours after the start of the salt spray test, but rust was observed in two bolts 336 hours after the start of the test. At 504 hours after the start of the test, rust was observed in three or more bolts, more than half of the bolts.

[0066] <Example 5> As an immersion treatment agent, sodium silicate was dissolved in deionized water to prepare 150 ml of a 0.1 mass % sodium silicate aqueous solution. The pH of the prepared immersion treatment agent was 10.2. Five bolts that had been subjected to the base treatment and immersion treatment were produced in the same manner as in Example 4, except that the immersion treatment was carried out using 150 ml of the prepared 0.1 mass % sodium silicate aqueous solution at a liquid temperature of 20°C instead of 150 ml of the 3 mass % sodium silicate aqueous solution at a liquid temperature of 20°C.

[0067] The base treatment (coating weight 12 g / m) prepared in this way 2 Five bolts that had been subjected to the immersion treatment (0.1 mass % sodium silicate aqueous solution; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, no rust was found on any of the five bolts even 840 hours after the start of the salt spray test.

[0068] Example 6 As an immersion treatment agent, sodium silicate was dissolved in deionized water to prepare 150 ml of a 0.3 mass % sodium silicate aqueous solution. The pH of the prepared immersion treatment agent was 10.3. Five bolts that had been subjected to the base treatment and immersion treatment were produced in the same manner as in Example 4, except that the immersion treatment was carried out using 150 ml of the prepared 0.3 mass % sodium silicate aqueous solution at a liquid temperature of 20°C instead of 150 ml of the 3 mass % sodium silicate aqueous solution at a liquid temperature of 20°C.

[0069] The base treatment (coating weight 12 g / m) prepared in this way2 Five bolts that had been subjected to a dipping treatment (0.3 mass % sodium silicate aqueous solution; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, even 840 hours after the start of the salt spray test, no rust was observed in any of the five bolts. At 1008 hours after the start of the test, rust was observed in one bolt, and even at 1344 hours after the start of the test, rust was still observed in only one bolt.

[0070] Example 7 As an immersion treatment agent, sodium silicate was dissolved in deionized water to prepare 150 ml of a 0.5 mass % sodium silicate aqueous solution. The pH of the prepared immersion treatment agent was 10.9. Five bolts that had been subjected to the base treatment and immersion treatment were produced in the same manner as in Example 4, except that the immersion treatment was carried out using 150 ml of the prepared 0.5 mass % sodium silicate aqueous solution at a liquid temperature of 20°C instead of 150 ml of the 3 mass % sodium silicate aqueous solution at a liquid temperature of 20°C.

[0071] The base treatment (coating weight 12 g / m) prepared in this way 2 Five bolts that had been subjected to a dipping treatment (0.5 mass % sodium silicate aqueous solution; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, even 1680 hours after the start of the salt spray test, no rust was observed in any of the five bolts. At 1848 hours after the start of the test, rust was observed in one bolt, and even at 2016 hours after the start of the test, rust was still observed in only one bolt.

[0072] Example 8 As an immersion treatment agent, sodium silicate was dissolved in deionized water to prepare 150 ml of a 1 mass % sodium silicate aqueous solution. The pH of the prepared immersion treatment agent was 11.1. Five bolts that had been subjected to the base treatment and immersion treatment were produced in the same manner as in Example 4, except that the immersion treatment was carried out using 150 ml of the prepared 1 mass % sodium silicate aqueous solution at a liquid temperature of 20°C instead of 150 ml of the 3 mass % sodium silicate aqueous solution at a liquid temperature of 20°C.

[0073] The base treatment (coating weight 12 g / m) prepared in this way 2 Five bolts that had been subjected to the immersion treatment (1 mass % sodium silicate aqueous solution; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, no rust was found on any of the five bolts even 2184 hours after the start of the salt spray test.

[0074] Example 9 As an immersion treatment agent, sodium silicate was dissolved in deionized water to prepare 150 ml of a 5 mass % sodium silicate aqueous solution. The pH of the prepared immersion treatment agent was 11.5. Five bolts that had been subjected to the base treatment and immersion treatment were produced in the same manner as in Example 4, except that the immersion treatment was carried out using 150 ml of the prepared 5 mass % sodium silicate aqueous solution at a liquid temperature of 20°C instead of 150 ml of the 3 mass % sodium silicate aqueous solution at a liquid temperature of 20°C.

[0075] The base treatment (coating weight 12 g / m) prepared in this way 2 Five bolts that had been subjected to the immersion treatment (5 mass% sodium silicate aqueous solution; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, no rust was found on any of the five bolts even 1176 hours after the start of the salt spray test.

[0076] Example 10 As an immersion treatment agent, sodium silicate was dissolved in deionized water to prepare 150 ml of a 10 mass % sodium silicate aqueous solution. The pH of the prepared immersion treatment agent was 11.6. Five bolts that had been subjected to the base treatment and immersion treatment were produced in the same manner as in Example 4, except that the immersion treatment was carried out using 150 ml of the prepared 10 mass % sodium silicate aqueous solution at a liquid temperature of 20°C instead of 150 ml of the 3 mass % sodium silicate aqueous solution at a liquid temperature of 20°C.

[0077] The base treatment (coating weight 12 g / m) prepared in this way 2 Five bolts that had been subjected to a dipping treatment (10% by mass sodium silicate aqueous solution; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, even 1680 hours after the start of the salt spray test, no rust was observed in any of the five bolts. At 1848 hours after the start of the test, rust was observed in one bolt, and even at 2016 hours after the start of the test, rust was still observed in only one bolt.

[0078] Example 11 As an immersion treatment agent, sodium silicate was dissolved in deionized water to prepare 150 ml of a 15 mass % sodium silicate aqueous solution. The pH of the prepared immersion treatment agent was 11.6. Five bolts that had been subjected to the base treatment and immersion treatment were produced in the same manner as in Example 4, except that the immersion treatment was carried out using 150 ml of the prepared 15 mass % sodium silicate aqueous solution at a liquid temperature of 20°C instead of 150 ml of the 3 mass % sodium silicate aqueous solution at a liquid temperature of 20°C.

[0079] The base treatment (coating weight 12 g / m) prepared in this way 2Five bolts that had been subjected to a dipping treatment (15% by mass sodium silicate aqueous solution; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, even 1680 hours after the start of the salt spray test, no rust was observed in any of the five bolts. At 1848 hours after the start of the test, rust was observed in one bolt, and even at 2016 hours after the start of the test, rust was still observed in only one bolt.

[0080] Example 12 As an immersion treatment agent, sodium dihydrogen phosphate was dissolved in deionized water to prepare 150 ml of a 5 mass % aqueous solution of sodium dihydrogen phosphate. The pH of the prepared immersion treatment agent was 4.3. Five bolts that had been subjected to the base treatment and immersion treatment were produced in the same manner as in Example 4, except that the immersion treatment was carried out using 150 ml of the prepared 5 mass % aqueous solution of sodium dihydrogen phosphate at a liquid temperature of 20°C instead of 150 ml of the 3 mass % aqueous solution of sodium silicate at a liquid temperature of 20°C.

[0081] The base treatment (coating weight 12 g / m) prepared in this way 2 Five bolts that had been subjected to the immersion treatment (sodium dihydrogen phosphate aqueous solution; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, no rust was found on any of the five bolts even 1008 hours after the start of the salt spray test.

[0082] Example 13 As an immersion treatment agent, ammonium zirconium carbonate ("Baycoat 20" (trade name) manufactured by Nippon Light Metal Co., Ltd.) was dissolved in deionized water to prepare 150 ml of a 5 mass % aqueous solution of ammonium zirconium carbonate. The pH of the prepared immersion treatment agent was 9.2. Five bolts that had been subjected to the base treatment and immersion treatment were produced in the same manner as in Example 4, except that the immersion treatment was carried out using 150 ml of the prepared 5 mass % aqueous solution of ammonium zirconium carbonate at a liquid temperature of 20°C instead of 150 ml of the 3 mass % aqueous solution of sodium silicate at a liquid temperature of 20°C.

[0083] The base treatment (coating weight 12 g / m) prepared in this way 2 Five bolts that had been subjected to a dipping treatment (ammonium zirconium carbonate aqueous solution; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, even at 1008 hours after the start of the salt spray test, no rust was observed on any of the five bolts, and at 1176 hours after the start of the test, rust was observed on only one bolt.

[0084] Example 14 As an immersion treatment agent, sodium nitrate was dissolved in deionized water to prepare 150 ml of a 5 mass % sodium nitrate aqueous solution. The pH of the prepared immersion treatment agent was 6.8. Five bolts that had been subjected to the base treatment and immersion treatment were produced in the same manner as in Example 4, except that the immersion treatment was performed using 150 ml of the prepared 5 mass % sodium nitrate aqueous solution at a liquid temperature of 20°C instead of 150 ml of the 3 mass % sodium silicate aqueous solution at a liquid temperature of 20°C.

[0085] The base treatment (coating weight 12 g / m) prepared in this way 2Five bolts that had been subjected to a dipping treatment (sodium nitrate aqueous solution; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, even 504 hours after the start of the salt spray test, no rust was observed on any of the five bolts, and at 672 hours after the start of the test, rust was observed on only one bolt.

[0086] Example 15 As an immersion treatment agent, potassium sulfate was dissolved in deionized water to prepare 150 ml of a 5 mass % potassium sulfate aqueous solution. The pH of the prepared immersion treatment agent was 5.8. Five bolts that had been subjected to the base treatment and immersion treatment were produced in the same manner as in Example 4, except that the immersion treatment was carried out using 150 ml of the prepared 5 mass % potassium sulfate aqueous solution at a liquid temperature of 20°C instead of 150 ml of the 3 mass % sodium silicate aqueous solution at a liquid temperature of 20°C.

[0087] The base treatment (coating weight 12 g / m) prepared in this way 2 Five bolts that had been subjected to the immersion treatment (potassium sulfate aqueous solution; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, no rust was found on any of the five bolts even 504 hours after the start of the salt spray test.

[0088] Example 16 As an immersion treatment agent, sodium molybdate was dissolved in deionized water to prepare 150 ml of a 5 mass % sodium molybdate aqueous solution. The pH of the prepared immersion treatment agent was 8.1. Five bolts that had been subjected to the base treatment and immersion treatment were produced in the same manner as in Example 4, except that the immersion treatment was performed using 150 ml of the prepared 5 mass % sodium molybdate aqueous solution at a liquid temperature of 20°C instead of 150 ml of the 3 mass % sodium silicate aqueous solution at a liquid temperature of 20°C.

[0089] The base treatment (coating weight 12 g / m) prepared in this way 2) and immersion treatment (sodium molybdate aqueous solution; bolt surface temperature 265°C to 300°C), five bolts were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, even 336 hours after the start of the salt spray test, no rust was observed on any of the five bolts, and at 504 hours after the start of the test, rust was observed on only one bolt.

[0090] <Comparative Example 5> A silane coupling agent ("A187T" manufactured by Momentive Performance Materials Japan, LLC) was dissolved in deionized water to prepare 150 ml of a 5% by mass aqueous solution of the silane coupling agent. Five bolts were subjected to the base treatment and immersion treatment in the same manner as in Example 4, except that the immersion treatment was carried out using 150 ml of the prepared 5% by mass aqueous solution of the silane coupling agent at a liquid temperature of 20°C instead of 150 ml of the 3% by mass aqueous solution of sodium silicate at a liquid temperature of 20°C.

[0091] The base treatment (coating weight 12 g / m) prepared in this way 2 ) and immersion treatment (silane coupling agent aqueous solution; bolt surface temperature 265°C to 300°C), five bolts were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and corrosion resistance was evaluated. As a result, no rust was observed in any of the five bolts 168 hours after the start of the salt spray test, but rust was observed in one bolt 336 hours after the start of the test. At 504 hours after the start of the test, rust was observed in more than half of the bolts (three or more bolts).

[0092] Example 17 During base treatment, the coating weight of the zinc and aluminum-containing coating was increased to 14 g / m by changing the rotation speed when applying and centrifuging the coating using the dip spin method. 2 Five bolts were produced by the base treatment and immersion treatment in the same manner as in Example 1, except that the above-mentioned was changed to the above.

[0093] The base treatment (coating weight 14 g / m) prepared in this way 2 Five bolts that had been subjected to the immersion treatment (sodium silicate aqueous solution; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, no rust was found on any of the five bolts even 1008 hours after the start of the salt spray test.

[0094] <Comparative Example 6> Five bolts that had been subjected to only the base treatment were produced in the same manner as in Example 17, except that after the base treatment, the bolts were not immersed in a 3 mass % sodium silicate aqueous solution, but were simply cooled to room temperature.

[0095] The base treatment (coating weight 14 g / m) prepared in this way 2 ) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1 to evaluate corrosion resistance. As a result, no rust was observed in any of the five bolts 168 hours after the start of the salt spray test, but rust was observed in two bolts 336 hours after the start of the test. At 504 hours after the start of the test, rust was observed in three or more bolts, more than half of the bolts.

[0096] Example 18 As an immersion treatment agent, sodium dihydrogen phosphate was dissolved in deionized water to prepare 150 ml of a 5 mass % aqueous solution of sodium dihydrogen phosphate. The pH of the prepared immersion treatment agent was 4.3. Five bolts that had been subjected to the base treatment and immersion treatment were produced in the same manner as in Example 17, except that the immersion treatment was carried out using 150 ml of the prepared 5 mass % aqueous solution of sodium dihydrogen phosphate at a liquid temperature of 20°C instead of 150 ml of the 3 mass % aqueous solution of sodium silicate at a liquid temperature of 20°C.

[0097] The base treatment (coating weight 14 g / m) prepared in this way 2Five bolts that had been subjected to the immersion treatment (sodium dihydrogen phosphate aqueous solution; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, no rust was found on any of the five bolts even 840 hours after the start of the salt spray test.

[0098] Example 19 As an immersion treatment agent, potassium sulfate was dissolved in deionized water to prepare 150 ml of a 5 mass % potassium sulfate aqueous solution. The pH of the prepared immersion treatment agent was 5.8. Five bolts that had been subjected to the base treatment and immersion treatment were produced in the same manner as in Example 17, except that the immersion treatment was carried out using 150 ml of the prepared 5 mass % potassium sulfate aqueous solution at a liquid temperature of 20°C instead of 150 ml of the 3 mass % sodium silicate aqueous solution at a liquid temperature of 20°C.

[0099] The base treatment (coating weight 14 g / m) prepared in this way 2 Five bolts that had been subjected to the immersion treatment (potassium sulfate aqueous solution; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, no rust was found on any of the five bolts even 672 hours after the start of the salt spray test.

[0100] <Comparative Example 7> As an immersion treatment agent, sodium citrate was dissolved in deionized water to prepare 150 ml of a 5 mass % sodium citrate aqueous solution. Five bolts that had been subjected to the base treatment and immersion treatment were produced in the same manner as in Example 17, except that the immersion treatment was carried out using 150 ml of the prepared 5 mass % sodium citrate aqueous solution at a liquid temperature of 20°C instead of 150 ml of the 3 mass % sodium silicate aqueous solution at a liquid temperature of 20°C.

[0101] The base treatment (coating weight 14 g / m) prepared in this way 2) and immersion treatment (sodium citrate aqueous solution; bolt surface temperature 265°C to 300°C), five bolts were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and corrosion resistance was evaluated. As a result, rust was confirmed in more than half of the bolts (three or more bolts) 168 hours after the start of the salt spray test.

[0102] Example 20 During base treatment, the coating weight of the zinc and aluminum-containing coating was increased to 18 g / m by changing the rotation speed when applying and centrifuging the coating using the dip spin method. 2 Five bolts were produced by the base treatment and immersion treatment in the same manner as in Example 1, except that the above-mentioned was changed to the above.

[0103] The base treatment (coating weight 18 g / m) prepared in this way 2 Five bolts that had been subjected to a dipping treatment (sodium silicate aqueous solution; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, even 1008 hours after the start of the salt spray test, no rust was observed on any of the five bolts. Even 1848 hours after the start of the test, no rust was observed on any of the five bolts, and at 2016 hours after the start of the test, rust was observed on only one bolt.

[0104] <Comparative Example 8> Five bolts that had been subjected to only the base treatment were produced in the same manner as in Example 20, except that after the base treatment, the bolts were not immersed in a 3 mass % sodium silicate aqueous solution, but were cooled to room temperature.

[0105] The base treatment (coating weight 18 g / m) prepared in this way 2) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1 to evaluate corrosion resistance. As a result, no rust was observed in any of the five bolts 504 hours after the start of the salt spray test, but rust was observed in more than half of the bolts (three or more bolts) 672 hours after the start of the test.

[0106] <Example 21> As an immersion treatment agent, lithium silicate was dissolved in deionized water to prepare 150 ml of a 3 mass % lithium silicate aqueous solution. The pH of the prepared immersion treatment agent was 11.0. Five bolts that had been subjected to the base treatment and immersion treatment were produced in the same manner as in Example 20, except that the immersion treatment was carried out using 150 ml of the prepared 3 mass % lithium silicate aqueous solution at a liquid temperature of 20°C instead of 150 ml of the 3 mass % sodium silicate aqueous solution at a liquid temperature of 20°C.

[0107] The base treatment (coating weight 18 g / m) prepared in this way 2 Five bolts that had been subjected to a dipping treatment (lithium silicate aqueous solution; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, even 2184 hours after the start of the salt spray test, no rust was observed on any of the five bolts. At 2352 hours after the start of the test, rust was observed on one bolt.

[0108] <Example 22> As an immersion treatment agent, potassium silicate was dissolved in deionized water to prepare 150 ml of a 3 mass % potassium silicate aqueous solution. The pH of the prepared immersion treatment agent was 11.4. Five bolts that had been subjected to the base treatment and immersion treatment were produced in the same manner as in Example 20, except that the immersion treatment was carried out using 150 ml of the prepared 3 mass % potassium silicate aqueous solution at a liquid temperature of 20°C instead of 150 ml of the 3 mass % sodium silicate aqueous solution at a liquid temperature of 20°C.

[0109] The base treatment (coating weight 18 g / m) prepared in this way 2Five bolts that had been subjected to a salt spray test in accordance with JIS Z-2371 and immersion treatment (potassium silicate aqueous solution; bolt surface temperature 265°C to 300°C) were subjected to the same salt spray test as in Example 1, and their corrosion resistance was evaluated. As a result, even after 1,848 hours from the start of the salt spray test, no rust was observed on any of the five bolts. After 2,016 hours from the start of the test, rust was observed on one bolt, and even after 2,352 hours from the start of the test, rust was still observed on only one bolt.

[0110] Example 23 After carrying out the base treatment in the same manner as in Example 4, five bolts were removed from the electric furnace and their surface temperatures were confirmed to be 265°C to 300°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 3% by mass sodium silicate aqueous solution at a liquid temperature of 0°C for approximately 60 seconds, then removed and dried to produce five bolts that had undergone the base treatment and immersion treatment.

[0111] The base treatment (coating weight 12 g / m) prepared in this way 2 ) and immersion treatment (0°C sodium silicate aqueous solution; bolt surface temperature 265°C to 300°C), five bolts were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and corrosion resistance was evaluated. As a result, even at 1176 hours after the start of the salt spray test, no rust was observed on any of the five bolts, and even at 1680 hours after the start of the test, rust was only observed on one bolt.

[0112] Example 24 Five bolts were prepared by base treatment and immersion treatment in the same manner as in Example 23, except that the temperature of the immersion treatment agent, 150 ml of 3 mass % sodium silicate aqueous solution, was changed to 50°C.

[0113] The base treatment (coating weight 12 g / m) prepared in this way 2Five bolts that had been subjected to a dipping treatment (a sodium silicate aqueous solution at 50°C; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, even after 1176 hours from the start of the salt spray test, no rust was observed on any of the five bolts, and even after 1680 hours from the start of the test, rust was only observed on one bolt.

[0114] Example 25 Five bolts were prepared by base treatment and immersion treatment in the same manner as in Example 23, except that the temperature of the immersion treatment agent, 150 ml of 3 mass % sodium silicate aqueous solution, was changed to 90°C.

[0115] The base treatment (coating weight 12 g / m) prepared in this way 2 Five bolts that had been subjected to the immersion treatment (a 90°C sodium silicate aqueous solution; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, no rust was found on any of the five bolts even 1176 hours after the start of the salt spray test.

[0116] <Example 26> After carrying out the base treatment in the same manner as in Example 4, five bolts were removed from the electric furnace and their surface temperatures were confirmed to be 265°C to 300°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 3% by mass aqueous solution of sodium dihydrogen phosphate at a liquid temperature of 0°C for approximately 60 seconds, then removed and dried to produce five bolts that had undergone the base treatment and immersion treatment.

[0117] The base treatment (coating weight 12 g / m) prepared in this way 2Five bolts that had been subjected to a dipping treatment (aqueous sodium dihydrogen phosphate solution at 0°C; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, even after 1176 hours from the start of the salt spray test, no rust was observed on any of the five bolts, and even after 1680 hours from the start of the test, rust was only observed on one bolt.

[0118] Example 27 Five bolts were produced that had undergone base treatment and immersion treatment in the same manner as in Example 26, except that the liquid temperature of the immersion treatment agent, 150 ml of 3 mass % sodium dihydrogen phosphate aqueous solution, was changed to 50°C.

[0119] The base treatment (coating weight 12 g / m) prepared in this way 2 ) and immersion treatment (50°C sodium dihydrogen phosphate aqueous solution; bolt surface temperature 265°C to 300°C), five bolts were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, even 840 hours after the start of the salt spray test, no rust was observed on any of the five bolts, and even 1176 hours after the start of the test, rust was only observed on one bolt.

[0120] Example 28 After carrying out the base treatment in the same manner as in Example 4, five bolts were removed from the electric furnace and their surface temperatures were confirmed to be 265°C to 300°C using an infrared radiation thermometer. They were then immersed for approximately 10 seconds in a 3% by mass aqueous solution of sodium silicate at a liquid temperature of 25°C, with a weight equal to one time the total weight of the bolts to be immersed, and then removed and dried to produce five bolts that had undergone the base treatment and immersion treatment.

[0121] The base treatment (coating weight 12 g / m) prepared in this way 2Five bolts that had been subjected to a dipping treatment (a sodium silicate aqueous solution with a weight equal to one time of the total weight of the bolts; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, no rust was found on any of the five bolts even 2,352 hours after the start of the salt spray test.

[0122] Example 29 Five bolts were prepared by base treatment and immersion treatment in the same manner as in Example 28, except that the amount of immersion treatment agent, a 3% by mass aqueous solution of sodium silicate, was changed to three times the total weight of the bolts.

[0123] The base treatment (coating weight 12 g / m) prepared in this way 2 ) and immersion treatment (a sodium silicate aqueous solution with a weight three times the total weight of the bolts; bolt surface temperature 265°C to 300°C), a salt spray test was conducted in accordance with JIS Z-2371 in the same manner as in Example 1 to evaluate corrosion resistance. As a result, no rust was found on any of the five bolts even 2352 hours after the start of the salt spray test.

[0124] Example 30 Five bolts were prepared by base treatment and immersion treatment in the same manner as in Example 28, except that the amount of immersion treatment agent, a 3% by mass aqueous solution of sodium silicate, was changed to five times the total weight of the bolts.

[0125] The base treatment (coating weight 12 g / m) prepared in this way 2 ) and immersion treatment (sodium silicate aqueous solution with a weight five times the total weight of the bolts; bolt surface temperature 265°C to 300°C), a salt spray test was conducted in accordance with JIS Z-2371 in the same manner as in Example 1 to evaluate corrosion resistance. As a result, no rust was found on any of the five bolts even 2520 hours after the start of the salt spray test.

[0126] Example 31 Five bolts were prepared by base treatment and immersion treatment in the same manner as in Example 28, except that the amount of immersion treatment agent, a 3% by mass aqueous solution of sodium silicate, was changed to a weight 10 times the total weight of the bolts.

[0127] The base treatment (coating weight 12 g / m) prepared in this way 2 ) and immersion treatment (a sodium silicate aqueous solution with a weight 10 times the total weight of the bolts; bolt surface temperature 265°C to 300°C), a salt spray test was conducted in accordance with JIS Z-2371 in the same manner as in Example 1 to evaluate corrosion resistance. As a result, even 2016 hours after the start of the salt spray test, no rust was confirmed in any of the five bolts, and even 2352 hours after the start of the test, rust was confirmed in only one bolt.

[0128] <Comparative Example 9> In the same manner as in Example 1, a base coat treatment agent containing zinc flakes as the main component was prepared.

[0129] Next, five M6 hex flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method (dip spin method) with centrifugal shake-off. After that, they were preheated in an electric furnace at 100°C for 10 minutes, and then baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum. The coating weight was 12 g / m 2 Hereinafter, the treatment for forming the coating containing zinc and aluminum will be referred to as the "base treatment."

[0130] The five bolts were then removed from the electric furnace and allowed to cool to room temperature, producing five bolts that had only been subjected to the base treatment.

[0131] Five of the thus-prepared bolts that had been subjected to only the base treatment were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, in the same manner as in Example 1. As a result, no rust was observed in any of the five bolts 168 hours after the start of the salt spray test, but rust was observed in two bolts 336 hours after the start of the test, and rust was observed in three or more bolts, more than half of the bolts, 504 hours after the start of the test.

[0132] Example 32 As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0133] The five bolts were then removed from the electric furnace and allowed to cool to room temperature (approximately 25°C), after which they were immersed in 150 ml of a 3% by mass sodium silicate aqueous solution (pH 11.5) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0134] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (sodium silicate aqueous solution; bolt surface temperature: room temperature (approximately 25°C)) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, even 672 hours after the start of the salt spray test, no rust was observed in any of the five bolts, and even 840 hours after the start of the test, rust was only observed in two bolts.

[0135] Example 33 As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0136] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 35°C and 60°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 3% by mass sodium silicate aqueous solution (pH 11.5) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0137] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (sodium silicate aqueous solution; bolt surface temperature 35°C to 60°C) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, even after 840 hours from the start of the salt spray test, no rust was observed in any of the five bolts, and even after 1008 hours from the start of the test, rust was only observed in two bolts.

[0138] Example 34 As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0139] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 65°C and 100°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 3% by mass sodium silicate aqueous solution (pH 11.5) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0140] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (sodium silicate aqueous solution; bolt surface temperature 65°C to 100°C) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, even 672 hours after the start of the salt spray test, no rust was observed in any of the five bolts, and even 840 hours after the start of the test, rust was only observed in two bolts.

[0141] Example 35 As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0142] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 105°C and 140°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 3% by mass sodium silicate aqueous solution (pH 11.5) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0143] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (sodium silicate aqueous solution; bolt surface temperature 105°C to 140°C) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, even 672 hours after the start of the salt spray test, no rust was observed in any of the five bolts, and even 840 hours after the start of the test, rust was only observed in two bolts.

[0144] Example 36 As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0145] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 145°C and 180°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 3% by mass sodium silicate aqueous solution (pH 11.5) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0146] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (sodium silicate aqueous solution; bolt surface temperature 145°C to 180°C) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, even 672 hours after the start of the salt spray test, no rust was observed in any of the five bolts, and at 840 hours after the start of the test, rust was observed in only one bolt. Even at 1008 hours after the start of the test, rust was observed in only one bolt.

[0147] Example 37 As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0148] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 185°C and 220°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 3% by mass sodium silicate aqueous solution (pH 11.5) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0149] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (sodium silicate aqueous solution; bolt surface temperature 185°C to 220°C) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, even at 1176 hours after the start of the salt spray test, no rust was observed in any of the five bolts, and even at 1344 hours after the start of the test, rust was only observed in one bolt.

[0150] Example 38 As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0151] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 225°C and 260°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 3% by mass sodium silicate aqueous solution (pH 11.5) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0152] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (sodium silicate aqueous solution; bolt surface temperature 225°C to 260°C) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, even at 1176 hours after the start of the salt spray test, no rust was observed in any of the five bolts, and even at 1344 hours after the start of the test, rust was only observed in one bolt.

[0153] Example 39 As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0154] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 265°C and 300°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 3% by mass sodium silicate aqueous solution (pH 11.5) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0155] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (sodium silicate aqueous solution; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, even at 1176 hours after the start of the salt spray test, no rust was observed in any of the five bolts, and even at 1344 hours after the start of the test, rust was only observed in one bolt.

[0156] <Example 40> As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0157] The five bolts were then removed from the electric furnace and allowed to cool to room temperature (approximately 25°C), after which they were immersed in 150 ml of a 3% by mass aqueous solution of sodium dihydrogen phosphate (pH 4.4) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0158] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (sodium dihydrogen phosphate aqueous solution; bolt surface temperature: room temperature (approximately 25°C)) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, even 336 hours after the start of the salt spray test, no rust was observed in any of the five bolts, and even 504 hours after the start of the test, rust was only observed in two bolts.

[0159] <Example 41> As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0160] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 35°C and 60°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 3% by mass aqueous solution of sodium dihydrogen phosphate (pH 4.4) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0161] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (sodium dihydrogen phosphate aqueous solution; bolt surface temperature 35°C to 60°C) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, even 336 hours after the start of the salt spray test, no rust was observed in any of the five bolts, and even 504 hours after the start of the test, rust was only observed in two bolts.

[0162] <Example 42> As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0163] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 65°C and 100°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 3% by mass aqueous solution of sodium dihydrogen phosphate (pH 4.4) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0164] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (sodium dihydrogen phosphate aqueous solution; bolt surface temperature 65°C to 100°C) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, even 336 hours after the start of the salt spray test, no rust was observed in any of the five bolts, even 504 hours after the start of the test, rust was observed in only one bolt, and even 672 hours after the start of the test, rust was observed in only two bolts.

[0165] <Example 43> As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0166] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 105°C and 140°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 3% by mass aqueous solution of sodium dihydrogen phosphate (pH 4.4) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0167] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (sodium dihydrogen phosphate aqueous solution; bolt surface temperature 105°C to 140°C) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, even 504 hours after the start of the salt spray test, no rust was observed in any of the five bolts, and even 672 hours after the start of the test, rust was only observed in two bolts.

[0168] <Example 44> As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0169] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 145°C and 180°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 3% by mass aqueous solution of sodium dihydrogen phosphate (pH 4.4) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0170] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (sodium dihydrogen phosphate aqueous solution; bolt surface temperature 145°C to 180°C) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, even 504 hours after the start of the salt spray test, no rust was observed in any of the five bolts, even 840 hours after the start of the test, rust was observed in only one bolt, and even 1008 hours after the start of the test, rust was observed in only two bolts.

[0171] Example 45 As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0172] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 185°C and 220°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 3% by mass aqueous solution of sodium dihydrogen phosphate (pH 4.4) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0173] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (sodium dihydrogen phosphate aqueous solution; bolt surface temperature 185°C to 220°C) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, no rust was found on any of the five bolts, even 840 hours after the start of the salt spray test.

[0174] <Example 46> As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0175] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 225°C and 260°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 3% by mass aqueous solution of sodium dihydrogen phosphate (pH 4.4) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0176] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (sodium dihydrogen phosphate aqueous solution; bolt surface temperature 225°C to 260°C) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, even 672 hours after the start of the salt spray test, no rust was observed in any of the five bolts, and even 840 hours after the start of the test, rust was only observed in one bolt.

[0177] Example 47 As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0178] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 265°C and 300°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 3% by mass aqueous solution of sodium dihydrogen phosphate (pH 4.4) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0179] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (sodium dihydrogen phosphate aqueous solution; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, no rust was found on any of the five bolts, even 840 hours after the start of the salt spray test.

[0180] <Example 48> As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0181] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 65°C and 100°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 5% by mass aqueous solution of ammonium zirconium carbonate (pH 9.1) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0182] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (ammonium zirconium carbonate aqueous solution; bolt surface temperature 65°C to 100°C) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, even 336 hours after the start of the salt spray test, no rust was observed in any of the five bolts, even 504 hours after the start of the test, rust was observed in only one bolt, and even 672 hours after the start of the test, rust was observed in only two bolts.

[0183] <Example 49> As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0184] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 105°C and 140°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 5% by mass aqueous solution of zirconium ammonium carbonate (pH 9.1) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0185] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (aqueous solution of ammonium zirconium carbonate; bolt surface temperature 105°C to 140°C) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, even 504 hours after the start of the salt spray test, no rust was observed in any of the five bolts, and even 672 hours after the start of the test, rust was only observed in two bolts.

[0186] Example 50 As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0187] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 145°C and 180°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 5% by mass aqueous solution of zirconium ammonium carbonate (pH 9.1) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0188] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (aqueous solution of ammonium zirconium carbonate; bolt surface temperature 145°C to 180°C) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, even 840 hours after the start of the salt spray test, no rust was observed in any of the five bolts, and even 1008 hours after the start of the test, rust was only observed in one bolt.

[0189] <Example 51> As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0190] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 145°C and 180°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 5% by mass aqueous solution of zirconium ammonium carbonate (pH 9.1) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0191] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (aqueous solution of ammonium zirconium carbonate; bolt surface temperature 145°C to 180°C) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, even 840 hours after the start of the salt spray test, no rust was observed in any of the five bolts, and even 1008 hours after the start of the test, rust was only observed in one bolt.

[0192] <Example 52> As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0193] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 225°C and 260°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 5% by mass aqueous solution of zirconium ammonium carbonate (pH 9.1) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0194] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (ammonium zirconium carbonate aqueous solution; bolt surface temperature 225°C to 260°C) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, no rust was found on any of the five bolts, even 1176 hours after the start of the salt spray test.

[0195] <Example 53> As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0196] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 265°C and 300°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 5% by mass aqueous solution of ammonium zirconium carbonate (pH 9.1) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0197] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (ammonium zirconium carbonate aqueous solution; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, no rust was found on any of the five bolts, even 1176 hours after the start of the salt spray test.

[0198] <Comparative Example 10> As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0199] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 145°C and 180°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 5% by mass potassium sulfate aqueous solution (pH 5.8) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0200] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (potassium sulfate aqueous solution; bolt surface temperature 145°C to 180°C) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, no rust was observed in any of the five bolts 168 hours after the start of the salt spray test, but rust was observed in one bolt 336 hours after the start of the test, and rust was observed in two or more bolts 504 hours after the start of the test.

[0201] <Example 54> As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0202] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 225°C and 260°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 5% by mass potassium sulfate aqueous solution (pH 5.8) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0203] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (potassium sulfate aqueous solution; bolt surface temperature 225°C to 260°C) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, even 336 hours after the start of the salt spray test, no rust was observed in any of the five bolts, even 504 hours after the start of the test, rust was observed in only one bolt, and even 672 hours after the start of the test, rust was observed in only two bolts.

[0204] Example 55 As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0205] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 265°C and 300°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 5% by mass potassium sulfate aqueous solution (pH 5.8) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0206] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (potassium sulfate aqueous solution; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, even 504 hours after the start of the salt spray test, no rust was observed in any of the five bolts, and even 672 hours after the start of the test, rust was only observed in one bolt.

[0207] <Comparative Example 11> As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0208] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 145°C and 180°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 5% by mass sodium nitrate aqueous solution (pH 6.8) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0209] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (sodium nitrate aqueous solution; bolt surface temperature 145°C to 180°C) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, no rust was observed in any of the five bolts 168 hours after the start of the salt spray test, but rust was observed in one bolt 336 hours after the start of the test, and rust was observed in two or more bolts 672 hours after the start of the test.

[0210] Example 56 As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0211] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 225°C and 260°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 5% by mass aqueous solution of sodium nitrate (pH 6.8) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0212] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (sodium nitrate aqueous solution; bolt surface temperature 225°C to 260°C) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, even 336 hours after the start of the salt spray test, no rust was observed in any of the five bolts, even 504 hours after the start of the test, rust was observed in only one bolt, and even 672 hours after the start of the test, rust was observed in only two bolts.

[0213] Example 57 As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0214] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 265°C and 300°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 5% by mass aqueous solution of sodium nitrate (pH 6.8) at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0215] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (sodium nitrate aqueous solution; bolt surface temperature 265°C to 300°C) were subjected to a salt spray test in accordance with JIS Z-2371 to evaluate corrosion resistance, as in Example 1. As a result, even 504 hours after the start of the salt spray test, no rust was observed in any of the five bolts, and even 672 hours after the start of the test, rust was only observed in one bolt.

[0216] <Comparative Example 12> As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0217] The five bolts were then removed from the electric furnace and allowed to cool to room temperature (approximately 25°C), after which they were immersed in 150 ml of a 5% by mass aqueous solution of sodium citrate at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0218] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (sodium citrate aqueous solution; bolt surface temperature: room temperature (approximately 25°C)) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, rust was confirmed in one of the five bolts 168 hours after the start of the salt spray test. Rust was confirmed in two bolts 336 hours after the start of the test.

[0219] <Comparative Example 13> As in Comparative Example 9, five M6 hexagonal flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method with centrifugal shake-off (dip spin method).The bolts were then preheated in an electric furnace at 100°C for 10 minutes and baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum.

[0220] The five bolts were then removed from the electric furnace and their surface temperatures were confirmed to be between 225°C and 260°C using an infrared radiation thermometer. They were then immersed in 150 ml of a 5% by mass sodium citrate aqueous solution at a liquid temperature of 25°C for approximately 10 seconds, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0221] Five bolts thus prepared that had been subjected to the base treatment and immersion treatment (sodium citrate aqueous solution; bolt surface temperature 225°C to 260°C) were subjected to a salt spray test in accordance with JIS Z-2371 in the same manner as in Example 1, and their corrosion resistance was evaluated. As a result, rust was confirmed in one of the five bolts 168 hours after the start of the salt spray test. Rust was confirmed in two bolts 336 hours after the start of the test.

[0222] <Example 58> As an immersion treatment agent, sodium silicate was dissolved in deionized water to prepare a 5% by mass aqueous solution of sodium silicate. The pH of the prepared immersion treatment agent was 11.5 (20°C).

[0223] Next, a cold-rolled steel plate measuring 150 mm × 70 mm × 0.8 mm was degreased with dichloromethane and then heated for 15 minutes in an electric furnace at 330°C. The cold-rolled steel plate was removed from the electric furnace, and its surface temperature was confirmed to be 265°C to 300°C using an infrared radiation thermometer. The plate was then immersed in 150 ml of the prepared 5 mass % sodium silicate aqueous solution at a liquid temperature of 20°C for approximately 10 seconds, then removed and dried.

[0224] The immersion-treated cold-rolled steel sheets were then subjected to a salt spray test in accordance with JIS Z-2371 to evaluate their corrosion resistance. Figures 1A and 1B show photographs of the immersion-treated cold-rolled steel sheets 1 hour and 5 hours after the start of the salt spray test, respectively.

[0225] <Comparative Example 14> A cold-rolled steel sheet for evaluating corrosion resistance was prepared in the same manner as in Example 58, except that after heating in an electric furnace at 330°C for 15 minutes, the sheet was cooled to room temperature without being immersed in an aqueous sodium silicate solution.

[0226] The unimmersed cold-rolled steel sheets were then subjected to a salt spray test in accordance with JIS Z-2371 to evaluate their corrosion resistance. Figures 2A and 2B show photographs of the immersed cold-rolled steel sheets taken 1 hour and 5 hours after the start of the salt spray test, respectively.

[0227] The cold-rolled steel sheet of Example 58, which had been immersed in a sodium silicate aqueous solution, showed less rust formation than the cold-rolled steel sheet of Comparative Example 14, which had not been immersed.

[0228] Example 59 A zinc flake-based basecoat treatment was prepared by uniformly mixing the following ingredients: Deionized water 39.06% by mass Zinc flakes 32.12% by mass Aluminum flakes 5.08% by mass DPG (dipropylene glycol) 10.29% by mass Synperonic® 13 / 6.5 3.15% by weight Silquest® A187 8.66% by weight Schwego foam (registered trademark) 0.40% by mass Nipar® S10 0.71% by weight Aerosol® TR70 0.53% by weight

[0229] The products listed above are listed under the following trade names: Synperonic® 13 / 6.5: Polyoxyethylene (6.5) Isotridecanol Surfactant Silquest® A187: gamma-glycidoxypropyltrimethoxysilane Schwego foam®: Defoamer Nipar® S10: 1-Nitropropane Aerosol® TR70: Anionic surfactant (bistridecylsodium sulfosuccinate)

[0230] As an immersion treatment agent, sodium silicate was dissolved in deionized water so that the sodium silicate content was 1% by mass, to prepare 1000 ml of a 1% by mass aqueous sodium silicate solution.

[0231] Next, five M10 hex flange bolts were vapor degreased with dichloromethane and shot blasted, and then coated with the prepared base coat treatment agent using the immersion method (dip spin method) with centrifugal shake-off. After that, they were preheated in an electric furnace at 100°C for 10 minutes, and then baked in an electric furnace at 330°C for 30 minutes to form a coating containing zinc and aluminum. The coating weight was 14 g / m 2 Hereinafter, the treatment for forming the coating containing zinc and aluminum will be referred to as the "base treatment."

[0232] The five bolts were removed from the electric furnace and their surface temperatures were confirmed to be between 185°C and 220°C using an infrared radiation thermometer. They were then immersed in 1000 ml of the prepared 1% by mass sodium silicate aqueous solution at a liquid temperature of 20°C for approximately one minute, then removed and dried to produce five bolts that had undergone base treatment and immersion treatment.

[0233] The surface friction coefficients of five bolts that had been subjected to the base treatment and immersion treatment (1 mass% sodium silicate aqueous solution; bolt surface temperature 185°C to 220°C) prepared in this manner were measured in accordance with the ISO16047 HH method, and the average value was calculated, resulting in an average friction coefficient of 0.243.

[0234] Furthermore, five bolts that had been subjected to the base treatment and immersion treatment (1 mass % sodium silicate aqueous solution; bolt surface temperature 185°C to 220°C) prepared in this manner were subjected to a salt spray test in accordance with JIS Z-2371, and the occurrence of rust on the bolts was checked every 168 hours from the start of the test to evaluate corrosion resistance. As a result, at 1176 hours after the start of the salt spray test, no rust was confirmed on any of the five bolts, and at 1344 hours after the start of the test, rust was confirmed on only one bolt.

[0235] Example 60 Sodium silicate was used as the immersion treatment agent at 1% by mass, and BYK's "AQUACER 593" (trade name) (hereinafter referred to as "lubricant a") was used as the lubricant at 1% by mass. Sodium silicate and lubricant a were dissolved and mixed in deionized water to prepare 1000 ml of a 1% by mass sodium silicate aqueous solution containing 1% by mass lubricant a. Five bolts were subjected to the base treatment and immersion treatment in the same manner as in Example 59, except that the immersion treatment was carried out using 1000 ml of the prepared 1% by mass sodium silicate aqueous solution containing 1% by mass lubricant a at a liquid temperature of 20°C instead of the 1000 ml of the 1% by mass sodium silicate aqueous solution at a liquid temperature of 20°C. Lubricant a (BYK's "AQUACER 593") is a water-based emulsion based on modified polypropylene wax.

[0236] For five bolts prepared in this manner that had been subjected to base treatment and immersion treatment (1 mass % sodium silicate aqueous solution containing 1 mass % lubricant a; bolt surface temperature 185°C to 220°C), the surface friction coefficients were measured in accordance with the ISO 16047 HH method, as in Example 59, and the average value was calculated, resulting in an average friction coefficient of 0.173.

[0237] Furthermore, five bolts thus prepared that had been subjected to the base treatment and immersion treatment (1 mass % sodium silicate aqueous solution containing 1 mass % lubricant a; bolt surface temperature 185°C to 220°C) were subjected to a salt spray test in accordance with JIS Z-2371, as in Example 59. The bolts were checked for rust every 168 hours from the start of the test to evaluate their corrosion resistance. As a result, no rust was found on any of the five bolts, even 1,176 hours after the start of the salt spray test.

[0238] <Example 61> Sodium silicate and lubricant a were dissolved and mixed in deionized water so that the immersion treatment agent contained 1% by mass of sodium silicate and the lubricant contained 5% by mass of BYK's "AQUACER 593" (trade name) (lubricant a). Five bolts that had been subjected to the base treatment and the immersion treatment were produced in the same manner as in Example 59, except that the immersion treatment was carried out using 1000 ml of the prepared 1% by mass sodium silicate aqueous solution containing 5% by mass of lubricant a at a liquid temperature of 20°C instead of the 1% by mass sodium silicate aqueous solution at a liquid temperature of 20°C.

[0239] For five bolts prepared in this manner that had been subjected to base treatment and immersion treatment (1 mass % sodium silicate aqueous solution containing 5 mass % lubricant a; bolt surface temperature 185°C to 220°C), the surface friction coefficients were measured in accordance with the ISO 16047 HH method, as in Example 59, and the average value was calculated, resulting in an average friction coefficient of 0.154.

[0240] Furthermore, five bolts thus prepared that had been subjected to the base treatment and immersion treatment (1 mass % sodium silicate aqueous solution containing 5 mass % lubricant a; bolt surface temperature 185°C to 220°C) were subjected to a salt spray test in accordance with JIS Z-2371, as in Example 59. The occurrence of rust on the bolts was checked every 168 hours from the start of the test to evaluate corrosion resistance. As a result, no rust was confirmed on any of the five bolts, even 1,176 hours after the start of the salt spray test.

[0241] <Example 62> The immersion treatment agent contained 1% sodium silicate by mass, and the lubricant contained 3% by mass of BYK's "AQUACER 497" (trade name) (hereinafter referred to as "lubricant b") by mass. Sodium silicate and lubricant b were dissolved and mixed in deionized water to prepare 1000 ml of a 1% by mass sodium silicate aqueous solution containing 3% by mass of lubricant b. Five bolts were subjected to the base treatment and immersion treatment in the same manner as in Example 59, except that the immersion treatment was performed using 1000 ml of the prepared 1% by mass sodium silicate aqueous solution containing 3% by mass of lubricant b at a liquid temperature of 20°C instead of the 1% by mass sodium silicate aqueous solution at a liquid temperature of 20°C. Lubricant b (BYK's "AQUACER 497") is a water-based emulsion based on paraffin wax.

[0242] For five bolts prepared in this manner that had been subjected to base treatment and immersion treatment (1 mass % sodium silicate aqueous solution containing 3 mass % lubricant b; bolt surface temperature 185°C to 220°C), the surface friction coefficients were measured in accordance with the ISO 16047 HH method, as in Example 59, and the average value was calculated, resulting in an average friction coefficient of 0.111.

[0243] Furthermore, five bolts thus prepared that had been subjected to the base treatment and immersion treatment (1 mass % sodium silicate aqueous solution containing 3 mass % lubricant b; bolt surface temperature 185°C to 220°C) were subjected to a salt spray test in accordance with JIS Z-2371, as in Example 59. The bolts were checked for rust every 168 hours from the start of the test to evaluate their corrosion resistance. As a result, no rust was found on any of the five bolts, even 1008 hours after the start of the salt spray test.

[0244] <Example 63> Sodium silicate and lubricant b were dissolved and mixed in deionized water so that the immersion treatment agent contained 1% by mass of sodium silicate and the lubricant contained 5% by mass of BYK's "AQUACER 497" (trade name) (lubricant b). 1000 ml of a 1% by mass aqueous solution of sodium silicate containing 5% by mass of lubricant b was prepared. Five bolts that had been subjected to the base treatment and immersion treatment were produced in the same manner as in Example 59, except that the immersion treatment was carried out using 1000 ml of the prepared 1% by mass aqueous solution of sodium silicate containing 5% by mass of lubricant b at a liquid temperature of 20°C instead of the 1% by mass aqueous solution of sodium silicate at a liquid temperature of 20°C.

[0245] For five bolts prepared in this manner that had been subjected to base treatment and immersion treatment (1 mass % sodium silicate aqueous solution containing 5 mass % lubricant b; bolt surface temperature 185°C to 220°C), the surface friction coefficients were measured in accordance with the ISO 16047 HH method, as in Example 59, and the average value was calculated, resulting in an average friction coefficient of 0.098.

[0246] Furthermore, five bolts thus prepared that had been subjected to the base treatment and immersion treatment (1 mass % sodium silicate aqueous solution containing 5 mass % lubricant b; bolt surface temperature 185°C to 220°C) were subjected to a salt spray test in accordance with JIS Z-2371, as in Example 59. The bolts were checked for rust every 168 hours from the start of the test to evaluate their corrosion resistance. As a result, no rust was found on any of the five bolts, even 1008 hours after the start of the salt spray test.

[0247] <Example 64> Sodium silicate was used as the immersion treatment agent at 1% by mass, and BYK's "AQUACER 1547" (trade name) (hereinafter referred to as "lubricant c") was used as the lubricant at 3% by mass. Sodium silicate and lubricant c were dissolved and mixed in deionized water to prepare 1000 ml of a 1% by mass sodium silicate aqueous solution containing 3% by mass lubricant c. Five bolts were subjected to the base treatment and immersion treatment in the same manner as in Example 59, except that the 1000 ml of the 1% by mass sodium silicate aqueous solution containing 3% by mass lubricant c at a liquid temperature of 20°C was used instead of the 1000 ml of the 1% by mass sodium silicate aqueous solution at a liquid temperature of 20°C. Lubricant c (BYK's "AQUACER 1547") is a water-based emulsion based on modified polyethylene wax.

[0248] For five bolts prepared in this manner that had been subjected to base treatment and immersion treatment (1 mass % sodium silicate aqueous solution containing 3 mass % lubricant c; bolt surface temperature 185°C to 220°C), the surface friction coefficients were measured in accordance with the ISO 16047 HH method, as in Example 59, and the average value was calculated, resulting in an average friction coefficient of 0.120.

[0249] Furthermore, five bolts thus prepared that had been subjected to the base treatment and immersion treatment (1 mass % sodium silicate aqueous solution containing 3 mass % lubricant c; bolt surface temperature 185°C to 220°C) were subjected to a salt spray test in accordance with JIS Z-2371, as in Example 59. The occurrence of rust on the bolts was checked every 168 hours from the start of the test to evaluate corrosion resistance. As a result, no rust was confirmed on any of the five bolts, even 1008 hours after the start of the salt spray test.

[0250] Example 65 Sodium silicate and lubricant c were dissolved and mixed in deionized water so that the immersion treatment agent contained 1% by mass of sodium silicate and the lubricant contained 5% by mass of BYK's "AQUACER 1547" (trade name) (lubricant c). 1000 ml of a 1% by mass aqueous solution of sodium silicate containing 5% by mass of lubricant c was prepared. Five bolts that had been subjected to the base treatment and immersion treatment were produced in the same manner as in Example 59, except that the immersion treatment was carried out using 1000 ml of the prepared 1% by mass aqueous solution of sodium silicate containing 5% by mass of lubricant c at a liquid temperature of 20°C instead of the 1% by mass aqueous solution of sodium silicate at a liquid temperature of 20°C.

[0251] For five bolts prepared in this manner that had been subjected to base treatment and immersion treatment (1 mass % sodium silicate aqueous solution containing 5 mass % lubricant c; bolt surface temperature 185°C to 220°C), the surface friction coefficients were measured in accordance with the ISO 16047 HH method, as in Example 59, and the average value was calculated, resulting in an average friction coefficient of 0.105.

[0252] Furthermore, five bolts thus prepared that had been subjected to the base treatment and immersion treatment (a 1% by mass sodium silicate aqueous solution containing 5% by mass of lubricant c; bolt surface temperature 185°C to 220°C) were subjected to a salt spray test in accordance with JIS Z-2371, as in Example 59. The bolts were checked for rust every 168 hours from the start of the test to evaluate their corrosion resistance. As a result, no rust was found on any of the five bolts, even 1008 hours after the start of the salt spray test.

[0253] <Example 66> The immersion treatment agent contained 1% sodium silicate by mass, and the lubricant contained 3% by mass of "Lubron LDW-410" (trade name) manufactured by Daikin Industries, Ltd. (hereinafter referred to as "lubricant d") by mass. Sodium silicate and lubricant d were dissolved and mixed in deionized water to prepare 1000 ml of a 1% by mass sodium silicate aqueous solution containing 3% by mass of lubricant d. Five bolts were subjected to base treatment and immersion treatment in the same manner as in Example 59, except that the immersion treatment was performed using 1000 ml of the 1% by mass sodium silicate aqueous solution containing 3% by mass of lubricant d at a liquid temperature of 20°C instead of the 1% by mass sodium silicate aqueous solution at a liquid temperature of 20°C. Lubricant d ("Lubron LDW-410" manufactured by Daikin Industries, Ltd.) is a dispersion of low-molecular-weight fluororesin particles dispersed in water.

[0254] For five bolts prepared in this manner that had been subjected to base treatment and immersion treatment (1 mass % sodium silicate aqueous solution containing 3 mass % lubricant d; bolt surface temperature 185°C to 220°C), the surface friction coefficients were measured in accordance with the ISO 16047 HH method, as in Example 59, and the average value was calculated, resulting in an average friction coefficient of 0.166.

[0255] Furthermore, five bolts thus prepared that had been subjected to the base treatment and immersion treatment (1 mass % sodium silicate aqueous solution containing 3 mass % lubricant d; bolt surface temperature 185°C to 220°C) were subjected to a salt spray test in accordance with JIS Z-2371, as in Example 59. The occurrence of rust on the bolts was checked every 168 hours from the start of the test to evaluate corrosion resistance. As a result, no rust was confirmed on any of the five bolts, even 1008 hours after the start of the salt spray test.

[0256] Example 67 Sodium silicate and lubricant d were dissolved and mixed in deionized water so that the immersion treatment agent contained 1% by mass of sodium silicate, and the lubricant contained 5% by mass of "Lubron LDW-410" (trade name) manufactured by Daikin Industries, Ltd. (lubricant d). 1000 ml of a 1% by mass aqueous solution of sodium silicate containing 5% by mass of lubricant d was prepared. Five bolts that had been subjected to the base treatment and immersion treatment were produced in the same manner as in Example 59, except that the immersion treatment was carried out using 1000 ml of the prepared 1% by mass aqueous solution of sodium silicate containing 5% by mass of lubricant d at a liquid temperature of 20°C instead of the 1% by mass aqueous solution of sodium silicate at a liquid temperature of 20°C.

[0257] For five bolts prepared in this manner that had been subjected to base treatment and immersion treatment (1 mass % sodium silicate aqueous solution containing 5 mass % lubricant d; bolt surface temperature 185°C to 220°C), the surface friction coefficients were measured in accordance with the ISO 16047 HH method, as in Example 59, and the average value was calculated, resulting in an average friction coefficient of 0.173.

[0258] Furthermore, five bolts thus prepared that had been subjected to the base treatment and immersion treatment (1 mass % sodium silicate aqueous solution containing 5 mass % lubricant d; bolt surface temperature 185°C to 220°C) were subjected to a salt spray test in accordance with JIS Z-2371, as in Example 59. The occurrence of rust on the bolts was checked every 168 hours from the start of the test to evaluate corrosion resistance. As a result, no rust was confirmed on any of the five bolts, even 1008 hours after the start of the salt spray test.

[0259] Example 68 Sodium silicate and lubricant a were dissolved and mixed in deionized water so that the immersion treatment agent contained 1% by mass of sodium silicate and the lubricant contained 3% by mass of BYK's "AQUACER 593" (trade name) (lubricant a). Five bolts that underwent base treatment and immersion treatment were produced in the same manner as in Example 59, except that the immersion treatment was performed at a surface temperature of 235°C to 270°C using 1000 ml of the prepared 1% by mass sodium silicate aqueous solution containing 3% by mass of lubricant a, instead of the 1000 ml of the 1% by mass sodium silicate aqueous solution at a liquid temperature of 20°C.

[0260] For five bolts prepared in this manner that had been subjected to base treatment and immersion treatment (1 mass % sodium silicate aqueous solution containing 3 mass % lubricant a; bolt surface temperature 235°C to 270°C), the surface friction coefficients were measured in accordance with the ISO 16047 HH method, as in Example 59, and the average value was calculated, resulting in an average friction coefficient of 0.162.

[0261] Furthermore, five bolts thus prepared that had been subjected to the base treatment and immersion treatment (1 mass % sodium silicate aqueous solution containing 3 mass % lubricant a; bolt surface temperature 235°C to 270°C) were subjected to a salt spray test in accordance with JIS Z-2371, as in Example 59. The occurrence of rust on the bolts was checked every 168 hours from the start of the test to evaluate corrosion resistance. As a result, no rust was confirmed on any of the five bolts, even 1,176 hours after the start of the salt spray test.

[0262] Example 69 Sodium silicate and lubricant a were dissolved and mixed in deionized water so that the immersion treatment agent contained 1% by mass of sodium silicate and the lubricant contained 3% by mass of BYK's "AQUACER 593" (trade name) (lubricant a). Five bolts that underwent base treatment and immersion treatment were produced in the same manner as in Example 59, except that the immersion treatment was performed at a surface temperature of 85°C to 120°C using 1000 ml of the prepared 1% by mass sodium silicate aqueous solution containing 3% by mass of lubricant a, instead of the 1% by mass sodium silicate aqueous solution at a liquid temperature of 20°C.

[0263] For five bolts prepared in this manner that had been subjected to base treatment and immersion treatment (1 mass % sodium silicate aqueous solution containing 3 mass % lubricant a; bolt surface temperature 85°C to 120°C), the surface friction coefficients were measured in accordance with the ISO 16047 HH method, as in Example 59, and the average value was calculated, resulting in an average friction coefficient of 0.166.

[0264] Furthermore, five bolts thus prepared that had been subjected to the base treatment and immersion treatment (1 mass % sodium silicate aqueous solution containing 3 mass % lubricant a; bolt surface temperature 85°C to 120°C) were subjected to a salt spray test in accordance with JIS Z-2371, as in Example 59. The occurrence of rust on the bolts was checked every 168 hours from the start of the test to evaluate corrosion resistance. As a result, no rust was confirmed on any of the five bolts, even 672 hours after the start of the salt spray test.

[0265] <Comparative Example 15> Five bolts that had been subjected to only the base treatment were produced in the same manner as in Example 59, except that after the base treatment, the bolts were not immersed in a 1% by mass sodium silicate aqueous solution, but were simply cooled to room temperature.

[0266] The surface friction coefficients of five bolts thus produced that had been subjected to only the base treatment were measured in accordance with the ISO 16047 HH method, as in Example 59, and the average value was calculated, resulting in an average friction coefficient of 0.228.

[0267] Furthermore, five of the thus-prepared bolts that had been subjected to only the base treatment were subjected to a salt spray test in accordance with JIS Z-2371, as in Example 59, and the occurrence of rust on the bolts was checked every 168 hours from the start of the test to evaluate corrosion resistance. As a result, no rust was confirmed on any of the five bolts 168 hours after the start of the salt spray test, but rust was confirmed on two or more bolts 336 hours after the start of the test. [Industrial Applicability]

[0268] According to the present invention, it is possible to easily impart superior rust prevention performance to metal materials or alloy materials, and it is also possible to provide articles having superior rust prevention performance compared to conventional articles.

Claims

1. The method includes a step of treating a workpiece containing a metal or an alloy and heated to a temperature exceeding 180° C., or a workpiece having a film or layer containing a metal or an alloy on its surface and heated to a temperature exceeding 180° C., with an aqueous solution containing an inorganic salt, the aqueous solution containing an inorganic salt is an aqueous solution containing at least one selected from sodium silicate, lithium silicate, potassium silicate, sodium dihydrogen phosphate, potassium sulfate, sodium nitrate, sodium molybdate, and ammonium zirconium carbonate; 2. The method for rust prevention treatment, wherein the object to be treated contains iron, or the film or layer contains at least one member selected from the group consisting of zinc and aluminum.

2. 2. The method of claim 1, wherein the temperature of the object to be treated exceeds 220° C. when the object is treated with the aqueous solution.

3. 3. The method for rust prevention treatment according to claim 1, wherein the content of the inorganic salt in the aqueous solution containing the inorganic salt is 0.1% by mass or more.

4. 4. The method for rust prevention according to claim 1, wherein the aqueous solution containing the inorganic salt further contains a lubricant.

5. 5. The method for rust prevention according to claim 1, wherein the aqueous solution containing the inorganic salt has a pH of 4 or higher.

6. 6. The rust prevention method according to claim 1, wherein the method does not include a step of heating the object to 200° C. or higher after the treatment with the aqueous solution.

Citation Information

Patent Citations

  • Antirust paint

    CN102719118A

  • JP1975116331A

  • Surface treatment of metal strips

    JP1979148142A

  • Method of manufacturing minimized spangle galvanized steel sheet excellent in blackening resistance

    JP2001140052A