Heat seal paper
Patent Information
- Application Number
- JP2022187274
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-11-24
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-07-28
AI Technical Summary
【0007】 本発明によれば、包装用途に好適に用いられる、ヒートシール適性を有すると共に、良好なブロッキング耐性を有するヒートシール紙を提供することができる。アンチブロッキング剤として、顔料とワックスを併用することにより、状況に応じて必要なブロッキング耐性を付与することができる。
Smart Images

Figure 0007584157000001
Abstract
Description
[Technical field]
[0001] The present invention relates to heat seal paper, and more particularly to heat seal paper having heat sealing suitability that is suitable for use in packaging applications such as packaging materials, bags, containers, boxes, cups, and lids. [Background technology]
[0002] In recent years, plastic waste has become a major issue due to concerns that plastic that has been released into the environment as garbage will not decompose for a long time and will have a negative impact on the ecosystem. As a countermeasure, it has been proposed to replace plastic with biomass-derived materials and paper, which is a biodegradable material. Meanwhile, conventionally, when paper packaging materials are formed into packaging materials for food, bags, containers, boxes, cups, lids, and the like, it has been common to laminate a thermoplastic resin, typically a polyolefin resin such as polyethylene, polypropylene, or polymethylpentene, onto the packaging material by extrusion lamination or the like to impart heat sealing suitability.
[0003] However, these thermoplastic resin laminates use about 10 to 30 g / m2 of thermoplastic resin, which is not enough to reduce the amount of plastic. For this reason, currently, wrapping paper is provided in which a water or solvent dispersion containing a thermoplastic resin dispersion is applied onto a paper substrate, resulting in a thinner and lighter coating layer (Patent Document 1, etc.). However, heat is required during the paint drying process when laminating coating layers by coating, and also when forming paper packaging materials into packaging materials for food, bags, containers, boxes, cups, lids, etc. If heat remains after each process (if the thermoplastic resin remains softened), blocking can occur, resulting in defective products. In addition, coated paper is stored rolled up until it is formed, but there is a problem of blocking occurring during long-term storage at room temperature. For this reason, it is necessary to provide packaging paper that combines good blocking resistance with heat sealing suitability. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6580291 DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a heat sealable paper that has heat sealing suitability and good blocking resistance and is suitable for use in packaging applications such as packaging materials, bags, containers, boxes, cups, and lids. [Means for solving the problem]
[0006] The means for solving the problems of the present invention are as follows. 1. A paper substrate having a coating layer containing a thermoplastic resin on at least one surface thereof, the coating layer contains at least a pigment as an antiblocking agent, A heat sealable paper, characterized in that the amount of pigment in the coating layer is less than 200 parts by mass per 100 parts by mass of thermoplastic resin. 2. A paper substrate having a coating layer containing a thermoplastic resin on at least one surface thereof, the coating layer contains at least a wax as an antiblocking agent, A heat sealable paper, characterized in that the amount of wax in the coating layer is 1.2 parts by mass or more per 100 parts by mass of thermoplastic resin. 3. A heat sealable paper according to 1 or 2, characterized in that it contains both wax and a pigment as anti-blocking agents. 4. The heat sealable paper described in any one of 1. to 3., wherein the coating layer contains a thermoplastic resin having a glass transition temperature of 100° C. or lower. 5. The heat sealable paper described in any one of 1. to 4., wherein the coating layer contains carnauba wax. 6. The heat sealable paper according to any one of 1. to 5., wherein the thermoplastic resin contained in the coating layer is an ethylene acrylic acid copolymer resin. Effect of the Invention
[0007] According to the present invention, it is possible to provide a heat seal paper that is suitable for use in packaging applications and has heat sealing suitability and good blocking resistance. By using a pigment and a wax in combination as an anti-blocking agent, it is possible to impart the necessary blocking resistance depending on the situation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The present invention relates to a heat-sealable paper having a coating layer containing a thermoplastic resin on at least one side of a paper base material, the coating layer containing one or more anti-blocking agents selected from waxes or pigments, and the coating layer having heat-sealing suitability.
[0009] (Paper base material) The paper base material is obtained by papermaking a paper material containing pulp, filler, various auxiliaries, etc. When the heat seal paper of the present invention is used for applications in which it comes into contact with food, it is preferable to use materials that comply with food safety standards, such as materials that are approved as food additives or have FDA certification, for each material in the paper base material.
[0010] Pulps include chemical pulps of wood such as bleached kraft pulp (NBKP), unbleached kraft pulp (NUKP), bleached kraft pulp (LBKP), unbleached kraft pulp (LUKP), and sulfite pulp (SP), mechanical pulps of wood such as ground pulp (GP), refiner ground pulp (RGP), stone ground pulp (SGP), chemi-ground pulp (CGP), semi-chemical pulp (SCP), thermomechanical pulp (TMP), and chemi-thermomechanical pulp (CTMP), non-wood pulps obtained from kenaf, bagasse, bamboo, hemp, straw, and the like, and waste paper pulp made from waste paper and having the ink contained therein removed in a deinking process. Among these, chemical pulps such as LBKP and NBKP, which are less likely to be contaminated with foreign matter, are preferred, and it is also preferred that the amount of waste paper pulp blended is small. Specifically, the amount of chemical pulp is preferably 80% or more, and particularly preferably 100%. The amount of recycled paper pulp is preferably 10% or less, more preferably 1% or less, and most preferably zero.
[0011] Examples of fillers that can be used include known fillers such as inorganic fillers such as talc, kaolin, calcined kaolin, clay, heavy calcium carbonate, light calcium carbonate, white carbon, zeolite, magnesium carbonate, barium carbonate, titanium dioxide, zinc oxide, silicon oxide, amorphous silica, aluminum hydroxide, calcium hydroxide, magnesium hydroxide, zinc hydroxide, barium sulfate, and calcium sulfate, and organic fillers such as urea-formalin resin, polystyrene resin, phenol resin, and hollow microparticles. Note that fillers are not essential materials and may not be used.
[0012] Examples of various auxiliary agents include sizing agents such as rosin, alkyl ketene dimer (AKD), alkenyl succinic anhydride (ASA), polyacrylamide polymers, polyvinyl alcohol polymers, cationic starch, various modified starches, urea-formaldehyde resin, melamine-formaldehyde resin, and other dry strength agents, wet strength agents, retention agents, drainage improvers, coagulants, aluminum sulfate, bulking agents, dyes, fluorescent brighteners, pH adjusters, defoamers, UV inhibitors, anti-fading agents, pitch control agents, slime control agents, and the like, and can be selected and used as appropriate as needed.
[0013] The method of manufacturing (papermaking) the paper base material is not particularly limited, and known manufacturing (papermaking) methods and papermaking machines can be selected, such as a Fourdrinier papermaking machine, a cylinder papermaking machine, a short wire papermaking machine, a twin-wire papermaking machine such as a gap former type or a hybrid former type (on-top former type). The pH during papermaking may be in the acidic range (acidic papermaking), pseudo-neutral range (pseudo-neutral papermaking), neutral range (neutral papermaking), or alkaline range (alkaline papermaking), and after papermaking in the acidic range, an alkaline agent may be applied to the surface of the paper layer. The paper base material may be one layer, or may be composed of two or more layers.
[0014] Furthermore, the surface of the paper substrate can be treated with various chemicals. Examples of chemicals that can be used include oxidized starch, hydroxyethyl etherified starch, enzyme-modified starch, polyacrylamide, polyvinyl alcohol, surface sizing agents, water-resistant agents, water retention agents, thickeners, lubricants, etc., and these can be used alone or in combination of two or more. Furthermore, these various chemicals can be used in combination with pigments. Examples of pigments include kaolin, clay, engineered kaolin, delaminated clay, heavy calcium carbonate, light calcium carbonate, mica, talc, titanium dioxide, barium sulfate, calcium sulfate, zinc oxide, silicic acid, and silicates. Inorganic pigments such as colloidal silica and satin white, and organic pigments such as solid, hollow or core-shell type pigments can be used alone or in combination of two or more.
[0015] The method for treating the surface of the paper substrate is not particularly limited, but known coating devices such as a rod metering size press, a pond type size press, a gate roll coater, a spray coater, a blade coater, and a curtain coater can be used. Examples of the paper base material obtained in this manner include various known types of paper, such as fine paper, medium quality paper, coated paper, one-sided glossy paper, kraft paper, one-sided glossy kraft paper, bleached kraft paper, glassine paper, paperboard, white paperboard, and liner.
[0016] The basis weight of the paper substrate can be appropriately selected depending on the desired qualities and handling properties, but is usually preferably 20 g / m2 or more and 600 g / m2 or less. In the case of heat seal paper used for packaging purposes such as packaging materials for food, bags, containers, boxes, cups, and lids, it is more preferable to use 25 g / m2 or more and 600 g / m2 or less, and in the case of heat seal paper used for bags, lids, or soft packaging materials described below, it is more preferable to use 30 g / m2 or more and 150 g / m2 or less, and in the case of heat seal paper used for containers, boxes, and cups, it is more preferable to use 150 g / m2 or more and 350 g / m2 or less. In addition, a soft packaging material is a packaging material composed of a material with high flexibility, and generally refers to a packaging material made of thin and flexible materials such as paper, film, and aluminum foil, either alone or bonded together. In addition, in terms of shape, it refers to a packaging material such as a bag that maintains a three-dimensional shape by putting contents in it. The density of the paper base material can be appropriately selected depending on the desired qualities, ease of handling, etc., but is usually preferably 0.5 g / cm3 or more and 1.0 g / cm3 or less.
[0017] (Coating layer) The coating layer contains a thermoplastic resin and one or more antiblocking agents selected from wax and pigments. The coating layer may be provided on both sides of the heat seal paper, but is provided on at least one side. The coating layer has heat sealability. Having heat sealability means that it can be bonded to an object by applying heat and pressure. By having heat sealability, it becomes easier to mold the coating layer into a packaging form, maintain the shape, and ensure the sealability, particularly in packaging applications such as packaging materials for food, bags, containers, boxes, cups, and lids.
[0018] ·Thermoplastic resin The thermoplastic resin used in the present invention can be any resin used in the papermaking field for forming a heat seal layer, and can be any resin having a glass transition temperature of 100°C or less. The glass transition temperature of the thermoplastic resin is preferably -20°C or more and 85°C or less. The melting point of the thermoplastic resin is preferably 80°C or more and 120°C or less. Examples of the thermoplastic resin that can be used include low density polyethylene (LDPE), high density polyethylene (HDPE), linear low density polyethylene (LLDPE), polypropylene (PP), polyvinyl acetate (PVAc), polyester resin (PET), ethylene methacrylic acid copolymer resin (EMAA), ethylene methyl acrylate copolymer resin (EMA), ethylene acrylic acid copolymer resin (EAA), ethylene vinyl acetate copolymer resin (EVA), styrene acrylic acid ester copolymer resin, polylactic acid resin, etc. The thermoplastic resin can be used alone or in a mixture of two or more kinds. Among these, ethylene acrylic acid copolymer resin, which has high heat sealability, is preferred.
[0019] ·Anti-blocking agent The heat seal paper of the present invention contains a pigment or a wax as an antiblocking agent, and may contain both a pigment and a wax as an antiblocking agent. (Pigments) The pigment used in the present invention is not particularly limited, and inorganic pigments such as kaolin, clay, engineered kaolin, delaminated clay, heavy calcium carbonate, light calcium carbonate, mica, talc, titanium dioxide, barium sulfate, calcium sulfate, zinc oxide, silicic acid, silicate salts, colloidal silica, and satin white, and organic pigments such as solid, hollow, and core-shell pigments can be used. In addition, one type of pigment can be used or two or more types can be mixed. Among these, heavy calcium carbonate is preferred because it has excellent blocking resistance without impairing heat sealability.
[0020] In the present invention, the amount of pigment is less than 200 parts by mass, and more preferably 150 parts by mass or less, per 100 parts by mass of thermoplastic resin, in terms of dry weight. If the amount of pigment is 200 parts by mass or more, the heat sealing temperature may become too high, or the heat sealing may take a long time. In addition, the amount of pigment is preferably 50 parts by mass or more, and more preferably 80 parts by mass or more, per 100 parts by mass of thermoplastic resin, in terms of dry weight. If the amount of pigment is less than 50 parts by mass, the blocking resistance may be insufficient.
[0021] (wax) The wax used in the present invention is not particularly limited, and may be a paraffin wax mainly composed of an alkane compound, a natural oil-based wax derived from animals and plants such as carnauba or lanolin, a silicone-containing wax containing silicone or a silicone compound, or a fluorine-containing wax containing a fluorine compound. The wax may be used alone or in combination of two or more kinds. Among these, carnauba wax is preferred.
[0022] In the present invention, the amount of wax is 1.2 parts by mass or more, preferably 1.5 parts by mass or more, and more preferably 2.5 parts by mass or more, per 100 parts by mass of thermoplastic resin, in terms of dry weight. If the amount of wax is less than 1.2 parts by mass, sufficient blocking resistance may not be obtained. In addition, the wax is preferably contained in an amount of 15 parts by mass or less, more preferably 10 parts by mass or less, per 100 parts by mass of thermoplastic resin, in terms of dry weight. If the amount of wax is more than 15 parts by mass, blocking resistance is hardly improved, and costs increase.
[0023] Both pigment and wax are anti-blocking agents, but pigment mainly contributes to blocking resistance in a heated state during processing, while wax mainly contributes to blocking resistance during long-term storage. By using pigment and wax together as anti-blocking agents, it is possible to impart blocking resistance required depending on the situation. The blending ratio of pigment and wax can be adjusted depending on the situation in which blocking resistance is required, and for example, the wax can be 1 part by mass or more and 200 parts by mass or less per 100 parts by mass of pigment in dry weight.
[0024] The coating method of the coating layer is not particularly limited, and coating can be performed using a known coating device and coating system. For example, the coating device can be a blade coater, a bar coater, an air knife coater, a curtain coater, a spray coater, a roll coater, a reverse roll coater, a size press coater, a gate roll coater, etc. In addition, the coating system can be an aqueous coating using a solvent such as water, or a solvent-based coating using a solvent such as an organic solvent. Since the heat seal paper of the present invention may be used in applications where it comes into contact with food, etc., it is preferable to use an aqueous coating from the viewpoint of food safety. The viscosity, solid content, and other properties of the coating solution can be appropriately adjusted depending on the coating device and coating system used.
[0025] The coating amount (dry weight) of the coating layer must be between 3g / m2 and 20g / m2 per side. If the coating amount is less than 3 g / m2 per side, the heat sealability decreases. In addition, even if the coating amount exceeds 20 g / m2 per side, the heat sealability hardly improves. The coating layer may be one layer or may be two or more layers. When the coating layer is composed of two or more layers, the total coating weight of all the coating layers is within the above range. It is preferable to set the above.
[0026] The heat seal paper of the present invention may be any paper having a coating layer and a paper substrate, and may further include a sealing layer, It may have other layers such as a print layer, a light-shielding layer, a water-resistant layer, an oil-resistant layer, a water vapor barrier layer, a gas barrier layer, etc. It is preferable to have a filler layer between the coating layer and the paper substrate. This reduces the occurrence of coating defects such as pinholes and streaks in the coating layer. This can improve water resistance and oil resistance. The heat seal paper of the present invention is used for packaging materials such as food packaging materials, bags, containers, boxes, cups, and lids. It is possible to make a heat seal paper for use in packaging applications. EXAMPLES
[0027] (Evaluation method) (1) Heat sealability (Heat seal conditions) Two square test pieces with a side length of 100 mm were cut out from the obtained heat seal paper, and the coating layer The two were brought into contact with each other, and the pressure was applied at a temperature of 160°C, a pressure of 2kgf / cm2, and a pressure time of 0.5 seconds. Heat sealed. When the heat-sealed test piece is peeled off by hand, the peeled part is visually observed and evaluated according to the following criteria: The heat sealability was evaluated. ○: Peeling within the paper base (paper base is destroyed) ×: Peeling between coating layers
[0028] (2) Blocking property A This evaluation assumes that the product will be stored in a warehouse or similar. According to ASTM D918-81, Standard Test Method for Blocking Resistance of Paper and Paperboard, the coating layers were placed in contact with each other and stored at 60°C and 75% RH for 24 hours to evaluate the degree of blocking. If the evaluation was ○, there was no problem in practical use. [Evaluation Criteria] ◎: No blocking ○: Mild blocking, easy to peel off ×: Strong blocking and cannot be easily peeled off
[0029] (3) Blocking property B This evaluation assumes that the hot coating layer will stick to various pieces of equipment when it comes into contact with them during product manufacturing or processing. The humidity-conditioned sample (23°C, RH50%) was passed through a hot roll press (roll pressure 0.5MPa, processing speed 2m / min, arbitrary roll temperature) so that the coated surface came into contact with the metal roll, and the degree of adhesion of the coated surface to the metal roll was evaluated. If the evaluation was ○, there was no problem in practical use. [Evaluation Criteria] ◎: No sticking or damage to the coated surface was observed when the roll temperature was 70°C. ○: When the roll temperature was 60°C, no sticking was observed and no damage was observed on the coated surface. ×: When the roll temperature was 60°C, the coating layer stuck to the metal roll, and damage to the coating surface was observed, such as the coating layer being taken off by the metal roll.
[0030] [Example 1] (Preparation of Coating Fluid for Coating Layer) A thermoplastic resin (Michelman: MICHEM PRIME 498345N.S) and kaolin (Imerys: Varisurf HX, aspect ratio 95) were adjusted to a solid content mass ratio of 100.0 / 100.0 parts, respectively, to obtain a coating solution for the coating layer.
[0031] (Preparation of heat seal paper) The coating solution for the coating layer was applied to one side of a paper substrate (cup base paper with a basis weight of 200 g / m2) by the bar blade method so that the dry coating amount was 10.0 g / m2, and then dried to obtain a heat seal paper.
[0032] [Example 2] A heat seal paper was obtained in the same manner as in Example 1, except that heavy calcium carbonate (FMT-100, manufactured by Fimatec Corporation) was used as the pigment. [Example 3] Except for the pigment being light calcium carbonate (Tunex E, manufactured by New Lime Co., Ltd.), A heat seal paper was obtained in the same manner as in Example 1.
[0033] [Example 4] The coating solution for the coating layer was a thermoplastic resin (MICHEM PRIM manufactured by Michelman Co., Ltd.). E 498345N.S) and carnauba wax (Michelman: MICHEM LUBE 160RPH.S) in a solid content mass ratio of 100.0 / 2.9 parts, respectively. A heat seal paper was obtained in the same manner as in Example 1, except that the heat seal paper was prepared as described above.
[0034] [Example 5] The solid mass ratio of the thermoplastic resin to the wax was 100.0 / 6.1. Heat seal paper was obtained in the same manner as in 4. [Example 6] The coating solution for the coating layer was a thermoplastic resin (MICHEM PRIM manufactured by Michelman Co., Ltd.). E 498345N.S) and kaolin (Imeris: Varisurf HX), carnauba wax The solid content of the mixture was 160RPH.S (Michelman: MICHEM LUBE). The mass ratio was adjusted to 100.0 / 100.0 / 2.9 parts, respectively. A heat seal paper was obtained in the same manner as in Example 1.
[0035] [Comparative Example 1] Thermoplastic resin (Michelman: MICHEM PRIME 498345N The heat seal was prepared in the same manner as in Example 1, except that a coating solution for the coating layer containing only .S) was used. We obtained the paper.
[0036] [Comparative Example 2] The solid mass ratio of thermoplastic resin to kaolin was 100.0 / 200.0 parts. In the same manner as in Example 1, a heat seal paper was obtained. [Comparative Example 3] The solid mass ratio of thermoplastic resin to wax was 100.0 / 1.1 parts. In the same manner as in Example 1, a heat seal paper was obtained.
[0037] [Table 1]
[0038] The heat-sealed papers obtained in Examples 1 to 6 of the present invention were excellent in blocking resistance. The heat-sealed papers obtained in Examples 1 to 3, which contained a pigment as an anti-blocking agent, were excellent in operational suitability, and the heat-sealed papers obtained in Examples 4 and 5, which contained a wax as an anti-blocking agent, were particularly excellent in long-term storage. The heat-sealed paper obtained in Example 6, which contained both a pigment and a wax as an anti-blocking agent, was excellent in both long-term storage property and operational suitability. The heat-sealed paper obtained in Comparative Example 1, which did not contain an antiblocking agent, and the heat-sealed paper obtained in Comparative Example 3, which contained a small amount of the wax as an antiblocking agent, were poor in blocking resistance. The heat-sealed paper obtained in Comparative Example 2, which contained a large amount of the pigment as an antiblocking agent, was excellent in blocking resistance, but was poor in heat sealing suitability to begin with.
Claims
1. A coating layer containing a thermoplastic resin is provided on at least one surface of a paper substrate, The paper base material has a basis weight of 20 g / m 2 More than 600g / m 2 is as follows: The coating layer contains at least one type selected from a wax or a pigment as an antiblocking agent, A heat seal paper characterized in that the thermoplastic resin contained in the coating layer contains an ethylene acrylic acid copolymer resin (excluding those in which the coating layer contains a rosin derivative).
2. 2. The heat seal paper according to claim 1, wherein the amount of wax in the coating layer is 1.2 parts by mass or more per 100 parts by mass of the thermoplastic resin.
3. 2. The heat seal paper according to claim 1, wherein the amount of pigment in the coating layer is less than 200 parts by mass per 100 parts by mass of the thermoplastic resin.
4. 4. The heat sealable paper according to claim 1, further comprising both a wax and a pigment as an anti-blocking agent.
5. 5. The heat seal paper according to claim 1, wherein the coating layer contains a thermoplastic resin having a glass transition temperature of 100° C. or lower.
6. The heat sealable paper according to any one of claims 1 to 5, characterized in that the coating layer contains carnauba wax.
Citation Information
Patent Citations
Heattsensitive adhesive paper
JP1980021456A
Laminated sheet having low temperature heat sealing property
JP1989093349A
Water-resistant and oil-resistant paper usable for for bag making, or the like
JP2002013095A
Moisture proof sheet
JP2003049397A
Coating composition containing low mfi ethylene acrylic acid copolymer
JP2003529624A