Alumina filler for thermally conductive resin composition, thermally conductive resin composition, and method for producing alumina filler for thermally conductive resin composition

Polished fused alumina particles with enhanced specific surface area and fine particles address the high cost and hardness issues of conventional fillers, resulting in a cost-effective, thermally conductive resin composition with improved moldability and thermal conductivity.

JP7584225B2Active Publication Date: 2024-11-15MITSUBISHI MATERIALS CORP +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020045795
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-16
Publication Date
2024-11-15
Estimated Expiration
2040-03-16

AI Technical Summary

Technical Problem

Existing thermally conductive resin compositions face challenges with high manufacturing costs and increased hardness due to the use of spherical alumina particles or rounded fused alumina particles, which also complicate the kneading process and reduce filling ability.

Method used

The use of polished fused alumina particles with a specific surface area increased by 25% and containing at least 1% by mass of fine particles less than 1 μm, along with a particle polishing step that enhances the specific surface area and average particle diameter, results in a lower-cost alumina filler with improved moldability and thermal conductivity.

Benefits of technology

The proposed alumina filler allows for a thermally conductive resin composition with enhanced thermal conductivity and reduced hardness, achieving better shape followability and cost-effectiveness by increasing the filler content without compromising kneading efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584225000007
    Figure 0007584225000007
  • Figure 0007584225000008
    Figure 0007584225000008
  • Figure 0007584225000009
    Figure 0007584225000009
Patent Text Reader

Abstract

To provide an alumina filler for a thermally conductive resin composition from which a thermally conductive resin composition that is excellent in thermal conductivity and has low hardness can be obtained at low cost, a thermally conductive resin composition using the same, and a method for producing the alumina filler for the thermally conductive resin composition.SOLUTION: An alumina filler for a thermally conductive resin composition containing electro-fused alumina particles contains 1 mass% or more of fine electro-fused alumina particles of 1 μm or less in the electro-fused alumina particles.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an alumina filler for a thermally conductive resin composition, a thermally conductive resin composition, and a method for producing the alumina filler for a thermally conductive resin composition. [Background technology]

[0002] In recent years, with the development of electric vehicles and fuel cell vehicles, electric components are becoming larger in current and the amount of heat generated by the electric components is also increasing. For example, lithium ion batteries for automobiles generate a large amount of heat in order to continuously output a large current of power for a long period of time, and it is necessary to efficiently dissipate the large amount of heat generated to the outside. For this reason, resin materials (thermally conductive resin compositions) with excellent thermal conductivity are generally used as packages for electric components that output a large current, such as lithium ion batteries.

[0003] Conventionally, a thermally conductive resin composition is a composition in which an inorganic filler having excellent thermal conductivity is dispersed in a resin material having excellent insulating properties and moldability. As the inorganic filler, fused alumina (Al 2 O 3 ) Alumina filler consisting of crystalline particles is commonly used.

[0004] The thermal conductivity of the thermally conductive resin composition can be improved by increasing the content of alumina filler. For example, in order to obtain a thermally conductive resin composition with a high thermal conductivity of 5 W / mk or more, it is necessary to knead 1100 parts by mass or more of alumina filler with 100 parts by mass of the resin material.

[0005] However, on the other hand, increasing the alumina filler content increases the hardness of the resulting thermally conductive resin composition, reducing its fillability (shape conformability) in the area of ​​use, and also makes it difficult to uniformly mix the alumina filler into the resin material during production.

[0006] For this reason, for example, Patent Document 1 discloses a resin composition that uses spherical alumina particles as an alumina filler, thereby keeping the hardness low even at a high content and allowing easy kneading. Moreover, Patent Document 2 discloses rounded fused alumina particles having an average particle size of 5 to 4000 μm and a circularity of 0.85 or more. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent No. 4361997 [Patent Document 2] Patent No. 4817683 Summary of the Invention [Problem to be solved by the invention]

[0008] However, the spherical alumina particles used in the resin composition disclosed in Patent Document 1 have a problem in that the manufacturing process is complicated and the manufacturing cost is high. In addition, although the rounded fused alumina particles disclosed in Patent Document 2 use inexpensive fused alumina as a manufacturing raw material, there was a problem in that the yield of the rounded fused alumina particles obtained after classification was low, resulting in high costs.

[0009] The present invention has been made in consideration of the above circumstances, and has an object to provide an alumina filler for a thermally conductive resin composition, which enables a thermally conductive resin composition having excellent thermal conductivity and low hardness to be obtained at low cost, a thermally conductive resin composition using the alumina filler, and a method for producing the alumina filler for a thermally conductive resin composition. [Means for solving the problem]

[0010] In order to solve the above problems, the present invention proposes the following means. That is, the alumina filler for a thermally conductive resin composition of the present invention is an alumina filler for a thermally conductive resin composition containing electrically fused alumina particles which are ground products of raw material alumina particles, and the electrically fused alumina particles have a 2-hour sedimentation test in water. On top The alumina powder contains 1 mass % or more of fine fused alumina particles as clear solids, and the specific surface area of ​​the fused alumina particles is 25% or more larger than the specific surface area of ​​the raw alumina particles.

[0011] According to the present invention, by containing at least 1 mass % or more of fine fused alumina particles of 1 μm or less, it is possible to realize an alumina filler for a thermally conductive resin composition that is excellent in moldability because the hardness is not too high when kneaded with a resin, and that can form a thermally conductive resin composition containing a large amount of filler. In addition, since expensive rounded alumina particles are not used, it is possible to realize a low-cost alumina filler for a thermally conductive resin composition.

[0013] The thermally conductive resin composition of the present invention is characterized in that it contains the alumina filler for a thermally conductive resin composition described in each of the above items in a resin.

[0014] In the present invention, the alumina filler for a thermally conductive resin composition may be contained in an amount of 1200 parts by mass or more relative to 100 parts by mass of the resin.

[0015] The method for producing an alumina filler for a thermally conductive resin composition of the present invention is a method for producing an alumina filler for a thermally conductive resin composition described in each of the above items, and is characterized by having a particle polishing step in which a slurry obtained by mixing the fused alumina particles and a solvent is swirled at a peripheral speed of 10 m / sec or more to cause the fused alumina particles to collide with each other and be polished.

[0016] In the present invention, the particle polishing step may be carried out for a period of time ranging from 3 minutes to 60 minutes.

[0017] In the present invention, the particle polishing step may be a step of increasing the specific surface area of ​​the fused alumina particles by 25% or more compared to the specific surface area of ​​the fused alumina particles before the particle polishing step is carried out.

[0018] In the present invention, the particle polishing step may be a step of increasing the average particle diameter D50 of the fused alumina particles by -15% or more compared to the average particle diameter D50 of the fused alumina particles before the particle polishing step is carried out. Effect of the Invention

[0019] According to the present invention, it is possible to provide an alumina filler for a thermally conductive resin composition, which enables a thermally conductive resin composition having excellent thermal conductivity and low hardness to be obtained at low cost, a thermally conductive resin composition using the alumina filler, and a method for producing the alumina filler for a thermally conductive resin composition. [Brief description of the drawings]

[0020] [Figure 1] 1 is a micrograph showing an electrically fused alumina particle according to an embodiment of the present invention. [Diagram 2] 1 is a micrograph showing conventional raw alumina particles. [Diagram 3] 1 is a graph showing the relationship between the number of parts by mass of alumina particles and the thermal conductivity of the obtained thermally conductive resin composition. [Figure 4] Photographs showing a two-hour sedimentation test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, an alumina filler for a thermally conductive resin composition according to one embodiment of the present invention, a thermally conductive resin composition using the alumina filler, and a method for producing the alumina filler for a thermally conductive resin composition will be described with reference to the drawings. Note that the following embodiments are specifically described to better understand the gist of the invention, and do not limit the present invention unless otherwise specified.

[0022] (Alumina filler for thermally conductive resin composition) An alumina filler for a thermally conductive resin composition (hereinafter referred to as an alumina filler) is a thermally conductive material to be mixed with a resin to obtain a thermally conductive resin composition. The alumina filler according to one embodiment of the present invention is a fine powder of alumina (Al 2 O 3 ).

[0023] Alumina was used as the filler for the thermally conductive resin composition because it has a relatively high thermal conductivity of about 30 W / m·K.

[0024] The alumina filler of the present embodiment contains fused alumina particles obtained by polishing raw material alumina particles (fused alumina particles), and specifically contains at least 1 mass % or more of fine fused alumina particles of 1 μm or less. In the following description, the term "fine fused alumina particles" refers to fused alumina particles having a size of 1 μm or less, and the term "fused alumina particles" simply refers to fused alumina particles with no particular particle size restriction.

[0025] The reason why fused alumina particles produced by, for example, the reductive melting of bauxite in an electric arc furnace are used as the raw alumina particles that are the raw material for producing the polished fused alumina particles is that they have a large particle diameter and a broad particle size distribution, and can be mixed with resins, etc. at a high filling rate, thereby enhancing the thermal conductivity of the thermally conductive resin composition.

[0026] In the alumina filler of this embodiment, the specific surface area of ​​the fused alumina particles is 25% or more larger than that of the raw alumina particles. That is, in the manufacturing method of the alumina filler described later, the raw alumina particles are polished to use fused alumina particles whose specific surface area is increased by 25% or more.

[0027] In this embodiment, the specific surface area is the surface area per unit mass (m 2 / g) In this embodiment, the specific surface area was measured by the BET method (molecule with a known adsorption occupancy area is adsorbed onto the powder particle surface with liquid nitrogen, and the specific surface area of ​​the sample is calculated from the amount of adsorption). The specific surface area was measured using a fully automatic gas adsorption measurement device (Autosorb-iQ: Quantachrome Instruments Japan).

[0028] Furthermore, the electrically fused alumina particles contained in the alumina filler of this embodiment have a total solid mass relative to the supernatant solid mass in a 2-hour sedimentation test in water of at least 0.3 mass%, preferably 2.0 mass% or more, and more preferably 5.0 mass% or more.

[0029] In the sedimentation test in this embodiment, the sample electrofused alumina particles are suspended in water to a concentration of 2.4 mass % to form a slurry, and this slurry is poured into a container so that the liquid level is 20 mm and left to stand for 2 hours. Thereafter, the supernatant is separated and the water is evaporated at 90°C, the mass of the residual solids is measured, and the ratio (percentage) of the mass of the residual solids to the total solids mass of the slurry is calculated.

[0030] The alumina filler of this embodiment as described above contains at least 1 mass % of fine fused alumina particles of 1 μm or less, and thus can realize an alumina filler that has high thermal conductivity when kneaded with a resin at a low cost compared to a case in which spherical alumina particles are used. Furthermore, by mixing the alumina filler of this embodiment with a resin, a thermally conductive resin composition with low hardness and excellent shape conformability can be obtained.

[0031] (Thermal conductive resin composition) The thermally conductive resin composition of the present embodiment is made of a resin containing the alumina filler of the present embodiment. For example, it may be a paste-like composition in which 1200 parts by mass or more of the alumina filler of the present embodiment is mixed with 100 parts by mass of resin. For example, the thermally conductive resin composition of the present embodiment can be obtained by mixing 1200 parts by mass to 1500 parts by mass of the alumina filler of the present embodiment with 100 parts by mass of resin.

[0032] The resin to be mixed with the alumina filler is not particularly limited, and any known resin can be used.Specific examples include hydrocarbon resins, unsaturated polyester resins, acrylic resins, vinyl ester resins, epoxy resins, xylene formaldehyde resins, guanamine resins, diallyl phthalate resins, phenol resins, furan resins, polyimide resins, melamine resins, and urea resins.

[0033] The thermally conductive resin composition of this embodiment has a hardness reduced by 9% to 57% at the same blending ratio, compared to a conventional thermally conductive resin composition in which raw material alumina particles (electrically fused alumina particles) and resin are mixed. This reduction in hardness, that is, softening, increases the fluidity of the thermally conductive resin composition of this embodiment. As a result, the thermally conductive resin composition of this embodiment can improve the shape conformability at the filled portion, and can efficiently transfer heat by adhering to the heat transfer object without gaps. In addition, compared to a conventional thermally conductive resin composition in which raw material alumina particles (electrically fused alumina particles) and resin are mixed, a large amount of filler can be mixed when the hardness is the same, so the thermally conductive resin composition of this embodiment can improve thermal conductivity.

[0034] (Method of manufacturing alumina filler for thermally conductive resin composition) The alumina filler for a thermally conductive resin composition of this embodiment is produced by carrying out a particle polishing step of polishing raw material alumina particles (electrically fused alumina particles). In the particle polishing process, a slurry in which raw alumina particles and a solvent are mixed is swirled at a peripheral speed of 10 m / sec or more, and the raw alumina particles are polished by colliding with each other.

[0035] In the particle polishing process, commercially available fused alumina powder can be used as raw alumina particles (fused alumina particles). Since it is preferable that the raw fused alumina powder does not contain particles with a diameter exceeding 100 μm in consideration of the surface roughness of the composition, fused alumina powder that has passed through a sieve with a mesh size of 100 μm is used. The raw material alumina particles (fused alumina particles) may be, for example, fused alumina particles containing less than 1% fine fused alumina particles.

[0036] A stable liquid that does not dissolve alumina, such as water, is used as a solvent for forming a slurry from the raw material fused alumina powder. In this embodiment, ion-exchanged water is used as the solvent. When water is used as the solvent, the concentration of the raw material alumina particles may be, for example, about 70% by mass to 80% by mass.

[0037] An example of a means for forming a slurry of raw alumina particles and water and polishing the resulting slurry is an emulsification / dispersion device (Aspec Disperser ZERO, manufactured by Hiroshima Metal & Machinery Co., Ltd.). In this emulsification / dispersion device, an agitation rotor rotates at high speed within a water-cooled stator. When the raw alumina particles and water described above are introduced into the gap between the stator and the agitation rotor, the rotation of the agitation rotor causes the raw alumina particles to become homogeneously dispersed in the water, forming a slurry (dispersion liquid), and the raw alumina particles collide with each other in this slurry, causing self-polishing.

[0038] The rotation speed of the rotor may be a peripheral speed of 10 m / sec or more. This allows the slurry to swirl and flow at a peripheral speed of 10 m / sec or more, and the raw alumina particles can be polished efficiently. The polishing time of the raw alumina particles in this particle polishing process may be in the range of 3 minutes to 60 minutes. If the polishing time is less than 3 minutes, there is a concern that the specific surface area will not be large enough relative to the raw alumina particles. In addition, if the polishing is performed for a long time, the alumina particles may be crushed and the particles may become too fine. If the particles become too fine, the viscosity may become too high when kneaded with the resin, resulting in poor moldability, or a sufficient amount of filler may not be mixed, resulting in insufficient improvement in thermal conductivity.

[0039] The raw material alumina particles and water may be supplied to the emulsification / dispersion device as two separate liquids, or may be supplied as a premixed slurry.

[0040] Other methods for forming a slurry of raw alumina particles and water and polishing the slurry include bead mills and ball mills, but there are concerns that the crushing effect is too great and that the quality may be reduced due to the inclusion of media such as beads and balls.

[0041] After the above-mentioned particle polishing step, polished fused alumina particles are obtained by solid-liquid separation through filtration and moisture removal through drying. The alumina filler for a thermally conductive resin composition of this embodiment contains 1 mass % or more of fine fused alumina particles having a size of 1 μm or less obtained by the above-mentioned method.

[0042] In this way, the average particle diameter D50 of the fused alumina particles obtained by colliding and polishing raw alumina particles does not change significantly from that of the raw alumina particles. For example, the average particle diameter D50 of the fused alumina particles is larger than the average particle diameter D50 of the raw alumina particles by -15% or more, and is at most about 15%.

[0043] The average particle diameter D50 in this embodiment is the median diameter, that is, the particle diameter at which the cumulative frequency is 50%. The average particle diameter D50 was measured using a laser diffraction scattering type particle size distribution measuring device (MT3300EXII: Microtrack Bell Corporation).

[0044] When raw alumina particles are polished, the average particle diameter D50 of the fused alumina particles is always smaller than the average particle diameter D50 of the raw alumina particles. In other words, in principle, the average particle diameter D50 of the fused alumina particles is never greater than the average particle diameter D50 of the raw alumina particles. However, if fine particles are not sufficiently recovered after polishing, the apparent average particle diameter D50 of the fused alumina particles may be larger.

[0045] On the other hand, the specific surface area of ​​the polished fused alumina particles is significantly increased from that of the raw alumina particles. For example, the change in the specific surface area of ​​the polished fused alumina particles relative to that of the raw alumina particles is at least 25% and at most about 150%.

[0046] This is believed to be the result of the raw alumina particles colliding with each other to slightly round off the sharp corners of the raw alumina particles, resulting in an increase in the number of fine fused alumina particles. FIG. 1 shows a micrograph of the fused alumina particles of this embodiment, and FIG. 2 shows a micrograph of the conventional raw alumina particles. According to this micrograph, it can be seen that the corners of the fused alumina particles after polishing are rounded off on particles of several μm or more, and the number of fine fused alumina particles of 1 μm or less has increased. In this way, the increase in the number of fine fused alumina particles makes it possible to increase the filler content in the resin composition when used as an alumina filler, thereby improving thermal conductivity.

[0047] The alumina filler of this embodiment can be one in which the average particle diameter D50 of the fused alumina particles is larger by -15% or more than the average particle diameter D50 of the raw alumina particles, and more preferably in the range of -15% or more and +15% or less.

[0048] (Method for producing thermally conductive resin composition) In the method for producing the thermally conductive resin composition of the present embodiment, the alumina filler containing the polished electrically fused alumina particles of the present embodiment described above is kneaded into a resin. To knead the alumina filler into the resin, for example, a rotation-revolution type mixer (Mixertaro, manufactured by Thinky Corporation) can be used.

[0049] The thermally conductive resin composition of this embodiment is made of a resin containing the alumina filler of this embodiment. For example, the thermally conductive resin composition of this embodiment can be produced by adding 1200 to 1500 parts by mass of the alumina filler of this embodiment to 100 parts by mass of resin and kneading with a mixer. At this time, the alumina filler contains polished fused alumina particles, so that the amount of the alumina filler can be increased while keeping the hardness or viscosity of the obtained thermally conductive resin composition at the same level, compared to the case where the raw material alumina particles are used as the alumina filler as it is. This allows a thermally conductive resin composition with high thermal conductivity to be obtained.

[0050] Although one embodiment of the present invention has been described above, this embodiment is presented as an example and is not intended to limit the scope of the invention. This embodiment can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the gist of the invention. This embodiment and its modifications are included in the scope of the invention and its equivalents described in the claims, as well as in the scope and gist of the invention. EXAMPLES

[0051] The results of verifying the effects of the present invention are shown below. (Verification example 1) As raw alumina particles (electrically fused alumina particles), electrically fused alumina powder V325F (average particle diameter D50 = 11.1 μm: manufactured by Nippon Light Metal Co., Ltd.) was used. The raw alumina particles were made into a slurry with a concentration of 72 mass% with ion-exchanged water, and the raw alumina particles were subjected to a polishing process using an emulsifier / disperser (Aspec Disperser ZERO manufactured by Hiroshima Metal & Machinery Co., Ltd.) with the peripheral speed of the stirring rotor set to 35 m / s and the time set to 60 minutes. As a result, electrically fused alumina particles of Verification Example 1 (hereinafter referred to as polished alumina particles 1) were obtained.

[0052] Then, the electrically fused alumina particles 1 and a butadiene-based polymer (R-45HT: manufactured by Idemitsu Kosan Co., Ltd. (hereinafter referred to as resin 1)) were kneaded using a rotation-revolution type mixer (Awatori Rentaro: manufactured by Thinky Corporation) to obtain a thermally conductive resin composition of Verification Example 1. FIG. 3 shows a graph showing the relationship between the parts by mass (PHR) of raw alumina particles and polished alumina particles 1 added per 100 parts by mass of resin 1 and the thermal conductivity of the resulting thermally conductive resin composition. The thermal conductivity was measured by a disk heat flow meter method (made by our company, based on JIS A 1412-1 or ASTM D5470, with an aluminum rod).

[0053] 3, the measured value of the thermal conductivity of the thermally conductive resin composition does not change significantly between the case where raw alumina particles are added to resin 1 and the case where polished fused alumina particles 1 are added. Therefore, it was confirmed that there is no difference in the filling state between the raw alumina particles and the polished fused alumina particles 1. On the other hand, in the case of raw alumina particles, a maximum of 1200 parts by mass of raw alumina particles could be added per 100 parts by mass of resin, whereas in the case of polished fused alumina particles, 1400 parts by mass could be added. Therefore, the thermally conductive resin composition using polished fused alumina particles as a filler was able to increase the thermal conductivity because a larger amount of filler could be added.

[0054] (Verification example 2) As raw alumina particles (electrically fused alumina particles), electrically fused alumina powder V325F (average particle size D50 = 11.1 μm: manufactured by Nippon Light Metal Co., Ltd.) was used (hereinafter referred to as raw material 1). 1270 g of this raw material 1 was used and mixed with 680 g of ion-exchanged water to form a slurry, and raw material 1 was subjected to a polishing treatment using an emulsifying / dispersing device (Aspec Disperser ZERO manufactured by Hiroshima Metal & Machinery Co., Ltd.) with a peripheral speed of 35 m / s and a time of 3 minutes (sample 01), 30 minutes (sample 02), 45 minutes (sample 03), and 60 minutes (sample 04). Then, 100 parts by mass of Resin 1 and 1,400 parts by mass each of Raw Material 1 and Samples 01 to 04 were kneaded together to prepare a thermally conductive resin composition of Verification Example 2.

[0055] Table 1 shows the specific surface area and average particle size D50 of raw material 1 and samples 01 to 04, and the rate of change of each compared to raw material 1. Table 1 also shows the hardness of each thermally conductive resin composition using raw material 1 and samples 01 to 04, and the rate of change of each compared to the thermally conductive resin composition using raw material 1. The instruments used for each measurement are as follows. Measurement of specific surface area: BET method, fully automatic gas adsorption measurement device (Autosorb-iQ: Quantachrome Instruments Japan) Measurement of average particle diameter D50: Laser diffraction scattering method, particle size distribution measuring device (MT3300EXII: Microtrack Bell Co., Ltd.) Hardness measurement: Durometer (Asker Rubber Hardness Tester Type A: Kobunshi Keiki Co., Ltd.)

[0056] [Table 1]

[0057] (Verification example 3) As raw alumina particles (electrically fused alumina particles), a uniform mixture of 75 mass% of electrically fused alumina powder V325F (average particle size D50 = 11.1 μm: manufactured by Nippon Light Metal Co., Ltd.) and 25 mass% of electrically fused alumina powder F220 (average particle size D50 = 60 μm: manufactured by Nippon Light Metal Co., Ltd.) was used (hereinafter referred to as raw material 2). 1270 g of this raw material 2 was mixed with 680 g of ion-exchanged water to form a slurry, and raw material 2 was subjected to a polishing treatment using an emulsifier / disperser (Aspec Disperser ZERO manufactured by Hiroshima Metal & Machinery Co., Ltd.) at a peripheral speed of 32 m / s for a time of 15 minutes (sample 11), 30 minutes (sample 12), and 45 minutes (sample 13). Then, 100 parts by mass of Resin 1 and 1,400 parts by mass each of Raw Material 2 and Samples 11 to 13 were kneaded together to prepare a thermally conductive resin composition of Verification Example 3.

[0058] Table 2 shows the specific surface area and average particle size D50 of raw material 2 and samples 11 to 13, and the rate of change of each relative to raw material 2. Table 2 also shows the hardness of each thermally conductive resin composition using raw material 2 and samples 11 to 13, and the rate of change of each relative to the thermally conductive resin composition using raw material 2. The instruments used for each measurement were the same as those in Verification Example 1.

[0059] [Table 2]

[0060] (Verification example 4) As raw alumina particles (electrically fused alumina particles), a uniform mixture of 50 mass% of electrically fused alumina powder V325F (average particle size D50 = 11.1 μm: manufactured by Nippon Light Metal Co., Ltd.) and 50 mass% of electrically fused alumina powder F220 (average particle size D50 = 60 μm: manufactured by Nippon Light Metal Co., Ltd.) was used (hereinafter referred to as raw material 3). 1270 g of this raw material 3 was mixed with 680 g of ion-exchanged water to form a slurry, and raw material 3 was subjected to a polishing treatment using an emulsifier / disperser (Aspec Disperser ZERO manufactured by Hiroshima Metal & Machinery Co., Ltd.) at a peripheral speed of 32 m / s for a time of 15 minutes (sample 21), 30 minutes (sample 22), and 45 minutes (sample 23). Then, 100 parts by mass of Resin 1 and 1,400 parts by mass each of Raw Material 3 and Samples 21 to 23 were kneaded together to prepare a thermally conductive resin composition of Verification Example 4.

[0061] Table 3 shows the specific surface area and average particle size D50 of raw material 3 and samples 21 to 23, and the rate of change for each of them relative to raw material 3. Table 3 also shows the hardness of each of the thermally conductive resin compositions using raw material 3 and samples 21 to 23, and the rate of change for each of the thermally conductive resin compositions using raw material 3. The instruments used for each measurement were the same as those in Verification Example 1.

[0062] [Table 3]

[0063] (Verification example 5) As raw alumina particles (electrically fused alumina particles), electrically fused alumina powder V325F (average particle size D50 = 11.1 μm: manufactured by Nippon Light Metal Co., Ltd.) was pulverized and classified by a jet mill (model number STJ-200: manufactured by Seishin Enterprise Co., Ltd.) to obtain an electrically fused alumina powder having an average particle size D50 = 3.9 μm (hereinafter referred to as raw material 4). 720 g of this raw material 4 was mixed with 680 g of ion-exchanged water to form a slurry, and raw material 4 was subjected to a polishing treatment using an emulsifier / disperser (Aspec Disperser ZERO manufactured by Hiroshima Metal & Machinery Co., Ltd.) with a peripheral speed of 32 m / s and a time of 30 minutes (sample 31) and 60 minutes (sample 32). Then, 100 parts by mass of Resin 1 and 1100 parts by mass each of Raw Material 4, Samples 31, and 32 were kneaded together to prepare a thermally conductive resin composition of Verification Example 5.

[0064] Table 4 shows the specific surface area and average particle size D50 of raw material 4, samples 31, and 32, and the rate of change relative to raw material 4. Table 4 also shows the hardness of each thermally conductive resin composition using raw material 4, samples 31, and 32, and the rate of change relative to the thermally conductive resin composition using raw material 4. The instruments used for each measurement are the same as those in Verification Example 1.

[0065] [Table 4]

[0066] According to the results shown in Tables 1 to 4, it was confirmed that by polishing the commercially available fused alumina powders, raw materials 1 to 4, respectively, it is possible to increase only the specific surface area (+25% to +146%) without significantly changing the average particle diameter D50 (within the range of -15% to +10%).

[0067] Furthermore, it was confirmed that the thermally conductive resin compositions of this embodiment, which were prepared using samples 01-04, 11-13, 21-23, 31, and 32 obtained by polishing raw materials 1-4, have reduced hardness (-9% to -57%) and improved shape conformability compared to conventional thermally conductive resin compositions prepared using raw materials 1-4.

[0068] (Verification example 6) Using the raw material 1 and sample 04 of the above-mentioned verification example 1, 400 parts by mass and 600 parts by mass of resin 1 were kneaded with 100 parts by mass, respectively, to prepare thermally conductive resin compositions (compositions 1 to 4), and the viscosities were measured. The viscosities and the rate of change in viscosity are shown in Table 5. The instruments used for the measurements are as follows: Viscosity measurement: B-type viscometer (PM-2A, manufactured by Malcom Co., Ltd.)

[0069] [Table 5]

[0070] According to the results shown in Table 5, it was confirmed that, compared with the conventional thermally conductive resin compositions 1 and 2 using raw material 1, thermally conductive resin compositions 3 and 4 using sample 04, which is the polished fused alumina particles of this embodiment, have a reduced viscosity (-37% to -59%) and improved shape conformability.

[0071] (Verification example 7) A two-hour sedimentation test was conducted on raw material 1, sample 04, and fused alumina powder (sample 05) obtained by grinding raw material 1 with a bead mill (manufactured by IMEX Co., Ltd.: peripheral speed 7.2 m / s) in the above-mentioned Verification Example 1 to identify their properties.

[0072] The test method was to mix 1 g of each of the fused alumina powders (raw material 1, sample 04, and sample 05) with 40 g of ion-exchanged water to prepare a slurry (each with a concentration of 2.4% by mass), and pour it into a sample tube with a lid (inner diameter 10 mm) so that the liquid level was 20 mm high. After leaving it to stand at room temperature for 2 hours, the supernatant solids were separated and their mass was measured. The ratio of the supernatant solids mass to the total solids mass was calculated. The results are shown in Table 6. The test conditions are shown in Figure 4.

[0073] [Table 6]

[0074] According to the results shown in Table 6, it was found that the polished fused alumina powders of this embodiment (samples 04 and 05) had total solid mass relative to the supernatant solid mass of 5.7% by mass and 0.3% by mass, respectively, compared to the fused alumina powder of Raw Material 1 (Raw Material 1). It was also found that the ratio of the total solid mass to the supernatant solid mass tends to increase as the polishing time of the fused alumina powder of Raw Material 1 becomes longer.

[0075] From these results, it was confirmed that fine fused alumina particles of 1 μm or less, which are fine enough to float on water, are formed by polishing the fused alumina particles (raw material 1). The formation of such fine polished fused alumina particles of 1 μm or less increases the specific surface area of ​​samples 04 and 05 relative to raw material 1, and improves the thermal conductivity.

Claims

1. An alumina filler for a thermally conductive resin composition, comprising fused alumina particles which are abraded raw alumina particles, The fused alumina particles contain 1 mass % or more of fine fused alumina particles which are supernatant solids in a 2-hour sedimentation test in water, An alumina filler for a thermally conductive resin composition, characterized in that the specific surface area of ​​the electrically fused alumina particles is 25% or more larger than the specific surface area of ​​the raw material alumina particles.

2. A thermally conductive resin composition comprising the alumina filler for thermally conductive resin compositions according to claim 1 in a resin.

3. 3. The thermally conductive resin composition according to claim 2, wherein the alumina filler for thermally conductive resin compositions is contained in an amount of 1,200 parts by mass or more per 100 parts by mass of the resin.

4. A method for producing the alumina filler for a thermally conductive resin composition according to claim 1, comprising the steps of: A method for producing an alumina filler for a thermally conductive resin composition, comprising a particle polishing step of rotating a slurry of a mixture of fused alumina particles and a solvent at a peripheral speed of 10 m / sec or more to cause the fused alumina particles to collide with each other and be polished.

5. 5. The method for producing an alumina filler for a thermally conductive resin composition according to claim 4, wherein the particle polishing step is carried out for a period of time ranging from 3 minutes to 60 minutes.

6. 6. The method for producing an alumina filler for a thermally conductive resin composition according to claim 4 or 5, characterized in that the particle polishing step is a step of increasing the specific surface area of ​​the fused alumina particles by 25% or more compared to the specific surface area of ​​the fused alumina particles before the particle polishing step is performed.

7. The method for producing an alumina filler for a thermally conductive resin composition according to any one of claims 4 to 6, characterized in that the particle polishing step is a step of increasing the average particle diameter D50 of the fused alumina particles by -15% or more compared to the average particle diameter D50 of the fused alumina particles before the particle polishing step is carried out.

Citation Information

Patent Citations

  • JP1973017683B1

  • Composite powder

    JP2002020652A

  • Aluminum oxide powder composition and heat-conductive molding containing the same

    JP2003342021A

  • Alumina products and their use in high thermal conductivity polymer compositions

    JP2019521061A

  • Spherical alumina powder and resin composition

    JP4361997B2