Refining quartz flour by removing fine particles of refractory minerals.
The elutriation process in a fluidized bed reactor effectively separates refractory mineral particles from quartz powder, addressing the inadequacies of existing methods and producing high-purity quartz suitable for advanced industrial applications.
Patent Information
- Application Number
- JP2020119141
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-07-12
- Filing Date
- 2020-07-10
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-07-10
AI Technical Summary
Existing methods are inadequate for effectively removing refractory mineral particulates, particularly those containing rare earth metals and radioactive elements, from quartz powder, which are detrimental to the quality of fused silica products used in optical fibers and semiconductor manufacturing.
An elutriation process in a fluidized bed reactor is used to separate fine refractory mineral particles from quartz powder by exploiting differences in size and density, with a controlled upward flow of a liquid phase, allowing the refractory minerals to be transported upwards and separated from the quartz powder.
The process efficiently removes refractory mineral particles, including rare earth and radioactive contaminants, resulting in high-purity quartz powder suitable for critical applications in optical fibers and semiconductor manufacturing.
Smart Images

Figure 0007584246000005 
Figure 0007584246000006 
Figure 0007584246000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a process for purifying quartz flour by removing fine particles of refractory minerals from the quartz flour, including certain minerals containing rare earth compounds. The invention is further directed to the use of an elutriation process to remove these fine particles of refractory minerals from the quartz flour. Finally, the invention also relates to quartz flour produced according to the claimed invention and having a low content of such fine particles of refractory minerals. [Background technology]
[0002] Fused silica glass, glass made by melting purified natural quartz powder, is used today in many industrial applications. Its use in light bulbs, laboratory equipment, and the like has long been known, and it has been used as a container or contact material in semiconductor manufacturing, and even in the manufacture of optical fibers. However, for some of these latter applications, the purity achieved by currently known quartz refining procedures is less than ideal. For this reason, the majority of optical fibers are now made entirely from synthetic fumed silica, and for high quality semiconductor applications, synthetic glass is also desirable.
[0003] In the early days of optical fiber for telecommunications, the majority of fibers were composed of glass made by melting highly refined natural quartz crystals. However, as the industry progressed, fiber breakage became a serious problem, and it was discovered that the main cause of such breakage was due to discrete micron- or submicron-sized refractory mineral particles, typically minerals such as monazite and xenotime, i.e. mixtures of rare earth element phosphates and sometimes rare earth element oxides, that were not removed by the quartz refining techniques then available. These particulates are present to a greater or lesser extent in all sources of natural quartz crystals, and are particularly prominent in the quartz obtained from pegmatite rocks, which constitute the main source of high-purity quartz flour used in industry today.
[0004] In these commercially available refined quartz powders, these refractory refractory particles generally have a size of less than 25 μm, typically less than 5 μm, and in fact the majority are much smaller, typically less than 1 μm, i.e., the size of colloidal particles. Without being bound by any theory, it is believed that their small size allows them to assume a surface potential when in aqueous suspension, allowing them to be electrostatically bound to silica particles by forces that prevail over the gravitational and attractive forces that affect larger sized particles. This interaction is more pronounced at particle sizes less than 10 μm. Furthermore, because these particles are very inert and have very high melting points, it has been found that they are difficult to remove from the quartz powder, while it has been found impossible to remove them from the resulting fused quartz glass products.
[0005] Fiber breakage studies have shown that particles smaller than 0.5 μm in size can cause breakage in optical fibers if present in the cladding glass. As a result, for many years the majority of the fiber optic manufacturing industry has sought synthetic fused silica, which can be guaranteed to be free of such particles.
[0006] More recently, it has also become evident that for certain applications in the semiconductor industry, it is desirable to replace some critical quartz glass components with components made from synthetic fused silica, because there is a risk that occasional refractory mineral particles will be exposed to the surface of the quartz glass and enter the environment as dust particles, which will reach the wafers being processed and reduce the yield. It is also noted that some of these refractory mineral particles contain thorium and uranium, and the presence of such radioactive species is particularly undesirable in semiconductor manufacturing processes. Finally, these insoluble particulates can present problems in certain processes for the melting of quartz, because under certain circumstances they can provide nucleation sites for the growth of bubbles in the fused quartz product.
[0007] In summary, the presence of refractory mineral particulates, when they are present in quartz powder materials, creates problems with respect to the final optical quality, particularly with respect to the quality required for most important semiconductor plasma etching applications, and for use in the manufacture of cladding for optical fibers.
[0008] If these refractory minerals could be eliminated, or at least substantially reduced, during the quartz refining process, fused silica glass would be a potential alternative to synthetic silica in some of the applications mentioned above.
[0009] Currently, the standard method of producing high purity quartz flour for fusion involves crushing and grinding the raw material (typically pegmatite rock), sieving, magnetic separation, froth flotation, and leaching (washing) with an acid, for example hydrofluoric acid, optionally mixed with another mineral acid (e.g. hydrochloric, nitric or sulfuric acid). The quartz flour is then washed with pure water and dried before being used to make fused quartz.
[0010] In addition, the quartz powder may be subjected to high-temperature treatment in reactive gases, for example, through a rotary kiln in the presence of a chlorine-containing atmosphere, for example, Cl2 or HCl. Such high-temperature chlorination treatments as part of the process for producing high-purity quartz powder are described, for example, in EP 0737653 and US 7837955. During such high-temperature chlorination treatments, impurity particles such as refractory minerals present inside the particles may cause voids in the quartz particles, which may cause the refractory minerals to become exposed or even liberated on the quartz powder surface. Thus, when high-temperature chlorination or other high-temperature treatment steps are performed in quartz powder purification, it is expected that the refractory mineral fine particles will be exposed, and their removal will be facilitated by an appropriate process.
[0011] Despite the various refinements provided by known processes, the quartz flours available today still retain some degree of refractory minerals that make them unacceptable for most critical applications.
[0012] The state of the art for the purification of quartz powder can be summarized as follows: China Patent Publication No. 106082238 discloses a process for the production of quartz powder, in which the starting material is granulated (crushed and finely ground) and subjected to a high-temperature chlorination process. After the high-temperature chlorination process, the obtained quartz powder is further subjected to two successive process steps, in which the first process step is quenching the quartz powder with water, and the second step is leaching the quartz powder with an acid mixture, including hydrofluoric acid, hydrochloric acid, sulfuric acid and oxalic acid. During this leaching step, ultrasonic treatment may be applied. Then, the solid phase is separated from the liquid phase by filtration, and the solid residue is then washed and dried. CN106082238 does not teach or suggest the same problem of removing insoluble refractory mineral particles from quartz flour as the present invention, and even if the leaching process may lead to the release of some refractory mineral particles that may be attached to the quartz flour particles, the refractory mineral particles that are the subject of the present invention are insoluble in the acid mixture and have a small particle size, so that they are expected to remain attached to the quartz flour particles and become contaminants in the subsequent conventional filtration process, unless some form of elutriation is used to achieve the separation. No analytical charts are provided, and there is no evidence that significant separation of the refractory mineral particles from the quartz flour has been achieved.
[0013] East German Patent 160967 discloses a process for the purification of quartz flour, in which the starting material is first subjected to a crushing and grinding process and then treated with hydrochloric acid. In the next step, the quartz flour is subjected to a high-temperature chlorination process and treated with hydrofluoric acid. After this acid treatment, the acid is separated from the quartz flour by filtration. Since the refractory minerals remain unaffected by the treatment with hydrofluoric acid, the acid separation suggested by East German Patent 160967 cannot be expected to lead to the removal of refractory mineral particles from the quartz flour, and the analytical diagrams presented do not provide any evidence to the contrary.
[0014] JP 62-30632 discloses a process for producing high purity quartz glass from natural siliceous raw materials. During this manufacturing procedure, the quartz powder is subjected to a chlorination treatment and then purified by immersion in a mixture of hydrofluoric and nitric acids. After washing with nitric acid and then with water, the quartz powder is filtered and dried. Analysis diagrams show that a significant reduction in the content of alkali metals (lithium, sodium and potassium) is achieved by this process, and also that of the radioactive element uranium is greatly reduced. No effort is made to separate the refractory mineral particles. Furthermore, the immersion and washing treatments described in this Japanese prior art document do not result in the separation of the refractory mineral particles from the quartz powder.
[0015] US Patent 4,804,422 discloses a process for treating quartz flour that can be obtained from pegmatite-based raw materials after initial beneficiation by crushing and flotation and magnetic separation. Quartz flour, usually with a particle size of less than 0.5 mm, is treated in hydrofluoric acid for a time sufficient to dissolve at least 40% by weight of the quartz sand, washed with demineralized water, and then treated with hot hydrochloric acid for at least 30 minutes. This latter step is said to be useful in reducing the level of phosphate impurities; however, it has been found that this procedure does not eliminate all of the refractory mineral fines. There is no indication that any attempt was made to separate these refractory mineral fines by elutriation. A filter is provided at the top of the treatment column to prevent particles from escaping the column and to allow the acid to pass onward through a circulation pump, but it is clear that any particles collected by the filter remain in the leaching vessel along with the quartz flour being treated. Thus, at the end of the process, the refractory minerals are well mixed with the larger quartz particles and may even adhere to the quartz powder particles. Removal of fine particles can only be avoided by operating at low flow rates to allow elutriation and by additionally using fine (submicron) filters in the circulation path of the liquid phase, which are not used in the disclosed process. Without such fine filters, the micron- and submicron-sized particles that pass through the filters would remain in the circulating acid and return to the leaching vessel. The powder product after such a process is expected to retain significant levels of refractory particulate contaminants.
[0016] China Patent Publication No. 102303870 describes a process for leaching quartz sand in a fluidized bed. The various configurations described all incorporate a cylindrical fluidized vessel in which the particles are suspended in an upward flow of heated acid, which is recirculated by a pump. At the top of the vessel, the acid overflows into a surrounding trough and the entrained sand particles are collected in a "sand basin". This "sand basin" is apparently used to settle and remove the sand particles ("settling") before the acid passes to the pump. Refractory mineral fine particles, for example with a particle size of less than 5 μm, do not settle at this point but remain in suspension which is recirculated with the flowing acid. Thus, there is no disclosure of how to remove the refractory mineral fine particles with a particle size of less than 5 μm.
[0017] China Patent Publication No. 104843718 discloses a process for anaerobic chlorination of silica, in which chlorination is carried out in a vertical chlorination reactor, followed by treatment in an acid extraction tank and flotation in a gravity tank to remove impurities. This prior art document disclosure does not provide any specific conditions for flotation in a gravity tank. Furthermore, it does not mention which impurities are removed from silica in the flotation procedure.
[0018] US Patent 9776194 discloses an analytical method for detecting the presence of large particles of refractory minerals (so-called heavy minerals) in quartz flour, i.e. particles of a size comparable to that of quartz sand, but does not provide a satisfactory method of how to remove such impurities in the manufacturing process. The method described in US Patent 9776194 consists of conditioning quartz flour suspected of containing refractory minerals such as heavy mineral particles into an aqueous pulp using a flotation agent; subjecting the conditioned pulp to flotation to obtain tailings; combining the tailings with an aqueous solution having a density less than that of the heavy minerals larger than quartz that are to be separated; and finally centrifuging the combination to bring about the sedimentation of the refractory minerals. Although this technique may be useful for testing the presence of refractory minerals in quartz flour analytical samples, it requires an aqueous solution of expensive chemical reagents (e.g. sodium heteropolytungstate) and requires the samples to be centrifuged at high speeds, which is possible for samples of limited size but is not suitable for practical purification of quartz on an industrial scale. Furthermore, when performed previously on commercially available high purity quartz powder, this analytical technique has not revealed the presence of refractory mineral particulates less than 10 μm in size.
[0019] US Patent 6,746,655 relates to a method for cleaning SiO2 particles by loading the particles into a vertical reactor and treating them with an upward flow of fluidizing gas (HCl) (thus forming a fluidized bed) at a temperature of at least 1000°C to form gaseous metal chlorides or other volatile compounds that can be removed from the reactor as exhaust gas. The flow rate is set to at least 10 cm / s and the retention time can be approximately 12 hours. The method is used to remove metallic contaminants of Li, Na, Mg, Cu, Fe, Ni, Cr, Mn, V, Ba, Pb, C, B and Zr, and there is no mention of separating refractory mineral particles from quartz powder. Furthermore, US Patent 6,746,655 does not disclose a filter with a pore size of 0.7 μm or less, and only relates to a dust separator for separating contaminants in the form of fine dust and condensed compounds from an exhaust gas stream. The process disclosed therein is not an elutriation process and no liquid fluid is used.
[0020] EP 1 942 078 A1 relates to a method for purifying silica powder, according to which the silica powder is fluidized (in a fluidized bed) and contacted with a purification gas (HCl or Cl2) at high temperature (1200°C), thereby removing the highly ionic impurities (alkaline impurities) of the silica powder. For this purpose, the fluidized silica powder is placed in a magnetic field. As in the method of US Pat. No. 6,746,655, in this method the impurities (for example Li, Na, K) come into contact with the purification gas on the surface of the silica powder, react and evaporate (to chlorine gas, etc.), and the gas produced is discharged. In essence, the process of EP 1 942 078 A1 is a purification process by reaction of the impurities in a hot gas stream, which is removed as vapor. The process of elutriation in a liquid medium is not described.
[0021] Canadian Patent Publication 1184740 relates to a method for producing high purity silica, according to which impurities such as iron oxides and feldspars and other alumina and calcia bearing compounds can be removed from silica or quartz concentrates (both from the surface and from plugs) by treating the concentrates with an aqueous solution containing 3 to 20% by weight of HF at temperatures above about 50° C. and with stirring for several hours. The impurities (feldspars, alumina and calcia bearing compounds) dissolve at a greater rate than the silica and can be separated as slime (desliming or flotation) or washed away with water. According to Canadian Patent Publication 1184740, the quartz or silica concentrate has already been subjected to a pre-treatment (beneficiation) such as size separation, wet or dry screening, magnetic separation, flotation or a combination of these. Furthermore, there is no mention of the content of rare earth minerals either before or after the treatments described. Summary of the Invention [Problem to be solved by the invention]
[0022] There is thus a need for new processes for the purification of quartz flour that make it possible to remove contaminating refractory mineral particles from the quartz flour.
[0023] It is therefore an object of the present invention to provide a method for the purification of quartz flour, from which refractory mineral fines are efficiently removed. [Means for solving the problem]
[0024] This problem is solved in a first embodiment of the present invention by a process for the purification of quartz flour, comprising a step of separating fine particles of a refractory mineral from the quartz flour by an elutriation step, in which the fine particles of the refractory mineral comprise minerals containing rare earth metals and / or thorium and / or uranium, and in which the elutriation step is carried out in a fluidized bed reactor, in which a controlled upward flow of the liquid elutriate phase is provided, whereby the fine particles of the refractory mineral are carried upwards in the fluidized bed reactor, whereas the quartz flour remains in the lower region of the fluidized bed reactor.
[0025] Furthermore, this problem is solved in a second aspect of the invention by a process for the purification of quartz flour, which comprises a step of separating fine particles of refractory mineral from the quartz flour by an elutriation step, in which the purified quartz flour has a size of 75 μm to 1000 μm and the refractory mineral has a particle size of less than 50 μm. In this second aspect of the invention, it is understood that the elutriation step is preferably carried out in a fluidized bed reactor, in which a controlled upward flow of the liquid elutriation phase is provided, whereby the fine particles of refractory mineral are carried upwards in the fluidized bed reactor, while the quartz flour remains in the lower region of the fluidized bed reactor.
[0026] Surprisingly, it has been found that contaminating refractory mineral particles can be removed from quartz flour during a novel purification process which firstly ensures that the refractory minerals do not remain bound to the quartz crystals and secondly, the quartz flour is subjected to an elutriation step.
[0027] In the present invention, elutriation refers to a process for separating particles based on their size, shape and / or density, usually using a liquid flow that flows in a direction opposite to the settling direction. Thus, as used in the present invention, elutriation is a reverse settling process in which the particles to be separated, i.e., quartz particles and refractory mineral particles, are dispersed in an upwardly flowing fluid flow, thereby allowing them to be separated from the quartz powder particles by using a vertically oriented liquid flow, despite the greater density of the refractory mineral fine particles. However, in the present invention, despite their greater density (unusually), the refractory mineral fine particles float more than the quartz particles in the upward flow of liquid and emerge in the overflow liquid and may be separated therefrom, leaving the less dense quartz particles in the elutriation vessel.
[0028] The present invention is therefore based on the discovery that it is possible to separate small sized, heavy rare earth particles from larger particles of low density quartz sand by upward elutriation of the rare earth particles, despite their high density.
[0029] In the present invention, refractory particulates are understood to mean solid particles of minerals or other synthetic inorganic materials that have a high melting point and / or are heat resistant, these particles generally having a particle size of less than 50 μm, in particular less than 25 μm, in particular less than 10 μm, in particular less than 5 μm, in particular less than 1 μm.
[0030] In one embodiment, the refractory minerals include rare earth materials, such as rare earth minerals (= minerals containing rare earth metals) and / or rare earth metals. Thus, the process according to the invention is particularly suitable for separating and removing rare earth materials as refractory minerals from quartz flour. Rare earth materials in the sense of the invention are so-called "heavy minerals", including, but not limited to, all types of monazite (mixtures of rare earth element phosphates) and xenotime (i.e. rare earth mineral complexes containing yttrium phosphate as the main component). In addition to these rare earth materials, the rare earth materials removed from the quartz flour may contain low levels of radioactive metals, such as thorium and uranium. Such minerals may be present in the bulk quartz crystal flour in relatively small amounts (less than 1 ppm), but have proven difficult to remove by standard methods in the industry and, as already dealt with above, even these small levels are undesirable for transparent fused quartz glass products.
[0031] Thus, the rare earth materials removed from the quartz flour are mostly rare earth phosphates and are selected from the group consisting of, for example, monazite-(Ce)(Ce,La,Nd,Th)PO4, monazite-(La)(La,Ce,Nd)PO4, monazite-(Nd)(Nd,La,Ce)PO4, monazite-(Sm)(Sm,Gd,Ce,Th)PO4 and yttrium orthophosphate (YPO4) including various other rare earth elements, and potentially xenotime in combination with Ca, U, Th, Si, F and As. Furthermore, it has been found that the process step of elutriation also offers the possibility of removing radioactive materials such as thorium and uranium from the quartz flour.
[0032] Exemplary monazite and xenotime particles found in commercially available purified quartz powder and analyzed by laser ablation (LA) ICP-MS analysis had the chemical compositions shown in Table 1 below.
[0033] [Table 1]
[0034] Table 1 shows the analysis of several individual particles of composite rare earth particles extracted from commercial quartz powder using the method of US Pat. No. 9,776,194.
[0035] Although fines of other refractory minerals may be present, monazite and xenotime have been found to predominate, and so the material separated from the quartz flour is hereinafter collectively referred to as RE (i.e. Rare Earth) fines.
[0036] The process for the purification of quartz flour according to the invention can be generally summarized as follows: As already explained, this process for the purification of quartz flour comprises a step of separating the RE fine particles from the quartz flour by an elutriation step.
[0037] The elutriation step according to the invention may be carried out in a fluidized bed reactor. Fluidized bed reactors are known to those skilled in the art. In this type of reactor, a fluid (usually a gas or liquid, preferably a liquid) is passed through a slurry of quartz powder to be purified at a sufficient velocity to suspend at least a portion of the solids so that they behave as if they were a fluid. This process is known as fluidization. In the present invention, a fluidized bed reactor can be used with a reactive fluid such as hydrofluoric acid to carry out an etching reaction on the surface of the quartz particles during elutriation. Alternatively, the suspended powder can be treated with an inert fluid such as water to carry out elutriation without reacting the powder with the fluid.
[0038] The solid matter material in the fluidized bed reactor (i.e., quartz powder with RE fines) is typically supported by a porous plate known as a distributor. A fluid, referred to here as the liquid elutriation phase, is then forced up through the solid material via the distributor. At low flow rates, the solids remain in place and the fluid passes through the voids in the material. As the flow rate is increased, the reactor reaches a stage where the force of the fluid on the solids is sufficient to cause fluidization of all the particles. In the present invention, the vessel is preferably cone-shaped, tapering to a smaller diameter towards the bottom. Thus, the upward velocity of the fluid decreases with increasing height. In this case, a separation of the quartz particles occurs according to their size, with the larger particles of quartz accumulating in the lower region of the fluidized bed reactor (immediately adjacent to the distributor) and the smaller quartz particles rising to the top. Although the density of the RE fines is greater than that of quartz, it has been found that these fines rise to the top of the fluidized bed reactor due to their much smaller size. At this stage, the intended separation of the quartz powder and the RE particles occurs.
[0039] Thus, the process according to the invention includes a step of separating the RE fines from the quartz powder by an elutriation step, in which a controlled upward flow of a liquid elutriation phase is provided, whereby the RE fines are carried upward in the fluidized bed reactor, whereas the quartz powder particles remain in the lower region of the fluidized bed reactor, which is the region of the fluidized bed reactor in close proximity to the distributor, where the quartz powder remains during the upward flow of the liquid elutriation phase.
[0040] Thus, one particular feature of the present invention is that the process according to the invention is carried out in a fluidized bed reactor. The technical term fluidized bed reactor is meant in the present invention to mean an elutriation vessel that allows the fluidization of suspended particles when it is required to keep all particles in homogeneous or heterogeneous suspension. In that sense, the elutriation vessel used in the process according to the present invention is an elutriation vessel that may be used to allow leaching of powders in acid and that has the potential to be used under conditions that allow fluidization, optionally including elutriation. In the process according to the present invention, the RE fines carried upwards in the fluidized bed are preferably discharged from the fluidized bed reactor together with the liquid elutriation phase or are separated from the liquid elutriation phase, which can then be recycled.
[0041] Since the liquid elutriate phase is preferably recycled from the top of the fluidized bed reactor to the bottom of the fluidized bed, the removed RE fines should preferably be removed from the liquid elutriate before being recycled.
[0042] Thus, in one further preferred embodiment of the process according to the invention, the liquid elutriate phase is recycled into the elutriation step and the RE fines are separated from the liquid elutriate phase, for example by filtration.
[0043] The RE particulates are separated from the elutriate phase by filtering the elutriate phase, preferably using a filter with a pore size of 0.7 μm or less.
[0044] To separate the RE fines from the quartz powder prior to the elutriation step, it is further preferred that the separation of the RE fines from the quartz powder is assisted by ultrasonic agitation or agitation caused by a liquid or gas flow.
[0045] It may also be desirable to provide suitable heating to the vessel, to the recirculated liquid, or to both during the acid treatment and subsequent elutriation. Deagglomeration of fine particles from larger quartz particles may be promoted by pH control, by the addition of deflocculating agents, surfactants, chelating agents, etc., and may be facilitated by ultrasonic agitation or other means. Heating of the liquid phase may be useful in increasing the effectiveness of some of these processes.
[0046] For the sake of completeness, it is noted that elutriation can be applied during any stage where an upward flow of liquid is achieved, in particular during etching (such as etching with HF), during subsequent washing (such as washing with HCl) and during water washing, and can be carried out during one or more of these steps.
[0047] During the process, it is useful to perform a dilute HCl wash after the HF leaching step, because if the HF leaching is followed immediately by a water wash, a silica gel precipitate may be prepared by hydrolysis of the hexafluorosilicic acid present in this liquid phase. This is undesirable, but is less of a problem if the etching acid mixture already contains an acid other than HF, such as HCl or NO3.
[0048] As outlined in more detail below, the elutriation step according to the invention may be carried out in the sequence of process steps for the purification of quartz flour, in particular before or after the calcination and / or high-temperature chlorination steps of the quartz flour. Most of the other process steps for the purification of quartz flour are known to those skilled in the art.
[0049] Under elutriation conditions, the fluidized bed leaching and washing operations result in the separation of the quartz powder by particle size, with the smaller quartz particles rising to the upper region of the leaching vessel. Thus, after the elutriation step, it is preferable for the refined quartz powder to be homogenous before removal from the fluidized bed reactor. This ensures that when the slurry of quartz particles is drained from the reactor, the particle size distribution of the powder is consistent and uniform throughout the batch. Homogenization of the refined quartz powder may be accomplished by agitation, particularly by a liquid or gas flow, or by ultrasonic agitation.
[0050] The quartz powder to be refined usually has a size of 75 μm to 1000 μm, preferably 75 μm to 250 μm, whereas the RE fine particles usually have a particle size of less than 50 μm, in particular less than 25 μm, in particular less than 10 μm, in particular less than 5 μm, in particular less than 1 μm.
[0051] As described in more detail below, the liquid elutriation phase is preferably the leaching acid used to leach the quartz powder during the typical production process. In such a case, the filter for removing RE particulates from the liquid elutriation phase used in the recycle mode is preferably an acid-resistant filter. Alternatively, or additionally, the liquid elutriation phase may include a water stream used to remove traces of leaching acid and soluble products prior to removing the purified quartz from the vessel.
[0052] Furthermore, the liquid elutriate phase is in particular an aqueous acid other than hydrofluoric acid, and is used to wash the powder after acid leaching.
[0053] Furthermore, the liquid elutriate phase is in particular water and is used to wash the powder after leaching with acid.
[0054] The source of quartz flour used as starting material in the purification process according to the invention may be derived from pegmatites, i.e. coarse-grained granitic igneous rocks. These typically contain an intimate mixture of feldspar, mica and quartz crystals, as well as a diverse range of RE fines. A significant degree of purification of quartz is possible by processes such as grinding, leaching, flotation and others; indeed, flotation is a standard technique in the industry. McEwen et al., "One-Stage Flotation of Alkali Feldspar, Ilmenite, Rutile, Garnet and Monazite on a Mixed Cationic / Anionic Collector", Institute of Mining Engineers, AIME, vol. 260, pp 97-100 (1976), describes the flotation of feldspar and other heavy minerals from quartz using cationic / anionic collectors. However, these techniques do not result in complete separation of the contaminant species, and many smaller RE fine crystals remain in the quartz flour and cannot be removed by conventional methods for quartz purification.
[0055] Despite the fact that the density of the RE particles is much higher than that of the quartz particles, the small size of the contaminants, RE particles, surprisingly makes it possible to separate them from the quartz powder particles by a process step of elutriation.
[0056] The elutriation process for refining quartz powder is described in more detail below.
[0057] Firstly, it is advantageous that the RE fines to be removed from the quartz flour are exposed from the quartz flour, and secondly, it is advantageous to ensure that the RE fines do not remain attached to the much larger quartz crystal particles during the elutriation process. This first aspect is preferably achieved by a suitable pre-treatment of the quartz flour before elutriation, and the second aspect is preferably achieved by a suitable rising speed of the liquid elutriation phase. Adhesion of the RE fines to the quartz particles (agglomeration), e.g. due to differences in surface charge, may be overcome by continuous or intermittent ultrasonic agitation, by selection of pH, or by other means.
[0058] One suitable pretreatment of the quartz powder may be, for example, an acid leaching and washing step of the quartz powder in a preferred fluidized bed reactor, which is then operated in a specific elutriation mode. Alternatively, these steps may be carried out overall at low fluid flow rates, adjusted to allow elutriation at each stage throughout the process.
[0059] Operating the fluidized bed in elutriation mode means that acid (used for the leaching process) or water (used for the washing process) is brought into the fluidized bed at an upward flow rate selected to ensure that the majority of the quartz particles remain in the lower region of the vessel, while the RE fines are carried upwards and removed from the fluidized bed system over a weir at the top of the vessel. As mentioned above, this separation can be facilitated by using a cone-shaped fluidized bed vessel.
[0060] Alternatively or additionally, the acid leaching step may precede the high temperature chlorination step, since the high temperature treatment in chlorination may liberate some of the RE fines that would otherwise remain attached to the quartz particles, although it may be advantageous to carry out the leaching, washing and elutriation after the chlorination step.
[0061] The chlorination step is a common process step in the purification procedure of quartz flour and is referred to the known state of the art.
[0062] The high density of RE fines (e.g., monazite has a specific gravity of 4.6 to 5.7 and xenotime has a specific gravity of 4.4 to 5.1) compared to the specific gravity of quartz crystals (quartz grains have a specific gravity of 2.65) may make elutriation an impractical means of raising the RE fines. However, it has been found possible to operate a fluidized bed reactor under conditions in which the quartz grains sink and the RE fines float. This occurs because the sizes of the respective particles are significantly different. The particle size of the quartz powder of interest is typically in the range of 75 μm to 250 μm, whereas the RE fines that we are trying to eliminate are typically less than 10 μm, often less than 5 μm, and the majority (by number) less than 1 μm in size.
[0063] The smaller or lighter particles will rise to the top (overflow) because their terminal settling velocity is less than the velocity of the ascending fluid. The terminal velocity, or settling velocity, of spherical particles in any fluid medium can be estimated using Stokes' equation if the flow is laminar and the particles are in dilute suspension. From this calculation, the velocity of the ascending fluid can be specified according to the specific conditions in the fluidized bed reactor. Due to the non-spherical shape of the particles and the high particle concentration at least in the lower region of the vessel, this calculation provides a useful guide to the preferred velocity range required to suspend the RE fine particles relative to the quartz particles.
[0064] It is assumed that many, perhaps all, of the smallest RE particles are attached to the quartz grains by chemical or physical bonds or may even be contained inside some of the particles. Thus, a means must be found that allows such RE particles to be liberated into the liquid medium. Such means may include, as already mentioned above, leaching or etching of the quartz powder with acid, optionally under the influence of ultrasonic agitation, and high-temperature calcination or heat treatment, optionally in a chlorine-containing environment, prior to the elutriation process, which may also be facilitated by ultrasonic agitation.
[0065] Agitation of the fluidized bed may alternatively be achieved without liquid recirculation by introducing a gas, e.g. nitrogen, into the lower part of the fluidized bed, in which case the vessel is provided with an outlet for the gas leading to a scrubber. Thus, a vessel of conical construction, fed with gas or circulated acid or water, allows gentle agitation of the quartz particles and homogenization in terms of particle size, but in a slow controlled elutriation mode, where the upward flow of the liquid exceeds the settling velocity of the RE fines, these RE fines may rise against the quartz particles in the bath and exit the vessel via an overflow, at which time filtration of the liquid may take place.
[0066] The overflow used to remove the liquid elutriation medium together with the RE fines is preferably equipped with a filter to remove the RE fines from the liquid elutriation medium before it is recycled to the lower part of the fluidized bed reactor. The filter used preferably has a pore size equal to or less than 0.7 μm and removes impurity minerals before returning to the lower part of the fluidized bed. [Brief description of the drawings]
[0067] [Figure 1] FIG. 1 shows a schematic diagram of one process pathway according to the present invention. [Diagram 2] FIG. 2 shows a variation of the process described in FIG. [Diagram 3] FIG. 3 shows a variation of the process described in FIG. [Figure 4] FIG. 4 shows a further route of the process according to the invention. [Diagram 5] FIG. 5 shows a schematic of a fluidized bed reactor. [Figure 6] FIG. 6 shows an SEM image of the microparticles, most of which are less than 5 μm in size, but also contain larger particles such as 10 μm or 20 μm. [Figure 7A]FIG. 7A is a graph showing plots of particle settling velocity in water at 20° C. for quartz and rare earth phosphates. [Figure 7B] FIG. 7B is a graph showing plots of particle settling velocity in water at 60° C. for quartz and rare earth phosphates. [Figure 7C] FIG. 7C is a graph showing plots of particle settling velocity in hydrofluoric acid at 25° C. for quartz and rare earth phosphates. [Figure 8] FIG. 8 is a diagram of an experimental elutriation column incorporating ultrasonic agitation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0068] In the following, several preferred embodiments for carrying out the elutriation step into a general purification process of quartz powder are described with reference to Figures 1 to 4. In all of these embodiments, the quartz powder used as starting material is subjected to a standard preliminary treatment 1 (S1), such as crushing, grinding, sieving, magnetic and / or gravity separation, and flotation, which typically results in quartz particles with the desired particle size distribution and substantially free of extraneous minerals, but still contaminated with RE fines.
[0069] Figure 1 shows a schematic diagram of one process route according to the invention. The quartz flour used as starting material is preferably pre-treated in step 1 (S1) by one or more of the following steps: crushing, grinding, sieving, magnetic and gravitational separation, and flotation. In a second process step S2, the pre-treated starting material is subjected to acid leaching, for example with hydrofluoric acid, which can be used in combination with a mineral acid such as hydrochloric acid or nitric acid. In a third step S3, the leached quartz flour is washed and elutriated according to the invention. Elutriation achieves the intended removal of RE fines from the quartz flour, and the quartz fraction is finally subjected to a drying step S4 and, optionally, a packaging step S5.
[0070] Figure 2 shows a variation of the process described in Figure 1, in which the leached and dried powder may subsequently be treated by a high temperature chlorination step S6 after the elutriation step S3 and drying step S4 and before the packaging step S5. This additional high temperature chlorination step S6 provides further purification, i.e. removal of traces of alkali metals, particularly sodium and potassium, and removal of certain transition metals, such as iron.
[0071] Figure 3 shows a variation of the process described in Figure 1, where the quartz powder may additionally be treated by high temperature chlorination S6 before the elutriation step S3. This allows for the removal of certain impurities such as volatile chlorides, but it is believed that the high temperature chlorination process may also cause some decrepitation of the quartz particles, allowing for the exposure and possibly liberation of some of the bound rare earth fines. This may be followed by the leaching, washing and elutriation steps proposed here to provide improved removal of the RE fines.
[0072] Figure 4 shows a further route of the process according to the invention. After preliminary treatment steps S1, such as crushing, grinding, sieving, magnetic and gravity separation, and flotation, the quartz flour is leached S2.1 with an acid, such as a mixture of hydrofluoric and hydrochloric acids, and a first washing and elutriation step S3.1 is carried out to remove a first portion of the RE fines of interest. After a drying step S4, a high-temperature chlorination S6 is carried out, and a second acid leaching step S2.2 with the same or a similar acid is carried out before the second washing and elutriation step S3.2, resulting in further removal of the RE fines. This second removal of the RE fines by elutriation is particularly advantageous, since the high-temperature chlorination step S6 carried out after the first elutriation step S3.1 may result in further release of the RE fines. Finally, the usual process steps of drying S4 and packaging S5 are carried out. This embodiment of Figure 4 achieves the purest quartz flour.
[0073] As noted above, it may be advantageous to operate all or most of the acid leaching and washing steps with controlled fluid flow to allow progressive elutriation of the RE particulates during each stage of the process.
[0074] The leaching step carried out in the process according to the invention described in the above embodiments uses an acid, typically hydrofluoric acid, optionally with an additional mineral acid, such as hydrochloric acid or nitric acid. The acid may be heated by reaction with the quartz powder or by an external heating means. Leaching with hydrofluoric acid may be followed by a rinse with dilute hydrochloric acid, followed by a water wash.
[0075] The process according to the invention usually ends with washing the quartz powder to remove the acid and discharging the quartz particles from the vessel. Since the quartz is classified by particle size during the elutriation process, it has been found to be advantageous to agitate the fluidized bed well prior to discharging to allow thorough mixing of the quartz particles. This may be done by providing a strong flow of fluid to the top of the bath, or alternatively by introducing a gas, e.g. nitrogen, at the bottom of the fluidized bed to agitate it. It is then possible to provide a uniform quartz powder with a uniform particle size distribution when the slurry of quartz particles is discharged, as is generally required. This powder can then be dried, packaged, stored, transported, or used immediately by conventional means.
[0076] It is possible for the acid leaching step, and even the water washing step, to be carried out in separate vessels, however it is also possible to use a single vessel for all these operations, and a suitable vessel is a fluidized bed reactor as shown diagrammatically in Figure 5.
[0077] The vessel 10 and associated piping are made from a suitable acid resistant material, such as polypropylene, PTFE, or an alternative polymer, or from a metal or other material coated with a polymer. The lower region of the vessel 10 is preferably tapered or conical in shape to ensure that the velocity of the rising liquid is gradually reduced and to aid in the separation of fine particles during the elutriation stage of the process. At the bottom of the vessel is a membrane of a suitable porous material that will retain the quartz particles but allow the passage of liquid, as well as the fluidizing gas. A suitable material for this membrane is typically porous PTFE, although alternative materials are available.
[0078] The quartz powder to be treated may be introduced into the vessel through the inlet 11. The acid (or later water) may be introduced at the bottom of the vessel and flows upwards to form a fluidized bed. Since fluidization by liquid recirculation leads to the possibility of overflow of the quartz powder, if fluidization without elutriation is required, it is preferable to achieve agitation and mixing of the fluidized bed by introducing a fluidizing gas (e.g. nitrogen) at the inlet 14 once the vessel 10 is filled with liquid. Under these circumstances, the gas may be exhausted through the outlet vent 23 and directed to a suitable scrubber to remove any splashes or acid vapors. Alternatively, in a mode where gradual separation of particles occurs, it is possible to operate with a lower acid throughput, and the smallest particles may be carried to the top of the vessel and appear in the overflowing liquid.
[0079] Following acid leaching of the suspended quartz particles and optional rinsing with dilute hydrochloric acid, where the fluidized bed can be well agitated, the suspended powder is washed with high purity water, also optionally with gas agitation of the fluidized bed, which is then operated at elutriation, i.e. reduced liquid flow chosen to allow the RE fines to float but the (larger) quartz particles to settle. By slowly recirculating the water, the powder in the fluidized bed is allowed to separate by particle size. As a result of the tapered shape of the vessel, the upward velocity of the fluid decreases with increasing height. Thus, the larger quartz particles with faster settling velocity accumulate towards the lower part (bottom) of the vessel, while the smaller quartz particles accumulate higher at the top of the vessel. The RE fines with slower settling velocity float upwards and become accumulated in the upper region of the vessel 12 as the vessel fills with liquid, then overflowing through the peripheral weir 19. They are then collected in a fine filter 20 having a pore size equal to or smaller than 0.7 μm, while the elutriate liquid may be recirculated.
[0080] In FIG. 5 the following reference numbers are used: 10 Fluidized Bed Leaching and Washing Vessel 11. Inlet for refined quartz powder 12 Fluidized bed in elutriation mode 13. Refined quartz powder outlet 14 Optional fluidizing gas inlet 15 Liquid Circulation Pump 16 Leaching acid inlet 17 Washing water inlet 18 Liquid outlet 19 Perimeter Weir 20 Fine filters for refractory powders 21 Particles in surface liquids 22 Particulate outlet 23 Aeration gas vent 24 Ultrasound Probe During the acid treatment and subsequent elutriation, it may also be desirable to provide suitable heating to the vessel, to the recirculated liquid, or to both. Deagglomeration of fine particles from larger quartz particles may be promoted by pH control, by the addition of deflocculating agents, chelating agents, etc., and may be facilitated by ultrasonic agitation or other means. Heating of the liquid phase may be useful in increasing the effectiveness of some of these processes.
[0081] Although a single vessel of suitable design is sufficient to ensure a high level of removal of RE particles, which in the present situation constitute a contaminant, it is also possible to use a second or further vessel connected in series. Thus, the overflow from the first vessel may be directed directly to the inlet of a second, larger, vessel of increasing diameter. In this way, a more precise separation of the RE particles can be achieved if necessary.
[0082] Following displacement of the fines, and prior to discharging the slurry of quartz particles from the bed, it is preferred to efficiently agitate the slurry, for example by passing a gas (e.g., nitrogen) upwardly through the bed, or alternatively by introducing a high flow rate of water, to mix the layers of separated quartz. Once adequately homogenized, the slurry can be discharged via outlet 13 into a suitable container for filtering and subsequent drying by conventional means.
[0083] The invention also relates to the use of an elutriation process for refining quartz flour by removing rare earth minerals, which is characterized in particular by the above-mentioned features of the claimed process.
[0084] Finally, the present invention relates to a purified quartz powder obtained according to the above-mentioned purification process. Such a purified quartz powder is novel in view of the quartz powders known in the prior art. The above-mentioned process according to the present invention provides the ability to separate RE fine particles from larger particles of quartz from a mixture of quartz grains doped with such fine particles. The purified quartz powder according to the present invention therefore contains a reduced level of RE fine particles compared to the quartz powder obtained by the process according to, for example, US Pat. No. 6,746,655; EP 1,942,078; and CA 1,184,740. The processes described in these prior art documents are inadequate for reducing RE fine particles from quartz, at least in terms of the efficiency provided for the first time by the method according to the present invention. EXAMPLES
[0085] The present invention will now be described in more detail by reference to the following examples, which do not limit the invention as claimed.
[0086] First, an experimental validation of the method was performed by elutriation trials based on a mixture of a typical purified quartz powder and a known loading of RE particles previously extracted from a bulk of such quartz powder. Numerically, the majority of these particles are less than 5 μm in size. However, occasionally larger particles of 10 μm or even 20 μm in size can be seen in the SEM pictures (Figure 6).
[0087] The quartz powder used in these trials was commercially available refined quartz powder, which was further processed by a high-temperature chlorination purification process (typically the purity of the quartz powder is greater than 99.998% SiO2 and the nominal particle size is 85-225 μm), to which pre-obtained and weighed RE fines from such quartz powder were added as seen in Figure 6.
[0088] Example 1 A slurry was prepared containing 20 g of purified quartz powder spiked with 0.0125 g of RE particulates. The slurry, contained in a glass container, was stirred in a commercial ultrasonic cleaning bath for 2 minutes and then added to an elutriation column where the water was slowly flowing at a rate such that all the quartz particles fell while the water overflowed at the top. The overflowing water was filtered through a 0.7 μm pore size glass fiber filter. The filter and residue were then treated with dilute hydrofluoric acid to dissolve the glass fibers, leaving behind a residue of quartz and RE particulates. Following removal of the hydrofluoric acid, the elutriated particulates were processed using a density separation method that is part of the analytical process described in U.S. Patent No. 9,776,194. Using this process, 0.0025 g of RE particulates were recovered, representing a 20% recovery of such particles from the original quartz sample.
[0089] The refined quartz flour used as starting material in this Example 1 did not correspond to the final quartz flour obtained by the process carried out in this example.
[0090] The starting material purified quartz powder is commercially available and has not been further processed to remove RE particulates. The fact that only added RE particulates and not more RE particulates are removed does not mean that the starting material is free of RE particulates, because this example is performed on a small scale, which contains very little RE particulates in the starting material, and also, it may be necessary to use, for example, HF etching, to liberate some of the existing RE particulates from the quartz powder. The difference in weighed particulates will be minimal, but still exists.
[0091] Example 2 The above trial was repeated, i.e. 20 grams of quartz was doped with 0.0085 grams of RE particulate. Following elutriation, 0.0032 g of RE particulate was recovered using the same technique, indicating separation and recovery of 38 wt. % of the RE particulate from the original quartz powder.
[0092] Example 3 The above example was repeated, but the upward flow of water was measured at a rate of 120 mm / min and elutriation was for 90 minutes. 20 grams of quartz doped with 0.0095 grams of RE particulate was treated and 0.0064 grams of RE particulate was recovered, indicating separation and recovery of 67% by weight of the RE particulate from the original quartz powder.
[0093] The viscous drag of water on a spherical particle at 20°C is given by Stokes' law, and the density of quartz in water at 20°C (2.65 g / cm 3 ) and typical rare earth phosphates (4.75 g / cm 3 ), a model of the elutriation process leads to the plot shown in Figure 7A for the particle settling velocities of these two materials. At an upward velocity of about 240 mm / min, quartz particles larger than about 67 μm are allowed to settle, whereas rare earth phosphate particles smaller than about 45 μm appear to rise and can be removed from the bulk of the quartz sand.
[0094] The examples given above provide guidance regarding the operating conditions, and the skilled person can easily find the preferred upward flow rate through simple experimentation. The applied flow rate depends on the nature of the fluid medium, the operating temperature and viscosity, and also on the shape of the vessel. Furthermore, the calculations according to Stokes' equation given above provide sufficient guidance. It is also known that temperature and viscosity can have a large effect. Elutriation can be advantageous (e.g. during acid leaching) when carried out with heated fluid. The effect of both these parameters in water at 60°C can be seen in Figure 7B, from which it may be concluded that at an upward flow rate of 240 mm / min, quartz particles larger than 45 μm may be expected to settle, whereas rare earth phosphate particles smaller than 30 μm may be expected to rise and appear in the overflowing fluid.
[0095] A further option is to operate the leaching process in elutriation mode. Values are available for the density and viscosity of aqueous hydrofluoric acid (30% wt) in the temperature range of 25° C. FIG. 7C shows the predicted settling velocities of quartz and RE fines under these conditions. The plot shows that at an upward velocity of 240 mm / min, quartz particles larger than 70 μm are predicted to fall, whereas RE fines smaller than 45 μm are predicted to rise and be carried out of the vessel in the overflow liquid and removed.
[0096] Based on the above, and because the nominal particle size range of quartz is 85-225 μm (as noted earlier), it was decided to conduct more quantitative experiments in a water column with an upflow velocity of 240 mm / min.
[0097] Example 4 An experimental elutriation column incorporating ultrasonic agitation was constructed from PVC parts as shown in Figure 8. The column (30) itself consisted of a cylindrical tube with an internal diameter of 68 mm and a length of 500 mm, and was equipped with an overflow (32) at its upper end. At the lower end was a water inlet (31) and a porous PTFE plate (33) through which water was fed at a known flow rate. An ultrasonic probe (34, QSonica Q55) allowed ultrasonic agitation with controlled power when required.
[0098] Ultrasonic agitation is not required, but is believed to be useful in aiding the detachment of the RE particulates from the quartz particles. Thus, during operation in elutriation mode, and when elutriation of RE particulates is desired, ultrasonic agitation should be applied at low power, or alternatively intermittently, and for only short periods of time, so as not to induce violent motion in the liquid phase.
[0099] The elutriator was connected to a source of demineralized water with a temperature of approximately 20° C. and the flow rate was adjusted to give an average ascending velocity of 240 mm / min in the column.
[0100] A slurry containing 40.0 grams of quartz particles doped with 0.0112 grams of RE particulate was added to the open top of the elutriation column. Ultrasonic agitation was applied to the slurry for 15 seconds (amplitude on the control box was set at 70). The elutriator was allowed to run for 30 minutes, during which time ultrasonic agitation was applied for 10 seconds every 5 minutes.
[0101] Particles washed from the top of the column were collected on a Whatman® GF / F glass fiber filter disc, which nominally retains 0.7 μm particles.
[0102] The glass filter was subsequently dissolved in hydrofluoric acid leaving a residue of RE particulates and quartz. After removal of the hydrofluoric acid, the RE particulates and remaining quartz particles were separated using the heavy mineral analysis method described in U.S. Patent No. 9,776,194, and 0.0101 g of RE particulates were recovered, representing separation and recovery of 90.2% by weight of the RE particulates from the original quartz powder.
[0103] Operating under these conditions, the elutriation process also removed some of the fine quartz particles from the starting material, i.e. 1.0190 g, or 2.5% by weight of the quartz introduced at the start. The majority of these quartz particles (75%) were below 80 μm in size (the lower limit specified for the quartz powder to be treated).
[0104] Thus, the potential of elutriation to remove a significant portion of the RE fines from the refined quartz powder is evident from these figures.
[0105] Example 5 Analysis of commercially available and literature-described quartz glass powders The average analyses over a period of several years for one grade of powder are given below in Table 2 (ppM), which were obtained by laboratory analysis by the applicant, as well as analyses of fused quartz ingots made from these powders.
[0106] [Table 2]
[0107] It is noted that the zirconium content appears to have increased as a result of melting, but the most likely explanation is that some zirconia dissolved as a result of melting the quartz glass and was made more soluble by the hydrofluoric acid used to prepare the analysis solution. The only rare earth impurity routinely analyzed is yttrium, which is present on average in amounts just above 0.1 ppM; however, this value has varied over time, ranging between 0.05 ppM and 0.32 ppM. The other rare earth elements thorium and uranium are also present in smaller amounts, but may be expected to vary over a similar range, depending on the quality of the ore body from which the quartz is extracted.
[0108] When these powders are fused into glass, the elements listed in the table above may be present in the glass in a soluble form and thus may be relatively uniformly distributed in the solution. Furthermore, they may also be soluble in the acid (usually hydrofluoric acid) used to prepare the solution for analysis, making such analysis relatively easy. However, most rare earth elements are not listed in the table above, i.e. thorium and uranium are present at much lower levels, but may exist as individual particles and may remain undissociated and undissolved in the glass during and after melting. Analyzing these localized impurities is problematic, especially since they may be present at concentrations below 1 ppm. Their concentrations in the glass may vary greatly from sample to sample, and furthermore, they are often in the form of refractory phosphate complexes that are insoluble in the acid used to prepare the solution for analysis. This means that analysts must rely on alternative techniques that can measure low levels of impurities, such as neutron activation analysis of glasses made by melting powders, but even then, moderately sized samples may not contain significant amounts of relevant particulate matter.
[0109] As an example, two ingots of melt-produced fused quartz were prepared using two batches of powder from the same source and subjected to neutron activation analysis with the results shown in Table 3. These results illustrate the range of variation that can occur in the concentrations of these significant impurities.
[0110] [Table 3]
[0111] In a further set of analytical data on powders developed by the applicant over a period of time working with several high purity quartz powders from two different sources, the levels of cerium, yttrium, thorium and uranium were generally found to be within the ranges shown below in Table 4. These powders were fused into glasses in both rod and tube form by melting in a crucible made from a refractory metal and continuously drawing the product through a die set in the bottom of the crucible.
[0112] [Table 4]
[0113] Although these values may seem relatively small, it should be noted that these impurities are not uniformly distributed but exist as numerous particulates, most of which are submicron in size (see Figure 6), each of which can cause fiber breakage or yield loss when the glass is used in certain semiconductor applications.
[0114] Particulate contamination has been detected in fused quartz produced by various techniques, e.g., flame melting, electrical melting, in molten glass drawn from an electrically heated refractory metal crucible, and in glass formed by plasma jet melting of quartz crystal powder (e.g., U.S. Pat. No. 6,269,663) and deposited on the outer surface of an optical fiber preform to form a cladding layer composed of fused natural quartz powder.
[0115] In these commercially available refined quartz flours, such refractory particulates are generally all less than 25 μm in size, typically less than 5 μm, and in fact the majority are much smaller, typically less than 1 μm. Because of their extreme inertness and very high melting points, it has proven difficult to eliminate them from the quartz flour.
[0116] As previously mentioned, fiber breakage studies have shown that particles smaller than 0.5 μm in size can cause optical fiber breakage when present in the cladding glass. As a result, for many years the majority of the fiber optic industry has sought synthetic fused silica that can be guaranteed to be free of such particles.
[0117] High quality fused quartz parts are also used in the manufacture of semiconductor wafers, and here too, in certain applications, these refractory particles may be a possible cause of yield loss. Fused quartz parts are used to support wafers during etching of the surface of the wafer in a plasma etching process involving fluorine-containing gases, during which some etching of the quartz parts may occur. This would be acceptable since the product of such etching is gaseous, i.e., silicon tetrafluoride, SiF4. However, if refractory particulates are exposed to this process, dust may be produced that may contaminate the wafer and lead to unacceptable yield loss. It should also be noted that some of these refractory mineral particles contain thorium and uranium, and the presence of such radioactive species is particularly undesirable in semiconductor manufacturing processes.
[0118] Thus, it is clear that for both fiber optic and semiconductor applications, fused silica may be acceptable if such particulates are eliminated, or at least substantially reduced, during the quartz refining process, otherwise critical applications will require the use of synthetic fused silica, which is free of such refractory inclusions.
Claims
1. 1. A process for the purification of quartz flour, comprising a step of separating fine particles of refractory minerals from quartz flour by an elutriation step, the fine particles of refractory minerals comprising rare earth metal-containing minerals and / or thorium and / or uranium, and characterized in that the elutriation step is carried out in a fluidized bed reactor, in which a controlled upward flow of a liquid elutriate phase is provided, whereby the fine particles of refractory minerals are carried upward in the fluidized bed reactor, while the quartz flour remains in a lower region of the fluidized bed reactor.
2. 2. The process of claim 1, wherein the fine particles of refractory mineral carried upward in the fluidized bed are either discharged externally from the fluidized bed reactor or separated from the liquid elutriate phase.
3. 3. The process of claim 2, characterized in that the liquid elutriate phase is recycled in the elutriation step and the fine particles of refractory minerals contained therein are separated from the elutriate phase by filtration.
4. 4. The process of claim 3, characterized in that the fine particles of the refractory mineral are separated from the elutriate phase by filtration using a filter having a pore size of 0.7 μm or less.
5. 5. The process of claim 4, wherein the filter is an acid-resistant filter.
6. 6. The process of claim 1, wherein the separation of the fine particles of refractory mineral from the quartz flour is facilitated by ultrasonic agitation before or during elutriation.
7. 7. The process of any one of claims 1 to 6, characterized in that the elutriation step is carried out before or after the calcination step and / or the high-temperature chlorination step.
8. 8. The process of claim 1, wherein the particle size distribution of the purified quartz powder is homogenized before removal from the fluidized bed reactor.
9. 9. The process according to claim 8, characterized in that the homogenization of the refined quartz powder is carried out by stirring, in particular by a liquid or gas flow or by ultrasound.
10. 10. The process of claim 1, wherein the quartz flour to be refined has a size of between 75 μm and 1000 μm, whereas the rare earth minerals have a particle size of less than 50 μm.
11. 11. The process of any one of claims 1 to 10, characterized in that the liquid elutriate phase is a leaching acid, in particular an aqueous acid solution comprising one or more of hydrofluoric acid, hydrochloric acid, nitric acid, and sulfuric acid.
12. 1. A process for the purification of quartz flour, comprising a step of separating fine particles of refractory minerals from quartz flour by an elutriation process, characterized in that the quartz flour to be purified has a size of between 75 μm and 1000 μm, whereas the fine particles of refractory minerals have a particle size of less than 50 μm.
13. Use of an elutriation process for refining quartz flour by removing rare earth minerals, characterized by the features of any one of claims 1 to 12.
Citation Information
Patent Citations
Kojundosuishofun no seizohoho
JP1976028596A
Artificial net inside system device
JP1980040545A
Purification of quartz sand
JP1987187138A