Low Melting Point Copolyamide Powder

A copolyamide-based powder with a low melting point and high intrinsic viscosity forms coatings at low temperatures, addressing the issue of heat-sensitive surfaces and achieving coatings with enhanced mechanical properties and thickness.

JP7584407B2Active Publication Date: 2024-11-15ARKEMA FRANCE SA
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021522413
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-10-24
Filing Date
2019-10-23
Publication Date
2024-11-15
Estimated Expiration
2039-10-23

AI Technical Summary

Technical Problem

Existing coating technologies for metal surfaces, particularly those that are heat-sensitive, require high temperatures that can damage the surface, and do not produce coatings with good mechanical properties.

Method used

A copolyamide-based powder with a melting point of 160°C or lower and an intrinsic viscosity of 160°C or higher is used, optionally combined with a second polymer, to form coatings at relatively low temperatures, achieving good mechanical properties and increased thickness.

Benefits of technology

The solution allows for coating heat-sensitive surfaces at temperatures below 230°C, resulting in coatings with improved mechanical properties and thickness, suitable for applications where high temperatures are not feasible.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584407000001
    Figure 0007584407000001
  • Figure 0007584407000002
    Figure 0007584407000002
  • Figure 0007584407000003
    Figure 0007584407000003
Patent Text Reader

Abstract

The present invention is 0.8 (g / 100g) -1 The present invention relates to a copolyamide-based powder for forming a coating on a surface, the powder having an intrinsic viscosity of 0.8 (g / 100g) or more, wherein the copolyamide has a melting point of 160°C or less. -1 The present invention also relates to the use of such powders for coating surfaces and to a method of coating surfaces using such powders.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to low melting point copolyamide-based powders and the use of these powders for coating surfaces. [Background technology]

[0002] Coating metal surfaces is extremely prevalent in industry, with a wide variety of applications in motor vehicle and fluid transfer areas, as well as in the electrical and electronics industries, among others.

[0003] Polyamides are commonly used for coating metal or other surfaces.

[0004] For example, EP 0 866 736 describes a method for coating aluminum or iron substrates using powders formed from polyamides containing branched amines.

[0005] US 2002 / 0031614 describes a method for coating with a hot-melt adhesive based on thermoplastic or crosslinkable copolyamides.

[0006] FR 2304998 relates to powder plastic coatings obtained by reacting epoxy compounds with copolyamides.

[0007] The articles "A new UV-curable powder coating based on a α,ω-unsaturated copolyamide 6 / 11 / 12" by N'Negue Mintsa et al. (European Polymer Journal, 2009, vol. 45, pages 2043-2052) and "Production of a polyamide-based "UV powder" coating" by N'Negue Mintsa (INSA de Rouen, 2008) describe a coating powder comprising copolyamide 6 / 11 / 12 and a photoinitiator.

[0008] US 4 172 161 describes the coating of glass bottles with a powdered copolyamide containing at least 30% by weight of lauryllactam.

[0009] Polyamides may also be used in mastics.

[0010] US 2015 / 0024130 and US 2013 / 0177704 describe powdered mastics comprising copolyamide resins for encapsulating electronic devices.

[0011] In coating applications, the surface to be coated may be heat sensitive. For example, the surface may be made of a heat sensitive metal such as a zinc-aluminum alloy or may undergo a heat sensitive chemical process. The heat sensitivity of these surfaces precludes the use of high coating application temperatures that may damage the surface to be coated. [Prior art documents] [Patent documents]

[0012] [Patent Document 1] EP 0 866 736 [Patent Document 2] US 2002 / 0031614 [Patent Document 3] FR 2304998 [Patent Document 4] US 4 172 161 [Patent Document 5] US 2015 / 0024130 [Patent Document 6] US 2013 / 0177704 [Non-patent literature]

[0013] [Non-Patent Document 1] “A new UV-curable powder coating based on a α,ω-unsaturated copolyamide 6 / 11 / 12” by N’Negue Mintsa et al. (European Polymer Journal, 2009, vol. 45, pages 2043-2052) [Non-Patent Document 2] “Production of a polyamide-based “UV powder” coating” by N’Negue Mintsa (INSA de Rouen, 2008) Summary of the Invention [Problem to be solved by the invention]

[0014] There is therefore a real need to provide polyamide coating powders, in particular for coating metal surfaces, which allow application at relatively low temperatures, e.g. below 230° C., and at the same time are able to form coatings having good mechanical properties. [Means for solving the problem]

[0015] First, the present invention is 0.8 (g / 100 g) -1 and a copolyamide-based powder for forming a coating on a surface, the copolyamide having an intrinsic viscosity of 160° C. or less, wherein the copolyamide has a melting point of 160° C. or less.

[0016] According to an embodiment, the copolyamide is selected from the group consisting of copolyamide 6 / 11, copolyamide 6 / 12, copolyamide 6.6 / 11, copolyamide 6.6 / 12, copolyamide 6.10 / 11, copolyamide 6 / 12 / 11, copolyamide Pip.12 / 12 (Pip stands for piperazine), copolyamide 6 / 6.6 / 12, copolyamide 6 / Pip.12 / 12 or combinations thereof.

[0017] According to an embodiment, the copolyamide is present in an amount equal to or greater than 80% by weight, preferably equal to or greater than 90% by weight, more preferably equal to or greater than 95% by weight, relative to the total weight of the powder.

[0018] According to an embodiment, the powder also comprises a second polymer having a melting point lower than the melting point of the copolyamide.

[0019] According to an embodiment, the second polymer is a second copolyamide and / or an epoxy resin.

[0020] According to an embodiment, the second polymer has a melting point of 130° C. or less.

[0021] According to an embodiment, the second polymer is present in an amount of less than or equal to 10% by weight, preferably less than or equal to 5% by weight, relative to the total weight of the powder.

[0022] According to an embodiment, the powder also comprises one or more additives selected from the group consisting of pigments or dyes, anti-crater or spreading agents, reducing agents, antioxidants, reinforcing fillers, UV stabilizers, flow agents, and corrosion inhibitors.

[0023] According to an embodiment, the mass of the additive is 0-30%, preferably 0-10%, more preferably 0-5% relative to the total mass of the powder.

[0024] According to an embodiment, the copolyamide has a melting point below 150°C, preferably below 145°C.

[0025] According to an embodiment, the powder has a (g / 100g) -1 The intrinsic viscosity is preferably 0.9 or more, more preferably 1 or more.

[0026] According to an embodiment, the powder comprises copolyamide-based particles having a volume median diameter Dv50 between 10 and 400 μm, preferably between 50 and 200 μm.

[0027] The invention also relates to a film which may be obtained by melting the powder described above.

[0028] The present invention relates to the use of the above powder for coating a surface, the coating having a viscosity of 0.8 (g / 100 g) or less. -1 The present invention also relates to the use of a composition having an intrinsic viscosity of 100 or more.

[0029] According to an embodiment, the surface is an optionally treated metal surface.

[0030] According to an embodiment, the coating is a film having a thickness of 100 to 550 μm, preferably 200 to 500 μm.

[0031] The present invention also relates to a method for coating a surface, preferably a metal surface, comprising the following steps: - placing said powder in contact with a surface; - The process of melting the powder.

[0032] According to an embodiment, the step of placing the powder in contact with the surface comprises the steps of: - heating the surface at a temperature above the melting point of the copolyamide, preferably at least 30°C above the melting point of the copolyamide; - Submerging the surface in a fluidized bed containing the powder.

[0033] According to an embodiment, the step of placing the surface in contact with the powder comprises the steps of: - electrically charging the powder; - spraying an electrically charged powder onto a surface; - heating the surface coated with the powder to a temperature above the melting point of the copolyamide, preferably at least 30°C above the melting point of the copolyamide.

[0034] According to an embodiment, the step of placing the surface in contact with the powder comprises the steps of: - heating the surface to a temperature above the melting point of the copolyamide, preferably to a temperature at least 30°C above the melting point of the copolyamide; - The process of spraying a powder onto a surface.

[0035] The invention also relates to an article comprising a surface covered with a coating which may be obtained by melting said powder. Effect of the Invention

[0036] The present invention makes it possible to satisfy the above-mentioned needs, and more particularly to provide a polyamide powder which allows both application at relatively low temperatures (hence suitable for coating heat-sensitive surfaces such as heat-sensitive metal surfaces) and the production of coatings with increased thickness and good mechanical properties.

[0037] This is 0.8(g / 100g) -1 This is achieved by using a powder based on a low melting point (i.e. below 160° C.) copolyamide having an intrinsic viscosity of at least 1000 nm. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0038] The invention will now be described in more detail in the following specification, in a non-limiting manner.

[0039] Unless otherwise indicated, all amount percentages are by weight.

[0040] In the present invention, the term "copolyamide-based" should be understood to mean "based on one or more copolyamides", which is also the case for all other components (e.g. the term "epoxy resin" should be understood to mean "one or more epoxy resins").

[0041] powder According to a first aspect, the present invention provides a 0.8 (g / 100g) -1 The present invention relates to a copolyamide-based powder having an intrinsic viscosity of at least 100° C., in which the copolyamide has a melting point of at most 160° C. This powder is intended to form a coating on a surface.

[0042] The melting point may be measured by standard ISO 11357-3 Plastics - Differential Scanning Calorimetry (DSC) Part 3.

[0043] Intrinsic viscosity is measured using an Ubbelohde tube. Measurements are performed on 75 mg samples at 20°C in m-cresol at a concentration of 0.5% (m / m). Intrinsic viscosity is (g / 100g) -1 It is expressed in units of and is calculated according to the following formula: Intrinsic viscosity=ln(t s / t0)×1 / C (C=m / p×100) Here, t s is the flow time of the solution, t0 is the flow time of the solvent, m is the mass of the sample whose viscosity is to be determined and p is the mass of the solvent. This measurement corresponds to standard ISO 307, apart from the fact that the measurement temperature is 20°C instead of 25°C.

[0044] The term "copolyamide" means the product of the polymerization of at least two different monomers: - monomers of the amino acid or aminocarboxylic acid type, preferably α,ω-aminocarboxylic acids; - lactam-type monomers, optionally substituted, containing from 3 to 18 carbon atoms in the main ring; - "diamine diacid" monomers derived from the reaction of an aliphatic diamine containing from 2 to 36 carbon atoms, preferably from 4 to 18 carbon atoms, with a carboxylic diacid containing from 4 to 36 carbon atoms, preferably from 4 to 18 carbon atoms; and - their mixtures (in the case of a mixture of amino acid type monomers and lactam type monomers, the monomers containing different carbon numbers);

[0045] In the copolyamides of this specification, the term "monomer" is to be understood as meaning "repeating unit". In fact, it is special when the repeating unit of a polyamide (PA) consists of a combination of a diacid and a diamine. It is considered that the combination of a diamine and a diacid corresponds to a monomer, i.e. a diamine, diacid pair (in equimolar amounts). This is explained by the fact that individually, the diacid or the diamine are the only structural units and are not sufficient to be polymerized by themselves.

[0046] Amino-type monomers: Examples of α,ω-amino acids include those containing from 4 to 18 carbon atoms, such as aminocaproic acid, 7-aminoheptanoic acid, 11-aminoundecanoic acid, N-heptyl-11-aminoundecanoic acid, and 12-aminododecanoic acid.

[0047] Lactam monomers: Examples of lactams include those containing from 3 to 18 carbon atoms in the main ring, which may be substituted, such as β,β-dimethylpropiolactam, α,α-dimethylpropiolactam, amylolactam, caprolactam, also known as lactam 6, capryllactam, also known as lactam 8, oenantholactam, and lauryllactam, also known as lactam 12.

[0048] Monomers of the "diamine diacid" type: Examples of dicarboxylic acids include acids containing 4 to 36 carbon atoms, such as the sodium or lithium salts of adipic acid, sebacic acid, azelaic acid, suberic acid, isophthalic acid, succinic acid, 1,4-cyclohexyldicarboxylic acid, terephthalic acid, sulfoisophthalic acid, dimerized fatty acids (these dimerized fatty acids have a dimer content of at least 98% and are preferably hydrogenated), and dodecanedioic acid HOOC-(CH2). 10 -COOH and tetradecanedioic acid.

[0049] The term "fatty acid dimer" or "dimerized fatty acid" more specifically refers to the product of the dimerization reaction of fatty acids (usually containing 18 carbon atoms, often a mixture of oleic and / or linoleic acids), preferably a mixture containing 0-15% C18 monoacids, 60%-99% C36 diacids, and 0.2%-35% triacids or C54 or higher polyacids.

[0050] Examples of diamines include those with 2 to 36 carbon atoms, preferably 4 to 18 carbon Aliphatic diamines containing 1,2-diamino-1,2,3-trimethyl-1,6-diaminohexane, 1,5-diaminohexane, 2,2,4-trimethyl-1,6-diaminohexane, diamine polyols, isophorone diamine (IPD), methyl pentamethylene diamine (MPMD), bis(aminocyclohexyl)methane (BACM), bis(3-methyl-4-aminocyclohexyl)methane (BMACM), meta-xylene diamine and bis-p-aminocyclohexylmethane.

[0051] Examples of diamine diacids include more specifically diamine diacids derived from the condensation of 1,6-hexamethylenediamine with a diacid containing from 6 to 36 carbon atoms and diamine diacids derived from the condensation of 1,10-decamethylenediamine with a diacid containing from 6 to 36 carbon atoms.

[0052] As examples of monomers of the "diamine diacid" type, mention may be made in particular of the monomers: 6.6, 6.10, 6.11, 6.12, 6.14, 6.18:. Mention may be made of monomers derived from the condensation of decane diamine with C6 to C36 diacids, in particular of the monomers: 10.10, 10.12, 10.14, 10.18:. In the numerical notation XY, as is conventional, X represents the number of carbon atoms from the diamine residue and Y represents the number of carbon atoms from the diacid residue.

[0053] The copolyamide preferably comprises at least one of the following monomers: 4.6, 4.T, 5.6, 5.9, 5.10, 5.12, 5.13, 5.14, 5.16, 5.18, 5.36, 6, 6.6, 6.9, 6.10, 6.12, 6.13, 6.14, 6.16, 6.18, 6.36, 6.T, 9, 10.6, 10.9, 10.10, 10.12, 10.13, 10.14, 10.16, 10.18, 10.36, 10.T, 11, 12, 12.6, 12.9, 12.10, 12.12, 12.13, 12.14, 12.16, 12.18, 12.36, 12.T and mixtures thereof.

[0054] Examples of copolyamides produced from the various types of monomers mentioned above include those derived from the condensation products of at least two α,ω-aminocarboxylic acids, or two lactams, or one lactam and one α,ω-aminocarboxylic acid. Also included are those derived from the condensation products of at least one α,ω-aminocarboxylic acid (or lactam), at least one diamine and at least one dicarboxylic acid. Also included are those derived from the condensation products of an aliphatic diamine with an aliphatic dicarboxylic acid, and at least one other monomer selected from aliphatic diamines other than the aforementioned and aliphatic diacids other than the aforementioned.

[0055] In a particularly advantageous manner, the copolyamide according to the invention is copolyamide 6 / 11, copolyamide 6 / 12, copolyamide 6.6 / 11, copolyamide 6.6 / 12, copolyamide 6.10 / 11, copolyamide 6 / 12 / 11, copolyamide Pip.12 / 12, copolyamide 6 / 6.6 / 12, copolyamide 6 / Pip.12 / 12 or combinations thereof.

[0056] In the numerical designation X, X represents the number of carbon atoms from an amino acid or lactam residue. The numerical designation X / Y, polyamide (PA) Z.Z' / Y etc. relates to copolyamides where X, Y, Z.Z' etc. represent homopolyamide units as defined above.

[0057] The term "copolyamide-based" means that the powder comprises at least 50% by weight of copolyamide. However, in embodiments, the powder comprises copolyamide in an amount of 55% by weight or more, or 60% by weight or more, or 65% by weight or more, or 70% by weight or more, or 75% by weight or more, or 80% by weight or more, or 85% by weight or more, or 90% by weight or more, or 95% by weight or more, or 98% by weight or more, or 99% by weight or more, or 99.5% by weight or more.

[0058] The copolyamide according to the invention has a melting point of 160° C. or less. Preferably, the copolyamide has a melting point of 150° C. or less, more preferably 145° C. or less. The copolyamide may also have a melting point of 155° C. or less, or 140° C. or less, or 135° C. or less, or 130° C. or less, or 125° C. or less.

[0059] The powder according to the invention has an intrinsic viscosity of 0.8 or more. Advantageously, it has an intrinsic viscosity of 0.9 or more, more preferably 1 or more. In certain embodiments, the powder has an intrinsic viscosity of 0.85 or more, or 0.95 or more, or 1.05 or more, or 1.1 or more, or 1.15 or more, or 1.2 or more, or 1.25 or more, or 1.3 or more. In the above, the intrinsic viscosity is expressed in g / 100 g. -1 It is expressed in units of.

[0060] Preferably, the volume median diameter Dv50 of the powdered copolyamide-based particles is 10-400 μm, more preferably 50-200 μm. The Dv50 of the powdered copolyamide-based particles of the present invention may be 10-50 μm, or 50-100 μm, or 100-150 μm, or 150-200 μm, 200-250 μm, 250-300 μm, 300-350 μm, or 350-400 μm.

[0061] Dv50 corresponds to the particle size of the 50th percentile (by volume) of the cumulative particle size distribution. It may be determined by laser particle size analysis.

[0062] The powder may also contain, apart from the copolymer having a melting point below 160° C., a second polymer having a melting point below that of the copolyamide.

[0063] The presence of the second polymer may allow better heat conduction of the powder during the application of the coating and improve the melting of the powder particles. In particular, the particles of the second polymer may dissolve before the particles of the copolyamide during the coating process. The second molten polymer will then allow the coagulation of the particles of the copolyamide and improve their melting. This may make it possible to obtain a coating of increased thickness when compared to the coating obtained with a powder that does not contain the second polymer. In addition, especially in the case of metal surfaces, the presence of the second polymer may make it possible to improve the adhesion of the coating to the surface and may help to produce a coating with a flawless appearance.

[0064] The second polymer may be a second copolyamide, such as the copolyamides mentioned above, in particular the second copolyamide may be copolyamide 6 / 6.6 / 11 / 12, copolyamide 6 / 11, copolyamide 6 / 12, copolyamide 6.6 / 11, copolyamide 6.6 / 12, copolyamide 6.10 / 11, copolyamide 6 / 12 / 11, copolyamide Pip.12 / 12, copolyamide 6 / 6.6 / 12, copolyamide 6 / Pip.12 / 12 or combinations thereof.

[0065] The second polymer may also be an epoxy resin. An example of an epoxy resin that may be used in the present invention is a sulfonamide resin. Epoxy resins that may be used in the present invention include bisphenol A diglycidyl ether, bisphenol F diglycidyl ester, novolac resin glycidyl ether, novolac cresol epoxy resin, novolac phenolic epoxy resin, novolac alkylphenolic epoxy resin, epoxy acrylic resin, hydrogenated bisphenol A diglycidyl ether, hydrogenated bisphenol AD ​​diglycidyl ether, diglycidyl ether of polyols such as propylene glycol or pentaerythritol, epoxy resins obtained by reacting aliphatic or aromatic carboxylic acids with epichlorohydrin, epoxy resins obtained by reacting aliphatic or aromatic amines with epichlorohydrin, heterocyclic epoxy resins, epoxy resins containing spiro nuclei, and modified resins containing epoxy groups. The above epoxy resins may be used alone or in combination.

[0066] The second polymer may be a mixture of these epoxy resins.

[0067] The second polymer may have a melting point of 155° C. or less, or 150° C. or less, or 145° C. or less, or 140° C. or less, or 135° C. or less, or 130° C. or less, or 125° C. or less, or 120° C. or less, or 115° C. or less, or 110° C. or less. Preferably, the second polymer has a melting point of 130° C. or less.

[0068] Preferably, the second polymer is present in an amount of 10% by weight or less, more preferably 5% by weight or less, based on the total weight of the powder. For example, the second polymer may be present in a range of 0-1%, or 1%-2%, or 2%-3%, or 3%-4%, or 4%-5%, or 5%-6%, or 6%-7%, or 7%-8%, or 8%-9%, or 9%-10% by weight, based on the total weight of the powder.

[0069] The powder according to the invention may also comprise one or more additives selected from the group consisting of pigments or dyes, anti-crater or spreading agents, reducing agents, antioxidants, reinforcing fillers, UV stabilizers, flow agents, corrosion inhibitors or mixtures thereof. These additives are preferably present in an amount of 0-30%, more preferably 0-10%, even more preferably 0-5%, for example 0-5%, or 5%-10%, or 10%-15%, or 15%-20%, or 20%-25%, or 25%-30% by weight relative to the total weight of the powder.

[0070] The reinforcing filler may be of any type suitable for preparing polyamide-based powders. However, fillers selected from the group consisting of talc, calcium carbonate, manganese carbonate, potassium silicate, aluminum silicate, dolomite, magnesium carbonate, quartz, boron nitride, kaolin, wollastonite, titanium dioxide, glass beads, mica, carbon black, quartz, mixtures of mica and chlorite, feldspar, and dispersed nanometer fillers such as carbon nanotubes and silica are preferred. In a particularly preferred manner, the filler is calcium carbonate.

[0071] The pigment may be of any type known to those skilled in the art, preferably the pigment is selected from the group consisting of titanium dioxide, carbon black, cobalt oxide, nickel titanate, molybdenum disulfide, aluminum flake, iron oxide, zinc oxide, organic pigments such as phthalocyanine and anthraquinone derivatives, and zinc phosphate.

[0072] The dyes may be of any type known to those skilled in the art. Preferably, the dyes according to the present invention are selected from the group consisting of azo dyes, anthraquinone dyes, indigo-based dyes, triarylmethane dyes, chlorine dyes, and polymethine dyes.

[0073] The anti-crater and / or spreading agent may be of any type known to a person skilled in the art. Preferably, the anti-crater and / or spreading agent is selected from the group consisting of polyacrylate derivatives.

[0074] The UV stabilizer may be of any type known to those skilled in the art. Preferably, the UV stabilizer is selected from the group consisting of resorcinol derivatives, benzotriazoles, phenyltriazines and salicylates.

[0075] The antioxidant may be of any type known to those skilled in the art. Preferably, the antioxidant is selected from the group consisting of copper iodide in combination with potassium iodide, phenol derivatives and hindered amines.

[0076] The fluidizing agent may be of any type known to those skilled in the art. Preferably, the fluidizing agent is selected from the group consisting of alumina and silica.

[0077] The corrosion inhibitor may be of any type known to those skilled in the art. Preferably, the corrosion inhibitor is selected from the group consisting of phosphosilicates and borosilicates.

[0078] In an embodiment, the powder according to the invention consists essentially of or consists of the copolyamide, optionally a second polymer, and optionally one or more of the above additives.

[0079] The present invention also relates to a film that may be obtained by melting the above powder. Preferably, the film has a thickness of 100 to 550 μm, more preferably 200 to 500 μm. In an embodiment, the film has a thickness of 100 to 150 μm, or 150 to 200 μm, or 200 to 250 μm, or 250 to 300 μm, or 300 to 350 μm, or 350 to 400 μm, or 400 to 450 μm, or 450 to 500 μm, or 500 to 550 μm.

[0080] Method for producing powder The powder according to the invention may be prepared by mixing the components (i.e. the copolyamide having a melting point below 160° C. and any other components such as a second polymer having a melting point lower than that of the copolyamide, pigments or dyes, anti-crater or spreading agents, reducing agents, antioxidants, reinforcing fillers, UV stabilizers, flow agents and corrosion inhibitors) in the molten state, in particular in a mixer. If the powder comprises only the copolyamide, said copolyamide is melted. The mixture (or the copolyamide alone) is then allowed to solidify before being milled.

[0081] Alternatively, for example, only some of the polymeric components (including copolyamides having a melting point below 160° C.) can be melt mixed and then milled after solidification. The resulting particles are then dry-mixed in powder form with other components, such as pigments.

[0082] The temperature in the melt mixing step is preferably 150°C to 300°C, more preferably 180°C to 270°C.

[0083] The milling step may be carried out by any method, preferably the milling is selected from the group consisting of a hammer mill, a knife mill, a disc mill, an air-jet mill, and a cryogenic mill.

[0084] The purification method may also include a step of selecting powder particles having a desired particle size.

[0085] For surface coating According to another aspect, the present invention relates to the use of the above powder for coating a surface. The surface may be fully or partially coated. According to the present invention, the coating is preferably at least 0.8 (g / 100) -1 The intrinsic viscosity of the coating may be different from that of the powder. In particular, the intrinsic viscosity of the coating may be higher than that of the powder due to the fact that one or more polymerization reactions may be more or less carried out or restarted during application of the coating.

[0086] The use of the powder according to the invention for coating a surface differs from its use as a mastic or adhesive, in particular that after application the coating often forms a solid layer that is essentially non-deformable, and furthermore the coating is not used to bond two substrates together.

[0087] The surface is preferably a metallic surface, the term "metallic surface" meaning a surface comprising, consisting essentially of, or consisting of one or more metals.

[0088] The metal surface may be of any kind, preferably the metal surface is a part selected from the group consisting of normal or galvanized steel parts, aluminum parts, or aluminum alloy parts.

[0089] The surfaces, preferably metal surfaces, more preferably surfaces of conventional steel, aluminum or aluminum alloy parts, may be subjected to one or more surface treatments well known to those skilled in the art, preferably selected from the group consisting of coarse degreasing, alkaline degreasing, brushing, shot-blasting or sandblasting, fine degreasing, hot rinsing, phosphoric acid degreasing, iron / zinc / tri-cation phosphating, chromating, cold rinsing, and chrome rinsing. Thus, the powder may be used to coat treated or untreated metal surfaces.

[0090] The present invention is particularly advantageous for the coating of heat-sensitive surfaces, in particular heat-sensitive metal surfaces. For the purposes of the present invention, the term "heat-sensitive" means "not functioning well with applications at temperatures above 250°C". Such surfaces are, for example, surfaces comprising alloys of zinc and aluminum. They may also be surfaces that have undergone a heat-sensitive treatment. The present invention allows the coating of surfaces that do not function well with applications at temperatures below 250°C, for example the present invention may allow the coating of surfaces that do not function well with applications at temperatures above 230°C.

[0091] Advantageously, the surfaces to be coated are selected from the group consisting of smooth or shot-blasted degreased steel, phosphate degreased steel, iron or zinc phosphated steel, Sendzimir galvanized steel, electro-galvanized steel, bath-galvanized steel, electrophoretically-treated steel, chromated steel, anodized steel, corundum sandblasted steel, degreased aluminium, smooth or shot-blasted aluminium, chromated aluminium, cast iron and other metal alloys.

[0092] In certain embodiments, the coating has an intrinsic viscosity of 0.85 or more, or 0.9 or more, or 0.95 or more, or 1.05 or more, or 1 or more, or 1.1 or more, or 1.15 or more, or 1.2 or more, or 1.25 or more, or 1.3 or more, wherein the intrinsic viscosity is (g / 100 g) -1 It is expressed in units of.

[0093] Preferably, the coating is a film having a thickness of 100 to 500 μm, more preferably 200 to 500 μm. In an embodiment, the film has a thickness of 100 to 150 μm, or 150 to 200 μm, or 200 to 250 μm, or 250 to 300 μm, or 300 to 350 μm, or 350 to 400 μm, or 400 to 450 μm, or 450 to 500 μm, or 500 to 550 μm.

[0094] A subject of the invention is also a method for coating a surface, comprising the following steps: - placing said powder in contact with a surface; - The process of melting the powder.

[0095] The powder may be applied onto or placed in contact with a surface by a number of coating techniques well known to those skilled in the art. Preferably, coating according to the present invention is carried out by a method selected from the group consisting of submersion in a fluidized bed, electrostatic spraying and hot dusting.

[0096] The coating may in particular be carried out by immersion in a fluidized bed. Thus, the step of placing the surface in contact with the powder may comprise the following steps: - heating the surface to a temperature above the melting point of the copolyamide; - Submerging the surface in a fluidized bed containing the powder.

[0097] The coated surface is preheated to a temperature that allows for melting of the powder according to the invention. The surface is then submerged in a fluidized bed containing the powder according to the invention. The powder melts on contact with the surface and forms a coating thereon. The coated surface is then preferably cooled, for example in ambient air.

[0098] Preferably, the fluidizing air for fluidizing the composition is cool, clean and oil-free.

[0099] Preferably, the surface heating temperature is 250° C. or less, more preferably 230° C. or less. Therefore, the surface heating temperature may be 150 to 250° C., preferably 170 to 230° C.

[0100] Also, preferably, the surface is heated to a temperature at least 30° C. higher than the melting point of the copolyamide, more preferably 30 to 120° C. higher than the melting point of the copolyamide.

[0101] Preferably, the duration of immersion of the surface in the fluidized bed is 1-10 seconds, more preferably 3-7 seconds. The step of immersing the surface in the fluidized bed may be carried out one or more times (each immersion having a duration preferably of 1-10 seconds, more preferably 3-7 seconds).

[0102] Alternatively, the coating may be applied by electrostatic spraying, and the step of placing the surface in contact with the powder may include the steps of: - electrically charging the powder; - spraying an electrically charged powder onto the surface; - heating the surface coated with the powder to a temperature above the melting point of the copolyamide.

[0103] Coating by electrostatic spraying process consists of depositing electrostatically charged powder particles on a surface, especially at room temperature. The powder may be electrostatically charged during its passage through the nozzle of the spraying device. The composition thus charged may then be sprayed onto the article comprising the surface to be coated, connected to zero potential. The coated article may then be placed in an oven at a temperature that allows the composition to melt.

[0104] The powder spraying device can be of any kind. Preferably, the nozzle is brought to a high potential of about 10-100 kv of negative or positive polarity. This powder spraying device is an electrostatic gun that charges the powder by corona effect and / or triboelectricity.

[0105] Preferably, the powder flow rate in the spray device is between 10 and 200 g / min, more preferably between 50 and 120 g / min.

[0106] Preferably, the temperature of electrostatic application of the powder is 15°C to 25°C.

[0107] Preferably, the surface is left in the oven for between 3 and 15 minutes.

[0108] Advantageously, the heating temperature of the powder-coated surface may be below 250° C., more preferably below 230° C. Thus, the surface heating temperature may be between 150 and 250° C., preferably between 170 and 230° C.

[0109] The heating temperature of the powder-coated surface may preferably be at least 30° C. higher than the melting point of the copolyamide, more preferably 30-60° C. higher than the melting point of the copolyamide.

[0110] The surface is then cooled, for example to room temperature.

[0111] In another embodiment, the coating is performed by warm powdering. The step of placing the powder in contact with the surface comprises the steps of: - heating the surface to a temperature above the melting point of the copolyamide; - spraying a powder onto a surface.

[0112] The surface heating temperature may be as described above in connection with coating by immersion in a fluidized bed, and is preferably at least 30° C. above the melting point of the copolyamide, more preferably 30 to 120° C. above the melting point of the copolyamide.

[0113] The surface may then be allowed to cool, for example to room temperature. The sprayed powder may or may not be electrostatically charged.

[0114] The properties described above in connection with the use of powders to coat surfaces (particularly with respect to the surface, the intrinsic viscosity of the coating and the thickness of the coating film) may be applied in the same way to the coating method.

[0115] According to another aspect, the invention relates to an article comprising a surface covered with a coating which may be obtained by melting the powder described above.

[0116] The article preferably comprises: - the transfer of fluids, especially in the form of pipes, fittings, pumps or valves - Power vehicles, especially in the form of spline shafts, sliding door rails or springs - In particular for articles of wirework in the form of dish-washing baskets or springs. EXAMPLES

[0117] The following examples illustrate the invention without limiting it.

[0118] Synthesis of copolyamide powders The starting material (i.e. copolyamide) was introduced into a 14 L autoclave together with water, antioxidant (Irganox 1098) and phosphoric acid. The medium was rendered inert by vacuum and nitrogen injection four times in succession. The medium was then stirred and heated under autogenous pressure at a temperature of 280° C. for 3 hours. A vacuum to atmospheric pressure was then applied with a ramp of 2 hours, gradually lowering the temperature to 230° C. The medium was then stirred under a vigorous stream of nitrogen, increasing the viscosity until the desired stirring torque was reached. The medium was then transferred through a bar die into a water bath and then into the granulator.

[0119] The granules were then freeze-milled into powder form. Dv50 is 100 μm.

[0120] Preparation of the composition (coating powder) The following compositions were prepared by dry mixing of the ingredients in the amounts (given in parts) set out in the table below: [Table 1]

[0121] [Table 2] Pip = piperazine

[0122] The polyamides used have the following melting points and intrinsic viscosities: [Table 3]

[0123] Coating Formulations and Properties The coatings were deposited on the metal by submerging the various compositions (powders) in a fluidized bed.

[0124] The parameters for application of the coating by immersion in a fluidized bed are as follows: [Table 4]

[0125] [Table 5]

[0126] The coating thickness, appearance, gloss (at angles of 20° and 60°), intrinsic viscosity and mechanical properties (stress at break, yield point and elongation at break) were determined.

[0127] The intrinsic viscosity was measured as described above. The gloss was measured according to standard ISO 2813. The breaking stress, the yield point and the elongation at break were measured according to standard ISO 527-3.

[0128] The results are listed in the table below. [Table 6]

[0129] [Table 7] ND = Not Determined

[0130] Compositions 11 and 12 correspond to comparative examples.

[0131] The inherent viscosity of the coating is 0.8 (g / 100g) -1 It was found that if the coating powder was a polyamide powder with a relatively high melting point (186°C), it was impossible to apply the coating at a low temperature (230°C).

Claims

1. A copolyamide-based powder for forming coatings on surfaces, having a viscosity of 0.8 (g / 100 g) measured at 20° C. -1 or more, and the copolyamide has a melting point of 160° C. or less, and The powder, wherein the copolyamide is selected from the group consisting of: (i) a copolyamide which is a condensation product of at least two α,ω-aminocarboxylic acids, or two lactams, or one lactam and one α,ω-aminocarboxylic acid; (ii) a copolyamide which is a condensation product of at least one α,ω-aminocarboxylic acid or lactam, at least one aliphatic diamine having 2 to 36 carbon atoms and which may be saturated and cyclized, and at least one aliphatic dicarboxylic acid; and (iii) a copolyamide resulting from the condensation of an aliphatic diamine with an aliphatic dicarboxylic acid and at least one other aliphatic diamine selected from aliphatic diamines other than the above and an aliphatic dicarboxylic acid other than the above.

2. 2. The powder of claim 1, wherein the copolyamide is selected from the group consisting of copolyamide 6 / 11, copolyamide 6 / 12, copolyamide 6.6 / 11, copolyamide 6.6 / 12, copolyamide 6.10 / 11, copolyamide 6 / 12 / 11, copolyamide Pip.12 / 12 (Pip stands for piperazine), copolyamide 6 / 6.6 / 12, copolyamide 6 / Pip.12 / 12 or combinations thereof.

3. 3. Powder according to claim 1 or 2, wherein the copolyamide is present in an amount of 80% by weight or more, based on the total weight of the powder.

4. 4. Powder according to any one of claims 1 to 3, which also comprises a second polymer having a melting point lower than the melting point of the copolyamide.

5. 5. The powder of claim 4, wherein the second polymer is a second copolyamide and / or an epoxy resin.

6. 6. The powder according to claim 4 or 5, wherein the second polymer has a melting point of 130° C. or less.

7. 7. Powder according to any one of claims 4 to 6, wherein the second polymer is present in an amount of up to 10% by weight, relative to the total weight of the powder.

8. 8. The powder of claim 1, further comprising one or more additives selected from the group consisting of pigments or dyes, anti-crater or spreading agents, reducing agents, antioxidants, reinforcing fillers, UV stabilizers, flow agents, and corrosion inhibitors.

9. 9. The powder according to claim 8, wherein the mass of the additive is between 0 and 30% relative to the total mass of the powder.

10. 10. Powder according to any one of claims 1 to 9, wherein the copolyamide has a melting point below 150°C.

11. (g / 100g) -1 11. The powder according to claim 1, having an intrinsic viscosity of at least 0.

9.

12. 12. Powder according to any one of claims 1 to 11, comprising copolyamide-based particles having a volume median diameter Dv50 of 10 to 400 μm.

13. A method for obtaining a film comprising the steps of melting a powder according to any one of claims 1 to 12 and forming a film from the melt.

14. Use of the powder according to any one of claims 1 to 12 for coating a surface, wherein the coating has a viscosity of 0.8 (g / 100g) -1 Use having an intrinsic viscosity of at least 100%.

15. 15. The use according to claim 14, wherein the surface is an optionally treated metal surface.

16. The use according to claim 14 or 15, wherein the coating is a film having a thickness of from 100 to 550 μm.

17. 1. A method for coating a surface comprising the steps of: - placing said surface in contact with a powder according to any one of claims 1 to 12; - melting said powder.

18. placing the surface in contact with a powder comprises the steps of: - heating said surface to a temperature above the melting point of the copolyamide; - submerging the surface in a fluidized bed containing a powder.

19. placing the surface in contact with a powder comprises the steps of: - electrically charging the powder; - spraying an electrically charged powder onto said surface; The method according to claim 17, comprising the step of heating the surface coated with powder to a temperature above the melting point of the copolyamide.

20. placing the surface in contact with a powder comprises the steps of: - heating said surface to a temperature above the melting point of the copolyamide; A method according to claim 17, comprising the step of: - spraying a powder onto said surface.

21. An article comprising a surface covered with a coating obtained by melting a powder according to any one of claims 1 to 12.

Citation Information

Patent Citations

  • Coating of un-primed metals with polyamide powder coating compositions

    EP0866736A1

  • Resistance electrique ceramique et son procede de realisation

    FR2304998A1

  • JP1980500236A

  • Electrostatic coating of moldings with thermoplastic and crosslinkable copolyamide hot-melt adhesives

    US20020031614A1

  • Powdery sealant and sealing method

    US20130177704A1