New Products
A two-step condensation reaction between inorganic and organic network forming agents on pigments enhances chemical resistance and optical properties, addressing the trade-off in existing coatings.
Patent Information
- Application Number
- JP2021545992
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-18
- Filing Date
- 2020-02-05
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-02-05
AI Technical Summary
Existing protective coatings for pigments, particularly aluminum pigments, improve chemical resistance at the expense of optical properties, creating a trade-off that compromises their overall performance.
A method involving a two-step condensation-type reaction between inorganic and organic functional network forming agents is applied to pigments, resulting in a hybrid coating that enhances both chemical resistance and optical properties.
The method produces pigments with improved chemical resistance and optical properties, reducing the likelihood of ignition and improving gasification stability compared to previous coating methods.
Smart Images

Figure 0007584424000014 
Figure 0007584424000015 
Figure 0007584424000016
Abstract
Description
[Technical field]
[0001] The present invention relates to a new form of protective coating that can be applied to substrates such as pigments. The present invention also relates to a new method of treating pigments, including in particular pigments having the new protective coating of the present invention applied thereto, to provide them with improved properties. In particular, the present invention allows for the production of stabilized fine pigments (e.g. aluminum pigments) having an excellent combination of optical properties (e.g. gloss and / or brightness) and chemical resistance. [Background technology]
[0002] 2. Background of the Invention Protective coatings are known in the art. For example, metallic effect pigments, such as those based on aluminum, bronze, iron oxide or steel, may react with water, acids or bases in coating or ink formulations, and therefore the addition of a protective coating to such pigments may be used to improve their chemical resistance. However, one drawback associated with applying such a protective coating to a pigment is that it may generally be expected to adversely affect the optical properties of the pigment. As such, there is often a trade-off between the potentially competing objectives of optimizing chemical resistance with a pigment and also maintaining good optical properties. For example, among the known commercially coated aluminum (Al) pigments, those sold by Eckart under the trade name "PCU" have been described as the best Al pigment product on the market in terms of chemical resistance. However, this useful attribute comes at the expense of the optical properties of the pigment. This is shown, for example, in Figure 2, which is an image of two polymeric powder coating samples. One of them is of PCU1000 pigment and the other is of pigment particles having the same particle size (i.e., 15 μm) but with a different protective coating sold by Schlenk under the trade name POWDAL 8500. As explained in more detail below, the POWDAL 8500 product is found to have better optical properties but inferior chemical resistance.
[0003] Other coated pigments that have been discussed in the art include those described in CN106317969, CN106700662, WO9638506 and US20110195244, which include coatings prepared using polyaddition reactions. Summary of the Invention
[0004] The present invention is based on the discovery that a particular method of coating a pigment leads to a product having a surprisingly advantageous combination of both chemical resistance and optical properties. That is, the present invention provides a method of coating a substrate comprising the step of (a) subjecting an inorganic network former and an organofunctional network former to a condensation type reaction, and thereafter (b) one or more further steps in which the inorganic network former and the organofunctional network former are subjected to a condensation type reaction.
[0005] The present invention also provides a method for preparing a coated substrate, comprising one or more steps in which an inorganic network former and an organofunctional network former are subjected to a condensation type reaction in the presence of a product, said product being obtainable by subjecting an inorganic network former and an organofunctional network former to a condensation type reaction in the presence of a substrate. This aspect of the invention focuses only on step (b) of the method of the invention defined above. The preferred aspects of the invention outlined herein apply correspondingly to this embodiment.
[0006] In this regard, it has been found that the coated substrates prepared by the above process allow for a combination of high chemical resistance and good optical properties that would not be obtainable using previous coating methods. It is also believed that the coating resulting from the above process is more effective at reducing the likelihood of ignition during subsequent processing and handling compared to coatings applied using previous coating methods. It is also believed that the coating resulting from the above process is more effective at improving gasification stability compared to coatings applied using previous coating methods. However, the exact structural differences resulting from using a method comprising two steps (a) and (b) may not always be immediately amenable to simple and immediate characterization, and therefore the novel products are best defined by reference to the particular combination of properties they exhibit. That is, the present invention also provides coated substrates obtainable by the above defined method of the present invention. The present invention also provides coated substrates having (i) a chemical resistance score of 12 or less in the "Test Method for Measuring Chemical Resistance of Coated Pigments" further described below, and (ii) a gloss dispersion value (X) of ≦5.0 [where: - X=Y / (13-Chemical Resistance Score of Coated Pigment), - Y is the percentage change in gloss resulting from the addition of the coating to the pigment, calculated as (100*(Y1-Y2) / Y1); - Y1 is the gloss of the uncoated pigment, and - Y2 is the gloss of the coated pigment (wherein the gloss is measured by preparing a sample containing a coated or uncoated pigment according to steps (a) to (g) of the "Test Method for Measuring Chemical Resistance of Coated Pigments" further described below, and then measuring the gloss at 60° using a gloss meter).
[0007] Furthermore, the present invention relates to a pigment having a chemical resistance of less than 12 in the "Test Method for Measuring Chemical Resistance of Coated Pigments" further described below, and (ii) a lightness dispersion L of ≥ 90. A or L B Value [where: - L A is calculated as (100*(1+(Q2-Q1) / Q1)), - Q1 is the color value at 15° of the uncoated pigment, and - Q2 is the color value of the coated pigment at 15°; - L B is calculated as (100*(1+(Q4-Q3) / Q3)), - Q3 is the color value at -15° of the uncoated pigment, and - Q4 is the lightness of the coated pigment at -15° (wherein the color values at 15° and -15° are measured by preparing a sample containing a coated or uncoated pigment according to steps (a) to (g) of the "Test method for measuring the chemical resistance of coated pigments" further described below, and then using a gloss meter).
[0008] Further, the present invention provides a composition having an MIE*surface area (where MIE is the minimum ignition energy and surface area is the surface area measured by the BET method) of at least 40 mJ m 2 / g (preferably at least 55 mJ m 2 The present invention provides a coated metal pigment or a coated metal oxide pigment having a value of (A / g).
[0009] Further, the present invention relates to a pigment having (i) a gassing stability score of ≥ 700 seconds (preferably ≥ 1000 seconds) in the "Test Method for Measuring Gassing Stability of Coated Pigments" further described below, and (ii) a gloss dispersion value (X) of ≤ 5.0, where: - X=Y / (13-Chemical Resistance Score of Coated Pigment), - Y is the percentage change in gloss resulting from the addition of the coating to the pigment, calculated as (100*(Y1-Y2) / Y1); - Y1 is the gloss of the uncoated pigment, and - Y2 is the gloss of the coated pigment (wherein the gloss is measured by preparing a sample containing a coated or uncoated pigment according to steps (a) to (g) of the "Test Method for Measuring Chemical Resistance of Coated Pigments" further described below, and then measuring the gloss at 60° using a gloss meter).
[0010] Further, the present invention relates to a pigment having (i) a gassing stability of ≧700 seconds (preferably ≧1000 seconds) in the “Test Method for Measuring Gassing Stability of Coated Pigments” further described below, and (ii) a lightness dispersion L of ≧90. A or L B Value (where: - L A is calculated as (100*(1+(Q2-Q1) / Q1)), - Q1 is the color value at 15° of the uncoated pigment, and - Q2 is the color value of the coated pigment at 15°; - L B is calculated as (100*(1+(Q4-Q3) / Q3)), - Q3 is the color value at -15° of the uncoated pigment, and - Q4 is the lightness of the coated pigment at -15° (wherein the color values at 15° and -15° are measured by preparing a sample containing a coated or uncoated pigment according to steps (a) to (g) of the "Test Method for Measuring Chemical Resistance of Coated Pigments" further described below, and then using a gloss meter).
[0011] It has been found that PVD pigments are particularly prone to chemical attack, and protective coatings applied to other pigment types may not function effectively on PVD pigments. However, it is believed that the coatings of the present invention provide PVD pigments with a higher level of chemical resistance than was previously possible. That is, the present invention also provides coated PVD metal pigments or coated PVD metal oxide pigments having a chemical resistance score of 12 or less in the "Test Method for Measuring the Chemical Resistance of Coated Pigments" described herein.
[0012] The present invention also provides a coated PVD metal pigment or a coated PVD metal oxide pigment having a gassing stability score of ≧700 seconds (preferably ≧1000 seconds) in the “Test Method for Measuring Gassing Stability of Coated Pigments” described herein.
[0013] The invention also provides a coated PVD metal pigment or a coated PVD metal oxide pigment having a gassing stability score of < 5ml after 21 days in the "Extended Gassing Test Method" described herein.
[0014] The present invention also provides a method comprising applying one or more surface modifiers to a coated substrate of the present invention as defined above, wherein the substrate is a pigment.
[0015] The present invention also relates to a method for producing a pigment-based substrate. (i) coating a substrate by the method defined above, or (ii) preparing a coated substrate by the method defined above, and then applying one or more surface modifiers to the coated substrate; The present invention provides a method comprising:
[0016] The present invention also relates to a method of treating a pigment comprising simultaneously, separately or sequentially applying one or more surface modifiers to the pigment, wherein the one or more surface modifiers are (a) both (i) an organophosphorus compound, and (ii) a compatibilizer, as further defined below, wherein a majority of the compatibilizer does not become covalently bonded to the pigment; (b) both (i) a fatty acid, and (ii) a compatibilizer, as further defined below, wherein a majority of the compatibilizer does not become covalently bonded to the pigment; or (c) comprising both (i) an organofunctional network former, and (ii) an organophosphorus compound. That is, by way of example, the invention provides a method of treating a pigment comprising simultaneously, separately or sequentially applying to the pigment one or more surface modifiers, wherein the one or more surface modifiers comprise an organophosphorus compound and a compatibilizer, as further defined below, and wherein a majority of the compatibilizer does not become covalently bonded to the pigment.
[0017] The invention also provides a pigment having on its surface (a) an organophosphorus compound and a compatibilizer as further defined below, where a majority of the compatibilizer is not covalently bonded to the pigment; (b) a fatty acid and a compatibilizer as further defined below, where a majority of the compatibilizer is not covalently bonded to the pigment; or (c) an organofunctional network former and an organophosphorus compound. (That is, by way of example, the invention provides a pigment having on its surface an organophosphorus compound and a compatibilizer as further defined below, where a majority of the compatibilizer is not covalently bonded to the pigment.)
[0018] The invention also provides an article of manufacture comprising a coated substrate of the invention as defined herein, the article being a varnish, an automotive finish, a paint, a printing ink, a powder coating material, an architectural paint, a plastic, a security printing ink, a ceramic, a glass or a cosmetic.
[0019] The present invention also provides a method of coating an article comprising electrostatically applying a powder coating material to the article, and optionally curing the applied coating material, wherein the powder coating material comprises a coating substrate of the present invention as defined herein.
[0020] The present invention also provides a coated article comprising the inventive coated substrate as defined herein. [Brief description of the drawings]
[0021] Description of the drawings [Figure 1] FIG. 1 shows images of two test samples, each prepared from a polymer powder and a coated pigment of the present invention, that were subjected to a chemical resistance test. [Diagram 2] FIG. 2 shows, for comparison, images of two corresponding samples, each prepared from a different commercially available pigment. [Diagram 3] Each of Figures 3 to 5 shows images of two samples after chemical resistance testing. In any particular figure, the two samples differ only in the pigments used to prepare them (one of the invention and the other a commercial product). The formulation for each pair of samples (in each figure) differed in composition and / or how it was made. In other words, the invention was compared to a commercial product in a variety of different powder coating environments. [Figure 4]Each of Figures 3 to 5 shows images of two samples after chemical resistance testing. In any particular figure, the two samples differ only in the pigments used to prepare them (one of the invention and the other a commercial product). The formulation for each pair of samples (in each figure) differed in composition and / or how it was made. In other words, the invention was compared to a commercial product in a variety of different powder coating environments. [Diagram 5] Each of Figures 3 to 5 shows images of two samples after chemical resistance testing. In any particular figure, the two samples differ only in the pigments used to prepare them (one of the invention and the other a commercial product). The formulation for each pair of samples (in each figure) differed in composition and / or how it was made. In other words, the invention was compared to a commercial product in a variety of different powder coating environments. [Figure 6] Figure 6 shows images of drawdown samples made using the liquid coating after chemical testing. The sample on the left was made using the coated pigment of the present invention, and the sample on the right was made using a commercial pigment product. [Figure 7] FIG. 7 illustrates a gasification rig suitable for use in the test procedures discussed below in connection with Examples 41D and 41E. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Detailed Description Base material The substrate for use in the present invention is not particularly limited. It can be a large-scale material such as a panel or spar, or a small-scale material such as a particulate product, e.g., flakes or platelets.
[0023] Preferably, the substrate has a d of at least 1 μm, more preferably at least 2 μm, at least 3 μm, at least 4 μm, or at least 5 μm. 50d) flake or platelet products (e.g. pigments) having a high 50 The value is preferably 2000 μm or less, such as 1500 μm or less, 1000 μm or less, 500 μm or less, 200 μm or less, 150 μm or less, 100 μm or less, 80 μm or less, 60 μm or less, 50 μm or less, 40 μm or less, 35 μm or less, 30 μm or less, or 25 μm or less. 50 Typical ranges of values are from 2 to 2000 μm, preferably from 3 to 1000 μm, more preferably from 4 to 500 μm, even more preferably from 5 to 100 μm, even more preferably from 5 to 50 μm, and even more preferably from 5 to 25 μm. 50 The value is preferably determined by laser diffraction methods.
[0024] Preferably, the substrate is a flake or platelet product (e.g., pigment) having an average aspect ratio of at least 5, more preferably at least 10, at least 25, at least 50, at least 75, at least 100, at least 110, at least 120, at least 130, at least 140, at least 150, at least 160, at least 170, at least 180, at least 190, or at least 200. The average aspect ratio is preferably 2000 or less, such as 1500 or less, 1000 or less, or 750 or less. Suitable ranges of average aspect ratios are from 5 to 2000, preferably 50 to 2000, more preferably 100 to 2000, even more preferably 120 to 2000, even more preferably 150 to 2000 and more preferably still 200 to 2000. The average aspect ratio may be measured by taking the average (mean) aspect ratio of 30 (preferably 50, more preferably 100) individual flakes or platelets in a flake or platelet product as measured by a microscope such as a scanning electron microscope (SEM), transmission electron microscope (TEM) or atomic force microscope (AFM), where the aspect ratio of a particular flake or platelet is defined as the longest diameter of the flake or platelet divided by its thickness. Preferably, the aspect ratio of an individual flake or platelet product is measured by scanning electron microscopy, for example using a Hitachi™ 4000PLUS instrument.
[0025] Preferably, the substrate has an aspect ratio of at least 100 (such as at least 120) and a d of 50 μm or less, 40 μm or less, 35 μm or less, 30 μm or less, or 25 μm or less. 50 It has a value.
[0026] Preferably, the substrate is ≧2 m 2 / g or ≥ 3m 2 / g etc. ≧1m 2 / g as measured by the BET method. In some embodiments, it is ≥ 4 m 2 / g or ≥ 5m 2 / g.
[0027] Preferably, the substrate has a d of 35 μm or less (such as 30 μm or less or 25 μm or less). 50 value and an aspect ratio of at least 120, such as at least 150, or at least 200.
[0028] The substrate may comprise (or consist essentially of) an inorganic material such as mica or glass, and / or it may comprise (or consist essentially of) a metal, either elemental or alloyed. The substrate may comprise (or consist essentially of) an inorganic material or a metal with a coating of one or more metal oxide layers. Preferably, the substrate is a metal or a metal oxide. More preferably, the substrate is a metal flake or platelet, where the metal is preferably aluminum, bronze, copper or zinc, and most preferably aluminum. Examples of suitable aluminum pigments are SPARKLE SILVER Elite 010, SPARKLE SILVER Elite 012, SPARKLE SILVER Elite 011 LM and SPARKLE SILVER Elite 015 LM available from Silberline Manufacturing Co., US.
[0029] In a preferred embodiment, the substrate is a metal pigment, more preferably an aluminum, bronze, copper or zinc pigment, most preferably an aluminum pigment. When the substrate is a metal (e.g. Al) pigment, the proportion of metal (e.g. Al) is preferably ≧90 wt. %, such as ≧95, ≧98, ≧99, ≧99.5 or ≧99.9, of the total weight of the uncoated metal (e.g. Al) pigment.
[0030] Substrates for use in the present invention (e.g., metal flake or platelet pigments) can be produced by known means. For example, metal flake or platelet pigments can be produced by a grinding process, such as ball milling. In another embodiment, metal flake or platelet pigments can be produced by a vacuum metallization process, such as by physical vapor deposition (PVD). In a further embodiment, metal flake or platelet pigments can be produced by forming a metal oxide layer on the product of the grinding or vacuum metallization process described above.
[0031] Inorganic Network Formers For the avoidance of doubt, the claims and the specification generally refer to the presence of "one" inorganic network former, although it is of course possible for multiple different types of inorganic network formers to be present at a particular step of the method of the invention, i.e. references herein to "an inorganic network former" are intended to refer to the situation where one inorganic network former is present alone, or where two or more inorganic network formers are present together.
[0032] The inorganic network former is preferably a compound represented by the formula (I) MX n (I) (In the formula, M is Si, Al, Ti, Zr, B, Fe, Mg, Mn, Sb, Cr, Zn and / or Ce; - each X is independently an optionally hydrolyzable and / or condensable group selected from halogen, -OH, or -OR, and / or one, two or three pairs of X moieties together represent a divalent chelating ligand, where each R group is a C group, the carbon chain of which is optionally interrupted by one or more heteroatoms selected from N, O and S; 1-10 is an alkyl group, and - n is an integer from 2 to 6, corresponding to the oxidation state of M.
[0033] Of course, not all possible values of n (2 to 6) will always be possible for every option of M. One skilled in the art will recognize which options of n are possible for a particular option of M, given the possible oxidation states of that option. For example, when M is Sb(V), n may preferably be 5; when M is Si, Ti or Zr, n may preferably be 4; when M is Al, Ce, Fe(III), SB(III) or B, n may preferably be 3; and when M is Zn, Fe(II) or Mg, n may preferably be 2.
[0034] In a preferred embodiment, the inorganic network former is a compound of formula (I) where M is Si, Al, Ti, Zr or Fe; 1-6 and n is 2, 3 or 4. In a further preferred embodiment, M is Si; X is methoxy or ethoxy; and n is 4. Typically, the inorganic network former is tetraethoxysilane (TEOS).
[0035] Organofunctional Network Formers For the avoidance of doubt, the claims and specification will generally refer to the presence of "one" organofunctional network former, although it is of course possible for multiple different types of organofunctional network formers to be present at a particular step of the method of the present invention, i.e., references herein to an "organofunctional network former" are intended to refer to the situation where one organofunctional network former is present alone, or where two or more organofunctional network formers are present together.
[0036] The organofunctional network former is preferably represented by formula (II) R 1 i R 2 j R 3 k Six (4-i-j-k) (II) (In the formula, - each of i, j, and k is independently 0 or 1, with the proviso that at least one of i, j, and k is 1; - R 1 , R 2 and R 3 is independently an organic group, with the proviso that R 1 , R 2 and R 3 at least one of is a reactive organic group, and - each X is independently a halogen, -OH, -OR 7 or -Y, and / or a pair of X moieties together represent a divalent chelating ligand, where 〇 Each R 7 are independently an organic group, preferably a C in which the carbon chain is optionally interrupted by one or more heteroatoms selected from N, O and S. 1-10 is an alkyl group, and Each Y is independently -(OR 4 -O-Si(R 5 ) m (X') 2-m -) n R 6 where: ■ Each R 4 are independently a divalent organic group, ■ Each R 5 are independently an organic group; ■ each m is independently 0, 1, or 2; ■ Each X' is a halogen, -OH, or -OR. 7 and / or one or more pairs of geminal X′ moieties together represent a divalent chelating ligand, where each R 7 are independently an organic group; ■ n is 1 to 10, and ■ R 6 is an organic group.
[0037] The reactive organic group of the above compound of formula (II) is preferably a hydrocarbyl group having one or more substituents selected from epoxy, amino, hydroxyl, thiol, acrylate, methacrylate, vinyl, allyl, alkenyl, alkynyl, carboxyl, carboxylic anhydride, isocyanate, cyanate, ureido and carbamate.
[0038] Preferably, the organofunctional network former is a compound selected from aminoalkyltrialkoxysilanes, N-(alkyl)-aminoalkyltrialkoxysilanes, N-aminoalkyl-aminoalkyl(alkyl)dialkoxysilanes, N-aminoalkyl-aminoalkyltrialkoxysilanes, epoxyalkyltrialkoxysilanes, mercaptoalkyltrialkoxysilanes, alkacryloxyalkyltrialkoxysilanes (e.g. methacryloxyalkyltrialkoxysilanes) and ureidoalkyltrialkoxysilanes. Preferably, the alkyl moieties are each independently selected from C 1-10 Alkyl, more preferably C 1-4 C such as alkyl 1-6 Preferably, the alkoxy moiety is selected from C 1-10 Alkoxy, more preferably C 1-4 Alkoxy etc. C 1-6 They are alkoxy (typically they are ethoxy or methoxy, most commonly ethoxy).
[0039] For example, suitable organofunctional network formers include the following: Examples of suitable silanes include 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-(n-butyl)-3-aminopropyltrimethoxysilane, N-(n-butyl)-3-aminopropyltriethoxysilane, N-2-aminoethyl-3-aminopropyl(methyl)dimethoxysilane, N-2-aminoethyl-3-aminopropyl(methyl)diethoxysilane, N-2-aminoethyl-3-aminopropyltrimethoxysilane, N-2-aminoethyl-3-aminopropyltriethoxysilane, 3-glycidyloxypropyltriethoxysilane, 3-glycidyloxypropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-ureidopropyltrimethoxysilane, and 3-ureidopropyltriethoxysilane.
[0040] Suitable agents in this regard are commercially available.For example, agents with epoxy groups are available under the trade name Dynasylan®, such as Dynasylan® GLYEO and Dynasylan® GLYMO, from Evonik Resource Efficiency GmbH, Germany, and agents with amino groups are also available under the trade name Dynasylan®, such as Dynasylan® AMEO (3-aminopropyltriethoxysilane), Dynasylan® AMMO (3-aminopropyltrimethoxysilane), Dynasylan® DAMO (N-2-aminoethyl-3-aminopropyltrimethoxysilane) and Dynasylan® TRIAMO (triaminofunctional propyltrimethoxysilane), from Evonik Resource Efficiency GmbH, Germany.
[0041] method As stated above, the present invention provides a method for coating a substrate, comprising the steps of: (a) subjecting an inorganic network former and an organofunctional network former to a condensation type reaction; And afterwards: (b) one or more (e.g., one or two) further steps in which the inorganic network former and the organofunctional network former are subjected to a condensation type reaction. The present invention provides a method comprising:
[0042] It has been found that applying hybrid coatings in this manner, i.e. using two or more separate steps of subjecting inorganic network formers and organic functional network formers to condensation type reactions, produces coated substrates with surprisingly superior properties compared to the corresponding coated substrates prepared by subjecting (for example) the equivalent total amount of inorganic network formers and organic functional network formers to condensation type reactions in a single step (the properties are particularly beneficial when the substrate is a metal pigment, such as an aluminum pigment).It is believed that one reason for this may be related to the fact that introducing reagents in two steps can promote the formation of chemical bonds between the organic functional moieties present on the substrate after step (a) and the organic functional moieties of the organic functional network former used in step (b).For example, if the organic functional network former in step (a) is characterized by epoxy moieties, then the condensation type reaction in step (a) can be expected to produce a substrate with terminal hydroxyl groups.If the organic functional network former in step (b) is characterized by epoxy moieties, then those moieties can react with the terminal hydroxyl groups present after step (a). That is, in a preferred aspect, the organofunctional network former in step (b) comprises an organofunctional moiety that can (and does) react with an organofunctional moiety present on the substrate surface after step (a) (and derived from the organofunctional network former used in step (a)) to form a chemical bond, such as a covalent bond. That said, this possible explanation (related to the potential promotion of chemical bond formation between the organofunctional moieties) is also believed to be only one of many reasons why the method of the present invention provides a superior coating, and thus, in order to enjoy some of the advantages of the present invention, it may be preferred, but not essential, that the organofunctional network former in step (b) is capable of reacting with one or more organofunctional moieties present on the substrate surface after step (a) to form a chemical bond.
[0043] For example, a preferred embodiment is - the organofunctional network former in step (a) comprises one or more epoxy, amino, mercapto, and / or ureido moieties; and the organofunctional network former in step (b) comprises one or more epoxy or alkacrylic (e.g. methacrylic) moieties; or - the organofunctional network former in step (a) comprises one or more alkacrylic (e.g. methacrylic) moieties; and The organofunctional network former in step (b) contains one or more amino, mercapto, and / or ureido moieties (preferably one or more amino moieties). Includes:
[0044] Further preferred embodiments include those in which the organofunctional network former in step (a) comprises one or more epoxy or amino moieties; and the organofunctional network former in step (b) comprises one or more epoxy or alkacrylic (e.g. methacrylic) moieties (preferably one or more epoxy moieties).
[0045] In one preferred embodiment of the method of the present invention: - the inorganic network former in each of steps (a) and (b) is a tetraalkoxysilane; - the organofunctional network former in step (a) is an epoxysilane or an aminosilane, and The organofunctional network former in step (b) is an epoxysilane.
[0046] From the definition of the inventive method above, and in particular the fact that it is a method for coating a substrate, it will be understood that step (a) should be carried out in the presence of a substrate (to be coated), and likewise step (b) should be carried out in the presence of a substrate already coated during step (a). That is to say, the present (inventive) method for coating a substrate comprises (a) a step of coating the substrate by subjecting an inorganic network former and an organofunctional network former to a condensation type reaction in the presence of said substrate, and then (b) one or more further steps in which said substrate is further coated by subjecting an inorganic network former and an organofunctional network former to a condensation type reaction in the presence of the substrate coated in step (a).
[0047] As indicated above, the method of the invention may involve more than two condensation type reactions, such as three or more such reactions. For example, in one embodiment, the method of the invention comprises: (a) subjecting an inorganic network former and an organofunctional network former to a condensation type reaction; And afterwards: (b) a first further step of subjecting the inorganic network former and the organofunctional network former to a condensation type reaction, and then a second (and optionally more) further step of subsequently subjecting the inorganic network former and the organofunctional network former to a condensation type reaction.
[0048] Carrying out three or more such condensation-type reaction steps may impart further enhanced properties to the coated pigment. In this regard, however, as indicated above, it is not just the case that additional reactions are carried out to create a thicker (and therefore more protective) overall layer. Rather, the advantages of the method of the present invention arise over a corresponding product in which the same amount of overall coating is applied in fewer steps, such as in a single step.
[0049] It is preferred that the condensation type reaction in step (a) proceeds to a significant degree of completeness (e.g., ≧30% complete, ≧40% complete, ≧50% complete, ≧60% complete, ≧70% complete, ≧80% complete, or ≧90% complete) before any subsequent condensation type reaction in step (b). When step (b) includes multiple steps in which the inorganic network former and the organofunctional network former are subjected to condensation type reactions, it is further preferred that each condensation type reaction proceeds to a significant degree of completeness (i.e., ≧30% complete, ≧40% complete, ≧50% complete, ≧60% complete, ≧70% complete, ≧80% complete, or ≧90% complete) before any subsequent condensation type reaction.
[0050] Preferably, the condensation type reaction in step (a) proceeds for ≧5 minutes, such as ≧10 minutes, ≧15 minutes, ≧20 minutes, ≧30 minutes, ≧45 minutes, ≧60 minutes, ≧75 minutes, ≧90 minutes, or ≧120 minutes or more, before step (b). When step (b) includes multiple steps in which the inorganic network former and the organofunctional network former are subjected to condensation type reactions, it is further preferred that each condensation type reaction proceeds to a significant degree of completeness (e.g., proceeds for ≧5 minutes, such as ≧10 minutes, ≧15 minutes, ≧20 minutes, ≧30 minutes, ≧45 minutes, ≧60 minutes, ≧75 minutes, ≧90 minutes, or ≧120 minutes or more) before any subsequent condensation type reaction. In both steps, there is no specific upper limit to the length of the reaction, but in general, it is unnecessary to continue the reaction for more than, for example, 10 hours, since no additional advantage would be expected (typically the reaction may be stopped after ≦5 hours, such as ≦4 hours or ≦3 hours).
[0051] In a preferred embodiment, the condensation type reaction (preferably all such reactions) in step (a) and / or (b) of the method of the present invention is carried out in the presence of a catalyst. The catalyst may be an acid or a base. Preferably, the catalyst is a Bronsted base or Lewis base catalyst, preferably a nitrogen-based Bronsted base or nitrogen-based Lewis base catalyst. Suitable nitrogen-based Bronsted base or nitrogen-based Lewis base catalysts may be ammonia, amines (including polyamines), amino alcohols or nitrogen-containing aromatic or heteroaromatic compounds. Particularly preferred nitrogen-based Bronsted base or nitrogen-based Lewis base catalysts include ethylenediamine (EDA), monoethanolamine (MEA) and N-methylimidazole (NMI). Such agents may be used directly or mixed with a solvent.
[0052] In a preferred embodiment, the condensation type reactions (preferably all such reactions) in steps (a) and / or (b) of the process of the present invention are carried out in a solvent. Preferably, the solvent is an aprotic solvent, more preferably a C 1-6 Alkanol or C 1-6 Alkoxy-C 1-6 and an alcohol, such as an alkanol. Suitable solvents include isopropanol (IPA) and 1-methoxy-2-propanol.
[0053] In a preferred embodiment, the condensation type reactions (preferably all such reactions) in steps (a) and / or (b) of the process of the invention are carried out at elevated temperatures. The appropriate temperature will depend on the particular reagents present, and in particular any solvents that may be used. Preferred temperatures are those of ≧50° C., such as ≧60° C., ≧70° C., or ≧80° C. The temperature is preferably ≦200° C., such as ≦170° C., ≦150° C., or ≦130° C.
[0054] In steps (a) and / or (b) (preferably both) in the process of the present invention, the molar ratio of inorganic network former to organofunctional network former may be defined as X:1. Preferably, X is ≧0.5, such as ≧1, ≧2, ≧3, ≧4, ≧5, ≧6, ≧7, or ≧8. Preferably, X is ≦200, such as ≦160, ≦140, ≦120, ≦110, or ≦100. Typical ranges are from 1 to 120, or from 5 to 120.
[0055] The absolute amounts of inorganic and organofunctional network formers used will depend on the available surface area of the substrate being coated. For pigment substrates, the surface area will of course depend on the particle size. These agents may be used in amounts that provide the coated substrate with a coating having a thickness of Y. Preferably Y is ≧2 nm, such as ≧3 nm, ≧4 nm, ≧5 nm, ≧6 nm, ≧7 nm, or ≧8 nm. Preferably Y is ≦300 nm, such as ≦250, ≦200, ≦150, ≦120, ≦100, ≦90, ≦90, ≦80, ≦70, ≦60, or ≦50 nm. A typical range is 5-70 nm.
[0056] The coating obtainable by the method of the present invention may have a relatively high silicon content. In a preferred aspect, the silicon content of the coating may be ≧12%, such as ≧13%, ≧14%, or ≧15%, as measurable by EDS.
[0057] Considering the total amount of inorganic network former and organofunctional network former used in the process of the present invention, there is a range of variation in the proportion of each used in step (a) versus step (b) (particularly when step (b) comprises multiple separate condensation type reactions). However, for both inorganic network former and also organofunctional network former, if the ratio of the amount used in a condensation type reaction in the process to the amount used in any other condensation type reaction in the same process is defined as Z:1, then preferably Z is in the range of 0.1 to 10, such as 0.2 to 5.
[0058] In each of steps (a) and (b) of the method of the invention, a condensation type reaction leads, preferably via a sol-gel process, to the formation of a network that is (mainly) inorganic in nature, but also contains organic moieties derived from the organofunctional network former. For example, in the preferred situation where the inorganic network former is a tetraalkoxysilane, the reaction can lead to the formation of a network based on Si and O, but also containing organic moieties derived from the organofunctional network former.
[0059] In a preferred aspect of the method of the present invention, in step (a), the condensation type reaction occurs in the presence of a dispersing agent. The dispersing agent is preferably an agent composed of inert particles, such as metal oxide particles, for example amorphous metal oxide particles such as AEROXIDE Alu C, AEROXIDE Alu 130, AEROSIL 200 or ACEMATT OK412 available from Evonik. Preferably, the dispersing agent is in the form of nanoparticles. Suitable agents include fumed silica and colloidal silica. The presence of a dispersing agent can facilitate processing and can also help increase the chemical resistance of the coated substrate.
[0060] In one particularly preferred aspect, the method of coating a substrate (of the invention) comprises the steps of: (a) subjecting an inorganic network former and an organofunctional network former to a condensation type reaction in the presence of a solvent and a catalyst, said reaction preferably proceeding for ≧5 minutes; And after (b) one or more further steps in which the inorganic network former and the organofunctional network former are subjected to a condensation type reaction in the presence of a solvent and a catalyst. [where: - the substrate is an aluminum pigment; - each inorganic network former is independently a tetraalkoxysilane; - each organofunctional network former is independently a compound selected from aminoalkyltrialkoxysilanes, N-(alkyl)-aminoalkyltrialkoxysilanes, N-aminoalkyl-aminoalkyl(alkyl)dialkoxysilanes, N-aminoalkyl-aminoalkyltrialkoxysilanes, epoxyalkyltrialkoxysilanes, mercaptoalkyltrialkoxysilanes, alkacryloxyalkyltrialkoxysilanes (e.g., methacryloxyalkyltrialkoxysilanes) and ureidoalkyltrialkoxysilanes, wherein the alkyl moieties are each independently selected from C 1-10 alkyl, and alkoxy moieties are each independently selected from C 1-10 alkoxy (and preferably the organofunctional network former in step (b) comprises an organofunctional moiety that reacts with the organofunctional moieties present on the substrate surface after step (a) and derived from the organofunctional network former used in step (a) to form chemical bonds); and - in each of steps (a) and (b), the molar ratio of inorganic network former to organofunctional network former is X:1, where X is from 1 to 120; Includes.
[0061] Coated Substrate As mentioned above, the present invention provides a coated substrate obtainable by the method of the present invention as defined herein (for the avoidance of doubt, this includes a coated substrate to which one or more surface modifiers have been applied, as further described below). The preferred features of the present invention described in the previous and next sections apply equally to the coated substrate of the present invention. For example, the coating in the coated substrate of the present invention may have a thickness Y, where preferably Y is ≧2 nm, such as ≧3 nm, ≧4 nm, ≧5 nm, ≧6 nm, ≧7 nm, or ≧8 nm, and preferably Y is ≦300 nm, such as ≦250, ≦200, ≦150, ≦120, ≦100, ≦90, ≦90, ≦80, ≦70, ≦60, or ≦50 nm. A typical range is 5 to 70 nm.
[0062] The coated substrate is preferably a coated aluminum pigment. In this regard, as indicated above, it is believed that the method of the present invention allows the preparation of aluminum pigments having a combination of high chemical resistance and good optical properties that would not be possible to obtain using previous coating methods, and also allows the application of coatings that are more effective in reducing the possibility of ignition during subsequent processing and handling, compared to coatings applied using previous coating methods, and also allows the application of coatings that are more effective in improving gasification stability, compared to coatings applied using previous coating methods, plus PVD aluminum pigments with chemical resistance that would not be possible to obtain using previous coating methods. To this end, the products provided by the present invention include: - coated metal pigments or coated metal oxide pigments (i) having a chemical resistance score of 12 or less in the "Test method for measuring the chemical resistance of coated pigments" further defined below, and (ii) having a gloss dispersion value (X) as defined above of ≦5.0 (this type of product is referred to below as the first pigment); - (i) having a chemical resistance of less than 12 according to the "Test Method for Determining the Chemical Resistance of Coated Pigments" further defined below; and (ii) a lightness dispersion L, as defined above, of ≥ 90. A or L B coated metal pigments or coated metal oxide pigments, the value of which is (products of this type are referred to below as second pigments); - MIE*surface area (where MIE is the minimum ignition energy and surface area is the surface area measured by the BET method) of at least 40 mJ m 2 / g (preferably at least 55 mJ m 2 / g) (products of this type are referred to below as third pigments); - coated metal pigments or coated metal oxide pigments, (i) having a gassing stability score of ≥ 700 seconds (preferably ≥ 1000 seconds) in the "Test method for measuring the gassing stability of coated pigments" further described below, and (ii) having a gloss dispersion value (X) as defined above of ≤ 5.0 (this type of product is referred to below as the fourth pigment); - (i) having a gassing stability score of ≥ 700 seconds (preferably ≥ 1000 seconds) in the "Test method for measuring the gassing stability of coated pigments" further described below, and (ii) a lightness dispersion L as defined above of ≥ 90. A or L B coated metal pigments or coated metal oxide pigments having a value (this type of product is referred to below as the fifth pigment); - Coated PVD metal pigments or coated PVD metal oxide pigments having a chemical resistance score of 12 or less in the "Test method for determining the chemical resistance of coated pigments" further defined below (this type of product is referred to below as the sixth pigment); - coated PVD metal pigments or coated PVD metal oxide pigments, having a gassing stability score of ≥ 700 seconds (preferably ≥ 1000 seconds) in the "Test method for determining the gassing stability of coated pigments" further described below (this type of product is referred to below as the seventh pigment); and - A coated PVD metal pigment or a coated PVD metal oxide pigment having a gassing stability score of ≦5 ml after 21 days in the extended gassing test method further defined below in Example 41 (this type of product is referred to below as pigment no. 8).
[0063] Preferred aspects of the pigment in each of these embodiments are independently the same as those described above in relation to the substrate for use in the method of the present invention (when the substrate is a pigment). That is, the preferred choices for metals and metal oxides are the same as those set forth above for the substrate for use in the method of the present invention. Aluminum and copper oxide are particularly preferred, with aluminum being most preferred. Further preferred aspects for each of these embodiments are described below.
[0064] For each of the first and sixth pigments (independently), it is preferred that the pigment has a chemical resistance score of 11.5 or less, such as 11 or less, in the above test.
[0065] It is preferred that the second pigment have a chemical resistance score of 11 or less in the above test.
[0066] For each of the third, fourth, fifth, seventh and eighth pigments, it is preferred (independently) that the pigment has a chemical resistance score of 12 or less, more preferably 11.5 or less, such as 11 or less, in the "Test Method for Measuring Chemical Resistance of Coated Pigments" further defined below.
[0067] In some particularly preferred aspects for each of the first, second, third, fourth, fifth, sixth, seventh and eighth pigments, the chemical resistance score may be even lower, such as (independently) 10.5 or less, 10 or less, 9.5 or less, 9 or less, 8.5 or less, or 8 or less.
[0068] For each of the second, third, fifth, sixth, seventh and eighth pigments, it is preferred that (independently) the pigment has a gloss dispersion value (X), as defined above (relative to the first pigment), of ≦5.0.
[0069] For each of the first, second, third, fourth, fifth, sixth, seventh and eighth pigments, it is preferred (independently) that the gloss variance value (X) is ≦4.5 or less, such as ≦4.0 or ≦3.5. Typically, the gloss variance is a positive number because the gloss of the pigment is usually reduced when a coating is applied to the pigment, but there is no particular lower limit to the gloss variance value (X). Typical ranges for the gloss variance value are 0.1 to 5.0, such as 0.2 to 4.5, 0.3 to 4.0, 0.4 to 3.5 or 0.5 to 3.5.
[0070] For each of the first, third, fourth, sixth, seventh and eighth pigments, (independently) the lightness distribution L (relative to the second pigment) as defined above A Values of ≧90% are preferred.
[0071] For each of the first, second, third, fourth, fifth, sixth, seventh and eighth pigments, (independently) L A is particularly preferably ≧92%, such as ≧94%, ≧96%, ≧98%, ≧100%, ≧102%, ≧104% or ≧105%.
[0072] For each of the first, third, fourth, sixth, seventh and eighth pigments (independently), the lightness dispersion L B Values of ≧90% are preferred.
[0073] For each of the first, second, third, fourth, fifth, sixth, seventh and eighth pigments, (independently) LB is particularly preferably ≧92%, such as ≧94%, ≧96%, ≧98%, ≧100%, ≧102%, ≧104% or ≧105%.
[0074] That is, for each of the first, second, third, fourth, fifth, sixth, seventh and eighth pigments, (independently) L A and L B It is preferred that at least one (and typically both) of L is ≧90%, such as ≧92%, ≧94%, ≧96%, ≧98%, ≧100%, ≧102%, ≧104% or ≧105%. A and L B More preferably, none of the above is >150%. A and L B None of the above is >140%, and more preferably still L A and L B None of the above is >130%. A Typical ranges for are 90 to 140%, such as 92 to 135%, 94 to 130%, or 96 to 125%. B Typical ranges for L are 90 to 140%, such as 92 to 135%, 94 to 130%, or 96 to 125%. A and L B are both within the range of 90 to 140%, or 92 to 135%, or 94 to 130%, or 96 to 125%.
[0075] For each of the first, second, fourth, fifth, sixth, seventh, and eighth pigments (independently), an MIE* surface area, where MIE is the minimum ignition energy and surface area is the surface area measured by the BET method, of at least 40 mJ m 2 / g (preferably at least 55 mJ m 2 Pigments having a value of (1 / g) are preferred.
[0076] For each of the first, second, third, fourth, fifth, sixth, seventh, and eighth pigments, (independently) the pigment has an MIE* surface area of at least 50 mJ m, such as at least 60, at least 70, at least 80, at least 90, or at least 100. 2 In some aspects, the pigment preferably has a MIE* surface area of at least 110, or at least 120 mJ m 2 / g. Generally, the pigment has a MIE* surface area of at least 55 mJ m 2 It is preferred that the value of .beta. / g.
[0077] For each of the first, second, third, sixth and eighth pigments (independently), it is preferred that the pigment has a gassing stability score of ≧700 seconds (preferably ≧1000 seconds) in the "Test Method for Measuring Gassing Stability of Coated Pigments" further described below.
[0078] For each of the first, second, third, fourth, fifth, sixth, seventh and eighth pigments (independently), it is preferred that the pigment has a gassing stability score of ≧800 seconds, more preferably ≧900 seconds, and more preferably even ≧1000 seconds in the "Test Method for Measuring Gassing Stability of Coated Pigments" further described below. In some embodiments, it can be even higher, such as ≧1100, ≧1200, ≧1300, or ≧1400 seconds.
[0079] In certain embodiments, the present invention provides a composition having an MIE*surface area of ≥ 40 mJ m2, where MIE is the minimum ignition energy and surface area is the surface area measured by the BET method. 2 / g (preferably ≥ 50 mJ m, such as ≥ 60, ≥ 70, ≥ 80, ≥ 90, ≥ 100, ≥ 110, or ≥ 120) 2 / g), and the pigment has a gloss dispersion value (X) as defined above of ≦5.0 (preferably ≦4.5, such as ≦4.0 or ≦3.5). In this regard, the pigment has a MIE* surface area of at least 55 mJ m 2 It is generally preferred to have a value of / g.
[0080] In another embodiment, the present invention provides a composition having a MIE*surface area of ≥ 40 mJ m2, where MIE is the minimum ignition energy and surface area is the surface area measured by the BET method. 2 / g (preferably ≥ 50 mJ m, such as ≥ 60, ≥ 70, ≥ 80, ≥ 90, ≥ 100, ≥ 110, or ≥ 120) 2 / g), and the pigment has a lightness dispersion L as defined above of ≥ 90 A or L B value (L above) A and L B (further preferred options for also apply to this embodiment), the present invention provides a coated metal pigment or a coated metal oxide pigment, in which the pigment has an MIE* surface area of at least 55 mJ m 2 It is generally preferred to have a value of / g.
[0081] For all of the above inventive coated metal pigments and coated metal oxide pigments, the MIE is preferably ≧5 mJ, such as ≧6 mJ, ≧7 mJ, ≧8 mJ, ≧9 mJ, or ≧10 mJ.
[0082] For all of the above coated metal pigments and coated metal oxide pigments of the present invention, the surface area is preferably ≥ 2 m 2 / g or ≥ 3m 2 / g etc. ≧1m 2 / g. In some embodiments, it is ≧4m 2 / g or ≥ 5m 2 / g.
[0083] For all of the coated metal pigments and coated metal oxide pigments of the present invention described above, it is preferred that the pigments have a gassing stability score in the "Extended Gassing Test Method" described below in Example 41 of ≦5 ml after 21 days, more preferably ≦4 ml, more preferably still ≦3 ml, even more preferably ≦2 ml, and most preferably ≦1 ml after 21 days. Typically, it is 0 ml. This is especially the case for PVD pigments.
[0084] Surface modification of coated substrates The present invention provides a method comprising applying one or more surface modifiers to a coated substrate of the present invention as defined above. The present invention also provides a method comprising coating a substrate by a method of the present invention as defined above and subsequently applying one or more surface modifiers to the coated substrate.
[0085] Preferably, the one or more surface modifiers are: (a) both (i) an organophosphorus compound, and (ii) a compatibilizer having a molecular weight of 5000 or less, wherein the organophosphorus compound and the compatibilizer are applied simultaneously, separately or sequentially; (b) both (i) a fatty acid, and (ii) a compatibilizer having a molecular weight of 5000 or less, wherein the fatty acid and the compatibilizer are applied simultaneously, separately or sequentially; (c) both (i) an organofunctional network former, and (ii) an organophosphorus compound, wherein the organofunctional network former and the organophosphorus compound are applied simultaneously, separately, or sequentially. Includes.
[0086] In one preferred aspect, the one or more surface modifiers include both (i) an organophosphorus compound and (ii) a compatibilizer having a molecular weight of 5,000 or less, and wherein the organophosphorus compound and the compatibilizer are applied simultaneously, separately or sequentially.
[0087] In another preferred aspect, the one or more surface modifiers include both (i) a fatty acid, and (ii) a compatibilizer having a molecular weight of 5,000 or less, and wherein the organophosphorus compound and the compatibilizer are applied simultaneously, separately or sequentially.
[0088] In another preferred aspect, the one or more surface modifiers include both (i) an organofunctional network former, and (ii) an organophosphorus compound, and wherein the organofunctional network former and the organophosphorus compound are applied simultaneously, separately or sequentially.
[0089] The organophosphorus compound is preferably represented by formula (III): IXP(O)(OR 1 )(OR 2 ) (III) [In the formula, - R 1 and R 2 are each independently H, an optionally substituted hydrocarbyl, an optionally substituted amine, a polyether, an ammonium ion, an alkali metal, or an alkaline earth metal (preferably R 1 and R 2 is H), - X is divalent and is (a) a linear or branched hydrocarbon chain, wherein said hydrocarbon chain is optionally interrupted by one or more heteroatoms selected from O, S and N; (b) an optionally substituted carbocycle, wherein said ring is selected from cycloalkyl, cycloalkenyl, aryl and fused hydrocarbon groups; or (c) an optionally substituted heterocycle containing one or more heteroatoms selected from O, S and N (preferably X is C 4-14 alkylene); and - I is H or an initiator moiety for polymerization (preferably I is H)] It is a compound of the formula:
[0090] The compatibilizer preferably has a molecular weight of ≦5,000, such as ≦4,000, ≦3,000, ≦2,000, or ≦1,500. The compatibilizer preferably has a molecular weight of ≧200, such as ≧300, ≧400, or ≧500.
[0091] The compatibilizer is preferably an organic compound, more preferably a resin. More preferably, the compatibilizer is a melamine resin, an isocyanate resin, a polyurethane resin or an acrylic resin, most preferably a C 1-4 Alcohol-etherified melamine-formaldehyde resins (preferred choices for the alcohol in this embodiment are methanol, ethanol and propanol) or isophorone diisocyanate trimer resins. An example of a suitable commercially available compatibilizer is Luwipal® 072 available from BASF, Germany.
[0092] The fatty acid is preferably a compound of the formula RC(O)OH, where R is an aliphatic saturated or unsaturated hydrocarbon group. That is, R can be an alkyl, alkenyl or alkynyl group. Preferably, R is an alkyl or alkenyl group.
[0093] R is typically linear, but can be linear or branched.
[0094] Preferably, R has 3 to 29 carbons, i.e., the fatty acid is 4-30 More preferably, R has 3 to 27 carbon atoms, e.g., it is a linear C 3-27 Alkyl group or linear C 3-27 R is often a linear, saturated or unsaturated, aliphatic hydrocarbon group having 10 to 24 carbon atoms, such as a linear C 11-25 Alkyl group or linear C 11-25 An alkenyl group. The unsaturated aliphatic hydrocarbon group may contain multiple double bonds, such as 1 to 4 double bonds, for example 1 or 2 double bonds, and typically 1 double bond.
[0095] Examples of saturated fatty acids are butyric acid (C4), valeric acid (C5), caproic acid (C6), enanthic acid (C7), caprylic acid (C8), pelargonic acid (C9), capric acid (C10), undecylic acid (C11), lauric acid (C12), tridecylic acid (C13), myristic acid (C14), pentadecanoic acid (C15), palmitic acid (C16), These include margaric acid (C17), stearic acid (C18), nonadecylic acid (C19), arachidic acid (C20), henicosylic acid (C21), behenic acid (C22), tricosylic acid (C23), lignoceric acid (C24), pentacosylic acid (C25), cerotic acid (C26), heptacosylic acid (C27) and montanic acid (C28).
[0096] Examples of unsaturated fatty acids include α-linolenic acid (C18:3), stearidonic acid (C18:4), eicosapentaenoic acid (C20:5), docosahexaenoic acid (C22:6), linoleic acid (C18:2), γ-linolenic acid (C18:3), dihomo-γ-linolenic acid (C20:3), arachidonic acid (C20:4), adrenic acid (C22:4), palmitoleic acid (C16:1), vaccenic acid (C18:1), paulic acid (C20:1), oleic acid (C18:1), elaidic acid (C trans-18:1), gondonic acid (C20:1), erucic acid (C22:1), nervonic acid (C24:1) and mead acid (C20:3).
[0097] The notation CM:N fatty acids (where M and N are integers) used herein means that the fatty acid contains M carbon atoms and N double bonds. The two double bonds are usually not adjacent (i.e., attached to the same carbon atom), but the N double bonds can be in any position (cis or trans configuration). That is, C18:0 (or simply C18) covers only octadecanoic acid (stearic acid), and C18:1 includes all fatty acids with 18 carbons and one double bond, such as oleic acid ((Z)-octadec-9-enoic acid) and vaccenic acid ((E)-octadec-11-enoic acid).
[0098] Convenient fatty acids to use include stearic acid, oleic acid and vaccenic acid, and especially oleic acid. It may sometimes be convenient to use mixtures of fatty acids.
[0099] The organofunctional network former for use as a surface modifier is preferably defined in the same way as above in the context of the method of the present invention (i.e. the method of coating a substrate), i.e. preferably the organofunctional network former is a compound of formula (II) as defined above, in which the reactive organic group is preferably a hydrocarbyl group having one or more substituents selected from epoxy, amino, hydroxyl, thiol, acrylate, methacrylate, vinyl, allyl, alkenyl, alkynyl, carboxyl, carboxylic anhydride, isocyanate, cyanate, ureido and carbamate (amino being most preferred). That is, the organofunctional network former can be a compound selected from aminoalkyltrialkoxysilanes, N-(alkyl)-aminoalkyltrialkoxysilanes, N-aminoalkyl-aminoalkyl(alkyl)dialkoxysilanes, N-aminoalkyl-aminoalkyltrialkoxysilanes, epoxyalkyltrialkoxysilanes, mercaptoalkyltrialkoxysilanes, alkacryloxyalkyltrialkoxysilanes (e.g., methacryloxyalkyltrialkoxysilanes), and ureidoalkyltrialkoxysilanes (aminoalkyltrialkoxysilanes are most preferred). Preferably, the alkyl moieties are each independently selected from C 1-10 Alkyl, more preferably C 1-4 C such as alkyl 1-6 Preferably, the alkoxy moiety is selected from C 1-10 Alkoxy, more preferably C 1-4 Alkoxy etc. C 1-6 alkoxy (typically they are ethoxy or methoxy, most commonly ethoxy). And specific examples of suitable organofunctional network formers are: 3-Aminopropyltrimethoxysilane, 3-Aminopropyltriethoxysilane, N-(n-butyl)-3-aminopropyltrimethoxysilane, N-(n-butyl)-3-aminopropyltriethoxysilane, N-2-Aminoethyl-3-aminopropyl(methyl)dimethoxysilane, N-2-Aminoethyl-3-aminopropyl(methyl)diethoxysilane, N-2-Aminoethyl-3-aminopropyltrimethoxysilane, N-2-Aminoethyl-3-aminopropyltriethoxysilane, 3-Glycidyl Oxypropyltriethoxysilane, 3-glycidyloxypropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-ureidopropyltrimethoxysilane, and 3-ureidopropyltriethoxysilane (of which the amino-containing options are most preferred, especially 3-aminopropyltrimethoxysilane and 3-aminopropyltriethoxysilane) Includes.
[0100] The organophosphorus compound is preferably used in an amount of ≧0.01 wt.%, such as ≧0.04 wt.%, ≧0.08 wt.%, ≧0.1 wt.%, or ≧0.2 wt.%, based on the total weight of the coated pigment. The organophosphorus compound is preferably used in an amount of ≦15 wt.%, such as ≦10 wt.%, ≦5 wt.%, ≦4 wt.%, ≦3 wt.%, ≦2 wt.%, or ≦1 wt.%, based on the total weight of the coated pigment. That is, the preferred amount may be 0.1 to 10 wt.%.
[0101] The compatibilizer is preferably used in an amount of ≧0.01 wt.%, such as ≧0.04 wt.%, ≧0.08 wt.%, ≧0.1 wt.%, or ≧0.2 wt.%, based on the total weight of the coated pigment. The compatibilizer is preferably used in an amount of ≦15 wt.%, such as ≦10 wt.%, ≦5 wt.%, ≦4 wt.%, ≦3 wt.%, ≦2 wt.%, or ≦1 wt.%, based on the total weight of the coated pigment. That is, the preferred amount may be 0.1 to 10 wt.%.
[0102] The fatty acid is preferably used in an amount of ≧0.01 wt.%, such as ≧0.04 wt.%, ≧0.08 wt.%, ≧0.1 wt.%, or ≧0.2 wt.%, based on the total weight of the coated pigment. The fatty acid is preferably used in an amount of ≦15 wt.%, such as ≦10 wt.%, ≦5 wt.%, ≦4 wt.%, ≦3 wt.%, ≦2 wt.%, or ≦1 wt.%, based on the total weight of the coated pigment. That is, the preferred amount may be 0.1 to 10 wt.%.
[0103] The organofunctional network former (when used as a surface modifier) is preferably used in an amount of ≧0.01 wt.%, such as ≧0.04 wt.%, ≧0.08 wt.%, ≧0.1 wt.%, or ≧0.2 wt.%, based on the total weight of the coated pigment. The organofunctional network former is preferably used in an amount of ≦15 wt.%, such as ≦10 wt.%, ≦5 wt.%, ≦4 wt.%, ≦3 wt.%, ≦2 wt.%, or ≦1 wt.%, based on the total weight of the coated pigment. That is, the preferred amount may be 0.1 to 10 wt.%.
[0104] The weight ratio of the organophosphorus compound to the compatibilizer (in an aspect where both are used in combination) is preferably from 10:1 to 1:10, such as from 5:1 to 1:5, 3:1 to 1:3, or 2:1 to 1:2.
[0105] The weight ratio of fatty acid to compatibilizer (in an aspect where both are used in combination) is preferably from 10:1 to 1:10, such as from 5:1 to 1:5, 5:1 to 1:3, or 4:1 to 1:2.
[0106] The weight ratio of organofunctional network former to organophosphorus compound (in an aspect where both are used in combination) is preferably from 10:1 to 1:10, such as from 5:1 to 1:5, 3:1 to 1:3, or 2:1 to 1:2.
[0107] In one aspect of the invention, when an organophosphorus compound and a compatibilizer are applied, the method includes the steps of applying the organophosphorus compound to the pigment and then applying the compatibilizer to the pigment, but more typically, when an organophosphorus compound and a compatibilizer are applied, the method includes the steps of applying the compatibilizer to the pigment and then applying the organophosphorus compound to the pigment.
[0108] In one aspect of the invention, when a fatty acid and a compatibilizer are applied, the method includes the steps of applying the fatty acid to the pigment and then applying the compatibilizer to the pigment, however, more typically, when a fatty acid and a compatibilizer are applied, the method includes the steps of applying the compatibilizer to the pigment and then applying the fatty acid to the pigment.
[0109] In one aspect of the invention, when an organofunctional network former and an organophosphorus compound are applied, the method includes the steps of applying the organophosphorus compound to the pigment and then applying the organofunctional network former to the pigment, however, more typically, when an organofunctional network former and an organophosphorus compound are applied, the method includes the steps of applying the organofunctional network former to the pigment and then applying the organophosphorus compound to the pigment.
[0110] When applying the organic phosphorus compound to the coated substrate, a basic catalyst can be preferably used. The preferred basic catalysts are EDA, MEA and NMI. Such agents can be used directly or mixed with a solvent.
[0111] When applying fatty acid to coated substrate, a basic catalyst may be preferably used. Preferred basic catalysts are EDA, MEA and NMI. Such agents may be used directly or mixed with a solvent.
[0112] When the compatibilizer is applied to the coated substrate, a basic catalyst may be preferably used. Preferred basic catalysts are EDA, MEA and NMI. Such agents may be used directly or mixed with a solvent.
[0113] When applying the organic functional network former to the coated substrate, a basic catalyst may be preferably used. Preferred basic catalysts are EDA, MEA and NMI. Such agents may be used directly or mixed with a solvent.
[0114] It has been found that the use of a combination of an organophosphorus compound and a compatibilizer as defined above as a surface modifier for pigments, particularly coated pigments, offers surprising advantages in terms of the pigment's ability to withstand shear effects when used in polymer powder applications. It is believed that the use of a combination of a fatty acid and a compatibilizer as defined above as a surface modifier for pigments, particularly coated pigments, offers similar advantages as the combination of an organofunctional network former and an organophosphorus compound. Furthermore, it has been found that the use of a combination of (a) an organophosphorus compound and a compatibilizer as defined above, (b) a fatty acid and a compatibilizer as defined above, or (c) an organofunctional network former and an organophosphorus compound as a surface modifier for pigments, particularly coated pigments, offers surprising advantages in terms of the pigment's ability to avoid gassing in water-based applications. It is believed that these advantages occur with pigments in general and are not limited to the coated pigments of the present invention as defined herein. Thus, as stated above: - in one embodiment, the present invention provides a method of treating a pigment (any pigment, but preferably a coated pigment such as the coated pigment of the present invention), comprising simultaneously, separately or sequentially applying to the pigment one or more surface modifiers, wherein said one or more surface modifiers comprise an organophosphorus compound and a compatibilizer as defined above, and wherein a majority of the compatibilizer does not become covalently bonded to the pigment; In another embodiment, the present invention provides a method for treating a pigment (any pigment, but preferably a coated pigment, such as the coated pigment of the present invention), comprising simultaneously, separately or sequentially applying one or more surface modifiers to the pigment, wherein said one or more surface modifiers comprise a fatty acid and a compatibilizer as defined above, and wherein a majority of the compatibilizer does not become covalently bonded to the pigment; and In another embodiment, the present invention provides a method for treating a pigment (any pigment, but preferably a coated pigment such as the coated pigment of the present invention) comprising simultaneously, separately or sequentially applying one or more surface modifiers to the pigment, wherein said one or more surface modifiers comprise an organofunctional network former and an organophosphorus compound.
[0115] The preferred aspects of the surface modification of the present invention defined above apply equally to each of these three embodiments (independently).
[0116] In a further embodiment, the present invention provides a pigment (preferably a coated pigment of the present invention) having on its surface an organophosphorus compound and a compatibilizer as defined above, wherein a majority of the compatibilizer is not covalently bonded to the pigment. The preferred aspects of the surface modification of the present invention defined above apply equally to this embodiment.
[0117] In a further embodiment, the present invention provides a pigment (preferably a coated pigment of the present invention) having on its surface a fatty acid and a compatibilizer as defined above, wherein a majority of the compatibilizer is not covalently bonded to the pigment. The preferred aspects of the surface modification of the present invention defined above apply equally to this embodiment.
[0118] In a further embodiment, the present invention provides a pigment (preferably a coated pigment of the present invention) having on its surface an organofunctional network former and an organophosphorus compound as defined above. The preferred aspects of the surface modification of the present invention defined above apply equally to this embodiment.
[0119] Application and Use of Coated Pigments In view of their beneficial properties, the coated pigments of the present invention can be used for a wide range of purposes: they can be incorporated into products such as varnishes, automotive finishes, paints, printing inks, powder coating materials, architectural paints, plastics, security printing inks, ceramics, glass or cosmetics. In one preferred embodiment, the present invention provides a powder coating material comprising the coated pigment of the present invention as defined herein and further comprising a polymer.
[0120] In another preferred embodiment, the present invention provides an aqueous coating composition (such as a paint) comprising the coated pigment of the present invention as defined herein. Particularly preferred pigments in the context of this embodiment include those in which (a) the pigment has an organofunctional network former and an organophosphorus compound on its surface, and / or (b) the pigment is obtained or obtainable by a process comprising applying one or more surface modifiers to the pigment simultaneously, separately or successively, wherein said one or more surface modifiers comprise an organofunctional network former and an organophosphorus compound. A preferred aspect of the present invention described above in the section entitled "Surface modification of the coated substrate" applies equally to both cases (a) and (b). It may also be noted that in both cases (a) and (b), the pigment is preferably a coated pigment of the present invention, i.e. a pigment as defined above in the section entitled "Coated substrate". That is, in this embodiment, the pigment is preferably obtainable by a process comprising coating a pigment substrate and then applying one or more surface modifiers to the (so obtained) coated pigment substrate, wherein - a method of coating a pigment substrate comprising a step (a) of subjecting an inorganic network former and an organofunctional network former to a condensation type reaction, and thereafter (b) one or more further steps of subjecting an inorganic network former and an organofunctional network former to a condensation type reaction, and applying one or more surface modifiers to the (so obtained) coated pigment substrate, wherein said one or more surface modifiers comprise both (i) an organofunctional network former, and (ii) an organophosphorus compound.
[0121] The coated pigments of the present invention may be advantageously used in the form of a powder coating material. That is, the present invention provides a method of coating an article, comprising electrostatically applying to the article a powder coating material comprising the coated pigments of the present invention (and optionally a polymer) as defined herein, and, optionally, curing the applied coating material. The article could be an automobile.
[0122] The present invention also provides a coated article comprising the inventive coated substrate as defined herein. EXAMPLES
[0123] Examples 1 to 9 - Preparation of Coated Substrates The following examples provide details regarding the preparation of particular coated pigments of the present invention.
[0124] Example 1 Two Layers (First Epoxy Functionalized, Second Epoxy Functionalized) Reactants: Initial supply: 0.1 kg of Al flakes in paste form, d between 10 and 15 μm 50 (Amount refers to non-volatile content) First layer applied: 0.1 kg Tetraethylsilicate (TEOS) 3g of epoxy alkyl trialkoxy silane Second layer application: 0.1kg TEOS 5g of epoxy alkyl trialkoxy silane Surface treatment part A: 1g alcohol-etherified melamine-formaldehyde resin in isobutanol (amount refers to the amount of resin) Surface treatment part B: 2g of octylphosphonic acid diluted in IPA process:
[0125] [Table 1]
[0126] Example 2 Two Layers (First Amino-Functionalized, Second Epoxy-Functionalized) Reactants: The coated pigment was prepared in the same manner as in Example 1, using 2 g of N-aminoalkyl-aminoalkyltrialkoxysilane instead of 3 g of epoxyalkyltrialkoxysilane in the first layer application. The filtrate in step 8 was yellow and clear, pH 8-9. The product yield was 158 g.
[0127] Example 3 Two Layers (First Epoxy Functionalized, Second Epoxy Functionalized) Reactants: Initial supply: 0.1 kg of Al flakes in paste form, d between 10 and 15 μm 50 (Amount refers to non-volatile content) First layer applied: 0.1 kg Tetraethylsilicate (TEOS) 3g of epoxy alkyl trialkoxy silane Second layer application: 0.1kg TEOS 6g of epoxy alkyl trialkoxy silane Surface treatment part A: 1g alcohol-etherified melamine-formaldehyde resin in isobutanol (amount refers to the amount of resin) Surface treatment part B: 3 g of octylphosphonic acid diluted in 1-methoxy-2-propanol (80% solution in water) (amount refers to the amount of octylphosphonic acid in water) process:
[0128] [Table 2]
[0129] Example 4 Three Layers (1st, 2nd and 3rd Epoxy Functionalization) Reactants: Initial supply: 0.1 kg of Al flakes in paste form, d between 10 and 15 μm 50 (Amount refers to non-volatile content) First layer applied: 0.1 kg Tetraethylsilicate (TEOS) 2g of epoxy alkyl trialkoxy silane Second layer application: 0.1kg TEOS 3g of epoxy alkyl trialkoxy silane Third layer application: 0.03kg TEOS 5g of epoxy alkyl trialkoxy silane Surface treatment part A: 1g alcohol-etherified melamine-formaldehyde resin in isobutanol (amount refers to the amount of resin) Surface treatment part B: 3g of octylphosphonic acid diluted in IPA (80% solution in water) (amount refers to the amount of octylphosphonic acid in water) process:
[0130] [Table 3]
[0131] Example 5 Three Layers (1st, 2nd and 3rd Epoxy Functionalization) Reactants: Initial supply: 0.1 kg of Al flakes in paste form, d between 10 and 15 μm 50 (Amount refers to non-volatile content) First layer applied: 0.1 kg Tetraethylsilicate (TEOS) 2g of epoxy alkyl trialkoxy silane Second layer application: 0.1kg TEOS 3g of epoxy alkyl trialkoxy silane Third layer application: 0.03kg TEOS 5g of epoxy alkyl trialkoxy silane Surface treatment part A: 1g alcohol-etherified melamine-formaldehyde resin in isobutanol (amount refers to the amount of resin) Surface treatment part B: 3 g of octylphosphonic acid diluted in 1-methoxy-2-propanol (80% solution in water) (amount refers to the amount of octylphosphonic acid in water) process:
[0132] [Table 4]
[0133] Example 6 One Layer (Epoxy Functionalized) [Comparative Example] Reactants: Initial supply: 0.1 kg of Al flakes in paste form, d between 10 and 15 μm 50 (Amount refers to non-volatile content) First (only) layer application: 0.2 kg Tetraethyl Silicate (TEOS) 9g of epoxy alkyl trialkoxy silane Surface treatment part A: 1g alcohol-etherified melamine-formaldehyde resin in isobutanol (amount refers to the amount of resin) Surface treatment part B: 3 g of octylphosphonic acid diluted in 1-methoxy-2-propanol (80% solution in water) (amount refers to the amount of octylphosphonic acid in water) process:
[0134] [Table 5]
[0135] Example 7 Two Layers (First Epoxy Functionalized, Second Epoxy Functionalized) Reactants: Initial supply: 0.1 kg of Al flakes in paste form, d between 10 and 15 μm 50 (Amount refers to non-volatile content) First layer applied: 0.1 kg Tetraethylsilicate (TEOS) 4g of epoxy alkyl trialkoxy silane Second layer application: 0.1kg TEOS 5g of epoxy alkyl trialkoxy silane Surface treatment part A: 1g alcohol-etherified melamine-formaldehyde resin in isobutanol (amount refers to the amount of resin) Surface treatment part B: 3 g of octylphosphonic acid diluted in 1-methoxy-2-propanol (80% solution in water) (amount refers to the amount of octylphosphonic acid in water) process:
[0136] [Table 6]
[0137] Example 8 Three Layers (1st, 2nd and 3rd Epoxy Functionalization) Reactants: Initial supply: 0.1 kg of Al flakes in paste form, d between 10 and 15 μm 50 (Amount refers to non-volatile content) First layer applied: 0.1 kg Tetraethylsilicate (TEOS) 2g of epoxy alkyl trialkoxy silane Second layer application: 0.1kg TEOS 3g of epoxy alkyl trialkoxy silane Third layer application: 0.03kg TEOS 5g of epoxy alkyl trialkoxy silane Surface treatment part A: 1g alcohol-etherified melamine-formaldehyde resin in isobutanol (amount refers to the amount of resin) Surface treatment part B: 3 g of octylphosphonic acid diluted in 1-methoxy-2-propanol (80% solution in water) (amount refers to the amount of octylphosphonic acid in water) process:
[0138] [Table 7]
[0139] Example 9 Three Layers (1st, 2nd and 3rd Epoxy Functionalization) Reactants: Initial supply: 0.1 kg of Al flakes in paste form, d between 10 and 15 μm 50 (Amount refers to non-volatile content) First layer applied: 0.1 kg Tetraethylsilicate (TEOS) 2g of epoxy alkyl trialkoxy silane Second layer application: 0.1kg TEOS 3g of epoxy alkyl trialkoxy silane Third layer application: 0.03kg TEOS 5g of epoxy alkyl trialkoxy silane Surface treatment part A: 1g alcohol-etherified melamine-formaldehyde resin in isobutanol (amount refers to the amount of resin) Surface treatment part B: 3 g of octylphosphonic acid diluted in 1-methoxy-2-propanol (80% solution in water) (amount refers to the amount of octylphosphonic acid in water) process:
[0140] [Table 8]
[0141] Examples 10 to 40 - Application and Evaluation of Coated Pigments The following section describes how the coated pigments of the present invention can be formulated into a powder coating and then applied to an article.
[0142] Determining the Chemical Resistance of Coated Pigments The basic method is to blend powder pigments with powder coatings, apply them to a surface with a spray gun, then apply drops of acid and base for different periods of time and evaluate their effect. A more detailed description of the method is as follows:
[0143] Test methods for determining the chemical resistance of coated pigments The chemical resistance score may be determined by the following method: (a) The coated pigment is charged directly into a mixing vessel along with a polyester powder, where the coated pigment has an average particle size (d 50) ≧20 microns, then 188 g of polymer powder was used with 12 g of coated pigment, and the coated pigment had an average particle size (d 50 )<20 microns, then use 192g of polymer powder with 8g of coated pigment; (b) if all of the coated pigment is not below the level of the mixing tool in the mixing vessel, shaking the mixing vessel to bring all of the coated pigment below the level of the mixing tool; (c) blending the polyester powder and the coated pigment for 2*30 seconds at ambient temperature (preferred equipment is a Thermomix™ 3300, company Vorwerk, mixing is carried out at blender level 1); (d) transferring the resulting powder preparation into a plastic bag; (e) The powder preparation was sprayed using an electrostatic spray gun with a circular metal nozzle and a 30 mm deflector (a suitable spray gun is Typ: WX-101 TC) with the following parameters: Powder hose connection: 2 bar Purge airf connection: 0.5kg / cm 2 Material flow controller: 50% Voltage: 70kV Gun panel distance: 30 cm onto a steel panel (a suitable panel is 10*15cm panel, Type D-46, available from Q-Lab); wherein the amount of formulation applied is sufficient to provide a thickness of 50 to 75 microns after the following curing step (f). (and here, if spitting and / or caking occurs with the spray gun then the test is abandoned and started over);
[0144] (f) curing the thus applied preparation using a baking time of 160°C for 8 minutes; (g) keeping the resulting sample at ambient temperature for at least 24 hours; (h) placing the sample horizontally on a magnetic pad and placing 15 to 17 mm drops thereon of the following solutions: (i) a 10 wt % aqueous solution of hydrochloric acid, (ii) a 1 M aqueous solution of sodium hydroxide, and (iii) a 10 wt % aqueous solution of sodium hydroxide (NaOH), whereby the drops are placed in a time sequence such that all drops can be removed simultaneously after 240 minutes, and for each solution the panel is exposed for 1 drop 30 minutes, 1 drop 60 minutes, 1 drop 120 minutes, 1 drop 180 minutes, and 1 drop 240 minutes; (i) all drops are simultaneously removed from the sample by rinsing with water; (j) Each of the 15 drop regions was visually assessed for the degree of greying according to the following scheme: 0 no attack 0.5 Only slight changes are visible at certain angles 1 Slight graying 2 Graying, pigmentation still visible) 3 Complete graying, no visible pigmentation) Assign a score from 0 to 3 based on (k) The scores for each drop region are then summed to provide a total score from 0 to 45.
[0145] Steps (a) to (g) can also be carried out using uncoated pigments in connection with the measurement of the lightness loss value defined herein. Polyester powder is not particularly limited in this context, since its purpose is only to act as a carrier for coated pigments. Convenient polyester powders to use are those that do not contain triglycidyl isocyanurate (TGIC), are suitable for producing glossy paint films, and / or have high flow coating properties (e.g. FA-9005-GL412 powder available from Ganzlin Beschichtungspulver GmbH).
[0146] Test Method for Measuring the Gloss of Coated Pigments The gloss may be measured by preparing a sample containing the coated or uncoated pigment according to steps (a) to (g) of the "Test method for measuring the chemical resistance of coated pigments" described in the description, and then measuring the gloss at 60° using a gloss meter. An example of a suitable gloss meter is the Rhopoint Instruments Novo-Gloss 60° gloss meter.
[0147] Test Method for Measuring the Lightness of Coated Pigments The color values at 15° and -15° can be measured by preparing samples containing coated or uncoated pigments according to steps (a) to (g) of the "Test method for determining the chemical resistance of coated pigments" described in the description, and then using a spectrophotometer. An example of a suitable spectrophotometer is the BYK-mac i 23mm spectrophotometer.
[0148] Test Method for Measuring the Minimum Ignition Energy (MIE) of Coated Pigments The MIE provides a measure of the minimum energy of an electric spark that will result in ignition of a cloud of particulate matter under specified test conditions. To measure the MIE, particulate matter is dispersed in an explosion chamber to form a cloud, and a spark of known energy is passed through the cloud. By varying the particle concentration, the level of turbulence, and the spark energy, the lowest energy that can ignite the cloud can be determined. The MIE is preferably measured in accordance with BS ISO / IEC 80079-20-2.
[0149] Test Method for Measuring Surface Area of Coated Pigments As used herein, references to surface area are intended to refer to the surface area as determined by the BET method. Such surface area may be measured in accordance with ASTM B922-17.
[0150] Examples 10 to 26 - Chemical resistance and optical properties of coated pigments Various pigments were tested according to the test methods described above, with the results set forth in the following table. Examples 10 to 21 are of the present invention. The samples tested for these examples were each prepared using either (i) one of the coated pigments described in one of the examples above, or (ii) an alternative coated pigment prepared in a similar manner using different reagents (the differences are noted in the table). Example 22 was the corresponding pigment that lacked any coating at all, and was included as a comparative example. Examples 23 to 26 included coated pigments where the coating was not done using the process of the present invention - again, the differences are noted in the table.
[0151] [Table 9]
[0152] From the results in the above table, it can be seen that the examples of the present invention enjoy an excellent combination of high chemical resistance and good optical properties. Also, a comparison of the chemical resistance scores of Examples 16 and 19 reveals that the use of an organophosphorus compound (in combination with a compatibilizer) for surface modification has the effect of enhancing the pigment's ability to withstand shear effects when used in polymer powder applications.
[0153] Examples 27 to 30 - Comparison with commercial products To further illustrate the invention and also to demonstrate the differences between the coatings of the invention and those used in the art, two coated pigments of the invention were compared to two major commercially available coated pigments. The pigments were subjected to a chemical resistance test using a modified version of the above-mentioned "Test Method for Measuring Chemical Resistance of Coated Pigments" where a different polymer powder was used, namely Alesta AP RAL 9005 HAA commercially available from Axalta Coatings, for the polyesters specified, and where only two solutions were used in step (h), namely solutions (iv) (5% aqueous NaOH) and (v) (20% aqueous HCl), and where drops of solution were left on the samples for periods of 1, 2, 3 and 24 hours (instead of the periods stated in step (h)). Images of the samples after testing are reproduced in Figures 1 and 2. The samples were all prepared and tested in the same way using different coated pigments - so that the coated pigments used in each sample were as follows: A sample labeled "35-1" was prepared using the coated pigment of Example 1 (this sample will hereafter be referred to as Example 27); A sample labeled "35-2" was prepared using the coated pigment of Example 2 (this sample will hereafter be referred to as Example 28); A sample labeled "PCU1000" was prepared using the commercial product PCU 1000 Aluminium Powder sold by Eckart, which is described as the best Al pigment product on the market in terms of chemical resistance (albeit at the expense of some of its optical properties) and is believed to feature an inner inorganic coating derived from TEOS and an outer organic coating based on acrylates (this sample is hereafter referred to as Example 29 and is a comparative example); and The sample labeled "POWDAL 8500" was prepared using POWDAL 8500, a commercially available coated Al pigment product sold by Schlenk that is believed to be primarily based on SiO2 (this sample is hereafter referred to as Example 30 and is a comparative example).
[0154] In all four of the samples shown in Figures 1 and 2, the placement of the drops was the same as shown for the samples containing POWDAL 8500, i.e., the sodium hydroxide drop was placed on the left side of each sample and the hydrochloric acid drop was placed on the right. The coated pigments in each case were of comparable particle size - as shown in the images, the coated pigments had particle sizes (d 50 It may also be noted that the
[0155] In terms of results, the images for Examples 29 and 30 (in Figure 2) show that, as expected, the samples prepared using the PCU 1000 product are superior to the samples prepared using POWDAL 8500 in terms of chemical resistance in the presence of both acid and base, but also have a poorer optical appearance in terms of image brightness and clarity. However, the two samples prepared using the coated pigments of the present invention in Examples 27 and 28 (in Figure 1) perform significantly better than either of the samples prepared using the commercial products, and despite this, they also have a superior optical appearance comparable to that of the samples prepared using POWDAL 8500.
[0156] Examples 31 to 34 - Further comparison with commercial products To further illustrate the invention and also to demonstrate the differences between the coated pigment of Example 1 and the commercially available coated pigment PCU 1000 (discussed in Example 29 above), both coated pigments were compared in three different tests, each of which was a modified version of the above-mentioned "Test method for measuring the chemical resistance of coated pigments" using a clear coat polymer powder, namely polyester powder AR-0134-GL440 021 Transparent, PT 910 available from Ganzlin Beschichtungspulver GmbH. Images of the samples after testing are reproduced in Figures 4 and 5. In each individual figure, two adjacent samples were prepared in the same way and differed only in the coated pigment used. The method used to prepare the samples in Figures 4 and 5 differed in whether significant shear was applied, with the sample in Figure 4 being blended / mixed without the use of a blender device (i.e. no significant shear was applied), while the sample in Figure 5 was blended / mixed in a blender device (i.e. significant shear was applied). Samples prepared using the coated pigment of Example 1 appear on the left side of each of Figures 4 and 5 and are hereafter referred to as Examples 31 and 33, respectively. Samples prepared using the coated pigment PCU 1000 appear on the right side of each of Figures 4 and 5 and are hereafter referred to as Examples 32 and 34, respectively (these are comparative examples).
[0157] In the samples shown in Figures 4 and 5, the drop arrangement was the same as that shown in Figure 3. It may also be noted that the coated pigments in each case were of comparable particle size (as previously reported in Examples 27 to 30 above).
[0158] Consistent with the results seen in Examples 27 through 30, the samples of Examples 31 and 33 (prepared using the coated pigment of Example 1) are seen to be consistently equal to or better than the samples of Examples 32 and 34 (prepared using commercial PCU 1000) in terms of chemical resistance (superior results for each of the samples are seen in the early stages of testing using 1M sodium hydroxide (NaOH)), but also have superior optical appearance in terms of image brightness and clarity.
[0159] Examples 35 and 36 - Further comparison with commercial products To further illustrate the invention and also to demonstrate the differences between the coated pigment of the invention and the commercial coated pigment PCU 1000 (discussed in Example 29 above), both coated pigments were compared in further tests carried out according to the above "Test method for measuring the chemical resistance of coated pigments" and images of the samples after testing are reproduced in Figure 3. The two samples in Figure 3 were prepared in the same way and only differed in the coated pigment used. An example of the invention (hereinafter referred to as Example 35) was prepared using the coated pigment of Example 1. A comparative example (hereinafter referred to as Example 36) was prepared using a pigment coated with PCU 1000.
[0160] Consistent with the results seen in Examples 27 through 34, the sample of Example 35 is seen to perform significantly better in terms of chemical resistance than the sample of Example 36. The sample of Example 35 is also seen to have superior optical appearance as evidenced by the brightness and clarity of the image.
[0161] Examples 37 and 38 - Further comparison with commercial products Corresponding drawdown samples were prepared using liquid coatings made by dispersing 0.5 g of pigment in 9.5 g of water-based paint (available from Plantag Coatings under product number 74254.X) using a magnetic stirrer, using (i) the coated pigment of Example 1 as the pigment (this is the sample labeled MA35-13 74524.X in FIG. 6, hereafter referred to as Example 37), and (ii) the commercially available coated pigment PCU 1000 discussed in Example 29 above (this is the sample labeled PCU1000 WC, hereafter referred to as Example 38). The samples differed only in the identity of the coated pigment.
[0162] Consistent with the results seen in Examples 27 through 36, the sample of Example 37 is seen to perform significantly better in terms of chemical resistance than the sample of Example 38. The sample of Example 37 is also seen to have superior optical appearance as evidenced by the brightness and clarity of the image.
[0163] Examples 39 and 40 - Minimum Ignition Energy (MIE) Testing First, as Example 39, the coated pigment of Example 15 above was subjected to MIE testing. Second, as Example 40, MIE was performed by applying the coating in the same manner as in Example 15 above, but with a different Al-based flake, i.e., a d of about 10 μm. 50 Both coated pigments were tested using a 7m 2 The MIE was measured according to BS ISO / IEC 80079-20-2.
[0164] The coated pigments of Examples 39 and 40 were both found to have an MIE between 10 and 20 mJ. This is comparable to, for example, the commercially available coated pigment PCU 1000 (d 50= 15 μm, MIE reported as > 3 and < 10 mJ) and PCUplus 800 (d 50 = 8 μm, MIE reported as > 1 but < 3 mJ).
[0165] Example 41 - Gasification stability Examples 41A to 41C - Determination of gassing stability of coated pigments in an accelerated gassing test method Metal pigments can react with water to produce hydrogen. For example, Al pigments can react with water according to the formula 2Al+6H2O→2Al(OH)3+3H2. The reaction proceeds faster in acidic or alkaline solutions. The degree of H2 generation can be used to measure the gasification stability of the coated pigment. In this regard, an accelerated gasification method can be used, the details of which follow below.
[0166] Test method for determining the gasification stability of coated pigments (a) 0.5 g of pasty pigment was weighed into a 250 ml Erlenmeyer flask (the amount refers to the non-volatile content); (b) Measure out 10 ml of butyl glycol and add it to the paste; (c) Place a magnetic stir bar in the flask and place it in a 29°C water bath; (d) stirring the mixture at 250 rpm until completely dispersed and monitoring the temperature of the dispersion with an electronic thermometer probe; (e) once the mixture is completely dispersed and equilibrated at 29°C, add 50 ml of sodium hydroxide / butyl glycol solution preheated to 29°C using a measuring cylinder to the dispersion (to prepare the sodium hydroxide / butyl glycol solution, weigh 5.00 g of sodium hydroxide into a 1 liter flask, add 500 g of deionized water, then add 5.00 g of butyl glycol, then add an additional 490 g of deionized water, then stir until completely dissolved); (f) take a bubble counter filled with 30 ml of water, (quickly) attach the head of the bubble counter to the flask, and simultaneously start an electronic timer; and (g) Once all of the water has been displaced from the lower chamber of the bubble counter, stop the timer.
[0167] The reaction flask should be washed with a small amount of 1 molar hydrochloric acid before reuse to remove any deposits that may form during the reaction (residue on the glass can affect future results).
[0168] Example 41A Reactants: Initial supply: 140 g aluminum paste, 70% in mineral spirits (98 g solids), d 50 8~20μm First layer application: 30g Tetraethyl Silicate (TEOS) 0.2g 3-glycidyloxypropyltrimethoxysilane Second layer applied: 15g TEOS 0.5g 3-glycidyloxypropyltrimethoxysilane Surface treatment part A: 0.8 g alcohol-etherified melamine-formaldehyde resin in isobutanol (amount refers to amount of resin) Surface treatment part B: 2.7g oleic acid process:
[0169] [Table 10]
[0170] Example 41B The coated pigment was prepared in the same manner as in Example 41A, using 2.0 g of octylphosphonic acid as surface treatment part B. The filtrate in step 6 was yellow and clear, pH 8-9. The product yield was 158 g.
[0171] Example 41C The coated pigment was prepared in the same manner as in Example 41A, using 1.0 g of 3-aminopropyltriethoxysilane as surface treatment part A and 2.0 g of octylphosphonic acid as surface treatment part B. The filtrate in step 6 was yellow and clear, pH 8-9. The product yield was 153 g.
[0172] The samples of Examples 41A through 41C were tested according to the "Test Method for Measuring Gassing Stability of Coated Pigments" procedure outlined above. A commercially available coated pigment product sold by Eckart under the name Hydrolan 2156 was also tested (for comparison). The time for the sample to produce 30 ml of hydrogen was recorded. Accelerated gasification test results:
[0173] [Table 11]
[0174] Examples 41D and 41E - Determination of gassing stability of coated pigments in an extended gassing test method The coated pigments may also be tested according to an extended gasification test method, including the steps described below, and using the apparatus shown in FIG. 7 (for the avoidance of doubt, the test described below is not the "Test Method for Measuring the Gasification Stability of Coated Pigments" referenced elsewhere in this specification):
[0175] Extended Gasification Test Method 10.0 g of pigment is added to 10.0 g of a 1:1 mixture of propylene glycol methyl ether / 1-methoxy-2-propanol (commercially available as Dowanol PM) and propylene glycol n-butyl ether (commercially available as Dowanol PnB) in a 400 ml beaker using a palette knife to create a smooth, creamy dispersion without any lumps (butyl glycol can be used as a possible alternative to the combination of the two mentioned ethers). To the resulting mixture, add 200 g of a solution that can be made by (i) mixing 3 parts of an acrylic emulsion (commercially available as Joncryl 537 resin dispersion) in 1 part of distilled water in a beaker, and (ii) stirring rapidly using a mechanical paddle stirrer. The resulting mixture is then stirred for 10 minutes using a magnetic stirrer. 200 g of the resulting mixture is then added to a 200 ml cylindrical flask, making sure that no paint is attached to the neck joint [where it leads to the Ledde head (the Ledde head can be prepared by transferring water to the lower chamber through the central glass tube in the upper chamber using a pipette, the water level in the lower chamber is just below the neck of the tube)]. The cap of the Ledde head is then replaced and loosely closed. The Ledde head and (filled) cylindrical flask are then placed in an oven preset at 52° C. (It is preferable to use a separate oven, ideally an incubator oven). The temperature is then allowed to stabilize - a stable temperature is 2 hours if the paint is in an incubator oven, or 3 hours if the paint is in a convection oven). At this 2 (or 3) hour re-zero point, the Ledde head is removed from the oven (close the oven door after removal to minimize heat loss) and some silicone-based grease is applied to the tapered base. The (second) oven door is then opened and the Ledde head is connected to the cylindrical flask by gently twisting the handle (note that water moves from the lower chamber up the central tube towards / into the upper chamber, indicating a good seal between the two). The Quick Fit Joint Clamp is then applied.The top screw cap is then tightened and then loosened 1 / 4 turn to allow for slight ventilation. The oven door is then closed and the temperature is allowed to stabilise for a further 10 minutes. After this, the door is quickly opened, the gas rig is removed and any displaced water in the upper chamber of the Ledde head is pipetted out. The cap is then replaced (loosely) and the rig is placed back into the oven from which gas evolution is measured. Visual inspection can be carried out through the inner glass door of the incubator without disturbing the temperature of the paint. The final gas evolution can be measured by loosening the Ledde head cap and pipetting the displaced water from the upper chamber into a pre-tared beaker. The weight of the water removed is expressed in ml.
[0176] Examples 41D and 41E - Determination of gassing stability of coated PVD pigments in an extended gassing test method Example 41D Reactants: Initial supply: 170.0 g aluminum paste, 10% in 1-methoxy-2-propanol (17 g solids), d 50 6~15μm First layer applied: 6.0 g tetraethyl silicate (TEOS) 0.2g 3-glycidyloxypropyltrimethoxysilane Second layer applied: 3g TEOS 0.4g 3-glycidyloxypropyltrimethoxysilane Surface treatment part A: 0.7 g alcohol-etherified melamine-formaldehyde resin in isobutanol (amount refers to amount of resin) Surface treatment part B: 0.8 g octylphosphonic acid process:
[0177] [Table 12]
[0178] Example 41E The coated pigment was prepared in the same manner as in Example 41D, using 0.4g of 3-aminopropyltriethoxysilane as surface treatment part A. The filtrate in step 6 was yellow and clear, pH 8-9. The yield of the product was 180g.
[0179] The samples of Examples 41D and 41E were tested according to the Extended Gasification Test Procedure outlined above. A commercially available coated pigment product sold by Eckart under the trade name HYDROSHINE WS3003 was also tested (for comparison). The results after 5 and 21 days are listed below.
[0180] [Table 13]
Claims
1. 1. A method of coating a substrate, comprising the steps of: (a) subjecting an inorganic network former and an organofunctional network former to a condensation type reaction; And afterwards: (b) one or more further steps in which the inorganic network former and the organofunctional network former are subjected to a condensation type reaction. Including, Where: the substrate is a metallic pigment, - the inorganic network former in each of steps (a) and (b) is independently a tetraalkoxysilane; - the organofunctional network former in step (a) is an epoxyalkyltrialkoxysilane or an aminosilane, and - the organofunctional network former in step (b) is an epoxyalkyltrialkoxysilane, and when the organofunctional network former in step (a) is an epoxyalkyltrialkoxysilane, the weight ratio of the non-volatile content of the organofunctional network former applied in step (a) to the non-volatile content of the organofunctional network former applied in step (b) is from 1.25 to 2.0, wherein the aminosilane is: Aminoalkyltrialkoxysilanes, N-(alkyl)-aminoalkyltrialkoxysilanes, N-aminoalkyl-aminoalkyl(alkyl)dialkoxysilanes, and N-aminoalkyl-aminoalkyltrialkoxysilane is selected from And here: The alkyl moieties in the epoxyalkyltrialkoxysilane and aminosilane are each independently C 1-6 alkyl, The alkoxy moieties in the epoxyalkyltrialkoxysilane and aminosilane are each independently C 1-6 alkoxy; and Each alkoxy moiety in the tetraalkoxysilane is C 1-6 The method is alkoxy.
2. 10. The method of claim 1, wherein part (b) comprises one or two further steps in which the inorganic network former and the organofunctional network former undergo a condensation type reaction.
3. 3. The method of claim 1 or 2, wherein the substrate comprises or is an aluminum, bronze, copper or zinc pigment.
4. 4. The method according to claim 3, wherein the substrate is an aluminum pigment and the proportion of aluminum is ≥ 99% by weight, based on the total weight of the uncoated aluminum pigment.
5. The inorganic network former has the formula (I): MX n (I) (In the formula, M is Si, X is methoxy or ethoxy, and - n is 4.
6. The aminosilane is: 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-(n-butyl)-3-amino-propyltrimethoxysilane, N-(n-butyl)-3-amino-propyltriethoxysilane, N-2-aminoethyl-3-aminopropyl(methyl)dimethoxysilane, N-2-aminoethyl-3-aminopropyl(methyl)diethoxysilane, N-2-aminoethyl-3-aminopropyltrimethoxysilane, and N-2-aminoethyl-3-aminopropyltriethoxysilane is selected from Each epoxyalkyltrialkoxysilane is: 3-glycidyloxypropyltriethoxysilane, and 3-Glycidyloxypropyltrimethoxysilane The method according to any one of claims 1 to 5, wherein the compound is selected from the group consisting of
7. The coated metal pigment is (i) subjected to the following test methods to determine the chemical resistance of the coated pigment: (a) charging the coated pigment directly into a mixing vessel with a polyester powder, where if the coated pigment has an average particle size (d50) as measured by laser diffraction of ≥ 20 microns then 188 g of polymer powder is used with 12 g of coated pigment, and if the coated pigment has an average particle size (d50) as measured by laser diffraction < 20 microns then 192 g of polymer powder is used with 8 g of coated pigment; (b) if all of the coated pigment is not below the level of the mixing tool in the mixing vessel, shaking the mixing vessel to bring all of the coated pigment below the level of the mixing tool; (c) blending the polyester powder and coated pigment for 2*30 seconds at ambient temperature; (d) transferring the resulting powder preparation into a plastic bag; (e) The powder formulation was sprayed using an electrostatic spray gun with a circular metal nozzle and a 30 mm deflector with the following parameters: Powder hose connection: 2 bar Purge air connection: 0.5 kg / cm2 Material flow controller: 50% Voltage: 70 kV Gun panel distance: 30 cm Apply onto steel panels using; wherein the amount of formulation applied is sufficient to provide a thickness of 50 to 75 microns after the curing step (f) below. (and where spitting and / or caking occurs with the spray gun then the test is abandoned and started over); (f) Curing the thus applied formulation using a baking time of 160°C for 8 minutes; (g) keeping the resulting sample at ambient temperature for at least 24 hours; (h) placing the sample horizontally on a magnetic pad and placing 15 to 17 mm drops thereon of the following solutions: (i) a 10 wt % aqueous solution of hydrochloric acid, (ii) a 1 M aqueous solution of sodium hydroxide, and (iii) a 10 wt % aqueous solution of sodium hydroxide (NaOH), whereby the drops are placed in a time sequence such that all drops can be removed simultaneously after 240 minutes, and for each solution the panel is exposed for 1 drop 30 minutes, 1 drop 60 minutes, 1 drop 120 minutes, 1 drop 180 minutes, and 1 drop 240 minutes; (i) all drops are simultaneously removed from the sample by rinsing with water; (j) Each of the 15 drop regions was visually assessed for the degree of greying, using the following scheme: 0 No attack 0.5 Only slight changes are visible at certain angles 1. Slight graying 2) Graying and pigmentation are still visible 3 Complete graying, no visible pigmentation) Assign a score between 0 and 3 based on (k) the scores for each drop region are then summed to provide a total score from 0 to 45; (ii) a gloss dispersion (X) of ≦5.0, - X=Y / (13-chemical resistance score of coated pigment), - Y is the percent change in gloss resulting from the addition of the coating to the pigment, calculated as (100*(Y1-Y2) / Y1); - Y1 is the gloss of the uncoated pigment, and - Y2 is the gloss of the coated pigment 7. The method according to any one of claims 1 to 6, wherein the gloss is measured by preparing a sample containing a coated or uncoated pigment according to steps (a) to (g) of the test method for measuring the chemical resistance of coated pigments and then measuring the gloss at 60° using a gloss meter.
8. The coated metal pigment (i) has a chemical resistance of less than 12 according to the Test Method for Measuring Chemical Resistance of Coated Pigments; and (ii) a lightness dispersion L of ≥ 90. A Or L B value [wherein: - L A is calculated as (100*(1+(Q2-Q1) / Q1)), - Q1 is the color value at 15° of the uncoated pigment, and - Q2 is the lightness at 15° of the coated pigment; - L B is calculated as (100*(1+(Q4-Q3) / Q3)), - Q3 is the color value at -15° of the uncoated pigment, and - Q4 is the lightness of the coated pigment at -15° 8. The method according to claim 1, wherein the color values at 15° and −15° are measured by preparing a sample comprising a coated or uncoated pigment according to steps (a) to (g) of the test method for measuring the chemical resistance of coated pigments and then using a gloss meter.
9. The coated metal pigment has an MIE*surface area of at least 40 mJ m2, where MIE is the minimum ignition energy and surface area is the surface area measured by the BET method. 2 The method according to any one of claims 1 to 8, wherein the value of x is 0.01 to 0.
25.
10. The coated metal pigment (i) has a gassing stability score of ≥ 700 seconds in the Test Method for Measuring Gassing Stability of Coated Pigments; and (ii) a gloss dispersion (X) of ≤ 5.0, wherein: - X=Y / (13-chemical resistance score of coated pigment), - Y is the percent change in gloss resulting from the addition of the coating to the pigment, calculated as (100*(Y1-Y2) / Y1); - Y1 is the gloss of the uncoated pigment, and - Y2 is the gloss of the coated pigment 10. The method according to any one of claims 1 to 9, wherein the gloss is measured by preparing a sample containing a coated or uncoated pigment according to steps (a) to (g) of the test method for measuring the chemical resistance of coated pigments and then measuring the gloss at 60° using a gloss meter.
11. The coated metal pigment (i) has a gassing stability of ≥ 700 seconds according to the Test Method for Measuring Gassing Stability of Coated Pigments; and (ii) a lightness dispersion L A Or L B value (wherein: - L A is calculated as (100*(1+(Q2-Q1) / Q1)), - Q1 is the color value at 15° of the uncoated pigment, and - Q2 is the lightness at 15° of the coated pigment; - L B is calculated as (100*(1+(Q4-Q3) / Q3)), - Q3 is the color value at -15° of the uncoated pigment, and - Q4 is the lightness of the coated pigment at -15° (wherein the color values at 15° and −15° are measured by preparing samples containing coated or uncoated pigments according to steps (a) to (g) of the test method for determining the chemical resistance of coated pigments and then using a gloss meter).
12. 12. The method of any one of claims 1 to 11, wherein the substrate is a PVD metal pigment and the coated metal pigment has a chemical resistance score of 12 or less in a test method for measuring chemical resistance of coated pigments.
13. 13. The method of any one of claims 1 to 12, wherein the substrate is a PVD metal pigment and the coated metal pigment has a gassing stability score of ≥ 700 seconds in a test method for measuring gassing stability of coated pigments.
14. 14. The method of any one of claims 1 to 13, wherein the substrate is a PVD metal pigment and the coated metal pigment has a gassing stability score of < 5ml after 21 days in an extended gassing test method.
15. The substrate has a d of (i)≦30 μm 50 The method of claim 1 , wherein the metallic pigment has (i) an average aspect ratio of at least 100 and (ii) a mean aspect ratio of at least 100.
16. The method of claim 1, further comprising applying one or more surface modifiers to the coated metal pigment substrate after steps (a) and (b).
17. said one or more surface modifiers (a) both (i) an organophosphorus compound, and (ii) a compatibilizer having a molecular weight of 5000 or less, wherein the organophosphorus compound and the compatibilizer are applied simultaneously, separately or sequentially; (b) both (i) a fatty acid, and (ii) a compatibilizer having a molecular weight of 5000 or less, where the fatty acid and the compatibilizer are applied simultaneously, separately or sequentially; or (c) both (i) an organofunctional network former, and (ii) an organophosphorus compound, where the organofunctional network former and the organophosphorus compound are applied simultaneously, separately or sequentially.
17. The method of claim 16, comprising:
18. 17. The method of claim 16, wherein the one or more surface modifiers include both (i) an organophosphorus compound, and (ii) a compatibilizer having a molecular weight of 5,000 or less, and wherein the organophosphorus compound and the compatibilizer are applied simultaneously, separately or sequentially.
19. The organophosphorus compound has the formula (III): I-X-P(O)(OR 1 )(OR 2 ) (III) [In the formula, - R 1 and R 2 are each independently H, an optionally substituted hydrocarbyl, an optionally substituted amine, a polyether, an ammonium ion, an alkali metal, or an alkaline earth metal; - X is divalent and is (a) a linear or branched hydrocarbon chain, wherein said hydrocarbon chain is optionally interrupted by one or more heteroatoms selected from O, S and N, (b) an optionally substituted carbocycle, wherein said ring is selected from cycloalkyl, cycloalkenyl, aryl and fused hydrocarbon groups, or (c) an optionally substituted heterocycle containing one or more heteroatoms selected from O, S and N; and - I is H or an initiator moiety for polymerization. The method of claim 18, wherein the compound is
20. - R 1 and R 2 is H; - X is C 4-14 alkylene; and I is H, 20. The method of claim 19.
21. 21. The method of any one of claims 18 to 20, wherein the compatibilizer is a melamine resin, an isocyanate resin, a polyurethane resin or an acrylic resin.
22. The compatibilizer is C 1-4 The method according to claim 18, wherein the resin is an alcohol-etherified melamine-formaldehyde resin or an isophorone diisocyanate trimer resin.
23. 18. The method of claim 17, wherein the one or more surface modifiers comprise both (i) a fatty acid, and (ii) a compatibilizer having a molecular weight of 5000 or less, wherein the fatty acid and the compatibilizer are applied simultaneously, separately or sequentially, the fatty acid being a compound of formula R-C(O)OH, where R is an alkyl or alkenyl group having from 3 to 29 carbons, and the compatibilizer is as defined in claim 21 or 22.
24. 20. The method of claim 17, wherein the one or more surface modifiers comprise both (i) an organofunctional network former, and (ii) an organophosphorus compound, wherein the organofunctional network former and the organophosphorus compound are applied simultaneously, separately or sequentially, and the organofunctional network former is an aminoalkyltrialkoxysilane, and the organophosphorus compound is as defined in claim 19 or 20.
25. 1. A method for producing a product or article comprising a coated metal pigment, the method comprising: - coating a metal pigment by a method as defined in any one of claims 1 to 6, - optionally thereafter applying one or more surface modifiers to the coated metal pigment; and - further processing the coated metal pigment into an article comprising the coated metal pigment. wherein the product is a varnish, an automotive finish, a paint, a printing ink, a powder coating material, an architectural paint, a plastic, a security printing ink, a ceramic, a glass or a cosmetic.
26. 26. The method of claim 25, wherein the product is a powder coating material further comprising a polymer.
27. 26. The method of claim 25, wherein the product is an aqueous coating composition comprising the coated metal pigment of any one of claims 7 to 14.
28. 28. The method of claim 27, wherein the coated metal pigment (a) has an organofunctional network former and an organophosphorus compound on its surface, and / or (b) is obtained or is obtainable by a method comprising applying one or more surface modifiers to the pigment simultaneously, separately or sequentially, wherein the one or more surface modifiers comprise an organofunctional network former and an organophosphorus compound.
29. 26. The method according to claim 25, wherein the product is a coating material and the method is a method of coating an article, comprising electrostatically applying a powder coating material as defined in claim 25 or 26 to an article and, optionally, curing the applied coating material.
30. 30. The method of claim 29, wherein the article is an automobile.
31. 31. The method of claim 29 or 30, wherein the coated metal pigment substrate is a coated metal pigment according to any one of claims 7 to 9, 12 and 15.
Citation Information
Patent Citations
Corrosion-resistant aqueous aluminum pigment with shielding effects
CN106167632A
Novel aluminum pigment
JP2002226733A
Highly corrosion-resistant flaky metal pigment, method for producing the same and interference color pigment with metallic luster comprising the metal pigment as base
JP2003041150A
Method for treating metal flake with phosphonic acid derivative
JP2003183542A