Golf balls
A golf ball with a polyurethane coating film having specific dynamic viscoelastic properties improves spin performance on approach shots by enhancing interaction with the wedge face.
Patent Information
- Application Number
- JP2020171228
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-10-09
AI Technical Summary
Existing golf balls do not achieve optimal spin performance on approach shots due to inadequate properties of their coating films.
The golf ball features a coating film with a polyurethane base resin that has a loss modulus of 0.2 × 10^8 Pa or higher and a peak temperature of loss tangent (tan δ) at 0°C or lower, measured under specific dynamic viscoelasticity conditions, enhancing the film's interaction with the wedge face during shots.
The improved coating film enhances the spin performance of the golf ball on approach shots by better penetrating the score lines of the wedge, resulting in increased spin rates.
Smart Images

Figure 0007585700000008 
Figure 0007585700000001 
Figure 0007585700000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a golf ball having a coating. [Background technology]
[0002] A coating is provided on the surface of the golf ball body, and it has been proposed to improve the properties of the golf ball by improving the coating.
[0003] Patent Document 1 describes a golf ball having a core, a cover positioned on the outside of the core, and a paint layer positioned on the outside of the cover, the cover having a Shore D hardness of 61 or less, and the paint layer having a Martens hardness of 2.0 mgf / μm. 2 The following golf ball is disclosed:
[0004] Patent Document 2 describes a golf ball having a golf ball body and a coating film provided on the surface of the golf ball body, the coating film having a Martens hardness of 2.0 mgf / μm 2 and the ratio of the 50% modulus to the 10% modulus (50% modulus / 10% modulus) is 1.6 or greater.
[0005] Patent Document 3 describes a golf ball having a golf ball body and a coating film provided on the surface of the golf ball body, the coating film having a storage modulus (E') of 1.00×10 in a temperature range of 120° C. to 150° C. as measured under specific measurement conditions using a dynamic viscoelasticity device. 7 dyn / cm 2 That's it, 1.00 x 10 8 dyn / cm 2 or less and having a loss tangent (tan δ) at 10° C. of 0.050 or more.
[0006] Patent Document 4 discloses a golf ball having a golf ball body and a coating film covering the golf ball body, characterized in that the peak temperature of the loss tangent tan δ obtained by measuring the dynamic viscoelasticity of the coating film is 50°C or less and the peak height is less than 0.8.
[0007] Patent Document 5 describes a golf ball having a golf ball body and at least one layer of coating film provided on the surface of the golf ball body, The coating film is an outermost layer coating film located on the outermost layer of a golf ball, and contains, as a base resin, a polyurethane obtained by reacting (A) a polyisocyanate composition with (B) a polyol composition, and the (B) polyol composition contains a urethane polyol as a polyol component, and the outermost layer coating film has a peak temperature of loss tangent (tan δ) of -40°C to 40°C as measured under specific conditions using a dynamic viscoelasticity device.
[0008] Patent Document 6 describes a golf ball having a golf ball body and at least one layer of coating film provided on the surface of the golf ball body, in which the base resin constituting the outermost layer of the coating film is a polyurethane obtained by reacting (A) a polyol composition and (B) a polyisocyanate composition, and the loss modulus (E") at −50° C. obtained by measuring the dynamic viscoelasticity of the polyurethane under the following conditions is 1.00×10 8 A golf ball having a tensile strength of 0.1 Pa or higher is disclosed. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2011-67595 A [Patent Document 2] JP 2011-217820 A [Patent Document 3] JP 2014-14383 A [Patent Document 4] JP 2017-209298 A [Patent Document 5] JP 2020-69309 A [Patent Document 6] JP 2020-99669 A Summary of the Invention [Problem to be solved by the invention]
[0010] An object of the present invention is to provide a novel golf ball that has excellent spin performance on approach shots. [Means for solving the problem]
[0011] The golf ball of the present invention is a golf ball having a golf ball body and at least one layer of coating film provided on the surface of the golf ball body, the base resin constituting the outermost layer of the coating film is polyurethane; The dynamic viscoelasticity of the polyurethane is measured under the following conditions, and the loss modulus (E") at -50°C is 0.2 x 10 8 Pa or more, and the peak temperature of the loss tangent (tan δ) is 0° C. or less. <Measurement conditions> Measurement mode: Sine wave tension Measurement temperature range: -120℃~100℃ Heating rate: 3℃ / min Excitation frequency: 10Hz Measurement distortion: 0.05%
[0012] If the impact speed during an approach shot is 16 m / s and the unevenness of the face land of the wedge is a few μm, the vibration that the paint film of the golf ball receives during the approach shot is 10 7 Hz. At room temperature, 7The dynamic viscoelasticity of a coating film with a vibration of 10 Hz, when converted using time-temperature conversion, is equivalent to the dynamic viscoelasticity measured at -50°C and a frequency of 10 Hz. The inventors discovered that the spin performance of approach shots can be improved by controlling the loss modulus and the peak temperature of the loss tangent (tan δ) measured at -50°C and a frequency of 10 Hz of the polyurethane constituting the outermost layer of the coating film of a golf ball, and thus completed the present invention. Effect of the Invention
[0013] The coating film used in the present invention is soft. According to the present invention, a golf ball having excellent spin performance on approach shots can be obtained. [Brief description of the drawings]
[0014] [Figure 1] 1 is a partially cutaway cross-sectional view showing a golf ball according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The golf ball of the present invention is a golf ball having a golf ball body and at least one layer of coating film provided on the surface of the golf ball body, the base resin constituting the outermost layer of the coating film is polyurethane; The dynamic viscoelasticity of the polyurethane is measured under the following conditions, and the loss modulus (E") at -50°C is 0.2 x 10 8 Pa or more, and the peak temperature of the loss tangent (tan δ) is 0° C. or less. <Measurement conditions> Measurement mode: Sine wave tension Measurement temperature range: -120℃~100℃ Heating rate: 3℃ / min Excitation frequency: 10Hz Measurement distortion: 0.05%
[0016] The polyurethane constituting the outermost layer of the coating of the golf ball of the present invention has a loss modulus (E") of 0.2 x 10 at -50°C, as determined by measuring the dynamic viscoelasticity under the following conditions:8 Pa or more. <Measurement conditions> Measurement mode: Sine wave tension Measurement temperature range: -120℃~100℃ Heating rate: 3℃ / min Excitation frequency: 10Hz Measurement distortion: 0.05%
[0017] From the viewpoint of improving the spin performance of an approach shot, the loss modulus (E") is 0.3×10 8 Pa or more is more preferable, and 0.5×10 8 More preferably, the pressure is 5.0×10 Pa or more. 9 Pa or less, and 9.0×10 8 Pa or less, and more preferably 8.0×10 8 It is more preferable that the pressure is 0.1 Pa or less.
[0018] The polyurethane constituting the outermost layer of the coating of the golf ball of the present invention has a storage modulus (E') at 0°C obtained by measuring the dynamic viscoelasticity under the above-mentioned conditions of 0.05 × 10 8 Pa or higher, 3.0×10 9 Pa or less. The contact time between the golf ball and the wedge face during an approach shot is about 500 μsec. This corresponds to the coating film cutting into the score line of the wedge about 2000 times per second (=2000 Hz). The dynamic viscoelasticity of the coating film with vibration of 2000 Hz at room temperature corresponds to the dynamic viscoelasticity measured at 0°C and a frequency of 10 Hz when converted by time-temperature conversion. Therefore, the inventors of the present invention focused on the storage modulus (E') measured at 0°C and a frequency of 10 Hz. By using a polyurethane with the storage modulus (E') within the above range, the coating film cuts into the score line of the wedge well. As a result, the spin performance is improved.
[0019] From the viewpoint of improving the spin performance of an approach shot, the storage modulus (E') is 0.1 x 10 8 Pa or more is more preferable, and 0.3×10 8More preferably, the surface tension is 9.0×10 Pa or more. 8 Pa or less, and more preferably 7.0×10 8 It is more preferable that the pressure is 0.1 Pa or less.
[0020] The polyurethane constituting the outermost layer of the coating of the golf ball of the present invention has a peak temperature of loss tangent (tan δ) obtained by measuring the dynamic viscoelasticity under the above-mentioned conditions, which is preferably 0° C. or lower, more preferably less than −40° C., even more preferably −45° C. or lower, preferably −90° C. or higher, more preferably −60° C. or higher, and even more preferably −55° C. or higher. If the peak temperature of loss tangent (tan δ) is within the above-mentioned range, the ratio of loss modulus / storage modulus at −50° C. increases, improving the approach spin performance.
[0021] The 10% modulus of the polyurethane constituting the outermost layer of the coating of the golf ball of the present invention is 1 kgf / cm 2 (0.10 MPa) or more is preferable, and 3 kgf / cm is more preferable. 2 (0.29MPa) or more, more preferably 5kgf / cm 2 (0.49MPa) or more, 50kgf / cm 2 (4.9 MPa) or less is preferable, and 40 kgf / cm 2 (3.9 MPa) or less, more preferably 30 kgf / cm 2 (2.9 MPa) or less. The 10% modulus of the polyurethane of the outermost coating film is 1 kgf / cm 2 If it is more than 50kgf / cm, the coating film will have low adhesion and will be less likely to get dirty. 2 If the ball is below this value, the coating's coefficient of kinetic friction will be large, increasing the amount of spin on approach shots when the ball is biting into the grass.
[0022] The base resin constituting the outermost layer of the coating film is polyurethane. The polyurethane has a polyisocyanate component and a polyol component as constituent components. The polyurethane used in the present invention preferably contains an olefin diol having a linear structure as the polyol component. The olefin diol is preferably a compound having a linear main chain structure, an olefin skeleton having an ethylenically unsaturated carbon-carbon double bond, and having hydroxy groups at both ends of the main chain.
[0023] The polyurethane used in the present invention is preferably a polyurethane obtained by reacting (A) a polyol composition with (B) a polyisocyanate composition. First, the polyol composition and the polyisocyanate composition will be described.
[0024] The polyol composition (A) contains a polyol having at least two hydroxy groups.The polyol composition (A) preferably contains an olefin diol having a linear structure as a polyol component.
[0025] The olefin monomer constituting the olefin diol is not limited as long as it is a hydrocarbon having a polymerizable unsaturated carbon-carbon double bond. The olefin is preferably a cycloolefin. That is, the olefin diol is preferably a poly(cycloolefin) diol. The poly(cycloolefin) diol is a ring-opening polymer of a cycloolefin. That is, the poly(cycloolefin) diol is a compound having a linear main chain structure, which is a skeleton formed by ring-opening polymerization of a cycloolefin, and having hydroxy groups at both ends of the main chain.
[0026] The olefin diol is preferably obtained by ring-opening polymerization of a cycloolefin monomer, and more preferably obtained by metathesis ring-opening polymerization of a cycloolefin monomer.
[0027] The cis / trans ratio (molar ratio) of the double bonds present in the repeating units constituting the olefin diol is not particularly limited, but is preferably 10 / 90 or more, more preferably 40 / 60 or less, and even more preferably 30 / 70 or less. The cis / trans ratio of the cycloolein ring-opening polymer is 13 It can be determined by C-NMR spectroscopy.
[0028] The olefin diol can be obtained, for example, by polymerizing a cycloolefin monomer using a metathesis polymerization catalyst and a chain transfer agent represented by the general formula (1) described later.
[0029] (Cycloolefin Monomer) The cycloolefin monomer is a compound having a ring structure formed by carbon atoms and having a polymerizable carbon-carbon double bond in the ring structure. In this specification, the term "polymerizable carbon-carbon double bond" refers to a carbon-carbon double bond involved in chain polymerization (metathesis ring-opening polymerization).
[0030] Examples of the ring structure of the cycloolefin monomer include a monocycle, a polycycle, a condensed polycycle, a bridged ring, and a combination polycycle thereof. The number of carbon atoms constituting each ring structure is not particularly limited, but is preferably 4 or more, more preferably 5 or more, more preferably 30 or less, more preferably 20 or less, and even more preferably 15 or less. The cycloolefin monomer may have a hydrocarbon group having 1 to 30 carbon atoms, such as an alkyl group, an alkenyl group, an alkylidene group, or an aryl group, or a polar group, such as a carboxyl group or an acid anhydride group, as a substituent.
[0031] As the cycloolefin monomer, a monocyclic cycloolefin monomer and a polycyclic cycloolefin monomer are preferable.
[0032] Examples of monocyclic cycloolefin monomers include cyclopentene, 3-methylcyclopentene, 4-methylcyclopentene, 3,4-dimethylcyclopentene, 3,5-dimethylcyclopentene, 3-chlorocyclopentene, cyclohexene, 3-methylcyclohexene, 4-methylcyclohexene, 3,4-dimethylcyclohexene, 3-chlorocyclohexene, cycloheptene, etc. Among these, cyclopentene is preferred as the monocyclic cycloolefin monomer.
[0033] Examples of the polycyclic cycloolefin monomer include compounds containing a norbornene ring (hereinafter, may be simply referred to as "norbornene compounds"). Examples of the polycyclic cycloolefin monomer include dicyclopentadiene, methyldicyclopentadiene, dihydrodicyclopentadiene (tricyclo[5.2.1.0 2,6 ]deca-8-ene.) and other dicyclopentadienes; tetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-methyltetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-ethyltetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-cyclohexyltetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-cyclopentyltetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-methylenetetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-ethylidenetetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-vinyltetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-propenyltetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-cyclohexenyltetracyclo[6.2.1.13,6 .0 2,7 ]dodec-4-ene, 9-cyclopentenyltetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-phenyltetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene and other tetracyclododecenes; 2-norbornene, 5-methyl-2-norbornene, 5-ethyl-2-norbornene, 5-butyl-2-norbornene, 5-hexyl-2-norbornene, 5-decyl-2-norbornene, 5-cyclohexyl-2-norbornene, 5-cyclopentyl-2-norbornene, 5-ethylidene-2-norbornene, 5-vinyl-2-norbornene, 5-propenyl-2-norbornene, 5-cyclohexenyl-2-norbornene, 5-cyclopentenyl-2-norbornene, 5-phenyl-2-norbornene, tetracyclo[9.2.1.0 2,10 .0 3,8 ]tetradeca-3,5,7,12-tetraene (also called 1,4-methano-1,4,4a,9a-tetrahydro-9H-fluorene), tetracyclo[10.2.1.0 2,11 .0 4,9 ]pentadeca-4,6,8,13-tetraene (also called 1,4-methano-1,4,4a,9,9a,10-hexahydroanthracene); and other norbornenes. Among these, examples of polycyclic cycloolefin monomers include 2-norbornene, dicyclopentadiene, tetracyclo[9.2.1.0 2,10 .0 3,8 ]Tetradeca-3,5,7,12-tetraene, tetracyclo[6.2.1.1 3,6 .0 2,7 ]Dodec-4-ene is preferred.
[0034] The cycloolefin monomers can be used alone or in combination of two or more kinds.
[0035] The olefin diol used in the present invention is preferably a copolymer having the monomer unit obtained by ring-opening polymerization of the monocyclic cycloolefin monomer and the monomer unit obtained by ring-opening polymerization of the polycyclic cycloolefin monomer, and more preferably a copolymer having the monomer unit obtained by ring-opening polymerization of the monocyclic cycloolefin monomer and the monomer unit obtained by ring-opening polymerization of the polycyclic cycloolefin monomer.By having the monomer unit obtained by ring-opening polymerization of the polycyclic cycloolefin monomer as a copolymerization component, the obtained olefin diol becomes easy to be liquefied.
[0036] The content of monomer units obtained by ring-opening polymerization of monocyclic cycloolefin monomers is preferably 60 mass% or more, more preferably 65 mass% or more, and even more preferably 70 mass% or more, preferably 95 mass% or less, more preferably 92 mass% or less, and preferably 90 mass% or less, based on 100 mass% of all monomer units constituting the olefin diol.
[0037] The content of monomer units obtained by ring-opening polymerization of polycyclic cycloolefin monomers is preferably 5% by mass or more, more preferably 8% by mass or more, and even more preferably 10% by mass or more, preferably 40% by mass or less, more preferably 35% by mass or less, and even more preferably 30% by mass or less, based on 100% by mass of all monomer units constituting the olefin diol.
[0038] The monomer unit composition ratio in the cycloolefin ring-opening copolymer is, for example, 1 It can be determined by H-NMR spectroscopy.
[0039] The olefin diol used in the present invention is preferably a cyclopentene-norbornene ring-opening copolymer having a monomer unit obtained by ring-opening polymerization of cyclopentene as the monocyclic cycloolefin monomer and a monomer unit obtained by ring-opening polymerization of a norbornene compound as the polycyclic cycloolefin monomer. The cyclopentene-norbornene ring-opening copolymer is more preferably a copolymer consisting of a monomer unit obtained by ring-opening polymerization of cyclopentene and a monomer unit obtained by ring-opening polymerization of a norbornene compound.
[0040] (Metathesis Polymerization Catalyst) The metathesis polymerization catalyst used in the present invention is not particularly limited as long as it is capable of subjecting the cycloolefin monomer to metathesis ring-opening polymerization.
[0041] The metathesis polymerization catalyst may be a complex formed by bonding a plurality of ions, atoms, polyatomic ions and / or compounds to a transition metal atom. The transition metal atom may be an atom of group 5, group 6 or group 8 (long-form periodic table, the same applies below). The atom of each group is not particularly limited, but the atom of group 5 is preferably tantalum. The atom of group 6 is preferably molybdenum or tungsten. The atom of group 8 is preferably ruthenium or osmium.
[0042] Among these, complexes of ruthenium or osmium of group 8 are preferred, and ruthenium carbene complexes are particularly preferred. Ruthenium carbene complexes have excellent catalytic activity during bulk polymerization, and can efficiently produce resin molded articles with little odor derived from residual unreacted monomers. In addition, complexes of ruthenium or osmium of group 8 are relatively stable against oxygen and moisture in the air, and are not easily deactivated.
[0043] Examples of ruthenium carbene complexes include benzylidene(1,3-dimesityl-4-imidazolidin-2-ylidene)(tricyclohexylphosphine)ruthenium dichloride, benzylidene(1,3-dimesityl-4,5-dibromo-4-imidazolin-2-ylidene)(tricyclohexylphosphine)ruthenium dichloride, (1,3-dimesityl-4-imidazolin-2-ylidene)(3-phenyl-1H-inden-1-ylidene)(tricyclohexylphosphine)ruthenium dichloride, (1,3-di Mesityl-4-imidazolidin-2-ylidene)(3-methyl-2-buten-1-ylidene)(tricyclopentylphosphine)ruthenium dichloride, Benzylidene(1,3-dimesityl-octahydrobenzimidazol-2-ylidene)(tricyclohexylphosphine)ruthenium dichloride, Benzylidene[1,3-di(1-phenylethyl)-4-imidazolin-2-ylidene](tricyclohexylphosphine)ruthenium dichloride, Benzylidene(1,3-dimesityl-2,3-dihydrobenzimidazol-2-ylidene)(tricyclohexylphosphine)ruthenium dichloride Benzylidene(tricyclohexylphosphine)(1,3,4-triphenyl-2,3,4,5-tetrahydro-1H-1,2,4-triazol-5-ylidene)ruthenium dichloride, (1,3-diisopropylhexahydropyrimidin-2-ylidene)(ethoxymethylene)(tricyclohexylphosphine)ruthenium dichloride, benzylidene(1,3-dimesityl-4-imidazolidin-2-ylidene)pyridine ruthenium ruthenium dichloride, (1,3-dimesityl-4-imidazolin-2-ylidene)(2-phenylethylidene)(tricyclohexylphosphine)ruthenium dichloride, (1,3-dimesityl-4-imidazolin-2-ylidene)(2-phenylethylidene)(tricyclohexylphosphine)ruthenium dichloride, (1,3-dimesityl-4,5-dibromo-4-imidazolin-2-ylidene)[(phenylthio)methylene](tricyclohexylphosphine)ruthenium dichloride, (1,3-dimesityl-4,Ruthenium complex compounds each having one heteroatom-containing carbene compound and one neutral electron donor compound other than a heteroatom-containing carbene compound bonded thereto, such as 5-dibromo-4-imidazolin-2-ylidene)(2-pyrrolidone-1-ylmethylene)(tricyclohexylphosphine)ruthenium dichloride;
[0044] Ruthenium complex compounds bound to two neutral electron donor compounds other than heteroatom-containing carbene compounds, such as benzylidenebis(tricyclohexylphosphine)ruthenium dichloride and (3-methyl-2-buten-1-ylidene)bis(tricyclopentylphosphine)ruthenium dichloride;
[0045] Ruthenium complex compounds in which two heteroatom-containing carbene compounds are bonded, such as benzylidenebis(1,3-dicyclohexyl-4-imidazolidin-2-ylidene)ruthenium dichloride and benzylidenebis(1,3-diisopropyl-4-imidazolin-2-ylidene)ruthenium dichloride; and the like.
[0046] Further examples of ruthenium carbene complexes include (1,3-dimesityl-4-imidazolin-2-ylidene)(phenylvinylidene)(tricyclohexylphosphine)ruthenium dichloride, (t-butylvinylidene)(1,3-diisopropyl-4-imidazolin-2-ylidene)(tricyclopentylphosphine)ruthenium dichloride, and bis(1,3-dicyclohexyl-4-imidazolin-2-ylidene)phenylvinylideneruthenium dichloride.
[0047] The amount of the metathesis polymerization catalyst used, in terms of the molar ratio of (metal atoms in the catalyst:cycloolefin monomer), is usually in the range of 1:2,000 to 1:2,000,000, preferably 1:5,000 to 1:1,000,000, and more preferably 1:10,000 to 1:500,000.
[0048] If desired, the metathesis polymerization catalyst can be used by dissolving or suspending it in a small amount of an inert solvent. Examples of such solvents include chain aliphatic hydrocarbons such as n-pentane, n-hexane, n-heptane, liquid paraffin, and mineral spirits; alicyclic hydrocarbons such as cyclopentane, cyclohexane, methylcyclohexane, dimethylcyclohexane, trimethylcyclohexane, ethylcyclohexane, diethylcyclohexane, decahydronaphthalene, dicycloheptane, tricyclodecane, hexahydroindene, and cyclooctane; aromatic hydrocarbons such as benzene, toluene, and xylene; nitrogen-containing hydrocarbons such as nitromethane, nitrobenzene, and acetonitrile; and oxygen-containing hydrocarbons such as diethyl ether and tetrahydrofuran. Among these, it is preferable to use industrially common aromatic hydrocarbons, aliphatic hydrocarbons, and alicyclic hydrocarbons. In addition, liquid antioxidants, liquid plasticizers, and liquid elastomers may be used as solvents as long as they do not reduce the activity of the metathesis polymerization catalyst.
[0049] The metathesis polymerization catalyst can be used in combination with an activator (cocatalyst) for the purpose of controlling the polymerization activity and improving the polymerization reaction rate.
[0050] As the activator, alkylated, halides, alkoxylated and aryloxylated compounds of aluminum, scandium and tin can be used, and specific examples thereof include trialkoxyaluminum, triphenoxyaluminum, dialkoxyalkylaluminum, alkoxydialkylaluminum, trialkylaluminum, dialkoxyaluminum chloride, alkoxyalkylaluminum chloride, dialkylaluminum chloride, trialkoxyscandium, tetraalkoxytitanium, tetraalkoxytin and tetraalkoxyzirconium.
[0051] The amount of the activator used, in terms of the molar ratio of (metal atoms in the catalyst:activator), is usually in the range of 1:0.05 to 1:100, preferably 1:0.2 to 1:20, and more preferably 1:0.5 to 1:10.
[0052] In addition, when a complex of a Group 5 or Group 6 transition metal atom is used as the metathesis polymerization catalyst, the metathesis polymerization catalyst and the activator are preferably dissolved in the monomer before use. However, they may be suspended or dissolved in a small amount of solvent within a range that does not substantially impair the properties of the product.
[0053] (Chain transfer agent) When a cycloolefin monomer is subjected to the metathesis ring-opening polymerization, it is preferable to use a compound represented by the following general formula (1) as a chain transfer agent. HO-X-CH=CH-Y-OH (1)
[0054] In general formula (1), X and Y each independently represent an alkylene group having a carbon number of 1 to 30. The number of carbon atoms in the alkylene group of X and Y is preferably 1 or more, preferably 2 or more, and more preferably 3 or more, and is preferably 20 or less, more preferably 15 or less, and still more preferably 10 or less. The alkylene group may have a linear structure or a branched structure.
[0055] By incorporating the chain transfer agent represented by the general formula (1), -OH groups derived from the chain transfer agent are bonded to both ends of the cycloolefin polymer. That is, an olefin diol having hydroxy groups at both ends of the main chain, which has a ring-opened cycloolefin skeleton as a repeating unit, is obtained.
[0056] Specific examples of the alkylene group of X or Y include a methylene group, an ethylene group, a propylene group, a butylene group, a pentylene group, a hexylene group, a heptylene group, an octylene group, a nonylene group, and a decylene group.
[0057] Specific examples of the chain transfer agent include butenediol (for example, 2-butene-1,2-diol), pentenediol, hexenediol (for example, 3-hexene-2,5-diol), octenediol (for example, 4-octene-1,8-diol), and nonenediol.
[0058] The amount of the chain transfer agent used is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, based on 100 parts by mass of the cycloolefin monomer.
[0059] (Other compounding agents) In the metathesis ring-opening polymerization of a cycloolefin monomer, in addition to the cycloolefin monomer, the metathesis polymerization catalyst, and the chain transfer agent, other compounding agents such as a polymerization regulator, a polymerization reaction retarder, a reactive fluidizing agent, a flame retardant, an antioxidant, and a colorant may be added as desired.
[0060] The polymerization regulator is blended for the purpose of controlling the polymerization activity or improving the polymerization reaction rate. Specific examples thereof include trialkoxyaluminum, triphenoxyaluminum, dialkoxyalkylaluminum, alkoxydialkylaluminum, trialkylaluminum, dialkoxyaluminum chloride, alkoxyalkylaluminum chloride, dialkylaluminum chloride, trialkoxyscandium, tetraalkoxytitanium, tetraalkoxytin, and tetraalkoxyzirconium. These polymerization regulators may be used alone or in combination of two or more. The amount of the polymerization regulator used is usually 1:0.05 to 1:100, preferably 1:0.2 to 1:20, more preferably 1:0.5 to 1:10, in terms of the molar ratio of (metal atom in metathesis polymerization catalyst:polymerization regulator).
[0061] The metathesis polymerization reaction of the cycloolefin monomer may be carried out in a solventless state or in a solution. When the polymerization is carried out in a solution, the solvent used is not particularly limited as long as it is inert in the polymerization reaction and can dissolve the cycloolefin monomer and the ruthenium-carbene complex used in the polymerization, but it is preferable to use a hydrocarbon solvent or a halogen-based solvent. Examples of the hydrocarbon solvent include aromatic hydrocarbons such as benzene, toluene, xylene, and ethylbenzene; aliphatic hydrocarbons such as n-hexane, n-heptane, and n-octane; alicyclic hydrocarbons such as cyclohexane, cyclopentane, and methylcyclohexane; and the like. Examples of the halogen-based solvent include alkyl halogens such as dichloromethane and chloroform; and aromatic halogens such as chlorobenzene and dichlorobenzene; and the like.
[0062] In addition, it is preferable to use an ether-based solvent or a ketone-based solvent as the polymerization solvent, from the viewpoint of being able to dissolve well the chain transfer agent having a hydroxyl group and the polymerization catalyst containing a ruthenium compound. Examples of the ether-based solvent include diethyl ether, cyclopentyl methyl ether, 1,2-dimethoxyethylene, and tetrahydrofuran. Examples of the ketone-based solvent include acetone, 2-butanone, acetophenone acetone, methyl isopropyl ketone, methyl n-butyl ketone, methyl isobutyl ketone, methyl amyl ketone, methyl isoamyl ketone, methyl n-hexyl ketone, and methyl nonyl ketone. These may be used alone or in combination of two or more.
[0063] The temperature for polymerizing the cycloolefin monomer is preferably -100°C or higher, more preferably -50°C or higher, even more preferably 0°C or higher, and particularly preferably 20°C or higher. The polymerization temperature is not particularly limited, but is preferably less than 100°C, more preferably less than 90°C, even more preferably less than 80°C, and particularly preferably less than 70°C. If the polymerization temperature is too high, the molecular weight of the resulting cycloolefin ring-opening polymer may be too low, and if the polymerization temperature is too low, the polymerization rate may be slow, resulting in poor productivity.
[0064] The polymerization reaction time is preferably 1 minute to 72 hours, more preferably 5 hours to 20 hours. After the polymerization conversion rate reaches a predetermined value, a known polymerization terminator is added to the polymerization system to terminate the polymerization, thereby producing a cycloolefin ring-opening polymer.
[0065] The olefin diol is preferably in a liquid state at room temperature. The viscosity of the olefin diol at 25° C. is preferably 50 mPa·s or more, more preferably 100 mPa·s or more, and even more preferably 300 mPa·s or more, and is preferably 30,000 mPa·s or less, more preferably 20,000 mPa·s or less, and even more preferably 15,000 mPa·s or less.
[0066] The glass transition temperature (Tg) of the olefin diol is preferably -90°C or higher, more preferably -85°C or higher, and even more preferably -80°C or higher, and is preferably 0°C or lower, more preferably -20°C or lower, and even more preferably -30°C or lower.
[0067] The number average molecular weight of the olefin diol is preferably 800 or more, more preferably 900 or more, even more preferably 1000 or more, and is preferably 6000 or less, more preferably 5000 or less, even more preferably 4000 or less. If the number average molecular weight of the olefin diol is 800 or more, the distance between crosslinking points in the coating film is long, and the coating film becomes soft, so that the spin performance is improved. If the number average molecular weight is 6000 or less, the distance between crosslinking points in the coating film is not too long, and the coating film has good stain resistance. The number average molecular weight of the olefin diol component can be determined by GPC.
[0068] The olefin diol used in the present invention does not include diene polymers having hydroxyl groups at both ends of the molecular chain (for example, polybutadiene having hydroxyl groups at both ends (Poly bd R-45HT manufactured by Idemitsu Kosan Co., Ltd.), polypentadiene having hydroxyl groups at both ends, polyhexadiene having hydroxyl groups at both ends, etc.).
[0069] In a preferred embodiment of the present invention, the polyol composition (A) contains a linear olefin diol as a polyol component. Also, in a more preferred embodiment of the present invention, the polyol composition (A) contains a urethane polyol, and the urethane polyol contains a linear olefin diol as a constituent component.
[0070] The urethane polyol is a compound having a plurality of urethane bonds in a molecule and two or more hydroxyl groups in one molecule. An example of the urethane polyol is a urethane prepolymer obtained by reacting a polyol with a polyisocyanate under conditions in which the hydroxyl groups of the polyol are in excess relative to the isocyanate groups of the polyisocyanate.
[0071] In a more preferred embodiment of the present invention, the first polyol component constituting the urethane polyol contains an olefin diol having a linear structure. The details of the olefin diol are as described above.
[0072] The urethane polyol may contain, in addition to the olefin diol, another polyol as a first polyol component constituting the urethane polyol.
[0073] The other polyol may contain a low molecular weight polyol component having a molecular weight of less than 500 and a high molecular weight polyol component having an average molecular weight of 500 or more. Examples of the low molecular weight polyol component include diols such as ethylene glycol, diethylene glycol, triethylene glycol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, and 1,6-hexanediol; and triols such as glycerin, trimethylolpropane, and hexanetriol. Examples of the high molecular weight polyol component include polyether diols and polyester diols. The second polyol component may be used alone or in combination of two or more.
[0074] Examples of polyether diols that can constitute the urethane polyol include polyoxyethylene glycol, polyoxypropylene glycol, and polyoxytetramethylene glycol, and among these, polyoxytetramethylene glycol is preferred.
[0075] The urethane polyol preferably contains a triol component and a diol component as a polyol component. The triol component is preferably trimethylolpropane. The mixing ratio of the triol component and the diol component (triol component / diol component) is preferably 1.0 or more, more preferably 1.2 or more, and is preferably 2.6 or less, more preferably 2.4 or less, in terms of the molar ratio of OH groups.
[0076] The polyol composition may contain a second polyol as a polyol component in addition to the urethane polyol. That is, the second polyol is a polyol that is directly contained in the polyol composition and does not constitute the urethane polyol. Examples of the second polyol include polyether polyols such as polyoxyethylene glycol (PEG), polyoxypropylene glycol (PPG), and polyoxytetramethylene glycol (PTMG); condensation polyester polyols such as polyethylene adipate (PEA), polybutylene adipate (PBA), and polyhexamethylene adipate (PHMA); lactone polyester polyols such as poly-ε-caprolactone (PCL); polycarbonate polyols such as polyhexamethylene carbonate; and acrylic polyols. The second polyol may be used alone or in a mixture of two or more kinds.
[0077] The content of the urethane polyol in the polyol contained in the polyol composition is preferably 60% by mass or more, more preferably 70% by mass or more, and further preferably 80% by mass or more. It is also preferable that the polyol composition contains only the urethane polyol as the polyol.
[0078] The first polyisocyanate component that can constitute the urethane polyol is not particularly limited as long as it has two or more isocyanate groups, and examples thereof include aromatic polyisocyanates such as 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, a mixture of 2,4-toluene diisocyanate and 2,6-toluene diisocyanate (TDI), 4,4'-diphenylmethane diisocyanate (MDI), 1,5-naphthylene diisocyanate (NDI), 3,3'-bitrylene-4,4'-diisocyanate (TODI), xylylene diisocyanate (XDI), tetramethylxylylene diisocyanate (TMXDI), and paraphenylene diisocyanate (PPDI); 4,4'-dicyclohexylmethane diisocyanate (H 12 MDI), hydrogenated xylylene diisocyanate (H 6Examples of the polyisocyanate include alicyclic polyisocyanates or aliphatic polyisocyanates such as hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), and norbornene diisocyanate (NBDI). These polyisocyanates may be used alone or in combination of two or more kinds.
[0079] The urethane polyol preferably has an olefin diol content of 55% by mass or more, more preferably 58% by mass or more, and even more preferably 60% by mass or more. The olefin diol forms soft segments in the coating film. Therefore, if the olefin diol content is 55% by mass or more, the spin performance of the resulting golf ball is further improved.
[0080] The number average molecular weight of the urethane polyol is preferably 1500 or more, more preferably 2000 or more, and even more preferably 2500 or more, and is preferably 100000 or less, more preferably 80000 or less, and even more preferably 50000 or less. If the number average molecular weight of the urethane polyol is 1500 or more, the distance between the crosslinking points in the coating film becomes longer, and the coating film becomes softer, so that the spin performance is improved. If the number average molecular weight is 100000 or less, the distance between the crosslinking points in the coating film does not become too long, and the coating film has good stain resistance. The number average molecular weight of the urethane polyol component may be measured, for example, by gel permeation chromatography (GPC) using polystyrene as a standard substance, tetrahydrofuran as an eluent, and an organic solvent-based GPC column (for example, "Shodex (registered trademark) KF series" manufactured by Showa Denko KK) as a column.
[0081] The hydroxyl value of the urethane polyol is preferably 10 mgKOH / g or more, more preferably 15 mgKOH / g or more, and even more preferably 20 mgKOH / g or more, and is preferably 200 mgKOH / g or less, more preferably 190 mgKOH / g or less, and even more preferably 180 mgKOH / g or less.
[0082] The hydroxyl value of the polyol contained in the polyol composition is preferably 10 mgKOH / g or more, more preferably 15 mgKOH / g or more, even more preferably 20 mgKOH / g or more, and is preferably 400 mgKOH / g or less, preferably 300 mgKOH / g or less, more preferably 200 mgKOH / g or less, even more preferably 170 mgKOH / g or less, and particularly preferably 160 mgKOH / g or less. If the hydroxyl value of the polyol component is within the above range, the adhesion of the coating film to the golf ball body is improved. In the present invention, the hydroxyl value can be measured, for example, by the acetylation method in accordance with JIS K 1557-1.
[0083] Next, the polyisocyanate composition will be described. The polyisocyanate composition contains one or more polyisocyanates. For example, the polyisocyanate may be a compound having at least two isocyanate groups. In addition, the polyisocyanate directly contained in the polyisocyanate composition may be called the second polyisocyanate from the viewpoint of distinguishing it from the first polyisocyanate constituting the urethane polyol.
[0084] Examples of the second polyisocyanate include aromatic diisocyanates such as 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, a mixture of 2,4-toluene diisocyanate and 2,6-toluene diisocyanate (TDI), 4,4'-diphenylmethane diisocyanate (MDI), 1,5-naphthylene diisocyanate (NDI), 3,3'-bitrylene-4,4'-diisocyanate (TODI), xylylene diisocyanate (XDI), tetramethylxylylene diisocyanate (TMXDI), and paraphenylene diisocyanate (PPDI); 12 MDI), hydrogenated xylylene diisocyanate (H 6Examples of the polyisocyanate include alicyclic diisocyanates or aliphatic diisocyanates such as HDI, hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), and norbornene diisocyanate (NBDI); and triisocyanates such as allophanate, biuret, isocyanurate, and adduct of these diisocyanates. In the present invention, it is preferable to use only one type of polyisocyanate as the polyisocyanate, but two or more types of polyisocyanates may be used. When only one type of polyisocyanate is used, an isocyanurate of HDI, an adduct of HDI, or a biuret of HDI is preferable, and an isocyanurate of HDI is most preferable. This is because the loss modulus of the resulting polyurethane at -50°C is large.
[0085] The allophanate is, for example, a triisocyanate obtained by reacting a diisocyanate with a low molecular weight diol to form a urethane bond, and then further reacting the diisocyanate with the urethane bond. The adduct is a triisocyanate obtained by reacting a diisocyanate with a low molecular weight triol such as trimethylolpropane or glycerin. The biuret is, for example, a triisocyanate having a biuret bond represented by the following formula (2). The isocyanurate of a diisocyanate is, for example, a triisocyanate represented by the following formula (3).
[0086] [ka] TIFF0007585700000002.tif89160 [In formulas (2) and (3), R represents a residue obtained by removing an isocyanate group from a diisocyanate.]
[0087] The polyisocyanate composition preferably contains a triisocyanate. The content of the triisocyanate in the polyisocyanate contained in the polyisocyanate composition is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more. Most preferably, the polyisocyanate composition contains only triisocyanate as the polyisocyanate.
[0088] The amount of isocyanate groups (NCO%) of the polyisocyanate contained in the polyisocyanate composition is preferably 0.5% by mass or more, more preferably 1% by mass or more, even more preferably 2% by mass or more, and is preferably 45% by mass or less, more preferably 40% by mass or less, and even more preferably 35% by mass or less. The amount of isocyanate groups (NCO%) of the polyisocyanate can be expressed as 100 x [the number of moles of isocyanate groups in the polyisocyanate x 42 (the molecular weight of NCO)] / the total mass (g) of the polyisocyanate.
[0089] Specific examples of the polyisocyanate include Burnock D-800, Burnock DN-950, and Burnock DN-955 manufactured by DIC Corporation; Desmodur N75MPA / X, Desmodur N3300, Desmodur L75(C), and Sumidur E21-1 manufactured by Sumika Bayer Urethane Co., Ltd.; Coronate HX and Coronate HK manufactured by Nippon Polyurethane Industry Co., Ltd.; Duranate 24A-100, Duranate 21S-75E, Duranate TPA-100, and Duranate TKA-100 manufactured by Asahi Kasei Chemicals Corporation; and VESTANAT T1890 manufactured by Degussa.
[0090] The polyurethane used in the present invention preferably contains an isocyanurate of a diisocyanate as a polyisocyanate component. The diisocyanate is preferably hexamethylene diisocyanate and / or isophorone diisocyanate.
[0091] The base resin constituting the outermost layer of the coating film of the golf ball of the present invention contains polyurethane obtained by reacting the polyol composition with the polyisocyanate composition. In the reaction between the polyol composition and the polyisocyanate composition, the molar ratio (NCO group / OH group) of the isocyanate group (NCO group) of the polyisocyanate composition to the hydroxyl group (OH group) of the polyol composition is preferably 0.5 or more, more preferably 0.6 or more, and even more preferably 0.8 or more. If the molar ratio (NCO group / OH group) is 0.5 or more, the crosslinking density is high and the stain resistance of the coating film obtained is better. If the molar ratio (NCO group / OH group) is too large, the amount of isocyanate groups becomes excessive, and the coating film obtained becomes hard and brittle, and the appearance is also deteriorated. Therefore, the molar ratio (NCO group / OH group) is preferably 2.0 or less, more preferably 1.8 or less, and even more preferably 1.6 or less. The reason why an excessive amount of isocyanate groups in a coating material results in a poor appearance of the resulting coating film is believed to be that an excessive amount of isocyanate groups increases the reaction between the moisture in the air and the isocyanate groups, resulting in the generation of a large amount of carbon dioxide gas.
[0092] The coating film of the golf ball of the present invention is preferably formed from a paint containing a polyol composition and a polyisocyanate composition. The paint may be a so-called two-component curing paint consisting of a first agent containing a polyol composition and a second agent containing a polyisocyanate composition. The paint may be either a water-based paint using water as a main dispersion medium or a solvent-based paint using an organic solvent as a dispersion medium. In the case of a solvent-based paint, preferred solvents include toluene, isopropyl alcohol, xylene, methyl ethyl ketone, methyl ethyl isobutyl ketone, ethylene glycol monomethyl ether, ethylbenzene, propylene glycol monomethyl ether, isobutyl alcohol, and ethyl acetate.
[0093] The two-component curing paint has a total solid content of the first and second parts of preferably 30% by mass or more, more preferably 31% by mass or more, even more preferably 32% by mass or more, and preferably 45% by mass or less, more preferably 44% by mass or less, even more preferably 43% by mass or less. If the solid content is 30% by mass or more, the paint can be applied uniformly more easily, and the uniformity of the thickness of the coating film is improved, and if it is 45% by mass or less, the leveling property of the paint is good, unevenness of the coating film surface is reduced, and the appearance of the golf ball is improved.
[0094] The paint may further contain, as necessary, additives that may be generally contained in paints for golf balls, such as fillers, ultraviolet absorbers, antioxidants, light stabilizers, fluorescent brightening agents, anti-blocking agents, leveling agents, slip agents, and viscosity modifiers.
[0095] Next, a method for applying the curable coating material of the present invention will be described. The method for applying the curable coating material is not particularly limited, and any known method can be used, such as spray coating or electrostatic coating.
[0096] In the case of spray coating using an air gun, the polyol component and the polyisocyanate component may be supplied by respective pumps and continuously mixed in a line mixer arranged just before the air gun, and the resulting mixture may be spray coated, or the polyol and the polyisocyanate may be spray coated separately using an air spray system equipped with a mixing ratio control mechanism. The coating may be spray coated in one go, or multiple coats may be applied.
[0097] The curable paint applied to the golf ball body can be dried at a temperature of 30° C. to 70° C. for 1 hour to 24 hours to form a coating.
[0098] The golf ball of the present invention has a golf ball body and at least one layer of coating film provided on the surface of the golf ball body, and the base resin constituting the outermost layer of the coating film is not particularly limited, so long as it is a polyurethane obtained by reacting (A) a polyol composition and (B) a polyisocyanate composition.
[0099] When the coating film is a single layer, the base resin of the single layer coating film may be a polyurethane obtained by reacting (A) a polyol composition with (B) a polyisocyanate composition.
[0100] When the coating film has a multi-layer structure of two or more layers, the base resin constituting the coating film of the outermost layer may be a polyurethane obtained by reacting (A) a polyol composition with (B) a polyisocyanate composition. The base resin constituting the layers other than the outermost layer is not particularly limited, and examples thereof include polyurethane, epoxy resin, and acrylic resin.
[0101] In a more preferred embodiment of the present invention, the golf ball has a golf ball body and a two-layer coating film provided on the surface of the golf ball body, and the base resin constituting the outer layer coating film is a polyurethane obtained by reacting (A) a polyol composition and (B) a polyisocyanate composition.
[0102] The thickness of the coating film of the golf ball of the present invention is not particularly limited, but is preferably 5 μm or more, more preferably 6 μm or more, even more preferably 10 μm or more, and particularly preferably 15 μm or more. If the coating film is less than 5 μm, the coating film tends to wear away due to continuous use. In addition, the amount of spin on an approach shot increases by increasing the coating film thickness. In addition, the coating film thickness is preferably 50 μm or less, more preferably 45 μm or less, and even more preferably 40 μm or less. If the coating film thickness is greater than 50 μm, the effect of the dimples may decrease, and the flight performance of the golf ball may decrease. The coating film thickness can be measured, for example, by using a microscope (VHX-1000 manufactured by Keyence Corporation) on the cross section of the golf ball. In addition, when the paint has a multi-layer structure, it is preferable that the thickness of the entire coating film formed is within the above range.
[0103] The golf ball of the present invention is not particularly limited as long as it is a golf ball having a golf ball body and at least one layer of coating film provided on the surface of the golf ball body. The structure of the golf ball body is not particularly limited, and it may be a one-piece golf ball, a two-piece golf ball, a three-piece golf ball, a four-piece golf ball, a multi-piece golf ball having five or more pieces, or a thread-wound golf ball. In any case, the present invention can be suitably applied.
[0104] 1 is a partially cutaway cross-sectional view showing a golf ball according to one embodiment of the present invention. Golf ball 1 has a spherical core 2, a cover 3 that encases spherical core 2, and a coating 4 provided on the surface of cover 3. A large number of dimples 31 are formed on the surface of cover 3. The portions of the surface of cover 3 other than dimples 31 are lands 32.
[0105] The golf ball body preferably has a core and at least one layer of cover covering the core. The slab hardness of the cover composition is preferably set appropriately according to the desired performance of the golf ball. For example, in the case of a distance-type golf ball that emphasizes flight distance, the slab hardness of the cover composition is preferably 50 or more, more preferably 55 or more, and more preferably 80 or less, and more preferably 70 or less in Shore D hardness. By making the slab hardness of the cover composition 50 or more, a golf ball with a high launch angle and low spin can be obtained in driver shots and iron shots, and the flight distance is increased. In addition, by making the slab hardness of the cover composition 80 or less, a golf ball with excellent durability can be obtained. In addition, in the case of a spin-type golf ball that emphasizes controllability, the slab hardness of the cover composition is preferably less than 50, more preferably 20 or more, and more preferably 25 or more in Shore D hardness. If the slab hardness of the cover composition is less than 50 in Shore D hardness, the spin amount of the approach shot is increased. Furthermore, by making the slab hardness 20 or more, the abrasion resistance is improved.
[0106] The cover material constituting the cover is not particularly limited, and examples thereof include various resins such as ionomer resin, polyester resin, urethane resin such as thermoplastic urethane resin or two-component curing urethane resin, polyamide resin, thermoplastic polyamide elastomer commercially available under the trade name "Pebax (registered trademark)" (e.g., "Pebax 2533") from Arkema Co., Ltd., thermoplastic polyester elastomer commercially available under the trade name "Hytrel (registered trademark)" (e.g., "Hytrel 3548", "Hytrel 4047") from Toray DuPont Co., Ltd., thermoplastic polyurethane elastomer commercially available under the trade name "Elastollan (registered trademark)" (e.g., "Elastollan XNY97A") from BASF Japan Ltd., thermoplastic styrene elastomer commercially available under the trade name "Tefabloc (registered trademark)" from Mitsubishi Chemical Corporation, or thermoplastic polyester elastomer commercially available under the trade name "Primalloy". The cover materials may be used alone or in combination of two or more kinds.
[0107] In addition to the resin components described above, the cover may contain pigment components such as white pigments (e.g., titanium oxide), blue pigments, and red pigments, specific gravity adjusters such as calcium carbonate and barium sulfate, dispersants, antioxidants, ultraviolet absorbers, light stabilizers (e.g., bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate), fluorescent materials, or fluorescent brighteners, to the extent that the performance of the cover is not impaired.
[0108] The manner in which the cover is molded using the cover composition is not particularly limited, but examples thereof include a manner in which the cover composition is directly injection molded onto the core, or a manner in which a hollow shell is molded from the cover composition, the core is covered with a plurality of shells, and compression molded (preferably, a method in which a hollow half shell is molded from the cover composition, the core is covered with two half shells, and compression molded). The golf ball body with the molded cover is removed from the mold, and is preferably subjected to surface treatment such as deburring, cleaning, and sandblasting as necessary. Also, a mark can be formed as desired.
[0109] The total number of dimples formed on the cover is preferably 200 to 500 inclusive. If the total number of dimples is less than 200, the effect of the dimples is difficult to obtain. If the total number of dimples is more than 500, the size of each dimple becomes small, making it difficult to obtain the effect of the dimples. The shape (shape in plan view) of the dimples formed is not particularly limited, and may be a circle; a polygon such as an approximately triangular, approximately rectangular, approximately pentagonal, or approximately hexagonal; or other irregular shape; or may be used alone or in combination of two or more types.
[0110] In the present invention, the ratio of the total area of all dimples to the surface area of a virtual sphere is called the occupation ratio. A virtual sphere is a golf ball (spherical body) when dimples are not present. In the golf ball of the present invention, the occupation ratio of dimples is preferably 60% or more, more preferably 63% or more, even more preferably 66% or more, preferably 90% or less, more preferably 87% or less, and even more preferably 84% or less. If the occupation ratio is too high, the contribution of the coating film to the coefficient of friction is reduced. Also, if the occupation ratio is too low, the flight performance is reduced.
[0111] The area of a dimple is the area of the region enclosed by the outline when looking at the center of the golf ball from infinity. For a circular dimple, the area S is calculated using the following formula: S = (Di / 2) 2 π (Di: dimple diameter)
[0112] The diameter of the golf ball is preferably 40mm to 45mm. From the viewpoint of meeting the standards of the United States Golf Association (USGA), the diameter is preferably 42.67mm or more. From the viewpoint of air resistance, the diameter is preferably 44mm or less, and more preferably 42.80mm or less. The mass of the golf ball is preferably 40g or more and 50g or less. From the viewpoint of obtaining large inertia, the mass is preferably 44g or more, and more preferably 45.00g or more. From the viewpoint of meeting the standards of the USGA, the mass is preferably 45.93g or less.
[0113] Next, the cores used in wound golf balls, two-piece golf balls and multi-piece golf balls, as well as the one-piece golf ball body will be described.
[0114] A known rubber composition (hereinafter, sometimes simply referred to as a "rubber composition for the core") can be used for the core and the one-piece golf ball body. For example, a rubber composition containing a base rubber, a co-crosslinking agent, and a crosslinking initiator can be molded by hot pressing.
[0115] As the base rubber, it is preferable to use high-cis polybutadiene having cis bonds of 40% by mass or more, preferably 70% by mass or more, more preferably 90% by mass or more, which is advantageous for resilience. As the co-crosslinking agent, α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms or its metal salt is preferable, and metal salt of acrylic acid or metal salt of methacrylic acid is more preferable. As the metal salt, zinc, magnesium, calcium, aluminum, and sodium are preferable, and zinc is more preferable. The amount of the co-crosslinking agent used is preferably 20 parts by mass or more and 50 parts by mass or less per 100 parts by mass of the base rubber. As the crosslinking initiator, an organic peroxide is preferably used. Specifically, organic peroxides such as dicumyl peroxide, 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, and di-t-butyl peroxide can be mentioned, and among these, dicumyl peroxide is preferably used. The amount of the crosslinking initiator mixed is preferably at least 0.2 part by mass, and more preferably at least 0.3 part by mass, and is preferably at most 3 parts by mass, and more preferably at most 2 parts by mass, per 100 parts by mass of the base rubber.
[0116] The core rubber composition may further contain an organic sulfur compound. As the organic sulfur compound, diphenyl disulfides, thiophenols, and thionaphthols can be suitably used. The amount of the organic sulfur compound is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, and preferably 5.0 parts by mass or less, more preferably 3.0 parts by mass or less, per 100 parts by mass of the base rubber. The core rubber composition may further contain a carboxylic acid and / or a salt thereof. As the carboxylic acid and / or a salt thereof, a carboxylic acid having 1 to 30 carbon atoms and / or a salt thereof is preferred. The amount of the carboxylic acid and / or a salt thereof is 1 part by mass or more and 40 parts by mass or less, per 100 parts by mass of the base rubber.
[0117] The core rubber composition may further contain, in addition to the base rubber, co-crosslinking agent, crosslinking initiator, and organic sulfur compound, a weight adjuster such as zinc oxide or barium sulfate, an antiaging agent, color powder, etc. The hot press molding conditions for the core rubber composition may be appropriately set according to the rubber composition, but it is usually preferable to heat the core rubber composition at 130°C to 200°C for 10 to 60 minutes, or to heat the core rubber composition at 130°C to 150°C for 20 to 40 minutes, and then heat the core rubber composition at 160°C to 180°C for 5 to 15 minutes in two stages.
[0118] In the case where the golf ball of the present invention is a multi-piece golf ball such as a three-piece golf ball, a four-piece golf ball, a five-piece golf ball or more, the intermediate layer provided between the core and the outermost cover layer may be, for example, a thermoplastic resin such as polyurethane resin, ionomer resin, polyamide resin, or polyethylene; a thermoplastic elastomer such as a styrene elastomer, a polyolefin elastomer, a polyurethane elastomer, or a polyester elastomer; or a cured product of a rubber composition. Here, examples of the ionomer resin include a copolymer of ethylene and α,β-unsaturated carboxylic acid in which at least a part of the carboxyl groups is neutralized with a metal ion, or a ternary copolymer of ethylene, α,β-unsaturated carboxylic acid, and α,β-unsaturated carboxylic acid ester in which at least a part of the carboxyl groups is neutralized with a metal ion. The intermediate layer may further contain a specific gravity adjuster such as barium sulfate or tungsten, an antioxidant, a pigment, or the like. The intermediate layer may be called an inner cover layer or an outer core layer depending on the configuration of the golf ball. EXAMPLES
[0119] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the following examples, and all modifications and embodiments that do not deviate from the spirit of the present invention are included within the scope of the present invention.
[0120] [Evaluation method] (1) Weight average molecular weight (Mw) and number average molecular weight (Mn) of olefin diol The weight average molecular weight (Mw) and number average molecular weight (Mn) of olefin diols were measured using a gel permeation chromatography (GPC) system HLC-8220 (Tosoh Corporation) with two H-type columns HZ-M (Tosoh Corporation) connected in series, tetrahydrofuran as the solvent, and a column temperature of 40°C. The detector used was a differential refractometer RI-8320 (Tosoh Corporation). The weight average molecular weight (Mw) and number average molecular weight (Mn) of olefin diols were measured in terms of polystyrene.
[0121] (2) Glass transition temperature (Tg) of olefin diol Using a differential scanning calorimeter (DSC, product name "X-DSC7000", manufactured by Hitachi High-Tech Science Corporation), measurements were performed from -150°C to 40°C at a heating rate of 10°C / min, and the glass transition temperature (Tg) was calculated from the measurement results.
[0122] (3) Viscosity of Olefin Diol The melt viscosity at 25°C was measured using a Brookfield viscometer DV-II+Pro (manufactured by Brookfield). A cone-plate type was used, and CPE-52 was used as the cone (spindle). The shear rate during the measurement was set to 1.2 sec according to the viscosity. -1 ~10sec -1 was adjusted between.
[0123] (4) Measurement of dynamic viscoelasticity The storage modulus E', loss modulus E'', and loss tangent tan δ of the coating film were measured under the following conditions. Equipment: Dynamic viscoelasticity measuring device Rheogel-E4000 manufactured by UBM Measurement sample: A paint containing a base agent and a hardener was dried and hardened at 40°C for 4 hours to produce a coating film with a thickness of 0.11-0.14 mm. A sample piece with a width of 4 mm and a clamp distance of 20 mm was cut out from this coating film. Measurement mode: Sine wave tension Measurement temperature: -120℃~100℃ Heating rate: 3℃ / min Measurement data capture interval: 3℃ Excitation frequency: 10Hz Measurement distortion: 0.05%
[0124] (5) 10% modulus of coating The tensile properties of the coating film were measured according to JIS K7161 (2014). Specifically, a coating material containing a polyisocyanate composition and a polyol composition was dried and cured at 40°C for 4 hours to produce a coating film (thickness 0.05 mm). This coating film was punched out into a test piece type 2 (parallel part width 10 mm, gauge length 50 mm) specified in JIS K7127 (1999) to produce a test piece. A tensile test was performed on this test piece using a precision universal testing machine (Shimadzu Corporation, Autograph (registered trademark)). The test conditions were a gripper distance of 100 mm, a tensile speed of 50 mm / min, and a test temperature of 23°C. The tensile stress at 10% strain (10% modulus) was then recorded.
[0125] (6) Dry spin rate on approach shots Sd (rpm) A sand wedge (Cleveland Golf RTX-3 (58°)) was attached to a swing machine manufactured by Golf Laboratory, and a golf ball was hit at a head speed of 16 m / sec. The spin rate (rpm) was measured by continuously photographing the hit golf ball. The measurement was performed eight times for each golf ball, and the average value was taken as the spin rate.
[0126] (7) Rough spin rate Sr (rpm) on approach shots from the rough A sand wedge (Cleveland Golf RTX-3 (58°)) was attached to a Golf Laboratory swing machine. A golf ball with two pieces of wild grass attached to its surface was used, and the golf ball was hit with a head speed of 16 m / s with the wild grass between the sand wedge face and the golf ball, and the spin rate (rpm) was measured. The spin rate was measured by taking a series of photographs of the hit golf ball. The wild grass was attached to the golf ball with cellophane tape so that the wild grass and the grooves on the face were perpendicular when the sand wedge face and the golf ball came into contact. Each golf ball was measured eight times, and the average value of the data obtained was calculated.
[0127] [Manufacturing golf balls] 1. Preparation of the Center The rubber composition for the center shown in Table 1 was kneaded and then hot-pressed at 170°C for 20 minutes in upper and lower molds having hemispherical cavities to obtain a spherical center with a diameter of 39.7 mm. The amount of barium sulfate was adjusted so that the mass of the golf ball was 45.3 g.
[0128] [Table 1] Polybutadiene rubber: JSR Corporation, "BR730 (high cis polybutadiene)" Zinc acrylate: Nisshoku Techno Fine Chemical Co., Ltd., "ZN-DA90S" Zinc oxide: "Ginrei R" manufactured by Toho Zinc Co., Ltd. Barium sulfate: Sakai Chemical Industry Co., Ltd., "Barium Sulfate BD" Diphenyl disulfide: Sumitomo Seika Chemicals Dicumyl peroxide: NOF Corporation, "Percumyl (registered trademark) D"
[0129] 2. Preparation of intermediate layer composition and cover composition The materials shown in Tables 2 and 3 were mixed in a twin-screw extruder to prepare pellets of an intermediate layer composition and a cover composition. The extrusion conditions were a screw diameter of 45 mm, a screw rotation speed of 200 rpm, and a screw L / D of 35, and the mixture was heated to 200 to 260°C at the die of the extruder.
[0130] [Table 2] Surlyn® 8945: Sodium ion neutralized ethylene-methacrylic acid copolymer ionomer resin manufactured by DuPont Himilan (registered trademark) AM7329: Zinc ion neutralized ethylene-methacrylic acid copolymer ionomer resin manufactured by Mitsui DuPont Polychemicals Co., Ltd.
[0131] [Table 3] Elastollan (registered trademark) XNY82A: Thermoplastic polyurethane elastomer manufactured by BASF Japan Ltd. Tinuvin (registered trademark) 770: bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate, manufactured by BASF Japan Ltd.
[0132] 3. Preparation of Spherical Cores The intermediate layer composition obtained above was directly injection molded onto the spherical center to form an intermediate layer having a thickness of 1.0 mm that covered the center, thereby producing a spherical core. The upper and lower molds for molding have a hemispherical cavity and a hold pin that can be advanced and retreated to support the spherical center. When molding the intermediate layer, the hold pin is pushed out and the center is inserted and held, and the intermediate layer composition heated to 260°C is injected in 0.3 seconds into the mold closed with a pressure of 80 tons, cooled for 30 seconds, and the mold is opened to remove the spherical core.
[0133] 4. Forming the half shell The half shells were compressed by putting the pellets of the cover composition into each recess of the lower mold of the half shell molding die, and pressing the pellets to form the half shells. The compression molding was performed under the conditions of a molding temperature of 170°C, a molding time of 5 minutes, and a molding pressure of 2.94 MPa.
[0134] 5.Cover molding The spherical core obtained above was concentrically covered with two half shells, and a cover having a thickness of 0.5 mm was formed by compression molding under the conditions of a molding temperature of 145°C, a molding time of 2 minutes, and a molding pressure of 9.8 MPa.
[0135] 6. Paint Preparation Preparation of the first agent (polyol composition) As the polyol component, polyoxytetramethylene glycol (PTMG) or olefin diol (PCP1 to PCP4), trimethylolpropane (TMP) was dissolved in a solvent (toluene / methyl ethyl ketone = 1 / 2, mass ratio) to 50 mass%. Dibutyltin laurate was added as a catalyst to the polyol component to be 0.1 mass% based on the solid content. While maintaining this polyol solution at 80 ° C, isophorone diisocyanate (IPDI) as a polyisocyanate component was added dropwise. After dropping, stirring was continued until the isocyanate disappeared, and then cooled to room temperature, and a solvent (toluene / methyl ethyl ketone = 1 / 2, mass ratio) was added to prepare a urethane polyol (solid content: 30 mass%). The composition of each urethane polyol is shown in Table 4.
[0136] [Table 4]
[0137] The following polyolefin diols were used: PCP1: Liquid polycyclopentene (poly(cyclopentene)diol) with hydroxyl groups at both ends, manufactured by Zeon Corporation, number average molecular weight 1000 PCP2: Liquid polycyclopentene (poly(cyclopentene)diol) with hydroxyl groups at both ends, manufactured by Zeon Corporation, number average molecular weight 2000 PCP3: Liquid polycyclopentene (poly(cyclopentene)diol) with hydroxyl groups at both ends, manufactured by Zeon Corporation, number average molecular weight 3100 PCP4: Liquid polycyclopentene (poly(cyclopentene)diol) with hydroxyl groups at both ends, manufactured by Zeon Corporation, number average molecular weight 4100
[0138] Preparation of second agent (polyisocyanate composition) Polyisocyanate composition No. 1: Isocyanurate of hexamethylene diisocyanate (Sumidur N3300, manufactured by Sumika Covestro Urethane Co., Ltd.) Polyisocyanate composition No. 2: A mixture of an isocyanurate of hexamethylene diisocyanate (Sumidur N3300, manufactured by Sumika Covestro Urethane Co., Ltd.) and an isocyanurate of isophorone diisocyanate (Desmodur Z4470, manufactured by Sumika Covestro Urethane Co., Ltd.) in a molar ratio of 1:1 A mixed solvent of methyl ethyl ketone, n-butyl acetate, and toluene was added as a solvent to the polyisocyanate compositions Nos. 1 and 2, and the concentration of the polyisocyanate component was adjusted to 60% by mass.
[0139] Preparation of paint The second agent was added to the first agent (urethane polyol) prepared above so as to obtain the NCO / OH molar ratio shown in Table 5, to prepare a coating material.
[0140] 7. Formation of coating film The surface of the golf ball body obtained above was sandblasted and marked, and then paint was applied with a spray gun and the paint was dried in an oven at 40°C for 24 hours to obtain a golf ball with a diameter of 42.7 mm and a mass of 45.3 g. The thickness of the coating was 20 μm. The coating was performed by placing the golf ball body on a rotating body equipped with three prongs, rotating the rotating body at 300 rpm, and moving the air gun vertically at a spray distance (7 cm) from the golf ball body. The interval between each recoat was 1.0 second. The spray conditions of the air gun were as follows: recoat; 2 times, spray air pressure; 0.15 MPa, pressure tank air pressure; 0.10 MPa, application time per time; 1 second, ambient temperature; 20°C to 27°C, ambient humidity; 65% or less. The evaluation results of the obtained golf ball are shown in Table 5.
[0141] [Table 5]
[0142] Golf balls No. 2 to No. 5, 7, 8, and 10 are golf balls having a golf ball body and at least one layer of coating film provided on the surface of the golf ball body, The base resin constituting the outermost layer of the coating film is a polyurethane obtained by reacting (A) a polyol composition with (B) a polyisocyanate composition, and the dynamic viscoelasticity of the polyurethane is measured under the following conditions, and the loss modulus (E") at -50°C is 0.2 x 10 8 Pa or more, and the peak temperature of the loss tangent (tan δ) is 0° C. or less. Golf balls Nos. 2 to 5, 7, 8 and 10 have excellent spin performance. [Industrial Applicability]
[0143] The present invention is suitably applicable to painted golf balls. [Explanation of symbols]
[0144] 1: Golf ball, 2: Spherical core, 3: Cover, 4: Coating, 31: Dimples, 32: Land
Claims
1. A golf ball having a golf ball body and at least one layer of coating film provided on a surface of the golf ball body, the base resin constituting the outermost layer of the coating film is polyurethane; The polyurethane is a polyurethane obtained by reacting (A) a polyol composition with (B) a polyisocyanate composition, the polyol composition (A) contains a urethane polyol, the urethane polyol contains an olefin diol having a linear structure as a constituent component, The golf ball is characterized in that the dynamic viscoelasticity of the polyurethane is measured under the following conditions, and the loss modulus (E") at -50°C is 0.3 x 108 Pa or more and 1.9 x 108 Pa or less, and the peak temperature of the loss tangent (tan δ) is -55°C or more and -40°C or less. <Measurement conditions> Measurement mode: Sine wave tension Measurement temperature range: -120℃ to 100℃ Heating rate: 3°C / min Excitation frequency: 10Hz Measured distortion: 0.05%
2. 2. The golf ball according to claim 1, wherein the polyurethane has a storage modulus (E') at 0° C. of 0.1×10 8 Pa or more and 0.7×10 8 Pa or less.
3. 3. The golf ball according to claim 1, wherein the linear olefin diol is a compound having a linear main chain which is formed by ring-opening polymerization of a cycloolefin and has hydroxy groups at both ends of the main chain.
4. 4. The golf ball according to claim 3, wherein the linear olefin diol is a copolymer having a monomer unit obtained by ring-opening polymerization of a monocyclic cycloolefin monomer and a monomer unit obtained by ring-opening polymerization of a polycyclic cycloolefin monomer.
5. 5. The golf ball according to claim 3, wherein the linear olefin diol is a copolymer having a monomer unit obtained by ring-opening polymerization of cyclopentene and a monomer unit obtained by ring-opening polymerization of a compound having a norbornene ring.
6. (B) A golf ball described in any one of claims 1 to 5, characterized in that the polyisocyanate composition contains an isocyanurate of a diisocyanate as a polyisocyanate component.
7. 7. The golf ball according to claim 6, wherein the diisocyanate is hexamethylene diisocyanate and / or isophorone diisocyanate.
Citation Information
Patent Citations
Golf ball
JP2011067595A
Golf ball
JP2011217820A
Golf ball
JP2014014383A
Golf ball
JP2017209298A
Golf ball
JP2020069309A