Apparatus and method for producing polymer thin film

The described method and apparatus efficiently produce polymer thin films with specific shapes by applying polymeric material to a textured mold, transferring it to a stretchable sheet, and peeling off the film, addressing productivity and complexity issues in existing methods while ensuring only the desired shape is collected.

JP7585836B2Active Publication Date: 2024-11-19TORAY INDUSTRIES INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021017069
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-11
Filing Date
2021-02-05
Publication Date
2024-11-19
Estimated Expiration
2041-02-05

Smart Images

  • Figure 0007585836000001
    Figure 0007585836000001
  • Figure 0007585836000002
    Figure 0007585836000002
  • Figure 0007585836000003
    Figure 0007585836000003
Patent Text Reader

Abstract

To provide a method for efficiently continuously and uniformly manufacturing a polymer thin film having a specific shape, and a manufacturing apparatus for realizing the manufacturing method.SOLUTION: A manufacturing method for manufacturing a polymer thin film having a specific shape of the present invention includes: conveying a mold in which an irregularity is formed on a surface and a shape of a top surface of a convex part is a specific shape; applying a coating material containing a polymer material to a surface on which the irregularity is formed so as to cover the top surface of the convex part; forming a polymer film by drying the applied polymer material; transferring the polymer film formed on the top surface of the convex part to a transfer sheet by pressing the surface formed with the irregularity against one surface of the elastic transfer sheet; and collecting the polymer thin film peeled off from the transfer sheet by stretching or expanding and contracting the transfer sheet at least once, and peeling off the transferred polymer film from the transfer sheet to obtain the polymer thin film.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method and an apparatus for producing a polymer thin film having a specific shape by applying a polymer material onto a mold having a specific shape and then peeling and recovering the material. [Background technology]

[0002] As a method for producing a polymer thin film having a specific shape, there is a method in which a polymer material is applied onto a mold having a specific shape, and before drying, the polymer material is transferred onto a water-soluble polymer film separate from the polymer material, and the water-soluble polymer is then dissolved in water to obtain a polymer thin film having a specific shape (e.g., Patent Documents 1 and 2).

[0003] However, the methods of Patent Documents 1 and 2 require a process of applying a sacrificial film as a water-soluble polymer film and then dissolving the water-soluble polymer film to remove the polymer film, which makes the process complicated and reduces productivity.

[0004] To solve this problem, Patent Document 3 discloses a method for producing a polymer thin film having a specific shape without using a sacrificial film. Specifically, Patent Document 3 discloses a method for producing a polymer thin film by carrying out the following steps in order. (a) A stretchable mold is transported, the mold having projections and recesses formed on its surface, the top surfaces of the projections having a specific shape. (b) A polymeric material is applied to the surface on which the projections are formed so as to cover the top surfaces of the projections of the transported mold. (c) The applied polymer material is dried to form a polymer film. (d) The mold is stretched or contracted one or more times to peel off the dried polymer film from the top surface of the protrusions to obtain a thin polymer film. (e) The polymer thin film is peeled off from the mold and collected.

[0005] According to Patent Document 3, the process of applying a sacrificial film as a water-soluble polymer film, then dissolving the water-soluble polymer film, and extracting the polymer film can be omitted, which is said to reduce the cost of polymer film production and improve productivity. In addition, since there is no process of dissolving the water-soluble polymer film and the polymer film can be collected in a dry state, it can be handled as fine particles, which is said to expand the range of applications. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2006 / 025592 [Patent Document 2] International Publication No. 2008 / 050913 [Patent Document 3] International Publication No. 2019 / 116951 Summary of the Invention [Problem to be solved by the invention]

[0007] In the method for producing a polymer thin film described in Patent Document 3, when the mold is expanded and contracted to peel off the polymer film from the top surface of the convex parts of the mold, the part between the convex parts of the mold also expands and contracts, so that the thin thread-like polymer film that is applied to this part and dried may peel off together. If the polymer film peels off from this part, not only the polymer thin film having a specific shape but also the thread-like polymer thin film will be collected together. If the application does not cause any particular problem even if some polymer thin films other than the polymer thin film having a specific shape are mixed in, this is acceptable, but if the application is such that only the polymer thin film having a specific shape can be used, it is necessary to select only the polymer thin film having a specific shape after collection, which may be troublesome.

[0008] The present invention provides a method for efficiently, continuously and uniformly producing a polymer thin film having a specific shape, and a production apparatus for implementing the production method. [Means for solving the problem]

[0009] The polymer thin film manufacturing apparatus of the present invention that solves the above problems is an apparatus for manufacturing a polymer thin film having a specific shape, comprising: A mold having projections and recesses formed on its surface, the top surfaces of the projections having the specific shape; a mold supplying means for supplying the mold; a coating unit that coats a coating material including a polymer material on the surface on which the projections and recesses are formed so as to cover the top surfaces of the projections of the mold transported by the mold supply means; a drying unit located downstream of the coating unit in the conveying direction and drying the coated polymer material to form a polymer film; A transfer sheet supplying means for supplying a stretchable transfer sheet; a transfer unit, which is located downstream of the drying unit in the conveying direction, for pressing one surface of the transfer sheet supplied by the transfer sheet supplying means against the surface of the mold on which the concaves and convexes are formed, thereby transferring the polymer coating formed on the top surfaces of the convex portions of the mold to the transfer sheet; a peeling unit for peeling the transferred polymer film from the transfer sheet by stretching or stretching the transfer sheet one or more times to obtain a polymer thin film; and a recovery unit for recovering the polymer thin film peeled off from the transfer sheet.

[0010] Further, a manufacturing method of the present invention that solves the above-mentioned problems is a manufacturing method for manufacturing a polymer thin film having a specific shape, comprising the steps of: Transporting a mold having projections and recesses formed on its surface, the top surfaces of the projections having the specific shape; Next, a coating material including a polymer material is applied to the surface on which the projections and recesses are formed so as to cover the top surfaces of the projections of the transported mold; Next, the applied polymer material is dried to form a polymer film; Next, one surface of a transfer sheet having elasticity is pressed against the surface of the mold on which the projections and recesses are formed, so that the polymer coating formed on the top surfaces of the projections of the mold is transferred to the transfer sheet; The transfer sheet is then stretched or flexed one or more times to peel the transferred polymer coating from the transfer sheet to obtain the polymer thin film, and the polymer thin film peeled from the transfer sheet is recovered. Effect of the Invention

[0011] According to the present invention, a polymeric material is directly applied onto a textured film, a specific shape is imparted to the polymeric material, and then the polymeric material is transferred onto an elastic transfer sheet, and the polymeric thin film can be recovered in a dry state.

[0012] Since the process of applying a sacrificial film as a water-soluble polymer film and then dissolving the water-soluble polymer film to extract the polymer film as in the conventional technology can be omitted, the cost of polymer film production can be reduced and the productivity can be improved. In addition, since the present invention does not require a process of dissolving the water-soluble polymer film and can collect the polymer film in a dry state, it can be handled as fine particles, and the applications can be expanded.

[0013] Furthermore, the present invention makes it possible to efficiently produce only thin polymer films having specific shapes in a continuous and uniform manner. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a schematic cross-sectional view of an apparatus for producing a polymer thin film of the present invention. [Diagram 2] Figure 2 is a schematic diagram of an example of a mold applied to the present invention, in which (a) shows a mold with a circular top surface of the protrusion, and (b) shows a mold with a polygonal top surface of the protrusion. [Diagram 3] FIG. 3 is a schematic cross-sectional view of a peeling unit of the polymer thin film production apparatus of the present invention. [Figure 4] FIG. 4 is a schematic cross-sectional view of an apparatus for producing a polymer thin film according to another embodiment of the present invention. [Diagram 5] FIG. 5 is a schematic cross-sectional view of an apparatus for producing a polymer thin film according to another embodiment of the present invention. [Figure 6] FIG. 6 is a schematic cross-sectional view of an apparatus for producing a polymer thin film according to another embodiment of the present invention. [Figure 7] FIG. 7 is a schematic diagram showing a state in which a polymer coating is formed on the top surface of a convex portion of a mold. [Figure 8] FIG. 8 is a schematic diagram showing the behavior of the thin polymer film and the transfer sheet in the peeling unit used in the present invention. [Figure 9] FIG. 9 is a photograph of a laminate of a transfer sheet and a polymer thin film obtained in the middle of the production method of the present invention, observed with an electron microscope. [Figure 10] FIG. 10 is a photograph of the polymer thin film having a specific shape produced in Example 1, observed by an electron microscope. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The apparatus for producing a polymer thin film having a specific shape according to the present invention includes at least the following devices or members (a) to (i). (a) A mold having projections and recesses formed on its surface, the top faces of the projections having the specific shape described above. (b) A mold supply means for supplying and transporting the mold. (c) a coating unit that applies a coating material containing a polymeric material to the surface of the mold on which the projections and recesses are formed so as to cover the top surfaces of the projections of the mold transported by the mold supplying means. (d) a drying unit located downstream of the coating unit in the conveying direction, for drying the coated polymer material to form a polymer film. (e) A transfer sheet having elasticity. (f) A transfer sheet supplying means for supplying and transporting the transfer sheet. (g) a transfer unit, which is located downstream of the drying unit in the mold transport direction, and presses one side of the transfer sheet supplied by the transfer sheet supply means against the mold surface on which the concaves and convexes are formed, thereby transferring the polymer coating formed on the top surfaces of the convex portions of the mold to the transfer sheet. (h) a peeling unit for peeling the transferred polymer film from the transfer sheet by stretching or expanding the transfer sheet one or more times to obtain a thin polymer film. (i) a recovery unit for recovering the polymer thin film peeled off from the transfer sheet;

[0016] FIG. 1 is a schematic cross-sectional view of an example of a polymer thin film manufacturing apparatus according to the present invention. FIG. 2 is a schematic cross-sectional view of an example of a mold applied to the present invention. FIG. 2(a) is a schematic cross-sectional view of a mold with a circular top surface and FIG. 2(b) is a schematic cross-sectional view of a mold with a polygonal top surface of a convex portion. The top surface 15a of the convex portion 15 having an uneven structure on the surface of the mold 11 has a shape corresponding to the specific shape of the polymer thin film 16 to be finally obtained. The polymer thin film 16 manufacturing apparatus 10 applies a coating material 13 containing a polymer material so as to cover the top surface 15a of the convex portion 15 of the mold 11 having an uneven surface, dries the coating material 13 to form a polymer film 14, transfers the polymer film 14 to one side of a transfer sheet 51 having elasticity, peels off the polymer film 14 by the expansion and contraction of the transfer sheet 51 to obtain a polymer thin film 16, and collects the polymer thin film 16 having a specific shape that is the same as the top surface 15a of the convex portion 15 by a collection unit 80.

[0017] The coating material 13 containing a polymeric material may be one in which the polymeric material is dissolved in a solvent, or one in which the polymeric material is melted by heating. In consideration of ease of application, it is preferable to select one in which the polymeric material is dissolved in a solvent, since this makes it easy to adjust the viscosity and solid content of the coating material 13.

[0018] 1, the apparatus 10 for producing a polymer thin film 16 of the present invention includes a roll-shaped mold 11 having an uneven surface, a mold supplying means 20 for driving and transporting the mold 11, a coating unit 30 for coating the surface of the mold 11 with a coating material 13, a drying unit 40 for drying the applied coating material 13, a roll-shaped stretchable transfer sheet 51, a transfer sheet supplying means 50 for driving and transporting the transfer sheet 51, a transfer unit 60 for transferring a polymer film 14 from the surface of the mold 11 to one side of the transfer sheet 51, a peeling unit 70 for peeling the polymer film 14 from the transfer sheet 51, and a recovery unit 80 for recovering the peeled polymer thin film 16. The outline of each component is as follows.

[0019] The roll-shaped mold 11 has an uneven surface, and the top surface 15a of the protrusions 15 has a specific shape, such as a circle (see FIG. 2(a)) or a polygon (see FIG. 2(b)). The mold 11 is made of a material that is resistant to chemicals such as the solvent used in the coating material 13, and preferably has a uniform thickness so that the coating material 13 can be uniformly applied. Here, chemical resistance means that the volume change rate when the mold 11 is immersed in the chemical used in the coating material 13 at room temperature for 72 hours in a test based on JIS-K-6258 (2003 edition) is 5% or less. Without chemical resistance, the surface of the mold 11 may swell due to the chemical, which may hinder the peeling of the polymer film 14 or cause the unevenness of the surface of the mold 11 to collapse, so it is preferable that the mold 11 has chemical resistance.

[0020] The mold supplying means 20 includes an unwinding roll 21 that unwinds the mold 11 wound in a roll shape, a winding roll 22 that winds up the unwound mold 11, a driving roll 23 that transports the mold 11 at a constant speed, a driving means (not shown) that rotates each roll, and guide rolls 21a, 22a to match the mold transport path. It is preferable that the transport tension of the unwinding roll 21 and the winding roll 22 can be adjusted, and it is preferable to control the tension so that the amount of elongation of the mold 11 in the transport direction during transport is 1% or less. The transport speed of the mold 11 is adjusted by the driving roll 23 arranged opposite the nip roll 24.

[0021] The coating unit 30 may be any unit capable of uniformly, continuously and consistently coating the coating material 13 in the width direction of the mold 11. For example, the coating unit 30 may have a structure in which a discharger consisting of a slit die 31 as shown in FIG. 1 is combined with a liquid delivery mechanism capable of continuously supplying a fixed amount of coating material. In order to maintain the gap between the discharge tip surface of the slit die 31 and the mold 11 with high precision, a support roll 32 may be disposed on the opposite side of the coating surface of the mold 11. It is also preferable to provide a position adjustment mechanism that allows the position of the slit die 31 to be adjusted left and right with high resolution.

[0022] The drying unit 40 is preferably equipped with a heating means such as hot air or far infrared rays in order to quickly dry the applied coating material 13. In addition, it may be equipped with a local exhaust device for recovering or exhausting the evaporated solvent.

[0023] The roll-shaped stretchable transfer sheet 51 has a surface for transferring the polymer film 14, and the surface may be smooth or may have minute irregularities. If the surface is smooth, the contact area with the polymer film 14 during transfer is large, allowing for good transfer. On the other hand, if the surface has minute irregularities, the contact area with the polymer film 14 is small when peeling off the polymer film 14, allowing for good peeling. Either surface shape of the transfer sheet 51 may be selected depending on the polymer thin film 16 that is ultimately desired.

[0024] The transfer sheet supplying means 50 includes an unwinding roll 52 that unwinds the transfer sheet 51, a take-up roll 53 that takes up the unwound transfer sheet 51, drive rolls 55 and 56 that transport the transfer sheet 52 at a constant speed, a drive means (not shown) that rotates each roll, and guide rolls 52a and 53a to match the transport path of the transfer sheet 51. It is preferable that the transport tension of the unwinding roll 52 and the take-up roll 53 can be adjusted, and it is preferable to control the tension so that the amount of elongation in the transport direction of the transfer sheet 51 during transport is 10% or less. The transport speed of the transfer sheet 51 is adjusted by a drive roll 55 arranged opposite the nip roll 73 and a drive roll 56 arranged opposite the nip roll 74.

[0025] The transfer unit 60 includes a nip roll 62 that supports the mold 11 during transfer, and a nip roll 61 that presses the mold 11 so that the surface on which the projections and recesses are formed comes into contact with one surface of the transfer sheet 51. Although not shown, it is preferable to include a driving means for driving each roll and a heating means for heating each roll.

[0026] The peeling unit 70 includes the nip roll 73, the drive roll 55, the nip roll 74, and the drive roll 56, which function as a tension blocking mechanism for blocking the tension applied to the transport of the transfer sheet 51 in the peeling section, which is a transport path connecting the nip roll 73, the tension adjusting roll 75, and the nip roll 74, and the tension adjusting roll 75, which functions as a tension adjusting mechanism for adjusting the tension for stretching the transfer sheet 51 to the elongation required for peeling the polymer film 14 from the transfer sheet 51. It is preferable to block the tension generated by the transfer sheet supplying means 50 by nipping the transfer sheet 51 between the nip roll 73 and the drive roll 55, and between the nip roll 74 and the drive roll 56, which function as a tension blocking mechanism. It is sufficient for the tension adjusting mechanism to be able to extend the length of the transfer sheet 51 to the length required for peeling the polymer film 14 from the transfer sheet 51. Specifically, a mechanism is preferred in which tension is applied by tension adjustment roll 75 to transfer sheet 51 held by nip roll 73 and drive roll 55, and nip roll 74 and drive roll 56, from the side of transfer sheet 51 opposite to the side to which polymer coating 14 is transferred, thereby stretching transfer sheet 51. According to the inventors' investigations, it is preferable that the length of transfer sheet 51 can be stretched to at least twice the length of the peeling section before tension is applied.

[0027] The recovery unit 80 includes a means for recovering the polymer thin film 16 peeled off from the transfer sheet 51. The recovery means preferably uses a suction nozzle 81 connected to a negative pressure generator 82 such as a vacuum pump. Alternatively, a recovery method may be used in which a liquid is made to flow over the polymer coating 14 transferred to the transfer sheet 51, and the polymer thin film 16 is dispersed in the liquid. In addition, in any case where any recovery means is used, it is preferable to place a collection material 83 such as a nonwoven fabric or a membrane filter in the path along which the polymer thin film 16 flows in order to collect the polymer thin film 16 recovered by the recovery means.

[0028] A series of manufacturing operations by the manufacturing apparatus 10 for the polymer thin film 16 is as follows. The mold 11 is unwound from the unwinding roll 21, passes through the coating unit 30, the drying unit 40, and the transfer unit 60, and is wound up on the winding roll 22. The mold supplying means 20 gives the mold 11 a certain tension required for transportation, and the mold supplying means 20 conveys the mold 11 at a predetermined speed by the rotation of the driving roll 23. The transfer sheet 51 is unwound from the unwinding roll 52, passes through the transfer unit 60, the peeling unit 70, and the recovery unit 80, and is wound up on the winding roll 53. The transfer sheet supplying means 50 gives the transfer sheet 51 a certain tension required for transportation, and the mold supplying means 50 conveys the transfer sheet 51 at the same speed as the transport speed of the mold 11 by the rotation of the driving rolls 55 and 56. The coating unit 30 applies the coating material 13 containing a polymer material so as to cover the top surface 15a of the protrusion 15 of the mold 11. After coating, the coating material 13 passes through the drying unit 40, whereby the solvent remaining in the coating material 13 evaporates, and a polymer film 14 having a specific shape of the top surface 15a is formed on the top surface 15a of the convex portion 15 of the mold 11. Then, the nip rolls 61 and 62 of the transfer unit 61 press the surface of the mold 11 on which the concaves and convexes are formed and one surface of the transfer sheet 51 to be in contact with each other, so that the polymer film 14 is transferred from the top surface of the convex portion of the mold 11 to the transfer sheet 51. Then, the mold 11 with the polymer film 14 transferred to the transfer sheet 51 is taken up by the take-up roll 22 as it is. The transfer sheet 51 to which the polymer film 14 has been transferred is sandwiched between the nip roll 73 and the drive roll 55, and between the nip roll 74 and the drive roll 56 of the peeling unit 70, so that it is isolated from the transport tension, and in addition, tension is applied by the tension adjustment roll 75. The transfer sheet 51 to which tension is applied stretches in accordance with the tension. At this time, if the transfer sheet 51 is stretched beyond the length to which the polymer coating 14, which has been dried by volatilizing the solvent, can stretch, the polymer coating 14 cannot keep up with the amount of stretching, and peeling occurs at the lamination interface between the transfer sheet 51 and the polymer coating 14, i.e., the interface between the polymer coating 14 and the surface of the transfer sheet 51, causing the polymer thin film 16 to float from the transfer sheet.According to the inventors' investigations, if the transfer sheet 51 is stretched by 200% or more, the polymer coating 14 can be almost certainly peeled off from the transfer sheet 51. Since a suction nozzle 81 controlled to a negative pressure by a negative pressure generator 82 such as a vacuum pump is installed on the surface of the transfer sheet 51 in the peeling unit 70, the polymer thin film 16 peeled off from the transfer sheet 51 is sucked to the side with lower pressure and is captured by a nonwoven fabric-like collector 83 installed between the suction nozzle 81 and the negative pressure generator 82. The transfer sheet 51 from which the polymer thin film 16 has been collected is wound up as it is on the winding roll 53. The above operations are performed continuously.

[0029] The above-mentioned device configuration and operation make it possible to form a polymer thin film 16 having a specific shape. Only the polymer film 14 at the portion where the top surface 15a of the convex portion 15 of the mold 11 contacts the transfer sheet 51 is transferred to the transfer sheet 51, so that the polymer thin film 16 having a uniform shape can be transferred with high precision. Furthermore, by using the slit die 31 as the coating unit 30, it is possible to coat only the amount of polymer material required to form the polymer thin film 16, thereby reducing material costs.

[0030] Furthermore, in the peeling unit 70, the transfer sheet 51 is stretched and contracted to peel off the polymer coating 14 from the surface of the transfer sheet 51 to form the polymer thin film 16, and in the recovery unit 80, the polymer thin film 16 is recovered by suction, so that the recovered polymer thin film 16 is in a dry state, making it easy to handle and expanding the range of uses. The mold 11 taken up on the winding roll 22 and the transfer sheet 51 taken up on the winding roll 53 only need to be managed so that they are replaced when they deteriorate or when defects occur, and the costs for the mold 11 and the transfer sheet 51 can be kept low.

[0031] Next, the configuration of each part will be described in detail with reference to Figs. 1 to 6. The mold 11 has a fine uneven structure on the surface, and can be wound up in a roll. A surface uneven structure in which the protrusions 15 are arranged in a close-packed manner is suitable. This is because the area occupancy rate of the top surface 15a of the protrusions 15 relative to the total area of ​​the mold 11 increases, so that when the coating material 13 is applied, a larger amount of the polymer thin film 16 is obtained and the stability of the application increases. As shown in Fig. 2, the shape of the top surface 15a of the protrusions 15 can be exemplified as a circle (Fig. 2(a)) or a polygon (Fig. 2(b)). The shape of the top surface 15a does not need to be geometrically perfect when viewed from the surface on which the unevenness is formed, and may be approximately circular or approximately polygonal as long as it is recognizable as being similar to each shape. As for the shape of the protrusions 15, the area of ​​the top surface 15a is preferably 3000 to 10000 µm 2 More preferably, the area of ​​the top surface 15a is 5000 to 1800 μm. 2 It is preferable that the recesses are columnar with a height of 50 to 100 μm and are arranged in a close-packed manner when viewed from the surface on which the unevenness is formed. The width of the recesses in the close-packed arrangement (the distance between adjacent protrusions 15) is preferably made small within the range in which the unevenness structure can be processed, and is preferably 50 μm or less, and more preferably 20 μm or less. The material used for the mold 11 may be any of thermosetting resin, thermoplastic resin, and photocurable resin, but thermoplastic resin is suitable because it is relatively easy to impart an unevenness structure to it. For example, polyester-based resins such as polyethylene terephthalate, polyethylene-2,6-naphthalate, polypropylene terephthalate, and polybutylene terephthalate; polyolefin-based resins such as polyethylene, polystyrene, polypropylene, polyisobutylene, polybutene, and polymethylpentene; polyamide-based resins, polyimide-based resins, polyether-based resins, polyesteramide-based resins, polyetherester-based resins, acrylic resins, polycarbonate-based resins, and polyvinyl chloride-based resins are preferably used, but it is more preferable to select an appropriate material in consideration of chemical resistance to the chemicals used in the coating material 13.

[0032] The mold supplying means 20 includes an unwinding roll 21 that unwinds the mold 11 from the mold 11 wound in a roll shape, a winding roll 22 that winds up the unwound mold 11, a driving roll 23 that transports the mold 11 at a constant speed, a driving means (not shown) that rotates each roll, and guide rolls 21a and 22a to match the transport path of the mold. As the driving means for driving each roll, it is preferable that the transport tension applied to the mold 11 can be adjusted. It is preferable that the transport tension can be adjusted in the range of 1N to 100N with a resolution of 0.1N. As a driving means for determining the transport speed of the mold 11, a driving roll 23 is provided. The driving force is transmitted to the mold 11, and the mold 11 can be transported at a set speed. The driving roll 23 is connected to a driving means such as a motor (not shown) and can rotate while controlling the speed. The transport speed is preferably in the range of 1 to 30 m / min, and the productivity can be increased while the coating material 13 containing a polymer material is applied with high precision.

[0033] Also, it is preferable to provide a mold meandering correction mechanism in order to stably transport the mold 11. A preferred embodiment of the mold meandering suppression mechanism, as shown in Fig. 1, has one or more end detection sensors 28 that detect the position of the end of the mold 11 on the transport path of the mold 11, and controllers 27 that adjust the transport position of the mold 11 by controlling the movements of the unwinding roll 21 and the winding roll 22 based on the detected values.

[0034] The driving means for the unwinding roll 21 and the winding roll 22 is preferably one that can adjust the position of each roll in a direction perpendicular to the conveying direction of the mold 11. A structure that adjusts the amount of movement in the desired direction based on the value from the end detection sensor 28 is preferable. By providing the above-mentioned meandering suppression mechanism for the mold 11, the coating position of the coating material 13 can be kept constant, making it possible to form a polymer thin film 16 of uniform thickness and shape.

[0035] The coating unit 30 is disposed upstream of the drying unit 40 in the conveying process of the mold 11 in the conveying direction, and includes a slit die 31 and a coating material supply mechanism connected thereto. The slit die 31 faces the mold 11 so that the coating material 13 containing a polymeric material can be applied to the surface on which the uneven surface structure is formed. In order to form a uniform coating film, it is preferable that the distance between the slit die 31 and the mold 11 is kept uniform with high precision, and it is preferable to arrange the support roll 32 so as to support the mold 11 from the surface opposite to the surface on which the uneven surface structure is formed, as shown in FIG. 1. Here, it is preferable that the distance between the slit die 31 and the mold 11 can be controlled so that the distance between the discharge surface of the slit die 31 and the top surface 15a of the convex portion 15 on the surface of the mold 11 is 10 μm to 500 μm. The precision of the distance (the distance between the slit die 31 and the top surface 15a) in the direction perpendicular to the conveying direction is preferably 10 μm or less, more preferably 3 μm or less. In order to achieve the precision of the present invention, the straightness and rotational runout of the support roll 32 are preferably 5 μm or less, and more preferably 1 μm or less. Although a coating method using a slit die 31 is exemplified here, other coating methods may be used.

[0036] The coating material supply mechanism may be one that can continuously and uniformly deliver the coating material 13 according to the target film thickness. For example, a fixed amount of liquid delivery using a syringe pump or a tube pump, or a constant pressure delivery using compressed air and a pressure adjustment mechanism may be selected, but it is preferable to select a fixed amount of liquid delivery that allows easy calculation of the amount of coating material 13 delivered when the transport speed of the mold 11 is changed.

[0037] The transfer sheet 51 is stretchable and can be wound into a roll. The amount of elongation of the transfer sheet 51 in a direction parallel to the conveying direction is preferably 200% or more, but considering the allowable amount of elongation until breakage, the stretch breakage rate is more preferably 300% or more. Here, the stretch breakage rate is a value defined in JIS-C-2151 (2006 edition), and is a value obtained by dividing the length of the transfer sheet 51 at the time when the transfer sheet 51 breaks when a tensile force is applied by the length of the transfer sheet 51 before the tensile force is applied. The recovery rate representing the dimensional recovery rate after stretching is preferably 95% or more, and more preferably 98% or more, after being stretched to an elongation of 300%. A high recovery rate after stretching not only promotes peeling of the polymer film 14 and the transfer sheet 51, but also allows the transfer sheet 51 to be used repeatedly.

[0038] The surface of the transfer sheet 51 to which the polymer film is transferred may be smooth or may have minute projections and recesses. When minute projections and recesses are formed, the projections and recesses do not need to be geometrically perfect when viewed from the surface on which the projections and recesses are formed, and may be approximately circular or approximately polygonal as long as they are recognizable as being similar to each other. The shape of the projections is preferably such that the top surface area of ​​the projections is 1 to 1000 μm. 2 More preferably, the top surface area is 5 to 500 μm. 2 It is preferable that the recesses are columnar with a height of 5 to 50 μm and arranged in a close-packed manner when viewed from the surface on which the unevenness is formed. The width of the recesses (the interval between adjacent protrusions) in the close-packed arrangement is preferably made small within the range in which the unevenness structure can be processed, and is preferably 50 μm or less, and more preferably 10 μm or less. The material of the transfer sheet 51 to be applied may be any of thermosetting resins, thermoplastic resins, and photocurable resins, but thermosetting resins are suitable because they have high elasticity and recovery rate, and are relatively easy to impart with an unevenness structure. For example, silicone rubber, urethane rubber, nitrile rubber, fluororubber, ethylene propylene rubber, chloroprene rubber, polyurethane, styrene butadiene rubber, etc. are preferably used.

[0039] The surface free energy of the transfer sheet 51 is preferably greater than the surface free energy of the mold 11. When the surface free energy of the transfer sheet 51 is greater than the surface free energy of the mold 11, the polymer coating 14 formed on the surface of the mold 11 can be transferred efficiently.

[0040] The surface free energy of the transfer sheet 51 may be improved by performing a surface treatment on the surface of the transfer sheet 51. The suitable surface free energy of the transfer sheet 51 varies depending on the material of the mold 11, but is preferably 10 mJ / m 2 More than 60mJ / m 2 More preferably, 30 mJ / m or less. 2 More than 50mJ / m 2 The surface free energy of the transfer sheet 51 is 10 mJ / m or less. 2 If the surface free energy is 60 mJ / m or more, the polymer film 14 is easily peeled off from the mold 11 during transfer, and the polymer film 14 is less likely to remain on the surface of the mold 11. 2 If it is equal to or less than this, when recovering the polymer thin film 16 from the transfer sheet 51, the polymer thin film 16 will be easily peeled off from the transfer sheet, and thus the polymer thin film 16 will be easily recovered. Either a dry process or a wet process may be used as the surface treatment method, but in the case of a wet process, the treatment agent may be transferred to the polymer film 14 by contacting with the polymer film 14, so it is preferable to use a dry process. As the surface treatment by the dry process, plasma treatment, corona treatment, UV treatment, etc. are preferably used, but other surface treatment methods may also be used.

[0041] The transfer sheet supplying means 50 includes an unwinding roll 52 that unwinds the transfer sheet 51 from the transfer sheet 51 wound in a roll shape, a winding roll 53 that winds up the unwound transfer sheet 51, drive rolls 55 and 56 that transport the transfer sheet 51 at a constant speed, a drive means (not shown) that rotates each roll, and guide rolls 52a, 54, and 53a that match the transport path of the transfer sheet 51. As the drive means for driving each roll, since the transfer sheet 51 has elasticity, it is preferable that the transport tension applied to the transfer sheet 51 can be adjusted to prevent the transfer sheet 51 from being unnecessarily stretched due to tension. It is preferable that the transport tension can be adjusted in the range of 1N to 100N with a resolution of 0.1N. As the drive means for determining the transport speed of the transfer sheet 51, a drive roll 55 and a drive roll 56 are provided. The driving roll 55 and the driving roll 56 are disposed opposite the nip roll 73 and the nip roll 74, respectively, and are pressed by the nip roll 73 and the nip roll 74 through the transfer sheet 51, so that the driving force is transmitted to the transfer sheet 51, and the transfer sheet can be transported at a set speed. It is preferable that the driving means of the driving roll 56 is connected to the end of the driving roll 55 by a chain or a belt, so that it can rotate in conjunction with the driving roll 55, or that it can rotate independently using a motor that can synchronize the speed with the driving roll 55. The driving roll 55 is connected to a driving means such as a motor (not shown) and can rotate while controlling the speed. The speed at which the transfer sheet 51 is transported is preferably the same as the transport speed of the mold 11. By setting the transport speed to the same as that of the mold 11, it is possible to increase productivity while transferring the polymer film 14 with high precision.

[0042] Although not shown, it is preferable to provide a transfer sheet meandering correction mechanism, similar to the mold supply means, in order to stably transport the transfer sheet 51. The driving means for the unwinding roll 52 and the winding roll 53 is preferably one that can adjust the position of each roll in a direction perpendicular to the transport direction of the transfer sheet 51. By providing a meandering suppression mechanism for the transfer sheet 51, the relative position with the mold 11 can be kept constant, so that the uneven surface of the mold 11 can be brought into contact with one side of the transfer sheet evenly during transfer.

[0043] The transfer unit 60 is disposed downstream of the drying unit 40 in the conveying direction in the mold 11 conveying process. The transfer unit 60 includes nip rolls 61 and 62 that press the mold 11 and the transfer sheet 51 together so that the surface of the mold 11 on which the concaves and convexes are formed and one surface of the transfer sheet 51 come into contact with each other. The material of the nip roll 61 may be either metal or nonmetal. In the case of nonmetal, for example, when rubber is used, silicone rubber, EPDM (ethylene-propylene-diene rubber), neoprene, CSM (chlorosulfonated polyethylene rubber), urethane rubber, NBR (nitrile rubber), ebonite, etc. can be used. When a higher elastic modulus and hardness are required, a hard pressure-resistant resin (e.g., polyester resin) with improved toughness can be used. The rubber hardness of the elastic body is preferably in the range of 70 to 97° according to the ASTM D2240:2005 (Shore D) standard. When the hardness is 70° or more, the deformation amount of the elastic body is not too large, and the width of the pressurized contact between the mold 11 and the transfer sheet 51 is not too large, so that excessive frictional force is not generated. As a result, there is no concern that excessive friction will be generated between the surface of the mold 11 on which the unevenness is formed and the transfer sheet 51, causing damage to the polymer film 14. Conversely, when the hardness is 97° or less, the deformation amount of the elastic body is not too small, so that an appropriate frictional force is generated with an appropriate pressurized contact width, so that the transfer of the polymer film 14 can be promoted. The processing accuracy of the nip rolls 61 and 62 is preferably 0.03 mm or less in cylindricity tolerance and 0.03 mm or less in circumferential runout tolerance defined in JIS B 0621 (1984 edition). When each is 0.03 mm or less, no partial gap is generated between the nip rolls 61 and 62 during nipping, so that the laminate of the transfer sheet 51 and the polymer film 14 can be pressed with a uniform force in the width direction, and the transfer is successful.

[0044] The nip rolls 61 and 62 are preferably provided with a heating means. By heating and softening the polymer film 40 dried by the drying unit 40, the polymer film 14 may be efficiently transferred from the uneven surface of the mold 11 to the transfer sheet 51. As the heating means, a heater may be disposed inside the roll, or heating may be performed from the outside immediately before the mold 11 and the transfer sheet 51 are pressed by the nip rolls 61 and 62. When the polymer film 14 is a thermoplastic resin, the heating temperature is preferably 1 to 50 degrees higher than the glass transition temperature of the polymer material that is the main component of the polymer film 14, and more preferably 5 to 10 degrees higher. By heating at a temperature in this range, the polymer film 14 can be softened without destroying the shape of the specific shape 15, and the transfer may be successful.

[0045] The peeling unit 70 is disposed downstream of the transfer unit 60 in the conveying direction in the transfer sheet conveying process. The peeling unit 70 is composed of a tension blocking mechanism that blocks tension propagation from the upstream side of the peeling unit 70 in the conveying direction and tension propagation from the downstream side of the peeling unit 70 in the conveying direction, and a tension adjusting mechanism that adjusts the tension of the transfer sheet in the peeling section. The tension blocking mechanism is composed of a nip roll 73, a driving roll 55, a nip roll 74, and a driving roll 56. As shown in FIG. 3(a), it is preferable to block the conveying tension generated by the transfer sheet supplying means 50 by nipping the transfer sheet 51 at two points, the nip roll 73 and the driving roll 55, and the nip roll 74 and the driving roll 56. The tension adjusting mechanism is composed of a tension adjusting roll 75. It is preferable that the tension adjusting roll 75 is a mechanism that can extend the length of the transfer sheet 51 in the peeling section to three times or more the length of the peeling section before tension is applied. As shown in FIG. 3(b), the tension adjustment roll 75 is preferably a mechanism that presses down the transfer sheet 51 held by the nip rolls 73 and 74 from the side opposite to the side to which the polymer film 14 is transferred. Specifically, the tension adjustment mechanism is preferably a mechanism in which the freely rotatable tension adjustment roll 75 is connected to the tip of the rod of an air cylinder. By making the roll freely rotatable, friction with the transfer sheet 51 during tension application can be reduced, and transport can be prevented from being impeded. In addition, by applying an air cylinder, the stroke of the air cylinder can be controlled to control the tension, that is, the amount of stretch of the transfer sheet, so that a complex mechanism is not required, and the control mechanism required for tension control is also simplified. As the air cylinder, a double-acting air cylinder is preferably used. In order to efficiently peel off the polymer coating 14 from the transfer sheet 51, it is preferable to stretch the transfer sheet 51 to 200% or more and then contract it to 100% or less, performing this extension and contraction operation once or multiple times. If a double-acting air cylinder is used, this extension and contraction motion can be repeated at high speed, resulting in extremely efficient peeling.

[0046] The tension adjustment roll 75 may be made of either metal or non-metal, but it is preferable to select a material that reduces friction with the transfer sheet 51. The surface roughness is preferably such that the arithmetic mean roughness Ra is 1.6 μm or less as defined in JIS B 0601 (2001 edition). If Ra is 1.6 μm or less, there is no concern that the surface shape of the tension adjustment roll 75 will be transferred to the back surface of the transfer sheet 51 when tension is applied.

[0047] The processing accuracy of the nip rolls 73, 74 and the driving rolls 55, 56 is preferably 0.03 mm or less in cylindricity tolerance and 0.03 mm or less in circumferential runout tolerance defined in JIS B 0621 (1984 edition). If each is 0.03 mm or less, no partial gap is formed between the driving rolls 55, 56 and the nip rolls 73, 74 during nipping, so that the laminate of the transfer sheet 51 and the polymer film 14 can be pressed with a uniform force in the width direction, and conveyance and tension control are good. In addition, the surface roughness of each roll is preferably 1.6 μm or less in arithmetic mean roughness Ra defined in JIS B 0601 (2001 edition). If Ra is 1.6 μm or less, there is no concern that the surface shape of each roll will be transferred to the surface of the polymer film 14 or the back surface of the transfer sheet 51 during pressing.

[0048] The materials of the nip rolls 73, 74 and the driving rolls 55, 56 may be either metal or nonmetal. In the case of nonmetal, for example, when rubber is used, silicone rubber, EPDM (ethylene propylene diene rubber), neoprene, CSM (chlorosulfonated polyethylene rubber), urethane rubber, NBR (nitrile rubber), ebonite, etc. can be used. When a higher elastic modulus and hardness are required, a hard pressure-resistant resin (e.g. polyester resin) with improved toughness can be used. The rubber hardness of the elastic body is preferably in the range of 70 to 97° according to the ASTM D2240:2005 (Shore D) standard. When the hardness is 70° or more, the deformation amount of the elastic body is not too large, and the pressure contact width with the polymer film 14 is not too large, so that excessive frictional force is not generated in the polymer film 14. As a result, there is no concern that the polymer film 14 will peel off from the transfer sheet 51. Conversely, if the hardness is 97° or less, the deformation amount of the elastic body does not become too small, so that an appropriate frictional force is generated with an appropriate pressure contact width, enabling tension control and transportation.

[0049] The recovery unit 80 preferably includes one or more suction nozzles 81 connected to a negative pressure generator 82 such as a vacuum pump. The form of the suction nozzle 81 is not particularly limited, but it is preferable that the suction nozzle 81 includes a plurality of nozzles with small suction ports in order to efficiently suck the polymer thin film 16 at a high flow rate. Furthermore, it is preferable to install a collection material 83 in the path between the suction nozzle 81 and the negative pressure generator 82 in order to collect the polymer thin film 16 recovered by suction. The form of the collection material 83 is not particularly limited, but it is preferable that the pore size is smaller than the specific shape of the polymer thin film 16 and that the collection material has a high porosity in order to reduce pressure loss. More specifically, it is preferable to use a membrane filter, a nonwoven fabric filter, or the like.

[0050] FIG. 4 is a schematic cross-sectional view of another embodiment of the polymer thin film manufacturing apparatus of the present invention. In this polymer thin film manufacturing apparatus 90, another coating unit 91 and drying unit 95 are provided between the drying unit 40 and the transfer unit 60. After the polymer film 14 is formed on the mold 11 through the coating unit 30 and drying unit 40 on the upstream side in the conveying direction, another polymer film 94 can be laminated on the polymer film 14 through the coating unit 91 and drying unit 95 on the downstream side in the conveying direction. At this time, by making the polymer material contained in the coating material 13 applied from the slit die 31 of the coating unit 30 on the upstream side in the conveying direction and the polymer material contained in the coating material 93 applied from the slit die 92 of the coating unit 91 on the downstream side in the conveying direction different types, a laminate of polymer thin films made of different polymer materials can be obtained. The number of sets of coating units and drying units to be added may be added according to the number of polymer materials to be laminated, and there is no particular limit. Furthermore, when three or more layers of polymeric materials are laminated, the polymeric materials in all layers may be different types of polymeric materials, or only the polymeric materials in adjacent layers may be different types of polymeric materials.

[0051] FIG. 5 is a schematic cross-sectional view of another embodiment of the polymer thin film manufacturing apparatus of the present invention. As shown in FIG. 5, in the polymer thin film manufacturing apparatus 100, the coating material 13 is not directly applied to the mold 11, but the coating substrate 103 coated with the coating material 13 is sandwiched together with the mold 11 between the nip roll 33 and the drive roll 34, so that the coating material 13 is transferred and applied to the surface of the mold 11 before the coating material 13 dries. That is, the coating unit 30 of the polymer thin film manufacturing apparatus 100 shown in FIG. 5 is composed of a slit die 31, a coating substrate unwinding roll 101, a coating substrate winding roll 102, a coating substrate 103, a nip roll 33, and a drive roll 34. The coating substrate 103 unwound from the coating substrate unwinding roll 101 has the coating material 13 applied to the surface facing the mold 11 by the slit die 31, and then is sandwiched together with the mold 11 between the nip roll 33 and the drive roll 34 to transfer the coating material 13 to the surface of the mold 11. The coating substrate 103 with the coating material 13 transferred to the mold 11 is taken up by the coating substrate take-up roll 102. The mold 11 with the coating material 13 transferred to the top surfaces 15a of the projections 15 passes through the drying unit 40, and then the transfer unit 60 transfers the polymer film to the transfer sheet 51, and the mold 11 is taken up by the take-up roll 22. The transfer sheet 51 with the polymer film transferred has the polymer film 14 peeled off by the peeling unit 70, and the polymer thin film 16 is collected by the recovery unit 80 and taken up by the take-up roll 53. In the device shown in FIG. 5, it is possible to prevent the coating material 13 from flowing into the recesses, i.e., into the areas other than the top surfaces 15a of the projections 15 of the mold 11, and it is possible to obtain the polymer thin film 16 with the shape of the top surfaces 15a transferred well.

[0052] FIG. 6 is a schematic cross-sectional view of another embodiment of the polymer thin film manufacturing apparatus of the present invention. As shown in FIG. 6, in the polymer thin film 16 manufacturing apparatus 200, the transfer sheet 51 can be transported and the polymer thin film 16 can be peeled off without applying friction from the nip rolls to the surface of the polymer thin film 16. The drive roll 201 and tension adjustment roll 202 are suction rolls, and a mechanism is provided that can adsorb and transport the side of the transfer sheet 51 opposite to the side on which the polymer film is transferred. In the peeling unit 70, the transport tension in the peeling section is blocked by the transfer sheet 51 being adsorbed by the drive roll 201 and the tension adjustment roll 202. As a tension adjustment mechanism, tension is applied to the transfer sheet 51 between the drive roll 201 and the tension adjustment roll 202 by driving and rotating the tension adjustment roll 202 at a rotation speed faster than the drive roll 201, which is driven and rotated at the transport speed of the transfer sheet, and the transfer sheet 51 stretches by an amount corresponding to the speed difference between the drive roll 201 and the tension adjustment roll 202. Furthermore, even when the driving roll 201 and the tension adjusting roll 202 are driven and conveyed at the same speed, the transfer sheet 51 can be stretched by increasing the distance between the driving roll 201 and the tension adjusting roll 202 while the transfer sheet 51 is being conveyed. The transfer sheet 51 from which the polymer thin film 16 has been collected by the collection unit 80 passes through the tension adjusting roll 202, and is again subjected to the conveying tension from the winding roll 53 and taken up by the winding roll 53 while moving along the guide roll 53a. In the device shown in FIG. 6, conveyance, tension interruption, and stretching of the transfer sheet can be performed without applying friction to the surface of the polymer thin film 16, so that damage to the polymer thin film 16 and deformation caused by friction with the roll when the transfer sheet is stretched can be prevented.

[0053] The roll-shaped mold 11 can be manufactured by the manufacturing apparatus and manufacturing method disclosed in International Publication No. 2019 / 116951. The stretchable transfer sheet 51 can also be manufactured by the same manufacturing apparatus and manufacturing method.

[0054] Next, a method for producing a polymer thin film having a specific shape according to the present invention will be described. The method is characterized in that a mold having an uneven surface and the top surfaces of the protrusions having the specific shape is transported, a coating material containing a polymer material is applied to the surface with the unevenness formed thereon so as to cover the top surfaces of the protrusions of the transported mold, the applied polymer material is then dried to form a polymer film, one side of an elastic transfer sheet is then pressed against the surface of the mold with the unevenness formed thereon to transfer the polymer film formed on the top surfaces of the protrusions of the mold to the transfer sheet, the transfer sheet is then stretched or stretched one or more times to peel the transferred polymer film from the transfer sheet to obtain a polymer thin film, and the polymer thin film peeled from the transfer sheet is recovered, thereby producing a polymer thin film having a specific shape.

[0055] Next, a method for producing a polymer thin film 16 will be described with reference to FIG. 1, FIG. 7, and FIG. 8. In a preparation stage, a coating material 13 containing a polymer material is prepared and filled in a tank of a coating material supplying means connected to a slit die 31. The mold 11 is pulled out from the unwinding roll 21, passed along the guide roll 21a, passed through the coating unit 30, the drying unit 40, and the transfer unit 60, and taken up by the take-up roll 22 along the guide roll 22a. At this time, a certain tension required for transport is applied to the mold 11 by the mold supplying means 20. The transfer sheet 51 is pulled out from the unwinding roll 52, passed along the guide roll 52a, passed through the transfer unit 60, the peeling unit 70, and the recovery unit 80, and taken up by the take-up roll 53 along the guide roll 53a. At this time, a certain tension required for transport is applied to the transfer sheet 51 by the transfer sheet supplying means 50. In addition, the distance between the discharge tip surface of the slit die 31 and the surface of the mold 11 is set to a predetermined distance, and the coating material supplying means is set to send the coating material 13 under conditions corresponding to the film thickness. The drying unit 40 is heated at a constant temperature by a heating means (not shown).

[0056] Next, the drive roll 23 is driven, and the mold 11 is nipped and pressed between the nip roll 24 and the drive roll 23, thereby transporting the mold 11 at a constant speed. Next, the drive rolls 55 and 56 are driven, and the transfer sheet 51 is nipped and pressed between the nip roll 73 and the drive roll 55, and between the nip roll 74 and the drive roll 56, thereby transporting the transfer sheet 51 at the same speed as the mold 11 is transported.

[0057] Next, the nip roll 61 of the transfer unit 50 is lowered, and the application surface of the mold 11 and one surface of the transfer sheet 51 are pressed between the nip roll 61 and the nip roll 62 so that they come into contact with each other.

[0058] Next, the coating material supplying means of the coating unit 30 is operated to start feeding the coating material 13. The coating material 13, which contains a polymer material, is discharged from the discharge port of the slit die 31 and is uniformly applied to the top surface 15a of the protrusions 15 on the surface of the mold 11, and is transported to the drying unit 40. As it passes through the drying unit 40, the solvent remaining inside the coating material 13 gradually volatilizes, and when the evaporation of the solvent is completed, the polymer material of a specific shape is laminated as a film on the top surface 15a of the protrusions 15 of the mold 11 (FIG. 7).

[0059] Subsequently, in the process of passing through the transfer unit 60, the surface of the mold 11 on which the concaves and convexes are formed and the surface of the transfer sheet 51 are pressed against each other via the polymer film 14, so that the polymer film 14 is transferred from the top surface 15a of the convex portion 15 of the mold 11 to the transfer sheet. The mold 11 on which the polymer film 14 has been transferred to the transfer sheet 51 is directly subjected to a transport tension by the mold supplying means and taken up by the take-up roll 22. The transfer sheet 51 on which the polymer film 14 has been transferred is transported to the peeling unit 70, and enters a peeling section in which the transport tension is blocked and the transfer sheet 51 is sandwiched between two pairs of rolls, the nip roll 73 and the driving roll 55, and the nip roll 74 and the driving roll 56, which are tension blocking mechanisms. A tension adjusting roll 75, which is a tension adjusting mechanism, applies tension to the transfer sheet 51 from the back side of the transfer sheet 51, and the transfer sheet 51 is stretched to an elongation of 200% or more compared to before the tension is applied. Here, the polymer film 14 is laminated on the surface of the transfer sheet 51 from which tension has been blocked by the tension blocking mechanism (FIG. 8(a)). On the surface of the transfer sheet 51 stretched by the tension adjusting roll 75, the polymer film 14 that cannot keep up with the amount of stretch of the transfer sheet 51 floats up, and the polymer thin film 16 peels off (FIG. 8(b)). The polymer thin film 16 peeled off from the transfer sheet 51 is sucked by a suction nozzle 81 connected to a negative pressure generator 82 of a recovery unit 80, and is recovered by a collector 83 installed in the suction path. The transfer sheet 51 from which the polymer thin film 16 has been peeled off passes through the nip roll 74, and is again subjected to the transport tension of the transfer sheet supply means 50, and is taken up onto the take-up roll 53.

[0060] The polymer material used as the polymer thin film 16 is not particularly limited, but is preferably one that can peel off the polymer thin film 16 from the transfer sheet 51 by utilizing the difference in the stretching and breaking rate between the polymer material and the transfer sheet 51. The stretching and breaking rate of the polymer material is preferably 100% or less, more preferably 50% or less. Furthermore, the polymer thin film 16 used in medical products, cosmetics, etc. is preferably one that has biodegradability, and specifically, preferably, is a polymer containing a homopolymer and / or a copolymer containing at least one or more polymers selected from polyester-based resins such as polylactic acid, polyglycolic acid, polydioxanone, and polycaprolactone, polyether-based resins such as polyethylene glycol, polymethacrylate-based resins such as polymethyl methacrylate, polyethyl methacrylate, and polyhydroxyethyl methacrylate, polysaccharides or polysaccharide esters such as cellulose acetate, alginic acid, and chitosan, and polyvinyl-based resins such as polyvinyl acetate, polyvinyl alcohol, and polyvinylpyrrolidone, and more preferably, from the viewpoint of economy, polylactic acid, polyglycolic acid, polydioxanone, polycaprolactone, polyethylene glycol, polymethyl methacrylate, and copolymers thereof. In industrial applications such as paints, biodegradability is not necessarily required, and for example, polyester-based resins such as polyethylene terephthalate, polyethylene-2,6-naphthalate, polypropylene terephthalate, and polybutylene terephthalate; polyolefin-based resins such as polyethylene, polystyrene, polypropylene, polyisobutylene, polybutene, and polymethylpentene; polyamide-based resins, polyimide-based resins, polyether-based resins, polyesteramide-based resins, polyetherester-based resins, acrylic resins, polycarbonate-based resins, and polyvinyl chloride-based resins are also preferably used.

[0061] FIG. 10 shows an example of the form of a polymer thin film having a specific shape produced by the production method of the present invention. FIG. 9(a) is a scanning electron microscope photograph of a cut-out region of a laminate of polymer film 14 and mold 11. Polymer film 14 is uniformly applied to top surface 15a of protrusion 15, and transfers the specific shape of top surface 15a with high precision. FIG. 9(b) is a scanning electron microscope photograph of a cut-out region of a laminate of polymer thin film 16 and transfer sheet 51 after transfer sheet 51 has expanded or contracted. Polymer thin film 16 with the specific shape formed therein is peeled off from transfer sheet 51 due to expansion or contraction of transfer sheet 51.

[0062] The specific shape of the polymer thin film 16 of the present invention is not particularly limited, but is preferably any one of a circle, an ellipse, and a polygon when projected onto a two-dimensional plane so as to maximize the area of ​​the specific shape. In addition, since it is not necessary for the shape to be geometrically perfect and it is sufficient to be similar to each shape, it is also preferable for the shape to be any one of a substantially circle, a substantially ellipse, and a substantially polygon. From the viewpoint of ease of overlapping of the polymer thin films 16 with each other, a circle, a substantially circle, a polygon, or a substantially polygon is more preferable.

[0063] The polymer thin film 16 having a specific shape obtained by the present invention has a minute flat shape generally called a flake shape, a disk shape, or the like, and by controlling the cross-sectional shape and Young's modulus, the adhesive force between the polymer thin films 16 can be strengthened when the polymer thin films 16 are overlapped, and they do not collapse when an external force is applied, and can maintain a stable shape as an assembly of polymer thin films 16. Furthermore, since each film is a thin film, it has excellent conformability and adhesion to organs such as the skin and internal organs.

[0064] Because of these effects, the polymer thin film 16 having a specific shape obtained by the present invention is suitable for use as a component that requires a micron-sized size and a nano-sized thickness, such as medical films for covering internal wounds utilizing biodegradability, for covering external wounds, adhesion prevention materials, skin care products, and external skin materials such as cosmetic materials utilizing a micro-thin film shape. EXAMPLES

[0065] [Example 1] The material of the mold 11 has a surface free energy of 42.6 mJ / m 2 A cycloolefin polymer film (product name: Zeonorfilm ZF14, manufactured by Zeon Corporation) was used. A contact angle meter (model: CA-X, manufactured by Kyowa Interface Science Co., Ltd.) was used to measure the surface free energy of the mold 11. The contact angles between the mold 11 and each of the reagents, pure water, ethylene glycol, formamide, and methylene iodide, whose surface free energies are known, were measured, and the surface free energy of the mold 11 was calculated by applying the extended FOWKES theory.

[0066] The surface unevenness structure of the mold 11 was such that the specific shape of the top surface 15a of the protrusions 15 was a regular hexagon with a diagonal length of 100 μm, and the columnar protrusions of the protrusions 15 with a height of 50 μm were arranged in a close-packed arrangement with a width of the recess of 20 μm. A roll-shaped mold 11 was produced so that the width of the mold 11 was 300 mm and the length of the mold 11 was 300 m, and the produced mold 11 was attached so as to be transportable to the device shown in FIG.

[0067] The material of the transfer sheet 51 has a surface free energy of 10.6 mJ / m after curing. 2 A two-component curing silicone rubber (product name: RBL-9101-05, manufactured by Dow Corning Toray Co., Ltd.) was used, which was prepared by mixing two components, stirring, and then degassing. The uneven structure on the surface of the transfer sheet 51 had a top surface shape of a circle with a diameter of 5 μm, and columnar protrusions with a height of 5 μm were arranged in a square shape such that the center-to-center distance between the circles of the convex parts was 10 μm. A roll-shaped transfer sheet 51 was prepared so that the width of the transfer sheet 51 was 300 mm and the length of the transfer sheet 51 was 300 m, and the prepared transfer sheet was attached so that it could be transported to the device shown in FIG. 1.

[0068] The coating material 13 was prepared by dissolving a polymeric material, polylactic acid (manufactured by Wako Pure Chemical Industries, Ltd.), in ethyl acetate (CAS No. 141-78-6, manufactured by Wako Pure Chemical Industries, Ltd.), and was mixed so that the concentration of polylactic acid in the entire coating material 13 was 2.5 mass %.

[0069] The mold 11 was conveyed with an unwinding tension of 10 N, a winding tension of 10 N, and a conveying speed of 3 m / min, and at the same time, the transfer sheet 51 was conveyed with an unwinding tension of 10 N, a winding tension of 10 N, and a conveying speed of 3 m / min, and then in the transfer unit 60, the mold 11 and the transfer sheet 51 were nipped with nip rolls 61 and 62 at a pressure of 5 MPa so that the surface on which the unevenness was formed was in contact with the surface on which the unevenness was formed. As the coating unit 30, a slit die 31 having an extrusion width of 290 mm and a slit width of 100 μm was used, and the distance between the slit die 31 and the surface of the mold 11 was set to 100 μm, and the coating material 13 was applied at an extrusion speed such that the film thickness of the polymer film 14 after drying at the conveying speed was 150 nm.

[0070] The drying unit 40 utilized the high volatility of ethyl acetate and used a drying space whose temperature was adjusted to a constant value of 40°C.

[0071] In the peeling unit 80, the transfer sheet 51 was clamped between the nip roll 73 and the driving roll 55, and between the nip roll 74 and the driving roll 56, each with a pressure of 0.2 MPa, and the tension applied to the transfer sheet 51 in the peeling section was set to approximately 0 N. When the tension applied to the transfer sheet 51 reached approximately 0 N, a freely rotatable tension adjustment roll 75 connected to the tip of a rod of an air cylinder, as a tension adjustment mechanism, was pressed against the surface of the transfer sheet 51 opposite to the surface on which the unevenness was formed. The stroke of the air cylinder was adjusted so that the elongation amount of the transfer sheet 51 in the peeling section was 200%, and the length of the transfer sheet 51 in the peeling section was extended from 200 mm to 400 mm.

[0072] The polymer thin film 16 peeled off from the transfer sheet 51 due to the stretching of the transfer sheet 51 was collected by the suction nozzle of the collection unit 80, and was collected by a nonwoven fabric filter (product name FS6200, manufactured by Japan Vilene Co., Ltd.) as a collection material 83 installed between the suction nozzle 81 and a negative pressure generating device 82 such as a vacuum pump. The collection rate of the polymer thin film 16 was 30%.

[0073] As a result of observing the collected polymer thin film 16, it was confirmed that the polymer thin film 16 had a shape substantially identical to the shape of the top surface 15a of the mold 11. Fig. 10 shows the result of observing the surface of the polymer thin film 16 having a specific shape obtained in this Example 1 with a scanning electron microscope.

[0074] [Example 2] The mold 11 and the coating material 13 used were the same as those in the first embodiment. The material of the transfer sheet 51 has a surface free energy of 10.6 mJ / m after curing. 2 A two-component curing silicone rubber (product name: RBL-9101-05, manufactured by Dow Corning Toray Co., Ltd.) was used, which was mixed with two components, stirred, and then degassed, and a roll-shaped transfer sheet 51 was produced in the same manner as described in Example 1. Next, a corona treatment was performed on the surface of the transfer sheet 51, thereby increasing the surface free energy of the transfer sheet 51 to 45.5 mJ / m 2 Using the corona-treated transfer sheet 51, a polymer thin film 16 was formed and collected in the same manner as described in Example 1. As a result, it was confirmed that the polymer thin film 16 had a shape substantially identical to that of the top surface 15a of the mold 11. The recovery rate of the polymer thin film 16 was 90%. [Industrial Applicability]

[0075] The polymer thin film obtained by the apparatus and method for producing a polymer thin film having a specific shape of the present invention can accumulate by overlapping each other while showing high conformability to the adherend, and can form a film showing high adhesion and stability. For example, it is ideal for hemostasis during surgery, wound dressing materials, adhesion prevention materials, cosmetic materials, transdermal absorption materials, etc. It can also be used as a coating agent by dispersing it in an aqueous solvent. [Explanation of symbols]

[0076] 10, 90, 100, 200: Polymer thin film manufacturing equipment 11, 11A: Mold 13, 93: Coating material 14, 94: Polymer film 15: Convex 15a: Top 16:Polymer thin film 20: Mold supply means 21, 52, 410: Unwinding roll 21a, 22a, 52a, 53a: Guide rolls 22, 53, 360, 370, 450: Winding roll 23, 55, 56: Driving roll 27: Controller 28: Edge detection sensor 30, 91: Coating unit 31, 92, 330: Slit die 32: Support roll 24, 33, 61, 62, 73, 74, 421: Nip roll 40, 95: Drying unit 50: Transfer sheet supply means 51: Transfer sheet 60: Transcription unit 70: Peeling unit 75, 202: Tension adjustment roll 80: Recovery unit 81: Suction nozzle 82: Negative pressure generator 83: Collection material 101: Coating substrate unwinding roll 102: Coating substrate winding roll 103: Base material for coating

Claims

1. A manufacturing apparatus for manufacturing a polymer thin film having a specific shape, comprising: a mold having a surface formed with projections and recesses, the top surface of each projection having the specific shape; a mold supplying means for supplying the mold; a coating unit that coats a coating material including a polymer material on the surface on which the projections and recesses are formed so as to cover the top surfaces of the projections of the mold transported by the mold supply means; a drying unit that is located downstream of the coating unit in a conveying direction of the mold and dries the coated polymer material to form a polymer coating; A transfer sheet supplying means for supplying a transfer sheet having a stretchable property and having a concavo-convex shape on one side thereof; a transfer unit, which is located downstream of the drying unit in a conveying direction of the mold, and which presses the surface of the transfer sheet, on which the projections and recesses are formed, supplied by the transfer sheet supplying means, against the surface of the mold on which the projections and recesses are formed, thereby transferring the polymer coating formed on the top surfaces of the projections of the mold to the transfer sheet; a peeling unit for peeling the transferred polymer film from the transfer sheet by stretching the transfer sheet or by stretching the transfer sheet one or more times to obtain a polymer thin film; and a recovery unit that recovers the polymer thin film peeled off from the transfer sheet.

2. 2. The apparatus for producing a thin polymer film according to claim 1, wherein said transfer unit is provided with a heating means.

3. A method for producing a polymer thin film having a specific shape, comprising the steps of: Transporting a mold having projections and recesses formed on its surface, the top surfaces of the projections having the specific shape; Next, a coating material including a polymer material is applied to the surface on which the projections and recesses are formed so as to cover the top surfaces of the projections of the transported mold; Next, the applied polymer material is dried to form a polymer film; Next, a surface of a transfer sheet having one surface on which projections and recesses are formed and having elasticity is pressed against the surface of the mold on which projections and recesses are formed, thereby transferring the polymer coating formed on the top surfaces of the projections of the mold to the transfer sheet; Next, the transfer sheet is stretched or stretched one or more times, the transferred polymer film is peeled off from the transfer sheet to obtain a polymer thin film, and the polymer thin film peeled off from the transfer sheet is recovered.

4. The method for producing a polymer thin film according to claim 3 , wherein the polymer film formed on the top surface of the convex portion of the mold is transferred to the transfer sheet while being heated.

5. The method for producing a polymer thin film according to claim 3 or 4, wherein the surface free energy of the transfer sheet is greater than the surface free energy of the mold.

6. The surface free energy of the transfer sheet is 10 mJ / m 2 60mJ / m or more 2 The method for producing a polymer thin film according to any one of claims 3 to 5, wherein the polymer thin film is:

Citation Information

Patent Citations

  • Image forming device

    JP1997114282A

  • Image receiving sheet for heat-sensitive transfer recording

    JP1998081076A

  • Thin-filmy polymeric structure and method of preparing the same

    WO2006025592A1

  • Thin film-like polymer structure and method for preparing the same

    WO2008050913A1

  • Method and apparatus for manufacturing surface-structured film

    WO2016208353A1