Resin composition, electronic component, and method for producing resin film
A resin composition with protic polar groups and a specific crosslinking agent forms a resin film with enhanced ITO wrinkle suppression, chemical resistance, and heat resistance, addressing the limitations of conventional films in electronic components.
Patent Information
- Application Number
- JP2021526891
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-28
- Filing Date
- 2020-06-18
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-06-18
AI Technical Summary
Conventional resin films used in electronic components, such as those for ITO electrodes, suffer from issues with wrinkle formation, chemical resistance, and heat resistance, necessitating improvements in ITO wrinkle suppression performance, chemical resistance, and heat resistance.
A resin composition containing a polymer with protic polar groups and a specific crosslinking agent, along with optional additives like phenolic antioxidants and radiation-sensitive compounds, is used to form a resin film with enhanced ITO wrinkle suppression, chemical resistance, and heat resistance.
The resin film exhibits excellent ITO wrinkle suppression, chemical resistance, and heat resistance, enabling high-performance electronic components with improved stability and functionality.
Smart Images

Figure 0007586075000001 
Figure 0007586075000002 
Figure 0007586075000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, an electronic component, and a method for producing a resin film. In particular, the present invention relates to a resin composition that can be suitably used for forming an insulating film or the like used in an electronic component, an electronic component having a resin film made of the resin composition, and a method for producing such a resin film. [Background technology]
[0002] 2. Description of the Related Art Electronic components such as liquid crystal display devices, organic EL display devices, integrated circuit elements, and solid-state imaging elements are provided with various resin films as planarizing films, protective films, insulating films, and the like.
[0003] For example, Patent Document 1 proposes a photosensitive resin composition used to form a permanent film, which contains a polymer having a cyclic olefin structural unit, has a PED (Post Exposure Delay) measured under specific conditions of 10% or less, and has a swelling ratio measured under specific conditions (B) of 20% or less. The photosensitive resin composition according to Patent Document 1 can improve production stability when used in the manufacture of an electronic device having a permanent film. Furthermore, the photosensitive resin composition according to Patent Document 1 may optionally contain a crosslinking agent such as an epoxy compound.
[0004] Patent Document 2 proposes a photosensitive resin composition used to form a sacrificial film, which contains a specific alkali-soluble resin and a photosensitizer, and when the photosensitive resin composition is heat-treated at 115° C. for 3 minutes to form a resin film, the static contact angle of water with the resin film is 76° or more and 95° or less. Furthermore, the photosensitive resin composition according to Patent Document 2 may optionally contain a crosslinking agent such as an epoxy compound. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2015 / 141525 [Patent Document 2] JP 2017-111447 A Summary of the Invention [Problem to be solved by the invention]
[0006] In recent years, improvements have been made to improve the performance of ITO (Indium Tin Oxide) electrodes, which are a type of transparent electrode used in a variety of applications. In order to improve the performance of the ITO electrode, it is preferable that the ITO film provided on the ITO electrode has no or few wrinkles. If the ITO film is wrinkled, the light transmittance of the laminate may deteriorate, which may lead to a decrease in the performance of the ITO electrode. Therefore, it is desirable that the resin film provided adjacent to or close to the ITO film can exhibit a performance of suppressing the occurrence of wrinkles on the surface of the ITO film when the ITO film is formed on the surface. Hereinafter, in this specification, the performance of "suppressing the occurrence of wrinkles on the surface of the ITO film" is referred to as "ITO wrinkle suppression performance".
[0007] In addition, when forming a resin film using a resin composition, various chemical solutions are generally used. If the resin film has an appropriate resistance, i.e., chemical resistance, to such chemical solutions, it is possible to form a resin film as designed. Therefore, the resin film is required to have excellent chemical resistance.
[0008] Furthermore, in recent years, in the process of forming an ITO film when forming an ITO electrode, it has been considered to form and heat an ITO film under high temperature conditions in order to obtain an ITO film that can exhibit excellent performance. Therefore, the resin film is required to have little film loss under high temperature conditions, i.e., excellent heat resistance.
[0009] Thus, in recent years, resin films are required to be excellent in all of "ITO wrinkle suppression performance," "chemical resistance," and "heat resistance." However, the resin films formed using the above-mentioned conventional resin compositions have room for improvement in terms of improving these attributes in a well-balanced manner.
[0010] Therefore, an object of the present invention is to provide a resin composition capable of forming a resin film having excellent ITO wrinkle suppression performance, chemical resistance, and heat resistance. Another object of the present invention is to provide a high-performance electronic component having a resin film formed using the resin composition of the present invention. A further object of the present invention is to provide a method for producing a resin film, which can efficiently produce the resin film of the present invention using the resin composition of the present invention. [Means for solving the problem]
[0011] The present inventors have conducted extensive research to solve the above problems, and have found that a resin composition containing a polymer (A) having a protonic polar group and a specific crosslinking agent (B) that satisfies a specific composition makes it possible to form a resin film that is excellent in ITO wrinkle suppression performance, chemical resistance, and heat resistance, thereby completing the present invention.
[0012] That is, the present invention aims to advantageously solve the above-mentioned problems, and the resin composition of the present invention is a resin composition containing a polymer (A) having a protic polar group and a crosslinking agent (B) containing a compound represented by the following formula (1), and is characterized in that the polymer (A) having a protic polar group contains a cyclic olefin polymer (A-1) having a protic polar group, and the proportion of monomer units having a protic polar group is 51 mol % or more, and the polymer (A) contains a polyamideimide resin (A-2) having a protic polar group. [ka] [In formula (1), each of the multiple R's independently represents an alkyl group having 1 to 6 carbon atoms or an alkoxy group having 1 to 6 carbon atoms; 1 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms, and m, n, p, and q each represent an integer of 0 to 4. In this way, by incorporating into the resin composition a specific polymer (A) having a protic polar group and a crosslinking agent (B) satisfying the above-mentioned specific structure, it is possible to form a resin film that is excellent in ITO wrinkle suppression performance, chemical resistance, and heat resistance.
[0013] Here, it is preferable that the resin composition of the present invention further contains a phenol-based antioxidant (C). If the resin composition further contains the phenol-based antioxidant (C), the light transmittance of the obtained resin film can be increased.
[0014] In the resin composition of the present invention, the content of the phenolic antioxidant (C) is preferably 0.3 parts by mass or more and 15 parts by mass or less relative to 100 parts by mass of the polymer (A) having a protonic polar group. If the content of the antioxidant (C) relative to the polymer (A) is within the above range, the light transmittance of the obtained resin film can be further improved, and the ITO wrinkle suppression performance can be further improved, and the antioxidant (C) can be prevented from easily bleeding out from the obtained resin film.
[0015] In the resin composition of the present invention, the polymer (A) having a protonic polar group is preferably a cyclic olefin polymer having a carboxyl group. By including a cyclic olefin polymer having a carboxyl group in the resin composition, the ITO wrinkle suppression performance of the obtained resin film can be further improved.
[0016] In addition, in the resin composition of the present invention, the polymer (A) having a protonic polar group is the cyclic olefin polymer (A-1) having a protonic polar group, and the cyclic olefin polymer (A-1) having a protonic polar group is preferably a ring-opening polymer. If the polymer (A) having a protonic polar group is a ring-opening polymer, the processability of the obtained resin film can be improved.
[0017] In the resin composition of the present invention, the content of the crosslinking agent (B) is preferably 5 parts by mass or more and 160 parts by mass or less relative to 100 parts by mass of the polymer (A) having a protonic polar group. If the content of the crosslinking agent (B) is within the above-mentioned range, the ITO wrinkle suppression performance, chemical resistance, and light transmittance of the obtained resin film can be improved.
[0018] Furthermore, it is preferable that the resin composition of the present invention further contains at least one of a compound having two or more alkoxymethyl groups and a compound having two or more methylol groups. If the resin composition further contains at least one of a compound having two or more alkoxymethyl groups and a compound having two or more methylol groups, the chemical resistance of the obtained resin film can be further improved.
[0019] Furthermore, the resin composition of the present invention may further contain a radiation-sensitive compound (D). If the resin composition contains the radiation-sensitive compound (D), a resin film having a desired pattern can be well formed by patterning the resin film. Here, the radiation-sensitive compound (D) is preferably a quinone diazide compound.
[0020] The present invention also aims to advantageously solve the above problems, and the electronic component of the present invention is characterized by comprising a resin film made of any one of the above-mentioned resin compositions. The resin film formed using the above-mentioned resin composition is excellent in ITO wrinkle suppression performance, chemical resistance, and heat resistance, so that the electronic component having the resin film can fully exhibit the desired functions and has high performance.
[0021] The present invention also aims to advantageously solve the above problems, and the method for producing a resin film of the present invention is characterized by including a step of heating a coating film formed using a resin composition at 100° C. or higher. By heating a coating film formed using any of the above-mentioned resin compositions at 100° C. or higher, a resin film having excellent ITO wrinkle suppression performance, chemical resistance, and heat resistance can be efficiently produced. Effect of the Invention
[0022] According to the present invention, it is possible to provide a resin composition capable of forming a resin film having excellent ITO wrinkle suppression performance, chemical resistance, and heat resistance. Furthermore, according to the present invention, it is possible to provide a high-performance electronic component having a resin film formed using the resin composition of the present invention. Furthermore, according to the present invention, it is possible to provide a method for producing a resin film, which can efficiently produce the resin film of the present invention using the resin composition of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Hereinafter, an embodiment of the present invention will be described in detail. The resin composition of the present invention can be used to form a resin film. Such a resin film can be suitably provided on an electronic component having an ITO electrode. The electronic component of the present invention is provided with a resin film obtained by using the resin composition of the present invention. Moreover, such a resin film can be efficiently manufactured according to the method for manufacturing a resin film of the present invention using the resin composition of the present invention.
[0024] (Resin composition) The resin composition of the present invention is characterized by containing a polymer (A) having a protic polar group that satisfies the specified conditions described below, and a crosslinking agent (B) containing a compound represented by the following formula (1): [ka] [In formula (1), each of the multiple R's independently represents an alkyl group having 1 to 6 carbon atoms or an alkoxy group having 1 to 6 carbon atoms;1 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms, and m, n, p, and q each represent an integer of 0 to 4. Furthermore, the resin composition of the present invention may further contain, optionally, a phenol-based antioxidant (C), at least one of a compound having two or more alkoxymethyl groups and a compound having two or more methylol groups, and other additives.
[0025] In addition, the resin composition of the present invention contains a polymer (A) having a protonic polar group that satisfies a certain condition, and a crosslinking agent (B) that satisfies the above-mentioned specified structure, so that it has excellent ITO wrinkle suppression performance, chemical resistance, and heat resistance. This is presumably because the presence of a crosslinked structure in the resin film, in which the protonic polar group contained in the polymer (A) that satisfies a certain condition is crosslinked by the crosslinking agent (B), contributes to increasing the glass transition temperature of the resin film, increasing the elastic modulus of the resin film in a high-temperature environment, increasing the tensile strength of the resin film in a high-temperature environment, and suppressing the resin film from excessively swelling when immersed in a chemical.
[0026] <Polymer (A) Having Protonic Polar Group> The polymer (A) having a protic polar group is characterized by satisfying at least one of the following: it contains a cyclic olefin polymer (A-1) having a protic polar group, and the proportion of monomer units having a protic polar group is 51 mol % or more; and it contains a polyamideimide resin (A-2) having a protic polar group.
[0027] The polymer (A) having a protic polar group is a polymer in which a protic polar group is bonded to a skeleton structure. Here, the "protic polar group" refers to a group containing an atom in which hydrogen is directly bonded to an atom belonging to Group 15 or Group 16 of the periodic table. The atom to which hydrogen is directly bonded is preferably an atom in the second or third period of Group 15 or Group 16 of the periodic table, more preferably an oxygen atom, a nitrogen atom, or a sulfur atom, and particularly preferably an oxygen atom.
[0028] Specific examples of such protic polar groups include polar groups having an oxygen atom such as a hydroxyl group, a carboxyl group (hydroxycarbonyl group), a sulfonic acid group, and a phosphoric acid group; polar groups having a nitrogen atom such as a primary amino group, a secondary amino group, a primary amide group, and a secondary amide group (imide group); and polar groups having a sulfur atom such as a thiol group. Among these, those having an oxygen atom are preferred, and a carboxyl group is more preferred. In the present invention, there is no particular limitation on the number of protic polar groups bonded to the protic polar group-containing polymer (A), and different types of protic polar groups may be contained.
[0029] The skeleton of the polymer (A) having a protonic polar group is either (1) a polymer having a cyclic structure (alicyclic or aromatic ring) derived from a cyclic olefin monomer in the main chain, or (2) a polyamideimide. Note that even if a polymer has an amide bond and an imide bond in the repeating unit and can be called a "polyamideimide resin", a polymer having a cyclic structure derived from a cyclic olefin monomer in the main chain is considered to fall under the "polymer having a cyclic structure (alicyclic or aromatic ring) derived from a cyclic olefin monomer in the main chain" described in (1) above.
[0030] Furthermore, from the viewpoint of further improving the ITO wrinkle suppression performance of the obtained resin film, it is preferable to use at least a polymer having a skeleton (1) in the main chain, which has a cyclic structure (alicyclic or aromatic ring) derived from a cyclic olefin monomer, as the polymer (A) having a protonic polar group, in other words, it is preferable that the polymer (A) having a protonic polar group at least contains a cyclic olefin polymer. Hereinafter, as the polymer (A) having a protonic polar group, the cyclic olefin polymer is sometimes referred to as "cyclic olefin polymer (A-1)", and the polyamideimide resin having a protonic polar group is sometimes referred to as "polyamideimide resin (A-2)". In addition, as the polymer (A) having a protonic polar group, one type of polymer may be used alone, or multiple types of polymers may be used in combination. More specifically, as the polymer (A) having a protic polar group, one or more kinds of cyclic olefin polymers (A-1) or one or more kinds of polyamideimide resins (A-2) may be used, or one or more kinds of cyclic olefin polymers (A-1) and one or more kinds of polyamideimide resins (A-2) may be used in combination. Among them, as mentioned above, it is preferable that the polymer (A) having a protic polar group at least contains a cyclic olefin polymer (A-1), and it is more preferable that the polymer (A) having a protic polar group is a cyclic olefin polymer (A-1).
[0031] <<Cyclic olefin polymer (A-1)>> The cyclic olefin polymer (A-1) may be a polymer of one or more cyclic olefin monomers, or a copolymer of one or more cyclic olefin monomers with a monomer copolymerizable therewith. In the present invention, it is preferable to use at least a cyclic olefin monomer (a) having a protic polar group as a monomer for forming the cyclic olefin polymer (A-1).
[0032] The cyclic olefin monomer (a) having a protic polar group (hereinafter, may be simply referred to as "cyclic olefin monomer (a)") is not particularly limited, and specific examples of the cyclic olefin monomer (a) having a protic polar group (hereinafter, may be appropriately referred to as "monomer (a)") include 2-hydroxycarbonylbicyclo[2.2.1]hept-5-ene, 2-methyl-2-hydroxycarbonylbicyclo[2.2.1]hept-5-ene, 2-carboxymethyl-2-hydroxycarbonylbicyclo[2.2.1]hept-5-ene, 2-hydroxy ... 2,3-dihydroxycarbonylbicyclo[2.2.1]hept-5-ene, 2-hydroxycarbonyl-3-hydroxycarbonylmethylbicyclo[2.2.1]hept-5-ene, 3-methyl-2-hydroxycarbonylbicyclo[2.2.1]hept-5-ene, 3-hydroxymethyl-2-hydroxycarbonylbicyclo[2.2.1]hept-5-ene, 2-hydroxycarbonyltricyclo[5.2.1.0 2,6 ]Deca-3,8-diene, 4-hydroxycarbonyltetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-9-ene, 4-methyl-4-hydroxycarbonyltetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-9-ene, 4,5-dihydroxycarbonyltetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-9-ene, 4-carboxymethyl-4-hydroxycarbonyltetracyclo[6.2.1.1 3,6 .0 2,7]dodec-9-ene, N-(hydroxycarbonylmethyl)bicyclo[2.2.1]hept-5-ene-2,3-dicarboximide, N-(hydroxycarbonylethyl)bicyclo[2.2.1]hept-5-ene-2,3-dicarboximide, N-(hydroxycarbonylpentyl)bicyclo[2.2.1]hept-5-ene-2,3-dicarboximide, N-(dihydroxycarbonylethyl)bicyclo[2.2.1]hept-5-ene-2,3-dicarboximide, N-(dihydroxycarbonylpropyl)bicyclo[2.2.1]hept-5-ene-2,3-dicarboximide, N-(hydroxycarbonylphen 2-(4-hydroxyphenyl)bicyclo[2.2.1]hept-5-ene, 2-methyl-2-(4-hydroxyphenyl)bicyclo[2.2.1]hept-5-ene, 4-(4-hydroxyphenyl)tetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-9-ene, 4-methyl-4-(4-hydroxyphenyl)tetracyclo[6.2.1.1 3,6 .0 2,7]dodec-9-ene, 2-hydroxybicyclo[2.2.1]hept-5-ene, 2-hydroxymethylbicyclo[2.2.1]hept-5-ene, 2-hydroxyethylbicyclo[2.2.1]hept-5-ene, 2-methyl-2-hydroxymethylbicyclo[2.2.1]hept-5-ene, 2,3-dihydroxymethylbicyclo[2.2.1]hept-5-ene, 2-(hydroxyethoxycarbonyl)bicyclo[2.2. 1]hept-5-ene, 2-methyl-2-(hydroxyethoxycarbonyl)bicyclo[2.2.1]hept-5-ene, 2-(1-hydroxy-1-trifluoromethyl-2,2,2-trifluoroethyl)bicyclo[2.2.1]hept-5-ene, 2-(2-hydroxy-2-trifluoromethyl-3,3,3-trifluoropropyl)bicyclo[2.2.1]hept-5-ene, 3-hydroxytricyclo[5.2.1.0 2,6 ]Deca-4,8-diene, 3-hydroxymethyltricyclo[5.2.1.0 2,6 ]Deca-4,8-diene, 4-hydroxytetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-9-ene, 4-hydroxymethyltetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-9-ene, 4,5-dihydroxymethyltetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-9-ene, 4-(hydroxyethoxycarbonyl)tetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-9-ene, 4-methyl-4-(hydroxyethoxycarbonyl)tetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-9-ene, N-(hydroxyethyl)bicyclo[2.2.1]hept-5-ene-2,3-dicarboximide, N-(hydroxyphenyl)bicyclo[2.2.1]hept-5-ene-2,3-dicarboximide, and other hydroxyl group-containing cyclic olefins can be mentioned. Among these, from the viewpoint of further improving the ITO wrinkle suppression performance of the obtained resin film, carboxyl group-containing cyclic olefins are preferred, and 4-hydroxycarbonyltetracyclo[6.2.1.13,6 .0 2,7 ]dodec-9-ene is particularly preferred. As the cyclic olefin monomer (a), one or more kinds of monomers can be used.
[0033] The content ratio of the units derived from the cyclic olefin monomer (a) in the cyclic olefin polymer (A-1) is preferably 51 mol% or more, more preferably 55 mol% or more, more preferably 99 mol% or less, more preferably 90 mol% or less, even more preferably 80 mol% or less, and even more preferably 75 mol% or less, based on the total repeating units constituting the cyclic olefin polymer (A-1) being 100 mol%. The content ratio of the units derived from the cyclic olefin monomer (a) may be 100 mol%. By setting the content ratio of the units derived from the cyclic olefin monomer (a) within the above range, the ITO wrinkle suppression performance, chemical resistance, and heat resistance of the obtained resin film can be improved in a more balanced manner.
[0034] The cyclic olefin polymer (A-1) used in the present invention may be a copolymer obtained by copolymerizing a cyclic olefin monomer (a) having a protonic polar group with a monomer (b) copolymerizable therewith. Examples of such copolymerizable monomers include a cyclic olefin monomer (b1) having a polar group other than a protonic polar group, a cyclic olefin monomer (b2) having no polar group, and a monomer (b3) other than a cyclic olefin (hereinafter referred to as "monomer (b1)", "monomer (b2)", and "monomer (b3)" as appropriate). Here, the monomers (b1) to (b3) can be used within a range that does not affect the properties. The cyclic olefin polymer (A-1) is preferably composed of a monomer (a) and a monomer (b1). Furthermore, among the monomers (b1) listed below, it is preferable to use N-(2-ethylhexyl)-bicyclo[2.2.1]hept-5-ene-2,3-dicarboximide, which is a cyclic olefin having an N-substituted imide group.
[0035] Specific examples of the polar group other than the protic polar group contained in the cyclic olefin monomer (b1) having a polar group other than the protic polar group include an ester group (collectively referring to an alkoxycarbonyl group and an aryloxycarbonyl group), an N-substituted imide group, an epoxy group, a halogen atom, a cyano group, a carbonyloxycarbonyl group (an acid anhydride residue of a dicarboxylic acid), an alkoxy group, a carbonyl group, a tertiary amino group, a sulfone group, an acryloyl group, etc. Among them, the polar group other than the protic polar group is preferably an ester group, an N-substituted imide group, or a cyano group, more preferably an ester group or an N-substituted imide group, and particularly preferably an N-substituted imide group.
[0036] Specific examples of the monomer (b1) include the following cyclic olefins. Examples of cyclic olefins having an ester group include 5-acetoxybicyclo[2.2.1]hept-2-ene, 5-methoxycarbonylbicyclo[2.2.1]hept-2-ene, 5-methyl-5-methoxycarbonylbicyclo[2.2.1]hept-2-ene, 9-acetoxytetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-methoxycarbonyltetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-ethoxycarbonyltetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-n-propoxycarbonyltetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-isopropoxycarbonyltetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-n-butoxycarbonyltetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-methyl-9-methoxycarbonyltetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-methyl-9-ethoxycarbonyltetracyclo[6.2.1.1 3,6 .02,7 ]dodec-4-ene, 9-methyl-9-n-propoxycarbonyltetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-methyl-9-isopropoxycarbonyltetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-methyl-9-n-butoxycarbonyltetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-(2,2,2-trifluoroethoxycarbonyl)tetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-methyl-9-(2,2,2-trifluoroethoxycarbonyl)tetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene and the like. Examples of cyclic olefins having an N-substituted imide group include N-phenylbicyclo[2.2.1]hept-5-ene-2,3-dicarboximide, N-(2-ethylhexyl)-1-isopropyl-4-methylbicyclo[2.2.2]oct-5-ene-2,3-dicarboximide, N-(2-ethylhexyl)-bicyclo[2.2.1]hept-5-ene-2,3-dicarboximide, N-[(2-ethylbutoxy)ethoxypropyl]-bicyclo[2.2.1]hept-5-ene-2,3-dicarboximide, and N-(endo-bicyclo[2.2.1]hept-5-ene-2,3-diyldicarbonyl)dimethyl aspartate. Examples of cyclic olefins having a cyano group include 9-cyanotetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-methyl-9-cyanotetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 5-cyanobicyclo[2.2.1]hept-2-ene, and the like. Examples of cyclic olefins having halogen atoms include 9-chlorotetracyclo[6.2.1.1 3,6 .0 2,7]dodec-4-ene, 9-methyl-9-chlorotetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene and the like. These cyclic olefin monomers (b1) having a polar group other than a protic polar group may be used alone or in combination of two or more kinds.
[0037] Specific examples of the cyclic olefin monomer (b2) having no polar group include bicyclo[2.2.1]hept-2-ene (also called "norbornene"), 5-ethyl-bicyclo[2.2.1]hept-2-ene, 5-butyl-bicyclo[2.2.1]hept-2-ene, 5-ethylidene-bicyclo[2.2.1]hept-2-ene, 5-methylidene-bicyclo[2.2.1]hept-2-ene, 5-vinyl-bicyclo[2.2.1]hept-2-ene, tricyclo[5.2.1.0 2,6 ]Deca-3,8-diene (common name: dicyclopentadiene), tetracyclo[10.2.1.0 2,11 0 4,9 ]Pentadeca-4,6,8,13-tetraene, tetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene (also called "tetracyclododecene"), 9-methyl-tetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-ethyl-tetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-methylidene-tetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-ethylidene-tetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-vinyl-tetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-propenyl-tetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, pentacyclo[9.2.1.1 3,9 .0 2,10 .0 4,8]Pentadeca-5,12-diene, cyclopentene, cyclopentadiene, 9-phenyl-tetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, tetracyclo[9.2.1.0 2,10 .0 3,8 ]Tetradeca-3,5,7,12-tetraene, pentacyclo[9.2.1.1 3,9 .0 2,10 .0 4,8 ]pentadec-12-ene, and the like. These cyclic olefin monomers (b2) having no polar group may be used alone or in combination of two or more kinds.
[0038] Specific examples of the monomer (b3) other than the cyclic olefin include linear olefins. Examples of the chain olefin include α-olefins having 2 to 20 carbon atoms, such as ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene; and non-conjugated dienes, such as 1,4-hexadiene, 4-methyl-1,4-hexadiene, 5-methyl-1,4-hexadiene, and 1,7-octadiene. These monomers (b3) other than cyclic olefins can be used either alone or in combination of two or more.
[0039] The cyclic olefin polymer (A-1) is obtained by homopolymerizing the cyclic olefin monomer (a) or, if desired, copolymerizing it with at least one monomer selected from the monomers (b1) to (b3). The polymerization method is not particularly limited, and any polymerization method can be adopted. Among them, it is preferable to adopt a ring-opening polymerization method. If the cyclic olefin polymer (A-1) as the polymer (A) having a protic polar group is a ring-opening polymer, the processability of the obtained resin film can be improved. More specifically, it is preferable that the cyclic olefin polymer (A-1) is a ring-opening polymer containing a structure according to the following formula (RO-COP). [ka] [In the above formula (RO-COP), R 1 and R 2 represents hydrogen or a group or structure corresponding to each of the above-mentioned monomers (a), (b1), and (b2). 1 and R 2 may together form a ring structure.
[0040] Furthermore, the polymer obtained by polymerization may be further hydrogenated. In this specification, the hydrogenated polymer is also included in the cyclic olefin polymer (A-1) having a protic polar group. When the cyclic olefin polymer (A-1) is a hydrogenated polymer, it is preferable that 95.0% or more of the carbon-carbon double bonds contained in the main chain and the part other than the main chain are hydrogenated, more preferably 97.0% or more, and even more preferably 99.0% or more.
[0041] The cyclic olefin polymer (A-1) can also be obtained by introducing a protic polar group into a cyclic olefin polymer not having a protic polar group using a known modifier, and optionally hydrogenating the polymer. Here, hydrogenation may be performed on the polymer before the protic polar group is introduced. The cyclic olefin polymer (A-1) may also be obtained by a method in which a protic polar group is further introduced into a cyclic olefin polymer having a protic polar group.
[0042] In addition, when the cyclic olefin polymer (A-1) is a polymer obtained by hydrogenating a ring-opening polymer containing a structure according to the above formula (RO-COP), it is preferable that the cyclic olefin polymer (A-1) contains a structure according to the following formula: [ka] [In the above formula, R 1 and R 2 represents hydrogen, a group or structure corresponding to each of the above-mentioned monomers (a), (b1), and (b2), or a hydride thereof. 1 and R 2 may together form a ring structure.
[0043] [Occupancy ratio of monomer units having protic polar groups in polymer (A-1)] If the proportion of the monomer unit having a protonic polar group in the polymer (A-1) is 51 mol% or more, the reaction between the crosslinking agent (B) and the protonic polar group occurs at a sufficient frequency, and the crosslinked structure is formed at a sufficient frequency, so that the ITO wrinkle suppression performance, chemical resistance, and heat resistance of the obtained resin film can be improved in a balanced manner. Furthermore, the proportion of the monomer unit having a protonic polar group in the polymer (A-1) is preferably 55 mol% or more, preferably 100 mol% or less, more preferably 80 mol% or less, and even more preferably 75 mol% or less. If the proportion of the monomer unit having a protonic polar group in the polymer (A-1) is 55 mol% or more, the ITO wrinkle suppression performance, chemical resistance, and heat resistance of the obtained resin film can be improved in a more balanced manner. When the proportion of the monomer units having a protic polar group in the polymer (A-1) is not more than the above upper limit, the tensile strength and tensile elongation properties of the resulting resin film can be improved in a well-balanced manner.
[0044] <<Polyamide-imide resin (A-2)>> The "polyamideimide resin (A-2)" as the polymer (A) having a protonic polar group is a polymer (i.e., a polyamideimide resin) having an amide bond and an imide bond in the repeating unit, and is a polymer having a protonic polar group. The polyamideimide resin (A-2) can also be obtained by a method of introducing a protonic polar group into a polyamideimide having no protonic polar group using a known modifier. The polyamideimide resin (A-2) may also be obtained by a method of further introducing a protonic polar group into a polyamideimide having a protonic polar group. Therefore, among the various polyamideimides listed below, those having a protonic polar group can be used as is or further modified to introduce a protonic polar group, and those not having a protonic polar group can be used after being modified using a known modifier to introduce a protonic polar group.
[0045] The polyamideimide resin (A-2) may be a polyamideimide having a branched structure or a polyamideimide having a linear structure. Among them, the polyamideimide is preferably a polyamideimide having a branched structure. If the polyamideimide resin (A-2) is a polyamideimide having a branched structure, the chemical resistance of the resin composition can be improved.
[0046] Examples of polyamideimides having a branched structure include compounds having a structural unit represented by the following formula (2) and a structural unit represented by the following formula (3) and having one or more terminal structures represented by the following structural formulas (α), (β) and (γ), compounds represented by the following formula (4), polyamideimide resins having a branched structure (Unidic EMG-793, manufactured by DIC Corporation), and polyamideimide resins having a branched structure (Unidic EMG-1015, manufactured by DIC Corporation).
[0047] [ka] (In the above formula (2), R1 represents an organic group having a cyclic aliphatic structure having 6 to 13 carbon atoms.)
[0048] [ka] (In the above formula (3), R1 represents an organic group having a cyclic aliphatic structure with 6 to 13 carbon atoms, and R2 represents a linear hydrocarbon structure having a number average molecular weight of 700 to 4500.)
[0049] [ka]
[0050] [ka]
[0051] [ka]
[0052] [ka] (In the formula (4), n is an integer of 2 or more and 200 or less.)
[0053] The polyamideimide resin having a protic polar group and having the structure represented by the above formula (4) can be obtained, for example, by reacting an isophorone diisocyanate isocyanurate represented by the following formula (5) with trimellitic anhydride. [ka]
[0054] In this reaction, a multifunctional polyol containing two or more hydroxyl groups may be added as a chain transfer agent to introduce a moiety having a urethane structure into a partial structure of the above formula (4). By introducing a moiety having a urethane structure into a partial structure of the above formula (4), the physical properties of the polyamideimide having a branched structure can be controlled. An example of the moiety having a urethane structure is a moiety represented by the following formula (6).
[0055] [ka] (In the above formula (6), R1 represents an organic group having a cyclic aliphatic structure with 6 to 13 carbon atoms, and R2 represents a linear hydrocarbon structure having a number average molecular weight of 700 to 4500.)
[0056] Moreover, examples of polyamideimides having a linear structure include compounds represented by the following formula (7).
[0057] [ka] (In the above formula (7), n is an integer of 2 or more and 400 or less.)
[0058] The compound represented by the above formula (7) can be obtained by reacting trimellitic anhydride with isophorone diisocyanate.
[0059] <Crosslinking agent (B)> The crosslinking agent (B) is a compound that acts to enhance the ITO wrinkle suppression performance, chemical resistance, and heat resistance of the resin film by forming a crosslinked structure in the resin film. The crosslinking agent (B) is characterized by containing a compound represented by the following formula (1). By containing the compound represented by the following formula (1), the crosslinking agent (B) can impart high heat resistance to the resin film compared to epoxy resins that have been conventionally used as crosslinking agents. Furthermore, the crosslinking agent (B) may contain, in addition to the compound represented by the following formula (1), a dimer of the compound represented by the following formula (1) and other polymers. [ka] [In formula (1), each of the multiple R's independently represents an alkyl group having 1 to 6 carbon atoms or an alkoxy group having 1 to 6 carbon atoms; 1 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms, and m, n, p, and q each represent an integer of 0 to 4.
[0060] where R and R 1 The alkyl group having 1 to 6 carbon atoms that can be included is not particularly limited, and examples thereof include alkyl groups having a straight chain, branched chain, or cyclic structure such as a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, etc. Among these, the alkyl group having 1 to 6 carbon atoms is preferably a methyl group or an ethyl group, and more preferably a methyl group. In addition, R and R 1 The alkoxy group having 1 to 6 carbon atoms that can be included is not particularly limited, and examples thereof include alkoxy groups having a straight chain, branched chain, or cyclic structure such as a methoxy group, an ethoxy group, a propoxy group, a butoxy group, a pentoxy group, a hexoxy group, etc. Among these, the alkoxy group having 1 to 6 carbon atoms is preferably a methoxy group, an ethoxy group, or a propoxy group, and more preferably a methoxy group. From the viewpoint of further improving the heat resistance of the resulting resin film, it is preferable that m, n, p, and q are all "0", in other words, the compound represented by formula (1) has no substituents. In this case, hydrogen atoms are bonded to all positions in formula (1) where "R" can be bonded. Also, R 1 are preferably all hydrogen atoms.
[0061] Furthermore, the compound satisfying formula (1) is preferably a compound having no substituent and satisfying the following structure (1-α) in which three glycidyl ether groups are bonded at predetermined positions. When the crosslinking agent (B) contains a compound satisfying the following structure (1-α), the crosslinking agent (B) may contain a compound satisfying the following structure (1-β), which is a dimer of a compound satisfying the following structure (1-α). Such a crosslinking agent (B) is commercially available as "Techmore VG3101L" manufactured by Printec Co., Ltd. [ka]
[0062] <<Crosslinking agent (B) content>> The content of the crosslinking agent (B) in the resin composition relative to 100 parts by mass of the polymer (A) having a protic polar group is preferably 5 parts by mass or more, more preferably 15 parts by mass or more, even more preferably 25 parts by mass or more, and preferably 160 parts by mass or less, more preferably 140 parts by mass or less, and even more preferably 55 parts by mass or less. If the content of the crosslinking agent (B) relative to the polymer (A) having a protic polar group is the above-mentioned lower limit value or more, the ITO wrinkle suppression performance, chemical resistance, and light transmittance of the obtained resin film can be improved. In addition, if the content of the crosslinking agent (B) relative to the polymer (A) having a protic polar group is the above-mentioned upper limit value or less, the ITO wrinkle suppression performance and chemical resistance of the obtained resin film can be further improved. In addition, when the crosslinking agent (B) contains both the compound represented by formula (1) and the dimer of the compound represented by formula (1), it is preferable that the total content of these satisfies the above-mentioned preferred range.
[0063] <Phenol-based antioxidants (C)> As the phenol-based antioxidant (C), a conventionally known one can be used. For example, the phenol-based antioxidant (C) may be an acrylate compound such as 2-t-butyl-6-(3-t-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate, 2,4-di-t-amyl-6-[1-(3,5-di-t-amyl-2-hydroxyphenyl)ethyl]phenyl acrylate; 2,6-di-t-butyl-4-methylphenol, 2,6-di-t-butyl-4-ethylphenol, octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2,2'-methylene-bis(4-methyl-6-t-butylphenol), 4,4'-butylidene-bis(6-t -butyl-m-cresol), 4,4'-thiobis(3-methyl-6-t-butylphenol), bis(3-cyclohexyl-2-hydroxy-5-methylphenyl)methane, 3,9-bis[2-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane, 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], triethylene glycol Alkyl-substituted phenolic compounds such as bis[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionate] and tocopherol; triazine group-containing phenolic compounds such as 6-(4-hydroxy-3,5-di-t-butylanilino)-2,4-bis-octylthio-1,3,5-triazine, 6-(4-hydroxy-3,5-dimethylanilino)-2,4-bis-octylthio-1,3,5-triazine, 6-(4-hydroxy-3-methyl-5-t-butylanilino)-2,4-bis-octylthio-1,3,5-triazine, and 2-octylthio-4,6-bis-(3,5-di-t-butyl-4-oxyanilino)-1,3,5-triazine; and the like can be used.Among them, alkyl-substituted phenolic compounds are preferred, and pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] is more preferred. The compound as the phenolic antioxidant (C) does not have two or more alkoxymethyl groups or two or more methylol groups.
[0064] <<Phenol-based antioxidant (C) content>> The content of the phenolic antioxidant (C) in the resin composition is preferably 0.3 parts by mass or more, more preferably 1 part by mass or more, more preferably 15 parts by mass or less, more preferably 10 parts by mass or less, and even more preferably 8 parts by mass or less, based on 100 parts by mass of the polymer (A) having a protic polar group. If the content of the phenolic antioxidant (C) based on the polymer (A) having a protic polar group is equal to or more than the above lower limit, the light transmittance of the resulting resin film can be improved. If the content of the phenolic antioxidant (C) based on the polymer (A) having a protic polar group is equal to or less than the above upper limit, the ITO wrinkle suppression performance of the resulting resin film can be further improved, and the antioxidant (C) can be prevented from easily bleeding out in the resulting resin film.
[0065] <Compounds having two or more alkoxymethyl groups and compounds having two or more methylol groups> The compound having two or more alkoxymethyl groups and the compound having two or more methylol groups are components that can act to further enhance the ITO wrinkle suppression performance of the obtained resin film. Furthermore, by blending the compound having two or more alkoxymethyl groups and the compound having two or more methylol groups in the resin composition, the chemical resistance of the resin film can be improved. From the viewpoint of further exerting such effects, it is preferable that the resin composition contains at least a compound having two or more alkoxymethyl groups.
[0066] <<Compounds having two or more alkoxymethyl groups>> Examples of compounds having two or more alkoxymethyl groups include phenol compounds in which two or more alkoxymethyl groups are directly bonded to an aromatic ring, melamine compounds in which an amino group is substituted with two or more alkoxymethyl groups, and urea compounds in which an amino group is substituted with two or more alkoxymethyl groups.
[0067] Examples of phenol compounds in which two or more alkoxymethyl groups are directly bonded to an aromatic ring include dimethoxymethyl-substituted phenol compounds such as 2,6-dimethoxymethyl-4-t-butylphenol and 2,6-dimethoxymethyl-p-cresol; tetramethoxymethyl-substituted biphenyl compounds such as 3,3',5,5'-tetramethoxymethyl-4,4'-dihydroxybiphenyl (for example, trade name "TMOM-BP", manufactured by Honshu Chemical Industry Co., Ltd.) and 1,1-bis[3,5-di(methoxymethyl)-4-hydroxyphenyl]-1-phenylethane; and hexamethoxymethyl-substituted triphenyl compounds such as 4,4',4"-(ethylidyne)tris[2,6-bis(methoxymethyl)phenol] (for example, trade name "HMOM-TPHAP-GB", manufactured by Honshu Chemical Industry Co., Ltd.).
[0068] Examples of melamine compounds in which the amino group is substituted with two or more alkoxymethyl groups include N,N'-dimethoxymethylmelamine, N,N',N"-trimethoxymethylmelamine, N,N,N',N"-tetramethoxymethylmelamine, N,N,N',N',N"-pentamethoxymethylmelamine, N,N,N',N',N",N"-hexamethoxymethylmelamine (for example, trade names "Nikarac MW-390LM" and "Nikarac MW-100LM", both manufactured by Sanwa Chemical Co., Ltd.), and polymers thereof.
[0069] Examples of urea compounds substituted with two or more alkoxymethyl groups include those sold under the trade names "Nicalac MX270", "Nicalac MX280", and "Nicalac MX290" (all manufactured by Sanwa Chemical Co., Ltd.).
[0070] <<Compounds with two or more methylol groups>> An example of a compound having two or more methylol groups is a phenol compound in which two or more methylol groups are directly bonded to an aromatic ring. Examples of phenol compounds in which two or more methylol groups are directly bonded to an aromatic ring include 2,4-dihydroxymethyl-6-methylphenol, 2,6-bis(hydroxymethyl)-p-cresol, 4-tertiary-butyl-2,6-bis(hydroxymethyl)phenol, bis(2-hydroxy-3-hydroxymethyl-5-methylphenyl)methane (trade name "DM-BIPC-F", manufactured by Asahi Organic Chemicals Co., Ltd.), bis(4-hydroxy-3-hydroxymethyl-5-methylphenyl)methane (trade name "DM-BIOC-F", manufactured by Asahi Organic Chemicals Co., Ltd.), and 2,2-bis(4-hydroxy-3,5-dihydroxymethylphenyl)propane (trade name "TM-BIP-A", manufactured by Asahi Organic Chemicals Co., Ltd.).
[0071] Among the above-mentioned compounds having two or more alkoxymethyl groups and compounds having two or more methylol groups, N,N,N',N',N",N"-hexamethoxymethylmelamine, which is a type of compound having two or more alkoxymethyl groups, is preferred from the viewpoint of high reactivity.
[0072] <<Content of compounds having two or more alkoxymethyl groups and compounds having two or more methylol groups>> In the case where the resin composition contains both or either one of a compound having two or more alkoxymethyl groups and a compound having two or more methylol groups, the total content of these is preferably 1 part by mass or more and 100 parts by mass or less per 100 parts by mass of the polymer (A) having a protonic polar group. If the total content of the compound having two or more alkoxymethyl groups and the compound having two or more methylol groups is within the above range, the ITO wrinkle suppression performance of the resin film can be further improved. In particular, if the total content of the compound having two or more alkoxymethyl groups and the compound having two or more methylol groups is below the above upper limit, film reduction in the curing process under high temperature conditions such as 100 ° C. or more can be suppressed, and the heat resistance of the resin film can be further improved.
[0073] <Other additives> The resin composition of the present invention may optionally contain additives other than those described above. Examples of such additives include a polyfunctional epoxy compound having a structure different from that of the crosslinking agent (B), a silane coupling agent, a surfactant, an antioxidant different from the phenolic antioxidant (C) described above, and a radiation-sensitive compound (D), etc.
[0074] <<Multifunctional epoxy compound with a different structure from crosslinker (B)>> Specific examples of polyfunctional epoxy compounds having a structure different from that of the crosslinking agent (B) include, for example, an epoxy compound having a dicyclopentadiene skeleton (trade name "HP-7200", manufactured by DIC Corporation), a 1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol (a 15-functional alicyclic epoxy resin having a cyclohexane skeleton and terminal epoxy groups, trade name "EHPE3150", manufactured by Daicel Corporation), and epoxidized 3-cyclohexene-1,2-dicarboxylate bis(3-cyclohexenylmethyl)-modified ε-caprolactone (an aliphatic cyclic trifunctional epoxy resin, trade name "Epoxy". "Lead GT301", Daicel Corporation), butanetetracarboxylic acid tetra(3,4-epoxycyclohexylmethyl) modified ε-caprolactone (aliphatic cyclic tetrafunctional epoxy resin, trade name "Epolead GT401", Daicel Corporation), 3,4-epoxycyclohexenylmethyl-3',4'-epoxycyclohexenecarboxylate (trade name "Celloxide 2021", "Celloxide 2021P", Daicel Corporation), ε-caprolactone modified 3',4'-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate (trade name "Celloxide 2081", Daicel Corporation), 1,2:8,Epoxy compounds having an alicyclic structure such as 9-diepoxylimonene (trade name "Celloxide 3000", manufactured by Daicel Corporation); and bisphenol A type epoxy compounds (trade names "jER825", "jER827", "jER828EL", "jERYL980", manufactured by Mitsubishi Chemical Corporation, and trade names "EPICLON840" and "EPICLON850", manufactured by DIC Corporation), bisphenol F type epoxy compounds (trade names "jER806", "jER807", "jERYL983U", manufactured by Mitsubishi Chemical Corporation, and trade names "EPICLON830" and "EPICLON835", manufactured by DIC Corporation), hydrogenated bisphenol A type epoxy compounds (trade names "jERY X8000, "jERYX8034" manufactured by Mitsubishi Chemical Corporation, trade name "ST-3000" manufactured by Nippon Steel & Sumitomo Metal Corporation, trade name "RIKA RESIN HBE-100" manufactured by New Japan Chemical Co., Ltd., trade name "EPOLITE 4000" manufactured by Kyoei Chemical Co., Ltd.), long-chain bisphenol A type epoxy resin (trade name "EXA-4816", "EXA-4850-150", "EXA-4850-1000" manufactured by DIC Corporation), EO-modified bisphenol A type epoxy compound (trade name "ADEKA RESIN EP-4000L", "ADEKA RESIN EP-4010L" manufactured by ADEKA Corporation), phenol novolac type multifunctional epoxy compound (trade name "jER152" manufactured by Mitsubishi Chemical Corporation), 1,6-bis(2,Polyfunctional epoxy compounds having a naphthalene skeleton such as 3-epoxypropan-1-yloxy)naphthalene (product name "HP-4032D", manufactured by DIC Corporation), dicyclopentadiene dimethanol diglycidyl ether (product names "ADEKA RESIN EP-4000L", "ADEKA RESIN EP-4088L", manufactured by ADEKA Corporation), glycidylamine type epoxy resins (product names "jER630", manufactured by Mitsubishi Chemical Corporation, product names "TETRAD-C", "TETRAD-X", manufactured by Mitsubishi Gas Chemical Company, Inc.), linear alkyl polyfunctional epoxy compounds (product name "SR-TMP", manufactured by Sakamoto Pharmaceutical Co., Ltd.), polyfunctional epoxy poly Examples of the epoxy compounds include butadiene (trade name "Epolead PB3600", manufactured by Daicel Corporation), (trade name "Epolead PB4700", manufactured by Daicel Corporation), glycerin glycidyl polyether compound (trade name "SR-GLG", manufactured by Sakamoto Yakuhin Kogyo Co., Ltd.), diglycerin polyglycidyl ether compound (trade name "SR-DGE", manufactured by Sakamoto Yakuhin Kogyo Co., Ltd.), polyglycerin polyglycidyl ether compound (trade name "SR-4GL", manufactured by Sakamoto Yakuhin Kogyo Co., Ltd.), and epoxy compounds having no alicyclic structure such as an epoxy compound having a structure represented by the following formula (X) ("WHR-991S", manufactured by Nippon Kayaku Co., Ltd.). These may be used alone or in combination of two or more kinds. Among them, epoxy compounds having an alicyclic structure, i.e., alicyclic epoxy compounds, are preferred. By blending an alicyclic epoxy compound in the resin composition, the transparency of the obtained resin film can be increased.
[0075] [ka]
[0076] The content of the polyfunctional epoxy compound having a structure different from that of the crosslinking agent (B) in the resin composition is preferably 100 parts by mass or less per 100 parts by mass of the polymer (A) having a protonic polar group. If the content of the epoxy group-containing compound is 100 parts by mass or less, the chemical resistance of the resin film can be efficiently improved. In addition to the above-mentioned specific crosslinking agent (B), when the resin composition contains a polyfunctional epoxy compound having a structure different from that of the crosslinking agent (B), it is preferable that the total content of the crosslinking agent (B) and the polyfunctional epoxy compound having a structure different from that of the crosslinking agent (B) satisfies the suitable range of the content of the crosslinking agent (B) relative to 100 parts by mass of the polymer (A) having a protonic polar group in the resin composition described above in the item <<Content of the crosslinking agent (B)>>.
[0077] <<Silane coupling agents, surfactants, and antioxidants>> The silane coupling agent functions to enhance the adhesion between the resin film obtained by using the resin composition of the present invention and the substrate on which the resin film is formed.The silane coupling agent is not particularly limited, and any known agent can be used (for example, see JP 2015-94910 A).More specifically, alkoxysilanes such as glycidoxypropyltrimethoxysilane can be suitably used as the silane coupling agent. The content of the silane coupling agent is usually from 0.01 to 10 parts by mass per 100 parts by mass of the polymer (A) having a protic polar group.
[0078] The surfactant is a component that can improve the coatability of the resin composition of the present invention. The surfactant is not particularly limited, and known silicone surfactants, fluorine surfactants, polyoxyalkylene surfactants, methacrylic acid copolymer surfactants, acrylic acid copolymer surfactants, etc. can be used (see, for example, International Publication No. 2017 / 163981). Among them, silicone surfactants such as organosiloxane polymers can be preferably used as the surfactant. The content of the surfactant is usually from 0.01 part by mass to 1 part by mass per 100 parts by mass of the polymer (A) having a protic polar group.
[0079] The antioxidant different from the above-mentioned phenol-based antioxidant (C) is a component that can enhance the stability of the resin composition of the present invention. The antioxidant is not particularly limited, and known antioxidants such as phosphorus-based antioxidants, sulfur-based antioxidants, amine-based antioxidants, and lactone-based antioxidants can be used (for example, see International Publication No. 2017 / 163981).
[0080] The silane coupling agent, the surfactant, and the antioxidant different from the above-mentioned phenol-based antioxidant (C) can each be used alone or in combination of two or more. The amount of the silane coupling agent, the surfactant, and the antioxidant different from the above-mentioned phenol-based antioxidant (C) to be blended in the resin composition can be adjusted as desired.
[0081] <<Radiation-sensitive compound (D)>> The radiation-sensitive compound (D) is a compound that can cause a chemical reaction when irradiated with radiation. Here, the radiation is not particularly limited, and examples thereof include visible light; ultraviolet light; X-rays; single-wavelength light such as g-rays, h-rays, and i-rays; laser light such as KrF excimer laser light and ArF excimer laser light; and particle beams such as electron beams. The radiation-sensitive compound (D) is not particularly limited, and an acetophenone compound, a triarylsulfonium salt, and an azide compound can be used. Among them, an azide compound such as a quinone diazide compound can be preferably used. The radiation-sensitive compound (D) can be used alone or in combination of two or more kinds. The amount of the radiation-sensitive compound (D) to be mixed in the resin composition can be adjusted arbitrarily. If the resin composition contains the radiation-sensitive compound (D), a resin film having a desired pattern can be well formed by patterning the resin film.
[0082] <Solvent> The solvent that may be optionally contained in the resin composition of the present invention is not particularly limited, and any solvent known as a solvent for resin compositions can be used. Examples of such solvents include linear ketones, alcohols, alcohol ethers, esters, cellosolve esters, propylene glycols, diethylene glycols such as diethylene glycol ethyl methyl ether, saturated γ-lactones, halogenated hydrocarbons, aromatic hydrocarbons, and polar solvents such as dimethylacetamide, dimethylformamide, and N-methylacetamide (see, for example, International Publication No. 2015 / 033901). These solvents may be used alone or in combination of two or more. The amount of the solvent in the resin composition is not particularly limited, and is preferably 10 parts by mass or more, preferably 10,000 parts by mass or less, more preferably 5,000 parts by mass or less, and even more preferably 1,000 parts by mass or less, relative to 100 parts by mass of the polymer (A) having a protic polar group.
[0083] <Method of producing resin composition> The resin composition of the present invention can be prepared by mixing the above-mentioned components by a known method and optionally filtering them. Here, for mixing, known mixers such as stirrers, agitators, ball mills, sand mills, bead mills, pigment dispersers, crushers, ultrasonic dispersers, homogenizers, planetary mixers, and film mixes can be used. In addition, for filtering the mixture, a general filtering method using a filter medium such as a filter can be used.
[0084] (Method of manufacturing resin film) The resin film made of the resin composition of the present invention can be produced by the method for producing a resin film of the present invention, which includes a step (curing step) of heating the coating film formed using the above-mentioned resin composition of the present invention at 100°C or higher. The method for producing a resin film of the present invention may further include a step (coating film forming step) of forming a coating film using the resin composition of the present invention on a substrate on which the resin film is to be formed. Furthermore, it is also possible to form a patterned resin film using a resin composition containing a radiation-sensitive compound (D) as the resin composition of the present invention. In this case, an operation of patterning the coating film is carried out when forming the coating film, and further, a bleaching step may be carried out after the coating film forming step and before the curing step.
[0085] <Coating film formation process> The method for disposing the coating film on the substrate on which the resin film is to be formed is not particularly limited, and can be carried out according to a known method such as a coating method or a film lamination method. The formation of a coating film by the coating method can be carried out by coating a resin composition on a substrate and then drying by heating (pre-baking). As a method for coating the resin composition, various methods such as spray coating, spin coating, roll coating, die coating, doctor blade, bar coating, screen printing, inkjet, etc. can be adopted. The heating and drying conditions vary depending on the types and blending ratios of the components contained in the resin composition, but the heating temperature is usually 30 to 150°C, preferably 60 to 120°C, and the heating time is usually 0.5 to 90 minutes, preferably 1 to 60 minutes, more preferably 1 to 30 minutes.
[0086] In addition, the formation of the coating film by the film lamination method can be carried out by applying the resin composition onto a substrate for forming a B-stage film such as a resin film or a metal film, drying by heating (pre-baking) to obtain a B-stage film, and then laminating this B-stage film onto a substrate. The application of the resin composition onto the substrate for forming a B-stage film and the drying by heating of the resin composition can be carried out in the same manner as the application of the resin composition and the drying by heating in the above-mentioned coating method. The lamination can be carried out using a pressure bonding machine such as a pressure laminator, a press, a vacuum laminator, a vacuum press, or a roll laminator.
[0087] Patterning of the coating film, which is an optional operation, can be carried out using a known patterning method, such as a method in which the coating film before patterning is irradiated with radiation to form a latent image pattern, and then the coating film having the latent image pattern is brought into contact with a developer to make the pattern visible.
[0088] Here, the radiation is not particularly limited as long as it can cause a chemical reaction in the radiation-sensitive compound (D) to improve the solubility of the radiation-exposed portion in the developer, and any radiation can be used.Specifically, for example, visible light; ultraviolet light; X-rays; single-wavelength light such as g-rays, h-rays, and i-rays; laser beams such as KrF excimer laser beams and ArF excimer laser beams; particle beams such as electron beams; and the like can be used.These radiations can be used alone or in combination of two or more.
[0089] As the developer, a known alkaline developer such as an aqueous solution of an alkaline compound can be used. The method and conditions for bringing the coating film into contact with the developer are not particularly limited, and known methods and conditions can be used.
[0090] Furthermore, if necessary, a bleaching step may be carried out to deactivate the radiation-sensitive compound (D) contained in the resin composition. In the bleaching step, any radiation may be irradiated to the entire surface of the coating film. For the radiation irradiation, the method exemplified for forming the latent image pattern above may be used. Furthermore, the resin film may be heated simultaneously with or after the radiation irradiation. By deactivating the radiation-sensitive compound (D) in the bleaching step, the transparency of the obtained resin film can be further increased.
[0091] <Curing process> In the curing process, the coating is heated (post-baked) at a temperature of 100°C or higher to harden it.
[0092] The coating film can be heated using, for example, a hot plate, an oven, or the like, without any particular limitation. The heating may be performed under an inert gas atmosphere, if necessary. Examples of the inert gas include nitrogen, argon, helium, neon, xenon, krypton, and the like. Among these, nitrogen and argon are preferred, and nitrogen is particularly preferred.
[0093] Here, the temperature at which the coating film is heated in the curing step must be 100° C. or higher, preferably 150° C. or higher, more preferably 200° C. or higher, and even more preferably 250° C. or higher. By using the resin composition of the present invention, a good film can be formed even when the temperature at which the coating film is heated is as high as 100° C. or higher. Furthermore, the upper limit of the temperature at which the coating film is heated in the curing step is not particularly limited, but is preferably 400° C. or lower. The time for heating the coating film in the curing step can be appropriately selected depending on the area and thickness of the coating film, the equipment used for heating, and the like, and can be, for example, 10 to 120 minutes.
[0094] The resin film that has been subjected to this curing step preferably has a transmittance of 95% or more for light with a wavelength of 400 nm. The "transmittance" can be measured according to the method described in the Examples.
[0095] (Electronic component) The electronic component of the present invention includes a resin film made of the resin composition of the present invention described above. And since the electronic component of the present invention includes a resin film formed from the resin composition of the present invention, which is excellent in ITO wrinkle suppression performance, chemical resistance, and heat resistance, it has high performance.
[0096] <Type of electronic component> The type of the electronic component of the present invention is not particularly limited. For example, since the resin film made of the resin composition of the present invention is excellent in ITO wrinkle suppression performance, chemical resistance, and heat resistance, the electronic component of the present invention can be an electronic component provided with an ITO electrode in which an ITO film is disposed on the surface of the resin film made of the resin composition of the present invention. Further, for example, the resin film of the present invention may be an interlayer insulating film of a redistribution layer provided in a semiconductor device.
Example
[0097] Hereinafter, the present invention will be specifically described based on examples, but the present invention is not limited to these examples. In the following description, “%” and “parts” representing amounts are based on mass unless otherwise specified. Also, the pressure is gauge pressure. In the examples and comparative examples, the ITO wrinkle suppression performance, chemical resistance, heat resistance (weight loss on heating), and light transmittance of the resin film were evaluated using the following methods, respectively.
[0098] <ITO wrinkle suppression performance> The resin compositions obtained in the Examples and Comparative Examples were applied onto a glass substrate (Corning 1737, Corning) by spin coating, and dried (pre-baked) at 120°C for 2 minutes using a hot plate to form a coating film. Next, the temperature was raised from 30°C to 250°C at 10°C / min in a nitrogen atmosphere using an oven, and then post-baked at 250°C for 60 minutes to form a resin film with a thickness of 2 μm. An ITO transparent electrode was formed on this resin film with a thickness of 40 nm using a sputtering device (Shibaura Eletec Corporation, "i-Miller CFS-4EP-LL", stage temperature 30°C). The glass substrate of the obtained laminate with an ITO transparent electrode was cut into 1.5 cm squares to prepare a test piece. The glass substrate side of the prepared test piece was placed on a hot plate heated at 200°C for 5 minutes, and then cooled to room temperature. Next, the surface of the ITO transparent electrode side of the test piece was observed under an optical microscope (100x), and the ratio of the area of the wrinkled part to the total area of the resin film surface (1.5cm x 1.5cm) was calculated and evaluated according to the following criteria. The area of the wrinkled part was extracted by binarizing the image obtained by the optical microscope. A: No wrinkles on the surface of the resin film. B: Wrinkles are formed on the surface of the resin film, but the area of the wrinkles is less than 1 / 4 of the total area of the resin film surface. C: Wrinkles are formed on the surface of the resin film, but the area of the wrinkled part is 1 / 4 or more of the total area of the resin film surface. <Chemical resistance> The resin compositions obtained in the examples and comparative examples were applied onto a glass substrate (Corning 1737, manufactured by Corning Incorporated) by spin coating, and then heated and dried (pre-baked) at 120°C for 2 minutes using a hot plate to form a coating film. Next, the temperature was raised from 30°C to 250°C at 10°C / min in a nitrogen atmosphere using an oven, and then post-baked at 250°C for 60 minutes to obtain a resin film with a thickness of 2 μm, and the thickness T1 was measured. The obtained resin film was immersed in a monoethanolamine-dimethyl sulfoxide mixture (mixing ratio: monoethanolamine: dimethyl sulfoxide = 7:3, manufactured by Tokyo Ohka Kogyo Co., Ltd., "TOK106") at 40°C for 2 minutes, and then rinsed with pure water for 30 seconds, and the thickness T2 was measured. From the measured values of T1 and T2, the swelling ratio (%): (T2-T1) / T1×100 was calculated and evaluated according to the following criteria. A: Swelling rate is 3% or less. B: Swelling rate is more than 3% and less than 8%. C: Swelling rate is more than 8%. <Heat resistance (heat loss)> Using a sputtering device (Shibaura Eletech Corporation, "i-Miller CFS-4EP-LL"), the resin compositions obtained in the Examples and Comparative Examples were spin-coated onto a silicon wafer on which an aluminum thin film had been formed to a thickness of 100 nm, and then the silicon wafer was heated at 120°C for 2 minutes using a hot plate (film-forming step). Next, the temperature was raised from 30°C to 250°C at a rate of 10°C / min in a nitrogen atmosphere, and then heat-treated at 250°C for 60 minutes to obtain a resin film, thereby obtaining a laminate having a resin film with a thickness of 10 μm on one side (curing step). The obtained laminate was immersed in a 0.5 mol / L hydrochloric acid solution, and the aluminum thin film located between the silicon wafer and the resin film was dissolved in the hydrochloric acid solution to peel off the resin film from the silicon wafer. The peeled off resin film was then washed with water and dried. The dried resin film was heated to 300°C under a nitrogen atmosphere at a heating rate of 10°C / min using a differential thermal thermogravimetric simultaneous measurement device (Seiko Instruments Inc., TG / DTA6200), and the mass W0 of the sample when it reached 300°C and the mass W1 of the sample when it was held at 300°C for 1 hour were measured, and the value of the heat loss: (W0-W1) / W0×100(%) was calculated from these values and evaluated according to the following criteria. The smaller the heat loss, the more excellent the heat resistance of the resin film. A: Weight loss at 300℃ is less than 4%. B: Weight loss at 300℃ is 4% or more but less than 8%. C: Heat loss at 300℃ is 8% or more. <Light transmittance> The resin compositions obtained in the Examples and Comparative Examples were applied onto a glass substrate (Corning 1737, manufactured by Corning Incorporated) by spin coating, and then heated and dried (pre-baked) at 120°C for 2 minutes using a hot plate to form a coating film with a thickness of 2 μm (coating film formation step). Next, the temperature was raised from 30°C to 250°C at a rate of 10°C / min in a nitrogen atmosphere using an oven, and then post-baked at 250°C for 60 minutes to obtain a laminate consisting of a resin film and a glass substrate (curing step). The light transmittance (%) of the obtained laminate at a wavelength of 400 nm was measured using a spectrophotometer V-560 (manufactured by JASCO Corporation). Furthermore, the laminate obtained above was heated (additional heating) at 250° C. for 1 hour in an air atmosphere, and then the light transmittance (%) for light with a wavelength of 400 nm was measured in the same manner as above. The light transmittance (%) of the resin film was calculated as a converted value assuming that the thickness of the resin film was 2 μm, using a glass substrate without a resin film as a blank, and was evaluated according to the following criteria. A: Light transmittance is 96% or more. B: Light transmittance is 93% or more but less than 96%. C: Light transmittance is less than 93%.
[0099] (Synthesis Example 1: Synthesis of Cyclic Olefin Polymer (a-1) Having Protic Polar Groups) As a cyclic olefin polymer (a-1) having a protic polar group, a polymer in which the proportion of monomer units having a protic polar group was 60 mol % was obtained. 40 mol % of N-(2-ethylhexyl)-bicyclo[2.2.1]hept-5-ene-2,3-dicarboximide as a cyclic olefin having an N-substituted imide group and 4-hydroxycarbonyltetracyclo[6.2.1.1 3,6 .0 2,7 100 parts of a monomer mixture consisting of 60 mol % of ]dodec-9-ene, 2 parts of 1,5-hexadiene, 0.02 parts of (1,3-dimesitylimidazolin-2-ylidene)(tricyclohexylphosphine)benzylidene ruthenium dichloride (synthesized by the method described in Org. Lett., Vol. 1, p. 953, 1999), and 200 parts of diethylene glycol ethyl methyl ether were charged into a nitrogen-substituted glass pressure-resistant reactor and reacted at 80°C for 4 hours with stirring to obtain a polymerization reaction liquid. The obtained polymerization reaction liquid was then placed in an autoclave and stirred at 150°C and a hydrogen pressure of 4MPa for 5 hours to carry out a hydrogenation reaction, thereby obtaining a polymer solution containing a hydrogenated polymer as a cyclic olefin polymer (a-1) having a protonic polar group. The polymerization conversion rate of the obtained cyclic olefin polymer (a-1) was 99.7%, the weight average molecular weight in terms of polystyrene was 7,150, the number average molecular weight was 4,690, the molecular weight distribution was 1.52, and the hydrogenation rate was 99.7%. The solid content concentration of the obtained polymer solution of the cyclic olefin polymer (a-1) was 34.4% by mass.
[0100] (Synthesis Example 2: Synthesis of Cyclic Olefin Polymer (a-2) Having Protic Polar Groups) As a cyclic olefin polymer (a-2) having a protic polar group, a polymer in which the proportion of monomer units having a protic polar group was 70 mol % was obtained. In the monomer mixture used in the polymerization reaction, N-(2-ethylhexyl)-bicyclo[2.2.1]hept-5-ene-2,3-dicarboximide was used as a cyclic olefin having an N-substituted imide group, and 4-hydroxycarbonyltetracyclo[6.2.1.1 was used as a cyclic olefin having a protic polar group. 3,6 .0 2,7 The blend ratio of 4-hydroxycarbonyltetracyclo[6.2.1.1]dodec-9-ene in the resulting polymer (a-2) was changed. 3,6 .0 2,7 Cyclic olefin polymer (a-2) was obtained in the same manner as in Synthesis Example 1, except that the occupancy ratio of the monomer unit derived from dodeca-9-ene was 70 mol % and the amount of 1,5-hexadiene was 2.7 parts. The polymerization conversion rate of the obtained cyclic olefin polymer (a-2) was 99.7%, the weight average molecular weight in terms of polystyrene was 5,390, the number average molecular weight was 3,480, the molecular weight distribution was 1.55, and the hydrogenation rate was 99.7%. The solid content concentration of the polymer solution of the obtained cyclic olefin polymer (a-2) was 34.4 mass %.
[0101] (Synthesis Example 3: Synthesis of Cyclic Olefin Polymer (a-3) Having Protic Polar Group) As a cyclic olefin polymer (a-3) having a protic polar group, a polymer in which the proportion of monomer units having a protic polar group was 50 mol % was obtained. In the monomer mixture used in the polymerization reaction, N-(2-ethylhexyl)-bicyclo[2.2.1]hept-5-ene-2,3-dicarboximide was used as a cyclic olefin having an N-substituted imide group, and 4-hydroxycarbonyltetracyclo[6.2.1.1 was used as a cyclic olefin having a protic polar group. 3,6 .0 2,7 The blend ratio of 4-hydroxycarbonyltetracyclo[6.2.1.1]dodec-9-ene in the resulting polymer (a-3) was changed. 3,6 .0 2,7Cyclic olefin polymer (a-3) was obtained in the same manner as in Synthesis Example 1, except that the occupancy ratio of the monomer unit derived from dodec-9-ene was 50 mol % and the amount of 1,5-hexadiene was 2.7 parts. The polymerization conversion rate of the obtained cyclic olefin polymer (a-3) was 99.7%, the weight average molecular weight in terms of polystyrene was 4,310, the number average molecular weight was 2,890, the molecular weight distribution was 1.49, and the hydrogenation rate was 99.7%. The solid content concentration of the polymer solution of the obtained cyclic olefin polymer (a-3) was 34.4 mass %.
[0102] (Synthesis Example 4: Synthesis of Cyclic Olefin Polymer (a-4) Having No Protonic Polar Group) Tetracyclo[6.5.0.1 2,5 .0 8,13 ] 80 mol parts of trideca-3,8,10,12-tetraene (MTF), 20 mol parts of N-(4-phenyl)-(5-norbornene-2,3-dicarboximide) (NBPI), 6 mol parts of 1-hexene, 590 mol parts of anisole, and 0.015 mol parts of 4-acetoxybenzylidene (dichloro) (4,5-dibromo-1,3-dimesityl-4-imidazolin-2-ylidene) (tricyclohexylphosphine) ruthenium (C1063, manufactured by Wako Pure Chemical Industries, Ltd.) as a ruthenium-based polymerization catalyst were charged into a nitrogen-substituted pressure-resistant glass reactor, and a polymerization reaction was carried out at 80 ° C. for 1 hour with stirring to obtain a solution of a ring-opened polymer. When this solution was measured by gas chromatography, it was confirmed that substantially no monomer remained, and the polymerization conversion rate was 99% or more. The resulting ring-opening polymer solution was then placed in a nitrogen-purged autoclave equipped with a stirrer and stirred at 150°C and a hydrogen pressure of 7 MPa for 5 hours to carry out a hydrogenation reaction. The resulting hydrogenation reaction solution was concentrated to obtain a solution of a cyclic olefin polymer (a-4) having no protic polar groups (solid content concentration: 55.5%). The resulting cyclic olefin polymer (a-4) having no protic polar groups had a weight average molecular weight of 50,000, a number average molecular weight of 20,000, and a hydrogenation rate of 97%.
[0103] Example 1 291 parts of the solution of the cyclic olefin polymer (a-1) having a protic polar group obtained in Synthesis Example 1 (100 parts of the cyclic olefin polymer (A-1) having an occupancy ratio of monomer units having a protic polar group of 51 mol % or more), a compound as a crosslinking agent (B) which is a mixture of a compound satisfying the following formula (1-α) and a compound satisfying the following formula (1-β) ("Techmore A resin composition was prepared by mixing and dissolving 10 parts of "VG3101L", the compound of formula (1-α): the compound of formula (1-β) = 9:1 (by mass), 0.1 parts of an organosiloxane polymer (manufactured by Shin-Etsu Chemical Co., Ltd., product name "KP-341") as a surfactant, 2 parts of pentaerythritol tetrakis [3- (3, 5-di-tert-butyl-4-hydroxyphenyl) propionate] (trade name "Irganox1010FF", manufactured by BASF) as an antioxidant, 2 parts of glycidoxypropyltrimethoxysilane (manufactured by XIAMETER, product name "OFS-6040") as a silane coupling agent, and 41 parts of diethylene glycol ethyl methyl ether (manufactured by Toho Chemical Co., Ltd., product name "EDM-S") as a solvent. The mixture was then filtered through a polytetrafluoroethylene filter having a pore size of 0.45 μm. The resin film formed using the obtained resin composition was subjected to various evaluations as described above. The results are shown in Table 1. [ka]
[0104] (Examples 2 to 3, 7 to 9) Resin compositions were prepared in the same manner as in Example 1, except that the blending amount of the crosslinking agent (B) and the blending amount of the solvent were changed as shown in Table 1. The obtained resin composition was then used for evaluation in the same manner as in Example 1. The results are shown in Table 1.
[0105] Example 4 A resin composition was prepared in the same manner as in Example 1, except that the blending amount of the crosslinking agent (B) and the blending amount of the solvent were changed as shown in Table 1, and 15 parts of N,N,N',N',N",N"-hexamethoxymethylmelamine (product name "Nikarac MW-100LM", manufactured by Sanwa Chemical Co., Ltd.) was blended as a compound having two or more alkoxymethyl groups. The obtained resin composition was then used for evaluation in the same manner as in Example 1. The results are shown in Table 1.
[0106] Example 5 A resin composition was prepared in the same manner as in Example 1, except that the polymer (a-2) synthesized in Synthesis Example 2 above, in which the occupancy ratio of monomer units having a protic polar group is 70 mol %, was used as the cyclic olefin polymer (A-1) in which the occupancy ratio of monomer units having a protic polar group is 51 mol % or more, and the blending amounts of the crosslinking agent (B) and the solvent were changed as shown in Table 1, respectively. The obtained resin composition was then used for evaluation in the same manner as in Example 1. The results are shown in Table 1.
[0107] Example 6 Instead of the predetermined cyclic olefin polymer (A-1), a polyamideimide resin (A-2) having a protonic polar group was used. As the polyamideimide resin (A-2), 229 parts of a propylene glycol methyl ether acetate and n-butanol mixed solution of a polyamideimide resin having a branched structure (DIC Corporation, Unidic EMG-793, 100 parts as a branched polyamideimide resin (a-5) having a carboxyl group) was used, and the blending amounts of the crosslinking agent (B) and the solvent were changed as shown in Table 1, respectively. The resin composition was prepared in the same manner as in Example 1. The obtained resin composition was then used for evaluation in the same manner as in Example 1. The results are shown in Table 1.
[0108] (Examples 10 to 11) Resin compositions were prepared in the same manner as in Example 1, except that the blending amounts of the crosslinking agent (B), the antioxidant (C), and the solvent were changed as shown in Table 1. The obtained resin composition was then used for evaluation in the same manner as in Example 1. The results are shown in Table 1.
[0109] Example 12 A resin composition was prepared in the same manner as in Example 1, except that 20 parts of an ester (2.0 moles) of 4,4'-[1-[4-[1-[4-hydroxyphenyl]-1-methylethyl]phenyl]ethylidene]bisphenol and 6-diazo-5,6-dihydro-5-oxo-1-naphthalenesulfonic acid chloride (1,2-naphthoquinone diazide-5-sulfonic acid chloride) (manufactured by Bigen Specialty Chemical Co., Ltd., product name "TPA-520") was blended as the radiation-sensitive compound (D), and the blending amounts of the crosslinking agent (B) and the solvent were changed as shown in Table 1. The obtained resin composition was then used for evaluation in the same manner as in Example 1. The results are shown in Table 1.
[0110] Example 13 A resin composition was prepared in the same manner as in Example 1, except that the antioxidant (C) was not added and the amounts of the crosslinking agent (B) and the solvent added were changed as shown in Table 1. The obtained resin composition was then used for evaluation in the same manner as in Example 1. The results are shown in Table 1.
[0111] Example 14 As the polymer (A) having a protic polar group, a predetermined cyclic olefin polymer (A-1) and a predetermined polyamideimide resin (A-2) were used in the blending ratio shown in Table 1. Furthermore, the blending amount of the solvent was changed as shown in Table 1. A resin composition was prepared in the same manner as in Example 1 except for these points. The obtained resin composition was then used for evaluation in the same manner as in Example 1. The results are shown in Table 1.
[0112] Example 15 The amount of the crosslinking agent (B) and the amount of the solvent were changed as shown in Table 1, and 15 parts of N,N,N',N',N",N"-hexamethoxymethylmelamine (product name "Nikarak MW-100LM", manufactured by Sanwa Chemical Co., Ltd.) was added as a compound having two or more alkoxymethyl groups, and 20 parts of an ester (2.0 mol) of 4,4'-[1-[4-[1-[4-hydroxyphenyl]-1-methylethyl]phenyl]ethylidene]bisphenol and 6-diazo-5,6-dihydro-5-oxo-1-naphthalenesulfonic acid chloride (1,2-naphthoquinone diazide-5-sulfonic acid chloride) (manufactured by Bigen Specialty Chemical Co., Ltd., product name "TPA-520") was added as a radiation-sensitive compound (D). The resin composition was prepared in the same manner as in Example 1. The obtained resin composition was then used for evaluation in the same manner as in Example 1. The results are shown in Table 1.
[0113] Comparative Example 1 A resin composition was prepared in the same manner as in Example 1, except that the crosslinking agent (B) was not blended, and instead 30 parts of butanetetracarboxylic acid tetra(3,4-epoxycyclohexylmethyl)-modified ε-caprolactone (manufactured by Daicel Corporation, product name "Epolead GT401"), which is a multifunctional epoxy compound having a structure different from that of the crosslinking agent (B), was blended, and the blending amount of the solvent was changed as shown in Table 1. The obtained resin composition was then used for evaluation in the same manner as in Example 1. The results are shown in Table 1.
[0114] Comparative Example 2 A resin composition was prepared in the same manner as in Example 1, except that the crosslinking agent (B) was not used, and instead, 30 parts of a bisphenol A type epoxy compound (manufactured by Mitsubishi Chemical Corporation, "jER828EL"), which is a multifunctional epoxy compound having a structure different from that of the crosslinking agent (B), was used, and the amount of the solvent was changed as shown in Table 1. The obtained resin composition was then used for evaluation in the same manner as in Example 1. The results are shown in Table 1.
[0115] Comparative Example 3 A resin composition was prepared in the same manner as in Example 1, except that a solution of polymer (a-3) (100 parts as polymer (a-3)) obtained according to the above Synthesis Example 3, in which the occupancy ratio of monomer units having a protic polar group was 50 mol %, was used instead of the solution of a predetermined cyclic olefin polymer (A-1), and the blending amounts of crosslinking agent (B) and solvent were changed as shown in Table 1, respectively. The obtained resin composition was then used for evaluation in the same manner as in Example 1. The results are shown in Table 1.
[0116] Comparative Example 4 A resin composition was prepared in the same manner as in Example 1, except that a solution of a cyclic olefin polymer (a-4) having no protic polar group obtained according to Synthesis Example 4 (100 parts as polymer (a-4)) was used instead of the solution of a specified cyclic olefin polymer (A-1), the amount of the crosslinking agent (B) having a specified structure was changed to 30 parts, and the solvent was changed to 310 parts of anisole. The obtained resin composition was then used for evaluation in the same manner as in Example 1. The results are shown in Table 1.
[0117] [Table 1]
[0118] From Table 1, it can be seen that the resin compositions of Examples 1 to 15, which contain a specific polymer (A) having a protonic polar group and a crosslinking agent (B) satisfying a specific structure, were able to form resin films excellent in ITO wrinkle suppression performance, chemical resistance, and heat resistance. Also, from Table 1, it can be seen that in the cases of Comparative Examples 1 and 2, which used resin compositions not containing a crosslinking agent (B) satisfying a specific structure, it was not possible to form resin films in which ITO wrinkle suppression performance, chemical resistance, and heat resistance were all simultaneously at high levels. Furthermore, from Table 1, it can be seen that in Comparative Example 3, which used a cyclic olefin polymer in which the occupancy ratio of monomer units having a protonic polar group was less than 51 mol%, and Comparative Example 4, which used a cyclic olefin polymer not having a protonic polar group, the heat resistance of the obtained resin films was excellent, but the ITO wrinkle suppression performance and chemical resistance were low. [Industrial Applicability]
[0119] According to the resin composition of the present invention, a resin film having excellent ITO wrinkle suppression performance, chemical resistance, and heat resistance can be formed. Furthermore, according to the present invention, it is possible to provide a high-performance electronic component having a resin film formed using the resin composition of the present invention. Furthermore, according to the present invention, it is possible to provide a method for producing a resin film, which can efficiently produce the resin film of the present invention using the resin composition of the present invention.
Claims
1. A resin composition comprising a polymer (A) having a protic polar group and a crosslinking agent (B) containing a compound represented by the following formula (1), wherein the polymer (A) having a protic polar group is The composition contains a cyclic olefin polymer (A-1) having a protic polar group, and the proportion of monomer units having a protic polar group is 51 mol % or more; and Contains a polyamideimide resin (A-2) having a protic polar group; At least one of the following is satisfied: The polyamideimide resin (A-2) having a protic polar group is a polyamideimide having a branched structure. Resin composition. 【Chemistry 1】 ・・・(1) In formula (1), each of the R's is independently an alkyl group having 1 to 6 carbon atoms or an alkoxy group having 1 to 6 carbon atoms; 1 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms, and m, n, p, and q each represent an integer of 0 to 4.
2. The resin composition according to claim 1 , further comprising a phenol-based antioxidant (C).
3. The resin composition described in claim 2, wherein the content of the phenol-based antioxidant (C) per 100 parts by mass of the polymer (A) having a protonic polar group is 0.3 parts by mass or more and 15 parts by mass or less.
4. The resin composition according to any one of claims 1 to 3, wherein the polymer (A) having a protic polar group is a cyclic olefin polymer having a carboxyl group.
5. the polymer (A) having a protic polar group is the cyclic olefin polymer (A-1) having a protic polar group, The resin composition according to any one of claims 1 to 4, wherein the cyclic olefin polymer (A-1) having a protic polar group is a ring-opening polymer.
6. The resin composition according to any one of claims 1 to 5, wherein the content of the crosslinking agent (B) relative to 100 parts by mass of the polymer (A) having a protonic polar group is 5 parts by mass or more and 160 parts by mass or less.
7. The resin composition according to any one of claims 1 to 6, further comprising at least one of a compound having two or more alkoxymethyl groups and a compound having two or more methylol groups.
8. The resin composition according to any one of claims 1 to 7, further comprising a radiation-sensitive compound (D).
9. The resin composition according to claim 8 , wherein the radiation-sensitive compound (D) is a quinone diazide compound.
10. An electronic component comprising a resin film made of the resin composition according to any one of claims 1 to 9.
11. A method for producing a resin film, comprising a step of heating a coating film formed using the resin composition according to any one of claims 1 to 9 at 100°C or higher.
Citation Information
Patent Citations
Photosensitive resin composition and method for manufacturing electronic device
JP2017111447A
Photosensitive resin composition, resin film prepared therewith, and electronic apparatus including resin film
JP2018124502A
Photosensitive resin composition and electronic device
WO2015141525A1
Photosensitive resin composition, cured film, element comprising cured film, organic el display device comprising cured film, method for producing cured film, and method for producing organic el display device
WO2019065351A1