Method for producing aqueous polytetrafluoroethylene dispersion

By polymerizing non-fluorinated monomers and tetrafluoroethylene without surfactants, and using controlled amounts of additives, the method addresses the issue of fluorine-based oligomers and low CFT in PTFE dispersions, resulting in stable and environmentally friendly PTFE products with improved film integrity.

JP7586090B2Active Publication Date: 2024-11-19AGC INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021553650
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-10-29
Filing Date
2020-10-28
Publication Date
2024-11-19
Estimated Expiration
2040-10-28

AI Technical Summary

Technical Problem

The production of polytetrafluoroethylene (PTFE) using hydrocarbon-containing surfactants leads to chain transfer reactions, resulting in the formation of undesirable fluorine-based oligomers as by-products, and the coating films formed from PTFE dispersions have a low critical film thickness (CFT) that is prone to cracking.

Method used

A method involving the polymerization of non-fluorinated monomers in an aqueous medium, followed by polymerizing tetrafluoroethylene without surfactants, and adding a nonionic surfactant to concentrate the emulsion, while controlling the amounts of non-fluorinated monomers and nucleating additives to create a hydrophobic environment for stable polymerization, thereby reducing fluorine-based oligomers and increasing CFT.

Benefits of technology

This method produces PTFE dispersions with minimal fluorine-based oligomers and enhances the critical film thickness, reducing cracking and improving environmental sustainability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586090000001
    Figure 0007586090000001
Patent Text Reader

Abstract

The purpose of the present invention is to provide a method which is for producing a polytetrafluoroethylene aqueous dispersion, and by which the amount of a fluorine-based oligomer produced as a by-product is reduced and the CFT of a film to be formed is great. A method for producing a polytetrafluoroethylene aqueous dispersion includes: step A1 for polymerizing a non-fluorine-based monomer in an aqueous medium to obtain a solution 1 containing a polymer containing a unit based on a non-fluorine-based monomer; step A2 for polymerizing tetrafluoroethylene in the solution 1 without substantially adding a surfactant to the solution 1 to obtain an aqueous emulsion containing polytetrafluoroethylene particles, and step A3 for adding a nonionic surfactant to the aqueous emulsion and then concentrating the aqueous emulsion to obtain a polytetrafluoroethylene aqueous dispersion, wherein the amount of the non-fluorine-based monomer used is at most 200 mass ppm with respect to the amount of tetrafluoroethylene supplied to a polymerization system.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an aqueous polytetrafluoroethylene dispersion. [Background technology]

[0002] Polytetrafluoroethylene is used in a variety of applications due to its excellent properties. Conventionally, fluorosurfactants such as perfluorooctanoates have been used in the production of polytetrafluoroethylene, but from an environmental perspective, it has been desired to refrain from using fluorosurfactants. In view of this, a method has been proposed as a new method for producing polytetrafluoroethylene, in which a hydrocarbon-containing surfactant is used when polymerizing tetrafluoroethylene (Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Special Publication No. 2016-537499 Summary of the Invention [Problem to be solved by the invention]

[0004] On the other hand, when a hydrocarbon-containing surfactant is used, a chain transfer reaction occurs with the hydrocarbon-containing surfactant during polymerization of tetrafluoroethylene. Therefore, in the method using this hydrocarbon-containing surfactant, the presence of fluorine-based oligomers (especially fluorine-based oligomers having hydrophilic functional groups) with various chain length distributions, which has never been confirmed in the conventional method using a fluorine-based surfactant, was confirmed in the product. As described above, such fluorine-based oligomers are by-products generated by the hydrocarbon-containing surfactant being the starting point of chain transfer. The presence of such by-products is undesirable from an environmental perspective.

[0005] Furthermore, for aqueous dispersions containing polytetrafluoroethylene particles, it is desirable that the coating film formed has a large critical film thickness (hereinafter, also referred to as CFT). The CFT corresponds to the thickness at which cracks start to occur when an aqueous dispersion containing polytetrafluoroethylene particles is applied to form a coating film having a certain thickness or more and then baked.

[0006] An object of the present invention is to provide a method for producing an aqueous polytetrafluoroethylene dispersion which produces less fluorine-based oligomer by-products and forms a coating film with a large CFT. [Means for solving the problem]

[0007] As a result of intensive research, the present inventors have found that the above problems can be solved by the following configuration.

[0008] (1) Step A1 of polymerizing a non-fluorinated monomer in an aqueous medium to obtain a solution 1 containing a polymer containing units based on the non-fluorinated monomer; A step A2 of polymerizing tetrafluoroethylene in solution 1 without adding a surfactant to solution 1 to obtain an aqueous emulsion containing polytetrafluoroethylene particles; A step A3 of adding a nonionic surfactant to the aqueous emulsion and then concentrating the aqueous emulsion to obtain an aqueous polytetrafluoroethylene dispersion, A method for producing an aqueous polytetrafluoroethylene dispersion, wherein the amount of a non-fluorinated monomer used is 200 ppm by mass or less relative to the amount of tetrafluoroethylene supplied to a polymerization system. (2) The method for producing an aqueous polytetrafluoroethylene dispersion according to (1), wherein the non-fluorinated monomer is a monomer represented by the formula (1) described below. (3) The method for producing an aqueous polytetrafluoroethylene dispersion according to (1) or (2), wherein the content of polytetrafluoroethylene particles in the aqueous polytetrafluoroethylene dispersion is 50 to 70 mass % based on the total amount of the aqueous polytetrafluoroethylene dispersion. (4) The method for producing an aqueous polytetrafluoroethylene dispersion according to any one of (1) to (3), wherein the content of the nonionic surfactant in the aqueous polytetrafluoroethylene dispersion is 1 to 20 mass % based on the mass of polytetrafluoroethylene. (5) A step B1 of mixing at least one nucleating additive selected from the group consisting of polyalkylene oxide compounds and hydrocarbon-containing surfactants with an oxidizing agent in an aqueous medium to obtain a solution 2; A step B2 of polymerizing tetrafluoroethylene in solution 2 without adding a surfactant to solution 2 to obtain an aqueous emulsion containing polytetrafluoroethylene particles; and a step B3 of adding a nonionic surfactant to the aqueous emulsion and then concentrating the aqueous emulsion to obtain an aqueous polytetrafluoroethylene dispersion, A method for producing an aqueous polytetrafluoroethylene dispersion, wherein the amount of a nucleation additive used is 100 ppm by mass or less relative to the amount of tetrafluoroethylene supplied to a polymerization system. (6) The method for producing an aqueous polytetrafluoroethylene dispersion according to (5), wherein the content of polytetrafluoroethylene particles in the aqueous polytetrafluoroethylene dispersion is 50 to 70 mass % based on the total amount of the aqueous polytetrafluoroethylene dispersion. (7) The method for producing an aqueous polytetrafluoroethylene dispersion according to (5) or (6), wherein the nucleation additive is a polyalkylene oxide compound. (8) The method for producing an aqueous polytetrafluoroethylene dispersion according to any one of (5) to (7), wherein the amount of the oxidizing agent used is 0.5 to 100 ppm by mass based on the total mass of the aqueous medium. (9) The method for producing an aqueous polytetrafluoroethylene dispersion according to any one of (5) to (8), wherein the content of the nonionic surfactant in the aqueous polytetrafluoroethylene dispersion is 1 to 20 mass % based on the mass of polytetrafluoroethylene. Effect of the Invention

[0009] According to the present invention, there can be provided a method for producing an aqueous polytetrafluoroethylene dispersion in which the production of fluorine-based oligomer by-products is reduced and the CFT of the formed coating film is large. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The terms used in the present invention have the following meanings. The term "unit" refers to a general term for an atomic group derived from one monomer molecule, which is formed directly by polymerization of a monomer. A numerical range expressed using "~" means that the range includes the numerical values ​​before and after "~" as the lower and upper limits.

[0011] The characteristic features of the method for producing an aqueous polytetrafluoroethylene (hereinafter also referred to as "PTFE") dispersion of the present invention include using solution 1 containing a polymer containing units based on a non-fluorinated monomer (hereinafter also referred to as a "specific polymer") and an aqueous medium, or using solution 2 obtained by mixing at least one nucleation additive selected from the group consisting of polyalkylene oxide compounds and hydrocarbon-containing surfactants with an oxidizing agent in an aqueous medium, not using a surfactant substantially when polymerizing tetrafluoroethylene (hereinafter also referred to as "TFE"), and adjusting the amounts of non-fluorinated monomer and nucleation additive used. Solution 1 and Solution 2 provide a hydrophobic environment in which TFE polymerization can proceed well, and furthermore, by substantially not using a surfactant, TFE polymerization can proceed stably while suppressing the occurrence of chain transfer. As a result, the generation of fluorine-based oligomers as by-products can be suppressed. In addition, it has been found that the CFT of the coating film formed can be increased by adjusting the amount of non-fluorine-based monomer and nucleation additive used. The fluorine-based oligomer mainly includes oligomers having about 6 to 34 carbon atoms and formed by linking CF2.

[0012] <<First embodiment>> A first embodiment of the method for producing an aqueous PTFE dispersion includes an embodiment having the following three steps. Step A1: A step of polymerizing a non-fluorinated monomer in an aqueous medium to obtain a solution 1 containing a specific polymer. Step A2: A step of polymerizing TFE in solution 1 without substantially adding a surfactant to solution 1 to obtain an aqueous emulsion containing PTFE particles. Step A3: A step of adding a nonionic surfactant to the aqueous emulsion and then concentrating the aqueous emulsion to obtain a PTFE aqueous dispersion. In the first embodiment, the amount of the non-fluorinated monomer used is 200 mass ppm or less relative to the amount of TFE supplied to the polymerization system. The present invention will now be described in detail with reference to the above preferred embodiment.

[0013] <Process A1> Step A1 is a step of polymerizing a non-fluorinated monomer in an aqueous medium to obtain a solution 1 containing a specific polymer. In the following, first, the materials used in step A1 will be described in detail, and then the procedure of step A1 will be described in detail.

[0014] (Non-fluorinated monomer) The non-fluorine-based monomer is a monomer that does not contain a fluorine atom. The non-fluorine-based monomer usually has a polymerizable group, and the number of the polymerizable groups is preferably 1 to 3, and more preferably 1. The polymerizable group is preferably an ethylenically unsaturated group, more specifically, an acryloyl group, a methacryloyl group, a vinyl ether group, a vinyl ester group, a vinyl group, or an allyl group, and an acryloyl group, a methacryloyl group, a vinyl ester group, or a vinyl ether group is preferred.

[0015] The non-fluorinated monomer is preferably a monomer represented by formula (1). Formula (1) CH2=CR 11 -L 1 -R 12 R 11 represents a hydrogen atom or an alkyl group. The alkyl group preferably has 1 to 3 carbon atoms, and more preferably 1 carbon atom. L 1represents a single bond, -CO-O-*, -O-CO-* or -O-. * represents R 12 For example, L 1 is -CO-O-*, formula (1) is CH2=CR 11 -CO-OR 12 Represents. R 12 represents a hydrogen atom, an alkyl group, an alkenyl group, or a nitrile group. 1 If is a single bond, R 12 is a nitrile group. The alkyl group and the alkenyl group preferably have 1 to 10 carbon atoms, more preferably have 1 to 6 carbon atoms, and further preferably have 1 to 4 carbon atoms. The alkyl group may be linear or cyclic. When the alkyl group is cyclic, it corresponds to a cycloalkyl group. The alkenyl group may be linear or cyclic.

[0016] The monomer represented by formula (1) is preferably a monomer selected from the group consisting of a monomer represented by formula (1-1), a monomer represented by formula (1-2), a monomer represented by formula (1-3), and a monomer represented by formula (1-4). Formula (1-1) CH2=CR 11 -CO-OR 13 Formula (1-2) CH2=CR 11 -O-CO-R 14 Formula (1-3) CH2=CR 11 -OR 15 Formula (1-4) CH2=CR 11 -R 16 R 11 The definition is as described above. R 13 represents a hydrogen atom, an alkyl group, or an alkenyl group, and is preferably an alkyl group having 1 to 6 carbon atoms or an alkenyl group having 1 to 6 carbon atoms. R 14 represents an alkyl group, preferably an alkyl group having 1 to 3 carbon atoms, and more preferably a methyl group. R15 represents an alkyl group, preferably a linear alkyl group or a cyclic alkyl group. R 16 represents a nitrile group.

[0017] Examples of non-fluorine-based monomers include methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, butyl acrylate, butyl methacrylate, hexyl methacrylate, cyclohexyl methacrylate, vinyl methacrylate, vinyl acetate, acrylic acid, methacrylic acid, acrylonitrile, methacrylonitrile, ethyl vinyl ether, and cyclohexyl vinyl ether. The non-fluorine-based monomers may be used alone or in combination of two or more kinds. As the non-fluorine-based monomer, a monomer represented by formula (1-1) or a monomer represented by formula (1-2) is preferable, and R 13 More preferred is a monomer represented by formula (1-1) in which R is an alkyl group. The monomer represented by formula (1-1) and the monomer represented by formula (1-2) have an ester group or a carboxy group, which are hydrophilic groups, and therefore the monomer and its polymer have hydrophilicity. Therefore, it is considered that the monomer and its polymer can be stably dispersed in an aqueous medium without requiring a surfactant, particularly at low concentrations.

[0018] (Specific polymer) The specific polymer is a polymer containing units based on a non-fluorine-based monomer. The specific polymer usually contains only units based on non-fluorine-based monomers, but may contain units based on fluorine-based monomers within a range that does not impair the effects of the present invention. That is, in addition to non-fluorine-based monomers, fluorine-based monomers may be used in step A1. The fluorine-based monomer is a monomer having a fluorine atom, and an example of the fluorine-based monomer is TFE. The content of units based on a non-fluorinated monomer in the specific polymer is preferably 90% by mass or more, more preferably 95% by mass or more, relative to all units in the specific polymer, and the upper limit is 100% by mass.

[0019] (aqueous medium) Examples of the aqueous medium include water and a mixture of water and a water-soluble organic solvent. Examples of the water-soluble organic solvent include tert-butanol, propylene glycol, and dipropylene glycol. In the case of a mixture of water and a water-soluble organic solvent, the concentration of the water-soluble organic solvent is preferably 10% by mass or less. The aqueous medium is preferably water alone.

[0020] (Polymerization initiator) In step A1, a polymerization initiator may be used. That is, a polymerization initiator may be used when polymerizing the non-fluorine-based monomer. As the polymerization initiator, a water-soluble radical initiator or a water-soluble oxidation-reduction catalyst is preferable. As the water-soluble radical initiator, preferred are persulfates such as ammonium persulfate and potassium persulfate, water-soluble organic peroxides such as disuccinic acid peroxide, bisglutaric acid peroxide, and tert-butyl hydroperoxide. As the water-soluble oxidation-reduction catalyst, a combination of an oxidizing agent such as bromic acid or a salt thereof, chloric acid or a salt thereof, persulfuric acid or a salt thereof, permanganic acid or a salt thereof, hydrogen peroxide, etc., and a reducing agent such as sulfurous acid or a salt thereof, hydrogen sulfite or a salt thereof, thiosulfuric acid or a salt thereof, organic acid, etc. is preferred. Among these, a combination of bromic acid or a salt thereof and sulfurous acid or a salt thereof (e.g., ammonium sulfite), and a combination of permanganic acid or a salt thereof (e.g., potassium permanganate) and oxalic acid are more preferred. As the polymerization initiator, ammonium persulfate alone or a mixture of a persulfate and disuccinic acid peroxide is preferred, and ammonium persulfate alone or a mixture of ammonium persulfate and disuccinic acid peroxide is more preferred. The polymerization initiator may be used alone or in combination of two or more kinds. As for the method of charging the polymerization initiator, the entire amount may be charged into the polymerization system before the start of the polymerization reaction, or the initiator may be added to the polymerization system continuously or intermittently.

[0021] (Step A1) In step A1, a non-fluorine-based monomer is polymerized in an aqueous medium. Specifically, it is preferable to mix a non-fluorine-based monomer with an aqueous medium and polymerize the non-fluorine-based monomer in the resulting mixed liquid. As described above, a fluorine-based monomer may be used in combination, if necessary.

[0022] The amount of the non-fluorinated monomer used is 200 ppm by mass or less, preferably 1 to 150 ppm by mass or less, more preferably 5 to 100 ppm by mass, and further preferably 5 to 50 ppm by mass, relative to the amount of TFE supplied to the polymerization system (amount of TFE used) used in step A2 described later. As a method for feeding the non-fluorinated monomer, it is preferable to initially add it all at once, that is, to feed the entire amount of the non-fluorinated monomer into the polymerization system before starting the polymerization reaction.

[0023] The content of the non-fluorinated monomer in the dispersion obtained by mixing the non-fluorinated monomer with the aqueous medium is preferably from 0.000015 to 0.0030 mass %, more preferably from 0.000075 to 0.0023 mass %, based on the total mass of the dispersion. Since the entire amount of the non-fluorinated monomer is usually polymerized to form the specific polymer, the concentration of the specific polymer in the obtained solution 1 falls within the above-mentioned numerical range. The non-fluorinated monomer concentration and the specific polymer concentration are concentrations when the obtained solution 1 is used in step A2 without diluting it with an aqueous medium. When the obtained solution 1 is diluted with an aqueous medium to have the above specific polymer concentration and the diluted solution is used in step A2, a high-concentration solution is produced in step A1 according to the dilution ratio. The dilution ratio is not particularly limited, but is preferably 10 times or less.

[0024] The amount of the polymerization initiator used is preferably from 0.2 to 1000% by mass, more preferably from 0.2 to 500% by mass, based on the total amount of the non-fluorinated monomers.

[0025] The amount of the polymerization initiator used is preferably from 0.1 to 1000 mol %, more preferably from 0.1 to 300 mol %, based on the total amount of non-fluorinated monomers.

[0026] The polymerization temperature of the non-fluorinated monomer is preferably from 10 to 95° C., more preferably from 50 to 90° C. The polymerization time is preferably from 5 to 400 minutes, more preferably from 5 to 300 minutes, and further preferably from 5 to 200 minutes. The pressure conditions during polymerization are preferably reduced pressure conditions or normal pressure conditions, and among these, 0 to 2.0 MPa is preferred, 0 to 1.0 MPa is more preferred, and 0 to 0.5 MPa is even more preferred. Alternatively, the polymerization may be carried out in a TFE atmosphere. Note that the polymerization of the non-fluorinated monomer in an aqueous medium usually proceeds preferentially over the polymerization of TFE.

[0027] By the above step A1, a solution 1 containing a specific polymer is obtained. The specific polymer may be dissolved in solution 1, or may be dispersed in the aqueous medium in the form of particles. During polymerization of TFE in step A2 described below, the specific polymer is not an emulsifier, but it is presumed that the specific polymer exists at the boundary between the aqueous medium and the PTFE particles due to the balance of interfacial tension between the two, thereby contributing to the stabilization of the dispersion of the PTFE particles in the aqueous medium. The particle size of the specific polymer particles is preferably from 0.1 to 100 nm, more preferably from 0.1 to 50 nm.

[0028] Incidentally, the solution 1 obtained in the step A1 may contain unreacted non-fluorinated monomers. In addition, the atmosphere in the polymerization system in the step A1 may be a TFE-containing atmosphere in consideration of the step A2. In such a case, it is considered that a part of the specific polymer in the step A2 may become a polymer containing TFE units. From another point of view, the PTFE particles obtained in step A2 are not limited to particles consisting of a physical mixture of a specific polymer and PTFE, but may be particles containing a TFE copolymer having units based on a non-fluorinated monomer.

[0029] <Process A2> Step A2 is a step of polymerizing TFE in solution 1 obtained in step A1 without substantially adding a surfactant to solution 1 to obtain an aqueous emulsion containing PTFE particles. In the following, first, the materials used in step A2 will be described in detail, and then the procedure of step A2 will be described in detail.

[0030] (TFE) In step A2, TFE is used.

[0031] (Other Monomers) In step A2, a monomer other than TFE may be further used within the range that does not impair the effects of the present invention. The other monomers include monomers having a polar group (hereinafter, simply referred to as "specific monomers"). The polar group in the specific monomer exhibits an interaction with the aqueous medium, and is presumed to be located between TFE and the aqueous medium during the polymerization of TFE, and to exhibit a surfactant-like function. As a result, the polymerization of TFE proceeds well, and the occurrence of chain transfer is also suppressed.

[0032] Examples of the polar group contained in the specific monomer include a sulfonic acid group, a sulfonate group, a carboxylic acid group, a carboxylate group, a phosphonic acid group, and a phosphonate group. Among them, the group represented by formula (A) or the group represented by formula (B) is preferred, and the group represented by formula (A) is more preferred, in terms of further suppressing the generation of fluorine-based oligomers. Formula (A) -SO3M Formula (B) -COOM In formula (A) and formula (B), M represents a hydrogen atom, NH4, or an alkali metal atom. Examples of the alkali metal atom include a lithium atom, a sodium atom, and a potassium atom.

[0033] The specific monomer usually has a polymerizable group, and the number of the polymerizable groups is preferably 1 to 3, and more preferably 1. The polymerizable group is preferably an ethylenically unsaturated group, more specifically, an acryloyl group, a methacryloyl group, a vinyl ether group, a vinyl ester group, a vinyl group, or an allyl group, and an acryloyl group, a methacryloyl group, a vinyl ester group, or a vinyl ether group is preferred.

[0034] The specific monomer is preferably a monomer represented by formula (3) in that the production of fluorine-based oligomers is further suppressed. Formula (3) CR 31 R 32 =CR 33 -L 3 -R 34 In formula (3), R 31 and R 32 each independently represents a hydrogen atom or a fluorine atom.

[0035] R 33 represents a hydrogen atom, a fluorine atom, or an alkyl group which may be substituted with a fluorine atom. Among these, a hydrogen atom or a fluorine atom is preferred in that it has better copolymerizability with TFE. The term "alkyl group which may be substituted with a fluorine atom" refers to an alkyl group in which at least one hydrogen atom may be substituted with a fluorine atom. The alkyl group which may be substituted with a fluorine atom preferably has 1 to 3 carbon atoms, and more preferably 1 carbon atom.

[0036] L 3 represents a single bond or a divalent linking group. Among these, a single bond is preferred in that it has better copolymerizability with TFE. Examples of the divalent linking group include a divalent hydrocarbon group (which may be a divalent saturated hydrocarbon group, a divalent aromatic hydrocarbon group, an alkenylene group, or an alkynylene group. The divalent saturated hydrocarbon group may be linear, branched, or cyclic, and an example of the group is an alkylene group. The number of carbon atoms is preferably 1 to 20. The divalent aromatic hydrocarbon group preferably has a carbon number of 5 to 20, and an example of the group is a phenylene group. Alternatively, the group may be an alkenylene group having a carbon number of 2 to 20, or an alkynylene group having a carbon number of 2 to 20), a divalent heterocyclic group, -O-, -S-, -SO2-, -C(O)-, -Si(R a )2-, -N(R b )-, and combinations of two or more of these. a R represents an alkyl group (preferably having 1 to 10 carbon atoms) or a phenyl group. b represents a hydrogen atom or an alkyl group (preferably having 1 to 10 carbon atoms). Examples of groups that combine two or more of the above groups include -OC(O)-, -C(O)N(R b )-, alkylene group-O-alkylene group, alkylene group-OC(O)-alkylene group, alkylene group-Si(R a )2-phenylene group -Si(R a )2 are examples. The divalent hydrocarbon group may have a substituent. Examples of the substituent include a halogen atom (e.g., a fluorine atom, a chlorine atom). In other words, the hydrogen atom in the divalent hydrocarbon group may be substituted with a halogen atom.

[0037] R 34 represents a group represented by the above formula (A) or a group represented by the above formula (B).

[0038] The monomer represented by formula (3) is preferably a monomer selected from the group consisting of a monomer represented by formula (3-1), a monomer represented by formula (3-2), a monomer represented by formula (3-3), a monomer represented by formula (3-4), a monomer represented by formula (3-5), and a monomer represented by formula (3-6), and is more preferably a monomer represented by formula (3-1). Formula (3-1) CR 31 R 32 =CR 33 -R 34 Formula (3-2) CR 31 R 32 =CR 33 -(CF2) m1 -R 34 Formula (3-3) CR 31 R 32 =CR 33 -(CF2C(CF3)F) m2 -R 34 Formula (3-4) CR 31 R 32 =CR 33 -O-(CFR 35 ) m3 -R 34 Formula (3-5) CR 31 R 32 =CR 33 -O-(CF2CFR 35 O) m4 -CF2CF2-R 34 Formula (3-6) CR 31 R 32 =CR 33 -CF2-O-(CF(CF3)CF2O) m5 -CF(CF3)-R 34

[0039] In formulas (3-1) to (3-6), R 31 ~R 34 The definition is as described above. In formula (3-2), m1 represents an integer of 1 to 10. In formula (3-3), m2 represents an integer of 1 to 5. In formula (3-4), m3 represents an integer of 1 to 10. 35 represents a fluorine atom or CF3. In formula (3-5), m4 represents an integer of 1 to 10. 35 The definition is as described above. In formula (3-6), m5 represents 0 or an integer of 1 to 10.

[0040] A specific example of the specific monomer is ammonium vinyl sulfonate. The specific monomer may be used alone or in combination of two or more kinds.

[0041] (Polymerization initiator) In step A2, a polymerization initiator may be used. That is, a polymerization initiator may be used during polymerization of TFE. The polymerization initiator used may be the polymerization initiator described in step A1. As the polymerization initiator, a mixture of a persulfate and disuccinic acid peroxide is preferred, and a mixture of ammonium persulfate and disuccinic acid peroxide is more preferred. The amount of the polymerization initiator used is preferably 0.10% by mass or more, more preferably 0.10 to 1.5% by mass, and even more preferably 0.20 to 1.0% by mass, based on the total amount of TFE supplied to the polymerization system.

[0042] (Stabilizing agent) In step A2, a stabilizing agent may be used. As the stabilizing aid, paraffin wax, fluorine-based solvent, and silicone oil are preferable, and paraffin wax is more preferable. Paraffin wax may be liquid, semi-solid, or solid at room temperature. Among them, saturated hydrocarbons having 12 or more carbon atoms are preferable. The melting point of paraffin wax is preferably 40 to 65°C, and more preferably 50 to 65°C. The stabilizing aids may be used alone or in combination of two or more.

[0043] (others) In step A2, a monomer other than TFE and the specific monomer may be used within a range that does not impair the effects of the present invention. In view of the superiority of various properties of PTFE, however, the amount of TFE used is preferably 99.5 mass% or more, and more preferably 99.8 mass% or more, based on the total amount of the monomers used in step A2.

[0044] (Step A2) In step A2, substantially no surfactant is added to solution 1. That is, in step A2, polymerization of TFE is carried out in solution 1 without substantially adding a new surfactant to solution 1. A surfactant is a compound having a hydrophilic group (e.g., a polar group) and a hydrophobic group (e.g., a hydrocarbon group). The definition of the polar group is the same as the definition of the polar group contained in the specific monomer. The surfactant may be a known surfactant, such as a nonionic surfactant or an ionic surfactant, and more specifically, may be a hydrocarbon-containing surfactant or a fluorine-containing surfactant. The definition of the hydrocarbon-containing surfactant is as described below. In step A2, it is preferable that at least one selected from the group consisting of a hydrocarbon-containing surfactant and a fluorine-containing surfactant is not substantially added to solution 1. The above-mentioned "substantially not added" means that no surfactant is added, or even if a surfactant is added, the amount of the surfactant added is 200 mass ppm or less with respect to the total mass of solution 1. There is no particular lower limit, but 0 mass ppm is preferable. In other words, it is preferable not to add a surfactant to solution 1 in step A2.

[0045] TFE is added to the polymerization system (i.e., polymerization reaction vessel) by a conventional method. For example, TFE is added to the polymerization system continuously or intermittently so that the polymerization pressure becomes a predetermined pressure. When a polymerization initiator is used, the polymerization initiator may be added to the polymerization system all at once or in portions.

[0046] When the specific monomer is used, the amount of the specific monomer used relative to the total amount of TFE is preferably 0.150% by mass or less, that is, the amount of the specific monomer charged relative to the total amount of TFE charged is preferably 0.150% by mass or less. From the viewpoint of the stability of the emulsion during polymerization, the amount of the specific monomer used relative to the total amount of TFE is preferably 0.100% by mass or less, more preferably 0.090% by mass or less, and from the viewpoint of improving the molecular weight, the amount of the specific monomer used relative to the total amount of TFE is preferably 0.005% by mass or more, more preferably 0.010% by mass or more. When two or more types of specific monomers are used, the total amount of the specific monomers used may be within the above range.

[0047] When the specific monomer is used, the amount of the specific monomer used relative to the total amount of TFE is preferably 0.150 mol % or less. In other words, the amount of the specific monomer charged relative to the total amount of TFE charged is preferably 0.150 mol % or less. From the viewpoint of the stability of the emulsion during polymerization, the amount of the specific monomer used relative to the total amount of TFE is preferably 0.100 mol% or less, more preferably 0.090 mol% or less. Also, from the viewpoint of improving the molecular weight, the amount of the specific monomer used relative to the total amount of TFE is preferably 0.001 mol% or more, more preferably 0.005 mol% or more. When two or more types of specific monomers are used, the total amount of the specific monomers used may be within the above range.

[0048] The polymerization temperature is preferably 10 to 95° C., and more preferably 15 to 90° C. The polymerization pressure is preferably 0.5 to 4.0 MPa, and more preferably 0.6 to 3.5 MPa. The polymerization time is preferably 50 to 520 minutes, and more preferably 50 to 450 minutes, and even more preferably 50 to 300 minutes.

[0049] Incidentally, step A1 and step A2 may be carried out consecutively in the same polymerization reaction vessel. In the production method of the present invention, it is sufficient that the specific polymer is formed in step A1, and step A2 may be carried out before the non-fluorinated monomer is completely consumed in step A1.

[0050] By the above procedure, an aqueous emulsion in which PTFE is dispersed in particulate form (aqueous emulsion containing PTFE particles) is obtained. The concentration of the PTFE particles in the aqueous emulsion is preferably 10 to 45% by mass, more preferably 10 to 30% by mass, and even more preferably 10 to 25% by mass, based on the total amount of the aqueous emulsion. Within the above range, the PTFE particles in the aqueous emulsion can be more easily coagulated, and the clouding of the coagulated liquid can be suppressed. The average primary particle size of the PTFE particles is preferably from 100 to 500 nm, more preferably from 150 to 300 nm. The average primary particle size of the PTFE particles corresponds to D50 measured by a laser scattering particle size distribution analyzer.

[0051] The PTFE in the PTFE particles obtained by the above procedure usually contains TFE units as the main component. The main component means that the content of TFE units is 99.700 mass% or more, preferably 99.900 mass% or more, based on the total units of PTFE. The upper limit is 100 mass%. When PTFE contains units based on a specific monomer, the content of the units based on the specific monomer is preferably 0.005 to 0.150 mass %, more preferably 0.010 to 0.100 mass %, based on the total units of PTFE. When two or more specific monomers are used, the total content of the units based on the specific monomers may be within the above range. When PTFE contains units based on a non-fluorine-based monomer, the content of the units based on the non-fluorine-based monomer is preferably 200 ppm by mass or less, more preferably 1 to 150 ppm by mass, further preferably 5 to 100 ppm by mass, and particularly preferably 5 to 50 ppm by mass, based on all units of PTFE. When two or more kinds of non-fluorine-based monomers are used, the total content of the units based on the respective non-fluorine-based monomers may be within the above range.

[0052] <Process A3> Step A3 is a step of adding a nonionic surfactant to the aqueous emulsion obtained in step A2, and then concentrating the aqueous emulsion to obtain a PTFE aqueous dispersion. That is, it is a step of adding a nonionic surfactant to the low-concentration aqueous PTFE dispersion obtained in step A2 (corresponding to the above aqueous emulsion), and then concentrating the low-concentration aqueous PTFE dispersion to obtain a high-concentration aqueous PTFE dispersion (corresponding to the above aqueous PTFE dispersion). By carrying out step A3, an aqueous PTFE dispersion showing a PTFE particle concentration higher than the PTFE particle concentration of the aqueous dispersion is obtained. In the following, first, the materials used in step A3 will be described in detail, and then the procedure of step A3 will be described in detail.

[0053] (Nonionic surfactant) The nonionic surfactant includes a nonionic surfactant. As the nonionic surfactant, a nonionic surfactant represented by formula (4) or a nonionic surfactant represented by formula (5) is preferred. Formula (4):R 41 -OAH Formula (5):R 51 -C6H4-OBH In the formula, R 41 represents an alkyl group having 8 to 18 carbon atoms. A represents a polyoxyalkylene chain composed of 5 to 20 oxyethylene groups and 0 to 2 oxypropylene groups. In the formula, R 51 represents an alkyl group having 4 to 12 carbon atoms. B represents a polyoxyethylene chain composed of 5 to 20 oxyethylene groups. As the nonionic surfactant, a nonionic surfactant represented by formula (6) is also preferred. Formula (6):R 61 -ODH In the formula, R 61 represents an alkyl group having 8 to 18 carbon atoms. D represents a polyoxyalkylene chain composed of 5 to 20 oxyethylene groups and 0.1 to 3 oxybutylene groups.

[0054] In formula (4), R41 The number of carbon atoms in the alkyl group represented by the formula (I) is 8 to 18, preferably 10 to 16, and more preferably 12 to 16. When the number of carbon atoms is 18 or less, the PTFE particles are less likely to settle even when the PTFE aqueous dispersion is left to stand for a long period of time, and the storage stability is excellent. When the number of carbon atoms is 8 or more, the surface tension of the PTFE aqueous dispersion is low, and the permeability and wettability are excellent. In formula (4), the hydrophilic group A is preferably a polyoxyalkylene chain having an oxyethylene group number of 7 to 12 and an oxypropylene group number of 0 to 2. In particular, when the number of oxypropylene groups in A is 0.5 to 1.5, good defoaming properties are obtained, which is preferred.

[0055] In formula (5), R 51 The number of carbon atoms in the alkyl group represented by the formula (I) is 4 to 12, preferably 6 to 10, and more preferably 8 to 9. When the number of carbon atoms in the alkyl group is 4 or more, the surface tension of the PTFE aqueous dispersion is low, and the permeability and wettability are excellent. When the number of carbon atoms is 12 or less, the PTFE particles are unlikely to settle even if the PTFE aqueous dispersion is left to stand for a long period of time, and the storage stability is excellent. In the formula (5), the number of oxyethylene groups in the hydrophilic group B is preferably 6 to 16, and more preferably 7 to 12.

[0056] In formula (6), R 61 The number of carbon atoms in the alkyl group represented by the formula (I) is 8 to 18, preferably 10 to 16, and more preferably 12 to 16. When the number of carbon atoms is 18 or less, the PTFE particles are less likely to settle even when the PTFE aqueous dispersion is left to stand for a long period of time, and the storage stability is excellent. When the number of carbon atoms is 8 or more, the surface tension of the PTFE aqueous dispersion is low, and the permeability and wettability are excellent. In formula (6), the hydrophilic group D is preferably a polyoxyalkylene chain having 7 to 12 oxyethylene groups and 0.1 to 3 oxybutylene groups. In particular, when the number of oxybutylene groups in D is 0.5 to 2, good defoaming properties are obtained, which is preferable. Furthermore, the number of oxybutylene groups is more preferably 0.7 to 1.7, and even more preferably 0.9 to 1.5. The number of oxyethylene groups is preferably 6 to 15, and more preferably 7 to 12.

[0057] The average molecular weight of the nonionic surfactant represented by formula (4), the average molecular weight of the nonionic surfactant represented by formula (5), and the average molecular weight of the nonionic surfactant represented by formula (6) are each preferably 450 to 800, more preferably 500 to 750, and even more preferably 550 to 700.

[0058] Examples of the nonionic surfactant represented by formula (4) include 13 H 27 -(OC2H4) 10 -OH, C 12 H 25 -(OC2H4) 10 -OH, C 10 H 21 CH(CH3)CH2-(OC2H4)9-OH, C 13 H 27 -(OC2H4)9-OCH(CH3)CH2-OH, C 16 H 33 -(OC2H4) 10 -OH, HC(CH 11 )(C7H 15 )-(OC2H4)9-OH. Commercially available products include Tergitol (registered trademark) 15S series manufactured by Dow and Lionol (registered trademark) TD series manufactured by Lion Corporation. The nonionic surfactant represented by formula (5) is, for example, CH 17 -C6H4-(OC2H4) 10 -OH, CH 19 -C6H4-(OC2H4) 10 Commercially available products include Triton (registered trademark) X series manufactured by Dow and Nikkol (registered trademark) OP series and NP series manufactured by Nikko Chemical Co., Ltd. Examples of the nonionic surfactant represented by formula (6) include C 13 H 27 OCH2CH(C2H5)O(C2H4O)8H,C 10 H 21 CH(CH3)CH2OCH2CH(C2H5)O(C2H4O)8H,C 12 H 25OCH2CH(C2H5)O(C2H4O)8H, C8H 17 OCH2CH(C2H5)O(C2H4O) 10 H, C 13 H 27 OCH2CH2OCH2CH(C2H5)O(C2H4O)8H,C 10 H 21 CH(CH3)CH2O(C2H4O)9CH2CH(C2H5)OH,C 16 H 33 OC2H4OCH(C2H5)CH2O(C2H4O)9H,C 12 H 25 OCH2CH(C2H5)O(C2H4O)8CH2CH(C2H5)OH,C 13 H 27 OCH(CH3)CH(CH3)O(C2H4O)8H,C 12 H 25 OCH(CH3)CH(CH3)O(C2H4O)8H,C 13 H 27 O(CH2)4O(C2H4O)8H,C 12 H 25 O(CH2)2CH(CH3)O(C2H4O)8H.

[0059] The nonionic surfactant represented by formula (4) and / or the nonionic surfactant represented by formula (5) may be used alone or in combination of two or more kinds. The nonionic surfactant represented by formula (6) may be used alone or in combination of two or more kinds. Furthermore, the nonionic surfactant represented by formula (6) can be used in combination with a nonionic surfactant represented by formula (4) or a nonionic surfactant represented by formula (5). In addition, a nonionic surfactant is a mixture of multiple substances with different molecular structures, and the number of carbon atoms in the alkyl group in the nonionic surfactant, and the number of oxyethylene groups, oxypropylene groups, and oxybutylene groups in the polyoxyalkylene chain are treated as average values. Each value is not limited to an integer.

[0060] (Step A3) The method for concentrating the aqueous emulsion is not particularly limited, and any conventionally known method can be used. Examples of the concentrating method include centrifugal sedimentation, electrophoresis, and phase separation, as described on page 32 of Fluorine Resin Handbook (edited by Satokawa Takaomi, published by Nikkan Kogyo Shimbun, Ltd.).

[0061] The electrophoresis method is a method that utilizes the fact that PTFE particles are negatively charged. Specifically, a nonionic surfactant is dissolved in an aqueous emulsion in an amount of 1 to 10% by mass (preferably 2 to 8% by mass) relative to the mass of PTFE. Next, a voltage of 50 to 500 V / m (preferably 100 to 300 V / m) is applied to the obtained aqueous emulsion in a container having a semipermeable membrane such as a cellulose membrane, the PTFE particles are electrophoresed, and the PTFE aqueous dispersion that accumulates on the surface of the semipermeable membrane and then settles to the bottom due to the difference in specific gravity is collected. The pH of the aqueous emulsion before concentration is preferably 2 to 10, more preferably 3 to 9.

[0062] The phase separation method is a method in which PTFE particles are precipitated by heating and leaving for a certain period of time. Specifically, 8 to 20% by mass (preferably 12 to 18% by mass) of a nonionic surfactant is dissolved in an aqueous emulsion relative to the mass of PTFE. Next, the resulting aqueous emulsion is heated at 50 to 100°C (preferably 60 to 90°C) and left for 1 to 100 hours (preferably 5 to 20 hours), and the PTFE aqueous dispersion that has accumulated at the bottom due to the difference in specific gravity is collected.

[0063] In addition, during concentration, an anionic surfactant (e.g., ammonium laurate, triethanolamine laurate, sodium lauryl sulfate, ammonium lauryl sulfate, triethanolamine lauryl sulfate, etc.) may be added to the aqueous PTFE emulsion in an amount of 0.20 mass% or less based on the mass of PTFE to speed up the concentration. These additives not only speed up the concentration of the aqueous PTFE emulsion, but also have the effect of improving the viscosity and dispersion stability.

[0064] After adding the nonionic surfactant to the aqueous emulsion obtained in step A2, the polymerization initiator residue and the like may be adsorbed and removed with an ion exchange resin or the like before concentrating the aqueous emulsion. This removes the excess water-soluble ionic compounds, improves the coating performance of the PTFE aqueous dispersion, and makes it easier to apply it to insulating materials.

[0065] The concentration of PTFE particles in the PTFE aqueous dispersion obtained by the above procedure is preferably 15 to 70 mass %, more preferably 20 to 70 mass %, based on the total mass of the PTFE aqueous dispersion. The PTFE aqueous dispersion having a PTFE particle concentration of 15 to 70 mass % can be preferably used for impregnating a cloth or string made of woven fibers such as glass fiber with the PTFE aqueous dispersion, mixing with inorganic powder or plastic powder, or adding a small amount to a paint. In particular, in applications where the PTFE aqueous dispersion is used for coating or for processing into PTFE fibers, the concentration of the PTFE particles is preferably 50 to 70% by mass, and more preferably 52 to 68% by mass. The pH of the aqueous PTFE dispersion is preferably 2-13, and more preferably 3-11.

[0066] The PTFE constituting the PTFE particles in the PTFE aqueous dispersion includes not only homopolymers of TFE but also so-called modified PTFE containing polymerization units based on copolymerization components copolymerizable with TFE, such as halogenated ethylenes such as chlorotrifluoroethylene, halogenated propylenes such as hexafluoropropylene, and fluorovinyl ethers such as perfluoro(alkyl vinyl ether), in trace amounts that are substantially incapable of melt processing.

[0067] The content of the nonionic surfactant in the aqueous PTFE dispersion is preferably from 1 to 20 mass %, more preferably from 1.5 to 15 mass %, and even more preferably from 2 to 10 mass %, based on the mass of PTFE. When the content is 1% by mass or more, the PTFE aqueous dispersion has excellent mechanical stability and excellent wettability, and when the content is 20% by mass or less, the coating film is less likely to crack, and the PTFE product has excellent durability. In particular, in order to improve wettability during coating and to make cracks less likely to occur, the content of the nonionic surfactant in the PTFE aqueous dispersion is particularly preferably 3 to 10% by mass.

[0068] The surface tension of the aqueous PTFE dispersion is preferably 24 to 35 mN / m, more preferably 25 to 32 mN / m. When the surface tension is 24 mN / m or more, the defoaming property is excellent, and when it is 35 mN / m or less, repellency is unlikely to occur.

[0069] The PTFE aqueous dispersion may contain one or more of a fluorine-free emulsifier, various leveling agents, preservatives, colorants, fillers, organic solvents, aqueous ammonia, and other known components. Furthermore, when the aqueous PTFE dispersion contains a viscosity modifier such as polyethylene oxide or polyurethane, the aqueous PTFE dispersion has excellent mechanical stability.

[0070] From the viewpoint of ease of application, the viscosity of the aqueous PTFE dispersion is preferably 300 mPa·s or less at 23° C., more preferably 3 to 100 mPa·s, and even more preferably 5 to 50 mPa·s. The thickening temperature of the aqueous PTFE dispersion is preferably 30 to 60° C., more preferably 35 to 55° C., and even more preferably 40 to 50° C. When the thickening temperature is within the above range, viscosity changes due to fluctuations in application temperature are unlikely to occur, and repellency is unlikely to occur.

[0071] <<Second embodiment>> A second embodiment of the method for producing an aqueous PTFE dispersion includes an embodiment having the following three steps. Step B1: A step of mixing at least one nucleating additive selected from the group consisting of polyalkylene oxide compounds and hydrocarbon-containing surfactants with an oxidizing agent in an aqueous medium to obtain a solution 2. Step B2: A step of polymerizing TFE in the solution 2 obtained in step B1 without substantially adding a surfactant to the solution 2 to obtain an aqueous emulsion containing PTFE particles. Step B3: A step of adding a nonionic surfactant to the aqueous emulsion and then concentrating the aqueous emulsion to obtain a PTFE aqueous dispersion. In the second embodiment, the amount of the nucleation additive used is 100 ppm by mass or less relative to the amount of TFE supplied to the polymerization system. The present invention will now be described in detail with reference to the above preferred embodiment.

[0072] <Process B1> Step B1 is a step of mixing at least one nucleation additive selected from the group consisting of polyalkylene oxide compounds and hydrocarbon-containing surfactants with an oxidizing agent in an aqueous medium to obtain a solution 2. In the following, first, the materials used in step B1 will be described in detail, and then the procedure of step B1 will be described in detail.

[0073] (Polyalkylene oxide compound) The polyalkylene oxide compound is a compound for forming nuclei (seeds) during the polymerization of TFE, that is, it corresponds to a nucleation additive. The polyalkylene oxide compound is a compound containing a polyalkylene oxide chain, and examples of the polyalkylene oxide chain include a polymethylene oxide chain, a polyethylene oxide chain, a polypropylene oxide chain, and a polytetramethylene oxide chain.

[0074] The polyalkylene oxide compound preferably has a surface tension in water at a concentration of 1000 ppm greater than about 40 dynes / cm, more preferably greater than about 42 dynes / cm, and even more preferably greater than about 45 dynes / cm, and preferably less than or equal to about 73 dynes / cm.

[0075] The number average molecular weight of the polyalkylene oxide compound is preferably 50-2,000, more preferably 100-1,500, and even more preferably 150-1,300.

[0076] The polyalkylene oxide compound is preferably a compound represented by formula (2) in that the formation of fluorine-based oligomers is further suppressed. Formula (2) R 21 -(OL 2 ) n -OR 22 In formula (2), R 21 and R 22 each independently represents a hydrogen atom, an alkyl group, an acryloyl group, or a methacryloyl group. L 2 represents an alkylene group having 1 to 4 carbon atoms, which may be linear or branched. n represents 1 to 50.

[0077] Examples of the polyalkylene oxide compound include polyethylene glycol, polyethylene glycol acrylate, polyethylene glycol methacrylate, polyethylene glycol methyl ether, polyethylene glycol dimethyl ether, polyethylene glycol butyl ether, polypropylene glycol, polypropylene glycol acrylate, polypropylene glycol methacrylate, polypropylene glycol dimethacrylate, polypropylene glycol methyl ether, polypropylene glycol dimethyl ether, polypropylene glycol butyl ether, polypropylene glycol dimethacrylate, and polytetramethylene glycol.

[0078] The polyalkylene oxide compounds may be used alone or in combination of two or more.

[0079] (Hydrocarbon-containing surfactants) Hydrocarbon-containing surfactants are surfactants that contain hydrocarbons. More specifically, at least some of the monovalent substituents on carbon atoms are hydrogen atoms, and they can also be substituted with halogen atoms such as fluorine and chlorine atoms. In preferred hydrocarbon-containing surfactants, at least 75%, preferably at least 85%, more preferably at least 95% of the monovalent substituents on carbon atoms are hydrogen atoms.

[0080] Hydrocarbon-containing surfactants include, for example, hydrocarbon surfactants and siloxane surfactants. A hydrocarbon surfactant refers to a surfactant that does not contain silicon atoms, and in which 100% of the monovalent substituents substituted on carbon atoms are hydrogen atoms, and therefore does not contain halogen atoms such as chlorine atoms and fluorine atoms. By siloxane surfactant is meant a hydrocarbon-containing surfactant having a hydrophobic group that includes a siloxane backbone that contains multiple siloxane units.

[0081] The hydrocarbon surfactant is preferably an anionic hydrocarbon surfactant, which means a hydrocarbon surfactant having a negatively charged hydrophilic portion such as a carboxylic acid group, a sulfonic acid group, a sulfate group, a phosphonic acid group, or a phosphate group, and a hydrocarbon portion such as an alkyl group as a hydrophobic portion. An example of an anionic hydrocarbon surfactant is a highly branched C10 tertiary carboxylic acid supplied as Versatic® 10 by Resolution Performance Products. Other examples of anionic hydrocarbon surfactants include the sodium linear alkyl polyether sulfonates supplied by BASF as their Avanel® S series.

[0082] As the anionic hydrocarbon surfactant, an anionic hydrocarbon surfactant represented by formula (7) is also preferred. Equation (7) R 71 -L 7 -M R71 represents an alkyl group. The alkyl group may be linear, branched, or cyclic, and is preferably linear. The number of carbon atoms in the alkyl group is, for example, 6 to 20. L 7 is -ArSO3 - , -SO3 - , -SO4 - , -PO3 - , -PO4 - , or -COO - Here, Ar represents an arylene group. M represents a monovalent cation. Examples of the monovalent cation include H + , Na + , K + , NH4 + Examples include: An example of the anionic hydrocarbon surfactant represented by formula (7) is sodium dodecyl sulfate.

[0083] Another example of an anionic hydrocarbon surfactant is the sulfosuccinate surfactant Lankropol® K8300 available from Akzo Nobel Surface Chemistry LLC.

[0084] As the hydrocarbon surfactant, nonionic hydrocarbon surfactants are also preferred. Nonionic hydrocarbon surfactants do not have a charged group, but have a hydrophobic portion that is often a long chain hydrocarbon. The hydrophilic portion of nonionic hydrocarbon surfactants includes water-soluble functional groups such as polyethylene oxide chains obtained from the polymerization of ethylene oxide. Nonionic hydrocarbon surfactants include block copolymers having various types of polyalkylene oxide blocks, such as polyethylene oxide and polypropylene oxide.

[0085] Suitable nonionic hydrocarbon surfactants include those described in paragraphs 0043 to 0052 of JP-A No. 2016-537499.

[0086] Suitable siloxane surfactants include those described in US Pat. Nos. 6,841,616 (Wille et al.) and 7,977,438 (Brothers et al.).

[0087] (Oxidizing agent) The oxidizing agent includes, for example, hydrogen peroxide and a polymerization initiator. Examples of the polymerization initiator include the compounds exemplified as the polymerization initiator described in the above step A1. As the polymerization initiator, a persulfate is preferable, and ammonium persulfate or potassium persulfate is more preferable.

[0088] The aqueous medium may be the aqueous medium used in step A1.

[0089] (Step B1) In step B1, a nucleating additive and an oxidizing agent are mixed in an aqueous medium to obtain a solution 2. In other words, in this step, the nucleating additive is exposed to an oxidizing agent in an aqueous medium. When the nucleating additive and the oxidizing agent are mixed in an aqueous medium, a solution in which lipophilic nucleation sites are dispersed in the aqueous medium is obtained. More specifically, when the nucleating additive such as a polyalkylene oxide compound and a hydrocarbon-containing surfactant is mixed with the oxidizing agent, the hydrophilic portion of the nucleating additive is decomposed, and the hydrophobic portion of the nucleating additive becomes a lipophilic nucleation site. The lipophilic nucleating sites are dispersed in the aqueous medium, and the fluoropolymer can be finely dispersed in these sites. Since the lipophilic nucleation site has excellent affinity with TFE, polymerization of TFE is likely to proceed in solution 2 containing the lipophilic nucleation site. In other words, the lipophilic nucleation site can be a hydrophobic environment for TFE polymerization.

[0090] The amount of the nucleation additive used is 100 ppm by mass or less, preferably 1 to 50 ppm by mass or less, and more preferably 1 to 25 ppm by mass, based on the amount of TFE supplied to the polymerization system (amount of TFE used) used in step B2 described below. The amount of the oxidizing agent used is preferably from 0.5 to 100 ppm by mass, and more preferably from 0.5 to 50 ppm by mass, based on the total mass of the aqueous medium. The temperature when the nucleation additive and the oxidizing agent are mixed is preferably from 20 to 120°C, more preferably from 40 to 120°C. The mixing time when the nucleation additive and the oxidizing agent are mixed is preferably 0.05 to 1.0 hour.

[0091] It is preferred to add a water-soluble inorganic salt to the aqueous medium before or during mixing of the nucleation additive and the oxidizing agent. The addition of a water-soluble inorganic salt is useful for increasing the number of fluoropolymer particles formed during nucleation. The amount of the water-soluble inorganic salt used is preferably from 0.01 to 80 ppm by mass, and more preferably from 1 to 50 ppm by mass, based on the total mass of the aqueous medium. Examples of water-soluble inorganic salts include sodium sulfite, sodium hydrogen sulfite, sodium chloride, potassium sulfite, potassium hydrogen sulfite, potassium carbonate, ammonium oxalate, sodium tetraborate, sodium acetate, ammonium carbonate, ammonium dihydrogen phosphate, and diammonium phosphate. Sulfite salts are preferred, and sodium sulfite and ammonium sulfite are more preferred.

[0092] <Process B2> Step B2 is a step of polymerizing TFE in solution 2 obtained in step B1 without substantially adding a surfactant to solution 2 to obtain an aqueous emulsion containing PTFE particles. This step is carried out in the same manner as in the above-mentioned step A2, except that solution 2 is used instead of solution 1, and therefore a description thereof will be omitted. The various properties of the PTFE obtained in step B2 are as described above for the various properties of the PTFE obtained in step A2. Note that the above "substantially not added" means that no surfactant is added, or even if added, the addition amount of the surfactant is 200 mass ppm or less based on the total mass of Solution 2. The lower limit is not particularly limited, but 0 mass ppm is preferred. That is, in Step B2, it is preferable not to add a surfactant to Solution 2.

[0093] <Step B3> Step 3 is a step of adding a nonionic surfactant to the aqueous emulsion obtained in Step B2, and then concentrating the aqueous emulsion to obtain a PTFE aqueous dispersion. That is, a nonionic surfactant is added to the low-concentration PTFE aqueous dispersion (corresponding to the above aqueous emulsion) obtained in Step B2, and then the low-concentration PTFE aqueous dispersion is concentrated to obtain a high-concentration PTFE aqueous dispersion (corresponding to the above PTFE aqueous dispersion). By carrying out Step B3, a PTFE aqueous dispersion showing a PTFE particle concentration higher than the PTFE particle concentration of the aqueous dispersion is obtained. In this step, since the same procedure as in Step A3 described above is carried out except that the aqueous emulsion obtained in Step B2 is used instead of the aqueous emulsion obtained in Step A2, the description thereof is omitted. Various properties of the PTFE aqueous dispersion obtained by Step B3 are as described for the various properties of the PTFE aqueous dispersion obtained by Step A3.

[0094] Note that after adding a nonionic surfactant to the aqueous emulsion obtained in Step B2 and before concentrating the aqueous emulsion, polymerization initiator residues and the like may be adsorbed and removed by an ion exchange resin or the like. Thereby, excess water-soluble ionic compounds are removed, the coating film performance of the PTFE aqueous dispersion is improved, and the application to insulating materials becomes easy.

[0095] <<PTFE Products>> PTFE products mean films, sheets, fibers mainly composed of PTFE obtained using a PTFE aqueous dispersion, heat-resistant articles having a PTFE coating film, and articles containing PTFE as a secondary component.

[0096] Examples of PTFE products include packings made by impregnating a PTFE aqueous dispersion into a substrate made of woven cloth or braided string made of glass fiber, aramid fiber, carbon fiber, or other synthetic or natural fibers, and then drying the substrate; heat-resistant conveyor belts, architectural membrane structure sheets, packings, and printed circuit board materials made by impregnating a PTFE aqueous dispersion into a substrate made of woven cloth or braided string made of heat-resistant fibers such as glass fiber, aramid fiber, or carbon fiber, and then baking the substrate at a temperature above the melting point of PTFE; kitchen appliances such as frying pans and electric kettles made by coating a metal plate such as aluminum or stainless steel with a PTFE aqueous dispersion containing a pigment or heat-resistant resin, and then baking the coated metal plate; binders made by kneading a PTFE aqueous dispersion with powdered active materials for batteries such as carbon, manganese dioxide, and nickel hydroxide; molding materials made by mixing a PTFE aqueous dispersion to prevent dripping during combustion of plastic moldings such as polycarbonate and ABS resin, and Molded bodies (anti-dripping agents); powders with reduced dust generation obtained by mixing aqueous PTFE dispersions with chemical fertilizers, lime, incineration ash, etc.; sliding materials such as oil-free bearings, in which a mixture of a paste made by mixing a filler such as lead, zinc, or carbon powder with an aqueous PTFE dispersion and coating it on a porous material; PTFE fibers obtained by adding a thickener such as viscose to an aqueous PTFE dispersion, pressurizing and spinning it in a coagulation bath and then sintering it; ultra-thin PTFE sheets obtained by coating a heat-resistant sheet substrate such as an aluminum plate or stainless steel plate with an aqueous PTFE dispersion, sintering it, and then peeling off the PTFE layer; coil insulation, interlayer insulation film, and electrical insulation materials obtained by casting an aqueous PTFE dispersion and having heat resistance, high insulation properties, and low dielectric tangent capabilities, and used in motors, transformers, relays, switches, etc.; paints, resins, and rubber materials with improved lubricity and anti-fouling properties due to the addition of an aqueous PTFE dispersion.

[0097] The PTFE product is obtained by coating or mixing the PTFE aqueous dispersion, and then drying or heat treating it at a temperature of room temperature to 420° C. The temperature of the drying or heat treatment is preferably 50 to 400° C., and more preferably 100 to 395° C. The PTFE content in the PTFE product varies depending on the application, but is preferably from 0.01 to 100% by mass, more preferably from 0.1 to 100% by mass, and even more preferably from 1 to 100% by mass. EXAMPLES

[0098] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto. Examples 1 to 6 described below correspond to examples, and Example 7 corresponds to a comparative example.

[0099] The various measurement and evaluation methods are as follows. (A) Average primary particle size of PTFE particles (hereinafter also referred to as "PPS") An aqueous PTFE dispersion was used as a sample, and the particle size distribution was measured using a laser scattering particle size distribution analyzer (manufactured by Horiba, Ltd., product name "LA-920"). (B) Standard Specific Gravity (hereinafter referred to as "SSG") Measured in accordance with ASTM D4895-04. 12.0 g of sample (PTFE powder) was weighed and held in a cylindrical mold with an inner diameter of 28.6 mm at 34.5 MPa for 2 minutes. This was placed in a 290°C oven and heated at 120°C / hr. After being held at 380°C for 30 minutes, the temperature was lowered at 60°C / hr and held at 294°C for 24 minutes. The sample was held in a desiccator at 23°C for 12 hours, and then the specific gravity of the sample relative to water at 23°C was measured and used as the standard specific gravity. The smaller the SSG value, the larger the molecular weight. (C) PTFE concentration and surfactant concentration Approximately 7 g of the PTFE aqueous dispersion was placed in an aluminum dish (mass W0) and weighed (mass W1). The PTFE concentration and surfactant concentration (ratio of surfactant to PTFE mass) were calculated using the following formula from the mass after drying at 120°C for 1 hour (mass W2) and the mass after drying at 380°C for 35 minutes (mass W3). PTFE concentration (mass%)=[(W3-W0) / (W1-W0)]×100 Surfactant concentration (mass% / PTFE) = [(W2-W3) / (W3-W0)] x 100 (D) Viscosity The viscosity of the PTFE aqueous dispersion was measured using a Brookfield viscometer with a #1 spindle at a liquid temperature of 23° C. and at 60 rpm. (E) pH The pH of the PTFE aqueous dispersion was measured by the glass electrode method. (F)Surface tension The surface tension of the PTFE aqueous dispersion was measured by the ring method using a platinum wire ring. (G) CFT (Crack Thickness Limit) Using an applicator with a continuously variable coating thickness up to 200 μm, the PTFE aqueous dispersion was applied onto an aluminum plate with a thickness of 0.5 mm, dried at 120°C for 10 minutes, and then baked at 380°C for 10 minutes. The PTFE coating was observed, and the thickness of the tip of the crack that had occurred was measured at five points using a permscope, and the average value (μm) was calculated and used as the CFT (crack critical thickness). (H) Measurement of fluorinated oligomers A sample (PTFE powder) was subjected to Soxhlet extraction with ethanol for 5 hours, and the ethanol extract was subjected to LC / MS analysis to quantify oligomers of CF2 chains with carbon numbers of 6 to 34, mainly using perfluorooctyl sulfonic acid and perfluorooctanoic acid as standards. Cases where the presence of oligomers was confirmed were recorded as "present," and cases where they were not confirmed were recorded as "absent." In the LC / MS analysis, an Agilent 1260 series HPLC / 6460MS was used, and the Imtakt Cadenza CD-C18 2 mmφ×100 mm 3 μm particle size column was used. In addition, a gradient of an aqueous ammonium acetate solution and methanol was applied during the measurement.

[0100] (Example 1) [Process A1] Paraffin wax (1500 g) and deionized water (60 L) were charged into a 100 L stainless steel autoclave. After replacing the air in the autoclave with nitrogen, the pressure was reduced and i-butyl methacrylate (i-BMA) (0.1 g) and deionized water (0.5 L) were poured into the autoclave. Next, the inside of the autoclave was brought to a state of atmospheric pressure or less, and the solution in the autoclave was heated to 75° C. while being stirred. After that, a solution of ammonium persulfate (0.055 g) as a polymerization initiator dissolved in deionized water (1 L) was injected into the autoclave, and i-butyl methacrylate was polymerized.

[0101] [Process A2] After 20 minutes, the pressure was increased to 1.96 MPa with TFE, and a solution of ammonium persulfate (0.54 g) and disuccinic acid peroxide (concentration 80% by mass, the remainder being water) (53 g) dissolved in warm water (1 L) at approximately 70°C was injected into the autoclave. After the internal pressure of the autoclave had dropped to 1.89 MPa, TFE was added so as to maintain the pressure at 1.96 MPa, and polymerization of TFE was allowed to proceed. When the amount of TFE added reached 9 kg, the reaction was terminated and the TFE in the autoclave was released into the atmosphere. The polymerization time was 94 minutes. The solids concentration (PTFE particle concentration) of the aqueous emulsion was about 11 mass %. The average primary particle size of the PTFE particles in the aqueous emulsion was 0.24 μm (240 nm). A part of the obtained aqueous emulsion was adjusted to 20°C and stirred to aggregate the PTFE particles, and a PTFE powder was obtained. Next, this PTFE powder was dried at 275°C together with an aqueous ammonium carbonate solution. The SSG of the obtained PTFE powder was 2.201. Furthermore, no by-product fluorine-based oligomers were found in the obtained PTFE powder.

[0102] [Process A3] The aqueous emulsion obtained in step A2 was treated with a nonionic surfactant (a) (Newcol 1308FA, manufactured by Nippon Nyukazai Co., Ltd. 13 H 27-(OC2H4)8-OCH(CH3)CH2-OH) was dissolved at a ratio of 2.7% by mass relative to the PTFE mass, ammonium laurate was dissolved at 0.06% by mass relative to the PTFE mass, and triethanolamine lauryl sulfate was dissolved at 0.02% by mass relative to the PTFE mass, and the solution was concentrated by electrophoresis. The supernatant was removed to obtain an aqueous PTFE dispersion having a PTFE concentration of 65.8% by mass and a nonionic surfactant (a) concentration of 2.1% by mass relative to the PTFE mass. This PTFE aqueous dispersion was mixed with a nonionic surfactant (b) (Newcol G1301H, C 13 H 27 -OCH2CH(C2H5)-(OC2H4)8-OH) at 1.2 mass% relative to the mass of PTFE, and a nonionic surfactant (c) (Newcol FAA09801, manufactured by Nippon Nyukazai Co., Ltd., C 13 H 27 -OCH2CH(C2H5)-(OC2H4) 11 -OH) at 1.2% by mass relative to the PTFE mass, PEO at 0.1% by mass relative to the PTFE mass, water and aqueous ammonia were added, and nonionic surfactant (a) was added so that the content of nonionic surfactant (a) relative to the PTFE mass was 2.4% by mass, to obtain a PTFE aqueous dispersion with a PTFE concentration of 60.5% by mass and a pH of 10.2. The viscosity of the obtained PTFE aqueous dispersion at 23°C was 25.8 mPa s, pH = 10.2, and surface tension was 30 (mN / m). The average primary particle diameter of the PTFE particles in the PTFE aqueous dispersion was the same as the average primary particle diameter of the PTFE particles measured in the above aqueous emulsion.

[0103] The crack limit film thickness was measured using this aqueous PTFE dispersion. The evaluation results of the obtained aqueous PTFE dispersion are shown in Table 1.

[0104] (Example 2) [Process B1] Paraffin wax (1500 g) and deionized water (60 L) were charged into a 100 L stainless steel autoclave. After replacing the air in the autoclave with nitrogen, the pressure was reduced and PEG1000 (number average molecular weight: 1000, polyethylene glycol) (0.05 g) and deionized water (1 L) were poured into the autoclave. Next, the pressure inside the autoclave was lowered below atmospheric pressure, and the solution inside the autoclave was heated to 75° C. while being stirred. Then, a solution of ammonium persulfate (0.11 g) as an oxidizing agent dissolved in deionized water (1 L) was injected into the autoclave.

[0105] [Process B2] After 10 minutes, the pressure was increased to 1.96 MPa with TFE, and a solution of ammonium persulfate (0.54 g) and disuccinic acid peroxide (concentration 80% by mass, the remainder being water) (53 g) dissolved in warm water (1 L) at approximately 70°C was injected into the autoclave. After the internal pressure of the autoclave had dropped to 1.89 MPa, TFE was added so as to maintain the pressure at 1.96 MPa, and polymerization of TFE was allowed to proceed. When the amount of TFE added reached 9 kg, the reaction was terminated and the TFE in the autoclave was released into the atmosphere. The polymerization time was 88 minutes. The solids concentration (PTFE particle concentration) of the aqueous emulsion was about 11 mass %. The average primary particle size of the PTFE particles in the aqueous emulsion was 0.24 μm (240 nm). A part of the obtained aqueous emulsion was adjusted to 20°C and stirred to aggregate the PTFE particles, and a PTFE powder was obtained. Next, this PTFE powder was dried at 275°C together with an aqueous ammonium carbonate solution. The SSG of the obtained PTFE powder was 2.204. Furthermore, no by-product fluorine-based oligomers were found in the obtained PTFE powder.

[0106] [Process B3] The aqueous emulsion obtained in step B2 was concentrated in the same manner as in Example 1 to obtain an aqueous PTFE dispersion. The average primary particle size of the PTFE particles in the aqueous PTFE dispersion was the same as the average primary particle size of the PTFE particles measured in the aqueous emulsion. The evaluation results are shown in Table 1.

[0107] (Example 3) Instead of the nonionic surfactant (a), a nonionic surfactant (d) (Tergitol TMN100X, manufactured by DOW Co., Ltd.) was used. 12 H 25 -(OC2H4) 10 A PTFE aqueous dispersion was obtained in the same manner as in Example 1, except that a PTFE copolymer having the formula (I-OH) was used instead. The evaluation results are shown in Table 1.

[0108] (Example 4) Except for using the nonionic surfactant (d) instead of the nonionic surfactant (a), an aqueous PTFE dispersion was obtained in the same manner as in Example 2. The evaluation results are shown in Table 1.

[0109] (Example 5) [Process A1] Paraffin wax (1500 g) and deionized water (60 L) were charged into a 100 L stainless steel autoclave. After replacing the air in the autoclave with nitrogen, the pressure was reduced and i-butyl methacrylate (i-BMA) (0.1 g) and deionized water (0.5 L) were poured into the autoclave. Next, the inside of the autoclave was brought to a state of atmospheric pressure or less, and the solution in the autoclave was heated to 75° C. while being stirred. After that, a solution of ammonium persulfate (0.055 g) as a polymerization initiator dissolved in deionized water (1 L) was injected into the autoclave, and i-butyl methacrylate was polymerized.

[0110] [Process A2] After 20 minutes, the autoclave was pressurized to 1.96 MPa with TFE, and a solution of ammonium persulfate (0.54 g) and disuccinic acid peroxide (concentration 80% by mass, remaining water) (53 g) dissolved in warm water (1 L) at about 70 ° C. was injected into the autoclave. Next, TFE was added so that the internal pressure in the autoclave was kept at 1.96 MPa, and polymerization of TFE was allowed to proceed. After adding 1 kg of TFE, a solution of ammonium vinyl sulfonate (5.0 g) dissolved in deionized water (1.5 L) was added, and ammonium vinyl sulfonate was supplied while checking the amount of TFE supplied with a flow meter so that ammonium vinyl sulfonate was 0.15 g per 1 kg of TFE supplied. When the amount of TFE added reached 9 kg, the reaction was terminated and the TFE in the autoclave was released into the atmosphere. The polymerization time was 97 minutes. The solids concentration of the aqueous emulsion (concentration of modified PTFE) was about 12 mass %. The average primary particle size of the modified PTFE particles in the aqueous emulsion was 0.21 μm. A part of the obtained aqueous emulsion was adjusted to 20°C and stirred to aggregate the modified PTFE particles, and a modified PTFE powder was obtained. Next, this modified PTFE powder was dried at 275°C together with an aqueous ammonium carbonate solution. The SSG of the obtained modified PTFE powder was 2.193. Furthermore, no by-product fluorine-based oligomers were found in the resulting modified PTFE powder.

[0111] [Process A3] The aqueous emulsion obtained in step A2 was concentrated in the same manner as in Example 1 to obtain an aqueous PTFE dispersion. The average primary particle diameter of the PTFE particles in the aqueous PTFE dispersion was the same as the average primary particle diameter of the PTFE particles measured in the aqueous emulsion. The evaluation results are shown in Table 1. The evaluation results are shown in Table 1.

[0112] (Example 6) Except for using the nonionic surfactant (d) instead of the nonionic surfactant (a), a PTFE aqueous dispersion was obtained in the same manner as in Example 5. The evaluation results are shown in Table 1.

[0113] (Example 7) In [Step B1] of (Example 2), the amount of PEG1000 used was changed from 0.05g to 0.39g, and in [Step B2] of (Example 2), TFE was added so as to maintain the internal pressure in the autoclave at 1.96MPa. When polymerizing TFE, 1kg of TFE was added, and then a solution of sodium lauryl sulfate (SLS) dissolved in deionized water was added while checking the amount of TFE supplied with a flow meter so that 1.48g of SLS was supplied per 1kg of TFE supplied. Except for changing the drying temperature from 275°C to 220°C, a PTFE powder was obtained according to the same procedure as in (Example 2) above. The obtained PTFE powder contained a fluorine-based oligomer group (H(CF2CF2) n SO3H (n = 3-16) was detected at a total of 230 ppm by mass, with a distribution with peaks around n = 9 and 10. Fluorine-based oligomers were detected, and because it is impossible to completely remove them using ion exchange resins, etc., concentration was not performed.

[0114] In Table 1, the column "Amount of non-fluorinated monomer used" indicates the amount of non-fluorinated monomer used relative to the amount of TFE supplied to the polymerization system. The column "Amount of nucleation additive used" indicates the amount of nucleation additive used relative to the amount of TFE fed to the polymerization system.

[0115] [Table 1]

[0116] As shown in Table 1, according to the production method of the present invention, an aqueous PTFE dispersion exhibiting the desired effects can be produced. The entire contents of the specification, claims, drawings and abstract of Japanese Patent Application No. 2019-196139, filed on October 29, 2019, are hereby incorporated by reference as the disclosure of the specification of the present invention.

Claims

1. A step A1 of polymerizing a non-fluorinated monomer in an aqueous medium to obtain a solution 1 containing a polymer containing units based on the non-fluorinated monomer; A step A2 of polymerizing tetrafluoroethylene in the solution 1 without adding a surfactant to the solution 1 to obtain an aqueous emulsion containing polytetrafluoroethylene particles; A step A3 of adding a nonionic surfactant to the aqueous emulsion and then concentrating the aqueous emulsion to obtain an aqueous polytetrafluoroethylene dispersion, A method for producing an aqueous polytetrafluoroethylene dispersion, comprising the steps of: A method for producing an aqueous polytetrafluoroethylene dispersion, wherein the content of the polytetrafluoroethylene particles in the aqueous polytetrafluoroethylene dispersion is 50 to 70 mass % based on the total amount of the aqueous polytetrafluoroethylene dispersion.

2. The method for producing an aqueous polytetrafluoroethylene dispersion according to claim 1, wherein the non-fluorinated monomer is a monomer represented by formula (1): Formula (1) CH 2 =CR 11 -L 1 -R 12 In formula (1), R 11 represents a hydrogen atom or an alkyl group. 1 represents a single bond, -CO-O-*, -O-CO-* or -O-. * represents R 12 represents the bonding position with 12 represents a hydrogen atom, an alkyl group, an alkenyl group, or a nitrile group. 1 When is a single bond, R 12 is a nitrile group.

3. 3. The method for producing an aqueous polytetrafluoroethylene dispersion according to claim 1, wherein the content of the nonionic surfactant in the aqueous polytetrafluoroethylene dispersion is 1 to 20 mass % based on the mass of polytetrafluoroethylene.

4. A step B1 of mixing at least one nucleating additive selected from the group consisting of polyalkylene oxide compounds and hydrocarbon-containing surfactants with an oxidizing agent in an aqueous medium to obtain a solution 2; A step B2 of polymerizing tetrafluoroethylene in the solution 2 without substantially adding a surfactant to the solution 2 to obtain an aqueous emulsion containing polytetrafluoroethylene particles; and a step B3 of adding a nonionic surfactant to the aqueous emulsion and then concentrating the aqueous emulsion to obtain an aqueous polytetrafluoroethylene dispersion, A method for producing an aqueous polytetrafluoroethylene dispersion, comprising the steps of: The method for producing an aqueous polytetrafluoroethylene dispersion, wherein the nucleating additive is a polyalkylene oxide compound.

5. 5. The method for producing an aqueous polytetrafluoroethylene dispersion according to claim 4, wherein the content of the polytetrafluoroethylene particles in the aqueous polytetrafluoroethylene dispersion is 50 to 70 mass% based on the total amount of the aqueous polytetrafluoroethylene dispersion.

6. 6. The method for producing an aqueous polytetrafluoroethylene dispersion according to claim 4, wherein the amount of the oxidizing agent used is 0.5 to 100 ppm by mass based on the total mass of the aqueous medium.

7. The method for producing an aqueous polytetrafluoroethylene dispersion according to any one of claims 4 to 6, wherein the content of the nonionic surfactant in the aqueous polytetrafluoroethylene dispersion is 1 to 20 mass% based on the mass of polytetrafluoroethylene.

Citation Information

Patent Citations

  • Fluoropolymer dispersions containing little or no low molecular weight fluorinated surfactants

    JP2005501956A

  • Aqueous dispersion of polytetrafluoroethylene with a small amount of fluorinated surfactant

    JP2007511657A

  • Nitrogen-containing carboxylic acid derivative, method for producing nitrogen-containing carboxylic acid derivative

    JP2009029723A

  • Use of polyalkylene oxides to form nuclei in the aqueous polymerization of fluoromonomers

    JP2016537499A

  • Modified polytetrafluoroethylene, molded article, and method for producing stretched porous material

    WO2019065640A1