Positive electrode active material powder, positive electrode, lithium ion battery, and method for producing positive electrode active material powder
Coating lithium-nickel composite oxide in lithium ion batteries with lithium-tungsten composite oxide, particularly Li4W5O5 phase, addresses capacity deterioration by inhibiting electrolyte reactions, thereby improving capacity retention.
Patent Information
- Application Number
- JP2022113229
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-07-14
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-07-14
AI Technical Summary
Lithium ion batteries experience capacity deterioration due to the reaction between the newly generated surface of crushed positive electrode active material powder and the electrolyte during high-temperature storage, leading to a decrease in capacity retention rate.
The positive electrode active material powder is composed of lithium-nickel composite oxide with a Ni ratio of 0.5 or more, coated with lithium-tungsten composite oxide, particularly with a phase composition of Li4W5O5, which inhibits the reaction between the nascent surface and electrolytes, enhancing capacity retention.
The use of lithium-tungsten composite oxide coating on lithium-nickel composite oxide improves the capacity retention rate during high-temperature storage by promoting the formation of Li4W5O5 phase, which provides a protective effect against electrolyte reactions.
Smart Images

Figure 0007586147000005 
Figure 0007586147000006 
Figure 0007586147000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a positive electrode active material powder, a positive electrode, a lithium ion battery, and a method for producing a positive electrode active material powder. [Background technology]
[0002] JP 2021-018895 A (Patent Document 1) discloses a coating containing tungsten oxide and lithium tungstate. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2021-018895 Summary of the Invention [Problem to be solved by the invention]
[0004] There is a demand for lithium ion batteries (hereinafter, abbreviated as "batteries") with higher output. For example, the specific surface area of the positive electrode active material powder can be increased by crushing the positive electrode active material powder. It is expected that the increase in the specific surface area will increase the reaction area and improve the output.
[0005] However, crushing the positive electrode active material powder may generate new surfaces. The new surfaces are active. During high-temperature storage, the new surfaces may react with the electrolyte, which may accelerate capacity degradation. In other words, the capacity retention rate may decrease.
[0006] Therefore, an object of the present disclosure is to improve the capacity retention rate. [Means for solving the problem]
[0007] The technical configuration and effects of the present disclosure will be described below. However, the mechanism of action in this specification includes assumptions. The mechanism of action does not limit the technical scope of the present disclosure.
[0008] 1. The positive electrode active material powder contains a lithium nickel composite oxide and a lithium tungsten composite oxide. In the lithium nickel composite oxide, the ratio of the substance amount of Ni to the total substance amount of atoms other than Li and oxygen is 0.5 or more. The lithium tungsten composite oxide is attached to at least a part of the surface of the lithium nickel composite oxide. 30% or more of the lithium tungsten composite oxide is composed of the Li4WO5 phase.
[0009] Hereinafter, lithium nickel composite oxide may be abbreviated as "LNO". Lithium tungsten composite oxide may be abbreviated as "LWO". In LNO, the ratio of the amount of substance of Ni to the total amount of substances of atoms other than Li and oxygen may be abbreviated as "Ni ratio".
[0010] It has been proposed to coat the surface of LNO with LWO by subjecting a mixture of LNO and WO3 to heat treatment. LWO can have a protective effect on the nascent surface. That is, LWO can inhibit the reaction between the nascent surface and the electrolyte. The main phase of LWO is usually the Li2WO4 phase.
[0011] LNO with a Ni ratio of 0.5 or more may be called a "high nickel material". By disintegrating the high nickel material, a large amount of active Li may be generated on the new surface. According to the new findings of the present disclosure, in a Li-rich reaction system, the formation of the Li4WO5 phase may be promoted compared to the formation of the Li2WO4 phase. The Li4WO5 phase has a better protective effect during high-temperature storage than the Li2WO4 phase. By making the composition ratio of the Li4WO5 phase in LWO 30% or more, it is expected that the capacity retention rate during high-temperature storage will be improved.
[0012] 2. In the positive electrode active material powder described in the above item "1," the lithium tungsten composite oxide may contain, for example, 54% or more of a Li4WO5 phase, with the remainder being a Li2WO4 phase.
[0013] When the composition ratio of the Li4WO5 phase is 54% or more, an improvement in the capacity retention rate is expected.
[0014] 3. In the positive electrode active material powder according to the above item "1" or "2," the lithium nickel composite oxide may be represented by, for example, the following formula (1). Li (1+x) Ni y Co z Mn (1-y-z) M a O (2-b) C b …(1) In the above formula (1), x, y, z, a, and b satisfy the relationships 0≦x≦0.7, 0.5≦y≦0.8, 0.1≦z≦0.2, 0≦a≦0.1, and 0≦b≦0.5. M is at least one selected from the group consisting of Zr, Mo, W, Mg, Ca, Na, Fe, Cr, Zn, Si, Sn, Al, and Ag. C is at least one selected from the group consisting of F, Cl, and Br.
[0015] 4. The coverage rate of the surface of the lithium nickel composite oxide with the lithium tungsten composite oxide may be, for example, 11 to 25%. The coverage is calculated by the following formula (2). θ=r w / (r w +r Ni +r Co +r Mn ) …(2) In the above formula (2), θ represents the coverage rate. w , r Ni , r Co , and r Mn is measured by X-ray photoelectron spectroscopy. w indicates the atomic ratio of W. Ni indicates the atomic ratio of Ni. Co indicates the atomic ratio of Co. Mn indicates the atomic ratio of Mn.
[0016] Hereinafter, "the coverage of the surface of LNO with LWO" may be abbreviated as "coverage." When the coverage is in the range of 11 to 25%, the Li4WO5 phase tends to be easily generated.
[0017] 5. The positive electrode active material powder according to any one of the above items "1" to "4" may have a D50 of, for example, 1.2 to 2.7 μm.
[0018] When D50 is 1.2 to 2.7 μm, the Li4WO5 phase tends to be generated.
[0019] 6. The positive electrode contains the positive electrode active material powder according to any one of the above items "1" to "5".
[0020] 7. A lithium ion battery comprising the positive electrode described in "6" above.
[0021] 8. A method for producing a positive electrode active material powder includes the following steps (a) to (c): (a) A lithium nickel composite oxide is crushed to prepare a crushed powder. (b) A mixture is prepared by mixing the crushed powder with WO3. (c) The mixture is subjected to a heat treatment to produce a positive electrode active material powder. The positive electrode active material powder includes a lithium nickel composite oxide and a lithium tungsten composite oxide. In the lithium nickel composite oxide, the ratio of the substance amount of Ni to the total substance amount of atoms other than Li and oxygen is 0.5 or more. The lithium tungsten composite oxide is attached to at least a part of the surface of the lithium nickel composite oxide. At least 30% of the lithium tungsten composite oxide is composed of a Li4WO5 phase.
[0022] Hereinafter, an embodiment of the present disclosure (hereinafter may be abbreviated as "the present embodiment") and an example of the present disclosure (hereinafter may be abbreviated as "the present embodiment") will be described. However, the present embodiment and the present embodiment do not limit the technical scope of the present disclosure. The present embodiment and the present embodiment are illustrative in all respects. The present embodiment and the present embodiment are non-restrictive. The technical scope of the present disclosure encompasses all modifications within the meaning and scope equivalent to the description of the claims. For example, it is originally intended that any configuration may be extracted from the present embodiment and the present embodiment, and that they may be arbitrarily combined. [Brief description of the drawings]
[0023] [Figure 1] FIG. 1 is a schematic flow chart of a method for producing a positive electrode active material powder in this embodiment. [Diagram 2] FIG. 2 is a conceptual diagram of a lithium ion battery in this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] <Terms and definitions> The words "comprise," "include," "have," and variations thereof (e.g., "consisting of") are open-ended. The open-ended form may or may not include additional elements in addition to the required elements. The words "consisting of" are closed-ended. However, the closed form does not exclude additional elements that are normally associated with the technology or that are unrelated to the technology disclosed. The words "consisting essentially of..." are semi-closed. The semi-closed form allows for the addition of elements that do not substantially affect the basic and novel characteristics of the technology disclosed.
[0025] Expressions such as "may" and "may" are used in the permissive sense, meaning "to have the possibility," rather than in the obligatory sense, meaning "to have to."
[0026] For example, a numerical range such as "m to n%" includes an upper limit and a lower limit. That is, "m to n%" indicates a numerical range of "m% or more and n% or less." Furthermore, "m% or more and n% or less" includes "more than m% and less than n%." Furthermore, a numerical value arbitrarily selected from within the numerical range may be set as a new upper limit or lower limit. For example, a new numerical range may be set by arbitrarily combining a numerical value within the numerical range with a numerical value described in another part of this specification, in a table, in a figure, or the like.
[0027] Unless otherwise specified, the order of execution of the steps, operations, and the like included in various methods is not limited to the order described. For example, the steps may proceed simultaneously. For example, the steps may be performed in sequence.
[0028] All numerical values are modified by the term "about." The term "about" may mean, for example, ±5%, ±3%, ±1%, etc. All numerical values may be approximations that may vary depending on the application of the disclosed technology. All numerical values may be expressed with significant figures. Measurements may be average values of multiple measurements. The number of measurements may be three or more, five or more, or ten or more. In general, the more measurements are taken, the more reliable the average value is expected to be. Measurements may be rounded off based on the number of significant figures. Measurements may include errors associated with, for example, the detection limits of the measuring device.
[0029] When a compound is expressed by a stoichiometric composition formula (e.g., "LiCoO2", etc.), the stoichiometric composition formula is merely a representative example of the compound. The compound may have a non-stoichiometric composition. For example, when lithium cobalt oxide is expressed as "LiCoO2", unless otherwise specified, the lithium cobalt oxide is not limited to the composition ratio of "Li / Co / O=1 / 1 / 2" and may contain Li, Co, and O in any composition ratio. Furthermore, doping, substitution, etc. with trace elements may also be allowed.
[0030] "D50" refers to the particle size at which the cumulative frequency of the smaller particle size reaches 50% in the volume-based particle size distribution. The particle size distribution can be measured by a laser diffraction particle size distribution measuring device. The measurement sample can be prepared by dispersing the powder in water by ultrasonic treatment.
[0031] 《Composition ratio of Li4WO5 phase and Li2WO4 phase》 The composition ratio of the Li4WO5 phase and the Li2WO4 phase in LWO can be determined by analyzing the XAFS (X-ray Absorption Fine Structure) spectrum of the positive electrode active material powder. The beamline "BL5S1" at the "Aichi Synchrotron Light Center" is one example of a facility that can measure XAFS spectra.
[0032] The standard spectrum of Li4WO5 is measured by the following procedure. A mixture of LiOH and WO3 is heat-treated at 950°C for 10 hours to produce Li4WO5. A mixture is prepared by mixing 1 part by mass of Li4WO5 and 99 parts by mass of boron nitride using a dancing mill. A pellet sample is formed by pressing the mixture with a pressure of 30 kN using a tablet press. For example, a hydraulic press or the like may be used. The pellet sample is placed on a stage. The XAFS spectrum of Li4WO5 is measured by the transmission method.
[0033] The standard spectrum of Li2WO4 is measured by the following procedure. Commercially available Li2WO4 powder (e.g., manufactured by Kishida Chemical Co., Ltd.) is prepared. As described above, a pellet sample containing Li2WO4 and boron nitride is prepared. The XAFS spectrum of Li2WO4 is measured by the transmission method.
[0034] Similarly to the above, a pellet sample containing the measurement target (positive electrode active material powder) and boron nitride is prepared. Note that, for example, instead of the pellet sample, an electrode (positive electrode) containing a positive electrode active material powder, a conductive material, a binder, etc. may be used as the measurement sample. The XAFS spectrum of the positive electrode active material powder is measured by a fluorescence method.
[0035] The XAFS spectrum is analyzed by the XAFS analysis software "Athena". The XAFS spectrum of the positive electrode active material powder is fitted to the standard spectrum of Li4WO5 and the standard spectrum of Li2WO4. This allows the composition ratio of the Li4WO5 phase and the composition ratio of the Li2WO4 phase in the positive electrode active material powder to be identified.
[0036] Coverage The coverage is measured by X-ray photoelectron spectroscopy (XPS). For example, an XPS device manufactured by ULVAC-PHI, Inc., product name: PHI X-tool (or equivalent) may be used. The positive electrode active material powder is set in the XPS device. Narrow scan analysis is performed. The measurement data is processed by analysis software. For example, an analysis software manufactured by ULVAC-PHI, Inc., product name: MulTiPak (or equivalent) may be used. By analyzing the measurement data, the W4f 7 / 2 , Ni2p 3 / 2 , Co2p 3 / 2 , Mn2p 3 / 2 The atomic ratio of each atom is calculated from the area of each peak. The coverage is calculated using the following formula (2). The coverage is expressed as a percentage. θ=r w / (r w +r Ni +r Co +r Mn ) …(2) In the above formula (2), θ represents the coverage rate (%). w indicates the atomic ratio of W. Ni indicates the atomic ratio of Ni. Co indicates the atomic ratio of Co. Mn indicates the atomic ratio of Mn.
[0037] <Cathode active material powder> The positive electrode active material powder is an aggregate of particles. The positive electrode active material powder has a high proportion of fine particles and can have a large specific surface area. By using the positive electrode active material powder, the reaction area during current application is increased, and it is expected that the output will be improved.
[0038] 《Particle size distribution》 The D50 of the positive electrode active material powder may be, for example, 7 μm or less, 2.7 μm or less, or 1.6 μm or less. The smaller the D50, the higher the composition ratio of the Li4WO5 phase tends to be. The D50 of the positive electrode active material powder may be, for example, 1.2 μm or more, 1.4 μm or more, or 1.5 μm or more. The D50 of the positive electrode active material powder may be, for example, 1.2 to 2.7 μm.
[0039] The width of the particle size distribution may be, for example, 0.1 to 10 μm. That is, the minimum value (Dmin) may be 0.1 μm and the maximum value (Dmax) may be 10 μm. The width of the particle size distribution may be, for example, 0.2 to 4 μm.
[0040] Coverage The positive electrode active material powder includes composite particles. The composite particles include LNO and LWO. That is, the positive electrode active material powder includes LNO and LWO. LNO is a base material of the composite particles. LWO is a coating material. LWO is attached to at least a part of the surface of LNO. For example, LWO may cover the entire surface of LNO. For example, LWO may cover a part of the surface of LNO. LWO may be distributed in an island shape on the surface of LNO. The coverage may be, for example, 11% or more, 12% or more, 14% or more, 16% or more, or 18% or more. The coverage may be, for example, 25% or less, or 22% or less. When the coverage is 11 to 25% or less, the composition ratio of the Li4WO5 phase tends to be high.
[0041] The composite particles may have any shape, for example, a spherical shape, an ellipsoidal shape, a flake shape, a cylindrical shape, or the like.
[0042] Lithium tungsten composite oxide LWO may have the effect of protecting the nascent surface of LNO. On the surface of LNO, LWO may be in the form of a film or particles. LWO may include a plurality of phases. 30% or more of LWO is the Li4WO5 phase. The remainder of LWO excluding the Li4WO5 phase (hereinafter may be abbreviated as "the remainder") may include, for example, a Li2WO4 phase or the like. LWO may include, for example, 30% or more of the Li4WO5 phase and the remaining Li2WO4 phase. For example, the ratio of the Li4WO5 phase to the total of the Li4WO5 phase and the Li2WO4 phase may be 30% or more.
[0043] The remainder is, for example, Li6WO6 phase, Li2W4O 13 phase, Li2W2O7 phase, Li6W2O9 phase, Li2W2O7 phase, Li2W5O 16 Phase, Li9W 19 O 55 Phase, Li3W 10 O 30 Phase, Li 18 W5O 15 The total composition ratio of phases other than the Li4WO5 phase and the Li2WO4 phase may be, for example, 10% or less, 5% or less, 1% or less, or 0.1% or less.
[0044] By having a Li4WO5 phase ratio of 30% or more, an improvement in capacity retention is expected. The Li4WO5 phase ratio may be, for example, 34% or more, 54% or more, 61% or more, or 63% or more. The Li4WO5 phase ratio may be, for example, 71% or less, 66% or less, or 64% or less. The LWO may contain, for example, 54% or more of the Li4WO5 phase and the balance Li2WO4 phase. The LWO may contain, for example, 54 to 71% of the Li4WO5 phase and the balance Li2WO4 phase.
[0045] Lithium nickel composite oxide LNO causes a positive electrode reaction. LNO may have any crystal structure. LNO may have, for example, a layered rock salt structure. LNO includes Li, Ni, and O (oxygen). LNO may consist of Li, Ni, and O. LNO is a host-guest system. Ni and O may form a host structure. Li behaves as a guest. The host structure may include additional atoms in addition to Ni and O. The host structure may include, for example, at least one selected from the group consisting of Co, Mn, and Al. However, the Ni ratio of LNO is 0.5 or more. When the Ni ratio is 0.5 or more, the composition ratio of the Li4WO5 phase tends to be high. The Ni ratio may be, for example, 0.6 or more, 0.7 or more, 0.8 or more, or 0.9 or more.
[0046] LNO may be represented, for example, by the following formula (1). Li (1+x) Ni y Co z Mn (1-y-z) M a O (2-b) C b …(1) In the above formula (1), x, y, z, a, and b satisfy the relationships 0≦x≦0.7, 0.5≦y≦0.8, 0.1≦z≦0.2, 0≦a≦0.1, and 0≦b≦0.5. M is at least one selected from the group consisting of Zr, Mo, W, Mg, Ca, Na, Fe, Cr, Zn, Si, Sn, Al, and Ag. C is at least one selected from the group consisting of F, Cl, and Br.
[0047] In the above formula (1), y may satisfy, for example, 0.5≦y≦0.6, 0.6≦y≦0.7, or 0.7≦y≦0.8.
[0048] Generally, LNO may be a secondary particle formed by agglomeration of a large amount of primary particles. LNO may usually contain 100 or more primary particles. The LNO in this embodiment is crushed. The secondary particles after crushing are composed of a relatively small amount of primary particles. LNO may be crushed to the primary particle level. The secondary particles after crushing may be composed of, for example, 30 or less, 20 or less, 10 or less, 5 or less, or 3 or less primary particles. The primary particles may exist alone. The number of primary particles contained in the secondary particles can be measured in a SEM (Scanning Electron Microscope) image of the positive electrode active material powder. In the SEM image, for example, when two primary particles overlap, the primary particle at the back is not confirmed. However, in this embodiment, the number that can be confirmed in the SEM image is considered to be the number of primary particles contained in the secondary particles.
[0049] The primary particles can have any shape, for example, they can be spherical, ellipsoidal, flake-like, cylindrical, etc.
[0050] <Method of manufacturing positive electrode active material powder> 1 is a schematic flow chart of the method for producing a positive electrode active material powder in this embodiment. Hereinafter, the "method for producing a positive electrode active material powder in this embodiment" may be abbreviated as "this production method." This production method includes "(a) crushing," "(b) mixing," and "(c) heat treatment."
[0051] (a) Disintegrate The present manufacturing method includes preparing a pulverized powder by pulverizing LNO. A new surface may be generated by pulverizing LNO. That is, the pulverized powder includes a new surface. The LNO may be prepared by any method. For example, the LNO may be synthesized by a coprecipitation method. For example, the LNO may be synthesized by the following procedure.
[0052] Sulfates such as Ni are prepared. An acidic aqueous solution is formed by dissolving the sulfates in water. For example, an acidic aqueous solution can be formed by dissolving nickel sulfate, cobalt sulfate, and manganese sulfate in water. For example, a neutralization reaction can occur by dropping an alkaline aqueous solution into the acidic aqueous solution. The alkaline aqueous solution may contain, for example, an NaOH aqueous solution and an ammonia solution. A precipitate can be formed by the neutralization reaction. The precipitate is considered to contain a composite hydroxide (precursor). A dried product is formed by washing and drying the precipitate. A mixture is formed by mixing the dried product with a lithium compound. The lithium compound may contain, for example, Li2CO3, LiOH, etc. The mixture is subjected to a heat treatment. The heat treatment can also be called "calcination". The heat treatment temperature may be, for example, 500 to 1000°C. The heat treatment time may be, for example, 5 to 30 hours. LNO is synthesized in the above manner.
[0053] In the present manufacturing method, any disintegration device may be used. For example, a jet mill or the like may be used. For example, the disintegration process may be performed under an inert gas atmosphere. For example, the disintegration process may be performed under a nitrogen atmosphere. By performing the disintegration process under an inert gas atmosphere, the Li4WO5 phase tends to be easily generated. For example, the disintegrated powder may be further subjected to classification, granulation, and the like.
[0054] 《(b) Mixture》 The present manufacturing method includes preparing a mixture by mixing the crushed powder with WO3. This allows WO3 to adhere to at least a part of the newly created surface generated by crushing. WO3 is a precursor of LWO. The D50 of WO3 may be smaller than the D50 of the crushed powder, for example. The D50 of WO3 may be, for example, 0.1 to 2.7 μm, or 0.5 to 1 μm. The amount of WO3 to be blended may be, for example, 0.1 to 2 parts by substance, or 0.5 to 1 part by substance, relative to 100 parts by substance of LNO. Parts by substance are also referred to as "molar parts".
[0055] The mixing method is arbitrary. For example, wet mixing or dry mixing may be performed. For example, a ball mill, a mechanofusion device, etc. may be used.
[0056] (c) Heat Treatment The present manufacturing method includes manufacturing a positive electrode active material powder by subjecting the mixture to a heat treatment. The heat treatment may cause active Li on the nascent surface to react with WO3. This is believed to produce LWO. In the present manufacturing method, any heat treatment device may be used. For example, an electric furnace, a muffle furnace, or the like may be used. The heat treatment temperature may be, for example, 200 to 700°C. The heat treatment time may be, for example, 1 to 10 hours.
[0057] The Li4WO5 phase tends to be generated in Li-rich reaction systems. In this manufacturing method, various conditions are combined so that the composition ratio of the Li4WO5 phase in LWO is 30% or more. Factors that affect the composition ratio of the Li4WO5 phase include, for example, the "Ni ratio of LNO," "crushing level (D50 after crushing)," "amount of WO3 blended," "heat treatment temperature," and "heat treatment time."
[0058] <Lithium-ion battery> FIG. 2 is a conceptual diagram of a lithium ion battery in this embodiment. Hereinafter, the "lithium ion battery in this embodiment" may be abbreviated as "this battery." This battery 100 may be a liquid battery, a polymer battery, or an all-solid-state battery. That is, this battery 100 may contain a liquid electrolyte (electrolytic solution), a gel electrolyte, or a solid electrolyte.
[0059] The battery 100 may include an exterior body (not shown). The exterior body may house the power generating element 150. The exterior body may have any shape. The exterior body may be, for example, a pouch made of a metal foil laminate film, or a case made of metal. The case may be, for example, cylindrical or rectangular.
[0060] This battery 100 includes a power generation element 150. The power generation element 150 includes a positive electrode 110, a separator 130, a negative electrode 120, and an electrolyte (not shown). The power generation element 150 may also be referred to as an electrode body, an electrode group, etc. The power generation element 150 may be, for example, a laminated type or a wound type.
[0061] 《Positive Electrode》 The positive electrode 110 may be, for example, sheet-shaped. The positive electrode 110 may include, for example, a positive electrode current collector and a positive electrode active material layer. The positive electrode current collector may include, for example, Al foil or the like. The positive electrode active material layer may be disposed on the surface of the positive electrode current collector. The positive electrode active material layer contains the aforementioned positive electrode active material powder. As long as the positive electrode 110 contains the aforementioned positive electrode active material powder, the positive electrode 110 may further contain additional positive electrode active material powder. For example, the positive electrode active material layer may further contain LiFePO4 or the like. In addition to the positive electrode active material powder, the positive electrode active material layer may further contain a conductive material, a binder, etc. The positive electrode active material layer may contain, for example, acetylene black (AB), polyvinylidene fluoride (PVDF), etc.
[0062] 《Negative Electrode》 The negative electrode 120 may be, for example, sheet-shaped. The negative electrode 120 may include, for example, a negative electrode current collector and a negative electrode active material layer. The negative electrode current collector may include, for example, Cu foil or the like. The negative electrode active material layer may be disposed on the surface of the negative electrode current collector. The negative electrode active material layer contains a negative electrode active material. The negative electrode active material may be powdery or sheet-shaped. The negative electrode active material may include, for example, natural graphite, artificial graphite, soft carbon, hard carbon, Si, SiO x (0 < x < 2), Si-based alloy, Sn, SnO x (0 < x < 2), Li, Li-based alloy, and Li4Ti5O 12 and may contain at least one selected from the group consisting of. The negative electrode active material layer may further contain a conductive material, a binder, etc. The negative electrode active material layer may contain, for example, vapor-grown carbon fiber (VGCF), carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), etc.
[0063] <Separator> The separator 130 is interposed between the positive electrode 110 and the negative electrode 120. The separator 130 separates the positive electrode 110 from the negative electrode 120. In the case of a liquid battery, the separator 130 may include, for example, a porous sheet made of resin. In the case of an all-solid-state battery, the separator 130 may include, for example, a solid electrolyte layer.
[0064] 《Electrolytes》 The electrolyte can form an ion conduction path. The liquid electrolyte includes, for example, a lithium salt and a solvent. The lithium salt may include, for example, LiPF6 or the like. The solvent may include, for example, ethylene carbonate (EC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC) or the like. The solid electrolyte may include, for example, a sulfide (Li3PS4 or the like). EXAMPLES
[0065] <Sample preparation> Positive electrode active material powders No. 1 to 15 were produced as follows (see Table 1 below). Hereinafter, for example, "positive electrode active material powder No. 1" may be abbreviated as "No. 1".
[0066] No.1~4 Nickel sulfate, cobalt sulfate, and manganese sulfate were dissolved in water to prepare an acidic aqueous solution. The compounding ratio (ratio of amounts of substances) of the solutes was "nickel sulfate / cobalt sulfate / manganese sulfate = 5 / 2 / 3". The ratio of amounts of substances is also written as "molar ratio". A precipitate was formed by dropping an aqueous NaOH solution and an aqueous ammonia solution into the acidic aqueous solution. The precipitate contained a composite hydroxide. A dried product was formed by washing and drying the precipitate. A mixture was formed by mixing the dried product with Li2CO3. The mixture was subjected to heat treatment. The heat treatment temperature was 870°C. The heat treatment time was 15 hours. As a result, LNO was synthesized. No. 1 to 4 (crushed powder) were produced by subjecting LNO to a crushing process and a classification process. No. 1 to 4 have different crushing conditions.
[0067] No.5 Except for the change in the solute ratio (substance ratio) to "nickel sulfate / cobalt sulfate / manganese sulfate = 6 / 2 / 2," LNO was synthesized in the same manner as No. 1. No. 5 was produced by subjecting LNO to crushing and classification processes.
[0068] No.6 LNO was synthesized in the same manner as No. 1, except that the solute mixing ratio (substance ratio) was changed to "nickel sulfate / cobalt sulfate / manganese sulfate = 8 / 1 / 1." No. 6 was produced by subjecting LNO to crushing and classification processes.
[0069] No.7 A mixture was prepared by mixing No.1 LNO (crushed powder) and WO3 (D50=1μm). The compounding ratio (ratio of substance amounts) was "LNO / WO3=100 / 0.5". The mixture was subjected to heat treatment. The heat treatment temperature was 500°C. The heat treatment time was 4 hours. As a result, a positive electrode active material powder was produced.
[0070] No.8-10, 14 and 15 Positive electrode active material powders were prepared in the same manner as No. 7, except that the LNO (crushed powder) of No. 1 was replaced by the LNO (crushed powder) of No. 2 to No. 6.
[0071] No.11 The Li on the newly formed surface was reduced by washing the LNO (crushed powder) of No. 4 with water. A positive electrode active material powder was produced in the same manner as No. 10, except that the crushed powder after washing with water was mixed with WO3.
[0072] No.12 A positive electrode active material powder was prepared in the same manner as No. 10, except that the compounding ratio (ratio of substances) of LNO and WO3 was changed to "LNO / WO3 = 100 / 0.75".
[0073] No.13 A positive electrode active material powder was prepared in the same manner as No. 10, except that the compounding ratio (ratio of substances) of LNO and WO3 was changed to "LNO / WO3 = 100 / 1."
[0074] <Evaluation> The composition ratio of the Li4WO5 phase and the Li2WO4 phase was measured for each positive electrode active material powder. The measurement results are shown in Tables 1 to 4 below.
[0075] Test batteries for evaluation were prepared. The test battery configuration was as follows:
[0076] positive electrode Positive electrode active material powder: Samples obtained above (No. 1 to 15) Conductive material: AB Binder: PVDF
[0077] negative electrode Negative electrode active material: natural graphite Binder: CMC, SBR
[0078] Separator: Porous sheet (thickness 24 μm) Electrolyte: Electrolyte [LiPF6 (1mol / L), EC+DMC+EMC]
[0079] A high-temperature storage test was carried out. The storage temperature was 70° C. The capacity retention rate after storage was measured. The capacity retention rate indicates the ratio of the capacity after storage to the capacity before storage. The measurement results are shown in Tables 1 to 4 below.
[0080] <Results and Discussion>
[0081] [Table 1]
[0082] [Table 2]
[0083] In Table 2 above, the smaller the D50 after crushing, the higher the composition ratio of the Li4WO5 phase. This is thought to be because the smaller the D50 after crushing, the more newly formed surfaces there are, and the more likely a Li-rich reaction system is formed. The higher the composition ratio of the Li4WO5 phase, the greater the effect of improving the capacity retention rate.
[0084] [Table 3]
[0085] In Table 3 above, after crushing, active Li is reduced by washing with water, and as a result, the composition ratio of the Li4WO5 phase tends to decrease (No. 11).
[0086] In Table 3 above, the coverage rate increases as the amount of WO3 increases (No. 10, 12, 13). On the other hand, the composition ratio of the Li4WO5 phase gradually decreases. This is thought to be because the quantitative balance between Li and WO3 changes as the amount of WO3 increases. When the coverage rate exceeds 22%, the effect of improving the capacity retention rate becomes smaller. It is thought that the frequency of formation of the Li4WO5 phase decreases due to a shortage of Li.
[0087] [Table 4]
[0088] In Table 4 above, when the Ni ratio of LNO is 0.5 or more, the effect of improving the capacity retention rate is shown to be independent of the Ni ratio. [Explanation of symbols]
[0089] 100 battery, 110 positive electrode, 120 negative electrode, 130 separator, 150 power generating element.
Claims
1. Having a D50 of 1.2 to 2.7 μm, A lithium nickel composite oxide; Lithium tungsten composite oxide Including, In the lithium nickel composite oxide, the ratio of the amount of Ni to the total amount of atoms other than Li and oxygen is 0.5 or more; the lithium tungsten composite oxide is attached to at least a portion of a surface of the lithium nickel composite oxide, The lithium tungsten composite oxide contains 54% or more of a Li 4 WO 5 phase and the remainder of a Li 2 WO 4 phase, The composition ratio of the Li 4 WO 5 phase and the Li 2 WO 4 phase is determined by analysis of an XAFS spectrum. Cathode active material powder.
2. The lithium nickel composite oxide has the formula (1): Li (1+x) Ni y Co z Mn (1-y-z) M a O (2-b) C b …(1) It is expressed as In the formula (1), x, y, z, a, and b satisfy the relationships: 0≦x≦0.7, 0.5≦y≦0.8, 0.1≦z≦0.2, 0≦a≦0.1, and 0≦b≦0.5; M is at least one selected from the group consisting of Zr, Mo, W, Mg, Ca, Na, Fe, Cr, Zn, Si, Sn, Al, and Ag; C is at least one selected from the group consisting of F, Cl, and Br; The positive electrode active material powder according to claim 1 .
3. a coverage rate of the surface of the lithium nickel composite oxide by the lithium tungsten composite oxide is 11 to 25%, The coverage is calculated by the formula (2): θ=r w / (r w +r Ni +r Co +r Mn ) …(2) It is calculated by In the formula (2), θ represents the coverage ratio, r w , r Ni , r Co , and r Mn is measured by X-ray photoelectron spectroscopy, r w indicates the atomic ratio of W, r Ni represents the atomic ratio of Ni, r Co indicates the atomic ratio of Co, r Mn indicates the atomic ratio of Mn, The positive electrode active material powder according to claim 2 .
4. The positive electrode active material powder according to any one of claims 1 to 3 is included. Positive electrode.
5. The positive electrode according to claim 4, Lithium-ion battery.
6. A method for producing a positive electrode active material powder according to any one of claims 1 to 3, comprising the steps of: (a) preparing a pulverized powder including a fresh surface by pulverizing a lithium nickel composite oxide under an inert gas atmosphere; (b) Mixing the crushed powder with WO 3 preparing a mixture by mixing (c) subjecting the mixture to a heat treatment to produce a positive electrode active material powder; Including, The crushed powder is mixed with WO 3 without being washed with water. A method for producing a positive electrode active material powder.
Citation Information
Patent Citations
Positive electrode active material for nonaqueous electrolyte secondary battery and manufacturing method for the same, and nonaqueous electrolyte secondary battery using the positive electrode active material
JP2016111000A
Positive electrode active material for lithium ion secondary battery and method of manufacturing the same
JP2020166931A
Non-aqueous electrolyte secondary battery
JP2021018895A
Positive electrode active substance for non-aqueous electrolyte secondary battery, and method for producing same
WO2016140207A1