Negative pole piece, electrochemical device and electronic equipment

A double-layer negative electrode structure with silicon and graphite layers, using chemically bonded binders, addresses the instability of silicon-based electrodes, enhancing cycle stability and energy density in lithium-ion batteries.

CN119069655APending Publication Date: 2024-12-03HUAWEI TECH CO LTD
View PDF 0 Cites 7 Cited by

Patent Information

Application Number
CN202310630263.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Current lithium-ion batteries face limitations due to the low specific capacity of graphite negative electrodes and the instability of silicon-based electrodes, leading to issues such as volume change, structural damage, and poor cycle performance when used in high-energy-density applications.

Method used

A double-layer negative electrode structure is designed with a silicon-based active material layer between a graphite-based active material layer and a current collector, using binders with acidic and active groups to form chemical bonds, enhancing interface compatibility and reducing volume expansion and side reactions.

Benefits of technology

The solution improves cycle stability, reduces interface issues, and enhances the bonding performance between layers, resulting in improved electrochemical performance and energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069655A_ABST
    Figure CN119069655A_ABST
Patent Text Reader

Abstract

The invention relates to a negative electrode plate, an electrochemical device and electronic equipment. The negative electrode plate provided by the invention comprises a negative electrode current collector and a negative electrode active layer arranged on at least one side of the negative electrode current collector, the negative electrode active layer comprises a first active material layer and a second active material layer which are stacked, and the first active material layer is located between the second active material layer and the negative electrode current collector; the first active material layer comprises a silicon-based negative electrode active material and a first binder containing an acidic group; the second active material layer comprises a graphite negative electrode active material and a second binder containing a first active group, and chemical bond connection is formed between the first active group and the acidic group. According to the negative pole piece, the comprehensive specific capacity of the negative pole piece can be improved, the cycling stability can be improved, the volume expansion of the pole piece is inhibited, and the electrochemical performance of an electrochemical device is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of electrochemical technology, and in particular to a negative electrode sheet, an electrochemical device and an electronic device. Background Art

[0002] Lithium-ion batteries have been widely used in electronic products, electric vehicles, and large-scale energy storage due to their high energy density, long service life, and low self-discharge rate. Currently, commercial lithium-ion batteries mainly use graphite as the negative electrode material. The theoretical capacity of graphite material is 372mAh / g, which limits the further improvement of battery energy density. In order to solve the problem that the current graphite negative electrode has a low specific capacity and cannot meet the needs of high-energy-density lithium-ion batteries, the use of silicon-based, phosphorus-based and other negative electrode materials with higher theoretical capacity is currently a more promising solution. However, since the performance of pure silicon negative electrode such as cycle stability and first coulomb efficiency cannot meet commercial needs, the industry currently generally adopts a negative electrode strategy that uses a mixture of graphite + silicon-based negative electrode materials.

[0003] At present, graphite + silicon-based negative electrodes are directly mixed together when the slurry is dispersed. Although some disadvantages of silicon negative electrodes are avoided to a certain extent, this composite negative electrode prepared by direct mixing still has certain problems. First, the stress accumulation caused by the volume change of silicon particles in this conventional composite negative electrode when lithium is extracted and inserted will inhibit the embedding of lithium ions into graphite, resulting in the decline of graphite capacity. Secondly, the large volume change of randomly dispersed silicon particles when lithium is extracted and inserted will also destroy the overall structure of the electrode and affect the cycle performance of the electrode. In addition, due to the different surface properties of silicon and graphite, this difference will also cause problems with the bonding of the binder, leading to problems such as powder loss and cracking.

[0004] Therefore, how to prepare a negative electrode with high capacity, low expansion and high cycle stability is still one of the current research focuses. Summary of the invention

[0005] The purpose of the present application is to provide a negative electrode plate, an electrochemical device and an electronic device. By stacking two different negative electrode active materials in layers, the expansion of the two layers of negative electrode materials can be suppressed, the rate performance of the negative electrode plate can be comprehensively improved, and the interface problem between the two layers of negative electrode materials can be solved, the connection stability of the two layers of negative electrode materials can be improved, the problems of plate delamination, cracking and powder loss can be avoided, the contact resistance can be improved, and the electrochemical performance of the electrochemical device can be comprehensively improved.

[0006] In a first aspect, the present application provides a negative electrode plate, the negative electrode plate comprising:

[0007] A negative electrode current collector, a negative electrode active layer disposed on at least one side of the negative electrode current collector;

[0008] The negative electrode active layer comprises a first active material layer and a second active material layer stacked together, wherein the first active material layer is located between the second active material layer and the negative electrode current collector;

[0009] The first active material layer includes a silicon-based negative electrode active material and a first binder containing an acidic group;

[0010] The second active material layer includes a graphite-based negative electrode active material and a second binder containing a first active group, wherein the first active group is chemically bonded to the acidic group.

[0011] In some embodiments, the first reactive group reacts with the acidic group to form at least one of a carboxylate group, a sulfonate group, a phosphate group, an amide group, an ether group, a carbamate group, or a urea group.

[0012] In some embodiments, the acidic group includes at least one of a carboxyl group, a sulfonic acid group, and a phosphate group.

[0013] In some embodiments, the first reactive group includes at least one of a hydroxyl group, an amino group, an epoxy group, an isocyanate group, and an aziridine group.

[0014] In some embodiments, the mass content of the acidic groups in the first active material layer is 0.0001% to 5%.

[0015] In some embodiments, the mass content of the first active group in the second active material layer is 0.0001% to 5%.

[0016] In some embodiments, the first active material layer further includes a first conductive agent, the mass content of the first conductive agent in the first active material layer is A1%; the second active material layer further includes a second conductive agent, the mass content of the first conductive agent in the first active material layer is A2%, and A1>A2.

[0017] In some embodiments, the mass content of the first binder in the first active material layer is B1%; the mass content of the second binder in the second active material layer is B2%, and B1>B2.

[0018] In some embodiments, the mass content of the first binder in the first active material layer is 3% to 10%.

[0019] In some embodiments, the first binder includes at least one of acrylic copolymers containing acidic groups, acrylate copolymers containing acidic groups, acrylonitrile copolymers containing acidic groups, polyvinyl alcohol containing acidic groups and derivatives thereof, polyimide containing acidic groups and derivatives thereof, epoxy resin copolymers containing acidic groups, nitrile rubber containing acidic groups, and hydrogenated nitrile rubber containing acidic groups.

[0020] In some embodiments, the first active material layer further includes a coupling agent; the mass content of the coupling agent in the first active material layer is 0% to 1%.

[0021] In some embodiments, the coupling agent includes at least one of a silane coupling agent, an aziridine coupling agent, an epoxy coupling agent, an isocyanate coupling agent, and a polyol coupling agent.

[0022] In some embodiments, the mass content of the second binder in the second active material layer is 0.5% to 2%.

[0023] In some embodiments, the second binder includes at least one of a polyurethane emulsion containing a first active group, a styrene-butadiene emulsion containing a first active group, an acrylate emulsion containing a first active group, a styrene-acrylic emulsion containing a first active group, an ethylene-propylene emulsion containing a first active group, and an EVA emulsion containing a first active group.

[0024] In some embodiments, the second active material layer further includes a dispersant; the mass content of the dispersant in the second active material layer is 0.5% to 2%.

[0025] In some embodiments, the dispersant includes at least one of sodium carboxymethylcellulose, lithium carboxymethylcellulose, cellulose nanofibers, sodium alginate, chitosan, guar gum, carrageenan, and gelatin.

[0026] In some embodiments, the mass content of the first conductive agent in the first active material layer is A1%, 2≤A1≤10.

[0027] In some embodiments, the mass content of the second conductive agent in the second active material layer is A2%, 0.1≤A2≤1.5.

[0028] In some embodiments, the first conductive agent and the second conductive agent each independently include at least one of conductive carbon black, carbon nanotubes, graphene, conductive graphite, and carbon fiber.

[0029] In some embodiments, the silicon-based negative electrode active material includes at least one of elemental silicon, silicon-oxygen compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys.

[0030] In some embodiments, the graphite-based negative electrode active material includes at least one of natural graphite, artificial graphite and carbon material.

[0031] In some embodiments, the thickness of the negative electrode current collector is 1 μm to 50 μm.

[0032] In some embodiments, the thickness of the negative electrode active layer is 10 μm to 100 μm.

[0033] In some embodiments, the negative electrode current collector includes at least one of copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, and a polymer substrate coated with a conductive metal.

[0034] In some embodiments, a conductive coating is further provided on the surface of the negative electrode current collector, and the conductive coating includes at least one of conductive carbon black, carbon nanotubes, graphene, conductive graphite and carbon fiber.

[0035] In some embodiments, the thickness ratio of the first active material layer to the second active material layer is R, 1≤R≤15.

[0036] In a second aspect, the present application provides an electrochemical device, which includes the negative electrode sheet described in the first aspect.

[0037] In a third aspect, the present application provides an electronic device, wherein the electronic device comprises the above-mentioned electrochemical device.

[0038] Compared with the prior art, this application has at least the following beneficial effects:

[0039] The negative electrode plate provided by the present application is formed by forming a first active material layer and a second active material layer stacked with a graphite-based negative electrode active material and a silicon-based negative electrode active material, respectively, and the first active material layer containing the silicon-based negative electrode active material is located between the second active material layer and the negative electrode current collector to form a double-layer structure composite negative electrode plate. On the one hand, since the graphite-based negative electrode active material and the silicon-based negative electrode active material are separated from each other, the mutual crosstalk caused by the volume change of different active materials during the charge and discharge cycle can be avoided, and the damage to the graphite material structure caused by the expansion of the silicon-based material during the charge and discharge process can be avoided. On the other hand, the first active material layer is closer to the negative electrode current collector, which can effectively reduce its side reaction with the electrolyte, avoid the rapid performance attenuation and interface layer thickening caused by the direct contact of the silicon-based negative electrode active material with the electrolyte, and improve the cycle performance of the plate.

[0040] Secondly, in order to solve the interface problems between the double active layers and the interface problems between the first active material layer and the negative electrode current collector, a first binder containing an acidic group is introduced into the first active material layer, and a second binder containing a first active group is introduced into the second active material layer. The first active group and the acidic group can react chemically with each other, so that a chemical bond is formed between the first active group and the acidic group, thereby improving the interface compatibility and affinity, improving the bonding performance between the interfaces, and avoiding the problems of electrode demolding, cracking, and powder falling. In addition, the acidic groups in the first active material layer can also be coordinated and complexed with the metal ions on the negative electrode current collector, thereby enhancing the bonding performance between the negative electrode current collector and the negative electrode active layer and improving the contact resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] The present application is further described below in conjunction with the accompanying drawings and embodiments.

[0042] Figure 1 A schematic diagram of the system structure of the lithium-ion battery provided in this application;

[0043] Figure 2 A schematic diagram of the structure of the negative electrode provided in this application;

[0044] Figure 3 A cycle comparison curve diagram of the lithium ion battery provided by Example 1 of the present application and Comparative Examples 1 to 2;

[0045] Figure 4a This is a SEM image of the negative electrode active layer of the negative electrode sheet provided in Example 1 of the present application after cycling;

[0046] Figure 4b This is a SEM image of the negative electrode active layer of the negative electrode sheet provided in Comparative Example 1 of the present application after cycling;

[0047] Figure 4c This is a SEM image of the negative electrode active layer of the negative electrode sheet provided in Comparative Example 2 of the present application after cycling;

[0048] Figure 4d This is a cross-sectional SEM image of the negative electrode active layer of the negative electrode sheet provided in Example 1 of the present application after cycling;

[0049] Figure 4e This is a cross-sectional SEM image of the negative electrode active layer of the negative electrode sheet provided in Comparative Example 1 of the present application after cycling;

[0050] Figure 4f This is a cross-sectional SEM image of the negative electrode active layer of the negative electrode sheet provided in Comparative Example 2 of the present application after cycling;

[0051] Figure 2 middle:

[0052] 10- negative electrode current collector;

[0053] 20- first active material layer;

[0054] 30 - Second active material layer. DETAILED DESCRIPTION

[0055] In order to better understand the technical solution of the present application, the embodiments of the present application are described in detail below with reference to the accompanying drawings.

[0056] It should be clear that the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present application.

[0057] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0058] It should be understood that the term "and / or" used in this article is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0059] Figure 1 A schematic diagram of a lithium-ion battery provided for this application, such as Figure 1 As shown, it includes a positive electrode sheet, a negative electrode sheet, an electrolyte, a diaphragm and a corresponding circuit, wherein during the charging process, under the action of an external circuit, lithium ions are deintercalated from the positive electrode active material and embedded into the negative electrode through the electrolyte diaphragm, while the positive electrode loses electrons and flows out from the external circuit through the current collector; the discharge process is the opposite, lithium ions are deintercalated from the negative electrode back to the positive electrode, while electrons move from the negative electrode to the positive electrode through the external circuit to release energy externally. The electrolyte is the carrier for lithium ions to be transmitted between the positive and negative electrodes, and the ion-conducting but electronically insulating diaphragm ensures the migration of lithium ions while separating the positive and negative electrodes to prevent short circuits.

[0060] The positive and negative active materials are the main parts of lithium batteries that perform energy storage functions, and determine the energy density, cycle performance and safety performance of the battery cell. After determining the positive electrode material system, the capacity of the negative electrode material is crucial to improving the energy density of the entire battery cell. Using silicon-based, phosphorus-based and other negative electrode materials with high theoretical capacity to prepare batteries is currently the most promising solution. While maintaining the high capacity of such negative electrode materials, improving their cycle stability, reducing volume expansion, and improving rate performance through electrode structure design will help improve the capacity, life, safety and fast charging capabilities of current lithium batteries, improve the integration of electronic products, electric vehicles, and energy storage devices, and enhance product competitiveness.

[0061] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer located on the surface of the positive electrode current collector, and the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer located on the surface of the negative electrode current collector.

[0062] Battery energy density is positively correlated with the negative electrode gram capacity. Compared with graphite materials (theoretical capacity 372mAh / g), the use of silicon-based negative electrode materials (Si~4200mAh / g) or phosphorus-based negative electrode materials (P~2760mAh / g) with higher gram capacity is undoubtedly the preferred route to improve battery energy density. However, silicon-based negative electrode materials undergo huge volume changes (200%~300%) during the battery cycle. The dramatic volume changes cause the volume of the negative electrode sheet to expand greatly, and the destruction and crushing of the negative electrode active material particles cause the battery capacity to decay rapidly. At present, the industry generally adopts a negative electrode strategy that uses a mixture of graphite + silicon-based negative electrode materials.

[0063] At present, graphite + silicon-based negative electrodes are directly mixed together when the slurry is dispersed. Although some disadvantages of silicon negative electrodes are avoided to a certain extent, this composite negative electrode prepared by direct mixing still has certain problems. First, the stress accumulation caused by the volume change of silicon particles in this conventional composite negative electrode when lithium is extracted and inserted will inhibit the embedding of lithium ions into graphite, resulting in the decline of graphite capacity. Secondly, the large volume change of randomly dispersed silicon particles when lithium is extracted and inserted will also destroy the overall structure of the electrode and affect the cycle performance of the electrode. In addition, due to the different surface properties of silicon and graphite, this difference will also cause problems with the bonding of the binder, resulting in problems such as powder falling and cracking. This conventional composite negative electrode has poor cycle stability and rapid capacity decay.

[0064] Therefore, how to prepare a negative electrode with high capacity, low expansion and high cycle stability is still one of the current research focuses.

[0065] Based on this, in the first aspect, the present application provides a negative electrode sheet, such as Figure 2 As shown, the negative electrode plate includes:

[0066] A negative electrode current collector 10, a negative electrode active layer disposed on at least one side of the negative electrode current collector;

[0067] The negative electrode active layer includes a first active material layer 20 and a second active material layer 30 stacked together, wherein the first active material layer 20 is located between the second active material layer 30 and the negative electrode current collector 10;

[0068] The first active material layer 20 includes a silicon-based negative electrode active material and a first binder containing an acidic group;

[0069] The second active material layer 30 includes a graphite-based negative electrode active material and a second binder containing a first active group, wherein the first active group is chemically bonded to the acidic group.

[0070] In the above scheme, the graphite-based negative electrode active material and the silicon-based negative electrode active material are respectively formed into a first active material layer and a second active material layer which are stacked, and the first active material layer containing the silicon-based negative electrode active material is located between the second active material layer and the negative electrode current collector, so as to form a double-layer structure composite negative electrode plate. On the one hand, since the graphite-based negative electrode active material and the silicon-based negative electrode active material are separated from each other, the mutual crosstalk caused by the volume change of different active materials during the charge and discharge cycle can be avoided, and the damage to the graphite material structure caused by the expansion of the silicon-based material during the charge and discharge process can be avoided. On the other hand, the first active material layer is closer to the negative electrode current collector, which can effectively reduce its side reaction with the electrolyte, avoid the problems such as rapid performance attenuation and thickening of the interface layer caused by the direct contact of the silicon-based negative electrode active material with the electrolyte, and improve the cycle performance of the plate.

[0071] Secondly, in order to solve the interface problems between the double active layers and the interface problems between the first active material layer and the negative electrode current collector, a first binder containing an acidic group is introduced into the first active material layer, and a second binder containing a first active group is introduced into the second active material layer. The first active group and the acidic group can react chemically with each other, so that a chemical bond is formed between the first active group and the acidic group, thereby improving the interface compatibility and affinity, improving the bonding performance between the interfaces, and avoiding the problems of electrode demolding, cracking, and powder falling. In addition, the acidic groups in the first active material layer can also be coordinated and complexed with the metal ions on the negative electrode current collector, thereby enhancing the bonding performance between the negative electrode current collector and the negative electrode active layer and improving the contact resistance.

[0072] The negative electrode current collector 10 is generally a structure or part for collecting current, and the negative electrode current collector 10 can be any material in the art suitable for being used as a negative electrode current collector 10 for lithium-ion batteries. Exemplarily, the negative electrode current collector 10 can include but is not limited to metal foil, and more specifically can include but is not limited to at least one of copper foil, nickel foil, stainless steel foil, titanium foil, foamed nickel, foamed copper, and a polymer substrate covered with a conductive metal.

[0073] In some embodiments, the negative electrode current collector 10 is selected from copper foil, and the thickness of the negative electrode current collector 10 is 1 μm to 50 μm, specifically 1 μm, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 45 μm or 50 μm, etc., and of course, it can also be other values ​​within the above range, which is not limited here. Preferably, the thickness of the negative electrode current collector 10 is 3 μm to 10 μm.

[0074] In some embodiments, the surface of the negative electrode current collector 10 is further provided with a conductive coating (not shown), and the conductive coating is arranged between the negative electrode current collector and the negative electrode active layer. The conductive coating includes at least one of conductive carbon black, carbon nanotubes, graphene, conductive graphite and carbon fiber. The thickness of the conductive layer is 0.2μm to 2.0μm, and can be specifically 0.2μm, 0.4μm, 0.6μm, 0.7μm, 0.8μm, 0.9μm, 1.0μm, 1.2μm, 1.3μm, 1.5μm or 2.0μm, etc., and of course it can also be other values ​​within the above range, which are not limited here. When the thickness of the conductive layer is too large, the DC impedance of the battery increases; when the thickness of the conductive layer is too small, the rate performance of the battery is affected. Preferably, the thickness of the conductive layer is 1.0μm to 2.0μm. It can be understood that the provision of the conductive coating can improve the conductivity between the negative electrode current collector and the negative electrode active layer and reduce the contact resistance.

[0075] Furthermore, the negative electrode active layer includes a first active material layer 20 and a second active material layer 30 which are stacked.

[0076] In some embodiments, the first active material layer 20 includes a silicon-based negative electrode active material and a first binder containing an acidic group. The silicon-based negative electrode active material includes at least one of elemental silicon, a silicon-oxygen compound, a silicon-carbon compound, a silicon-nitrogen compound, and a silicon alloy. For example, the silicon-oxygen compound may be silicon monoxide. The silicon alloy may be a silicon-magnesium alloy, a silicon-lithium alloy, and the like.

[0077] In some embodiments, the silicon-carbon composite material can be a silicon-carbon composite material obtained by carbon coating a silicon material, a silicon-carbon composite material obtained by sintering a silicon material, a silicon-carbon composite material obtained by ball milling a silicon material and a carbon material, or a silicon-carbon composite material obtained by chemical vapor deposition a silicon material and a carbon material, etc. It can also be a composite material of silicon oxide and carbon material, which is not limited here. In the present application, a silicon-based negative electrode active material with a gram capacity greater than 600 mAh / g can be selected to increase the specific capacity of the negative electrode sheet.

[0078] In some other embodiments, the first active material layer 20 may further include a phosphorus-based material, the phosphorus-based material including at least one of elemental phosphorus and a phosphorus-carbon composite. For example, the elemental phosphorus includes at least one of red phosphorus, black phosphorus, purple phosphorus or blue phosphorus. For example, the phosphorus-carbon composite is prepared by compounding elemental phosphorus and a carbon material by ball milling or vapor deposition, and the carbon material includes at least one of graphite, carbon nanotubes, porous carbon, hard carbon, soft carbon or graphene, which is not limited here.

[0079] It can be understood that the active material in the first active material layer is a silicon-based negative electrode active material or a phosphorus-based material with a relatively high theoretical capacity, which can improve the comprehensive specific capacity of the negative electrode sheet.

[0080] In the present application, the first active material layer 20 includes a first binder and a first conductive agent. Specifically, the first binder contains an acidic group, and the acidic group includes at least one of a carboxyl group, a sulfonic acid group, and a phosphate group. It can be understood that the acidic group is easy to chemically react with the first active group in the second active material layer 30, thereby improving the bonding between the two layers.

[0081] In some embodiments, the mass content of the acidic group in the first active material layer is 0.0001% to 5%, and can be specifically 0.0001%, 0.0005%, 0.001%, 0.002%, 0.005%, 0.01%, 0.05%, 0.1%, 0.5%, 0.8%, 0.9%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%, etc., and of course it can also be other values ​​within the above range, which is not limited here.

[0082] The first conductive agent may be at least one of conductive carbon black, carbon nanotubes, graphene, conductive graphite and carbon fiber. Specifically, the carbon nanotubes may be single-walled carbon nanotubes (abbreviated as SWCNT), multi-walled carbon nanotubes (abbreviated as MWCNT), etc., which are not limited here.

[0083] In some embodiments, the mass content of the first conductive agent in the first active material layer is A1%, 2≤A1≤10. For example, the mass content of the first conductive agent may be 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%, etc., and may also be other values ​​within the above range, which is not limited here.

[0084] It can be understood that the silicon-based negative electrode active material in the first active material layer 20 has a large volume expansion during the charge and discharge process. In order to suppress the volume expansion, a high-strength first binder is added to the first active material layer to improve the bonding stability between the first active material layer and the negative electrode current collector and the second active material layer. In addition, the first binder having an acidic group can also undergo ion coordination and complexation with metal ions on the surface of the negative electrode current collector, and can also enhance the bonding force between the negative electrode current collector and the first active material layer.

[0085] In some embodiments, the first binder may be a polymer binder material, which may have high strength and anti-expansion properties, good adhesion to silicon-based negative electrode active materials, stable adhesion to negative electrode current collectors, and high peeling force. Exemplarily, the first binder includes at least one of an acrylic copolymer containing an acidic group, an acrylate copolymer containing an acidic group, an acrylonitrile copolymer containing an acidic group, polyvinyl alcohol containing an acidic group and its derivatives, polyimide containing an acidic group and its derivatives, epoxy resin copolymer containing an acidic group, nitrile rubber containing an acidic group, and hydrogenated nitrile rubber containing an acidic group.

[0086] In some embodiments, the mass content of the first binder in the first active material layer is B1%, specifically 3% to 10%, for example 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%, etc., and of course it can also be other values ​​within the above range, which is not limited here.

[0087] In other embodiments, the first active material layer further includes a coupling agent, which is mainly a small molecule compound with multiple functional groups, which can undergo intermolecular crosslinking with the polymer material in the first binder and can also improve the coupling effect between the polymer material and the silicon-based active material. Specifically, the coupling agent includes at least one of a silane coupling agent, an aziridine coupling agent, an epoxy coupling agent, an isocyanate coupling agent, and a polyol coupling agent.

[0088] In some embodiments, the mass content of the coupling agent in the first active material layer is 0% to 1%, and can be 0%, 0.1%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9% or 1%, etc., and can also be other values ​​within the above range, which is not limited here.

[0089] In some embodiments, the second active material layer 30 includes a graphite-based negative electrode active material and a second binder containing a first active group, wherein the first active group is chemically bonded to the acidic group.

[0090] Specifically, the first reactive group reacts with the acidic group to form at least one of a carboxylate group, a sulfonate group, a phosphate group, an amide group, an ether group, a carbamate group or a urea group.

[0091] In some embodiments, the graphite-based negative electrode active material includes at least one of natural graphite, artificial graphite and a carbon material. For example, the carbon material may be carbon black, carbon fiber, carbon nanotube, graphene, hard carbon, etc., which are not limited here.

[0092] In some embodiments, the graphite negative electrode active material may be a composite of graphite and carbon, or a composite material obtained by coating a graphite material with carbon, which is not limited here. It can be understood that the active material in the second active material layer is a graphite negative electrode active material with a low theoretical capacity, but the graphite negative electrode active material has excellent low expansion and can improve the cycle stability of the negative electrode sheet.

[0093] In the present application, the second active material layer 30 includes a second binder and a second conductive agent. Specifically, the second binder contains a first active group, and the first active group includes at least one of a hydroxyl group, an amino group, an epoxy group, an isocyanate group, and an aziridine group.

[0094] In some embodiments, the mass content of the compound containing the first active group in the second active material layer is 0.0001% to 5%, specifically 0.0001%, 0.0005%, 0.001%, 0.002%, 0.005%, 0.01%, 0.05%, 0.1%, 0.5%, 0.8%, 0.9%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%, etc., and of course, it can also be other values ​​within the above range, which are not limited here. The first active group can undergo a chemical cross-linking reaction with the acidic group to improve the bonding strength between the first active material layer and the second active material layer, achieve high interfacial bonding strength between the layers, and reduce interfacial contact resistance.

[0095] The second conductive agent may be at least one of conductive carbon black, carbon nanotubes, graphene, conductive graphite and carbon fiber. Specifically, the carbon nanotubes may be single-walled carbon nanotubes (abbreviated as SWCNT), multi-walled carbon nanotubes (abbreviated as MWCNT), etc., which are not limited here.

[0096] In the present application, the mass content of the second conductive agent in the second active material layer is A2%, 0.1≤A2≤1.5, and A1>A2. It can be understood that due to the difference in conductivity between silicon-based negative electrode active materials and graphite negative electrode active materials, the conductivity of silicon-based negative electrode active materials is poor, while the conductivity of graphite negative electrode active materials is good. The present application optimizes the battery performance by adjusting the ratio of conductive agents in the two active material layers, increasing the mass content of the conductive agent in the first active material layer, and reducing the mass content of the conductive agent in the second active material layer, so as to achieve low addition of the overall conductive agent without affecting the rate performance, increase the active material load, and improve the energy density. Exemplarily, the mass content of the second conductive agent can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 1% or 1.5%, etc., and of course it can also be other values ​​within the above range, which are not limited here.

[0097] As an optional technical solution of the present application, the second active material layer includes a second binder and a dispersant. It can be understood that the graphite negative electrode active material has a small volume change during the charge and discharge process, and is located on the surface of the negative electrode sheet and in direct contact with the electrolyte. In order to obtain a better rate performance, it is necessary to select a second binder with better affinity with the electrolyte and reduce the content of the second binder.

[0098] In some embodiments, the second binder is mainly a binder material with high rate performance, high flexibility, good electrolyte compatibility, and strong hydrophobicity, preferably an emulsion binder. Exemplarily, the emulsion binder can be a polyurethane emulsion containing a first active group, a styrene-butadiene emulsion containing a first active group, an acrylate emulsion containing a first active group, a styrene-acrylic emulsion containing a first active group, an ethylene-propylene emulsion containing a first active group, an EVA emulsion containing a first active group, etc. After the negative electrode sheet is dried, the second binder in the negative electrode sheet mainly includes at least one of polyurethane, acrylate, copolymer of butadiene and styrene, copolymer of styrene-acrylate, copolymer of vinyl acetate-butyl acrylate, and copolymer of ethylene-vinyl acetate.

[0099] In some embodiments, the mass content of the second binder in the second active material layer is B2%, 0.5≤B2≤2, and B1>B2. It can be understood that due to the large volume expansion of the silicon-based active material in the first active material layer, adding more binder can avoid the cracking and powder loss of the pole piece caused by the expansion of the silicon-based active material. Therefore, controlling B1>B2 can suppress the overall volume expansion of the pole piece. For example, the mass content of the second binder can be 0.5%, 0.8%, 1.0%, 1.2%, 1.5%, 1.8%, 1.9% or 2%, etc., and of course it can also be other values ​​within the above range, which are not limited here.

[0100] In some embodiments, the dispersant is mainly a natural polysaccharide dispersant, which plays a role in thickening and dispersing, and can react with the graphite surface to play a role in uniform dispersion. Specifically, the dispersant includes at least one of sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, cellulose nanofibers, sodium alginate, chitosan, guar gum, carrageenan and gelatin.

[0101] In some embodiments, the thickness ratio of the first active material layer to the second active material layer is R, 1≤R≤15, and the value of R can be 1, 1.1, 1.5, 2.0, 2.5, 3, 4, 5, 8, 10, 12, 14 or 15, etc., which is not limited here. It can be understood that the thickness of the first active material layer with a higher gram capacity is greater than the thickness of the second active material layer with a lower gram capacity, which can improve the energy density of the negative electrode sheet.

[0102] In this application, the binders in the two layers of negative electrode active material achieve molecular-scale cross-linking and coupling, which can effectively improve the connection between the two layers of active material and solve the performance loss caused by the interface. In addition, it also helps to reduce the processing difficulty of the double-layer electrode and avoid the problems of demolding and cracking.

[0103] This double-layer structure design can achieve high active material utilization and good structural stability of the negative electrode. Since the first active material layer and the second active material layer are independently stacked and relatively separated, the crosstalk between graphite materials and silicon-based materials can be avoided during the cycle, and the damage to the structure of graphite materials caused by the volume expansion of silicon-based negative electrode materials can be avoided. The second active material layer is located on the surface of the negative electrode sheet, which can also effectively reduce the side reaction between the first active material layer and the electrolyte and improve the cycle performance of the composite negative electrode.

[0104] In a second aspect, the present application also provides a method for preparing a double-layer negative electrode sheet, the preparation method comprising the following steps:

[0105] (1) Preparation of a slurry for the first active material layer.

[0106] In some embodiments, the selected silicon-based negative electrode active material, the first conductive agent, the first binder, and the coupling agent may be mixed in a preset ratio and fully stirred and dispersed to obtain a first electrode slurry with satisfactory viscosity and fineness.

[0107] Specifically, the solvent used for slurry mixing can be selected from one or more of water, methanol, ethanol, N-methylpyrrolidone (abbreviated as NMP), N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), preferably water or NMP.

[0108] In some embodiments, the slurry viscosity is controlled at 2000-10000 mPa·s, specifically 2000 mPa·s, 5000 mPa·s, 6000 mPa·s, 8000 mPa·s, 9000 mPa·s or 10000 mPa·s, preferably 4000-6000 mPa·s. The slurry solid content is controlled at 40%-60%, specifically 40%, 45%, 50%, 55%, 60%, etc., preferably 45%-50%.

[0109] (2) Preparation of a slurry for the second active material layer.

[0110] In some embodiments, the selected graphite-based negative electrode active material, the second conductive agent, the second binder, and the dispersant can be mixed in a preset ratio and fully stirred and dispersed to obtain a second electrode slurry with a viscosity and fineness that meet the standards. The solvent used for slurry mixing, the slurry viscosity, and the solid content in the slurry are as described above and will not be repeated here.

[0111] (3) Negative electrode production.

[0112] In some embodiments, two electrode slurries are double-coated by a coating process. The first negative electrode slurry can be first coated on the negative electrode current collector according to the required coating thickness. After drying, a second negative electrode slurry is coated on the first active material layer, and the negative electrode sheet is obtained after sufficient drying. In other embodiments, a dedicated double-layer coating device can also be used to directly coat and dry two layers of electrode slurry at the same time, and the double-layer negative electrode sheet described above can be directly obtained by one coating. After the negative electrode sheet is manufactured, the material is subjected to a high-temperature baking treatment according to the temperature required for the cross-linking reaction to achieve the occurrence of chemical cross-linking reactions within and between layers.

[0113] In some embodiments, the coating drying temperature is controlled at 50°C to 110°C, and a step-by-step drying process can be used, and the drying temperature is preferably 60°C to 90°C. It should be understood that the high-temperature baking cross-linking temperature of the negative electrode plate can be adapted according to different cross-linking reactions. Specifically, the high-temperature baking treatment temperature is controlled at 60°C to 140°C, and the high-temperature baking treatment temperature is preferably 80°C to 120°C.

[0114] As an optional technical solution of the present application, the negative electrode active layer on the negative electrode current collector can be a single-sided coating or a double-sided coating. Single-sided coating means that the active material layer can be coated on any side of the current collector, and double-sided coating means that the negative electrode active layer is coated on both sides of the current collector.

[0115] In a third aspect, the present application provides an electrochemical device, the electrochemical device comprising the negative electrode sheet described in the second aspect. It can be understood that the above electrochemical device, in addition to the negative electrode sheet, generally also includes a positive electrode sheet, a separator and an electrolyte.

[0116] The positive electrode plate comprises a positive electrode current collector and a positive electrode active layer arranged on the surface of the positive electrode current collector, wherein the positive electrode active layer comprises a positive electrode active material, a conductive material and a binder.

[0117] As an optional technical solution of the present application, the positive electrode current collector can be aluminum foil or nickel foil, etc., which is not limited here. As an optional technical solution of the present application, the positive electrode active material includes at least one of lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium manganese oxide, lithium iron manganese phosphate, lithium vanadium phosphate, lithium vanadium oxyphosphate, lithium iron phosphate and lithium titanate.

[0118] The conductive material includes at least one of conductive graphite, conductive carbon black, acetylene black, carbon nanotubes and graphene.

[0119] The binder can improve the bonding between the positive electrode active material particles and also improve the bonding between the positive electrode active material and the positive electrode current collector. Optionally, the binder includes at least one of polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylic (ester) styrene-butadiene rubber, epoxy resin or nylon.

[0120] In the above electrochemical device, the electrolyte includes a lithium salt and a solvent, and the lithium salt includes at least one of lithium perchlorate (LiClO4), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), and lithium trifluoromethylsulfonate (LiCF3SO3). The solvent includes at least one of ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC). The electrolyte also includes additives, and the type of additives is not particularly limited. It can be a negative electrode film-forming additive, a positive electrode film-forming additive, or an additive that can improve certain battery properties, such as an additive that improves the battery overcharge performance, an additive that improves the battery high temperature performance, an additive that improves the battery low temperature performance, etc.

[0121] As an optional technical solution of the present application, the isolation membrane is selected from a composite of one or more of polyethylene film, polypropylene film, and polyvinylidene fluoride film. Of course, an inorganic or organic coating can also be coated on the surface of the isolation membrane substrate according to actual needs to enhance the hardness of the battery cell or improve the adhesion between the isolation membrane and the cathode and anode interfaces.

[0122] In a specific embodiment, the electrochemical device may be a primary battery, a secondary battery, a solid-state battery or a lithium-ion battery, which is not limited here.

[0123] In some embodiments, the preparation of the battery comprises the following steps:

[0124] The prepared negative electrode sheet is subjected to rolling, striping, die-cutting, assembly and other processes, and is matched with a suitable positive electrode sheet to prepare a lithium-ion battery. The battery manufacturing process can be lamination or winding. The battery specifications can be cylindrical cells, soft-pack cells, square-shell cells or other types of lithium-ion batteries.

[0125] Environment and equipment required for preparation: planetary high-speed stirring and dispersing equipment, extrusion coating equipment, transfer coating equipment, vacuum heating equipment, lithium-ion battery production equipment, clean room, etc., not limited here.

[0126] In a fourth aspect, the present application further provides an electronic device, wherein the electronic device is the electrochemical device described in the third aspect. The electrochemical device of the present application has good cycle performance and safety performance, and therefore, the above electrochemical device is applied in the electronic device, so that the electronic device has good safety performance and can also extend the service life of the electronic device.

[0127] The electronic devices in this application may specifically be mobile phones, computers, tablet computers, smart bracelets, smart watches, etc., without limitation herein.

[0128] The above are only preferred embodiments of the present application and are not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application should be included in the scope of protection of the present application.

[0129] The present application is further described below by taking lithium-ion batteries as an example through specific embodiments and comparative examples.

[0130] Example 1

[0131] (1) Preparation of slurry for the first active material layer

[0132] The first binder (acrylic acid-acrylonitrile copolymer 5%), the first conductive agent (1% conductive carbon black and 1% multi-walled carbon nanotubes) and the silicon-based negative electrode active material (silicon oxide material SiO 93%) were mixed evenly, an appropriate amount of deionized water was added, and high-speed dispersion stirring was performed for 5 hours to obtain a uniform slurry with a solid content of 50%, which was used as the first negative electrode slurry.

[0133] (2) Preparation of slurry for the second active material layer

[0134] The dispersant (sodium carboxymethyl cellulose CMC-Na-1%), the second binder (2% styrene-butadiene rubber emulsion, the polymer of the styrene-butadiene rubber emulsion is copolymerized with epoxy acrylate monomer), the second conductive agent (1% conductive carbon black) and the graphite negative electrode active material (graphite 96%) are mixed evenly, an appropriate amount of deionized water is added, and the mixture is dispersed and stirred at a high speed for 5 hours to obtain a uniform slurry with a solid content of 50%, which is used as the second negative electrode slurry.

[0135] (3) Preparation of negative electrode sheet

[0136] The slurry of the first active material layer was coated on a 10 μm copper foil, and the loading of the coated first active material was 2 mg / cm 2 , dried, and then the slurry of the second active material layer was coated on the first active material layer. The loading of the coated second active material was 8 mg / cm 2 After drying, vacuum bake at 110℃ for 12h for later use.

[0137] (4) Production of positive electrode

[0138] 97g of lithium cobalt oxide, 0.5g of carbon nanotubes, and 2.5g of polyvinylidene fluoride (PVDF) were mechanically mixed, and then N-methylpyrrolidone (NMP) was added as a solvent to prepare a slurry with a solid content of 65wt%, and stirred evenly to obtain a uniform positive electrode slurry. The positive electrode slurry was coated on one surface of an aluminum foil current collector with a thickness of 12μm and dried at 90°C. After the above steps were completed, the single-sided coating of the positive electrode plate was completed. After that, the above steps were repeated on the other surface of the positive electrode plate. After roller pressing, a positive electrode plate coated with positive electrode active materials on both sides was obtained, wherein the compaction density of the positive electrode plate was 4.0g / cc and the active material loading was 22mg / cm 2 .

[0139] (5) Production of lithium-ion batteries

[0140] The positive electrode sheet, separator (Celgard 2400), and negative electrode sheet prepared above are stacked in order to obtain a bare cell. The bare cell is placed in an aluminum-plastic film packaging bag, dried and injected with an electrolyte (a mixed solution of 1 mol / L LiPF6 ethylene carbonate (EC) and diethyl carbonate (EMC) (v / v=1:1), with an addition amount of 10 wt% fluoroethylene carbonate), and then vacuum packaged, allowed to stand, formed, degassed, etc. to obtain a lithium-ion battery.

[0141] Example 2

[0142] The preparation method of this embodiment is basically the same as that of embodiment 1, except that the first binder used in step (1) is an acrylic acid-acrylonitrile copolymer containing benzenesulfonic acid groups.

[0143] Example 3

[0144] The preparation method of this embodiment is basically the same as that of embodiment 1, except that the first conductive agent used in step (1) is 1% single-walled carbon nanotubes.

[0145] Example 4

[0146] The preparation method of this embodiment is basically the same as that of embodiment 1, except that in step (1), the coating is performed with an active substance loading of 1 mg / cm 2 In step (2), the active material loading is 9 mg / cm 2 .

[0147] Example 5

[0148] The preparation method of this embodiment is basically the same as that of embodiment 1, except that a ternary aziridine coupling agent of 0.3% of the total solid mass is added in step (1) to improve the strength of the binder.

[0149] Example 6

[0150] The preparation method of this embodiment is basically the same as that of embodiment 1, except that the first binder used in step (1) is a polyimide copolymerized with a carboxylic acid monomer.

[0151] Example 7

[0152] The preparation method of this embodiment is basically the same as that of embodiment 1, except that the first binder used in step (1) is an acrylic copolymer containing a phosphate group.

[0153] Example 8

[0154] The preparation method of this embodiment is basically the same as that of embodiment 1, except that the silicon-based negative electrode active material in step (1) is a silicon-carbon negative electrode material.

[0155] Example 9

[0156] The preparation method of this embodiment is basically the same as that of embodiment 1, except that the second binder used in step (2) is a styrene-butadiene emulsion copolymerized with acrylamide monomer.

[0157] Example 10

[0158] The preparation method of this embodiment is basically the same as that of embodiment 1, except that the second binder used in step (2) is a styrene-acrylic emulsion copolymerized with acrylamide monomer.

[0159] Embodiment 11

[0160] The preparation method of this embodiment is basically the same as that of embodiment 1, except that the dispersant used in step (2) is lithium carboxymethyl cellulose.

[0161] Example 12

[0162] The preparation method of this embodiment is basically the same as that of embodiment 1, except that the battery assembly in step (3) adopts a winding process to produce a soft-pack battery cell.

[0163] Example 13

[0164] The preparation method of this embodiment is basically the same as that of embodiment 1, except that the second binder used in step (2) is a styrene acrylic emulsion copolymerized with hydroxyethyl acrylate.

[0165] Embodiment 14

[0166] The preparation method of this embodiment is basically the same as that of embodiment 1, except that 0.2% of a blocked water-based isocyanate coupling agent is added in step (2).

[0167] Embodiment 15

[0168] The preparation method of this embodiment is basically the same as that of embodiment 1, except that 0.2% of aziridine coupling agent is added in step (2).

[0169] Comparative Example 1

[0170] The difference from Example 1 is:

[0171] Preparation of negative electrode

[0172] After the silicon oxide negative electrode material and the graphite negative electrode material were mixed in a weight ratio of 2:8, 5% acrylic copolymer battery binder, 5% superconductive carbon black and 90% of the above mixed negative electrode powder were evenly dispersed, and an appropriate amount of deionized water was added. The mixture was dispersed and stirred at high speed for 5 hours to obtain a uniform slurry with a solid content of 50%. The slurry was coated on a smooth copper foil to obtain a negative electrode sheet. The coating active material loading was 10 mg / cm 2 .

[0173] Comparative Example 2

[0174] The difference from Example 1 is:

[0175] (3) Preparation of negative electrode sheet

[0176] The slurry of the second active material layer was coated on a 10 μm copper foil, and the loading of the coated second active material was 8 mg / cm 2 , dried, and then the slurry of the first active material layer was coated on the second active material layer. The loading of the coated first active material was 2 mg / cm 2 After drying, vacuum bake at 110℃ for 12h for later use.

[0177] It can be understood that in this comparative example, the second negative electrode slurry (graphite negative electrode) is first applied, and then the first negative electrode slurry (silicon-based negative electrode) is applied.

[0178] Performance Test:

[0179] (1) Test of average coulombic efficiency and capacity retention rate of lithium-ion batteries:

[0180] The capacity retention rate of the soft-pack lithium-ion batteries of Examples 1 to 15 and Comparative Examples 1 to 2 after being divided into capacities at a low rate and then cycled for 100 cycles at a charge and discharge rate of 0.2C / 0.2C, wherein 0.2C means that the battery charging C rate (charge and discharge rate) is 0.2C, and 0.2C means that the battery discharging C rate (charge and discharge rate) is 0.2C.

[0181] (2) Test of the expansion rate of the negative electrode plate: The lithium-ion batteries of Examples 1 to 15 and Comparative Examples 1 to 2 were charged and discharged 50 times and then charged to 100% of the battery state of charge (SOC). The batteries were then taken out and the plates were disassembled. The surface of the negative electrode plate was cleaned with dimethyl carbonate solvent and then dried. The thickness of different areas of the negative electrode plate was measured using a micrometer. The average value was taken. The difference between the average value and the initial thickness of the negative electrode plate was divided by the initial thickness of the negative electrode plate (the thickness of the remaining part after excluding the thickness of the current collector). The resulting value is the expansion rate of the negative electrode plate.

[0182] Table 1. Performance test results of Examples 1 to 15 and Comparative Examples 1 to 2

[0183]

[0184] like Figure 3 As shown, the lithium battery of the composite electrode prepared in Example 1 still has a capacity retention rate of 98.05% after 100 cycles, while the lithium battery cycle capacity of the composite electrode of Comparative Example 1 using a conventional composite electrode and Comparative Example 2 using a composite electrode with a graphite-on-silicon coating structure rapidly decreases, and the capacity retention rates after 100 cycles are only 83.91% and 85.05%, respectively. The coulomb efficiency of the lithium battery in Example 1 exceeds 99.5% after 4 cycles. The average coulomb efficiencies of the batteries in Example 1, Comparative Example 1, and Comparative Example 2 in the first 100 cycles are 99.71%, 99.61%, and 99.63%, respectively. This shows that the double-layer structure effectively improves the cycle stability of the composite negative electrode.

[0185] like Figures 4a to 4f As shown, the electron microscope was used to examine Example 1 ( Figure 4a and Figure 4d ), Comparative Example 1( Figure 4b and Figure 4e ) and Comparative Example 2 ( Figure 4c and Figure 4f ) was observed for the post-cycle electrode sheet morphology. In Example 1, the first active material layer is located on the surface of the negative electrode current collector, and the second active material layer is located on the surface of the first active material layer, which ensures the contact and electronic conduction between the silicon-based negative electrode active material and the negative electrode current collector, and maximizes the performance of the second active material layer, and avoids the contact between the silicon-based negative electrode active material and the electrolyte, inhibits the occurrence of side reactions, and successfully achieves the minimum electrode expansion after 100 cycles of the battery.

[0186] According to the test data of Example 1 and Comparative Examples 1 and 2, it can be seen that the expansion is significantly suppressed when the first active material layer (silicon-based) is at the bottom layer. Figure 4d As shown, after 100 cycles, the thickness of the negative electrode sheet of Example 1 is 42.5 um, wherein the thickness of the first active material layer is about 12.5 um.

[0187] In Comparative Example 1, the silicon-based negative electrode active material is conventionally composited with graphite. The stress accumulation caused by the volume change of silicon particles during lithium intercalation and deintercalation will inhibit the intercalation of lithium ions into graphite, leading to the decline of graphite capacity, and will also destroy the overall structure of the electrode, affecting the cycle performance of the electrode. Figure 4e As shown, after 100 cycles, the thickness of the negative electrode plate of Comparative Example 1 is 47.5 um, and it can be seen that the expansion of the electrode plate is significantly improved compared with Example 1.

[0188] In Comparative Example 2, the silicon-based negative electrode active material is located on the surface. During the cycle, the silicon-based active material directly contacts the electrolyte, and the side reaction between the negative electrode active material and the electrolyte intensifies. The silicon-based negative electrode active material will produce a huge volume expansion, deteriorating the battery performance and causing a large number of cracks. Figure 4f As shown, after 100 cycles, the thickness of the negative electrode plate of Comparative Example 2 is 57.5um, wherein the thickness of the first active material layer is about 37.5um, and the first active material layer located on the surface of the electrode plate undergoes a huge volume expansion, so that the overall electrode plate expansion is also significantly improved compared to Example 1.

[0189] In summary, the graphite-based negative electrode active material and the silicon-based negative electrode active material are respectively formed into a first active material layer and a second active material layer which are stacked, and the first active material layer containing the silicon-based negative electrode active material is located between the second active material layer and the negative electrode current collector, so as to form a double-layer structure composite negative electrode plate. On the one hand, since the graphite-based negative electrode active material and the silicon-based negative electrode active material are separated from each other, the mutual crosstalk caused by the volume change of different active materials during the charge and discharge cycle can be avoided, and the damage to the graphite material structure caused by the expansion of the silicon-based material during the charge and discharge process can be avoided. On the other hand, the first active material layer is closer to the negative electrode current collector, which can effectively reduce its side reaction with the electrolyte, avoid the rapid performance attenuation and thickening of the interface layer caused by the direct contact of the silicon-based negative electrode active material with the electrolyte, and improve the cycle performance of the plate.

Claims

1. A negative electrode plate, characterized in that: The negative electrode plate comprises: A negative electrode current collector, a negative electrode active layer disposed on at least one side of the negative electrode current collector; The negative electrode active layer comprises a first active material layer and a second active material layer stacked together, wherein the first active material layer is located between the second active material layer and the negative electrode current collector; The first active material layer includes a silicon-based negative electrode active material and a first binder containing an acidic group; The second active material layer includes a graphite-based negative electrode active material and a second binder containing a first active group, wherein the first active group is chemically bonded to the acidic group.

2. The negative electrode sheet according to claim 1, characterized in that: It meets at least one of the following characteristics: 1) the first reactive group reacts with the acidic group to form at least one of a carboxylate group, a sulfonate group, a phosphate group, an amide group, an ether group, a carbamate group or a urea group; 2) the acidic group includes at least one of a carboxyl group, a sulfonic acid group and a phosphate group; 3) the first reactive group comprises at least one of a hydroxyl group, an amino group, an epoxy group, an isocyanate group and an aziridine group; 4) The mass content of the acidic groups in the first active material layer is 0.0001% to 5%; 5) The mass content of the first active group in the second active material layer is 0.0001% to 5%.

3. The negative electrode sheet according to claim 1, characterized in that: The first active material layer further includes a first conductive agent, the mass content of the first conductive agent in the first active material layer is A1%; the second active material layer further includes a second conductive agent, the mass content of the first conductive agent in the first active material layer is A2%, and A1>A2.

4. The negative electrode sheet according to claim 1 or 3, characterized in that: The mass content of the first binder in the first active material layer is B1%; the mass content of the second binder in the second active material layer is B2%, and B1>B2.

5. The negative electrode sheet according to claim 1, characterized in that: The mass content of the first binder in the first active material layer is 3% to 10%; and / or, The first binder includes at least one of an acrylic copolymer containing an acidic group, an acrylate copolymer containing an acidic group, an acrylonitrile copolymer containing an acidic group, polyvinyl alcohol containing an acidic group and its derivatives, polyimide containing an acidic group and its derivatives, an epoxy resin copolymer containing an acidic group, a nitrile rubber containing an acidic group, and a hydrogenated nitrile rubber containing an acidic group.

6. The negative electrode sheet according to claim 5, characterized in that: The first active material layer further includes a coupling agent; the mass content of the coupling agent in the first active material layer is 0% to 1%; and / or, The coupling agent includes at least one of a silane coupling agent, an aziridine coupling agent, an epoxy coupling agent, an isocyanate coupling agent and a polyol coupling agent.

7. The negative electrode sheet according to claim 1, characterized in that: The mass content of the second binder in the second active material layer is 0.5% to 2%; and / or, The second binder includes at least one of a polyurethane emulsion containing a first active group, a styrene-butadiene emulsion containing a first active group, an acrylate emulsion containing a first active group, a styrene-acrylic emulsion containing a first active group, an ethylene-propylene emulsion containing a first active group, and an EVA emulsion containing a first active group.

8. The negative electrode sheet according to claim 7, characterized in that: The second active material layer further comprises a dispersant; the mass content of the dispersant in the second active material layer is 0.5% to 2%; and / or, The dispersant includes sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, cellulose nanofibers, sodium alginate, chitosan DD231407I-MS At least one of sugar, guar gum, carrageenan and gelatin.

9. The negative electrode sheet according to claim 3, characterized in that: It meets at least one of the following characteristics: 1) The mass content of the first conductive agent in the first active material layer is A1%, 2≤A1≤10; 2) The mass content of the second conductive agent in the second active material layer is A2%, 0.1≤A2≤1.5; 3) The first conductive agent and the second conductive agent each independently include at least one of conductive carbon black, carbon nanotubes, graphene, conductive graphite and carbon fiber.

10. The negative electrode sheet according to claim 1, characterized in that: It meets at least one of the following characteristics: 1) The silicon-based negative electrode active material includes at least one of elemental silicon, silicon-oxygen compounds, silicon-carbon composites, silicon-nitrogen composites and silicon alloys; 2) The graphite-based negative electrode active material includes at least one of natural graphite, artificial graphite and carbon material; 3) The thickness of the negative electrode current collector is 1 μm to 50 μm; 4) The thickness of the negative electrode active layer is 10 μm to 100 μm; 5) The negative electrode current collector comprises at least one of copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, and a polymer substrate covered with a conductive metal; 6) The surface of the negative electrode current collector is also provided with a conductive coating, and the conductive coating includes at least one of conductive carbon black, carbon nanotubes, graphene, conductive graphite and carbon fiber.

11. The negative electrode sheet according to any one of claims 1 to 10, characterized in that: A thickness ratio of the first active material layer to the second active material layer is R, 1≤R≤15.

12. An electrochemical device, characterized in that: The electrochemical device comprises the negative electrode sheet according to any one of claims 1 to 11.

13. An electronic device, characterized in that: The electronic device comprises the electrochemical device according to claim 12.

Citation Information

Cited By

  • Secondary battery and electric equipment

    CN119786770A

  • Positive electrode slurry and preparation method and application thereof

    CN121035212A

  • A positive electrode slurry, a method for preparing the same, and an application thereof

    CN121035212B

  • Battery cell, battery device and electric device

    WO2026188565A1

  • Negative electrode sheet, secondary battery and electronic device

    WO2026208234A1