Hollow fiber membrane and its manufacturing method
A hollow fiber membrane with a controlled layer structure and manufacturing gradient enhances strength and stability, ensuring prolonged high-performance filtration of turbid liquids.
Patent Information
- Application Number
- JP2022527193
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-08-27
- Filing Date
- 2022-04-28
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-04-28
AI Technical Summary
Existing hollow fiber membranes face issues with poor strength and rapid deterioration of separation performance under high-pressure conditions, leading to reduced water permeability and stability, especially when filtering liquids with turbid components or organic matter.
A hollow fiber membrane with a specific layer structure of spherical structures, where the average diameter and constriction diameter vary across the thickness, combined with a controlled temperature gradient during manufacturing to enhance strength and water permeability.
The membrane maintains high separation performance and water permeability over extended periods, even under high-pressure conditions, effectively filtering liquids with turbid components or organic matter.
Smart Images

Figure 0007586176000006 
Figure 0007586176000007 
Figure 0007586176000008
Abstract
Description
[Technical field]
[0001] The present invention relates to a hollow fiber membrane and a method for producing the same. [Background technology]
[0002] Separation membranes such as microfiltration membranes and ultrafiltration membranes are used for purposes such as clarification, concentration and separation in water treatment, food and pharmaceutical applications. In recent years, as the range of applications for separation membranes has expanded, their use in applications where difficult-to-filter liquids or high-precision separation are required has been considered, and there is an increasing demand for separation membranes that combine both filterability and separation properties.
[0003] Patent Document 1 discloses a porous hollow fiber membrane containing a vinylidene fluoride resin, in which the pore size of the hollow fiber membrane has a gradient structure in which the pore size gradually decreases toward at least one of the inner and outer peripheral surfaces. It also describes that this hollow fiber membrane has excellent permeability, fractionation characteristics, and strength.
[0004] Patent Document 2 discloses a hollow fiber membrane having spherical structures formed from a polyvinylidene fluoride resin by a thermally induced phase separation method, and having larger spherical structures within 10 μm from the outer surface than those near the inner surface. It describes that by having large spherical structures near the outer surface, the membrane is less likely to clog and continuously maintains high water permeability, and that the homogeneous inner layer provides high strength.
[0005] Furthermore, Patent Document 2 discloses a method for producing such a membrane, in which a temperature gradient is applied to a polyvinylidene fluoride resin solution before solidification in the thickness direction of the separation membrane. Specifically, it describes that the spherical structures on the surface on the heated side are coarsened by heating a die used to form the hollow fiber. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2015 / 146469 [Patent Document 2] International Publication No. 2016 / 006611 Summary of the Invention [Problem to be solved by the invention]
[0007] The hollow fiber membrane disclosed in Patent Document 1 has a three-dimensional mesh structure in which the pore size of the hollow fiber membrane gradually decreases toward one side. Such a membrane is inferior in strength and is not suitable for operations that place a large load on the membrane, such as external pressure cross-flow filtration. In addition, since the layer having the separation function of such a membrane is very thin, the separation function is easily reduced by membrane damage during operation. Therefore, it is difficult to maintain a stable separation function for a long period of time.
[0008] The membrane of Patent Document 2 has a relatively small and homogeneous spherical structure inside, which can block components in the liquid, and can maintain separation performance for a long time. In addition, since a large spherical structure exists near the outer surface, clogging components (components that cause clogging) can be captured inside. On the other hand, the area that can capture clogging components remains only near the outer surface. Therefore, there is a problem that the time that permeability can be maintained is shortened for liquids to be filtered, especially liquids with a large amount of turbid components or organic components, and depending on conditions such as operating time. In response to this, there is a demand for a longer time that permeability can be maintained even for liquids that are difficult to filter.
[0009] An object of the present invention is to provide a hollow fiber membrane using a polyvinylidene fluoride resin, which is capable of maintaining separation properties and water permeability, and a method for producing the same. [Means for solving the problem]
[0010] In order to achieve the above object, the present invention includes the following aspects 1 to 19. 1. A hollow fiber membrane having a layer of resin spherical structure, The thickness L of the layer of the spherical structure is 60 μm or more and 500 μm or less, The layer of the spherical structure has a first surface and a second surface, in the region Sa of 10×(n - 1) to 10×n μm from the first surface, n the average diameter Da of the spherical structure, n and in the region Sb of 10×(n - 1) to 10×n μm from the second surface, n the average diameter Db of the spherical structure, n satisfy Da1 > Db2, and the minimum value i of the natural number i that satisfies the following conditions (1) and (2), min is 3 ≤ i min ≤ (L - 20) / 10, which is a hollow fiber membrane. (1) Da1 / Da i ≥ 1.1 (2) -0.3 μm ≤ Da i -Db2 ≤ 0.3 μm However, the n is a natural number, and in 3 ≤ i min ≤ (L - 20) / 10, the decimal part of (L - 20) / 10 is truncated. small 2. i min ≤ L×0.75 / 10, the hollow fiber membrane according to 1 above. However, in i min ≤ L×0.75 / 10, the decimal part of L×0.75 / 10 is truncated. 3. 1.10 < Da1 / Da imin < 4.00, the hollow fiber membrane according to 1 or 2 above. 4. 0.50 μm < Db2 < 2.00 μm, the hollow fiber membrane according to any one of 1 to 3 above. 5. 1.00 ≤ Da1 / Da2 ≤ 1.10, the hollow fiber membrane according to any one of 1 to 4 above. 6. The first surface is the filtrate side, the hollow fiber membrane according to any one of 1 to 5 above. 7. The first surface is the outer surface of the hollow fiber membrane, the hollow fiber membrane according to any one of 1 to 6 above. 8. When the throat diameter obtained by the pore network model analysis for the hollow fiber membrane is taken as the constriction diameter of the spherical structure gap, in the region Sa of 10×(n - 1) to 10×n μm from the first surface,n The average diameter of the constriction between the spherical structures in n and, A region Sb of 10×(n−1) to 10×n μm from the second surface n The average diameter of the constriction between the spherical structures in n For da1>db2, and The smallest natural number j that satisfies the following conditions (1) and (2) min j is 3 or less min 8. The hollow fiber membrane according to any one of 1 to 7 above, wherein L=(L−20) / 10. (1)da1 / da j ≧1.15 (2)da j -db2≦0.10μm However, the above 3≦j min In the case of (L-20) / 10 or less, the decimal places of (L-20) / 10 are rounded down. 9.j min 9. The hollow fiber membrane according to 8 above, wherein L×0.5 / 10. However, the above j min For L×0.5 / 10, round down to the nearest integer. 10. The region Sa obtained by the pore network model analysis. n Number of throats in Na n and the region Sb n Number of throats in Nb n About Na1 <Nb2であり、かつ The smallest natural number k that satisfies the following conditions (3) and (4) min k≦3 min 10. The hollow fiber membrane according to claim 8 or 9, wherein the elastic modulus is less than or equal to (L-20) / 10. (3) Na1 / Na k ≦0.90 (4)Nb2-Na k ≦400 pieces However, the above 3≦k min In the case of (L-20) / 10 or less, the decimal places of (L-20) / 10 are rounded down. However, the analysis region in the above analysis is a rectangular parallelepiped including any 50 μm square on the first surface and a 50 μm square on the second surface facing the first surface. 11.0.10 μm < db2 < 10.0 μm, and the hollow fiber membrane according to any one of 8 to 10 above. 12. The spherical structure is made of a polyvinylidene fluoride resin, a hydrophilic polymer is present on the surface and inside of the spherical structure, and the hollow fiber membrane according to any one of 1 to 11 above, containing 1.0 part by mass or more of the hydrophilic polymer with respect to 100 parts by mass of the polyvinylidene fluoride resin. 13. When the ratio (mass %) of the hydrophilic polymer to the polyvinylidene fluoride resin after immersing the hollow fiber membrane in an aqueous sodium hypochlorite solution (pH 12.5) at 60 °C with a concentration of 3000 ppm for 30 hours is P1, and the ratio (mass %) of the hydrophilic polymer to the polyvinylidene fluoride resin before the immersion is P0, the percentage of the ratio P1 / P0 of P1 to P0 is 70% or less, and the hollow fiber membrane according to 12 above. 14. (a) A step of dissolving a polyvinylidene fluoride resin in a poor solvent to obtain a polyvinylidene fluoride resin solution, (b) A step of holding the polyvinylidene fluoride resin solution at a temperature at which the formation of primary nuclei proceeds, (c) After the step (b), discharging the polyvinylidene fluoride resin solution in a hollow fiber shape through a pipe and a die, and applying a temperature gradient in the thickness direction of the polyvinylidene fluoride resin solution in at least one of the pipe or the die, and (d) After the step (c), a step of solidifying the polyvinylidene fluoride resin solution by solid-liquid type thermally induced phase separation by immersing the polyvinylidene fluoride resin solution in a cooling bath, A method for producing a hollow fiber membrane, wherein the temperature gradient ΔT (°C) applied in the step (c) and the time t (seconds) for applying the temperature gradient satisfy 50 ≤ ΔT × t ≤ 300. 15. In the step (c), the thickness Ls of the polyvinylidene fluoride resin that imparts a temperature gradient satisfies 5 < Ls / L < 40 with respect to the thickness L of the spherical structure layer, and the method for manufacturing the hollow fiber membrane according to 14 above. 16. The temperature T2 (°C) in the step (b), the temperature T4 (°C) of the cooling bath in the step (d), and the crystallization temperature Tc (°C) of the polyvinylidene fluoride resin satisfy (Tc - T4) / (T2 - T4) < 0.50, and the method for manufacturing the hollow fiber membrane according to 14 or 15 above. 17. The method for manufacturing the hollow fiber membrane according to 16 above, which satisfies 15 < Tc - T4 < 35. 18. After the step (d), the method for manufacturing the hollow fiber membrane according to any one of 14 to 17 above, further including the following steps (e) and (f). (e) A step of introducing a hydrophilic polymer into the hollow fiber membrane (f) A step of performing heat treatment at 100°C or higher after the step (e) 19. In the step (e), the method for manufacturing the hollow fiber membrane according to 18 above, including passing an aqueous solution in which a hydrophilic polymer is dissolved through the hollow fiber membrane and then performing radiation irradiation.
Advantages of the Invention
[0011] According to the present invention, it is possible to provide a hollow fiber membrane capable of maintaining separation performance and water permeability and a method for manufacturing the same.
Brief Description of the Drawings
[0012] [Figure 1] FIG. 1 is an electron micrograph of the vicinity of the first surface and the second surface in the radial cross-section of the hollow fiber membrane. [Diagram 2] FIG. 2 is a schematic diagram showing a method for calculating the average diameter of the spherical structure. [Diagram 3] FIG. 3 is a diagram showing the result of measuring the average diameter of the spherical structure with respect to the distance from the first surface. [Figure 4] FIG. 4 is a diagram illustrating an analytical image of the pore network model of the hollow fiber membrane. [Diagram 5] FIG. 5 is a top view showing a specific example of the configuration of the die used for manufacturing the hollow fiber membrane. [Figure 6] FIG. 6 is a cross-sectional view of the base shown in FIG. 5 taken along line AA. [Figure 7] FIG. 7 is a bottom view of the base shown in FIG. [Figure 8] FIG. 8 is a diagram showing examples of the shape of a pipe. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, the embodiments of the present invention will be described, but the present invention is not limited to the following embodiments, and can be modified as desired without departing from the gist of the present invention. In this specification, a ratio (percentage, part, etc.) based on weight is the same as a ratio (percentage, part, etc.) based on mass.
[0014] The hollow fiber membrane according to the embodiment of the present invention has a layer of a resin spherical structure, and the thickness L of the layer of the spherical structure is 60 μm or more and 500 μm or less. The layer of the spherical structure has a first surface and a second surface, and a region Sa of 10 × (n-1) to 10 × n μm from the first surface. n The average diameter Da of the spherical structures in n and a region Sb of 10×(n−1) to 10×n μm from the second surface. n The average diameter of the spherical structures in n For Da1>Db2, the smallest natural number i that satisfies the following conditions (1) and (2) is min 3≦i min <=(L-20) / 10. (1) Da1 / Da i ≧1.1 (2)-0.3μm≦Da i -Db2≦0.3μm Here, n is a natural number, and 3≦i min ≦(L-20) / 10, (L-20) / 10 small Round down to a few points.
[0015] <Hollow fiber membrane> The hollow fiber membrane according to the embodiment of the present invention has a layer of a resin having a spherical structure. The hollow fiber membrane may be composed of only a layer of a spherical structure, or may have other layers. The layer of a resin having a spherical structure refers to a layer of a spherical structure composed of a resin.
[0016] The resin constituting the layer of the spherical structure is preferably a thermoplastic resin made of a chain polymer, and polyvinylidene fluoride resin is particularly preferable because of its high chemical resistance. Here, the polyvinylidene fluoride resin means a resin containing at least one of vinylidene fluoride homopolymer and vinylidene fluoride copolymer. The polyvinylidene fluoride resin may contain a plurality of types of vinylidene fluoride copolymer. In other words, the spherical structure is preferably made of a polyvinylidene fluoride resin. The fact that the spherical structure is made of a polyvinylidene fluoride resin means that the thermoplastic resin component constituting the spherical structure is substantially composed of a polyvinylidene fluoride resin. Even when the spherical structure is made of a polyvinylidene fluoride resin, it may contain, in addition to the thermoplastic resin, other resins that are miscible with the thermoplastic resin and polyhydric alcohols or surfactants at a ratio of 50% by weight or less. The spherical structure may contain other unavoidable impurities, and the content of the impurities is preferably, for example, 1% by weight or less.
[0017] The vinylidene fluoride copolymer is a polymer having a vinylidene fluoride residue structure, and is typically a copolymer of vinylidene fluoride monomer and other fluorine-based monomers. The other fluorine-based monomers include, for example, one or more monomers selected from the group consisting of vinyl fluoride, tetrafluoroethylene, hexafluoropropylene, and trifluorochloroethylene. In addition, as a monomer other than the above fluorine-based monomer, a monomer such as ethylene may be copolymerized to the extent that the effect of the present invention is not impaired.
[0018] The layer of the spherical structure may contain, in addition to the thermoplastic resin, another resin miscible with the thermoplastic resin, and a polyhydric alcohol or a surfactant in an amount of 50% by weight or less. In this specification, the term "spherical structure" refers to a solid portion having a substantially circular cross section perpendicular to the length direction of the hollow fiber membrane (i.e., parallel to the radial direction of the hollow fiber membrane), and a structure formed by connecting the solid portions as described below. When referring to a portion having a substantially circular cross section, rather than the entire structure, it may be called a "solid portion." The term "substantially circular" includes a perfect circle and an ellipse. The solid portions are connected to each other by sharing a part of them in the surface direction or thickness direction of the separation membrane (hollow fiber membrane). The shape of the cross section parallel to the length direction of the hollow fiber membrane is not particularly limited, and may be any shape, such as a substantially circular shape or a columnar shape.
[0019] The separation membrane (hollow fiber membrane) has a spherical structure, which gives it high strength and elongation, and also has high water permeability due to the presence of voids between the spherical solid parts. During filtration, it is preferable that the first surface is disposed upstream in the filtration direction and the second surface is disposed downstream in the filtration direction. The liquid to be filtered preferably flows from the first surface to the second surface. In other words, it is preferable that the first surface is on the liquid to be filtered side. In other words, when used in so-called external pressure filtration, the outer surface of the hollow fiber membrane is the first surface and the inner surface is the second surface, and when used in internal pressure filtration, the inner surface of the hollow fiber membrane is the first surface and the outer surface is the second surface.
[0020] Next, the diameter of the spherical structure with respect to the position in the thickness direction of the hollow fiber membrane will be described with reference to FIG. In the following, for convenience, the outer surface of the hollow fiber membrane is referred to as the first surface, and the inner surface is referred to as the second surface. Figure 1 shows electron microscope photographs of the radial cross section of the hollow fiber membrane, where (a) shows the vicinity of the first surface, and (b) shows the vicinity of the second surface.
[0021] In the cross section, the regions separated by 10 μm intervals from the first surface, 0 to 10 μm, 10 μm to 20 μm, . . . 10×(1-n) μm to 10×n μm, are denoted by symbols Sa1, Sa2, . . . Sa n In addition, the regions separated by 10 μm intervals from the second surface, 0 to 10 μm, 10 μm to 20 μm, . . . 10×(1-n) to 10×n μm . . . are denoted by symbols Sb1, Sb2, . . . Sb nThat is, the area of 10×(n−1) to 10×n μm from the first surface is designated as Sa. n The area from 10×(n-1) to 10×n μm from the second surface is Sb n Here, n is a natural number.
[0022] As shown in Figure 1, a photograph is taken so that the arc that is the first surface of the hollow fiber membrane can be seen. At this time, the tangent to the center of the arc that forms the first surface is aligned with the horizontal direction in the photograph. In the obtained photograph, a straight line Ma1 is drawn that passes through the intersection of the arc that forms the first surface and the left and right ends of the photograph. The straight line Ma1 is preferably parallel to the horizontal direction of the photograph, but may be inclined.
[0023] Furthermore, a line Ma2 parallel to this line is drawn at a position 10 μm closer to the second surface than the line Ma1. Similarly, lines Ma3, Ma4...Ma n The area Sa1 is the area between the lines Ma1 and Ma2. n is a line parallel to the line Ma1 and is drawn 10×n μm from the line Ma1 in the second surface direction. n In the picture, the line Ma n and the line Ma (n+1) It is the area between.
[0024] Similarly, take a photograph of the second surface so that the arc can be confirmed. At this time, align the tangent of the center of the arc forming the second surface with the horizontal direction in the photograph. In the obtained photograph, draw a straight line Mb1 that passes through the intersection of the arc forming the first surface and the left and right ends of the photograph. It is preferable that the straight line Mb1 is parallel to the horizontal direction of the photograph, but it may be inclined.
[0025] Furthermore, the line Ma n Similarly, draw straight lines at 10 μm intervals from the second surface. In other words, draw a straight line Mb2 parallel to the straight line Mb1 at a position 10 μm closer to the first surface than the straight line Mb1. By repeating the same operation, draw straight lines Mb3...Mb n We can draw the region Sb n is the line Mb n and Mb(n+1) It is the area between.
[0026] Area Sa n The average diameter Da of the spherical structures in n , area Sb n The average diameter of the spherical structures in n is calculated as follows: First, an electron microscope photograph of the cross section in the radial direction is taken. The magnification at which the photograph is taken is not particularly limited as long as it is possible to measure the lengths of 15 or more spherical structures. For example, if the average diameter of the spherical structures is 1 to 3 μm, it is preferable to observe at a magnification of 1000 to 5000 times, since this ensures a sufficient number of spherical structures to calculate the average diameter.
[0027] In the photographing direction (the direction perpendicular to the paper surface of Figs. 1 and 2), solid parts that overlap with other spheres and are located behind the other spheres are excluded from the measurement object. The solid parts located behind the other spheres are exemplified as X1 to X4 in Fig. 2. In addition, solid parts that are interrupted by the outer edge of the photographed image are also excluded from the measurement object.
[0028] Of the remaining solid parts, for those that are not connected to other solid parts, such as solid part X5 shown in Figure 2, i.e., those whose entire outline can be confirmed, their long diameters (shown by the dashed line in Figure 2) are measured.
[0029] On the other hand, in solid parts connected to other solid parts, part of the outline cannot be confirmed. Therefore, when only part of the outline of a solid part can be confirmed, the whole image is estimated and measured as follows. For spheres X6, X7, etc. with a continuous outline, the longest line segment with both ends located on the outline is drawn, and the length is taken as the major axis. For spheres X8 to X10 with discontinuous outlines, the longest line segment with both ends located on one or two of the outlines is taken as the major axis. However, in the following cases (A) or (B), the corresponding solid part is excluded from the measurement target. (A) When the identifiable contour line is less than 50% of the entire approximately circular contour line predicted for the solid part (e.g., X11, 12). (B) When both ends of the above line segment are on both ends of a single continuous contour line (e.g. X8). In addition, if the tissue is interrupted at the edge of the electron micrograph used for judgment, the diameter of the spherical structures at that edge of the tissue is not measured. In this way, the diameter of the spherical structures (the major axis of the spherical structures) in each solid part to be measured is measured, and the arithmetic mean of these is calculated to determine the area Sa. n The average diameter Da of the spherical structures in n and the region Sb n The average diameter of the spherical structures in n is obtained.
[0030] The results of measuring the average diameter of the spherical structures in the thickness direction in FIG. 1 using this method are shown in FIG. 3. The horizontal axis is the distance in the thickness direction from the first surface, and the vertical axis is the average diameter of the spherical structures in each region. For convenience of drawing, the average diameter Da n is plotted at a distance of 10×(n−1) μm from the first surface, and for example, the average diameter Da3 of region Sa3 is plotted at a distance of 20 μm in the thickness direction.
[0031] The average diameter Da1 of the spherical structures in region Sa1 and the average diameter Db2 of region Sb2 satisfy the relational expression Da1>Db2. Since the average diameter Da1 of region Sa1 near the first surface is larger than the average diameter Db2 of region Sb2 near the second surface, the liquid resistance near the first surface is reduced, thereby improving water permeability.
[0032] The present inventors further determined the minimum value i of a natural number i that satisfies the following conditions (1) and (2): min 3≦i min It was found that permeability and separation properties are maintained for a long time when the above 3≦i min ≦(L-20) / 10, (L-20) / 10 small The values below a few points are rounded down. As will be described later, L represents the thickness of the layer of the spherical structure. (1) Da1 / Da i ≧1.1 (2)-0.3μm≦Da i -Db2≦0.3 μm Value i min is in the above range, that is, the area Sa has an average diameter smaller than the average diameter Da1 in the area closest to the first surface and is equivalent to the average diameter Db2 of the spherical structure in the area Sb2. i is located closer to the second surface than Sa2. This allows the clogging components to be dispersed more widely in the thickness direction of the membrane. As a result, it is possible to extend the operating period. min ≧3 is preferred, and i min ≧5 is preferred, i min More preferably, ≧1 / 2×L / 10. min For numbers ≧1 / 2×L / 10, round down to the nearest integer.
[0033] In Figure 3, the average diameter of the spherical structures decreases from the first surface to the second surface, i min At this time, Da1 / Da5=1.29, which satisfies condition (1). In the example of Figure 3, the film thickness (thickness L of the layer with the spherical structure) is 240 μm, so 3≦i min ≦(L-20) / 10 is also satisfied.
[0034] The thickness L of the spherical structure layer (hollow fiber membrane) is preferably 60 μm or more and 500 μm or less in consideration of water permeability and strength and elongation, more preferably 100 μm or more and 500 μm or less in consideration of dispersion of blocked sites in the thickness direction by depth filtration, and even more preferably 150 μm or more and 350 μm or less in consideration of membrane area.
[0035] In addition, the above value i min i min It is preferable that the thickness of the entire film is within the range of 3 / 4 from the first surface. min In the case of L×0.75 / 10 or less, the decimal places of L×0.75 / 10 are rounded down. Under this condition, the value i minFor all natural numbers m greater than and less than or equal to (L - 20) / 10, it is preferable that the following condition (4) is satisfied. (4) -0.30 ≤ Da m -Db2 ≤ 0.30
[0036] Since the regions satisfying the above (4) have mutually close average diameters, i min In the range where < m ≤ (L - 20) / 10, the structure is homogeneous. Also, from the definition of the range of m, since the region occupied by the homogeneous structure in terms of film thickness is 1 / 4 or more, sufficient separability can be obtained. Further, even when the film surface is damaged during film formation or operation, since the thickness of the layer with a homogeneous structure is within this range, deterioration of separability and blocking property can be suppressed. The layer with a uniform structure is preferably at least 10 μm or more. The layer with a uniform structure is more preferably 20 μm or more, and even more preferably 30 μm or more.
[0037] Also, it is preferable that 1.10 < Da1 / Da imin < 4.00. Since Da1 / Da imin is greater than 1.10, the dispersion of clogging components in the thickness direction is promoted. Also, since Da1 / Da n is less than 4.00, high strength can be maintained. The relationship of Da1 / Da i is more preferably 1.15 < Da1 / Da imin < 3.50, and even more preferably 1.20 < Da1 / Da imin < 3.00.
[0038] Also, it is preferable that 0.50 μm < Db2 < 2.00 μm. Since the average diameter Db2 of the spherical structure near the second surface is greater than 0.50 μm, a hollow fiber membrane with high water permeation performance can be obtained. Also, since Db2 is less than 2.00 μm, blocking property suitable for sterilization etc. can be imparted.
[0039] In addition, it is preferable that 1.00≦Da1 / Da2≦1.10. When Da1 / Da2 is 1.00 or more, the average diameter of the spherical structure is reduced from the first surface, so that a more preferable structure can be obtained in the present invention. When Da1 / Da2 is 1.10 or less, the average diameter of the spherical structure is gradually reduced from the first surface, so that i min This allows for a larger size, which is expected to improve filterability.
[0040] In addition, it is preferable that the first surface is the outer surface of the hollow fiber membrane (the outer surface of the hollow fiber membrane is the first surface). By having the first surface be the outer surface of the hollow fiber membrane, the membrane area can be made large.
[0041] Next, the relationship between the necking diameter of the spherical structure gap and the position in the thickness direction of the hollow fiber membrane will be described with reference to FIG. Figure 4 shows pore network model analysis images of a hollow fiber membrane, where (a) is near the first surface and (b) is near the second surface. The upper side of both images is the membrane surface. The pore network model is a model in which the void portion of a porous body is mechanically divided at constrictions, and spheres (hereinafter sometimes referred to as pores) corresponding to the volume of the divided regions and tubes (hereinafter sometimes referred to as throats) corresponding to the area of the divided surfaces are created, and the void portion of the porous body is represented as a network structure of pores and throats.
[0042] For pore network model analysis, a three-dimensional image formed by superimposing electron microscope photographs can be used. The size of the analysis area is not particularly limited. However, when the average diameter of the spherical structures is 1 to 3 μm, a three-dimensional image formed by superimposing photographs of a 50 μm square is preferable, since it ensures a sufficient number of constrictions in the gaps between the spherical structures for analysis.
[0043] Generally, the permeability of porous media is quantitatively analyzed by performing Hagen-Poiseuille flow analysis of the water flow in the throat. Here, if the porosity in the analysis area is equal, the larger the average throat diameter, i.e. the average neck diameter, the higher the permeability.
[0044] It is preferable that the average constriction diameter da1 of the spherical structure gap in the region Sa1 and the average constriction diameter db2 of the region Sb2 satisfy the relational expression da1>db2. That is, when the throat diameter obtained by pore network model analysis of the hollow fiber membrane is the constriction diameter of the spherical structure gap, the region Sa of 10×(n−1) to 10×n μm from the first surface n The average diameter of the constriction between the spherical structures in n and a region Sb of 10×(n−1) to 10×n μm from the second surface. n The average diameter of the constriction between the spherical structures in n It is preferable that da1>db2. When the average constriction diameter da1 of the region Sa1 near the first surface is larger than the average constriction diameter db2 of the region Sb2 near the second surface, the liquid resistance near the first surface is reduced, and water permeability is improved.
[0045] The present inventors further determined the minimum value j of a natural number j that satisfies the following conditions (1) and (2): min j is 3 or less min It was found that permeability and separation properties are maintained for a long time when the above 3≦j min In the case of (L-20) / 10 or less, the decimal places of (L-20) / 10 are rounded down. (1)da1 / da j ≧1.15 (2)da j -db2≦0.10μm Value j min is in the above range, that is, the area Sa has an average constriction diameter smaller than the average constriction diameter da1 in the area closest to the first surface and equivalent to the average constriction diameter db2 in the area Sb2. j is located closer to the second surface than Sa2. This allows the clogging components to be dispersed more widely in the thickness direction of the membrane. As a result, it is possible to extend the operating period. min ≧3 is preferred, j min More preferably, j is ≧5. min It is more preferable that L x 0.5 / 10. minWhen it is ≦ L×0.5 / 10, the decimal part of L×0.5 / 10 is truncated.
[0046] In addition, the region Sa created by the above analysis n The number of throats Na in n and the region Sb n The number of throats Nb in n It is preferable that Na1 < Nb2. That is, the number of throats Na in the region Sa obtained by the pore network model analysis n The number of throats Na in n and the region Sb n The number of throats Nb in n It is preferable that Na1 < Nb2. By having a large number of throats in the vicinity of the second surface, the number of branches of the permeation path increases and the detour performance at the time of clogging improves.
[0047] The region Sa n The number of throats Na in n refers to the number of throats whose center of gravity points are in the region Sa n and not all (the whole) of the throats need to be within the region Sa n to fit. The inventors further found that the minimum value k of the natural number k satisfying the following conditions (3) and (4) min is 3 ≦ k min ≦ (L - 20) / 10, and the water permeability and separation property are maintained for a long time. However, in the above 3 ≦ k min ≦ (L - 20) / 10, the decimal part of (L - 20) / 10 is truncated. (3) Na1 / Na k ≧ 0.90 (4) Nb2 - Na k ≦ 400 pieces However, the analysis region in the above analysis is a rectangular parallelepiped including a 50 μm square of any part of the first surface and a 50 μm square of the second surface facing the first surface, and Sa n and Sb n are regions of 50 μm × 50 μm × 10 μm.
[0048] The value kmin being within the above range means that there is a region Sa having a number of throats greater than the number of throats Na1 in the region closest to the first surface and equal to the number of throats Nb2 in the region Sb2 k is located closer to the second surface than Sa2. As a result, clogging components can be more widely dispersed in the film thickness direction. Consequently, it becomes possible to extend the operation period. k min k ≧ 3 is preferable, and k min k ≧ 5 is more preferable. Also, k min k ≦ L×0.5 / 10 is even more preferable. However, in k min ≦ L×0.5 / 10, the decimal part of L×0.5 / 10 is rounded down.
[0049] Also, it is preferable that 0.10 μm < db2 < 10.0 μm. Or, it is preferable that 0.1 μm < db2 < 10 μm. Since the average dilation diameter db2 of the gaps between the spherical structures near the second surface is larger than 0.10 μm, a hollow fiber membrane with high water permeability can be obtained. Also, since db2 is smaller than 10.0 μm, it is possible to impart a blocking property suitable for sterilization and the like.
[0050] Next, in the hollow fiber membrane according to the embodiment of the present invention, it is also preferable that a hydrophilic polymer is present on the surface and inside of the spherical structure. Thereby, excellent antifouling properties can be realized while maintaining water permeability. Examples of the hydrophilic polymer include polymers containing vinyl alcohol, ethylene glycol, vinyl pyrrolidone, methacrylic acid, allyl alcohol, cellulose, and vinyl acetate. Further, examples of the copolymer polymer containing a hydrophilic group include polyvinyl alcohol with a saponification degree of less than 99%, vinyl pyrrolidone·vinyl acetate copolymer polymer, vinyl pyrrolidone·vinyl caprolactam copolymer polymer, vinyl pyrrolidone·vinyl alcohol copolymer polymer, etc. It is preferable to contain at least one of these.
[0051] The content of the hydrophilic polymer is preferably 1.0 part by mass or more relative to 100 parts by mass of the hydrophobic polymer, more preferably 1.0 part by mass or more and 6.0 parts by mass or less, and even more preferably 1.0 part by mass or more and 4.0 parts by mass or less, relative to 100 parts by mass of the hydrophobic polymer. If the content of the hydrophilic polymer is more than 6.0 parts by mass, the hydrophilic polymer may narrow the flow path, resulting in a decrease in liquid permeability. For example, if the spherical structure is made of polyvinylidene fluoride resin, the content of the hydrophilic polymer per 100 parts by mass of the polyvinylidene fluoride resin is preferably within the above range.
[0052] Furthermore, in the hollow fiber membrane according to the embodiment of the present invention, when the ratio (mass%) of the hydrophilic polymer to the polyvinylidene fluoride resin after the hollow fiber membrane is immersed in a 3000 ppm sodium hypochlorite aqueous solution (pH 12.5) at 60°C for 30 hours is P1, and the ratio (mass%) of the hydrophilic polymer to the polyvinylidene fluoride resin before the immersion is P0, the percentage of the ratio P1 to the P0, P1 / P0, is preferably 70% or less. The hydrophilic polymer present on the surface of the spherical structure is removed from the hollow fiber membrane by immersing it in a sodium hypochlorite aqueous solution, but the hydrophilic polymer present inside remains. Therefore, P1 / P0 represents the mass ratio of the hydrophilic polymer inside the spherical structure to the total mass of the hydrophilic polymer. The content of hydrophilic polymer in the hollow fiber membrane can be quantified by X-ray photoelectron spectroscopy (XPS), attenuated total reflection infrared spectroscopy (ATR-IR), proton nuclear magnetic resonance spectroscopy (1H-NMR), etc. 1 The case where a hollow fiber membrane containing a fluororesin-based hydrophobic polymer is used for H-NMR will be explained as an example. 1 To quantify the amount of hydrophilic polymer introduced by H-NMR, a 2 cm hollow fiber membrane was dissolved in 1 mL of dimethyl sulfoxide. 1 For example, when the spherical structure is made of polyvinylidene fluoride resin, this measurement is carried out at two arbitrary points of the hollow fiber membrane, and the amount of hydrophilic polymer is calculated when the ratio of the detected PVDF resin is taken as 100.
[0053] <Manufacturing method of hollow fiber membrane> A method for producing a hollow fiber membrane according to an embodiment of the present invention includes the following steps (a) to (d) when the spherical structures are made of a polyvinylidene fluoride resin. (a) A step of dissolving a polyvinylidene fluoride resin in a poor solvent to obtain a polyvinylidene fluoride resin solution. (b) maintaining the polyvinylidene fluoride resin solution under conditions in which the formation of primary nuclei proceeds. (c) after the step (b), a step of discharging a polyvinylidene fluoride resin solution in the form of a hollow fiber through a pipe and a die, and imparting a temperature gradient in the thickness direction of the polyvinylidene fluoride resin solution in at least one of the pipe and the die. (d) after the step (c), a step of solidifying the polyvinylidene fluoride resin solution by solid-liquid type thermally induced phase separation by immersing the polyvinylidene fluoride resin solution in a cooling bath.
[0054] In addition, it is preferable that the temperature gradient ΔT (° C.) and the time t (seconds) for which the temperature gradient is applied in the step (c) are within the range of 50≦ΔT×t≦300.
[0055] In step (a), a poor solvent is used to induce solid-liquid type thermally induced phase separation in the subsequent step (d). Examples of solvents that induce solid-liquid type thermally induced phase separation include medium-chain alkyl ketones, esters, organic carbonates, and mixtures thereof, such as cyclohexanone, isophorone, γ-butyrolactone, methyl isoamyl ketone, dimethyl sulfoxide, and propylene carbonate.
[0056] The higher the resin concentration in the resin solution, the easier it is to form primary nuclei, and therefore the smaller the average diameter of the spherical structures, resulting in a separation membrane with high strength and elongation. However, the lower the resin concentration in the resin solution, the higher the porosity of the separation membrane produced, and the higher the water permeability. From these viewpoints, in order to achieve both water permeability and strength and elongation, the resin concentration in the resin solution is preferably 30% by weight or more and 60% by weight or less.
[0057] The temperature T1°C during dissolution in step (a) is preferably equal to or higher than the crystallization temperature Tc°C. The crystallization temperature Tc can be measured using a differential scanning calorimetry (DSC) device. The crystallization temperature Tc is the rising temperature of the crystallization peak observed in the process of sealing a mixture of the same composition as the resin solution used for film formation in a sealed DSC vessel, heating it to the dissolution temperature at a heating rate of 10°C / min, holding it for 30 minutes to dissolve it uniformly, and then cooling it at a heating rate of 10°C / min.
[0058] Specifically, the temperature T1°C is preferably (Tc+20)°C or higher, and more preferably (Tc+30)°C or higher. The temperature T1°C is preferably (Tc+100)°C or lower, and more preferably (Tc+90)°C or lower. More specifically, the temperature T1°C is preferably 100°C or higher, and more preferably 110°C or higher. The temperature T1°C is preferably 200°C or lower, and more preferably 190°C or lower.
[0059] Furthermore, in order to uniformly form spherical structures by solid-liquid thermally induced phase separation, it is preferable that the polyvinylidene fluoride resin solution is uniformly dissolved, and therefore the dissolution time is preferably 2 hours or more, and more preferably 4 hours or more.
[0060] The resin solution may contain other additives.
[0061] Step (b) is a step of holding the polyvinylidene fluoride resin solution under conditions that allow the formation of primary nuclei. The process of forming the spherical structure is considered to be a crystallization process based on the results of X-ray diffraction, etc. In general, the first crystals that form when a crystalline polymer such as polyvinylidene fluoride resin crystallizes are called primary nuclei. This primary nucleus grows and becomes a single spherical structure.
[0062] The growth of the spherical structures continues until they collide with each other, at which point the growth stops, and the final particle size of the spherical structures depends on the number of primary nuclei initially generated. In other words, it is considered that it is preferable to form a large number of primary nuclei to obtain small microspherical structures, and it is preferable to form a small number of primary nuclei to obtain large giant spherical structures. In other words, in controlling the spherical structures, it is effective to control the progress of the formation of primary nuclei.
[0063] The progress of the formation of primary nuclei in the resin solution can be controlled by temperature, pressure and / or time. Specifically, the primary nuclei formation temperature T2 is preferably equal to or higher than the temperature of the cooling bath in step (d), more preferably equal to or higher than the crystallization temperature Tc°C, and even more preferably equal to or higher than (Tc+20)°C. In addition, the temperature at which the resin is dissolved is preferably equal to or lower than T1°C, and more preferably equal to or lower than (Tc+55)°C.
[0064] The pressure of the resin solution is preferably 0.5 MPa or more, more preferably 0.8 MPa or more. By keeping the resin solution under this pressure, the formation of primary nuclei at the above temperature proceeds stably. The upper limit of the pressure is preferably 3.0 MPa.
[0065] The time for maintaining the conditions for the formation of primary nuclei is preferably 10 seconds or more, and more preferably 20 seconds or more. The formation of primary nuclei of crystals in thermally induced phase separation proceeds gradually in a region from the melting temperature to the crystallization temperature Tc or higher (referred to as the "metastable region" in this specification), but by subjecting the resin solution to the above conditions, the number of primary nuclei that form relatively stably can be controlled.
[0066] Specifically, step (c) is to extrude the resin solution from step (b) into a hollow fiber shape from a tubular forming die. At this time, the resin solution may be sent to the forming die via a pipe provided in the latter stage of step (b) and the former stage of step (c). An example of the shape of the forming die is shown in FIG. 5. As shown in FIG. 5, a die 1 for producing a hollow fiber membrane includes an inner nozzle 11 and an annular nozzle 12 provided on the outside of the inner nozzle 11 so as to surround the inner nozzle. As shown in FIGS. 6 and 7, the inner nozzle 11 includes an inner nozzle inlet 111 and an inner nozzle outlet 112, and the annular nozzle 12 includes an annular nozzle inlet 121 and an annular nozzle outlet 122. The resin solution is extruded from the annular nozzle of the outer tube, and at the same time, a fluid forming a hollow portion is extruded from the nozzle of the inner tube, so that the resin solution is molded (processed) into a hollow shape. An example of the shape of the piping is shown in Fig. 8. A piping 2 is connected to a die 1, and more specifically, a piping outlet 132 and an annular nozzle inlet 121 are connected. A resin solution is introduced from the piping inlet 131, and the resin solution discharged from the piping outlet 132 is introduced into the annular nozzle 12 from the annular nozzle inlet 121.
[0067] Furthermore, step (c) includes a step of providing a temperature gradient in the thickness direction of the polyvinylidene fluoride resin solution in at least one of the pipe or the spinneret. "Providing a temperature gradient in the thickness direction" refers to making the temperature of one part in the thickness direction of the resin solution flowing through the pipe or the resin solution formed into the shape of a hollow fiber in the spinneret different from the temperature of the other part. For example, in the resin solution formed into a hollow fiber shape, it refers to making the temperature relatively higher from one surface to the other surface.
[0068] As a specific method for providing a temperature gradient in the thickness direction, for example, at least one of the following (1) to (3) may be carried out. (1) The temperature of the die 1 is made higher or lower than the temperature of the resin solution being supplied. (2) The temperature of the pouring liquid passing through the inner nozzle 11 of the die 1 is made higher or lower than the temperature of the resin solution being supplied. (3) The temperature of the upstream pipe that delivers the resin solution to the nozzle 1 is made higher or lower than the temperature of the resin solution being supplied. By carrying out at least one of the above (1) to (3), the spherical structures near either the outer surface or the inner surface of the hollow fiber membrane can be made larger than the spherical structures near the other surface. The temperature of the spinneret 1, the temperature of the injection liquid, and the temperature of the piping in the above (1) to (3) are each represented as T3 (°C).
[0069] In the method of increasing the temperature relatively, it is possible to lower the resin temperature in areas other than the area where it is desired to form spherical structures having a large average diameter, but in this case, the effect of reducing the size of the spherical structures on the side where the resin temperature is lowered is smaller than the effect of increasing the size of the spherical structures by increasing the resin temperature, because the formation of primary nuclei proceeds gradually in the metastable region as described above.
[0070] For example, when a temperature gradient is applied to a resin solution in a relatively short time by cooling at a specific temperature, the conditions are insufficient for the formation of primary nuclei. On the other hand, the primary nuclei after formation are relatively greatly affected by the increase in temperature of the resin solution and are reduced, and the number of spherical structures after solidification is reduced. In other words, the primary nuclei of a resin solution change differently in response to temperature changes of increasing and decreasing temperature.
[0071] Therefore, in the case of changing the diameter of the spherical structures by "applying a temperature gradient", a process of partially increasing the temperature of the resin solution is preferably used.
[0072] The means for controlling the temperature in the above (1) to (3) (temperature control means) is not limited to a specific device or method. Examples of the temperature control means are shown below. In the above (1), the die may be heated by a heater disposed around the die, or the die may be heated by a mold temperature regulator before use. In the above (2), the injection liquid may be heated by a heater or the like before it reaches the base 1. The injection liquid may be heated before it is passed through the piping connected to the base 1, or the piping itself may be heated by a heater. In the above (3), the piping may be heated by a heater or a mold temperature regulator, etc. Regarding the shape of the piping, a circular tubular piping is preferred from the viewpoint of providing a temperature gradient in the thickness direction of the hollow fiber membrane. Moreover, the "temperature" T3 in the above (1) to (3) is the set temperature of each temperature control means (for example, a heater or a mold temperature regulator).
[0073] In terms of "providing a temperature gradient in the thickness direction", the above-mentioned (1) method of increasing the temperature of the die 1 and (2) method of increasing the temperature of the injection liquid are preferable in terms of suppressing unevenness in the temperature gradient in the circumferential direction of the hollow fiber membrane. In the above-mentioned (3) method of increasing the temperature of the pipe in the front stage of feeding the liquid to the die 1, it is necessary to design the pipe and die so that the resin solution that is heated near the wall surface of the pipe in the pipe is also passed near the wall surface in the die 1. However, compared to the case of heating the die 1, it is not necessary to heat the injection liquid. As will be described later, the injection liquid may boil and air bubbles may be mixed in depending on the heating conditions, so the method (3) in which only the resin solution can be heated is also preferable. In this case, it is preferable to control the temperature of the die 1 in the rear stage to a temperature of T2 to T3 in order to suppress cooling.
[0074] In addition, when heating the pipes, it is preferable to heat the pipes laid in the vertical direction. In the case of a pipe laid in the horizontal direction, the resin solution is mixed in the pipe due to its own weight, so it is difficult to maintain the temperature gradient in the thickness direction, but in the case of a pipe laid in the vertical direction, the mixing of the resin solution in the thickness direction can be suppressed.
[0075] In the process of applying a temperature gradient, if the temperature gradient ΔT (℃) and the time t (seconds) for applying the temperature gradient are 50≦ΔT×t≦300, what is the minimum value i of the natural number i that satisfies the following conditions (1) and (2)? min 3≦i min <=(L-20) / 10. (1) Da1 / Da i ≧1.1 (2)-0.3μm≦Da i - Db2 ≤ 0.3 μm. Here, the temperature gradient ΔT is the absolute value of T3 - T2, and the time t is the time during which the resin solution flows through the pipe or base to which the temperature gradient is applied (referred to as the residence time). By ΔT×t≧50, a thermal gradient can be applied to the deep part in the thickness direction of the resin solution, so that a gradient can also be generated in the diameter of the spherical structure from the surface of the membrane to the deep part in the thickness direction. If ΔT×t is too large, the thermal uniformity in the thickness direction of the resin solution increases, so the diameter of the spherical structure in the obtained membrane also becomes uniform in the thickness direction. On the other hand, by ΔT×t≦300, a gradient of the spherical structure as described above can be formed. Therefore, 50≦ΔT×t≦300 is preferable, and 60≦ΔT×t≦250 is more preferable.
[0076] The time t for applying the temperature gradient is preferably 0.1 second or more and 20 seconds or less, and more preferably more than 5 seconds and 10 seconds or less. The time t for applying the temperature gradient (heating time when the resin solution is heated) is the time it takes for the resin solution to pass through the base when a temperature gradient is applied to the resin solution by heating the base 1 for the hollow fiber membrane shown in FIGS. 5 to 7. Also, when a temperature gradient is applied to the resin solution by heating the pipe upstream of the base 1, the time t is the time it takes to pass through the pipe. For example, as shown in FIG. 8, when the resin solution is supplied from the pipe 2 to the base 1 and the outer peripheral portion of the pipe 2 is heated, the time it takes for the resin to pass from the pipe inlet 131 to the pipe outlet 132 is the time t.
[0077] Furthermore, in step (c), it is preferable that the thickness Ls of the polyvinylidene fluoride resin to which the temperature gradient is applied satisfies 5 < Ls / L < 40 with respect to the thickness L of the layer of the spherical structure. The thickness Ls of the polyvinylidene fluoride resin to which the temperature gradient is applied is the channel thickness of the pipe to which the temperature gradient is applied. For example, when a temperature gradient is applied to the base 1 as shown in FIG. 6, since the polyvinylidene fluoride resin passes through the annular nozzle 12, the thickness Ls of the polyvinylidene fluoride resin is the thickness of the annular nozzle 12. That is, it is the value obtained by subtracting the inner diameter from the outer diameter of the annular nozzle 12 and dividing by 2.
[0078] Also, when applying a temperature gradient to the pipe in the previous stage of feeding liquid to the nozzle 1, if the pipe through which the polyvinylidene fluoride resin passes is a circular pipe, its radius becomes the thickness Ls of the polyvinylidene fluoride resin. When the pipe has a shape other than a circular pipe, the equivalent circular radius of the pipe becomes the thickness Ls of the polyvinylidene fluoride resin. The equivalent circular radius is a value obtained by 2×A / P from the cross-sectional area A of the pipe and the wetted edge length P of the pipe. The wetted edge length P is the perimeter of the part in contact with the liquid in the pipe cross-section.
[0079] The pipe position for calculating the thickness Ls is the position closest to the heat source. When the heat source is a heat source that heats at a point such as a heat medium or a rod heater that passes liquid through the mold, it is the channel thickness at the position closest to the heat source in the pipe through which the polyvinylidene fluoride resin passes. When the heat source is a band heater or a double pipe that heats the pipe in a plane, it is the channel thickness at the center position within the range covered by the heat source in the length direction of the pipe through which the polyvinylidene fluoride resin passes.
[0080] By having Ls / L > 5, heat transfer across the entire thickness of the spherical structure layer is prevented, and a structure can be obtained in which the spherical structure on the first surface side, such as the hollow fiber membrane according to the embodiment of the present invention, is coarse and the spherical structure on the second surface side is dense. By having Ls / L < 40, it is possible to prevent only the spherical structure in the region Sa1 on the first surface side from becoming coarse, and a structure can be obtained in which the size of the spherical structure attenuates up to the second surface side. 10 < Ls / L < 40 is more preferable, and 15 < Ls / L < 35 is even more preferable.
[0081] The polyvinylidene fluoride resin solution discharged in a hollow fiber shape passes through the air and then is immersed in a cooling bath. At this time, it is preferably passed through the air for 0.3 seconds or more. The time of passing through the air is the time from when the polyvinylidene fluoride resin solution discharged from the nozzle in step (c) reaches the cooling bath, convenience which will be hereinafter described as the "idle running time" above.
[0082] A free-running time of 0.3 seconds or more is preferable because it ensures time for the heat applied in step (c) to be transferred to the inner surface. It is preferably 1 second or more, and more preferably 1.5 seconds or more. In addition, since cooling from the outer surface progresses when the free-running time is long, it is preferably 5 seconds or less, and more preferably 3 seconds or less.
[0083] The idle time can be calculated using the following formula: Idle time (sec) = Idle distance (m) / Take-up speed in cooling bath (m / sec) Here, the free running distance is the length of a straight line drawn vertically downward from the bottom of the die to the top surface of the cooling bath. The take-up speed in the cooling bath can be calculated from the rotation speed (rpm) of the cooling bath roll and the roll diameter (m) using the following formula. π is the constant of the circumference of a circle. For example, if a roll with a diameter of 0.2 m rotates at a speed of 10 rpm, the take-up speed is approximately 0.1 m / sec. Take-off speed (m / sec) = Roll rotation speed (rpm) / 60 × π × Roll diameter (m) When passing through air, the temperature, humidity, solvent vapor concentration, etc. may be adjusted.
[0084] In step (d), after step (c), the polyvinylidene fluoride resin solution is immersed in a cooling bath to solidify the polyvinylidene fluoride resin solution by solid-liquid type thermally induced phase separation. Thermally induced phase separation is a method in which a resin solution dissolved in a poor solvent or a good solvent at a temperature equal to or higher than the crystallization temperature Tc is solidified by cooling. Examples of thermally induced phase separation include the following (A) and (B). (A) Liquid-liquid type: A resin solution that is uniformly dissolved at high temperatures separates into a thick phase and a thin phase of resin as the temperature drops due to a decrease in the dissolving ability of the solution. (B) A resin solution that is uniformly dissolved at high temperatures drops below the crystallization temperature Tc as the temperature drops, causing crystallization and phase separation into a polymer solid phase and a polymer dilute solution phase. This is a solid-liquid type.
[0085] In the liquid-liquid type, a fine three-dimensional network structure is formed by the dense phase, whereas in the solid-liquid type, a spherical structure is formed. Therefore, the solid-liquid type is preferably used for producing the separation membrane according to the embodiment of the present invention.
[0086] The cooling bath is preferably a mixed liquid containing a poor solvent or good solvent with a concentration of 50% by weight to 95% by weight and a non-solvent with a concentration of 5% by weight to 50% by weight. By setting the non-solvent concentration to 50% by weight or less, solidification by thermally induced phase separation can be promoted preferentially over solidification by non-solvent induced phase separation. Note that, although the solidification rate increases with a lower concentration of the good solvent, it is possible to promote solidification and smooth the surface of the separation membrane by lowering the temperature of the cooling bath even if the concentration of the good solvent is high.
[0087] As the poor solvent, it is preferable to use the same poor solvent as that of the resin solution. Examples of good solvents include lower alkyl ketones such as N-methyl-2-pyrrolidone, dimethylsulfoxide, dimethylacetamide, dimethylformamide, methyl ethyl ketone, acetone, tetrahydrofuran, tetramethylurea, and trimethyl phosphate, esters, amides, and mixtures thereof.
[0088] Examples of non-solvents include water, hexane, pentane, benzene, toluene, methanol, ethanol, carbon tetrachloride, o-dichlorobenzene, trichloroethylene, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butylene glycol, pentanediol, hexanediol, low molecular weight polyethylene glycol, and other aliphatic hydrocarbons, aromatic hydrocarbons, aliphatic polyhydric alcohols, aromatic polyhydric alcohols, chlorinated hydrocarbons, other chlorinated organic liquids, and mixed solvents thereof.
[0089] In this specification, a "good solvent" refers to a solvent that can dissolve 5% by weight or more of a solute even at a low temperature below 60° C. A "poor solvent" refers to a solvent that cannot dissolve 5% by weight or more of a solute at a low temperature below 60° C., but can dissolve 5% by weight or more in a high temperature range of 60° C. or higher and below the melting point of a polyvinylidene fluoride resin. A "non-solvent" refers to a solvent that does not dissolve or swell a solute up to the melting point of the solute or the boiling point of the solvent.
[0090] By lowering the cooling bath temperature T4 below the crystallization temperature Tc of polyvinylidene fluoride resin, solid-liquid phase separation is induced. Below, we will explain the relationship between the cooling bath temperature T4, the crystallization temperature Tc, and the primary nucleation temperature T2.
[0091] In solid-liquid thermally induced phase separation, crystallization (hereinafter also referred to as nucleation) occurs due to cooling, and the resulting crystal nuclei grow, resulting in phase separation into a polymer solid phase and a polymer dilute solution phase. In solid-liquid phase separation, it is believed that growth occurs starting from the primary nuclei formed in step (b), and random nucleation and growth does not start from the primary nuclei. In growth starting from the primary nuclei, the number of spherical structures generated correlates with the number of primary nuclei. The growth of the spherical structures continues until they come into contact with the surrounding spherical structures, so if the number of primary nuclei is small, growth is promoted and coarse spherical structures are generated, and if the number of primary nuclei is small, dense spherical structures are generated.
[0092] This growth starting from the primary nuclei and random nucleation and growth not starting from the primary nuclei depend on the cooling rate of the resin solution. That is, it depends on the difference between the primary nucleation temperature T2 and the cooling bath temperature T4. The smaller the difference, the easier the former crystallization will proceed, and the larger the difference, the easier the latter crystallization will proceed. That is, in step (c), when a temperature gradient is applied in the thickness direction of the hollow fiber membrane and the resin solution in a state in which the number of primary nuclei changes in the thickness direction is rapidly cooled, random nucleation occurs regardless of the number of primary nuclei, so that a structure in which the average diameter of the spherical structures changes in the thickness direction of the hollow membrane is unlikely to occur. On the other hand, when a resin solution in a state in which the number of primary nuclei changes in the thickness direction is gradually cooled, growth starting from the primary nuclei progresses, and a hollow fiber membrane in which the average diameter of the spherical structures changes in the thickness direction can be obtained.
[0093] The crystallization temperature Tc is also affected by the cooling rate of the resin solution. The faster the cooling rate, the higher the crystallization temperature, and the faster the phase separation will proceed. The cooling rate depends on the difference between the primary nucleation temperature T2 and the cooling bath temperature T4.
[0094] In the method for producing a hollow fiber membrane according to an embodiment of the present invention, after much trial and error in consideration of the above-mentioned characteristics, it was discovered that by producing the membrane under the following temperature conditions, the average diameter of the spherical structures in the thickness direction of the hollow membrane changes, thereby arriving at the present invention. (Tc-T4) / (T2-T4)<0.50
[0095] T2 - T4 is a parameter representing the overall cooling rate, while Tc - T4 is a parameter contributing to growth. It has been found that by reducing the temperature difference contributing to growth within the overall cooling rate, growth starting from primary nuclei proceeds. More preferably, (Tc - T4) / (T2 - T4) < 0.45, and even more preferably, (Tc - T4) / (T2 - T4) < 0.40. In the method for manufacturing a hollow fiber membrane according to an embodiment of the present invention, it is preferable to satisfy the relationship of 15 < Tc - T4 < 35. When Tc - T4 is greater than 15°C, it is possible to suppress the coagulation time from becoming too long and prevent the manufacturing equipment from becoming excessively large. Also, when Tc - T4 is less than 35°C, it has been found that the growth starting from the above-mentioned primary nuclei proceeds.
[0096] Also, T2 - T4 is preferably less than 100°C, and more preferably less than 80°C.
[0097] The hollow fiber membrane coagulated in step (d) may be manufactured through the following steps thereafter. After step (d), it is also preferable to expand the voids between the spherical structures to improve water permeability and perform stretching to enhance the breaking strength. The temperature around the membrane during stretching is preferably 50°C or higher and 140°C or lower, more preferably 55°C or higher and 120°C or lower, and even more preferably 60°C or higher and 100°C or lower. The stretching ratio is preferably 1.1 times or more and 4 times or less, more preferably 1.1 times or more and 2 times or less.
[0098] When stretching is performed under a temperature condition of 50°C or higher, stable and uniform stretching can be achieved. When stretching is performed under a temperature condition of 140°C or lower, since stretching is performed at a temperature lower than the melting point (177°C) of the polyvinylidene fluoride - based resin, the membrane does not melt even when stretched, and the voids can be expanded while maintaining the membrane structure, thereby improving the water permeability.
[0099] Also, stretching is preferably performed in a liquid because temperature control is easier. However, stretching may also be performed in a gas such as steam.
[0100] Although water is the preferred liquid because it is simple, low molecular weight polyethylene glycol or the like can also be preferably used when stretching is performed at a temperature of about 90°C or higher. On the other hand, when such stretching is not performed, the water permeability and breaking strength decrease compared to when stretching is performed, but the breaking elongation and blocking property improve. Therefore, the presence or absence of a stretching step and the stretching ratio in the stretching step can be appropriately set depending on the application of the separation membrane.
[0101] The above-mentioned temperature conditions are applied to the temperature of the liquid when the stretching is performed in a liquid, and to the temperature of the gas when the stretching is performed in a gas. Note that these manufacturing methods are applicable to any thermoplastic resin that forms a spherical structure by thermally induced phase separation without any particular limitation.
[0102] Also, after step (d), a heat treatment may be performed. The glass transition temperature of polyvinylidene fluoride resin is around -49°C, and depending on the usage environment, shrinkage progresses gradually. Therefore, by thermally shrinking the resin in advance at a temperature higher than the usage temperature, it is possible to suppress shrinkage during use. It is preferable to perform heat treatment at a temperature higher than the usage temperature by 10°C, more preferably at a temperature higher than the usage temperature by 20°C, until shrinkage disappears.
[0103] In addition, it is preferable to further include the following steps (e) and (f) after the step (d). (e) A step of introducing a hydrophilic polymer into the hollow fiber membrane. (f) a step of carrying out a heat treatment at 100° C. or more after the step (e).
[0104] A method for introducing a hydrophilic polymer into a hollow fiber membrane will be described. Examples of the method include passing an aqueous solution of a hydrophilic polymer through or immersing the hollow fiber membrane to physically adsorb the hydrophilic polymer, or irradiating the membrane with radiation to insolubilize the hydrophilic polymer, or forming a covalent bond through a chemical reaction with a reactive group present in the hollow fiber membrane. In particular, irradiation with radiation is preferred because it allows the hydrophilic polymer to adhere more firmly to the surface of the spherical structure. That is, in step (e), it is preferred to pass an aqueous solution of a hydrophilic polymer through the hollow fiber membrane and then irradiate the membrane with radiation.
[0105] Furthermore, by the above-mentioned hydrophilic polymer introduction process, it is possible to adhere the hydrophilic polymer to the surface of the spherical structures, thereby improving the dirt resistance, as compared to, for example, a method in which a film is formed after kneading a hydrophilic polymer into a film-forming solution.
[0106] If the concentration of the hydrophilic polymer aqueous solution is too low, a sufficient amount of hydrophilic polymer will not be introduced. Therefore, the copolymer (hydrophilic polymer) concentration in the aqueous solution is preferably 10 ppm or more, more preferably 100 ppm or more, and most preferably 500 ppm or more. However, if the concentration of the hydrophilic polymer in the aqueous solution is too high, there is a concern that the amount of elution from the module will increase, so the copolymer (hydrophilic polymer) concentration in the aqueous solution is preferably 100,000 ppm or less, and more preferably 10,000 ppm or less.
[0107] In addition, when the hydrophilic polymer is poorly soluble or insoluble in water, the hydrophilic polymer may be dissolved in an organic solvent that does not dissolve the hollow fiber or a mixed solvent of water and an organic solvent that is compatible with water and does not dissolve the hollow fiber. Specific examples of the organic solvent that can be used for the organic solvent or the mixed solvent include alcohol solvents such as methanol, ethanol, and propanol, but are not limited to these.
[0108] Furthermore, if the ratio of the organic solvent in the mixed solvent is high, the hollow fibers may swell, which may result in changes in the pore size of the hollow fiber membrane, etc. Therefore, the mass fraction of the organic solvent in the mixed solvent is preferably 60% or less, more preferably 10% or less, and most preferably 1% or less.
[0109] The radiation irradiation may be α-rays, β-rays, γ-rays, X-rays, ultraviolet rays, or electron beams. Here, from the viewpoint of safety and simplicity, radiation methods using γ-rays or electron beams are preferred. The radiation exposure dose is preferably 15 kGy or more, more preferably 25 kGy or more. By using 15 kGy or more, the hydrophilic polymer can be effectively introduced. In addition, the above-mentioned exposure dose is preferably 100 kGy or less. If the exposure dose exceeds 100 kGy, the copolymer may be prone to three-dimensional crosslinking or decomposition of the ester group portion of the vinyl carboxylate monomer unit.
[0110] In order to suppress the crosslinking reaction during irradiation with radiation, an antioxidant may be used. The antioxidant refers to a substance that has the property of easily donating electrons to other molecules, and examples thereof include water-soluble vitamins such as vitamin C, polyphenols, and alcohol solvents such as methanol, ethanol, and propanol, but are not limited thereto. These antioxidants may be used alone or in combination of two or more kinds. When using an antioxidant, safety must be taken into consideration, so that antioxidants with low toxicity such as ethanol and propanol are preferably used.
[0111] The amount of the hydrophilic polymer introduced into the hollow fiber membrane can be quantified by attenuated total reflection infrared spectroscopy (ATR-IR) as described above. If necessary, it can also be quantified by X-ray photoelectron spectroscopy (XPS) or the like.
[0112] It is also preferable to heat-treat the hollow fiber membrane after introducing the hydrophilic polymer into the hollow fiber membrane. Examples of the heat-treating process of the hollow fiber membrane include a method of applying heat in a dry state and a method of applying heat under humid conditions such as water vapor. By performing the heat treatment, a part of the polyvinylidene fluoride resin shrinks, and a part of the hydrophilic polymer can be incorporated into the inside of the spherical structure. If the heat treatment temperature is too low, a sufficient amount of the hydrophilic polymer is not introduced, so the heat treatment temperature is preferably 100°C or higher, more preferably 120°C or higher, and most preferably 150°C or higher. On the other hand, if the heat treatment temperature is too high, it will exceed the melting point of polyvinylidene fluoride, and after the hollow fiber membrane is dissolved, the micropores will be blocked and the water permeability will decrease. Therefore, the heat treatment temperature is preferably below the melting point of the vinylidene fluoride copolymer. EXAMPLES
[0113] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0114] (1) Area Sa n The average diameter Da n , the thickness L of the layer of the spherical structure (film thickness L) A cross section perpendicular to the length of the hollow fiber membrane (cross section parallel to the thickness direction) was photographed at 1000x magnification using a Hitachi electron microscope (SU1510) so that the arc forming the first surface was captured. In the photograph obtained, straight lines Ma1, Ma2...Ma n At 10μm intervals, draw a straight line Ma n and Ma n+1 , the area enclosed by the left and right edges of the photo Sa n The major axis of all measurable spherical structures was measured. The arithmetic mean was calculated to obtain the average diameter Da n obtained. A first surface and an area Sa are recorded in one image. n When the images could not be aligned, multiple fields of view were photographed at the same magnification, with the fields shifted in the thickness direction so that some of the fields overlapped. The photographs were then joined together so that the same structures overlapped, resulting in a continuous image in the thickness direction. The thickness L of the layer of the spherical structure (membrane thickness L) was determined by the following method. The membrane thickness L is calculated from the outer diameter and inner diameter of the hollow fiber membrane by L = (outer diameter - inner diameter) / 2. The outer diameter and inner diameter of the hollow fiber membrane are measured by cutting the hollow fiber membrane on a plane perpendicular to the axial direction with a single-edged blade or the like, observing the cross section with a microscope or the like, and measuring the diameter of the circle. If the circle is flattened, the length of the longest diameter part of the circle (major axis) and the length of the shortest diameter part (minor axis) can be measured and the average of the two can be used as the diameter.
[0115] (2) Average diameter Db2 of region Sb2 A cross section perpendicular to the length of the hollow fiber membrane (cross section parallel to the thickness direction) was photographed at 1000x magnification using an electron microscope. In the image obtained, straight lines Mb1, Mb2, and Mb3 were drawn from the second surface of the separation membrane to the first surface, and the major diameters of all measurable spherical structures in the area Sb bounded by Mb2, Mb3, and the left and right ends of the photograph were measured. The arithmetic mean of the obtained values was calculated to obtain the average diameter Db2.
[0116] (3) Area Sa n Average diameter of the constriction (average diameter of the constriction) da n and the number of throats Na n , area Sb n Average constriction diameter (average diameter of constriction) db n and the number of throats Nb n After coating the hollow fiber membrane with RuO4, the voids were filled with resin, and 200 photographs of a cross section perpendicular to the length of the hollow fiber membrane (cross section parallel to the thickness direction) were taken at 250 μm intervals using the focused ion beam etching function of an FEI electron microscope (HeliosG4 CX). Photographs were taken of cubes with sides of 50 μm each, starting from the part tangent to the arc that forms the first surface toward the second surface, and the rectangular parallelepiped formed by connecting the cubes was analyzed using a pore network model. The center of gravity and throat diameter of each throat were determined, and the area Sa n The average throat diameter of the throat with the center of gravity of is the average neck diameter da n Calculate as follows: and add the throat number Na nIn addition, as an analysis target using the pore network model, a cube with a side length of 50 μm was photographed from the part tangent to the arc forming the second surface toward the first surface, and the area Sb n Average constriction diameter (average diameter of constriction) db n and the number of throats Nb n was calculated.
[0117] (4) Water permeability of separation membrane A small module with a length of about 10 cm was prepared, consisting of 1 to 10 hollow fiber membranes. Distilled water was fed from the first surface and filtered at a temperature of 25°C and a filtration differential pressure of 18.6 kPa. The amount of permeated water (m 3 ) and the value obtained is expressed as unit time (hr) and unit effective membrane area (m 2 ) and calculated per 50 kPa.
[0118] (5) Crystallization temperature Tc of polyvinylidene fluoride resin solution Using a Seiko Electronics DSC-620-0, a mixture of polyvinylidene fluoride resin and solvent, which is the same composition as the film-forming polymer stock solution, was sealed in a sealed DSC vessel, heated to the dissolution temperature at a heating rate of 10°C / min, and held for 30 minutes to dissolve uniformly. After that, the temperature at which the crystallization peak began to rise during the cooling process at a rate of 10°C / min was taken as the crystallization temperature Tc.
[0119] (6) Evaluation of operation with actual liquid A commercially available unfiltered beer containing brewer's yeast, "Ginga Kogen Beer" (product name; hereafter referred to as "evaluation beer"), was used. 2 L of evaluation beer maintained at 0°C was prepared in a vessel, and the evaluation beer was pumped from this vessel through the outer surface of the hollow fiber membrane and returned to the vessel, while the filtrate filtered by the hollow fiber membrane was collected in a vessel different from the vessel containing the evaluation beer. At that time, the inlet and outlet pressures of the evaluation beer to the module and the pressure on the filtration side were made meable. The evaluation beer was introduced so that it flowed at a membrane surface linear velocity of 1.5 m / sec. The filtration rate was also adjusted to 1 m / d, and constant flow filtration was performed. In this state, the evaluation beer was perfused at 5±3°C over the outer surface of the hollow fiber membrane, and cross-flow filtration was continued in which a portion of it was filtered. As operation continued, the hollow fiber membrane was clogged, causing the water permeability to decrease, but because it was constant flow filtration, the transmembrane pressure difference (TMP) would increase. TMP was calculated using the following formula. where Pi is the inlet pressure, Po is the outlet pressure and Pf is the pressure on the filtration side. TMP = ((Pi + Po) / 2) - Pf The time [h] it took for the TMP to reach 150 kPa was measured, and the beer throughput was calculated using the formula below. If high water permeability can be maintained for a long period of time, the beer throughput will be large. If water permeability decreases quickly, the beer throughput will be small. Beer throughput [L / m 2 ] = filtration rate 100 [L / m 2 / h] × time for pressure to rise to 150 kPa [h].
[0120] (7) Inhibition property For the evaluation beer, the unfiltered liquid and the filtrate were sampled and left to stand at room temperature for 30 minutes, and the turbidity was measured using a nephelometric turbidimeter. The rejection rate was then calculated using the following formula. Rejection rate (%) = (unprocessed turbidity - filtrate turbidity) / unprocessed turbidity
[0121] (8) Measurement of hydrophilic polymer (coating polymer) content A 2 cm hollow fiber membrane was dissolved in 1 mL of dimethyl sulfoxide and then analyzed using a JNM-ECZ400R (manufactured by JEOL Ltd.). 1The measurement was performed at two arbitrary points of the hollow fiber membrane, and the amount of hydrophilic polymer was calculated when the ratio of detected PVDF was set to 100. In the examples and comparative examples, the following abbreviations were used for hydrophilic polymers. PVP: Polyvinylpyrrolidone PVP / PVAc: Vinylpyrrolidone / vinyl acetate random copolymer PEG: Polyethylene glycol PEGMA: Polyethylene glycol methacrylate
[0122] (9) Chemical wash durability The hollow fiber membrane with the hydrophilic polymer introduced was immersed in ethanol for 30 minutes, then immersed in pure water for 60 minutes to wet it, and then washed in an oven at 95 ° C for 5 hours. Thereafter, it was immersed in an aqueous solution containing sodium hypochlorite at an effective chlorine concentration of 3000 ppm and further containing sodium hydroxide at a concentration of 0.04 mass% for 30 hours, and then washed with running water for 2 hours. The hydrophilic polymer content of this hollow fiber membrane was measured in the same manner as the above-mentioned hydrophilic polymer content measurement. From the results, the percentage of the ratio (mass%) of the hydrophilic polymer to PVDF obtained in (9) relative to the ratio (mass%) of the hydrophilic polymer to PVDF obtained in (8) was calculated and shown in the table as "coat polymer residual rate after immersion in chemical solution".
[0123] [Example 1] 38% by weight of vinylidene fluoride homopolymer with a weight average molecular weight of 417,000 and 62% by weight of gamma-butyrolactone were dissolved at 150°C. This resin solution was held at 100°C (primary nucleus holding temperature T2), which is within the range of (Tc+20)°C to (Tc+55)°C, for 20 seconds under a pressure of 1.2 MPa. After that, the resin solution was sent to the die through a pipe whose outer periphery was heated to 108°C (T3). The residence time in the pipe heated to 108°C was 7.05 seconds (time to apply temperature gradient), and the radius of the pipe was 4.0 mm (thickness Ls of polyvinylidene fluoride resin to which temperature gradient was applied). While the resin solution was passed through the outer tube of the die, a 90% by weight aqueous solution of γ-butyrolactone at 100°C was discharged from the inner tube of the die at the same time. The discharged resin solution was solidified for 5 minutes in a bath of 90% by weight aqueous solution of γ-butyrolactone at a temperature of 25°C (cooling bath temperature T4). After solidification, the obtained membrane was washed with water and stretched 1.5 times in warm water at 95°C. After stretching, the hollow fiber membrane was washed with water, immersed in 30% glycerin for 2 hours, and then air-dried overnight. It was then subjected to heat treatment under steam at 125°C for 1 hour. The cross section perpendicular to the longitudinal direction of the obtained hollow fiber membrane has a spherical structure, the average diameter Da1 of the region Sa1 is 2.62 μm, the average diameter Db2 of the region Sb2 is 1.84 μm, and the natural number i min The average diameter Da5 of the spherical structures in the region Sa5 was 2.02 μm. The average constriction diameter da1 of the region Sa1 was 1.40 μm, the average constriction diameter db2 of the region Sb2 was 1.14 μm, and the natural number j that satisfies the above conditions (1) and (2) was min The average diameter of the constriction between the spherical structures in the region Sa5 was 1.20 μm. The pure water permeability of this membrane was 3.6 m / hr, and the beer filtration capacity was 400 L / m 2 The rejection rate was 92%, and permeability and separation properties were maintained for a long period of time.
[0124] [Example 2] 38% by weight of vinylidene fluoride homopolymer with a weight average molecular weight of 417,000 and 62% by weight of gamma-butyrolactone were dissolved at 150°C. This resin solution was kept at 100°C, within the range of (Tc+20)°C to (Tc+55)°C, for 20 seconds under a pressure of 1.2 MPa. The resin solution was then sent to the die through a pipe whose outer periphery was heated to 125° C. The residence time of the resin solution in the pipe heated to 125° C. was 7.05 seconds, and the radius of the pipe was 4.0 mm. While the resin solution was passed through the outer tube of the die, a 90% by weight aqueous solution of γ-butyrolactone at 100°C was discharged from the inner tube of the double-tube die at the same time. The discharged resin solution was solidified for 1 minute in a bath of 90% by weight aqueous solution of γ-butyrolactone at a temperature of 25°C. After solidification, the obtained membrane was washed with water and stretched 1.5 times in warm water at 95°C. After stretching, the hollow fiber membrane was washed with water, immersed in 30% glycerin for 2 hours, and then air-dried overnight. It was then subjected to a heat treatment under steam at 125°C for 1 hour. The cross section perpendicular to the longitudinal direction of the obtained hollow fiber membrane has a spherical structure, the average diameter Da1 of the region Sa1 is 3.40 μm, the average diameter Db2 of the region Sb2 is 2.15 μm, and the natural number i min The average diameter Da5 of the spherical structures in the region Sa5 was 2.30 μm. The average constriction diameter da1 of the region Sa1 was 1.45 μm, the average constriction diameter db2 of the region Sb2 was 1.14 μm, and the natural number j that satisfies the above conditions (1) and (2) was min The average diameter of the constriction between the spherical structures in the region Sa5 was 5, and the average diameter of the constriction da5 between the spherical structures in the region Sa5 was 1.24 μm. The pure water permeability of this membrane was 4.4 m / hr, and the beer filtration capacity was 700 L / m 2 The rejection rate was 82%, and permeability and separation ability were maintained for a long period of time.
[0125] [Example 3] 36% by weight of vinylidene fluoride homopolymer with a weight average molecular weight of 417,000 and 64% by weight of gamma-butyrolactone were dissolved at 150°C. This resin solution was kept at 99°C, within the range of (Tc+20)°C to (Tc+55)°C, for 20 seconds under a pressure of 1.2 MPa. The resin solution was then sent to the die through a pipe whose outer periphery was heated to 108° C. The residence time of the resin solution in the pipe heated to 108° C. was 9.50 seconds, and the radius of the pipe was 4.0 mm. While the resin solution was passed through the outer tube of the die, a 90% by weight aqueous solution of γ-butyrolactone at 100°C was discharged from the inner tube of the die at the same time. The discharged resin solution was solidified for 5 minutes in a bath of 90% by weight aqueous solution of γ-butyrolactone at a temperature of 25°C. After solidification, the obtained membrane was washed with water and stretched to 1.5 times its original length in warm water at 95°C. After the stretching, the hollow fiber membrane was washed with water, immersed in 30% glycerin for 2 hours, and then air-dried overnight. It was then subjected to a heat treatment under steam at 125°C for 1 hour. The cross section perpendicular to the longitudinal direction of the obtained hollow fiber membrane has a spherical structure, the average diameter Da1 of the region Sa1 is 3.70 μm, the average diameter Db2 of the region Sb2 is 1.86 μm, and the natural number i min The average diameter Da6 of the spherical structures in the region Sa6 was 2.10 μm. The average constriction diameter da1 of the region Sa1 was 1.66 μm, the average constriction diameter db2 of the region Sb2 was 1.27 μm, and the natural number j that satisfies the above conditions (1) and (2) was min The average diameter of the constriction between the spherical structures in the region Sa6 was 1.29 μm. The pure water permeability of this membrane was 4.6 m / hr, and the beer filtration capacity was 450 L / m 2 The rejection rate was 91%, and permeability and separation properties were maintained for a long period of time.
[0126] [Example 4] 38% by weight of vinylidene fluoride homopolymer with a weight average molecular weight of 417,000 and 62% by weight of dimethyl sulfoxide were dissolved at 120° C. This resin solution was kept at 75° C., within the range of (Tc+20)° C. or more and (Tc+55)° C. or less, for 20 seconds under a pressure of 1.2 MPa. The resin solution was then delivered to a die heated to 85°C and discharged 5.8 seconds after entering the die. The width of the flow passage in the annular nozzle of the die was 1.75 mm. While the resin solution was passed through the outer tube of the die, a 90% by weight aqueous solution of dimethyl sulfoxide at 75°C was discharged from the inner tube of the die at the same time. The discharged resin solution was solidified for 5 minutes in a bath of 90% by weight aqueous solution of dimethyl sulfoxide at a temperature of 18°C. After solidification, the obtained membrane was washed with water and stretched to 1.5 times its original length in warm water at 95°C. After the stretching, the hollow fiber membrane was washed with water, immersed in 30% glycerin for 2 hours, and then air-dried overnight. It was then subjected to a heat treatment under steam at 125°C for 1 hour. The cross section perpendicular to the longitudinal direction of the obtained hollow fiber membrane has a spherical structure, the average diameter Da1 of the region Sa1 is 3.52 μm, the average diameter Db2 of the region Sb2 is 1.90 μm, and the natural number i min The average diameter Da7 of the spherical structures in the region Sa7 was 1.90 μm. The average constriction diameter da1 of the region Sa1 was 1.50 μm, the average constriction diameter db2 of the region Sb2 was 1.27 μm, and the natural number j that satisfies the above conditions (1) and (2) was min The average diameter of the constriction between the spherical structures in the region Sa7 was 1.31 μm. The pure water permeability of this membrane was 4.3 m / hr, and the beer filtration capacity was 480 L / m 2 The rejection rate was 90%, and permeability and separation properties were maintained for a long period of time.
[0127] [Example 5] 38% by weight of vinylidene fluoride homopolymer with a weight average molecular weight of 417,000 and 62% by weight of gamma-butyrolactone were dissolved at 150°C. This resin solution was kept at 98°C, within the range of (Tc+20)°C to (Tc+55)°C, for 20 seconds under a pressure of 1.2 MPa. The resin solution was then sent to the die through a pipe whose outer periphery was heated to 132° C. The residence time of the resin solution in the pipe heated to 132° C. was 7.05 seconds, and the radius of the pipe was 4.0 mm. While the resin solution was passed through the outer tube of the die, a 90% by weight aqueous solution of γ-butyrolactone at 100°C was discharged from the inner tube of the die at the same time. The discharged resin solution was solidified for 5 minutes in a bath of 90% by weight aqueous solution of γ-butyrolactone at a temperature of 25°C. After solidification, the obtained membrane was washed with water and stretched to 1.5 times its original length in warm water at 95°C. After the stretching, the hollow fiber membrane was washed with water, immersed in 30% glycerin for 2 hours, and then air-dried overnight. It was then subjected to a heat treatment under steam at 125°C for 1 hour. The cross section perpendicular to the longitudinal direction of the obtained hollow fiber membrane has a spherical structure, the average diameter Da1 of the region Sa1 is 4.30 μm, the average diameter Db2 of the region Sb2 is 2.24 μm, and the natural number i min is 12, and the area Sa 12 The average diameter Da of the spherical structures in 12 The average constriction diameter da1 of the region Sa1 was 1.55 μm, the average constriction diameter db2 of the region Sb2 was 1.24 μm, and the natural number j that satisfies the above conditions (1) and (2) was min is 12, and the area Sa 12 The average diameter of the constriction between the spherical structures is da 12 The pure water permeability of this membrane was 5.1 m / hr, and the beer filtration capacity was 720 L / m 2 The rejection rate was 81%, and permeability and separation ability were maintained for a long period of time.
[0128] [Example 6] 38% by weight of vinylidene fluoride homopolymer with a weight average molecular weight of 417,000 and 62% by weight of gamma-butyrolactone were dissolved at 150°C. This resin solution was kept at 97°C, within the range of (Tc+20)°C to (Tc+55)°C, for 20 seconds under a pressure of 1.2 MPa. The resin solution was then sent to the die through a pipe whose outer periphery was heated to 140° C. The residence time of the resin solution in the pipe heated to 140° C. was 6.83 seconds, and the radius of the pipe was 4.0 mm. While the resin solution was passed through the outer tube of the die, a 90% by weight aqueous solution of γ-butyrolactone at 100°C was discharged from the inner tube of the die at the same time. The discharged resin solution was solidified for 5 minutes in a bath of 90% by weight aqueous solution of γ-butyrolactone at a temperature of 25°C. After solidification, the obtained membrane was washed with water and stretched to 1.5 times its original length in warm water at 95°C. After the stretching, the hollow fiber membrane was washed with water, immersed in 30% glycerin for 2 hours, and then air-dried overnight. It was then subjected to a heat treatment under steam at 125°C for 1 hour. The cross section perpendicular to the longitudinal direction of the obtained hollow fiber membrane has a spherical structure, the average diameter Da1 of the region Sa1 is 4.60 μm, the average diameter Db2 of the region Sb2 is 2.29 μm, and the natural number i min is 17, and the area Sa 12 The average diameter Da of the spherical structures in 12 The average constriction diameter da1 of the region Sa1 was 1.86 μm, the average constriction diameter db2 of the region Sb2 was 1.32 μm, and the natural number j that satisfies the above conditions (1) and (2) was min is 17, and the area Sa 17 The average diameter of the constriction between the spherical structures is da 17 The pure water permeability of this membrane was 5.8 m / hr, and the beer filtration capacity was 800 L / m 2 The rejection rate was 72%, and permeability was maintained for a long period of time, but separation performance was somewhat deteriorated.
[0129] [Comparative Example 1] A hollow fiber membrane was obtained in the same manner as in Example 1, except that the temperature of the outer periphery of the pipe was set to 100°C. The cross section perpendicular to the longitudinal direction of the obtained hollow fiber membrane had a spherical structure, but the average diameter Da1 of region Sa1 was 1.83 μm, the average diameter Db2 of region Sb2 was 1.79 μm, and there was no natural number i that satisfied the above-mentioned conditions (1) and (2). The average constriction diameter da1 of the region Sa1 was 1.14 μm, the average constriction diameter db2 of the region Sb2 was 1.14 μm, and no natural number j existed that satisfied the above conditions (1) and (2). The pure water permeability of this membrane is 2.0 m / hr, and the beer filtration capacity is 150 L / m 2Although the separation ability was high with a rejection rate of 96%, the permeability could not be maintained for a long period of time.
[0130] [Comparative Example 2] 38% by weight of vinylidene fluoride homopolymer with a weight average molecular weight of 417,000 and 62% by weight of gamma-butyrolactone were dissolved at 150°C. This resin solution was held at 95°C, which is within the range of (Tc+20)°C to (Tc+55)°C, for 20 seconds under a pressure of 1.2MPa, and then sent to a die whose outer tube was heated to 99°C. The resin solution was discharged 1.68 seconds after entering the die. While the resin solution was passed through the outer tube of the die, a 95°C 90% by weight aqueous solution of gamma-butyrolactone was simultaneously discharged from the inner tube of the die. The discharged resin solution was solidified for 5 minutes in a bath of 90% by weight of gamma-butyrolactone at a temperature of 5°C. After solidification, the obtained membrane was washed with water and stretched 1.5 times in warm water at 95°C. The stretched hollow fiber membrane was washed with water, immersed in 30% glycerin for 2 hours, air-dried overnight, and then heat-treated in steam at 125°C for 1 hour. The cross section perpendicular to the longitudinal direction of the obtained hollow fiber membrane had a spherical structure, but the average diameter Da1 of the region Sa1 was 2.58 μm, the average diameter Db2 of the region Sb2 was 1.86 μm, and the natural number i min The average diameter Da2 of the spherical structures in the region Sa2 was 1.96 μm. The average constriction diameter da1 of the region Sa1 was 1.39 μm, the average constriction diameter db2 of the region Sb2 was 1.14 μm, and the natural number j that satisfies the above conditions (1) and (2) was min The average diameter of the constriction between the spherical structures in the region Sa2 was 1.15 μm. The pure water permeability of this membrane was 2.5 m / hr, and the beer filtration capacity was 250 L / m 2 Although the separation ability was high with a rejection rate of 96%, the permeability could not be maintained for a long period of time.
[0131] [Comparative Example 3] 38% by weight of vinylidene fluoride homopolymer with a weight average molecular weight of 417,000 and 62% by weight of dimethyl sulfoxide were dissolved at 120°C. This resin solution was held at 75°C, which is within the range of (Tc+20)°C to (Tc+55)°C, for 20 seconds under a pressure of 1.2MPa, and then the outer tube was sent to a die heated to 80°C. The resin solution was discharged 1.68 seconds after entering the die. While the resin solution was passed through the outer tube of the die, a 90% by weight aqueous solution of dimethyl sulfoxide at 75°C was simultaneously discharged from the inner tube of the die. The discharged resin solution was solidified for 5 minutes in a bath at 5°C consisting of a 90% by weight aqueous solution of dimethyl sulfoxide. After solidification, the obtained membrane was washed with water and stretched to 1.5 times in warm water at 95°C. The hollow fiber membrane after stretching was washed with water, immersed in 30% glycerin for 2 hours, and then air-dried overnight. Thereafter, the plate was subjected to a heat treatment in steam at 125° C. for 1 hour. The cross section perpendicular to the longitudinal direction of the obtained hollow fiber membrane has a spherical structure, the average diameter Da1 of the region Sa1 is 2.54 μm, the average diameter Db2 of the region Sb2 is 1.81 μm, and the natural number i min The average diameter Da2 of the spherical structures in the region Sa2 was 1.89 μm. The average constriction diameter da1 of the region Sa1 was 1.34 μm, the average constriction diameter db2 of the region Sb2 was 1.10 μm, and the natural number j that satisfies the above conditions (1) and (2) was min The average diameter of the constriction between the spherical structures in the region Sa2 was 1.14 μm. The pure water permeability of this membrane was 2.7 m / hr, and the beer filtration capacity was 220 L / m 2 Although the separation ability was high with a rejection rate of 96%, the permeability could not be maintained for a long period of time.
[0132] [Comparative Example 4] 38% by weight of vinylidene fluoride homopolymer with a weight-average molecular weight of 417,000 and 62% by weight of dimethyl sulfoxide were dissolved at 120°C. This resin solution was held at 75°C, within the range of (Tc+20)°C to (Tc+55)°C, for 20 seconds under a pressure of 1.2 MPa, and then the outer tube was sent to a die heated to 138°C. The resin solution was discharged 5.23 seconds after entering the die. While the resin solution was passed through the outer tube of the die, a 90% by weight aqueous solution of γ-butyrolactone at 75°C was discharged from the inner tube of the die at the same time. The discharged resin solution was solidified for 5 minutes in a bath of 90% by weight aqueous solution of γ-butyrolactone at a temperature of 5°C. After solidification, the obtained membrane was washed with water and stretched to 1.5 times its original length in warm water at 95°C. After the stretching, the hollow fiber membrane was washed with water, immersed in 30% glycerin for 2 hours, and then air-dried overnight. It was then subjected to a heat treatment under steam at 125°C for 1 hour. The cross section perpendicular to the longitudinal direction of the obtained hollow fiber membrane has a spherical structure, the average diameter Da1 of the region Sa1 is 3.35 μm, the average diameter Db2 of the region Sb2 is 3.11 μm, and the natural number i min did not exist. The pure water permeability of this membrane was 7.8 m / hr, and it was not subjected to beer filtration tests.
[0133] The manufacturing conditions for each hollow fiber membrane are shown in Tables 1 and 2, and the evaluation results of the obtained hollow fiber membranes are shown in Tables 3 and 4. i ", etc. The specific numerical value of the item expressed by including the value of n = i is i as i min In other words, in Tables 3 and 4, "Da1 / Da i The value shown in the line is actually "Da1 / Da imin " This is also true when i is j or k.
[0134] [Table 1]
[0135] [Table 2]
[0136] [Table 3]
[0137] [Table 4]
[0138] [Example 7] PVP / PVAc (Kollidon VA64; manufactured by BASF) was used as a hydrophilic polymer (coating polymer). The hollow fiber membrane prepared in Example 1 was immersed for 1 hour in a 1.0 mass% ethanol aqueous solution in which 1000 ppm of the prepared hydrophilic polymer consisting of a vinylpyrrolidone / vinyl acetate random copolymer was dissolved, and then the hollow fiber membrane was irradiated with 25 kGy of gamma rays to introduce the vinylpyrrolidone / vinyl propanoate random copolymer into the hollow fiber membrane, followed by heat treatment in an oven at 150°C for 1 hour. The obtained hollow fiber membrane was 1 H-NMR measurements were performed to measure the PVP / PVAc content (parts by mass of hydrophilic polymer when the polyvinylidene fluoride resin is taken as 100 parts by mass), and the pure water permeability was measured after the introduction of the hydrophilic polymer and after chemical washing.
[0139] [Example 8] The hydrophilic polymer was introduced in the same manner as in Example 7, except that PEG was used as the hydrophilic polymer, and the results in Table 5 were obtained.
[0140] [Example 9] The hydrophilic polymer was introduced in the same manner as in Example 7, except that PEGMA was used as the hydrophilic polymer, and the results in Table 5 were obtained.
[0141] [Example 10] After heat treatment in an oven at 125°C for 1 hour, the hollow fiber membrane prepared in Example 1 was immersed for 1 hour in a 1.0 mass% aqueous ethanol solution in which 10,000 ppm of PVP / PVAc was dissolved, and then irradiated with 25 kGy of gamma rays to introduce PVP / PVAc into the hollow fiber membrane.
[0142] [Table 5]
[0143] Although the present invention has been described in detail and with reference to specific embodiments, it is apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on Japanese patent applications filed on April 28, 2021 (Patent Application No. 2021-075668), June 30, 2021 (Patent Application No. 2021-108523), and August 27, 2021 (Patent Application No. 2021-138656), the contents of which are incorporated herein by reference. [Industrial Applicability]
[0144] The hollow fiber membrane of the present invention is preferably used for water treatment applications such as wastewater treatment, water purification, and industrial water production, as well as for food and pharmaceutical production, etc. The hollow fiber membrane of the present invention is also preferably used as a microfiltration membrane or ultrafiltration membrane for these applications. [Explanation of symbols]
[0145] 1 Base 2 Piping 11 Inner nozzle 12 Annular nozzle 111 Inner nozzle inlet 112 Inner nozzle outlet 121 Annular nozzle inlet 122 Annular nozzle outlet 131 Pipe inlet 132 Piping outlet
Claims
1. A hollow fiber membrane having a layer of a spherical structure made of a polyvinylidene fluoride resin, The thickness L of the layer of the spherical structure is 60 μm or more and 500 μm or less, the layer of spherical structure has a first surface and a second surface; A region Sa from 10×(n−1) to 10×n μm from the first surface n The average diameter Da of the spherical structure n and a region Sb of 10×(n−1) to 10×n μm from the second surface. n The average diameter Db of the spherical structure n About Da 1 >Db 2 and The smallest natural number i that satisfies the following conditions (1) and (2) min 3≦i min A hollow fiber membrane having a viscosity of ≦(L−20) / 10. (1) Yes 1 / Da i ≧1.1 (2)-0.3μm≦Da i -Db 2 ≦0.3μm Here, n is a natural number, and 3≦i min In the case of ≦(L-20) / 10, the decimal places of (L-20) / 10 are rounded down.
2. i min 2. The hollow fiber membrane according to claim 1, wherein L x 0.75 / 10. However, the above i min In the case of L×0.75 / 10, the decimal point of L×0.75 / 10 is rounded down.
3. 1.10<Da 1 / Da imin The hollow fiber membrane according to claim 1 or 2, wherein the molecular weight is less than 4.
00.
4. 0.50 μm<Db 2 3. The hollow fiber membrane of claim 1, wherein the thickness of the hollow fiber membrane is less than 2.00 μm.
5. 1.00≦Da 1 / Da 2 3. The hollow fiber membrane according to claim 1 or 2, wherein the molecular weight is ≦1.
10.
6. The hollow fiber membrane according to claim 1 or 2, wherein the first surface is a side on which a liquid to be filtered is disposed.
7. 3. The hollow fiber membrane according to claim 1 or 2, wherein the first surface is an outer surface of the hollow fiber membrane.
8. When the throat diameter obtained by the pore network model analysis of the hollow fiber membrane is set as the constriction diameter of the spherical structure gap, A region Sa from 10×(n−1) to 10×n μm from the first surface n The average diameter of the constriction between the spherical structures da n and, A region Sb of 10×(n−1) to 10×n μm from the second surface n The average diameter of the constriction between the spherical structures db n About 1 >db 2 and The minimum value j of a natural number j that satisfies the following conditions (1) and (2) min 3≦j min 3. The hollow fiber membrane according to claim 1 or 2, wherein L is less than or equal to (L-20) / 10. (1)da 1 / da j ≧1.15 (2)da j -db 2 ≦0.10μm However, the above 3≦j min In the case of ≦(L-20) / 10, the decimal places of (L-20) / 10 are rounded down.
9. j min 9. The hollow fiber membrane according to claim 8, wherein L x 0.5 / 10. However, the above j min In the case of L×0.5 / 10, the decimal places of L×0.5 / 10 are rounded down.
10. The region Sa obtained by the pore network model analysis n Number of throats in Na n and the region Sb n Number of throats in Nb n About Na 1 <Nb 2 and The minimum value k of a natural number k that satisfies the following conditions (3) and (4) min k min The hollow fiber membrane according to claim 8, wherein the value is ≦(L−20) / 10. (3)Na 1 / Na k ≦0.90 (4) Nb 2 -Na k ≦400 pieces However, the above 3≦k min In the case of ≦(L-20) / 10, the decimal places of (L-20) / 10 are rounded down. However, the analysis region in the above analysis is a rectangular parallelepiped including any 50 μm square on the first surface and a 50 μm square on the second surface opposite to the first surface.
11. 0.10 μm<d b 2 9. The hollow fiber membrane of claim 8, wherein the thickness is < 10.0 μm.
12. A hydrophilic polymer is present on the surface and inside of the spherical structure, 3. The hollow fiber membrane according to claim 1, comprising 1.0 part by mass or more of the hydrophilic polymer per 100 parts by mass of the polyvinylidene fluoride resin.
13. 13. The hollow fiber membrane according to claim 12, wherein a ratio (mass%) of the hydrophilic polymer to the polyvinylidene fluoride resin after the hollow fiber membrane is immersed in a 3000 ppm sodium hypochlorite aqueous solution (pH 12.5) at 60°C for 30 hours is defined as P1, and a ratio (mass%) of the hydrophilic polymer to the polyvinylidene fluoride resin before the immersion is defined as P0, and a percentage of P1 to P0, P1 / P0, is 70% or less.
14. (a) dissolving a polyvinylidene fluoride resin in a poor solvent to obtain a polyvinylidene fluoride resin solution; (b) maintaining the polyvinylidene fluoride resin solution at a temperature at which the formation of primary nuclei proceeds; (c) after the step (b), discharging the polyvinylidene fluoride resin solution in a hollow fiber shape through a pipe and a die, and providing a temperature gradient in the thickness direction of the polyvinylidene fluoride resin solution in at least one of the pipe and the die; and (d) after the step (c), a step of immersing the polyvinylidene fluoride resin solution in a cooling bath to solidify the polyvinylidene fluoride resin solution by solid-liquid type thermally induced phase separation, A method for producing a hollow fiber membrane, wherein the temperature gradient ΔT (° C.) and the time t (seconds) for imparting the temperature gradient in the step (c) are 50≦ΔT×t≦300.
15. 15. The method for producing a hollow fiber membrane according to claim 14, wherein in the step (c), a thickness Ls of the polyvinylidene fluoride resin that imparts a temperature gradient is in the range of 5<Ls / L<40, relative to a thickness L of the layer of the spherical structure.
16. The method for producing a hollow fiber membrane according to claim 14 or 15, wherein the temperature T2 (°C) in the step (b), the temperature T4 (°C) of the cooling bath in the step (d), and the crystallization temperature Tc (°C) of the polyvinylidene fluoride resin satisfy (Tc-T4) / (T2-T4)<0.
50.
17. The method for producing a hollow fiber membrane according to claim 16, wherein 15<Tc-T4<35 is satisfied.
18. The method for producing a hollow fiber membrane according to claim 14 or 15, further comprising the following steps (e) and (f) after the step (d): (e) A step of introducing a hydrophilic polymer into the hollow fiber membrane (f) a step of performing a heat treatment at 100° C. or higher after the step (e)
19. 20. The method for producing a hollow fiber membrane according to claim 18, further comprising passing an aqueous solution having a hydrophilic polymer dissolved therein through the hollow fiber membrane, followed by irradiating the membrane with radiation in the step (e).
Citation Information
Patent Citations
Permanent hydrophilic polyvinylidene fluoride membrane and production method thereof
CN108211809A
Hollow fiber membrane, manufacturing method of hollow fiber membrane, and production method of beer, wine or japanese sake using hollow fiber membrane
JP2019130522A
Method for preparing composite multilayer porous hollow membrane and device and product thereof
US20120085698A1
Hollow fiber film and method for production thereof
WO2003031038A1
Microporous membrane and manufacturing process therefor
WO2014054658A1
Cited By
Hollow fiber membrane and method for manufacturing the same
JP2023033237A