Biaxially Oriented Polypropylene Film
A biaxially oriented polypropylene film with enhanced crystallinity and molecular structure addresses the issues of rigidity and heat resistance, ensuring shape retention and reducing wrinkles, making it suitable for packaging uses.
Patent Information
- Application Number
- JP2023125649
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-10-28
- Filing Date
- 2023-08-01
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2039-12-19
AI Technical Summary
Existing biaxially oriented polypropylene films lack sufficient rigidity and heat resistance, particularly at high temperatures, and tend to develop wrinkles during heat sealing, limiting their use in applications requiring strength and shape retention.
A biaxially oriented polypropylene film with specific crystallinity, melting point, and molecular structure enhancements, including a polypropylene resin composition with controlled mesopentad fraction, melt flow rate, and molecular weight distribution, combined with a precise stretching process to achieve high orientation and reduced heat shrinkage.
The film exhibits excellent rigidity and heat resistance at high temperatures, maintaining shape and preventing wrinkles during heat sealing, enabling thinner films suitable for packaging applications.
Smart Images

Figure 0007586240000001 
Figure 0007586240000002 
Figure 0007586240000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a biaxially oriented polypropylene film having excellent rigidity and heat resistance. More specifically, the present invention relates to a biaxially oriented polypropylene film that is suitable for use as a packaging bag because it is easy to maintain the shape of the bag when made into a packaging bag and has few wrinkles at the sealed portion when heat sealed. [Background technology]
[0002] Biaxially oriented polypropylene films are used for packaging and industrial applications because they are moisture-proof and have the necessary rigidity and heat resistance. In recent years, as the range of applications expands, higher performance is required, and in particular, improved rigidity is expected. In addition, due to environmental considerations, there is a demand for maintaining strength even when the volume is reduced (film thickness is reduced), but to achieve this, it is essential to significantly improve rigidity. As a means of improving rigidity, it is known that the crystallinity and melting point of polypropylene resin can be improved by improving the catalyst and process technology used during polymerization of polypropylene resin. However, despite these improvements, there has been no biaxially oriented polypropylene film with sufficient rigidity.
[0003] In the manufacturing process of biaxially oriented polypropylene film, a method has been proposed in which, after stretching in the width direction, the film is subjected to a first-stage heat treatment while relaxing at a temperature equal to or lower than that during width direction stretching, and then a second-stage heat treatment is performed at a temperature between the first-stage temperature and the width direction stretching temperature (see, for example, Reference 1, etc.), and a method in which, after width direction stretching, further stretching is performed in the longitudinal direction (see, for example, Reference 2, etc.). However, although the film described in Patent Document 2 has excellent rigidity, wrinkles tend to occur in the sealed portion after heat sealing, and the heat resistance is poor. In addition, the orientation of the film described in Patent Document 1 is low, and the rigidity is insufficient. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. WO2016 / 182003 [Patent Document 2] JP 2013-177645 A Summary of the Invention [Problem to be solved by the invention]
[0005] The object of the present invention is to solve the above-mentioned problems. That is, the present invention relates to a biaxially oriented polypropylene film that is excellent in film rigidity and heat resistance at a high temperature of 150° C. More specifically, the present invention aims to provide a biaxially oriented polypropylene film that is easy to maintain the bag shape when made into a packaging bag, and that has few wrinkles at the sealed portion and around it when heat-sealed.
[0006] As a result of intensive research by the inventors to achieve this object, it has been found that a biaxially oriented polypropylene film having excellent film rigidity and heat resistance at a high temperature of as high as 150°C can be obtained by producing a biaxially oriented polypropylene film in which the half-width of the peak derived from oriented crystals in the width direction is 27° or less in the azimuth angle dependence of the polypropylene α-crystal (110) plane obtained by wide-angle X-ray diffraction measurement, and the tan δ area obtained from the ratio (E” / E’) of the storage modulus (E') to the loss modulus (E”) obtained by dynamic viscoelastic measurement is 0.2 or more and 0.4 or less in the width direction.
[0007] In this case, it is preferable that the heat shrinkage rate of the biaxially oriented polypropylene film at 120°C is 2.0% or less in the longitudinal direction and 5.0% or less in the width direction, and that the heat shrinkage rate at 120°C in the longitudinal direction is smaller than the heat shrinkage rate at 120°C in the width direction.
[0008] In this case, it is preferable that the refractive index Ny in the longitudinal direction of the biaxially oriented polypropylene film is 1.5230 or more and ΔNy is 0.0220 or more.
[0009] Furthermore, in this case, it is preferable that the haze of the biaxially oriented polypropylene film is 5.0% or less.
[0010] Furthermore, in this case, it is preferable that the polypropylene resin constituting the biaxially oriented polypropylene film has a mesopentad fraction of 97.0% or more.
[0011] Furthermore, in this case, it is preferable that the polypropylene resin constituting the biaxially oriented polypropylene film has a crystallization temperature of 105° C. or higher and a melting point of 160° C. or higher.
[0012] Furthermore, in this case, it is preferable that the polypropylene resin constituting the biaxially oriented polypropylene film has a melt flow rate of 4.0 g / 10 min or more.
[0013] Furthermore, in this case, it is preferable that the amount of components having a molecular weight of 100,000 or less in the polypropylene resin constituting the biaxially oriented polypropylene film is 35% by mass or more.
[0014] Furthermore, in this case, it is preferable that the degree of orientation of the biaxially oriented polypropylene film is 0.85 or more. Effect of the Invention
[0015] The biaxially oriented polypropylene film of the present invention has high rigidity and excellent heat resistance at a high temperature of 150° C., so that the bag shape is easily maintained when made into a packaging bag, and there are few wrinkles in the sealed portion when heat sealed, so that a biaxially oriented polypropylene film suitable for use as a packaging bag can be obtained. In addition, since the biaxially oriented polypropylene film has excellent rigidity, it can maintain its strength even when the film thickness is reduced, and can be used suitably for applications requiring higher rigidity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The biaxially oriented polypropylene film of the present invention will be described in more detail below. The biaxially oriented polypropylene film of the present invention is made of a polypropylene resin composition containing a polypropylene resin as a main component. Here, "main component" means that the proportion of the polypropylene resin in the polypropylene resin composition is 90% by mass or more, more preferably 93% by mass or more, even more preferably 95% by mass or more, and particularly preferably 97% by mass or more.
[0017] (Polypropylene resin) The polypropylene resin used in the present invention may be a polypropylene homopolymer or a copolymer with ethylene and / or an α-olefin having 4 or more carbon atoms. A propylene homopolymer that does not substantially contain ethylene and / or an α-olefin having 4 or more carbon atoms is preferred, and even if it contains ethylene and / or an α-olefin having 4 or more carbon atoms, the amount of the ethylene and / or α-olefin having 4 or more carbon atoms is preferably 1 mol% or less. The upper limit of the amount of the component is more preferably 0.5 mol%, further preferably 0.3 mol%, and particularly preferably 0.1 mol%. When it is within the above range, the crystallinity is likely to be improved. Examples of the α-olefin component having 4 or more carbon atoms that constitutes such a copolymer include 1-butene, 1-pentene, 3-methylpentene-1, 3-methylbutene-1, 1-hexene, 4-methylpentene-1, 5-ethylhexene-1, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-heptadecene, 1-octadecene, and 1-eicosene. The polypropylene resin may be a homopolymer of two or more different kinds of polypropylene, a copolymer with ethylene and / or an α-olefin having 4 or more carbon atoms, or a mixture of these.
[0018] (stereoregularity) The mesopentad fraction ([mmmm]%), which is an index of stereoregularity of the polypropylene resin used in the present invention, is preferably within the range of 97.0 to 99.9%, more preferably within the range of 97.5 to 99.7%, even more preferably within the range of 98.0 to 99.5%, and particularly preferably within the range of 98.5 to 99.3%. If it is 97.0% or more, the crystallinity of the polypropylene resin is increased, and the melting point, crystallinity, and crystal orientation of the crystals in the film are improved, making it easier to obtain rigidity and heat resistance at high temperatures. If it is 99.9% or less, it is easier to reduce costs in terms of polypropylene production, and the film is less likely to break during film formation. It is more preferable that it is 99.5% or less. The mesopentad fraction is measured by the nuclear magnetic resonance method (the so-called NMR method). In order to set the mesopentad fraction of the polypropylene resin within the above-mentioned range, a method of washing the obtained polypropylene resin powder with a solvent such as n-heptane, a method of appropriately selecting a catalyst and / or a co-catalyst, and a method of appropriately selecting the components of the polypropylene resin composition are preferably adopted.
[0019] (Melting temperature) The lower limit of the melting temperature (Tm) of the polypropylene resin constituting the biaxially oriented polypropylene film of the present invention, as measured by DSC, is preferably 160°C, more preferably 161°C, even more preferably 162°C, and even more preferably 163°C. When Tm is 160° C. or higher, rigidity and heat resistance at high temperatures are easily obtained. The upper limit of Tm is preferably 170° C., more preferably 169° C., even more preferably 168° C., still more preferably 167° C., and particularly preferably 166° C. If Tm is 170° C. or less, it is easy to suppress an increase in cost in terms of polypropylene production, and breakage during film formation is difficult. The melting temperature can also be further increased by blending a crystal nucleating agent with the above-mentioned polypropylene resin. Tm is the main endothermic peak temperature associated with melting, which is observed when 1 to 10 mg of a sample is packed into an aluminum pan and set in a differential scanning calorimeter (DSC), melted at 230°C for 5 minutes in a nitrogen atmosphere, cooled to 30°C at a scanning rate of -10°C / min, held for 5 minutes, and then heated again at a scanning rate of 10°C / min.
[0020] (crystallization temperature) The lower limit of the crystallization temperature (Tc) of the polypropylene resin constituting the biaxially oriented polypropylene film of the present invention, as measured by DSC, is 105° C., preferably 108° C., and more preferably 110° C. When Tc is 105° C. or higher, crystallization is likely to proceed during width direction stretching and the subsequent cooling step, and rigidity and heat resistance at high temperatures are likely to be obtained. The upper limit of Tc is preferably 135° C., more preferably 133° C., even more preferably 132° C., still more preferably 130° C., particularly preferably 128° C., and most preferably 127° C. If Tc is 135° C. or lower, it is difficult to increase the cost of polypropylene production, and the film is difficult to break during film formation. Tc is the main exothermic peak temperature observed when 1 to 10 mg of a sample is packed into an aluminum pan, set in a DSC, melted at 230°C for 5 minutes in a nitrogen atmosphere, and cooled to 30°C at a scanning rate of -10°C / min. The crystallization temperature can be further increased by adding a crystal nucleating agent to the polypropylene resin.
[0021] (Melt Flow Rate) The melt flow rate (MFR) of the polypropylene resin constituting the biaxially oriented polypropylene film of the present invention, when measured in accordance with JIS K7210 (1995), condition M (230°C, 2.16 kgf), is preferably 4.0 to 30 g / 10 min, more preferably 4.5 to 25 g / 10 min, even more preferably 4.8 to 22 g / 10 min, particularly preferably 5.0 to 20 g / 10 min, and most preferably 6.0 to 20 g / 10 min. When the melt flow rate (MFR) of the polypropylene resin is 4.0 g / 10 min or more, a biaxially oriented polypropylene film with low thermal shrinkage is easily obtained. Furthermore, when the melt flow rate (MFR) of the polypropylene resin is 30 g / 10 min or less, the film formability is easily maintained.
[0022] From the viewpoint of film properties, the lower limit of the melt flow rate (MFR) (230°C, 2.16 kgf) of the polypropylene resin constituting the film is preferably 5.0 g / 10 min, more preferably 5.5 g / 10 min, even more preferably 6.0 g / 10 min, particularly preferably 6.3 g / 10 min, and most preferably 6.5 g / 10 min. When the melt flow rate (MFR) of the polypropylene resin is 5.0 g / 10 min or more, the amount of low molecular weight components in the polypropylene resin constituting the film is large. Therefore, by adopting a width direction stretching process in the film production process described below, the oriented crystallization of the polypropylene resin is further promoted and the crystallinity of the film is more likely to be increased. In addition, the entanglement of polypropylene molecular chains in the amorphous portion is reduced, making it easier to increase heat resistance. In order to set the melt flow rate (MFR) of the polypropylene resin within the above range, a method of controlling the average molecular weight or molecular weight distribution of the polypropylene resin is preferably adopted.
[0023] That is, the lower limit of the amount of components having a molecular weight of 100,000 or less in the GPC cumulative curve of the polypropylene resin constituting the film of the present invention is preferably 35 mass%, more preferably 38 mass%, even more preferably 40 mass%, particularly preferably 41 mass%, and most preferably 42 mass%. The upper limit of the amount of components having a molecular weight of 100,000 or less in the GPC cumulative curve is preferably 65% by mass, more preferably 60% by mass, and even more preferably 58% by mass. When the amount of components having a molecular weight of 100,000 or less in the GPC cumulative curve is 65% by mass or less, the film strength is unlikely to decrease. In this case, if the polypropylene resin contains high molecular weight components with long relaxation times or long-chain branched components, the amount of components with a molecular weight of 100,000 or less contained in the polypropylene resin can be easily adjusted without significantly changing the overall viscosity, making it easier to improve film formability without significantly affecting rigidity or thermal shrinkage.
[0024] (molecular weight distribution) The polypropylene resin used in the present invention has a lower limit of mass average molecular weight (Mw) / number average molecular weight (Mn), which is an index of the breadth of the molecular weight distribution, of preferably 3.5, more preferably 4.0, even more preferably 4.5, and particularly preferably 5.0. The upper limit of Mw / Mn is preferably 30, more preferably 25, even more preferably 23, particularly preferably 21, and most preferably 20. Mw / Mn can be obtained by gel permeation chromatography (GPC). When Mw / Mn is within the above range, it is easy to increase the amount of components having a molecular weight of 100,000 or less.
[0025] The molecular weight distribution of polypropylene resin can be adjusted by polymerizing components of different molecular weights in a series of plants in multiple stages, blending components of different molecular weights offline in a kneader, polymerizing by blending catalysts with different performance, or using a catalyst that can achieve a desired molecular weight distribution. The shape of the molecular weight distribution obtained by GPC may be a gentle molecular weight distribution with a single peak in a GPC chart with the logarithm (logM) of molecular weight (M) on the horizontal axis and the differential distribution value (weight fraction per logM) on the vertical axis, or a molecular weight distribution with multiple peaks or shoulders.
[0026] (Method for producing biaxially oriented polypropylene film) The biaxially oriented polypropylene film of the present invention is preferably obtained by preparing an unstretched sheet made of a polypropylene resin composition mainly composed of the above-mentioned polypropylene resin, and biaxially stretching the sheet. As the method of biaxial stretching, any of the inflation simultaneous biaxial stretching method, the tenter simultaneous biaxial stretching method, and the tenter sequential biaxial stretching method can be used, but it is preferable to adopt the tenter sequential biaxial stretching method from the viewpoint of film formation stability and thickness uniformity. In particular, it is preferable to stretch in the longitudinal direction and then in the width direction, but a method of stretching in the width direction and then in the longitudinal direction may also be used.
[0027] Next, the method for producing the biaxially oriented polypropylene film of the present invention will be described below, but is not necessarily limited thereto. The biaxially oriented polypropylene film of the present invention may have a layer having another function laminated on at least one side. Lamination may be performed on one or both sides. In that case, the resin composition of the other layer or the central layer may be the polypropylene resin composition described above. It may also be different from the polypropylene resin composition described above. The number of layers to be laminated may be one, two, or three or more layers per side, but one or two layers are preferred from the viewpoint of production. As a lamination method, for example, coextrusion by a feed block method or a multi-manifold method is preferred. In particular, for the purpose of improving the processability of the biaxially oriented polypropylene film, a resin layer having heat sealability can be laminated within a range that does not deteriorate the properties. In addition, in order to impart printability, corona treatment can be performed on one or both sides.
[0028] In the following, an example of a single layer will be described in which a tenter sequential biaxial stretching method is adopted. First, a resin composition containing a polypropylene resin is heated and melted in a single-screw or twin-screw extruder, extruded into a sheet from a T-die, and cooled and solidified by being placed on a cooling roll. In order to promote solidification, it is preferable to further cool the sheet cooled by the cooling roll by immersing it in a water tank.
[0029] The sheet is then stretched in the longitudinal direction between two pairs of heated stretching rolls by increasing the rotation speed of the rear stretching roll, to obtain a uniaxially stretched film.
[0030] The uniaxially stretched film is then preheated, and stretched in the width direction at a specific temperature while holding the film ends in a tenter-type stretching machine to obtain a biaxially stretched film. This width direction stretching step will be described in detail later.
[0031] After the width direction stretching step is completed, the biaxially stretched film is heat-treated at a specific temperature to obtain a biaxially oriented film. In the heat treatment step, the film may be relaxed in the width direction.
[0032] The biaxially oriented polypropylene film thus obtained can be subjected to a corona discharge treatment on at least one side, if necessary, and then wound up on a winder to obtain a film roll.
[0033] Each step will be described in detail below. (Extrusion process) First, a polypropylene resin composition mainly composed of polypropylene resin is heated and melted in a range of 200°C to 300°C using a single-screw or twin-screw extruder, and the sheet-shaped molten polypropylene resin composition is extruded from a T-die and cooled and solidified by contacting it with a metal cooling roll. The obtained unstretched sheet is preferably further placed in a water tank. The temperature of the cooling roll, or the cooling roll and water bath, is preferably in the range of 10° C. to Tc. When it is desired to increase the transparency of the film, it is preferable to cool and solidify the film with a cooling roll having a temperature of 10 to 50° C. If the cooling temperature is 50° C. or less, the transparency of the unstretched sheet is likely to increase, and it is preferably 40° C. or less, and more preferably 30° C. or less. In order to increase the degree of crystal orientation after sequential biaxial stretching, it may be preferable to set the cooling temperature to 40° C. or more, but when a propylene homopolymer having a mesopent fraction of 97.0% or more is used as described above, it is preferable to set the cooling temperature to 40° C. or less in order to easily perform the stretching in the next step and to reduce thickness unevenness, and it is more preferable to set the cooling temperature to 30° C. or less. The thickness of the unstretched sheet is preferably 3500 μm or less in terms of cooling efficiency, more preferably 3000 μm or less, and can be appropriately adjusted depending on the film thickness after sequential biaxial stretching. The thickness of the unstretched sheet can be controlled by the extrusion speed of the polypropylene resin composition and the lip width of the T-die, etc.
[0034] (Longitudinal stretching process) The lower limit of the longitudinal stretching ratio is preferably 3 times, more preferably 3.5 times, and particularly preferably 3.8 times. Within the above range, strength is easily increased and thickness unevenness is reduced. The upper limit of the longitudinal stretching ratio is preferably 8 times, more preferably 7.5 times, and particularly preferably 7 times. Within the above range, width direction stretching is easily performed in the width direction stretching step, and productivity is improved. The lower limit of the longitudinal stretching temperature is preferably Tm-40°C, more preferably Tm-37°C, and even more preferably Tm-35°C. Within this range, the subsequent width direction stretching becomes easy and thickness unevenness is reduced. The upper limit of the longitudinal stretching temperature is preferably Tm-7°C, more preferably Tm-10°C, and even more preferably Tm-12°C. Within this range, the heat shrinkage rate is easily reduced, and there is little deterioration in quality due to difficulty in applying the film to the stretching rolls and increasing surface roughness. The longitudinal stretching may be performed in two or more stages using three or more pairs of stretching rolls.
[0035] (Preheating process) Prior to the width direction stretching step, the uniaxially stretched film after the longitudinal stretching is heated in the range of Tm to Tm+25°C to soften the polypropylene resin composition. By setting the temperature at or above Tm, softening proceeds and width direction stretching becomes easier. By setting the temperature at or below Tm+25°C, orientation proceeds during transverse stretching and rigidity is easily developed. The temperature is more preferably Tm+2 to Tm+22°C, and particularly preferably Tm+3 to Tm+20°C. Here, the maximum temperature in the preheating step is defined as the preheating temperature.
[0036] (Width direction stretching process) In the transverse stretching step after the preheating step, a preferred method is as follows.
[0037] In the width direction stretching step, a section (early section) is provided in which stretching is performed at a temperature of Tm-10°C or more and the preheating temperature or less. In this case, the early section may start when the preheating temperature is reached, or when the temperature is lowered after reaching the preheating temperature to a temperature lower than the preheating temperature. The lower limit of the temperature in the early section in the width direction stretching step is preferably Tm-9° C., more preferably Tm-8° C., and even more preferably Tm-7° C. When the stretching temperature in the early section is within this range, stretching unevenness is unlikely to occur. The first section is followed by a second section (later section) in which the film is stretched at a temperature lower than that of the first section and not lower than Tm-70° C. and not higher than Tm-5° C. The upper limit of the stretching temperature in the latter section is preferably Tm-8° C., more preferably Tm-10° C. When the stretching temperature in the latter section is within this range, stiffness is easily developed. The lower limit of the stretching temperature in the latter section is preferably Tm-65° C., more preferably Tm-60° C., and further preferably Tm-55° C. When the stretching temperature in the latter section is within this range, film formation is likely to be stable. At the end of the latter section, i.e., immediately after the final width direction stretching ratio is reached, the film can be cooled. The cooling temperature is preferably equal to or lower than the temperature of the latter section, and is from Tm-80° C. to Tm-15° C., more preferably from Tm-80° C. to Tm-20° C., even more preferably from Tm-80° C. to Tm-30° C., and particularly preferably from Tm-70° C. to Tm-40° C. The temperature in the early section and the late section can be gradually decreased, or can be decreased in stages or in one stage, and each can be constant. Gradual decrease in temperature makes the film less likely to break and also tends to reduce the thickness variation of the film. In addition, it is preferable because the thermal shrinkage rate is also easily reduced and the film is less likely to whiten. The temperature may be gradually lowered from the end of the first section to the start of the second section in the width direction stretching step, or may be lowered stepwise or in one step.
[0038] The lower limit of the stretching ratio at the end of the first section of the width direction stretching step is preferably 4 times, more preferably 5 times, even more preferably 6 times, and particularly preferably 6.5 times. The upper limit of the stretching ratio at the end of the first section is preferably 15 times, more preferably 14 times, and even more preferably 13 times.
[0039] The lower limit of the final width direction stretching ratio in the width direction stretching step is preferably 5 times, more preferably 6 times, further preferably 7 times, and particularly preferably 8 times. When it is 5 times or more, the rigidity is easily increased and the thickness unevenness is easily reduced. The upper limit of the stretching ratio in the transverse direction is preferably 20 times, more preferably 17 times, and further preferably 15 times. When it is 20 times or less, the heat shrinkage rate is easily reduced, and the film is less likely to break during stretching.
[0040] In this way, by using a highly crystalline polypropylene resin with high stereoregularity and a high melting point, and adopting the above-mentioned width direction stretching process, the molecules of the polypropylene resin are highly aligned in the main orientation direction (which corresponds to the width direction in the above-mentioned width direction stretching process) even if the stretching ratio is not extremely large, so that crystals with very strong crystal orientation and high melting points in the obtained biaxially oriented film are easily produced. In addition, the orientation of the amorphous parts between the crystals is also increased in the main orientation direction (corresponding to the width direction in the width direction stretching process described above), and since there are many crystals with high melting points around the amorphous parts, the stretched polypropylene molecules in the amorphous parts are less likely to relax at temperatures lower than the melting point of the crystals, and tend to maintain their tensed state. Therefore, the entire biaxially oriented film can maintain high rigidity even at high temperatures. It should also be noted that the adoption of such a width direction stretching step tends to reduce the heat shrinkage rate at a high temperature of 150° C. The reason for this is that since there are many crystals with high melting points around the amorphous parts, the elongated polypropylene resin molecules in the amorphous parts are less likely to relax at temperatures lower than the melting points of the crystals, and moreover, there is less entanglement between the molecules.
[0041] Another noteworthy point is that by increasing the low molecular weight component of the polypropylene resin, the crystallization degree of the film is more likely to be increased, and the entanglement of the polypropylene resin molecular chains in the amorphous portion is lessened, weakening the heat shrinkage stress and further reducing the heat shrinkage rate. Considering that in the past, if either the strength or the heat shrinkage rate was improved, the other property tended to decrease, this is a groundbreaking development.
[0042] (Heat treatment process) The biaxially oriented film can be heat treated, if desired, to further reduce the heat shrinkage. The upper limit of the heat treatment temperature is preferably Tm+10° C., more preferably Tm+7° C. By setting the temperature at Tm+10° C. or less, rigidity is easily exhibited, the film surface does not become too rough, and the film is less likely to whiten. The lower limit of the heat treatment temperature is preferably Tm-10° C., more preferably Tm-7° C. If the temperature is lower than Tm-10° C., the heat shrinkage rate may become high. By adopting the above-mentioned width direction stretching process, the highly oriented crystals formed in the stretching process are unlikely to melt even when heat treatment is performed at a temperature between Tm-10°C and Tm+10, and the thermal shrinkage rate can be reduced without decreasing the rigidity of the obtained film. In order to adjust the thermal shrinkage rate, the film may be relaxed (relaxed) in the width direction during heat treatment. The upper limit of the relaxation rate is preferably 10%. Within the above range, the film strength is less likely to decrease and the film thickness fluctuation is likely to be small. It is more preferably 8%, even more preferably 7%, even more preferably 3%, particularly preferably 2%, and most preferably 0%.
[0043] (film thickness) The thickness of the biaxially oriented polypropylene film of the present invention is set according to each application, but in order to obtain the strength of the film, the lower limit of the film thickness is preferably 2 μm, more preferably 3 μm, even more preferably 4 μm, particularly preferably 8 μm, and most preferably 10 μm. When the film thickness is 2 μm or more, the film is easily rigid. The upper limit of the film thickness is preferably 100 μm, more preferably 80 μm, even more preferably 60 μm, particularly preferably 50 μm, and most preferably 40 μm. When the film thickness is 100 μm or less, the cooling rate of the unstretched sheet during the extrusion process is unlikely to be reduced. The biaxially oriented polypropylene film of the present invention is usually produced as a roll having a width of about 2000 to 12000 mm and a length of about 1000 to 50000 m, and wound into a film roll. It is then slit according to the intended use and provided as a slit roll having a width of about 300 to 2000 mm and a length of about 500 to 5000 m. The biaxially oriented polypropylene film of the present invention can be used to obtain a longer film roll.
[0044] (Thickness uniformity) The lower limit of the thickness uniformity of the biaxially oriented polypropylene film of the present invention is preferably 0%, more preferably 0.1%, even more preferably 0.5%, and particularly preferably 1%. The upper limit of the thickness uniformity is preferably 20%, more preferably 17%, even more preferably 15%, particularly preferably 12%, and most preferably 10%. Within the above range, defects are unlikely to occur during post-processing such as coating and printing, and the film is easy to use in applications requiring precision. The measurement method was as follows: A test piece 40 mm wide was cut out from a steady region where the film properties were stable in the length direction of the film, and the film thickness was measured continuously over 20,000 mm using a film feeder manufactured by Micron Measurement Instruments Co., Ltd. (product number: A90172) and a continuous film thickness measuring instrument manufactured by Anritsu Corporation (product name: K-313A wide-range high-sensitivity electronic micrometer), and the thickness uniformity was calculated using the following formula. Thickness uniformity (%) = [(maximum thickness value - minimum thickness value) / average thickness value] x 100
[0045] (Film characteristics) The biaxially oriented polypropylene film of the present invention is characterized by the following properties. Here, the "longitudinal direction" of the biaxially oriented polypropylene film of the present invention is the direction corresponding to the flow direction in the film manufacturing process, and the "width direction" is the direction perpendicular to the flow direction in the film manufacturing process. For polypropylene films whose flow direction in the film manufacturing process is unknown, wide-angle X-rays are incident perpendicularly to the film surface, and the scattering peaks originating from the (110) plane of the α-type crystals are scanned in the circumferential direction, and the direction with the largest diffraction intensity in the obtained diffraction intensity distribution is defined as the "width direction," and the direction perpendicular to that is defined as the "longitudinal direction."
[0046] (Half-width of diffraction peak due to oriented crystals) In the azimuth angle dependence of the scattering peak of the (110) plane of the polypropylene α-type crystals obtained by wide-angle X-ray measurement perpendicular to the film surface of the biaxially oriented polypropylene film of the present invention, the upper limit of the half-width (Wh) of the diffraction peak derived from the oriented crystals in the width direction of the film is 27°, preferably 26°, more preferably 25°, even more preferably 24°, and particularly preferably 23°. If the half-width (Wh) is 27° or less, the rigidity of the film is easily increased. The lower limit of Wh is preferably 13°, more preferably 14°, and even more preferably 15°.
[0047] (tanδ area) The tan δ area, obtained from the loss tangent (tan δ) obtained as the ratio (E" / E') of the storage modulus (E') to the loss modulus (E") measured by a dynamic mechanical analyzer (DMA) of the biaxially oriented polypropylene film of the present invention, is preferably 0.35 in the longitudinal direction, more preferably 0.32 or less, even more preferably 0.3 or less, and particularly preferably 0.29 or less. The tan δ area in the longitudinal direction is preferably 0.1 or more, more preferably 0.13 or more, even more preferably 0.15 or more, and particularly preferably 0.16 or more. The tan δ area in the width direction is 0.4 or less, more preferably 0.37, even more preferably 0.35, and particularly preferably 0.33. The tan δ area in the width direction is 0.2 or more, preferably 0.21 or more, more preferably 0.22 or more, and particularly preferably 0.23 or more. When the tan δ area obtained by DMA measurement is within this range, the strength of the biaxially oriented polypropylene film is significantly increased, and even if the film is thin, it maintains its stiffness and strength, which can greatly contribute to reducing the volume of the film. As described above, it is not easy to set the tan δ area obtained by DMA measurement in the longitudinal and transverse directions to a specific range, and in order to obtain such characteristics, a great deal of trial and error was carried out, and they were finally achieved.
[0048] The biaxially oriented polypropylene film of the present invention preferably has the following characteristics and structure. (Young's modulus at 23°C) The lower limit of the Young's modulus in the longitudinal direction of the biaxially oriented polypropylene film of the present invention at 23 ° C. is preferably 2.0 GPa, more preferably 2.1 GPa, even more preferably 2.2 GPa, particularly preferably 2.3 GPa, and most preferably 2.4 GPa. At 2.0 GPa or more, the rigidity is high, so that the bag shape when made into a packaging bag is easily maintained, and the film is less likely to deform during processing such as printing. The upper limit of the Young's modulus in the longitudinal direction is preferably 4.0 GPa, more preferably 3.8 GPa, even more preferably 3.7 GPa, particularly preferably 3.6 GPa, and most preferably 3.5 GPa. At 4.0 GPa or less, practical production is easy and the balance of the properties in the longitudinal direction and the width direction is easily improved.
[0049] The lower limit of the Young's modulus in the width direction at 23°C of the biaxially oriented polypropylene film of the present invention is preferably 6.0 GPa, more preferably 6.3 GPa, even more preferably 6.5 GPa, and particularly preferably 6.7 GPa. At 6.0 GPa or more, the rigidity is high, so that the bag shape when made into a packaging bag is easily maintained, and the film is less likely to deform during processing such as printing. The upper limit of the Young's modulus in the width direction is preferably 15 GPa, more preferably 13 GPa, and even more preferably 12 GPa. At 15 GPa or less, practical production is easy and the balance of the properties in the longitudinal direction and the width direction is easily improved. The Young's modulus can be kept within the range by adjusting the stretch ratio and relaxation rate, or by adjusting the temperature during film formation.
[0050] (Young's modulus at 80℃) The lower limit of the Young's modulus in the longitudinal direction of the biaxially oriented polypropylene film of the present invention at 80° C. is preferably 0.5 GPa, more preferably 0.7 GPa. At 0.5 GPa or more, printing pitch deviation is unlikely to occur when transferring high-temperature printing ink. The upper limit of the Young's modulus in the longitudinal direction at 80° C. is preferably 3.0 GPa, more preferably 2.5 GPa. At 3.0 GPa or more, practical production is easy.
[0051] The lower limit of the Young's modulus in the width direction at 80°C is preferably 2.5 GPa, more preferably 2.8 GPa, and even more preferably 3.0 GPa. At 2.5 GPa or more, printing pitch deviation is unlikely to occur when transferring high-temperature printing ink. The upper limit of the Young's modulus in the width direction at 80°C is preferably 5.0 GPa, more preferably 4.7 GPa, and even more preferably 4.5 GPa. At 5.0 GPa or less, practical production is easy. The Young's modulus at 80° C. can be kept within the range by adjusting the stretch ratio, stretching temperature and heat setting temperature.
[0052] (Stress at 23℃ 5% elongation) The lower limit of the stress (F5) at 5% elongation in the longitudinal direction of the biaxially oriented polypropylene film of the present invention at 23°C is 40 MPa, preferably 42 MPa, more preferably 43 MPa, even more preferably 44 MPa, and particularly preferably 45 MPa. At 40 MPa or more, the film has high rigidity, so that the shape of the bag when made into a packaging bag is easily maintained, and the film is less likely to deform during processing such as printing. The upper limit of F5 in the longitudinal direction is preferably 70 MPa, more preferably 65 MPa, even more preferably 62 MPa, especially preferably 61 MPa, and most preferably 60 MPa. At 70 MPa or less, practical production is easy and the vertical-width balance is easily improved. The lower limit of F5 in the width direction of the biaxially oriented polypropylene film of the present invention at 23°C is 160 MPa, preferably 165 MPa, more preferably 168 MPa, and even more preferably 170 MPa. At 160 MPa or more, the rigidity is high, so that the bag shape when made into a packaging bag is easily maintained, and the film is less likely to deform during processing such as printing. The upper limit of F5 in the width direction is preferably 250 MPa, more preferably 245 MPa, and even more preferably 240 MPa. At 250 MPa or less, practical production is easy and the vertical-width balance is easily improved. F5 can be kept within the range by adjusting the stretch ratio and relaxation rate, or by adjusting the temperature during film formation. (Stress at 80℃ 5% elongation) The lower limit of the stress (F5) of the biaxially oriented polypropylene film of the present invention at 80°C when elongated by 5% in the longitudinal direction is 15 MPa, preferably 17 MPa, more preferably 19 MPa, and even more preferably 20 MPa. At 15 MPa or more, the film has high rigidity, so that the shape of the bag when made into a packaging bag is easily maintained, and the film is less likely to deform during processing such as printing. The upper limit of F5 at 80°C in the longitudinal direction is preferably 40 MPa, more preferably 35 MPa, even more preferably 30 MPa, and particularly preferably 25 MPa. At 40 MPa or less, practical production is easy and the vertical-width balance is easily improved. The lower limit of F5 in the width direction of the biaxially oriented polypropylene film of the present invention at 80°C is 75 MPa, preferably 80 MPa, more preferably 85 MPa, even more preferably 90 MPa, and particularly preferably 95 MPa. At 75 MPa or more, the rigidity is high, so that the bag shape when made into a packaging bag is easily maintained, and the film is less likely to deform during processing such as printing. The upper limit of F5 in the width direction at 80°C is preferably 150 MPa, more preferably 140 MPa, and even more preferably 130 MPa. At 140 MPa or less, practical production is easy and the vertical-width balance is easily improved. The 80° C. F5 can be kept within the range by adjusting the stretch ratio and relaxation rate, or by adjusting the temperature during film formation.
[0053] (Heat shrinkage rate at 120℃) The upper limit of the heat shrinkage rate in the longitudinal direction of the biaxially oriented polypropylene film of the present invention at 120°C is preferably 2.0%, more preferably 1.7%, and even more preferably 1.5%. If it is 2.0% or less, printing pitch deviation is unlikely to occur when transferring printing ink. The upper limit of the heat shrinkage rate in the transverse direction at 120°C is preferably 5.0%, more preferably 4.5%, and even more preferably 4.0%. If it is 5.0% or less, wrinkles are unlikely to occur during heat sealing. If the longitudinal heat shrinkage rate at 120°C is smaller than the transverse heat shrinkage rate at 120°C, printing pitch deviation is less likely to occur when transferring printing ink. The thermal shrinkage rate at 120°C and the balance of the thermal shrinkage rates in the longitudinal and transverse directions can be kept within the range by adjusting the stretch ratio, stretching temperature, and heat setting temperature. (Heat shrinkage rate at 150℃) The upper limit of the heat shrinkage rate in the longitudinal direction of the biaxially oriented polypropylene film of the present invention at 150°C is preferably 10%, more preferably 8.0%, and particularly preferably 7.0%. The upper limit of the heat shrinkage rate in the width direction at 150°C is preferably 30%, more preferably 25%, and particularly preferably 20%. When the heat shrinkage rate in the longitudinal direction is 10% or less and the heat shrinkage rate in the width direction is 30% or less, wrinkles are unlikely to occur during heat sealing, and when the heat shrinkage rate in the longitudinal direction at 150°C is 7.0% or less and the heat shrinkage rate in the width direction at 150°C is 20% or less, distortion when the zipper part is fused to the opening part is small, which is preferable. In order to reduce the heat shrinkage rate at 150°C, it is effective to adjust the stretching ratio, film-forming temperature, and relaxation rate, or to set the lower limit of the amount of components with a molecular weight of 100,000 or less to 35% by mass when measuring the gel permeation chromatography (GPC) cumulative curve of the polypropylene resin constituting the film.
[0054] (Refractive Index) The lower limit of the refractive index (Nx) in the longitudinal direction of the biaxially oriented polypropylene film of the present invention is preferably 1.4950, more preferably 1.4970, and even more preferably 1.4980. If it is 1.4950 or more, the rigidity of the film is easily increased. The upper limit of the refractive index (Nx) in the longitudinal direction is preferably 1.5100, more preferably 15070, and even more preferably 1.5050. If it is 1.5100 or less, the film is likely to have an excellent balance of properties in the longitudinal direction and the width direction.
[0055] The lower limit of the refractive index (Ny) in the width direction of the biaxially oriented polypropylene film of the present invention is 1.5230, preferably 1.5235, and more preferably 1.5240. If it is 1.5230 or more, the rigidity of the film is easily increased. The upper limit of the refractive index (Ny) in the width direction is preferably 1.5280, more preferably 1.5275, and even more preferably 1.5270. If it is 1.5280 or less, the film is likely to have an excellent balance of properties in the longitudinal direction and the width direction.
[0056] The lower limit of the refractive index (Nz) in the thickness direction of the biaxially oriented polypropylene film of the present invention is preferably 1.4960, more preferably 14965, and even more preferably 1.4970. If it is 1.4960 or more, the rigidity of the film is easily increased. The upper limit of the refractive index (Nz) in the thickness direction is preferably 1.5020, more preferably 1.5015, and even more preferably 1.5010. If it is 1.5020 or less, the heat resistance of the film is easily increased. The refractive index can be adjusted within the range by adjusting the stretch ratio, stretching temperature, and heat setting temperature.
[0057] (△Ny) The lower limit of ΔNy of the biaxially oriented polypropylene film of the present invention is 0.0220, preferably 0.0225, more preferably 0.0228, and even more preferably 0.0230. If it is 0.0220 or more, the rigidity of the film tends to be high. The upper limit of ΔNy is preferably 0.0270 as a practical value, more preferably 0.0265, even more preferably 0.0262, and particularly preferably 0.0260. If it is 0.0270 or less, the thickness unevenness tends to be good. ΔNy can be kept within the range by adjusting the stretch ratio, stretching temperature, and heat setting temperature of the film. ΔNy is calculated by the following formula, where Nx, Ny, and Nz are the refractive indices along the length, width, and thickness directions of the film, respectively, and it means the degree of orientation in the width direction in the overall orientation of the film in the length, width, and thickness directions. △Ny=Ny-[(Nx+Nz) / 2]
[0058] (Face orientation coefficient) The lower limit of the plane orientation coefficient (ΔP) of the biaxially oriented polypropylene film of the present invention is preferably 0.0135, more preferably 0.0138, and even more preferably 0.0140. If it is 0.0135 or more, the balance in the plane direction of the film is good, and the thickness unevenness is also good. The upper limit of the plane orientation coefficient (ΔP) is preferably 0.0155 as a practical value, more preferably 0.0152, and even more preferably 0.0150. If it is 0.0155 or less, it is likely to have excellent heat resistance at high temperatures. The plane orientation coefficient (ΔP) can be adjusted within the range by adjusting the stretch ratio, stretching temperature, and heat setting temperature. The plane orientation coefficient (ΔP) was calculated using the formula: [(Nx+Ny) / 2]-Nz.
[0059] (X-ray orientation degree) The lower limit of the degree of X-ray orientation of the biaxially oriented polypropylene film of the present invention, calculated from Wh by the following formula, is preferably 0.85, more preferably 0.855, and even more preferably 0.861. By making it 0.85 or more, it is easy to increase the rigidity. X-ray orientation degree=(180-Wh) / 180 The upper limit of the degree of X-ray orientation is preferably 0.928, more preferably 0.922, and further preferably 0.917. By setting it to 0.928 or less, film formation is likely to be stable.
[0060] (Hayes) The upper limit of the haze of the biaxially oriented polypropylene film of the present invention is preferably 5.0%, more preferably 4.5%, even more preferably 4.0%, particularly preferably 3.5%, and most preferably 3.0%. If it is 5.0% or less, it is easy to use in applications where transparency is required. The lower limit of the haze is preferably 0.1% as a practical value, more preferably 0.2%, even more preferably 0.3%, and particularly preferably 0.4%. If it is 0.1% or more, it is easy to manufacture. The haze can be kept within the range by adjusting the cooling roll (CR) temperature, the width direction stretching temperature, the tenter preheating temperature before width direction stretching, the width direction stretching temperature, or the heat setting temperature, or the amount of the component having a molecular weight of 100,000 or less of the polypropylene resin, but it may become large by adding an antiblocking agent or providing a seal layer.
[0061] (Practical properties of film) The practical properties of the biaxially oriented polypropylene film of the present invention will now be described.
[0062] (Tensile breaking strength) The lower limit of the longitudinal tensile breaking strength of the biaxially oriented polypropylene film of the present invention is preferably 90 MPa, more preferably 95 MPa, and even more preferably 100 MPa. If it is 90 MPa or more, printing pitch deviation is unlikely to occur when transferring printing ink, and the durability of the packaging bag is likely to be excellent. The upper limit of the longitudinal tensile breaking strength is preferably 200 MPa as a practical value, more preferably 190 MPa, and even more preferably 180 MPa. If it is 200 MPa or less, film breakage and packaging bag breakage are likely to be reduced. The lower limit of the tensile breaking strength in the width direction of the biaxially oriented polypropylene film of the present invention is preferably 320 MPa, more preferably 340 MPa, and even more preferably 350 MPa. If it is 320 MPa or more, printing pitch deviation is unlikely to occur when transferring printing ink, and the durability of the packaging bag is likely to be excellent. The upper limit of the tensile breaking strength in the width direction is preferably 500 MPa as a practical value, more preferably 480 MPa, and even more preferably 470 MPa. If it is 500 MPa or less, film breakage and packaging bag breakage are likely to be reduced. The tensile breaking strength can be controlled within the range by adjusting the stretch ratio, stretching temperature and heat setting temperature.
[0063] (Tensile elongation at break) The lower limit of the longitudinal tensile elongation at break of the biaxially oriented polypropylene film of the present invention is preferably 50%, more preferably 55%, and even more preferably 60%. If it is 50% or more, the film breakage and the packaging bag breakage are likely to be reduced. The upper limit of the longitudinal tensile elongation at break is preferably 230%, more preferably 220%, and even more preferably 210%, as a practical value. If it is 230% or less, printing pitch deviation is unlikely to occur when transferring printing ink, and the durability of the packaging bag is also likely to be excellent.
[0064] The lower limit of the tensile elongation at break in the width direction of the biaxially oriented polypropylene film of the present invention is preferably 10%, more preferably 15%, and even more preferably 17%. If it is 10% or more, film breakage and packaging bag breakage are likely to be reduced. The upper limit of the tensile elongation at break in the width direction is preferably 60%, more preferably 55%, and even more preferably 50%. If it is 60% or less, printing pitch deviation is unlikely to occur when transferring printing ink, and the durability of the packaging bag is likely to be excellent. The tensile elongation at break can be adjusted within the range by adjusting the stretch ratio, stretching temperature, and heat setting temperature.
[0065] (bending resistance) The lower limit of bending resistance in the longitudinal direction of the biaxially oriented polypropylene film of the present invention at 23°C is preferably 0.3 mN·cm, more preferably 0.33 mN·cm, and even more preferably 0.35 mN·cm. If it is 0.3 mN·cm or more, the film can be thinned or is suitable for applications requiring rigidity. The lower limit of bending resistance in the transverse direction is preferably 0.5 mN·cm, more preferably 0.55 mN·cm, and even more preferably 0.6 mN·cm. If it is 0.5 mN·cm or more, the film can be thinned or is suitable for applications requiring rigidity.
[0066] (Loop stiffness stress) The lower limit of the longitudinal loop stiffness stress S (mN) of the biaxially oriented polypropylene film of the present invention at 23° C. is preferably 0.00020×t 3 and more preferably 0.00025×t 3 and more preferably 0.00030×t 3 and particularly preferably 0.00035×t 3 0.00020×t 3 If this is the case, the shape of the package can be easily maintained. The upper limit of the longitudinal loop stiffness stress S (mN) at 23° C. is preferably 0.00080×t 3 and more preferably 0.00075×t 3 and more preferably 0.00072×t 3 and particularly preferably 0.00070×t 3 0.00080×t 3 If it is less than this, it is easy to manufacture in practice. The lower limit of the loop stiffness stress S (mN) in the width direction of the biaxially oriented polypropylene film of the present invention at 23° C. is preferably 0.0010×t 3 and more preferably 0.0011×t 3 and more preferably 0.0012×t 3 and particularly preferably 0.0013×t 30.0010×t 3 If this is the case, the shape of the package can be easily maintained. The upper limit of the loop stiffness stress S (mN) in the width direction at 23° C. is preferably 0.0020×t 3 and more preferably 0.0019×t 3 and more preferably 0.0018×t 3 and particularly preferably 0.0017×t 3 0.0020×t 3 If it is less than this, it is easy to manufacture in practice.
[0067] The loop stiffness stress is an index of the stiffness of a film, but it also depends on the thickness of the film. The measurement method is as follows. Two strips of 110 mm x 25.4 mm were cut out with the longitudinal direction of the film as the long axis (loop direction) or the width direction of the film as the long axis (loop direction). These were clamped with a clip to create measurement loops with one side of the film as the inner surface of the loop and the other side as the inner surface of the loop, with the long axis of the strip in the longitudinal direction and the width direction of the film. The measurement loop with the long axis of the strip in the longitudinal direction of the film was set in the chuck of a loop stiffness tester DA manufactured by Toyo Seiki Co., Ltd. with the width direction perpendicular, and the clip was removed, and the loop stiffness stress was measured with a chuck interval of 50 mm, a pressing depth of 15 mm, and a compression speed of 3.3 mm / sec. The measurements were made five times for the loop stiffness stress and thickness with one side of the film facing the inner surface of the loop, and then five times for the other side facing the inner surface of the loop. Using the data from these 10 measurements, the cube of the thickness (μm) of each test piece was plotted on the horizontal axis and the loop stiffness stress (mN) on the vertical axis, and the curve was approximated with a straight line with an intercept of 0 to determine the slope a. The slope a represents a characteristic value specific to the film that does not depend on thickness and determines stiffness. The slope a was used as the evaluation value for stiffness. The measurement loop in which the long axis of the strip was in the width direction of the film was also measured in the same way.
[0068] (Wrinkles during heat sealing) To form a bag for packaging food, the contents are filled into a bag that has already been made, and the film is heated to melt and fuse to seal it. In addition, the same process is often used when making a bag while filling it with food. Usually, a sealant film made of polyethylene or polypropylene is laminated on the base film, and the sealant film surfaces are fused together. The heating method is to apply pressure from the base film side with a heating plate to hold down the film and seal it, and the seal width is often about 10 mm. At this time, the base film is also heated, and the shrinkage at that time causes wrinkles. In terms of bag durability, it is better to have fewer wrinkles, and it is also better to have fewer wrinkles to increase purchasing desire. The sealing temperature may be around 120°C, but a higher sealing temperature is required to increase the bag making processing speed, and even in that case, it is preferable that the shrinkage is small. When a zipper is fused to the opening of the bag, sealing at an even higher temperature is required.
[0069] (Print pitch deviation) Packaging films are often basically made up of a laminated film of a printed base film and a sealant film. Bag making machines are used to manufacture bags, and various types of bags are used, including three-sided bags, standing bags, and gusset bags. Print pitch deviation is thought to occur because tension and heat are applied to the film during the printing process, causing the film base material to expand and contract. Eliminating defective products due to print pitch deviation is important in terms of efficient use of resources and increasing purchasing motivation.
[0070] (Film processing) Printing on the biaxially oriented polypropylene film of the present invention can be carried out by letterpress printing, lithographic printing, intaglio printing, stencil printing or transfer printing, depending on the application. Also, it can be used as a laminate with heat sealability by laminating an unstretched sheet, uniaxially stretched film, or biaxially stretched film made of low density polyethylene, linear low density polyethylene, ethylene-vinyl acetate copolymer, polypropylene, or polyester as a sealant film. When gas barrier properties or heat resistance is to be improved, an unstretched sheet, uniaxially stretched film, or biaxially stretched film made of aluminum foil, polyvinylidene chloride, nylon, ethylene-vinyl alcohol copolymer, or polyvinyl alcohol can be provided as an intermediate layer between the biaxially oriented polypropylene film and the sealant film. An adhesive applied by dry lamination or hot melt lamination can be used to laminate the sealant film. To improve the gas barrier properties, aluminum or inorganic oxides can be vapor-deposited onto the biaxially oriented polypropylene film, the intermediate layer film, or the sealant film. Vacuum deposition, sputtering, and ion plating can be used as the vapor deposition method, but vacuum deposition of silica, alumina, or a mixture thereof is particularly preferred.
[0071] The biaxially oriented polypropylene film of the present invention can be made suitable for packaging fresh produce such as vegetables, fruits, flowers, and other plants that require high freshness by containing an anti-fog agent, such as fatty acid esters of polyhydric alcohols, amines of higher fatty acids, amides of higher fatty acids, or ethylene oxide adducts of amines or amides of higher fatty acids, in an amount of 0.2 to 5 mass %.
[0072] In addition, various additives for improving qualities such as slipperiness and antistatic properties, for example, lubricants such as wax and metal soaps for improving productivity, plasticizers, processing aids, heat stabilizers, antioxidants, antistatic agents, ultraviolet absorbers, etc. can also be blended within a range that does not impair the effects of the present invention.
[0073] (Industrial Applicability) Since the biaxially oriented polypropylene film of the present invention has the above-mentioned excellent properties not available in the prior art, it can be preferably used for packaging bags, and the thickness of the film can be made thinner than in the prior art.
[0074] Furthermore, it is also suitable for applications that require high temperatures, such as insulating films for capacitors and motors, backsheets for solar cells, barrier films for inorganic oxides, and base films for transparent conductive films such as ITO, as well as applications that require rigidity, such as separate films. In addition, it is now possible to use coating agents, inks, and laminating adhesives that were previously difficult to use, enabling coating and printing processes at high temperatures, which is expected to improve production efficiency. EXAMPLES
[0075] The present invention will be described in detail below with reference to examples. The characteristics were measured and evaluated by the following methods. (1) Melt flow rate The melt flow rate (MFR) was measured in accordance with JIS K 7210 at a temperature of 230° C. and a load of 2.16 kgf.
[0076] (2) Meso-pentad fraction The mesopentad fraction ([mmmm]%) of polypropylene resin is measured as follows: 13 The mesopentad fraction was calculated according to the method described in Zambelli et al., Macromolecules, Vol. 6, p. 925 (1973). 13 C-NMR measurements were performed using a BRUKER AVANCE500 at 110°C after dissolving 200 mg of a sample in a 8:2 mixture of o-dichlorobenzene and deuterated benzene at 135°C.
[0077] (3) Number average molecular weight, weight average molecular weight, amount of components with molecular weights of 100,000 or less, and molecular weight distribution of polypropylene resin The molecular weight was determined by gel permeation chromatography (GPC) using monodisperse polystyrene as the standard in terms of PP. When the baseline was unclear, the baseline was set to the lowest point of the high molecular weight tail of the elution peak closest to the elution peak of the standard substance. The GPC measurement conditions are as follows. Equipment: HLC-8321PC / HT (Tosoh Corporation) Detector: RI Solvent: 1,2,4-trichlorobenzene + dibutylhydroxytoluene (0.05%) Column: TSK gelguard column HHR (30) HT (7.5 mm I.D. x 7.5 cm) x 1 + TSK gel GMHHR-H (20) HT (7.8 mm I.D. x 30 cm) x 3 Flow rate: 1.0mL / min Injection volume: 0.3mL Measurement temperature: 140℃ The number average molecular weight (Mn) and the mass average molecular weight (Mw) are the molecular weights (M i ) number of molecules (N i ) is defined by the following formula: Number average molecular weight: Mn=Σ(N i M i ) / ΣN i Mass average molecular weight: Mw=Σ(N i M i 2 ) / Σ(N i M i ) Here, the molecular weight distribution can be obtained by Mw / Mn. In addition, the proportion of components having a molecular weight of 100,000 or less was determined from the integral curve of the molecular weight distribution obtained by GPC.
[0078] (4) Crystallization temperature (Tc), melting temperature (Tm) Heat measurements were performed under nitrogen atmosphere using a TA Instruments Q1000 differential scanning calorimeter. Approximately 5 mg was cut out from the polypropylene resin pellets and sealed in an aluminum pan for measurement. The temperature was raised to 230°C and held for 5 minutes, then cooled to 30°C at a rate of -10°C / min, and the exothermic peak temperature was taken as the crystallization temperature (Tc). The heat of crystallization (△Hc) was calculated by setting a baseline so that the area of the exothermic peak was smoothly connected from the start of the peak to the end of the peak. The temperature was held at 30°C for 5 minutes, and then raised to 230°C at 10°C / min, and the main endothermic peak temperature was taken as the melting temperature (Tm).
[0079] (5) Film thickness The thickness of the films was measured using a Seiko EM Millitron 1202D.
[0080] (6) Hayes Measurements were performed at 23°C in accordance with JIS K7105 using an NDH5000 manufactured by Nippon Denshoku Industries Co., Ltd.
[0081] (7) X-ray half-width, degree of orientation The measurements were made using an X-ray diffractometer (Rigaku Corporation, RINT2500) by the transmission method. X-rays with a wavelength of 1.5418 Å were used, and a scintillation counter was used as the detector. The film was stacked to a thickness of 500 μm to prepare a sample. The sample stage was placed at the diffraction peak position (diffraction angle 2θ = 14.1°) of the (110) plane of the α-crystal of polypropylene resin, and the sample was rotated 360° around the axis in the thickness direction of the film to obtain the azimuth angle dependence of the diffraction intensity of the (110) plane. From this azimuth angle dependence, the half-width Wh of the diffraction peak resulting from the oriented crystals in the width direction of the film was obtained. In addition, the degree of X-ray orientation was calculated using Wh according to the following formula. X-ray orientation degree=(180-Wh) / 180
[0082] (8)tanδ area Dynamic viscoelasticity measurements were performed using a TA Instruments Japan RSA-G2, with a 4 mm wide film sample set in the device with a chuck distance of 10 mm, and the temperature was raised from -60°C to 160°C at a rate of 5°C / min under a nitrogen atmosphere with a load of 10 g and a frequency of 10 Hz. The loss tangent (tan δ) area was obtained from the ratio of the obtained storage modulus (E') to the loss modulus (E") (storage modulus / loss modulus).
[0083] (9) Refractive index, △Ny, and plane orientation coefficient Measurements were made at a wavelength of 589.3 nm and a temperature of 23°C using an Abbe refractometer manufactured by Atago Co., Ltd. The refractive indices along the longitudinal and width directions of the film were designated Nx and Ny, respectively, and the refractive index along the thickness direction was designated Nz. ΔNy was calculated using Nx, Ny, and Nz using the formula Ny-[(Nx+Nz) / 2]. The plane orientation coefficient (ΔP) was calculated using the formula [(Nx+Ny) / 2]-Nz.
[0084] (10) Tensile test The tensile strength of the film in the longitudinal and transverse directions was measured at 23°C according to JIS K 7127. Samples were cut out from the film to a size of 15 mm x 200 mm, and the chuck width was set to 100 mm in a tensile tester (Instron 5965 dual column tabletop tester manufactured by Instron Japan Co., Ltd.). The tensile test was performed at a tensile speed of 200 mm / min. From the obtained strain-stress curve, the Young's modulus was calculated from the slope of the linear portion at the beginning of elongation, and the stress at 5% elongation (F5) was calculated. The tensile breaking strength and tensile breaking elongation were the strength and elongation, respectively, at the time when the sample broke. The measurements were carried out in a thermostatic chamber at 80° C. to determine the Young's modulus and F5 at 80° C. The measurements were carried out by setting the chuck in the thermostatic chamber, which had been set to 80° C. in advance, and holding the sample there for 1 minute before measurement.
[0085] (11)Heat shrinkage rate The measurement was performed according to the following method in accordance with JIS Z 1712. The film was cut into pieces of 20 mm width and 200 mm length in both the longitudinal and transverse directions of the film, and was heated for 5 minutes by hanging them in a hot air oven at 120°C or 150°C. The length after heating was measured, and the thermal shrinkage rate was calculated as the ratio of the shrunken length to the original length.
[0086] (12) Bending resistance and sagging amount It was determined according to the following procedure in accordance with JIS L 1096B (slide method). A test piece of 20 mm x 150 mm was prepared, and after aligning the top surface of the tester body with that of the moving table, the test piece was placed on the table of the tester so that it protruded 50 mm, and a weight was attached. Then, the handle was gently turned to lower the sample table, and the amount of sagging (δ) was measured at the point when the free end of the sample left the sample table. This amount of sagging δ, the film thickness, the size of the test piece, and the film density of 0.91 g / cm 3 The bending resistance (Br) was calculated using the following formula. Br=WL 4 / 8δ Br: Bending resistance (mN cm) W: Gravity per unit area of the test piece (mN / cm 2 ) L: Length of test piece (cm) δ: sagging amount (cm)
[0087] (13) Loop stiffness stress Ten strip-shaped test pieces measuring 110 mm x 25.4 mm were cut out with the longitudinal direction of the film as the long axis of the strip (loop direction) or the width direction of the film as the long axis of the strip (loop direction). These were clamped with a clip to create measurement loops in which one side of the film was the inner surface of the loop and the other side was the inner surface of the loop, with the long axis of the strip being in the longitudinal direction and the width direction of the film. The measurement loop in which the long axis of the strip was in the longitudinal direction of the film was set in the chuck of a loop stiffness tester DA manufactured by Toyo Seiki Seisakusho Co., Ltd. with the width direction perpendicular, the clip was removed, and the loop stiffness stress was measured with a chuck interval of 50 mm, a pressing depth of 15 mm, and a compression speed of 3.3 mm / sec. The measurement was performed five times to measure the loop stiffness stress and thickness with one side of the film being the inner surface of the loop, and then five times to measure with the other side being the inner surface of the loop. Using the data from these 10 runs, the cube of the thickness (μm) of each test piece was plotted on the horizontal axis and the loop stiffness stress (mN) on the vertical axis, and the line was approximated with an intercept of 0 to determine the slope a. The slope a was used as the evaluation value for stiffness. The measurement loop in which the long axis of the strip was in the width direction of the film was also measured in the same manner.
[0088] Example 1 As the polypropylene resin, propylene homopolymer PP-1 (Sumitomo Chemical Co., Ltd., Sumitomo Noblen FLX80E4) with MFR = 7.5 g / 10 min, Tc = 116.2 ° C, Tm = 162.5 ° C was used. The sheet was extruded from a T-die at 250 ° C into a sheet, contacted with a cooling roll at 20 ° C, and then put into a water bath at 20 ° C as it is. Thereafter, the sheet was stretched 4.5 times in the longitudinal direction with two pairs of rolls at 145 ° C, then both ends were clamped with clips, introduced into a hot air oven, preheated at 170 ° C, and then stretched 6 times in the width direction at 160 ° C as the first stage, and subsequently stretched 1.36 times at 145 ° C as the second stage, thereby performing a total stretching of 8.2 times. Immediately after the width direction stretching, the sheet was cooled at 100 ° C while being held by the clip, and then heat-set at 163 ° C. The thickness of the film thus obtained was 18.7 μm. The structure of the polypropylene resin is shown in Table 1, and the film-forming conditions are shown in Table 2. As for the physical properties, as shown in Table 3, a film with high rigidity and low thermal shrinkage at high temperatures was obtained.
[0089] Example 2 As the polypropylene resin, 80 parts by weight of PP-1 and 20 parts by weight of propylene homopolymer PP-2 (manufactured by Sumitomo Chemical Co., Ltd., EL80F5) having MFR=11g / 10min, [mmmm]=98.8%, Tc=116.5°C, and Tm=161.5°C were blended and used. The same procedure was followed as in Example 1, except that the longitudinal stretching temperature was 142°C, the first-stage widthwise stretching temperature was 162°C, and the heat setting temperature was 165°C. The thickness of the obtained film was 21.3 μm. Table 1 shows the structure of the polypropylene resin, and Table 2 shows the film-forming conditions. As shown in Table 3, the film had high rigidity and low heat shrinkage at high temperatures.
[0090] Example 3 The same procedure was followed as in Example 2, except that 3% relaxation was performed during heat setting. The thickness of the obtained film was 21.1 μm. Table 1 shows the structure of the polypropylene resin, and Table 2 shows the film formation conditions. As shown in Table 3, the physical properties of the film obtained were high rigidity and low thermal shrinkage at high temperatures.
[0091] Example 4 The same procedure as in Example 2 was carried out, except that the longitudinal stretching temperature was 145°C, and the cooling temperature immediately after the widthwise stretching was 140°C. The thickness of the obtained film was 18.9 μm. Table 1 shows the structure of the polypropylene resin, and Table 2 shows the film-forming conditions. As for the physical properties, as shown in Table 3, a film with high rigidity was obtained.
[0092] Example 5 The same procedure was followed as in Example 2, except that after the width direction stretching, the film was not cooled but was heat-set at 165°C while still being held by the clips. The thickness of the obtained film was 19.5 µm. Table 1 shows the structure of the polypropylene resin, and Table 2 shows the film-forming conditions. As for the physical properties, as shown in Table 3, a film with high rigidity and low thermal shrinkage at high temperatures was obtained.
[0093] Example 6 The same procedure as in Example 2 was carried out except that the second-stage stretching temperature in the width direction was 155°C. The thickness of the film thus obtained was 20.3 µm. Table 1 shows the structure of the polypropylene resin, and Table 2 shows the film-forming conditions. As for the physical properties, as shown in Table 3, a film having high rigidity and low thermal shrinkage at high temperatures was obtained.
[0094] Example 7 The same procedure as in Example 2 was carried out except that the longitudinal stretching ratio was 4.8 times. The thickness of the obtained film was 19.1 μm. Table 1 shows the structure of the polypropylene resin, and Table 2 shows the film-forming conditions. As shown in Table 3, the physical properties of the obtained film were high in rigidity and low in heat shrinkage at high temperatures.
[0095] Example 8 The same procedure as in Example 2 was carried out except that in the width direction stretching, the first stage stretching ratio was 6.6 times, the second stage stretching ratio was 1.5 times, and the total stretching ratio was 9.9 times. The thickness of the obtained film was 20.1 μm. Table 1 shows the structure of the polypropylene resin, and Table 2 shows the film-forming conditions. As for the physical properties, as shown in Table 3, a film having high rigidity and low heat shrinkage at high temperatures was obtained.
[0096] Comparative Example 1 PP-1 was used as the polypropylene resin, and the extrusion was performed at 250°C from a T-die into a sheet, contacted with a cooling roll at 20°C, and then directly put into a water tank at 20°C. Then, the film was stretched 4.5 times in the longitudinal direction at 143°C, and stretched 8.2 times with a preheating temperature of 170°C and a stretching temperature of 158°C during widthwise stretching in the tenter, and then heat-set at 168°C. The thickness of the obtained film was 18.6 μm. Table 1 shows the structure of the polypropylene resin, Table 2 shows the film-forming conditions, and Table 3 shows the physical properties. As shown in Table 3, the physical properties were low in rigidity.
[0097] Comparative Example 2 The same procedure as in Comparative Example 1 was repeated, except that a blend of 80 parts by weight of PP-1 and 20 parts by weight of PP-2 was used as the polypropylene resin. The thickness of the obtained film was 20.0 μm. Table 1 shows the structure of the polypropylene resin, Table 2 shows the film-forming conditions, and Table 3 shows the physical properties. As shown in Table 3, the physical properties were low in rigidity.
[0098] Comparative Example 3 As the polypropylene resin, PP-3 (manufactured by Japan Polypropylene Corporation, FL203D) with MFR=3g / 10min, Tc=117.2℃, and Tm=160.6℃ was used. The resin was extruded from a T-die at 250℃ into a sheet, brought into contact with a cooling roll at 20℃, and then put into a water bath at 20℃. The resin was then stretched 4.5 times in the longitudinal direction at 135℃, and stretched in the transverse direction with a tenter at a preheating temperature of 166℃, a temperature of the first stretching stage of 155℃, a temperature of the second stretching stage of 139℃, a cooling temperature of 95℃, and a heat setting temperature of 158℃. The thickness of the obtained film was 19.2μm. Table 1 shows the structure of the polypropylene resin, Table 2 shows the film-forming conditions, and Table 3 shows the physical properties. As shown in Table 3, the physical properties showed a high thermal shrinkage rate at high temperatures.
[0099] Comparative Example 4 As a polypropylene raw material, PP-4 (Sumitomo Chemical Co., Ltd., FS2012) with MFR=2.7g / 10min, Tc=114.7℃, and Tm=163.0℃ was used. The sheet was extruded from a T-die at 250℃ into a sheet, brought into contact with a cooling roll at 20℃, and then put into a water tank at 20℃. The sheet was then stretched 4.5 times in the longitudinal direction at 145℃, and in the transverse direction stretching with a tenter, the preheating temperature was 170℃, the temperature of the first stretching stage was 160℃, the temperature of the second stretching stage was 145℃, the cooling temperature was 100℃, and the heat setting temperature was 163℃. The thickness of the obtained film was 21.2μm. Table 1 shows the structure of the polypropylene resin, Table 2 shows the film formation conditions, and Table 3 shows the physical properties. As shown in Table 3, the physical properties showed a high thermal shrinkage rate at high temperatures.
[0100] Comparative Example 5 PP-4 was used as the polypropylene resin. The polypropylene resin was extruded into a sheet from a T-die at 250°C, brought into contact with a cooling roll at 20°C, and then directly put into a water tank at 20°C. After that, the film was stretched 5.8 times in the longitudinal direction at 130°C, heated in a tenter at a preheating temperature of 167°C, and then stretched 8.6 times in the transverse direction at a stretching temperature of 161°C, and then heat-set at 130°C while applying 10% relaxation, and then heat-set in the second stage at 140°C. The thickness of the obtained film was 13.4 μm. Table 1 shows the structure of the polypropylene resin, Table 2 shows the film-forming conditions, and Table 3 shows the physical properties. As shown in Table 3, the physical properties showed a high thermal shrinkage rate at high temperatures.
[0101] [Table 1]
[0102] [Table 2]
[0103] [Table 3]
Claims
1. A biaxially oriented polypropylene film made of a polypropylene resin composition containing 90 mass% or more of a polypropylene resin having a mesopentad fraction of 97.0% or more and 99.9% or less and a melt flow rate of 4.0 g / 10 min or more and 30 g / 10 min or less, wherein in the azimuth angle dependence of the polypropylene α-crystal (110) plane obtained by wide-angle X-ray diffraction measurement, the half-width of a peak derived from oriented crystals in the width direction is 27° or less, the stress at 5% elongation at 80°C is 15 MPa or more in the longitudinal direction and 75 MPa or more in the width direction, and the tan δ area obtained from the ratio (E" / E') of the storage modulus (E') to the loss modulus (E") obtained by dynamic viscoelasticity measurement is 0.2 to 0.4 in the width direction.
2. The biaxially oriented polypropylene film according to claim 1, wherein the 120°C heat shrinkage of the biaxially oriented polypropylene film is 2.0% or less in the longitudinal direction and 5.0% or less in the transverse direction, and the 120°C heat shrinkage in the longitudinal direction is smaller than the 120°C heat shrinkage in the transverse direction.
3. 3. The biaxially oriented polypropylene film according to claim 1, wherein the refractive index Ny in the width direction of the biaxially oriented polypropylene film is 1.5230 or more and ΔNy is 0.0220 or more.
4. The biaxially oriented polypropylene film according to any one of claims 1 to 3, wherein the haze of the biaxially oriented polypropylene film is 5.0% or less.
5. The biaxially oriented polypropylene film according to any one of claims 1 to 4, wherein the polypropylene resin is a polypropylene homopolymer and / or a propylene copolymer containing 1 mol% or less of ethylene and / or an α-olefin component having 4 or more carbon atoms.
6. The biaxially oriented polypropylene film according to any one of claims 1 to 5, wherein the polypropylene resin constituting the biaxially oriented polypropylene film has a crystallization temperature of 105°C or higher and a melting point of 160°C or higher.
7. The biaxially oriented polypropylene film according to any one of claims 1 to 6, wherein the amount of components of the polypropylene resin constituting the biaxially oriented polypropylene film having a molecular weight of 100,000 or less is 35% by mass or more.
8. The biaxially oriented polypropylene film according to any one of claims 1 to 7, wherein the degree of orientation of the biaxially oriented polypropylene film is 0.85 or more.
Citation Information
Patent Citations
Easily tearable cast film
JP2006117956A
Biaxially oriented polypropylene film and method for producing the same
JP2013177645A
Biaxially oriented polypropylene film for capacitor, metal film laminated film, and film capacitor
JP2016188361A
Laminated film
JP2017226161A
Stretched polypropylene film
WO2015012324A1