Dispersion resin, coloring composition for color filters, color filter and solid-state image pickup device

By using a dispersion resin with a high refractive index and pigment dispersion resin, the sensitivity and thickness issues of solid-state image sensors are addressed, enhancing sensitivity and image quality.

JP7586262B1Active Publication Date: 2024-11-19TOYO INK MFG CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023174160
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-10-06
Publication Date
2024-11-19
Estimated Expiration
2043-10-06

AI Technical Summary

Technical Problem

The sensitivity characteristics of solid-state image sensors deteriorate due to oblique light incidence and color mixture, especially in small camera modules, necessitating improved sensitivity and reduced color filter thickness.

Method used

A dispersion resin with a refractive index of 1.54 or more is used to increase the refractive index of color filters, combined with a pigment dispersion resin to prevent particle aggregation, enhancing sensitivity characteristics and allowing for thinner color filters.

Benefits of technology

The solution improves sensitivity characteristics by increasing the refractive index of color filters, reducing thickness, and preventing light mixing, resulting in better image quality and sensitivity in solid-state image sensors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586262000001_ABST
    Figure 0007586262000001_ABST
Patent Text Reader

Abstract

The present invention provides a dispersion resin having an increased refractive index, a coloring composition for color filters having a high refractive index and containing the dispersion resin, a color filter, and a solid-state imaging device having improved sensitivity characteristics. The dispersion resin has a first portion that has affinity for the pigment and a second portion that functions to prevent aggregation of the pigment particles. The dispersion resin has a refractive index of 1.54 or more at a wavelength of 594 nm.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a dispersion resin, a coloring composition for a color filter, a color filter, and a solid-state imaging device. [Background technology]

[0002] The unit pixels of solid-state imaging devices are becoming smaller and smaller, becoming smaller than 1.0μm square (a square with one side measuring 1μm in plan view).In addition, as electronic devices (smartphones, digital cameras, etc.) incorporating solid-state imaging devices become smaller and thinner, technology is needed to ensure and further improve sensitivity characteristics. To improve the sensitivity characteristics of solid-state imaging elements, it is necessary to reduce the height in the vertical direction (shrink in three dimensions) by thinning the color filters in response to the miniaturization of unit pixels (shrink in two dimensions).

[0003] In particular, in a compact camera module in which a solid-state imaging element is integrated with an optical lens, etc., the light incident on the end of the solid-state imaging element becomes obliquely incident light, which deteriorates the sensitivity characteristics of the solid-state imaging element, and the deterioration of sensitivity shading is likely to become significant. Patent Document 1 discloses a technique for improving the sensitivity characteristics of a solid-state imaging element and reducing color mixing by providing a partition wall with a refractive index lower than that of a color filter and forming a color filter in the opening of the partition wall. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2019 / 064993 Summary of the Invention [Problem to be solved by the invention]

[0005] According to the studies of the present inventors, in order to further improve the sensitivity characteristics of a solid-state imaging device, it is effective to increase the refractive index of the color filters. In view of the above circumstances, the present invention focuses on the dispersion resin used to disperse pigments, and provides a dispersion resin with an increased refractive index, a coloring composition for color filters and a color filter having a high refractive index, and a solid-state imaging element with improved sensitivity characteristics. [Means for solving the problem]

[0006] According to one aspect of the present invention, there is provided a dispersing resin to be mixed with a pigment. The dispersing resin has a first portion having affinity with the pigment and a second portion that functions to prevent aggregation of the pigment particles. The dispersing resin has a refractive index of 1.54 or more at a wavelength of 594 nm.

[0007] According to this aspect, the refractive index of the color filter can be increased, thereby improving the sensitivity characteristics of the solid-state imaging device. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a perspective view showing a camera module. [Diagram 2] FIG. 2 is a vertical cross-sectional view showing the configuration of the camera body. [Diagram 3] FIG. 3 is an enlarged view of a portion of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, the dispersion resin, the coloring composition for color filters, the color filter, and the solid-state imaging device of the present invention will be described in detail based on preferred embodiments shown in the drawings. It should be noted that the following description is merely illustrative of the present invention and is not intended to limit the scope of the present invention. It goes without saying that other embodiments may also fall within the scope of the present invention as long as they conform to the spirit of the present invention. For example, in the present invention, a "step" does not only mean a step that can be distinguished from others, but also a step that is combined with other operations, a step that is actually distributed among a plurality of steps, a step that contains other process elements, and a step in which the operations of a plurality of steps can be combined and carried out in one step may all fall within the scope of the present invention as long as they are in accordance with the spirit of the invention. The terms used in this specification are defined below. The refractive index is a value measured by forming a film with a thickness of 1 μm. A graft copolymer is a polymer with a structure in which a side polymer chain is bonded to a main chain. A dispersing resin is a dispersant for a polymer.

[0010] <Camera module and solid-state image sensor> Fig. 1 is a perspective view showing a camera module. Fig. 2 is a vertical cross-sectional view showing the configuration of a camera body. Fig. 3 is an enlarged view of a part of Fig. 2. In the following description, the upper side in Figs. 2 and 3 will also be referred to as "top" or "upper", and the lower side will also be referred to as "bottom" or "lower". 1 includes a camera body 1 having a solid-state imaging element, a connector C, and a flexible wiring board B that electrically connects the camera body 1 and the connector C. Note that a rigid wiring board may be used instead of the flexible wiring board B.

[0011] As shown in FIG. 2, the camera body 1 has a solid-state imaging element 2 and an optical system 3 joined to the upper side of the solid-state imaging element 2 via a joint 4. The solid-state imaging element 2 includes a light-receiving substrate 21, a bonding substrate 22 formed so as to be in close contact with the lower side of the light-receiving substrate 21, and a cover substrate 23 bonded to the upper side of the light-receiving substrate 21 via a spacer 24. Here, for example, a silicon substrate is used for the bonding substrate 22. A logic circuit substrate may be formed (laminated) on the silicon substrate. The logic circuit substrate formed as the bonding substrate 22 may be a multi-layer laminate substrate further including a DRAM (Dynamic Random Access Memory) substrate or the like. The light-receiving substrate 21 will be described in detail later.

[0012] The bonding substrate 22 has a substrate 221, a wiring layer (not shown) formed on the surface and / or inside the substrate 221, a plurality of vias (conductive portions) 222 provided through the substrate 221, and connection terminals 223 provided corresponding to and electrically connected to each of the vias 222. The substrate 221 is made of, for example, an insulating material such as a hard resin material or a ceramic material, etc. The vias 222 and the connection terminals 223 are each made of, for example, a conductive material.

[0013] The spacer 24 is made of various adhesive materials, and spacer particles can be mixed in as necessary. The spacer 24 can also be made of a frame formed of a metal material, a ceramic material, or the like. The cover substrate 23 is made of a material having optical transparency, such as a glass material (including quartz) or a resin material.

[0014] The optical system 3 includes a housing 31 having an opening 311 formed therein, a first convex lens 32 and a second convex lens 33 arranged within the housing 31, and an infrared cut filter 34 joined to the underside of the housing 31 via a joint 35. The joint 35 and the joint 4 can each be made of, for example, an acrylic resin adhesive, an epoxy resin adhesive, a vinyl chloride resin adhesive, or the like.

[0015] In order to ensure light shielding properties inside the camera body 1, the housing 31 is made of a material that is black or dark in color, or a material that has light shielding properties. Both the first convex lens 32 and the second convex lens 33 have a convex curved surface that protrudes downward. As shown in Fig. 2, incident light that has passed through the opening 311 of the housing 31 is diffused when passing through the first convex lens 32 and the second convex lens 33, and enters the solid-state imaging element 2.

[0016] 3, the light-receiving substrate 21 includes a substrate 211, a plurality of photodiodes (photoelectric conversion elements) 212, an insulating film 213, partition walls 216, a color filter 215, and a microlens 217. In addition, in order to prevent the drawing from becoming difficult to see, hatching indicating a cross section is omitted in FIG. The light that has passed through the microlens 217 and the color filter 215 is incident on and received by the photodiode 212. That is, the solid-state imaging element 2 includes the color filter 215 and a plurality of photodiodes 212 that receive the light that has passed through the color filter 215.

[0017] The substrate (base) 211 can be composed of, for example, a silicon substrate, an InGaAs substrate, etc. In addition, a base layer may be formed on the surface of the substrate 211 for the purposes of improving adhesion, preventing diffusion of substances, improving flatness, etc. The substrate 211 may be integrally formed with the substrate 221 of the bonded substrate 22 by, for example, plasma bonding. In this case, the solid-state imaging element 2 is also called a back-illuminated solid-state imaging element.

[0018] A plurality of photodiodes 212 are provided on the upper surface (one surface) of the substrate 211. The plurality of photodiodes 212 may be formed integrally with the substrate 211, or may be disposed (mounted) on the upper surface of the substrate 211. The photodiode 212 can be composed of, for example, a silicon photodiode, an InGaAs photodiode, a monolayer of an organic or inorganic photoelectric conversion layer and a laminate including an organic or inorganic photoelectric conversion layer, a monolayer of a photoelectric conversion layer including quantum dots and a laminate including a photoelectric conversion layer containing quantum dots, etc.

[0019] Here, in the lower left part of FIG. 2, an enlarged plan view of a portion of the light-receiving substrate 21 enclosed by a dotted line is shown. In this specification, in a plan view of the light-receiving substrate 21, a region including a photodiode 212 and the center of a partition wall 216 formed between adjacent photodiodes 212 is defined as a "unit pixel 210." The size of the photodiode 212 in a plan view is not particularly limited, but is preferably about 0.8 μm square, and can be changed to a larger or smaller size as necessary.

[0020] An insulating film 213 is provided on the multiple photodiodes 212 . The insulating film 213 can be composed of, for example, a silicon oxide film, a silicon oxynitride film, a silicon oxynitride film, a hafnium oxide film, an aluminum oxide film, a zirconium oxide film, a tantalum oxide film, a titanium oxide (TiO2) film, or the like. A partition wall 216 is provided on the insulating film 213 (that is, on the upper surface side of the substrate 211). The partition wall 216 stands on the upper surface of the insulating film 213 along the gaps so as to separate the multiple photodiodes 212.

[0021] A color filter 215 is provided so as to fill the space defined by the partition walls 216 and to cover the upper surface of the partition walls 216 (the surface opposite to the substrate 211). The color filter 215 has a red filter unit 215R, a green filter unit 215G, and a blue filter unit 215B provided corresponding to the multiple photodiodes 212, respectively. Each of the filter units 215R, 215G, and 215B is formed of a coloring composition for color filters, which will be described later. That is, the color filter 215 includes a plurality of filter units 215R, 215G, and 215B that are filled in spaces partitioned by at least the partition walls 216 and are made of a coloring composition for color filters.

[0022] It is preferable that the red filter unit 215R has a high transmittance for light with wavelengths of approximately 580 nm or more, and a transmittance as low as possible for light with other wavelengths. It is preferable that the green filter unit 215G has a high transmittance for light having a wavelength of about 480 nm or more and 600 nm or more, and has a transmittance as low as possible for light having other wavelengths. It is preferable that blue filter unit 215B has a high transmittance for light with a wavelength of approximately 400 nm or more and 500 nm or less, and has a transmittance as low as possible for light with other wavelengths.

[0023] In addition to the red filter unit 215R, the green filter unit 215G, and the blue filter unit 215B, the color filter 215 may have a yellow filter unit, a cyan filter unit, a magenta filter unit, a clear filter unit that is substantially transparent to visible light, a neutral density filter unit whose spectral transmittance of visible light is approximately constant (flat), a near-infrared absorbing filter unit, a near-infrared transmitting filter unit, and the like.

[0024] A microlens 217 is provided on the color filter 215 (the side opposite to the substrate 211). The microlens 217 has a plurality of convex curved surfaces 2171 that protrude upward (the side opposite to the color filter 215). The microlens 217 can be made of, for example, a styrene-acrylic copolymer resin, silicon nitride, or the like. An anti-reflection layer may be additionally provided between the microlens 217 and the color filter 215 .

[0025] Thickness of red filter unit 215R (thickest part) T R is the thickness (thickest part) of the green filter unit 215G. G and the thickness (thickest part) of the blue filter unit 215B, T B Generally, the thickness T of the red filter unit 215R is preferably equal to or smaller than the thickness T of the red filter unit 215R. R is the thickness T of the green filter unit 215G G and the thickness T of the blue filter unit 215B B It is difficult to make it thinner, but this can be achieved by using the red composition described below. According to this configuration, the color filter 215 can be made thinner, and the height of the light receiving substrate 21 (solid-state imaging element 2) can be reduced, thereby improving the sensitivity characteristics.

[0026] Thickness T of red filter unit 215R R , thickness T of green filter unit 215G G and the thickness T of the blue filter unit 215B B The maximum value is preferably 0.55 μm or less, more preferably 0.5 μm or less, and further preferably 0.45 μm or less. The light receiving substrate 21 (solid-state imaging element 2) provided with such a thin color filter 215 can be made sufficiently low-profile. The lower limit of the maximum value is not particularly limited, but is preferably 0.2 μm or more, more preferably 0.25 μm or more, and even more preferably 0.3 μm or more. This allows the color filter 215 to exhibit necessary and sufficient spectral characteristics. As a result, the solid-state imaging element 2 can obtain high-quality images.

[0027] In particular, the thickness T R The red filter unit 215R having a diameter of 0.55 μm preferably has a transmittance of 80% or more for light with a wavelength of 620 nm, a transmittance of 10% or less for light with a wavelength of 530 nm, and a refractive index of 1.8 or more for light with a wavelength of 650 nm. Such a red filter unit 215R exhibits excellent light-collecting characteristics, and can further improve the sensitivity characteristics of the solid-state imaging element 2. The transmittance of the red filter unit 215R for light with a wavelength of 620 nm is more preferably 85% or more, and even more preferably 90% or more. The transmittance of the red filter unit 215R for light with a wavelength of 530 nm is more preferably 8% or less, and even more preferably 6% or less. The refractive index of the red filter unit 215R with respect to light with a wavelength of 650 nm is more preferably 1.85 or more, and even more preferably 1.9 or more.

[0028] The refractive index of the red filter unit 215R for light with a wavelength of 650 nm is n R The refractive index of the green filter unit 215G for light with a wavelength of 550 nm is n GThe refractive index of the blue filter unit 215B for light with a wavelength of 450 nm is n B Then, n R > n G ≧ n B It is preferable to set the angle so as to satisfy the following relationship. This allows the red light, which is focused at a smaller angle by the microlens 217, to be refracted (focused) at a larger angle when entering the red filter unit 215R. This allows more light to reach the photodiode 212. As a result, better sensitivity characteristics can be obtained at the end of the light-receiving substrate 21.

[0029] When the refractive indexes of filter units 215R, 215G, and 215B are set to satisfy the above relationship, the composition of the colored resin composition for forming filter units 215R, 215G, and 215B may be adjusted by selecting, for example, one of the type and amount of colorant (pigment) to be used, the type and amount of colorant binder, the type and amount of dispersion resin, and the like. Refractive index n R The specific value of is not particularly limited, but is preferably 1.7 or more, more preferably 1.75 or more, and even more preferably 1.8 or more. Refractive index n G The specific value of is not particularly limited, but is preferably 1.6 or more, more preferably 1.63 or more, and even more preferably 1.7 or more. Also, the refractive index n B The specific value of is not particularly limited, but is preferably 1.6 or more, more preferably 1.63 or more, and even more preferably 1.64 or more.

[0030] The partition 216 is entirely made of the refractive index n R , the refractive index n of the green filter unit 215G G and the refractive index n of the blue filter unit 215B B It is composed of a low refractive index portion having a lower refractive index. According to this configuration, due to the total reflection of light (prevention of light transmission), the light that passes through the filter units 215R, 215G, and 215B is reflected by the partition 216 and guided to the photodiode 212, thereby further improving the sensitivity characteristics of the light receiving substrate 21 (solid-state imaging element 2). The critical angle can be made smaller by increasing the difference between the refractive index of filter units 215R, 215G, and 215B and the refractive index of partition wall 216. Therefore, the sensitivity characteristic of light-receiving substrate 21 is more likely to be improved.

[0031] In addition, the refractive index of each filter unit (n R , n G , n B The difference between the refractive index of the partition wall 216 and the refractive index of the thin film 214 is preferably 0.01 or more, more preferably 0.1 or more, and even more preferably 0.2 or more. In this case, the critical angle can be made smaller, and the total reflection characteristic of the partition wall 216 can be improved. Although the specific value of the refractive index of the partition 216 is not particularly limited, the refractive index for light with a wavelength of 450 nm is preferably 1.44 or less, more preferably 1.42 or less, and even more preferably 1.4 or less.

[0032] 3, the width W of the partition 216 is preferably 50 nm to 300 nm, more preferably 50 nm to 280 nm, and further preferably 50 nm to 260 nm. In this case, it is possible to prevent or suppress deterioration of the total reflection of light, and to ensure a good pixel size (size of the photodiode 212) while maintaining the mechanical strength of the partition 216. As shown in FIG. 3, the height (thickness) H of the partition wall 216 is smaller than the thickness (T R , T G , T B) and is preferably 0.52 μm or less. In this way, the partition walls 216 are formed thinner than the color filters 215 and the upper surfaces of the partition walls 216 are covered by the color filters 215, whereby it is possible to suppress white light mixing through the partition walls 216 and also to make the light-receiving substrate 21 sufficiently low in height.

[0033] The partition walls 216 are preferably made of a composition containing a resin material and inorganic particles. The resin material may be at least one selected from, for example, siloxane resin, fluorine-based resin, and the like. The inorganic particles include, for example, at least one type selected from SiO particles, SiOC particles, hollow silica particles, metal fillers, carbon particles (e.g., carbon black), and the like. Among these, from the viewpoint of increasing the strength of the partition wall 216, silica particles are preferably used as the inorganic particles. Among these, hollow silica particles are particularly preferably used as the inorganic particles because they can increase the strength of the partition wall 216 and reduce the refractive index.

[0034] The thickness of the color filter 215 may be set to be approximately equal to or slightly smaller than the height of the partition wall 216. In this case, the light receiving substrate 21 (solid-state imaging element 2) can be made thinner (reduced in height). The color filter 215 is formed (configured) using the coloring composition for color filters of the present invention (hereinafter, also abbreviated as "coloring composition"). The coloring composition contains at least a pigment and a dispersing resin (the dispersing resin of the present invention).

[0035] <<Pigments>> It is preferable that the pigment has a particle size as small as possible. In consideration of dispersibility in the coloring composition and handling of the pigment, the average particle size of the pigment is preferably 0.001 μm or more and 0.1 μm or less, and more preferably 0.005 μm or more and 0.05 μm or less. It is preferable that the pigment contains particles having a particle size in the range of 0.01±0.005 μm in an amount of 75% by mass or more based on the total mass of the pigment. Here, the average particle size refers to the particle size (D50) at which the volume ratio of particles is 50% when the volume ratio of particles is accumulated from the smallest particle size in the volume particle size distribution. The average particle size can be measured by a general particle size distribution meter, for example, a dynamic light scattering type particle size distribution meter.

[0036] As the pigment, an inorganic pigment or an organic pigment can be used. Examples of inorganic pigments include metal compounds such as metal oxides and metal complex salts, etc. Specific examples thereof include metal oxides containing metals such as aluminum, iron, cobalt, cadmium, lead, copper, titanium, magnesium, chromium, zinc, and antimony, and composite oxides containing the above metals. On the other hand, organic pigments are, for example, color index (hereinafter referred to as "CI") Pigment Yellow 11, 24, 31, 53, 83, 93, 99, 108, 109, 110, 138, 139, 147, 150, 151, 154, 155, 167, 180, 185, 199; CI Pigment Orange 36, 38, 43, 71; CI Pigment Red 81, 105, 122, 149, 150, 155, 171, 175, 176, 177, 209, 220, 224, 242, 254, 255, 264, 270; CI Pigment Violet 19, 23, 32, 39; CI Pigment Blue 1, 2, 15, 15:1, 15:3, 15:6, 16, 22, 60, 66; CI Pigment Green 7, 36, 37, 58, 59, 62, 63; CI Pigment Brown 25, 28, etc.

[0037] The organic pigments may be used alone, or in order to increase color purity, two or more kinds of them may be used in combination. Specifically, as the red pigment, an anthraquinone-based pigment, a perylene-based pigment, or a diketopyrrolopyrrole-based pigment can be used alone, or at least one of these can be used in combination with a disazo-based yellow pigment, an isoindoline-based yellow pigment, a quinophthalone-based yellow pigment, a perylene-based red pigment, or the like. For example, an anthraquinone pigment may be CI Pigment Red 177, a perylene pigment may be CI Pigment Red 155 or CI Pigment Red 224, and a diketopyrrolopyrrole pigment may be CI Pigment Red 254.

[0038] From the viewpoint of color reproducibility, it is preferable to use a red pigment in combination with a yellow pigment such as CI Pigment Yellow 138 or CI Pigment Yellow 139. In this case, the mass ratio of the red pigment to the yellow pigment is preferably 100:5 or more and 100:50 or less, and more preferably 100:10 or more and 100:30 or less. If the mass ratio is within the above range, the light transmittance of the red filter unit 215R can be suppressed and the color purity can be improved. When different kinds of red pigments are used in combination, the mass ratio thereof can be adjusted according to the chromaticity.

[0039] As the green pigment, a halogenated phthalocyanine pigment can be used alone or in combination with a disazo yellow pigment, a quinophthalone yellow pigment, an azomethine yellow pigment or an isoindoline yellow pigment. As the green pigment, for example, CI Pigment Green 7, 36, 37, 58, 59, 62, 63, etc. are preferable. In addition, it is preferable to use these green pigments in combination with a yellow pigment, for example, CI Pigment Yellow 83, CI Pigment Yellow 138, CI Pigment Yellow 139, CI Pigment Yellow 150, CI Pigment Yellow 180, or CI Pigment Yellow 185. In this case, the mass ratio of the green pigment to the yellow pigment is preferably 100:5 or more and 100:150 or less, and more preferably 100:30 or more and 100:120 or less. If the mass ratio is in the above range, the transmittance of light with a wavelength of 400 nm or more and 450 nm or less in the green filter unit 215G can be suppressed, and the color purity can be improved.

[0040] As the blue pigment, a phthalocyanine pigment can be used alone or in combination with a dioxazine purple pigment. As the blue pigment, for example, it is preferable to use CI Pigment Blue 15:6 and CI Pigment Violet 23 in combination. In this case, the mass ratio of the blue pigment to the purple pigment is preferably 100:0 or more and 100:30 or less, and more preferably 100:0 or more and 100:10 or less.

[0041] It is preferable that the pigment is subjected to a micronizing treatment and then mixed with other raw materials. Examples of the method for the pulverization treatment include wet grinding, dry grinding, and solution deposition. Among these, the method of the micronization is preferably salt milling using a kneader method, which is a type of wet grinding. The salt milling treatment is a treatment in which a mixture of a pigment, a water-soluble inorganic salt, and a water-soluble organic solvent is mechanically kneaded while being heated using a kneader, and then the water-soluble inorganic salt and the water-soluble organic solvent are removed by washing with water.

[0042] As the kneading machine, for example, a batch type or continuous type kneading machine such as a kneader, a two-roll mill, a three-roll mill, a ball mill, an attritor, a sand mill, or a planetary type mixer can be suitably used. The water-soluble inorganic salt is a compound that acts as a grinding aid, and the high hardness of the inorganic salt is utilized to grind the pigment during salt milling. By optimizing the conditions for salt milling the pigment, it is possible to obtain a pigment having a very fine primary particle size, a narrow distribution width, and a sharp particle size distribution.

[0043] Examples of the water-soluble inorganic salt include sodium chloride, barium chloride, potassium chloride, sodium sulfate, etc. Among these, the water-soluble inorganic salt is preferably sodium chloride (table salt) because it is inexpensively available. From the viewpoints of both treatment efficiency and production efficiency, the amount of the water-soluble inorganic salt used is preferably from 50 parts by mass to 2,000 parts by mass, and more preferably from 300 parts by mass to 1,000 parts by mass, per 100 parts by mass of the pigment.

[0044] The water-soluble organic solvent wets the pigment and the water-soluble inorganic salt. As the water-soluble organic solvent, a compound that dissolves (is miscible) in water but does not substantially dissolve water-soluble inorganic salts is preferably used. The water-soluble organic solvent is preferably a high-boiling solvent having a boiling point of 120° C. or higher, from the viewpoint of being less likely to volatilize due to the temperature rise during salt milling.

[0045] Examples of the water-soluble organic solvent include 2-methoxyethanol, 2-butoxyethanol, 2-(isopentyloxy)ethanol, 2-(hexyloxy)ethanol, diethylene glycol, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, triethylene glycol, triethylene glycol monomethyl ether, liquid polyethylene glycol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, dipropylene glycol, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, and liquid polypropylene glycol. The amount of the water-soluble organic solvent used is preferably 5 parts by mass or more and 1,000 parts by mass or less, and more preferably 50 parts by mass or more and 500 parts by mass or less, relative to 100 parts by mass of the pigment.

[0046] When the pigment is subjected to the salt milling treatment, a resin may be added, if necessary. The type of resin is not particularly limited, and natural resins, modified natural resins, synthetic resins, synthetic resins modified with natural resins, etc. can be used. The resin is preferably solid at room temperature and insoluble in water, and more preferably partially soluble in the above organic solvents. The amount of the resin used is preferably 5 parts by mass or more and 200 parts by mass or less with respect to 100 parts by mass of the pigment.

[0047] Furthermore, by finely dispersing the above pigment in, for example, an acrylic resin, a maleic acid resin, a vinyl chloride-vinyl acetate copolymer, an ethyl cellulose resin, or the like to produce a powdered processed pigment, a coloring composition having good dispersibility and dispersion stability can be obtained. The coloring composition can be suitably used in the form of a powder, a paste, a pellet, a paste, or the like.

[0048] <<Dispersion resin>> The dispersing resin is mixed with the pigment as described above for use. This dispersing resin has a first portion and a second portion, and the first portion has a higher affinity for the pigment than the second portion. For this reason, the dispersion resin is coordinated to the pigment particles so that the first site is on the pigment particle side and the second site is on the opposite side (solvent side) to the pigment particles, whereby the second site acts as a steric repulsion site, preventing the pigment particles from aggregating together, thereby making it possible to obtain a coloring composition with excellent dispersion stability. That is, the dispersing resin has a first portion that has affinity for the pigment, and a second portion that functions to prevent aggregation of the pigment particles.

[0049] The dispersion resin has a refractive index of 1.54 or more at a wavelength of 594 nm. By using a dispersion resin having such a high refractive index, a color filter 215 (especially the red filter unit 215R) having a high refractive index can be formed. Therefore, even if the solid-state imaging element is made thin (low profile), it is possible to obtain a solid-state imaging element having excellent sensitivity characteristics. The refractive index of the dispersion resin at a wavelength of 594 nm may be 1.54 or more, but is preferably 1.54 to 1.65, and more preferably 1.55 to 1.63. In this case, the above-mentioned effects can be further improved. Note that a dispersion resin having a refractive index exceeding the upper limit may reduce the dispersibility of the pigment.

[0050] The refractive index of the dispersing resin can be adjusted by appropriately designing the molecular structure of the dispersing resin. According to the studies of the present inventors, the refractive index of a dispersing resin containing an aromatic ring in particular tends to be high. Here, the aromatic ring includes an aromatic aliphatic ring and an aromatic heterocycle, which may be monocyclic or polycyclic. The polycyclic aromatic ring may be a bonded type in which a plurality of aromatic rings are bonded (e.g., a biphenyl ring, etc.) or a condensed type in which a plurality of aromatic rings are condensed (e.g., a naphthalene ring, etc.). The proportion of aromatic rings in the total mass of the dispersion resin is preferably 25% by mass or more, more preferably 30% by mass or more and 80% by mass or less, and even more preferably 35% by mass or more and 75% by mass or less. By including aromatic rings in such a proportion, the refractive index of the dispersion resin can be set within the above range. Note that increasing the proportion of aromatic rings beyond the above upper limit value is a trade-off with the dispersibility of the pigment.

[0051] The dispersing resin may contain aromatic rings only in the first portion, only in the second portion, or both in the first portion and the second portion. However, it is preferable that the dispersing resin mainly contains aromatic rings in the second portion. This makes it possible to sufficiently increase the refractive index of the dispersing resin while preventing or suppressing a decrease in the affinity of the dispersing resin for the pigment. In addition, the function of preventing aggregation between pigment particles tends to be improved. The dispersing resin preferably has a weight average molecular weight of 5,000 to 50,000, more preferably 6,000 to 40,000, and even more preferably 7,000 to 25,000. A dispersing resin having such a weight average molecular weight can highly effectively prevent aggregation of pigment particles. The weight average molecular weight is a value calculated as polystyrene equivalent, measured by gel permeation chromatography (GPC).

[0052] Examples of the dispersing resin include a graft copolymer (hereinafter also referred to as a "graft copolymer") in which the second portion branches out and extends from the first portion, a block copolymer (hereinafter also referred to as a "block copolymer") in which the first portion and the second portion are bonded at their ends, and a random copolymer in which the first portion and the second portion are bonded randomly. Among these, the dispersing resin is preferably a graft copolymer or a block copolymer. A dispersing resin with such a molecular structure exhibits a good balance between the affinity with the pigment due to the first portion and the action of the second portion as a steric repulsion portion.

[0053] Graft copolymer The graft copolymer preferably has an acidic group (e.g., a carboxyl group, a phosphoric acid group, a sulfonic acid group) at the first site, and more preferably contains an aromatic ring to which a total of three or more carboxyl groups or carboxyl group residues are directly bonded at the first site. In this case, the first site of the graft copolymer has an acidic group (particularly a carboxyl group) that has the properties of a strong acid, and therefore can exhibit extremely high affinity for pigment particles whose surface exhibits basic properties. Such a graft copolymer can also be called an acidic dispersion resin. In addition, a part or the whole of such aromatic ring may be replaced with another aromatic ring to which two carboxyl group residues are directly bonded. Examples of such another aromatic ring include a naphthalene type aromatic ring, a bisphenol A type aromatic ring, and a biphenyl type aromatic ring.

[0054] The graft copolymer is preferably a polyester in which the constituent units of the first moiety are linked by ester bonds. The first moiety containing an ester bond is formed by a reaction between a compound (monomer) having a carboxyl group (or an acid anhydride group) and a compound (monomer) having a hydroxyl group. This reaction is preferable because it can be relatively easily caused and the compounds used in the reaction are relatively easily available. The second part of the graft copolymer is not particularly limited in its molecular structure as long as it can act as a steric repulsion part, but is preferably a polymer part of a monomer having an ethylenically unsaturated bond. The chain length (weight average molecular weight) of such a polymer part can be adjusted relatively easily. In addition, there is also an advantage that a substituent (side chain) according to the purpose, such as polymerizability (e.g., photopolymerizability, etc.) or alkali solubility, can be easily introduced into the polymer part. As the monomer having an ethylenically unsaturated bond (hereinafter also referred to as "unsaturated monomer"), a monomer having a group containing a double bond, a monomer having a (meth)acryloyl group, etc. are preferably used.

[0055] In this specification, unless otherwise specified, when "(meth)acryloyl", "(meth)acryl", "(meth)acrylic acid", "(meth)acrylate", or "(meth)acrylamide" is used, it means "acryloyl and / or methacryloyl", "acrylic and / or methacrylic", "acrylic acid and / or methacrylic acid", "acrylate and / or methacrylate", or "acrylamide and / or methacrylamide", respectively.

[0056] Such a graft copolymer can be prepared, for example, by (I) reacting at least one acid anhydride selected from the group consisting of tetracarboxylic acid anhydrides and tricarboxylic acid anhydrides with a vinyl polymer having a hydroxyl group near the end, which is synthesized separately, or by (II) reacting the acid anhydride with a hydroxyl group-containing thiol, followed by a polymerization reaction initiated by the thiol group of the thiol to form a vinyl polymer moiety. In other words, the graft copolymer is a resin (polymer) composed of a polyester portion (first portion) having a carboxyl group and a vinyl polymer portion (second portion).

[0057] Examples of the tetracarboxylic dianhydride include aliphatic tetracarboxylic dianhydrides and aromatic tetracarboxylic dianhydrides. Specific examples of the aliphatic tetracarboxylic dianhydride include 1,2,3,4-butane tetracarboxylic dianhydride, 1,2,3,4-cyclobutane tetracarboxylic dianhydride, 1,3-dimethyl-1,2,3,4-cyclobutane tetracarboxylic dianhydride, 1,2,3,4-cyclopentane tetracarboxylic dianhydride, 2,3,5-tricarboxycyclopentylacetic dianhydride, 3,5,6-tricarboxynorbornane-2-acetic dianhydride, 2,3,4,5-tetrahydrofuran tetracarboxylic dianhydride, 5-(2,5-dioxotetrahydrofural)-3-methyl-3-cyclohexene-1,2-dicarboxylic dianhydride, and bicyclo[2,2,2]-oct-7-ene-2,3,5,6-tetracarboxylic dianhydride.

[0058] Specific examples of the aromatic tetracarboxylic dianhydride include pyromellitic dianhydride, ethylene glycol ditrimellitic anhydride, propylene glycol ditrimellitic anhydride, butylene glycol ditrimellitic anhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-biphenylsulfone tetracarboxylic dianhydride, 1,4,5,8-naphthalene tetracarboxylic dianhydride, 2,3,6,7-naphthalene tetracarboxylic dianhydride, and the like. tetracarboxylic dianhydride, 3,3',4,4'-biphenyl ether tetracarboxylic dianhydride, 3,3',4,4'-dimethyldiphenylsilane tetracarboxylic dianhydride, 3,3',4,4'-tetraphenylsilane tetracarboxylic dianhydride, 1,2,3,4-furan tetracarboxylic dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenyl sulfide dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenyl sulfone dianhydride Anhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenylpropane dianhydride, 3,3',4,4'-perfluoroisopropylidenediphthalic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, bis(phthalic acid)phenylphosphine oxide dianhydride, p-phenylene-bis(triphenylphthalic acid) dianhydride, m-phenylene-bis(triphenylphthalic acid) dianhydride, bis(triphenylphthalic acid)-4,4'-diphenyl dianhydride, bis(triphenylphthalic)-4,4'-diphenylmethane dianhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, 9,9-bis[4-(3,4-dicarboxyphenoxy)phenyl]fluorene dianhydride, 3,4-dicarboxy-1,2,3,4-tetrahydro-1-naphthalene succinic dianhydride, and 3,4-dicarboxy-1,2,3,4-tetrahydro-6-methyl-1-naphthalene succinic dianhydride.

[0059] Examples of the aromatic tetracarboxylic dianhydride include compounds represented by the following general formula (1) or (2).

[0060] General formula (1): [ka] [In general formula (1), k is 1 or 2.]

[0061] General formula (2): [ka] [In general formula (2), Q1 is a direct bond, -O-, -CO-, -COOCH2CH2OCO-, -SO2-, -C(CF3)2-, a group represented by the following general formula (3), or a group represented by the following general formula (4)]

[0062] General formula (3): [ka]

[0063] General formula (4): [ka]

[0064] Among these, as the tetracarboxylic dianhydride, from the viewpoint of excellent adsorption to the pigment, aromatic tetracarboxylic dianhydrides are preferable, and tetracarboxylic dianhydrides having two or more aromatic rings are more preferable. The aromatic tetracarboxylic dianhydride may be used in combination with an aliphatic tetracarboxylic dianhydride.

[0065] Examples of tricarboxylic acid anhydrides include benzenetricarboxylic acid anhydride (1,2,3-benzenetricarboxylic acid anhydride, trimellitic acid anhydride [1,2,4-benzenetricarboxylic acid anhydride], etc.), naphthalene tricarboxylic acid anhydride (1,2,4-naphthalene tricarboxylic acid anhydride, 1,4,5-naphthalene tricarboxylic acid anhydride, 2,3,6-naphthalene tricarboxylic acid anhydride, 1,2,8-naphthalene tricarboxylic acid anhydride, etc.), 3,4,4'-benzophenone tricarboxylic acid anhydride, 3,4,4'-biphenyl ether tricarboxylic acid anhydride, 3,4,4'-biphenyl tricarboxylic acid anhydride, 2,3,2'-biphenyl tricarboxylic acid anhydride, 3,4,4'-biphenyl methane tricarboxylic acid anhydride, and 3,4,4'-biphenyl sulfone tricarboxylic acid anhydride. Among these, trimellitic anhydride is preferred as the tricarboxylic acid anhydride.

[0066] In the present invention, the unsaturated monomer preferably used is an unsaturated monomer having an aromatic ring. Examples of the unsaturated monomer having an aromatic ring include (meth)acrylates such as benzyl (meth)acrylate, phenylene (meth)acrylate, phenoxyethyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, and 3-methyl-3-oxetanyl (meth)acrylate; phenoxyethyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, phenoxytetraethylene glycol (meth)acrylate, phenoxyhexaethylene glycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, and paracumylphenoxy. Examples of the polyalkylene glycol (meth)acrylates include (poly)alkylene glycol (meth)acrylates such as ethyl (meth)acrylate, para-cumylphenoxyethylene glycol (meth)acrylate, para-cumylphenoxypolyethylene glycol (meth)acrylate, nonylphenoxypolyethylene glycol (meth)acrylate, nonylphenoxypolypropylene glycol (meth)acrylate, and nonylphenoxypoly(ethylene glycol-propylene glycol) (meth)acrylate; styrenes such as styrene and α-methylstyrene (vinyl toluene); and carbazoles such as vinyl carbazole.

[0067] As the unsaturated monomer, in addition to the unsaturated monomer having an aromatic ring, other unsaturated monomers can also be used. Examples of other unsaturated monomers include linear or branched alkyl (meth)acrylates; cyclic alkyl (meth)acrylates; (meth)acrylates having a hydroxyl group; (poly)alkylene glycol monoalkyl ether (meth)acrylates; (meth)acrylates having an alkyloxysilyl group; fluoroalkyl (meth)acrylates; (meth)acryloxy-modified polydimethylsiloxanes (silicone macromers); vinyl ethers; and vinyl fatty acids.

[0068] Examples of linear or branched alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth), tertiary butyl (meth)acrylate, isoamyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cetyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, isomyristyl (meth)acrylate, stearyl (meth)acrylate, and isostearyl (meth)acrylate.

[0069] Examples of the cyclic alkyl (meth)acrylate include cyclohexyl (meth)acrylate, tertiary butyl cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and isobornyl (meth)acrylate. Examples of (meth)acrylates having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxypropyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 5-hydroxy-3-methylpentyl (meth)acrylate, neopentyl glycol mono(meth)acrylate, and cyclohexanediol mono(meth)acrylate.

[0070] Examples of (poly)alkylene glycol monoalkyl ether (meth)acrylates include 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-methoxypropyl (meth)acrylate, diethylene glycol monomethyl ether (meth)acrylate, diethylene glycol monoethyl ether (meth)acrylate, diethylene glycol mono-2-ethylhexyl ether (meth)acrylate, dipropylene glycol monomethyl ether (meth)acrylate, triethylene glycol monomethyl ether (meth)acrylate, triethylene glycol monoethyl ether (meth)acrylate, tripropylene glycol monomethyl ether (meth)acrylate, tetraethylene glycol monomethyl ether (meth)acrylate, polyethylene glycol monomethyl ether (meth)acrylate, polypropylene glycol monomethyl ether (meth)acrylate, polyethylene glycol monolauryl ether (meth)acrylate, polyethylene glycol monostearyl ether (meth)acrylate, and octoxypolyethylene glycol-polypropylene glycol (meth)acrylate.

[0071] Examples of (meth)acrylates having an alkyloxysilyl group include 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, and 3-acryloxypropyltrimethoxysilane. Examples of the fluoroalkyl(meth)acrylate include trifluoroethyl(meth)acrylate, octafluoropentyl(meth)acrylate, perfluorooctylethyl(meth)acrylate, and tetrafluoropropyl(meth)acrylate.

[0072] Examples of vinyl ethers include ethyl vinyl ether, n-propyl vinyl ether, isopropyl vinyl ether, n-butyl vinyl ether, and isobutyl vinyl ether. Examples of the fatty acid vinyl include vinyl acetate and vinyl propionate.

[0073] The hydroxyl-containing thiol is preferably a compound having two hydroxyl groups and one thiol group. Examples of hydroxyl group-containing thiols include 1-mercapto-1,1-methanediol, 1-mercapto-1,1-ethanediol, 3-mercapto-1,2-propanediol (thioglycerol), 2-mercapto-1,2-propanediol, 2-mercapto-2-methyl-1,3-propanediol, 2-mercapto-2-ethyl-1,3-propanediol, 1-mercapto-2,2-propanediol, 2-mercaptoethyl-2-methyl-1,3-propanediol, and 2-mercaptoethyl-2-ethyl-1,3-propanediol.

[0074] The equivalent ratio of the acid anhydride group in the acid anhydride to the hydroxyl group in the hydroxyl group-containing thiol, acid anhydride group / hydroxyl group, is preferably 0.15 to 1.25, more preferably 0.3 to 1. This further improves the dispersion stability of the pigment by the graft copolymer. The weight average molecular weight of the vinyl polymer portion in the graft copolymer is preferably from 1,000 to 20,000, and more preferably from 3,000 to 15,000. When the vinyl polymer portion has an appropriate weight average molecular weight, the dispersion stability of the pigment by the graft copolymer is further improved.

[0075] The proportion of the vinyl polymer portion (second portion) in the total mass of the graft copolymer is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more and 80% by mass or less, which makes it possible to prevent a decrease in the affinity of the graft copolymer for the pigment and to fully exert the steric repulsion provided by the second portion of the graft copolymer. The acid value of the graft copolymer is preferably 5 mgKOH / g or more and 200 mgKOH / g or less, more preferably 10 mgKOH / g or more and 170 mgKOH / g or less, and even more preferably 20 mgKOH / g or more and 150 mgKOH / g or less. When the graft copolymer has an appropriate acid value, the dispersion stability of the pigment by the graft copolymer is further improved.

[0076] Block copolymers The block copolymer preferably has a basic group at the first site, and more preferably contains at least one selected from the group consisting of a tertiary amino group and a quaternary ammonium group at the first site. In this case, the first site of the block copolymer has a tertiary amino group or a quaternary ammonium group that has basic properties, and therefore can exhibit extremely high affinity for pigment particles whose surfaces exhibit acidic properties. Such a block copolymer can also be called a basic dispersion resin. The molecular structure of the first and second parts of the block copolymer is not particularly limited as long as they can act as a part exhibiting affinity with the pigment and a part of steric repulsion, respectively, but it is preferable that both are polymer parts of a monomer (unsaturated monomer) having an ethylenically unsaturated bond. The chain length (weight average molecular weight) of such a polymer part can be adjusted relatively easily. As the unsaturated monomer, a monomer having a group containing a double bond, a monomer having a (meth)acryloyl group, etc. are preferably used.

[0077] Block copolymers are similar to graft copolymers, except that the molecular structure of the first portion is different and the molecular structure is linear overall, i.e., the molecular structure of the second portion is similar in graft copolymers and block copolymers. The block copolymer is preferably an AB block polymer or a BAB block polymer, synthesized by living radical polymerization. For example, an AB block polymer can be produced by first synthesizing A (first portion) and then synthesizing B (second portion). Also, a BAB block polymer can be produced by first synthesizing B (second portion), then synthesizing A (first portion), and then synthesizing B (second portion). It goes without saying that the order of synthesizing A (first portion) and B (second portion) is arbitrary.

[0078] The first portion preferably contains at least one type selected from the group consisting of structural units (repeating units) represented by the following general formulas (5) to (7).

[0079] General formula (5): [ka] [In the general formula (5), R1 to R3 each independently represent a hydrogen atom or a chain or cyclic hydrocarbon group which may have a substituent, and two or more of R1 to R3 may be bonded to each other to form a cyclic structure; R4 represents a hydrogen atom or a methyl group; X represents a divalent linking group; Y - indicates a counter anion.

[0080] General formula (6): [ka] [In the general formula (6), R5 and R6 each independently represent a hydrogen atom or a chain or cyclic hydrocarbon group which may have a substituent, and R5 and R6 may be bonded to each other to form a cyclic structure. R4 represents a hydrogen atom or a methyl group, and X represents a divalent linking group.]

[0081] General formula (7): [ka] [In the general formula (7), R7 is a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, an aryl group having 6 to 20 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, an acyl group, an oxy radical group, or an OR 12R 12 represents a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, an aryl group having 6 to 20 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, or an acyl group; R8, R9, and R 10 , R 11 each independently represents a methyl group, an ethyl group, or a phenyl group; R4 represents a hydrogen atom or a methyl group; and X represents a divalent linking group.

[0082] In general formula (5), R1 to R3 are, for example, preferably an alkyl group having 1 to 4 carbon atoms which may have a substituent, or an aralkyl group having 7 to 16 carbon atoms which may have a substituent, and more preferably a methyl group, an ethyl group, a propyl group, a butyl group, or a benzyl group. In general formula (6), R5 and R6 are preferably, for example, an alkyl group having 1 to 4 carbon atoms which may have a substituent, and more preferably a methyl group, an ethyl group, a propyl group, or a butyl group.

[0083] In R7 of the general formula (7), examples of the alkyl group having 1 to 18 carbon atoms include linear, branched and cyclic alkyl groups, specific examples of which include a methyl group, an ethyl group, a normal propyl group, an isopropyl group, a n-butyl group, a t-butyl group, a n-hexyl group, a cyclohexyl group, a n-octyl group and a hexadecyl group. Examples of the aryl group having 6 to 20 carbon atoms include a phenyl group, a 1-naphthyl group, and a 2-naphthyl group. Examples of aralkyl groups having 7 to 12 carbon atoms include groups in which an alkyl group having 1 to 8 carbon atoms is bonded to an aryl group having 6 to 10 carbon atoms. Specific examples thereof include a benzyl group, a phenethyl group, an α-methylbenzyl group, and a 2-phenylpropan-2-yl group. Examples of the acyl group include an alkanoyl group and an aroyl group having a carbon number of 2 to 8. Specific examples thereof include an acetyl group and a benzoyl group. Among these, R7 in general formula (7) is preferably a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or an oxy radical group, more preferably a hydrogen atom or a methyl group, and even more preferably a methyl group.

[0084] In the general formulas (5) to (7), the divalent linking group X is, for example, a methylene group, an alkylene group having 2 to 10 carbon atoms, an arylene group, -CONH-R 13 -,-COO-R 14 -(However, R 13 and R 14 are each independently a single bond, a methylene group, an alkylene group having 2 to 10 carbon atoms, or an ether group (alkyloxyalkyl group) having 2 to 10 carbon atoms. 14 - is preferred. In addition, in the general formula (5), the counter anion Y - For example, Cl - , Br - , I - , ClO4 - , BF4 - , CH3COO - , PF6 - etc.

[0085] Examples of monomers forming the structural unit represented by general formula (5) include alkyl (meth)acrylate-based quaternary ammonium salts such as (meth)acryloyloxyethyl trimethyl ammonium chloride, (meth)acryloyloxyethyl triethyl ammonium chloride, (meth)acryloyloxyethyl dimethyl benzyl ammonium chloride, and (meth)acryloyloxyethyl methyl morpholino ammonium chloride; alkyl (meth)acryloyl amide-based quaternary ammonium salts such as (meth)acryloyl aminopropyl trimethyl ammonium chloride, (meth)acryloyl aminoethyl triethyl ammonium chloride, and (meth)acryloyl aminoethyl dimethyl benzyl ammonium chloride; dimethyl diallyl ammonium methyl sulfate; and trimethyl vinyl phenyl ammonium chloride.

[0086] Examples of monomers forming the structural unit represented by general formula (6) include (meth)acrylates having a tertiary amino group, such as N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, N,N-dimethylaminopropyl (meth)acrylate, and N,N-diethylaminopropyl (meth)acrylate; and (meth)acrylamides having a tertiary amino group, such as N,N-dimethylaminoethyl (meth)acrylamide, N,N-diethylaminoethyl (meth)acrylamide, N,N-dimethylaminopropyl (meth)acrylamide, and N,N-diethylaminopropyl (meth)acrylamide.

[0087] Examples of the monomer that forms the structural unit represented by general formula (7) include compounds represented by the following structural formulas: In the following structural formulas, R4 represents a hydrogen atom or a methyl group.

[0088] [ka]

[0089] Among the above compounds, the monomer forming the structural unit represented by general formula (7) is preferably 2,2,6,6-tetramethylpiperidyl methacrylate or 1,2,2,6,6-pentamethylpiperidyl methacrylate, and more preferably 1,2,2,6,6-pentamethylpiperidyl methacrylate.

[0090] The structural units represented by the general formulas (5) to (7) may be contained alone or in combination of two or more kinds, and may be contained in any form of random copolymerization, block copolymerization, or graft copolymerization, but are preferably contained in the form of a block copolymer. It may contain structural units other than the structural units represented by the general formulas (5) to (7). For the formation of monomer units other than the structural units represented by the general formulas (5) to (7) in the first portion of the block copolymer, and for the synthesis of the second portion, monomers that can be used in the synthesis of the vinyl polymer portion can be used.

[0091] The radical polymerization initiator used in producing a block copolymer by living radical polymerization is preferably, for example, an azo compound or a peroxide. Examples of azo compounds include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(methyl isobutyrate), 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethyl-4-methoxyvaleronitrile), dimethyl 2,2'-azobis(2-methylpropionate), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-hydroxymethylpropionitrile), and 2,2'-azobis[2-(2-imidazolin-2-yl)propane].

[0092] Examples of peroxides include benzoyl peroxide, t-butyl perbenzoate, cumene hydroperoxide, diisopropyl peroxydicarbonate, di-n-propyl peroxydicarbonate, di(2-ethoxyethyl)peroxydicarbonate, t-butyl peroxyneodecanoate, t-butyl peroxypivalate, (3,5,5-trimethylhexanoyl)peroxide, dipropionyl peroxide, and diacetyl peroxide. The above polymerization initiators may be used alone or in combination of two or more kinds.

[0093] The reaction temperature during the polymerization reaction is preferably 40° C. or higher and 150° C. or higher, and more preferably 50° C. or higher and 110° C. or higher. The reaction time is preferably from 3 to 30 hours, and more preferably from 5 to 20 hours. The living radical polymerization can be carried out by a known polymerization method, but is preferably RAFT polymerization (reversible addition-fragmentation chain transfer polymerization). RAFT polymerization is a method of radically polymerizing monomers in the presence of a RAFT agent, and has the advantage that the molecular weight and molecular weight distribution of the resulting polymer or copolymer can be easily controlled.

[0094] RAFT agents are compounds that have a chain transfer effect and a polymerization initiation effect. Examples of such RAFT agents include dithiobenzoate type compounds, trithiocarbonate type compounds, dithiocarbamate type compounds, xanthate type compounds, and the like, or disulfide type compounds that are precursors of these. Examples of dithiobenzoate type compounds include 2-cyano-2-propyl dithiobenzoate, 4-cyano-4-(thiobenzoylthio)pentanoic acid, and 2-phenyl-2-propyl benzodithioate.

[0095] Trithiocarbonate type compounds include, for example, 4-[(2-carboxyethylsulfanylthiocarbonyl)sulfanyl]-4-cyanopentanoic acid, 2-{[(2-carboxyethyl)sulfanylthiocarbonyl]sulfanyl}propanoic acid, 4-cyano-4-[(dodecylsulfanylthiocarbonyl)sulfanyl]pentanoic acid, 2-cyano-2-[(dodecylsulfanylthiocarbonyl)sulfanyl]propane, 2-[(dodecylsulfanylthiocarbonyl)sulfanyl]propanoic acid, 4-cyano-4-[(dodecylsulfanylthiocarbonyl)sulfanyl]pe trithiocarbonate, methyl trithiocarbonate, 2-methyl-2-[(dodecylsulfanylthiocarbonyl)sulfanyl]propanoic acid, S,S-dibenzyl trithiocarbonate, trithiocarbonate = bis[4-(allyloxycarbonyl)benzyl], trithiocarbonate = bis[4-(2,3-dihydroxypropoxycarbonyl)benzyl], trithiocarbonate = bis{4-[ethyl-(2-acetyloxyethyl)carbamoyl]benzyl}, trithiocarbonate bis{4-[ethyl-(2-hydroxyethyl)carbamoyl]benzyl}, trithiocarbonate = bis[4-(2-hydroxyethoxycarbonyl)benzyl], and the like.

[0096] Examples of dithiocarbamate compounds include 2'-cyanobutan-2'-yl 4-chloro-3,5-dimethylpyrazole-1-carbodithioate, 2'-cyanobutan-2'-yl 3,5-dimethylpyrazole-1-carbodithioate, cyanomethyl 3,5-dimethylpyrazole-1-carbodithioate, and cyanomethyl N-methyl-N-phenyldithiocarbamate. Examples of disulfide type compounds include bis(dodecylsulfanylthiocarbonyl) disulfide, bis(thiobenzoyl) disulfide, and the like. The above-mentioned RAFT agents are suitable for use in the production of AB block polymers.

[0097] Among these, from the viewpoint of easy reaction control during synthesis, trithiocarbonate-type compounds are preferred as the RAFT agent, and 4-cyano-4-[(dodecylsulfanylthiocarbonyl)sulfanyl]pentanoic acid, 2-cyano-2-[(dodecylsulfanylthiocarbonyl)sulfanyl]propane, methyl 4-cyano-4-[(dodecylsulfanylthiocarbonyl)sulfanyl]pentanoate, bis{4-[ethyl-(2-hydroxyethyl)carbamoyl]benzyl} trithiocarbonate, and bis(dodecylsulfanylthiocarbonyl)disulfide are more preferred. The amount of the RAFT agent used is preferably 0.1 parts by mass or more and 10 parts by mass or less based on 100 parts by mass of the monomer.

[0098] It is preferable to use an organic solvent for the synthesis of the block copolymer. Examples of the organic solvent include ethyl acetate, n-butyl acetate, isobutyl acetate, toluene, xylene, acetone, hexane, methyl ethyl ketone, cyclohexanone, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, and diethylene glycol monobutyl ether acetate. The organic solvents may be used alone or in combination of two or more kinds.

[0099] The proportion of the second portion in the total mass of the block copolymer is preferably 30% by mass or more, more preferably 35% by mass or more, and even more preferably 40% by mass or more and 45% by mass or less, which makes it possible to prevent a decrease in steric repulsion caused by the second portion of the block copolymer and to allow the block copolymer to exhibit excellent affinity for the pigment. The amine value of the block copolymer is preferably from 10 mgKOH / g to 200 mgKOH / g, more preferably from 20 mgKOH / g to 150 mgKOH / g, and even more preferably from 30 mgKOH / g to 100 mgKOH / g. A block copolymer having an appropriate amine value has improved affinity (adsorption) for pigments and solubility in solvents, and further enhances the dispersion stability of the pigment.

[0100] The content of the dispersion resin is preferably 3% by mass or more and 35% by mass or less, more preferably 5% by mass or more and 30% by mass or less, and even more preferably 10% by mass or more and 25% by mass or less, based on the non-volatile content of the coloring composition. By using an appropriate amount of the dispersion resin, the resistance to the stripping solution in the dry etching process and the refractive index are excellent, and the dispersion stability of the coloring composition is further improved. By designing the structure of the monomer used, the basic dispersion resin may also be synthesized as a graft copolymer.

[0101] <<Dye derivatives>> The coloring composition may contain a dye derivative, if necessary. The dye derivative is a compound having an acidic group, a basic group, a neutral group, or the like in the organic dye residue. Examples of dye derivatives include compounds having an acidic group such as a sulfo group, a carboxy group, or a phosphate group, or amine salts thereof, sulfonamide groups, compounds having a basic group such as a tertiary amino group at the terminal, and compounds having a neutral group such as a phenyl group or a phthalimidoalkyl group.

[0102] Examples of organic pigments include diketopyrrolopyrrole pigments, anthraquinone pigments, quinacridone pigments, dioxazine pigments, perinone pigments, perylene pigments, thiazine indigo pigments, triazine pigments, benzimidazolone pigments, indole pigments such as benzoisoindole, isoindoline pigments, isoindolinone pigments, quinophthalone pigments, naphthol pigments, threne pigments, metal complex pigments, and azo pigments such as azo, disazo, and polyazo.

[0103] The dye derivative may be used alone or in combination of two or more of the above compounds. The amount of the dye derivative used is preferably 1 part by mass or more and 100 parts by mass or less, more preferably 3 parts by mass or more and 70 parts by mass or less, and even more preferably 5 parts by mass or more and 50 parts by mass or less, relative to 100 parts by mass of the organic pigment. By adding a dye derivative to an organic pigment and carrying out a micronization treatment such as acid pasting, acid slurry, dry milling, salt milling, or solvent salt milling, the dye derivative is adsorbed onto the surface of the organic pigment, and the organic pigment can be dispersed more finely than in the case where the dye derivative is not added.

[0104] <<Organic ingredients>> The colouring composition may further contain an organic component. When the filter units 215R, 215G, and 215B are formed by a dry etching method, i.e., when a cured product of the coloring composition is processed by a dry etching method, it is preferable that the coloring composition contains, as an organic component, a copolymer having a first structural unit (first repeating unit) having a polymerizable group in a side chain, and a second structural unit (second repeating unit) having an acidic group or a basic group in a side chain. Such a coloring composition may be a composition that is cured by heat and / or light. From the viewpoint of uniformity of curing and increasing the pigment content in the coloring composition, it is preferable that the coloring composition is a composition that is cured at least by heat (hereinafter, also referred to as "coloring thermosetting composition").

[0105] Hereinafter, the copolymer having the first structural unit and the second structural unit will also be referred to as a "curable copolymer". By including the first structural unit, it is possible to impart curability to the curable copolymer, and by including the second structural unit, it is possible to enhance the dispersibility of the pigment by the curable copolymer. Therefore, it is possible to obtain a coloring composition containing a large amount of pigment by reducing the amount of components other than the pigment (dispersant, thermosetting compound, curing agent, etc.). In addition, by forming the filter units 215R, 215G, and 215B using this coloring composition, it is possible to further reduce the thickness.

[0106] A preferred method for introducing a polymerizable group into a curable copolymer is to add a compound having a polymerizable group to a copolymer having an acidic group or a hydroxyl group in a side chain by reaction.

[0107] Examples of the polymerizable group include an allyl group, a vinyl group, a styryl group, an acryloyl group, and a methacryloyl group, with an acryloyl group and a methacryloyl group being preferred. Examples of monomers having a polymerizable group include acrylic acid, methacrylic acid, allyl methacrylate, allyl acrylate, vinyl methacrylate, vinyl acrylate, 2-(vinyloxy)ethyl methacrylate, p-vinyloxystyrene, p-{2-(vinyloxy)ethyl}styrene, etc. Among these, acrylic acid and methacrylic acid are preferred.

[0108] A preferred method for introducing an acidic group or a basic group into the curable copolymer is to copolymerize a monomer having an acidic group or a basic group. The "acidic group or basic group" (hereinafter also referred to as "dispersing group") can be selected from various functional groups.

[0109] Examples of the acidic group include a carboxyl group, a sulfonic acid group, a phosphate group, etc. Among these, from the viewpoint of the dispersion stability of the pigment, the acidic group is preferably a carboxyl group or a phosphate group, and more preferably a carboxyl group. Examples of monomers having an acidic group include acrylic acid, methacrylic acid, itaconic acid, aspartic acid, and sulfonic acid, with acrylic acid, methacrylic acid, and aspartic acid being preferred. Examples of the monomer having a hydroxyl group include 2-methacryloyloxyethyl isocyanate and 2-acryloyloxyethyl isocyanate.

[0110] Examples of the basic group include an amino group, a guanidino group, an imidazole group, a secondary amino group, a tertiary amino group, and a quaternary ammonium group. The monomer having a basic group is preferably, for example, N,N-dimethyllaurylamine or N,N-dimethylpalmitylamine, and more preferably N,N-dimethylpalmitylamine.

[0111] When the pigment has an acidic group on the surface, a curable copolymer containing a basic group (e.g., a primary to tertiary amino group) is preferred, and when the pigment has a basic group on the surface, a curable copolymer containing an acidic group (e.g., a carboxyl group) is preferred. From the above viewpoints, the copolymer is more preferably a copolymer containing an allyl group and a pigment adsorption group (dispersing group). The allyl group may be polymerized (cured) by heat. The thermal curing method is preferred because it is easy to uniformly cure the coloring composition and does not require an initiator. In addition, it is easy to increase the pigment content in the non-volatile content (total non-volatile content) of the coloring composition. Here, the "non-volatile content (total non-volatile content) of the coloring composition" refers to all components excluding the solvent from the coloring composition.

[0112] As an embodiment in which a compound having a polymerizable group is added to a copolymer having an acidic group or a basic group in a side chain by reaction, a method in which a copolymer is synthesized from a monomer having an acidic group or a basic group and a monomer having a reactive functional group such as a hydroxyl group or a carboxyl group, and then the copolymer is reacted with a monomer having a reactive functional group that reacts with the reactive functional group is also preferred. Examples of the method include a method of reacting a copolymer having a hydroxyl group with 2-methacryloyloxyethyl isocyanate, and a method of reacting a copolymer having a carboxyl group with glycidyl methacrylate.

[0113] The weight average molecular weight of the curable copolymer is preferably 3,000 or more and 300,000 or less, more preferably 5,000 or more and 100,000 or less, and even more preferably 7,000 or more and 70,000 or less. Furthermore, the ratio of polymerizable groups to dispersing groups (polymerizable groups / dispersing groups) is preferably, in molar ratio, 95 / 5 or more and 5 / 95 or less, more preferably 85 / 15 or more and 15 / 85 or less, and even more preferably 75 / 25 or more and 25 / 75 or less.

[0114] The content of the curable copolymer in the non-volatile matter of the coloring composition varies slightly depending on the type of the curable copolymer, and is not particularly limited, but is preferably 50% by mass or less, more preferably 0.1% by mass or more and 45% by mass or less, and even more preferably 0.5% by mass or more and 40% by mass or less. In addition to the curable copolymer, the coloring composition may also contain a thermosetting compound, which is an optional component, as described below. In this case, the total content of the curable copolymer and the thermosetting compound in the coloring composition is preferably 50% by mass or less, more preferably 0.2% by mass or more and 50% by mass or less, and even more preferably 1% by mass or more and 30% by mass or less, in the non-volatile content (mass) of the coloring composition.

[0115] The organic component may contain a binder other than the curable copolymer in addition to the curable copolymer from the viewpoint of improving the ease of adjusting the thickness of the coating film (liquid coating) of the coloring composition, etc. In this embodiment (dry etching application), the binder does not need to be alkali-soluble, and it is sufficient that it is soluble in an organic solvent. Examples of such binders include polymers having a carboxyl group in the side chain, such as methacrylic acid copolymers, acrylic acid copolymers, itaconic acid copolymers, crotonic acid copolymers, maleic acid copolymers, and partially esterified maleic acid copolymers, and acidic cellulose derivatives having a carboxyl acid in the side chain.

[0116] In addition to the above, other useful binders include adducts of acid anhydrides added to polymers having hydroxyl groups, polyhydroxystyrene resins, polysiloxane resins, poly(2-hydroxyethyl (meth)acrylate), polyvinylpyrrolidone, polyethylene oxide, polyvinyl alcohol, and the like. Also, a monomer having hydrophilicity may be copolymerized. Examples of such monomers include alkoxyalkyl (meth)acrylate, hydroxyalkyl (meth)acrylate, glycerol (meth)acrylate, (meth)acrylamide, N-methylolacrylamide, secondary or tertiary alkylacrylamide, dialkylaminoalkyl (meth)acrylate, morpholine (meth)acrylate, N-vinylpyrrolidone, N-vinylcaprolactam, vinylimidazole, vinyltriazole, methyl (meth)acrylate, ethyl (meth)acrylate, branched or linear propyl (meth)acrylate, branched or linear butyl (meth)acrylate, and phenoxyhydroxypropyl (meth)acrylate.

[0117] Among these, from the viewpoint of heat resistance, polyhydroxystyrene-based resins, polysiloxane-based resins, acrylic-based resins, acrylamide-based resins, and acrylic / acrylamide copolymers are preferred as binders, and from the viewpoint of developability control, acrylic-based resins, acrylamide-based resins, and acrylic / acrylamide copolymer resins are preferred. Examples of the acrylic resin include copolymers made of monomers selected from benzyl (meth)acrylate, (meth)acrylic acid, hydroxyethyl (meth)acrylate, (meth)acrylamide, etc. Examples of such copolymers include benzyl methacrylate / methacrylic acid copolymer, benzyl methacrylate / benzyl methacrylamide copolymer, KS Resist-106 (manufactured by Osaka Organic Chemical Industry Co., Ltd.), and Cyclomer P series (manufactured by Daicel Chemical Industries, Ltd.).

[0118] The weight average molecular weight of the binder is 1,000 or more and 2×10 5 It is preferable that the ratio is 2,000 or more and 1×10 or less. 5 More preferably, it is 5,000 or more and 5×10 4 It is even more preferable that: The coloring composition can provide adhesion to an underlying layer, etc., when a cured film is formed by dispersing a pigment at a high content in a curable copolymer (and a binder as necessary), and can also contribute to film-forming properties during spin coating or slit coating.

[0119] In this embodiment (dry etching application), it is not necessary to add a monomer (polymerizable compound) or a photopolymerization initiator, which are essential components in the photolithography method, to the coloring composition. Therefore, the non-volatile content (total non-volatile content) of the coloring composition, in other words, the pigment content in the filter units 215R, 215G, and 215B, which are the cured products of the coloring composition, can be set to 65 mass% or more. This can improve the spectral characteristics of the filter units 215R, 215G, and 215B. The content of the pigment in the coloring composition is preferably 65% ​​by mass or more and less than 100% by mass, more preferably 70% by mass or more and 98% by mass or less, and even more preferably 75% by mass or more and 95% by mass or less, based on the non-volatile content of the coloring composition. In this case, the spectral characteristics and color reproducibility of the filter units 215R, 215G, and 215B are high, and the curability of the coloring composition can be good.

[0120] <<Other ingredients>> The coloring composition may contain other components in addition to the above components. ·dye In the coloring composition, dyes may be used in combination with the pigments described above. Examples of the dye include triphenylmethane dyes, anthraquinone dyes, benzylidene dyes, oxonol dyes, cyanine dyes, phenothiazine dyes, pyrrolopyrazole azomethine dyes, xanthene dyes, phthalocyanine dyes, benzopyran dyes, and indigo dyes.

[0121] ·Thermosetting compounds The thermosetting compound may contain a thermosetting compound as an auxiliary. The thermosetting compound is not particularly limited as long as it can be cured by heating, and examples thereof include epoxy compounds, oxetane compounds, benzoguanamine compounds, rosin-modified maleic acid compounds, rosin-modified fumaric acid compounds, melamine compounds, urea compounds, and blocked isocyanate compounds. Among these, epoxy compounds, oxetane compounds, melamine compounds, and blocked isocyanate compounds are preferred, and epoxy compounds are more preferred.

[0122] (Epoxy compounds) Examples of the epoxy compound include glycerol polyglycidyl ether, sorbitol polyglycidyl ether, polycondensates of bisphenol (bisphenol A, bisphenol F, bisphenol S, biphenol, bisphenol AD, etc.), phenol (phenol, alkyl-substituted phenol, aromatic-substituted phenol, naphthol, alkyl-substituted naphthol, dihydroxybenzene, alkyl-substituted dihydroxybenzene, dihydroxynaphthalene, etc.) and various aldehydes (formaldehyde, acetaldehyde, alkyl aldehyde, benzaldehyde, alkyl-substituted benzaldehyde, hydroxybenzaldehyde, naphthaldehyde, glutaraldehyde, phthalaldehyde, crotonaldehyde, cinnamaldehyde, etc.), polycondensates of phenol and various diene compounds (dicyclopentadiene, terpene, vinylcyclohexene, norbornadiene, vinylnorbornene, tetrahydrofuran ... Examples of the epoxy resin include polymers of phenols and ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, acetophenone, benzophenone, etc.), polycondensates of phenols and aromatic dimethanols (benzene dimethanol, α,α,α',α'-benzene dimethanol, biphenyl dimethanol, α,α,α',α'-biphenyl dimethanol, etc.), polycondensates of phenol and aromatic dichloromethyls (α,α'-dichloroxylene, bischloromethylbiphenyl, etc.), polycondensates of bisphenol and various aldehydes, glycidyl ether epoxy resins obtained by glycidylating alcohols, alicyclic epoxy resins, heterocyclic epoxy resins, aliphatic epoxy resins, glycidyl amine epoxy resins, and glycidyl ester epoxy resins.

[0123] Commercially available epoxy compounds include, for example, Epicoat 807, 815, 825, 827, 828, 190P, and 191P manufactured by Yuka Shell Epoxy Co., Ltd., and TECHMORE manufactured by Mitsui Chemicals, Inc. VG3101L, EPPN-201, 501H, 502H, EOCN-102S, 103S, 104S, 1020 manufactured by Nippon Kayaku Co., Ltd., Epicoat 1004, 1256, JER1032H60, 157S65, 157S70, 152, 154 manufactured by Japan Epoxy Resins Co., Ltd., Celloxide 2021, EHPE-3150, Epolead GT401 manufactured by Daicel Chemical Industries, Denacol EX-211, 212, 252, 313, 314, 321, 411, 421, 512, 521, 611, 612, 614, 614B, 622, 711, 721 manufactured by Nagase ChemteX Corporation, TEPIC-L, H, S manufactured by Nissan Chemical Industries, and EPICLON manufactured by DIC Corporation Examples include 830, 840, 850, 860, 1050, 3050, 4050, N-660, N-670, N-740, N-770, N865, HP-7200, HP-4700, HP-4770, HP-5000, HP-6000, and HP-9500.

[0124] From the viewpoints of high temperature and high humidity resistance and solvent resistance, the epoxy compound is preferably a compound having 2 to 50 epoxy groups in the molecule. The epoxy equivalent of the epoxy compound is preferably 50 g / eq or more and 400 g / eq or less, and more preferably 100 g / eq or more and 200 g / eq or less. The epoxy equivalent is defined as the mass of an epoxy compound containing one equivalent of an epoxy group. The thermosetting compounds can be used alone or in combination of two or more kinds. The content of the thermosetting compound is preferably from 0.5 to 20% by mass, and more preferably from 1 to 15% by mass, based on 100% by mass of the nonvolatile content of the photosensitive composition.

[0125] Photopolymerization initiator The coloring composition may additionally contain a photopolymerization initiator. Examples of the photopolymerization initiator include a benzophenone compound, an acetophenone compound, an oxime ester compound, an acylphosphine compound, a quinone compound, a borate compound, and a carbazole compound.

[0126] Commercially available photopolymerization initiators include acetophenone compounds such as Omnirad 907, 369E, 379EG, 127, 184, 1173, and 2959 manufactured by IGM Resins, acylphosphine compounds such as Omnirad 819 and TPO manufactured by IGM Resins, and oxime compounds such as IRGACURE OXE-01, 02, 03, and 04 manufactured by BASF Japan, N-1919, NCI-730, 831, and 930 manufactured by ADEKA, TRONLY TR-PBG-301, 304, 305, 309, 314, 345, 358, 380, 365, 610, 3054, and 3057 manufactured by Changzhou New Strength Materials Co., Ltd. Examples of such resins include Omnirad 1312, 1314, and 1316 manufactured by Resins Co., Ltd., SPI-02, 03, 04, 05, 06, and 07 manufactured by Samyang Corporation, and DFI-020, 306, and EOX-01 manufactured by Daito Chemistrys Co., Ltd. Among these, oxime ester compounds are preferred in terms of photocurability, and compounds represented by the following general formula (6) and compounds represented by the following general formula (7) are preferred in terms of further improving heat resistance and pattern shape.

[0127] [ka]

[0128] In formula (6), R1 and R2 each independently represent a hydrogen atom or an alkyl group having 1 to 8 carbon atoms, and R3 represents a hydrogen atom or a monovalent substituent. In the general formula (7), X1 and X2 each independently represent a carbonyl bond (-CO-) or a single bond. R4 represents an alkyl group having 1 to 20 carbon atoms, and R5 and R6 each independently represent a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, a heterocyclic group having 2 to 30 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an arylalkyl group having 7 to 30 carbon atoms. R7 and R8 each independently represent an alkyl group having 1 to 20 carbon atoms, a heterocyclic group having 2 to 30 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an arylalkyl group having 7 to 30 carbon atoms.

[0129] In general formula (6), R1 and R2 each independently represent a hydrogen atom or an alkyl group having 1 to 8 carbon atoms. The alkyl group having 1 to 8 carbon atoms may be linear, branched, or cyclic, or may be a combination of these, and examples thereof include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a t-butyl group, a pentyl group, an isopentyl group, a hexyl group, a heptyl group, an octyl group, a 2-ethylhexyl group, a cyclopentyl group, a cyclopentylmethyl group, a cyclohexyl group, a cyclohexylmethyl group, a cyclohexylmethyl group, etc. Among these, a linear alkyl group having 3 to 8 carbon atoms is preferred, and a linear alkyl group having 4 to 6 carbon atoms is more preferred.

[0130] In general formula (6), R3 represents a hydrogen atom or any monovalent substituent. Examples of the monovalent substituent include an alkyl group having 1 to 20 carbon atoms, such as a methyl group or an ethyl group; an alkoxy group having 1 to 20 carbon atoms, such as a methoxy group or an ethoxy group; a halogen atom, such as F, Cl, Br, or I; an acyl group having 1 to 20 carbon atoms; an alkyl ester group having 1 to 20 carbon atoms; an alkoxycarbonyl group having 1 to 20 carbon atoms; a halogenated alkyl group having 1 to 20 carbon atoms, an aromatic ring group having 4 to 20 carbon atoms; an amino group; an aminoalkyl group having 1 to 20 carbon atoms; a hydroxyl group; a nitro group; a cyano group; a benzoyl group which may have a substituent; and a thenoyl group which may have a substituent. Examples of the substituent that the benzoyl group or thenoyl group may have include an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, and an alkoxycarbonyl group having 1 to 10 carbon atoms. Among these, from the viewpoint of radical generation efficiency, a hydrogen atom and a nitro group are preferred, and a hydrogen atom is more preferred.

[0131] Examples of methods for producing the compound represented by general formula (6) include those described in JP-T-2019-507108 and JP-T-2019-528331. Specific examples of the compound represented by formula (6) are shown below, but the present invention is not limited to these.

[0132] [ka]

[0133] In the general formula (7), X1 and X2 each independently represent a carbonyl bond (-CO-) or a single bond. Among them, from the viewpoint of solubility in an organic solvent, at least one of X1 and X2 is preferably a carbonyl bond (-CO-), and both are more preferably carbonyl bonds (-CO-).

[0134] In the general formula (7), R4 represents an alkyl group having 1 to 20 carbon atoms. The alkyl group having 1 to 20 carbon atoms may be any of linear, branched, cyclic, or combinations thereof, and may be substituted with a halogen atom, an amino group, a nitro group, or the like. Examples include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a t-butyl group, an amyl group, an isoamyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, an isooctyl group, a 2-ethylhexyl group, a nonyl group, a decyl group, a cyclopentyl group, a cyclopentylmethyl group, a cyclohexyl group, a cyclohexylmethyl group, and a cyclohexylmethyl group. Among these, an ethyl group, a propyl group, and an isopropyl group are preferred.

[0135] In general formula (7), R5 and R6 each independently represent a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, a heterocycle having 2 to 30 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an arylalkyl group having 7 to 30 carbon atoms. The alkyl group having 1 to 20 carbon atoms may be any of linear, branched, cyclic, or combinations thereof, and may be substituted with a halogen atom, an amino group, a nitro group, or the like. Examples include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a t-butyl group, an amyl group, an isoamyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, an isooctyl group, a 2-ethylhexyl group, a nonyl group, an isononyl group, a decyl group, an isodecyl group, an undecyl group, a dodecyl group, a hexadecyl group, a cyclopentyl group, a cyclopentylmethyl group, a cyclohexyl group, a cyclohexylmethyl group, and a cyclohexylmethyl group. Among these, a pentyl group, a hexyl group, a heptyl group, a cyclopentyl group, a cyclopentylmethyl group, a cyclohexyl group, a cyclohexylmethyl group, and a cyclohexylmethyl group are preferred.

[0136] Examples of the heterocyclic group having 2 to 30 carbon atoms include a pyridyl group, a pyrimidyl group, a furyl group, a tetrahydrofuryl group, a dioxolanyl group, an imidazolidyl group, an oxazolidyl group, a piperidyl group, and a morpholinyl group. Examples of the aryl group having 6 to 30 carbon atoms include a phenyl group, a tolyl group, a xylyl group, an ethylphenyl group, a naphthyl group, and an anthryl group, and may also be an aryl group substituted with a halogen atom, an amino group, a nitro group, or the like. Examples of the arylalkyl group having 7 to 30 carbon atoms include a benzyl group, an α-methylbenzyl group, an α,α-dimethylbenzyl group, and a phenylethyl group, and may also be an arylalkyl group substituted with a halogen atom, an amino group, a nitro group, or the like. Among these, R5 and R6 are more preferably a linear alkyl group having 1 to 20 carbon atoms and a cyclic alkyl group having 1 to 20 carbon atoms.

[0137] In general formula (7), R7 and R8 each independently represent an alkyl group having 1 to 20 carbon atoms, a heterocyclic group having 2 to 30 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an arylalkyl group having 7 to 30 carbon atoms. The alkyl group having 1 to 20 carbon atoms may be any of linear, branched, cyclic, or combinations thereof, and may also be an alkyl group substituted with a halogen atom, an amino group, a nitro group, or the like. Examples include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a t-butyl group, an amyl group, an isoamyl group, a pentyl group, a hexyl group, a cyclopentyl group, a cyclopentylmethyl group, and a cyclohexyl group. Among these, from the viewpoint of reactivity, a methyl group, an ethyl group, a propyl group, and an isopropyl group are preferred.

[0138] Examples of the heterocyclic group having 2 to 30 carbon atoms include a pyridyl group, a pyrimidyl group, a furyl group, a tetrahydrofuryl group, a dioxolanyl group, an imidazolidyl group, an oxazolidyl group, a piperidyl group, and a morpholinyl group. Examples of the aryl group having 6 to 30 carbon atoms include a phenyl group, a tolyl group, a xylyl group, an ethylphenyl group, a naphthyl group, an anthryl group, etc., and may also be an aryl group substituted with a halogen atom, an amino group, a nitro group, etc. Among these, a phenyl group is preferred from the viewpoint of reactivity. Examples of the arylalkyl group having 7 to 30 carbon atoms include a benzyl group, an α-methylbenzyl group, an α,α-dimethylbenzyl group, and a phenylethyl group, and may also be an arylalkyl group substituted with a halogen atom, an amino group, a nitro group, or the like.

[0139] Among these, from the viewpoint of reactivity, R7 and R8 are preferably a methyl group, an ethyl group, or a phenyl group, and more preferably a methyl group or an ethyl group. The compound represented by general formula (7) can be produced by, for example, the method described in JP-A-2017-523465. Specific examples of the compound represented by formula (7) are shown below, but the present invention is not limited to these.

[0140] [ka]

[0141] The content of the photopolymerization initiator is preferably 0.5% by mass or more and 20% by mass or less, based on 100% by mass of the nonvolatile content of the colored composition.

[0142] When a photopolymerization initiator is used, a sensitizer and a light stabilizer can be used in combination. Specific examples thereof include benzoin, benzoin methyl ether, 9-fluorenone, 2-chloro-9-fluorenone, 2-methyl-9-fluorenone, 9-anthrone, 2-bromo-9-anthrone, 2-ethyl-9-anthrone, 9,10-anthraquinone, 2-ethyl-9,10-anthraquinone, 2-t-butyl-9,10-anthraquinone, 2,6-dichloro-9,10-anthraquinone, xanthone, 2-methylxanthone, 2-methoxyxanthone, 2-ethoxyxanthone, thioxanthone, 2,4-diethylthioxanthone, acridone, 10-butyl-2-chloroacridone, benzyl, and dibenzylacetone. , p-(dimethylamino)phenyl styryl ketone, p-(dimethylamino)phenyl-p-methyl styryl ketone, benzophenone, p-(dimethylamino)benzophenone (or Michler's ketone), p-(diethylamino)benzophenone, benzanthrone, benzothiazole compounds, 5-(2H-benzotriazol-2-yl)-4-hydroxy-3-tert-butylbenzenepropanoate methyl (Tinuvin 1130), 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl]-5-[3-(dodecyloxy)-2-hydroxypropoxy]phenol (Tinuvin 400), and the like.

[0143] Other photopolymerization initiators include, for example, vicinal polyketolualdonyl compounds, α-carbonyl compounds, acyloin ethers, aromatic acyloin compounds substituted with α-hydrocarbons, polynuclear quinone compounds, combinations of triaryl imidazole dimer / p-aminophenyl ketone, combinations of benzothiazole compounds / trihalomethyl-s-triazine compounds, and the like.

[0144] Hardener When an epoxy resin is used as the thermosetting compound, it is preferable to add a curing agent to the coloring composition. Specific examples of the curing agent include diethylenetriamine, metaphenylenediamine, tris(dimethylaminomethyl)phenol, phthalic anhydride, polyamide resin, polysulfide resin, boron trifluoride-monoethylamine complex, phenol resin, and dicyandiamide.

[0145] These curing agents are compounds that react with epoxy groups by heating, and are polymerized to increase the crosslink density and harden. The content of the curing agent in the coloring composition is preferably as small as possible in order to form a thin film, and is preferably 35% by mass or less, more preferably 30% by mass or less, and even more preferably 25% by mass or less, based on the thermosetting compound.

[0146] ·Curing catalyst The coloring composition may contain a curing catalyst. When an epoxy resin is used as the curable compound, the curing catalyst that can be suitably used includes, for example, an imidazole compound, a boron trifluoride complex (particularly, an amine complex), a tertiary amine (guanidine, biguanide), a titanate ester, a phosphine derivative, and the like. The amount of the curing catalyst used is, in terms of mass ratio, preferably 1 / 10 or more and 1 / 1,000 or less, more preferably 1 / 20 or more and 1 / 500 or less, and even more preferably 1 / 30 or more and 1 / 250 or less, relative to the epoxy resin having an epoxy equivalent of 150 or more and 200 or less.

[0147] Examples of commercially available curing catalysts include, but are not limited to, the imidazole silane series "IS-1000", "IS-1000D", "IM-1000", "SP-1000", "IA-1000A", "IA-100P", "IA-100F", "IA-100AD", "IA-100FD", "IM-100F", "IS-3000", and "IS-4000" (all manufactured by Japan Energy Corporation), "1B2PZ", and "SFZ" (all manufactured by Shikoku Kasei Co., Ltd.).

[0148] ·solvent The coloring composition may contain at least one solvent. The solvent is preferably selected in consideration of the solubility of each component, the coatability of the colored composition, safety, and the like. Examples of the solvent include ketones, aromatic hydrocarbons, esters, and ethers. Examples of the ketone include methyl ethyl ketone, cyclohexanone, 2-heptanone, and 3-heptanone. Examples of aromatic hydrocarbons include toluene and xylene.

[0149] Examples of the ester include ethyl acetate, n-butyl acetate, isobutyl acetate, amyl formate, isoamyl acetate, isobutyl acetate, butyl propionate, isopropyl butyrate, ethyl butyrate, butyl butyrate, alkyl esters, methyl lactate, ethyl lactate, methyl oxyacetate, ethyl oxyacetate, butyl oxyacetate, methyl methoxyacetate, ethyl methoxyacetate, butyl methoxyacetate, methyl ethoxyacetate, ethyl ethoxyacetate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, 3-ethoxypropionate, Examples of the methyl 2-methoxypropionate, ethyl 3-ethoxypropionate, methyl 2-methoxypropionate, ethyl 2-methoxypropionate, propyl 2-methoxypropionate, methyl 2-ethoxypropionate, ethyl 2-ethoxypropionate, methyl 2-methoxy-2-methylpropionate, ethyl 2-ethoxy-2-methylpropionate, methyl pyruvate, ethyl pyruvate, propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, methyl 2-oxobutanoate, and ethyl 2-oxobutanoate.

[0150] Examples of the ether include diethylene glycol dimethyl ether, tetrahydrofuran, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, and propylene glycol monopropyl ether acetate.

[0151] Dispersants A dispersant may be added to the coloring composition as an auxiliary agent in order to improve the dispersibility of the pigment. Examples of the dispersant include cationic surfactants, fluorine-based surfactants, polymer dispersants, etc. The dispersants may be used alone or in combination of two or more kinds. For example, a graft copolymer having a specific acid amide group-containing monomer and a quaternary ammonium salt monomer residue in the main chain has an excellent effect of finely dispersing a pigment, and can be used as a dispersant. By using the graft copolymer, the pigment can be finely dispersed while reducing the consumption of energy and time. In addition, the dispersed pigment does not aggregate or settle even over time, and can maintain dispersion stability for a long period of time. The content of the dispersant in the coloring composition is usually preferably 0.1 parts by mass or more and 50 parts by mass or less with respect to 100 parts by mass of the pigment.

[0152] <Method of preparing coloring composition> Next, an example of a method for preparing a colored composition will be described. In the following description, the curable copolymer (and the binder, if necessary) may be referred to as a "curable resin." The coloring composition can be suitably prepared by using a pigment dispersion in which a pigment is dispersed in the presence of a curable resin. A suitable method for dispersing a pigment is to use a pigment having fine particles with a sharp particle size distribution, specifically, a method using a pigment having an average particle size of about 0.01 μm and containing 75% or more by mass of pigment particles having a particle size in the range of 0.01±0.005 μm.

[0153] Examples of dispersion methods for adjusting the particle size distribution of pigments to the above range include a combination of dry dispersion (kneading dispersion treatment) in which dispersion is performed in a high viscosity state using a kneader, two-roll mill, etc., and wet dispersion (fine dispersion treatment) in which dispersion is performed in a relatively low viscosity state using a three-roll mill, bead mill, etc. In the dispersion method, it is also preferable to co-disperse two or more pigments, or to use no solvent or to use as little solvent as possible during the kneading dispersion treatment. In order to reduce the solvent shock, it is preferable to add the curable resin separately (using two portions) during the kneading dispersion treatment and the fine dispersion treatment. It is also preferable to use a curable resin with excellent solubility in order to prevent the pigment particles from re-aggregating when moving from the kneading dispersion treatment to the fine dispersion treatment. Furthermore, it is also effective to use high hardness ceramics or beads with small particle size for the beads of the bead mill used in the fine dispersion treatment.

[0154] It is particularly preferable to use two or more pigments, disperse these pigments in a high-viscosity state of 50,000 mPa s or more, and then disperse them in a low-viscosity state of 1,000 mPa s or less. Generally, these pigments are synthesized and then dried by various methods before being supplied. Usually, they are dried from an aqueous medium and supplied as a powder, but since drying water requires a large latent heat of evaporation, a large amount of thermal energy is applied to dry the pigment into a powder. For this reason, pigments usually form aggregates (secondary particles) consisting of aggregates of primary particles.

[0155] In the method for preparing the colored composition, it is preferable to first prepare a pigment dispersion in which the pigment is dispersed in the curable resin. Specifically, it is preferable to carry out a kneading and dispersing treatment on the pigment and the curable resin so that the viscosity after the kneading and dispersing treatment becomes relatively high, 50,000 mPa·s or more (preferably 50,000 mPa·s or more and 100,000 mPa·s or less). Here, the kneading and dispersion treatment may be high-viscosity dispersion or dry dispersion.

[0156] Next, if necessary, a curable resin, other dispersants, etc. are added to the pigment dispersion after the kneading and dispersion treatment, and it is preferable to perform a fine dispersion treatment so that the viscosity after the fine dispersion treatment becomes relatively low, that is, 1,000 mPa s or less (preferably 100 mPa s or less). The fine dispersion treatment may be a low viscosity dispersion or a wet dispersion.

[0157] In the kneading dispersion treatment, the ratio of the solvent to the dispersed material is preferably 0% by mass or more and 20% by mass or less. In this way, when dispersion is performed without using much solvent, it is possible to promote wetting of the pigment particle surface with the constituent components of the vehicle, mainly composed of the resin component. Therefore, it is possible to convert the interface formed by the pigment particle surface from a solid / gas interface between the pigment particle and air to a solid / solution interface between the pigment particle and the vehicle solution. When the interface formed by the pigment particle surface is converted from air to a solution and mixed and stirred, it is possible to disperse the pigment into a fine state close to primary particles.

[0158] Thus, in order to highly disperse a pigment, it is effective to convert the interface formed by the surface of the pigment particles from air to a solution. Such conversion requires strong shearing and compressive forces. For this reason, in the kneading dispersion treatment, it is preferable to use a kneader capable of exerting strong shearing and compressive forces and to use a highly viscous material as the material to be kneaded. In addition, during the fine dispersion treatment, it is preferable to mix and stir the mixture together with fine particle dispersion media such as glass or ceramic. Furthermore, the ratio of the solvent during the fine dispersion treatment is preferably 20% by mass or more and 90% by mass or less of the material to be dispersed.

[0159] During the fine dispersion treatment, it is necessary to distribute the pigment particles uniformly and stably down to a minute size. Therefore, it is preferable to use a disperser capable of applying impact and shear forces to the aggregated pigment particles and to use a low-viscosity material as the dispersed material. A colored composition can be prepared by adding a curing catalyst or a curing agent, and further a thermosetting compound, if necessary, to the pigment dispersion thus obtained, and further adding a solvent, if necessary.

[0160] When the filter units 215R, 215G, and 215B are formed by photolithography, an alkali-soluble resin is used as the binder.

[0161] <<Alkali-soluble resin>> The molecular weight of the alkali-soluble resin is not particularly limited, but the weight average molecular weight (Mw) is preferably 5000 or more and 100,000 or less, and the number average molecular weight (Mn) is preferably 1,000 or more and 20,000 or less. The alkali-soluble resin may be a resin having at least one group that promotes alkali solubility in the molecule (preferably a molecule having an acrylic copolymer or a styrene copolymer as the main chain).

[0162] As the alkali-soluble resin, from the viewpoint of heat resistance, polyhydroxystyrene-based resins, polysiloxane-based resins, acrylic-based resins, acrylamide-based resins, and acrylic / acrylamide copolymer resins are preferred, and from the viewpoint of controllability of developability, acrylic-based resins, acrylamide-based resins, and acrylic / acrylamide copolymer resins are preferred. Examples of groups that promote alkali solubility (hereinafter also referred to as "acid groups") include carboxyl groups, phosphoric acid groups, sulfonic acid groups, and phenolic hydroxyl groups. The acid groups are preferably soluble in organic solvents and developable with weak alkaline aqueous solutions, and are preferably groups derived from (meth)acrylic acid. These acid groups may be of one type only or of two or more types.

[0163] The alkali-soluble resin can be produced, for example, by a radical polymerization method. Polymerization conditions such as temperature, pressure, type and amount of radical initiator, type of solvent, etc., when producing the alkali-soluble resin by the radical polymerization method can be appropriately set. The alkali-soluble resin is preferably a polymer having a carboxylic acid in the side chain, and examples thereof include alkali-soluble phenolic resins such as methacrylic acid copolymers, acrylic acid copolymers, itaconic acid copolymers, crotonic acid copolymers, maleic acid copolymers, partially esterified maleic acid copolymers, novolac-type resins, acidic cellulose derivatives having a carboxyl group in the side chain, and polymers having a hydroxyl group to which an acid anhydride has been added.

[0164] In particular, a copolymer of (meth)acrylic acid and another monomer copolymerizable therewith is suitable as the alkali-soluble resin. Examples of the other monomer copolymerizable with (meth)acrylic acid include alkyl (meth)acrylates, aryl (meth)acrylates, and vinyl compounds. Examples of the alkyl (meth)acrylate and aryl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, tolyl (meth)acrylate, naphthyl (meth)acrylate, and cyclohexyl (meth)acrylate. Examples of the vinyl compound include styrene, α-methylstyrene, vinyl toluene, glycidyl methacrylate, acrylonitrile, vinyl acetate, N-vinylpyrrolidone, tetrahydrofurfuryl methacrylate, polystyrene macromonomer, polymethyl methacrylate macromonomer, N-phenylmaleimide, and N-cyclohexylmaleimide. These other monomers copolymerizable with (meth)acrylic acid may be used alone or in combination of two or more.

[0165] In addition, in order to improve the crosslinking efficiency of the coloring composition, an alkali-soluble resin having a polymerizable group may be used. Examples of the polymerizable group include a (meth)allyl group and a (meth)acryloyl group. As the alkali-soluble resin having a polymerizable group, an alkali-soluble resin having a polymerizable group in a side chain is useful. Examples of alkali-soluble resins containing a polymerizable group include the Dianarl NR series (manufactured by Mitsubishi Rayon Co., Ltd.), Photomer 6173 (manufactured by Diamond Shamrock Co., Ltd.), Viscoat R-264, KS Resist 106 (all manufactured by Osaka Organic Chemical Industry Co., Ltd.), Cyclomer P series, Plaxel CF200 series (all manufactured by Daicel Corporation), Ebecryl 3800 (manufactured by Daicel UCB Corporation), and Acricur RD-F8 (manufactured by Nippon Shokubai Co., Ltd.).

[0166] As the alkali-soluble resin, a multi-component copolymer such as a benzyl (meth)acrylate / (meth)acrylic acid copolymer, a benzyl (meth)acrylate / (meth)acrylic acid / 2-hydroxyethyl (meth)acrylate copolymer, or a benzyl (meth)acrylate / (meth)acrylic acid / other monomer copolymer is preferably used. In addition, examples of the alkali-soluble resin that can be suitably used include polymers copolymerized with 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate / polystyrene macromonomer / benzyl methacrylate / methacrylic acid copolymers, 2-hydroxy-3-phenoxypropyl acrylate / polymethyl methacrylate macromonomer / benzyl methacrylate / methacrylic acid copolymers, 2-hydroxyethyl methacrylate / polystyrene macromonomer / methyl methacrylate / methacrylic acid copolymers, and 2-hydroxyethyl methacrylate / polystyrene macromonomer / benzyl methacrylate / methacrylic acid copolymers. In addition, examples of commercially available alkali-soluble resins include FF-426 (manufactured by Fujikura Chemical Industries, Ltd.).

[0167] The acid value of the alkali-soluble resin is preferably 30 mgKOH / g or more and 500 mgKOH / g or less, more preferably 40 mgKOH / g or more and 400 mgKOH / g or less, even more preferably 50 mgKOH / g or more and 200 mgKOH / g or less, particularly preferably 60 mgKOH / g or more and 150 mgKOH / g or less, and most preferably 50 mgKOH / g or more and 120 mgKOH / g or less.

[0168] The content of the alkali-soluble resin in the coloring composition is preferably 0.1% by mass or more and 20% by mass or less, more preferably 0.5% by mass or more and 18% by mass or less, even more preferably 1% by mass or more and 15% by mass or less, particularly preferably 2% by mass or more and 12% by mass or less, and most preferably 3% by mass or more and 10% by mass or less, of the non-volatile content (total non-volatile content) of the coloring composition. The coloring composition may contain only one type of alkali-soluble resin, or may contain two or more types. When two or more types of alkali-soluble resins are contained, it is preferable to adjust the total content thereof to the above range. In this specification, the content of all resins including the dispersing resin and the binder in the colored composition is preferably from 3% by mass to 35% by mass, and more preferably from 10% by mass to 30% by mass.

[0169] When the filter units 215R, 215G, and 215B are formed by photolithography, the coloring composition may further contain a polymerizable compound and a photopolymerization initiator. <<Polymerizable compounds>> As the polymerizable compound, a monomer or oligomer having a polymerizable unsaturated group can be used. The polymerizable compound is preferably a compound having two or more polymerizable unsaturated groups, such as a vinyl group, a (meth)acryloyl group, or a (meth)allyl group.

[0170] Examples of the polymerizable compound include linear or branched alkyl (meth)acrylates; cyclic alkyl (meth)acrylates; fluoroalkyl (meth)acrylates; (meth)acryloxy-modified polydimethylsiloxanes (silicone macromers); (meth)acrylates having a heterocyclic ring; (meth)acrylates having an aromatic ring; (poly)alkylene glycol monoalkyl ether (meth)acrylates; (meth)acrylates having a carboxyl group; (meth)acrylates having a hydroxyl group; (poly)alkylene glycol di(meth)acrylates; di(meth)acrylates; (meth)acrylates having a tertiary amino group; trifunctional or higher polyfunctional (meth)acrylates; epoxy (meth)acrylates; (meth)acryloyl-modified resin oligomers; vinyls; vinyl ethers; amides; and acrylonitrile. The polymerizable compounds may be used alone or in combination of two or more kinds.

[0171] Examples of linear or branched alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth), tertiary butyl (meth)acrylate, isoamyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cetyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, isomyristyl (meth)acrylate, stearyl (meth)acrylate, and isostearyl (meth)acrylate.

[0172] Examples of cyclic alkyl (meth)acrylates include cyclohexyl (meth)acrylate, tertiary butyl cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, and isobornyl (meth)acrylate. Examples of the fluoroalkyl (meth)acrylate include trifluoroethyl (meth)acrylate, octafluoropentyl (meth)acrylate, perfluorooctylethyl (meth)acrylate, and tetrafluoropropyl (meth)acrylate.

[0173] Examples of the (meth)acrylate having a heterocycle include tetrahydrofurfuryl (meth)acrylate and 3-methyl-3-oxetanyl (meth)acrylate. Examples of the (meth)acrylate having an aromatic ring include benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, paracumylphenoxyethyl (meth)acrylate, paracumylphenoxypolyethylene glycol (meth)acrylate, and nonylphenoxypolyethylene glycol (meth)acrylate.

[0174] Examples of (poly)alkylene glycol monoalkyl ether (meth)acrylates include 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, 2-methoxypropyl (meth)acrylate, diethylene glycol monomethyl ether (meth)acrylate, diethylene glycol monoethyl ether (meth)acrylate, triethylene glycol monomethyl ether (meth)acrylate, triethylene glycol monoethyl ether (meth)acrylate, diethylene glycol mono-2-ethylhexyl ether (meth)acrylate, dipropylene glycol monomethyl ether (meth)acrylate, tripropylene glycol mono(meth)acrylate, polyethylene glycol monolauryl ether (meth)acrylate, and polyethylene glycol monostearyl ether (meth)acrylate.

[0175] Examples of (meth)acrylates having a carboxyl group include (meth)acrylic acid, acrylic acid dimer, 2-(meth)acryloyloxyethyl phthalate, 2-(meth)acryloyloxypropyl phthalate, 2-(meth)acryloyloxyethyl hexahydrophthalate, 2-(meth)acryloyloxypropyl hexahydrophthalate, ethylene oxide-modified succinic acid (meth)acrylate, β-carboxyethyl (meth)acrylate, and ω-carboxypolycaprolactone (meth)acrylate.

[0176] Examples of (meth)acrylates having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-acryloyloxyethyl-2-hydroxyethyl (meth)phthalate, diethylene glycol mono(meth)acrylate, dipropylene glycol mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, propylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, polytetramethylene glycol mono(meth)acrylate, poly(ethylene glycol-propylene glycol) mono(meth)acrylate, poly(ethylene glycol-tetramethylene glycol) mono(meth)acrylate, poly(propylene glycol-tetramethylene glycol) mono(meth)acrylate, and glycerol (meth)acrylate.

[0177] Examples of the (poly)alkylene glycol di(meth)acrylate include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, poly(ethylene glycol-propylene glycol) di(meth)acrylate, acrylate, poly(ethylene glycol-tetramethylene glycol) di(meth)acrylate, poly(propylene glycol-tetramethylene glycol) di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 2-ethyl,2-butyl-propanediol di(meth)acrylate, and the like.

[0178] Examples of the di(meth)acrylate include dimethylol dicyclopentane di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, stearic acid modified pentaerythritol di(meth)acrylate, ethylene oxide modified bisphenol A di(meth)acrylate, propylene oxide modified bisphenol A di(meth)acrylate, tetramethylene oxide modified bisphenol A di(meth)acrylate, ethylene oxide modified bisphenol F di(meth)acrylate, propylene oxide modified bisphenol F di(meth)acrylate, tetramethylene oxide modified bisphenol F di(meth)acrylate, zinc diacrylate, ethylene oxide modified phosphate triacrylate, and glycerol di(meth)acrylate.

[0179] Examples of the (meth)acrylate having a tertiary amino group include dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, and diethylaminopropyl (meth)acrylate.

[0180] Specific examples of trifunctional or higher polyfunctional (meth)acrylates include glycerol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.

[0181] Examples of epoxy (meth)acrylates include glycerol triglycidyl ether-(meth)acrylic acid adduct, glycerol diglycidyl ether-(meth)acrylic acid adduct, polyglycerol polyglycidyl ether-(meth)acrylic acid adduct, 1,6-butanediol diglycidyl ether, alkyl glycidyl ether-(meth)acrylic acid adduct, allyl glycidyl ether-(meth)acrylic acid adduct, phenyl glycidyl ether-(meth)acrylic acid adduct, styrene oxide-(meth)acrylic acid adduct, bisphenol A diglycidyl ether-(meth)acrylic acid adduct, propylene oxide modified bisphenol A diglycidyl ether-(meth)acrylic acid adduct, ... Examples of the epoxy resins that can be used include phthalic acid diglycidyl ether-(meth)acrylic acid adduct, epichlorohydrin-modified phthalic acid-(meth)acrylic acid adduct, epichlorohydrin-modified hexahydrophthalic acid-(meth)acrylic acid adduct, ethylene glycol diglycidyl ether-(meth)acrylic acid adduct, polyethylene glycol diglycidyl ether-(meth)acrylic acid adduct, propylene glycol diglycidyl ether-(meth)acrylic acid adduct, polypropylene glycol diglycidyl ether-(meth)acrylic acid adduct, phenol novolac type epoxy resin-(meth)acrylic acid adduct, cresol novolac type epoxy resin-(meth)acrylic acid adduct, and other epoxy resin-(meth)acrylic acid adducts.

[0182] Examples of the (meth)acryloyl-modified resin oligomer include (meth)acryloyl-modified isocyanurate, (meth)acryloyl-modified polyurethane, (meth)acryloyl-modified polyester, (meth)acryloyl-modified melamine, (meth)acryloyl-modified silicone, (meth)acryloyl-modified polybutadiene, and (meth)acryloyl-modified rosin. Examples of vinyl include styrene, α-methylstyrene, vinyl acetate, vinyl (meth)acrylate, and allyl (meth)acrylate.

[0183] Examples of vinyl ethers include hydroxyethyl vinyl ether, ethylene glycol divinyl ether, and pentaerythritol trivinyl ether. Examples of the amide include (meth)acrylamide, N-hydroxymethyl(meth)acrylamide, and N-vinylformamide.

[0184] The content of the polymerizable compound is preferably from 1% by mass to 30% by mass, more preferably from 3% by mass to 25% by mass, and even more preferably from 5% by mass to 20% by mass, based on the non-volatile content of the coloring composition. The above-mentioned polymerizable compounds may be used alone or in combination of two or more kinds. In addition, when the coloring composition is used in combination with a photolithography method, it is preferable that the coloring composition contains the above-mentioned polymerizable compound, but when the coloring composition is used in combination with a dry etching method, it is preferable that the coloring composition does not contain the above-mentioned polymerizable compound. <<Photopolymerization initiator>> The photopolymerization initiator is as described above.

[0185] The pigment used in the preparation of the coloring composition is preferably a compound having an aromatic ring, from the viewpoint of enhancing the spectral characteristics and refractive index corresponding to the solid-state imaging device 2. The pigments used in the preparation of the colored composition may be used alone or in combination of two or more kinds to increase color purity. The preferred ratio when two or more pigments are used in combination is as described above.

[0186] Red pigments include, for example, CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 12, 14, 15, 16, 17, 21, 22, 23, 31, 32, 37, 38, 41, 47, 48, 48:1, 48:2, 48:3, 48:4, 49, 49:1, 49:2, 50:1, 52:1, 52:2, 53, 53:1, 53:2, 53:3, 57, 57:1, 57:2, 58:4, 60, 63, 63: 1, 63:2, 64, 64:1, 68, 69, 81, 81:1, 81:2, 81:3, 81:4, 83, 88, 90:1, 101, 101:1, 104, 108, 108:1, 109, 112, 113, 114, 122, 123, 144, 146, 147, 149, 151, 166, 168, 169, 170, 172, 173, 174, 175, 176, 177, 178, 179, 180, 181, 182, 183, 184, 185, 186, 187, 188, 189, 190, 191, 192, 193, 194, 195, 196, 197, 198, 199, 200, 201, 202, 203, 204, 205, 206, 207, 208, 209, 210, 211, 212, 213, 214, 215, 216, 217, 218, 219, 220, 221, 222, 223, 224, 226, 227, 228, 229, 230, 231, 232, 233, 234, 235, 236, 237, 238, 239, 24 6, 177, 178, 179, 181, 184, 185, 187, 188, 190, 193, 194, 200, 202, 206, 207, 208, 209, 210, 214, 216, 220, 221, 224, 230, 231, 232, 233, 235, 236, 237, 238, 239, 242, 243, 245, 247, 249, 250, 25 1, 253, 254, 255, 256, 257, 258, 259, 260, 262, 263, 264, 265, 266, 267, 268, 269, 270, 271, 272, 273, 274, 275, 276, 277, 278, 279, 280, 281, 282, 283, 284, 285, 286, 287, 291, 295, 296, etc. Among these, CI Pigment Red 177, 254, 269, which are pigments having an aromatic ring, are preferred as red pigments because of their excellent refractive index, light resistance, heat resistance, and transparency.

[0187] Yellow pigments include, for example, CI Pigment Yellow 1, 2, 3, 4, 5, 6, 10, 12, 13, 14, 15, 16, 17, 18, 24, 31, 32, 34, 35, 35:1, 36, 36:1, 37, 37:1, 40, 42, 43, 53, 55, 60, 61, 62, 63, 65, 73, 74, 77, 81, 83, 93, 94, 95, 97, 98, 100, 101, 104, 106, 108, 109, 110, 113, 114, 115, 116, 117, 118, 119, 120, 1 23, 126, 127, 128, 129, 138, 139, 147, 150, 151, 152, 153, 154, 155, 156, 161, 162, 164, 166, 167, 168, 169, 170, 171, 172, 173, 174, 175, 176, 177, 179, 180, 181, 182, 185, 187, 188, 192, 193, 194, 196, 198, 199, 213, 214, 231, 233, etc. Among these, as the yellow pigment, CI Pigment Yellow 138, 139, 150, 185, 231, 233, which is a pigment having an aromatic ring, is preferable. Furthermore, it is particularly preferable to include CI Pigment Yellow 139 and 185 because of their high refractive index.

[0188] As the green pigment, for example, CI Pigment Green 7, 36, 37, 58, 59, 62, 63, etc. are preferable. In addition, it is preferable to use these green pigments in combination with a yellow pigment, for example, CI Pigment Yellow 83, CI Pigment Yellow 138, CI Pigment Yellow 139, CI Pigment Yellow 150, CI Pigment Yellow 180, or CI Pigment Yellow 185.

[0189] As the blue pigment, a phthalocyanine pigment can be used alone or in combination with a dioxazine purple pigment. As the blue pigment, for example, it is preferable to use CI Pigment Blue 15:6 and CI Pigment Violet 23 in combination.

[0190] The content of the pigment in the non-volatile content of the coloring composition is preferably 50% by mass or more and 95% by mass or less, and more preferably 60% by mass or more and 90% by mass or less. If the content of the pigment is within the above range, the refractive index of the filter unit 215 is further improved.

[0191] The coloring composition forming the filter unit 215 preferably contains 50% by mass or more and 95% by mass or less of pigment and 3% by mass or less and 50% by mass or less of resin in the non-volatile content. The pigment content is more preferably 60% by mass or more and 93% by mass or less, and even more preferably 65% ​​by mass or more and 90% by mass or less. The resin content is more preferably 7% by mass or more and 50% by mass or less, and even more preferably 10% by mass or more and 40% by mass or less. The coloring composition preferably contains 80% by mass or more, and more preferably 90% by mass or more, of a compound containing an aromatic ring in the non-volatile content thereof. Compounds containing an aromatic ring include resins, pigments, dye derivatives, and other additives.

[0192] When the filter unit 215 is formed by dry etching using a coloring composition, it is preferable to use a composition containing a pigment, a dispersion resin, etc. The dispersion resin preferably contains a thermal crosslinkable group. Similarly, when the filter unit 215 is formed by photolithography, a composition containing a pigment, a dispersing resin, an alkali-soluble resin, a photopolymerization initiator, a polymerizable compound, and the like is preferable.

[0193] Of the coloring compositions described above, the green composition contains as pigments a green pigment selected from CI Pigment Green 36, CI Pigment Green 58, and CI Pigment Green 63, and a yellow pigment selected from CI Pigment Yellow 150, CI Pigment Yellow 138, CI Pigment Yellow 231, and CI Pigment Yellow 185, and when a sample with a thickness of 0.6 μm is prepared, it is preferable that the absorbance at a maximum absorption wavelength of 400 to 500 nm is 1 or more, and the absorbance at a maximum absorption wavelength of 600 to 700 nm is 1 or more.

[0194] From the viewpoint of increasing the refractive index of the color filter 215, a filler having a high refractive index (for example, titanium dioxide particles) may be added to the coloring composition. In this case, if the amount of filler added is large, the coloring degree of the color filter decreases, and the function as a color filter is impaired. On the other hand, if the amount of filler added is small, the refractive index of the color filter cannot be increased, and the sensitivity characteristics of the solid-state imaging element deteriorate. In particular, when the solid-state imaging element is made thinner (the color filter is made thinner), the above-mentioned disadvantages become more prominent. That is, when a filler is used, it is difficult to increase the refractive index while maintaining the coloring degree of the color filter. Therefore, a color filter made using a coloring composition to which a filler is added cannot satisfy the above-mentioned characteristics.

[0195] In contrast, in the present invention, a dispersion resin having a high refractive index is used, so that it is not necessary to use a filler, or even if a filler is used, only a small amount is required, thereby making it possible to prevent the above-mentioned inconveniences. In the present invention, the addition of a filler to the colored composition is not excluded, so long as the degree of coloring of the color filter can be maintained and the refractive index can be increased.

[0196] Although the dispersion resin, the coloring composition for color filters, the color filter, and the solid-state imaging device have been described above, the present invention is not limited thereto. For example, the dispersion resin, the coloring composition for color filters, the color filter, and the solid-state imaging device of the present invention may be replaced with any configuration that exhibits the same function, or may be added with a configuration that exhibits any desired function. The dispersion resin of the present specification can also be used for applications such as inkjet inks and resin molded products. The camera module 100 can be mounted on electronic devices such as smartphones, digital cameras, tablets, and personal computers. The solid-state imaging element 2 may be directly built into the electronic device. In this case, the electronic device corresponds to the electronic device of the present invention.

[0197] Furthermore, it may be provided in the following aspects:

[0198] (1) A dispersion resin to be mixed with a pigment, the dispersion resin comprising a first portion having affinity for the pigment and a second portion functioning to prevent aggregation of the pigment particles, the dispersion resin having a refractive index of 1.54 or more at a wavelength of 594 nm.

[0199] (2) The dispersion resin according to (1) above, wherein the dispersion resin contains an aromatic ring, and the proportion of the aromatic ring in the total mass of the dispersion resin is 25 mass% or more.

[0200] (3) The dispersion resin according to (2) above, wherein the dispersion resin mainly contains the aromatic ring in the second portion.

[0201] (4) The dispersion resin according to (2) or (3) above, wherein the dispersion resin is a graft copolymer in which the second portion branches out and extends from the first portion, or a block copolymer in which the first portion and the second portion are bonded together at their ends.

[0202] (5) The dispersion resin according to (4) above, wherein the graft copolymer includes an aromatic ring to which a total of three or more carboxyl groups or carboxyl group residues are directly bonded in the first site.

[0203] (6) The dispersion resin according to (4) or (5) above, wherein the graft copolymer is a polyester in which the constituent units of the first portion are linked by ester bonds.

[0204] (7) The dispersion resin according to any one of (4) to (6) above, wherein the second portion of the graft copolymer is a polymer portion of a monomer having an ethylenically unsaturated bond.

[0205] (8) The dispersion resin according to any one of the above (4) to (7), wherein the proportion of the second portion in the total mass of the graft copolymer is 50 mass % or more.

[0206] (9) The dispersion resin according to (4) above, wherein the block copolymer contains at least one group selected from the group consisting of a tertiary amino group and a quaternary ammonium group in the first portion.

[0207] (10) The dispersion resin according to (9) above, wherein the block copolymer has a polymer moiety of a monomer having an ethylenically unsaturated bond in both the first portion and the second portion.

[0208] (11) The dispersion resin according to (9) or (10) above, wherein the proportion of the second portion in the total mass of the block copolymer is 30 mass% or more.

[0209] (12) The dispersing resin according to any one of (1) to (11) above, wherein the dispersing resin has a weight average molecular weight of 5,000 or more and 50,000 or less.

[0210] (13) A coloring composition for color filters, comprising at least a pigment and the dispersing resin according to any one of (1) to (12) above.

[0211] (14) The coloring composition for color filters according to the above (13), further comprising a polymerizable compound and a photopolymerization initiator.

[0212] (15) In the coloring composition for color filters according to (13) or (14) above, the green composition as the coloring composition for color filters contains, as the pigments, a green pigment selected from CI Pigment Green 36, CI Pigment Green 58, and CI Pigment Green 63, and a yellow pigment selected from CI Pigment Yellow 150, CI Pigment Yellow 138, CI Pigment Yellow 231, and CI Pigment Yellow 185, and when a sample having a thickness of 0.6 μm is prepared, the absorbance at a maximum absorption wavelength of 400 to 500 nm is 1 or more, and the absorbance at a maximum absorption wavelength of 600 to 700 nm is 1 or more.

[0213] (16) A color filter comprising a plurality of filter units filled in at least a space partitioned by partitions and made of the coloring composition for color filters according to any one of (13) to (15) above.

[0214] (17) A solid-state imaging element comprising the color filter according to (16) above and a plurality of photodiodes that receive light that has passed through the color filter. Of course, this is not the case.

[0215] Finally, although various embodiments according to the present disclosure have been described, these are presented as examples and are not intended to limit the scope of the invention. The novel embodiment can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. The embodiments and their modifications are included within the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims. EXAMPLES

[0216] The present invention will be described below with reference to examples. However, the present invention is not limited to the examples. In the examples, "parts" means "parts by mass" and "%" means "% by mass".

[0217] First, methods for measuring the average primary particle size of the pigment, the dispersed particle size, the weight average molecular weight (Mw) of the dispersed resin, the acid value of the dispersed resin, and the non-volatile content of the dispersed resin will be described.

[0218] 1.Measurement method (Average primary particle size of pigment) The average primary particle size of the pigment was measured by a common method of directly measuring the size of the primary particles from a transmission electron microscope (TEM) photograph. Specifically, the minor axis and major axis diameters of each pigment primary particle were measured, and the average was taken as the particle size of the pigment particle. Next, for 100 or more pigment particles, the volume (weight) of each particle was calculated by approximating it to a rectangular parallelepiped of the calculated particle size, and the volume average particle size was taken as the average primary particle size.

[0219] (Dispersed particle size) Using Nikkiso's Microtrac UPA-EX150, which employs dynamic light scattering (FFT power spectrum method), particle permeability was set to absorption mode, particle shape to non-spherical, and D50 was rounded to 5 nm increments to obtain the average diameter. The solvents used for the dispersions were used as dilution solvents for the measurements, and the samples treated with ultrasound were measured immediately after sample preparation.

[0220] (Weight average molecular weight (Mw) of dispersion resin) The weight average molecular weight (Mw) of the dispersed resin is the weight average molecular weight in terms of polystyrene measured using a TSKgel column (manufactured by Tosoh Corporation) and a GPC (manufactured by Tosoh Corporation, HLC-8120GPC) equipped with an RI detector, using THF as the developing solvent.

[0221] (Acid value of dispersing resin) 80 mL of acetone and 10 mL of water were added to 0.5 g to 1 g of the dispersion resin solution, and the solution was stirred to dissolve uniformly. The acid value of the dispersion resin solution was measured by titrating the solution with an automatic titrator ("COM-555" manufactured by Hiranuma Sangyo Co., Ltd.) using a 0.1 mol / L KOH aqueous solution as the titrant. The acid value per non-volatile content of the dispersion resin was calculated from the acid value of the dispersion resin solution and the concentration of the non-volatile content of the dispersion resin solution.

[0222] The acid value (mgKOH / g) of the dispersed resin in a dry state was calculated using the following formula. Acid value (mgKOH / g) = {(5.611 × α × F) / S} / (non-volatile matter concentration / 100) Where S is the amount of sample taken (g) α: Consumption of 0.1 mol / L potassium hydroxide ethanol solution (mL) F: Potency of 0.1 mol / L potassium hydroxide in ethanol

[0223] (Non-volatile content of dispersed resin) The conditions for determining the non-volatile content of the dispersed resin were a sample mass of approximately 1 g, drying conditions of 200°C, and drying time of 10 minutes.

[0224] 2. Preparation of dispersion resin solution 2-1. Preparation of graft copolymer (Example 1: Preparation of a solution of dispersion resin X1) A reaction vessel equipped with a gas inlet tube, a thermometer, a condenser, and a stirrer was charged with 75.0 parts of benzyl methacrylate, 20.0 parts of benzyl acrylate, 5.0 parts of methacrylic acid, and 25.0 parts of propylene glycol monomethyl ether acetate (PGMAc), and the atmosphere was replaced with nitrogen gas. The inside of the reaction vessel was heated to 50° C. with stirring, and 6.0 parts of 3-mercapto-1,2-propanediol was added. The temperature inside the reaction vessel was raised to 90° C., and a solution of 0.1 parts of 2,2′-azobisisobutyronitrile in 45.7 parts of PGMAc was added and reacted for 7 hours. Measurement of the non-volatile content confirmed that 95% had reacted.

[0225] Next, 9.7 parts of pyromellitic dianhydride, 31.5 parts of PGMAc, and 0.2 parts of 1,8-diazabicyclo-[5.4.0]-7-undecene as a catalyst were added, and the mixture was reacted at 120°C for 5 hours. The mixture was sampled and the acid value was measured, and it was confirmed that 96% of the acid anhydride had reacted. Next, 9.0 g of 3-methoxybutanol was added, and the mixture was reacted at 120° C. for 3 hours. The reaction was terminated by sampling and measuring the acid value, and confirming that 98% or more of the acid anhydride had reacted. After cooling to room temperature, PGMAc was added so that the non-volatile content was 40% by mass, and a solution of dispersion resin X1 with an acid value of 98.5 mgKOH / g and a weight average molecular weight of 8500 was obtained.

[0226] (Examples 2 to 9, Comparative Examples 1 to 2: Preparation of Solutions of Dispersion Resins X2 to X9, and Comparative Dispersion Resins Y1 to Y2) Solutions of dispersion resins X2 to X9 and comparative dispersion resins Y1 to Y2 were obtained in the same manner as for the solution of dispersion resin X1, except that the raw materials and blending amounts were as shown in Table 1. The blending amounts in the table are in parts.

[0227] (Example 10: Preparation of dispersion resin X10 solution) A reaction vessel equipped with a gas inlet tube, a thermometer, a condenser, and a stirrer was charged with 95 parts of benzyl methacrylate, 5 parts of methacrylic acid, and 45.4 parts of PGMAc, and the atmosphere was replaced with nitrogen gas. The inside of the reaction vessel was heated to 70°C, 6 parts of 3-mercapto-1,2-propanediol was added, and 0.12 parts of AIBN (azobisisobutyronitrile) was further added, and the reaction was carried out for 12 hours. It was confirmed that 95% had reacted by measuring the non-volatile content. Next, 19.2 parts of trimellitic anhydride, 70.3 parts of PGMAc, and 0.20 parts of DBU (1,8-diazabicyclo-[5.4.0]-7-undecene) as a catalyst were added, and the reaction was carried out for 7 hours at 120° C. The reaction was terminated when it was confirmed by measuring the acid value that 98% or more of the acid anhydride had been half-esterified. PGMAc was added to adjust the non-volatile content to 40%. In this manner, a dispersion resin X10 solution having an acid value of 90, a weight average molecular weight of 9000, a poly(meth)acrylate skeleton, and an aromatic carboxy group was obtained.

[0228] (Example 11: Preparation of dispersion resin X11 solution) A reaction vessel equipped with a gas inlet tube, a thermometer, a condenser, and a stirrer was charged with 95 parts of benzyl methacrylate, 5 parts of methacrylic acid, and 45.4 parts of PGMAc, and the atmosphere was replaced with nitrogen gas. The inside of the reaction vessel was heated to 70°C, 2 parts of 3-mercapto-1,2-propanediol was added, and 0.12 parts of AIBN (azobisisobutyronitrile) was further added, and the reaction was carried out for 12 hours. It was confirmed that 95% had reacted by measuring the non-volatile content. Next, 3.2 parts of pyromellitic anhydride, 70.3 parts of PGMAc, and 0.20 parts of DBU (1,8-diazabicyclo-[5.4.0]-7-undecene) as a catalyst were added, and the reaction was carried out for 7 hours at 120° C. The reaction was terminated when it was confirmed by measuring the acid value that 98% or more of the acid anhydride had been half-esterified. PGMAc was added to adjust the non-volatile content to 40%. In this manner, a dispersion resin X11 solution was obtained, which had an acid value of 47, a weight average molecular weight of 18,000, a poly(meth)acrylate skeleton, and an aromatic carboxy group.

[0229] (Example 12: Preparation of dispersion resin X12 solution) A reaction vessel equipped with a gas inlet tube, a thermometer, a condenser, and a stirrer was charged with 100 parts of benzyl methacrylate and 25.0 parts of PGMAc, and the atmosphere was replaced with nitrogen gas. The inside of the reaction vessel was heated to 50°C, and 6.0 parts of 3-mercapto-1,2-propanediol was added. The temperature was raised to 90°C, and a solution of 0.1 parts of 2,2'-azobisisobutyronitrile dissolved in 45.7 parts of PGMAc was added, and the reaction was carried out for 10 hours. It was confirmed that 95% had reacted by measuring the non-volatile content. Next, 14.5 parts of pyromellitic dianhydride (manufactured by Daicel Chemical Industries, Ltd.), 38.0 parts of PGMAc, and 0.2 parts of 1,8-diazabicyclo-[5.4.0]-7-undecene as a catalyst were added, and the mixture was reacted at 120° C. for 5 hours. Then, 12.1 g of 3-methoxybutanol was added, and the mixture was reacted at 120° C. for 3 hours. The reaction was terminated when it was confirmed by measuring the acid value that 98% or more of the acid anhydride had been half-esterified. After the reaction was completed, PGMAc was added so that the non-volatile content became 40% by mass, and a dispersion resin X12 solution having an acid value of 95 mgKOH / g and a weight average molecular weight of 9,500 was obtained.

[0230] (Example 13: Preparation of dispersion resin X13 solution) A reaction vessel equipped with a gas inlet tube, a thermometer, a condenser, and a stirrer was charged with 10 parts of OXE-30 ((3-ethyloxetan-3-yl)methyl methacrylate) manufactured by Osaka Organic Chemical Industry Co., Ltd., 5 parts of methacrylic acid, 20 parts of t-butyl methacrylate, 65 parts of benzyl methacrylate, and 45.4 parts of PGMAc, and the atmosphere was replaced with nitrogen gas. The inside of the reaction vessel was heated to 70°C, 6 parts of 3-mercapto-1,2-propanediol was added, and 0.12 parts of AIBN (azobisisobutyronitrile) was further added, and the reaction was carried out for 12 hours. It was confirmed that 95% had reacted by measuring the non-volatile content. Next, 9.7 parts of pyromellitic anhydride, 70.3 parts of PGMAc, and 0.20 parts of DBU (1,8-diazabicyclo-[5.4.0]-7-undecene) as a catalyst were added, and the reaction was carried out for 7 hours at 120° C. The reaction was terminated when it was confirmed by measuring the acid value that 98% or more of the acid anhydride had been half-esterified. PGMAc was added to adjust the non-volatile content to 40%. In this way, a dispersion resin X13 solution was obtained, which had an acid value of 75 mgKOH / g, a weight average molecular weight of 9000, a poly(meth)acrylate skeleton, and an aromatic carboxy group.

[0231] [Table 1]

[0232] [Table 2]

[0233] The abbreviations in the table are as follows: BzMA: benzyl methacrylate BzA: benzyl acrylate MMA: Methyl methacrylate EA: Ethyl acrylate MAA: Methacrylic acid t-BA: tert-butyl acrylate 2MTA: 2-Methoxyethyl acrylate 4ClSt: 4-chlorostyrene MPD: 3-mercapto-1,2-propanediol RUVA93: Polymerizable UV absorber (Otsuka Chemical Co., Ltd.)

[0234] AIBN: 2,2'-azobisisobutyronitrile PGMAc: Propylene glycol monomethyl ether acetate PMA: Pyromellitic dianhydride TMA: Trimellitic anhydride DBU: 1,8-diazabicyclo-[5.4.0]-7-undecene 3MB: 3-Methoxybutanol PGME: Propylene glycol monomethyl ether DAA: Diacetone alcohol HPMA: Hydroxypropyl methacrylate MOI: 2-methacryloyloxyethyl isocyanate (Karens MOI, manufactured by Showa Denko)

[0235] (Example 14: Preparation of dispersion resin X14 solution) In a reaction vessel equipped with a gas inlet tube, a thermometer, a condenser, and a stirrer, 6 parts of 1-thioglycerol, 9.7 parts of pyromellitic anhydride, 36.9 parts of PGMAc (methoxypropyl acetate), and 0.2 parts of DBU (1,8-diazabicyclo-[5.4.0]-7-undecene) were charged, and after replacing with nitrogen gas, the reaction was carried out at 120°C for 5 hours (first step). It was confirmed by measuring the acid value that 95% or more of the acid anhydride was half-esterified. Next, 20 parts of 2-hydroxypropyl methacrylate, 75 parts of benzyl methacrylate, 5 parts of methacrylic acid, and 66.3 parts of PGMAc were charged, the inside of the reaction vessel was heated to 80°C, 0.12 parts of 2,2'-azobis(2,4-dimethylvaleronitrile) was added, and the reaction was carried out for 12 hours (second step). It was confirmed that 95% had reacted by measuring the non-volatile content. Finally, 21.6 parts of 2-methacryloyloxyethyl isocyanate (MOI) and 0.1 parts of hydroquinone were added, and the reaction was carried out until disappearance of the peak at 2270 cm −1 due to the isocyanate group was confirmed by IR (third step). After the peak disappearance was confirmed, the reaction solution was cooled and the non-volatile content was adjusted with PGMAc to obtain a dispersion resin X13 solution with a non-volatile content of 40%. The acid value of the obtained dispersant was 68, the unsaturated double bond equivalent was 1593, and the weight average molecular weight was 10000. In addition, since the dispersion resin X14 has a methacryloyl group, it has thermosetting and photosetting properties.

[0236] (Example 15: Preparation of dispersion resin X15 solution) In a reaction vessel equipped with a gas inlet tube, a thermometer, a condenser, and a stirrer, 6 parts of 3-mercapto-1,2-propanediol, 14.5 parts of PMA, and 70.8 parts of PGMAc were charged and replaced with nitrogen gas. The inside of the reaction vessel was heated to 100 ° C and reacted for 5 hours. Then, 12.1 g of 3-methoxybutanol was added and reacted at 120 ° C for 3 hours. After confirming that 98% or more of the acid anhydride was half-esterified by measuring the acid value, the temperature in the system was cooled to 70 ° C, 100 parts of benzyl methacrylate was charged, and 38.0 parts of PGMAc in which 0.1 parts of 2,2'-azobisisobutyronitrile was dissolved was added and reacted for 10 hours. The reaction was terminated when it was confirmed that the polymerization had progressed to 95% by measuring the non-volatile content. After the reaction was completed, PGMAc was added so that the non-volatile content became 40% by mass, and a dispersion resin X15 solution having an acid value of 93 mgKOH / g and a weight average molecular weight of 10,800 was obtained.

[0237] (Example 16: Preparation of Dispersion Resin X16 Solution) A reaction vessel equipped with a gas inlet tube, a thermometer, a condenser, and a stirrer was charged with 12 parts of 3-mercapto-1,2-propanediol, 12 parts of PMA, 11 parts of trimellitic anhydride, and 35 parts of PGMAc, and the atmosphere was replaced with nitrogen gas. The inside of the reaction vessel was heated to 100°C and reacted for 7 hours. After confirming that 98% or more of the acid anhydride had been half-esterified by measuring the acid value, the temperature in the system was cooled to 70°C, and 160 parts of benzyl methacrylate, 20 parts of hydroxyethyl methacrylate, and 20 parts of 2-hydroxypropyl methacrylate were charged, and 200 parts of a PGMAc solution in which 0.5 parts of 2,2'-azobisisobutyronitrile had been dissolved was added, and the reaction was continued for 10 hours. It was confirmed that the polymerization had progressed to 95% by measuring the non-volatile content, and the reaction was terminated. PGMAc was added to adjust the non-volatile content to 40%, to obtain a dispersion resin X16 solution having an acid value of 53 and a weight average molecular weight of 10,000.

[0238] (Example 17: Preparation of dispersion resin X17 solution) A reaction vessel equipped with a gas inlet tube, a thermometer, a condenser, and a stirrer was charged with 12 parts of 3-mercapto-1,2-propanediol, 15 parts of PMA, 11 parts of neopentyl glycol, 14 parts of trimellitic anhydride, and 52 parts of PGMAc, and the atmosphere was replaced with nitrogen gas. The inside of the reaction vessel was heated to 100°C and reacted for 7 hours. After confirming that 98% or more of the acid anhydride had been half-esterified by measuring the acid value, the temperature in the system was cooled to 70°C, and 180 parts of benzyl methacrylate and 20 parts of 2-hydroxypropyl methacrylate were charged, and 200 parts of a PGMAc solution in which 0.5 parts of 2,2'-azobisisobutyronitrile had been dissolved was added, and the reaction was continued for 10 hours. It was confirmed that the polymerization had progressed to 95% by measuring the non-volatile content, and the reaction was terminated. PGMAc was added to adjust the non-volatile content to 40%, and a dispersion resin X17 solution having an acid value of 63 and a weight average molecular weight of 9,000 was obtained.

[0239] [Table 3]

[0240] 2-2. Production of block copolymers (Example 18: Preparation of Dispersion Resin X18 Solution) In a reaction vessel equipped with a gas inlet tube, a condenser, a stirring blade, and a thermometer, 80 parts of benzyl methacrylate, 1.0 part of methyl 4-cyano-4-[(dodecylsulfanylthiocarbonyl)sulfanyl]pentanoate, and 80 parts of PGMAc were charged, and the mixture was heated and stirred to 70° C. while flowing nitrogen. 0.11 parts of dimethyl 2,2'-azobis(isobutyrate) was charged thereto to initiate polymerization of the first block. Six hours and eight hours after the start of polymerization, 0.01 parts of dimethyl 2,2'-azobis(isobutyrate) was added, and one hour later, the polymerization solution was sampled and the non-volatile content was measured. The polymerization conversion rate was confirmed to be 95% or more based on the non-volatile content, and the polymerization of the first block was completed.

[0241] Next, 20 parts of dimethylaminoethyl methacrylate and 23 parts of PGMAc were charged into the reaction tank and stirred while maintaining the temperature at 70°C under a nitrogen atmosphere, and 0.09 parts of dimethyl 2,2'-azobis(isobutyrate) were charged to initiate polymerization of block A. 2 hours and 3 hours after the start of polymerization, 0.01 parts of dimethyl 2,2'-azobis(isobutyrate) were charged, and then 1 hour later, a sample of the polymerization solution was taken and the non-volatile content was measured. It was confirmed that the polymerization conversion rate was 95% or more based on the non-volatile content, and the polymerization of the second block was completed. PGMAc was added to the block copolymer solution synthesized above so that the non-volatile content was 40% by mass. In this way, a dispersion resin X18 solution was obtained with an amine value per non-volatile content of 71.4 mgKOH / g, a weight average molecular weight of 20,000, and a non-volatile content of 40% by mass.

[0242] (Example 19: Preparation of Dispersion Resin X19 Solution) A reaction apparatus equipped with a gas inlet tube, a condenser, a stirring blade, and a thermometer was charged with 80 parts of benzyl methacrylate and 13.2 parts of tetramethylethylenediamine, and the mixture was stirred at 50° C. for 1 hour while flowing nitrogen, and the atmosphere in the system was replaced with nitrogen. Next, 9.3 parts of ethyl bromoisobutyrate, 5.6 parts of cuprous chloride, and 133 parts of PGMAc were charged, and the temperature was raised to 110°C under a nitrogen stream to initiate polymerization of the first block. After polymerization for 4 hours, a sample was taken from the polymerization solution and the nonvolatile content was measured, and it was confirmed that the polymerization conversion rate was 98% or more based on the nonvolatile content.

[0243] Next, 61 parts of PGMAc and 25.0 parts of an aqueous solution of methacryloyloxyethyl trimethylammonium chloride (Sanyo Chemical Industries, Ltd. "DMC-80", non-volatile content 80%) as a monomer for the second block were added to the reactor, and the reaction was continued by stirring while maintaining the temperature at 110°C under a nitrogen atmosphere. Two hours after adding the methacryloyloxyethyl trimethylammonium chloride, a sample of the polymerization solution was taken and the non-volatile content was measured. It was confirmed that the polymerization conversion rate of the second part was 98% or more based on the non-volatile content, and the reaction solution was cooled to room temperature to stop the polymerization. PGMAc was added to the block copolymer solution synthesized above so that the non-volatile content was 40% by weight. In this way, a dispersion resin X19 solution was obtained with a quaternary ammonium salt value per non-volatile content of 29.4 mg KOH / g and a weight average molecular weight of 9800 (Mw).

[0244] (Example 20: Preparation of Dispersion Resin X20 Solution) In a reaction vessel equipped with a gas inlet tube, a condenser, a stirring blade, and a thermometer, 60 parts of benzyl methacrylate, 1.0 part of methyl 4-cyano-4-[(dodecylsulfanylthiocarbonyl)sulfanyl]pentanoate, and 80 parts of PGMAc were charged, and the mixture was heated and stirred to 70° C. while flowing nitrogen. 0.11 parts of dimethyl 2,2'-azobis(isobutyrate) was charged thereto to initiate polymerization of the first block. Six hours and eight hours after the start of polymerization, 0.01 parts of dimethyl 2,2'-azobis(isobutyrate) was added, and one hour later, the polymerization solution was sampled and the non-volatile content was measured. The polymerization conversion rate was confirmed to be 95% or more based on the non-volatile content, and the polymerization of the first block was completed.

[0245] Next, 40 parts of dimethylaminoethyl methacrylate and 23 parts of PGMAc were charged into the reaction vessel and stirred while maintaining the temperature at 70° C. under a nitrogen atmosphere, and 0.09 parts of dimethyl 2,2′-azobis(isobutyrate) was charged to initiate polymerization of the second block. Two hours and three hours after the start of polymerization, 0.01 parts of dimethyl 2,2'-azobis(isobutyrate) was added, and one hour later, the polymerization solution was sampled and the non-volatile content was measured. The polymerization conversion rate was confirmed to be 95% or more based on the non-volatile content, and the polymerization of the second block was completed. In this way, a precursor solution of a block copolymer having an amine value of 145.0 mgKOH / g per nonvolatile content and a weight average molecular weight of 24,000 was obtained.

[0246] In addition, 2.0 parts of benzyl chloride was added to the reactor, and the temperature was kept at 70°C under a nitrogen atmosphere for 3 hours while stirring to form pigment-affinity sites. Then, the reactor was cooled. Finally, PGMAc was added so that the non-volatile content became 40% by mass. In this way, a dispersion resin X20 solution was obtained having an amine value per non-volatile content of 120 mg KOH / g, a quaternary ammonium salt value of 18.0 mg KOH / g, and a non-volatile content of 40 wt %.

[0247] [Table 4]

[0248] The abbreviations in the table are as follows: DM: Dimethylaminoethyl methacrylate DMCMA: Methacryloyloxyethyl trimethyl ammonium chloride BzCl: benzyl chloride

[0249] (Refractive index of dispersed resin) The obtained dispersed resin was coated onto a transparent substrate of 100 μm thick easy-adhesion treated polyester film ("Cosmoshine A4100" manufactured by Toyobo Co., Ltd.) using a No. 20 bar coater so that the dry thickness was 2.0 μm, and then dried at 100°C for 10 minutes to produce a test film. The refractive index at 594 nm of the obtained test film was measured using a Metricon Prism Coupler Model 2010 and evaluated according to the following criteria.

[0250] 〇: 1.55 or higher △: 1.53 or more and less than 1.55 ×: Less than 1.53

[0251] [Table 5]

[0252] 3. Preparation of Binder Resin Solution Into a separable 4-neck flask (reaction vessel) equipped with a thermometer, a cooling tube, a nitrogen gas inlet tube, and a stirrer, 70.0 parts of PGMAc was charged, the temperature was raised to 80° C., and the atmosphere inside the reaction vessel was replaced with nitrogen. Thereafter, a mixture of 13.3 parts of n-butyl methacrylate, 4.6 parts of 2-hydroxyethyl methacrylate, 4.3 parts of methacrylic acid, 7.4 parts of paracumylphenol ethylene oxide modified acrylate (manufactured by Toagosei Co., Ltd., "Aronix M110"), and 0.4 parts of 2,2'-azobisisobutyronitrile was added dropwise from the dropping tube over a period of 2 hours to carry out polymerization. After the dropwise addition, the reaction was continued for another 3 hours and then terminated. After cooling to room temperature, about 2 g of the solution was sampled and dried by heating at 180°C for 20 minutes to measure the non-volatile content. Then, PGMAc was added so that the non-volatile content was 20 mass%, and a binder resin solution, which is an alkali-soluble resin, was prepared. The weight average molecular weight (Mw) of the resin was 26,000.

[0253] 4. Manufacturing of pigment dispersion (Preparation of ingredients) ((Pigment)) · PR254 (CI Pigment Red 254): "Irgaphor Red B-CF" manufactured by BASF Japan PB15:6 (CI Pigment Blue 15:6): Toyo Color "LIONOL BLUE ESP-S" PG36 (CI Pigment Green 36): CLARIANT "Green8G" PG58 (CI Pigment Green 58): DIC "FASTOGEN GREEN A110"

[0254] ·PY138 (CIPigment Yellow 138): (BASF “Paliotol Yellow K 0961HD”) PY150 (CI Pigment Yellow 150 (CLARIANT "Hostaperm Yellow HN4G") ·PY185(CIPigment Yellow 185(BASF "Paliotol Yellow D 1155") ·PY139(CIPigment Yellow 139(BASF "Paliotol Yellow L 2146HD")

[0255] ((Dye Derivatives)) Dye derivative 1: [ka]

[0256] Dye derivative 2: [ka]

[0257] Dye derivative 3: [ka]

[0258] (Production of Pigment Dispersion 1) 11.7 parts of PR254, 1.3 parts of basic derivative 1, 17.5 parts of the solution of dispersion resin X1, and 78.25 parts of PGMAc were mixed and stirred until homogeneous. The resulting mixture was then dispersed for 3 hours in an Eiger mill (Eiger Japan, "Mini Model M-250MKII") using zirconia beads with a diameter of 0.5 mm. Thereafter, the obtained dispersion was filtered through a filter having a pore size of 5.0 μm to obtain Pigment Dispersion 1 having a nonvolatile content of 20 mass %.

[0259] (Production of pigment dispersions 2 to 26) Pigment Dispersions 2 to 26 were obtained in the same manner as Pigment Dispersion 1, except that the raw materials and amounts charged were as shown in Table 6.

[0260] [Table 6]

[0261] 5. Preparation of photosensitive coloring composition (Preparation of ingredients) (polymerizable compound) Mixture of dipentaerythritol pentaacrylate and dipentaerythritol hexaacrylate (manufactured by Toagosei Chemical Industry Co., Ltd., "Aronix M-402") (Photopolymerization initiator) Ethan-1-one, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl], 1-(O-acetyloxime) (BASF Japan, "Irgacure OXE02") (sensitizer) 4,4'-Bis(diethylamino)benzophenone (manufactured by Hodogaya Chemical Co., Ltd., "EAB-F")

[0262] Example 21 First, 60.0 parts of pigment dispersion 1, 1.0 part of polymerizable compound, 0.25 parts of photopolymerization initiator, 0.05 parts of sensitizer, and 38.7 parts of propylene glycol monomethyl ether acetate (PGMAc) were mixed and stirred to be homogeneous. Thereafter, the obtained mixture was filtered through a filter having a pore size of 1 μm to obtain a colored composition 1.

[0263] (Examples 22 to 47) The same procedure as in Example 21 was carried out except that the ingredients and amounts thereof were changed to those shown in Table 7, to obtain Examples 22 to 47, respectively.

[0264] [Table 7]

[0265] 6. Evaluation of Dispersing Resins and Coloring Compositions Each test was carried out in the following manner.

[0266] <Filterability> 60 g of the obtained colored composition was subjected to a pressure of 0.05 MPas for a certain period of time through a 1.5 μm disk filter (manufactured by Tomsic, "Titan 3 PTF E FILTER"), and the amount of liquid passing through the disk filter during that time was evaluated. The larger the amount of liquid, the better the filterability.

[0267] The filterability was evaluated according to the following criteria. ○: The amount of liquid that passed through the filter was 45g or more (good) △: The amount of liquid that passed through the filter was 30g or more but less than 45g (practical) ×: The amount of liquid that passed through the filter was less than 30g (defective)

[0268] <Viscosity stability> The viscosity stability of the obtained colored composition was evaluated by the following method. The initial viscosity on the day after the preparation of the colored composition and the viscosity after accelerated aging at 40°C for one week were measured using an E-type viscometer (Toki Sangyo Co., Ltd.'s "ELD type viscometer") at 25°C and a rotation speed of 50 rpm. From these initial viscosity and viscosity over time values, the rate of change in viscosity over time was calculated using the following formula. The obtained results were evaluated according to the following criteria. [Change rate of viscosity over time] = |([Initial viscosity] - [Viscosity over time]) / [Initial viscosity]| x 100 [Evaluation Criteria] ○: Change rate less than 5% (good) △: Change rate is 5% or more but less than 10% (practical) ×: Change rate 10% or more (bad)

[0269] <Foreign matter evaluation> The obtained colored composition was applied by spin coating onto a glass substrate on which a black matrix had been formed in advance, and then dried in a clean oven at 70° C. for 20 minutes. Then, the substrate was cooled to room temperature, and exposed to ultraviolet light through a photomask using an ultra-high pressure mercury lamp.Then, the substrate was spray-developed with a 0.2% by mass aqueous solution of sodium carbonate at 23°C for 30 seconds, washed with ion-exchanged water, and dried.Furthermore, the substrate was heat-treated at 230°C for 30 minutes in a clean oven to form a striped colored pixel layer on the substrate.The prepared colored pixel layer was heat-treated at 230°C for 30 minutes to obtain a test substrate having a thickness of 2.0 μm. The number of foreign particles in the colored pixels was counted using the obtained test substrate. The surface was observed using a metal microscope (Olympus Systems Corporation, "BX60") for evaluation. The magnification was set to 500 times, and the number of foreign particles observable in any five visual fields was counted in transmission.

[0270] Then, the foreign matter was evaluated according to the following evaluation criteria. [Evaluation Criteria] ◎: The number of foreign objects is less than 3 (very good) ○: The number of foreign objects is 3 or more and less than 20 (good) △: The number of foreign objects is 21 or more and less than 100 (practical) ×: 100 or more foreign objects (defective)

[0271] <Refractive index> The test substrate prepared in the above foreign matter evaluation was used to evaluate the refractive index using a Metricon Prism Coupler Model 2010.

[0272] <Resolubility> The obtained colored composition was applied to a glass substrate by spin coating and prebaked at 100° C. for 3 minutes to obtain a test substrate having a thickness of 2.0 μm. The obtained test substrate was immersed in PGMAc for 5 minutes. The state of dissolution was then visually observed and the solubility was evaluated according to the following criteria. ○: Dissolved (good) ×: Peeling (defective)

[0273] [Table 8]

[0274] From the results in Table 5, the dispersion resins of the Examples had a good refractive index, whereas the comparative dispersion resins of the Comparative Examples had a low refractive index. From the results in Table 8, the colored compositions of the examples were excellent in filterability, storage stability, foreign matter evaluation, resolubility, and refractive index. On the other hand, the colored compositions of the comparative examples had inferior refractive indices. [Explanation of symbols]

[0275] 100: Camera module B:Flexible wiring board C: Connector 1: Camera body 2: Solid-state imaging element 21: Light receiving board 210: Unit pixel 211: Substrate 212: Photodiode 213: Insulating film 215: Color filter 215R: Red filter unit 215G: Green filter unit 215B: Blue filter unit 216: Bulkhead 217: Microlens 2171: Convex curved surface 22: Bonded substrate 221: Substrate 222: Via 223: Connection terminal 23: Cover board 24: Spacer 3:Optical system 31: Housing 311 :Aperture 32: First convex lens 33: Second convex lens 34: Infrared cut filter 35: Joint 4:Joint part H: Height W: Width

Claims

1. A dispersion resin containing an aromatic ring, which is used in admixture with a pigment, a first portion having affinity for the pigment; and a second portion that functions to prevent aggregation of the pigment particles. a proportion of the aromatic ring in the mass of the second portion is 27 mass% or more, The dispersion resin has a refractive index of 1.54 or more at a wavelength of 594 nm.

2. The dispersion resin according to claim 1, A dispersion resin, wherein the proportion of the aromatic rings in the total mass of the dispersion resin is 25 mass % or more.

3. The dispersion resin according to claim 2, The dispersion resin mainly contains the aromatic ring in the second portion.

4. The dispersion resin according to claim 2, The dispersion resin is a graft copolymer in which the second portion branches out and extends from the first portion, or a block copolymer in which the first portion and the second portion are bonded end-to-end.

5. The dispersion resin according to claim 4, The graft copolymer is a dispersion resin comprising an aromatic ring having a total of three or more carboxyl groups or carboxyl group residues directly bonded to the first site.

6. The dispersion resin according to claim 4, The graft copolymer is a dispersion resin in which the constituent units of the first portion are polyesters linked by ester bonds.

7. The dispersion resin according to claim 4, The graft copolymer is a dispersion resin, wherein the second portion is a polymer portion of a monomer having an ethylenically unsaturated bond.

8. The dispersion resin according to claim 4, A dispersion resin, wherein the proportion of the second portion to the total mass of the graft copolymer is 50 mass % or more.

9. The dispersion resin according to claim 4, The block copolymer comprises at least one group selected from the group consisting of a tertiary amino group and a quaternary ammonium group in the first portion.

10. The dispersion resin according to claim 9, The block copolymer is a dispersion resin, wherein both the first portion and the second portion are polymer portions of a monomer having an ethylenically unsaturated bond.

11. The dispersion resin according to claim 9, A dispersion resin, wherein the proportion of the second portion to the total mass of the block copolymer is 30 mass % or more.

12. The dispersion resin according to claim 1, The dispersion resin has a weight average molecular weight of 5,000 or more and 50,000 or less.

13. A coloring composition for color filters, comprising: A coloring composition for color filters, comprising at least a pigment and the dispersion resin according to any one of claims 1 to 12.

14. The coloring composition for color filters according to claim 13, The coloring composition for color filters further comprises a polymerizable compound and a photopolymerization initiator.

15. The coloring composition for color filters according to claim 13, The green composition, which is a coloring composition for color filters, contains a green pigment selected from C.I. Pigment Green 36, C.I. Pigment Green 58, and C.I. Pigment Green 63 as the pigment, and a yellow pigment selected from C.I. Pigment Yellow 150, C.I. Pigment Yellow 138, C.I. Pigment Yellow 231, and C.I. Pigment Yellow 185, and when a sample having a thickness of 0.6 μm is prepared, the absorbance at a maximum absorption wavelength of 400 to 500 nm is 1 or more, and the absorbance at a maximum absorption wavelength of 600 to 700 nm is 1 or more. Coloring composition for color filters.

16. A color filter, A color filter comprising a plurality of filter units, the filter units being filled in at least a space partitioned by partition walls and made of the coloring composition for color filters according to claim 13.

17. A solid-state imaging device, A color filter according to claim 16; and a plurality of photodiodes that receive light that has passed through the color filters.

Citation Information

Patent Citations

  • Aqueous pigment dispersion for inkjet ink, and aqueous pigment ink for inkjet printer

    JP2012021120A

  • Coloring composition for color filter and color filter

    JP2013210452A

  • Coloring composition for color filter, and color filter

    JP2018132636A

  • Dispersant composition, coloring composition, and color filter

    JP2021063180A

  • Colored composition, photosensitive colored composition, color filter, and solid state imaging element

    JP2021183663A