Method for fixing carbon dioxide, hardened cement body with fixed carbon dioxide and method for manufacturing the same
The use of potassium carbonate solutions at high concentrations efficiently fixes carbon dioxide in hardened cement, addressing inefficiencies and leakage risks, achieving rapid and substantial carbon dioxide immobilization in cement structures.
Patent Information
- Application Number
- JP2023090129
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-05-31
AI Technical Summary
Existing methods for fixing carbon dioxide in hardened cement are inefficient and pose risks of leakage when high concentrations are used, and liquid-phase carbonation technologies have low fixation efficiency due to pH and carbonate ion concentration issues.
A method involving the use of an aqueous solution of potassium carbonate with a concentration of 15% by mass or more, applied through immersion or sprinkling, to fix carbon dioxide in hardened cement bodies, accompanied by a carbon dioxide gas absorption step to enhance fixation efficiency.
The method allows for rapid and efficient fixation of carbon dioxide, achieving immobilization equivalent to 30 kg or more per ton within a short curing time, typically less than 24 hours, with minimal risk of leakage.
Smart Images

Figure 0007586444000005 
Figure 0007586444000006 
Figure 0007586444000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for immobilizing carbon dioxide, a hardened cement product having carbon dioxide immobilized therein by the method, and a method for producing the same. [Background technology]
[0002] In order to prevent global warming, there is a call for decarbonization, which would essentially reduce emissions of carbon dioxide, a type of greenhouse gas, to zero. In order to achieve the goal of decarbonization, in addition to controlling carbon dioxide emissions, attention is also being paid to carbon dioxide fixation (carbon fixation) technology, which fixes emitted carbon dioxide in a solid or liquid form.
[0003] At construction sites, attempts are being made to fix carbon dioxide in concrete, which is an architectural or civil engineering structure. To fix carbon dioxide in concrete, a conventional technology is used that utilizes the carbonation / carbonation reaction in which carbon dioxide is supplied to hardened cement and calcium carbonate is produced from cement hydrates such as calcium hydroxide.
[0004] However, when the carbon dioxide concentration is low, it takes a long time to fix the carbon dioxide. If the carbon dioxide concentration is increased to shorten the fixation time, there is a risk that the carbon dioxide will leak into the atmosphere, and therefore a sealed curing facility is required (see Patent Document 1). For this reason, carbon dioxide fixation has not yet been widely put to practical use.
[0005] Meanwhile, liquid-phase carbonation technology is also being considered, in which carbon dioxide is fixed by supplying water that has absorbed carbon dioxide (carbonated water, carbonated nanobubble water, etc.) to the hardened cement body (see Non-Patent Document 1). However, dissolving a large amount of carbon dioxide in water lowers the pH and reduces the carbonate ion concentration, so the efficiency of fixing carbon dioxide is not very high. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2023-022383 A [Non-patent literature]
[0007] [Non-Patent Document 1] Shogo Katamura, Yosaku Ikeo, Yukiko Nishioka, and Hayato Takeuchi, "Modification of recycled fine aggregate by CO2 fixation and its effect on basic physical properties of mortar," Published by the Japan Concrete Institute, Proceedings of the Japan Concrete Institute Annual Conference, Vol. 44, No. 1, June 15, 2022, pp. 1186-1191 Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the present invention is to provide a method for immobilizing carbon dioxide, which can efficiently immobilize carbon dioxide in a hardened cement body, a carbon dioxide-immobilized hardened cement body in which carbon dioxide has been immobilized by the immobilization method, and a method for producing the same. [Means for solving the problem]
[0009] The above object can be achieved by the following embodiment of the present invention. That is, the embodiment of the present invention is as follows. <1> A method for fixing carbon dioxide, comprising: a carbonate supplying step of supplying to a hardened cement body an aqueous solution of at least one carbonate selected from the group consisting of sodium carbonate, sodium hydrogen carbonate, potassium carbonate and potassium hydrogen carbonate. <2> The aqueous solution contains potassium carbonate, and the concentration of potassium carbonate in the aqueous solution is 15% by mass or more. <1> The method for fixation of carbon dioxide according to claim 1. <3> The method for supplying the aqueous solution to the hardened cement body is a method for immersing the hardened cement body in the aqueous solution. <1> The method for fixation of carbon dioxide according to claim 1. <4> The method for supplying the aqueous solution to the hardened cement body is a method for spraying the aqueous solution onto the hardened cement body. <1> The method for fixation of carbon dioxide according to claim 1. <5> The amount of carbon dioxide equivalent fixed per ton at the site where carbon dioxide is fixed is 30 kg or more. <1> The method for fixation of carbon dioxide according to claim 1. <6> A carbon dioxide gas absorption step of absorbing carbon dioxide gas into an aqueous solution containing potassium ions to obtain an aqueous solution of potassium carbonate, The carbon dioxide gas absorption step is carried out prior to the carbonate supply step. <1> >A method for fixing carbon dioxide described in. <7> <1> ~ <6> 2. A hardened cement product having carbon dioxide immobilized therein, in whole or in part, by the method for immobilizing carbon dioxide according to any one of claims 1 to 11. <8> <1> ~ <6> 2. A method for producing a hardened cement product having fixed carbon dioxide, comprising a step of fixing carbon dioxide in whole or in part by the method for fixing carbon dioxide according to any one of the above items 1 to 11. Effect of the Invention
[0010] According to the present invention, it is possible to provide a carbon dioxide fixation method capable of efficiently fixating carbon dioxide in a hardened cement body, a carbon dioxide-fixed hardened cement body in which carbon dioxide is fixed by the fixation method, and a method for producing the same. [Brief description of the drawings]
[0011] [Figure 1] 1 is a graph showing the results of Example 1 and Comparative Example 1. [Diagram 2] 1 is a graph showing the results of Example 2. [Diagram 3] 1 is a graph showing the results of Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The method for fixing carbon dioxide according to the present embodiment includes a carbonate supplying step of supplying an aqueous solution of at least one carbonate selected from the group consisting of sodium carbonate, sodium hydrogen carbonate, potassium carbonate, and potassium hydrogen carbonate (hereinafter referred to as "supply liquid") to the hardened cement body. The method for producing the hardened cement body with fixed carbon dioxide according to the present embodiment also includes a step of fixing carbon dioxide in whole or in part by the method for fixing carbon dioxide according to the present embodiment. Hereinafter, a method for immobilizing carbon dioxide and a method for producing a carbon dioxide-immobilized hardened cement product according to one embodiment of the present invention will be described together.
[0013] [Carbonate supply process] (hardened cement paste) The hardened cement body used in this embodiment is an object for immobilizing carbon dioxide, and can be used without any particular limitation as long as it is an object in which cement is hardened. Specific examples of the hardened cement body used in this embodiment include hardened cement paste and mortar, concrete, recycled aggregate, and concrete sludge.
[0014] In this embodiment, the hardened cement product may be in any shape, such as powder, particles, blocks, rods, plates, blocks, walls, decorative shapes, fixed shapes, amorphous shapes, etc. Furthermore, the hardened cement product may be a part of some object or structure, or may be movable property or real estate.
[0015] (supply liquid) In this embodiment, the liquid to be supplied to the hardened cement body is an aqueous solution of sodium carbonate, sodium hydrogen carbonate, potassium carbonate, potassium hydrogen carbonate, or a mixture of two or more of these carbonates. These alkali metal (sodium, potassium) ions can capture a large amount of carbon dioxide gas (carbon dioxide), and therefore can contribute to the efficient fixation of carbon dioxide.
[0016] Among these, potassium can take in a larger amount of carbon dioxide gas, so the feed liquid is preferably an aqueous solution containing potassium carbonate or potassium hydrogen carbonate, more preferably an aqueous solution containing potassium carbonate, and even more preferably an aqueous solution of potassium carbonate. In addition, an aqueous solution of potassium carbonate exhibits high alkalinity of pH 11 or more even at a low concentration, so in this respect it is also preferred as a feed liquid to maintain a high alkalinity as described below.
[0017] To increase the efficiency of carbon dioxide fixation, it is preferable that the concentration of alkali metal carbonate (including alkali metal hydrogencarbonate; hereinafter the same applies to "alkali metal carbonate") in the supplied liquid is high, and specifically, it is preferably 1 mass% or more, more preferably 5 mass% or more, and even more preferably 10 mass% or more. Note that, when the hardened cement body supplied (contacted with the liquid) is wet or contains moisture, the concentration of alkali metal carbonate in the supplied liquid may be adjusted taking into account the moisture content.
[0018] In addition, potassium carbonate has a higher solubility in water than sodium carbonate and can be at a higher concentration, and the concentration of potassium carbonate in the supply liquid is preferably 15 mass % or more, more preferably 20 mass % or more, and even more preferably 25 mass % or more.
[0019] In this embodiment, the preparation of the supply liquid is not particularly limited, and the supply liquid may be obtained as an industrial product or by-product, or may be supplied from an external source such as another company or other person. In addition, potassium carbonate contained in plant ash, biomass ash, etc. may be dissolved in water to obtain a supply liquid containing a predetermined amount of carbonate ions and potassium ions. Alternatively, the supply liquid may be obtained by the operation of the carbon dioxide gas absorption process described later.
[0020] (Supply of liquid to hardened cement paste) In the carbonate supplying step, the method of supplying the supply liquid to the hardened cement body is not particularly limited as long as the supply liquid can be brought into contact with the hardened cement body.Specific examples of the method include a method of immersing the hardened cement body in the supply liquid, a method of spraying the hardened cement body with the supply liquid, and a method of permeating the hardened cement body with the supply liquid.
[0021] When the size of the hardened cement body is small, the method of immersing the hardened cement body in the supply liquid is preferred because carbon dioxide can be efficiently fixed by impregnating the hardened cement body from the entire surface of the hardened cement body. On the other hand, when the size of the hardened cement body is large, or when it is a part of some object or structure, or when it is real estate, the method of sprinkling the supply liquid on the hardened cement body is preferred. There are no particular limitations on the method of sprinkling the supply liquid on the hardened cement body, and examples of the method include pouring the supply liquid with a hose or the like, and spraying the supply liquid in the form of a shower or mist with a spray or mister.
[0022] When supplying the liquid to the hardened cement body, the impregnation may be promoted by applying pressure or pressure to efficiently impregnate the inside of the hardened cement body with the liquid.
[0023] The pH of the supply liquid supplied in this embodiment is preferably 9 or more, and more preferably 11 to 14. Since the supply liquid supplied in this embodiment has a high pH, crystalline basic calcium carbonate and calcium carbonate are produced after passing through a stage where amorphous calcium carbonate is produced. In addition, since the supply liquid has a high pH, carbon dioxide after immobilization can exist in the form of carbonate ions, and acidic deterioration and the like are less likely to occur.
[0024] By supplying (contacting) the supply liquid to the hardened cement body, amorphous calcium carbonate and basic calcium carbonate are efficiently produced, and carbon dioxide is efficiently fixed. Amorphous calcium carbonate and basic calcium carbonate are produced by the reaction between calcium ions originally contained in the hardened cement body and carbonate ions contained in the supply liquid, so the carbonate ions in the supply liquid are consumed, making it possible to stably fix carbon dioxide in the hardened cement body.
[0025] Fixation of carbon dioxide by supplying (contacting) a supply liquid to a hardened cement body is efficient and has a fast reaction, so that the time required for fixation (curing time, number of curing days) can be shortened. Although it depends on the supply method of the supply liquid (contacting method), the fixation reaction can proceed even with a curing time of about 24 hours. Therefore, the curing time can be set to a shorter time, for example, 18 hours, 12 hours, 8 hours, or 4 hours, which is shorter than 24 hours. Fixation by carbon dioxide takes several days or more until the fixation reaction proceeds to a certain extent, so according to this embodiment (fixation by supplying a supply liquid), the curing time (number of curing days) can be significantly shortened.
[0026] The temperature of the liquid to be supplied to the hardened cement body is not particularly limited, and may be room temperature (for example, 20°C to 30°C). Lower temperatures are also acceptable, but since too low a temperature reduces reactivity, the temperature is preferably 5°C or higher, and more preferably 10°C or higher. In addition, for example, when a high concentration of alkali metal carbonate is contained in a high temperature state, the liquid may be supplied (contacted with the liquid) while maintaining a temperature at which the concentration is maintained, and then the temperature may be maintained, or the liquid may be allowed to take its natural course.
[0027] Furthermore, the environmental temperature when supplying the liquid to the hardened cement body is not particularly limited and may be room temperature (for example, 20° C. to 30° C.). In the case of a method in which the hardened cement body is immersed in the liquid to be supplied, it is not easily affected by the environmental temperature, but in the case of a method in which the hardened cement body is sprayed with the liquid to be supplied, the temperature of the liquid to be supplied is affected by the environmental temperature after the water is sprayed. Therefore, if it is desired to maintain the temperature of the liquid to be supplied, it is preferable to keep the temperature of the liquid to be the same or close to the environmental temperature (for example, within ±10° C., preferably within ±5° C.).
[0028] [Carbon dioxide absorption process] The method for fixation of carbon dioxide according to this embodiment may include a carbon dioxide absorption step of absorbing carbon dioxide into an aqueous solution containing potassium ions to obtain an aqueous solution of potassium carbonate.
[0029] The carbon dioxide gas absorption step is carried out prior to the carbonate supply step, and the aqueous potassium carbonate solution obtained in the carbon dioxide gas absorption step is used as a supply liquid in the subsequent carbonate supply step.
[0030] Examples of the aqueous solution containing potassium ions include an aqueous solution of potassium hydroxide, an aqueous solution of potassium carbonate, and an aqueous solution of potassium hydrogen carbonate.
[0031] Regarding the operation of the carbon dioxide gas absorption step, a part of the operation known as the so-called "chemical absorption method," which is a carbon dioxide separation and recovery technique in which carbon dioxide contained in exhaust gas having a high carbon dioxide concentration is absorbed in an alkaline solution to separate and recover the carbon dioxide from other components, can be applied to this embodiment as the operation of the carbon dioxide gas absorption step.
[0032] In particular, the hot potassium carbonate absorption method, in which carbon dioxide is absorbed into an aqueous potassium carbonate solution, can be suitably applied as the operation of the carbon dioxide gas absorption step. Examples of the hot potassium carbonate absorption method include the Benfield method and the Catacarb (registered trademark) method. The operation and conditions of the carbon dioxide gas absorption step have been publicly known, and the publicly known steps and conditions can be applied to the present embodiment.
[0033] The carbon dioxide absorption step can be easily performed in a closed space. The subsequent carbonate supply step can also be performed in a closed space, and even if the carbonate supply step is performed in an open space, there is little risk of carbon dioxide escaping as carbon dioxide gas because the carbon dioxide is contained in the supply liquid. Therefore, according to the carbon dioxide fixation method of this embodiment, there is little risk of carbon dioxide escaping throughout all steps including the carbon dioxide absorption step. In contrast, fixation of carbon dioxide using carbon dioxide gas is not easy to perform in a closed space.
[0034] [Carbon dioxide fixation hardened cement] A carbon dioxide-immobilized hardened cement body can be efficiently manufactured by going through a process of immobilizing carbon dioxide in whole or in part by the carbon dioxide immobilization method according to the above embodiment. The carbon dioxide-immobilized hardened cement body manufactured in this manner can be used as a construction member. By using an object or structure in which carbon dioxide is immobilized as a construction member, carbon dioxide can be immobilized semi-permanently. In this embodiment, "construction member" means a part or whole of an architectural structure or civil engineering structure, or construction materials (architectural materials and civil engineering materials) used in an architectural structure or civil engineering structure.
[0035] When hardened cement paste, mortar, or concrete is used as the hardened cement product, it can be used as a construction material consisting of or partially containing these, and is environmentally friendly because carbon dioxide can be fixed in the construction material. Also, when recycled aggregate is used as the hardened cement product, it can be used as an aggregate (construction material) with excellent resource saving properties as a recycled product, and since carbon dioxide can be fixed in the aggregate, it is environmentally friendly because it also saves resources.
[0036] Furthermore, when concrete sludge is used as the hardened cement body, it can be reused as concrete materials such as fine aggregate and coarse aggregate, or recycled road base material (all of these are construction materials), and carbon dioxide can be fixed in the concrete materials and recycled road base material, making it environmentally friendly.
[0037] According to the method for fixing carbon dioxide in the present embodiment, carbon dioxide can be fixed efficiently in the hardened cement body, and therefore when this is used as a building material, a large amount of carbon dioxide can be fixed in the building material. For example, it is possible to provide a construction material in which the carbon dioxide equivalent of 30 kg or more per ton is fixed in the portion where the carbon dioxide is fixed, which was not easy to fix until now.
[0038] The term "carbon dioxide equivalent" refers to the amount of carbon dioxide equivalent to CO2 out of the total amount of carbonate fixed as CaCO3, and is generally referred to as the "fixed CO2 amount." The fixed CO2 amount can be measured, for example, by the method carried out in the examples described below.
[0039] The above-described embodiment merely shows a representative form of the present invention, and the present invention is not limited to the embodiment. In other words, a person skilled in the art can implement the present invention by modifying it in various ways in accordance with conventionally known knowledge without departing from the gist of the present invention. As long as the carbon dioxide fixation method of the present invention and the construction member in which carbon dioxide is fixed by the method of the present invention are still included in the scope of the present invention even after such modification. EXAMPLES
[0040] The present invention will be described below with reference to examples, but the present invention is not limited to the following examples. Note that the operations of Example 1 of [Test 1] and Example 2 of [Test 2] were carried out in parallel.
[0041] [Test 1] <Example 1> (1) Preparation of sample A (hardened cement paste) We prepared recycled fine aggregate L (compliant with JISA 5023 Appendix A), which is a recycled material to which hardened cement body to be fixed for carbon dioxide is attached.
[0042] Prior to the test, measurements were taken in accordance with "JISA 1109: Test method for density and water absorption of fine aggregates" and the surface dry density was 2.23 g / cm 3 , Bulk dry density is 1.99g / cm 3 The water absorption rate was 12.50% (JISA 5023 recycled fine aggregate L standard value: 13.0% or less), the fine particle content was 3.4% (same: 10.0% or less), and the grain size was 5 mm or less.
[0043] The prepared recycled fine aggregate L sample A was left in an air-dried state, and a portion of the sample was taken to measure the CO2 content (before the test) described below. The remaining sample A was divided into smaller portions, and 100 g or more (required amount per test) x 10 (5 curing time levels, n=2) were evenly sampled.
[0044] (2) Preparation of supply liquid A (potassium carbonate aqueous solution) 30 g of potassium carbonate was added to 100 ml of water and thoroughly stirred to dissolve the potassium carbonate, thereby preparing a 23 mass % aqueous solution of potassium carbonate as the supply liquid A.
[0045] (3) Supply of liquid A to sample A (carbonate supply process) Approximately 100g of sample A was immersed in 400g or more of supplied liquid A (20°C) and left to stand in an environment of 20°C and 60% RH. The curing (standing) time was set to 5 levels: 3 hours, 9 hours, 15 hours, 24 hours (1 day), and 72 hours (3 days), and tests were performed with n=2 for each. After the curing time had elapsed, supplied liquid A was removed with a dropper or the like, and sample A was taken out.
[0046] (4) Drying of sample A The collected sample A was immersed in acetone and left to stand for 6 hours or more to remove free water, and then evacuated in a vacuum drying oven for 6 hours or more to make it completely dry.
[0047] (5) Post-treatment of sample A For the sample A in a completely dry state, while appropriately reducing the sample size, it was pulverized to about 100 μm using a ball mill, and then vacuum-dried to obtain a sample for the analysis test. Until the analysis test was carried out, sample A was stored in a desiccator.
[0048] <Comparative Example 1> (1) Preparation of Sample B (cement hardened body) In the same manner as in “(1) Preparation of Sample A (cement hardened body)” in Example 1, sample B for Comparative Example 1 was prepared (including measurement of moisture content and CO2 content). However, the number of samples taken was 6 (3 levels of curing time, n = 2).
[0049] (2) Supply of carbon dioxide gas to Sample B (carbonation curing) Sample B was evenly spread on a vat of appropriate size, placed in a carbonation curing tank, and carbonation curing was started. The curing environment in the carbonation curing tank was set to a carbon dioxide concentration of 17%, 20 °C, and 60% RH. The curing (standing) time was set at 3 levels: 24 hours (1 day), 48 hours (2 days), and 72 hours (3 days), and each was tested with n = 2. After the curing time elapsed, sample B was taken out of the carbonation curing tank and appropriately reduced in size. At this time, a part of the sample was taken to measure the moisture content after curing.
[0050] (3) Treatment after curing In the same manner as in “(4) Drying of Sample A” and “(5) Post-treatment of Sample A” in Example 1, sample B was dried, post-treated, and stored in a desiccator.
[0051] <Measurement of CO2 fixation amount> For samples A and B after each test obtained in Example 1 and Comparative Example 1, the CO2 content (after the test) was measured. Including the CO2 content (before the test) performed before each test in Example 1 and Comparative Example 1, the CO2 content was measured by the “wet analysis method”. The wet analysis method is a method of measuring the CO2 content by decomposing the sample with hydrochloric acid, introducing the generated carbon dioxide into a barium chloride and sodium hydroxide solution for absorption, and titrating with a hydrochloric acid standard solution.
[0052] From the measurement results of the CO2 content (before the test) and the CO2 content (after the test), the amount of fixed CO2 was calculated according to the following formula (1).
[0053]
number
[0054] The terms in the above formula (1) are as follows: CO 2Fix : Amount of CO2 fixed [kg / t] CO2′: CO2 content (before test) [%] CO2: CO2 content (after test) [%]
[0055] Since the test was performed with n=2 for each curing period in Example 1 and Comparative Example 1, the average of the two measured values was taken as the amount of fixed CO2. The results of the amount of fixed CO2 are shown in Table 1 below and in the graph of Figure 1.
[0056] [Table 1] *The figures in the table are the amount of CO2 fixed (kg / t).
[0057] <Consideration of the results of Example 1 and Comparative Example 1> As can be seen from Table 1 above and the graph in FIG. 1, the amount of CO2 fixed in Comparative Example 1 (CO2 gas (concentration 17%)) was 16.3 kg / t after 24 hours of curing and 27.3 kg / t after 72 hours of curing, whereas in Example 1 (immersion in potassium carbonate aqueous solution (concentration 23%)) it was 34.5 kg / t after 24 hours of curing and 38.2 kg / t after 72 hours of curing, demonstrating that the efficiency of CO2 fixation in the potassium carbonate aqueous solution is extremely high.
[0058] In Example 1, even with a curing time of only 3 hours, the amount of CO2 fixed was 20.7 kg / t, which is greater than the 24-hour curing time in Comparative Example 1. This result shows that the reaction proceeds gradually in fixation using CO2 gas, whereas the reaction proceeds instantly in a short period of time in the case of the potassium carbonate aqueous solution.
[0059] In Example 1, the results of X-ray diffraction confirmed that CO2 was fixed and existed as calcium carbonate, which is a stable phase, in all samples of each curing time. In Comparative Example 1, the results of X-ray diffraction confirmed the generation of calcium carbonate, and it was confirmed that CO2 was fixed in the hardened cement body by the generation of calcium carbonate in the same manner as in the conventional neutralization / carbonation reaction in both Example 1 and Comparative Example 1.
[0060] [Test 2] <Example 2> (1) Preparation of sample C (hardened cement paste) Sample C for Example 2 was prepared (including measurements of water content and CO2 content) in the same manner as in "(1) Preparation of Sample A (hardened cement body)" in Example 1. However, the number of samples taken was 6 (3 levels of potassium carbonate concentration, n=2).
[0061] (2) Preparation of supply liquids B to D (potassium carbonate aqueous solution) Three aqueous solutions of potassium carbonate were prepared as supply liquid B (30 mass%), supply liquid C (40 mass%) and supply liquid D (53 mass%) by adding potassium carbonate in different amounts relative to water and thoroughly stirring to dissolve the potassium carbonate so that the potassium carbonate concentrations were 30 mass%, 40 mass% and 53 mass%. Note that the potassium carbonate concentration of 53 mass% is the concentration of a saturated aqueous potassium carbonate solution.
[0062] (3) Supply of liquids B to D to sample C (carbonate supply process) Approximately 100 g of sample C was immersed in 400 g or more of each of supply liquids B to D (20°C) in an environment of 20°C and 60% RH, and left to stand. The curing (standing) time was 24 hours (1 day), and the test was performed with n=2. After the curing time had elapsed, supply liquids B to D were each removed with a dropper or the like, and sample C was taken out. Hereinafter, sample C immersed in supply liquid B will be referred to as sample CB, sample C immersed in supply liquid C as sample CC, and sample C immersed in supply liquid D as sample CD.
[0063] (4) Post-treatment after health preservation In the same manner as “(4) Drying of Sample A” and “(5) Post-treatment of Sample A” in Example 1, Sample CB, Sample CC, and Sample CD were each dried, post-treated, and stored in a desiccator.
[0064] <Measurement of CO2 fixation amount> For the samples CB, CC, and CD after each test obtained in Example 2, the CO2 content rate (after the test) was measured in the same manner as in Example 1. From the measurement results of the obtained CO2 content rate (before the test) and CO2 content rate (after the test), the CO2 fixation amount was calculated in the same manner as in Example 1.
[0065] In Example 2, since the test was conducted with n = 2 for each potassium carbonate concentration, the average of the two measured values was taken as the CO2 fixation amount. The results of the obtained CO2 fixation amount are as shown in the graph of Table 2 and Figure 2 below. In addition, Table 2 and Figure 2 include the results of the curing time of 24 hours in Example 1 as data for a potassium carbonate concentration of 23%.
[0066]
Table 2
[0067] <Discussion on the results of Example 2> As can be seen from the graph of Table 2 and Figure 2 above, the higher the potassium carbonate concentration of the supply liquid, the higher the efficiency of CO2 immobilization, and the highest CO2 immobilization efficiency is achieved at a concentration of 53% by mass, which is the concentration of saturated potassium carbonate aqueous solution.
[0068] In addition, in Example 2, as a result of X-ray diffraction, it was confirmed that for samples with any potassium carbonate concentration, CO2 was immobilized and existed as calcite (calcium carbonate), which is a stable phase.
[0069] [Test 3] <Example 3> (1) Preparation of sample D (hardened cement paste) A sludge cake was prepared from concrete sludge extracted from the washing wastewater of a mixer truck. After dewatering and pressing, the moisture content of the sludge cake was 45.1% and the CaO content was 66.5%.
[0070] The sludge cake was crushed to 10 mm or less using a jaw crusher, and the particle size was adjusted to 1.2 to 5 mm by sieving to obtain a sand-like concrete sludge. The obtained concrete sludge was immersed in acetone and left to stand for 6 hours or more to remove free water. It was then evacuated in a vacuum drying furnace for 6 hours or more to make it completely dry, and concrete sludge sample D was prepared as a hardened cement body to be used for fixation of carbon dioxide.
[0071] A portion of the prepared sample D was collected and the CO2 content (before the test) was measured in the same manner as in Example 1. The remaining sample D was divided into smaller portions, and approximately 200 g (amount required per test, depending on the amount of sample that can be collected) x 8 (2 levels of K2CO3 concentration, 2 levels of curing days, n=2) were collected equally.
[0072] (2) Preparation of supply liquids E to G (potassium carbonate aqueous solution) Three aqueous solutions of potassium carbonate were prepared as feed liquid E (15 mass%), feed liquid F (27 mass%), and feed liquid G (53 mass%) by adding potassium carbonate to water while varying the amount of potassium carbonate relative to the water and stirring thoroughly to dissolve the potassium carbonate so that the potassium carbonate concentrations were 15 mass%, 27 mass%, and 53 mass%.
[0073] The supply liquid G obtained here is the same as the supply liquid D obtained in Example 2, and corresponds to a saturated potassium carbonate aqueous solution concentration. The potassium carbonate aqueous solution concentration of supply liquid F, 27% by mass, is a concentration set based on an amount corresponding to the amount of calcium in the concrete sludge, and the 15% by mass of supply liquid E is a concentration set based on half the amount corresponding to the amount of calcium in the concrete sludge.
[0074] (3) Supply of Feed Liquids E - G to Sample D (Carbonate Supply Step) In an environment of 20°C and 60% RH, approximately 200 g of Sample D was immersed and left standing in each of Feed Liquids E - G (at 20°C) of 1000 g or more. The curing (standing) days were set at two levels of 1 day and 3 days, and each was tested with n = 2. After the curing days had passed, Feed Liquids E - G were removed with a dropper or the like, and Sample D was taken out. Hereinafter, Sample D immersed in Feed Liquid E is denoted as Sample DE, Sample D immersed in Feed Liquid F is denoted as Sample DF, and Sample D immersed in Feed Liquid G is denoted as Sample DG.
[0075] (4) Post - treatment after Curing In the same manner as in “(4) Drying of Sample A” and “(5) Post - treatment of Sample A” in Example 1, Samples DE, DF, and DG were each dried, post - treated, and stored in a desiccator.
[0076] <Measurement of CO2 Fixation Amount> For Samples DE, DF, and DG after each test obtained in Example 3, the CO2 content rate (after the test) was measured in the same manner as in Example 1. From the measurement results of the obtained CO2 content rate (before the test) and CO2 content rate (after the test), the CO2 fixation amount was calculated in the same manner as in Example 1.
[0077] In Example 3, since the test was conducted with n = 2 for each potassium carbonate concentration and each curing day, the average of the two measured values was taken as the CO2 fixation amount. The results of the obtained CO2 fixation amount are as shown in the graph of Table 3 and Figure 3 below.
[0078]
Table 3
[0079] <Discussion of the Results of Example 3> As can be seen from Table 3 and the graph in Figure 3 above, at all potassium carbonate concentrations, a large amount of carbon dioxide, about 120 g / t, can be fixed in a short curing time (1 day). This is presumably because concrete sludge as a hardened cement body is porous and has a large specific surface area, and contains a large amount of calcium components derived from cement hydrates such as calcium hydroxide, so that carbon dioxide can be fixed efficiently even in a short curing time. When the curing time is extended further to 3 days, the higher potassium carbonate concentration is able to fix even more carbon dioxide, but the fixation efficiency decreases with the extended curing period compared to the initial curing period.
[0080] In Example 3, the results of X-ray diffraction confirmed that CO2 was fixed and existed as calcite (calcium carbonate), which is a stable phase, for samples with any potassium carbonate concentration or curing period.
Claims
1. A method for fixing carbon dioxide in a hardened cement body, comprising a carbonate supplying step of supplying to the hardened cement body an aqueous solution of at least one carbonate selected from the group consisting of sodium carbonate, sodium hydrogen carbonate, potassium carbonate and potassium hydrogen carbonate, wherein the aqueous solution has a pH of 11 to 14 (excluding the case where the hardened cement body is an existing concrete structure, and a hole having a predetermined length is opened from the surface of the existing concrete structure toward the inside, and the aqueous solution is supplied to the hole).
2. 2. The method for fixation of carbon dioxide according to claim 1, wherein the aqueous solution contains potassium carbonate, and the concentration of potassium carbonate in the aqueous solution is 15 mass % or more.
3. 2. The method for fixation of carbon dioxide according to claim 1, wherein the method for supplying the aqueous solution to the hardened cement body comprises immersing the hardened cement body in the aqueous solution.
4. 2. The method for fixation of carbon dioxide according to claim 1, wherein the method for supplying the aqueous solution to the hardened cement body comprises a method for spraying the aqueous solution onto the hardened cement body.
5. 2. The method for immobilizing carbon dioxide according to claim 1, wherein the amount of immobilized carbon dioxide per ton at the site where carbon dioxide is immobilized is 30 kg or more.
6. A carbon dioxide gas absorption step of absorbing carbon dioxide gas into an aqueous solution containing potassium ions to obtain an aqueous solution of potassium carbonate, 2. The method for fixation of carbon dioxide according to claim 1, wherein the carbon dioxide gas absorption step is carried out prior to the carbonate supply step.
7. 7. A hardened cement product having carbon dioxide immobilized therein, the hardened cement product having carbon dioxide immobilized therein in whole or in part by the method for immobilizing carbon dioxide according to any one of claims 1 to 6.
8. A method for producing a carbon dioxide-immobilized hardened cement body, comprising a step of immobilizing carbon dioxide in the whole or part of the hardened cement body by the method for immobilizing carbon dioxide according to any one of claims 1 to 6.
Citation Information
Patent Citations
Method for capturing and sequestering carbon dioxide using alkaline industrial waste
CN115515701A
Concrete and method for producing the same
JP2021155311A
Method for recovering cement paste from waste concrete
JP2022126254A
Hydraulic composition and manufacturing method thereof
JP2022153131A
Method for fixing carbon dioxide, and aggregate and concrete using carbon dioxide-fixed material
JP2023022383A