Cement composition and method for producing the cement composition
The cement composition enhances strength development by using specific ratios of gypsum and blast furnace slag powder, addressing emission reduction challenges and promoting hydration reactions.
Patent Information
- Application Number
- JP2020061812
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-31
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-03-31
AI Technical Summary
Existing cement compositions face challenges in achieving sufficient strength development while reducing carbon dioxide emissions, as increasing gypsum or blast furnace slag powder content can lead to reduced strength and increased emissions.
A cement composition comprising cement clinker powder, gypsum powder, and blast furnace slag powder, with specific ratios of limestone powder and gypsum powder to promote hydration reactions, and using waste gypsum board as a raw material to enhance strength development without increasing emissions.
The composition achieves high-strength cement mixtures by promoting hydration reactions and reducing carbon dioxide emissions through optimized powder ratios and use of waste materials.
Smart Images

Figure 0007586652000012 
Figure 0007586652000001 
Figure 0007586652000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a cement composition comprising a mixture containing cement clinker powder, gypsum powder, limestone powder and blast furnace slag powder, and a method for producing the cement composition. [Background technology]
[0002] A cement composition generally comprises a mixture containing cement clinker powder, gypsum powder, and admixture powder. The following Patent Document 1 (Example 13) discloses a cement composition using limestone powder and blast furnace slag powder as the admixture powder.
[0003] In recent years, in order to reduce the amount of carbon dioxide emitted from a cement calciner, it has been considered to reduce the amount of cement clinker produced in the cement calciner, reduce the content of cement clinker powder in the cement composition, and increase the content of gypsum powder or blast furnace slag powder. However, if the content of gypsum powder or blast furnace slag powder in the cement composition is increased in this way, there is a risk that the strength development of the cement composition will not be sufficiently high depending on the composition of the cement composition.
[0004] In order to sufficiently increase the strength development of the cement composition, it is possible to adjust the quality of the cement clinker (for example, the composition of each of the multiple minerals in the cement clinker) in the cement firing process. However, when such an adjustment is made, it becomes necessary to input more fuel into the cement kiln, and therefore there is a risk that the amount of carbon dioxide emissions from the cement firing apparatus will increase even if the amount of cement clinker produced in the cement firing apparatus is reduced. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2019-172497 A Summary of the Invention [Problem to be solved by the invention]
[0006] Therefore, an object of the present invention is to provide a cement composition comprising a mixture containing cement clinker powder, gypsum powder, limestone powder and blast furnace slag powder, in which the strength development of the cement composition is enhanced by the gypsum powder and blast furnace slag powder. [Means for solving the problem]
[0007] The first aspect of the present invention relates to a cement composition as follows. This cement composition is a mixture containing cement clinker powder, gypsum powder, limestone powder, and blast furnace slag powder. The limestone powder and the blast furnace slag powder are contained in the mixture in a total amount of 10.0 mass% or less. The gypsum powder is contained in the mixture in a ratio of 0.6 mass% to 2.4 mass% in terms of SO3.
[0008] According to the first item, the mixture contains limestone powder and blast furnace slag powder in a total amount of 10.0% by mass or less, and the mixture contains gypsum powder in a proportion of 2.4% by mass or less in terms of SO3, so that the mixture contains a small amount of gypsum powder and admixture powder (limestone powder and blast furnace slag powder). In addition, the mixture contains gypsum powder in a proportion of 0.6% by mass or more in terms of SO3. Therefore, when this mixture is kneaded with water, the hydration reaction of the blast furnace slag powder is effectively promoted by the SO3 contained in the gypsum powder, and a high-strength cement kneaded product can be produced. In other words, the cement composition according to the first item increases the strength development of the mixture due to the gypsum powder and blast furnace slag powder contained in the mixture.
[0009] The second aspect of the present invention includes the following in the first aspect. That is, the SO3 content of the cement clinker powder is 0.80 mass% or more (preferably 0.94 mass% or more). The gypsum powder is contained in the mixture at a rate of 1.4 mass% or more (preferably 1.6 mass% or more) calculated as SO3.
[0010] According to the second item, when the mixture is kneaded with water, the large amount of SO3 contained in the gypsum powder suppresses the rapid hydration (flash setting) of the aluminate in the cement clinker powder, and the aluminate contained in the cement clinker powder reacts with the limestone powder. As a result, a large amount of SO3 is eluted from the cement clinker powder, and the large amount of SO3 eluted from the cement clinker powder promotes the hydration of the blast furnace slag powder, producing a high-strength cement mixture. In other words, the cement composition according to the second item further enhances the strength development of the mixture due to the gypsum powder and blast furnace slag powder contained in the mixture.
[0011] The second item above does not specify the composition range of each of the multiple minerals in the cement clinker powder, but specifies the content of a single chemical component (SO3) in the cement clinker powder. The cement clinker that is the source of the cement clinker powder in the second item can be easily produced by using waste with a high SO3 content as a cement raw material in a cement calcination device, and can be produced without inputting a large amount of fuel into the cement kiln to adjust the quality of the cement clinker. Therefore, the second item above does not emit a large amount of carbon dioxide in the cement clinker production process.
[0012] The third aspect of the present invention includes the following content in the above-mentioned second aspect: In other words, the mixture of the third aspect does not contain cement clinker powder having an SO3 content of 0.56 mass% or less.
[0013] According to the third item, the mixture does not contain any cement clinker powder with an SO3 content of 0.56 mass% or less, so the proportion of cement clinker powder with an SO3 content of 0.80 mass% or more (content in the mixture) is relatively high. Here, cement clinker powder with an SO3 content of 0.56 mass% or less cannot elute an amount of SO3 sufficient to promote the hydration of blast furnace slag powder even when mixed with water. Therefore, the cement composition according to the third item has a high proportion of "cement clinker that promotes the hydration of blast furnace slag powder" relative to the total amount of cement clinker powder, and the strength development of the mixture is further enhanced by the gypsum powder and blast furnace slag powder contained in the mixture.
[0014] The fourth aspect of the present invention is any one of the first to third aspects including the following: That is, when SO3 contained in the cement clinker powder is defined as clinker SO3, SO3 contained in the gypsum powder is defined as gypsum SO3, the ratio of the clinker SO3 to the mixture is defined as S1 mass%, and the ratio of the gypsum SO3 to the mixture is defined as S2 mass%, the total value of the S1 mass% and the S2 mass% is 2.60 mass% or more (preferably 2.65 mass% or more), and the ratio of the S2 mass% to the S1 mass% is 1.40 or more and 3.00 or less (preferably 1.497 or more and 2.837 or less).
[0015] According to the fourth item, the mixture contains a large amount of clinker SO3 and a large amount of gypsum SO3 in a balanced manner. Therefore, when this mixture is mixed with water, gypsum SO3 is dissolved from the gypsum powder in the initial mixing stage, and clinker SO3 is dissolved from the cement clinker powder after the initial mixing stage has passed. As a result, during the mixing stage, SO3 is dissolved continuously and without interruption from the gypsum powder and the cement clinker powder, and this SO3 promotes the hydration of the blast furnace slag powder continuously and without interruption. In other words, the cement composition according to the fourth item further enhances the strength development of the mixture due to the gypsum powder and blast furnace slag powder contained in the mixture.
[0016] The fifth aspect of the present invention is any one of the first to fourth aspects, including the following: When the TiO2 content, MnO content, P2O5 content, Na2O content and K2O content of the cement clinker powder are defined as T mass%, M mass%, P mass%, N mass% and K mass%, respectively, the physical property value "(T+M+P) / (N+0.658×K)" of the cement clinker powder is 0.80 or more and 1.40 or less.
[0017] According to the fifth item, the cement clinker powder contains evenly the promoting elements (Na2O and K2O) that promote the dissolution of SO3 contained in the cement clinker powder to the outside of the cement clinker powder during hydration of the cement clinker powder, and the inhibiting elements (TiO2, MnO, and P2O5) that inhibit the dissolution. Therefore, when the cement composition is kneaded with water (when the cement clinker powder contained in this cement composition is hydrated), a large amount of SO3 is dissolved from the cement clinker powder by the promoting elements, and the inhibiting elements prevent the dissolution rate of SO3 from the cement clinker powder from becoming excessively fast, so that a large amount of SO3 contained in the cement clinker powder is gradually dissolved from the cement clinker powder over a long period of time. In other words, when the cement composition is kneaded with water, a large amount of SO3 dissolved from the cement clinker powder can be gradually reacted with the limestone powder and the blast furnace slag powder, so that a cement mixture that exhibits high strength and high fluidity for a long period of time can be produced.
[0018] A sixth aspect of the present invention relates to a method for producing a cement composition as follows. The method includes a finishing step and a mixing step. In the finishing step, cement clinker is ground together with gypsum to produce a mixed powder. In the mixing step, the mixed powder, limestone powder, and blast furnace slag powder are mixed to produce a cement composition. The limestone powder and the blast furnace slag powder are contained in the cement composition in a total amount of 10.0 mass% or less. The gypsum powder is contained in the cement composition in a proportion of 0.6 mass% or more and 2.4 mass% or less in terms of SO3.
[0019] According to the sixth item, the limestone powder and the blast furnace slag powder are contained in the cement composition at a total ratio of 10.0 mass% or less, and the gypsum powder is contained in the cement composition at a ratio of 2.4 mass% or less in terms of SO3, so that the cement composition contains a small amount of gypsum powder and admixture powder (limestone powder and blast furnace slag powder). In addition, the gypsum powder is contained in the cement composition at a ratio of 0.6 mass% or more in terms of SO3. Therefore, when this cement composition is mixed with water, the hydration reaction of the blast furnace slag powder is effectively promoted by the SO3 contained in the gypsum powder, and a high-strength cement mixture can be produced. In other words, according to the sixth item, a cement composition in which strength development is enhanced by the gypsum powder and the blast furnace slag powder can be produced.
[0020] A seventh aspect of the present invention is the method according to the sixth aspect, further comprising a calcination step, in which the cement clinker is produced using waste gypsum boards as a cement raw material.
[0021] According to the seventh item, the strength development of the cement composition can be improved by utilizing the SO3 contained in the waste gypsum board, and the waste gypsum board can be effectively used as a raw material for the cement composition. Effect of the Invention
[0022] As described above, according to the present invention, it is possible to provide a cement composition comprising a mixture containing cement clinker powder, gypsum powder, limestone powder, and blast furnace slag powder, in which the strength development of the cement composition is enhanced by the gypsum powder and blast furnace slag powder. [Brief description of the drawings]
[0023] [Figure 1] 1 is an overall configuration diagram showing a cement production apparatus for producing a cement composition according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] FIG. 1 is an overall configuration diagram showing a cement manufacturing apparatus 1 for manufacturing a cement composition according to an embodiment of the present invention. As shown in FIG. 1, the cement manufacturing apparatus 1 includes a clinker silo 2, a finishing mill 3, a classifier 4, a mixer 5, and a cement silo 6. The clinker silo 2 stores clinker (not shown) discharged from a cement calciner (not shown). The finishing mill 3 pulverizes the clinker C discharged from the clinker silo 2 together with gypsum G to produce a pulverized material D (mixed powder). The classifier 4 classifies the pulverized material D discharged from the finishing mill 3 and separates it into coarse powder R and fine powder F. The mixer 5 mixes the fine powder F discharged from the classifier 4 together with limestone powder L and blast furnace slag powder S to produce a mixture M (cement composition). The cement silo 6 stores the mixture M discharged from the mixer 5. The classifier 4 also returns the coarse powder R to the finishing mill 3. When the finishing mill 3 receives the coarse powder R returned from the classifier 4, the finishing mill 3 pulverizes the clinker C together with the gypsum G and the coarse powder R to produce a pulverized product D.
[0025] The cement composition according to one embodiment of the present invention is composed of a mixture M containing a powder of clinker C, a powder of gypsum G, a powder of limestone L, and a powder of blast furnace slag S. The powder of limestone L and the powder of blast furnace slag S are contained in the mixture M in a total amount of 10.0 mass% or less. The powder of gypsum G is contained in the mixture M in a ratio of 0.6 mass% or more and 2.4 mass% or less in terms of SO3. Preferably, the SO3 content of the powder of clinker C is 0.80 mass% or more (more preferably 0.94 mass% or more), and the powder of gypsum G is contained in the mixture M in a ratio of 1.4 mass% or more (more preferably 1.6 mass% or more) in terms of SO3. More preferably, the mixture M does not contain a cement clinker powder having a SO3 content of 0.56 mass% or less.
[0026] If the SO3 contained in the powder of clinker C is defined as clinker SO3, the SO3 contained in the powder of gypsum G is defined as gypsum SO3, the ratio of clinker SO3 to mixture M is defined as S1 mass%, and the ratio of gypsum SO3 to mixture M is defined as S2 mass%, then in a cement composition according to one embodiment of the present invention, it is preferable that the total value of S1 mass% and S2 mass% is 2.60 mass% or more (preferably 2.65 mass% or more) and the ratio (proportion) of S2 mass% to S1 mass% is 1.40 or more and 3.00 or less (more preferably 1.497 or more and 2.837 or less).
[0027] Preferably, when the TiO2 content, MnO content, P2O5 content, Na2O content and K2O content of the powder of Clinker C are defined as T mass%, M mass%, P mass%, N mass% and K mass%, respectively, the physical property value of the powder of Clinker C, "(T+M+P) / (N+0.658×K)", is 0.80 or more and 1.40 or less.
[0028] The method for producing a cement composition according to one embodiment of the present invention includes a finishing step (a grinding step using a finishing mill 3 shown in FIG. 1) and a mixing step (a mixing step using a mixing device 5 shown in FIG. 1). In the finishing step, cement clinker (clinker C shown in FIG. 1) is ground together with gypsum (gypsum G shown in FIG. 1) to produce a mixed powder (a mixed powder of clinker C and gypsum G contained in the ground product D shown in FIG. 1). In the mixing step, the mixed powder, limestone powder (limestone powder L shown in FIG. 1), and blast furnace slag powder (blast furnace slag powder S shown in FIG. 1) are mixed to produce a cement composition (mixture M shown in FIG. 1). The method for producing a cement composition according to the present invention is not limited to a method using the cement production apparatus 1 shown in FIG. 1.
[0029] The method for producing a cement composition according to one embodiment of the present invention may further include a firing step (a step of producing clinker C shown in FIG. 1 in the upstream stage of the production apparatus 1 shown in FIG. 1). In this case, in this firing step, cement clinker (clinker C shown in FIG. 1) is produced using waste gypsum boards (not shown) as a cement raw material.
[0030] In the above embodiment, instead of or together with supplying the limestone powder L to the mixer 5, limestone (not shown) may be supplied to the finishing mill 3 together with the clinker C and gypsum G.
[0031] Next, an experimental example of the cement composition according to one embodiment of the present invention will be described. In this experimental example, various cement compositions were produced by mixing cement clinker powder (Cli1 to Cli6), gypsum powder, and admixture powder (limestone powder and blast furnace slag powder) in various ratios, and the "compressive strength at 28 days" of the cement mixture produced from each of these cement compositions was measured. Tables 1 to 4 show the composition or physical properties of the raw materials of the cement compositions used in this experimental example for each raw material. Tables 5 to 10 show the relationship between the composition of the cement composition produced in this experimental example and the strength development for each experimental example. Table 11 shows the physical property values of the cement composition produced in this experimental example for each experimental example.
[0032] In Tables 1 to 10, "clinker" means cement clinker powder, "gypsum" means gypsum powder, "admixture" means admixture powder, "limestone" means limestone powder, and "blast furnace slag" means blast furnace slag powder.
[0033] Table 1 shows the content (mass%) of each compound in the cement clinker powder (corresponding to the powder of clinker C shown in Figure 1) used in the above experimental example. In Table 1, ig.loss (Ignition Loss) means ignition raw material (volatile substance). Na2Oeq means total alkali. Total alkali is a value calculated by the formula "Na2O+0.658×K2O". f.CaO means free calcium oxide. Free calcium oxide refers to calcium oxide that remains without reacting with silicon dioxide or aluminum oxide when cement raw materials are burned.
[0034] [Table 1]
[0035] Table 2 shows the modulus of the cement clinker powder used in the above experimental example. In Table 2, HM (Hydraulic Modulus) indicates the hydraulic modulus, SM (Silica Modulus) indicates the silica modulus, IM (Iron Modulus) indicates the iron modulus, and AI (Activity Index) indicates the activity index. HM is the ratio of CaO to (SiO2 + Al2O3 + Fe2O3). SM is the ratio of SiO2 to (Al2O3 + Fe2O3). IM is the ratio of Al2O3 to Fe2O3. AI is the ratio of SiO2 to Al2O3. As shown in Table 2, the modulus of the cement clinker powder used in the above experimental example is as follows: HM is 2.15 to 2.21, SM is 2.18 to 2.42, IM is 1.87 to 2.18, and AI is 3.19 to 3.70.
[0036] Table 2 also shows the mineral composition of the cement clinker powder used in the above experimental example. The mineral composition shown in Table 2 was calculated by the Bogue formula. In Table 2, C3S is tricalcium silicate (3CaO·SiO2), C2S is dicalcium silicate (2CaO·SiO2), C3A is tricalcium aluminate (3CaO·Al2O3), and C4AF is tetracalcium aluminate ferroaluminate (4CaO·Al2O3·Fe2O3). As shown in Table 2, the mineral composition of the cement clinker powder used in the above experimental example is as follows: C3S is 55.2 mass% or more and 62.0 mass% or less, C2S is 12.7 mass% or more and 18.6 mass% or less, C3A is 10.1 mass% or more and 12.2 mass% or less, and C4AF is 9.1 mass% or more and 9.6 mass% or less.
[0037] Furthermore, Table 2 shows the physical property values of the cement clinker powder used in the above experimental example. These physical property values indicate the ratio of the strength development inhibition index value to the strength development promotion index value in the cement clinker powder. This strength development promotion index value is the total alkali content in the cement clinker powder. This strength development inhibition index value is the total content (mass%) of TiO2, MnO, and P2O5 in the cement clinker powder. As shown in Table 2, the above physical property values of the cement clinker powder used in this experimental example are 0.853 or more and 1.326 or less.
[0038] [Table 2]
[0039] Table 3 shows the chemical compositions of the limestone powder and blast furnace slag powder used in the above experimental examples.
[0040] [Table 3]
[0041] Table 4 shows the specific surface area (Blaine specific surface area) and activity index of the limestone powder and blast furnace slag powder used in the above experimental examples. Here, the activity index is at the time when the material is 28 days old.
[0042] [Table 4]
[0043] Tables 5 to 10 show the type of cement clinker powder used in the cement compositions, the SO3-equivalent gypsum powder content (mass%), limestone powder content (mass%), blast furnace slag powder content (mass%), total admixture powder content (total content of limestone powder and blast furnace slag powder: mass%), and the "compressive strength at 28 days (N / mm2)" of the cement mixtures produced from the obtained cement compositions. 2 )" relationship.
[0044] In Table 5, the set of Experimental Examples A1 to A3 shows the following. In a cement composition consisting of a mixture containing cement clinker powder, gypsum powder, limestone powder, and blast furnace slag powder, if the gypsum powder content is 1.2 mass% or more and 2.4 mass% or less in terms of SO3, the compressive strength of the cement mixture increases as the gypsum powder content of the cement composition increases. The set of Experimental Examples A4 to A6 shows the following. That is, even when the total content of limestone powder and blast furnace slag powder (total content of admixture powders) is changed from 7.5 mass% to 10.0 mass% in the set of Experimental Examples A1 to A3, the compressive strength of the cement mixture increases as the gypsum powder content of the cement composition increases.
[0045] In Table 5, the set of Experimental Examples A7 to A10, the set of Experimental Examples A11 to A14, the set of Experimental Examples A15 to A18, and the set of Experimental Examples A19 to A22 show the following. That is, even when the type of cement clinker powder is changed in the set of Experimental Examples A1 to A3, the compressive strength of the cement mixture increases as the gypsum powder content of the cement composition increases. Furthermore, even when the gypsum powder content is 0.6 mass% or more and less than 1.2 mass% in terms of SO3, the compressive strength of the cement mixture increases as the gypsum powder content of the cement composition increases.
[0046] In Table 5, the set of Experimental Examples A23 and A24 and the set of Experimental Examples A25 and A26 show the following: That is, even when the limestone powder content and the blast furnace slag powder content are changed in the set of Experimental Examples A1 and A2, the compressive strength of the cement mixture increases as the gypsum powder content of the cement composition increases.
[0047] [Table 5]
[0048] In Table 6, the set of Experimental Examples a1 to a24 shows the following: In a cement composition consisting of a mixture containing cement clinker powder, gypsum powder, and limestone powder, even if the gypsum powder content is 1.2 mass% or more and 2.4 mass% or less in terms of SO3, if blast furnace slag powder is not included, the compressive strength of the cement mixture decreases as the gypsum powder content of the cement composition increases.
[0049] [Table 6]
[0050] From the above, the following conclusions can be derived from the experimental examples shown in Tables 5 and 6. In other words, in a cement composition consisting of a mixture containing cement clinker powder, gypsum powder, limestone powder, and blast furnace slag powder, if the limestone powder and blast furnace slag powder are contained in a total amount of 10.0 mass% or less, and the gypsum powder is contained in an amount of 0.6 mass% to 2.4 mass% in terms of SO3, when this cement composition is mixed with water, the hydration reaction of the blast furnace slag powder is effectively promoted by the SO3 contained in the gypsum powder, and a high-strength cement mixture can be produced. In other words, such a cement composition has a high strength development due to the gypsum powder and blast furnace slag powder contained in the mixture.
[0051] Table 7 rearranges the experimental examples A1 to A26 shown in Table 5. The experimental examples A1 and A4 show the following. That is, in a cement composition consisting of a mixture containing cement clinker powder, gypsum powder, limestone powder, and blast furnace slag powder, if the gypsum powder content is 1.2 mass% in terms of SO3, the compressive strength of the cement mixture decreases as the blast furnace slag powder content of the cement composition increases. The experimental examples A2 and A5 and the experimental examples A3 and A6 show the following. That is, in the experimental examples A1 and A4, if the gypsum powder content is 1.8 mass% or more and 2.4 mass% or less in terms of SO3, the compressive strength of the cement mixture increases as the blast furnace slag powder content of the cement composition increases.
[0052] In Table 7, the set of Experimental Examples A7 and A11, the set of Experimental Examples A8 and A12, the set of Experimental Examples A9 and A13, the set of Experimental Examples A10 and A14, the set of Experimental Examples A15 and A19, the set of Experimental Examples A16 and A20, the set of Experimental Examples A17 and A21, and the set of Experimental Examples A18 and A22 show the following. That is, even if the type of cement clinker powder is changed in the sets of Experimental Examples A1 and A4, if the gypsum powder content is 1.2 mass% or less in terms of SO3, the compressive strength of the cement mixture decreases as the blast furnace slag powder content of the cement composition increases, and if the gypsum powder content is 1.8 mass% or more and 2.4 mass% or less in terms of SO3, the compressive strength of the cement mixture increases as the blast furnace slag powder content of the cement composition increases.
[0053] In Table 7, the set of Experimental Examples A23 and A25 and the set of Experimental Examples A24 and A26 show the following: That is, even when the limestone powder content and the blast furnace slag powder content are changed in the set of Experimental Examples A1 and A4 and the set of Experimental Examples A2 and A5, when the gypsum powder content is 1.2 mass% in terms of SO3, the compressive strength of the cement mixture decreases as the blast furnace slag powder content of the cement composition increases, and when the gypsum powder content is 1.8 mass% in terms of SO3, the compressive strength of the cement mixture increases as the blast furnace slag powder content of the cement composition increases.
[0054] [Table 7]
[0055] In Table 8, the set of Experimental Examples B1 and B2 shows that, even when the content of gypsum powder in the cement composition is 1.6 mass% in terms of SO3, the compressive strength of the cement mixture increases as the content of blast furnace slag powder in the cement composition increases.
[0056] [Table 8]
[0057] Table 9 is a rearrangement of the experimental examples a1 to a24 shown in Table 6. In Table 9, the set of experimental examples a1 to a24 shows the following: In a cement composition consisting of a mixture containing cement clinker powder, gypsum powder, and limestone powder, even if the total content of the admixture powder is 10.0 mass% or less and the content of the gypsum powder is 1.8 mass% or more and 2.4 mass% or less in terms of SO3, if blast furnace slag powder is not included, the compressive strength of the cement mixture decreases as the content of the admixture powder in the cement composition increases.
[0058] [Table 9]
[0059] In Table 10, the set of Experimental Examples b1 and b2 shows the following. That is, when Cli6 is used in the set of Experimental Examples A2 and A5 shown in Table 7, even if the gypsum powder content is 1.8 mass% in terms of SO3 and the total content of limestone powder and blast furnace slag powder (total content of admixture powder) is 10.0 mass% or less, the compressive strength of the cement mixture decreases as the blast furnace slag powder content of the cement composition increases. As shown in Table 1, the SO3 content of Cli1 to Cli5 (cement clinker powder used in Experimental Examples A1 to A26, B1 and B2) is 0.94 mass% or more, while the SO3 content of Cli6 used in Experimental Examples b1 and b2 is 0.56 mass%.
[0060] [Table 10]
[0061] From the above, the following conclusions can be derived from the experimental examples shown in Tables 7 to 10. That is, in a cement composition consisting of a mixture containing cement clinker powder, gypsum powder, limestone powder, and blast furnace slag powder, if the limestone powder and blast furnace slag powder are contained in a total amount of 10.0 mass% or less, the gypsum powder is contained in a ratio of 1.6 mass% to 2.4 mass% in terms of SO3, and the SO3 content of the cement clinker powder is 0.80 mass% or more (strictly 0.94 mass% or more), when this cement composition is kneaded with water, the rapid hydration (flash setting) of the aluminate in the cement clinker powder is suppressed by the large amount of SO3 contained in the gypsum powder, and the aluminate contained in the cement clinker powder reacts with the limestone powder. As a result, a large amount of SO3 is eluted from the cement clinker powder, and the hydration of the blast furnace slag powder is promoted by the large amount of SO3 eluted from the cement clinker powder, and a high-strength cement kneaded product is produced. In other words, in such a cement composition, the strength development of the mixture is further increased by the gypsum powder and blast furnace slag powder contained in the mixture.
[0062] Furthermore, cement clinker powder with an SO3 content of 0.56 mass% or less cannot elute an amount of SO3 sufficient to promote the hydration of blast furnace slag powder even when mixed with water. Therefore, if the cement composition does not contain cement clinker powder with an SO3 content of 0.56 mass% or less, the proportion of "cement clinker powder that promotes the hydration of blast furnace slag powder" relative to the total amount of cement clinker powder in the cement composition will be high, and the strength development of the cement composition will be further enhanced by the gypsum powder and blast furnace slag powder contained in the cement composition.
[0063] Next, Table 11 will be explained, but before that, Tables 5 and 10 will be mentioned again. Referring to the set of Experimental Examples A1 to A3, the set of Experimental Examples A4 to A6, the set of Experimental Examples A8 to A10, the set of Experimental Examples A12 to A14, the set of Experimental Examples A16 to A18, and the set of Experimental Examples A20 to A22 in Table 5, when the gypsum powder content increases from 1.2% by mass to 1.8% by mass in SO3 conversion, the compressive strength of the cement mixture increases rapidly, but when the gypsum powder content increases from 1.8% by mass to 2.4% by mass in SO3 conversion, the compressive strength of the cement mixture increases only slightly.
[0064] That is, among these experimental examples, "the experimental examples in which the gypsum powder content is 1.8 mass% or 2.4 mass% converted into SO3" (hereinafter referred to as "Experimental Example X Group") maximizes the strength development of the cement composition by the gypsum powder contained in the cement composition. Also, among these experimental examples, "the experimental example in which the gypsum powder content is 1.2 mass% converted into SO3" (hereinafter referred to as "Experimental Example Y1 Group") increases the strength development of the cement composition by the gypsum powder contained in the cement composition, but does not maximize it.
[0065] As described above in the explanation of Table 7, in the "experimental examples in which the gypsum powder content is 1.8 mass% or 2.4 mass% in terms of SO3" (experimental example X group), the compressive strength of the cement mixture increases as the blast furnace slag powder content of the cement composition increases. In the "experimental example in which the gypsum powder content is 1.2 mass% in terms of SO3" (experimental example Y1 group), the compressive strength of the cement mixture decreases as the blast furnace slag powder content of the cement composition increases. On the other hand, in the set of experimental examples b1 and b2 shown in Table 10 (hereinafter referred to as "experimental example Y2 group"), even though the gypsum powder content is 1.8 mass% in terms of SO3, the SO3 content of the cement clinker powder is low, so that the compressive strength of the cement mixture decreases as the blast furnace slag powder content of the cement composition increases.
[0066] Table 11 shows "S1+S2" and "S2 / S1" for each of the experimental example X group, the experimental example Y1 group, and the experimental example Y2 group. Note that if the SO3 contained in the cement clinker powder is defined as clinker SO3, the SO3 contained in the gypsum powder is defined as gypsum SO3, the ratio of the clinker SO3 to the cement composition is defined as S1 mass%, and the ratio of the gypsum SO3 to the cement composition is defined as S2 mass%, then "S1+S2" is the total value of S1 mass% and S2 mass%, and "S2 / S1" is the ratio (proportion) of S2 mass% to S1 mass%.
[0067] In the experimental example X group, "S1+S2" is 2.65 or more and 3.60 or less, and "S2 / S1" is 1.497 or more and 2.837 or less. In the experimental examples Y1 and Y2 groups, "S1+S2" is 2.40 or less, and "S2 / S1" is 0.998 or more and 3.571 or less. In other words, in the cement composition, "S1+S2" is 2.65 or more and 3.60 or less, and "S2 / S1" is 1.497 or more and 2.837 or less, so that the strength development of the cement composition is maximized by the gypsum powder and blast furnace slag powder contained in the cement composition. In addition, considering that "S1+S2" of experimental examples Y1 and Y2 is lower than "S1+S2" of experimental example X, even if "S1+S2" exceeds 3.60 in a cement composition, as long as "S2 / S1" is 1.497 or more and 2.837 or less, it is considered that the strength expression of the cement composition can be maximized by the gypsum powder and blast furnace slag powder contained in the cement composition.
[0068] [Table 11]
[0069] From the above, the following conclusion can be derived from the experimental examples shown in Table 11. That is, in a cement composition consisting of a mixture containing cement clinker powder, gypsum powder, limestone powder, and blast furnace slag powder, if the limestone powder and blast furnace slag powder are contained in a total amount of 10.0 mass% or less, the gypsum is contained in an amount of 0.6 mass% or more and 2.4 mass% or less in terms of SO3, "S1 + S2" is 2.60 or more (strictly 2.65 or more), and "S2 / S1" is 1.40 or more and 3.00 or less (strictly 1.497 or more and 2.837 or less), then a large amount of clinker SO3 and a large amount of gypsum SO3 are contained in a balanced manner in the cement composition.
[0070] Therefore, when this cement composition is mixed with water, gypsum SO3 is dissolved from the gypsum powder in the initial mixing stage, and clinker SO3 is dissolved from the cement clinker powder after the initial mixing stage. As a result, SO3 is dissolved continuously without interruption from the gypsum and cement clinker powder in the mixing stage, and this SO3 promotes the hydration of the blast furnace slag powder continuously without interruption. Therefore, it is considered that the strength development of such a cement composition is further increased by the gypsum powder and blast furnace slag powder contained in the mixture. [Explanation of symbols]
[0071] 1. Cement manufacturing equipment 2. Clinker silo 3 Finishing Mill 4 Classifier 5 Mixing device 6. Cement Silo C Clinker D. Crushed material F Fine powder G plaster L limestone powder M mixture R Coarse powder S Blast furnace slag powder
Claims
1. A cement composition comprising a mixture containing cement clinker powder, gypsum powder, limestone powder and blast furnace slag powder, The limestone powder and the blast furnace slag powder are contained in the mixture in a total amount of 10.0 mass% or less, The gypsum powder is added to the mixture. 3 It is contained in an amount of 0.6 mass% or more and 2.4 mass% or less, The cement clinker powder has a TiO 2 content, MnO content, P 2 O 5 Content rate, Na 2 O content and K 2 When the O content is defined as T mass%, M mass%, P mass%, N mass% and K mass%, respectively, the physical property value of the cement clinker powder "(T + M + P) / (N + 0.658 × K)" is 0.80 or more and 1.40 or less, A cement composition characterized in that, when the SO3 contained in the cement clinker powder is defined as clinker SO3, the SO3 contained in the gypsum powder is defined as gypsum SO3, the ratio of the clinker SO3 to the mixture is defined as S1 mass%, and the ratio of the gypsum SO3 to the mixture is defined as S2 mass%, the sum of the S1 mass% and the S2 mass% is 2.60 mass% or more, and the ratio of the S2 mass% to the S1 mass% is 1.40 or more and 3.00 or less.
2. The cement clinker powder SO 3 The content is 0.80% by mass or more, The gypsum powder is added to the mixture. 3 2. The cement composition according to claim 1, characterized in that it is contained in an amount of 1.4 mass% or more in terms of converted value.
3. In the mixture, SO 3 3. The cement composition according to claim 2, characterized in that it does not contain cement clinker powder having a content of 0.56 mass% or less.
4. A method for producing a cement composition, comprising: It is equipped with a finishing process and a mixing process, In the finishing step, the cement clinker is pulverized together with gypsum to produce a mixed powder containing cement clinker powder and gypsum powder, In the mixing step, the mixed powder, limestone powder, and blast furnace slag powder are mixed to produce a cement composition, The limestone powder and the blast furnace slag powder are contained in the cement composition in a total amount of 10.0 mass% or less, The gypsum powder is a component of the cement composition. 3 It is contained in an amount of 0.6 mass% or more and 2.4 mass% or less, The cement clinker powder has a TiO 2 content, MnO content, P 2 O 5 Content rate, Na 2 O content and K 2 When the O content is defined as T mass%, M mass%, P mass%, N mass% and K mass%, respectively, the physical property value of the cement clinker powder "(T + M + P) / (N + 0.658 × K)" is 0.80 or more and 1.40 or less, A method for producing a cement composition, characterized in that, when the SO3 contained in the cement clinker powder is defined as clinker SO3, the SO3 contained in the gypsum powder is defined as gypsum SO3, the ratio of the clinker SO3 to the mixture is defined as S1 mass%, and the ratio of the gypsum SO3 to the mixture is defined as S2 mass%, the sum of the S1 mass% and the S2 mass% is 2.60 mass% or more, and the ratio of the S2 mass% to the S1 mass% is 1.40 or more and 3.00 or less.
5. Further comprising a baking step; 5. The method for producing a cement composition according to claim 4, wherein in the burning step, the cement clinker is produced using waste gypsum board as a cement raw material.
Citation Information
Patent Citations
Cement composition and cement-based solidifying material
JP2009062260A
Cement clinker and cement composition
JP2012025635A
Method for producing cement clinker
JP2012197197A
Method for producing cement composition
JP2012246190A
Cement composition
JP2013189377A