Composition for forming peelable coating film, and peelable coating film
A coating film composition with elastomers and amino-modified silicone oil addresses the challenge of easy removal and cleaning, ensuring high peelability and solvent resistance, facilitating efficient film detachment and surface cleaning.
Patent Information
- Application Number
- JP2020158931
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-27
- Filing Date
- 2020-09-23
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-09-23
AI Technical Summary
Conventional antifouling coating films face challenges in easy removal and cleaning due to high adhesive strength, leading to reduced work efficiency, while compositions with high adhesiveness are difficult to peel off, lacking both removability and easy cleaning properties.
A composition for forming a peelable coating film containing an elastomer, such as silicone or urethane elastomer, and amino-modified silicone oil, with a breaking strength to peel adhesive strength ratio of 1.5 or more, optionally with a filler, to enhance peelability and solvent resistance.
The composition improves peelability and ease of cleaning, while maintaining resistance to solvents like hexane, ensuring the coating film can be easily removed without breaking, thus enhancing work efficiency.
Smart Images

Figure 0007586677000004 
Figure 0007586677000005 
Figure 0007586677000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a composition for forming a peelable coating film, and a peelable coating film. [Background technology]
[0002] Conventionally, in order to prevent adhesion of dirt and scratches to structures, a method of protecting the surfaces of structures and structural members with an antifouling coating film has been used. The above-mentioned antifouling coating film is adhered to the structure or the like until a predetermined time to protect the surface, and is required to be easily peeled off (peelable) as necessary. For example, Patent Documents 1 to 5 disclose protective films or compositions containing silicone or the like for the purpose of improving peelability.
[0003] Incidentally, when handling structural members (adherends) coated with an antifouling coating film in a factory or the like, paints, adhesives, solvents, etc. (hereinafter also referred to as adhesives, etc.) may unintentionally adhere to the surface of the antifouling coating film before the timing of repainting or peeling off the antifouling coating film. In such cases, cleaning work is required to remove the adhesives, etc., that have adhered to the coating film surface. In addition, the coating film may swell due to the solvent contained in the adhesives, etc., which significantly reduces the adhesion between the adherend and the coating film.
[0004] As an example of a coating film with excellent solvent resistance, Patent Document 6 discloses a coating composition with excellent solvent resistance, recoatability, graffiti removal, or graffiti prevention. The coating composition described in Patent Document 6 contains, as essential components, at least one compound selected from a liquid organosiloxane compound, an organometallic catalyst, an alkoxy group-containing organosilane compound having a primary amino group or a secondary amino group, an amino-modified silicone oil, and an amino group-containing organosiloxane compound, and at least one compound selected from a compound having two or more glycidyl groups in one molecule, a glycidyl group-containing silane compound, and a glycidyl group-containing silicone oligomer. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 10-249981 [Patent Document 2] Japanese Patent Application Publication No. 11-172160 [Patent Document 3] Special Publication No. 2018-524446 [Patent Document 4] JP 2018-59084 A [Patent Document 5] Japanese Patent Application Publication No. 60-137975 [Patent Document 6] Patent No. 4721667 Summary of the Invention [Problem to be solved by the invention]
[0006] However, in the conventional antifouling coating films (protective films) described in the above Patent Documents 1 to 5, when an adhesive or the like adheres to the film surface, the adhesive or the like is difficult to remove easily because of the high adhesive strength between the coating film and the adhesive, and this significantly reduces the working efficiency.
[0007] On the other hand, the coating composition described in Patent Document 6 provides a coating film formed from this composition that is easy to clean, but the coating film adheres strongly to the substrate and cannot be easily peeled off when necessary.
[0008] Thus, up to now, no coating film or composition for coating film has been developed that simultaneously satisfies the requirements of peelability and ease of cleaning.
[0009] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a composition for forming a peelable coating film, which can improve the peelability between the coating film and the substrate and the ease of cleaning the coating film surface, and can provide a coating film having excellent resistance to solvents such as hexane, and a peelable coating film made of said composition. [Means for solving the problem]
[0010] The present inventors have conducted intensive research to solve the above problems, and have found that using an elastomer such as a silicone elastomer or a urethane elastomer as the main component of a coating film-forming composition is effective in obtaining a coating film with excellent peelability and easy cleaning, and that the coating film is strong even at room temperature. However, even if the coating film is mainly composed of an elastomer, depending on the type of adhesive or the like attached to the surface, the coating film itself may swell and the easy cleaning property may decrease. Therefore, the present inventors have found that by adding an amino-modified silicone oil to the above composition, it is possible to obtain resistance to the solvent contained in the adhesive and maintain the easy cleaning property.
[0011] Furthermore, the inventors of the present application have used the ratio of the breaking strength to the peel adhesion strength of the coating film as an index of removability, and have found that adding a filler to the above composition is effective in improving removability. The present invention was made based on these findings.
[0012] That is, the objects of the present invention can be achieved by the following [1] to [4]. [1] A peelable coating film-forming composition comprising an elastomer and an amino-modified silicone oil, When a film is formed from the peelable coating film-forming composition, the breaking strength of the film in a tensile test is F B (N / 20mm), and the peel adhesive strength between the coating film and the SUS304 plate when the coating film is formed on the surface of the SUS304 plate is F G (N / 20mm), F B / F G is 1.5 or more, A composition for forming a peelable coating film. [2] The peelable coating film-forming composition according to [1], further comprising a filler. [3] The peelable coating film forming composition according to [1] or [2], wherein the elastomer is a silicone elastomer or a urethane elastomer. [4] A peelable coating film comprising the composition for forming a peelable coating film according to any one of [1] to [3]. Effect of the Invention
[0013] The present invention contains an elastomer and an amino-modified silicone oil in a composition, and appropriately limits the ratio between the breaking strength of the film made of the composition and the peel adhesive strength between the coating film made of the composition and an adherend. Therefore, it is possible to provide a peelable coating film forming composition that can improve the peelability between the coating film and the adherend and the easy cleaning of the coating film surface, and can provide a coating film that has excellent resistance to solvents such as hexane, and a peelable coating film made of the composition. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a cross-sectional view showing a structural member on which a peelable coating film according to this embodiment is formed. [Diagram 2] FIG. 2 is a cross-sectional view showing a peelable coating film having an adhesive or the like attached to its surface. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, an embodiment of the present invention will be described in detail. Fig. 1 is a cross-sectional view showing a structural member on which a peelable coating film according to an embodiment of the present invention is formed. As shown in Fig. 1, a peelable coating film forming composition according to an embodiment of the present invention is applied to the surface of a structural member (adherend) 31, and then dried to form a peelable coating film 21. This peelable coating film 21 is peeled off from the structural member 31 at a desired timing. In this specification, the ease with which the peelable coating film 21 can be peeled off from the structural member 31 is referred to as "peelability." In addition, in this specification, a "peelable coating film" refers to a coating film that can be peeled off into a sheet shape without cracking.
[0016] FIG. 2 is a cross-sectional view showing a peelable coating film having an adhesive or the like attached to its surface. When a structural member 31 is handled in a factory or the like, an adhesive or the like 22 may adhere to the surface of the peelable coating film 21. The adhesive or the like 22 needs to be removed before the peelable coating film 21 is peeled off from the structural member 31. In this specification, the ease with which the adhesive or the like 22 can be removed from the surface of the peelable coating film 21 is referred to as "ease of cleaning." Note that, although the adhesive or the like 22 is attached to the entire surface of the peelable coating film 21 in FIG. 2, the adhesive or the like 22 may adhere to only a portion of the surface of the peelable coating film 21. The peelable coating film-forming composition of this embodiment will be described in detail below.
[0017] [Composition for forming peelable coating film] The peelable coating composition of the present embodiment is a peelable coating composition containing an elastomer and an amino-modified silicone oil. In addition, a coating film is formed on the surface of a membrane and a SUS304 plate by the peelable coating composition, and the tensile breaking strength (hereinafter also referred to as breaking strength) of the film by a tensile test is F. B (N / 20mm), peel adhesion strength between the above coating and SUS304 plate is F G (N / 20mm), F B / F G is 1.5 or more. Each component contained in the peelable coating film-forming composition will now be described in more detail.
[0018] (Elastomer) The peelable coating film-forming composition of the present embodiment contains an elastomer. As described above, by containing an elastomer as a main component of the coating film-forming composition, the peelability and easy cleanability of the coating film formed by the composition can be improved.
[0019] The elastomer is not particularly limited, and any appropriate elastomer can be used. Examples of the elastomer include silicone elastomers, urethane elastomers, acrylic elastomers, rubber-like polymers, polyamide elastomers, polyethylene elastomers, styrene elastomers, and butadiene elastomers. The elastomers may be used alone or in combination.
[0020] Among these, silicone elastomers and urethane elastomers are preferred from the viewpoint of improving the peelability and cleanability of the coating film.
[0021] Examples of silicone elastomers that can be used in this embodiment include addition type silicone elastomers, condensation type silicone elastomers, and UV-curable silicone elastomers, and include those that form a crosslinked coating by application, heating, drying, UV irradiation, or the like.
[0022] Such silicone elastomer may be a one-liquid type silicone elastomer that dries by itself, or a two-liquid type silicone elastomer that contains a curing agent.Furthermore, it may be an emulsion type.
[0023] For example, KE-1950-10(A / B), KE-1950-20(A / B), KE-1950-30(A / B), KE-1950-35(A / B), KE-1950-40(A / B), KE-1950-50(A / B), KE-1950-60(A / B), KE-1950-70(A / B), KE-1987(A / B), KE-1988(A / B) manufactured by Shin-Etsu Chemical Co., Ltd., and LR7665 series and LR303 manufactured by Wacker Asahi Kasei Silicone Co., Ltd. 3 series manufactured by Momentive Corporation, TSE3032 series and LSR series manufactured by Momentive Corporation, and SM8706EX, SM7036EX, SM7060EX, SM7025EX, SM490EX, SM8701EX, SM8709SR, SM8716SR, IE-7045, IE-7046T, SH7024, BY22-744EX, BY22-818EX, FZ-4658, FZ-4634EX, and FZ-4602 manufactured by Dow Corning Toray Co., Ltd.
[0024] Examples of emulsion types include POLON-MF-56, KM-9771, KM-9774, KM-2002-T, KM-2002-L-1, and KM-9772 manufactured by Shin-Etsu Chemical Co., Ltd.
[0025] In addition, examples of urethane elastomers that can be used in this embodiment include polyurethane elastomers that are chain-extended by reacting an isocyanate group with a polyol. Examples of such polyurethane elastomers include those that have a carboxyl group obtained by using a carboxyl group-containing polyol as part of the polyol, and those that have a hydroxyl group at the end. Polyurethane elastomers that have a carboxyl group are preferably neutralized with a basic substance. Examples of commercially available products include "Superflex Series 110", "Superflex Series 150", "Superflex Series 460S", and "Superflex Series 470" manufactured by Daiichi Kogyo Seiyaku Co., Ltd., "Neolet's R9649" and "Neolet's R966" manufactured by Avecia, "Hydran WLS-210" and "Hydran WLS-250" manufactured by DIC Corporation, and "Permarine UA-310" manufactured by Sanyo Chemical Industries, Ltd.
[0026] By using urethane elastomer, the breaking strength F of the film described later can be increased without adding filler. B Peel adhesion strength F G F B / F G can be preferably set to 1.5 or more.
[0027] The acrylic elastomer may be a commercially available product, such as "High Heat Resistant Grade XB Series" manufactured by Aron Chemical Industries, Ltd., or "Polysol AP-4780N", "Polysol AP-609", "Polysol AP-691", or "Polysol AP-4795" manufactured by Showa Denko K.K.
[0028] Examples of the styrene elastomer include elastomers containing polystyrene as a hard segment and polybutadiene, polyisoprene, and copolymers of polybutadiene and polyisoprene as soft segments, as well as hydrogenated products thereof.
[0029] The content of the elastomer in the composition is preferably 20 to 98% by mass, more preferably 30 to 95% by mass, based on the total mass of the composition, such that a coating film having better peelability and easy cleanability can be obtained.
[0030] (Amino modified silicone oil) The peelable coating film forming composition of this embodiment contains amino-modified silicone oil in addition to the elastomer. The coating film formed by the composition containing amino-modified silicone oil together with elastomer has excellent resistance (solvent resistance) to solvents such as hexane contained in adhesives, etc., and can prevent the coating film from swelling when exposed to a solvent. This is thought to be because, among various modified silicone oils, amine has high polarity, which increases the resistance to solvents such as hexane.
[0031] Amino-modified silicone oil is a silicone oil in which some of the methyl groups of the silicone oil are replaced with aminoalkyl groups. The modified site may be a side chain, one end, both ends, or both ends of the side chain. It may also be an emulsion type.
[0032] As the amino-modified silicone oil, a commercially available amino-modified silicone oil can be used as it is. In particular, it is preferable to use an amino-modified silicone oil represented by the following general formula (1). By using the amino-modified silicone oil represented by this formula (1), high reliability can be obtained.
[0033] [ka]
[0034] In the above formula (1), R1, R2, and R3 are amino-modified alkyl groups or amino groups, for example, -C3H6-NH2, -C6H4-NH2, -C3H6-NH-C2H4-NH2, -C3H6-NH-CH 3、 -NH2, etc. R1, R2, and R3 may be the same or different from each other. R1, R2, and R3 may contain one or more of an alkyl group, an epoxy group, a carboxyl group, a methacryl group, a carbinol group, a hydroxyl group, a mercapto group, a polyether group, a phenyl group, a fluoroalkyl group, an aralkyl group, and hydrogen.
[0035] In the above formula (1), the repeat number m is a positive number from 0 to 50, and the repeat number n is a positive number from 0 to 50. Particularly preferably, m is in the range of 0-20, and n is in the range of 0-20.
[0036] Furthermore, as the amino-modified silicone oil represented by the above formula (1), a dimethylpolysiloxane modified at both ends with aminopropyl groups, in which m=0 to 40 and n=0 to 40 in formula (1), is particularly preferably used. Among these, a dimethylpolysiloxane modified at both ends with aminopropyl groups, in which m=0 to 20 and n=0 to 20 in formula (1), is particularly preferably used.
[0037] The amino-modified silicone oil represented by the above general formula (1) or the like can be obtained by a conventionally known production method.
[0038] Examples of amino-modified silicone oils include KF-868, KF-865, KF-864, KF-859, KF-393, KF-860, KF-877, KF-880, KF-8004, KF-8002, KF-8005, KF-867, X-22-3820W, KF-869, and KF-86 manufactured by Shin-Etsu Chemical Co., Ltd. 1, X-22-3939A, PAM-E, KF-8010, X-22-161A, X-22-161B, KF-8012, KF-8008, X-22-1660B-3, KF-857, KF-8001, KF-862, X-22-9192, KF-858, BY16-205, FZ-3 manufactured by Toray Dow Coating Co., Ltd. 760, SF8417, BY16-849, BY16-892, FZ-3785, BY16-872, BY16-213, BY16-203, BY16-898, BY16-890, BY16-891, BY16-893, BY16-871, BY16-853U, Chisso; FM-3311, FM-3321, FM-33 25. Momentive Performance Materials' TSF4702, TSF4703, TSF4704, TSF4705, TSF4706, TSF4707, TSF4708, TSF4709, XF42-B1989, XF42-B8922, XF42-C0330, XF49-C1109, SILSOFT Examples of such products include WACKER L652, WACKER L653, WACKER L655, WACKER L656, WACKER FINISH WR1100, WACKER FINISH WR1200, WACKER FINISH WR1300, WACKER FINISH WR1600, WACKER FINISH WT1250, and WACKER FINISH WT1650 manufactured by Wacker Asahi Kasei Silicones Co., Ltd.
[0039] Examples of emulsion types include PolonMF-14, PolonMF-14D, PolonMF-14EC, PolonMF-29, PolonMF-39, PolonMF-44, PolonMF-52, KM907, X-52-2265, PolonMF-51, and KM9771 manufactured by Shin-Etsu Chemical Co., Ltd., FZ-4632, FZ-4635, FZ-4640, FZ-4645, FZ-4658, FZ-4671, and FZ-4678 manufactured by Nippon Junker Co., Ltd., and SM8704C / SM8904 manufactured by Dow Toray Coating Co., Ltd.
[0040] The content of the amino-modified silicone oil in the composition is preferably 2 to 100 parts by weight, more preferably 5 to 80 parts by weight, based on 100 parts by weight of the elastomer. In such a range, the solvent resistance can be further improved. The amino-modified silicone oil may be used alone or in combination of two or more kinds.
[0041] <Membrane breaking strength F B / Peel adhesion of coating F G :1.5 or more> The ratio of the breaking strength of the film formed by the peelable coating composition of this embodiment in a tensile test to the peel adhesive strength between the coating film and the SUS304 plate when the coating film is formed on the SUS304 plate can be used as an index of the peelability of the coating film. Therefore, by appropriately adjusting the ratio of the breaking strength to the peel adhesive strength, a composition for forming a coating film having excellent peelability can be obtained. The reason for limiting the ratio of the breaking strength to the peel adhesive strength will be explained in more detail below.
[0042] The breaking strength measured by the tensile test is a strength indicating the resistance of the film to breaking when both ends of the film made of the peelable coating film forming composition of this embodiment are pulled in the direction away from each other. If the breaking strength is low, the coating film breaks when peeling it from the adherend, making peeling difficult. Also, if the adhesive strength between the coating film and the adherend is too high, the force required to peel the coating film from the adherend becomes large, and as a result, the coating film becomes more likely to break. Therefore, in order to easily peel the coating film without breaking it, the peel adhesive strength F G Breaking strength F B It is necessary that the ratio be equal to or greater than a predetermined value.
[0043] In the present invention, the breaking strength is calculated by preparing a test piece for a tensile test from the peelable coating composition as a sample, and measuring the breaking stress when the tensile test is performed. The breaking strength is measured by first applying the peelable coating composition as a sample to the surface of a PET substrate ("Lumirror S10#75" manufactured by Toray Industries, Inc.) having a thickness of 75 μm to a wet thickness of 500 μm using an applicator (YBA Baker Applicator manufactured by Yoshimitsu Seiki Co., Ltd.), drying at 35° C. for 3 days, and then cutting the sample into a rectangle having a width of 10 mm and a length of 100 mm to obtain a test piece. Then, both ends of the test piece are pulled by a tensile tester at room temperature, and the breaking stress of the test piece is measured, and the value converted assuming that the width of the test piece is 20 mm is defined as the breaking strength F. B (N / 20mm). At this time, the pulling speed is 300mm / min and the grip distance is 20mm.
[0044] There is no particular upper limit to the breaking strength, but in order to prevent the coating film from breaking when peeling it off from the substrate, it is preferably 0.3 (N / 20 mm) or more, and more preferably 0.8 (N / 20 mm) or more.
[0045] In addition, peel adhesive strength F GIn the measurement of peel adhesion strength F, first, a peelable coating film forming composition as a sample is applied to the surface of a SUS304 plate with a 2B treatment using an applicator (YBA Baker Applicator, manufactured by Yoshimitsu Seiki Co., Ltd.) so that the wet thickness is 500 μm. The applied composition is dried at 35° C. for 3 days, and then the coating film is cut to a width of 20 mm on the SUS304 plate to form a test piece. Then, a tensile tester is used to measure the stress when peeling the test piece from the SUS304 plate, and this is taken as the peel adhesion strength F. G The peel adhesion strength is measured at room temperature, with a peel angle of 180° and a peel speed of 300 mm / min.
[0046] The peel adhesive strength is preferably, for example, 0.2 to 15 (N / 20 mm), more preferably 0.5 to 12 (N / 20 mm), and even more preferably 1.0 to 10 (N / 20 mm), so that the adhesive strength between the adherend and the coating film can be maintained until the desired time and the coating film can be easily peeled off from the adherend.
[0047] The above breaking strength F B (N / 20mm) of the above peel adhesive strength F G (N / 20mm) ratio, F B / F G If F is less than 1.5, the coating film is likely to break when attempting to peel the coating film from the adherend at the desired time. B / F G is set to 1.5 or more, preferably 1.8 or more, and more preferably 2.0 or more. This makes it possible to obtain a coating film that can be easily peeled off from an adherend and has good workability. B / F G The composition of the peelable coating film forming composition is appropriately designed, and the breaking strength F B and peel adhesive strength F G can be adjusted to fall within a desired range.
[0048] (Filler) The peelable coating film-forming composition of this embodiment preferably contains a filler. The filler is a component that can improve the hardness of the coating film, and the above-mentioned F B / F G In order to adjust the viscosity and improve the peelability of the coating film, the addition of a filler is effective.
[0049] When a filler is added to the peelable coating film forming composition of this embodiment, the content of the filler in the composition is preferably 0 to 150 parts by weight, more preferably 0 to 100 parts by weight, based on 100 parts by weight of the elastomer. In such a range, the peelability of the coating film can be further improved. The content of the filler may be 2 parts by weight or more, or 5 parts by weight or more, based on 100 parts by weight of the elastomer.
[0050] Examples of the filler include silica particles, titanium oxide particles, alumina particles, calcium carbonate, magnesium hydroxide, mica, kaolin, talc, carbon black, layered silicate, clay minerals, and diatomaceous earth. The particle size is preferably an average particle size of 5 nm to 5000 nm. By adjusting the particle size within the above range, the adhesion between the coating film and the adherend can be further improved. The filler can be either a powder type or a water-dispersed type.
[0051] The filler may be a commercially available product. Examples of silica particles include the Snowtex (registered trademark) series (e.g., Snowtex (registered trademark)-XL, Snowtex (registered trademark)-YL, Snowtex (registered trademark)-ZL, Snowtex (registered trademark) PST-2, Snowtex (registered trademark) 20, Snowtex (registered trademark) 30, Snowtex (registered trademark) 30L, Snowtex (registered trademark) C, Snowtex (registered trademark) O, and Snowtex (registered trademark) 50, all of which are water-dispersible types, manufactured by Nissan Chemical Industries, Ltd.), the Adelite series (e.g., Adelite (registered trademark) AT-40, and Adelight (registered trademark) AT-50 (the above are water-dispersed types, manufactured by ADEKA Corporation), the AEROSIL (registered trademark) series (for example, the AEROSIL (registered trademark) RX series (RX50, RX200, RX300, etc.), the AEROSIL (registered trademark) RX series (RY50, RY200, RY200S, etc.), the AEROSIL (registered trademark) NY50 series, the AEROSIL (registered trademark) NAX series, the AEROSIL (registered trademark) R series, powder type, manufactured by Nippon Aerosil Co., Ltd.), and the like.
[0052] The above-mentioned peelable coating film forming composition may contain any suitable other oil within the range that does not impair the effect of the present invention. Examples of such other oils include various silicone oils such as dimethyl silicone oil, polyether modified silicone oil, phenyl modified silicone oil, carbinol modified silicone oil, mercapto modified silicone oil, carboxyl modified silicone oil, and long chain alkyl modified silicone oil, liquid paraffin, surfactant, liquid hydrocarbon, fluorinated oil, wax, petrolatum, animal fat, and fatty acid. These may be only one type or two or more types.
[0053] When the composition for forming a peelable coating contains such other oils, the ease of cleaning of the peelable coating may be further improved.
[0054] The peelable coating film-forming composition may contain any other suitable additives within the scope of not impairing the effects of the present invention, such as ultraviolet absorbers, light stabilizers, antioxidants, antiaging agents, antistatic agents, pigments, dyes, leveling agents, thickeners, etc.
[0055] The peelable coating film-forming composition of the present embodiment can be applied to an adherend and dried to form a coating film. A highly uniform coating film can be obtained even when dried at room temperature (25° C.).
[0056] The composition can be applied directly to any substrate by any known application method such as spraying, brushing, roller, curtain flow, roll, dip, or coater.
[0057] Specific examples of the adherend include various structures such as metal products, wood products, plastic products, glass products, medical parts (e.g., catheters, stents, gloves, tweezers, containers, guides, trays, etc.), painting-related parts (e.g., robot arms, painting booths, hangers, covering materials, ovens, etc.), buildings (interior and exterior wall surfaces, floors, and ceiling surfaces), electronic devices, transportation equipment (e.g., automobiles, motorcycles, railway vehicles, and ships, etc.), and the structural members that make up these structures.
[0058] <Removable coating film> The peelable coating film of this embodiment is made of the above-mentioned composition for forming a peelable coating film, and is a coating film that can improve the peelability between the coating film and the substrate and the ease of cleaning the coating film surface, as well as having excellent solvent resistance.
[0059] The thickness of the coating film may be any appropriate thickness depending on the application and the environment of use. The thickness of the coating film is preferably 50 μm to 1000 μm, more preferably 80 μm to 500 μm. If the thickness of the coating film is 50 μm or more, the effect of protecting the adherend can be sufficiently obtained. Also, if the thickness of the coating film is 1000 μm or less, the work efficiency when forming the coating film is excellent. The thickness of the coating film can be measured, for example, using RI-205 manufactured by PEAKOCK. EXAMPLES
[0060] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples in any way.
[0061] [Preparation of peelable coating film forming composition] The peelable coating film-forming composition was prepared by mixing 100 parts by mass of a silicone elastomer (silicone emulsion elastomer KM2002T: manufactured by Shin-Etsu Chemical Co., Ltd.) or a urethane elastomer (urethane emulsion elastomer Superflex 470: manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.) with various types and amounts of silicone oil and filler shown in Table 1 below.
[0062] [Evaluation of peelability] [Breaking strength F B Measurement of A test piece for a tensile test was prepared from the obtained peelable coating film-forming composition, and the tensile test was carried out to measure the breaking stress and the breaking strength F B asked for. In measuring the breaking strength, first, the peelable coating composition as a sample was applied to the surface of a 75 μm thick PET substrate ("Lumirror S10#75" manufactured by Toray Industries, Inc.) using an applicator (YBA Baker Applicator manufactured by Yoshimitsu Seiki Co., Ltd.) to a wet thickness of 500 μm, and then dried at 35° C. for 3 days. The sample was then cut into a rectangle 10 mm wide and 100 mm long to prepare a test specimen. The breaking stress (MPa) was measured by pulling both ends of the prepared test piece in the longitudinal direction using a tensile tester (AUTOGRAPH AGS-J / H 1kN: manufactured by Shimadzu Corporation). In this example, the breaking stress was measured at room temperature with a grip distance of 20 mm and a tensile speed of 300 mm / min, and the value converted assuming the test piece width of 20 mm was determined as the breaking strength F. B (N / 20mm). In addition, the length λ of the elongation of the test piece immediately before the test piece broke was measured, and the length λ was divided by the initial length (chuck distance) L0 of the test piece to calculate the breaking strain (%).
[0063] [Peel Adhesion F G Measurement of A test piece for measuring peel adhesion was prepared from the obtained peelable coating film forming composition, and the peel adhesion was measured. The test specimen was prepared by applying the above peelable coating composition to the surface of a 2B-treated SUS304 plate using an applicator (YBA Baker Applicator, manufactured by Yoshimitsu Seiki Co., Ltd.) to a wet thickness of 500 μm, drying at 35° C. for 3 days, and then cutting the coating film to a width of 20 mm on the SUS304 plate. A tensile tester (AUTOGRAPH AGS-J / H 1 kN, manufactured by Shimadzu Corporation) was used to measure the stress when peeling the test specimen from the SUS304 plate, and the peel adhesive strength F G The peel adhesive strength was measured at room temperature, with a peel angle of 180° and a peel speed of 300 mm / min. Furthermore, the breaking strength F B The above peel adhesive strength F G The peelability was evaluated by calculating the ratio of
[0064] [Evaluation of ease of cleaning] [Adhesive peel strength measurement] A test piece for measuring adhesive peel strength was prepared from the obtained peelable coating film-forming composition, and an adhesive-peel adhesion strength test was carried out to measure the adhesive peel strength. The method of preparing the test piece was as follows: first, the above peelable coating composition was applied to the surface of a SUS304 plate having a thickness of 2 mm and a surface treated with 2B using an applicator (YBA Baker Applicator: manufactured by Yoshimitsu Seiki Co., Ltd.) so that the wet thickness was 500 μm, and the plate was dried at 35 ° C. for 3 days. Next, an adhesive (GP100: manufactured by Konishi Co., Ltd.) was applied to a width of 30 mm on the dried coating film, and the plate was further dried at 35 ° C. for 24 hours. Then, a double-sided tape (No. 5000NS: manufactured by Nitto Denko Co., Ltd.) was attached to the surface of the adhesive, and a PET (PolyEthylene Terephthalate) plate (Lumirror (registered trademark) S10 # 75: manufactured by Toray Industries, Inc.) was attached to the adhesive via the double-sided tape, thereby preparing a test piece.
[0065] Then, in accordance with JIS K 6854-2, the SUS304 plate and the PET plate were pulled using a tensile tester (AUTOGRAPH AGS-J / H 1kN: manufactured by Shimadzu Corporation) to perform an adhesive-peel adhesion strength test to measure the adhesive peel strength. The adhesive peel strength was measured at room temperature, with a peel angle of 180° and a peel speed of 100 mm / min.
[0066] [Measurement of adhesive peel strength after immersion in hexane] A test piece for measuring the adhesive peel strength after immersion in hexane was prepared using the obtained peelable coating film forming composition, and an adhesive-peel adhesion strength test was carried out to measure the adhesive peel strength after immersion in hexane. The test piece was prepared as follows: first, the above peelable coating composition was applied to the surface of a 2 mm thick SUS304 plate with a 2B-treated surface using an applicator (YBA Baker Applicator, manufactured by Yoshimitsu Seiki Co., Ltd.) to a wet thickness of 500 μm, and then dried at 35° C. for 3 days. Next, the SUS304 plate with the coating formed on its surface was immersed in hexane for 1 hour, and then dried at 60° C. for 24 hours. After that, an adhesive (GP100, manufactured by Konishi Co., Ltd.) was applied to the dried coating film in a width of 30 mm, and then further dried at 35° C. for 24 hours. Thereafter, a double-sided tape (No. 5000NS: manufactured by Nitto Denko Corporation) was attached to the surface of the adhesive, and a PET (PolyEthylene Terephthalate) plate (Lumirror (registered trademark) S10#75: manufactured by Toray Industries, Inc.) was further attached so as to be bonded to the adhesive via the double-sided tape, thereby preparing a test specimen.
[0067] Then, in accordance with JIS K 6854-2, the SUS304 plate and the PET plate were pulled using a tensile tester (AUTOGRAPH AGS-J / H 1kN: manufactured by Shimadzu Corporation) to perform an adhesive peel strength test, thereby measuring the adhesive peel strength after immersion in hexane. The adhesive peel strength measurement was performed at room temperature, with a peel angle of 180° and a peel speed of 100mm / min. If the coating film peeled off from the SUS304 plate when the SUS304 plate and the PET plate were pulled using the tensile tester, the coating film and the SUS304 plate were adhered together using a double-sided tape (No. 5000NS: manufactured by Nitto Denko Corporation), and then an adhesive peel strength test was performed.
[0068] [Evaluation of Solvent Resistance] [Observation of the state of the coating after immersion in hexane] A test piece for observing solvent resistance was prepared from the obtained peelable coating film-forming composition, and the state of the coating film after immersion in hexane was observed to evaluate the solvent resistance. The test piece was prepared by applying the above peelable coating composition to the surface of a 2 mm thick SUS304 plate with a 2B-treated surface using an applicator (YBA Baker Applicator, manufactured by Yoshimitsu Seiki Co., Ltd.) to a wet thickness of 500 μm, and drying for 3 days at 35° C. The test piece was then immersed in hexane for 10 minutes, after which it was observed whether the coating had swelled or not and whether the coating had peeled off from the SUS304 plate.
[0069] The evaluation results of the peelability, cleanability and solvent resistance are shown in the following Table 2. The evaluation criteria for solvent resistance were ◯ when no swelling or peeling of the coating film was observed, and × when even a small amount of swelling or peeling of the coating film was observed.
[0070] [Table 1]
[0071] [Table 2]
[0072] Details of the product names in Table 1 above are as follows. Note that for KF6016, Silwet L7600, and Silwet L7602, the HLB value (Hydrophilic-Lipophilic Balance) is also shown.
[0073] <Polymer> · KM2002T: Silicone emulsion elastomer manufactured by Shin-Etsu Chemical Co., Ltd. Superflex 470: Manufactured by Daiichi Kogyo Seiyaku Co., Ltd., urethane emulsion elastomer
[0074] <Silicone oil> POLON-MF-51: Amino modified silicone oil manufactured by Shin-Etsu Chemical Co., Ltd. POLON-MF-14EC: Amino modified silicone oil (low viscosity) manufactured by Shin-Etsu Chemical Co., Ltd. KF6016: Polyether modified silicone oil (HLB value: 4.5), manufactured by Shin-Etsu Chemical Co., Ltd. Silwet L7600: Polyether modified silicone oil (HLB value: 14.3), manufactured by Dow Corning Toray Co., Ltd. Silwet L7602: Polyether modified silicone oil (HLB value: 7.3), manufactured by Dow Corning Toray Co., Ltd. X-51-1264: Epoxy modified silicone oil manufactured by Shin-Etsu Chemical Co., Ltd. KM9769: Mercapto-modified silicone oil, manufactured by Shin-Etsu Chemical Co., Ltd. KM9739: Phenyl-modified silicone oil, manufactured by Shin-Etsu Chemical Co., Ltd. KM862T: Dimethyl silicone oil, manufactured by Shin-Etsu Chemical Co., Ltd.
[0075] <Filler> STC: Snowtex C, manufactured by Nissan Chemical Co., Ltd. HOMOCAL-D: Shiraishi Kogyo Co., Ltd., calcium carbonate,
[0076] As shown in Tables 1 and 2 above, in Examples 1 to 5, coating films were formed using compositions containing silicone elastomer and amino-modified silicone oil, and the breaking strength F B Peel adhesion strength F G Ratio to F B / F G The value is 1.5 or more. Therefore, the film has excellent peelability and cleanability, and the solvent resistance evaluated by immersion in hexane also showed good results.
[0077] In addition, in Examples 6 and 7, a coating film was formed using a composition containing a urethane elastomer and an amino-modified silicone oil. The elastic effect of the urethane elastomer resulted in a higher breaking strength than that of the silicone elastomer, and the breaking strength F of the film was 100% without the addition of a filler. B Peel adhesion strength F G Ratio to F B / F Gcan be made 1.5 or more. Therefore, the peelability and easy cleaning are excellent, and the solvent resistance evaluated by immersion in hexane also showed good results. In addition, in Example 7, by increasing the amount of amino-modified silicone oil, the adhesive peel force was further reduced and the easy cleaning was good.
[0078] On the other hand, in Comparative Examples 1 and 3, the composition did not contain silicone oil, so the solvent resistance was reduced, and in particular, in Comparative Example 3, the ease of cleaning was also reduced. In Comparative Example 2, the coating film could not be peeled off from the SUS304 plate. In Comparative Examples 4 and 6 to 10, although the composition contained silicone oil, it was not amino-modified silicone oil, so the solvent resistance was reduced and the film swelled due to the solvent. In addition, the components contained in the silicone oil or silicone elastomer may flow out of the coating film due to swelling, so that in the ease of cleaning test, the coating film peeled off, some of the coating films became impossible to peel off, or some of the coating films became difficult to peel off due to a significant increase in the measured peel force. In Comparative Example 5, the solvent resistance was good, but the breaking stress was significantly reduced, making it impossible to peel off. [Explanation of symbols]
[0079] 21 Peelable coating 22 Adhesives, etc. 31 Structural members
Claims
1. A peelable coating film-forming composition comprising an elastomer and an amino-modified silicone oil, When a film is formed from the peelable coating film-forming composition, the breaking strength of the film in a tensile test is F B (N / 20 mm), and the peel adhesive strength between a coating film formed on the surface of a SUS304 plate and the SUS304 plate is F G (N / 20mm), F B / F G is 1.5 or more, the elastomer is a silicone elastomer or a urethane elastomer, The F B and F G are measured by the following method. A composition for forming a peelable coating film. (Method of Measuring F B ) The peelable coating composition was applied to the surface of a PET substrate having a thickness of 75 μm using an applicator to a wet thickness of 500 μm, and after drying at 35° C. for 3 days, a rectangle having a width of 10 mm and a length of 100 mm was cut into a test piece. Both longitudinal ends of the test piece were pulled using a tensile tester under conditions of a gripping distance of 20 mm, a pulling speed of 300 mm / min, and room temperature to measure the breaking stress, and the value converted assuming a width of the test piece of 20 mm was taken as the breaking strength F B . (Method of measuring FG) A peelable coating film was prepared by applying the composition for forming a peelable coating film using an applicator to the surface of a 2B-treated SUS304 plate so that the wet thickness was 500 μm, drying at 35° C. for 3 days, and then cutting the coating film onto the SUS304 plate so that it had a width of 20 mm. A tensile tester was then used to measure the stress when peeling the test piece from the SUS304 plate at room temperature, under conditions of a peel angle of 180° and a peel speed of 300 mm / min, and this was taken as the peel adhesive strength FG.
2. The peelable coating composition according to claim 1 , further comprising a filler.
3. A composition for forming a peelable coating film as described in claim 1 or 2, wherein the content of the elastomer is 20 to 98 mass% relative to the total mass of the composition, and the content of the amino-modified silicone oil is 2 to 100 parts by weight relative to 100 parts by weight of the elastomer.
4. A peelable coating film comprising the composition for forming a peelable coating film according to any one of claims 1 to 3.
Citation Information
Patent Citations
Ink for writing utensils
JP1985137975A
Antisticking material for aquatic organism
JP1990053878A
Plastic molding formed with protective film and its manufacture
JP1998249981A
Strippable paint
JP1999172160A
Coating composition containing epoxy resin and amino-functional silicone resin
JP2007523964A