Method for manufacturing spot-welded member, and spot-welded member

A two-stage spot welding process with overlapping nuggets and controlled pressure addresses bonding defects in high plate thickness ratio assemblies, ensuring strong and fatigue-resistant spot welded members.

JP7587148B2Active Publication Date: 2024-11-20NIPPON STEEL CORPORATION
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021050389
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-24
Publication Date
2024-11-20
Estimated Expiration
2041-03-24

AI Technical Summary

Technical Problem

Spot welding methods fail to adequately join thin metal plates on the surface of a plate assembly with a high plate thickness ratio, leading to bonding defects and reduced fatigue characteristics, particularly in automotive parts made from thin mild steel and high-strength steel.

Method used

A two-stage spot welding process is employed, where a first spot welding forms a nugget between a thin first metal plate and an internal metal plate, followed by a second spot welding that joins the first nugget with a thicker second metal plate, ensuring the nuggets overlap with a minimum distance of 1.0 mm and applying higher pressure to suppress bonding defects.

Benefits of technology

This method effectively prevents bonding failures in thin metal plates even with plate thickness ratios exceeding 6.0, enhancing the fatigue strength and joint integrity of the spot welded members.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587148000003
    Figure 0007587148000003
  • Figure 0007587148000004
    Figure 0007587148000004
  • Figure 0007587148000005
    Figure 0007587148000005
Patent Text Reader

Abstract

To provide a manufacturing method of a spot welding member capable of suppressing bonding failure even when a base material is a plate set whose surface is arranged with a thin plate, and having a high fatigue characteristic, and a spot welding member.SOLUTION: A manufacturing method of a spot welding member according to an aspect of the present invention includes the steps of: applying first spot welding to a first metal plate and an internal metal plate to form a first conjugate including a first nugget that bonds the first metal plate and the internal metal plate; and arranging a second metal plate thicker than the first metal plate so as to overlap with the internal metal plate of the first conjugate, and applying second spot welding to form a second nugget that bonds the internal metal plate of the first conjugate and the second metal plate. The first nugget and the second nugget overlap with each other.SELECTED DRAWING: Figure 1C
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a spot-welded component, and to a spot-welded component. [Background technology]

[0002] Spot welding is a resistance welding method in which overlapping base metals are sandwiched between the tips of electrodes, and electric current is passed through them while applying pressure, and the metals are melted and joined by the generated Joule heat. In lap resistance welding such as spot welding, the molten and solidified part that occurs at the weld is called a nugget.

[0003] Spot welding is used to manufacture various mechanical structural parts because it is highly efficient. For example, thousands of spot welds are formed per car during manufacturing. However, spot welding has the problem that welding defects are likely to occur in plate assemblies with a large plate thickness ratio. Here, a plate assembly refers to multiple metal plates stacked together. The plate thickness ratio of a plate assembly is the value obtained by dividing the total plate thickness of the metal plates that make up the plate assembly by the thickness of the thinner metal plate located on the surface of the plate assembly.

[0004] The nugget that joins the metal plates is formed in the center of the sheet assembly or in its vicinity. If the diameter of the nugget is small or if the nugget is formed away from the thin plate on the surface of the sheet assembly, the nugget and the thin plate on the surface of the sheet assembly will not overlap, resulting in poor joining of the thin plate. In particular, in sheet assemblies with a sheet thickness ratio of more than 6.0, there is a strong tendency for poor joining of the thin plate on the surface of the sheet assembly to occur.

[0005] Poor joints in spot welding are particularly problematic in the manufacture of automobile parts, for example. Automobile parts are composed of thin mild steel sheets that form the exterior and high-strength steel sheets that form the frame parts. In spot welding of such parts, the thin sheet that forms the exterior is inevitably placed on the outermost surface of the sheet assembly.

[0006] Furthermore, in spot welding between a high-strength steel plate and mild steel, the nugget tends to be formed biased toward the high-strength steel plate. This is because high-strength steel plate contains more alloy elements than mild steel, and these alloy elements increase the electrical resistance of the high-strength steel plate. In spot welding between a high-strength steel plate and mild steel, resistance heating occurs preferentially in the high-strength steel plate, which has a higher electrical resistance. Therefore, in spot welding between a high-strength steel plate and mild steel, the outer edge of the nugget formed does not reach the mild steel, and there is a risk of poor joining of the mild steel.

[0007] Thus, in resistance spot welding of sheet assemblies in which thin mild steel is arranged on the outermost surface, joint failure is likely to occur. In general, it is believed that joint failure is particularly likely to occur in sheet assemblies with a sheet thickness ratio exceeding 6.0. Reducing the sheet thickness ratio to a small value in order to avoid joint failure impairs the degree of freedom in designing mechanical structural components. Therefore, a technology for suppressing joint failure in spot welding of sheet assemblies with a high sheet thickness ratio is desired.

[0008] Patent Document 1 discloses a spot welding method in which a thin plate weldable member is overlapped on at least one of two overlapping thick plate weldable members, and these are sandwiched between a pair of electrodes while applying pressure and electricity to spot weld the welded members, wherein the thin plate weldable member is formed with a seating surface that is one step higher than the general part at the portion to be welded, and the tip of the electrode of the pair of electrodes that faces the thin plate weldable member is formed into a spherical surface, and at the beginning of welding, the seating surface of the thin plate weldable member is crushed with a low pressure to weld the thin plate weldable member and the adjacent thick plate weldable member, and then the two thick plate weldable members are welded together with a high pressure.

[0009] Patent Document 2 discloses a method for producing a resistance spot welded joint by resistance spot welding a plate assembly made up of multiple overlapping metal plates, the method comprising the steps of: (1) conducting the resistance spot welding in two stages, a first stage and a second stage; and (2) conducting the second stage with a higher pressure, a lower current or the same current, and a longer current flow time or the same current flow time as the first stage.

[0010] In both Patent Documents 1 and 2, an attempt is made to prevent poor joints in thin plates by dividing one spot welding into two stages and changing the welding conditions in the first stage and the second stage. However, even with these techniques, it is not possible to sufficiently prevent poor joints in plate assemblies with a high plate thickness ratio. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] JP 2003-71569 A [Patent Document 2] JP 2005-262259 A Summary of the Invention [Problem to be solved by the invention]

[0012] In view of the above circumstances, the present invention aims to provide a manufacturing method for a spot-welded component that is capable of suppressing poor joining even when a plate assembly with a thin plate arranged on the surface is used as the base material, and that has high fatigue characteristics, and a spot-welded component. [Means for solving the problem]

[0013] The gist of the present invention is as follows.

[0014] (1) A manufacturing method for a spot-welded component according to one embodiment of the present invention includes a step of performing a first spot welding on a first metal plate and an internal metal plate to form a first joined body having a first nugget that joins the first metal plate and the internal metal plate, and a step of overlapping a second metal plate thicker than the first metal plate on the internal metal plate of the first joined body and performing a second spot welding to form a second nugget that joins the internal metal plate and the second metal plate of the first joined body, thereby bonding the first nugget and the second nugget. (2) In the method for producing a spot-welded component described above in (1), the number of the inner metal plates subjected to the first spot welding may be two or more. (3) In the manufacturing method of spot-welded components described above in (1) or (2), the internal metal plate of the first joint body may be overlapped with one or more other internal metal plates and the second metal plate, and the second spot welding may be performed. (4) In the method for manufacturing a spot-welded component according to any one of the above (1) to (3), a welding point distance between the first nugget and the second nugget may be set to 1.0 mm or more. (5) The method for manufacturing a spot-welded member described in any one of (1) to (4) above may include one or both of a step of bonding the first metal plate and the internal metal plate using an adhesive before the first spot welding, and a step of bonding the internal metal plate of the first joined body and a metal plate overlapping it using an adhesive before the second spot welding. (6) In the manufacturing method of a spot-welded component described in any one of (1) to (5) above, a thickness ratio, which is a value obtained by dividing the total thickness of the metal plates of the spot-welded component by the thickness of the first metal plate, may be greater than 6.0. (7) In the manufacturing method of a spot-welded component described in any one of (1) to (6) above, the metal plate of the spot-welded component may be a steel plate, the tensile strength of the first metal plate may be 440 MPa or less, and the tensile strength of one or more of the metal plates other than the first metal plate may be 1350 MPa or more. (8) A spot-welded component according to another embodiment of the present invention comprises a first metal plate arranged on one surface of the spot-welded component, a second metal plate arranged on the other surface of the spot-welded component and thicker than the first metal plate, an internal metal plate arranged between the first metal plate and the second metal plate, a first nugget joining the first metal plate and the internal metal plate adjacent to it and spaced from the second metal plate, and a second nugget joining the second metal plate and the internal metal plate adjacent to it, wherein the first nugget and the second nugget are joined together. (9) In the spot-welded component described above in (8), the number of the internal metal plates may be two or more. (10) In the spot-welded component described above in (8) or (9), a distance between a center of a hit mark of the first nugget and a center of a hit mark of the second nugget may be 1.0 mm or more. (11) The spot-welded component according to any one of (8) to (10) above may further include an adhesive disposed between the metal plates of the spot-welded component. (12) In the spot-welded component described in any one of (8) to (11) above, a sheet thickness ratio, which is a value obtained by dividing the total sheet thickness of the metal plates of the spot-welded component by the sheet thickness of the first metal plate, may be greater than 6.0. (13) In the spot-welded component described in any one of (8) to (12) above, the metal plates of the spot-welded component may be steel plates, the first metal plate may have a tensile strength of 440 MPa or less, and one or more of the metal plates other than the first metal plate may have a tensile strength of 1350 MPa or more. Effect of the Invention

[0015] According to the present invention, it is possible to provide a manufacturing method for a spot-welded component and a spot-welded component that have high fatigue characteristics and are capable of suppressing poor joining even when a plate assembly with a thin plate arranged on the surface is used as the base material. [Brief description of the drawings]

[0016] [Figure 1A] FIG. 4 is a schematic diagram of a first spot weld S1. [Figure 1B] FIG. 13 is a schematic diagram of a second spot weld S2. [Figure 1C] 11 is a schematic cross-sectional view of the spot-welded member after completion of second spot welding S2. FIG. [Figure 2A] 1 is a cross-sectional photograph of Comparative Example 1. [Figure 2B] 1 is a cross-sectional photograph of Example 2 of the present invention. [Figure 2C] 1 is a cross-sectional photograph of Example 4 of the present invention. [Figure 2D]1 is a cross-sectional photograph of Example 8 of the present invention. [Diagram 3] 1 is a cross-sectional photograph of an example of the present invention after a break test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] In this embodiment, the plate assembly refers to a plurality of overlapping metal plates joined by spot welding. The plate thickness ratio of the plate assembly is a value obtained by dividing the total plate thickness of the metal plates constituting the plate assembly by the thickness of the thinner metal plate located on the surface of the plate assembly.

[0018] The present inventors have conducted extensive research into a method of spot welding a base material made of a plate assembly having a thin plate disposed on a surface thereof. As a result, the present inventors have found that it is advantageous to combine the following measures.

[0019] (1) A first spot weld is performed to join only some of all the metal plates to be welded, and a second spot weld is performed to join the first joint obtained by this to the remaining metal plates. Here, the first metal plate, which is the thinner of the two metal plates located on the surface of the spot welded member, is joined to the internal metal plate in the first spot weld. The total thickness of the first plate group, which is the target of the first spot welding, is smaller than the total thickness of the plate group consisting of all the metal plates. Therefore, the plate thickness ratio of the first plate group (the total plate thickness of the metal plates constituting the first plate group divided by the plate thickness of the above-mentioned first metal plate) is smaller than the plate thickness ratio of the plate group consisting of all the metal plates. Therefore, by performing the first spot welding, it is possible to suppress poor joining between the first metal plate and the internal metal plate.

[0020] (2) A first nugget obtained by the first spot welding and a second nugget obtained by the second spot welding are joined together. Simply performing spot welding twice was not able to sufficiently improve the strength, particularly the fatigue strength, of the spot-welded member. When the present inventors investigated the cause, they found that when vibration is applied to a spot-welded member in which the first nugget and the second nugget are separated, the vibration at the joint becomes significant. The fatigue life of such a spot-welded member was lower than the fatigue life of a welded member obtained by normal spot welding in which all metal plates are joined by one spot welding. On the other hand, when the first nugget and the second nugget were joined together and all metal plates were joined at the same place, the fatigue strength of the spot-welded member was sufficiently ensured.

[0021] However, in order to join the first nugget and the second nugget, the welding point of the first spot welding needs to be close to the welding point of the second spot welding, so the control accuracy of the welding position in the second spot welding needs to be improved.

[0022] In addition, an indentation is generated on the surface of the first metal plate after the first spot welding. The indentation is a depression on the surface of the base material generated by the electrode tip and the disk electrode as a result of welding in lap resistance welding such as spot welding. When the second spot welding is performed at the same location as the first spot welding, the indentation may become a disturbance and cause splashing. Therefore, in the second spot welding, it is preferable to reduce the adverse effects of the indentation by, for example, increasing the pressing force compared to the first spot welding.

[0023] A manufacturing method of a spot-welded member according to one aspect of the present invention, which was obtained based on the above findings, includes a step of performing a first spot welding on the first metal plate 111 and the internal metal plate 11n to form a first joined body 13 having a first nugget 141 that joins the first metal plate 111 and the internal metal plate 11n, and a step of overlapping a second metal plate 112 thicker than the first metal plate 111 on the internal metal plate 11n of the first joined body 13 and performing a second spot welding to form a second nugget 142 that joins the internal metal plate 11n and the second metal plate 112 of the first joined body, thereby joining the first nugget 141 and the second nugget 142. Hereinafter, a manufacturing method of a spot-welded member according to this embodiment will be described in detail.

[0024] (S1 First spot welding) First, as shown in Fig. 1A, a first plate set 12 is prepared by overlapping a first metal plate 111, which is a part of a plurality of metal plates 11 to be welded, and an internal metal plate 11n. A first spot welding is performed on the first plate set 12. A first nugget 141 that joins the first metal plate 111 and the internal metal plate 11n is formed by the first spot welding (see Fig. 1B). The first metal plate 111 is a metal plate disposed on one surface of a spot-welded member.

[0025] The first metal plate 111 is thinner than the second metal plate 112 described later. In normal spot welding in which all metal plates are welded at once, the thin first metal plate 111 may not be joined to the internal metal plate 11n. In this embodiment, the thin first metal plate 111 is incorporated into the first plate group 12, and the first spot welding is performed on the first plate group 12. Since the total plate thickness of the first plate group 12 is small, the plate thickness ratio of the first plate group 12 is smaller than the plate thickness ratio of the plate group consisting of all of the multiple metal plates 11 to be welded. The first spot welding can reliably join the first metal plate 111 and the adjacent internal metal plate 11n.

[0026] As long as this condition is satisfied, the conditions of the first spot welding are not particularly limited. Spot welding conditions can be appropriately adopted according to the material and thickness of the metal plates 11 constituting the first plate group 12, and the strength required for the spot welding member. In FIG. 1A, the first plate group 12 is composed of two metal plates 11, but the first plate group 12 may be composed of three or more metal plates 11. In other words, the number of inner metal plates 11n that are overlapped with the first metal plate 111 before the first spot welding may be two or more. However, in this case, it is desirable that the plate thickness ratio obtained by dividing the total plate thickness of the metal plates constituting the three or more plate group 12 by the plate thickness of the first metal plate 111 is 6.0 or less. Note that as long as the first metal plate 111 and the adjacent inner metal plate 11n are joined, poor joining between the inner metal plates 11n is permitted. This is because, during the subsequent second spot welding, a second nugget 142 is formed that is joined to the first nugget 141, and this poor joining is eliminated. The first nugget 141 may be any nugget that joins the first metal plate 111 and at least the adjacent inner metal plate 11n.

[0027] (S2 Second spot welding) 1B, among the multiple metal plates 11 to be welded, those not included in the first plate set 12 are welded to the first joined body 13. Specifically, the second metal plate 112 is placed on the inner metal plate 11n of the first joined body 13, and a second spot welding is performed therebetween. A second nugget 142 is formed by the second spot welding, joining the inner metal plate 11n of the first joined body 13 and the second metal plate 112 (see FIG. 1C). The second metal plate 112 is a metal plate disposed on the surface of the spot-welded member 1 opposite to the first metal plate 111.

[0028] The first metal plate 111 is the thinner of the two metal plates located on the surface of the spot-welded member. Therefore, when another metal plate 11 is placed on the first joined body 13, the first metal plate 111 and the other metal plate 11 must not be adjacent to each other. It is necessary to place the other metal plate 111 on the surface of the first joined body 13 opposite to the first metal plate 111.

[0029] Furthermore, in the second spot welding, it is necessary to join the first nugget 141 and the second nugget 142. When a load is applied between the first metal plate 111 and the second metal plate 112 in the spot-welded member 1 in which the first nugget 141 and the second nugget 142 are spaced apart, a moment is generated due to a shift in the load transmission position, resulting in significant stress concentration in the welded portion. Therefore, when the first nugget 141 and the second nugget 142 are spaced apart, there is a risk that the strength of the spot-welded member 1, particularly the fatigue strength, may be impaired.

[0030] Whether or not the two nuggets overlap can be determined by cutting the spot-welded member 1 along a plane passing through the nuggets and observing the cut surface. Also, the two nuggets can be joined by bringing the welding point of the second spot welding close to the welding point of the first spot welding.

[0031] As long as this condition is satisfied, the conditions of the second spot welding are not particularly limited. Spot welding conditions can be appropriately adopted according to the material and thickness of the metal plate 11, the strength required for the welded member, and the like. In the method exemplified in FIG. 1B, only one metal plate is joined to the first plate group 12. On the other hand, in the second spot welding, two or more metal plates may be joined to the first plate group 12. Specifically, when the second metal plate 112 is overlapped on the internal metal plate 11n of the first joined body, another internal metal plate 11n may be sandwiched between them. As long as the two nuggets can be joined, the number of internal metal plates 11n sandwiched between the internal metal plate 11n of the first joined body and the second metal plate 112 may be two or more.

[0032] By performing spot welding using the above-mentioned method, it is possible to suppress poor joining even when a plate assembly having a thin plate disposed on the surface is used as the base material, and it is possible to manufacture a spot-welded component having high fatigue properties. On the other hand, by following the conditions exemplified below, it is possible to manufacture the spot-welded component more suitably.

[0033] (Distance d between the first nugget 141 and the second nugget 142) The first nugget 141 and the second nugget 142 need to be overlapped. That is, the welding point of the second spot welding needs to be close to the welding point of the first spot welding. On the other hand, it is not necessary to completely match the welding point of the second spot welding with the welding point of the first spot welding. In addition, according to the results of the experiments conducted by the present inventors, it was found that the joint strength of the spot-welded member 1 can be further increased by setting the center distance d of the strike marks between the first nugget 141 and the second nugget 142 to 1.0 mm or more. That is, it was found that the joint strength of the spot-welded member 1 can be further increased by setting the welding point distance d between the first spot welding and the second spot welding to 1.0 mm or more. In other words, it is preferable that the welding point of the second spot welding and the welding point of the first spot welding are slightly offset from each other. Although the cause of this is not clear at this time, the inventors presume that the shunt current generated in the first nugget 141 during the second spot welding has a positive effect on the formation of the second nugget 142. In addition, in JIS Z 3001-6:2013, the term "welding point interval" is defined as "the distance between the centers of adjacent welding points." The welding point interval d according to this embodiment means the distance between the centers of the welding points of the first nugget 141 and the welding points of the second nugget 142. The "x" marks in FIG. 1C indicate the centers of the welding points. The shunt current refers to a current that flows in a parallel circuit formed by the existing welding points and the workpieces, in addition to the main welding current.

[0034] The center-to-center distance d between the dents and the welding point distance d are values ​​measured along a direction perpendicular to the thickness direction in a cross section that includes the center of the dents of the first nugget 141 and the center of the dents of the second nugget 142 and is parallel to the thickness direction of the spot-welded component 1. Hereinafter, d will be described with reference to FIG. 1C. FIG. 1C is a schematic diagram of the spot-welded component 1 in a cross section that includes the center of the dents of the first nugget 141 and the center of the dents of the second nugget 142 and is parallel to the thickness direction of the spot-welded component 1. The "x" marks in FIG. 1C indicate the centers of the dents, and the vertical direction of the paper is the thickness direction. The center-to-center distance d between the dents and the welding point distance d are measured along the horizontal direction of the paper in FIG. 1C.

[0035] (Pressure force during second spot welding) In general, in spot welding, it is preferable that the surface of the metal plate, which is the base material for welding, is smooth, and that the surface of the metal plate and the central axis of the welding electrode are perpendicular to each other. Irregularities on the surface of the metal plate and the inclination of the welding electrode become disturbances in spot welding and cause splashing. Note that splashing refers to the phenomenon in which the base material is locally overheated and melts and splashes during lap resistance welding such as spot welding, or the metal itself.

[0036] On the other hand, in the manufacturing method of the spot-welded member according to the present embodiment, a dent is formed on the surface of the first joint body 13. Furthermore, in order to join the two nuggets, the welding point of the second spot welding needs to be overlapped with this dent. Therefore, the dent caused by the first spot welding may become a disturbance in the second spot welding, which may cause unexpected defects such as expulsion.

[0037] When the occurrence of expulsion is not allowed, it is preferable to set the pressure applied during the second spot welding to 350 kgf (3.432 kN) or more, which can suppress the occurrence of expulsion and further improve the quality of the spot-welded member.

[0038] In the manufacturing method of the spot-welded member according to this embodiment, the metal plates 111 may be joined by using a means other than spot welding in combination. This makes it possible to further increase the joint strength of the spot-welded member 1.

[0039] (glue) An example of a joining means other than spot welding is an adhesive. For example, the first metal plate 111 and the internal metal plate 11n may be bonded together using an adhesive before the first spot welding. Also, the internal metal plate 11n of the first joined body 13 and the metal plate 11 (the second metal plate 112 or the internal metal plate 11n) overlapping therewith may be bonded together using an adhesive before the second spot welding. Bonding with an adhesive may be performed both before the first spot welding and before the second spot welding.

[0040] As described above, the type of metal plate 11 used in the manufacturing method of the spot-welded member according to the present embodiment is not particularly limited. In addition, as long as the first metal plate 111 is thinner than the second metal plate 112, the thickness of each of the multiple metal plates 11 is not particularly limited. According to the manufacturing method of the spot-welded member according to the present embodiment, poor joining of the thin first metal plate 111 can be suppressed, so that the range of material selection is expanded. A suitable example of the material will be described below.

[0041] (plate thickness ratio) The plate thickness ratio of the plate assembly is a value obtained by dividing the total plate thickness of the metal plates constituting the plate assembly by the thickness of the thinner of the metal plates located on the surface of the plate assembly. When the spot-welded member 1 is regarded as a plate assembly, the plate thickness ratio of the spot-welded member 1 is a value obtained by dividing the total plate thickness of the metal plates 11 included in the spot-welded member 1 by the plate thickness of the first metal plate 111. In the manufacturing method of the spot-welded member according to the present embodiment, the plate thickness ratio of the spot-welded member 1 may be more than 6.0. In normal spot welding, in order to suppress poor joining of thin plates, the plate thickness ratio is usually set to 6.0 or less. However, in the manufacturing method of the spot-welded member according to the present embodiment, poor joining of thin plates is suppressed by performing the first spot welding. Therefore, even if the plate thickness ratio of the spot-welded member 1 exceeds 6.0, poor joining does not occur.

[0042] (Metal plate material and tensile strength) Spot welding is widely used in the manufacture of automobile parts. Therefore, the manufacturing method of the spot-welded member according to the present embodiment may be applied to automobile parts. In this case, for example, the first metal plate 111 is an exterior part of an automobile that requires high workability. The other metal plates 11 are structural parts of an automobile that require high strength. Therefore, the metal plate 11 may be a steel plate, the tensile strength of the first metal plate 111 may be 440 MPa or less, and the tensile strength of one or more of the metal plates 11 other than the first metal plate 111 may be 1350 MPa or more. This facilitates the processing of the exterior part of the automobile and ensures the strength of the structural parts of the automobile.

[0043] In spot welding between a high-strength steel plate and mild steel, the nugget tends to be formed biased toward the high-strength steel plate. This is because high-strength steel plate contains more alloy elements than mild steel, and these alloy elements increase the electrical resistance of the high-strength steel plate. In spot welding between a high-strength steel plate and mild steel, resistance heating occurs preferentially in the high-strength steel plate, which has a high electrical resistance. When spot welding between a high-strength steel plate and mild steel is performed by conventional means, the outer edge of the nugget formed does not reach the mild steel, and there is a risk of poor joining of the mild steel. However, in the manufacturing method of the spot-welded member according to the present embodiment, poor joining of the thin plate is suppressed by performing the first spot welding. Therefore, even if the first metal plate 111 is made of mild steel and the other metal plate 11 is made of high-strength steel, poor joining does not occur. On the other hand, the material of the metal plate may be other than steel plate. For example, various materials such as aluminum plate and stainless steel plate can be used as the metal plate 11. When the metal plate arranged on the surface of the spot-welded member is thin, there is a risk of poor joining, regardless of the type of metal plate. In addition, the method for suppressing poor joining used in the method for joining spot-welded members according to this embodiment is applicable regardless of the material of the metal plate 11.

[0044] (nugget diameter) The sizes of the first nugget 141 and the second nugget 142 are not particularly specified. As long as the above-mentioned requirements are satisfied, an appropriate nugget diameter can be adopted according to the material, thickness, number, etc. of the metal plates 11. For example, when the sheet thickness of the first metal plate 111 is 0.4 mm to 0.9 mm and the total sheet thickness of the metal plates 11 of the spot-welded member 1 is 3.5 mm to 7.0 mm, it is preferable that the diameter of the first nugget 141 is 3√(t1) to 8√(t1) and the diameter of the second nugget 142 is 3√(t2) to 8√(t2). Here, the first nugget diameter is the width of the molten solidified portion measured along the overlapping surface between the first metal plate 111 and the adjacent internal metal plate 11n. The measurement of the width of the molten solidified portion is performed on a cross section (a cross section when measuring the above-mentioned welding point interval d) that includes the center of the strike mark of the first nugget 141 and the center of the strike mark of the second nugget 142 and is parallel to the plate thickness direction of the spot-welded member 1. As shown in FIG. 1C, the first nugget and the second nugget may be fused on the overlapping surface between the first metal plate 111 and the adjacent internal metal plate 11n. In this case, the width of the molten solidified portion including both the first nugget 141 and the second nugget 142 is regarded as the diameter of the first nugget 141. The second nugget diameter is the diameter of the molten solidified portion measured on the overlapping surface between the second metal plate 112 and the adjacent internal metal plate 11n. The measurement of the width of the molten solidified portion is performed on the above-mentioned cross section. t1 is the sheet thickness (mm) of the first metal sheet 111, and t2 is the sheet thickness (mm) of the second metal sheet 112. The nugget diameter can be controlled by appropriately changing the current application conditions according to the material, thickness, number, etc. of the metal sheets 11.

[0045] (Welding conditions) The conditions of the first spot welding and the second spot welding are not particularly specified. As long as the above-mentioned requirements are satisfied, appropriate welding conditions can be adopted according to the material, thickness, number, etc. of the metal plates 11. In each of the first spot welding and the second spot welding, the number of energizations may be one or more than two. Also, an upslope may be used at the start of energization and a downslope may be used at the end of energization. A suitable example of the welding conditions is a DR type electrode with an electrode tip of 5 mm to 8 mm, a pressure of 250 kgf to 700 kgf (2.451 kN to 6.864 kN), energization time: 12 cycles to 60 cycles (240 msec to 1200 msec), a current value: 6 kA to 12 kA, and a retention time of 1 cycle to 60 cycles (20 msec to 1200 msec).

[0046] Next, a spot-welded member according to another embodiment of the present invention will be described. As shown in Fig. 1C, the spot-welded member 1 according to this embodiment includes a first metal plate 111 arranged on one surface of the spot-welded member 1, a second metal plate 112 arranged on the other surface of the spot-welded member 1 and thicker than the first metal plate 111, an inner metal plate 11n arranged between the first metal plate 111 and the second metal plate 112, a first nugget 141 that joins the first metal plate 111 and the adjacent inner metal plate 11n and is spaced from the second metal plate 112, and a second nugget 142 that joins the second metal plate 112 and the adjacent inner metal plate 11n, and the first nugget 141 and the second nugget 142 are joined together.

[0047] The metal plates 111 of the spot-welded member 1 are roughly divided into a first metal plate 111 and a second metal plate 112 arranged on the surface of the member, and an internal metal plate 11n arranged inside the member. In the spot-welded member 1, the metal plates arranged on the surface of the member (particularly the first metal plate 111 having a thin plate thickness) are most likely to cause poor joining. Therefore, the thickness, number, and other configurations of the internal metal plates 11n arranged inside the member are not particularly limited. For example, the number of internal metal plates 11n illustrated in FIG. 1C is only one, but the number of internal metal plates 11n may be two or more.

[0048] The first metal plate 111 is joined to the adjacent inner metal plate 11n by the first nugget 141. The first nugget 141 is also spaced apart from the second metal plate 112 on the opposite side of the first metal plate 111. As a result, when looking at the cross section of the spot-welded member 1, the first nugget 141 is disposed in a position biased toward the first metal plate 111. As described above, in the spot-welded member 1, the metal plate (particularly the first metal plate 111 having a thin plate thickness) disposed on the surface of the member is most likely to have a poor joint. However, in the spot-welded member according to this embodiment, the first nugget 141 is disposed biased toward the first metal plate 111, thereby suppressing poor joints of the first metal plate 111.

[0049] The second metal plate 112 is joined to the adjacent inner metal plate 11n by the second nugget 142. The second nugget 142 is also joined to the first nugget 141. Therefore, when looking at a cross section of the spot-welded component 1, all of the metal plates 111 are joined at the same location. This makes it possible to suppress stress concentration at the joint due to the generation of a moment when a load is applied between the first metal plate 111 and the second metal plate 112, and to increase the fatigue strength of the spot-welded component 1.

[0050] The method for manufacturing the spot-welded member 1 according to this embodiment is not particularly limited, but for example, the above-mentioned method for manufacturing the spot-welded member is preferable. In addition, a preferable form of the spot-welded member 1 may be similar to the preferable form of the above-mentioned method for manufacturing the spot-welded member. Preferred forms of the spot-welded member 1 are exemplified below.

[0051] (Distance d between the first nugget 141 and the second nugget 142) In the spot-welded member 1 according to this embodiment, the distance d between the center of the dent in the first nugget 141 and the center of the dent in the second nugget 142 may be set to 1.0 mm or more. This has been found to further increase the joint strength of the spot-welded member 1. According to the results of experiments conducted by the present inventors, it has been found that the joint strength of the spot-welded member 1 can be further increased by setting the center distance d between the dents in the first nugget 141 and the second nugget 142 to 1.0 mm or more. In other words, it is preferable that the welding point of the second spot weld and the welding point of the first spot weld are slightly offset from each other.

[0052] (Falling) The spot-welded member 1 according to the present embodiment preferably does not include splashing. Splashing refers to a phenomenon in which the base material is locally overheated and melts and splashes in lap resistance welding such as spot welding, or the metal involved. Splashing impairs the appearance and strength of the spot-welded member 1 and pollutes the welding environment, so it is preferable to suppress it. The spot-welded member 1 according to the present embodiment has multiple nuggets at the same location, so splashing is likely to occur during manufacturing, particularly when the second nugget is formed. However, for example, the occurrence of splashing can be suppressed by setting the pressure applied during the second spot welding to 350 kgf (3.432 kN) or more.

[0053] (glue) The spot-welded member 1 according to this embodiment may have a joining means other than a nugget. For example, the spot-welded member 1 according to this embodiment may further include an adhesive disposed between the metal plates 11. The metal plates 11 are a term that collectively refers to the first metal plate 111, the second metal plate 112, and the inner metal plate 11n. The spot-welded member 1 according to this embodiment has three or more metal plates 11, and therefore has two or more joining interfaces. By disposing an adhesive at one or more joining interfaces, the rigidity and joining strength of the spot-welded member 1 can be further increased.

[0054] (plate thickness ratio) In the spot-welded member 1 according to this embodiment, the sheet thickness ratio, which is the value obtained by dividing the total sheet thickness of the metal sheets 11 of the spot-welded member 1 by the sheet thickness of the first metal sheet 111, may be more than 6.0. In a typical spot-welded member, the sheet thickness ratio is usually set to 6.0 or less to suppress poor joining of the thin sheet. However, in the spot-welded member 1 according to this embodiment, the first nugget 111 formed biased toward the first metal sheet 111 suppresses poor joining of the thin sheet. Therefore, even if the sheet thickness ratio of the spot-welded member 1 exceeds 6.0, poor joining does not occur.

[0055] (Metal plate material and tensile strength) In the spot-welded member 1 according to this embodiment, the metal plates 11 are steel plates, the first metal plate 111 has a tensile strength of 440 MPa or less, and one or more of the metal plates 11 other than the first metal plate 111 may have a tensile strength of 1350 MPa or more. This allows the spot-welded member 1 according to this embodiment to be suitably used as an automobile part.

[0056] (nugget diameter) In the spot-welded member 1 according to this embodiment, the first metal plate 111 may have a thickness of 0.4 mm to 0.9 mm, the metal plates 11 included in the spot-welded member 1 may have a total thickness of 3.5 mm to 7.0 mm, the first nugget 141 may have a diameter of 3√(t1) to 8√(t1), and the second nugget 142 may have a diameter of 3√(t2) to 8√(t2). t1 is the thickness (mm) of the first metal plate 111, and t2 is the thickness (mm) of the second metal plate 112. This can further increase the joint strength of the spot-welded member 1. EXAMPLES

[0057] The effects of one embodiment of the present invention will be explained more specifically with reference to an example. However, the conditions in the example are merely an example of conditions adopted to confirm the feasibility and effects of the present invention. The present invention is not limited to this example of conditions. Various conditions may be adopted in the present invention as long as they do not deviate from the gist of the present invention and the object of the present invention is achieved.

[0058] Various plate pairs shown in Table 1 were spot-welded to manufacture spot-welded members. Specifically, first, a first spot welding (first welding) was performed on steel plate 1 and steel plate 2 to form a first joint having a first nugget. Next, steel plate 3 (or steel plate 3 and steel plate 4) was superimposed on steel plate 2, and a second spot welding (second welding) was performed to form a second nugget. Destructive tests were performed on various spot-welded members obtained in this manner. However, in Example 1, the second welding was not performed, and only the first welding was performed on the plate pair formed by superimposing steel plates 1 to 3 in this order. In Example 7, the second welding was not performed, and only the first welding was performed on the plate pair formed by superimposing steel plates 1 to 4 in this order.

[0059] In the columns of "Steel Plate 1" to "Steel Plate 4" in Table 1, the tensile strength (unit: MPa), the coating type, and the thickness t (unit: mm) of the steel plates are listed in order. GA stands for galvannealed hot-dip coating. For steel plates without coating, the coating type is omitted. For reference, the sheet thickness ratio of the sheet combination composed of Steel Plate 1 to Steel Plate 4 is listed in Table 1. Among the spot-welded members obtained by welding these, in the one in which three steel plates are joined, Steel Plate 1 is regarded as the first metal plate 111, Steel Plate 3 is regarded as the second metal plate 112, and Steel Plate 2 is regarded as the inner metal plate 11n. In the welded member in which four steel plates are joined, Steel Plate 1 is regarded as the first metal plate 111, Steel Plate 4 is regarded as the second metal plate 112, and Steel Plates 2 and 3 are regarded as the inner metal plates 11n.

[0060] In the columns "First welding" and "Second welding" in Table 2, the electrode pressure (unit: kgf, 1 kgf is approximately 9.8 N), welding current value (unit: kA), and welding time (time during which welding current is passed, unit cycle, 1 cycle is 1 / 50 seconds) in the first spot welding are listed in that order. In Examples 9 and 10, the second welding was performed with two current passes. Two current passes are welding in which current is passed twice during one welding pressure pass. Table 2 also lists the no-current time (unit cycle) between the two current passes. In the two current passes, the pressure was constant. In Examples 1 and 7, the second welding was not performed, so the welding conditions were not listed in the "Second welding" column.

[0061] The distance between the first and second welds (unit: mm) is given in the column "Distance of second weld position" in Table 2. The distance between the weld points is the distance between the centers of adjacent weld points.

[0062] The destructive test was carried out by a chisel test as specified in JIS Z 3144:2013 "Field test method for spot and projection welds." Specifically, a chisel was pressed between steel plate 1 and steel plate 2 near the weld to apply a tensile force in the plate thickness direction of the weld, and it was judged whether the joint strength between steel plate 1 and steel plate 2 was good or not. The weld was broken between the steel plate 1 and the steel plate 2 of each test piece by driving a chisel. Then, the diameter of the weld (the diameter of the steel plate 1 remaining on the steel plate 2 after the break) was measured according to the method described in 7.2 "Measurement of the weld diameter and plug diameter" of JIS Z 3144:2013. For spot-welded members in which the diameter of the weld is 4.25√t (t is the thickness of the steel plate 1) or more, "◎" was recorded in the "First steel plate side destructive test result". For spot-welded members in which the diameter of the weld is 3√t or more and less than 4.25√t, "○" was recorded, and for spot-welded members in which the diameter of the weld is less than 3√t, "×" was recorded. In Example 5, the welding point interval of the first weld and the second weld was large, and the first nugget and the second nugget were not bonded. The destructive test of this Example 5 was performed on the second nugget. A cross-tensile fatigue test was also carried out by applying a load between steel plate 1 and steel plate 3 (between steel plate 1 and steel plate 4 in the case of four overlapping plates). The fatigue test was carried out in accordance with JIS Z 3138:1989 "Fatigue test method for spot welded joints". Results that passed the fatigue test are marked with "○", and results that failed are marked with "×".

[0063] [Table 1]

[0064] [Table 2]

[0065] Examples 1 and 7 were obtained by a conventional manufacturing method of spot-welded components in which spot welding was performed only once. In Examples 1 and 7, the plate thickness ratio was very large, so a joint failure occurred with respect to the steel plate 1, which was a thin plate arranged on the surface of the spot-welded component.

[0066] Example 5 was obtained by a manufacturing method of a spot-welded component in which spot welding was performed twice but the two nuggets were not joined. In Example 5, the sheet thickness ratio was also very large, so in the second nugget, a joint failure occurred with respect to the steel sheet 1, which was a thin sheet arranged on the surface of the spot-welded component. Although there is a possibility that a joint failure did not occur in the first nugget of Example 5, the welded component of Example 5 had insufficient fatigue resistance because all the steel sheets were not joined at the same location.

[0067] On the other hand, the spot-welded components obtained by the manufacturing method of the present invention, in which two spot welds are performed and two nuggets are joined, have high joint strength even though the thin plate is arranged on the surface and the plate thickness ratio is very high. Furthermore, since all the steel plates are joined at the same place, these spot-welded components have high fatigue resistance.

[0068] For reference, cross-sectional photographs of the nuggets of Examples 1, 2, 4, and 8 are shown in Figures 2A to 2D. In the cross-sectional photograph of Example 1 (Figure 2A), it can be seen that the nugget does not extend to the steel plate 1. On the other hand, in the spot-welded members of Examples 2 (Figure 2B), 4 (Figure 2C), and 8 (Figure 2D), the first nugget and the second nugget overlap, and the first nugget extends to the steel plate 1.

[0069] An example of a cross-sectional photograph after the destructive test is shown in Figure 3. In this spot-welded component, the steel plate 1 was well joined to the adjacent steel plate 2, so that a large amount of the steel plate 1 remained in the weld after the destructive test. [Explanation of symbols]

[0070] 1 Spot welding parts 11 Metal plate 111 First metal plate 112 Second Metal Plate 11n internal metal plate 12 First board assembly 13 First zygote 141 The First Nugget 142 The Second Nugget A electrode d Distance between the center of the impact mark on the first nugget and the center of the impact mark on the second nugget t1 Thickness of the first metal plate

Claims

1. performing a first spot welding on a first metal plate and an inner metal plate to form a first joined body having a first nugget joining the first metal plate and the inner metal plate; a step of overlapping a second metal plate thicker than the first metal plate on the internal metal plate of the first joined body, and performing second spot welding to form a second nugget joining the internal metal plate of the first joined body and the second metal plate; Equipped with The first nugget and the second nugget are bonded together. A manufacturing method for spot welded components.

2. The number of the inner metal plates subjected to the first spot welding is 2 or more. The method for manufacturing a spot-welded component according to claim 1 .

3. The second spot welding is performed by overlapping one or more other internal metal plates and the second metal plate on the internal metal plate of the first joint body.

3. The method for manufacturing a spot-welded component according to claim 1 or 2.

4. The distance between the first nugget and the second nugget is set to 1.0 mm or more. The method for manufacturing a spot-welded component according to any one of claims 1 to 3.

5. prior to the first spot welding, bonding the first metal plate and the inner metal plate with an adhesive; and a step of bonding the inner metal plate of the first joint body and a metal plate overlapping the inner metal plate with an adhesive prior to the second spot welding; The method for manufacturing a spot-welded component according to any one of claims 1 to 4, characterized in that the method further comprises one or both of the following:

6. A plate thickness ratio, which is a value obtained by dividing the total plate thickness of the metal plates of the spot-welded member by the plate thickness of the first metal plate, is set to be more than 6.

0. The method for manufacturing a spot-welded component according to any one of claims 1 to 5.

7. The metal plate of the spot welded member is a steel plate, The tensile strength of the first metal plate is 440 MPa or less, The tensile strength of at least one of the metal plates other than the first metal plate is 1350 MPa or more. The method for manufacturing a spot-welded component according to any one of claims 1 to 6.

8. A spot welded member, a first metal plate disposed on one surface of the spot welded component; a second metal plate disposed on the other surface of the spot welded member and having a thickness greater than that of the first metal plate; an inner metal plate disposed between the first metal plate and the second metal plate; a first nugget joining the first metal plate and the adjacent inner metal plate and spaced apart from the second metal plate; a second nugget joining the second metal plate and the adjacent inner metal plate; Equipped with the first nugget and the second nugget are joined together, The distance between the center of the dent of the first nugget and the center of the dent of the second nugget is 1.0 mm or more. Spot welded components.

9. The number of the internal metal plates is two or more.

9. The spot welded component according to claim 8.

10. The spot welded member further includes an adhesive disposed between the metal plates.

10. The spot-welded component according to claim 8 or 9.

11. A plate thickness ratio, which is a value obtained by dividing the total plate thickness of the metal plates of the spot-welded component by the plate thickness of the first metal plate, is greater than 6.

0. The spot welded component according to any one of claims 8 to 10.

12. The metal plate of the spot welded member is a steel plate, The tensile strength of the first metal plate is 440 MPa or less, At least one of the metal plates other than the first metal plate has a tensile strength of 1350 MPa or more. The spot welded component according to any one of claims 8 to 11.

Citation Information

Patent Citations

  • Spot welding method

    JP2003071569A

  • Method for manufacturing resistance spot welded joint

    JP2005262259A

  • Resistance spot welding method

    JP2008290099A

  • Resistance spot welding method of high-strength steel sheet

    JP2010172945A

  • Resistance spot welding method

    JP2013052413A