Room temperature curable polyorganosiloxane composition and electrical / electronic device
The polyorganosiloxane composition addresses additive mixing issues by using alkoxysilyl-capped polyorganosiloxane and silane compounds, ensuring stable, uniform dispersion and smooth films for electronic components, while avoiding solvent use.
Patent Information
- Application Number
- JP2020190812
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-17
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2040-11-17
AI Technical Summary
Conventional room-temperature-curable polyorganosiloxane compositions face challenges in uniformly mixing large amounts of additives, leading to precipitation or phase separation, and require solvent removal, which can harm the environment and components.
A polyorganosiloxane composition comprising polyorganosiloxane capped with alkoxysilyl groups, silane compounds, an organic titanium catalyst, and additives, allowing for increased additive content and stable curing without solvents, with components (B1) and (B2) adjusting viscosity and surface hardness.
The composition enables stable, uniform mixing and dispersion of additives, forming a smooth cured film with enhanced functional properties, suitable for electronic devices, and prevents environmental solvent release.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a room-temperature-curable polyorganosiloxane composition and an electric / electronic device, and in particular to a room-temperature-curable polyorganosiloxane composition that can increase the solubility of additives for imparting predetermined properties and increase the content thereof, and is useful as a coating material for electric / electronic devices, and an electric / electronic device having a cured coating of the room-temperature-curable polyorganosiloxane composition. [Background technology]
[0002] Conventionally, various room temperature curable polyorganosiloxane compositions that cure at room temperature to produce rubber-like cured products have been known. Among them, for applications such as coating materials and potting materials for electric and electronic components, those that undergo a curing reaction upon contact with moisture in the air and release alcohol, acetone, etc., which are less corrosive to metals when cured, are generally used because they are easy to work with, have little risk of corrosion of electrodes and wiring, and have excellent adhesive properties.
[0003] In particular, as conformal coating agents applied to protect the surfaces of electric / electronic components and circuit boards on which they are mounted from the environment in which they are used, coating materials made of low-viscosity room-temperature curable polyorganosiloxane compositions (see, for example, Patent Documents 1 and 2) and coating materials in which silicone resin is dissolved in a solvent are used.
[0004] However, in the case of a solvent-type coating material containing a silicone resin as a coating material made of such a low-viscosity room-temperature curable polyorganosiloxane composition, the solvent needs to be removed by heating during curing, and the evaporation of the solvent may cause a deterioration of the working environment and corrosion or deterioration of electric and electronic components and the circuit boards on which they are mounted. Furthermore, in order to improve the working environment, a large investment is required to recover the solvent without releasing it into the atmosphere.
[0005] In order to solve such problems, room temperature curable polyorganosiloxane compositions that have low viscosity, are solvent-free, and form cured coatings with good applicability are also known (see, for example, Patent Document 3).
[0006] Furthermore, various additives are often incorporated into such room temperature curable polysiloxane compositions in order to impart additional functions such as rust prevention and ultraviolet light resistance. However, when such additives are blended in large amounts, they cannot be mixed uniformly in the composition, and solid additives may precipitate or crystallize, and liquid additives may form a two-phase structure, making it difficult to increase the content. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 7-173435 [Patent Document 2] Japanese Patent Application Publication No. 7-238259 [Patent Document 3] International Publication No. 2014 / 017397 Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been made to solve the above problems, and has an object to provide a room-temperature curable polyorganosiloxane composition that allows the content of additives to be increased more than before, can enhance the functions imparted by the additives, and can stably form a cured coating. [Means for solving the problem]
[0009] The room-temperature-curable polyorganosiloxane composition of the present invention comprises (A) a polyorganosiloxane having both ends capped with alkoxysilyl groups, represented by the following general formula (1):
[0010] [ka] (In the formula, R 1 R is an alkyl group or an alkoxy-substituted alkyl group in which some of the hydrogen atoms of the alkyl group are substituted with alkoxy groups; 2 and R 3 is an unsubstituted monovalent hydrocarbon group or a monovalent hydrocarbon group in which some of the hydrogen atoms are substituted with halogen atoms or cyanoalkyl groups, and X is a divalent oxygen (oxy group) or a divalent hydrocarbon group. Also, a is 0 or 1, and n is a number such that the viscosity at 23°C is in the range of 5 to 10,000 mPa s.) Per 100 parts by mass of (B) (B1) a silane compound represented by the following general formula (2): R 4 b Si(OR 5 ) 4-b …(2) (In the formula, R 4 is a monovalent substituted or unsubstituted hydrocarbon group, R 5 represents a monovalent group selected from the group consisting of alkyl groups having 1 to 4 carbon atoms and alkoxyalkyl groups having a total of 1 to 6 carbon atoms, and b represents 0 or 1), or a partial hydrolysis condensate thereof, and (B2) a silane compound represented by the following general formula (3): R 6 2 Si(OR 7 ) 2 …(3) (In the formula, R 6 is a monovalent substituted or unsubstituted hydrocarbon group, R 7 (R) represents a monovalent group selected from the group consisting of alkyl groups having 1 to 4 carbon atoms and alkoxyalkyl groups having a total of 1 to 6 carbon atoms) or a partial hydrolysis condensate thereof; (C) 0.1 to 15 parts by mass of an organic titanium compound as a curing catalyst; and (D) 0.0001 to 10 parts by mass of an additive.
[0011] The electric / electronic device of the present invention is characterized in that it has a coating made of a cured product of the above-mentioned room-temperature-curable polyorganosiloxane composition of the present invention on the surface of an electrode and / or wiring.
[0012] In this specification, the term "alkoxysilyl group" refers to a group in which at least one alkoxy group is bonded to a silicon atom. In this specification, the term "dialkoxysilyl group" is also referred to as a difunctional group or a difunctional silyl group. Similarly, the term "trialkoxysilyl group" is also referred to as a trifunctional group or a trifunctional silyl group. Effect of the Invention
[0013] The room temperature curable polyorganosiloxane composition of the present invention allows the content of additives to be increased more than before, and the function imparted by the additives can be enhanced, and a cured coating can be stably formed. In addition, according to this room temperature curable polyorganosiloxane composition, it is preferable to suppress the formation of wrinkles and the like, and to make the surface of the cured coating smooth. Therefore, this room-temperature-curable polyorganosiloxane composition is useful as a coating material, potting material, etc. for electric and electronic devices, and is particularly suitable for applications such as conformal coating agents for coating electric and electronic components. [Brief description of the drawings]
[0014] [Figure 1] 1 is a cross-sectional view showing an example of an electric / electronic device of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, a room-temperature curable polyorganosiloxane composition and an electric / electronic device according to one embodiment of the present invention will be described. The room-temperature-curable polyorganosiloxane composition of the present embodiment is a polyorganosiloxane having both ends capped with alkoxysilyl groups, represented by the following general formula (1):
[0016] [ka] (In the formula, R 1R is an alkyl group or an alkoxy-substituted alkyl group in which some of the hydrogen atoms of the alkyl group are substituted with alkoxy groups; 2 and R 3 is an unsubstituted monovalent hydrocarbon group or a monovalent hydrocarbon group in which some of the hydrogen atoms are substituted with halogen atoms or cyanoalkyl groups, and X is a divalent oxygen (oxy group) or a divalent hydrocarbon group. Also, a is 0 or 1, and n is a number that provides a viscosity at 23°C in the range of 5 to 10,000 mPa s.) Per 100 parts by mass of (B) (B1) a silane compound represented by the following general formula (2): R 4 b Si(OR 5 ) 4-b …(2) (In the formula, R 4 is a monovalent substituted or unsubstituted hydrocarbon group, R 5 represents a monovalent group selected from the group consisting of alkyl groups having 1 to 4 carbon atoms and alkoxyalkyl groups having a total of 1 to 6 carbon atoms, and b represents 0 or 1), or a partial hydrolysis condensate thereof, and (B2) a silane compound represented by the following general formula (3): R 6 2 Si(OR 7 ) 2 …(3) (In the formula, R 6 is a monovalent substituted or unsubstituted hydrocarbon group, R 7 (represents a monovalent group selected from the group consisting of alkyl groups having 1 to 4 carbon atoms and alkoxyalkyl groups having a total of 1 to 6 carbon atoms) or a partial hydrolysis condensate thereof, (C) 0.1 to 15 parts by mass of an organic titanium compound as a curing catalyst, and (D) 0.0001 to 10 parts by mass of an additive. Each component will be described below.
[0017] In this embodiment, the polyorganosiloxane which is the component (A) serves as the base polymer of the present composition, and is a specified polyorganosiloxane capped at both ends with alkoxysilyl groups.
[0018] The component (A), polyorganosiloxane capped at both ends with alkoxysilyl groups, is, for example, a substantially linear polyorganosiloxane represented by the following general formula (1).
[0019] [ka]
[0020] In formula (1), R 1 is an alkyl group or an alkoxy-substituted alkyl group in which some of the hydrogen atoms of the alkyl group are substituted with alkoxy groups. 1 may be the same or different. 1 Specific examples of the alkyl group include a methyl group, an ethyl group, a propyl group, and a butyl group, and specific examples of the alkoxy-substituted alkyl group include a 2-methoxyethyl group, a 2-ethoxyethyl group, and a 3-methoxypropyl group. 1 is preferably a methyl group.
[0021] R 2 is an unsubstituted monovalent hydrocarbon group or a monovalent hydrocarbon group in which some of the hydrogen atoms are substituted with halogen atoms or cyanoalkyl groups. 2 may be the same or different. 3 Each R is an unsubstituted monovalent hydrocarbon group or a monovalent hydrocarbon group in which some of the hydrogen atoms are substituted with halogen atoms or cyanoalkyl groups. 3 may be the same or different from each other.
[0022] Above R 2 and R 3 Specific examples of the unsubstituted monovalent hydrocarbon group include alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, octyl, decyl, and dodecyl; cycloalkyl groups such as cyclohexyl; alkenyl groups such as vinyl and allyl, aryl groups such as phenyl, tolyl, and xylyl; and aralkyl groups such as benzyl, 2-phenylethyl, and 2-phenylpropyl.
[0023] Above R 2 and R 3 Examples of the substituted monovalent hydrocarbon group include the above monovalent hydrocarbon group in which some of the hydrogen atoms have been replaced with halogen atoms, such as halogenated alkyl groups such as chloromethyl, 3-chloropropyl, and 3,3,3-trifluoropropyl, and the above monovalent hydrocarbon group in which some of the hydrogen atoms have been replaced with cyanoalkyl groups, such as 3-cyanopropyl. R is preferred because it is easy to synthesize, has a low viscosity relative to its molecular weight, and provides good physical properties to the cured product (cured coating). 2 and R 3 is preferably a methyl group. However, when it is necessary to impart heat resistance or cold resistance to the cured coating, R 2 and / or R 3 It is preferable that a portion of the formula (I) is an aryl group such as a phenyl group.
[0024] In addition, X is a divalent oxygen atom (oxy group) or a divalent hydrocarbon group. The two X's may be the same or different. Examples of divalent hydrocarbons include alkylene groups such as methylene, ethylene, propylene, and trimethylene groups, and arylene groups such as phenylene groups. From the viewpoint of ease of synthesis, a divalent oxygen atom (oxy group) or an ethylene group is preferred, and an oxy group is particularly preferred.
[0025] In formula (1), a is 0 or 1, and n is a number that provides a viscosity at 23°C in the range of 5 to 10,000 mPa s, for example, an integer of 1≦n≦200. If the value of n is 200 or more, there is a risk of component (A) separating out from the composition. More preferably, the value of n is an integer of 1 to 100, and the viscosity is 5 to 5,000 mPa.
[0026] The polyorganosiloxane capped at both ends with alkoxysilyl groups, which is component (A), can be obtained, for example, by ring-opening polymerization or ring-opening copolymerization of a cyclic diorganosiloxane oligomer such as octamethylsiloxane in the presence of water using an acidic or alkaline catalyst to produce a diorganopolysiloxane containing hydroxyl groups at both ends, and then reacting this with methyltrimethoxysilane or the like to cap the hydroxyl groups at both ends with methoxy groups or the like.
[0027] The viscosity of this component (A) at 23°C is preferably 5 to 10,000 mPa·s, more preferably 5 to 5,000 mPa. When two or more types of polyorganosiloxanes are mixed as the component (A), it is preferable that the viscosity after mixing falls within the above range. In this specification, unless otherwise specified, the viscosity is a value measured at 23°C according to JIS K6249, for example, using a rotational viscometer (manufactured by Shibaura Semtec Co., Ltd., product name: Vismetron VDA-2) at rotation speeds of 30 rpm and 60 rpm, and rotor No. 2.
[0028] Regarding the above general formula (1), when two or more types of polyorganosiloxanes are mixed, for example, a preferred example is a mixture of (A1) a polyorganosiloxane having a viscosity of 5 to 200 mPa s at 23°C and (A2) a polyorganosiloxane having a viscosity of 500 to 100,000 mPa s at 23°C. In this case, component (A) preferably contains 50 to 100 mass% of (A1) a polyorganosiloxane having a viscosity of 5 to 200 mPa s at 23°C, more preferably 60 to 100 mass%, and even more preferably 70 to 100 mass%.
[0029] In consideration of workability and flowability, a low viscosity non-reactive siloxane, such as a polysiloxane containing a terminal trialkylsilyl group, may be blended with component (A) as necessary.
[0030] In this embodiment, component (B) is a crosslinking agent component that acts to crosslink the polyorganosiloxane of component (A). Component (B) is characterized in that it is a silane mixture that uses components (B1) and (B2) described below in combination.
[0031] In this embodiment, the component (B1) is a silane compound represented by the following general formula (2), or a partial hydrolysis condensate thereof. R 4 b Si(OR 5 ) 4-b ……(2) In formula (2), R 4 is an unsubstituted monovalent hydrocarbon group or a monovalent hydrocarbon group in which some of the hydrogen atoms are substituted with halogen atoms or cyanoalkyl groups, and R 2 Examples of R are the same as those of R, and a methyl group is preferable. 5 is an alkyl group or an alkoxy-substituted alkyl group, and R 1 Examples of the aryl group include the same groups as those shown below, and a methyl group is preferable. Furthermore, b is 0 or 1, and the average value of b is 0 to 1.0. The average value of b is preferably 0.5 to 1.0.
[0032] The value of b is the number of R bonded to a silicon atom in the silane compound represented by formula (2). 4 And the average value of this number b is 0 to 1.0, R 4 This means that one or more silane compounds, each having a value of 0 or 1 for b, which is the number of bonds, are blended together such that the average value of b is 0 to 1.0 by adjusting the molar ratio of each silane compound.
[0033] For example, when the average value of b is in the range of 0.8 to 1.0, the compound in which b is 0 in formula (2): Si(OR 5 ) 4 and a compound where b is 1: R 4 Si(OR 5 ) 3In the mixture of the two silane compounds, the compound where b is 1 is: R 4 Si(OR 5 ) 3 The blending ratio (molar ratio) of corresponds to the average value of b.
[0034] In this way, the silane compound, which is the component (B1), contains one or more of tetraalkoxysilanes in which the value of b in the general formula (2) is 0 and organotrialkoxysilanes in which the value of b is 1, and by adjusting the content ratio (molar ratio) of these, the average value of b described above is in the range of 0.8 to 1.0.
[0035] Among such components (B1), examples of the silane compound include tetramethoxysilane, tetraethoxysilane, methyltrimethoxysilane, vinyltrimethoxysilane, phenyltrimethoxysilane, methyltriethoxysilane, vinyltriethoxysilane, phenyltriethoxysilane, tetrapropoxysilane, tetraisopropoxysilane, tetrakis(ethoxyethoxy)silane, methyltris(methoxyethoxy)silane, vinyltris(methoxyethoxy)silane, etc. These silane compounds or their partial hydrolysis condensates may be used alone or in combination of two or more.
[0036] As the crosslinking agent, component (B1), it is preferable to use tetramethoxysilane, tetraethoxysilane, methyltrimethoxysilane, or vinyltrimethoxysilane, and it is particularly preferable to use methyltrimethoxysilane, because these crosslinking agents are easy to synthesize, do not impair the storage stability of the composition, are less corrosive to metals, and can achieve a high crosslinking reaction rate, i.e., a high curing rate.
[0037] When component (B1) is a partial hydrolysis condensate of a silane compound, it can be obtained, for example, by partially hydrolyzing methyltrimethoxysilane or the like in the presence of water with an acidic or alkaline catalyst, or by encapsulating the silanol groups generated by the partial hydrolysis with methyltrimethoxysilane or the like.
[0038] The number of Si atoms in one molecule of the silane compound or its partial hydrolysis condensate as component (B1) is preferably 1 or more and less than 10. That is, the silane compound as component (B1) preferably has one Si atom in one molecule, and the partial hydrolysis condensate thereof preferably has 2 to 9 Si atoms in one molecule.
[0039] The silane compound or partial hydrolysis condensate thereof serving as the component (B1) may be used alone or in combination of two or more.
[0040] In this embodiment, the component (B2) is a silane compound represented by the following general formula (3), or a partial hydrolysis condensate thereof. R 6 2 Si(OR 7 ) 2 ……(3) In formula (3), R 6 is an unsubstituted monovalent hydrocarbon group or a monovalent hydrocarbon group in which some of the hydrogen atoms are substituted with halogen atoms or cyanoalkyl groups, and R 4 and R of component (A) 2 Examples of R include the same groups as those shown in the above, and a methyl group, a vinyl group, etc. are preferred. 7 is an alkyl group or an alkoxy-substituted alkyl group, and R 5 and R of component (A) 1 Examples include the same groups as those shown in the above, with a methyl group, an ethyl group, and the like being preferred.
[0041] The number of Si atoms in one molecule of the silane compound or its partial hydrolysis condensate as component (B2) is preferably 1 or more and less than 10. That is, the silane compound as component (B2) preferably has one Si atom in one molecule, and the partial hydrolysis condensate thereof preferably has 2 to 9 Si atoms in one molecule.
[0042] Among such components (B2), examples of the silane compound include dimethyldimethoxysilane, dimethyldiethoxysilane, methylvinyldimethoxysilane, methylphenyldimethoxysilane, diphenyldimethoxysilane, etc. These silane compounds or their partial hydrolysis condensates may be used alone or in combination of two or more.
[0043] As the crosslinking agent (B2), it is preferable to use dimethyldimethoxysilane, dimethyldiethoxysilane, or methylvinyldimethoxysilane, and it is particularly preferable to use dimethyldimethoxysilane or methylvinyldimethoxysilane, because these are easy to synthesize, do not impair the storage stability of the composition, are less corrosive to metals, and can achieve a high crosslinking reaction rate, i.e., a high curing rate.
[0044] The base polymer of the room temperature curable polyorganosiloxane composition of this embodiment contains (A) a polyorganosiloxane capped with alkoxysilyl groups at both ends, and this (A) component is crosslinked with (B) component, which is a silane compound (B1) and (B2) or a partial hydrolysis condensate thereof. The total amount of (B1) and (B2) components is preferably 0.1 to 40 parts by mass, more preferably 0.5 to 30 parts by mass, relative to 100 parts by mass of (A) component. By making the total amount of (B1) and (B2) components 0.1 parts by mass or more, crosslinking can be sufficiently performed, a cured product (cured coating) with sufficient strength can be obtained, and the storage stability of the composition is good. On the other hand, when the total amount of (B1) and (B2) components is 40 parts by mass or less, the shrinkage rate during curing does not become too large, and the physical properties after curing can be maintained. In addition, the curing speed is prevented from becoming too slow, and economic disadvantages are unlikely to occur.
[0045] In addition, the blending ratio of the (B1) component to the (B2) component in the (B) component is preferably 1:99 to 90:10, more preferably 10:90 to 80:20, and even more preferably 20:80 or more and less than 50:50 in mass ratio. By using such blending ratio, the content of the (D) component described later can be increased more than before.
[0046] In the room temperature curable polyorganosiloxane composition of this embodiment, the organotitanium compound, component (C), is a curing catalyst that reacts the alkoxy groups of component (A) with the alkoxy groups of the crosslinking agent, component (B), in the presence of moisture to form a crosslinked structure.
[0047] (C) Examples of the organic titanium compound that is the curing catalyst include tetraethoxytitanium, tetrapropoxytitanium, tetrabutoxytitanium, diisopropoxy-bis(ethyl acetoacetate)titanium, diisopropoxy-bis(methyl acetoacetate)titanium, diisopropoxy-bis(acetylacetone)titanium, dibutoxy-bis(ethyl acetoacetate)titanium, and dimethoxy-bis(ethyl acetoacetate)titanium. These organic titanium compounds may be used alone or in combination of two or more. Among these, titanium chelates such as diisopropoxy-bis(ethyl acetoacetate)titanium are particularly preferred, since they have high catalytic activity even in trace amounts and can provide a composition with few impurities.
[0048] In addition, in the room temperature curable polyorganosiloxane composition, an organic tin compound such as dibutyltin dioctoate or dibutyltin dilaurate may be used as a curing catalyst to promote the reaction between the alkoxy groups of the base component and the reaction between the alkoxy groups of the base component and the alkoxy groups of the crosslinking agent, but when an organic tin compound is used as a curing catalyst together with the above-mentioned (A) component and (B) component, it takes too long to cure, which is not preferable.In this embodiment, the above-mentioned organic titanium compound is used from the viewpoint of the curability (curing speed) of the composition.
[0049] The amount of the organic titanium compound, which is the component (C), is 0.1 to 15 parts by mass, preferably 0.1 to 10 parts by mass, per 100 parts by mass of the component (A). By making it 0.1 part by mass or more, it can function sufficiently as a curing catalyst, and curing time is suppressed from being long, and curing is particularly sufficient in deep parts far from the surface in contact with air. In addition, by making it 15 parts by mass or less, an effect commensurate with the amount can be obtained, which is economically advantageous. In addition, storage stability can be maintained well.
[0050] In the room temperature curable polyorganosiloxane composition of the present embodiment, the additive component (D) is a component that is blended in the polyorganosiloxane composition containing the above components (A) to (C) in order to impart predetermined properties to the cured product.
[0051] The additive of component (D) may be any additive that is blended to impart predetermined properties to this type of composition, and examples thereof include pigments, dyes, and substances that enable visibility such as luminescence by ultraviolet light so that the application of the composition can be confirmed on the production line, as well as substances that deal with corrosive substances suspended in the air, such as sulfur compounds, nitrogen compounds, salt water, and the like, which cause corrosion of the circuit board wiring.
[0052] Examples of such additives include corrosion inhibitors for preventing corrosion of electrodes and wiring, luminescent agents that emit light and develop color when exposed to ultraviolet light or other electron beams, and color-developing agents. In recent years, the demand for such special functions has increased, and the required performance has also become higher. For example, ultraviolet luminescent agents (UV luminescent materials) are required to emit more light due to the trend toward speeding up line production and reducing labor (automatic detection). In addition, corrosion inhibitors are required to be maintained for a long period of time from the perspective of deterioration of the usage environment and their lifespan, and are desired to have characteristics and a longer lifespan than before. Therefore, the demand cannot be met with the conventional amount of addition. Therefore, it has become necessary to develop new materials that can withstand these demands, as well as to increase the amount of conventional materials.
[0053] Examples of the corrosion inhibitor and ultraviolet ray emitting agent (UV emitting material) include benzotriazoles, benzoxazoles, and derivatives thereof, and in particular, benzotriazoles are preferred. Specific examples of benzotriazoles include 1,2,3-benzotriazole, methyl-1H-benzotriazole, tolyltriazole, carboxybenzotriazole, sodium benzotriazole, sodium tolyltriazole, benzotriazole butyl ester, naphthotriazole (1H-naphtho[2,3-d]triazole), chlorobenzotriazole, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-aminophenyl)benzotriazole, 6-(2-benzotriazolyl)-4-tert-octyl-6'-tert-butyl-4'-methyl-2,2'-methylenebisphenol, 5-carboxybenzotriazole, 4-methyl-2-(2H-benzotriazol-2-yl)phenol, etc. These may be used alone or in combination of two or more. Of these, 1,2,3-benzotriazole, tolyltriazole, carboxybenzotriazole, and methyl-1H-benzotriazole are preferable.
[0054] Specific examples of benzoxazoles include benzoxazole, 5-amino-2-(m-aminophenyl)benzoxazole, 2-methylbenzoxazole, 2-mercaptobenzoxazole, 2,2'-p-phenylbis(5-aminobenzoxazole), 2,6-(4,4'-diaminodiphenyl)benzo[1,2-d:4,5-d']bisoxazole, etc. These may be used alone or in combination of two or more. Among these, benzoxazole is preferred.
[0055] Specific examples of UV luminescent agents (fluorescent whitening agents) include benzoxazolylthiophene derivatives (2,5-thiophenediylbis(5-tert-butyl-1,3-benzoxazole (trade name: Tinopal OB; powder)), distyryl biphenyl derivatives (4,4'-bis(2-sulfostyryl)biphenyl disodium salt (trade name: Tinopal NFW; liquid), bis(triazinylamino)stilbene disulfonic acid derivatives (trade name: Tinopal AMS-GX; granules), distyryl biphenyl derivatives (trade name: Tinopal CBS-X; granules, Tinopal CBS-CL, CBS-SP Slurry33; liquid), bis(triazinylamino)stilbene disulfonic acid derivatives (trade name: Tinopal DMA-X, DMA-X Conc.; granules), coumarin derivatives (trade name: Tinopal SWN Conc.; non-dust formulation) (all commercially available products manufactured by BASF).
[0056] Among these, 2,5-thiophenediylbis(5-tert-butyl-1,3-benzoxazole (trade name: Tinopal OB; powder)), which has a relatively small molecular weight and excellent solubility, and distyrylbiphenyl derivatives Tinopal CBS-CL and CBS-SP Slurry33; liquid are preferred, and from the viewpoints of compatibility with component (A) and luminescence performance, 2,5-thiophenediylbis(5-tert-butyl-1,3-benzoxazole is preferred.
[0057] The additive of component (D) can be used in either solid or liquid form, but is generally a relatively solid, and in the case of such a solid form, it is preferable to finely grind it by crushing, grinding, etc., since this can promote dissolution. Also, in order to improve its solubility and compatibility with component (A), it is necessary to add component (B) of the present invention.
[0058] The amount of the additive (D) blended is preferably 0.0001 to 10 parts by mass, and more preferably 0.001 to 5 parts by mass, per 100 parts by mass of the component (A). According to the present embodiment, even if the blending amount is such that dissolution or dispersion has been difficult in the past, it can be uniformly dissolved and dispersed.
[0059] More specifically, when the additive (D) is solid, the amount is preferably 0.001 to 5 parts by mass, and more preferably 0.01 to 2 parts by mass, per 100 parts by mass of the component (A).When the additive (D) is liquid, the amount is preferably 0.001 to 10 parts by mass, and more preferably 0.01 to 5 parts by mass, per 100 parts by mass of the component (A).
[0060] The room temperature curable polyorganosiloxane composition of the present embodiment contains the above-mentioned components (A) to (D) as essential components, but can also contain other components within a range that does not impair the effects of the present invention.
[0061] Examples of such other components include (E) adhesion promoters such as aminoalkylalkoxysilanes such as N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, and 3-aminopropyltriethoxysilane; ketiminoalkylalkoxysilanes such as partial hydrolysates of 3-trimethoxysilyl-N-(1,3-dimethylbutylidene)-1-propanamine and partial hydrolysates of 3-triethoxysilyl-N-(1,3-dimethylbutylidene)-1-propanamine; 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyl Examples of the isocyanurate include mercaptoalkylalkoxysilanes such as dimethoxysilane, epoxyalkylalkoxysilanes such as 3-glycidoxypropyltrimethoxysilane and 3-glycidoxypropyltriethoxysilane, isocyanatoalkylalkoxysilanes such as 3-isocyanatepropyltriethoxysilane and 3-isocyanatepropyltrimethoxysilane, ureidoalkylalkoxysilanes such as 3-ureidopropyltriethoxysilane, and (meth)acryloxyalkylalkoxysilanes such as 3-acryloxypropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane and 3-methacryloxypropyltriethoxysilane. Also, isocyanurate compounds such as tris(N-trialkoxysilylpropyl)isocyanurate can be used. Examples of the isocyanurate compounds include 1,3,5-tris(N-trimethoxysilylpropyl)isocyanurate. Among these, it is preferable to use one selected from ketiminoalkylalkoxysilanes, epoxyalkylalkoxysilanes, mercaptoalkylalkoxysilanes, ureidoalkylalkoxysilanes, (meth)acryloxyalkoxysilanes, and 1,3,5-tris(N-trimethoxysilylpropyl)isocyanurate.
[0062] From the viewpoint of compatibility with the composition, the amount of the adhesion promoter (E) is preferably 0.01 to 5 parts by mass per 100 parts by mass of the (A) component. If it is less than 0.01 part by mass, the effect of improving adhesion is small and is slow to appear. If it is added in an amount of more than 5 parts by mass, not only separation during storage and shrinkage of the cured product occur, but also storage stability and workability may deteriorate and yellowing may occur. The amount is more preferably in the range of 0.1 to 2 parts by mass.
[0063] In addition, the room temperature curable polyorganosiloxane composition of this embodiment may contain various additives, such as inorganic fillers, pigments, thixotropy imparting agents, viscosity modifiers for improving extrusion workability, ultraviolet absorbers, antifungal agents, heat resistance improvers, and flame retardants, which are generally used in this type of composition, as necessary, within the range that does not impair the effects of the present invention. Examples of inorganic fillers include fumed silica, calcined silica, precipitated silica, fumed titanium, and those whose surfaces have been hydrophobized with organochlorosilanes, polyorganosiloxanes, hexamethyldisilazane, etc. In addition, calcium carbonate, organic acid surface-treated calcium carbonate, diatomaceous earth, pulverized silica, aluminosilicate, magnesia, alumina, etc. may also be used. The amount of inorganic filler to be added is preferably 1 to 100 parts by mass, more preferably 3 to 50 parts by mass, per 100 parts by mass of component (A).
[0064] The room temperature curable polyorganosiloxane composition of this embodiment is obtained by mixing the above components (A) to (D) and various components blended as necessary in a moisture-blocking state. Such a room temperature curable polyorganosiloxane composition can be used as a so-called one-package room temperature curable composition that is stored as it is in a sealed container and cured only by exposing it to moisture in the air when used. In addition, the composition of this embodiment can also be used as a so-called multi-package room temperature curable composition in which, for example, a crosslinking agent and a curing catalyst are separately prepared, appropriately divided into 2 to 3 separate containers, and then mixed when used. The order of mixing each component is not particularly limited.
[0065] In addition, the room temperature curable polyorganosiloxane composition of this embodiment preferably has a viscosity of 5 to 1,000 mPa·s at 23°C, preferably 5 to 500 mPa·s, and more preferably 5 to 100 mPa·s. By having a viscosity of 5 to 1,000 mPa·s at 23°C, the composition has good applicability, and a coating film in which the additive component (D) is uniformly dispersed and dissolved can be obtained by a normal coating method. The coating film quickly cures at room temperature upon contact with moisture in the air. The additive (D) in the cured coating is also uniformly dispersed, so that a cured coating with stable properties can be obtained.
[0066] In addition, the cured coating obtained by curing this room temperature curable polyorganosiloxane composition is preferably uniform and wrinkle-free on its surface. If the cured coating is not uniform due to wrinkles on the surface, there is a concern that the durability of the coating itself and the protective effect on the coated object may be impaired. One of the causes of wrinkles is thought to be the microscopic difference in curability and hardness between the surface and its interior. The present inventors have found that by adding component (B2) in addition to component (B1), it is possible to adjust the curability of the surface and to suppress the hardness of the surface during curing. In use, it is possible to adjust the amounts and ratios of (B1) and (B2) in consideration of the balance of surface curability as necessary.
[0067] In addition, in order to improve the visibility of the coated object, it is preferable that the cured product has high transparency. In order to increase the transparency, it is preferable to match the refractive indexes of the components (B1) and (B2) with the component (A) as closely as possible, as one way of improving the compatibility between the components. If the refractive indexes are too far apart, the product may become cloudy (white) and the transparency may be impaired.
[0068] For example, the (A) component R is highly transparent. 3 In the case of polydimethylsiloxane, where R is an alkyl group, typically a methyl group, the R 4 , R 6 is preferably an alkyl group, for example a methyl group, and R 3In the case where a part of R is an aryl group such as a phenyl group, the refractive index of component (A) becomes high, so it is preferable to use components (B1) and (B2) that also contain an aryl group such as a phenyl group and have a similar refractive index. 3 Similarly, when the component (B1) and the component (B2) contain a fluoroalkyl group, it is preferable to use a component (B1) and a component (B2) that contain a fluoroalkyl group and have a similar refractive index. The refractive index in this case is relative to the sodium D line, and a general Abbe refractometer is used for measurement, but it is not limited thereto, and it can be used as a guide under the same conditions. For example, it can be measured with NAR-1T LIQUID manufactured by Atago Co., Ltd.
[0069] In this case, the difference in refractive index between the (A) component, the (B1) component, and the (B2) component is preferably 0.10 or less, more preferably 0.08 or less, even more preferably 0.06 or less, and particularly preferably 0.04 or less.
[0070] Therefore, the composition of the present embodiment is useful for applications such as coating materials and potting materials for electric and electronic devices, and is particularly suitable for applications such as conformal coating agents for protecting the surfaces of electric and electronic components and circuit boards on which these are mounted. Specifically, the composition is preferably used as a coating material for electrodes, wiring, etc. in electric and electronic devices in which semiconductor devices such as ICs, resistors, capacitors, and other electronic components are mounted on a wiring board formed by forming electrodes and wiring made of ITO, copper, aluminum, silver, gold, etc. on a substrate made of epoxy resin, phenolic resin, polyimide resin, etc., or a substrate made of ceramic such as alumina.
[0071] When the room temperature curable polyorganosiloxane composition of the present embodiment is used as a coating material for electrodes or wiring of a wiring board, the coating method may be a dipping method, a brush coating method, a spraying method, a dispensing method, or the like, and the thickness of the coating layer is usually 0.01 to 3 mm, preferably 0.05 to 2 mm.
[0072] Next, the electric / electronic device of the present embodiment will be described with reference to the drawings. Fig. 1 is a cross-sectional view showing an example of the electric / electronic device (device) according to the present embodiment.
[0073] The electric / electronic device 1 of this embodiment includes a wiring board 2 in which wiring 2b made of a conductor such as copper foil is formed on an insulating substrate 2a such as a glass epoxy substrate. Electric / electronic components such as an IC package 3 and a capacitor 4 are mounted at predetermined positions on one main surface of the wiring board 2 and electrically connected to the wiring 2b. The connection between the IC package 3 and the capacitor 4 and the wiring 2b is achieved by inserting the lead terminals 3a and 4a of these components into component holes (not shown) in the wiring board 2 and joining them via solder or the like.
[0074] Furthermore, on the component mounting surface of wiring board 2, a cured coating 5 made of a cured product of the room temperature curable polyorganosiloxane composition of the present embodiment described above is formed so as to cover the upper surfaces of IC package 3 and capacitor 4.
[0075] In the electric / electronic device 1 of this embodiment, the wiring board 2 and the electric / electronic components mounted on its main surface are covered with the cured coating 5 in which the additives are uniformly mixed and dispersed, and therefore the stability and reliability are high. Furthermore, even if the content of the additives is increased compared to conventional cases, mixing and dispersion can be stably performed, and the function to be imparted can be improved. EXAMPLES
[0076] The present invention will be described in more detail below with reference to examples, but the scope of the invention is not limited to these examples. In the examples, all "parts" refer to "parts by mass", and all viscosity values are shown at 23°C and a relative humidity of 50%. Moreover, Examples 1, 2, 3, 8, and 12 are "reference examples".
[0077] Example 1 (A1) 22.5 parts of polydimethylsiloxane (viscosity 590 mPa·s) in which both ends of the molecular chain are blocked with trimethoxysilyl groups, (A2) 52.5 parts of polydimethylsiloxane (viscosity 80 mPa·s) in which both ends of the molecular chain are blocked with trimethoxysilyl groups, (A'1) 11.0 parts of polydimethylsiloxane (viscosity 20 mPa·s), (B1-1) 7.5 parts of trimethyltrimethoxysilane, (B2-1) 4.0 parts of dimethyldimethoxysilane, (C1) 2.25 parts of diisopropoxy-bis(ethyl acetoacetate)titanium, (D1) 0.01 parts of 2,5-thiophenediylbis(5-t-butyl-1,3-benzoxazole), (D2) 0.2 parts of 1,2,3-benzotriazole, and (E1) 1,3,5-tris(N-trimethoxysilylpropyl)isocyanurate 0.15 parts of each were blended and mixed uniformly under a moisture-blocking condition to obtain Polyorganosiloxane Composition 1.
[0078] Example 2 Polyorganosiloxane composition 2 was obtained in the same manner as in Example 1, except that (B2-3) methylvinyldimethoxysilane was used instead of (B2-1) dimethyldimethoxysilane.
[0079] Example 3 Polyorganosiloxane composition 3 was obtained in the same manner as in Example 1, except that the amount of (A1) polydimethylsiloxane (viscosity 590 mPa s) capped at both molecular chain terminals with trimethoxysilyl groups was 18.5 parts, the amount of (A3) polydimethylsiloxane was 15.0 parts, and the amount of (D2) 1,2,3-benzotriazole was 0.3 parts.
[0080] Example 4 Polyorganosiloxane composition 4 was obtained in the same manner as in Example 3, except that the amount of (A1) polydimethylsiloxane (viscosity: 590 mPa s) capped at both molecular chain terminals with trimethoxysilyl groups was 11.0 parts and the amount of (B2-1) dimethyldimethoxysilane was 11.5 parts.
[0081] Example 5 Polyorganosiloxane composition 5 was obtained in the same manner as in Example 4, except that (B2-3) methylvinyldimethoxysilane was used instead of (B2-1) dimethyldimethoxysilane.
[0082] Example 6 Polyorganosiloxane composition 6 was obtained in the same manner as in Example 4, except that (B2-4) diphenyldimethoxysilane was used instead of (B2-1) dimethyldimethoxysilane.
[0083] Example 7 Polyorganosiloxane composition 7 was obtained in the same manner as in Example 4, except that (B2-5) methylphenyldimethoxysilane was used instead of (B2-1) dimethyldimethoxysilane.
[0084] Example 8 A polyorganosiloxane composition 8 was obtained in the same manner as in Example 4, except that (B2-2) dimethyldiethoxysilane was used instead of (B2-1) dimethyldimethoxysilane.
[0085] Example 9 Polyorganosiloxane composition 9 was obtained in the same manner as in Example 2, except that the blending amount of (B1-1) dimethyldimethoxysilane was changed to 5.5 and the blending amount of (B2-3) methylvinyldimethoxysilane was changed to 6.0.
[0086] Example 10 A polyorganosiloxane composition 10 was obtained in the same manner as in Example 2, except that the blending amount of (B1-1) dimethyldimethoxysilane was changed to 4.0 and the blending amount of (B2-3) methylvinyldimethoxysilane was changed to 7.5.
[0087] Example 11 A polyorganosiloxane composition 11 was obtained in the same manner as in Example 3, except that the blending amount of (B1-1) dimethyldimethoxysilane was changed to 5.5 and the blending amount of (B2-1) dimethyldimethoxysilane was changed to 6.0.
[0088] Example 12 A polyorganosiloxane composition 12 was obtained in the same manner as in Example 11, except that (B2-3) methylvinyldimethoxysilane was used instead of (B2-1) dimethyldimethoxysilane.
[0089] Example 13 A polyorganosiloxane composition 13 was obtained in the same manner as in Example 12, except that the blending amount of (B2-3) methylvinyldimethoxysilane was changed to 7.5.
[0090] Comparative Example 1 (A1) 22.5 parts of polydimethylsiloxane (viscosity 590 mPa s) terminated at both ends of the molecular chain with trimethoxysilyl groups, (A2) 52.5 parts of polydimethylsiloxane (viscosity 80 mPa s) terminated at both ends of the molecular chain with trimethoxysilyl groups, (A3) 15.0 parts of polydimethylsiloxane (viscosity 20 mPa s), (B1) 7.5 parts of trimethyltrimethoxysilane, (C1) 2.25 parts of diisopropoxy-bis(ethyl acetoacetate)titanium, (D1) 0.01 parts of 2,5-thiophenediylbis(5-t-butyl-1,3-benzoxazole), (D2) 0.1 parts of 1,2,3-benzotriazole, and (E1) 1,3,5-tris(N-trimethoxysilylpropyl)isocyanurate 0.15 parts of each of the components were blended and mixed uniformly under moisture protection to obtain a polyorganosiloxane composition C1.
[0091] Comparative Example 2 A polyorganosiloxane composition C2 was obtained in the same manner as in Comparative Example 1, except that the amount of 1,2,3-benzotriazole (D2) was 0.2 parts.
[0092] Comparative Example 3 A polyorganosiloxane composition C3 was obtained in the same manner as in Comparative Example 1, except that the amount of 1,2,3-benzotriazole (D2) was changed to 0.3 parts.
[0093] Comparative Example 4 A polyorganosiloxane composition C4 was obtained in the same manner as in Comparative Example 2, except that the blending amount of (A3) polydimethylsiloxane (viscosity 20 mPa·s) was 11.0 parts and the blending amount of (B1) trimethyltrimethoxysilane was 11.5 parts.
[0094] Comparative Example 5 A polyorganosiloxane composition C5 was obtained in the same manner as in Comparative Example 4, except that the amount of 1,2,3-benzotriazole (D2) was 0.3 parts.
[0095] Comparative Example 6 Polyorganosiloxane composition C6 was obtained in the same manner as in Comparative Example 3, except that the amount of (A2) polydimethylsiloxane (viscosity 80 mPa s) capped at both molecular chain terminals with trimethoxysilyl groups was 18.5 parts and the amount of (B1) methyltrimethoxysilane was 11.5 parts.
[0096] Comparative Example 7 A polyorganosiloxane composition C7 was obtained in the same manner as in Comparative Example 2, except that the blending amount of (B1) trimethyltrimethoxysilane was 11.5 parts.
[0097] Comparative Example 8 A polyorganosiloxane composition C8 was obtained in the same manner as in Comparative Example 7, except that the amount of 1,2,3-benzotriazole (D2) was 0.3 parts.
[0098] The refractive indexes of the materials of the (A) and (B) components used in the above examples and comparative examples were, respectively, (A1) component: 1.402, (A2) component: 1.399, (B1) component: 1.37, (B2-1) component: 1.37, (B2-2) component: 1.38, (B2-3) component: 1.40, (B2-4) component: 1.55, and (B2-5) component: 1.48. The refractive indexes of the (B1) and (B2-1) to (B2-3) components were close to each other within 0.3 compared to the (A) component, while the refractive index difference between the (B2-4) and (B2-5) components was relatively large. Here, the refractive index was measured using an Abbe refractometer (manufactured by Atago Co., Ltd., product name: NAR-1T LIQUID) for sodium D line.
[0099] The polyorganosiloxane compositions obtained in Examples 1 to 13 and Comparative Examples 1 to 8 were measured and evaluated for various properties by the methods described below. The results, together with the compositions, are shown in Tables 1 and 2 for Examples 1 to 13 and in Table 3 for Comparative Examples 1 to 8, respectively.
[0100] [exterior] The appearance of the polyorganosiloxane composition was visually observed (1) immediately after preparation at room temperature, (2) after cooling at 5°C for 3 days, and (3) after cooling at 5°C for 3 days and leaving at room temperature for 3 days, and evaluated according to the following criteria as to whether the components were uniformly mixed in the composition. <Evaluation criteria> OK: The additive (D) was uniformly dispersed and dissolved in the composition (including some translucency). Translucent: The composition was translucent because the (D) additive was unevenly dispersed or dissolved in the composition or because there was a large difference in refractive index. Precipitation: Precipitation was observed. NG: The presence of undissolved matter and re-precipitated matter was confirmed.
[0101] [viscosity] The viscosity of the polyorganosiloxane composition was measured according to JIS K6249 as follows: Using a rotational viscometer (manufactured by Shibaura Semtec Corporation, product name: Vismetron VDA-2), the viscosity was measured at rotation speeds of 30 rpm and 60 rpm with rotor No. 2.
[0102] [Hardened surface] The polyorganosiloxane composition was molded into sheets of 1 mm and 2 mm thickness, and then left to cure for 3 days at 23° C. and 50% RH. The cured surface was visually observed and evaluated according to the following criteria. <Evaluation criteria> Smooth: The entire cured surface was smooth. Wavy: Not wrinkled, but uneven in thickness. Slightly wrinkled: Wrinkles were observed on some parts of the cured surface. Wrinkled: Wrinkles were observed over the entire cured surface. Severely wrinkled: Wrinkles were visible all over the cured surface, and there was also significant waviness. In Examples 6 and 7, the difference in refractive index between component (A) and component (B) was relatively large, and cloudiness was observed, but in the other examples, the film was transparent and had good internal visibility.
[0103] [Tuck free time] The tack-free time of the polyorganosiloxane composition was measured according to JIS K6249 as follows: A sample was placed flat in an aluminum petri dish to prevent bubbles from entering (sample thickness: 3 mm), and then the surface was lightly touched with a fingertip washed with ethyl alcohol, and the time when the sample no longer adhered to the fingertip was measured and taken as the tack-free time. Furthermore, in order to evaluate the stability of the curing property, the polyorganosiloxane composition was sealed in a moisture-proof airtight container, and then treated at 70° C. for 5 days, after which the tack-free time was measured in the same manner as above.
[0104] [hardness] The hardness of the polyorganosiloxane composition was measured according to JIS K6249 as follows. The polyorganosiloxane composition was molded into a sheet having a thickness of 2 mm, and then allowed to stand at 23°C and 50% RH for 3 days to cure. Three of the cured sheets were then stacked, and the hardness was measured using a durometer (Type A).
[0105] [Corrosion test] The polyorganosiloxane composition was applied to a mounting substrate in a thickness of 100 μm, and cured at 23°C and 50% RH for 3 days. 2 After leaving the test pieces in an atmosphere of 50 ppm S at 85°C and 85% RH for 1000 and 2000 hours, the degree of discoloration of the copper parts on the board and the growth of the corroded parts were checked and evaluated according to the following criteria. (Corrosion degree evaluation) ○: Almost no corrosion is observed △~◯: No discoloration was observed on the copper foil, but a small amount of corrosion growth was observed on the edge of the copper foil. △: Slight discoloration is observed on the copper foil. ×: Significant discoloration is observed on the copper foil. In addition, in the case of the sample not containing (D2) 1,2,3-benzotriazole, significant discoloration was confirmed after 1000 hours.
[0106] [Table 1]
[0107] [Table 2]
[0108] [Table 3]
[0109] From Tables 1-2, it was found that the polyorganosiloxane compositions obtained in Examples 1-13 have a uniform viscosity suitable for thin film coating, and can dissolve and disperse additives uniformly, and can easily form a cured coating with a smooth cured surface. In addition, a large amount of corrosion inhibitor can be stably blended as an additive, and a cured coating with excellent corrosion resistance can be obtained.
[0110] In contrast, as can be seen from Table 3, when the (B2) component is not contained, precipitation and other problems occur even with a small increase in the amount of additive, as in Examples 2, 3, 5, 6, and 8. Correspondingly, when the amount of the crosslinking agent of the (B1) component is increased, as in Examples 4 and 7, the appearance is improved, but wrinkles become more likely to form on the surface of the cured coating. [Industrial Applicability]
[0111] The room-temperature-curable polyorganosiloxane of the present invention is useful as a coating material, potting material, etc. for electric and electronic devices, and is particularly suitable as a conformal coating agent for electric and electronic devices having electronic components mounted on a substrate. [Explanation of symbols]
[0112] 1...electrical / electronic device, 2...wiring board, 3...IC package, 4...capacitor, 5...cured coating of room-temperature-curable polyorganosiloxane composition
Claims
1. (A) A polyorganosiloxane having both ends capped with alkoxysilyl groups, represented by the following general formula (1): 【Chemistry 1】 (In the formula, R 1 represents an alkyl group or an alkoxy-substituted alkyl group in which some of the hydrogen atoms of the alkyl group are substituted with alkoxy groups; R 2 and R 3 is an unsubstituted monovalent hydrocarbon group or a monovalent hydrocarbon group in which some of the hydrogen atoms are substituted with halogen atoms or cyanoalkyl groups, and X is a divalent oxygen (oxy group) or a divalent hydrocarbon group. In addition, a is 0 or 1, and n is a number that provides a viscosity at 23°C in the range of 5 to 10,000 mPa·s.) Per 100 parts by mass, (B) (B1) A silane compound represented by the following general formula (2): R 4 b Si(OR 5 ) 4-b …(2) (In the formula, R 4 is a monovalent substituted or unsubstituted hydrocarbon group, R 5 represents a monovalent group selected from the group consisting of alkyl groups having 1 to 4 carbon atoms and alkoxyalkyl groups having a total of 1 to 6 carbon atoms, and b represents 0 or 1), or a partial hydrolysis condensate thereof, and (B2) a silane compound represented by the following general formula (3): R 6 2 Si(OR 7 ) 2 …(3) (In the formula, R 6 is a monovalent substituted or unsubstituted hydrocarbon group, R 7 represents a monovalent group selected from the group consisting of alkyl groups having 1 to 4 carbon atoms and alkoxyalkyl groups having 1 to 6 carbon atoms in total), or a partial hydrolysis condensate thereof; (C) 0.1 to 15 parts by mass of an organic titanium compound as a curing catalyst; (D) 0.0001 to 10 parts by mass of an additive; Contains The blending amounts of the component (B1) and the component (B2) are in a mass ratio ranging from 20:80 to 47.8:52.2, The room-temperature curable polyorganosiloxane composition, wherein the additive (D) is a benzotriazole or a benzoxazole.
2. The room temperature curable polyorganosiloxane composition according to claim 1, wherein the viscosity of the component (A) at 23°C is 5 to 5,000 mPa·s.
3. The component (A) contains (A1) a polyorganosiloxane having a viscosity of 5 to 200 mPa · s at 23 ° C. and (A2) a polyorganosiloxane having a viscosity of 500 to 100,000 mPa · s at 23 ° C., and the room temperature curable polyorganosiloxane composition according to claim 2, characterized in that it contains 50 to 100 mass% of the component (A1).
4. 4. The room-temperature-curable polyorganosiloxane composition according to claim 1, which is a coating composition for electrodes and / or wiring of electric and electronic devices.
5. 5. An electric or electronic device comprising a coating comprising a cured product of the room-temperature-curable polyorganosiloxane composition according to claim 1 on the surface of an electrode and / or wiring.
Citation Information
Patent Citations
Room-temperature-curing nonsolvent silicone coating composition for protecting mounted circuit board, protecting method for mounted circuit board, and mounted circuit board
JP1995173435A
Conformal coating agent
JP1995238259A
Method for protecting metallic electroconductive part of electric / electronic apparatus
JP2004149611A
Method of protecting transparent nonmetallic electroconductive part
JP2012236942A
Room temperature curable silicone composition and electrical / electronic equipment
JP2020510713A