Glass

A glass with a colored layer is achieved by heat-treating a metal film on the glass surface, addressing the need for selective light transmission and absorption, enhancing light control and decorative applications.

JP7587495B2Active Publication Date: 2024-11-20HOYA CORPORATION
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021519371
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-05-10
Filing Date
2020-04-30
Publication Date
2024-11-20
Estimated Expiration
2040-04-30

AI Technical Summary

Technical Problem

Existing technologies do not provide a method to form a colored layer on glass, which is necessary for applications requiring selective light transmission and absorption.

Method used

A glass with a colored layer is created by forming a metal film on the glass surface and heat-treating it in a reducing atmosphere, resulting in a colored layer that can be selectively applied to specific areas, allowing for both low and high transmittance regions.

Benefits of technology

The glass with a colored layer effectively blocks light in desired areas while maintaining high transmittance in others, providing enhanced light control and decorative properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587495000011
    Figure 0007587495000011
  • Figure 0007587495000012
    Figure 0007587495000012
  • Figure 0007587495000013
    Figure 0007587495000013
Patent Text Reader

Abstract

[Problem] To provide glass having a colored layer. [Solution] Glass having a colored layer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to glass having a colored layer. [Background technology]

[0002] Patent Document 1 discloses an invention in which the transmittance of glass is changed by heat treating the glass in an oxidizing atmosphere or a non-oxidizing atmosphere, but does not disclose the formation of a colored layer on glass. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2002-201041 A Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide glass having a colored layer. [Means for solving the problem]

[0005] The gist of the present invention is as follows. (1) Glass with a colored layer.

[0006] (2) The glass according to (1), which has a portion with low transmittance and a portion with high transmittance.

[0007] (3) The glass according to (1) or (2), which contains Bi ions as a glass component.

[0008] (4) The glass according to any one of (1) to (3), which is a phosphate glass.

[0009] (5) The glass according to any one of (1) to (4), having a refractive index of 1.70 or more.

[0010] (6) An optical element made of the glass according to any one of (1) to (5) above. Effect of the Invention

[0011] According to the present invention, a glass having a colored layer can be provided. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a schematic diagram showing an example of an embodiment of the present invention. [Diagram 2] FIG. 1 is a schematic diagram showing an example of an embodiment of the present invention. [Figure 3-1] FIG. 1 is a schematic diagram showing an example of an embodiment of the present invention. [Figure 3-2] FIG. 3-2 is a schematic diagram for explaining the embodiment of FIG. 3-1. [Figure 4] FIG. 1 is a schematic diagram showing an example of an embodiment of the present invention. [Figure 5-1] 1 is an image showing a sample in Example 1-1 and a ruler for reference. [Figure 5-2] 1 is an image showing a sample in Example 1-2 and a ruler for reference. [Figure 6-1] 1 is a graph showing the transmittance of a portion having a colored layer of a sample in Example 1-1. [Figure 6-2] 1 is a graph showing the transmittance of a portion having a colored layer of a sample in Example 1-2. [Figure 6-3] 1 is a graph showing the transmittance of a portion having a colored layer of a sample in Example 1-3. [Figure 7-1] 1 is a graph showing the transmittance of a portion having a colored layer of a sample in Example 2-1 for each thickness of the metal film. [Figure 7-2] 11 is a graph showing the transmittance of a portion having a colored layer of a sample in Example 2-2 for each thickness of the metal film. [Figure 8] 1 is a graph showing the relationship between the thickness of a metal film and OD for each heat treatment time for samples in Examples 2-1 and 2-2. [Figure 9] 1 is an image showing a sample in Example 5 and a ruler for reference. [Figure 10] 1 is a micrograph of a cross section of a portion of a sample in Example 7 having a colored layer. [Figure 11] 1 is a graph showing OD (wavelength 1100 nm) when the horizontal axis represents the amount removed in the thickness direction for the sample in Example 7. The values ​​in the graph are ΔOD. [Figure 12] 1 is a graph showing OD (wavelength 780 nm) when the horizontal axis represents the amount removed in the thickness direction for the sample in Example 7. The values ​​in the graph are ΔOD. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] In this embodiment, the glass according to the present invention will be described based on the content ratio of each component expressed in cation %. Therefore, hereinafter, unless otherwise specified, "%" for each content means "cation %".

[0014] The cationic % expression refers to the molar percentage when the total content of all cationic components is taken as 100%. The total content refers to the total content of multiple cationic components (including the case where the content is 0%). The cationic ratio refers to the ratio (ratio) of the content of each cationic component (including the total content of multiple cationic components) in the cationic % expression.

[0015] The content of the glass component can be quantified by known methods, such as inductively coupled plasma atomic emission spectrometry (ICP-AES), inductively coupled plasma mass spectrometry (ICP-MS), etc. In this specification and the present invention, the content of a component being 0% means that the component is substantially not contained, and it is acceptable for the component to be contained at an unavoidable impurity level.

[0016] In addition, in this specification, unless otherwise specified, the refractive index refers to the refractive index nd at the d line (wavelength 587.56 nm) of yellow helium.

[0017] Hereinafter, embodiments of the present invention will be described in detail.

[0018] The glass according to this embodiment has a colored layer. The colored layer is a portion of the glass that is colored, and is preferably present in the form of a layer extending from the glass surface toward the inside.

[0019] In the glass according to this embodiment, the colored layer may be present so as to cover the entire glass surface (on the entire surface of the glass), or may be present so as to cover a portion of the glass surface (on a portion of the glass surface).

[0020] The colored layer is a portion having a low transmittance for light incident on the glass. Therefore, in the glass according to this embodiment, of the light incident on the glass, the light that enters the colored layer is absorbed partially or entirely, and the intensity of the transmitted light is attenuated compared to the light that does not enter the colored layer. In other words, the glass according to this embodiment can have portions with low transmittance and portions with high transmittance.

[0021] In the glass according to this embodiment, the colored layer can be removed by grinding or polishing. In the glass according to this embodiment, the transmittance of the glass after the colored layer is removed is greater than the transmittance before the colored layer is removed.

[0022] In this embodiment, for example, in the case of glass having two opposing surfaces, the colored layer 2 may be provided on only one surface of the glass body 1 as shown in Figure 1, or on both surfaces as shown in Figure 2.

[0023] In addition, by selectively forming a colored layer on the glass surface as shown in Figure 3-1, it is possible to block light in the areas where the colored layer is present and transmit light in the areas where the colored layer is not present. For example, by forming the colored layer in a specific pattern, it is possible to give the glass functions such as slits, apertures, and pinholes.

[0024] In FIG. 3-1, since there is no colored layer 2 in the path A of light, the light passes from one surface to the other surface. Since there is a colored layer 2 in the path B, the light is absorbed by the colored layer 2. Also, since the colored layer 2 has the same composition as the non-colored part, there is no difference in refractive index inside the glass, and the light is not reflected at the boundary between the colored layer 2 and the non-colored part. In this case, the same effect as that when the colored layer 2 is provided over the entire thickness direction of the glass as shown in FIG. 3-2 can be obtained in terms of light transmission. As is well known, the relationship between the angle of incidence and the angle of refraction on the surface of glass is determined by the refractive index of the glass and the refractive index of the medium (e.g., air) in contact with the glass. The area where the colored layer is formed on the surface of the glass, the width of the slit, the diameter of the aperture, etc. can be determined by taking this relationship into consideration.

[0025] As described below, the glass according to this embodiment can be used in optical elements. From the viewpoint of use in optical elements, the glass according to this embodiment is preferably optical glass. However, the glass according to this embodiment can be used as ornaments, exteriors of small electronic devices, etc., making use of the decorative properties of the colored layer, and is therefore not limited to optical glass.

[0026] In the glass according to this embodiment, the colored layer and the non-colored portion have the same glass component composition, however, the valence of the glass components (cations) may differ between the colored layer and the non-colored portion.

[0027] The color of the colored layer is preferably a reduction color caused by a glass component, more preferably a reduction color caused by a transition metal. Examples of transition metals include Ti, Nb, W, and Bi. Therefore, the glass according to this embodiment preferably contains at least one ion selected from the group consisting of Ti ions, Nb ions, W ions, and Bi ions, more preferably Bi ions, as a glass component.

[0028] (Thickness of colored layer) The thickness of the colored layer is not particularly limited, but is preferably 1 to 300 μm, more preferably 20 to 200 μm, and further preferably 30 to 150 μm.

[0029] (OD) In the glass according to this embodiment, the spectral transmittance of the colored layer in the wavelength range from the visible range (400 nm to 760 nm) to the infrared range increases as the wavelength increases. On the other hand, the OD of the colored layer decreases as the wavelength increases. OD is optical density, and is expressed as a negative value of the common logarithm of the ratio of the incident light intensity I0 to the transmitted light intensity I, as shown in the following formula. OD=-log 10 (I / I o )

[0030] When the glass according to the present embodiment is composed of a colored layer and a non-colored portion having a large visible transmittance, the OD of the colored layer is large while the OD of the non-colored portion is small. In measuring the OD, when the measurement light passes through both the colored layer and the non-colored portion, the OD of the non-colored portion is sufficiently small, so that the OD of the colored layer becomes dominant.

[0031] In the glass according to this embodiment, the OD at a wavelength of 1100 nm of the portion having the colored layer is preferably 1.0 or more, more preferably 1.5 or more, while the OD at a wavelength of 1100 nm of the non-colored portion is preferably 0.15 or less, more preferably 0.1 or less.

[0032] Usually, the sensitivity range of optical sensors such as CCD and C-MOS sensors extends from the visible range to around 1100 nm. By providing a colored layer having an OD in the above range, a glass capable of blocking light over the entire sensitivity range of the optical sensor can be obtained. Therefore, the glass according to this embodiment is preferably one capable of controlling the transmittance of light rays in the wavelength range from the visible range to 1100 nm.

[0033] In addition, when a glass has two opposing surfaces and a colored layer is provided on both surfaces, the OD is approximately twice as large as when the same colored layer is provided on only one surface.

[0034] In the glass according to this embodiment, the OD decreases with increasing wavelength in the visible to near infrared wavelength range, so that in the portion having the colored layer, the OD at a wavelength of 780 nm is greater than the OD at a wavelength of 1100 nm.

[0035] Therefore, if there is a wavelength range that needs to be blocked, the glass is designed so that the OD is high at the longer wavelength side of that wavelength range. When designing glass that blocks only visible light, it is sufficient to set the OD high at the longer wavelength side of the visible light range (e.g., 780 nm). When designing glass that blocks light from the visible range to the near-infrared range, it is sufficient to set the OD high at a wavelength in the near-infrared range (e.g., 1100 nm). The OD can be controlled by adjusting the thickness of the colored layer and the degree of coloring.

[0036] (ΔOD) As described above, when the glass according to this embodiment is composed of a colored layer and a non-colored portion having a high transmittance in the visible range, the OD of the colored layer is large while the OD of the non-colored portion is small. In other words, when the colored layer is gradually removed in the thickness direction, the OD changes according to the amount of removal.

[0037] For glass having a colored layer according to this embodiment, the OD at a given wavelength is OD1 and the thickness is T1. When a given amount of the colored layer is removed in the thickness direction by polishing or the like, the OD at the same wavelength is OD2 and the thickness is T2. In this case, the change in OD per unit thickness, ΔOD, is calculated by the following formula: ΔOD=(OD1-OD2) / (T1-T2)

[0038] When measuring ΔOD at OD at a wavelength of 1100 nm or more, it is preferable to remove the colored layer in the thickness direction by 5 to 20 μm at a time. When measuring ΔOD at OD at a wavelength of less than 1100 nm, it is preferable to remove the colored layer in the thickness direction by 3 to 10 μm at a time. Then, the OD measurement and removal of the colored layer are repeated, and ΔOD is calculated according to the amount of the colored layer removed. For example, when the removal of the colored layer is repeated to reach a total of 20 μm of the amount of the colored layer removed in the thickness direction, (T1-T2) in the above formula is 20.

[0039] After the colored layer is removed repeatedly until it can no longer be visually confirmed, the removal is repeated 2 to 3 more times so that an additional 50 μm is finally removed from the area where the colored layer was. After each removal, the OD and glass thickness are measured and ΔOD is calculated.

[0040] Alternatively, after the colored layer has been repeatedly removed and the OD becomes less than 0.15, the portion where the colored layer was was removed in the thickness direction by 10 μm or more in multiple steps. Each time 10 μm or more is removed in the thickness direction, the OD and glass thickness are measured and ΔOD is calculated.

[0041] In the glass according to this embodiment, when ΔOD is preferably 0.04 or more, 0.05 or more, 0.07 or more, 0.09 or more, 0.12 or more, 0.15 or more, 0.18 or more, 0.20 or more, 0.25 or more, 0.30 or more, 0.34 or more, or 0.35 or more at wavelengths of 1100 nm and 780 nm, it can be evaluated that the colored layer remains. Also, when ΔOD is preferably 0.025 or less, 0.023 or less, 0.020 or less, 0.017 or less, 0.015 or less, or 0.010 or less at wavelengths of 1100 nm and 780 nm, it can be evaluated that the colored layer has been removed.

[0042] In the glass according to this embodiment, the boundary between the colored layer and the non-colored portion is clear. Here, the boundary between the colored layer and the non-colored portion is the region from when the degree of coloring in the colored layer becomes weak to when the coloring is sufficiently reduced. The degree of coloring can be evaluated by OD at a predetermined wavelength. Therefore, the state in which the degree of coloring changes near the boundary can be confirmed by the above ΔOD. That is, if a region in which OD changes significantly depending on the amount of the colored layer removed can be confirmed by ΔOD, that region can be determined as the boundary between the colored layer and the non-colored portion.

[0043] In the glass according to this embodiment, the boundary between the colored layer and the non-colored portion in the thickness direction can be within a range of several tens of μm. Therefore, when a cross section of the glass according to this embodiment is observed with an optical microscope or the like, the boundary between the colored layer and the non-colored portion can be relatively clearly seen.

[0044] Therefore, in the glass according to this embodiment, for example, the region where ΔOD is 0.04 or more can be regarded as the boundary between the colored layer and the non-colored portion. Also, the region where ΔOD is 0.04 or more, 0.05 or more, 0.07 or more, 0.09 or more, 0.12 or more, 0.15 or more, 0.18 or more, 0.20 or more, 0.25 or more, 0.30 or more, 0.34 or more, or 0.35 or more may be regarded as the boundary between the colored layer and the non-colored portion. And, in the glass according to this embodiment, the thickness of the region is preferably 40 μm or less, and more preferably 30 μm or less, 20 μm or less, 10 μm or less, and 5 μm or less in that order.

[0045] (Refractive Index) In the glass according to this embodiment, the refractive index nd is preferably 1.70 or more, more preferably 1.73 or more, 1.75 or more, 1.76 or more, 1.77 or more, 1.78 or more, 1.79 or more, and 1.80 or more in that order. The upper limit of the refractive index nd is not particularly limited, but is usually 2.5, and preferably 2.3.

[0046] In Fig. 4, a glass having two opposing surfaces is provided with a plurality of colored layers at a predetermined interval on each of the opposing portions of both surfaces so that the portions on which no colored layers are formed function as slits. In such a case, if the refractive index of the glass is low, when the angle of incidence of the light beam entering the slit portion is large (the light beam enters at a shallow angle), the light beam may pass through the adjacent slit as in route C, and the same effect as that of the element shown in Fig. 3-2 may not be obtained. If the refractive index of the glass is high as in the above range, the light beam is absorbed by the colored layer formed on the back surface of the glass as in route B, and the light beam does not pass through the adjacent slit, so the interval between the slits can be narrowed.

[0047] (Average linear expansion coefficient) In the glass according to this embodiment, the average linear expansion coefficient is preferably 50×10 -7 K -1 And even more, 60 x 10 -7 K -1 That's it, 70 x 10 -7 K -1 That's it, 75 x 10 -7 K -1 That's it, 80 x 10 -7 K -1 That's it, 85 x 10 -7 K -1 That's it, 90 x 10 -7 K -1 The upper limit of the average linear expansion coefficient is not particularly limited, but is usually 200×10 -7 K -1 and preferably 150×10 -7 K -1 By setting the average linear expansion coefficient within the above range, the strength of the glass can be increased when chemically strengthened.

[0048] The method for measuring the average linear expansion coefficient is in accordance with the Japan Optical Glass Industry Association standard JOGIS 08-2003 "Method for measuring thermal expansion of optical glass." However, the diameter of the rod-shaped sample is 5 mm.

[0049] (Acid resistance weight loss rate Da) In the glass according to this embodiment, the grade of the acid resistance weight loss rate Da is preferably 1 to 2, and more preferably 1.

[0050] The acid resistance weight loss rate Da is measured according to the provisions of the Japan Optical Glass Industry Association standard JOGIS06-2009. Specifically, powdered glass (particle size 425-600 μm) with a weight equivalent to the specific gravity is placed in a platinum cage, which is immersed in a quartz glass round-bottom flask containing a 0.01 mol / L nitric acid solution, and treated in a boiling water bath for 60 minutes, and the weight loss rate (%) before and after the treatment is measured. Table A shows the grades based on the acid resistance weight loss rate Da.

[0051] [Table A]

[0052] (Glass composition) Non-limiting examples of the composition of the glass according to this embodiment are shown below.

[0053] The glass according to the present embodiment is preferably a phosphate glass. Phosphate glass is a glass that contains mainly P as a network forming component. 5+ This refers to glass that contains P as a network forming component of glass. 5+ , B 3+ , Si 4+ , Al 3+ Here, the term "containing mainly phosphate as a glass network forming component" means that P 5+ The content of B 3+ , Si 4+ , Al 3+ The content of the phosphate glass can increase the degree of coloring in the colored layer.

[0054] In the glass according to this embodiment, P 5+ The lower limit of the content of P is preferably 10%, and more preferably 13%, 15%, 17%, and 20% in that order. 5+The upper limit of the content is preferably 50%, and more preferably 45%, 40%, 38%, 35%, 33%, and 30%, in that order.

[0055] P 5+ is a glass network forming component. 5+ If it contains too much, the melting property will deteriorate. 5+ The content is preferably within the above range.

[0056] In the glass according to this embodiment, B 3+ The upper limit of the content of is preferably 30%, more preferably 25%, 20%, 15%, 13%, and 10%, in that order. 3+ The lower limit of the content of is preferably 0.1%, more preferably 0.5%, 1%, 3%, and 5% in that order. 3+ The content may be 0%.

[0057] B 3+ is a glass network forming component and has the function of improving the melting property of glass. 3+ If the content of B is too high, the chemical durability tends to decrease. 3+ The content is preferably within the above range.

[0058] In the glass according to this embodiment, P 5+ B content 3+ The cationic ratio of the content [B 3+ / P 5+ The upper limit of the cation ratio [B 3+ / P 5+ ] may be 0.

[0059] In the glass according to this embodiment, Si 4+ The upper limit of the content of Si is preferably 10%, and more preferably 7%, 5%, 3%, 2%, and 1% in that order. 4+The lower limit of the Si content is preferably 0.1%, and more preferably 0.2%, 0.3%, 0.4%, and 0.5%, in that order. 4+ The content may be 0%.

[0060] S 4+ is a glass network forming component, and has the function of improving the thermal stability, chemical durability, and weather resistance of glass. 4+ If the content of Si is too high, the melting property of the glass decreases and the glass raw material tends to remain unmelted. 4+ The content is preferably within the above range.

[0061] In the glass according to this embodiment, Al 3+ The upper limit of the Al content is preferably 10%, and more preferably 7%, 5%, 3%, and 1% in that order. 3+ The content may be 0%.

[0062] Al 3+ It has the function of improving the chemical durability and weather resistance of glass. 3+ If the content of Al is too high, the thermal stability of the glass decreases, the glass transition temperature Tg increases, and the melting property tends to decrease. 3+ The content is preferably within the above range.

[0063] In the glass according to this embodiment, P 5+ , B 3+ , Si 4+ and Al 3+ The total content of [P 5+ +B 3+ +Si 4+ +Al 3+ The lower limit of the total content [P 5+ +B 3+ +Si 4+ +Al 3+ The upper limit of is preferably 60%, and more preferably 50%, 45%, 40%, 37%, and 35%, in that order.

[0064] The glass according to this embodiment preferably contains a transition metal as a glass component, more preferably contains at least one glass component selected from the group consisting of Ti ions, Nb ions, Bi ions and W ions, and further preferably contains Bi ions.

[0065] In the glass according to this embodiment, the lower limit of the Ti ion content is preferably 1%, more preferably 2% and 3% in that order. The upper limit of the Ti ion content is preferably 45%, more preferably 40%, 35%, 30%, 25%, 20%, 15%, and 12% in that order. Here, the Ti ion is Ti 4+ , Ti 3+ In addition, all Ti ions with different valences are included.

[0066] Ti ions, like Nb ions, W ions and Bi ions, contribute greatly to increasing the refractive index and also have the function of increasing the coloring of glass. On the other hand, if the content of Ti ions is too high, the melting property of glass decreases and glass raw materials tend to remain unmelted. Therefore, it is preferable that the content of Ti ions is within the above range.

[0067] In the glass according to this embodiment, the lower limit of the Nb ion content is preferably 1%, more preferably 5%, 10%, and 15% in that order. The upper limit of the Nb ion content is preferably 45%, more preferably 40%, 35%, 30%, 25%, 23%, and 20% in that order. Nb ions are Nb 5+ In addition, it includes all Nb ions with different valences.

[0068] Nb ions are a component that contributes to a high refractive index and increases the coloring of glass. They also have the function of improving the thermal stability and chemical durability of glass. On the other hand, if the content of Nb ions is too high, the thermal stability of glass tends to decrease. Therefore, it is preferable that the content of Nb ions is within the above range.

[0069] In the glass according to this embodiment, the upper limit of the W ion content is preferably 30%, more preferably 25%, 20%, 15%, and 13% in that order. The lower limit of the W ion content is preferably 0.5%, more preferably 1%, 2%, and 3% in that order. W ions are 6+ In addition, it includes all W ions with different valences.

[0070] W ions contribute to a high refractive index and also have the effect of increasing the coloring of the glass, so the content of W ions is preferably within the above range.

[0071] In the glass according to this embodiment, the upper limit of the content of Bi ions is preferably 40%, more preferably 35%, 30%, 28%, and 25% in that order. The lower limit of the content of Bi ions is preferably 0.5%, more preferably 1%, 2%, and 2.5% in that order. Bi ions are 3+ In addition, all Bi ions with different valences are included.

[0072] Bi ions contribute to a high refractive index and also have the effect of increasing the coloring of the glass, so the content of Bi ions is preferably within the above range.

[0073] In the glass according to this embodiment, the lower limit of the total content of Ti, Nb and W ions [Ti+Nb+W] is preferably 1%, more preferably 5%, 10%, 15%, 20% and 23% in that order. The upper limit of the total content [Ti+Nb+W] is preferably 60%, more preferably 55%, 50%, 45%, 40%, 38% and 35% in that order.

[0074] In the glass according to this embodiment, the upper limit of the total content of Ti, Nb, W and Bi ions [Ti+Nb+W+Bi] is preferably 80%, more preferably 75%, 70%, 68% and 65% in that order. The lower limit of the total content [Ti+Nb+W+Bi] is preferably 1%, more preferably 5%, 10%, 15%, 20%, 23% and 25% in that order.

[0075] In the glass according to this embodiment, P 5+ , B 3+ and Si 4+ The cation ratio of the total content of Ti ions, Nb ions, W ions and Bi ions to the total content of [(Ti + Nb + W + Bi) / (P 5+ +B 3+ +Si 4+ The lower limit of the cation ratio [(Ti+Nb+W+Bi) / (P 5+ +B 3+ +Si 4+ The upper limit of )] is preferably 4.0, and more preferably 3.5, 3.0, 2.7, and 2.5 in that order.

[0076] In the glass according to this embodiment, Ta 5+ The upper limit of the content of Ta is preferably 5%, and more preferably 3%, 2%, and 1% in that order. 5+ The content may be 0%.

[0077] Ta 5+ has the function of improving the thermal stability of the glass. 5+ If the content of Ta is too high, the refractive index of the glass tends to be low and the melting property tends to be deteriorated. 5+ The content is preferably within the above range.

[0078] In the glass according to this embodiment, Li + The upper limit of the content of Li is preferably 35%, and more preferably 30%, 27%, 25%, 23%, and 20% in that order.+ The lower limit of the content of Li is preferably 1%, and more preferably 2%, 3%, 5%, and 8% in that order. + The content may be 0%.

[0079] In the glass according to this embodiment, Na + The upper limit of the content of Na is preferably 40%, and more preferably 35%, 30%, 25%, 20%, and 18%, in that order. + The lower limit of the Na content is preferably 0.5%, and more preferably 1%, 1.5%, 3%, and 5% in that order. + The content may be 0%.

[0080] Glass is Li + or Na + The inclusion of Li makes it easier to chemically strengthen the glass. + or Na + If the content of Li is too high, the thermal stability of the glass may decrease. + and Na + The content of each of the above is preferably within the above range.

[0081] In the glass according to this embodiment, Li + and Na + The total content of [Li + +Na + The upper limit of the total content [Li + +Na + The lower limit of is preferably 1%, and more preferably 5%, 10%, 15%, and 20% in that order.

[0082] In the glass according to this embodiment, K + The upper limit of the content of is preferably 20%, more preferably 15%, 13%, 10%, 8%, 5%, and 3%, in that order. + The lower limit of the content of K is preferably 0.1%, more preferably 0.5%, 1.0%, and 1.2% in that order. +The content may be 0%.

[0083] K + has the function of improving the thermal stability of glass. + If the content is too high, the thermal stability tends to decrease. + The content is preferably within the above range.

[0084] In the glass according to this embodiment, Rb + The upper limit of the content of Rb is preferably 5%, more preferably 3%, 1%, and 0.5%, in that order. + The content may be 0%.

[0085] In the glass according to this embodiment, Cs + The upper limit of the Cs content is preferably 5%, more preferably 3%, 1%, and 0.5%, in that order. + The content may be 0%.

[0086] Rb + and Cs + On the other hand, if the content of these elements is too high, the refractive index nd decreases and the volatilization of glass components during melting may increase. + and Cs + The content of each of the above is preferably within the above range.

[0087] In the glass according to this embodiment, Mg 2+ The upper limit of the Mg content is preferably 15%, more preferably 10%, 5%, 3%, and 1% in that order. 2+ The content may be 0%.

[0088] In the glass according to this embodiment, Ca 2+ The upper limit of the content of Ca is preferably 15%, and more preferably 10%, 5%, 3%, and 1% in that order. 2+ The content may be 0%.

[0089] In the glass according to this embodiment, Sr 2+ The upper limit of the Sr content is preferably 15%, more preferably 10%, 5%, 3%, and 1% in that order. 2+ The content may be 0%.

[0090] In the glass according to this embodiment, Ba 2+ The upper limit of the Ba content is preferably 25%, and more preferably 20%, 18%, 15%, 10%, and 5% in that order. 2+ The content may be 0%.

[0091] Mg 2+ , Ca 2+ , Sr 2+ and Ba 2+ Each of these glass components functions to improve the thermal stability and meltability of the glass. On the other hand, if the content of these glass components is too high, the high refractive index may be lost and the thermal stability of the glass may be reduced. Therefore, it is preferable that the content of each of these glass components is within the above-mentioned range.

[0092] In the glass according to this embodiment, Mg 2+ , Ca 2+ , Sr 2+ and Ba 2+ The total content of [Mg 2+ +Ca 2+ +Sr 2+ +Ba 2+ The upper limit of is preferably 30%, and more preferably 25%, 20%, 18%, 15%, 10%, and 5%, in that order.

[0093] In the glass according to this embodiment, Zn 2+ The upper limit of the content of Zn is preferably 15%, and more preferably 10%, 8%, 5%, 3%, and 1% in that order. 2+ The lower limit of the content of Zn is preferably 0.1%, more preferably 0.3%, and even more preferably 0.5%. 2+ The content may be 0%.

[0094] Zinc2+ It has the function of improving the thermal stability of glass. On the other hand, Zn 2+ If the content is too high, the melting property may deteriorate. 2+ The content is preferably within the above range.

[0095] In the glass according to this embodiment, Zr 4+ The upper limit of the content of Zr is preferably 5%, more preferably 3%, 2%, and 1% in that order. 4+ The content may be 0%.

[0096] Zr 4+ has the function of improving the thermal stability of glass. 4+ If the content of Zr is too high, the thermal stability and meltability of the glass tend to decrease. 4+ The content is preferably within the above range.

[0097] In the glass according to this embodiment, Ga 3+ The upper limit of the Ga content is preferably 3%, more preferably 2% and further more preferably 1%. 3+ The lower limit of the content of Ga is preferably 0%. 3+ The content may be 0%.

[0098] In the glass according to this embodiment, In 3+ The upper limit of the content of In is preferably 3%, more preferably 2% and further more preferably 1%. 3+ The lower limit of the content of In is preferably 0%. 3+ The content may be 0%.

[0099] In the glass according to this embodiment, Sc 3+ The upper limit of the content of Sc is preferably 3%, more preferably 2% and further more preferably 1%. 3+ The lower limit of the content of Sc is preferably 0%. 3+ The content may be 0%.

[0100] In the glass according to this embodiment, Hf 4+ The upper limit of the content of Hf is preferably 3%, more preferably 2% and further more preferably 1%. 4+ The lower limit of the content of Hf is preferably 0%. 4+ The content may be 0%.

[0101] In the glass according to this embodiment, Lu 3+ The upper limit of the content of Lu is preferably 3%, more preferably 2% and further more preferably 1%. 3+ The lower limit of the content of Lu is preferably 0%. 3+ The content may be 0%.

[0102] In the glass according to this embodiment, Ge 4+ The upper limit of the content of Ge is preferably 3%, more preferably 2% and further more preferably 1%. 4+ The lower limit of the content is preferably 0%. 4+ The content may be 0%.

[0103] In the glass according to this embodiment, La 3+ The upper limit of the content of La is preferably 5%, more preferably 4% and further more preferably 3%. 3+ The lower limit of the content of La is preferably 0%. 3+ The content may be 0%.

[0104] In the glass according to this embodiment, Gd 3+ The upper limit of the content of Gd is preferably 5%, more preferably 4% and further more preferably 3%. 3+ The lower limit of the content of Gd is preferably 0%. 3+ The content may be 0%.

[0105] In the glass according to this embodiment, Y 3+ The upper limit of the content of Y is preferably 5%, more preferably 4% and further more preferably 3%. 3+ The lower limit of the content of Y is preferably 0%.3+ The content may be 0%.

[0106] In the glass according to this embodiment, Yb 3+ The upper limit of the content of Yb is preferably 3%, more preferably 2% and further more preferably 1%. 3+ The lower limit of the content of Yb is preferably 0%. 3+ The content may be 0%.

[0107] The cationic components of the glass according to this embodiment are mainly the components mentioned above, i.e., P 5+ , B 3+ , Si 4+ , Al 3+ , Ti ions, Nb ions, W ions, Bi ions, Ta 5+ , Li + , Na + , K + , Rb + , Cs + , Mg 2+ , Ca 2+ , Sr 2+ , B.A. 2+ , Zn 2+ , Zr 4+ , Ga 3+ , In 3+ , Sc 3+ , Hf 4+ , Lu 3+ , Ge 4+ , La 3+ , Gd 3+ , Y 3+ and Yb 3+ The total content of the above-mentioned components is preferably greater than 95%, more preferably greater than 98%, even more preferably greater than 99%, and even more preferably greater than 99.5%.

[0108] The glass according to this embodiment contains F as an anion component. - and O 2- It may contain ingredients other than F. - and O 2- The other anion components are Cl - , Br- , I - However, Cl - , Br - , I - All of these components are prone to volatilization during glass melting. The volatilization of these components can cause problems such as changes in glass properties, a decrease in glass homogeneity, and increased wear on melting equipment. - The content of Br is preferably less than 5 anion %, more preferably less than 3 anion %, even more preferably less than 1 anion %, particularly preferably less than 0.5 anion %, and even more preferably less than 0.25 anion %. - and I - The total content is preferably less than 5 anion %, more preferably less than 3 anion %, even more preferably less than 1 anion %, particularly preferably less than 0.5 anion %, even more preferably less than 0.1 anion %, and even more preferably 0 anion %.

[0109] The "anion %" refers to a molar percentage when the total content of all anion components is taken as 100%.

[0110] The glass according to this embodiment is preferably composed basically of the above-mentioned components, but may contain other components as long as the effects of the present invention are not impaired.

[0111] For example, the glass according to this embodiment may further contain an appropriate amount of copper (Cu) as a glass component in order to impart near-infrared light absorption properties to the glass. In addition, V, Cr, Mn, Fe, Co, Ni, Pr, Nd, Pm, Sm, Eu, Tb, Dy, Ho, Er, Tm, Ce, etc. may be contained. These increase the coloring of the glass and can be a source of fluorescence.

[0112] Further, the present invention does not exclude the inclusion of unavoidable impurities.

[0113] <Other ingredient composition> Pb, As, Cd, Tl, Be, and Se are all toxic, and therefore the glass of the present embodiment preferably does not contain these elements as glass components.

[0114] U, Th, and Ra are all radioactive elements, and therefore the glass of the present embodiment preferably does not contain these elements as glass components.

[0115] Sb 3+ , Sn 4+ , and Ce 4+ is a glass component that functions as a fining agent and can be added as an optional component. 3+ is a fining agent with a great fining effect.

[0116] Sb 3+ The content of Sb is converted to Sb2O3 and expressed as a percentage by mass. 3+ , Sn 4+ , and Ce 4+ The content ratio of the cationic components other than Sb is converted to oxide in the same manner as Sb2O3, and Sb 3+ , Sn 4+ , and Ce 4+ The content of Sb2O3 is expressed in mass% when the total content ratio of all cationic components other than Sb2O3 is 100 mass%. The content of Sb2O3 is preferably less than 2 mass%, more preferably less than 1 mass%, even more preferably less than 0.5 mass%, and even more preferably less than 0.2 mass%, less than 0.1 mass%, or less than 0.05 mass%. By setting the content of Sb2O3 in the above range, the clarity of the glass can be improved.

[0117] Sn 4+ and Ce 4+ The content of each element is expressed as an oxide equivalent. 3+ , Sn 4+ , and Ce 4+ The content ratio of the cationic components other than Sb is converted to oxide. 3+ , Sn 4+ , and Ce 4+The SnO2 content and CeO2 content are expressed in mass% when the total content ratio of all cationic components other than are 100 mass%. Each of the SnO2 and CeO2 contents is preferably less than 2 mass%, more preferably less than 1 mass%, further preferably less than 0.5 mass%, and even more preferably less than 0.1 mass%. Each of the SnO2 and CeO2 contents may be 0 mass%. By setting each of the SnO2 and CeO2 contents within the above ranges, the clarity of the glass can be improved.

[0118] (Glass manufacturing) The glass according to the present embodiment is obtained by preparing a colorless glass and forming a colored layer thereon. The colorless glass may be produced according to a known glass production method. For example, a plurality of compounds are mixed together to prepare a batch raw material, and the batch raw material is placed in a melting vessel to melt, clarify, and homogenize the raw material, and then the molten glass is formed and slowly cooled to obtain glass. Alternatively, the batch raw material is placed in a melting vessel to roughly melt (rough melt). The molten material obtained by the rough melting is quenched and crushed to produce cullet. The cullet is further placed in a melting vessel to be heated and remelted (remelt) to obtain molten glass, and the molten glass is further clarified and homogenized, and then the molten glass is formed and slowly cooled to obtain glass. A known method may be applied to the forming and slowly cooling of the molten glass.

[0119] Furthermore, the glass manufacturing process according to this embodiment may include a step of increasing the water content in the glass melt. Examples of steps of increasing the water content in the glass melt include a step of adding water vapor to the melting atmosphere and a step of bubbling a gas containing water vapor into the melt. Of these, it is preferable to include a step of adding water vapor to the melting atmosphere. By including a step of increasing the water content in the glass melt, the βOH value of the glass can be increased. By increasing the βOH value, glass with higher transparency can be obtained.

[0120] (Formation of colored layer) The colored layer can be formed by attaching a metal film to the glass surface and subjecting it to a heat treatment in a reducing atmosphere.

[0121] The metal constituting the metal film is preferably a metal that absorbs hydrogen ions in the atmosphere and reduces the glass components contained in the glass by transferring hydrogen ions and electrons. Among the glass components, a metal that reduces transition metals is more preferable. Specifically, Ni, Au, Ag, Pt, Pd, and Pt-Pd alloys can be mentioned.

[0122] The method for attaching a metal film to a glass surface is not particularly limited as long as the metal film can be attached so as to adhere closely to the glass surface. Examples of the method include vapor deposition, sputtering, plating, or application of a metal paste or plating liquid.

[0123] The reducing atmosphere may contain a gas having reducing power. An example of the gas having reducing power is hydrogen. Therefore, it is preferable to use a hydrogen-containing gas as the reducing atmosphere, and a forming gas containing hydrogen may be used. The forming gas is a mixed gas consisting of hydrogen and nitrogen, and usually contains about 3 to 5 volume % of hydrogen.

[0124] The heat treatment is performed at a temperature 200° C. lower than the glass transition temperature (Tg-200) and lower than the softening point. The heat treatment time can be appropriately adjusted depending on the desired degree of coloring, the area of ​​the colored layer, the thickness of the colored layer, etc.

[0125] After the heat treatment, the metal film is peeled off from the glass surface by any method, including, but not limited to, polishing or dissolving.

[0126] By the heat treatment in a reducing atmosphere, a colored layer is formed from the surface of the glass in contact with the metal film to the interior thereof.

[0127] The mechanism by which the colored layer is formed by the above method is not particularly limited, but is thought to be as follows. The color of the colored layer formed in this embodiment is considered to be a reduction color caused by glass components, and in particular, a reduction color caused by transition metals. Usually, even if a glass molded body is heat-treated in an atmosphere containing hydrogen at a low concentration of about 3 to 5 volume %, the glass hardly exhibits a reduction color. However, since the above-mentioned metal film absorbs hydrogen ions in the atmosphere, the portion of the glass in contact with the metal film is supplied with more hydrogen ions than the portion not in contact with the metal film, and as a result, the reduction reaction proceeds faster. Therefore, the portion of the glass in contact with the metal film is colored deeply. The amount of hydrogen ions absorbed by the metal film is large, so much that the hydrogen concentration in the atmosphere is reduced due to the absorption by the metal film. For this reason, the reduction reaction does not proceed easily in the portion not in contact with the metal film.

[0128] The reduction reaction of the glass components that causes coloring proceeds in all directions from the part in contact with the metal film. That is, when observed from the cross section of the glass, the colored layer is formed in the thickness direction from the glass surface in contact with the metal film, and when observed from the surface of the glass, it is formed radially from the part in contact with the metal film.

[0129] According to the above method, a colored layer that is more deeply colored can be formed. Therefore, even if the thickness of the colored layer is small, the transmittance can be sufficiently reduced. When the thickness of the colored layer is small, the range of the colored layer formed radially from the part that was in contact with the metal film, observed from the surface of the glass, is also small. In other words, according to the present embodiment, by adjusting the forming conditions of the colored layer, a colored layer having approximately the same shape as the metal film can be formed when observed from the surface of the glass.

[0130] (Manufacturing of optical elements, etc.) The optical element made of the glass according to this embodiment is obtained by preparing an uncolored optical element and forming a colored layer thereon. The uncolored optical element may be produced according to a known production method. For example, molten glass is poured into a mold and molded into a plate shape to produce a glass material. The obtained glass material is appropriately cut, ground, and polished to produce cut pieces of a size and shape suitable for press molding. The cut pieces are heated and softened, and press molded (reheat pressed) by a known method to produce an optical element blank that is similar to the shape of the optical element. The optical element blank is annealed, and then ground and polished by a known method to produce an optical element.

[0131] A colored layer can be formed on the produced optical element by the above-mentioned method. Alternatively, a colored layer may be formed during the production of the optical element.

[0132] The optically functional surface of the prepared optical element may be coated with an anti-reflection film, a total reflection film, or the like depending on the intended use.

[0133] According to one aspect of the present invention, an optical element made of the above glass can be provided. Examples of the type of optical element include lenses such as spherical lenses and aspherical lenses, and prisms. Examples of the lens shape include biconvex lenses, plano-convex lenses, biconcave lenses, plano-concave lenses, convex meniscus lenses, and concave meniscus lenses. The optical element can be manufactured by a method including a process of processing a glass molded body made of the above glass. Examples of the processing include cutting, machining, rough grinding, fine grinding, polishing, and the like.

[0134] An example of an optical element is an optical element for blocking light that is obliquely incident on the light receiving surface of an image sensor such as a CCD or C-MOS sensor. Conventionally, in order to block obliquely incident light on the light receiving surface of an image sensor, a method has been used in which black ink is applied to the portion of the cover glass surface of the image sensor where the obliquely incident light is to be blocked, thereby providing light blocking properties. This method has a problem in that light is reflected on the surface of the black ink at the boundary between the portion where the black ink is applied and the portion where the black ink is not applied, causing stray light and degrading the image quality of the image sensor. In addition, when the temperature of the ink rises, it degasses, causing the cover glass surface to become cloudy. In response to this, the glass of this embodiment is used, and a colored layer is provided at the portion where the obliquely incident light is to be blocked, and the cover glass is used, thereby solving the problems of stray light and clouding due to degassing.

[0135] According to one embodiment of the present invention, the decorative property of the colored layer can be utilized to make it possible to use the product as a decorative item, an exterior of a small electronic device, or the like. EXAMPLES

[0136] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0137] Glass samples having the glass compositions shown in Table 1 were prepared by the following procedure, and various evaluations were carried out.

[0138] [Table 1]

[0139] [Glass manufacturing] Oxides, hydroxides, metaphosphates, carbonates, and nitrates corresponding to the components of glass were prepared as raw materials, and the raw materials were weighed and mixed so that the composition of the resulting glass would be each composition shown in Table 1, and the raw materials were thoroughly mixed. The resulting mixed raw materials (batch raw materials) were placed in a platinum crucible and heated at 1100 to 1450°C for 2 to 3 hours to make molten glass. The molten glass was stirred to homogenize it and clarify it, and then cast into a mold preheated to an appropriate temperature. The cast glass was heat treated for about 1 hour near the glass transition temperature Tg, and allowed to cool to room temperature in a furnace. The glass was processed to a size of 40 mm in length, 10 mm in width, and 1.0 mm in thickness, and two faces measuring 40 mm x 10 mm were precision polished (optical polished) to obtain a glass sample.

[0140] [Confirmation of glass composition] The content of each glass component in the obtained glass sample was measured by inductively coupled plasma atomic emission spectrometry (ICP-AES), and it was confirmed that each composition was as shown in Table 1.

[0141] [Optical property measurements] The refractive index nd, specific gravity and glass transition temperature Tg of the obtained glass samples were measured, and the results are shown in Table 1.

[0142] (i) Refractive index nd The refractive index nd was measured by the refractive index measurement method of JIS B 7071-1.

[0143] (ii) Specific gravity The specific gravity was measured by the Archimedes method.

[0144] (iii) Glass transition temperature Tg The glass transition temperature Tg was measured using a thermomechanical analyzer (TMA4000S) manufactured by MAC Sciences at a heating rate of 4° C. / min.

[0145] [Average linear expansion coefficient] The average linear expansion coefficient was measured according to the Japan Optical Glass Industry Association standard JOGIS 08-2003 "Method of measuring thermal expansion of optical glass". The diameter of the rod-shaped sample was 5 mm. The results are shown in Table 1.

[0146] [Acid resistance weight loss rate Da] In accordance with the provisions of the Japan Optical Glass Industry Association standard JOGIS06-2009, the obtained glass sample was made into powder glass (particle size 425-600μm) with a weight equivalent to the specific gravity, placed in a platinum cage, immersed in a quartz glass round-bottom flask containing a 0.01mol / L nitric acid solution, and treated in a boiling water bath for 60 minutes, and the weight loss rate (%) before and after the treatment was measured. The weight loss rate was evaluated by a grade. The results are shown in Table 1.

[0147] Example 1: Formation of colored layers in samples with different glass compositions (Example 1-1) Of the obtained glass samples, a Pt-Pd film was formed in a pattern on one of the optically polished surfaces of the glass sample having the glass composition No. 1 by sputtering (sputtering current: 15 mA, film formation time: 900 sec).

[0148] The glass sample on which the Pt-Pd film was formed was heat-treated at 400°C for 5 hours while supplying forming gas (hydrogen 3 volume %, nitrogen 97 volume %) as a reducing atmosphere at a flow rate of 0.2 L / min. The Pt-Pd film was removed by polishing. A glass sample having a colored layer was obtained. The obtained glass sample is shown in Figure 5-1.

[0149] [Transmittance measurement] The external transmittance was measured at wavelengths of 300 to 2500 nm. The external transmittance is defined as the percentage of the transmitted light intensity relative to the incident light intensity when light is incident in the thickness direction of the glass sample [transmitted light intensity / incident light intensity x 100]. The external transmittance also includes the reflection loss of light rays on the sample surface. The results are shown in Figure 6-1. In the figure, the dashed line indicates the transmittance of the part with the colored layer, and the solid line indicates the transmittance of the same part before the colored layer was formed.

[0150] [OD measurement] For the portion having the colored layer, the incident light intensity I0 and the transmitted light intensity I at a wavelength of 1100 nm were measured, and the OD (optical density) was calculated using the following formula. For the same portion, the OD before the colored layer was formed was also calculated in the same manner. The results are shown in Table 2. OD=-log 10 (I / I0)

[0151] (Example 1-2) A glass sample having a colored layer was obtained in the same manner as in Example 1-1, except for using a glass sample having the glass composition of No. 2. The obtained glass sample is shown in FIG. The transmittance was measured in the same manner as in Example 1-1, and the results are shown in Figure 6-2. The OD was measured in the same manner as in Example 1-1, and the results are shown in Table 2.

[0152] (Examples 1-3) A glass sample having a colored layer was obtained in the same manner as in Example 1-1, except that a glass sample having the glass composition of No. 3 was heat-treated at 430° C. for 9 hours. The transmittance was measured in the same manner as in Example 1-1, and the results are shown in Figure 6-3. The OD was measured in the same manner as in Example 1-1, and the results are shown in Table 2.

[0153] [Table 2]

[0154] (Examples 1 to 4) A glass sample having the glass composition shown in Table 6 was prepared in the same manner as above. The glass component composition was confirmed in the same manner as above, and the refractive index nd, specific gravity, and glass transition temperature Tg were measured. In addition, a forming gas was supplied with the hydrogen concentration (volume %) and flow rate shown in Table 6, and heat treatment was performed at the treatment temperature and treatment time shown in Table 6. A glass sample having a colored layer was obtained in the same manner as in Example 1-1. OD was measured in the same manner as in Example 1-1. The results are shown in Table 6.

[0155] [Table 6]

[0156] Example 2: Formation of colored layers using metal films with different thicknesses (Example 2-1) On one of the optically polished surfaces of the glass sample having the glass composition of No. 3, Pt-Pd films having thicknesses of 28 nm, 256 nm, 288 nm, and 420 nm were formed by adjusting the film formation conditions.

[0157] The glass sample on which the Pt-Pd film was formed was heat-treated at 400°C for 4 hours while supplying forming gas (hydrogen 3 volume %, nitrogen 97 volume %) as a reducing atmosphere at a flow rate of 0.2 L / min. The Pt-Pd film was removed by polishing to obtain a glass sample having a colored layer.

[0158] The transmittance of the portion having the colored layer was measured in the same manner as in Example 1-1. The relationship between the thickness of the Pt-Pd film and the transmittance is shown in FIG. The OD of the portion having the colored layer was measured in the same manner as in Example 1-1. The relationship between the thickness of the Pt-Pd film and the OD is shown in FIG.

[0159] (Example 2-2) On one of the optically polished surfaces of the glass sample having the glass composition of No. 3, Pt-Pd films having thicknesses of 437 nm, 695 nm, 778 nm, and 892 nm were formed by adjusting the film formation conditions.

[0160] The glass sample on which the Pt-Pd film was formed was heat-treated at 400°C for 9 hours while supplying forming gas (hydrogen 3 volume %, nitrogen 97 volume %) as a reducing atmosphere at a flow rate of 0.2 L / min. The Pt-Pd film was removed by polishing to obtain a glass sample having a colored layer.

[0161] The transmittance was measured in the same manner as in Example 2-1. The relationship between the thickness of the Pt-Pd film and the transmittance is shown in FIG. The OD was measured in the same manner as in Example 2-1. The relationship between the thickness of the Pt-Pd film and the OD is shown in FIG.

[0162] From Figures 7-1, 7-2, and 8, it was found that the transmittance and OD of the portion having the colored layer depend on the heat treatment time, not on the thickness of the metal film.

[0163] Example 3: Formation of colored layers using different types of metal films (Example 3-1) Glass samples having a colored layer were obtained in the same manner as in Example 1-1, except that Au films with thicknesses of 15 nm and 300 nm were formed instead of the Pt-Pd film on the optically polished surface of a glass sample having the glass composition of No. 3, and heat-treated at 450°C for 7 hours. For the portion having the colored layer, OD was measured in the same manner as in Example 1-1.

[0164] (Example 3-2) A glass sample having a colored layer was obtained in the same manner as in Example 1-1, except that, instead of forming a Pt-Pd film on the optically polished surface of a glass sample having the glass composition of No. 3, an Ag paste was applied and the sample was heat-treated at 430°C for 10 hours. The OD was measured in the same manner as in Example 3-1, and the results are shown in Table 3.

[0165] [Table 3]

[0166] (Example 3-3) A glass sample having a colored layer was obtained in the same manner as in Example 1-1, except that a Ni film having a thickness of about 15 nm was formed on the optically polished surface of the glass sample having the glass composition of No. 3, instead of a Pt-Pd film, using a vacuum deposition machine, and heat-treated at 430°C for 7 hours. The OD was measured in the same manner as in Example 3-1. The results are shown in Table 9.

[0167] (Examples 3-4) A glass sample having a colored layer was obtained in the same manner as in Example 1-1, except that a commercially available Pd plating solution was applied to the optically polished surface of a 0.4 mm thick glass sample having the glass composition of No. 14 instead of a Pt-Pd film, and the Pd plating film was formed by drying at room temperature and then heat-treating at 410°C for 15 hours. The OD was measured in the same manner as in Example 3-1. The results are shown in Table 9.

[0168] [Table 9]

[0169] Example 4: Cross-sectional observation of glass with a colored layer (Example 4-1) A Pt-Pd film was formed on one of the optically polished surfaces of a glass sample having the glass composition of No. 3. In addition, a part of the optically polished surface of the same sample was polished using a #1000 abrasive, and a Pt-Pd film was also formed on that part.

[0170] The material was heat-treated at 400° C. for 5 hours while supplying forming gas (hydrogen 3 vol %, nitrogen 97 vol %) at a flow rate of 0.2 L / min. The Pt-Pd film was removed by polishing to obtain a glass sample having a colored layer.

[0171] The thickness of the colored layer was measured. The results are shown in Table 4. A micrograph of a cross section of a portion having a colored layer is also shown in Table 4. In the micrograph in Table 4, the right side is the glass, and the black part in the center is the colored layer.

[0172] (Example 4-2) An Au film was formed on one of the optically polished surfaces of the glass sample having the glass composition of No. 3. A glass sample having a colored layer was obtained in the same manner as in Example 4-1, except that the heat treatment was carried out at 450° C. for 7 hours.

[0173] Table 4 shows the thickness of the colored layer and a micrograph of the cross section of the portion having the colored layer. The OD of the portion having the colored layer was measured in the same manner as in Example 1-1. The results are shown in Table 4.

[0174] (Example 4-3) An Au film was formed on one of the optically polished surfaces of a glass sample having the glass composition of No. 3. A glass sample having a colored layer was obtained in the same manner as in Example 4-2, except that the Au film formation time was made longer than in Example 4-2.

[0175] Table 4 shows the thickness of the colored layer and a micrograph of the cross section of the portion having the colored layer. The OD was measured in the same manner as in Example 4-2, and the results are shown in Table 4.

[0176] (Example 4-4) A glass sample having a colored layer was obtained in the same manner as in Example 4-2, except that a Pt-Pd film was formed on both optically polished surfaces of the glass sample having the glass composition of No. 3.

[0177] Table 4 shows the thickness of the colored layer and a micrograph of the cross section of the portion having the colored layer. The OD was measured in the same manner as in Example 4-2, and the results are shown in Table 4.

[0178] [Table 4]

[0179] The surface polished using #1000 abrasive has a larger surface roughness than the optically polished surface. Table 4 shows that the thickness of the colored layer formed changes depending on the surface roughness of the glass.

[0180] Example 5: Formation of a colored layer having a dot pattern A Pt-Pd film was formed in a dot pattern on the optically polished surface of the glass sample having the glass composition of No. 3. The details are as follows.

[0181] A metal plate with a high level of flatness that can cover the glass surface and a dot pattern of openings was prepared. The metal plate was attached to the optically polished surface of the glass sample, and a Pt-Pd film was formed to fit the dot pattern of openings.

[0182] The metal plate was peeled off, and the glass sample having the Pt-Pd film formed in a dot pattern was heat-treated in the same manner as in Example 1-3 to obtain a glass sample having a colored layer. The resulting glass sample is shown in FIG.

[0183] Example 6: Change in transmittance by removing the colored layer A glass sample having a colored layer was obtained in the same manner as in Example 1-3, except that the glass sample having the glass composition of No. 3 was processed to have a thickness of 750 μm.

[0184] The cross section of the portion having the colored layer was observed under a microscope, and it was confirmed that the thickness of the colored layer was 110 μm. In addition, the OD of the portion having the colored layer was measured in the same manner as in Example 1-1. The results are shown in Table 5.

[0185] The obtained glass sample was polished from the side having the colored layer so that the thickness of the glass sample was 660 μm, and the OD of the same part was measured. The results are shown in Table 5.

[0186] Similarly, the glass samples were polished to thicknesses of 610 μm, 500 μm, and 380 μm, and the OD was measured for the same portions. The amount of change from the OD before polishing (no polishing allowance, i.e., no removal by polishing) was also calculated. The OD results are shown in Table 5. In Table 5, "polishing allowance" refers to the amount removed by polishing, and is shown as a thickness. [Table 5]

[0187] According to Table 5, when the polishing allowance (amount removed by polishing) of the glass sample exceeds 140 μm, the change in OD becomes small. When the colored layer of the glass sample is removed by polishing, only the non-colored portion (transparent area without coloring) remains. Therefore, even if the thickness is further reduced by polishing, the OD hardly changes. In other words, from the result of the OD change due to polishing, it is estimated that the thickness of the colored layer of the glass sample is more than 90 μm and less than 140 μm. This is consistent with the thickness of the colored layer (110 μm) based on the microscopic observation of the cross section. Note that the increase or decrease in OD when the polishing allowance (amount removed by polishing) is in the range of 140 to 370 μm is slight, and is considered to be a measurement error.

[0188] Example 7: Change in transmittance by removing the colored layer (2) A glass sample having a colored layer was obtained in the same manner as in Example 1-1, except that the glass sample having the glass composition of No. 3 was processed to have a thickness of 1 mm.

[0189] The cross section of the portion having the colored layer was observed under a microscope, and it was confirmed that the thickness of the colored layer was about 55 μm. A micrograph of the cross section of the portion having the colored layer is shown in FIG. 10. In addition, the OD at wavelengths of 1100 nm and 780 nm was measured for the portion having the colored layer in the same manner as in Example 1-1. Furthermore, the OD was measured when the portion having the colored layer was removed by 7 μm, 17 μm, 32 μm, 52 μm, 71 μm, and 83 μm in the thickness direction. The actual OD value, the change in OD compared to before removing the colored layer (OD1-OD2), and ΔOD at this time are shown in Tables 7 and 8. In addition, the actual OD value when the horizontal axis is the amount of removal in the thickness direction is shown in the graphs of FIGS. 11 and 12. The ΔOD was calculated by the following formula. ΔOD=(OD1-OD2) / (removal amount [μm])

[0190] [Table 7]

[0191] [Table 8] [Explanation of symbols]

[0192] 1 Glass body 2 colored layer

Claims

1. A glass having a colored layer including a region in which ΔOD at wavelengths of 1100 nm and 780 nm is 0.04 or more: The ΔOD is calculated as follows: For glass having a colored layer, the OD at a wavelength of 1100 nm or 780 nm is defined as OD1, and the thickness is defined as T1. When a predetermined amount of the colored layer is removed in the thickness direction by polishing or the like, the OD at the same wavelength is defined as OD2, and the thickness is defined as T2. In this case, ΔOD=(OD1-OD2) / (T1-T2).

2. The glass described in claim 1, wherein the OD of the colored layer at wavelengths of 1100 nm and 780 nm is 1.0 or more.

3. 10. The glass of claim 1 having areas of low and high transmittance.

4. 2. The glass according to claim 1, wherein the transmittance of the colored layer is smaller than the transmittance of a portion where the colored layer is not formed.

5. 5. The glass according to claim 1, wherein the composition of the colored layer is the same as the composition of the portion on which the colored layer is not formed.

6. The glass according to any one of claims 1 to 5, which contains Bi ions as a glass component.

7. The glass of any one of claims 1 to 6, which is a phosphate glass.

8. P 5+ The content of is 10 cation % to 50%, P 5+ B relative to the content of 3+ The cationic ratio of the content [B 3+ / P 5+ ] is 0.70 or less, S 4+ The content is 10 cation % or less, The glass according to claim 7, wherein the total content of Ti ions, Nb ions, W ions and Bi ions [Ti + Nb + W + Bi] is 1 cation % to 80 cation %.

9. The content of Ti ions is 1 cation % to 45 cation %; The content of Nb ions is 1 cation % to 45 cation %; The content of W ions is 30 cation % or less, The glass according to claim 8, wherein the content of Bi ions is 40 cation % or less.

10. 10. The glass according to claim 1, having a refractive index of 1.70 or more.

11. An optical element comprising the glass according to any one of claims 1 to 10.

Citation Information

Patent Citations

  • Method for manufacturing glass formed article, optical element obtained by the method, and method for treating glass

    JP2002201041A

  • Optical glass, optical element and preform

    JP2014156394A

  • Target for obtaining colored glazing

    JP2020517833A

  • Multi-core optical fiber

    JP2021148966A