Electrolytes, electrochemical devices and electronic devices

An electrolyte with phosphineoxypolycyano functional group compounds and other additives forms stable films on electrode surfaces, addressing the challenges of high-temperature storage and cycle performance in lithium ion batteries, enhancing their safety and efficiency.

JP7587501B2Active Publication Date: 2024-11-20NINGDE AMPEREX TECHNOLOGY LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021533327
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-23
Publication Date
2024-11-20
Estimated Expiration
2040-12-23

AI Technical Summary

Technical Problem

Lithium ion batteries face challenges in achieving thinner, lighter designs with higher energy density, diverse shapes, and improved safety, particularly in terms of high-temperature storage performance, cycle performance, and float charging performance.

Method used

The development of an electrolyte comprising specific compounds, such as phosphineoxypolycyano functional group compounds, combined with other additives like boron-based lithium salts and sulfur-oxygen double bond functional group-containing compounds, which form stable films on electrode surfaces to suppress electrolyte decomposition and improve oxidation resistance.

Benefits of technology

The electrolyte significantly enhances high-temperature storage performance, cycle performance, and float charging performance of lithium ion batteries by stabilizing transition metals and reducing gas generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587501000001
    Figure 0007587501000001
  • Figure 0007587501000002
    Figure 0007587501000002
  • Figure 0007587501000003
    Figure 0007587501000003
Patent Text Reader

Abstract

The present invention provides an electrolyte, an electrochemical device, and an electronic device that can improve high-temperature storage performance, cycle performance, and float charging performance. In one aspect of the invention, there is provided an electrolyte comprising a compound of formula IA, [Formula 1] TIFF2023510989000066.tif59166Here, A 1 , A 2 , A 3 is selected from formula IB and formula IC, R 11 , R 13 is a substituted or unsubstituted C1-C 10 Alkylene group, C2-C 10 Alkenylene group, C2-C 10 Alkynylene group, C3-C 10 Arenylene group, C6-C 10 Arylene group, C3-C 10 alicyclic hydrocarbylene groups, which, if substituted, contain halogen; R 12 is a halogen, substituted or unsubstituted C1-C 10 Alkyl groups, C2-C 10 Alkenyl groups, C2-C 10 Alkynyl groups, C3-C 10 Cumulative diene group, C6-C 10 Aryl groups, C3-C 10 An electrolyte selected from alicyclic hydrocarbyl groups, which, if substituted, contain a halogen.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of electrochemistry, and in particular to electrolytes, electrochemical devices and electronic devices. [Background technology]

[0002] Electrochemical devices such as lithium ion batteries have attracted widespread attention and are widely used due to their characteristics of high energy density, high power density, stable service life, etc. With the rapid development of technology, the diversification of market needs, and the future rise of energy storage systems and electric vehicle industries, there are many requirements for lithium ion batteries, such as thinner, lighter, more diverse shapes, higher safety, higher energy density, etc. Summary of the Invention

[0003] In some embodiments, the present invention provides an electrolyte comprising a compound of formula IA, [ka] Here, A 1 , A 2 , A 3 are each independently selected from formula IB and formula IC; A 1 , A 2 , and A 3 at least two of the formula IC, [ka] wherein in formula IA, n is selected from an integer from 1 to 10, m is selected from 0 and 1, and in formula IB and formula IC, R 11 , R 13 each independently represents a substituted or unsubstituted C-C 10 Alkylene groups, substituted or unsubstituted C2-C 10 Alkenylene groups, substituted or unsubstituted C2-C 10 Alkynylene groups, substituted or unsubstituted C3-C 10Allenylene group, substituted or unsubstituted C6-C 10 Arylene groups, substituted or unsubstituted C3-C 10 alicyclic hydrocarbylene groups, and when substituted, the substituents include halogen; R 12 each independently represents a halogen or a substituted or unsubstituted C-C 10 Alkyl groups, substituted or unsubstituted C2-C 10 Alkenyl groups, substituted or unsubstituted C2-C 10 Alkynyl groups, substituted or unsubstituted C3-C 10 Cumulative diene group, substituted or unsubstituted C6-C 10 Aryl groups, substituted or unsubstituted C3-C 10 When selected from the group consisting of alicyclic hydrocarbyl groups, the substituents provide an electrolyte that contains a halogen. The number 1 shown below represents the bonding site of two adjacent atoms.

number

[0004] In some embodiments, the compound represented by formula IA includes at least one of the compounds represented by formulas (I-1) to (I-30). [ka] [ka]

[0005] In some embodiments, the weight percentage of the compound represented by formula IA, based on the weight of the electrolyte, is between 0.01% and 10%.

[0006] In some embodiments, the electrolyte further comprises at least one of a compound represented by formula II-A, a compound represented by formula III-A, a compound represented by formula IV-A, a compound represented by formula VA, a compound represented by formula VB, and a polynitrile compound; [ka] Here, R 21 , R 22 are each independently selected from the group consisting of a substituted or unsubstituted C1-C5 alkyl group, a substituted or unsubstituted C2-C5 alkenyl group, and a substituted or unsubstituted C2-C5 alkynyl group, and when substituted, the substituents include halogen; R 21 and R 22 may be linked to form a cyclic structure, [ka] Here, A 31 , A 32 , A 33 , A 34 are each independently one selected from the group consisting of halogen, formula III-X, formula III-Y, and formula III-Z, and when formula III-Y is selected, A is selected so as to form a cyclic structure. 31 , A 32 , A 33 , A 34 wherein two or four are selected from formula III-Y; [ka] Here, R 31 , R 33 are each independently selected from the group consisting of a substituted or unsubstituted C1-C6 alkyl group and a substituted or unsubstituted C2-C6 alkenyl group; R 32are each independently selected from the group consisting of a substituted or unsubstituted C1-C6 alkylene group and a substituted or unsubstituted C2-C6 alkenylene group, and when substituted, the substituent includes a halogen; the number 1 represents the bonding site of two adjacent atoms; in formula III-Y, the O atom is bonded to the B atom in formula III-A; and k is 0 or 1; [ka] Here, x and y each independently represent 0 or 1. When one of the numbers 2 in formula IV-A represents a single bond, one of x and y is 1 and the other is 0. When both of the numbers 2 in formula IV-A represent single bonds, both of x and y are 1. When both of the numbers 2 in formula IV-A represent double bonds, both of x and y are 0. 42 , A 43 , A 45 , A 46 are each independently selected from the group consisting of halogen, a substituted or unsubstituted C1-C6 alkyl group, formula IV-B, formula IV-C, and formula IV-D, and when formula IV-C is selected, A is 42 , A 43 , A 45 , A 46 Two or four of A are selected from formula IV-C; 41 , A 44 are each independently selected from the group consisting of oxygen, halogen, a substituted or unsubstituted C1-C6 alkyl group, formula IV-B, formula IV-C, and formula IV-D, and when formula IV-C is selected, A 41 , A 44 are each selected from formula IV-C, where, if substituted, the substituents include halogen; A 41 , A 42 , A 43 , A 44 , A 45 , A 46 is not all fluorine, [ka] In formula IV-B, formula IV-C, and formula IV-D, R 41 , R 43 are each independently selected from the group consisting of a substituted or unsubstituted C1-C6 alkyl group and a substituted or unsubstituted C2-C6 alkenyl group; R 42 is selected from the group consisting of a substituted or unsubstituted C1-C6 alkylene group, a substituted or unsubstituted C2-C6 alkenylene group, and when substituted, the substituents include halogen; in formula IV-C, the O atom is bonded to the P atom in formula IV-A; z represents 0 or 1; [ka] Here, R 51 , R 52 , R 53 , R 54 are each independently a substituted or unsubstituted C1-C5 alkyl group, a substituted or unsubstituted C2-C 10 Alkenyl groups, substituted or unsubstituted C2-C 10 Alkynyl groups, substituted or unsubstituted C3-C 10 Alicyclic groups, substituted or unsubstituted C6-C 10 selected from the group consisting of an aryl group, a substituted or unsubstituted C1-C6 aliphatic heterocyclic group, a substituted or unsubstituted C1-C6 aromatic heterocyclic group, and a substituted or unsubstituted C1-C6 heteroatom-containing functional group, where when substituted, the substituents include halogens, and R 51 , R 52 may be bonded to form a ring structure, R 53 , R 54 may be bonded to form a ring structure, and the heteroatom in the heteroatom-containing functional group includes at least one of B, N, O, Si, P, and S. The following number 2 represents a single bond or a double bond.

number

[0007] In some embodiments, the electrolyte satisfies at least one of the following conditions: a) the weight percentage of the compound represented by formula II-A is 0.01% to 10% based on the weight of the electrolyte; b) the weight percentage of the compound represented by formula III-A is 0.1% to 5% based on the weight of the electrolyte; c) the weight percentage of the compound represented by formula IV-A is 0.1% to 5% based on the weight of the electrolyte; d) the sum of the weight percentages of the compound represented by formula VA and the compound represented by formula VB is 0.01% to 10% based on the weight of the electrolyte; and e) the weight percentage of the polynitrile compound is 0.1% to 10% based on the weight of the electrolyte.

[0008] In some embodiments, the compound represented by formula II-A includes at least one of the compounds represented by formulae (II-1) to (II-22). [ka]

[0009] In some embodiments, the compound of Formula III-A includes at least one of lithium tetrafluoroborate, lithium bis(oxalato)borate, and lithium difluoro(oxalato)borate.

[0010] In some embodiments, the compound of formula IV-A includes at least one of lithium difluorophosphate, lithium difluorobis(oxalato)phosphate, and lithium tetrafluoro(oxalato)phosphate.

[0011] In some embodiments, the compound represented by formula VA includes at least one of the compounds represented by formulae (V-1) to (V-16). [ka] The compound represented by formula VB includes at least one of the compounds represented by formulae (V-17) to (V-20). [ka]

[0012] In some embodiments, the polynitrile compound includes at least one of 1,2,3-tris(2-cyanoethoxy)propane, 1,3,6-hexanetricarbonitrile, 1,2-bis(2-cyanoethoxy)ethane, and adiponitrile.

[0013] In some embodiments, the present invention further provides an electrochemical device comprising a positive electrode sheet, a negative electrode sheet, a separator, and an electrolyte of the present invention.

[0014] In some embodiments, the present invention further provides an electronic device comprising an electrochemical device of the present invention.

[0015] The electrolyte of the present invention can significantly improve the high-temperature storage performance, cycle performance, and float charge performance of an electrochemical device using the electrolyte. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The disclosed embodiments are merely examples of the invention, which may be embodied in various forms, and it should be understood that the specific details disclosed in the specification of the invention should not be construed as limitations, but merely as a basis for the claims to teach those skilled in the art how to implement the invention in its various forms, and as a representative basis.

[0017] In the description of the present invention, unless otherwise specified and limited, terms such as "Additive A", "Additive B", "Additive C", "Additive D", "Additive E", "Additive F", etc. are used merely for descriptive purposes and cannot be understood as indicating or implying relative importance and relationships to one another. In the description of the present invention, unless otherwise specified and limited, letters and numbers in terms such as "Formula IA", "Formula IB", "Formula I-1", "Formula II-A", "Formula II-B", "Formula II-1", etc. are used merely for marking purposes and cannot be understood as indicating or implying relative importance, relationships to one another, or chemical elements.

[0018] In the description of this invention, unless otherwise specified, the functional groups of all compounds can be substituted or unsubstituted.

[0019] In the description of the present invention, unless otherwise specified, the term "heteroatom" refers to an atom other than C and H. In some embodiments, the heteroatom includes at least one of B, N, O, Si, P, and S. In the description of the present invention, the term "heteroatom-containing functional group" refers to a functional group that includes at least one heteroatom. In the description of the present invention, the term "heterocyclic group" refers to a cyclic group that includes at least one heteroatom. In some embodiments, the heterocyclic group includes at least one of an aliphatic heterocyclic group and an aromatic heterocyclic group.

[0020] In the description of this invention, the term "alicyclic hydrocarbyl group" refers to a cyclic hydrocarbon group of an aliphatic nature, which contains a closed carbon ring within the molecule.

[0021] In the description of the present invention, an alkylene group is a divalent group formed by removing one hydrogen atom from an alkyl group, an alkenylene group is a divalent group formed by removing one hydrogen atom from an alkenyl group, an alkynylene group is a divalent group formed by removing one hydrogen atom from an alkynyl group, an alkyleneoxy group is a divalent group formed by removing one hydrogen atom from an alkoxy group, and an arylene group is a divalent group formed by removing one hydrogen atom from an aryl group. In the description of the present invention, the structure of a divalent group that is not clearly described is interpreted according to the description in this paragraph.

[0022] In the present description, the cumulative diene group refers to a group in which two double bonds share one carbon, and the structural formula of the cumulative diene group is: [ka] It is.

[0023] In the description of the present invention, terms not clearly explained, substitutions in structural formulae, etc. should be understood according to known, general, and customary means or methods by those skilled in the art.

[0024] The electrolyte, electrochemical device, and electronic device of the present invention will be described in detail below.

[0025] [Electrolyte] <Additive A> In some embodiments, the electrolyte contains Additive A, where Additive A is at least one compound represented by Formula (IA). [ka] Here, A 1 , A 2 , A 3 are each independently selected from formula IB and formula IC; A 1 , A 2 , and A 3 at least two of the formula IC, [ka] wherein in formula (IA), n is selected from an integer from 1 to 10, m is selected from 0 and 1, and in formulas (IB) and (IC), R 11 , R 13 each independently represents a substituted or unsubstituted C-C 10 Alkylene groups, substituted or unsubstituted C2-C 10 Alkenylene groups, substituted or unsubstituted C2-C 10 Alkynylene groups, substituted or unsubstituted C3-C 10 Allenylene group, substituted or unsubstituted C6-C 10 Arylene groups, substituted or unsubstituted C3-C 10 alicyclic hydrocarbylene groups, and when substituted, the substituents include halogen; R 12 each independently represents a halogen or a substituted or unsubstituted C-C 10 Alkyl groups, substituted or unsubstituted C2-C 10 Alkenyl groups, substituted or unsubstituted C2-C 10 Alkynyl groups, substituted or unsubstituted C3-C 10 Cumulative diene groups, substituted or unsubstituted C6-C 10 Aryl groups, substituted or unsubstituted C3-C 10 Alicyclic hydrocarbyl groups, when substituted, include halogen. The number 1 shown below represents the bonding site of two adjacent atoms.

number

[0026] In the electrolyte of the present invention, additive A is a phosphineoxypolycyano functional group compound. The cyano (-CN) functional group contained in the structure of the phosphineoxypolycyano functional group compound can form a complex with the transition metal in the positive electrode active material of the electrochemical device, so that the transition metal on the surface of the positive electrode active material can be stabilized. At the same time, the phosphineoxypolycyano functional group compound has a phosphineoxy functional group in the molecule, so that it can improve the oxidation resistance of the transition metal complex, effectively inhibit the continuous decomposition of the electrolyte, and inhibit gas generation at high temperatures. Therefore, the electrolyte can significantly improve the high-temperature storage performance, cycle performance, and float charging performance of the electrochemical device.

[0027] In some embodiments, additive A includes at least one of the compounds represented by formulae (I-1) to (I-30). [ka] [ka]

[0028] In some embodiments, the weight percentage of additive A in the electrolyte is 0.01% to 10% relative to the weight of the electrolyte. In some embodiments, the weight percentage of additive A in the electrolyte may be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0%, 6.0%, 7.0%, 8.0%, or 9.0% relative to the weight of the electrolyte.

[0029] <Additive B> In some embodiments, the electrolyte may further include an additive B, and the additive B is at least one compound represented by formula (II-A). [ka] Here, R 21 , R 22are each independently selected from the group consisting of a substituted or unsubstituted C1-C5 alkyl group, a substituted or unsubstituted C2-C5 alkenyl group, and a substituted or unsubstituted C2-C5 alkynyl group, and when substituted, the substituents include halogen; R 21 and R 22 may be bonded to form a cyclic structure. Additive B is a carboxylic anhydride compound. When additive A and additive B are added to the electrolyte at the same time, the high-temperature storage performance of the electrochemical device can be further improved. The carboxylic anhydride can form a film on the surface of the positive electrode active material and the negative electrode active material, and can also neutralize the alkalinity of the active material on the surface of the positive electrode, which is believed to further suppress the decomposition of the electrolyte, reduce gas generation, and improve the high-temperature storage performance.

[0030] In some embodiments, Additive B includes at least one of the compounds represented by formulae (II-1) to (II-22). [ka]

[0031] In some embodiments, the mass percentage of additive B in the electrolyte is 0.01% to 10% relative to the mass of the electrolyte. In some embodiments, the mass percentage of additive B in the electrolyte may be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0%, 6.0%, 7.0%, 8.0%, or 9.0% relative to the mass of the electrolyte.

[0032] <Additive C> In some embodiments, the electrolyte may further include an additive C, and the additive C is at least one compound represented by formula (III-A). [ka] Here, A 31 , A 32 , A 33 , A34 are each independently one selected from the group consisting of halogen, formula (III-X), formula (III-Y), and formula (III-Z), and when formula (III-Y) is selected, A is 31 , A 32 , A 33 , A 34 wherein two or four are selected from formula (III-Y), [ka] Here, R 31 , R 33 are each independently selected from the group consisting of a substituted or unsubstituted C1-C6 alkyl group and a substituted or unsubstituted C2-C6 alkenyl group; R 32 are each independently selected from the group consisting of a substituted or unsubstituted C1-C6 alkylene group and a substituted or unsubstituted C2-C6 alkenylene group, and when substituted, the substituent includes a halogen; the number 1 represents the bonding site of two adjacent atoms; in formula (III-Y), the O atom bonds to the B atom in formula (III-A); and k is 0 or 1.

[0033] Additive C is a boron-based lithium salt compound. When additive A and additive C are added to the electrolyte at the same time, the high-temperature storage performance of the electrochemical device can be further improved. It is believed that the boron-based lithium salt compound forms a stable interfacial film on the surface of the positive electrode active material, further reducing the contact between the positive electrode and the electrolyte, reducing the decomposition of the electrolyte, and further improving the high-temperature storage performance.

[0034] In some embodiments, Additive C includes at least one of lithium tetrafluoroborate (LiBF4), lithium bis(oxalato)borate (LiBOB), and lithium difluoro(oxalato)borate (LiDFOB).

[0035] In some embodiments, the mass percentage of additive C in the electrolyte is 0.1% to 5% relative to the mass of the electrolyte. In some embodiments, the mass percentage of additive C in the electrolyte may be 0.2%, 0.3%, 0.5%, 1%, 2%, or 3% relative to the mass of the electrolyte.

[0036] <Additive D> In some embodiments, the electrolyte may further include an additive D, and the additive D is at least one compound represented by formula (IV-A). [ka] Here, x and y each independently represent 0 or 1. When one of the numbers 2 in formula (IV-A) represents a single bond, one of x and y is 1 and the other is 0. When both of the numbers 2 in formula (IV-A) represent single bonds, both of x and y are 1. When both of the numbers 2 in formula (IV-A) represent double bonds, both of x and y are 0. 42 , A 43 , A 45 , A 46 are each independently selected from the group consisting of halogen, a substituted or unsubstituted C1-C6 alkyl group, formula (IV-B), formula (IV-C), and formula (IV-D), and when formula (IV-C) is selected, A 42 , A 43 , A 45 , A 46 Two or four of A are selected from formula (IV-C); 41 , A 44 are each independently selected from the group consisting of oxygen, halogen, a substituted or unsubstituted C1-C6 alkyl group, formula (IV-B), formula (IV-C), and formula (IV-D), and when formula (IV-C) is selected, A 41 , A 44 are each selected from formula (IV-C), where, if substituted, the substituents include halogen; A 41 , A 42 , A 43 , A 44 , A45 , A 46 is not all fluorine, [ka] In formula (IV-B), formula (IV-C), and formula (IV-D), R 41 , R 43 are each independently selected from the group consisting of a substituted or unsubstituted C1-C6 alkyl group and a substituted or unsubstituted C2-C6 alkenyl group; R 42 is selected from the group consisting of substituted or unsubstituted C1-C6 alkylene groups and substituted or unsubstituted C2-C6 alkenylene groups, and when substituted, the substituent includes halogen, and in formula (IV-C), the O atom is bonded to the P atom in formula (IV-A), and z represents 0 or 1. The following number 2 represents a single bond or a double bond.

number

[0037] Additive D is a phosphorus-based lithium salt compound. When additive A and additive D are added to the electrolyte at the same time, the high-temperature storage performance of the electrochemical device can be further improved. It is believed that the phosphorus-based lithium salt compound forms an interface film on the surface of the positive electrode active material, and the interface film containing the phosphorus-based lithium salt compound has high oxidation resistance, which further suppresses the oxidative decomposition of the electrolyte, reduces gas generation, and further improves the high-temperature storage performance.

[0038] In some embodiments, Additive D includes at least one of lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalato)phosphate (LiDFOP), and lithium tetrafluoro(oxalato)phosphate (LiTFOP).

[0039] In some embodiments, the weight percentage of the additive D in the electrolyte is 0.1%-5% based on the weight of the electrolyte. In some embodiments, the weight percentage of the additive D in the electrolyte may be 0.2%, 0.3%, 0.5%, 1%, 2%, 3% based on the weight of the electrolyte.

[0040] <Additive E> In some embodiments, the electrolyte may further include an additive E, and the additive E is at least one of a compound represented by formula (VA) and a compound represented by formula (VB). [ka] Here, R 51 , R 52 , R 53 , R 54 are each independently a substituted or unsubstituted C1-C5 alkyl group, a substituted or unsubstituted C2-C 10 Alkenyl groups, substituted or unsubstituted C2-C 10 Alkynyl groups, substituted or unsubstituted C3-C 10 Alicyclic groups, substituted or unsubstituted C6-C 10 selected from the group consisting of an aryl group, a substituted or unsubstituted C1-C6 aliphatic heterocyclic group, a substituted or unsubstituted C1-C6 aromatic heterocyclic group, and a substituted or unsubstituted C1-C6 heteroatom-containing functional group, where when substituted, the substituents include halogens, and R 51 , R 52 may be bonded to form a ring structure, R 53 , R 54 may be bonded to form a ring structure, and the heteroatom in the heteroatom-containing functional group includes at least one of B, N, O, Si, P, and S.

[0041] Additive E is a compound containing a sulfur-oxygen double bond functional group. The compound containing a sulfur-oxygen double bond has a strong antioxidant ability, so that the electrolyte is less likely to be oxidized on the surface of the positive electrode active material. On the other hand, the compound containing a sulfur-oxygen double bond functional group can form a film on the surface of the negative electrode active material, so that the protection of the active material can be further strengthened.

[0042] In some embodiments, the compound represented by formula (VA) includes at least one of the compounds represented by formulas (V-1) to (V-16). [ka]

[0043] In some embodiments, the compound represented by formula (VB) includes at least one of the compounds represented by formulas (V-17) to (V-20). [ka]

[0044] In some embodiments, the mass percentage of the additive E in the electrolyte is 0.01% to 10%, preferably 0.1% to 8%, based on the mass of the electrolyte. In some embodiments, the mass percentage of the additive E in the electrolyte may be 0.02%, 0.05%, 0.2%, 0.3%, 0.4%, 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0%, 6.0%, 7.0%, or 9.0%, based on the mass of the electrolyte.

[0045] <Additive F> In some embodiments, the electrolyte may further include an additive F. The additive F is a polynitrile compound. In some embodiments, the polynitrile compound includes at least one of 1,2,3-tris(2-cyanoethoxy)propane, 1,3,6-hexanetricarbonitrile, 1,2-bis(2-cyanoethoxy)ethane, and adiponitrile.

[0046] Adding additive A and additive F to the electrolyte simultaneously can further improve the high-temperature storage performance and cycle performance of the electrochemical device. If too much additive A is added, the viscosity of the electrolyte becomes too high, which is thought to affect the dynamic performance of the electrochemical device and reduce the cycle performance. However, the addition of additive F can effectively prevent the viscosity of the electrolyte from becoming too high, effectively increase the stability of the positive electrode active material, and further reduce the decomposition of the electrolyte, thereby improving the high-temperature storage performance and cycle performance of the electrochemical device.

[0047] In some embodiments, the mass percentage of additive F in the electrolyte is 0.01% to 10%, preferably 0.5% to 5%, based on the mass of the electrolyte. In some embodiments, the mass percentage of additive F in the electrolyte may be 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0%, 6.0%, 7.0%, or 9.0%, based on the mass of the electrolyte.

[0048] In some embodiments, when Additive A and Additive F are added to the electrolyte simultaneously, the ratio of the mass percentage of Additive A to the mass percentage of Additive F is 0.01-1.

[0049] Regarding the additives of the present invention, when the electrolyte contains additive A, at least one of additive B, additive C, additive D, additive E, and additive F can also be added. By using additive A in combination with at least one of additive B, additive C, additive D, additive E, and additive F in the electrolyte, the electrochemical performance of the electrochemical device can be further improved.

[0050] <Organic solvent> In some embodiments, the electrolyte further comprises an organic solvent. The organic solvent is an organic solvent known in the art suitable for electrochemical devices, for example, a non-aqueous organic solvent is commonly used. In some embodiments, the non-aqueous organic solvent comprises at least one of carbonate-based solvents, carboxylic acid ester-based solvents, ether-based solvents, sulfone-based solvents, and other aprotic solvents.

[0051] In some embodiments, the carbonate based solvent comprises at least one of dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, dipropyl carbonate, ethylene carbonate, propylene carbonate, butylene carbonate.

[0052] In some embodiments, the carboxylic acid ester solvent comprises at least one of methyl formate, ethyl formate, ethyl acetate, propyl acetate, butyl acetate, methyl propionate, ethyl propionate, propyl propionate, 2,2-difluoroethyl acetate, 2,2-difluoroethyl acetate, gamma-butyrolactone, valerolactone, and butyrolactone.

[0053] In some embodiments, the ether solvent comprises at least one of ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, dibutyl ether, tetrahydrofuran, and 2-methyltetrahydrofuran.

[0054] In some embodiments, the sulfone solvent comprises at least one of ethyl vinyl sulfone, methyl isopropyl sulfone, isopropyl sec-butyl sulfone, and sulfolane.

[0055] In the present invention, the organic solvent in the electrolytic solution may be a non-aqueous organic solvent, which may be used alone or in combination of two or more. When a mixed solvent is used, the mixing ratio can be controlled to obtain electrochemical devices with different performances.

[0056] <Electrolyte salt> In some embodiments, the electrolyte further comprises an electrolyte salt. The electrolyte salt may be any electrolyte salt known in the art suitable for electrochemical devices. Appropriate electrolyte salts may be selected for various electrochemical devices. For example, for lithium ion batteries, the electrolyte salt typically uses a lithium salt.

[0057] In some embodiments, the lithium salt comprises at least one of an organic lithium salt or an inorganic lithium salt.

[0058] In some embodiments, the lithium salt used in the present invention includes at least one of an element fluorine and an element phosphorus.

[0059] In some embodiments, the lithium salt of the present invention is lithium hexafluorophosphate (LiPF6), lithium bissulfonimide (LiN(C y F 2y+1 SO2)(C z F 2z+1 SO2), where y and z are natural numbers.

[0060] In some embodiments, the concentration of the lithium salt in the electrolyte is about 0.5-3 mol / L, preferably about 0.5-2 mol / L, and more preferably about 0.8-1.5 mol / L, based on the total volume of the electrolyte.

[0061] In the present invention, the method for preparing the electrolyte solution is not limited, and the electrolyte solution can be prepared according to a conventional method for preparing an electrolyte solution well known to those skilled in the art.

[0062] [Electrochemical equipment] Next, the electrochemical device of the present invention will be described.

[0063] The electrochemical device of the present invention is, for example, a primary battery, a secondary battery, a fuel cell, a solar cell, or a capacitor. The secondary battery is, for example, a lithium secondary battery. The lithium secondary battery includes, but is not limited to, a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery, or a lithium ion polymer secondary battery.

[0064] In some embodiments, an electrochemical device includes a positive electrode sheet, a negative electrode sheet, a separator, and the electrolyte of the present invention.

[0065] In some embodiments, the electrochemical device of the present invention has a charge cutoff voltage of 4.2V or greater.

[0066] <Positive electrode sheet> The positive electrode sheet is a positive electrode sheet known in the art that can be used in an electrochemical device. In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer provided on the positive electrode current collector. The positive electrode active material layer includes a positive electrode active material, a positive electrode conductive agent, and a positive electrode binder.

[0067] The positive electrode active material may be used as a positive electrode active material in an electrochemical device, and may be any material known in the art that can reversibly insert and extract active ions. In some embodiments, the positive electrode active material includes a composite oxide including lithium and at least one selected from the group consisting of cobalt, manganese, and nickel.

[0068] In some embodiments, the positive electrode active material is: Li a A 1-b B b D2 (where 0.90≦a≦1.8, 0≦b≦0.5), Li a E 1-b B b O 2-c D c (Here, 0.90≦a≦1.8,0 <b≦0.5,0≦c≦0.05)、LiE 2-b B b 0 4-c D c (where 0≦b≦0.5, 0≦c≦0.05), Li a Ni 1-b-c Co b B c D α (where 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, 0<α≦2), Li a Ni 1-b-c Co b B c O 2-α F α (where 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, 0<α<2), Li a Ni 1-b-c Co b B c O 2-α F2 (where 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, 0<α<2), Li a Ni 1-b-c Mn b B c D α (Here, 0.90≦a≦1.8,0 <b≦0.5,0≦c≦0.05,0<α<2)、Li a Ni1-b-c Mn b B c O 2-α F α (where 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, 0<α<2), Li a Ni 1-b-c Mn b B c O 2-α F2 (where 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, 0<α<2), Li a Ni b E c G d O2 (where 0.90≦a≦1.8, 0≦b≦0.9, 0≦c≦0.5, 0.001≦d≦0.1), Li a Ni b Co c Mn d G e O2 (where 0.90≦a≦1.8, 0≦b≦0.9, 0≦c≦0.5, 0≦d≦0.5, 0.001≦e≦0.1), Li a NiG b O2 (where 0.90≦a≦1.8, 0.001≦b≦0.1), Li a CoG b O2 (where 0.90≦a≦1.8, 0.001≦b≦0.1), Li a MnG b O2 (where 0.90≦a≦1.8, 0.001≦b≦0.1), Li a Mn2G b O4 (where 0.90≦a≦1.8, 0.001≦b≦0.1), QO2, QS2, LiQS2, V2O5, LiV2O5, LiIO2, LiNiVO4, Li 3-f J2(PO4)3(0≦f≦2), Li 3-f Contains at least one of Fe2(PO4)3 (0≦f≦2) and LiFePO4.

[0069] In the above chemical formula, A is Ni, Co, Mn or a combination thereof; B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element or a combination thereof; D is O, F, S, P or a combination thereof; E is Co, Mn or a combination thereof; F is F, S, P or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V or a combination thereof; Q is Ti, Mo, Mn or a combination thereof; I is Cr, V, Fe, Sc, Y or a combination thereof; and J is V, Cr, Mn, Co, Ni, Cu or a combination thereof.

[0070] In some embodiments, the positive electrode active material D v 10 is 18 μm or less.

[0071] In some embodiments, the positive electrode active material has a specific surface area BET of 0.5 m 2 / g or less.

[0072] The positive electrode conductive agent is used to provide electrical conductivity to the positive electrode, and can improve the electrical conductivity of the positive electrode. The positive electrode conductive agent is a conductive material known in the art that can be used as the positive electrode active material layer. The positive electrode conductive agent can be selected from any conductive material as long as it does not cause chemical changes. In some embodiments, the positive electrode conductive agent includes at least one of the following: a carbon-based material such as natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, and carbon fiber; a metal-based material such as metal powder or metal fiber including copper, nickel, aluminum, silver, and the like; and a conductive polymer such as a polyphenylene derivative.

[0073] The positive electrode binder is a binder known in the art that can be used as the positive electrode active material layer. The positive electrode binder can improve the adhesion performance between the positive electrode active material particles and between the positive electrode active material particles and the positive electrode current collector. In some embodiments, the positive electrode binder includes at least one of polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, a polymer containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene butadiene rubber, acrylated styrene butadiene rubber, epoxy resin, and nylon.

[0074] In some embodiments, the positive electrode active material layer has a compressed density of 4.5 g / cm 3 In some embodiments, the positive electrode active material layer has a compressed density of 4.0-4.3 g / cm 3 It is.

[0075] The positive electrode current collector is a metal, and in some embodiments the metal is, for example but not limited to, aluminum foil.

[0076] In some embodiments, the positive electrode sheet construction is any positive electrode sheet construction known in the art that may be used in electrochemical devices.

[0077] In some embodiments, the method for preparing the positive electrode sheet is a method for preparing a positive electrode sheet known in the art that can be used in an electrochemical device. In some embodiments, the preparation of the positive electrode slurry typically involves adding a positive electrode active material and a binder, optionally adding a conductive material and a thickener, and dissolving or dispersing them in a solvent to prepare a positive electrode slurry. The solvent is removed by volatilization during a drying process. The solvent is a solvent known in the art that can be used as a positive electrode active material layer, such as, but not limited to, N-methylpyrrolidone (NMP).

[0078] <Negative electrode sheet> The negative electrode sheet is a well-known negative electrode sheet in the art that can be used in an electrochemical device. In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer provided on the negative electrode current collector. The negative electrode active material layer includes a negative electrode active material, a negative electrode conductive agent, and a negative electrode binder.

[0079] The negative electrode active material can be used as the negative electrode active material of an electrochemical device, and a well-known material in the art that can insert and desorb active ions and dope and undope active ions may be used.

[0080] In some embodiments, the negative electrode active material includes at least one of lithium metal, a lithium metal alloy, a material capable of doping / undoping lithium, a transition metal oxide, and a carbon material.

[0081] In some embodiments, the lithium metal alloy includes at least one metal selected from the group consisting of Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn, and lithium.

[0082] In some embodiments, the material capable of doping / undoping lithium is Si, SiO x (0 < x < 2), a Si / C composite, a Si-Q alloy (where Q is not Si and is an alkali metal, an alkaline earth metal, a Group 13-16 element, a transition element, a rare earth element, or a combination thereof), Sn, SnO z (0 < z < 2), a Sn / C composite, a Sn-R alloy (where R is not Sn and is an alkali metal, an alkaline earth metal, a Group 13-16 element, a transition element, a rare earth element, or a combination thereof), and includes at least one of them.

[0083] Here, exemplary elements of Q and R may be at least one of Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po.

[0084] In some embodiments, SiO x (0 < x < 2) is a porous silicon-based anode active material, and porous SiO x The average particle diameter D50 of the particles is 1 μm to 20 μm. In some embodiments, when measured on the surface, SiO x The average diameter of the pores of the particles is 30 nm to 500 nm, and SiO x The specific surface area of the particles is 5 m 2 / g to 50 m 2 / g. In some embodiments, the SiO x particle silicon-based anode active material may further contain at least one of Li2SiO3 and Li4SiO4.

[0085] In some embodiments, in the Si / C composite, carbon is not aggregated and dispersed in the form of lumps within the Si particles, but is uniformly dispersed within the Si particles in an atomic state. In some embodiments, the molar ratio of C to Si (i.e., C / Si) can be in the range greater than 0 and less than 18. In some embodiments, based on the total weight of the Si / C composite, the carbon content in the Si / C composite is 1% - 50%. In some embodiments, the particle diameter of the Si / C composite can be 10 nm - 100 μm.

[0086] The carbon material may be selected from various carbon materials known in the art that can be used as carbon-based negative electrode active materials in electrochemical devices. In some embodiments, the carbon material includes at least one of crystalline carbon and amorphous carbon. In some embodiments, the crystalline carbon is natural graphite or artificial graphite. In some embodiments, the crystalline carbon is amorphous, plate-shaped, platelet-shaped, spherical, or fibrous. In some embodiments, the crystalline carbon is low-crystalline carbon and high-crystalline carbon. In some embodiments, the low-crystalline carbon includes at least one of soft carbon and hard carbon. In some embodiments, the high-crystalline carbon includes at least one of natural graphite, crystalline graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, mesophase carbon beads, mesophase pitch, and high-temperature calcined charcoal. In some embodiments, the high-temperature calcined charcoal is coke derived from petroleum or coal tar pitch. In some embodiments, the amorphous carbon comprises at least one of soft carbon, hard carbon, mesophase pitch carbonization products, and combustion coke.

[0087] The negative electrode conductive agent is used to provide electrical conductivity to the negative electrode, and can improve the electrical conductivity of the negative electrode. The negative electrode conductive agent is a conductive material known in the art that can be used as the negative electrode active material layer. The negative electrode conductive agent can be selected from any conductive material as long as it does not cause chemical changes. In some embodiments, the negative electrode conductive agent includes at least one of the following: carbon-based materials such as natural graphite, artificial graphite, conductive carbon black, acetylene black, ketjen black, and carbon fibers; metal-based materials such as metal powders or metal fibers including copper, nickel, aluminum, and silver; and conductive polymers such as polyphenylene derivatives. The negative electrode binder is a binder known in the art that can be used as the negative electrode active material layer. In some embodiments, the negative electrode binder includes at least one of difluoroethylene-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyethylene, polypropylene, styrene butadiene rubber, acrylated styrene butadiene rubber, epoxy resin, and nylon.

[0088] The negative electrode current collector is a metal, in some embodiments, such as, but not limited to, copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, conductive metal-coated polymer substrates, and combinations thereof.

[0089] In some embodiments, the negative electrode sheet structure is any negative electrode sheet structure known in the art that may be used in an electrochemical device.

[0090] In some embodiments, the method for preparing the negative electrode sheet is a method for preparing a negative electrode sheet known in the art that can be used in an electrochemical device. In some embodiments, the preparation of the negative electrode slurry typically involves adding a negative electrode active material and a binder, optionally adding a conductive material and a thickener, and dissolving or dispersing them in a solvent to prepare a negative electrode slurry. The solvent is removed by volatilization during a drying process. The solvent is a solvent known in the art that can be used as a negative electrode active material layer, such as, but not limited to, water. The thickener is a thickener known in the art that can be used as a negative electrode active material layer, such as, but not limited to, sodium carboxymethyl cellulose.

[0091] <separator> The separator is a separator known in the art that can be used in electrochemical devices, such as, but not limited to, a polyolefin-based porous membrane. In some embodiments, the polyolefin-based porous membrane is a monolayer film or a multilayer film made of one or more materials selected from the group consisting of polyethylene (PE), ethylene-propylene copolymer, polypropylene (PP), ethylene-butene copolymer, ethylene-hexene copolymer, and ethylene-methyl methacrylate copolymer.

[0092] In some embodiments, the polyolefin-based porous film is coated with a coating layer. In some embodiments, the coating layer includes an organic coating layer and an inorganic coating layer. In some embodiments, the organic coating layer includes at least one of polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, polyacrylonitrile, polyimide, acrylonitrile-butadiene copolymer, acrylonitrile-styrene-butadiene copolymer, polymethyl methacrylate, polymethyl acrylate, polyethyl acrylate, acrylic acid-styrene copolymer, polydimethylsiloxane, sodium polyacrylate, and sodium carboxymethyl cellulose. In some embodiments, the inorganic coating layer includes at least one of SiO2, Al2O3, CaO, TiO2, ZnO2, MgO, ZrO2, and SnO2.

[0093] The present invention does not particularly limit the shape and thickness of the separator. The method for preparing the separator is a method for preparing a separator that can be used in an electrochemical device and is well known in the art.

[0094] <Outer case> In some embodiments, the electrochemical device further includes an outer casing, which may be used in electrochemical devices and is stable to the electrolyte used, as known in the art, including, but not limited to, metal-based outer casings.

[0095] [Electronic equipment] Finally, an electronic device of the present invention is described.

[0096] The electronic device of the present invention may be any electronic device, such as, but not limited to, a notebook computer, a pen-input computer, a mobile personal computer, an electronic book player, a mobile phone, a portable facsimile, a portable copy machine, a portable printer, a stereo headset, a video recorder, a liquid crystal television, a portable cleaner, a portable CD player, a mini CD, a walkie-talkie, an electronic notebook, a calculator, a memory card, a portable tape recorder, a radio, a backup power source, a motor, an automobile, a motorcycle, a bicycle assisted, a bicycle, a lighting device, a toy, a game machine, a clock, an electric tool, a flashlight, a camera, a large household storage battery, a lithium ion capacitor, etc. In addition to the above electronic devices, the electrochemical device of the present invention is also suitable for energy storage power plants, marine transportation tools, and air transportation tools. Air transportation devices include air transportation devices in the atmosphere and air transportation devices outside the atmosphere.

[0097] In some embodiments, an electronic device comprises the electrochemical device of the present invention.

[0098] The present invention will be further described below with reference to examples. In the following specific embodiments of the present invention, only the embodiment in which the battery is a lithium ion battery is shown, but the present invention is not limited thereto. In the following examples and comparative examples, all reagents, materials, and equipment used are commercially available or synthetically available unless otherwise specified.

[0099] Specific compounds used in the examples are as follows: Additive A: [ka] Additive B: Citric Acid Anhydride [ka] 2,3-Dimethylmaleic Anhydride [ka] Additive C: Lithium tetrafluoroborate (LiBF4), lithium difluoro(oxalato)borate (LiDFOB). Additive D: Lithium difluorophosphate (LiPO2F2), lithium tetrafluoro(oxalato)phosphate (LiTFOP). Additive E: 2,4-Butanesultone [ka] 1,3-Propane Sultone [ka] Ethylene Sulfate [ka] 4-Methylethylene sulfate [ka] Additive F: 1,2,3-Tris(2-cyanoethoxy)propane [ka] 1,3,6-Hexanetricarbonitrile [ka] Adiponitrile [ka] 1,2-Bis(2-cyanoethoxy)ethane [ka]

[0100] The lithium ion batteries of Examples 1-62, Comparative Examples 1-6, Examples S1-S11, and Comparative Example ' were all fabricated in the following manner.

[0101] (1) Preparation of electrolyte In an argon atmosphere glove box with a water content of less than 10 ppm, ethylene carbonate (abbreviated as EC), propylene carbonate (abbreviated as PC), diethyl carbonate (abbreviated as DEC), ethyl propionate (abbreviated as EP), and propyl propionate (abbreviated as PP) were uniformly mixed in a mass ratio of 1:1:1:1:1 to obtain a non-aqueous organic solvent, and completely dried lithium salt LiPF6 (1M) was dissolved in the non-aqueous organic solvent to obtain a base electrolyte. A predetermined mass of additive was added to the base electrolyte to prepare the electrolytes of Examples 1-62, Comparative Examples 1-6, Examples S1-S11, and Comparative Example S'.

[0102] (2) Preparation of positive electrode sheet The positive electrode active material LCO (molecular formula LiCoO2), conductive carbon black, and binder polyvinylidene fluoride (abbreviated as PVDF) were thoroughly stirred and mixed in a weight ratio of 97.9:0.9:1.2 with an appropriate amount of solvent N-methylpyrrolidone (abbreviated as NMP) to form a uniform positive electrode slurry. The slurry was applied to aluminum foil as a positive electrode current collector, dried, and cold pressed to obtain a positive electrode sheet.

[0103] (3) Preparation of negative electrode sheet A uniform negative electrode slurry was formed by thoroughly mixing the negative electrode active material graphite, the binder styrene butadiene rubber (SBR), and the thickener sodium carboxymethylcellulose (CMC) in a weight ratio of 97.4:1.4:1.2 with an appropriate amount of deionized water as a solvent. The slurry was applied to a negative electrode current collector Cu foil, dried, and cold pressed to obtain a negative electrode sheet.

[0104] (4) Preparation of separator A PE porous polymer film was used as the separator.

[0105] (5) Preparation of lithium-ion batteries The prepared positive electrode sheet, separator, and negative electrode sheet were stacked in order so that the separator was interposed between the positive electrode sheet and the negative electrode sheet to play the role of isolation, and then wound up to obtain an electrode assembly. The electrode assembly was placed in an exterior foil, and the liquid inlet was left open, and the electrolyte prepared above was poured through the liquid inlet. After going through processes such as vacuum packaging, standing, chemical formation, and shaping, the preparation of a lithium-ion battery was completed.

[0106] Next, the performance test procedures for the lithium ion batteries of Examples 1-62, Comparative Examples 1-6, Examples S1-S11, and Comparative Example S' will be described.

[0107] (1) High-temperature storage performance test at 4.45V The battery was charged at 25°C with a constant current of 0.5C up to 4.45V, then charged at a constant voltage until the current was 0.05C, the thickness of the lithium-ion battery was measured and recorded as d0, and placed in an oven at 85°C for 24h, at which time the thickness was monitored and recorded as d. The thickness expansion rate (%) of the lithium-ion battery after 24h of high temperature storage = (d-d0) / d0 x 100%. When the thickness expansion rate exceeded 50%, the test was stopped.

[0108] (2) High-temperature storage performance test at 4.5V The battery was charged at 25°C with a constant current of 0.5C up to 4.5V, then charged at a constant voltage until the current was 0.05C, the thickness of the lithium-ion battery was measured and recorded as d0, and placed in an oven at 85°C for 24h, at which time the thickness was monitored and recorded as d. The thickness expansion rate (%) of the lithium-ion battery after 24h of high temperature storage = (d-d0) / d0 x 100%. When the thickness expansion rate exceeded 50%, the test was stopped.

[0109] (3) Cycle performance test The battery was charged at 0.7C to 4.45V under conditions of 25°C, and then charged at a constant voltage of 4.45V to 0.05C. It was then discharged at a current of 1C to 3.0V, and the process of charging at 0.7C and discharging at 1C was repeated for 800 cycles, and the capacity retention rate at this time was recorded.

[0110] (4) Float charging performance test The battery was discharged at 0.5C to 3.0V at 25℃, then charged at 0.5C to 4.45V, constant voltage charged at 4.45V to 0.05C, the thickness of the lithium-ion battery was measured and recorded as d0, placed in an oven at 45℃ and constant voltage charged at 4.45V for 42 days, the thickness change was monitored and the thickness was recorded as d. Thickness expansion rate (%) of lithium-ion battery float charge = (d-d0) / d0×100%.

[0111] The types and contents of additives in the electrolytes used in Examples 1-62, Comparative Examples 1-6, Examples S1-S11, and Comparative Example S', and the performance test results of the lithium ion batteries are shown in Tables 1-4, respectively. Here, the contents of each additive are expressed as mass percentages relative to the mass of the electrolyte.

[0112] [Table 1] Note: The blank spaces in Table 1 indicate no addition.

[0113] From the examples and comparative examples in Table 1, it can be seen that compound I-5 as additive A can not only improve the 4.45V high temperature storage performance of lithium ion batteries, but also improve the 4.5V high temperature storage performance, and at the same time, the cycle performance of the battery is also greatly improved. For different charge cut-off voltages, the improvement effect is different. With increasing content, the degree of improvement first increases, then decreases, and finally tends to balance. Compounds I-11, I-12 and I-30, which are also additive A, also improve the high temperature storage performance and cycle performance of lithium batteries at various charge cut-off voltages to different degrees. Adding additive E to the electrolyte containing additive A further improves the high temperature storage performance and cycle performance of lithium batteries at different charge cut-off voltages.

[0114] The additive of Comparative Example 1 also contains a cyano group and a phosphinooxy group, but its high-temperature storage performance and cycle performance are far inferior to those of the examples containing Additive A. Additive A is a phosphineoxypolycyano functional group compound, and the cyano (-CN) functional group contained in its structure can form a complex with the transition metal in the positive electrode active material, so that the transition metal on the surface of the positive electrode active material can be stabilized, and since the molecule contains a phosphineoxy functional group, it can be attached to the surface of the positive electrode active material simultaneously with cyano to improve the oxidation resistance of the transition metal complex, which is believed to effectively suppress the continuous decomposition of the electrolyte and suppress gas generation at high temperatures.

[0115] [Table 2] Note: The blank spaces in Table 2 indicate no addition.

[0116] From the Examples and Comparative Examples in Table 2, it can be seen that when Additive C is added to an electrolyte solution containing Additive A, the high-temperature storage performance of the lithium-ion battery at 4.5 V is further improved.

[0117] [Table 3] Note: The blank spaces in Table 3 indicate no addition.

[0118] From the Examples and Comparative Examples in Table 3, it can be seen that the combined use of Additive A and Additive F can significantly improve the float charging performance of lithium ion batteries.

[0119] [Table 4] Note: The blank spaces in Table 4 indicate no addition.

[0120] From the Examples and Comparative Examples in Table 4, it can be seen that by using a combination of multiple types of Additives C to F and Additive A, the high-temperature storage performance of a lithium-ion battery can be significantly improved.

[0121] The lithium ion batteries of Examples 63-80 and Comparative Examples 7-9 were all fabricated in the following manner.

[0122] (1) Preparation of electrolyte In an argon atmosphere glove box with a water content of less than 10 ppm, ethylene carbonate (abbreviated as EC), propylene carbonate (abbreviated as PC), and diethyl carbonate (abbreviated as DEC) were mixed uniformly in a mass ratio of 3:3:4, and completely dried lithium salt LiPF6 (1M) was dissolved in the non-aqueous organic solvent to obtain a base electrolyte. A predetermined mass of additive was added to the base electrolyte to prepare the electrolytes of Examples 63-80 and Comparative Examples 7-9.

[0123] (2) Preparation of positive electrode sheet The positive electrode active material is NCM811 (molecular formula LiNi 0.8 Mn 0.1 Co 0.1O2), acetylene black as a conductive agent, and polyvinylidene fluoride (PVDF) as a binder were thoroughly stirred and mixed in a weight ratio of 96:2:2 with an appropriate amount of N-methylpyrrolidone (NMP) as a solvent to form a uniform positive electrode slurry. The slurry was applied to an aluminum foil as a positive electrode current collector, dried, and cold pressed to obtain a positive electrode sheet.

[0124] (3) Preparation of negative electrode sheet A uniform negative electrode slurry was formed by thoroughly mixing the negative electrode active material graphite, the binder styrene butadiene rubber (SBR), and the thickener sodium carboxymethylcellulose (CMC) in a weight ratio of 97.4:1.4:1.2 with an appropriate amount of deionized water as a solvent. The slurry was applied to a negative electrode current collector Cu foil, dried, and cold pressed to obtain a negative electrode sheet.

[0125] (4) Preparation of separator A PE porous polymer film was used as the separator.

[0126] (5) Preparation of lithium-ion batteries The prepared positive electrode sheet, separator, and negative electrode sheet were stacked in order so that the separator was interposed between the positive electrode sheet and the negative electrode sheet to play the role of isolation, and then wound up to obtain an electrode assembly. The electrode assembly was placed in an exterior foil, and the electrolyte prepared above was poured into the liquid inlet, leaving a liquid inlet. After vacuum packaging, standing, chemical formation, shaping, and other processes, the preparation of a lithium-ion battery was completed.

[0127] Next, the test process for the high-temperature storage performance at 85° C. of the lithium ion batteries of Examples 63-80 and Comparative Examples 7-9 will be described.

[0128] The battery was charged at 25°C with a constant current of 0.5C up to 4.25V, then charged at a constant voltage until the current was 0.05C, the thickness of the lithium-ion battery was measured and recorded as d0, and placed in an oven at 85°C for 24h, at which time the thickness was monitored and recorded as d. The thickness expansion rate (%) of the lithium-ion battery after 24h of high temperature storage = (d-d0) / d0 x 100%. When the thickness expansion rate exceeded 50%, the test was stopped.

[0129] The types and contents of additives in the electrolytes used in Examples 63-80 and Comparative Examples 7-9, and the performance test results of the lithium ion batteries are shown in Table 5. Here, the content of each additive is the mass percentage obtained with respect to the mass of the electrolyte.

[0130] [Table 5] Note: The blank spaces in Table 5 indicate no addition.

[0131] From the examples and comparative examples in Table 5, it can be seen that lithium difluorophosphate (LiPO2F2) and lithium tetrafluoro(oxalato)phosphate (LiTFOP) can form a film on the cathode, suppressing the continuous oxidation and continuous decomposition of the electrolyte, and reducing gas generation. Therefore, adding additive D to the electrolyte containing additive A can further improve the high-temperature storage performance.

[0132] The lithium ion batteries of Examples 81-96 and Comparative Examples 10-12 were all fabricated in the following manner.

[0133] (1) Preparation of electrolyte In an argon atmosphere glove box with a water content of less than 10 ppm, ethylene carbonate (abbreviated as EC), propylene carbonate (abbreviated as PC), diethyl carbonate (abbreviated as DEC), and ethyl propionate (abbreviated as EP) were mixed uniformly in a mass ratio of 1:2:6:1, and completely dried lithium salt LiPF6 (1M) was dissolved in the non-aqueous organic solvent to obtain a base electrolyte. A predetermined mass of additive was added to the base electrolyte to prepare the electrolytes of Examples 81-96 and Comparative Examples 10-12.

[0134] (2) Preparation of positive electrode sheet The positive electrode active material LCO (molecular formula LiCoO2), conductive carbon black, and binder polyvinylidene fluoride (abbreviated as PVDF) were thoroughly stirred and mixed in a weight ratio of 97.9:0.9:1.2 with an appropriate amount of solvent N-methylpyrrolidone (abbreviated as NMP) to form a uniform positive electrode slurry. The slurry was applied to aluminum foil as a positive electrode current collector, dried, and cold pressed to obtain a positive electrode sheet.

[0135] (3) Preparation of negative electrode sheet The negative electrode active materials, graphite, silicon-oxygen material, thickener, sodium carboxymethylcellulose (abbreviated as CMC), and modified polyacrylic acid were mixed in a weight ratio of 87:10:0.6:2.4 with an appropriate amount of deionized water solvent and thoroughly stirred to form a uniform negative electrode slurry. The slurry was applied to a negative electrode current collector, Cu foil, and then dried and cold pressed to obtain a negative electrode sheet.

[0136] (4) Preparation of separator A PE porous polymer film was used as the separator.

[0137] (5) Preparation of lithium-ion batteries The prepared positive electrode sheet, separator, and negative electrode sheet were stacked in order so that the separator was interposed between the positive electrode sheet and the negative electrode sheet to play the role of isolation, and then wound up to obtain an electrode assembly. The electrode assembly was placed in an exterior foil, and the electrolyte prepared above was poured into the liquid inlet, leaving a liquid inlet. After vacuum packaging, standing, chemical formation, shaping, and other processes, the preparation of a lithium-ion battery was completed.

[0138] Next, the test process for the high-temperature storage performance at 60° C. of the lithium ion batteries of Examples 81-96 and Comparative Examples 10-12 will be described.

[0139] The battery was charged at 25°C with a constant current of 0.5C to 4.45V, then charged at a constant voltage until the current was 0.05C, the thickness of the lithium-ion battery was measured and recorded as d0, and placed in an oven at 60°C for 12 days, the thickness was monitored and recorded as d, and the thickness was measured every 4 days. The thickness expansion rate (%) of the lithium-ion battery after 12 days of storage at 60°C = (d-d0) / d0 x 100%. When the thickness expansion rate exceeded 100%, the test was stopped.

[0140] The types and contents of additives in the electrolytes used in Examples 81-96 and Comparative Examples 10-12 and the performance test results of the lithium ion batteries are shown in Table 5. Here, the content of each additive is the mass percentage obtained with respect to the mass of the electrolyte.

[0141] [Table 6] Note: The blank spaces in Table 6 indicate no addition.

[0142] From the examples and comparative examples in Table 6, it can be seen that the high temperature storage performance of lithium ion batteries can be improved by combining compound II-8 or compound II-9 with additive A. Since compound II-8 or compound II-9 can form a film on the silicon anode, and additive A is used as a cathode protection additive, it is believed that additive A and additive B can both exert a synergistic effect to improve the high temperature storage performance of lithium ion batteries.

[0143] The above is merely an example of the present invention and is not intended to limit the present invention in any form. Although the preferred embodiment of the present invention is disclosed above, it is not intended to limit the present invention. Those skilled in the art may make any modifications within the scope of the technical solution of the present invention. Any modifications or modifications made using the technical content disclosed above are considered as equivalent embodiments and are all within the scope of the technical solution of the present invention.

Claims

1. An electrolyte comprising a compound represented by formula IA, 【number】 Here, A 1 , A 2 , A 3 are each independently selected from formula I-B and formula IC; A 1 , A 2 , and A 3 at least two of are of formula IC, 【number】 wherein in formula IA, n is selected from an integer from 1 to 10, and m is selected from 0 and 1; wherein in formula I-B and formula IC, the number 1 represents the bonding site of two adjacent atoms; Here, R 11 , R 13 each independently represents a substituted or unsubstituted C 1 -C 10 Alkylene group, substituted or unsubstituted C 2 -C 10 Alkenylene group, substituted or unsubstituted C 2 -C 10 Alkynylene group, substituted or unsubstituted C 3 -C 10 an allenylene group, a substituted or unsubstituted C 6 -C 10 Arylene group, substituted or unsubstituted C 3 -C 10 alicyclic hydrocarbylene groups, which, if substituted, include halogen; R 12 each independently represents a halogen atom, a substituted or unsubstituted C 1 -C 10 Alkyl group, substituted or unsubstituted C 2 -C 10 Alkenyl group, substituted or unsubstituted C 2 -C 10 Alkynyl group, substituted or unsubstituted C 3 -C 10 Cumulative diene groups, substituted or unsubstituted C 6 -C 10 Aryl group, substituted or unsubstituted C 3 -C 10 alicyclic hydrocarbyl groups, which, if substituted, include halogen; The electrolyte further comprises a compound represented by formula II-A: 【number】 Here, R 21 , R 22 each independently represents a substituted or unsubstituted C 1 -C 5 Alkyl group, substituted or unsubstituted C 2 -C 5 Alkenyl group, substituted or unsubstituted C 2 -C 5 alkynyl groups, and when substituted, the substituents include halogen; R 21 and R 22 may be linked to form a cyclic structure, The mass percentage of the compound represented by formula IA is 0.01% to 10%, and the mass percentage of the compound represented by formula II-A is 0.5% to 2.0%, based on the mass of the electrolyte solution. [0010]

2. The compound represented by formula IA includes at least one of the compounds represented by formulas (I-1) to (I-30). The electrolyte solution according to claim 1. 【Chemistry 3】 【Chemistry 4】

3. The electrolyte solution further contains at least one of a compound represented by formula III-A, a compound represented by formula IV-A, a compound represented by formula VA, a compound represented by formula V-B, and a polynitrile compound; 【number】 Here, A 31 , A 32 , A 33 , A 34 are each independently one selected from the group consisting of halogen, formula III-X, formula III-Y, and formula III-Z, and when formula III-Y is selected, A is 31 , A 32 , A 33 , A 34 wherein two or four are selected from formula III-Y; 【number】 Here, R 31 , R 33 each independently represents a substituted or unsubstituted C 1 -C 6 Alkyl group, substituted or unsubstituted C 2 -C 6 alkenyl groups, R 32 each independently represents a substituted or unsubstituted C 1 -C 6 Alkylene group, substituted or unsubstituted C 2 -C 6 alkenylene groups, which, when substituted, include halogen; Number 1 represents the bonding site of two adjacent atoms, In formula III-Y, the O atom is bonded to the B atom in formula III-A, and k is 0 or 1; 【number】 Where: The number 2 represents a single bond or a double bond, and x and y each independently represent 0 or 1. When one of the numbers 2 in formula IV-A represents a single bond, one of x and y is 1 and the other is 0; In the formula IV-A, when both of the numbers 2 represent single bonds, x and y are both 1; In formula IV-A, when both of the numbers 2 represent a double bond, x and y are both 0; A 42 , A 43 , A 45 , A 46 each independently represents a halogen atom, a substituted or unsubstituted C 1 -C 6 In the case where formula IV-C is selected, A is selected from the group consisting of an alkyl group, formula IV-B, formula IV-C, and formula IV-D, so as to form a cyclic structure. 42 , A 43 , A 45 , A 46 Two or four of A are selected from formula IV-C; 41 , A 44 each independently represents oxygen, halogen, substituted or unsubstituted C 1 -C 6 In the case where formula IV-C is selected, A is selected from the group consisting of an alkyl group, formula IV-B, formula IV-C, and formula IV-D, so as to form a cyclic structure. 41 , A 44 are each selected from formula IV-C, where, if substituted, the substituents include halogen; A 41 , A 42 , A 43 , A 44 , A 45 , A 46 is not all fluorine, 【number】 In formula IV-B, formula IV-C, and formula IV-D, R 41 , R 43 each independently represents a substituted or unsubstituted C 1 -C 6 Alkyl group, substituted or unsubstituted C 2 -C 6 alkenyl groups, R 42 is a substituted or unsubstituted C 1 -C 6 Alkylene group, substituted or unsubstituted C 2 -C 6 alkenylene groups, wherein, when substituted, the substituents include halogen; In formula IV-C, The O atom is bonded to the P atom in formula IV-A, z represents 0 or 1, 【number】 Here, R 51 , R 52 , R 53 , R 54 each independently represents a substituted or unsubstituted C 1 -C 5 Alkyl group, substituted or unsubstituted C 2 -C 10 Alkenyl group, substituted or unsubstituted C 2 -C 10 Alkynyl group, substituted or unsubstituted C 3 -C 10 an alicyclic group represented by the formula: 6 -C 10 Aryl group, substituted or unsubstituted C 1 -C 6 Aliphatic heterocyclic group, substituted or unsubstituted C 1 -C 6 Aromatic heterocyclic groups, substituted or unsubstituted C 1 -C 6 Heteroatom-containing functional groups, when substituted, include halogens, R 51 , R 52 may be bonded to form a cyclic structure, R 53 , R 54 may be bonded to form a ring structure, and the heteroatom in the heteroatom-containing functional group includes at least one of B, N, O, Si, P, and S. The electrolyte solution according to claim 1 . [0010] [0025]

4. An electrolyte that satisfies at least one of the following conditions: b) the mass percentage of the compound represented by formula III-A is 0.1% to 5% based on the mass of the electrolyte; c) the mass percentage of the compound represented by formula IV-A relative to the mass of the electrolyte is 0.1% to 5%; d) the total mass percentage of the compound represented by formula VA and the compound represented by formula VB is 0.01% to 10% relative to the mass of the electrolyte; and e) The electrolyte according to claim 3, wherein the mass percentage of the polynitrile compound is 0.1% to 10% based on the mass of the electrolyte.

5. The compound represented by formula II-A includes at least one of the compounds represented by formulas (II-1) to (II-22). The electrolyte solution according to claim 1. 【Chemistry 11】

6. 4. The electrolyte of claim 3, wherein the compound represented by formula III-A comprises at least one of lithium tetrafluoroborate, lithium bis(oxalato)borate, and lithium difluoro(oxalato)borate.

7. The electrolyte solution according to claim 3, wherein the compound represented by formula IV-A includes at least one of lithium difluorophosphate, lithium difluorobis(oxalato)phosphate, and lithium tetrafluoro(oxalato)phosphate.

8. The compound represented by formula VA includes at least one of the compounds represented by formulas (V-1) to (V-16), 【Chemistry 12】 The compound represented by formula V-B includes at least one of the compounds represented by formulas (V-17) to (V-20). The electrolyte solution according to claim 3. 【Chemistry 13】

9. The electrolyte according to claim 3, wherein the polynitrile compound comprises at least one of 1,2,3-tris(2-cyanoethoxy)propane, 1,3,6-hexanetricarbonitrile, 1,2-bis(2-cyanoethoxy)ethane, and adiponitrile.

10. An electrochemical device comprising a positive electrode sheet, a negative electrode sheet, a separator, and the electrolyte solution according to any one of claims 1 to 9.

11. An electronic device comprising the electrochemical device of claim 10.

Citation Information

Patent Citations

  • Electrolytic solution and lithium-ion battery employing same

    CN105958120A

  • Electrolyte, electrochemical device comprising the electrolyte and electronic device

    CN111628219A

  • Electrolyte, and electrochemical device and electronic device including same

    CN111740165A

  • High voltage lithium ion battery electrolyte and high voltage lithium ion battery

    JP2016536776A

  • Silicon-based energy storage devices with phosphorus containing electrolyte additives

    US20200144672A1