Secondary battery, battery module, battery pack and electric device

A core-shell structured lithium manganese phosphate positive electrode active material with dual coating layers and a specific non-aqueous electrolyte enhances lithium ion transport and reduces manganese ion elution, addressing low rate and cycle performance issues in lithium-ion batteries, resulting in improved battery performance.

JP7587708B2Active Publication Date: 2024-11-20CONTEMPORARY AMPEREX TECHNOLOGY (HONG KONG) LIMITED
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023547874
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-04-01
Publication Date
2024-11-20
Estimated Expiration
2042-04-01

AI Technical Summary

Technical Problem

Lithium manganese phosphate cathode active materials exhibit low rate performance and cycle performance, necessitating improvements in energy density, cycle stability, and safety.

Method used

A core-shell structured lithium manganese phosphate positive electrode active material is developed, incorporating a core of Li1+xMn1-yA yP1-zRzO4 with a dual coating layer of pyrophosphate and phosphate, along with a carbon-containing layer, and a non-aqueous electrolyte containing specific lithium salts and additives to enhance lithium ion transport and reduce manganese ion elution.

Benefits of technology

The solution significantly improves the rate performance, cycle performance, and high-temperature stability of lithium-ion batteries by reducing manganese ion elution and enhancing lithium ion conductivity, thereby improving the overall battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587708000034
    Figure 0007587708000034
  • Figure 0007587708000035
    Figure 0007587708000035
  • Figure 0007587708000036
    Figure 0007587708000036
Patent Text Reader

Abstract

The present application provides a secondary battery, a battery module, a battery pack, and an electric device. The secondary battery includes a positive electrode sheet and a non-aqueous electrolyte solution, and the positive electrode active material includes a core and a shell that covers the core. The core is Li 1+x Mn 1-y A y P 1-z R z O4, the shell comprises a first coating layer coating the core and a second coating layer coating the first coating layer, the first coating layer comprises pyrophosphate MP2O7 and phosphate XPO4, the second coating layer comprises carbon, the non-aqueous electrolyte comprises a first lithium salt and a first additive, the first lithium salt is LiN(C m F 2m+1 SO2)(C n F 2n+1 The first additive is one or more selected from the group consisting of Li(FSO2), Li(FSO2)2N, where m and n are positive integers, and the first additive comprises one or more of the compounds shown in Formula 1. The rate performance, cycle performance and high temperature stability of the manganese phosphate lithium secondary battery are improved. JPEG2024514739000035.jpg9170
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to the technical field of lithium batteries, and in particular to secondary batteries, battery modules, battery packs and electric devices. [Background technology]

[0002] In recent years, as the application scope of lithium ion batteries becomes wider and wider, lithium ion batteries are widely used in energy storage power systems such as hydroelectric, thermal, wind and solar power stations, as well as in multiple fields such as electric tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, etc. As lithium ion batteries have developed significantly, they also put forward higher requirements for their energy density, cycle performance and safety performance. Summary of the Invention [Problem to be solved by the invention]

[0003] Compared with other positive electrode active materials, lithium manganese phosphate positive electrode active material has high safety and cycle life, but a drawback of lithium manganese phosphate is its low rate performance, which is currently generally solved by means of coating, doping, etc. However, there is still a need to further improve the rate performance, cycle performance, high temperature stability, etc. of lithium manganese phosphate positive electrode active material. [Means for solving the problem]

[0004] The present application has been made in view of the above-mentioned problems, and its purpose is to provide a secondary battery, a battery module, a battery pack, and an electric device, thereby solving the problem of low rate performance and low cycle performance of lithium manganese phosphate secondary batteries.

[0005] In order to achieve the above object, a first aspect of the present application provides a secondary battery, comprising a positive electrode sheet and a non-aqueous electrolyte solution, wherein the positive electrode active material comprises a core and a shell covering the core, and the core is Li 1+x Mn 1-y A yP 1-z R z O 4 wherein x=-0.100 to 0.100, y=0.001 to 0.500, z=0.001 to 0.100, A is one or more selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge, and preferably one or more selected from the group consisting of Fe, Ti, V, Ni, Co, and Mg, R is one or more selected from the group consisting of B, Si, N, and S, the shell comprises a first coating layer coating the core and a second coating layer coating the first coating layer, and wherein the first coating layer is pyrophosphate MP 2 O 7 and phosphate XPO 4 wherein M and X are each independently one or more selected from the group consisting of Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, and Al; and the second coating layer comprises carbon; The non-aqueous electrolyte includes a first lithium salt and a first additive, and the first lithium salt is LiN(C m F 2m+1 SO 2 )(C n F 2n+1 SO 2 ), Li(FSO 2 ) 2 N, where m and n are positive integers; The first additive comprises one or more of the compounds shown in formula 1, [ka] R 1 is one or more R a represents any one of a C2-C10 alkylene group, a C2-C10 heteroalkylene group, a C6-C18 arylene group, a C2-C18 heteroarylene group, a C3-C18 divalent alicyclic group, and a C3-C18 heterodivalent alicyclic group, each of which may be substituted or unsubstituted by R a are halogen atoms, -CN, -NCO, -OH, -COOH, -SOOH, -COOR b, a C2-C10 alkyl group, a C2-C10 alkenyl group, a C2-C10 alkynyl group, and a C2-C10 oxaalkyl group; R b is any one selected from C1-C10 alkyl groups.

[0006] Unless otherwise stated, in the above chemical formula, when A is two or more elements, the above-mentioned limit on the numerical range of y is not only a limit on the stoichiometric number of each A element, but also a limit on the sum of the stoichiometric numbers of each A element. For example, when A is two or more elements A1, A2...An, the stoichiometric numbers y1, y2...yn of A1, A2...An must all be within the numerical range limited for y in this application, and the sum of y1, y2...yn must also be within the numerical range. Similarly, when R is two or more elements, the limit on the numerical range of the stoichiometric number of R in this application also has the above-mentioned meaning.

[0007] The lithium manganese phosphate positive electrode active material of the present invention has a core-shell structure with two coating layers, of which the core is Li 1+x Mn 1-y A y P 1-z R z O 4 The element A doped into the manganese site of the core lithium manganese phosphate is useful for reducing the lattice change rate of the lithium manganese phosphate in the process of lithium desorption, improving the structural stability of the lithium manganese phosphate positive electrode material, greatly reducing the dissolution of manganese, and reducing the oxygen activity on the particle surface. The element R doped into the phosphorus site is useful for changing the difficulty of the change in the distance of the Mn-O bond, thereby lowering the lithium ion transition barrier, promoting the lithium ion transition, and improving the rate performance of the secondary battery.

[0008] The first coating layer of the positive electrode active material of the present application includes pyrophosphate and phosphate. The transition barrier in the pyrophosphate of the transition metal is high (>1 eV), so that the elution of the transition metal can be effectively suppressed. The phosphate has excellent lithium ion conductivity and can reduce the lithium ion content on the surface. In addition, since the second coating layer is a carbon-containing layer, LiMnPO 4 The second coating layer can effectively improve the conductive performance and desolvation ability of the active material. In addition, the "barrier" effect of the second coating layer can further inhibit the transfer of manganese ions to the electrolyte and reduce the corrosion of the electrolyte to the active material.

[0009] Therefore, the present invention provides lithium manganese phosphate by doping with specific elements and coating the surface thereof, thereby effectively inhibiting the dissolution of manganese ions during the process of lithium desorption, and at the same time promoting the transition of lithium ions, thereby improving the rate performance of the cell and enhancing the cycle performance and high temperature performance of the secondary battery.

[0010] As shown in FIG. 1, in the present application, LiMnPO 4 As can be seen from the comparison of the XRD spectra before and after doping, the positive electrode active material of the present invention is LiMnPO 4 The position of the main characteristic peak is basically consistent with that before doping, explaining that there is no heterogeneous phase in the doped lithium manganese phosphate positive electrode active material, and the improvement of secondary battery performance is mainly due to element doping, not due to heterogeneous phase. 4 By simultaneously doping the Mn site and the P site of the positive electrode active material with a specific element in a specific amount and coating the surface of the compound with two layers, the positive electrode active material can be obtained, which greatly reduces the elution of transition metals and reduces the oxygen activity on the particle surface, promotes the transition of lithium ions, improves the conductive performance and desolvation performance of the material, improves the rate performance of the battery, and improves the cycle performance and high temperature performance of the secondary battery, while at the same time reducing the corrosion of the electrolyte against the active material.

[0011] At the same time, the non-aqueous electrolyte uses the first lithium salt as the main lithium salt, and due to its excellent thermal stability and hydrolysis resistance, it can effectively reduce the acidity of the electrolyte, reduce the elution of manganese ions, and improve the high-temperature cycle and storage performance. The isocyanate group compound shown in formula 1 is introduced into the non-aqueous electrolyte, which can react with traces of water in the battery to generate -NHCOOH, preventing the action of traces of water and the non-aqueous electrolyte to generate HF, further reducing the acidity of the electrolyte, reducing the elution of manganese ions, and further improving the high-temperature cycle and storage performance. In addition, the isocyanate group compound shown in formula 1 can also be formed on the negative electrode to form a uniform SEI film, which can reduce the reduction of the eluted Mn at the negative electrode, and further improving the high-temperature cycle and storage performance.

[0012] In some embodiments, the R 1 is one or more R a represents any one of a C2-C10 alkylene group, a C2-C10 oxyalkylene group, a C2-C10 azaalkylene group, a phenylene group, a naphthylene group, an anthrylene group, a cyclobutylene group, a cyclopentylene group, a cyclohexylene group, a biphenylene group, and a methylenediphenylene group, which may or may not be substituted by R 1 is one or more R a represents any one of a C2-C6 alkylene group, a phenylene group, a naphthylene group, an anthrylene group, a cyclobutylene group, a cyclopentylene group, a cyclohexylene group, a biphenylene group, and a methylenediphenylene group, which may be substituted or not substituted by R a contains one or more selected from a halogen atom, -CN, and a C2-C3 alkyl group, and / or R a The number of is 0, 1, 2, 3 or 4.

[0013] Preferably, the first additive comprises one or more of the following compounds: [ka] [ka]

[0014] In the first lithium salt, LiN(C m F 2m+1 SO 2 )(C n F 2n+1 SO 2 ) can be selected from any corresponding specific materials in the prior art, and in some embodiments, m, n each independently represent 0, 1, 2, 3 or 4, thereby providing excellent thermal stability.

[0015] In some embodiments of the present application, the first lithium salt is LiN(CF 3 SO 2 )(FSO 2 ), Li(CF 3 SO 2 ) 2 N, LiN(C 4 F 9 SO 2 )(FSO 2 ), the first additive is any one selected from the following compounds: [ka]

[0016] At this time, the advantages of both are fully exerted, and the acidity of the electrolyte and the elution of manganese ions are significantly reduced, so that the high-temperature cycle and storage performance of the lithium ion battery are significantly improved.

[0017] In some embodiments, based on the total weight of the non-aqueous electrolyte, the content of the first lithium salt is W1 wt%, where W1 is 0.1-48 (e.g., 0.1, 0.5, 1, 2, 3, 4, 5, 7, 10, 12, 14, 15, 16, 18, 20, 22, 25, 28, 30, 40, 45, or 48), preferably 5-20, to mitigate the corrosion problem of the aluminum foil caused by the first lithium salt at high operating voltages.

[0018] In some embodiments, the content of the first additive is W2 wt%, W2 is 0.01-20 (for example, 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 1, 2, 3, 4, 5, 8, 10, 12, 15, 18 or 20), preferably 0.1-10 or 0.3-5. When the mass ratio of the first additive in the electrolyte is within the above range, it not only reduces the acidity of the electrolyte and reduces the elution of manganese ions, but also avoids the deterioration of the negative electrode impedance, and further improves the high-temperature cycle and storage performance of the lithium ion battery, while not affecting the capacity and rate performance of the lithium ion battery.

[0019] In some embodiments, the above W2 / W1 is defined as M, and M is 0.001-3 (for example, 0.001, 0.002, 0.005, 0.007, 0.1, 0.2, 0.3, 0.4, 0.5, 1, 2 or 3), preferably 0.005-0.5. When W2 / W1 is in the above range, the two can exert a better synergistic effect, ensuring that the acidity of the system is low, the elution of manganese ions is reduced, and the lithium ion high temperature cycle and storage performance is excellent.

[0020] In order to control the content of the first lithium salt, the elution of manganese ions can be supplemented with the lithium salt in the non-aqueous electrolyte by adding a second lithium salt in some embodiments, that is, the non-aqueous electrolyte further includes a second lithium salt, and the second lithium salt is lithium difluorophosphate, lithium difluorodioxalate phosphate, lithium difluorooxalate borate, lithium bisoxalate borate, LiPF 6 , LiBF 4 The second lithium salt is added to the non-aqueous electrolyte as a lithium salt type additive, which is preferentially decomposed on the surface of the aluminum foil, and the decomposition product combines with the aluminum ion to produce an insoluble or poorly soluble precipitate that adheres to the surface of the aluminum foil, thereby forming a layer of passivation film, preventing direct contact between the aluminum foil and the electrolyte, protecting the aluminum foil, and further improving high-temperature cycle and storage performance in cooperation with the first lithium salt.

[0021] In some embodiments, based on the total weight of the non-aqueous electrolyte, the content of the second lithium salt is W3% by weight, W3 is 0.01-20, preferably 0.1-5 or 0.3-5. When the mass ratio of the second lithium salt in the electrolyte is within the above range, it can inhibit the corrosion of the aluminum foil, improve the high-temperature cycle and storage performance of the lithium ion battery, and do not deteriorate the capacity and rate performance of the lithium ion battery.

[0022] In some embodiments, (W2+W3) / W1 is defined as N, and N is 0.01-5 (for example, 0.01, 0.02, 0.05, 0.08, 0.1, 0.5, 0.8, 1.0, 2, 3, 4 or 5), preferably 0.02-1. When W2 / W1 and (W2+W3) / W1 are in the above range, the three can exert better synergistic effect, ensure low acidity of the system, reduce manganese ion leaching, and excellent lithium ion high temperature cycle and storage performance, while effectively inhibiting the corrosion of aluminum foil, improving the high temperature cycle and storage performance of lithium ion battery, and at the same time not deteriorating the capacity and rate performance of lithium ion battery.

[0023] In some embodiments, the non-aqueous electrolyte further comprises a second additive, the second additive comprises one or more of the following: cyclic carbonate compounds containing unsaturated bonds, halogen-substituted saturated cyclic carbonate compounds, sulfate compounds, sulfite compounds, sultone compounds, disulfonic acid compounds, nitrile compounds, aromatic compounds, isocyanate compounds, phosphazene compounds, cyclic acid anhydride compounds, phosphite compounds, phosphate compounds, and borate compounds. Those skilled in the art can select the corresponding second additive from the above materials according to actual needs, and the amount of the second additive used in the non-aqueous electrolyte can also be referred to the prior art, and the present application will not be described.

[0024] In some embodiments, the non-aqueous electrolyte further comprises an organic solvent, the type of which is not particularly limited and can be selected according to actual needs. Specifically, the organic solvent comprises one or more of a cyclic carbonate compound, a chain carbonate compound, and a carboxylic acid ester compound. Preferably, the organic solvent comprises one or more of the group consisting of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, γ-butyrolactone, methyl formate, ethyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, butyl propionate, and tetrahydrofuran.

[0025] In some embodiments, the coating amount of the first coating layer is C1% by weight, C1 being greater than 0 and less than or equal to 7, preferably 4-5.6, calculated based on the weight of the core, and / or the coating amount of the second coating layer is C2% by weight, C2 being greater than 0 and less than or equal to 6, preferably 3-5, calculated based on the weight of the core. When the coating amount of the first coating layer is within the above range, it is possible to further inhibit the elution of manganese ions and at the same time further promote the transport of lithium ions. In addition, the following situation can be effectively avoided. If the coating amount of the first coating layer is too small, it may cause the suppression effect of pyrophosphate against the elution of manganese ions to be insufficient, and at the same time, the improvement of the lithium ion transport performance is not significant. If the coating amount of the first coating layer is too large, it may cause the coating layer to be too thick, which may increase the battery impedance and affect the dynamic performance of the battery.

[0026] In some embodiments, the ratio of (W1+W2) / (C1+C2) is defined as Q, and Q is 0.1-10, preferably 0.5-5. When C is smaller than the above range, there is not enough lithium salt and additive to reduce the acidity of the electrolyte, and the inhibition effect on the dissolution of manganese ions is limited, and the high temperature cycle and storage performance cannot be significantly improved. When C is larger than the above range, the impedance due to the film formation is too large, which affects the battery capacity and rate performance of lithium ion, and makes it difficult to effectively improve them.

[0027] In some embodiments, in the positive electrode active material, the weight ratio of pyrophosphate to phosphate in the first coating layer is 1:3-3:1, preferably 1:3-1:1. The appropriate mixing ratio of pyrophosphate to phosphate can fully exert the synergistic effect of the two, and can effectively avoid the following situation: too much pyrophosphate and too little phosphate may cause an increase in battery impedance, and too much phosphate and too little pyrophosphate will not have a significant effect of suppressing the elution of manganese ions.

[0028] In any embodiment, the crystal plane spacing of the phosphate in the first coating layer is 0.345-0.358 nm, the included angle of the crystal direction (111) is 24.25 °-26.45 °, and the crystal plane spacing of the pyrophosphate in the first coating layer is 0.293-0.326 nm, the included angle of the crystal direction (111) is 26.41 °-32.57 °. When the crystal plane spacing and the included angle of the crystal direction (111) of the phosphate and pyrophosphate in the first coating layer are in the above range, the heterogeneous phase in the coating layer can be more effectively avoided, thereby further improving the theoretical capacity of the material, and further improving the cycle performance and rate performance of the secondary battery.

[0029] In any of the first to third embodiments, y is an arbitrary value selected from the range of 0.1 to 0.4. By selecting the value of y within this range, the theoretical capacity and rate performance of the first positive electrode active material can be further improved.

[0030] In any of the first to third aspects, M and X are independently one or more elements selected from Li and Fe.

[0031] In any embodiment, the ratio of y to 1-y is selected from 1:10-10:1, preferably 1:4-1:1, where y represents the sum of the stoichiometric numbers of Mn site doping elements. When the above conditions are met, the energy density and cycle performance of the secondary battery manufactured with the positive electrode sheet can be further improved.

[0032] In any embodiment, the ratio of z to 1-z is selected from 1:999-1:9, preferably 1:499-1:249, where z represents the sum of the stoichiometric numbers of the P-site doping elements. When the above condition is met, the energy density and cycle performance of the secondary battery manufactured by the positive electrode sheet can be further improved.

[0033] In any embodiment, in the first positive electrode active material, the crystallinity of the pyrophosphate and the phosphate is independently 10% to 100%, preferably 50% to 100%. In the first coating layer of the lithium manganese phosphate positive electrode active material of the embodiment, the pyrophosphate and the phosphate having a certain crystallinity maintain the stability of the structure of the first coating layer and help reduce lattice defects. On the one hand, this helps the pyrophosphate to fully exert the effect of inhibiting the dissolution of manganese ions, and on the other hand, the phosphate helps to reduce the content of surface lithium and the valence of surface oxygen, thereby reducing the interfacial side reaction between the positive electrode material and the electrolyte, reducing the consumption of the electrolyte, and improving the cycle performance and safety performance of the secondary battery.

[0034] In any embodiment, A is at least two elements selected from Fe, Ti, V, Ni, Co and Mg. Selecting doping elements within the above ranges helps to strengthen the doping effect, on the one hand, further reduce the lattice change rate, thereby inhibiting the dissolution of manganese and reducing the consumption of electrolyte and active lithium, and on the other hand, further reduce the surface oxygen activity, which helps to reduce the interface side reaction between the positive electrode active material and the electrolyte, thereby improving the cycle performance and high-temperature storage performance of the battery.

[0035] In any embodiment, the first positive electrode active material has a Li / Mn antisite defect concentration of 4% or less, preferably 2% or less. In the positive electrode active material of the present application, the Li / Mn antisite defect is LiMnPO 4 In the crystal lattice, Li + and Mn 2+ Li + The transport channel is one-dimensional, and Mn 2+ Li + Mn is difficult to transition in the transport channel and therefore the antisite defect 2+ Li + By controlling the Li / Mn antisite defect concentration to a low level, LiMnPO 4 The theoretical capacity and rate performance of the semiconductor device can be improved.

[0036] In any embodiment, the lattice change rate of the positive electrode active material is 6% or less, preferably 4% or less. LiMnPO 4 The lithium desorption process is a two-phase reaction. The interfacial stress between the two phases is determined by the magnitude of the lattice change rate. The smaller the lattice change rate, the smaller the interfacial stress, and the smaller the Li + Therefore, reducing the lattice change rate of the core is + This helps to improve the transport ability of the secondary battery, thereby improving the rate performance.

[0037] In any embodiment, the surface oxygen valence of the first positive electrode active material is -1.88 or less, preferably -1.98 to -1.88. This is because the higher the valence of the oxygen compound, the stronger its electron acquisition ability, i.e., stronger oxidizing property. In the first positive electrode active material of the present application, by controlling the surface valence of oxygen to a low level, the reaction activity of the positive electrode material surface can be reduced, and the interface side reaction between the positive electrode material and the electrolyte solution can be further reduced, thereby further improving the cycle performance and high-temperature storage performance of the secondary battery.

[0038] In any embodiment, the positive electrode active material has a compaction density at 3 tons (T) of 2.0 g / cm 3 or more, preferably 2.2 g / cm 3 The higher the compaction degree of the first positive electrode active material, that is, the greater the weight of the active material per unit volume, the more effective it is for improving the volumetric energy density of the secondary battery.

[0039] A second aspect of the present application further provides a battery module, the battery module including a secondary battery, the secondary battery being any one of the above-mentioned secondary batteries of the present application.

[0040] A third aspect of the present application further provides a battery pack, the battery pack including a battery module, the battery module being the above-mentioned battery module of the present application.

[0041] A fourth aspect of the present application further provides an electric device, the electric device including at least one of a secondary battery, a battery module, or a battery pack, the secondary battery, the battery module, and the battery pack all being the secondary battery, the battery module, and the battery pack provided by the present application.

[0042] As a result, the battery module and battery pack of the present application have high cycle performance and rate characteristics, and in particular, the high temperature stability is also significantly improved, and further provides an electric device having the secondary battery, battery module, or battery pack of the present application with high power cycle stability and high temperature operation stability. [Brief description of the drawings]

[0043] [Figure 1] FIG. 1 is an XRD spectrum of a positive electrode active material according to an embodiment of the present application. [Diagram 2] FIG. 2 is a schematic diagram of a secondary battery according to an embodiment of the present application. [Diagram 3] FIG. 3 is an exploded view of the secondary battery according to an embodiment of the present application shown in FIG. [Figure 4] FIG. 4 is a schematic diagram of a battery module according to an embodiment of the present invention. [Diagram 5] FIG. 5 is a schematic diagram of a battery pack according to an embodiment of the present invention. [Figure 6] FIG. 6 is an exploded view of the battery pack according to an embodiment of the present application shown in FIG. [Figure 7] FIG. 7 is a schematic diagram of an electrical device in which a secondary battery according to an embodiment of the present application is used as a power source. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0044] Hereinafter, with reference to the drawings as appropriate, embodiments specifically disclosing the secondary battery, battery module, battery pack, and electric device of the present application will be described in detail. However, unnecessary detailed description may be omitted. For example, detailed description of already well-known matters or duplicate description of the same actual configuration may be omitted. This is to avoid the following description becoming unnecessarily redundant and to facilitate understanding by those skilled in the art. Furthermore, the drawings and the following description are provided to enable those skilled in the art to fully understand the present application, and are not intended to limit the subject matter described in the claims.

[0045] The "ranges" disclosed herein are defined in the form of lower and upper limits, where a given range is defined by selecting one lower limit and one upper limit, and the selected lower and upper limits define the boundaries of the particular range. Ranges defined in this manner may or may not include the end values ​​and may be arbitrarily combined, i.e., any lower limit may be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are recited for a particular parameter, then ranges of 60-110 and 80-120 are also contemplated. Also, if the minimum range values ​​1 and 2 are recited, and the maximum range values ​​3, 4 and 5 are recited, then all of the following ranges are contemplated: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range "ab" represents an abbreviation for any combination of real numbers between a and b, where a and b are both real numbers. For example, the numerical range "0-5" represents all real numbers between "0-5" listed herein, with "0-5" being an abbreviation for these numerical combinations. Also, expressing a parameter as an integer ≧2 is equivalent to disclosing that the parameter is, for example, the integers 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0046] Unless otherwise stated, all the embodiments and optional embodiments in the present application can be combined with each other to form new technical solutions.

[0047] Unless otherwise stated, all technical features and optional technical features in the present application can be combined with each other to form new technical solutions.

[0048] Unless otherwise stated, all steps in this application may be performed in sequence or randomly, preferably in sequence. For example, the method may include steps (a) and (b), indicating that the method may include steps (a) and (b) performed in sequence, and may further include steps (b) and (a) performed in sequence. For example, the method mentioned above may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), may further include steps (a), (c) and (b), and may further include steps (c), (a) and (b).

[0049] Unless otherwise stated, the terms "comprise" and "include" referred to in this application may be open-ended or closed-ended. For example, the terms "comprise" and "include" may represent the inclusion or inclusion of other components not listed, or may represent the inclusion or inclusion of only the listed components.

[0050] In this application, unless otherwise stated, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, any of the following conditions satisfy the condition "A or B": A is true (or exists) and B is false (or does not exist), A is false (or does not exist) and B is true (or exists), or A and B are both true (or exist).

[0051] In this specification, the term "coating layer" refers to a layer of material coated on the core, which may completely or partially cover the core, and the use of "coating layer" is for ease of explanation only and is not intended to limit the present invention. Similarly, the term "thickness of the coating layer" refers to the thickness of the layer of material coated on the core in the radial direction of the core.

[0052] As used herein, the term "source" refers to a compound that provides an element, and by way of example, the types of "source" include, but are not limited to, carbonates, sulfates, nitrates, elements, halides, oxides, and hydroxides.

[0053] The inventors of the present application have found the following in their practical work: In the lithium manganese phosphate positive active material, manganese ion dissolution is serious during deep charge and discharge. In the prior art, lithium manganese phosphate was coated with lithium iron phosphate to reduce the interfacial side reaction, but such coating cannot prevent the transition of the dissolved manganese to the electrolyte. After the dissolved manganese is transferred to the negative electrode, it is reduced to metallic manganese. These generated metallic manganese correspond to a "catalyst" and can catalyze the decomposition of the SEI film (solid electrolyte interphase) on the surface of the negative electrode. Some of the generated by-products are gases, which are prone to causing battery expansion and affecting the safety performance of the secondary battery, and the other part is deposited on the surface of the negative electrode, blocking the passage of lithium ions into and out of the negative electrode, increasing the impedance of the secondary battery, and affecting the dynamic performance of the battery. In addition, in order to compensate for the lost SEI film, the electrolyte and active lithium inside the battery are constantly consumed, which has an irreversible effect on the capacity retention rate of the secondary battery.

[0054] After extensive research, the inventors found that the manganese ion dissolution is serious and the surface reaction activity is high in the lithium manganese phosphate positive electrode active material. 3+ Jahn-Teller effect and Li + It was found that this may be due to the change in the size of the channel. Therefore, the inventors have modified lithium manganese phosphate to significantly reduce the elution of manganese ions and the lattice change rate, thereby obtaining a positive electrode active material with high cycle performance, high temperature storage performance, and safety performance. [Secondary battery]

[0055] A secondary battery is also called a rechargeable battery or storage battery, and refers to a battery that can be continuously used by activating the active material through charging after the battery is discharged.

[0056] In general, a secondary battery includes a positive electrode sheet, a negative electrode sheet, a separator, and an electrolyte. During the charge and discharge process of the battery, active ions (e.g., lithium ions) are inserted and removed between the positive electrode sheet and the negative electrode sheet. The separator is placed between the positive electrode sheet and the negative electrode sheet, and mainly serves to prevent short circuits between the positive and negative electrodes, while allowing the active ions to pass through. The electrolyte is placed between the positive electrode sheet and the negative electrode sheet, and mainly serves to conduct the active ions.

[0057] An embodiment of the present application provides a secondary battery, comprising a positive electrode sheet and a non-aqueous electrolyte solution, wherein the positive electrode active material comprises a core and a shell covering the core, and the core is Li 1+x Mn 1-y A y P 1-z R z O 4 wherein x=-0.100 to 0.100, y=0.001 to 0.500, z=0.001 to 0.100, A is one or more selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge, and preferably one or more selected from the group consisting of Fe, Ti, V, Ni, Co, and Mg, R is one or more selected from the group consisting of B, Si, N, and S, the shell includes a first coating layer coating the core and a second coating layer coating the first coating layer, and the first coating layer is a pyrophosphate MP 2 O 7 and phosphate XPO 4 wherein M and X are each independently one or more selected from the group consisting of Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, and Al; the second coating layer comprises carbon; The non-aqueous electrolyte includes a first lithium salt and a first additive, and preferably, the first lithium salt is LiN(C m F 2m+1 SO 2)(C n F 2n+1 SO 2 ), Li(FSO 2 ) 2 N, wherein m and n are positive integers; The first additive comprises one or more of the compounds shown in formula 1, [ka] R 1 is one or more R a represents any one of a C2-C10 alkylene group, a C2-C10 heteroalkylene group, a C6-C18 arylene group, a C2-C18 heteroarylene group, a C3-C18 divalent alicyclic group, and a C3-C18 heterodivalent alicyclic group, each of which may be substituted or unsubstituted by R a are halogen atoms, -CN, -NCO, -OH, -COOH, -SOOH, -COOR b , a C2-C10 alkyl group, a C2-C10 alkenyl group, a C2-C10 alkynyl group, and a C2-C10 oxaalkyl group; R b is any one selected from C1-C10 alkyl groups.

[0058] The positive electrode sheet generally includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, the positive electrode film layer including a positive electrode active material.

[0059] For example, a positive electrode current collector has two opposing surfaces in the thickness direction of the positive electrode current collector, and a positive electrode film layer is disposed on either one or both of the two opposing surfaces of the positive electrode current collector.

[0060] In some embodiments, the positive electrode current collector may be a metal foil sheet or a composite current collector. For example, an aluminum foil may be used as the metal foil sheet. The composite current collector may have a base layer of a polymeric material and a metal layer formed on at least one side of the base layer of the polymeric material. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, silver alloy, etc.) on a polymeric material substrate (e.g., a substrate such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0061] The positive electrode active material of this application is the compound LiMnPO 4 where A, B, C and D are the compounds LiMnPO 4 The elements doped into the Li, Mn, P and O sites of lithium manganese phosphate are doped into the Li, Mn, P and O sites of lithium manganese phosphate. Without wishing to be limited by theory, it is currently believed that the improvement in the performance of lithium manganese phosphate is related to the reduction of the lattice change rate of lithium manganese phosphate during the lithium desorption process and the reduction of the surface activity. By reducing the lattice change rate, the lattice constant difference between the two phases at the grain boundary is reduced, the interfacial stress is reduced, and the Li +The interface transport ability of the positive electrode active material can be improved, thereby improving the rate performance of the positive electrode active material. High surface activity is likely to cause serious interface side reactions, which will aggravate gas generation, electrolyte consumption and interface destruction, thereby affecting the performance of the battery, such as cycle. In the present application, the lattice change rate is reduced by Li and Mn site doping. Mn site doping can further effectively reduce the surface activity, thereby suppressing the dissolution of manganese ions and the interface side reactions between the positive electrode active material and the electrolyte. P bit doping makes the change rate of Mn-O bond distance faster, lowers the small polaron transition barrier of the material, and thus benefits the electronic conductivity. O site doping has a good effect on reducing the interface side reactions. P site and O site doping further affects the manganese ion dissolution and kinetic performance of the antisite defects. Thus, doping can reduce the concentration of antisite defects in the material, improve the kinetic performance and theoretical capacity of the material, and further modify the particle morphology, thereby improving the compaction degree. The applicant unexpectedly found that the compound LiMnPO 4 It has been discovered that by simultaneously doping the Li site, Mn site, P site and O site of the above-mentioned lithium-ion secondary battery with specific elements in specific amounts as described herein, a significantly improved rate performance can be obtained, and at the same time, the dissolution of the doping elements at the Mn and Mn sites can be significantly reduced, significantly improved cycle performance and / or high temperature stability can be obtained, and the theoretical capacity and compaction density of the material can be improved.

[0062] At the same time, the non-aqueous electrolyte uses the first lithium salt as the main lithium salt, and due to its excellent thermal stability and hydrolysis resistance, it can effectively reduce the acidity of the electrolyte, reduce the elution of manganese ions, and improve the high-temperature cycle and storage performance. The isocyanate group compound shown in formula 1 is introduced into the non-aqueous electrolyte, which can react with a trace amount of water in the battery to generate -NHCOOH, prevent the action of a trace amount of water and the non-aqueous electrolyte to generate HF, further reduce the acidity of the electrolyte, reduce the elution of manganese ions, and further improve the high-temperature cycle and storage performance. In addition, the isocyanate group compound shown in formula 1 can also be formed on the negative electrode to form a uniform SEI film, which can reduce the reduction of the eluted Mn at the negative electrode, and further improve the high-temperature cycle and storage performance.

[0063] In some embodiments, the non-aqueous electrolyte includes a first lithium salt and a first additive, and the first lithium salt is present as a predominant lithium salt. m F 2m+1 SO 2 )(C n F 2n+1 SO 2 ) can be selected from any corresponding specific material in the art, and in some embodiments, m and n each independently represent 1, 2, or 3, thereby providing superior thermal stability. For example, the first lithium salt is LiN(C m F 2m+1 SO 2 )(C n F 2n+1 SO 2 ), Li(FSO 2 ) 2 N, for example, it is (fluorosulfonylimide) (trifluoromethanesulfonylimide) lithium Li (FSO 2 )(CF 3 SO 2 )N, lithium bis(trifluoromethanesulfonylimide) (LiN(CF 3 SO 2 ) 2), lithium bis(pentafluoroethanesulfonylimide) (LiN(C 2 F 5 SO 2 ) 2 ), (trifluoromethanesulfonylimido)(pentafluoroethanesulfonylimido)lithium (LiN(CF 3 SO 2 )(C 2 F 5 SO 2 ), (trifluoromethanesulfonylimido)(heptafluoropropanesulfonylimido)lithium (LiN(CF 3 SO 2 )(C 3 F 7 SO 2 )), (trifluoromethanesulfonylimido)(nonafluorobutanesulfonylimido)lithium (LiN(CF 3 SO 2 )(C 4 F 9 SO 2 )), (pentafluoroethanesulfonylimido)(heptafluoropropanesulfonylimido)lithium LiN(C 2 F 5 SO 2 )(C 3 F 7 SO 2 ), Li(FSO 2 ) 2 The material is selected from the group consisting of N and the like.

[0064] The isocyanate compound shown in 1 used in the present application can be selected from isocyanate-based compounds commonly used in electrolytes in the prior art, and in some embodiments, the above R 1 is one or more R a is any one of a C2-C10 alkylene group, a C2-C10 oxyalkylene group, a C2-C10 azaalkylene group, a phenylene group, a naphthylene group, an anthrylene group, a cyclobutylene group, a cyclopentylene group, a cyclohexylene group, a biphenylene group, and a methylenediphenylene group, which may or may not be substituted by R 1 is one or more R aand / or R a contains one or more selected from a halogen atom, -CN, and a C2-C3 alkyl group, and / or R in the compound represented by formula 1 a The number of is 0, 1, 2, 3 or 4.

[0065] Preferably, the first additive comprises one or more of the following compounds: [ka] [ka]

[0066] Each of the above compounds has good dispersibility in the solvent of the non-aqueous electrolyte, and reacts sufficiently with the small amount of water in the battery to form -NHCOOH can generate , it can prevent the generation of HF due to the action of a small amount of water and a non-aqueous electrolyte, and further reduce the acidity of the electrolyte, reduce the elution of manganese ions, and further improve high-temperature cycle and storage performance. In addition, each of the above isocyanate group compounds is easy to form a uniform SEI film at the negative electrode, which helps to reduce the reduction of eluted Mn at the negative electrode and further improve high-temperature cycle and storage performance.

[0067] In some embodiments of the present application, the first lithium salt is LiN(CF 3 SO 2 )(FSO 2 ), Li(CF 3 SO 2 ) 2 N, LiN(C 4 F 9 SO 2 )(FSO 2 ), the first additive is any one selected from the following compounds: [ka]

[0068] At this time, the advantages of both are fully exerted, and the acidity of the electrolyte and the elution of manganese ions are significantly reduced, so that the high-temperature cycle and storage performance of the lithium ion battery are significantly improved.

[0069] The first lithium salt can effectively improve the high-temperature cycle and storage performance of secondary batteries when used as the main lithium salt in non-aqueous electrolytes. However, under certain conditions, the material may corrode the lithium salt, for example, aluminum foil may corrode when the working voltage of a lithium-ion battery is >4.2V. The possible mechanism is that the original oxide film on the surface of the aluminum foil is destroyed in the electrolyte, exposing the more active aluminum, which is then oxidized to form Al. 3+ Generate ions and then FSI in the electrolyte - or TFSI - and Al 3+ Combined with soluble Al(FSI) 3 or Al(TFSI) 3 Forming Al(FSI) 3 or Al(TFSI) 3 The problem is that the first lithium salt dissolves and then causes corrosion of aluminum. Therefore, in order to alleviate the problem of corrosion of aluminum foil caused by the first lithium salt at high operating voltages, in some embodiments, based on the total weight of the non-aqueous electrolyte, the content of the first lithium salt is W1 wt%, where W1 is 0.1-48, preferably 5-20.

[0070] Based on controlling the content of the first lithium salt, in some embodiments, the lithium salt in the non-aqueous electrolyte can be supplemented by adding a second lithium salt, that is, the non-aqueous electrolyte further comprises a second lithium salt, and the second lithium salt is lithium difluorophosphate, lithium difluorodioxalate phosphate, lithium difluorooxalate borate, lithium bisoxalate borate, LiPF 6 , LiBF 4, LiAsF 6 The second lithium salt is added to the non-aqueous electrolyte as a lithium salt type additive, which is preferentially decomposed on the surface of the aluminum foil, and the decomposition product combines with the aluminum ion to produce an insoluble or poorly soluble precipitate that adheres to the surface of the aluminum foil, thereby forming a layer of passivation film, preventing direct contact between the aluminum foil and the electrolyte, protecting the aluminum foil, and further improving high-temperature cycle and storage performance in cooperation with the first lithium salt.

[0071] However, too much lithium salt type additive will also increase the impedance of positive and negative electrodes, resulting in abnormal lithium ion battery capacity and poor rate performance. In some embodiments, based on the total weight of the non-aqueous electrolyte, the content of the second lithium salt is W3% by weight, W3 is 0.01-20, preferably 0.1-10 or 0.3-5. When the mass ratio of the second lithium salt in the electrolyte is within the above range, it can inhibit the corrosion of aluminum foil, improve the high-temperature cycle and storage performance of the lithium ion battery, and not deteriorate the capacity and rate performance of the lithium ion battery.

[0072] The first additive can form a uniform SEI film on the negative electrode, reduce the reduction of dissolved Mn on the negative electrode, and improve high-temperature cycle and storage performance. However, too much isocyanate group compound also increases the negative electrode impedance, the lithium ion battery capacity is abnormal, and the rate performance is poor. Preferably, the content of the first additive is W2 wt%, W2 is 0.01-20, preferably 0.1-10 or 0.3-5, and when the mass ratio of the first additive in the electrolyte is within the above range, it not only reduces the acidity of the electrolyte and reduces the dissolution of manganese ions, but also avoids the deterioration of the negative electrode impedance, and improves the high-temperature cycle and storage performance of the lithium ion battery, and at the same time does not affect the performance of the lithium ion battery capacity and rate performance.

[0073] In some embodiments, W2 / W1 is defined as M, where M is 0.001-3, preferably 0.005-0.5. (W2+W3) / W1 is defined as N, where N is 0.01-2, preferably 0.02-1.

[0074] When W2 / W1 and (W2+W3) / W1 are within the above ranges, the three can exert better synergistic effects, the acidity of the system is low, the elution of manganese ions is reduced, and the high-temperature cycle and storage performance of lithium ion is excellent. At the same time, the corrosion of aluminum foil is effectively inhibited, and the high-temperature cycle and storage performance of lithium ion battery is improved, without impairing the capacity performance and rate performance of lithium ion battery.

[0075] In some embodiments, the non-aqueous electrolyte further comprises a second additive, the second additive comprising one or more of the following: cyclic carbonate compounds containing unsaturated bonds, halogen-substituted saturated cyclic carbonate compounds, sulfate compounds, sulfite compounds, sultone compounds, disulfonic acid compounds, nitrile compounds, aromatic compounds, phosphazene compounds, cyclic acid anhydride compounds, phosphite compounds, phosphate compounds, and borate compounds. Those skilled in the art can select the corresponding second additive from the above materials according to actual needs, and the amount of the second additive used in the non-aqueous electrolyte can also be referred to the prior art, and the present application will not be described.

[0076] In some embodiments, the non-aqueous electrolyte further comprises an organic solvent, the type of which is not particularly limited and can be selected according to actual needs. Specifically, the organic solvent comprises one or more of a cyclic carbonate compound, a chain carbonate compound, and a carboxylic acid ester compound. Preferably, the organic solvent comprises one or more of the group consisting of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, γ-butyrolactone, methyl formate, ethyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, butyl propionate, and tetrahydrofuran.

[0077] In some embodiments, A, C, and D of the positive electrode active material are each independently any one of the elements within the respective ranges above, and B is at least two elements, which allows the composition of the positive electrode active material to be more easily and accurately controlled.

[0078] In some embodiments, the coating amount of the first coating layer is C1% by weight, calculated based on the weight of the core, where C1 is greater than 0 and less than or equal to 7, and preferably 4 to 5.6. When the coating amount of the first coating layer is within the above range, it can further inhibit the elution of manganese ions and at the same time further promote the transport of lithium ions. In addition, it can effectively avoid the following situation: If the coating amount of the first coating layer is too small, it may cause the pyrophosphate to have an insufficient inhibitory effect on the elution of manganese ions, and at the same time, the improvement in the lithium ion transport performance is not significant; if the coating amount of the first coating layer is too large, it may cause the coating layer to be too thick, which may increase the battery impedance and affect the dynamic performance of the battery.

[0079] In some embodiments, the coating amount of the second coating layer is C2% by weight, calculated based on the weight of the core, where C2 is greater than 0 and less than or equal to 6, preferably 3 to 5. The carbon-containing layer as the second coating layer can exert a "barrier" function on the one hand, avoiding direct contact between the positive electrode active material and the electrolyte, thereby reducing the corrosion of the electrolyte to the active material, and improving the safety performance of the battery at high temperatures. On the other hand, it has a strong conductive ability and can reduce the internal resistance of the battery, thereby improving the dynamic performance of the battery. However, because the theoretical capacity of the carbon material is low, if the usage amount of the second coating layer is too large, it may reduce the theoretical capacity of the entire positive electrode active material. Therefore, when the coating amount of the second coating layer is in the above range, the dynamic performance and safety performance of the battery can be further improved without sacrificing the theoretical capacity of the positive electrode active material.

[0080] In some embodiments, the ratio of (W1+W2) / (C1+C2) is defined as Q, and Q is 0.1-10 (for example, 0.1, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10), preferably 0.5-5. When C is smaller than the above range, there is not enough lithium salt and additive to reduce the acidity of the electrolyte, and the inhibition effect on the dissolution of manganese ions is limited, and the high temperature cycle and storage performance cannot be significantly improved. When C is larger than the above range, the impedance due to film formation is too large, which affects the battery capacity and rate performance of lithium ion, and is difficult to effectively improve.

[0081] In some embodiments, the weight ratio of pyrophosphate to phosphate in the first coating layer is preferably 1:3-3:1, more preferably 1:3-1:1.

[0082] The appropriate mixing ratio of pyrophosphate and phosphate can fully exert the synergistic effect of the two, and can effectively avoid the following situations: too much pyrophosphate and too little phosphate may cause an increase in battery impedance, and too much phosphate and too little pyrophosphate will not have a significant effect on inhibiting the elution of manganese ions.

[0083] In some embodiments, preferably, the crystal plane spacing of the phosphate of the first coating layer is 0.345-0.358 nm and the included angle of the (111) crystal direction is 24.25°-26.45°, and the crystal plane spacing of the pyrophosphate of the first coating layer is 0.293-0.326 nm and the included angle of the (111) crystal direction is 26.41°-32.57°.

[0084] When the crystal plane spacing and the included angle of the (111) crystal direction of the phosphate and pyrophosphate in the first coating layer are within the above ranges, the heterogeneous phase in the coating layer can be effectively avoided, thereby improving the theoretical capacity, cycle performance and rate performance of the material.

[0085] In some embodiments, the ratio of y to 1-y in the core is preferably 1:10-10:1, preferably 1:4-1:1, where y represents the sum of the stoichiometric numbers of Mn site doping elements. When the above condition is met, the energy density and cycle performance of the positive electrode active material can be further improved.

[0086] In some embodiments, the ratio of z to 1-z in the core is preferably 1:9-1:999, preferably 1:499-1:249, where y represents the sum of the stoichiometric numbers of P-site doping elements. When the above condition is met, the energy density and cycle performance of the positive electrode active material can be further improved.

[0087] In some embodiments, the crystallinity of the pyrophosphate and the phosphate is preferably each independently 10% to 100%, more preferably 50% to 100%.

[0088] In the first coating layer of the lithium manganese phosphate positive active material of the present application, the pyrophosphate and phosphate with a certain crystallinity are useful for maintaining the structural stability of the first coating layer and reducing lattice defects, which on the one hand allows the pyrophosphate to fully exert the function of inhibiting the dissolution of manganese ions, and on the other hand allows the phosphate to reduce the surface lithium content and the valence of surface oxygen, thereby reducing the interfacial side reaction between the positive electrode material and the electrolyte, reducing the consumption of the electrolyte, and improving the cycle performance and safety performance of the battery.

[0089] In the present application, the crystallinity of pyrophosphate and phosphate can be adjusted, for example, by adjusting process conditions in the sintering process, such as sintering temperature, sintering time, etc. The crystallinity of pyrophosphate and phosphate can be measured by methods known in the art, such as X-ray diffraction method, density method, infrared spectroscopy, differential scanning calorimetry, and nuclear magnetic resonance absorption method.

[0090] In some embodiments, A is preferably at least two selected from Fe, Ti, V, Ni, Co, and Mg.

[0091] Doping the manganese sites in the lithium manganese phosphate positive electrode active material with two or more of the above elements simultaneously serves to enhance the doping effect, which on the one hand further reduces the lattice change rate, thereby inhibiting the dissolution of manganese and reducing the consumption of electrolyte and active lithium, and on the other hand further reduces the surface oxygen activity, which serves to reduce the interfacial side reactions between the positive electrode active material and the electrolyte, thereby improving the cycle performance and high-temperature storage performance of the battery.

[0092] In some embodiments, the positive electrode active material preferably has a Li / Mn antisite defect concentration of 4% or less, preferably 2% or less.

[0093] In the positive electrode active material of the present invention, the Li / Mn antisite defect is LiMnPO 4 In the crystal lattice, Li +and Mn 2+ Li + The transport channel is one-dimensional, and Mn 2+ Li + Mn is difficult to transition in the transport channel and therefore the antisite defect 2+ Li + By controlling the Li / Mn antisite defect concentration to a low level, LiMnPO 4 In the present application, the antisite defect concentration can be measured based on, for example, JIS K0131-1996.

[0094] In some embodiments, the lattice change rate of the positive electrode active material is preferably 6% or less, and more preferably 4% or less.

[0095] LiMnPO 4 The lithium desorption process is a two-phase reaction. The interfacial stress between the two phases is determined by the magnitude of the lattice change rate. The smaller the lattice change rate, the smaller the interfacial stress, and the smaller the Li + Therefore, reducing the lattice change rate of the core is + This helps to improve the transport ability of the secondary battery, thereby improving the rate performance.

[0096] In some embodiments, the button cell of the positive electrode active material preferably has an average discharge voltage of 3.5 V or more and a theoretical discharge capacity of 140 mAh / g or more, and preferably has an average discharge voltage of 3.6 V or more and a theoretical discharge capacity of 145 mAh / g or more.

[0097] Undoped LiMnPO 4 Although the average discharge voltage of the lithium secondary battery is above 4.0V, its theoretical discharge capacity is low, generally less than 120mAh / g, and therefore its energy density is low. By adjusting the lattice change rate through doping, its theoretical discharge capacity can be greatly improved, and the overall energy density is obviously improved while the average discharge voltage is slightly reduced.

[0098] In some embodiments, the surface oxygen valence of the positive electrode active material is preferably −1.88 or less, and more preferably −1.98 to −1.88.

[0099] This is because the higher the valence of the oxygen compound, the stronger its electron acquisition ability, i.e., its oxidizing property. In the lithium manganese phosphate positive electrode active material of the present application, by controlling the surface valence of oxygen to a low level, the reaction activity of the positive electrode material surface is reduced, and the interfacial side reaction between the positive electrode material and the electrolyte is reduced, thereby improving the cycle performance and high-temperature storage performance of the secondary battery.

[0100] In some embodiments, the positive electrode active material preferably has a compaction density at 3 ton (T) of 2.0 g / cm 3 or more, preferably 2.2 g / cm 3 That's all.

[0101] The higher the compaction degree of the positive electrode active material, i.e., the greater the weight of the active material per unit volume, the more useful it is for improving the volumetric energy density of the battery. In this application, the compaction degree can be measured, for example, according to GB / T24533-2009.

[0102] The positive electrode active material used in the secondary battery of the present application is produced by the following production method, which includes the following steps.

[0103] Li 1+x Mn 1-y A y P 1-z R z O 4 Provide core material including MP 2 O 7 XPO containing powder and carbon source 4 Provides suspension, core material, MP 2 O 7 Powder containing a carbon source XPO 4 The mixture is added to the suspension, mixed, and sintered to obtain the positive electrode active material.

[0104] In some embodiments, the step of providing a core material includes the following steps: Step (1): Mix and stir a source of manganese, a source of element A, and an acid in a container to obtain manganese salt particles doped with element A; Step (2): Mix the manganese salt particles doped with element A, a source of lithium, a source of phosphorus, and a source of element R in a solvent to obtain a slurry, and obtain lithium manganese phosphate doped with element A and element R after sintering under the protection of an inert gas atmosphere, where the lithium manganese phosphate doped with element A and element R is Li 1+x Mn 1-y A y P 1-z R z O 4 where x=-0.100-0.100, y=0.001-0.500, z=0.001-0.100, A is one or more selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, preferably one or more selected from Fe, Ti, V, Ni, Co and Mg, and R is one or more selected from B, Si, N and S.

[0105] Preferably, said step (1) is carried out at a temperature of 20-120° C., preferably 25-80° C., and / or said stirring in step (1) is carried out at 500-700 rpm for 60-420 minutes, preferably 120-360 minutes.

[0106] In some embodiments, the source of element A is one or more selected from the group consisting of an element A, a sulfate, a halide, a nitrate, an organic acid salt, an oxide, or a hydroxide, and / or the source of element R is one or more selected from the group consisting of an element R, a sulfate, a halide, a nitrate, an organic acid salt, an oxide, or a hydroxide, and an inorganic acid of element R.

[0107] In some embodiments, MP 2 O 7The powder is prepared by the following method: adding a source of element M and a source of phosphorus to a solvent to obtain a mixture, adjusting the pH of the mixture to 4-6, stirring and reacting sufficiently, and then drying and sintering, where M is one or more selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb or Al. Preferably, the drying step is drying at 100-300°C, preferably 150-200°C for 4-8h, and the sintering step is sintering at 500-800°C, preferably 650-800°C, in an inert gas atmosphere for 4-10h.

[0108] In some embodiments, the sintering temperature in the coating step is 500-800° C., and the sintering time is 4-10 h.

[0109] In some embodiments, the positive electrode film layer may further include other positive electrode active materials for secondary batteries known in the art. For example, the positive electrode active material may include at least one of lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other conventional materials that can be used as positive electrode active materials for secondary batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Here, examples of lithium transition metal oxides include lithium nickel oxides (e.g., LiNiO 2 ), lithium manganese oxide (e.g. LiMnO 2 , LiMn 2 O 4 ), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, and modified compounds thereof. An example of a lithium-containing phosphate having an olivine structure is lithium iron phosphate (e.g., LiFePO 4 (which may be abbreviated as LFP)), lithium iron phosphate and carbon composites, lithium manganese phosphate (e.g., LiMnPO 4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.

[0110] In some embodiments, the positive electrode membrane layer can further include an adhesive, which can include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.

[0111] In some embodiments, the positive electrode membrane layer may further include a conductive agent, for example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0112] In some embodiments, the positive electrode sheet can be manufactured in the following manner: Components for manufacturing the positive electrode sheet, such as a positive electrode active material, a conductive agent, an adhesive, and any other components, are dispersed in a solvent (e.g., N-methylpyrrolidone) to form a positive electrode slurry, and the positive electrode slurry is applied to a positive electrode current collector, and the positive electrode sheet can be obtained after processes such as drying and cold pressing. [Negative electrode sheet]

[0113] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, the negative electrode film layer including a negative electrode active material.

[0114] For example, the negative electrode current collector has two opposing surfaces in the thickness direction of the negative electrode current collector, and the negative electrode film layer is disposed on either one or both of the two opposing surfaces of the negative electrode current collector.

[0115] In some embodiments, the negative electrode current collector may be a metal foil sheet or a composite current collector. For example, a copper foil may be used as the metal foil sheet. The composite current collector may have a base layer of a polymeric material and a metal layer formed on at least one side of the polymeric material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, silver alloy, etc.) on a polymeric material substrate (e.g., a substrate such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE)).

[0116] In some embodiments, the negative electrode active material may be a negative electrode active material for batteries known in the art. For example, the negative electrode active material may include at least one of artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based material, tin-based material, and lithium titanate. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide, silicon carbon composite, silicon nitrogen composite, and silicon alloy. The tin-based material may be selected from at least one of elemental tin, tin oxygen compound, and tin alloy. However, the present application is not limited to these materials, and other conventional materials usable as a battery negative electrode active material may be used. Only one of these negative electrode active materials may be used alone, or two or more may be used in combination.

[0117] In some embodiments, the negative electrode membrane layer can further optionally include an adhesive, for example, the adhesive is selected from at least one of styrene butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0118] In some embodiments, the negative electrode film layer may further include a conductive agent, for example, the conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0119] In some embodiments, the negative electrode membrane layer may further optionally include other auxiliary agents, such as a thickening agent (eg, sodium carboxymethylcellulose (CMC-Na)).

[0120] In some embodiments, the negative electrode sheet can be manufactured in the following manner: Components for manufacturing the negative electrode sheet, such as a negative electrode active material, a conductive agent, an adhesive, and any other components, are dispersed in a solvent (e.g., deionized water) to form a negative electrode slurry, and the negative electrode slurry is applied to a negative electrode current collector, followed by processes such as drying and cold pressing, to obtain a negative electrode sheet. [Separator]

[0121] In some embodiments, the secondary battery further includes a separator. The present application does not particularly limit the type of separator, and any known porous structure separator having good chemical stability and mechanical stability can be selected.

[0122] In some embodiments, the material of the separator can be selected from at least one of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single layer film or a multi-layer composite film, and is not particularly limited. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, and is not particularly limited.

[0123] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be produced into an electrode assembly by a winding process or a stacking process.

[0124] In some embodiments, the secondary battery can include an exterior packaging used to package the electrode assembly and electrolyte.

[0125] In some embodiments, the exterior of the secondary battery may be a hard case, such as a hard plastic case, an aluminum case, a steel case, etc. The exterior of the secondary battery may be a soft pack, such as a bag-type soft pack. The material of the soft bag may be plastic, such as polypropylene, polybutylene terephthalate, polybutylene succinate, etc.

[0126] The present application does not particularly limit the shape of the secondary battery, which may be cylindrical, rectangular, or any other shape. For example, FIG. 2 shows an example of a secondary battery 5 with a rectangular structure.

[0127] In some embodiments, as shown in FIG. 3, the exterior may include a case 51 and a cover plate 53. Here, the case 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate surround and form a receiving cavity. The case 51 has an opening communicating with the receiving chamber, and the cover plate 53 may cover the opening, thereby sealing the receiving chamber. The positive electrode sheet, the negative electrode sheet and the separator may form an electrode assembly 52 by a winding process or a lamination process. The electrode assembly 52 is sealed in the receiving chamber. The electrolyte is impregnated in the electrode assembly 52. ​​The number of electrode assemblies 52 included in the secondary battery 5 may be one or more, and those skilled in the art may select according to specific actual needs.

[0128] In some embodiments, the secondary batteries can be assembled into a battery module, and the number of secondary batteries included in the battery module can be one or more, and the specific number can be selected by one skilled in the art according to the application and capacity of the battery module.

[0129] Fig. 4 shows an example of a battery module 4. As shown in Fig. 4, in the battery module 4, a plurality of secondary batteries 5 may be arranged in sequence along the longitudinal direction of the battery module 4. Of course, the batteries may be arranged in any other manner. Furthermore, the plurality of secondary batteries 5 may be fixed by a fastener.

[0130] Preferably, the battery module 4 may further include a casing having an accommodation space, and the multiple secondary batteries 5 are accommodated in the accommodation space.

[0131] In some embodiments, the battery modules can be further assembled into a battery pack, and the number of battery modules included in the battery pack can be one or more, and the specific number can be selected by those skilled in the art according to the application and capacity of the battery pack.

[0132] 5 and 6 show an example of a battery pack 1. As shown in Fig. 5 and 6, the battery pack 1 may include a battery box and a plurality of battery modules 4 installed in the battery box. The battery box includes an upper housing 2 and a lower housing 3, and the upper housing 2 may be covered by the lower housing 3, forming a sealed space for accommodating the battery modules 4. The plurality of battery modules 4 may be arranged in the battery box in any manner.

[0133] The present application further provides an electric device, which includes at least one of the secondary batteries, battery modules, or battery packs provided by the present application. The secondary batteries, battery modules, or battery packs may be used as a power source for the electric device, or may be used as an energy storage unit for the electric device. The electric device may include, but is not limited to, mobile equipment (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships, satellites, energy storage systems, etc.

[0134] The electric device can be a secondary battery, a battery module or a battery pack according to its usage requirements.

[0135] 7 shows an example of an electric device, such as a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. A battery pack or a battery module can be employed to meet the high power and high energy density demands of the secondary battery of the electric device. EXAMPLES

[0136] The following examples of the present application are described. The following examples are illustrative and are only for the purpose of explaining the present application, and should not be understood as limiting the present application. If no specific techniques or conditions are shown in the examples, they are carried out according to the techniques or conditions described in the literature in this field or according to the product specifications. The reagents or equipment used are not specified by manufacturer, and are all conventional products that can be obtained commercially.

[0137] Among them, the first additive is selected from the following compounds: [ka] Example 1-1 [Production of bilayer-coated lithium manganese phosphate positive electrode active material] (1) Preparation of co-doped lithium manganese phosphate cores

[0138] Preparation of Fe, Co and V co-doped manganese oxalate: 689.5 g of manganese carbonate (MnCO 3 (Calculation: 455.2 g, same below) and ferrous carbonate (FeCO 3 (Calculation is based on the following formula, and the same applies below), 4.6 g of cobalt sulfate (CoSO 4 (Calculation: 100 g, same below) and 4.9 g of vanadium dichloride (VCl 2The mixture is transferred to a reactor, and 5 liters of deionized water and 1260.6 g of oxalic acid dihydrate (C 2 H 2 O 4 .2H 2 The reaction vessel is heated to 80°C, stirred at a rotation speed of 600 rpm for 6 hours, and stopped until the reaction is completed (no bubbles are generated), to obtain a manganese oxalate suspension co-doped with Fe, Co, V and S. The suspension is then filtered, and the filter cake is dried at 120°C, and then polished to obtain manganese oxalate dihydrate particles co-doped with Fe, Co and V, with a median diameter Dv50 of 100 nm.

[0139] Preparation of lithium manganese phosphate co-doped with Fe, Co, V and S: Manganese oxalate dihydrate particles (1793.4 g) obtained in the previous step, 369.0 g of lithium carbonate (Li 2 CO 3 (Calculation is based on the following formula, and so on.) 1.6 g of dilute sulfuric acid with a concentration of 60% (60%H 2 SO 4 (Calculated in the same manner below) and 1148.9 g of ammonium dihydrogen phosphate (NH 4 H 2 PO 4 (Calculated by: ##EQU1## and the same below) is added to 20 liters of deionized water, and the mixture is stirred for 10 hours to mix it uniformly, to obtain a slurry. The slurry is transferred to a spray dryer for spray drying granulation, the drying temperature is set to 250°C, and dried for 4 hours to obtain a powder material. The powder material is sintered at 700°C for 4 hours in a protective atmosphere of nitrogen gas (90% by volume) + hydrogen gas (10% by volume), to obtain 1572.1g of Fe, Co, V and S co-doped lithium manganese phosphate. (2) Manufacture of lithium iron pyrophosphate and lithium iron phosphate

[0140] Preparation of lithium iron pyrophosphate powder: 4.77 g of lithium carbonate, 7.47 g of ferrous carbonate, 14.84 g of ammonium dihydrogen phosphate, and 1.3 g of oxalic acid dihydrate are dissolved in 50 mL of deionized water. The pH of the mixture is 5, and the mixture is stirred for 2 hours to fully react. The reaction solution is then heated to 80° C. and maintained at that temperature for 4 hours to obtain Li 2 FeP 2 O 7 The suspension is filtered, washed with deionized water, and dried at 120°C for 4 hours to obtain a powder. The powder is sintered at 650°C in a nitrogen gas atmosphere for 8 hours, and then naturally cooled to room temperature and polished to obtain Li. 2 FeP 2 O 7 A powder is obtained.

[0141] Preparation of lithium iron phosphate suspension: 11.1 g lithium carbonate, 34.8 g ferrous carbonate, 34.5 g ammonium dihydrogen phosphate, 1.3 g oxalic acid dihydrate and 74.6 g sucrose (C 12 H 22 O 11 (Calculated by the following formula, the same applies below) is dissolved in 150 mL of deionized water to obtain a mixture, which is then stirred for 6 hours to allow the mixture to react sufficiently. The temperature of the reacted solution is then raised to 120° C. and the temperature is maintained for 6 hours to obtain LiFePO 4 A suspension containing (3) Covering

[0142] 1572.1 g of the Fe, Co, V and S co-doped lithium manganese phosphate and 15.72 g of the lithium iron pyrophosphate (Li 2 FeP 2 O 7 ) powder produced in the previous step. 4 ) suspension, and after stirring and mixing uniformly, it is transferred to a vacuum oven and dried at 150°C for 6 hours. The resulting product is then dispersed using a sand mill. After dispersion, the resulting product is sintered in a nitrogen gas atmosphere at 700°C for 6 hours to obtain the target product, bilayer-coated lithium manganese phosphate. [Production of positive electrode sheets]

[0143] The above-prepared bilayer-coated lithium manganese phosphate positive electrode active material, conductive agent acetylene black, and adhesive polyvinylidene fluoride (PVDF) are added to N-methylpyrrolidone (NMP) in a weight ratio of 92:2.5:5.5, and mixed uniformly by stirring to obtain a positive electrode slurry. 2 The mixture is then uniformly applied to an aluminum foil according to the desired thickness, and the aluminum foil is then dried, cold pressed, and divided to obtain a positive electrode sheet. [Manufacturing of negative electrode sheets]

[0144] The negative electrode active material artificial graphite, hard carbon, conductive agent acetylene black, adhesive styrene butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC-Na) are dissolved in deionized water as a solvent in a weight ratio of 90:5:2:2:1, and then uniformly mixed and stirred to produce a negative electrode slurry. The negative electrode slurry is 0.117g / 1540.25mm 2 The negative electrode sheet is obtained by uniformly applying the paste to the negative electrode current collector copper foil according to the requirements, drying, cold pressing, and dividing. [Electrolyte production]

[0145] Argon atmosphere glove box (H 2 O<0.1ppm, O 2 <0.1 ppm), ethylene carbonate (EC) / ethyl methyl carbonate (EMC) were mixed uniformly in a volume ratio of 3 / 7 as organic solvents, and Li(CF 3 SO 2 ) 2 N (as the first lithium salt, the mass content in the electrolyte is 10%), Compound 1 (as the first additive, the mass content in the electrolyte is 1%), LiBF 4 (The mass content of the second lithium salt in the electrolyte is 1%.) is added and stirred uniformly to obtain an electrolyte. [Separator]

[0146] A commercially available PP-PE copolymer microporous film (Takko Technologies, model no. 20) having a thickness of 20 μm and an average pore size of 80 nm is used. [Manufacturing all batteries]

[0147] The positive electrode sheet, separator, and negative electrode sheet are stacked in order, the separator is placed between the positive and negative electrodes to serve as an insulator, and then wound up to obtain a bare cell. The bare cell is placed in an outer casing, the electrolyte is injected, and the whole cell (hereinafter also referred to as "full battery") is obtained. [Button battery manufacturing]

[0148] The bilayer-coated lithium manganese phosphate cathode active material prepared above, PVDF, and acetylene black are added to NMP in a weight ratio of 90:5:5, and stirred in a drying chamber to prepare a slurry. The slurry is applied to an aluminum foil, dried, and cold pressed to form a cathode sheet. The coating amount is 0.2 g / cm. 2 and the compaction degree is 2.0g / cm 3 It is.

[0149] The lithium sheet is used as the negative electrode, and the above electrolyte is used to assemble the lithium sheet together with the above prepared positive electrode sheet into a button battery (hereinafter also referred to as "button battery") in a button battery box. Examples 1-2 to 1-6

[0150] In the process of producing the co-doped lithium manganese phosphate core, vanadium dichloride and cobalt sulfate are not used, and 463.4 g of ferrous carbonate, 1.6 g of 60% dilute sulfuric acid, 1148.9 g of ammonium dihydrogen phosphate and 369.0 g of lithium carbonate are used. Except for this, the production conditions of the lithium manganese phosphate core in Examples 1-2 to 1-6 are the same as those in Example 1-1.

[0151] In addition, in the manufacturing process of lithium iron pyrophosphate and lithium iron phosphate and the process of coating the first coating layer and the second coating layer, the raw materials used were adjusted according to the ratio of the coating amount shown in Table 1 to the coating amount corresponding to Example 1-1, thereby obtaining the Li in Examples 1-2 to 1-6. 2 FeP 2 O 7 / LiFePO 4The amounts of sucrose used in Examples 1-2 to 1-6 were 12.6 g / 37.7 g, 15.7 g / 47.1 g, 18.8 g / 56.5 g, 22.0 / 66.0 g, and 25.1 g / 75.4 g, respectively, and the amount of sucrose used in Examples 1-2 to 1-6 was 37.3 g, except that the other conditions were the same as in Example 1-1. Examples 1-7 to 1-10

[0152] The conditions of Examples 1-7 to 1-10 are the same as those of Example 1-3, except that the amounts of sucrose used are 74.6 g, 149.1 g, 186.4 g, and 223.7 g, respectively, and the corresponding coating amounts of the carbon layer as the second coating layer are 31.4 g, 62.9 g, 78.6 g, and 94.3 g, respectively. Examples 1-11 to 1-14

[0153] In the manufacturing process of lithium iron pyrophosphate and lithium iron phosphate, the amount of various raw materials used is adjusted according to the coating amount shown in Table 1. 2 FeP 2 O 7 / LiFePO 4 The conditions of Examples 1-11 to 1-14 were the same as those of Example 1-7, except that the amounts of the components used were 23.6 g / 39.3 g, 31.4 g / 31.4 g, 39.3 g / 23.6 g, and 47.2 g / 15.7 g, respectively. Examples 1-15

[0154] 492.80 g of ZnCO was used instead of ferrous carbonate in the preparation of the co-doped lithium manganese phosphate cores. 3 Except for using the above, the conditions of Example 1-15 are the same as those of Example 1-14. Examples 1-16 to 1-18

[0155] Examples 1-16 use 466.4 g of NiCO instead of ferrous carbonate in the preparation of the co-doped lithium manganese phosphate cores. 3The conditions of Examples 1-17 to 1-19 are the same as those of Example 1-7, except that 5.0 g of zinc carbonate and 7.2 g of titanium sulfate are used in the preparation of the co-doped lithium manganese phosphate core in Example 1-17, 455.2 g of ferrous carbonate and 8.5 g of vanadium dichloride are used in the preparation of the co-doped lithium manganese phosphate core in Example 1-18, and 455.2 g of ferrous carbonate, 4.9 g of vanadium dichloride and 2.5 g of magnesium carbonate are used in the preparation of the co-doped lithium manganese phosphate core in Example 1-18. Examples 1-19 to 1-20

[0156] In Example 1-19, 369.4g of lithium carbonate is used in the preparation of the co-doped lithium manganese phosphate core, and 1.05g of 60% dilute nitric acid is used to replace dilute sulfuric acid. In Example 1-20, 369.7g of lithium carbonate is used in the preparation of the co-doped lithium manganese phosphate core, and 0.78g of tetraethoxycarbonyl is used to replace dilute sulfuric acid. Except for this, the conditions of Examples 1-19 to 1-20 are the same as those of Example 1-18. Examples 1-21 to 1-22

[0157] In the preparation process of the co-doped lithium manganese phosphate core of Example 1-21, 632.0g manganese carbonate, 463.30g ferrous carbonate, 30.5g vanadium dichloride, 21.0g magnesium carbonate and 0.78g tetraethoxy are used, and in the preparation process of the co-doped lithium manganese phosphate core of Example 1-22, 746.9g manganese carbonate, 289.6g ferrous carbonate, 60.9g vanadium dichloride, 42.1g magnesium carbonate and 0.78g tetraethoxy are used, except that the conditions of Examples 1-21 to 1-22 are the same as those of Example 1-20. Examples 1-23 to 1-24

[0158] In the preparation process of the co-doped lithium manganese phosphate core of Example 1-23, 804.6 g of manganese carbonate, 231.7 g of ferrous carbonate, 1156.2 g of ammonium dihydrogen phosphate, 1.2 g of boric acid (mass fraction 99.5%) and 370.8 g of lithium carbonate are used, and in the preparation process of the co-doped lithium manganese phosphate core of Example 1-24, 862.1 g of manganese carbonate, 173.8 g of ferrous carbonate, 1155.1 g of ammonium dihydrogen phosphate, 1.86 g of boric acid (mass fraction 99.5%) and 371.6 g of lithium carbonate are used, except that the conditions of Examples 1-23 to 1-24 are the same as those of Example 1-22. Examples 1-25

[0159] In Example 1-25, the conditions are the same as those in Example 1-20, except that 370.1 g of lithium carbonate, 1.56 g of tetraethoxycaprylamide and 1147.7 g of ammonium dihydrogen phosphate are used in the preparation of the co-doped lithium manganese phosphate core. Examples 1-26

[0160] In Example 1-26, the conditions are the same as those of Example 1-20, except that 368.3 g of lithium carbonate, 4.9 g of dilute sulfuric acid with a mass fraction of 60%, 919.6 g of manganese carbonate, 224.8 g of ferrous carbonate, 3.7 g of vanadium dichloride, 2.5 g of magnesium carbonate, and 1166.8 g of ammonium dihydrogen phosphate are used in the preparation of the co-doped lithium manganese phosphate core. Examples 1-27

[0161] In Example 1-27, the conditions are the same as those in Example 1-20, except that 367.9g of lithium carbonate, 6.5g of 60% dilute sulfuric acid, and 1145.4g of ammonium dihydrogen phosphate are used in the preparation of the co-doped lithium manganese phosphate core. Examples 1-28 to 1-33

[0162] In the preparation process of the co-doped lithium manganese phosphate core in Examples 1-28 to 1-33, 1034.5g manganese carbonate, 108.9g ferrous carbonate, 3.7g vanadium dichloride and 2.5g magnesium carbonate were used, the amounts of lithium carbonate used were 367.6g, 367.2g, 366.8g, 366.4g, 366.0g and 332.4g, respectively, the amounts of ammonium dihydrogen phosphate used were 1144.5g, 1143.4g, 1142.2g, 1141.1g, 1139.9g and 1138.8g, respectively, and the amounts of dilute sulfuric acid with a concentration of 60% were 8.2g, 9.8g, 11.4g, 13.1g, 14.7g and 16.3g, respectively, except that the conditions of Examples 1-28 to 1-33 were the same as those of Example 1-20. Examples 2-1 to 2-4 Example 2-1

[0163] Lithium iron pyrophosphate (Li 2 FeP 2 O 7 In the manufacturing process of Li 2 FeP 2 O 7 The crystallinity of LiFePO is controlled to 30%. 4 In the manufacturing process of LiFePO, the sintering temperature in the coating sintering step is 650°C and the sintering time is 2 hours. 4 Except for controlling the crystallinity to 30%, the other conditions are the same as those in Example 1-1. Example 2-2

[0164] Lithium iron pyrophosphate (Li 2 FeP 2 O 7 In the manufacturing process of Li 2 FeP 2 O 7 The crystallinity of LiFePO is controlled to 50%. 4In the manufacturing process of LiFePO, the sintering temperature in the coating sintering step is 650°C and the sintering time is 3 hours. 4 Except for controlling the crystallinity to 50%, the other conditions are the same as those in Example 1-1. Example 2-3

[0165] Lithium iron pyrophosphate (Li 2 FeP 2 O 7 In the manufacturing process of Li 2 FeP 2 O 7 The crystallinity of LiFePO is controlled to 70%. 4 In the manufacturing process of LiFePO, the sintering temperature in the coating sintering step is 650°C and the sintering time is 4 hours. 4 Except for controlling the crystallinity to 70%, the other conditions are the same as those in Example 1-1. Examples 2-4

[0166] Lithium iron pyrophosphate (Li 2 FeP 2 O 7 In the manufacturing process of Li, the sintering temperature in the powder sintering step is 650°C and the sintering time is 4 hours. 2 FeP 2 O 7 The crystallinity of LiFePO is controlled to 100%. 4 In the manufacturing process of LiFePO, the sintering temperature in the coating sintering step is 700°C and the sintering time is 6 hours. 4 Except for controlling the crystallinity of 100%, the other conditions are the same as those in Example 1-1. Examples 3-1 to 3-12

[0167] In the process of preparing manganese oxalate particles co-doped with Fe, Co and V, the heating temperature / stirring time in the reaction vessel of Example 3-1 was 60°C / 120 min, the heating temperature / stirring time in the reaction vessel of Example 3-2 was 70°C / 120 min, the heating temperature / stirring time in the reaction vessel of Example 3-3 was 80°C / 120 min, the heating temperature / stirring time in the reaction vessel of Example 3-4 was 90°C / 120 min, the heating temperature / stirring time in the reaction vessel of Example 3-5 was 100°C / 120 min, and the heating temperature / stirring time in the reaction vessel of Example 3-6 was 110°C / 120 min. The heating temperature / stirring time in the reaction vessel in Example 3-7 is 120°C / 120 minutes, the heating temperature / stirring time in the reaction vessel in Example 3-8 is 130°C / 120 minutes, the heating temperature / stirring time in the reaction vessel in Example 3-9 is 100°C / 60 minutes, the heating temperature / stirring time in the reaction vessel in Example 3-10 is 100°C / 90 minutes, the heating temperature / stirring time in the reaction vessel in Example 3-11 is 100°C / 150 minutes, and the heating temperature / stirring time in the reaction vessel in Example 3-12 is 100°C / 180 minutes, except that the other conditions in Examples 3-1 to 3-12 are the same as those in Example 1-1. Examples 4-1 to 4-7 Examples 4-1 to 4-4

[0168] Lithium iron pyrophosphate (Li 2 FeP 2 O 7 In the manufacturing process of lithium iron pyrophosphate (Li 2 FeP 2 O 7 In the manufacturing process of the sintered body, the sintering temperature and the sintering time in the sintering step are 700°C / 6 hours, 700°C / 6 hours, 700°C / 6 hours, and 600°C / 6 hours, respectively, except that the other conditions are the same as those in Examples 1-7. Examples 4-5 to 4-7

[0169] Except that the drying temperature / drying time in the drying step in the coating process is 150°C / 6 hours, 150°C / 6 hours, and 150°C / 6 hours, respectively, and the sintering temperature and sintering time in the sintering step in the coating process is 600°C / 4 hours, 600°C / 6 hours, and 800°C / 8 hours, respectively, the other conditions are the same as those in Examples 1-12. Comparative Example 1

[0170] Preparation of manganese oxalate: 1149.3 g of manganese carbonate was added to a reaction kettle, and 5 liters of deionized water and 1260.6 g of oxalic acid dihydrate (C 2 H 2 O 4 2H 2 The reaction vessel is heated to 80°C, stirred at a rotation speed of 600 rpm for 6 hours, and stopped until the reaction is completed (no bubbles are generated), to obtain a manganese oxalate suspension, which is then filtered, and the filter cake is dried at 120°C, and then polished to obtain manganese oxalate dihydrate particles with a median diameter Dv50 of 100 nm.

[0171] Preparation of carbon-coated lithium manganese phosphate: 1789.6 g of the above obtained manganese oxalate dihydrate particles, 369.4 g of lithium carbonate (Li 2 CO 3 (Calculation is based on the following formula, and the same applies below), 1150.1 g of ammonium dihydrogen phosphate (NH 4 H 2 PO 4 (Calculated as follows, and so on) and 31 g of sucrose (C 12 H 22 O 11 (Calculated by: , and the same applies below) is taken and added to 20 liters of deionized water, and the mixture is stirred for 10 hours to mix it evenly, to obtain a slurry. The slurry is transferred to a spray drying device for spray drying granulation, the drying temperature is set to 250°C, and dried for 4 hours to obtain a powder material. The powder material is sintered at 700°C for 4 hours in a nitrogen gas (90% by volume) + hydrogen gas (10% by volume) protective atmosphere to obtain a carbon-coated lithium manganese phosphate. Comparative Example 2

[0172] Except for using 689.5 g of manganese carbonate and separately adding 463.3 g of ferrous carbonate, the other conditions of Comparative Example 2 are the same as those of Comparative Example 1. Comparative Example 3

[0173] Other than using 1148.9 g of ammonium dihydrogen phosphate and 369.0 g of lithium carbonate, and separately adding 1.6 g of 60% dilute sulfuric acid, the other conditions of Comparative Example 3 are the same as those of Comparative Example 1. Comparative Example 4

[0174] Other than using 689.5 g of manganese carbonate, 1148.9 g of ammonium dihydrogen phosphate, and 369.0 g of lithium carbonate, and separately adding 463.3 g of ferrous carbonate and 1.6 g of 60% dilute sulfuric acid, the other conditions of Comparative Example 4 are the same as those of Comparative Example 1. Comparative Example 5

[0175] Other than the addition of the following steps, the other conditions of Comparative Example 5 are the same as those of Comparative Example 4.

[0176] Preparation of lithium iron pyrophosphate powder: 9.52 g of lithium carbonate, 29.9 g of ferrous carbonate, 29.6 g of ammonium dihydrogen phosphate, and 32.5 g of oxalic acid dihydrate are dissolved in 50 mL of deionized water. The pH of the mixture is 5, and the mixture is stirred for 2 hours to fully react. The reacted solution is then heated to 80° C. and maintained at that temperature for 4 hours to obtain Li 2 FeP 2 O 7 The suspension is filtered, washed with deionized water, and dried at 120°C for 4 hours to obtain a powder. The powder is sintered at 500°C in a nitrogen gas atmosphere for 4 hours, and then naturally cooled to room temperature and polished to obtain Li 2 FeP 2 O 7 When the crystallinity of Li is controlled to 5% and the carbon-coated material is manufactured, 2 FeP 2 O 7 The amount used is 62.8g. Comparative Example 6

[0177] Other than the addition of the following steps, the other conditions of Comparative Example 6 are the same as those of Comparative Example 4.

[0178] Preparation of lithium iron phosphate suspension: 14.7 g of lithium carbonate, 46.1 g of ferrous carbonate, 45.8 g of ammonium dihydrogen phosphate, and 50.2 g of oxalic acid dihydrate are dissolved in 500 mL of deionized water, and then the mixture is stirred for 6 hours to fully react. The reacted solution is then heated to 120° C. and maintained at that temperature for 6 hours to obtain LiFePO 4 A suspension containing lithium iron phosphate (LiFePO 4 In the manufacturing process of LiFePO, the sintering temperature in the coating sintering step is 600°C and the sintering time is 4 hours. 4 When the crystallinity of LiFePO is controlled to be other than 8% and a carbon-coated material is produced, 4 The amount used is 62.8g. Comparative Example 7

[0179] Preparation of lithium iron pyrophosphate powder: 2.38 g of lithium carbonate, 7.5 g of ferrous carbonate, 7.4 g of ammonium dihydrogen phosphate, and 8.1 g of oxalic acid dihydrate are dissolved in 50 mL of deionized water. The pH of the mixture is 5, and the mixture is stirred for 2 hours to fully react. The reaction solution is then heated to 80° C. and maintained at that temperature for 4 hours to obtain Li 2 FeP 2 O 7 The suspension is filtered, washed with deionized water, and dried at 120°C for 4 hours to obtain a powder. The powder is sintered at 500°C in a nitrogen gas atmosphere for 4 hours, and then naturally cooled to room temperature and polished to obtain Li 2 FeP 2 O 7 The crystallinity is controlled to 5%.

[0180] Preparation of lithium iron phosphate suspension: 11.1 g lithium carbonate, 34.7 g ferrous carbonate, 34.4 g ammonium dihydrogen phosphate, 37.7 g oxalic acid dihydrate and 37.3 g sucrose (C 12 H 22 O 11(Calculated by the following formula, the same applies below) is dissolved in 1500 mL of deionized water, and then the mixture is stirred for 6 hours to allow it to react sufficiently. The temperature of the reacted solution is then raised to 120° C. and the temperature is maintained for 6 hours to obtain LiFePO 4 A suspension containing

[0181] The obtained 15.7 g of lithium iron pyrophosphate powder was mixed with the lithium iron phosphate (LiFePO 4 ) and sucrose suspension, and the sintering temperature in the coating sintering step during the manufacturing process is 600°C and the sintering time is 4 hours, so that LiFePO 4 Except for controlling the crystallinity to 8%, the other conditions of Comparative Example 7 are the same as those of Comparative Example 4, and amorphous lithium iron pyrophosphate, amorphous lithium iron phosphate, and carbon-coated positive electrode active materials are obtained. Comparative Examples 8-11

[0182] Lithium iron pyrophosphate (Li 2 FeP 2 O 7 In the manufacturing process of lithium iron pyrophosphate (Li 2 FeP 2 O 7 In the manufacturing process of LiFePO, the sintering temperature and sintering time in the sintering step were 400° C. / 3 hours, 400° C. / 3 hours, and 350° C. / 2 hours in Comparative Examples 8 to 10, respectively. 4 In the manufacturing process of Li 2 FeP 2 O 7 / LiFePO 4 The amounts of each of the materials used were 47.2g / 15.7g, 15.7g / 47.2g, 62.8g / 0g, and 0g / 62.8g, respectively, and the other conditions were the same as those in Examples 1-7.

[0183] The processes of [production of positive electrode sheet], [production of negative electrode sheet], [production of electrolyte], [separator] and [production of battery] in the above examples and comparative examples are all the same as those in Example 1-1. [Correlation Parameter Test]

[0184] 1. Initial theoretical capacity test of button batteries: Charge the button battery manufactured above at 2.5-4.3V at 0.1C up to 4.3V, then charge it at a constant voltage of 4.3V until the current becomes 0.05mA or less, leave it for 5 minutes, and then discharge it at 0.1C down to 2.0V. The discharge capacity at this time is the initial theoretical capacity and is denoted as D0.

[0185] 2. Button cell average discharge voltage (V) test: The button battery manufactured as above is placed in a constant temperature environment of 25°C for 5 minutes, discharged to 2.5V at 0.1C, placed in a constant temperature environment of 25°C for 5 minutes, charged to 4.3V at 0.1C, and then charged at a constant voltage of 4.3V until the current is 0.05mA or less. Placed in a constant temperature environment of 25°C for 5 minutes, and then discharged to 2.5V at 0.1C. The discharge capacity at this time is the initial theoretical capacity and is denoted as D0, the discharge energy is the initial energy and is denoted as E0, and the average discharge voltage V of the button battery is E0 / D0.

[0186] 3. 60℃ expansion test of all batteries: The whole battery manufactured above is stored at 60℃ with 100% state of charge (SOC). Before, during and after storage, the open circuit voltage (OCV) and internal resistance (IMP) of the cell are measured to monitor the SOC, and the cell volume is measured. Here, every 48 hours of storage, the whole battery is taken out and left to stand for 1 hour, after which the open circuit voltage (OCV) and internal resistance (IMP) are measured, and after cooling to room temperature, the cell volume is measured by the drainage method. In the drainage method, the gravity F of the cell is first measured using a balance that automatically converts the unit of the dial data. 1 was measured alone, and then the cell was filled completely with deionized water (with a density of 1 g / cm 3 The gravity of the cell at this time, F 2 The buoyancy force F acting on the cell was measured. 浮き is F 1 -F2 Then, Archimedes' principle

number

number

[0187] From the OCV and IMP test results, the batteries of all the examples maintained an SOC of 99% or more until the end of storage in this experimental process.

[0188] After 30 days of storage, the cell volume is measured and the percentage increase in cell volume after storage relative to the cell volume before storage is calculated.

[0189] Also, measure the remaining capacity of the cell. Charge all the batteries at 2.5 to 4.3 V at 1 C up to 4.3 V, then charge at a constant voltage of 4.3 V until the current drops to 0.05 mA or less. Leave the battery to stand for 5 minutes, and record the charge capacity at this time as the remaining capacity of the cell.

[0190] 4. Cycle performance test of all batteries at 45℃: In a constant temperature environment of 45°C, charge all the batteries manufactured above at 2.5 to 4.3V at 1C to 4.3V, then charge at a constant voltage of 4.3V until the current is 0.05mA or less. Leave it for 5 minutes, then discharge it at 1C to 2.5V, and record the discharge capacity at this time as D0. Repeat the above charge and discharge cycle until the discharge capacity drops to 80% of D0. Record the number of cycles the battery has gone through at this time.

[0191] 5. Lattice change rate test: Under a constant temperature environment of 25°C, the prepared positive active material sample is placed in an XRD (model number is Bruker D8 Discover), the sample is tested at 1° / min, and the test data is compiled and analyzed, and the lattice constants a0, b0, c0 and v0 (a0, b0 and c0 indicate the length magnitudes in various directions of the unit lattice, and v0 indicates the volume of the unit lattice, which can be obtained directly from the XRD finishing results) are calculated based on the standard PDF card.

[0192] The positive electrode active material sample is made into a button cell by using the above-mentioned button cell manufacturing method, and the button cell is charged at a low rate of 0.05C until the current decreases to 0.01C. Then, the positive electrode sheet in the button cell is taken out and placed in dimethyl carbonate (DMC) for 8 hours. Then, it is dried, the powder is scraped off, and the particles with a particle size of less than 500 nm are selected. The sample is sampled and its unit cell volume v1 is calculated in the same manner as the above-mentioned fresh sample test, and (v0-v1) / v0×100% is the lattice change rate (unit cell volume change rate) before and after complete lithium desorption, as shown in the table.

[0193] 6. Li / Mn antisite defect concentration test: The XRD results measured by the "lattice change rate measurement method" are compared with the PDF (Powder Diffraction File) card of the standard crystal to obtain the Li / Mn antisite defect concentration. Specifically, the XRD results measured by the "lattice change rate measurement method" are introduced into the General Structure Analysis System (GSAS) software to automatically obtain the finishing results, which include the occupancy status of different atoms, and the Li / Mn antisite defect concentration is obtained by reading the finishing results.

[0194] 7. Transition metal elution test: After cycling at 45°C until the capacity was attenuated to 80%, the whole battery was discharged at a rate of 0.1 C to a cut-off voltage of 2.0 V. The battery was then disassembled, the negative electrode sheet was removed, and 30 unit area (1540.25 mm2) was placed on the negative electrode sheet. 2) wafers are randomly taken and inductively coupled plasma emission spectrum (ICP) is measured using an Agilent ICP-OES730. Based on the ICP results, the amount of Fe (if Fe is doped on the Mn site of the positive electrode active material) and Mn is calculated, and the amount of Mn (and Fe doped on the Mn site) dissolved after cycling is calculated. The test standard complies with EPA-6010D-2014.

[0195] 8. Surface oxygen value test: Take 5g of the above prepared positive active material sample and prepare a button cell according to the above button cell preparation method. Charge the button cell at a low rate of 0.05C and stop until the current decreases to 0.01C. Then take out the positive electrode sheet in the button cell and place it in dimethyl carbonate (DMC) and soak for 8 hours. Then dry it, scrape off the powder, and select the particles with a particle size of less than 500nm. Measure the obtained particles by electron energy loss spectroscopy (EELS, the model number of the equipment used is Talos F200S) to obtain the energy loss perimeter structure (ELNES), which reflects the state density and energy level distribution of the elements. Based on the state density and energy level distribution, calculate the number of occupied electrons by integrating the valence band state density data, and thereby estimate the valence of the surface oxygen after charging.

[0196] 9. Measurement of compaction level: 5g of the above-prepared positive active material powder was placed in a compaction mold (CARVER mold, model number 13mm, USA), and then the mold was placed in a compaction density device. A pressure of 3T was applied, and the powder thickness at pressure in the device (thickness after releasing pressure) was measured. The area of ​​the container used for the test was 1540.25mm 2 ) and calculate the compaction degree using ρ = m / v.

[0197] 10. Measurement of Crystallinity of Pyrophosphate and Phosphate by X-ray Diffraction Method Take 5 g of the above-prepared positive electrode active material powder, and measure the total scattering intensity by X-ray, which is the sum of the scattering intensity of the entire space of the material, and is related only to the intensity of the primary radiation, the chemical structure, and the total number of electrons participating in the diffraction, i.e., the mass, and not related to the alignment state of the sample. Then, separate the crystalline scattering and the non-crystalline scattering from the diffraction pattern, and the crystallinity is the ratio of the crystalline partial scattering to the total scattering intensity.

[0198] 11.Crystal plane spacing and included angle 1g of each of the positive electrode active material powders prepared above was placed in a 50mL test tube, and 10mL of alcohol with a mass fraction of 75% was poured into the test tube, which was then thoroughly stirred and dispersed for 30 minutes. Then, an appropriate amount of the above solution was taken with a clean disposable plastic straw and dropped onto a 300 mesh copper net, at which time some of the powder remained on the copper net. The sample was then connected to the copper net and transferred to a TEM (Talos F200s G2) sample cavity for testing, and a TEM test original image was obtained and the original image format (xx.dm3) was saved.

[0199] The original image obtained by the above TEM test is opened in Digital Micrograph software, and a Fourier transform (automatically completed by the software after a click) is performed to obtain a diffraction pattern. The distance from the diffraction spot to the center position in the diffraction pattern can be measured to obtain the crystal plane spacing, and the included angle can be calculated based on the Bragg equation.

[0200] [Table 1-1] [Table 1-2] [Table 1-3] [Table 1-4] [Table 1-5]

[0201] As can be seen from Examples 1-1 to 1-33 and Comparative Example 1-4, the presence of the first coating layer reduces the Li / Mn antisite defect concentration of the resulting material and the amount of Fe and manganese ions eluted after cycling, improves the button capacity of the battery, and improves the safety performance and cycle performance of the battery. When the Mn site and the phosphorus site are doped with other elements, the lattice change rate, antisite defect concentration, and amount of Fe and manganese ions eluted of the resulting material can be significantly reduced, the theoretical capacity of the battery can be improved, and the safety performance and cycle performance of the battery can be improved.

[0202] From the results of Examples 1-1 to 1-6, it can be seen that with the amount of the first coating layer increasing from 3.2% to 6.4%, the concentration of Li / Mn antisite defects in the resulting material gradually decreases, the amount of Fe and manganese ions leaching out after cycling gradually decreases, and the safety performance and cycle performance at 45°C of the corresponding battery are also improved, but the theoretical capacity of the button cell battery is slightly reduced. Preferably, when the total amount of the first coating layer is 4-5.6% by weight, the overall performance of the corresponding battery is optimal.

[0203] From the results of Examples 1-3 and 1-7 to 1-10, it can be seen that as the amount of the second coating layer increases from 1% to 6%, the concentration of Li / Mn antisite defects in the resulting material decreases gradually, the amount of Fe and manganese ions dissolved after cycling decreases gradually, and the safety performance and cycle performance at 45°C of the corresponding battery are also improved, but the theoretical capacity of the button cell is slightly reduced. Preferably, when the total amount of the second coating layer is 3-5% by weight, the overall performance of the corresponding battery is optimal.

[0204] As can be seen from Examples 1-11 to 1-15 and Comparative Examples 5-6, the first coating layer had Li 2 FeP 2 O 7 and LiFePO 4 exist simultaneously, especially Li 2 FeP 2 O 7 and LiFePO4 is 1:3-3:1, and especially when the weight ratio is 1:3-1:1, the improvement on the battery performance is more obvious.

[0205] [Table 2]

[0206] As can be seen from Table 2, with the gradual increase in the crystallinity of the pyrophosphate and phosphate in the first coating layer, the lattice change rate of the corresponding material, the Li / Mn antisite defect concentration, and the amount of Fe and Mn ions leached out gradually decrease, the button capacity of the battery gradually increases, and the safety performance and cycle performance also gradually improve.

[0207] [Table 3]

[0208] As can be seen from Table 3, by adjusting the reaction temperature and reaction time in the reaction vessel during the preparation of manganese oxalate particles, the properties of the cathode material of the present application can be further improved. For example, in the process of gradually increasing the reaction temperature from 60°C to 130°C, the lattice change rate and the concentration of Li / Mn antisite defects first decrease and then increase, and the corresponding post-cycle metal elution amount and safety performance also show similar rules, and the button capacity and cycle performance first increase and then decrease with increasing temperature. The reaction temperature can also be controlled invariably and the reaction time can be adjusted to show similar rules.

[0209] [Table 4-1] [Table 4-2]

[0210] As can be seen from Table 4, when lithium iron pyrophosphate is produced by the method of the present application, the performance of the obtained material can be improved by adjusting the drying temperature / time and sintering temperature / time in the production process, thereby improving the battery performance. As can be seen from Comparative Examples 8-11, when the drying temperature in the production process of lithium iron pyrophosphate is lower than 100°C or the temperature of the sintering step is lower than 400°C, the desired Li 2 FeP 2 O 7 cannot be obtained, thereby improving the material performance and the performance of the battery containing the resulting material. Examples 5-40

[0211] The positive electrode active material, button cell and full cell were manufactured in the same manner as in Example 1-18, but the composition of the electrolyte was changed, as shown in Table 5 below.

[0212] The performance data of the button cell batteries or full cell batteries of Examples 5-40 were measured according to the above-mentioned performance test method, and the results are shown in Table 6.

[0213] [Table 5-1] [Table 5-2] [Table 5-3]

[0214] [Table 6-1] [Table 6-2]

[0215] The electrolyte in all the batteries in Examples 1-1 to 1-33, 2-1 to 2-4, 3-1 to 3-12, and 4-1 to 4-4 was replaced as follows: Ethylene carbonate (EC) / ethyl methyl carbonate (EMC) were mixed uniformly in a volume ratio of 3 / 7, and 12.5% ​​by weight (calculated based on the weight of the organic solvent) of LiPF 6 Dissolve in the above organic solvent, stir evenly, and add the resulting electrolyte. Replace the button battery electrolyte as follows: 1 mol / L LiPF 6 The solution of ethylene carbonate (EC) + diethyl carbonate (DEC) + dimethyl carbonate (DMC) in a volume ratio of 1:1:1 was used as the electrolyte, and the amounts of Mn and Fe eluted (ppm), 0.1C button cell capacity (mAh / g), button cell average discharge voltage (V), 45°C capacity retention 80% cycle number, and 60°C storage cell expansion rate (%) of the button cells or all batteries of Comparative Examples 1-1 to 1-33, 2-1 to 2-4, 3-1 to 3-12, and 4-1 to 4-4 formed after cycling were detected according to the above-mentioned methods, and the detection results are recorded in Table 7.

[0216] [Table 7-1] [Table 7-2] [Table 7-3] [Table 7-4]

[0217] Furthermore, by comparing Table 7 with the data in Tables 1-3 above, it can be seen that the electrolyte composition of the present invention can further improve the energy density and cycle performance of the secondary battery.

[0218] The present application is not limited to the above-mentioned embodiment. The above-mentioned embodiment is merely an example, and any embodiment that has substantially the same configuration as the technical idea within the scope of the technical solution of the present application and has similar effects is included in the technical scope of the present application. In addition, various modifications that a person skilled in the art can make to the embodiment and other forms constructed by combining some of the components in the embodiment are also included in the scope of the present application, as long as they do not deviate from the gist of the present application. [Explanation of symbols]

[0219] 1: battery pack, 2: upper housing, 3: lower housing, 4: battery module, 5: secondary battery, 51: case, 52: electrode assembly, 53: Cover plate .

Claims

1. A secondary battery including a positive electrode sheet and a non-aqueous electrolyte solution, The positive electrode sheet includes a positive electrode active material, the positive electrode active material including a core and a shell covering the core, The core is Li 1+x Mn 1-y A y P 1-z R z O 4 wherein x=-0.100 to 0.100, y=0.001 to 0.500, z=0.001 to 0.100, A is one or more selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge, and R is one or more selected from the group consisting of B, Si, N, and S, The shell includes a first coating layer coating the core and a second coating layer coating the first coating layer, The first coating layer is a pyrophosphate MP 2 O 7 and phosphate XPO 4 wherein M and X are each independently one or more selected from the group consisting of Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, and Al; the second coating layer comprises carbon; the non-aqueous electrolyte solution comprises a first lithium salt and a first additive; The first lithium salt is LiN(C m F 2m+1 SO 2 ) (C n F 2n+1 SO 2 ), Li (FSO 2 ) 2 N, wherein m and n are positive integers; The first additive comprises one or more of the compounds shown in formula 1, 【Chemistry 1】 R 1 is one or more R a represents any one of a C2-C10 alkylene group, a C2-C10 heteroalkylene group, a C6-C18 arylene group, a C2-C18 heteroarylene group, a C3-C18 divalent alicyclic group, and a C3-C18 heterodivalent alicyclic group, each of which may be substituted or unsubstituted by R a are halogen atoms, -CN, -NCO, -OH, -COOH, -SOOH, -COOR b , a C2-C10 alkyl group, a C2-C10 alkenyl group, a C2-C10 alkynyl group, or a C2-C10 oxaalkyl group; R b is any one selected from C1 to C10 alkyl groups Secondary battery.

2. R 1 is one or more R a represents any one of a C2-C10 alkylene group, a C2-C10 oxyalkylene group, a C2-C10 azaalkylene group, a phenylene group, a naphthylene group, an anthrylene group, a cyclobutylene group, a cyclopentylene group, a cyclohexylene group, a biphenylene group, and a methylenediphenylene group, which are substituted or unsubstituted by And / or the R a contains one or more selected from a halogen atom, -CN, and a C2-C3 alkyl group, and / or the R in the compound shown in formula 1 a The number of is 0, 1, 2, 3 or 4 2. The secondary battery according to claim 1.

3. The first additive comprises one or more of the following compounds:

2. The secondary battery according to claim 1. 【Chemistry 2-1】 【Chemistry 2-2】

4. m and n each independently represent 0, 1, 2, 3, or 4; and / or the first lithium salt is LiN(CF 3 SO 2 ) (FSO 2 ), Li(CF 3 SO 2 ) 2 N, LiN (C 4 F 9 SO 2 ) (FSO 2 ) and the first additive is any one selected from the following compounds:

2. The secondary battery according to claim 1. 【Chemistry 3】

5. Based on the total weight of the non-aqueous electrolyte, the content of the first lithium salt is W1 wt%, W1 is 0.1-48; The content of the first additive is W2% by weight, W2 is 0.01-20; Define W2 / W1 as M, where M is 0.001-3.

2. The secondary battery according to claim 1.

6. The non-aqueous electrolyte solution further contains a second lithium salt, and the second lithium salt is lithium difluorophosphate, lithium difluorodioxalatophosphate, lithium difluorooxalatoborate, lithium bisoxalatoborate, LiPF 6 , LiBF 4 Contains one or more selected from 2. The secondary battery according to claim 1.

7. Based on the total weight of the non-aqueous electrolyte, the content of the second lithium salt is W3 wt%, W3 is 0.01-20; (W2+W3) / W1 is defined as N, where N is 0.01-5 The secondary battery according to claim 6.

8. The non-aqueous electrolyte further includes a second additive, and the second additive includes one or more of the group consisting of a cyclic carbonate compound containing an unsaturated bond, a halogen-substituted saturated cyclic carbonate compound, a sulfate ester compound, a sulfite ester compound, a sultone compound, a disulfonic acid compound, a nitrile compound, an aromatic compound, an isocyanate compound, a phosphazene compound, a cyclic acid anhydride compound, a phosphite ester compound, a phosphate ester compound, and a borate ester compound.

2. The secondary battery according to claim 1.

9. The non-aqueous electrolyte solution further contains an organic solvent, The organic solvent includes one or more of a cyclic carbonate compound, a chain carbonate compound, and a carboxylic acid ester compound.

2. The secondary battery according to claim 1.

10. Calculated based on the weight of the core, the coating amount of the first coating layer is C1% by weight, C1 being greater than 0 and less than or equal to 7; and / or Calculated based on the weight of the core, the coating amount of the second coating layer is C2% by weight, where C2 is greater than 0 and less than or equal to 6.

2. The secondary battery according to claim 1.

11. Calculated based on the weight of the core, the coating amount of the first coating layer is C1% by weight, C1 being greater than 0 and less than or equal to 7; and / or When calculated based on the weight of the core, the coating amount of the second coating layer is C2% by weight, where C2 is greater than 0 and less than or equal to 6; Define the ratio of (W1+W2) / (C1+C2) as Q, where Q is 0.1-10. The secondary battery according to claim 5.

12. The weight ratio of pyrophosphate to phosphate in the first coating layer is 1:3-3:

1.

2. The secondary battery according to claim 1.

13. The crystal plane spacing of the phosphate of the first coating layer is 0.345-0.358 nm, and the included angle of the crystal direction (111) is 24.25°-26.45°; The crystal plane spacing of the pyrophosphate of the first coating layer is 0.293-0.326 nm, and the included angle of the crystal direction (111) is 26.41°-32.57°.

2. The secondary battery according to claim 1.

14. In said core, the ratio of y to 1-y is 1:10-10:1 2. The secondary battery according to claim 1.

15. In said core, the ratio of z to 1-z is 1:9-1:999 2. The secondary battery according to claim 1.

16. The crystallinity of the pyrophosphate and the phosphate is independently 10% to 100%.

2. The secondary battery according to claim 1.

17. The A is at least two selected from Fe, Ti, V, Ni, Co and Mg.

2. The secondary battery according to claim 1.

18. The positive electrode active material has a Li / Mn antisite defect concentration of 4% or less.

2. The secondary battery according to claim 1.

19. The lattice change rate of the positive electrode active material is 6% or less.

2. The secondary battery according to claim 1.

20. The surface oxygen valence of the positive electrode active material is −1.88 or less.

2. The secondary battery according to claim 1.

21. The compaction density of the positive electrode active material at 3 tons is 2.0 g / cm 3 That's all.

2. The secondary battery according to claim 1.

22. A battery module comprising the secondary battery according to any one of claims 1 to 21.

23. A battery pack comprising the battery module according to claim 22.

24. 22. An electrical device comprising at least one selected from the secondary batteries according to any one of claims 1 to 21.

Citation Information

Patent Citations

  • Cathode active material, cathode and non-aqueous secondary battery

    CN103069624A

  • Lithium-enriched manganese-based anode material with fast ion conductor coating layer and surface heterostructure and preparation method of lithium-enriched manganese-based anode material

    CN103928664A

  • LiMn1-XFexPO4 positive electrode material having core-shell structure, and preparation method thereof, and lithium ion battery

    CN106058225A

  • Lithium manganese iron phosphate composite material, preparation method thereof and lithium ion battery

    CN114256448A

  • Nonaqueous electrolyte secondary battery, and method of manufacturing the same

    JP2011014379A