Method for producing copolymer latex for paper coating

The production method for copolymer latex using specific monomers and stages addresses piling and balance issues, resulting in improved ink setting and dry pick strength for enhanced printing efficiency.

JP7587742B2Active Publication Date: 2024-11-21NIPPON A & L INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020198017
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-30
Publication Date
2024-11-21
Estimated Expiration
2040-11-30

AI Technical Summary

Technical Problem

Existing copolymer latex for paper coating does not adequately address issues such as piling during offset printing, ink setting properties, and the balance between viscosity and dry pick strength, leading to reduced printing efficiency.

Method used

A method for producing copolymer latex through emulsion polymerization of specific monomers, including aliphatic conjugated diene, ethylenically unsaturated carboxylic acid, and vinyl cyanide monomers in multiple stages, with controlled ratios and additives, to achieve a balanced ink setting, viscosity, and dry pick strength.

Benefits of technology

The method results in copolymer latex with improved ink setting properties, viscosity, and dry pick strength, reducing piling and enhancing printing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587742000001
    Figure 0007587742000001
  • Figure 0007587742000002
    Figure 0007587742000002
Patent Text Reader

Abstract

To provide a method of producing copolymer latex for paper coating, having excellent balance of ink set property of a latex film, viscosity of the copolymer latex and dry pick strength of coated paper.SOLUTION: The method of producing copolymer latex for paper coating, carries out emulsion polymerization of an aliphatic conjugated diene monomer, an ethylenic unsaturated carboxylic monomer, a vinyl cyanide monomer, and optionally, other copolymerizable monomers, with the emulsion polymerization including at least three stages of polymerization process, the amount of the vinyl cyanide monomer used being 20 to 35 mass% (relative to 100 mass% of the total monomers), and the mass ratio of the vinyl cyanide monomer used in the third stage and thereafter being 20 to 45% relative to the total of the vinyl cyanide monomer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a copolymer latex for paper coating. [Background technology]

[0002] Coated paper is used for a great many printed matters due to its high printing effect. There has been a considerable increase in the number of periodicals such as quarterly and monthly papers that use coated paper on every page. In particular, most direct mail and product catalogs in mail order businesses use coated paper on every page.

[0003] Generally, paper coating compositions are water-based paints that are composed of a pigment dispersion in which a white pigment such as clay or calcium carbonate is dispersed in water, a binder for adhering and fixing the pigments to each other and to the base paper, and other additives. As binders, synthetic emulsion binders such as styrene-butadiene copolymer latexes and natural binders such as starch and casein are used. Among them, styrene-butadiene copolymer latexes have a large degree of freedom in quality design and are widely used today as the most suitable binder for paper coating compositions, and it is known that the performance of styrene-butadiene copolymer latexes greatly affects the performance of paper coating compositions or the quality of the final coated paper product.

[0004] Among the various printing methods, offset printing is a method in which the non-image areas of the printing plate on the plate cylinder are made hydrophilic and the image areas are made lipophilic, and dampening water is applied to the non-image areas during printing, after which ink is applied only to the image areas, and this ink is transferred to the paper via a blanket. Generally, offset printing uses ink with relatively strong tack, and coupled with the recent increase in printing speed, a problem called piling (a phenomenon in which ink and paper dust accumulate on the blanket) has become an issue. If piling worsens, it is necessary to stop the printing press and clean the blanket, which significantly reduces printing workability.

[0005] Patent Document 1 discloses that pick strength, blister resistance, and stickiness resistance can be improved by emulsion-polymerizing monomers of a specific composition in three or more separate steps and providing a specific relationship between the solubility parameter and glass transition temperature of the copolymer obtained from the monomer composition in each step.

[0006] Patent Document 2 discloses that the use of a copolymer latex for paper coating obtained by emulsion polymerization of monomers of a specific composition in the first and second and subsequent stages improves pick strength and redispersibility, and accelerates the ink setting property of coated paper. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2002-194006 A [Patent Document 2] JP 2010-065326 A Summary of the Invention [Problem to be solved by the invention]

[0008] However, little research has been done on the suppression of piling from the copolymer latex surface, and other performances required for copolymer latexes for paper coating have not yet reached a fully satisfactory level.

[0009] As a result of extensive investigations, the present inventors have found that piling can be suppressed by slowing down the ink setting property of the latex film itself, and have thus completed the present invention.

[0010] An object of the present invention is to provide a method for producing a copolymer latex for paper coating which has an excellent balance between the ink setting property of the latex film, the viscosity of the copolymer latex, and the dry pick strength of the coated paper. [Means for solving the problem]

[0011] The present invention provides a method for producing a copolymer latex for paper coating use, which comprises emulsion polymerization of an aliphatic conjugated diene monomer, an ethylenically unsaturated carboxylic acid monomer, a vinyl cyanide monomer, and, as necessary, other copolymerizable monomers, and the emulsion polymerization has at least three polymerization stages, the amount of the vinyl cyanide monomer used is 20 to 35 mass% (total of monomers: 100 mass%), and the mass ratio of the vinyl cyanide monomer used in the third stage or later to the total vinyl cyanide monomers is 20 to 45%. Effect of the Invention

[0012] According to the present invention, there can be provided a method for producing a copolymer latex for paper coating which has an excellent balance between the ink setting property of the latex film, the viscosity of the copolymer latex, and the dry pick strength of the coated paper. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The method for producing a copolymer latex according to the present embodiment is a method for producing a copolymer latex for paper coating by emulsion polymerization of an aliphatic conjugated diene monomer, an ethylenically unsaturated carboxylic acid monomer, a vinyl cyanide monomer, and, if necessary, other copolymerizable monomers, and the emulsion polymerization has at least three polymerization stages, in which the amount of the vinyl cyanide monomer used is 20 to 35 mass% (total of monomers: 100 mass%), and the mass ratio of the vinyl cyanide monomer used in the third stage or later to the total vinyl cyanide monomer is 20 to 45%.

[0014] The copolymer latex according to the present embodiment is obtained by emulsion polymerization of an aliphatic conjugated diene monomer, an ethylenically unsaturated carboxylic acid monomer, a vinyl cyanide monomer, and, if necessary, other copolymerizable monomers.

[0015] Examples of the aliphatic conjugated diene monomer include 1,3-butadiene, 2-methyl-1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, substituted linear conjugated pentadiene, and substituted and side-chain conjugated hexadienes. These can be used alone or in combination of two or more. In this embodiment, it is preferable to use 1,3-butadiene from the viewpoints of industrial ease of production, availability, and cost.

[0016] Examples of the ethylenically unsaturated carboxylic acid monomer include monocarboxylic acid monomers such as acrylic acid, methacrylic acid, and crotonic acid, dicarboxylic acid monomers such as maleic acid, fumaric acid, and itaconic acid, and anhydrides thereof. These monomers can be used alone or in combination of two or more.

[0017] Examples of vinyl cyanide monomers include acrylonitrile, methacrylonitrile, α-chloroacrylonitrile, and α-ethylacrylonitrile. These may be used alone or in combination of two or more. In the present embodiment, it is preferable to use acrylonitrile or methacrylonitrile from the viewpoints of industrial ease of production, availability, and cost.

[0018] Examples of other copolymerizable monomers include alkenyl aromatic monomers, unsaturated carboxylic acid alkyl ester monomers, unsaturated monomers containing a hydroxyalkyl group, and unsaturated carboxylic acid amide monomers.

[0019] Examples of the alkenyl aromatic monomer include styrene, α-methylstyrene, methyl-α-methylstyrene, vinyltoluene, and divinylbenzene. These may be used alone or in combination of two or more. In this embodiment, it is preferable to use styrene from the viewpoints of industrial ease of production, availability, and cost.

[0020] Examples of the unsaturated carboxylic acid alkyl ester monomer include methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, glycidyl methacrylate, dimethyl fumarate, diethyl fumarate, dimethyl maleate, diethyl maleate, dimethyl itaconate, monomethyl fumarate, monoethyl fumarate, and 2-ethylhexyl acrylate. These can be used alone or in combination of two or more. In this embodiment, it is preferable to use methyl methacrylate from the viewpoints of industrial ease of production, availability, and cost.

[0021] Examples of unsaturated monomers containing a hydroxyalkyl group include β-hydroxyethyl acrylate, β-hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxybutyl methacrylate, 3-chloro-2-hydroxypropyl methacrylate, di-(ethylene glycol) maleate, di-(ethylene glycol) itaconate, 2-hydroxyethyl maleate, bis(2-hydroxyethyl) maleate, and 2-hydroxyethyl methyl fumarate. These can be used alone or in combination of two or more.

[0022] Examples of the unsaturated carboxylic acid amide monomer include acrylamide, methacrylamide, N-methylolacrylamide, N-methylolmethacrylamide, and N,N-dimethylacrylamide. These can be used alone or in combination of two or more.

[0023] In addition to the above monomers, monomers that are typically used in emulsion polymerization, such as ethylene, propylene, vinyl acetate, vinyl propionate, vinyl chloride, and vinylidene chloride, can also be used.

[0024] The amount of the aliphatic conjugated diene monomer used is preferably 33 to 57% by mass, more preferably 36 to 53% by mass, and even more preferably 40 to 48% by mass, based on the total amount of monomer components constituting the copolymer. By setting the amount used within the above range, the adhesive strength and operability of the copolymer latex can be improved.

[0025] The amount of the ethylenically unsaturated carboxylic acid monomer used is preferably 2 to 15% by mass, more preferably 2.5 to 12% by mass, and even more preferably 3 to 10% by mass, based on the total amount of the monomer components constituting the copolymer. By setting the amount used within the above range, the adhesive strength and operability of the copolymer latex can be improved.

[0026] The amount of the vinyl cyanide monomer used is 20 to 35% by mass, preferably 22 to 33% by mass, and more preferably 25 to 31% by mass, based on the total amount of monomer components constituting the copolymer. By keeping the amount used within the above range, it is possible to obtain a copolymer latex that is excellent in balance between the ink setting property of the latex film, the viscosity of the copolymer latex, and the dry pick strength of the coated paper.

[0027] In the present embodiment, the mass ratio of the vinyl cyanide monomer used in the third or subsequent steps to the total vinyl cyanide monomers is 20 to 45%, preferably 23 to 40%, and more preferably 26 to 32%. By setting the mass ratio within the above range, it is possible to obtain a copolymer latex that is excellent in balance between the ink setting property of the latex film, the viscosity of the copolymer latex, and the dry pick strength of the coated paper.

[0028] The amount of other copolymerizable monomers used is preferably 0 to 46 mass %, more preferably 2 to 44 mass %, and even more preferably 5 to 40 mass %, based on the total amount of monomer components constituting the copolymer.

[0029] In addition to the monomer components constituting the copolymer, an emulsifier (surfactant), a polymerization initiator, and, if necessary, a chain transfer agent, a reducing agent, and the like can be blended into the reaction system of the emulsion polymerization according to this embodiment.

[0030] Examples of emulsifiers include anionic surfactants such as sulfate salts of higher alcohols, alkylbenzenesulfonates, alkyldiphenyletherdisulfonates, aliphatic sulfonates, aliphatic carboxylates, dehydroabietic acid salts, formalin condensates of naphthalenesulfonic acid, sulfate salts of nonionic surfactants, and nonionic surfactants such as alkyl esters, alkylphenyl ethers, and alkyl ethers of polyethylene glycols. These can be used alone or in combination of two or more. The amount of emulsifier to be used can be appropriately adjusted in consideration of the combination with other additives.

[0031] Examples of the polymerization initiator include water-soluble polymerization initiators such as lithium persulfate, potassium persulfate, sodium persulfate, and ammonium persulfate, and oil-soluble polymerization initiators such as cumene hydroperoxide, benzoyl peroxide, t-butyl hydroperoxide, acetyl peroxide, diisopropylbenzene hydroperoxide, and 1,1,3,3-tetramethylbutyl hydroperoxide. These can be used alone or in combination of two or more. Of these, it is preferable to use potassium persulfate, sodium persulfate, cumene hydroperoxide, or t-butyl hydroperoxide. The amount of the polymerization initiator is appropriately adjusted in consideration of the monomer composition, the pH of the polymerization reaction system, and the combination of other additives.

[0032] Examples of the chain transfer agent include alkyl mercaptans such as n-hexyl mercaptan, n-octyl mercaptan, t-octyl mercaptan, n-dodecyl mercaptan, t-dodecyl mercaptan, and n-stearyl mercaptan; xanthogen compounds such as dimethyl xanthogen disulfide and diisopropyl xanthogen disulfide; thiuram compounds such as tetramethylthiuram disulfide, tetraethylthiuram disulfide, and tetramethylthiuram monosulfide; and 2,6-di-t-butyl-4-methylphenol. phenolic compounds such as styrenated phenol; allyl compounds such as allyl alcohol; halogenated hydrocarbon compounds such as dichloromethane, dibromomethane, and carbon tetrabromide; vinyl ethers such as α-benzyloxystyrene, α-benzyloxyacrylonitrile, and α-benzyloxyacrylamide; and chain transfer agents such as triphenylethane, pentaphenylethane, acrolein, methacrolein, thioglycolic acid, thiomalic acid, 2-ethylhexyl thioglycolate, terpinolene, and α-methylstyrene dimer. These can be used alone or in combination of two or more. The amount of the chain transfer agent can be appropriately adjusted in consideration of the combination with other additives, etc.

[0033] Examples of reducing agents include sulfites, hydrogen sulfites, pyrosulfites, dithionites, dithionates, thiosulfates, formaldehyde sulfonates, and benzaldehyde sulfonates; carboxylic acids and their salts, such as L-ascorbic acid, erythorbic acid, tartaric acid, and citric acid; reducing sugars, such as dextrose and saccharose; and amines, such as dimethylaniline and triethanolamine. These can be used alone or in combination of two or more. Of these, L-ascorbic acid and erythorbic acid are preferred. The amount of reducing agent to be added can be appropriately adjusted in consideration of the combination with other additives.

[0034] In addition, in order to control the molecular weight and crosslinked structure of the copolymer, the reaction system according to this embodiment can contain saturated hydrocarbons such as pentane, hexane, heptane, octane, cyclohexane, and cycloheptane; unsaturated hydrocarbons such as pentene, hexene, heptene, cyclopentene, cyclohexene, cycloheptene, 4-methylcyclohexene, and 1-methylcyclohexene; and aromatic hydrocarbons such as benzene, toluene, and xylene. These can be used alone or in combination of two or more. Of these, it is preferable to use cyclohexene and toluene.

[0035] Furthermore, the reaction system according to the present embodiment may contain additives such as electrolytes, oxygen scavengers, chelating agents, dispersants, defoamers, antioxidants, preservatives, antibacterial agents, flame retardants, ultraviolet absorbing agents, etc. The types and amounts of these additives may be appropriately selected and used.

[0036] The gel content of the copolymer latex is preferably 80 to 100% by mass, more preferably 85 to 99% by mass, and even more preferably 90 to 98% by mass. By setting the gel content of the copolymer latex within the above range, the ink setting property of the latex film and the dry pick strength of the coated paper can be improved. The gel content of the copolymer latex can be adjusted, for example, by changing the amount of the chain transfer agent. The gel content of the copolymer latex can be measured by the method described in the Examples.

[0037] The average particle size of the copolymer latex is preferably 50 to 120 nm, more preferably 60 to 110 nm, and even more preferably 70 to 100 nm. By setting the average particle size of the copolymer latex within the above range, the dry pick strength of the coated paper can be improved. The average particle size of the copolymer latex can be adjusted, for example, by changing the amount of water or emulsifier when preparing the copolymer latex. The average particle size of the copolymer latex can be measured by dynamic light scattering according to JIS Z8826 using a photon correlation method.

[0038] The copolymer latex may be blended with functional additives such as preservatives, antioxidants, printability improvers, surfactants, etc., as necessary. The types and amounts of these additives may be appropriately selected and used.

[0039] The paper coating composition containing the copolymer latex according to this embodiment preferably contains pigments, other binders, auxiliaries, and the like, as necessary.

[0040] Examples of pigments that can be used include inorganic pigments such as kaolin clay, calcium carbonate, talc, barium sulfate, titanium oxide, aluminum hydroxide, zinc oxide, and satin white, and organic pigments such as polystyrene latex. These can be used alone or in combination of two or more.

[0041] Other binders include starch, modified starches such as oxidized starch and esterified starch, natural binders such as soybean protein and casein, water-soluble synthetic binders such as polyvinyl alcohol and carboxymethyl cellulose, synthetic latexes such as polyvinyl acetate latex and acrylic latex, etc. These can be used alone or in combination of two or more.

[0042] Examples of auxiliary agents include defoamers (polyglycols, fatty acid esters, phosphate esters, silicone oils, etc.), leveling agents (rothanol oil, dicyandiamide, urea, etc.), preservatives, fluorescent dyes, and color water retention enhancers (sodium alginate, etc.).

[0043] The content of the copolymer latex in the paper coating composition is preferably 1 to 20 parts by mass, and more preferably 2 to 15 parts by mass, in terms of solid content, per 100 parts by mass of the pigment. EXAMPLES

[0044] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples. Furthermore, unless otherwise specified, % and parts are based on mass.

[0045] <Measurement of average particle size of copolymer latex by photon correlation method> The copolymer latex was filtered through a 200 mesh wire screen and then measured with FPAR-1000 (manufactured by Otsuka Electronics).

[0046] <Measurement of gel content of copolymer latex> A latex film is prepared in a room temperature atmosphere. Approximately 1 g of the latex film is then weighed out and designated as Xg. This is then placed in 400 ml of toluene and allowed to swell and dissolve for 48 hours. This is then filtered through a weighed 300 mesh wire screen, after which the toluene is evaporated and dried. The mesh mass is subtracted from the dried mass, and the dried mass of the sample is weighed and designated as Yg. The gel content is calculated using the following formula. Gel content (mass%) = Y / X x 100

[0047] <Synthesis of copolymer latex (A, B, C, E, F, G, H, I, J)> In a pressure-resistant polymerization reactor, 150 parts of polymerization water and 1 part of potassium persulfate were charged, and after thorough stirring, each monomer and other compound shown in the first stage of Tables 1 and 2 were added and the temperature was raised to 70°C to start polymerization. For the second stage polymerization, when the polymerization conversion rate of the first stage exceeded 50%, each monomer and other compound for the second stage was added and polymerization was carried out. For the third stage polymerization, when the polymerization conversion rate up to the second stage exceeded 80%, each monomer and other compound for the third stage was added and polymerization was carried out. When the final polymerization conversion rate exceeded 95%, the polymerization was terminated. Next, the pH of the obtained copolymer latex was adjusted to 7 using sodium hydroxide, and unreacted monomers and other low-boiling compounds were removed by steam distillation to obtain copolymer latexes A, B, C, E, F, G, H, I, and J.

[0048] <Synthesis of copolymer latex (D)> In a pressure-resistant polymerization reactor, 150 parts of polymerization water and 1 part of potassium persulfate were charged, and after thorough stirring, each monomer and other compound shown in the first stage of Table 1 were added and the temperature was raised to 70°C to start polymerization. For the second stage polymerization, when the polymerization conversion rate of the first stage exceeded 50%, each monomer and other compound for the second stage were added and polymerized. For the third stage polymerization, when the polymerization conversion rate up to the second stage exceeded 80%, each monomer and other compound for the third stage were added and polymerized. For the fourth stage polymerization, when the polymerization conversion rate up to the third stage exceeded 85%, each monomer and other compound for the fourth stage were added and polymerized. When the final polymerization conversion rate exceeded 95%, the polymerization was terminated. Next, the pH of the obtained copolymer latex was adjusted to 7 using sodium hydroxide, and unreacted monomers and other low-boiling point compounds were removed by steam distillation to obtain copolymer latex D.

[0049] [Table 1]

[0050] [Table 2]

[0051] <Method for evaluating viscosity of copolymer latex> The viscosity of the copolymer latex, when the solid content was adjusted to 48%, was measured according to the measurement method of JIS K 6838. The obtained viscosity was judged as follows. ○: 500mPa·s or less △: 501~1000mPa·s ×: 1001mPa·s or more

[0052] <Method for evaluating the ink setting property of latex film> Copolymer latex is applied to polyester film at a coating weight of 12g / m 2 After drying in a 120°C oven for 1 minute, cut into strips of 1 cm width. All the synthesized copolymer latex strips are lined up and pasted on a mount. Then, the latex clear film sample is printed with an RI printer, and when a blank sheet is placed on top of the sample and pressed with a roll, the image is transferred to the blank sheet at cumulative intervals of 0.5, 10, 20, and 30 minutes from the edge of the sample, and the concentration is visually evaluated as follows. (Transfer density is high) ◎ > ○ > △ > × (Transfer density is low)

[0053] <Preparation of Paper Coating Composition> According to the formulation shown below, the copolymer latexes A to J obtained by the synthesis above were used and adjusted to pH 9.5 with sodium hydroxide to prepare paper coating compositions. (Formulation of Paper Coating Composition) Formulation Kaolin 40 parts Ground calcium carbonate 60 parts Modified starch 2 parts Copolymer latex 7 parts .... Solid concentration 67%

[0054] <Preparation of coated paper> Coated base paper (basis weight 55g / m 2 ) and the above paper coating composition was applied to each side at a coating amount of 10 g / m 2After drying, the resultant was calendered under conditions of a linear pressure of 60 kg / cm and a temperature of 50° C. to obtain a coated paper.

[0055] <Method for evaluating dry pick strength of coated paper> Each coated paper sample was printed simultaneously on an RI printing press, and the degree of picking was visually evaluated on a relative scale from grade 5 (excellent) to grade 1 (poor).

Claims

[Claim 1] The method for producing a copolymer latex for paper coating comprises emulsion polymerization of an aliphatic conjugated diene monomer, an ethylenically unsaturated carboxylic acid monomer, a vinyl cyanide monomer, and, as necessary, other copolymerizable monomers, the emulsion polymerization having at least three polymerization stages, the amount of the vinyl cyanide monomer used being 20 to 31% by mass (total of monomers being 100% by mass), the mass ratio of the vinyl cyanide monomer used in the third stage or later to the total vinyl cyanide monomers being 20 to 45%, the gel content being 85 to 100% by mass, and the average particle size measured by a photon correlation method being 70 to 110 nm.

Citation Information

Patent Citations

  • Method for producing copolymer latex

    JP2002194006A

  • Copolymer latex for paper coating and paper coating composition highly containing calcium carbonate

    JP2010065326A

  • Copolymer latex for paper coating and paper coating composition

    JP2011174211A

  • Copolymer latex for paper coating and composition for paper coating

    JP2011195972A

  • Copolymer latex for paper coating and composition for paper coating

    JP2011195973A