A lithium niobate solution with specific molar ratios and ammonium ions addresses stability issues, ensuring high dispersibility and solubility, leading to improved battery performance through stable coatings.
Patent Information
- Application Number
- JP2023128828
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-04-28
- Filing Date
- 2023-08-07
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2042-03-10
AI Technical Summary
Existing lithium niobate precursor solutions face issues with stability due to hydrogen peroxide concentration, leading to decomposition and instability, especially when concentrations are below certain thresholds, affecting dispersibility and solubility in water.
A lithium niobate solution with a lithium to niobium molar ratio of 0.8 to 2.0, containing ammonium ions and without hydrogen peroxide, with particle sizes less than 100 nm, ensuring high dispersibility and solubility in water, and improved storage stability.
The solution achieves stable lithium niobate dispersions with excellent long-term storage stability and uniform coating on positive electrodes, enhancing the performance of lithium ion secondary batteries.
Smart Images

Figure 0007588188000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a lithium niobate solution and a method for producing the same. [Background technology]
[0002] Lithium niobate is used as a nonlinear optical material in the form of a single crystal, and a technology is disclosed in Patent Document 1 in which a solution of lithium niobate is used to cover the surface of positive electrode active material particles of a lithium ion secondary battery, thereby reducing the interfacial resistance occurring between the positive electrode and electrolyte of the lithium ion secondary battery. Hydrogen peroxide water is added to the lithium niobate precursor aqueous solution disclosed in Patent Document 1 in order to improve storage stability. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-66570 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, Patent Document 1 discloses the following points to be noted regarding the lithium niobate precursor aqueous solution to which hydrogen peroxide has been added: if the concentration of hydrogen peroxide is less than 0.1 mol per mol of niobium, the generated niobium polyacid reacts with hydroxide ions and decomposes, if the amount of free hydrogen peroxide in the lithium niobate precursor aqueous solution is less than 0.01 mass %, it is difficult to maintain the stability of the precursor aqueous solution, and further, the presence of hydrogen peroxide in the lithium niobate precursor aqueous solution may cause a portion of the solubilized niobic acid to form an unstable peroxo complex.
[0005] In view of the above problems, the present invention provides a lithium niobate solution having high dispersibility in water, favorable solubility in water, and excellent storage stability, and a method for producing the same. [Means for solving the problem]
[0006] The lithium niobate solution of the present invention, which has been made to solve the above problems, is a lithium niobate solution containing lithium niobate having a lithium to niobium molar ratio Li / Nb of 0.8 to 2.0 and ammonium ions, and is characterized in that the lithium niobate particle size (D50) in the lithium niobate solution measured by dynamic light scattering method is 100 nm or less. In the lithium niobate solution of the present invention, when the lithium niobate (LiNbO3) in the lithium niobate solution has a molar ratio Li / Nb of 0.8 or more and 2.0 or less, the occurrence of precipitation from the solution can be suppressed, and the stability of the solution is improved. Moreover, the molar ratio Li / Nb of lithium to niobium in the lithium niobate solution is more preferably 0.9 or more and 1.5 or less, and even more preferably 0.9 or more and 1.2 or less.
[0007] Here, it is presumed that the lithium niobate in the lithium niobate solution of the present invention exists in the solution as ions in a state in which niobic acid and lithium are ionic bonded. In the lithium niobate solution of the present invention, hydroxide ions exist as anions, while halide ions such as fluoride ions and chloride ions are hardly present, and lithium is considered to exist as a cation. Therefore, niobium is NbO3 - These ions are thought to exist as anions such as those shown below, or as polyoxometalate (polyacid) ions in which multiple niobium atoms are bonded to oxygen atoms.
[0008] The lithium niobate solution of the present invention also contains ammonium ions in addition to lithium niobate. As will be described in detail later in the method for producing the lithium niobate solution of the present invention, in the production process, a reverse neutralization method is used in which an acidic niobium solution is added to ammonia water to produce a hydrous ammonium niobate cake, which is a precipitate slurry containing niobium, and then the lithium niobate solution of the present invention is produced. Therefore, it is considered that the ammonium ions substituted for the lithium ions are present in the solution as cations.
[0009] Methods for measuring the ammonium ion concentration in the solution include adding sodium hydroxide to the solution to distill off ammonia and quantifying the ammonium ion concentration using an ion meter, quantifying the N2 content in a gasified sample using a thermal conductivity meter, the Kjeldahl method, gas chromatography (GC), ion chromatography, and GC-MS (mass spectrometry).
[0010] The ammonium ion concentration of the ammonium ion contained in the lithium niobate solution of the present invention is preferably 0.001% by mass or more and 25% by mass or less, more preferably 0.5% by mass or more and 10% by mass or less, and even more preferably 1% by mass or more and 8% by mass or less.
[0011] Furthermore, the lithium niobate particle diameter (D50) in the lithium niobate solution measured by dynamic light scattering is preferably 100 nm or less in terms of high dispersibility. Furthermore, the lithium niobate particle diameter (D50) in the lithium niobate solution is preferably smaller in terms of stability due to less change over time, and also in terms of forming a good coating film without uncoated areas during film formation and ensuring a sufficient coating weight. The lithium niobate particle diameter (D50) in the lithium niobate solution is more preferably 80 nm or less, even more preferably 50 nm or less, particularly preferably 30 nm or less, more particularly preferably 20 nm or less, even more particularly preferably 10 nm or less, also particularly preferably 5 nm or less, and even more particularly preferably 3 nm or less. Thus, the lithium niobate particle diameter (D50) in the lithium niobate solution of the present invention is measured by dynamic light scattering, and the solution in which the lithium niobate particle diameter (D50) is 100 nm or less is the "lithium niobate solution" of the present invention.
[0012] Here, the dynamic light scattering method is a method in which a solution such as a suspension is irradiated with light such as a laser beam to measure the light scattering intensity from a group of particles undergoing Brownian motion, and the particle size and distribution are obtained from the temporal variation of the intensity. Specifically, the particle size distribution is evaluated in accordance with JIS Z 8828:2019 "Particle Size Analysis - Dynamic Light Scattering Method" using a Zeta Potential, Particle Size, and Molecular Weight Measurement System (Otsuka Electronics Co., Ltd.: ELSZ-2000). In addition, in order to remove dust and the like in the solution to be measured immediately before the measurement, the solution is filtered with a filter with a pore size of 2 μm, and ultrasonic treatment is performed for 3 minutes at 28 kHz with an ultrasonic cleaner (As One Co., Ltd.: VS-100III). The particle size (D50) refers to the median diameter (D50), which is the particle size that shows the 50% cumulative value of the cumulative distribution curve.
[0013] In the present invention, the term "solution" is not limited to a solute dispersed or mixed in a solvent in a monomolecular state, but also includes an aggregate in which a plurality of molecules are attracted to each other by intermolecular interactions, such as (1) polymer molecules, (2) solvated molecules, (3) molecular clusters, and (4) colloidal particles dispersed in a solvent.
[0014] In addition, the lithium niobate solution of the present invention preferably does not contain hydrogen peroxide. Generally, when niobium oxide is present in a solution as a polyacid ion, hydrogen peroxide is added to inhibit the niobium oxide from reacting with hydroxide ions and decomposing, thereby improving stability. However, the lithium niobate solution of the present invention can ensure long-term stability even in the absence of hydrogen peroxide due to the presence of ammonium ions in the solution.
[0015] The method of detecting hydrogen peroxide in a solution can be, for example, by using the standard addition method, to measure the relative intensity of absorbance with a standard solution of hydrogen peroxide, thereby confirming that the solution does not contain hydrogen peroxide. Specifically, a wavelength region in which a change in absorbance due to the formation of a peroxo complex is observed is found from the UV-visible absorption spectrum of a standard solution containing hydrogen peroxide of a known concentration, for example, 1 mass %, and a standard solution to which hydrogen peroxide is not added, and if the difference in absorbance between the standard solution to which hydrogen peroxide is not added and a sample with an unknown hydrogen peroxide concentration in that wavelength region is less than 1%, it can be confirmed that the sample with an unknown hydrogen peroxide concentration does not substantially contain hydrogen peroxide. If hydrogen peroxide is contained in the solution, hydrogen peroxide reacts with a niobium polyacid to form a peroxo complex, and therefore, by confirming the difference in absorbance with the standard solution to which hydrogen peroxide is not added as described above, it can be confirmed that hydrogen peroxide is not contained in the solution. In addition to the above-mentioned standard addition method, hydrogen peroxide in a solution may be qualitatively and quantitatively analyzed by, for example, using a commercially available hydrogen peroxide measurement kit, adding a reagent that undergoes a color reaction with hydrogen peroxide to the solution and measuring the color development, or by adding a reagent that undergoes a fluorescent reaction with hydrogen peroxide to the solution and measuring the light emission.
[0016] In addition, the lithium niobate solution of the present invention is preferably an aqueous solution. Since the lithium niobate in the lithium niobate solution of the present invention has high dispersibility in water and good solubility in water, pure water can be used as the solvent.
[0017] The lithium niobate solution of the present invention is characterized in that the lithium niobate concentration in the lithium niobate solution is 0.1 to 30 mass %. The lithium niobate solution of the present invention is characterized in that the lithium niobate concentration in the lithium niobate solution is 5 to 20 mass %. The lithium niobate concentration in the lithium niobate solution is preferably 0.1 to 30 mass % in terms of achieving both practicality and stability of the lithium niobate solution, more preferably 1 to 25 mass %, even more preferably 3 to 21 mass %, and particularly preferably 5 to 20 mass %.
[0018] Here, the lithium niobate concentration in the lithium niobate solution is calculated by diluting the solution with dilute hydrochloric acid as necessary, and measuring the weight fraction of Nb and the weight fraction of Li in terms of niobium oxide (Nb2O5) using ICP emission spectrometry (Agilent Technologies: AG-5110) in accordance with JIS K0116:2014. Note that the niobic acid in the lithium niobate solution of the present invention is not necessarily present in the form of Nb2O5. The content of niobic acid is shown in terms of Nb2O5 based on the convention for showing the niobium concentration.
[0019] The lithium niobate solution of the present invention can be used for coating a positive electrode or positive electrode material for a lithium ion secondary battery, or for coating a positive electrode or positive electrode material for an all-solid-state lithium ion battery. The lithium niobate solution of the present invention is suitable for coating a positive electrode for a lithium ion secondary battery or a positive electrode material, based on the results of a stability test over time in which the state of the solution after being left to stand for one month in an incubator set at room temperature (25°C) was visually observed, and a dynamic light scattering method was used to measure the particle size (D50) of the lithium niobate particles in the solution over time. The lithium niobate solution of the present invention is also suitable for coating a positive electrode for a lithium ion secondary battery or a positive electrode material, based on the results of a film-formability test in which the solution is applied to a glass substrate used as a substitute for a current collector of a positive electrode for a lithium ion secondary battery and the state of the coating is observed under an optical microscope, and a safety test in which the solution is mixed with a positive electrode active material and the presence or absence of foaming is visually confirmed.
[0020] The positive electrode active material for a lithium ion secondary battery of the present invention is characterized in that its surface is coated with the lithium niobate contained in the lithium niobate solution. By observing the coating state of the particle surface of the lithium niobate solution of the lithium niobate solution of the present invention by scanning electron microscope, it is possible to confirm that the surface of the positive electrode active material is coated with lithium niobate. The amount of lithium niobate coating the surface of the lithium ion secondary battery positive electrode active material of the present invention can be calculated by dissolving the lithium ion secondary battery positive electrode active material in an appropriate amount of hydrofluoric acid, and measuring the niobium weight fraction concentration of the lithium niobate coating the particle surface of the positive electrode active material using ICP emission spectrometry (manufactured by Agilent Technologies: AG-5110) in accordance with JIS K0116:2014. The niobium weight fraction concentration is preferably 1 or more, more preferably more than 1, even more preferably 1.1 or more, and particularly preferably 1.2 or more.
[0021] Furthermore, the lithium niobate solution of the present invention may contain components other than the components derived from lithium niobate and the components derived from ammonia (referred to as "other components") within a range that does not impair the action and effect of the solution. Examples of other components include Na, Mg, Si, K, Ca, Ti, Mn, Ni, Zn, Sr, Zr, Ta, Mo, Ba, and W. However, the other components are not limited to these. The content of other components in the lithium niobate solution of the present invention is preferably less than 5% by mass, more preferably less than 4% by mass, and even more preferably less than 3% by mass. It is assumed that the lithium niobate solution of the present invention contains unavoidable impurities, but not intentionally. The content of unavoidable impurities is preferably less than 0.01% by mass.
[0022] The lithium ion secondary battery of the present invention is characterized by having a positive electrode coated with the positive electrode active material. As described above, the positive electrode active material coated with the lithium niobate solution of the present invention is suitable for coating the surface of a positive electrode for a lithium ion secondary battery. Therefore, by coating the surface of a positive electrode with the positive electrode active material coated with the lithium niobate solution of the present invention, the performance of the lithium ion secondary battery can be improved.
[0023] The method for producing the lithium niobate solution of the present invention described above will be described below.
[0024] The method for producing a lithium niobate solution of the present invention includes the steps of: generating an acidic niobium solution containing niobium; obtaining a precipitate slurry containing niobium by a reverse neutralization method in which the acidic niobium solution is added to ammonia water; and maintaining a mixture of the obtained precipitate slurry containing niobium, lithium hydroxide, and pure water at 20°C to 100°C while stirring to obtain a lithium niobate solution.
[0025] First, in the step of producing an acidic niobium solution containing niobium, the acidic niobium solution refers to an acidic niobium solution containing fluoride ions obtained by solvent extraction of a solution in which niobium is dissolved in an acidic solution containing hydrofluoric acid. Note that, unless otherwise specified, niobium referred to in this specification includes niobic acid compounds.
[0026] Here, it is preferable to adjust the acidic niobium solution containing fluoride ions, for example, the niobium fluoride aqueous solution, to contain niobium at 1 to 100 g / L in terms of Nb2O5 by adding water (for example, pure water). In this case, it is preferable that the niobium concentration is 1 g / L or more in terms of Nb2O5, since it becomes a niobium acid compound hydrate that is easily soluble in water, and in consideration of productivity, it is more preferable that it is 10 g / L or more, and even more preferable that it is 20 g / L or more. On the other hand, it is preferable that the niobium concentration is 100 g / L or less in terms of Nb2O5, since it becomes a niobium acid compound hydrate that is easily soluble in water, and in order to synthesize a niobium acid compound hydrate that is easily soluble in water more reliably, it is more preferable that it is 90 g / L or less, even more preferable that it is 80 g / L or less, and particularly preferable that it is 70 g / L or less. In addition, the pH of the niobium fluoride aqueous solution is preferably 2 or less, more preferably 1 or less, from the viewpoint of completely dissolving niobium or niobium oxide.
[0027] Next, in the step of obtaining a precipitation slurry containing niobium by a reverse neutralization method in which the acidic niobium solution is added to ammonia water (hereinafter referred to as a reverse neutralization step), it is preferable to obtain a precipitation slurry containing niobium by adding an acidic niobium solution containing fluoride ions to ammonia water of a predetermined concentration, i.e., by the reverse neutralization method.
[0028] The ammonia concentration of the ammonia water used for reverse neutralization is preferably 10% by mass to 30% by mass. When the ammonia concentration is 10% by mass, niobium is less likely to remain undissolved, and niobium or niobic acid can be completely dissolved in water. On the other hand, when the ammonia concentration is 30% by mass or less, it is preferable because it is close to a saturated aqueous solution of ammonia.
[0029] From this viewpoint, the ammonia concentration of the ammonia water is preferably 10% by mass or more, more preferably 15% by mass or more, even more preferably 20% by mass or more, and particularly preferably 25% by mass, while the ammonia concentration is preferably 30% by mass or less, more preferably 29% by mass or less, and even more preferably 28% by mass or less.
[0030] In the reverse neutralization step, the amount of niobium fluoride aqueous solution added to ammonia water is preferably such that the molar ratio of NH3 / Nb2O5 is 95 or more and 500 or less, more preferably 100 or more and 450 or less, and even more preferably 110 or more and 400 or less. In addition, the amount of niobium fluoride aqueous solution added to ammonia water is preferably such that the molar ratio of NH3 / HF is 3.0 or more, more preferably 4.0 or more, and even more preferably 5.0 or more, from the viewpoint of generating amines or niobic acid compounds that dissolve in dilute ammonia water. On the other hand, from the viewpoint of reducing costs, the molar ratio of NH3 / HF is preferably 100 or less, more preferably 50 or more, and even more preferably 40 or more.
[0031] In the reverse neutralization step, the time for adding the niobium fluoride aqueous solution to the ammonia water is preferably within 1 minute, more preferably within 30 seconds, and even more preferably within 10 seconds. That is, it is preferable to add the niobium fluoride aqueous solution to the ammonia water in as short a time as possible, for example, all at once, rather than gradually adding the niobium fluoride aqueous solution over a long period of time, and to carry out the neutralization reaction. In addition, in the reverse neutralization step, since the acidic niobium fluoride aqueous solution is added to the alkaline ammonia water, the neutralization reaction can be carried out while maintaining a high pH. The niobium fluoride aqueous solution and the ammonia water can be used at room temperature.
[0032] The method for producing a lithium niobate solution of the present invention includes a step of removing fluoride ions from the niobium-containing precipitate slurry obtained by the reverse neutralization method to obtain a niobium-containing precipitate from which fluoride ions have been removed. Since the niobium-containing precipitate slurry obtained by the reverse neutralization method contains fluorine compounds such as ammonium fluoride as impurities, it is preferable to remove these.
[0033] Any method can be used to remove the fluorine compounds, and examples of such methods include filtration using a membrane such as reverse osmosis filtration, ultrafiltration, and microfiltration using aqueous ammonia or pure water, centrifugation, and other known methods. When removing fluoride ions from the niobium-containing precipitate slurry, temperature control is not particularly required, and the removal may be performed at room temperature.
[0034] Specifically, the niobium-containing precipitate slurry obtained by the reverse neutralization method is decanted using a centrifuge, and washing is repeated until the amount of liberated fluoride ions becomes 100 mg / L or less, thereby obtaining a niobium-containing precipitate from which the fluoride ions have been removed.
[0035] The cleaning solution used to remove fluoride ions is preferably ammonia water. Specifically, ammonia water of 5.0 mass% or less is preferable, ammonia water of 4.0 mass% or less is more preferable, ammonia water of 3.0 mass% or less is even more preferable, and ammonia water of 2.5 mass% is particularly preferable. When the ammonia water is 5.0 mass% or less, ammonia and ammonium ions are suitable for fluorine, and unnecessary cost increase can be avoided.
[0036] The niobium-containing precipitate thus obtained, from which the fluoride ions have been removed, is diluted with pure water or the like to obtain a precipitate slurry containing niobium from which the fluoride ions have been removed. The niobium concentration of the precipitate slurry containing niobium is measured by taking a portion of the slurry, drying it at 110°C for 24 hours, and then firing it at 1,000°C for 4 hours to produce Nb2O5. The weight of the Nb2O5 thus produced can be measured, and the niobium concentration of the slurry can be calculated from the weight.
[0037] The niobium-containing precipitate slurry from which the fluoride ions have been removed is mixed with lithium hydroxide monohydrate, and the mixture is stirred and maintained at 20°C to 100°C, thereby obtaining the lithium niobate solution of the present invention.
[0038] Specifically, the resulting niobium-containing precipitate slurry is mixed with lithium hydroxide monohydrate so that the final mixture has a lithium niobate concentration of 0.1 to 30 mass% in terms of Nb2O5 and a lithium to niobium molar ratio Li / Nb of 0.8 to 2.0, thereby obtaining a translucent white slurry. The translucent white slurry is stirred while maintaining the liquid temperature at 50°C to 100°C (for example, 70°C) for 1 to 24 hours, thereby obtaining a colorless and transparent lithium niobate solution of the present invention. In addition, pure water or an alkaline aqueous solution, for example, ammonia water, may be added to the mixture of the niobium-containing precipitate slurry and lithium hydroxide monohydrate, and mixed. The ammonia concentration of the ammonia water added to the mixture may be any concentration. For example, it may be 0.1 mass% to 30 mass%, and may be 10 mass% to 25 mass%.
[0039] The lithium niobate solution is then cooled to room temperature. The lithium niobate solution of the present invention can be dried to obtain lithium niobate powder.
[0040] The lithium niobate solution of the present invention obtained by the above-mentioned production method preferably has a pH of 9 or more in terms of the stability of the lithium niobate solution. Furthermore, the lithium niobate solution of the present invention more preferably has a pH of 10 or more, even more preferably 10.5 or more, and particularly preferably 11 or more.
[0041] Further, a method for producing the positive electrode active material for a lithium ion secondary battery coated with the lithium niobate solution of the present invention described above will be described below.
[0042] The method for producing a positive electrode active material for a lithium ion secondary battery coated with a lithium niobate solution is characterized by comprising the steps of: mixing a lithium niobate solution, a positive electrode active material, and an aqueous lithium hydroxide solution to produce a positive electrode active material slurry for a battery containing lithium niobate; and drying the positive electrode active material slurry for a battery containing lithium niobate.
[0043] First, a battery positive electrode active material, for example, LiMn2O4 (manufactured by Merck: spinel type, particle size <0.5 μm) is added to a lithium niobate aqueous solution obtained by diluting the lithium niobate solution of the present invention with pure water, to obtain a slurry containing lithium niobate. Then, while stirring the slurry containing lithium niobate, a lithium hydroxide aqueous solution is dropped and the slurry is kept at 90° C. for 10 minutes, to produce a battery positive electrode active material slurry containing lithium niobate.
[0044] In addition to the above-mentioned LiMn2O4, other examples of the positive electrode active material for batteries include LiCoO2, LiNiO2, LiFeO2, Li2MnO3, LiFePO4, LiCoPO4, LiNiPO4, LiMnPO4, and LiNi 0.5 Mn 1.5 O4, LiMn 1 / 3 Co 1 / 3 Ni 1 / 3 O2, LiCo 0.2 Ni 0.4 Mn 0.4 O2, Lithium Molybdate, LiMnO4, LiNi 0.8 Co 0.15 Al0.05 O2, LiMnO2 can be used.
[0045] Next, the battery positive electrode active material slurry containing lithium niobate is dried in an atmospheric drying furnace for 15 hours while maintaining the furnace temperature at 110°C, thereby producing a lithium ion secondary battery positive electrode active material coated with lithium niobate.
[0046] In the above-mentioned method for producing a positive electrode active material for a lithium ion secondary battery, the positive electrode active material for a battery is added, but it may be changed according to the application. For example, a dispersant, a pH adjuster, a colorant, a thickener, a wetting agent, a binder resin, etc. may be added. Effect of the Invention
[0047] The lithium niobate solution of the present invention has high dispersibility in water, good solubility in water, and excellent storage stability. BEST MODE FOR CARRYING OUT THEINVENTION
[0048] The lithium niobate solution according to the embodiment of the present invention will be further described below with reference to the following examples, although the present invention is not limited to these examples.
[0049] Example 1 100g of niobium pentoxide was dissolved in 200g of 55% hydrofluoric acid solution, and 830mL of ion-exchanged water was added to obtain a niobium fluoride aqueous solution containing 100g / L of niobium in terms of Nb2O5 (Nb2O5=8.84 mass%). 200mL of this niobium fluoride aqueous solution was added to 1L of ammonia water (NH3 concentration 25 mass%) in less than 1 minute (NH3 / Nb2O5 molar ratio=177.9, NH3 / HF molar ratio=12.2) to obtain a reaction liquid (pH11). This reaction liquid was a slurry of niobium acid compound hydrate, in other words, a slurry of niobium-containing precipitate.
[0050] Next, the reaction solution was decanted using a centrifuge and washed until the amount of liberated fluoride ions was 100 mg / L or less, to obtain a niobium-containing precipitate from which the fluoride ions had been removed. At this time, ammonia water was used as the washing liquid.
[0051] The niobium-containing precipitate from which the fluoride ions had been removed was then diluted with pure water to obtain a slurry. A portion of this slurry was dried at 110°C for 24 hours and then calcined at 1,000°C for 4 hours to produce Nb2O5, and the Nb2O5 concentration in the slurry was calculated from its weight.
[0052] Then, the slurry of the niobium-containing precipitate diluted with pure water was mixed with lithium hydroxide monohydrate and pure water so that the niobium concentration of the final mixture was 1 mass% in terms of Nb2O5 and the molar ratio of Li / Nb was 1, thereby obtaining a translucent slurry mixture. This mixture was stirred and held for 1 hour so that the liquid temperature was 50°C to 100°C, for example 70°C, and then a colorless and transparent lithium niobate aqueous solution according to Example 1 was obtained. The pH of the obtained lithium niobate aqueous solution according to Example 1 was 11.
[0053] Example 2 In Example 2, the same manufacturing method as in Example 1 was carried out, except that the niobium concentration of the translucent slurry mixture was 5 mass% in terms of Nb2O5, to obtain a colorless and transparent lithium niobate aqueous solution according to Example 2. The pH of the obtained lithium niobate aqueous solution according to Example 2 was 11.
[0054] Example 3 In Example 3, the same manufacturing method as in Example 1 was carried out, except that the niobium concentration of the translucent slurry mixture was 10 mass% in terms of Nb2O5, to obtain a colorless and transparent lithium niobate aqueous solution according to Example 3. The pH of the obtained lithium niobate aqueous solution according to Example 3 was 11.
[0055] Example 4 In Example 4, the same manufacturing method as in Example 1 was carried out, except that the niobium concentration of the translucent slurry mixture was 20 mass% in terms of Nb2O5, to obtain a colorless and transparent lithium niobate aqueous solution according to Example 4. The pH of the obtained lithium niobate aqueous solution according to Example 4 was 11.
[0056] Example 5 In Example 5, a colorless and transparent lithium niobate aqueous solution according to Example 5 was obtained by carrying out the same manufacturing method as in Example 1, except that the niobium concentration of the translucent slurry mixture was 10 mass% calculated as Nb2O5 and the molar ratio of Li / Nb was 2. The pH of the obtained lithium niobate aqueous solution according to Example 5 was 11.
[0057] Example 6 In Example 6, the same manufacturing method as in Example 1 was carried out, except that the niobium concentration of the translucent slurry mixture was 10 mass% in terms of Nb2O5 and the molar ratio of Li / Nb was 0.9, to obtain a colorless and transparent lithium niobate aqueous solution according to Example 6. The pH of the obtained lithium niobate aqueous solution according to Example 6 was 11.
[0058] Example 7 In Example 7, the translucent slurry mixture obtained in Example 1 was heated to 70°C in a water bath, held for 2 hours while stirring, and then cooled to room temperature. Pure water was added to replenish the moisture evaporated by this heating, and the concentration was adjusted so that the niobium concentration of the colorless and transparent slurry mixture was 5 mass% in terms of Nb2O5, thereby obtaining a colorless and transparent lithium niobate aqueous solution according to Example 7. The pH of the obtained lithium niobate aqueous solution according to Example 7 was 11.
[0059] Example 8 In Example 8, the translucent slurry mixture obtained in Example 1 was heated to 70°C in a water bath, held for 6 hours while stirring, and then cooled to room temperature. Pure water was added to replenish the moisture evaporated by this heating, and the concentration of niobium in the colorless and transparent slurry mixture was adjusted to 5 mass% in terms of Nb2O5, thereby obtaining a colorless and transparent lithium niobate aqueous solution according to Example 8. The pH of the obtained lithium niobate aqueous solution according to Example 8 was 11.
[0060] Example 9 In Example 9, the translucent slurry mixture obtained in Example 1 was heated to 70°C in a water bath, held for 25 hours while stirring, and then cooled to room temperature. Pure water was added to replenish the moisture evaporated by this heating, and the concentration of niobium in the colorless and transparent slurry mixture was adjusted to 5 mass% in terms of Nb2O5, thereby obtaining a colorless and transparent lithium niobate aqueous solution according to Example 9. The pH of the obtained lithium niobate aqueous solution according to Example 9 was 11.
[0061] Example 10 In Example 10, the same manufacturing method as in Example 1 was carried out, except that when the slurry of the niobium-containing precipitate according to Example 1 was mixed with lithium hydroxide monohydrate and pure water, a part of the pure water was replaced with ammonia water (NH3 concentration 25 mass%) so that the niobium concentration of the semi-transparent slurry mixture was 5 mass% in terms of Nb2O5 and 5.5 mass% in terms of NH3, to obtain a colorless and transparent lithium niobate aqueous solution according to Example 10. The pH of the obtained lithium niobate aqueous solution according to Example 10 was 11.
[0062] Example 11 In Example 11, the same manufacturing method as in Example 1 was carried out, except that when the slurry of the niobium-containing precipitate according to Example 1 was mixed with lithium hydroxide monohydrate and pure water so that the niobium concentration of the semi-transparent slurry mixture was 5 mass% in terms of Nb2O5 and the NH3 concentration was 10 mass%, a part of the pure water was replaced with ammonia water (NH3 concentration 25 mass%), and a colorless and transparent lithium niobate aqueous solution according to Example 11 was obtained. The pH of the obtained lithium niobate aqueous solution according to Example 11 was 11.
[0063] Example 12 In Example 12, the translucent slurry mixture obtained in Example 1 was heated to 70°C in a water bath, held for 6 hours while stirring, and then cooled to room temperature. In order to replenish the moisture evaporated by this heating, pure water was added, and the concentration was adjusted so that the niobium concentration of the colorless and transparent slurry mixture was 10 mass% in terms of Nb2O5, thereby obtaining a colorless and transparent lithium niobate aqueous solution according to Example 12. The pH of the obtained lithium niobate aqueous solution according to Example 12 was 11.
[0064] Example 13 In Example 13, the same manufacturing method as in Example 1 was carried out, except that when the slurry of the niobium-containing precipitate according to Example 1 was mixed with lithium hydroxide monohydrate and pure water, a part of the pure water was replaced with ammonia water (NH3 concentration 25 mass%) so that the niobium concentration of the semi-transparent slurry mixture was 10 mass% in terms of Nb2O5 and 8.2 mass% in terms of NH3, to obtain a colorless and transparent lithium niobate aqueous solution according to Example 13. The pH of the obtained lithium niobate aqueous solution according to Example 13 was 11.
[0065] Comparative Example 1 In Comparative Example 1, 35% hydrogen peroxide solution was added to the colorless and transparent lithium niobate aqueous solution according to Example 1 so that the molar ratio of H2O2 / Nb was 0.3, thereby obtaining a lithium niobate aqueous solution according to Comparative Example 1. The pH of the obtained lithium niobate aqueous solution according to Comparative Example 1 was 11.
[0066] Comparative Example 2 In Comparative Example 2, 35% hydrogen peroxide water was added to the colorless and transparent lithium niobate aqueous solution according to Example 1 so that the molar ratio of H2O2 / Nb was 1, thereby obtaining a lithium niobate aqueous solution according to Comparative Example 2. The pH of the obtained lithium niobate aqueous solution according to Comparative Example 2 was 8.
[0067] Comparative Example 3 In Comparative Example 3, the above-mentioned niobium fluoride aqueous solution was slowly added to 500 mL of 1% lithium hydroxide aqueous solution to obtain a microparticle dispersion having an Nb2O5 content of 5 mass% and a Li / Nb molar ratio of 1. Then, this microparticle dispersion was filtered and washed using an ultrafiltration device until the amount of liberated fluoride ions reached 100 mg / L, thereby obtaining a lithium niobate sol according to Comparative Example 3. The pH of the obtained lithium niobate sol according to Comparative Example 3 was 8.6.
[0068] Comparative Example 4 In Comparative Example 4, the translucent slurry mixture obtained in Example 1 was heated to 70°C in a water bath, held for 73 hours while stirring, and then cooled to room temperature. It was confirmed that a precipitate was generated by heating for 73 hours. In order to replenish the moisture evaporated by this heating, pure water was added, and the concentration was adjusted so that the niobium concentration of the slurry mixture was 5 mass% in terms of Nb2O5, thereby obtaining a lithium niobate aqueous solution according to Comparative Example 4. The pH of the obtained lithium niobate aqueous solution according to Comparative Example 4 was 11.
[0069] The following physical properties were measured for the lithium niobate aqueous solutions obtained in Examples 1 to 13 and Comparative Examples 1, 2, and 4, and the lithium niobate sol of Comparative Example 3. The measured physical property values and the measurement methods for the physical property values are shown below, and the measurement results are shown in Table 1.
[0070] <Elemental analysis> If necessary, the sample was appropriately diluted with dilute hydrochloric acid, and the Nb weight fraction and Li weight fraction calculated as Nb2O5 were measured using ICP emission spectrometry (Agilent Technologies: AG-5110) in accordance with JIS K0116:2014.
[0071] Quantitative analysis of ammonia 25 ml of sodium hydroxide solution (30 g / 100 ml) was added to 1 to 5 ml of the sample solution, and the mixture was boiled and distilled. The distillate (about 200 ml) was poured into a container containing 20 ml of pure water and 0.5 ml of sulfuric acid to separate ammonia. Next, the separated ammonia was transferred to a 250 ml measuring flask and the volume was adjusted to 250 ml with pure water. Furthermore, 10 ml of the solution adjusted to 250 ml was taken into a 100 ml measuring flask, 1 ml of sodium hydroxide solution (30 g / 100 mL) was added to the taken solution, and the volume was adjusted to 100 ml with pure water. The solution thus obtained was quantitatively analyzed using an ion meter (main unit: HORITA F-53, electrode: HORIBA 500 2A) to measure the ammonium ion concentration (mass%) contained in the solution.
[0072] <Qualitative analysis of hydrogen peroxide> The UV-visible absorbance spectra of a standard solution with no added hydrogen peroxide and a standard solution with added hydrogen peroxide to a concentration of 1% by mass calculated as H2O2 were measured, and the wavelength at which the rate of change in absorbance was greatest was designated "λ." Next, the absorbance at wavelength λ was similarly measured for a sample with an unknown hydrogen peroxide concentration, and if the ratio of the absorbance at wavelength λ of the sample with an unknown hydrogen peroxide concentration to the absorbance at wavelength λ of the standard solution with no added hydrogen peroxide was 1% or less, it was determined that no hydrogen peroxide was added to the sample.
[0073] The conditions for measuring the ultraviolet-visible absorption spectrum may be as follows. Equipment: UH4150 spectrophotometer (Hitachi High-Tech Science Corporation) Measurement mode: Wavelength scan Data mode: %T (transparent) Measurement wavelength range: 200~2,600nm Scan speed: 600nm / min Sampling interval: 2nm
[0074] Dynamic Light Scattering The particle size distribution was evaluated using a zeta potential, particle size, and molecular weight measurement system (Otsuka Electronics Co., Ltd.: ELSZ-2000) in accordance with JIS Z 8828:2019 "Particle size analysis - dynamic light scattering method". In addition, in order to remove dust and other particles in the solution to be measured immediately before the measurement, the solution was filtered with a filter with a pore size of 2 μm, and ultrasonic treatment was performed for 3 minutes at 28 kHz using an ultrasonic cleaner (As One Co., Ltd.: VS-100III). The particle size (D50) refers to the median size (D50), which is the particle size that shows the 50% cumulative value of the cumulative distribution curve. The "initial particle size D50 (nm)" in Table 1 refers to the lithium niobate particle size (D50) in the lithium niobate aqueous solution immediately after it is generated. In addition, "particle diameter over time D50 (nm)" in Table 1 refers to the lithium niobate particle diameter (D50) in the lithium niobate aqueous solution after being left to stand for one month in an incubator set at room temperature of 25°C.
[0075] <Stability test over time> The lithium niobate aqueous solutions of Examples 1 to 13 and Comparative Examples 1, 2, and 4, and the lithium niobate sol of Comparative Example 3 were left to stand for one month in an incubator set at room temperature 25°C, and then the presence or absence of white precipitation and gelation was visually observed. Those in which no white precipitation or gelation was observed were evaluated as having temporal stability and were marked with "○", and those in which even one white precipitation or gelation was observed were evaluated as not having temporal stability and were marked with "×". Here, gelation was judged by putting each tantalic acid compound dispersion into a plastic container, and when the container was turned upside down, the dispersion that did not fall quickly was judged to have gelled. In addition, the particle diameter (D50) of lithium niobate over time in the lithium niobate aqueous solutions of Examples 1 to 13 and Comparative Examples 1, 2, and 4, and in the lithium niobate sol of Comparative Example 3 after standing for one month was measured using the dynamic light scattering method described above.
[0076] <Film-forming test> The appearance of the coating film formed on the surface of the glass substrate, which is a substitute for the current collector, was evaluated by observing it with an optical microscope. The lithium niobate aqueous solutions of Examples 1 to 13 and Comparative Examples 1, 2, and 4, and the lithium niobate sol of Comparative Example 3 were dropped onto a 50 mm x 50 mm glass substrate that had been degreased and washed with acetone and dried using a syringe while being filtered through a filter with a pore size of 2 μm, and then coated by spin coating (1,500 rpm, 15 seconds). The coated area was then naturally dried to form a coating film on the glass substrate. The glass substrate was observed with an optical microscope (magnification: 40 times) in a central area of 15 mm x 15 mm of the coating film formed. When no bubbles, uneven coating, or cracks were observed, the glass substrate was evaluated as having excellent film-forming properties and was evaluated as "○", and when even one was observed, the glass substrate was evaluated as not having excellent film-forming properties and was evaluated as "×".
[0077] <Safety Testing> The lithium niobate aqueous solutions of Examples 1 to 13, Comparative Examples 1, 2, and 4, and the lithium niobate sol of Comparative Example 3 were added to a positive electrode active material, and the presence or absence of foaming was visually observed and evaluated. The lithium niobate aqueous solutions of Examples 1 to 13, Comparative Examples 1, 2, and 4, and 50 mL of the lithium niobate sol of Comparative Example 3 were all mixed together with 5 g of lithium manganate, which is a positive electrode active material, in a test container, and the presence or absence of foaming was visually observed. Those in which no foaming was observed were evaluated as safe and were marked with "○", and those in which even one foaming was observed were evaluated as unsafe and were marked with "×".
[0078] <Method for producing positive electrode active material> The coating observation was performed and the coating amount was measured for the positive electrode active materials coated with the lithium niobate aqueous solutions of Examples 1 to 13 and Comparative Examples 1, 2, and 4, and the lithium niobate sol of Comparative Example 3. The positive electrode active materials subjected to the coating observation and coating amount measurement were produced by the following production procedure.
[0079] The lithium niobate aqueous solution after standing at room temperature 25°C for one month was diluted with pure water so that the niobium concentration was 2.3 mass% in terms of Nb2O5. If the niobium concentration in the lithium niobate aqueous solution after standing for one month was less than 2.3 mass% in terms of Nb2O5, dilution was not performed. A positive electrode active material (lithium manganate) was added to the diluted lithium niobate aqueous solution so that the weight ratio of niobium / lithium manganate was 2 / 100, thereby obtaining a positive electrode active material slurry containing lithium niobate. Next, while stirring the obtained positive electrode active material slurry containing lithium niobate, 0.4 mol / L of lithium hydroxide aqueous solution was dropped so that the final molar ratio of Li / Nb was 2, and the mixture was stirred for 10 minutes while maintaining the liquid temperature at 90°C. The obtained positive electrode active material slurry containing lithium niobate was then dried in an atmospheric drying oven at 110° C. for 15 hours to obtain a positive electrode active material coated with lithium niobate.
[0080] <Coating Observation> The coating state of the particle surface of the positive electrode active material coated with lithium niobate was evaluated by observing it with a scanning electron microscope (SEM). Using a scanning electron microscope (SEM), five SEM images (20 μm × 20 μm) were observed at a magnification of 50,000 times under the condition of an acceleration voltage of 1 kV, and the coating state of the particle surface of the positive electrode active material was observed. Under the above observation conditions, the particle surface was evaluated as "○" when not even one uncoated area was observed within 1 μm square, and evaluated as "×" when even one uncoated area was observed.
[0081] <Measurement of coating amount> A suitable amount of hydrofluoric acid was added to the positive electrode active material coated with lithium niobate to obtain a solution in which the lithium niobate coating the surface of the positive electrode active material was dissolved.Then, the niobium weight fraction concentration in the solution in which the lithium niobate coating the surface of the positive electrode active material was dissolved was measured and calculated using ICP emission spectrometry (manufactured by Agilent Technologies: AG-5110) in accordance with JIS K0116:2014.
[0082] [Table 1]
[0083] As shown in Table 1, the lithium niobate aqueous solutions of Examples 1 to 13 had a lithium to niobium molar ratio Li / Nb of 0.8 or more and 2.0 or less, and the lithium niobate particle size (D50) in the aqueous solution was 100 nm or less as measured by dynamic light scattering, and all of the results of the stability over time test, film-forming test, and safety test were good.
[0084] The lithium niobate aqueous solutions according to Examples 1 to 13 did not contain hydrogen peroxide, but even after one month had passed, the particle size (D50) of lithium niobate over time was not significantly different from the initial particle size (D50), and the solution had excellent stability over time. The initial particle size (D50) and the particle size (D50) over time of lithium niobate in the lithium niobate aqueous solution according to Comparative Example 2 could not be measured due to gelation. In addition, it was confirmed that a precipitate was generated in the lithium niobate aqueous solution according to Comparative Example 4, and the initial particle size (D50) and the particle size (D50) over time of lithium niobate were not measured.
[0085] The lithium niobate aqueous solutions according to Examples 1 to 13 had improved stability during long-term storage when the lithium niobate concentration in the aqueous solutions was 0.1 to 30% by mass.
[0086] The positive electrode active materials coated with the lithium niobate aqueous solution according to Examples 1 to 13 were confirmed to be completely coated with the lithium niobate as a result of observing the coated state of the particle surface with an SEM. The niobium weight fraction concentration of the lithium niobate coating the surface of the positive electrode active materials was 1.0 mass% or more. On the other hand, the niobium weight fraction concentration of the lithium niobate coating the surface of the positive electrode active material coated with the lithium niobate aqueous solution according to Comparative Example 1 was 1.0 mass%, but as a result of observing the coated state of the particle surface with an SEM, uncoated portions were observed.
[0087] The inventions disclosed in this specification include, in addition to the configurations of each invention or embodiment, those that are specified by changing these partial configurations to other configurations disclosed in this specification, to the extent applicable, or those that are specified by adding other configurations disclosed in this specification to these configurations, or those that are specified as higher-level concepts by deleting these partial configurations to the extent that partial action and effects are obtained. [Industrial Applicability]
[0088] The lithium niobate aqueous solution according to the present invention has high dispersibility in water, good solubility in water, and excellent storage stability, and is therefore suitable for coating the positive electrode active material of a lithium ion secondary battery.
Claims
1. A lithium niobate solution containing lithium niobate having a lithium to niobium molar ratio Li / Nb of 0.8 to 2.0, and ammonium ions, The lithium niobate solution is characterized in that the lithium niobate particle diameter (D50) in the lithium niobate solution is 100 nm or less as measured by a dynamic light scattering method.
2. The lithium niobate solution described in claim 1, characterized in that the lithium niobate solution is filtered through a filter having a pore size of 2 μm, dropped onto a glass substrate (50 mm x 50 mm), and applied onto the glass substrate using spin coating (1,500 pm, 15 seconds), and when observed with an optical microscope (magnification: 40x), no air bubbles, uneven coating, or cracks are observed within the center (15 mm x 15 mm) of the coating film formed on the glass substrate.
3. The lithium niobate solution according to claim 1 or 2, further characterized in that it contains at least one selected from Na, Mg, Si, K, Ca, Ti, Mn, Ni, Zn, Sr, Zr, Ta, Mo, Ba and W.
4. A lithium niobate solution as described in claim 2 or 3, characterized in that the pH of the lithium niobate solution is 9 or higher.
5. 5. The lithium niobate solution according to claim 1, wherein the lithium niobate solution does not contain hydrogen peroxide.
6. The lithium niobate solution according to any one of claims 1 to 5, characterized in that the lithium niobate solution is an aqueous solution.
7. 7. The lithium niobate solution according to claim 1, wherein the lithium niobate solution has a concentration of 0.1 to 30 mass %.
8. A positive electrode active material for a lithium ion secondary battery, the surface of which is coated with the lithium niobate contained in the lithium niobate solution according to any one of claims 1 to 7.
9. A lithium ion secondary battery comprising a positive electrode coated with the positive electrode active material for lithium ion secondary batteries according to claim 8.
Citation Information
Patent Citations
Ammonium niobate sol, method for producing the same, coating liquid for forming thin film and thin film-supporting substrate
JP2011190115A
Solution containing lithium and niobium complex, and method of producing the same
JP2014210701A
Solution containing lithium and niobium complex, method for producing the same, and lithium ion battery
JP2015103321A
Solution and manufacturing method therefor, and manufacturing method of active material for secondary battery
JP2018002581A