Lithium nickel manganese composite oxide materials, secondary batteries and power consumption devices

Lithium nickel manganese composite oxides with controlled K values and coatings enhance secondary battery performance by improving cycle life, reducing ion loss, and minimizing gas generation, addressing the challenges of energy density and safety in secondary batteries.

JP7588208B2Active Publication Date: 2024-11-21CONTEMPORARY AMPEREX TECHNOLOGY (HONG KONG) LIMITED
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023501335
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-10-27
Publication Date
2024-11-21
Estimated Expiration
2041-10-27

AI Technical Summary

Technical Problem

Secondary batteries face challenges in achieving high energy density, cycle performance, safety performance, and ion elution, particularly in applications requiring high energy storage and power consumption.

Method used

The use of lithium nickel manganese composite oxide materials with a specific K value of 1 to 2, characterized by controlled volume median crystallite and particle sizes, and optionally coated with a fast lithium ion conductor layer, enhances the performance of secondary batteries by improving cycle performance, reducing ion elution, and minimizing gas generation.

Benefits of technology

The lithium nickel manganese composite oxide materials exhibit improved cycle performance, reduced ion elution, and decreased gas generation, making them suitable for high-energy density applications in secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588208000017
    Figure 0007588208000017
  • Figure 0007588208000018
    Figure 0007588208000018
  • Figure 0007588208000019
    Figure 0007588208000019
Patent Text Reader

Abstract

The present application provides a lithium nickel manganese composite oxide material, which has a K value of 1 to 2, and is calculated by the following formula: K=D v 50 / d v 50. where d v 50 is the volume median diameter of the crystal grains in the lithium nickel manganese composite oxide material, and D v 50 is the volume median particle size of the lithium nickel manganese composite oxide material.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to the field of secondary battery technology, in particular to lithium nickel manganese composite oxide materials, secondary batteries and power consuming devices. [Background technology]

[0002] 2. Description of the Related Art In recent years, secondary batteries have been widely used in energy storage power systems such as hydroelectric, thermal, wind and solar power plants, as well as in many fields such as power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, and aerospace.

[0003] As secondary batteries have undergone great development, higher requirements are being placed on their energy density, cycle performance, safety performance, and the like. Summary of the Invention

[0004] The present application relates to a cathode active material for a secondary battery (e.g., a lithium ion battery), which is capable of improving one or more performances of the battery, e.g., i) Improved cycle performance; ii) reduction of ionic leaching; The present invention aims to provide a lithium nickel manganese composite oxide material that can exhibit improved performance selected from the above.

[0005] In order to achieve the above object, the present application provides a lithium nickel-manganese-based composite oxide material. The lithium nickel-manganese composite oxide material has a K value of 1 to 2 (e.g., 1-1.1, 1.1-1.2, 1.2-1.3, 1.3-1.4, 1.4-1.5, 1.5-1.6, 1.6-1.7, 1.7-1.8, 1.8-1.9, 1.9-2), and the K value is calculated by the following formula: K=D v 50 / d v 50. Here, d vD 50 is the volume median crystallite diameter of the crystal grains of the lithium nickel manganese composite oxide material, v 50 is the volume median particle diameter of the lithium nickel manganese composite oxide material.

[0006] As a result, the present application provides a method for adjusting the K value of a lithium nickel manganese composite oxide material to within a range of 1 to 2, and thereby, when the lithium nickel manganese composite oxide material is used as a positive electrode active material for a secondary battery (e.g., a lithium ion battery), the battery exhibits one or more improved performances, for example i) Improved cycle performance; ii) reduction of ionic leaching; iii) reduced gassing.

[0007] In any embodiment, the volume median diameter d of the crystal grains of the lithium nickel manganese composite oxide material v 50 is 5 μm to 15 μm, optionally 5.5 μm to 11 μm. When used as a positive electrode active material in a secondary battery (eg, a lithium ion battery), this lithium nickel manganese composite oxide material exhibits improved performance of one or more batteries.

[0008] In any embodiment, the lithium nickel manganese composite oxide material has a volume median particle size D v 50 is 9 μm to 20 μm, optionally 9 μm to 11 μm. When used as a positive electrode active material in a secondary battery (eg, a lithium ion battery), this lithium nickel manganese composite oxide material exhibits improved performance of one or more batteries.

[0009] In any embodiment, the lithium nickel manganese composite oxide material includes a lithium nickel manganese composite oxide having a P4332 space group and a lithium nickel manganese composite oxide having an Fd-3m space group, and the content of the lithium nickel manganese composite oxide having the P4332 space group is greater than the content of the lithium nickel manganese composite oxide having the Fd-3m space group.

[0010] In any embodiment, the lithium nickel manganese composite oxide having the P4332 space group accounts for 50% or more, optionally 80% to 91%, by weight of the lithium nickel manganese composite oxide material.

[0011] In an optional embodiment, the lithium nickel manganese composite oxide material comprises Mn 3+ The lithium nickel manganese composite oxide material contains Mn 3+ The weight content of is less than 5 wt%, optionally between 1.0 wt% and 2.2 wt%.

[0012] In any embodiment, the specific surface area of ​​the lithium nickel manganese composite oxide material is 1 m 2 / g or less, selectively, 0.1m 2 / g~0.9m 2 / g.

[0013] In an optional embodiment, the lithium nickel manganese composite oxide material has a tap density of 1.9 g / cm 3 Above, optionally, 1.9 g / cm 3 ~3.0g / cm 3 It is.

[0014] In an optional embodiment, the lithium nickel manganese composite oxide material includes lithium nickel manganese composite oxide particles having a coating layer provided on at least a portion of the surface thereof, Optionally, the material of the coating layer includes at least one of aluminum oxide, titanium oxide, zirconium oxide, boron oxide, rare earth oxide, lithium salt, phosphate, borate, and fluoride; Optionally, the coating layer includes a high rate lithium ion conductor layer; Optionally, the coating layer has a multi-layer structure, and the coating layer includes an inner high-rate lithium ion conductor layer and an outer aluminum oxide layer.

[0015] In an optional embodiment, the high rate lithium ion conductor is selected from oxide-, phosphate-, borate-, sulfide-, and LiPON-based inorganic materials that have lithium ion conductivity.

[0016] In an optional embodiment, the high rate lithium ion conductor contains one or more of the elements phosphorous, titanium, zirconium, boron, and lithium.

[0017] In an optional embodiment, the high rate lithium ion conductor is selected from Li2BO3, Li3PO4, or combinations thereof.

[0018] In an optional embodiment, the general formula of the lithium nickel manganese composite oxide is as shown in Formula I:

number

[0019] According to a second aspect of the present application, there is provided a method for producing a lithium nickel manganese composite oxide, the method comprising the steps of: providing a precursor composition containing a lithium source, a nickel source, and a manganese source; and sintering the precursor composition to obtain a lithium nickel manganese composite oxide. The K value of the lithium nickel manganese composite oxide material is 1 to 2, and the K value is calculated according to the following formula:

number

[0020] In an optional embodiment, the general formula of the lithium nickel manganese composite oxide is as shown in Formula I:

number

[0021] In an optional embodiment, the method further comprises: i. the ratio of the volume median particle diameters of the nickel source and the lithium nickel manganese composite oxide material is 0.4 to 1; ii. the ratio of the volume median particle diameters of the manganese source and the lithium nickel manganese composite oxide material is 0.4 to 1; and iii. the volume median particle diameter of the lithium source is 1 to 20 μm (eg, 3 to 10 μm).

[0022] In an optional embodiment, the sintering comprises a first heat treatment step: The peak temperature in the first heat treatment step is 950° C. to 1200° C., and the heat retention time at the peak temperature in the first heat treatment step is 5 hours to 30 hours.

[0023] In any embodiment, the rate of temperature rise to the peak temperature of the first heat treatment is 5° C. / min or less, optionally 0.5 to 3° C. / min.

[0024] In an optional embodiment, the sintering further comprises a second heat treatment step after the first heat treatment step; The peak temperature of the second heat treatment step is 550° C. to 680° C., and the time of the second heat treatment step is 5 h to 50 h.

[0025] In an optional embodiment, the method further comprises ball milling the precursor composition prior to sintering; Optionally, the ball milling time is 2 h or more, for example, optionally 2 to 6 h.

[0026] According to a third aspect of the present application, there is provided a secondary battery, the secondary battery including a positive electrode plate, the positive electrode plate including a positive electrode active material, the positive electrode active material including the lithium nickel manganese composite oxide material according to any one of the first aspect of the present application or the lithium nickel manganese composite oxide produced by the method according to any one of the second aspect of the present application.

[0027] According to a fourth aspect of the present application, there is provided a power consuming device including the secondary battery of the third aspect of the present application. [Brief description of the drawings]

[0028] [Figure 1] 2 is a scanning electron microscope photograph of the lithium nickel manganese composite oxide material of Example 2a. [Diagram 2] 1 is a scanning electron microscope photograph of the lithium nickel manganese composite oxide material of Example 2b. [Diagram 3]1 is a scanning electron microscope photograph of the lithium nickel manganese composite oxide material of Example 2c. [Figure 4] 1 is a scanning electron microscope photograph of the lithium nickel manganese composite oxide material of Example 3b. [Diagram 5] 2 is a scanning electron microscope photograph of the lithium nickel manganese composite oxide material of Comparative Example 1. [Figure 6] 3 is a scanning electron microscope photograph of the lithium nickel manganese composite oxide material of Comparative Example 2. [Figure 7] 1 is a scanning electron microscope photograph of the lithium nickel manganese composite oxide material of Comparative Example 3. [Figure 8] 1 is a schematic diagram of a secondary battery according to an embodiment of the present application; [Figure 9] FIG. 1 is an exploded view of a secondary battery according to an embodiment of the present application. [Figure 10] 1 is a schematic diagram of a power consuming device in which a secondary battery according to an embodiment of the present application is used as a power source; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] Hereinafter, the present application will be described in detail with reference to the accompanying drawings. However, unnecessary detailed description may be omitted. For example, detailed description of well-known matters and duplicated description of structures that are actually the same may be omitted. This is to avoid the following description from becoming unnecessarily long and to allow those skilled in the art to easily understand. Note that the accompanying drawings and the following description are provided to allow those skilled in the art to fully understand the present application, and are not intended to limit the subject matter described in the claims.

[0030] The "ranges" disclosed herein are defined in the form of lower and upper limits, and a given range is defined by selecting one lower limit and one upper limit that define the boundaries of the particular range. Such defined ranges may or may not include the end values, and may be arbitrarily combined, i.e., any lower limit and any upper limit may be combined to form a range. For example, if ranges of 60-120 and 80-110 are listed for a particular parameter, it is conceivable that they are understood as ranges of 60-110 and 80-120. It is to be noted that if the minimum range values ​​listed are 1 and 2, and the maximum range values ​​listed are 3, 4, and 5, then all of the ranges of 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5 are conceivable. In this application, unless otherwise specified, the numerical range "a-b" is a shorthand expression representing any combination of real numbers between a and b, where a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed herein, and "0-5" is merely a shorthand for combinations of these numbers. Also, when a parameter is described as an integer ≧2, this is equivalent to disclosing that the parameter is, for example, the integers 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0031] Unless otherwise stated, all the embodiments and optional embodiments of the present application may be combined with each other to form a new technical solution.

[0032] Unless otherwise stated, all technical features and optional technical features in the present application may be combined with each other to form a new technical solution.

[0033] Unless otherwise stated, all steps in the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b) to mean that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method further includes step (c) as mentioned above to mean that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0034] Unless otherwise specified, the terms "comprise" and "comprises" referred to in this application may be open ended or closed ended. For example, the terms "comprise" and "comprises" may further include or include other ingredients not listed, or may include or include only the listed ingredients.

[0035] In this application, unless otherwise stated, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, any of the following conditions satisfy "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) but B is true (or exists); and A and B are both true (or exist).

[0036] [Secondary battery] A secondary battery is also called a rechargeable battery or a storage battery, and is a battery that can be used continuously after being discharged by activating the active material through a charging method.

[0037] A secondary battery generally includes a positive electrode plate, a negative electrode plate, a separator, and an electrolyte. During the charge and discharge process of the battery, active ions (e.g., lithium ions) shuttle between the positive electrode plate and the negative electrode plate to be absorbed and released. The separator is provided between the positive electrode plate and the negative electrode plate, and mainly serves to prevent short-circuiting between the positive and negative electrodes, while also allowing the active ions to pass through. The electrolyte mainly serves to conduct the active ions between the positive electrode plate and the negative electrode plate.

[0038] [Positive electrode plate] The positive electrode plate generally includes a positive electrode current collector and a positive electrode film layer provided on at least one surface of the positive electrode current collector, and the positive electrode film layer includes a positive electrode active material.

[0039] The positive electrode current collector has two surfaces opposing each other in the thickness direction of the positive electrode current collector, and the positive electrode film layer is provided on either one or both of the two opposing surfaces of the positive electrode current collector.

[0040] The positive electrode active material of the present invention includes a lithium nickel-manganese-based composite oxide material, and the K value of the lithium nickel-manganese composite oxide material is 1 to 2 (for example, 1-1.1, 1.1-1.2, 1.2-1.3, 1.3-1.4, 1.4-1.5, 1.5-1.6, 1.6-1.7, 1.7-1.8, 1.8-1.9, 1.9-2), and the K value is calculated by the following formula: K=D v 50 / d v 50, where d v D 50 is the volume median crystallite diameter of the crystal grains of the lithium nickel manganese composite oxide material, v 50 is the volume median particle diameter of the lithium nickel manganese composite oxide material.

[0041] Although the mechanism is unclear, the applicant believes that by adjusting the K value of the lithium nickel manganese composite oxide material to within the range of 1 to 2, when the lithium nickel manganese composite oxide material is used as a positive electrode active material for a secondary battery (e.g., a lithium ion battery), the battery exhibits one or more improved performances, for example i) Improved cycle performance; ii) reduction of ionic leaching; iii) reduced gassing.

[0042] The term "crystal grain" refers to the largest area in a material where atoms are regularly arranged repeatedly (a small amount of atomic-level point defects or line defects are allowed). The arrangement of atoms at the interface between adjacent crystal grains is different from the arrangement of atoms within the crystal grain. At the interface between adjacent crystal grains, atoms penetrate the contact surface (grain boundary) between the crystal grains continuously like a thin layer. For example, in the field of view of a scanning electron microscope, each nano- or micron-level area separated by a clear interface inside the particle is each crystal grain. Here, the approximate diameter of the crystal grain is called the grain size of the crystal grain. The morphology of the crystal grain can be observed with a scanning electron microscope.

[0043] The lithium nickel manganese composite oxide material contains a plurality of crystal grains (e.g., single crystal grains, polycrystalline grains). A single crystal grain is composed of one crystal grain. A polycrystalline grain is composed of a plurality of crystal grains, and grain boundaries exist between adjacent crystal grains.

[0044] The term "specific surface area" (also called BET specific surface area) is obtained by measuring the specific surface area of ​​a solid material with reference to GB / T 19587-2004 gas adsorption BET method.

[0045] The term "volume median particle size D v 50" was measured with reference to GB / T 19077-2016 Particle Size Analysis Laser Diffraction Method. The test equipment used was a Mastersizer 3000 laser granulometer.

[0046] The term "grain volume median diameter" was obtained by the following method: A lithium nickel manganese composite oxide material was observed using a scanning electron microscope (e.g., a Zeiss Sigma 300 field emission scanning electron microscope), and five regions were randomly selected during the photograph (or from the photograph), and the maximum grain diameter d max Determine 0.1d max From d max The grains in the grain size range up to 0.1d are defined as effective grains, and the grain size of the grains in this range is 0.1d max From d max The grains in the range up to 0.1d were statistically analyzed one by one. max The grains smaller than 100 are defined as fine grains, and no statistics are collected on the fine grains. The number of effective grains in one region is controlled to 100-150, and the grain size of each effective grain in each region is collected one by one. The method for measuring the grain size of a single grain may be as follows. A circumscribing circle with the minimum area (the circumscribing circle may be a perfect circle or an ellipse) is plotted for this grain, and if the circumscribing circle is a perfect circle, the diameter of the perfect circle is taken as the grain size of the grain. If the circumscribing circle is an ellipse, the average value of the length between the major axis and the minor axis of the ellipse is taken as the grain size of the grain. After collecting statistics on the grain sizes of the single effective grains in each region, they are recorded together as the grain size of n effective grains (d1, d2, d3...dn). Then, the "volume median diameter of the grains" d v 50 is calculated using the following formula.

[0047] JPEG0007588208000004.jpg2578

[0048] In an optional embodiment, the volume median diameter d of the crystal grains of the lithium nickel manganese composite oxide material v50 is 5 μm to 15 μm (e.g., 5 μm to 6 μm, 6 μm to 7 μm, 7 μm to 8 μm, 8 μm to 9 μm, 9 μm to 10 μm, 10 μm to 11 μm, 11 μm to 12 μm, 12 μm to 13 μm, 13 μm to 14 μm, 14 μm to 15 μm), optionally 5.5 μm to 11 μm, optionally 5.5 to 8 μm. Based on the above embodiment, the lithium nickel manganese composite oxide material is used in a secondary battery, and the secondary battery exhibits one or more improved performances.

[0049] In an optional embodiment, the volume median particle size D of the lithium nickel manganese composite oxide material v 50 is 9 μm to 20 μm (e.g., 9 μm to 10 μm, 10 μm to 11 μm, 11 μm to 12 μm, 12 μm to 13 μm, 13 μm to 14 μm, 14 μm to 15 μm, 15 μm to 16 μm, 16 μm to 17 μm, 17 μm to 18 μm, 18 μm to 19 μm, 19 μm to 20 μm), optionally 9 μm to 13 μm, optionally 9 to 11 μm. Based on the above embodiment, the lithium nickel manganese composite oxide material is used in a secondary battery, and the secondary battery exhibits one or more improved performances.

[0050] In an optional embodiment, the lithium nickel manganese composite oxide material includes a lithium nickel manganese composite oxide having a P4332 space group and a lithium nickel manganese composite oxide having an Fd-3m space group, and the content of the lithium nickel manganese composite oxide having the P4332 space group is greater than the content of the lithium nickel manganese composite oxide having the Fd-3m space group.

[0051] In any embodiment, the lithium nickel manganese composite oxide material comprises a lithium nickel manganese composite oxide having a P4332 space group, and the lithium nickel manganese composite oxide having the P4332 space group accounts for 50% or more, optionally 80%-91%, 50%-60%, 60-70%, 70-80%, 80%-90%, or 90%-95% of the weight of the lithium nickel manganese composite oxide material. Based on the above embodiment, the lithium nickel manganese composite oxide material is used in a secondary battery, and the secondary battery exhibits one or more improved performances.

[0052] In an optional embodiment, the lithium nickel manganese composite oxide material is Mn 3+ The lithium nickel manganese composite oxide material includes 3+ The weight content of is 5.5 wt% or less (for example, 1 wt% to 2 wt%, 2 wt% to 3 wt%, 3 wt% to 4 wt%, or 4 wt% to 5 wt%). Based on the above aspect, the lithium nickel manganese composite oxide material is used in a secondary battery, and the secondary battery exhibits one or more improved performance characteristics.

[0053] In an optional embodiment, the specific surface area of ​​the lithium nickel manganese composite oxide material is 1 m 2 / g or less, selectively, 0.1m 2 / g~0.9m 2 / g. According to the above embodiment, the lithium nickel manganese composite oxide material is used in a secondary battery, and the secondary battery exhibits one or more improved performance characteristics.

[0054] In an optional embodiment, the tap density of the lithium nickel manganese composite oxide material is 1.9 g / cm 3 Above, optionally, 1.9 g / cm 3 ~3.0g / cm 3 According to the above aspect, the lithium nickel manganese composite oxide material is used in a secondary battery, and the secondary battery exhibits one or more improved performances. Since the K value is 1 to 2 and the shape is regular, the powder is easily piled up more tightly during the tapping process, and therefore the tap density is high.

[0055] In an optional embodiment, the lithium nickel manganese composite oxide material includes lithium nickel manganese composite oxide particles having a coating layer provided on at least a portion of the surface.

[0056] In an optional embodiment, the coating layer material includes at least one of aluminum oxide, titanium oxide, zirconium oxide, boron oxide, rare earth oxides, lithium salts, phosphates, borates, and fluorides.

[0057] In an optional embodiment, the coating layer comprises a high rate lithium ion conductor layer.

[0058] In an optional embodiment, the coating layer has a multi-layer structure, the coating layer including an inner high rate lithium ion conductor layer and an outer aluminum oxide layer.

[0059] In an optional embodiment, the high rate lithium ion conductor is selected from oxide-, phosphate-, borate-, sulfide-, and LiPON-based inorganic materials that have lithium ion conductivity.

[0060] In an optional embodiment, the high rate lithium ion conductor contains one or more of the elements phosphorous, titanium, zirconium, boron, and lithium.

[0061] In any embodiment, the high rate lithium ion conductor is selected from Li2BO3, Li3PO4, or a combination thereof. According to the above aspect, the lithium nickel manganese composite oxide material is used in a secondary battery, and the secondary battery exhibits one or more improved performance characteristics.

[0062] In any embodiment, the high rate lithium ion conductor is a conductor having a current density of 1.0×10 -5 S cm -1A material having lithium ion conductivity. The high-rate lithium ion conductor is selected from oxide-based, phosphate-based, borate-based, sulfide-based and LiPON-based inorganic materials having lithium ion conductivity. The high-rate lithium ion conductor is selected from Li2BO3 or Li3PO4, for example.

[0063] In an optional embodiment, the general formula of the lithium nickel manganese composite oxide is as shown in Formula I:

number

[0064] In an optional embodiment, a=1 to 1.05.

[0065] In any embodiment, −0.1≦x≦0.1, for example −0.01≦x≦0.01, optionally x=0.

[0066] In any embodiment, −0.1≦y≦0.1, for example −0.01≦y≦0.01, optionally y=0.

[0067] In any embodiment, x+y≧0, 0≦x+y≦0.1, optionally x+y=0.

[0068] In some implementations, z=0 to 0.1, for example z=0.

[0069] In an optional embodiment, the lithium nickel manganese composite oxide is Li 1.01 Ni 0.49 Mn 1.51 He is O4.

[0070] In an optional embodiment, the lithium nickel manganese composite oxide is Li 1.02 Ni 0.5 Mn 1.4 Ti 0.1 He is O4.

[0071] In an optional embodiment, a method for producing a lithium nickel manganese composite oxide is provided, the method comprising the steps of: providing a precursor composition containing a lithium source, a nickel source, and a manganese source; and sintering the precursor composition to obtain a lithium nickel manganese composite oxide. The K value of the lithium nickel manganese composite oxide material is 1 to 2 (for example, 1 to 1.1, 1.1 to 1.2, 1.2 to 1.3, 1.3 to 1.4, 1.4 to 1.5, 1.5 to 1.6, 1.6 to 1.7, 1.7 to 1.8, 1.8 to 1.9, 1.9 to 2), and the K value is calculated according to the following formula:

number

[0072] In any embodiment, the lithium source may be selected from an oxide, hydroxide, salt of lithium, or a combination thereof. The nickel source may be selected from a nickel compound, hydroxide, salt of nickel, or a combination thereof. The manganese source may be selected from an oxide, hydroxide, salt of manganese, or a combination thereof. The lithium source may be selected from lithium carbonate, lithium hydroxide, lithium nitrate, lithium oxide, or a combination thereof. The nickel source may be selected from nickel hydroxide, nickel oxide, nickel nitrate, nickel carbonate, or a combination thereof. The manganese source may be selected from manganese hydroxide, manganese oxide, manganese nitrate, manganese carbonate, or a combination thereof.

[0073] In an optional embodiment, the nickel and manganese sources are nickel manganese hydroxides, e.g., Ni 0.25 Mn 0.75 It may be (OH)2.

[0074] In any embodiment, the ratio of the volume median particle diameters of the nickel source and the lithium nickel manganese composite oxide material is 0.4 to 1:1 (e.g., 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, or 1.0:1). The lithium nickel manganese composite oxide material obtained according to the above embodiment, when used as a positive electrode active material for a secondary battery (e.g., a lithium ion battery), exhibits one or more improved performances of the battery.

[0075] In any embodiment, the ratio of the volume median particle size of the manganese source to the lithium nickel manganese composite oxide material is 0.4 to 1:1 (e.g., 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, or 1.0:1). The lithium nickel manganese composite oxide material obtained according to the above embodiment, when used as a positive electrode active material for a secondary battery (e.g., a lithium ion battery), exhibits one or more improved performances of the battery.

[0076] In an optional embodiment, the lithium source has a volume median particle size of 1 to 20 μm (e.g., 3 to 10 μm). The lithium nickel manganese composite oxide material obtained according to the above embodiment, when used as a positive electrode active material for a secondary battery (e.g., a lithium ion battery), exhibits one or more improved performances of the battery.

[0077] In any embodiment, the sintering includes a first heat treatment step, the peak temperature of the first heat treatment step is 950°C to 1200°C (e.g., 950°C to 1000°C, 1000°C to 1050°C, 1050°C to 1100°C, 1100°C to 1150°C, 1150°C to 1200°C), and the warming time of the first heat treatment step at the peak temperature is 5h to 30h (e.g., 5h to 10h, 10h to 15h, 15h to 20h, 20h to 25h, 25h to 30h). The lithium nickel manganese composite oxide material obtained according to the above embodiment shows one or more improved performances of the battery as a positive electrode active material of a secondary battery (e.g., a lithium ion battery).

[0078] In any embodiment, the rate of temperature rise to the peak temperature in the first heat treatment step is 5° C. / min or less, optionally 0.5 to 3° C. / min, optionally 1 to 2° C. / min, 2 to 3° C. / min, 3 to 4° C. / min, or 4 to 5° C. / min. The lithium nickel manganese composite oxide material obtained according to the above embodiment, when used as a positive electrode active material for a secondary battery (e.g., a lithium ion battery), exhibits one or more improved battery performances.

[0079] In an optional embodiment, the sintering further includes a second heat treatment step after the first heat treatment step, the peak temperature of the second heat treatment step is 550°C to 680°C (e.g., 550°C to 570°C, 570°C to 590°C, 590°C to 610°C, 610°C to 630°C, 630°C to 650°C, 650°C to 670°C), and the time of the second heat treatment step is 5h to 50h (5h to 15h, 15h to 25h, 25h to 35h, 35h to 45h). The lithium nickel manganese composite oxide material obtained according to the above embodiment, as a positive electrode active material of a secondary battery (e.g., a lithium ion battery), exhibits one or more improved performances of the battery.

[0080] In an optional embodiment, the method for producing the lithium nickel manganese composite oxide further comprises ball milling the precursor composition before sintering, and optionally the ball milling time is 2 hours or more, for example, optionally 2 to 6 hours. The ball milling is performed to disperse the product after the first heat treatment. The lithium nickel manganese composite oxide material obtained according to the above embodiment shows one or more improved performances of the battery as a positive electrode active material of a secondary battery (e.g., a lithium ion battery).

[0081] In any embodiment, the content of the lithium nickel manganese composite oxide in the positive electrode active material may be 10 to 100 wt% (for example, 20 wt%, 30 wt%, 40 wt%, 50 wt%, 60 wt%, 70 wt%, 80 wt%, 90 wt%).

[0082] In some embodiments, the positive electrode active material may further include a positive electrode active material known in the art for use in batteries other than the lithium nickel manganese composite oxide described in any one of the above. For example, the other positive electrode active material may include at least one of a lithium-containing phosphate having an olivine structure, a lithium transition metal oxide, and a modified compound thereof, but the present application is not limited to these materials, and other conventional materials usable as a battery positive electrode active material may be used. These positive electrode active materials may be used alone or in combination of two or more. Here, examples of the lithium transition metal oxide include lithium cobalt oxide (e.g., LiCoO2), lithium nickel oxide (e.g., LiNiO2), lithium manganese oxide (e.g., LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (e.g., LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2(NCM 333 (may be abbreviated as))LiNi 0.5 Co 0.2 Mn 0.3 O2(NCM 523 (may be abbreviated as LiNi 0.5 Co 0.25 Mn 0.25 O2(NCM 211 (may be abbreviated as LiNi 0.6 Co 0.2 Mn 0.2 O2(NCM 622 (may be abbreviated as LiNi 0.8 Co 0.1 Mn 0.1 O2(NCM 811 Lithium nickel cobalt aluminum oxide (e.g., LiNi 0.85 Co 0.15 Al 0.05Examples of the lithium-containing phosphate having an olivine structure may include, but are not limited to, at least one of lithium iron phosphate (e.g., LiFePO4 (which may be abbreviated as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (e.g., LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium manganese iron phosphate, and a composite material of lithium manganese iron phosphate and carbon.

[0083] In some embodiments, the positive electrode membrane layer optionally further comprises an adhesive, which may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.

[0084] In some embodiments, the positive electrode membrane layer optionally further comprises a conductive agent, which may include at least one of superconducting carbon, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers, by way of example.

[0085] In some embodiments, the positive electrode current collector may be a metal foil sheet or a composite current collector. For example, the metal foil sheet may be an aluminum foil. The composite current collector may include a polymeric base layer and a metal layer formed on at least one surface of the polymeric substrate. The composite current collector may be formed by forming a metal material (such as aluminum, aluminum alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys) on a polymeric substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0086] In some embodiments, the positive electrode plate can be manufactured by the following method: The components for manufacturing the positive electrode plate, such as the positive electrode active material, conductive agent, adhesive, and any other components, are dispersed in a solvent (e.g., N-methylpyrrolidone) to form a positive electrode slurry, which is then applied onto a positive electrode current collector, and the positive electrode plate can be obtained through processes such as drying and cold pressing.

[0087] [Negative electrode plate] The negative electrode plate includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, the negative electrode film layer including a negative electrode active material.

[0088] For example, the negative electrode current collector has two opposing surfaces in the thickness direction of the negative electrode current collector, and the negative electrode film layer is provided on either one or both of the two opposing surfaces of the negative electrode current collector.

[0089] In some embodiments, the negative electrode current collector may employ a metal foil sheet or a composite current collector. For example, the metal foil sheet may employ a copper foil. The composite current collector may include a polymeric base layer and a metal layer formed on at least one surface of the polymeric substrate. The composite current collector may be formed by forming a metal material (such as copper, copper alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys) on a polymeric substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0090] In some embodiments, the negative electrode active material may be any negative electrode active material known in the art for use in batteries. For example, the negative electrode active material may include at least one of artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. The silicon-based material may be selected from at least one of silicon, silicon oxide, silicon carbon composite, silicon nitrogen composite, and silicon alloy. The tin-based material may be selected from at least one of tin, tin oxide, and tin alloy. However, the present application is not limited to these materials, and other conventional materials that can be used for battery negative electrode active materials may be used. These negative electrode active materials may be used alone or in combination of two or more.

[0091] In some embodiments, the negative electrode membrane layer optionally further comprises an adhesive, which may be selected from at least one of styrene butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethylmethacrylate (PMAA), and carboxymethyl chitosan (CMCS), by way of example.

[0092] In some embodiments, the negative electrode film layer optionally further comprises a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers, by way of example.

[0093] In some embodiments, the negative electrode membrane layer optionally further comprises other auxiliary agents, such as a thickening agent (eg, sodium carboxymethylcellulose (CMC-Na)).

[0094] In some embodiments, the negative electrode plate can be manufactured by the following method: Components for manufacturing the negative electrode plate, such as a negative electrode active material, a conductive agent, an adhesive, and any other components, are dispersed in a solvent (e.g., deionized water) to form a negative electrode slurry, which is then applied onto a negative electrode current collector, and the negative electrode plate can be obtained through processes such as drying and cold pressing.

[0095] [Electrolytes] The electrolyte serves to conduct ions between the positive and negative electrodes. The present application does not specifically limit the type of electrolyte, and it can be selected according to the needs. For example, the electrolyte may be liquid, gel, or all solid.

[0096] In some embodiments, the electrolyte is in liquid form and includes an electrolyte salt and a solvent.

[0097] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl imide), lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluoro(oxalato)borate, lithium bis(oxalato)borate, lithium difluorobis(oxalato)phosphate, and lithium tetrafluoro(oxalato)phosphate.

[0098] In some embodiments, the solvent may be selected from at least one of ethylene carbonate, propylene carbonate, methyl ethyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, sulfone, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.

[0099] In some embodiments, the electrolyte solution optionally further includes additives. For example, the additives may include an anode film-forming additive, a cathode film-forming additive, or an additive that can improve some performance of the battery, such as an additive that improves the overcharge performance of the battery, or an additive that improves the high temperature or low temperature performance of the battery.

[0100] [Separator] In some embodiments, the secondary battery further includes a separator. The present application does not particularly limit the type of separator, and any separator with a well-known porous structure having good chemical and mechanical stability may be selected.

[0101] In some embodiments, the material of the separator may be selected from at least one of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator may be a single layer thin film or a multi-layer composite thin film, and is not particularly limited. When the separator is a multi-layer composite thin film, the materials of each layer may be the same or different, and is not particularly limited.

[0102] In some embodiments, the positive and negative plates and the separator can be manufactured into an electrode component by a winding or lamination process.

[0103] In some embodiments, the secondary battery may include an exterior packaging, which may be used to package the electrode components and electrolyte.

[0104] In some embodiments, the exterior of the secondary battery may be a hard case, such as a hard plastic case, an aluminum case, a steel case, etc. The exterior of the secondary battery may be a soft bag, such as a pouch-type soft bag. The material of the soft bag may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0105] The present application does not particularly limit the shape of the secondary battery, which may be cylindrical, rectangular, or any other shape. For example, FIG. 8 shows a secondary battery 5 having a rectangular structure as an example.

[0106] In some embodiments, referring to FIG. 9, the exterior may include a case 51 and a cover plate 53. Here, the case 51 may include a bottom plate and a side plate connected on the bottom plate, and the bottom plate and the side plate form a surrounding chamber. The case 51 has an opening communicating with the chamber, and the cover plate 53 can be placed over the opening to close the chamber. The positive electrode plate, the negative electrode plate and the separator can be formed into an electrode component 52 by a winding process or a lamination process. The electrode component 52 is packaged in the chamber. The electrolyte is permeated into the electrode component 52. The number of electrode components 52 included in the secondary battery 5 may be one or more, and may be selected by those skilled in the art according to actual specific needs.

[0107] In some embodiments, the secondary batteries may be assembled into a battery module, and the number of secondary batteries included in the battery module may be one or more, with the specific number being selectable by one skilled in the art based on the application and capacity of the battery module.

[0108] The present application further provides a power consuming device. The power consuming device includes at least one of a secondary battery, a battery module, or a battery pack according to the present application. The secondary battery, the battery module, or the battery pack may be used as a power source for the power consuming device, or may be used as an energy storage unit for the power consuming device. The power consuming device may include, but is not limited to, mobile equipment (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships, satellites, and energy storage systems.

[0109] The power consuming device may be a secondary battery, a battery module, or a battery pack, depending on the needs of the usage.

[0110] 10 shows an example of a power consuming device, such as a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. To meet the high power and high energy density demands of the secondary battery of the power consuming device, a battery pack or battery module containing the secondary battery may be employed.

[0111] [Example] The following describes examples of the present application. The examples described below are illustrative and are used only to interpret the present application, and should not be understood as limiting the present application. In the examples, specific techniques or conditions are not specified, but are carried out according to techniques or conditions described in the literature in the field or product instructions. Reagents or equipment used that do not specify the manufacturer are all common products that can be purchased commercially.

[0112] Examples 1a-1b Production of lithium nickel manganese composite oxide (1) The corresponding precursor composition is mixed with the target product LiNi 0.5 Mn 1.5The precursor composition is provided in a ratio of 04 to 1000. The composition of the precursor composition is a lithium source (Li2CO3) and a nickel manganese source Ni 0.25 Mn 0.75 (OH)2. The volume median particle size D of the nickel manganese source precursor v 50(P) is D v 50(P)=xD v 50(C), where D v 50(C) is the volume median particle diameter of the nickel manganese composite oxide material product, and x=0.4 to 1. The details of the volume median particle diameter of the nickel manganese source precursor are as shown in Table 2. The precursor composition is mixed and ball milled for 3 hours to obtain a ball mill product.

[0113] (2) subjecting the ball mill product to a first heat treatment, the atmosphere of the first heat treatment being air, and the first heat treatment comprising: a) increasing the temperature from room temperature to a peak temperature at a preset heating rate c1 (°C / min); b) maintaining T1 at a peak temperature and maintaining t1 for a period of time; The heating rate, peak temperature and heat retention time (heat retention time at peak temperature) are as shown in Table 1. The product after the first heat treatment is cooled to room temperature. Lithium nickel manganese composite oxide Li 1.01 Ni 0.49 Mn 1.5 Get 1O4.

[0114] (3) The product of the previous step is subjected to a second heat treatment, the atmosphere of the second heat treatment is air, the peak temperature T2 and the heat retention time t2 of the second heat treatment are as shown in Table 1, and the product after the heat treatment is cooled to room temperature. Lithium nickel manganese composite oxide Li 1.01 Ni 0.49 Mn 1.51 Get O4.

[0115] Examples 2a-2c Manufacture of lithium nickel manganese composite oxide.

[0116] The differences between Examples 2a, 2b, and 2c and Example 1a are in the heating rate, peak temperature, and / or heat retention time in the first heat treatment and the second heat treatment, and the specific differences in the manufacturing method parameters are shown in Table 1. The physicochemical parameters of the lithium nickel manganese composite oxide are shown in Table 2.

[0117] Example 3a (1) The corresponding precursor composition is mixed with the target product LiNi 0.5 Mn 1.4 Ti 0.1 The composition of the precursor composition includes a lithium source (Li2CO3), a nickel source (Ni(OH)2), a manganese source (Mn(OH)2), and a dopant (nano-TiO2). The precursor composition is mixed and ball-milled for 3 h to obtain a ball-milled product. The details of the volume median particle size of the nickel manganese source precursor are shown in Table 2. (2) The ball mill product is subjected to a first heat treatment, and the first heat treatment temperature rise rate, peak temperature, and heat retention time at the peak temperature are as shown in Table 1. After the heat treatment, the product is cooled to room temperature.

[0118] (3) Polish the product of the previous step for 3 h.

[0119] (4) The above polished product is subjected to a second heat treatment, the heat treatment temperature and time are as shown in Table 1, and after the heat treatment, it is cooled to room temperature. Lithium nickel manganese (titanium added) composite oxide Li 1.02 Ni 0.5 Mn 1.4 Ti 0.1 The particle parameters of the lithium nickel manganese composite oxide are shown in Table 2.

[0120] Examples 3b, 3c, 3d The difference between Examples 3b, 3c, and 3d and Example 3a is step (3), which is specifically: (3) The first coating material is added to the product of the previous step in the target mixing ratio and polished for 3 h. The details of the first coating material and the amount added are shown in Table 1.

[0121] The details of the differences in the specific manufacturing method parameters are shown in Table 1. The particle parameters of the lithium nickel manganese composite oxide are shown in Table 2.

[0122] Examples 3e and 3f (1) The corresponding precursor composition is mixed with the target product LiNi 0.5 Mn 1.4 Ti 0.1 The precursor composition is provided with a component ratio of Li2CO3, Ni(OH)2, Mn(OH)2, and dopant (nano-TiO2). The precursor composition is mixed and ball-milled for 3 h to obtain a ball-milled product.

[0123] (2) The ball mill product is subjected to a first heat treatment, the heating rate, peak temperature and heat retention time of the first heat treatment being as shown in Table 1, and after the heat treatment, it is cooled to room temperature.

[0124] (3) The first coating material is added to the product of the previous step in the target mixing ratio and polished for 3 h. The details of the first coating material and the amount added are shown in Table 1.

[0125] (4) The polished product is subjected to a second heat treatment, the second heat treatment temperature and time being as shown in Table 1, and then cooled to room temperature.

[0126] (5) The second coating material is added to the product of the previous step in the target mixing ratio and polished for 3 h. The details of the second coating material and the amount added are shown in Table 1.

[0127] (6) The ground product is subjected to a third heat treatment, the heat treatment temperature and time being as shown in Table 1, and cooled to room temperature after the heat treatment to obtain a lithium nickel manganese composite oxide.

[0128] The details of the differences in the specific manufacturing method parameters are shown in Table 1. The particle parameters of the lithium nickel manganese composite oxide are shown in Table 2.

[0129] Comparative Example 1-3 Three different commercially available lithium nickel manganese composite oxide powders are provided, designated B1, B2, and B3, respectively.

[0130] Assembling a half cell (button cell) Using a lithium sheet as a counter electrode, the lithium nickel manganese composite oxide materials of the examples and comparative examples are assembled into a half cell.

[0131] Lithium nickel manganese composite oxide, conductive carbon black, and PVDF were mixed in a weight ratio of 90:5:5, and an appropriate amount of solvent was added and stirred uniformly to obtain a positive electrode slurry. The positive electrode slurry was applied to an aluminum foil and then dried to obtain a positive electrode plate. The amount of lithium nickel manganese composite oxide supported on the positive electrode plate was 0.015 g / cm. 2 It was.

[0132] A mixed solution containing 1 mol / LLiPF6 carbonate, phosphate ester, etc. was provided as the electrolyte.

[0133] A 12μm thick polypropylene film (Φ16mm) was used as a separator, and the lithium sheet, separator, and positive electrode plate were placed in that order, with the separator positioned between the metallic lithium sheet and the composite negative electrode plate to serve as an insulator. The electrolyte was injected, and the battery was assembled into a CR2030 button battery. The battery was left to stand for 24 hours to obtain a half-cell.

[0134] Manufacturing of soft bag batteries The lithium nickel manganese composite oxide materials of the examples and the comparative examples are assembled into soft bag batteries.

[0135] Lithium nickel manganese composite oxide, conductive carbon black, and PVDF were mixed in a weight ratio of 96:2.5:1.5, and an appropriate amount of solvent was added and stirred uniformly to obtain a positive electrode slurry. The positive electrode slurry was applied to an aluminum foil and then dried to obtain a positive electrode plate. The amount of lithium nickel manganese composite oxide supported on the positive electrode plate was 0.02 g / cm. 2 It was.

[0136] Graphite, conductive carbon black, and carboxymethyl cellulose were mixed in a weight ratio of 96:1:3, and an appropriate amount of solvent was added and stirred uniformly to obtain a negative electrode slurry. The negative electrode slurry was applied to a copper foil and then dried to obtain a negative electrode plate. The amount of graphite supported on the negative electrode plate was 0.008 g / cm. 2 It was.

[0137] The same electrolyte as in the button cell was used.

[0138] A 12μm thick polypropylene film (Φ16mm) was used as a separator, and the positive electrode plate, separator, and negative electrode plate prepared above were placed in order, the separator was placed between the positive and negative electrodes to serve as an insulator, and the plate was rolled and packaged in an aluminum plastic bag. An electrolyte was injected, and after packaging, the plate was converted and capacified to produce a soft bag battery cell.

[0139] Analysis Detection 1. Morphological observation, particle size detection and tap density detection 1 shows a scanning electron microscope photograph of the lithium nickel manganese composite oxide of Example 2a, in which the elliptical outlines show some representative grains, including grain I, grain II, grain III, and grain IV, and the grain sizes are 6.0 μm, 7.1 μm, 3.8 μm, and 3.9 μm, respectively.

[0140] FIG. 2 shows a scanning electron microscope photograph of the lithium nickel manganese composite oxide of Example 2b, in which the elliptical outline shows several representative crystal grains, including crystal grain I, crystal grain II, crystal grain III, crystal grain IV, and crystal grain V, and the crystal grain sizes are 3.1 μm, 3.8 μm, 8.2 μm, 7.5 μm, and 5.7 μm, respectively.

[0141] FIG. 3 shows a scanning electron microscope photograph of the lithium nickel manganese composite oxide of Example 2c, in which the elliptical outline shows several representative crystal grains, including crystal grain I, crystal grain II, and crystal grain III, and the crystal grain sizes are 9.3 μm, 6.0 μm, and 12.9 μm, respectively.

[0142] 4 shows a scanning electron microscope photograph of the lithium nickel manganese composite oxide of Example 3b, in which the circular outlines indicate some representative crystal grains, including crystal grain I, crystal grain II, crystal grain III, crystal grain IV, and crystal grain V, with particle size distributions of 4.2 μm, 6.6 μm, 9.5 μm, 9.6 μm, and 9.1 μm. The square outlines in the figure indicate the grain sizes of 0.1 μm, 0.2 μm, 0.4 μm, and 0.6 μm. max These fine grains were not counted in the statistical range.

[0143] FIG. 5 shows a scanning electron microscope photograph of the lithium nickel manganese composite oxide of Comparative Example 1. The circular outlines indicate some representative crystal grains, including crystal grain I, crystal grain II, and crystal grain III, with grain size distributions of 4.7 μm, 1.9 μm, and 3.5 μm. The square outlines in the figure indicate grain sizes of 0.1d max These fine grains were not counted in the statistical range.

[0144] FIG. 6 shows a scanning electron microscope photograph of the lithium nickel manganese composite oxide of Comparative Example 2. As shown in the figure, the circular outlines indicate some representative crystal grains, including crystal grain I, crystal grain II, and crystal grain III, and the grain size distributions are 1.5 μm, 1.6 μm, and 1.0 μm. The square outlines in the figure indicate the grain sizes of 0.1 dmax These fine grains were not counted in the statistical range.

[0145] Fig. 7 shows a scanning electron microscope photograph of the lithium nickel manganese composite oxide of Comparative Example 3. As shown in the figure, the circular outlines indicate some representative crystal grains, including crystal grain I, crystal grain II, crystal grain III, crystal grain IV, and crystal grain V, and the grain size distributions are 5.0 μm, 4.4 μm, 3.0 μm, 4.3 μm, and 2.8 μm. The square outlines in the figure indicate the grain sizes of 0.1d max These fine grains were not counted in the statistical range.

[0146] By the above method, the volume median diameter d of the crystal grains of the lithium nickel manganese composite oxide of the examples and the comparative examples was v 50 and volume median particle size D v 50 were detected, and the K value was calculated using the following formula.

[0147] JPEG0007588208000007.jpg958

[0148] The tap density test was based on the standard GB / T 5162-2006 "Determination of Tap Density of Metal Powders".

[0149] Detailed results are shown in Table 2.

[0150] 2. Battery performance detection 1. Mn 3+ Content (wt.%) and structural ratio of P4332 The half-cells of the examples and the comparative examples were used as test subjects. The discharge capacity (Q1) from 4.5 to 3.5 V and the total discharge capacity (Q2) from 4.9 to 3.5 V were measured, and the 4V platform capacity ratio x=Q1 / Q2 was calculated. The specific test method is as follows.

[0151] At 25°C, the button cell was charged at a constant current of 0.1 C up to a voltage of 4.9 V, then charged at a constant voltage of 0.05 C at 4.9 V, and after leaving the cell to stand for 5 min, it was discharged at a constant current of 0.1 C down to a voltage of 3.5 V. The discharge capacity from 4.5 to 3.5 V (Q1) and the total discharge capacity from 4.9 to 3.5 V (Q2) were extracted from the initial charge and discharge data.

[0152] Based on x, the following component characteristics (1) to (2) of the material can be reflected: (1) Based on x, Mn in lithium nickel manganese composite oxide material 3+ The content (r) can be calculated.

number

[0153] In the above formula, the coefficient 0.45 is LiNi 0.5 Mn 1.5 is the mass content of Mn in O4, and 1.5 is the 1.5 in the chemical formula (i.e., the stoichiometric ratio of Mn / Li).

[0154] (2) The spinel phase of the material contains the P4332 space group and the Fd-3m space group, and contains only the P4332 space group and the Fd-3m space group. The content (y) of nickel manganese composite oxide having the P4332 space group in the lithium nickel manganese composite oxide material can also be calculated based on x.

number

[0155] Mn 3+ Table 3 shows detailed statistical results for the content (r) and the content (y) of nickel manganese composite oxide having the P4332 space group.

[0156] II. Cycle performance The graphite soft bag batteries of the example and comparative example were used as test subjects.

[0157] At 25°C, the graphite soft bag battery was charged at a constant current of 0.3C to a voltage of 4.9V, then charged at a constant voltage of 4.9V until the current reached 0.05C, and after standing for 5 minutes, the graphite soft bag battery was discharged at a constant current of 0.33C to a voltage of 3.5V, which constituted one charge-discharge cycle process, and the discharge capacity of this cycle was the discharge capacity of the first cycle. All batteries were subjected to multiple cycle charge-discharge tests according to the above method, and the number of cycles for all batteries was recorded until the discharge capacity of all batteries was attenuated to 80%. The detailed statistical results are shown in Table 3.

[0158] 3. Gas generation and ion elution The graphite soft bag batteries of the example and comparative example were used as test subjects.

[0159] At 25°C, the graphite soft bag battery was charged at a constant current of 0.3C to a voltage of 4.9V, and then at 4.9V, it was charged at a constant voltage of 0.05C. This fully charged battery was placed in a constant temperature factory at 25°C, and during this process, the volume of the soft bag battery cell was measured every 10 days using the drainage method, and the increased volume was taken as the gas generation volume. After 100 days, the 100-day storage gas generation data was obtained, and after the test was completed, the battery was discharged at a constant current of 0.33C to 3.5V, and then discharged at a constant current of 0.05C to 3.5V, to obtain a fully discharged battery.

[0160] The fully discharged battery was disassembled, and the anode plate was separated. The anode plate was gently shaken in DMC solvent for 5s to remove the residual electrolyte on the anode surface, and then dried. The anode material was scraped off from the surface of the anode plate, and the Ni content (μg / g) and Mn content (μg / g) in the anode material were detected using inductively coupled plasma spectroscopy technology, which were taken as the Ni ion elution value and Mn ion elution value. The details of the test results of gas generation and ion elution are shown in Table 3.

[0161] [Table 1]

[0162] [Table 2]

[0163] [Table 3]

[0164] From the data in Table 3, the following conclusions can be drawn: (1) About K value The K value of the lithium nickel manganese composite oxides of Examples (1a-1b, 2a-2c) was in the range of 1.36 to 1.89, and the K value of the lithium nickel manganese composite oxide of Comparative Example (1-3) was in the range of 2.10 to 4.15.

[0165] From the battery performance test, it was found that the lithium nickel manganese composite oxide of the embodiment has the following advantages.

[0166] The lithium-nickel-manganese composite oxides of Examples (1a-1b, 2a-2c) were used as the positive electrode active material for lithium-ion batteries, and the number of cycles at which the lithium-ion batteries reached their cut-off capacity was 365 to 449, which was higher than the 120 to 283 cycles of the comparative examples. This indicates that the lithium-ion batteries using the materials of the Examples have improved cycle performance.

[0167] The lithium-nickel-manganese composite oxides of Examples (1a-1b, 2a-2c) were used as the positive electrode active material for lithium-ion batteries, and the Ni ion elution value of the lithium-ion batteries was 209μg / g to 308μg / g, which is lower than the 312μg / g to 367μg / g of the comparative examples. The Mn ion elution value of the lithium-ion batteries was 1665μg / g to 2072μg / g, which is lower than the 2571μg / g to 3021μg / g of the comparative examples. This shows that the lithium-ion batteries using the materials of the examples have reduced ion elution.

[0168] The lithium-nickel-manganese composite oxides of the examples (1a-1b, 2a-2c) are used as the positive electrode active material of the lithium-ion battery, and the gas generation rate of the lithium-ion battery is 27.2-35.6 ml / Ah, which is lower than the 36.9 ml / Ah to 49.2 ml / Ah of the comparative example. This means that the lithium-ion battery using the materials of the examples has reduced gas generation.

[0169] (2) Dope The lithium nickel manganese composite oxide of Example 3a was doped with Ti element, and this lithium nickel manganese composite oxide was used as a positive electrode active material for a lithium ion battery. The number of cycles at which the lithium ion battery reached its cutoff capacity was 481 cycles, the Ni ion elution value of the lithium ion battery was 262 μg / g, which was lower than 1895 μg / g of the comparative example, and the gas generation amount was 35.3 ml / Ah.

[0170] The lithium nickel manganese composite oxide of Example 3a exhibited better cycle performance, lower ion dissolution, and lower gas generation than Examples (1a-1b, 2a-2c), indicating that the doped lithium nickel manganese composite oxide has better performance.

[0171] (3) Coverage The lithium nickel manganese composite oxides of Examples 3b to 3e had a coating layer, and were used as positive electrode active materials for lithium ion batteries. The number of cycles at which the lithium ion batteries reached their cutoff capacity was 570 to 724 cycles, the Ni ion elution values ​​of the lithium ion batteries were 157 to 201 μg / g, the Mn ion elution values ​​of the lithium ion batteries were 1168 to 1592 μg / g, and the gas generation amounts of the lithium ion batteries were 16.6 to 25.7 ml / Ah.

[0172] The lithium nickel manganese composite oxides of Examples 3b-3e exhibited better cycle performance, lower ion elution, and lower gas generation than Example 3a, indicating that the lithium nickel manganese composite oxides having a coating layer have better performance. (4) Manufacturing process In order to obtain a lithium nickel manganese composite oxide having a K value in the range of 1 to 2, the following factors are key.

[0173] Factor 1: The first heat treatment temperature and the heat retention time. The peak temperature of the first heat treatment determines the upper limit and average value of the grain size, and is also the driving force for the growth and deformation of the grains. The peak temperature of the first heat treatment and the heat retention time jointly determine the size and shape of the grains. The peak temperature of the first heat treatment stage is preferably 950°C to 1200°C, and the heat retention time of the first heat treatment stage at the peak temperature is preferably 5h to 30h.

[0174] Factor 2: The heating rate of the first heat treatment. If the heating rate is too fast, localized thermal imbalance occurs, some crystal grains grow first, and a serious situation occurs in which large crystal grains absorb small crystal grains, resulting in serious blocking between crystal grains. The heating rate from room temperature to the peak temperature in the first heat treatment is preferably 5°C / min or less, and optionally 0.5 to 3°C / min.

[0175] Factor 3: Particle size of nickel source and manganese source precursor. The smaller the nickel source and manganese source precursor particles are, the more small particles must be combined to obtain the same target particle size, and the corresponding first heat treatment temperature must be increased, which leads to serious interparticle blocking in the finished product. If the nickel manganese precursor particles are too large, it is difficult to sinter them, and the first heat treatment temperature must be increased, which may lead to interparticle blocking. The ratio of the volume median particle size of the nickel source and manganese source precursor to the lithium nickel manganese composite oxide material is preferably 0.4 to 1, and optionally 0.6 to 0.8.

[0176] The manufacturing processes of the Examples (1a-1b, 2a-2c, 3a-3f) satisfied the above requirements, and therefore succeeded in obtaining a lithium nickel manganese composite oxide having a K value in the range of 1-2.

[0177] (5) P4332 structure content or Mn 3+ Regarding the content of As confirmed in Examples (1a-1b, 2a-2c, 3a-3f), the content of P4332 structure is 50% or more (or Mn 3+ The content of 5% or less is advantageous for the performance of the battery.

[0178] In order to obtain a lithium nickel manganese composite oxide mainly having a P4332 structure, the following factors are key.

[0179] Factor 1. The second heat treatment temperature and the warming time are consistent with the target grain size and the first heat treatment temperature and time. Since P4332 is a low-temperature phase, from a thermodynamic point of view, the lower the temperature, the more likely the P4332 structure is. However, from a kinetic point of view, the lower the temperature, the more unfavorable it is for atomic diffusion to cause a phase transition. The higher the first heat treatment temperature, the higher the Fd-3m structure content, and the longer the second heat treatment warming time must be. The larger the grains, the greater the relatively large diffusion force required, and the higher the second heat treatment temperature. The second heat treatment temperature also affects the second heat treatment time in the same way. The peak temperature of the second heat treatment stage is preferably 550°C to 680°C, and the warming time of the second heat treatment stage is preferably 5h to 50h.

[0180] Factor 2. Elemental components. The occurrence of the Fd-3m phase is related to the radius of each atom in the transition metal layer, and atoms with different radii (especially atoms with stable radii) can stabilize the crystal structure and improve the directionality of the Ni, Mn ordered array, and the doping of high-value ions such as Ti, Cr, and Zr and +1, +2 valence atoms at the Ni position are all correlated with it. The preferred doping element is Ti element.

[0181] It should be noted that the present application is not limited to the above-mentioned embodiment. The above-mentioned embodiment is merely an example, and any embodiment having substantially the same configuration as the technical idea and having the same action and effect within the scope of the technical solution of the present application is included in the technical scope of the present application. In addition, various modifications that a person skilled in the art can conceive of to the embodiment are implemented within the scope of the gist of the present application, and other forms constructed by combining some of the components in the embodiment are also included in the scope of the present application. [Explanation of symbols]

[0182] 5 secondary battery; 51 case; 52 electrode component; 53 cover plate

Claims

1. A lithium nickel manganese composite oxide material, the K value of the lithium nickel manganese composite oxide material being 1 to 2, the K value being calculated according to the following formula: [0010] Here, d v 50 is the volume median diameter of the crystal grains in the lithium nickel manganese composite oxide material, and D v 50 is the volume median particle size of the lithium nickel manganese composite oxide material; The volume median diameter d of the crystal grains of the lithium nickel manganese composite oxide material v 50 is between 5 μm and 15 μm, alternatively between 5.5 μm and 11 μm; The volume median particle diameter D of the lithium nickel manganese composite oxide material v 50 is a lithium nickel manganese composite oxide material having a particle size of 9 μm to 20 μm, optionally 9 μm to 11 μm.

2. The lithium nickel manganese composite oxide material is P4 3 The P4 comprises a lithium nickel manganese composite oxide having a Fd-32 space group and a lithium nickel manganese composite oxide having a Fd-3m space group. 3 The lithium nickel manganese composite oxide material according to claim 1, wherein the content of the lithium nickel manganese composite oxide of the 32 space group is greater than the content of the lithium nickel manganese composite oxide of the Fd-3m space group.

3. Said P4 3 The lithium nickel manganese composite oxide material according to claim 2, wherein the lithium nickel manganese composite oxide having 32 space group accounts for 50% or more, and optionally 80% to 91% of the weight of the lithium nickel manganese composite oxide material.

4. The lithium nickel manganese composite oxide material is Mn 3+ The lithium nickel manganese composite oxide material contains Mn 3+The lithium nickel manganese composite oxide material according to any one of claims 1 to 3, wherein the content of is 5.5 wt % or less, optionally 1.0 wt % to 2.2 wt %.

5. The specific surface area of ​​the lithium nickel manganese composite oxide material is 1 m 2 / g or less, optionally 0.1 m 2 / g to 0.9m 2 The lithium nickel manganese composite oxide material according to any one of claims 1 to 4, wherein the lithium nickel manganese composite oxide material has a molecular weight of 1.0 - 1.0 g.

6. The tap density of the lithium nickel manganese composite oxide material is 1.9 g / cm 3 Above, optionally, 1.9m 2 / g to 3.0 m 2 The lithium nickel manganese composite oxide material according to any one of claims 1 to 5, wherein the lithium nickel manganese composite oxide material has a molecular weight of 1.0 - 1.0 g.

7. The lithium nickel manganese composite oxide material includes lithium nickel manganese composite oxide particles having a coating layer provided on at least a portion of the surface thereof, Optionally, the material of the coating layer includes at least one of aluminum oxide, titanium oxide, zirconium oxide, boron oxide, rare earth oxide, lithium salt, phosphate, borate, and fluoride; Optionally, the coating layer includes a high rate lithium ion conductor layer; Optionally, the coating layer has a multi-layer structure, and the coating layer includes an inner high-speed lithium ion conductor layer and an outer aluminum oxide layer. The lithium nickel manganese composite oxide material according to any one of claims 1 to 6.

8. (1) the high-speed lithium ion conductor is selected from oxide-based, phosphate-based, borate-based, sulfide-based, and LiPON-based inorganic materials having lithium ion conductivity; (2) the high-rate lithium ion conductor contains one or more elements selected from the group consisting of phosphorus, titanium, zirconium, boron, and lithium; (3) The high-speed lithium ion conductor is Li 2 B.O. 3 , Li 3 P.O. 4 or a combination thereof; The lithium nickel manganese composite oxide material according to claim 7, characterized in that it has one or more of the following characteristics:

9. The general formula of the lithium nickel manganese composite oxide is as shown in Formula I, [0025] In formula I, element M is selected from Ti, Zr, W, Nb, Al, Mg, P, Mo, V, Cr, Zn, or combinations thereof; In formula I, element X is selected from F, Cl, I, or combinations thereof; In formula I, 0.9≦a≦1.1, −0.2≦x≦0.2, −0.2≦y≦0.3, and 0≦z≦1; Optionally, the element M is selected from Mg, Ti or a combination thereof; Optionally, the element X is F. The lithium nickel manganese composite oxide material according to claim 2 or 3.

10. A method for producing a lithium nickel manganese composite oxide, comprising the steps of: providing a precursor composition containing a lithium source, a nickel source, and a manganese source; and sintering the precursor composition to obtain a lithium nickel manganese composite oxide. The K value of the lithium nickel manganese composite oxide is 1 to 2, and the K value is calculated according to the following formula: [0030] Here, d v 50 is the volume median diameter of the crystal grains of the lithium nickel manganese composite oxide, Here, D v 50 is the volume median particle size of the lithium nickel manganese composite oxide, The volume median diameter d of the crystal grains of the lithium nickel manganese composite oxide material v50 is between 5 μm and 15 μm, alternatively between 5.5 μm and 11 μm; The volume median particle diameter D of the lithium nickel manganese composite oxide material v 50 is between 9 μm and 20 μm, alternatively between 9 μm and 11 μm; the ratio of the volume median particle diameters of the nickel source and the lithium nickel manganese composite oxide is 0.4 to 1; the ratio of the volume median particle diameters of the manganese source and the lithium nickel manganese composite oxide is 0.4 to 1; The sintering comprises a first heat treatment step, The peak temperature of the first heat treatment step is 950°C to 1200°C, and the holding time of the first heat treatment step at the peak temperature is 5h to 30h; The method for producing a lithium nickel manganese composite oxide, wherein the rate of temperature increase to the peak temperature of the first heat treatment is 5° C. / min or less.

11. The general formula of the lithium nickel manganese composite oxide is as shown in Formula I, [0045] In formula I, element M is selected from Ti, Zr, W, Nb, Al, Mg, P, Mo, V, Cr, Zn, or combinations thereof; In formula I, element X is selected from F, Cl, I, or combinations thereof; The method of claim 10, wherein in formula I, 0.9≦a≦1.1, −0.2≦x≦0.2, −0.2≦y≦0.3, and 0≦z≦1.

12. The method of claim 10 or 11, wherein the lithium source has a volume median particle size of 1 to 20 μm.

13. The method according to any one of claims 10 to 12, wherein the rate of temperature increase to the peak temperature of the first heat treatment is 0.5 to 3°C / min.

14. The sintering further comprises a second heat treatment step after the first heat treatment step; 14. The method according to any one of claims 10 to 13, wherein the peak temperature of the second heat treatment step is between 550°C and 680°C and the duration of the second heat treatment step is between 5h and 50h.

15. further comprising ball milling the precursor composition prior to sintering; Optionally, the ball milling time is 2 h or more, optionally 2 to 6 h.

16. A secondary battery including a positive electrode plate, the positive electrode plate including a positive electrode active material, the positive electrode active material including the lithium nickel manganese composite oxide material according to any one of claims 1 to 9.

17. A power consuming device comprising the secondary battery of claim 16.

Citation Information

Patent Citations

  • Lithium manganese nickel oxide cathode material having nickel manganese concentration gradient and preparation method thereof

    CN105226270A

  • Preparation method of micron-sized monocrystalline nickel manganese acid lithium cathode material

    CN110304665A

  • Spinel type single-crystal cobalt-free high-voltage lithium nickel manganese oxide positive electrode material, preparation method thereof and lithium ion battery

    CN113178566A

  • Method of producing composite cathode active material and composite cathode active material

    JP2018041586A

  • Method for producing partially coated positive electrode active material particle

    JP2021044099A