Hexagonal boron nitride agglomerated particles

By producing hexagonal boron nitride agglomerated particles through a reductive nitriding reaction, thermal anisotropy and void-related issues are addressed, resulting in resin compositions with improved thermal conductivity and dielectric strength while reducing weight.

JP7588551B2Active Publication Date: 2024-11-22TOKUYAMA CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021079939
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-05-10
Publication Date
2024-11-22
Estimated Expiration
2041-05-10

AI Technical Summary

Technical Problem

Hexagonal boron nitride agglomerated particles exhibit thermal anisotropy and high specific gravity, leading to reduced thermal conductivity and dielectric strength when used as a filler in resin compositions, and the presence of large voids can decrease insulation resistance.

Method used

The production of hexagonal boron nitride agglomerated particles through a reductive nitriding reaction using specific raw materials and conditions, resulting in fine, randomly oriented scale-like primary particles with minimal gaps, eliminating thermal anisotropy and reducing weight.

Benefits of technology

The solution provides resin compositions with enhanced thermal conductivity, high dielectric strength, and reduced weight by minimizing the impact of voids on dielectric strength and specific gravity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588551000003
    Figure 0007588551000003
  • Figure 0007588551000001
    Figure 0007588551000001
  • Figure 0007588551000002
    Figure 0007588551000002
Patent Text Reader

Abstract

To provide hexagonal boron nitride agglomerated particles capable of imparting extremely high insulation capacity and thermal conductivity to a resin composition obtained by filling a resin, and of reducing density.SOLUTION: Preferably, agglomerated particles of hexagonal boron nitride primary particles have a major diameter in the range of 5 to 10 μm, a major / minor diameter in the range of 1.0 to 1.3, and a circularity in the range of 0.3 to 0.8, the maximum diameter of the primary particles that can be confirmed on the surface of the agglomerated particles being 4 μm or less according to a SEM observation image with magnification of 10,000 times, the content of metallic impurity elements being 500 ppm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to novel hexagonal boron nitride agglomerated particles, specifically, to provide a resin composition obtained by filling the particles with the hexagonal boron nitride agglomerated particles, which can impart extremely high dielectric strength and thermal conductivity to the resin composition obtained by filling the particles with the hexagonal boron nitride agglomerated particles, and can reduce the density and weight of the resin composition. [Background technology]

[0002] Hexagonal boron nitride powder is generally a white powder having a hexagonal layered structure similar to that of graphite, and has many properties such as high thermal conductivity, high electrical insulation, high lubricity, corrosion resistance, mold releasability, high temperature stability, chemical stability, etc. Therefore, resin compositions filled with hexagonal boron nitride powder are suitably used as thermally conductive insulating sheets by molding.

[0003] Moreover, in recent years, there has been an increasing demand for insulating sheets with low dielectric constant, low dielectric tangent, and thermal conductivity for use in high-frequency devices, and the demand for hexagonal boron nitride powder, which has a lower dielectric constant than other highly thermally conductive fillers such as aluminum nitride and aluminum oxide, is also increasing.

[0004] In particular, for use as a low-density, thermally conductive insulating sheet for vehicles, hexagonal boron nitride powder, which has a lower specific gravity than other highly thermally conductive fillers such as aluminum nitride and aluminum oxide, is attracting attention.

[0005] The hexagonal boron nitride agglomerated particles constituting the hexagonal boron nitride powder contain primary particles consisting of scaly particles derived from the crystal structure, and the scaly particles have thermal anisotropy. Therefore, in the case of a thermally conductive insulating sheet using boron nitride powder containing the above-mentioned scaly particles as single particles as a filler, the scaly particles are oriented in the surface direction of the thermally conductive insulating sheet, so that heat is transferred in the c-axis direction of the scaly particles, which has low thermal conductivity, and the thermal conductivity of the thermally conductive insulating sheet in the thickness direction is low.

[0006] In order to improve the thermal anisotropy of hexagonal boron nitride particles having such a scale-like structure, a hexagonal boron nitride powder has been proposed that contains agglomerated particles in which the scale-like particles of hexagonal boron nitride are randomly oriented and aggregated.

[0007] For example, there have been proposed agglomerated particles in which scale-like particles are randomly oriented by spray-drying or the like and then reheating amorphous boron nitride powder, or agglomerated particles in which scale-like particles are randomly oriented, which are produced by press-molding a mixed powder of amorphous boron nitride powder and an auxiliary such as an oxide, sintering the mixture, and then crushing the sintered body in which scale-like particles are randomly oriented (see Patent Document 1). These agglomerated particles have large diameters of the scale-like particles, which are the primary particles constituting the agglomeration, and most of the primary particles have a size exceeding 10 μm. When the boron nitride powder made of the above agglomerated particles is filled in resin, the resin penetrates into the voids between the scale-like primary particles and fills the voids, making it difficult for large air bubbles to exist in the resin composition, and thus the boron nitride powder exhibits high insulation resistance.

[0008] However, there is still room for improvement in the insulation resistance. That is, when filled in resin, the resin easily penetrates into the large gaps, but if the gaps become smaller toward the center of the aggregated particles or if continuous long gaps are formed, there is a concern that relatively large voids that reduce the insulation resistance will remain in the resin composition. This tendency is particularly noticeable when the viscosity of the resin is high. In addition to the above problems, there is a concern that the sintered body may cause a decrease in insulation strength due to the inclusion of impurity elements as sintering aids.

[0009] Furthermore, in the case of the agglomerated particles in which the voids are reduced by allowing resin to penetrate into the voids within the agglomerated particles, the specific gravity of the boron nitride powder in the resin composition is almost the same as that of the bulk body, and it is not possible to reduce the weight of the resin composition. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2017-165609 A Summary of the Invention [Problem to be solved by the invention]

[0011] Therefore, an object of the present invention is to provide hexagonal boron nitride agglomerated particles which can eliminate the anisotropy of thermal conduction by agglomerating scaly primary particles of hexagonal boron nitride, thereby exhibiting high thermal conductivity when filled into a resin, while imparting extremely high dielectric strength to the resin composition obtained when filled into a resin, and further enabling the weight of such a resin composition to be reduced. [Means for solving the problem]

[0012] The present inventors have conducted extensive research to solve the above problems. As a result, they have confirmed that the hexagonal boron nitride agglomerated particles obtained by adopting a specific manufacturing method in which a reduction-nitridation reaction is carried out using an oxygen-containing boron compound, a carbon source, and an oxygen-containing calcium compound, which are known as raw materials for obtaining boron nitride by a reduction-nitridation method, have thermal anisotropy eliminated by aggregation, and the scale-like primary particles are small due to the generation of the agglomerated particles during the reaction, and therefore the gaps formed between the randomly oriented scale-like primary particles are extremely small, so that when the particles are filled into a resin, even if voids are formed in the gaps, the dielectric strength of the resin composition is not reduced, and the presence of such voids reduces the apparent density of the agglomerated particles, making it possible to reduce the weight of the resin composition, thereby solving all of the above problems, and have completed the present invention.

[0013] That is, according to the present invention, there is provided hexagonal boron nitride agglomerated particles (hereinafter also referred to as specific hexagonal boron nitride agglomerated particles), which are agglomerated particles of hexagonal boron nitride primary particles, characterized in that the major axis is 5 to 10 μm, the major axis / minor axis ratio is 1.0 to 1.3, the circularity is in the range of 0.3 to 0.8, and the maximum diameter of the primary particles that can be confirmed on the surface of the agglomerated particles in an SEM observation image at a magnification of 10,000 times is 4 μm or less.

[0014] The hexagonal boron nitride agglomerated particles preferably have a metal impurity element content of 500 ppm or less.

[0015] In addition, by using the specific hexagonal boron nitride agglomerated particles of the present invention together with pore-free hexagonal boron nitride single particles, it is possible to form a hexagonal boron nitride powder that covers the thermal anisotropy of single particles without reducing the dielectric strength. That is, according to the present invention, a hexagonal boron nitride powder containing specific hexagonal boron nitride agglomerated particles and hexagonal boron nitride single particles, the content ratio of the specific hexagonal boron nitride agglomerated particles is 5% or more, and the particle size at 50% cumulative volume frequency of the particle size distribution measured by a wet laser diffraction particle size distribution method (D 50 ) is 5 to 150 μm.

[0016] The hexagonal boron nitride powder obtained by mixing with the above-mentioned hexagonal boron nitride single particles preferably has a volume-based median pore diameter of 3.0 μm or less as measured by mercury intrusion porosimetry.

[0017] Furthermore, the present invention also provides a resin composition containing the above-mentioned boron nitride powder as a filler, which has excellent thermal conductivity and exhibits high dielectric strength, and a resin sheet made of the above-mentioned resin composition. Effect of the Invention

[0018] The specific hexagonal boron nitride agglomerated particles of the present invention are composed of agglomerated particles of fine hexagonal boron nitride scale-like primary particles, and exhibit the effect of eliminating the anisotropy of thermal conductivity due to agglomeration. In addition to the above characteristics, the agglomerated particles have fine pores on their surfaces, thereby exhibiting excellent characteristics not found in conventional agglomerates. That is, the primary particles constituting the specific hexagonal boron nitride agglomerated particles of the present invention are fine, so that the gaps between the particles are extremely small, and unlike the gaps between conventional plate-like particle agglomerated particles, the voids present in the gaps when filled into a resin have almost no effect on the dielectric strength, and a resin composition filled with hexagonal boron nitride powder containing this can exhibit extremely high dielectric strength. In addition, the gaps present in the agglomerated particles can reduce the weight of the hexagonal boron nitride powder, and therefore the weight of the resin composition obtained by filling it.

[0019] In addition, the specific hexagonal boron nitride agglomerated particles of the present invention can be produced without employing a sintering method that requires a sintering aid, and have a low content of impurity elements and can be highly purified, which makes it possible to minimize the decrease in the dielectric strength of the resin composition. [Brief description of the drawings]

[0020] [Figure 1] SEM photo of hexagonal boron nitride agglomerated particles obtained in Example 1 DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] (Hexagonal boron nitride agglomerated particles) The specific hexagonal boron nitride agglomerated particles of the present invention are agglomerated particles of hexagonal boron nitride primary particles, and are characterized in that the major axis is 5 to 10 μm, the major axis / minor axis ratio is 1.0 to 1.3, and the circularity is 0.3 to 0.8, and the maximum diameter of the primary particles that can be confirmed on the surface of the agglomerated particles in an SEM image at a magnification of 10,000 times is 4 μm or less.

[0022] In addition, the hexagonal boron nitride was identified as a hexagonal boron nitride powder by confirming that the sample powder had no peaks other than those of hexagonal boron nitride in the X-ray diffraction measurement. Here, the X-ray diffraction measurement was performed using a fully automatic horizontal multipurpose X-ray diffractometer SmartLab (trade name) manufactured by Rigaku Co., Ltd. The measurement conditions were a scan speed of 20 degrees / min, a step width of 0.02 degrees, and a scan range of 10 to 90 degrees. The GI value representing the crystallinity of the hexagonal boron nitride powder was calculated from the integrated intensity ratio (area ratio) of the (100), (101), and (102) diffraction lines of the X-ray diffraction spectrum of the hexagonal boron nitride powder by the formula, GI=[{(100)+(101)} / [(102)]. The GI value of the hexagonal boron nitride powder is 2.5 or less, and this has also been confirmed in the specific hexagonal boron nitride agglomerated particles obtained in the examples.

[0023] The specific hexagonal boron nitride agglomerated particles of the present invention are composed of agglomerates of scaly primary particles of hexagonal boron nitride, but such agglomerates can be obtained by employing specific reaction conditions for synthesizing hexagonal boron nitride to generate agglomerated particles, rather than by a manufacturing method such as conventional granulation or sintering methods in which scaly hexagonal boron nitride single particles that have already been produced are agglomerated.

[0024] Therefore, the specific hexagonal boron nitride agglomerated particles of the present invention are composed of fine hexagonal boron nitride scale-like primary particles, and the maximum diameter of the primary particles that can be confirmed on the surface of the agglomerated particles in a 10,000x SEM observation image is 4 μm or less, particularly 3 μm or less, and are composed of extremely small primary particles. As a result, the gaps within the agglomerated particles are extremely small, and when filled into a resin, the voids present in the gaps have almost no effect on the dielectric strength, and the resulting resin composition can exhibit extremely high dielectric strength. In addition, the presence of pores (gaps) within and on the surface of the agglomerated particles makes it possible to reduce the weight of the resin composition obtained by filling the hexagonal boron nitride powder.

[0025] The specific hexagonal boron nitride agglomerated particles of the present invention, having a major axis of 5 to 10 μm, a major axis / minor axis ratio of 1.0 to 1.3, and a circularity of 0.3 to 0.8, have excellent flowability when used in combination with other hexagonal boron nitride particles in a resin composition, and are effective in improving the fillability of the resin and the thermal conductivity of the resin composition.

[0026] The long diameter and short diameter were calculated from an SEM image at a magnification of 10,000. The circularity was calculated by calculating 4π×(area) / (perimeter) from an SEM image at a magnification of 10,000 using image analysis software. 2 was calculated using the formula:

[0027] According to the manufacturing method described later, it is difficult to manufacture a pure powder consisting of only the specific hexagonal boron nitride agglomerated particles of the present invention, and agglomerated particles having various shapes and sizes are generated. Therefore, it is preferable to use it as a powder having a high content of the specific hexagonal boron nitride agglomerated particles by removing coarse particles and fine particles by classification or the like.

[0028] As described above, the median diameter of the pores of the specific hexagonal boron nitride agglomerated particles of the present invention cannot be selectively measured, but it has been confirmed that the agglomerated particles constituting the hexagonal boron nitride powder obtained by the manufacturing method described below have a similar pore structure, and therefore the pore diameter of the hexagonal boron nitride powder can be measured to specify the median diameter of the pores of the specific hexagonal boron nitride agglomerated particles. In the present invention, the median diameter of the pores of such specific hexagonal boron nitride agglomerated particles is preferably 3.0 μm or less, preferably 2.8 μm, and more preferably 2.5 μm or less. Similarly, the pore volume of the pores having a pore diameter of 3 μm or less of the specific hexagonal boron nitride agglomerated particles of the present invention can be determined to be 0.5 cm or less. 3 / g or more, preferably 0.5 to 2.0 cm 3 It is preferred that the molecular weight is / g.

[0029] The pore volume-based median diameter and pore volume were calculated from the cumulative pore distribution in which pores of 0.0036 μm to 200 μm were measured by mercury intrusion porosimetry using an Autopore IV9520 manufactured by Micromeritics, and the pore diameter was plotted on the horizontal axis and the cumulative pore volume was plotted on the vertical axis.

[0030] The specific hexagonal boron nitride agglomerated particles of the present invention are obtained by a manufacturing method described below that does not use a sintering aid, so there is no decrease in purity due to the sintering aid and they are high purity, and when used as a filler in a resin composition that constitutes an insulating sheet, for example, they work together with the effect of the small pores to contribute to improving voltage resistance. That is, the specific hexagonal boron nitride agglomerated particles of the present invention preferably have an impurity element content of 500 ppm or less, particularly 400 ppm or less.

[0031] The impurity elements referred to here are calcium, magnesium, sodium, aluminum, lithium, strontium, iron, sulfur, nickel, chromium, manganese, silicon, phosphorus, titanium, barium, and cobalt. The content of the impurity elements refers to the total content of the impurity elements.

[0032] The impurity element content of the hexagonal boron nitride agglomerated particles is a value measured by X-ray fluorescence analysis of the hexagonal boron nitride powder obtained by the production described below. In the examples, a ZSX Primus2 (product name) manufactured by Rigaku Corporation was used as the X-ray fluorescence analyzer.

[0033] The specific hexagonal boron nitride agglomerated particles of the present invention have a C% of 0.04% or less and an O% of 0.4% or less, which, in combination with the low amounts of the impurity elements, is more effective in improving thermal conductivity and dielectric strength.

[0034] The O% of the hexagonal boron nitride agglomerated particles was measured using an oxygen / nitrogen analyzer EMGA-620 manufactured by Horiba, Ltd. The C% of the hexagonal boron nitride powder was measured using an EMIA-110 manufactured by Horiba, Ltd.

[0035] The specific hexagonal boron nitride agglomerated particles of the present invention can be used in combination with other hexagonal boron nitride particles to form a hexagonal boron nitride powder. The hexagonal boron nitride powder is essentially a mixture of hexagonal boron nitride powder consisting of the specific hexagonal boron nitride agglomerated particles and hexagonal boron nitride agglomerated particles inevitably produced in the reaction, and hexagonal boron nitride powder containing other hexagonal boron nitride particles. Therefore, the powder mixed with other hexagonal boron nitride particles is also called "mixed hexagonal boron nitride powder".

[0036] The mixed hexagonal boron nitride powder contains specific hexagonal boron nitride agglomerated particles and other hexagonal boron nitride particles, particularly hexagonal boron nitride single particles, and the content ratio of the specific hexagonal boron nitride agglomerated particles is 5% or more, preferably 10% or more, and more preferably 20% or more, and the particle size at 50% cumulative volume frequency of the particle size distribution measured by a wet laser diffraction particle size distribution method (D 50 ) is preferably 5 to 150 μm, and more preferably 20 to 100 μm.

[0037] In the present invention, the content ratio (%) of specific hexagonal boron nitride agglomerated particles in the hexagonal boron nitride powder, including the mixed hexagonal boron nitride powder, can be obtained by the following method. First, using a dry vibration sieve KFC-500-1D manufactured by KOWA Corporation, the hexagonal boron nitride powder was sieved up and down through a 45 μm sieve using a SUS mesh with an opening of 45 μm for 30 minutes, and the weight ratio X% of the particles that fell under the 45 μm sieve was obtained. Then, the specific hexagonal boron nitride agglomerated particles and other particles were separated from the SEM observation image of the recovered 45 μm sieve at a magnification of 500 times, and the SEM observation image area ratio Y% of the specific hexagonal boron nitride agglomerated particles that fell under the 45 μm sieve was obtained. Finally, the hexagonal boron nitride agglomerated particle ratio of the present invention is determined by multiplying the 45 μm sieve weight ratio X% by the 45 μm sieve hexagonal boron nitride agglomerated particle SEM observation image area ratio Y% (X×Y×0.01)%. For example, if the 45 μm sieve weight ratio X of the hexagonal boron nitride powder is 20 wt%, and the 45 μm sieve hexagonal boron nitride agglomerated particle SEM observation image area ratio Y is 60%, the hexagonal boron nitride agglomerated particle ratio Z of the present invention is calculated as 20×60×0.01=12%.

[0038] In the present invention, the other hexagonal boron nitride powder to be mixed is not particularly limited, but a powder consisting of hexagonal boron nitride single particles that suppresses the generation of voids after filling into a resin is preferable. The above-mentioned hexagonal boron nitride single particles are generally flat in shape and have anisotropy in thermal conduction, but when filled into a resin, the anisotropy is eliminated by contact with the hexagonal boron nitride agglomerated particles of the present invention, and excellent thermal conductivity can be exhibited.

[0039] The above-mentioned hexagonal boron nitride single particles preferably have an aspect ratio (ratio of the major axis to the thickness of the particle (major axis / thickness)) of 3 to 20, and a major axis of 1 to 30 μm. It is also possible to use hexagonal boron nitride agglomerated particles other than the specific hexagonal boron nitride agglomerated particles in combination, within a range that does not significantly impair the effects of the present invention provided by the specific hexagonal boron nitride agglomerated particles.

[0040] The hexagonal boron nitride powder of the present invention, which contains specific hexagonal boron nitride agglomerated particles, has a particle size at 50% cumulative volume frequency (D 50 ) is 5 to 150 μm, preferably 6 to 100 μm, and particularly preferably 7 to 80 μm.

[0041] In the present invention, the hexagonal boron nitride powder containing the specific hexagonal boron nitride agglomerated particles and other hexagonal boron nitride particles has a median diameter of pores of 3.0 μm or less, preferably 2.8 μm or less, and more preferably 2.5 μm or less, similar to the specific hexagonal boron nitride agglomerated particles. Also, the hexagonal boron nitride powder has a pore volume of pores having a pore diameter of 3 μm or less of 0.5 cm 3 / g or more, preferably 0.5 to 2.0 cm 3 As described above, in order to maintain the characteristics of the specific hexagonal boron nitride agglomerated particles, the other hexagonal boron nitride particles in the hexagonal boron nitride powder are preferably single particles.

[0042] The pore volume-based median diameter and pore volume can be measured in the same manner as in the specific hexagonal boron nitride agglomerated particles.

[0043] (Method for producing specific hexagonal boron nitride agglomerated particles) In the present invention, the method for producing the specific hexagonal boron nitride agglomerated particles is not particularly limited. A representative example of the production method is to mix an oxygen-containing boron compound having a residue on a 425 μm sieve of 3% by weight or less, a carbon source, and an oxygen-containing calcium compound in an amount of 0.63 to 0.73 in terms of B / C (element ratio) which is the ratio of the B source contained in the oxygen-containing boron compound to the C source contained in the carbon source, and a total amount of the oxygen-containing boron compound and the carbon source (B 2 O 3 and mixing 100 parts by mass of the mixture (calculated as C) with 4 to 12 parts by mass of an oxygen-containing calcium compound, calculated as CaO, and heating the resulting mixture to a maximum temperature of 1,910 to 2,000°C in a nitrogen atmosphere to perform reduction-nitridation. After that, by-products other than boron nitride present in the reaction product are removed by acid washing. By this production method, the hexagonal boron nitride powder containing the hexagonal boron nitride agglomerated particles of the present invention can be obtained.

[0044] (raw materials) The greatest feature of the manufacturing method of the present invention is that the raw materials, an oxygen-containing boron compound with a controlled particle size, a carbon source, and an oxygen-containing calcium compound, are mixed in a prescribed ratio as described below, and are reduced and nitrided at a high temperature of 1910° C. or higher. The role of each raw material is as follows:

[0045] (Oxygen-containing boron compound) In the above-mentioned production method, as the oxygen-containing boron compound as the raw material, any compound containing a boron atom can be used without any limitation. For example, boric acid, boric anhydride, metaboric acid, perboric acid, hypoboric acid, sodium tetraborate, sodium perborate, etc. can be used. In general, boric acid and boron oxide, which are easily available, are preferably used. In addition, it is preferable that the average particle size of the oxygen-containing boron compound used is such that the residue on a 425 μm sieve is 3% by mass or less, preferably 1.5% by mass or less. In particular, it is more preferable that the residue on a 300 μm sieve is 50% or less, and even more preferable that the residue on a 250 μm sieve is 70% or less. In other words, if the residue on the 425 μm sieve of the oxygen-containing boron compound is 3% by weight or more, coarse boron nitride agglomerated particles of 150 μm or more are likely to remain, and the remaining voids within the coarse agglomerated particles will increase, causing the median diameter of the pores in the resulting hexagonal boron nitride powder to exceed 3 μm, resulting in a decrease in dielectric strength.

[0046] (Oxygen-containing calcium compounds) In the above-mentioned production method, the oxygen-containing calcium compound forms a composite oxide with the oxygen-containing boron compound, thereby forming a composite oxide having a high melting point, and thus has the role of preventing the volatilization of the oxygen-containing boron compound.

[0047] In the above-mentioned production method, the oxygen-containing calcium compound used as the catalyst and the volatilization inhibitor for the oxygen-containing boron compound may be any known compound without any particular limitation, but an oxygen-containing calcium compound containing oxygen and calcium is preferably used. Examples of the oxygen-containing calcium compound include calcium carbonate, calcium bicarbonate, calcium hydroxide, calcium oxide, calcium nitrate, calcium sulfate, calcium phosphate, calcium oxalate, etc. Two or more of these compounds may be mixed and used. Among them, calcium oxide and calcium carbonate are preferably used.

[0048] The oxygen-containing calcium compound may be used in combination of two or more kinds. The average particle size of the oxygen-containing calcium compound is preferably 0.01 to 200 μm, more preferably 0.05 to 120 μm, and particularly preferably 0.1 to 80 μm.

[0049] (Carbon Source) In the above-mentioned production method, the carbon source may be any known carbon material acting as a reducing agent, without any particular limitation. Examples of the carbon source include amorphous carbon such as carbon black, activated carbon, and carbon fiber, crystalline carbon such as diamond, graphite, and nanocarbon, and pyrolytic carbon obtained by pyrolyzing monomers and polymers. Among them, highly reactive amorphous carbon is preferred, and carbon black is particularly preferred because it is industrially quality controlled. As the carbon black, acetylene black, furnace black, thermal black, and the like may be used. The average particle size of the carbon source is preferably 0.01 to 5 μm, more preferably 0.02 to 4 μm, and particularly preferably 0.05 to 3 μm. That is, by making the average particle size of the carbon source 5 μm or less, the reactivity of the carbon source is increased, and by making it 0.01 μm or more, the carbon source is easily handled.

[0050] In the above-mentioned production method, the form of the mixture containing the above-mentioned raw materials to be supplied to the reaction is not particularly limited. The mixture may be in a powder form as is, or may be formed into granules.

[0051] In the production method of the present invention, the method for mixing the raw materials is not particularly limited, and a general mixer such as a vibration mill, a bead mill, a ball mill, a Henschel mixer, a drum mixer, a vibration agitator, or a V-shaped mixer can be used.

[0052] In addition, the granulation method when granulation is performed can be carried out by a known method such as extrusion granulation, rolling granulation, granulation by a compactor, etc., using a binder as necessary. In this case, the size of the granules is preferably about 5 to 10 mm.

[0053] (Preparation of raw materials) In the above-mentioned manufacturing method, the reduction-nitridation reaction is carried out by supplying a carbon source and nitrogen, and in order to effectively obtain the desired hexagonal boron nitride agglomerated particles, the ratio of the B source and the carbon source contained in the oxygen-containing boron compound must be 0.63 to 0.73, preferably 0.65 to 0.72, calculated as B / C (element ratio). That is, if the molar ratio exceeds 0.73, the ratio of boron compounds that are not reduced and volatilize increases, and they tend to form a complex oxide with the Ca auxiliary, and the melting point of the complex oxide is low, and the plate-like particles tend to grow, making it difficult to obtain the desired agglomerated particles with small primary particles and pores. Also, if the molar ratio is less than 0.63, the carbon content is high, and there is a risk of carbon-derived impurities remaining.

[0054] In the above-mentioned production method, in order to effectively obtain the desired hexagonal boron nitride agglomerated particles, the total amount of the oxygen-containing boron compound and the carbon source (B 2 O 3 It is necessary to mix the oxygen-containing calcium compound in a ratio of 4 to 12 parts by mass, calculated as CaO, with 100 parts by mass of calcium hydroxide (calculated as C). If the amount of CaO converted is less than 4 parts by mass, the proportion of boron compounds that are not reduced and volatilize increases, resulting in a decrease in yield, and the remaining boron compounds and the resulting CaO-B 2 O 3 The melting point of the composite oxide is lowered, and the grain growth of the hexagonal boron nitride particles is promoted, which makes it difficult to form the desired aggregated particles having pores, which is undesirable. If the CaO equivalent mass part is 12 parts by mass or more, there is a risk that calcium-derived impurities will remain, which is undesirable.

[0055] In the present invention, by adjusting the particle size and composition ratio of the raw materials, the targeted excessive particle growth is prevented, and agglomerated particles having a small primary particle size can be produced with high selectivity. (Reduction Nitridation) In the above-mentioned production method, the nitrogen source can be supplied to the reaction system by a known means. For example, the most common method is to circulate nitrogen gas through the reaction system of the reaction device exemplified later. The nitrogen source to be used is not limited to the above-mentioned nitrogen gas, and is not particularly limited as long as it is a gas capable of nitridation in the reduction-nitridation reaction. Specifically, in addition to the above-mentioned nitrogen gas, ammonia gas can also be used. Also, a gas obtained by mixing nitrogen gas or ammonia gas with a non-oxidizing gas such as hydrogen, argon, or helium can also be used.

[0056] In the above-mentioned manufacturing method, in order to obtain a hexagonal boron nitride powder having high crystallinity and pores, it is necessary to adopt a heating temperature in the reduction-nitridation reaction of usually 1910°C to 2000°C, preferably 1920°C to 1980°C. By setting the heating temperature at 1910°C to 2000°C, the crystallinity of the hexagonal boron nitride particles is improved, the outer circumference of the primary particle shape becomes sharper, and the number of fine pores between the particles increases. Furthermore, if the temperature is less than 1910°C, the reduction-nitridation reaction does not proceed and it is difficult to obtain white hexagonal boron nitride with high crystallinity, and if the temperature exceeds 2000°C, the effect reaches a plateau, which is not only economically disadvantageous but also undesirably increases damage to the heating furnace.

[0057] The time for the reduction-nitridation reaction is appropriately determined, but is generally about 6 to 30 hours.

[0058] The above-mentioned production method can be carried out using a known reaction apparatus capable of controlling the reaction atmosphere, for example, an atmosphere-controlled high-temperature furnace in which heat treatment is performed by high-frequency induction heating or heater heating, and a batch furnace, as well as a continuous furnace such as a pusher-type tunnel furnace or a vertical reaction furnace, can also be used.

[0059] (acid washing) In the above-mentioned production method, the reaction product obtained by the above-mentioned reduction nitridation contains impurities such as a composite oxide composed of boron oxide-calcium oxide in addition to the hexagonal boron nitride powder, so it is preferable to wash it with an acid. There is no particular limitation on the method of acid washing, and any known method can be used without limitation. For example, there is a method in which the by-product-containing boron nitride obtained after the nitriding treatment is crushed and placed in a container, and dilute hydrochloric acid (5 to 20 mass % HCl) is added in an amount 5 to 10 times the amount of the hexagonal boron nitride powder containing the impurities, and the mixture is allowed to come into contact for 4 to 8 hours.

[0060] As the acid used in the above-mentioned acid washing, other than hydrochloric acid, nitric acid, sulfuric acid, acetic acid, etc. can also be used.

[0061] After the acid washing, the boron nitride is washed with pure water to remove the remaining acid. The washing method involves filtering the acid, dispersing the acid-washed boron nitride in the same amount of pure water as the acid used, and filtering again.

[0062] (Dry) The conditions for drying the hydrous aggregate after the acid washing and water washing are preferably drying in the air or under reduced pressure at 50 to 250° C. The drying time is not particularly specified, but it is preferable to dry until the moisture content approaches 0%.

[0063] (classification) The dried boron nitride powder is preferably crushed as necessary, and then subjected to removal of coarse particles using a sieve or the like, removal of fine powder using air flow classification or the like, and wet classification to obtain a hexagonal boron nitride powder having a high content of specific hexagonal boron nitride agglomerated particles. The classification is particularly preferably a dry sieve classification process, and the mesh size is preferably 30 to 90 μm.

[0064] (Applications of boron nitride powder) The use of the boron nitride powder containing the hexagonal boron nitride agglomerated particles of the present invention is not particularly limited, and it can be applied to known uses without particular limitation. An example of a suitable use is use as a filler in a resin for the purpose of improving electrical insulation and imparting thermal conductivity. In the above-mentioned use of the boron nitride powder, the obtained resin composition has high thermal conductivity and high electrical insulation with a dielectric strength of 80 kV / mm or more.

[0065] The resin composition of the present invention can be used for known applications without any restrictions, but by mixing it with a resin described later to form a thermally conductive resin composition or a thermally conductive molded body, it can be preferably used for applications such as thermal interface materials such as polymer-based heat dissipation sheets and phase change sheets, organic heat dissipation sheets such as heat dissipation tapes, heat dissipation greases, heat dissipation adhesives, and gap fillers, heat dissipation paints such as heat dissipation paints and heat dissipation coats, heat dissipation resin substrates such as PWB-based resin substrates and CCL-based resin substrates, insulating layers for metal-based substrates such as aluminum-based substrates and copper-based substrates, sealing materials for power devices, and interlayer insulating films.

[0066] Furthermore, when the boron nitride powder of the present invention is prepared into a resin composition, it can be mixed with a thermally conductive filler such as aluminum nitride or aluminum oxide, which is a common highly thermally conductive insulating filler.

[0067] Examples of the resin include thermoplastic resins such as polyolefin, vinyl chloride resin, methyl methacrylate resin, nylon, and fluororesin; thermosetting resins such as epoxy resin, phenol resin, urea resin, melamine resin, unsaturated polyester resin, silicone resin, and bismaleimide triazine resin; fluororesin, liquid crystal polymer, and synthetic rubber.

[0068] The resin composition may contain, as necessary, known additives such as polymerization initiators, curing agents, polymerization inhibitors, polymerization retarders, coupling agents, plasticizers, UV absorbers, pigments, dyes, antibacterial agents, organic fillers, organic-inorganic composite fillers, etc., as compounding agents for resin compositions. In addition, other inorganic fillers may be contained within the range that does not impair the effects of the present invention.

[0069] The boron nitride powder of the present invention can also be used as a raw material for boron nitride processed products such as cubic boron nitride and boron nitride molded products, a nucleating agent for engineering plastics, a phase change material, a solid or liquid thermal interface material, a release agent for molten metal or molten glass molds, cosmetics, and a raw material for composite ceramics. EXAMPLES

[0070] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0071] In the examples, the values ​​measured were those obtained by the following methods.

[0072] [Median pore diameter based on volume (μm)] [Volume of pores smaller than 3 μm (cm 3 / g)] The pore volume median diameter D1 of the sample hexagonal boron nitride powder was measured by mercury intrusion porosimetry. The pore volume median diameter and the volume of pores of 3 μm or less were calculated from the cumulative pore distribution obtained by plotting the pore diameter on the horizontal axis and the cumulative pore volume on the vertical axis when determining the pore distribution from 0.0036 μm to 200 μm. The calculation was performed using an Autopore IV9520 manufactured by Micromeritics.

[0073] [Particle size at 50% cumulative volume frequency of wet particle size distribution of hexagonal boron nitride powder (D2) (μm)] For the sample hexagonal boron nitride powder, the particle size at 50% cumulative volume frequency of the particle size distribution (D 50 ) was measured. The particle size distribution of the hexagonal boron nitride powder was measured using a particle size distribution analyzer MT3000 manufactured by Nikkiso Co., Ltd. The measurement sample was prepared by the following method. First, 20 g of ethanol was added as a dispersion medium to a 50 mL screw tube bottle, and 1 g of hexagonal boron nitride powder was dispersed in the ethanol. The particle size at 50% cumulative volume frequency of the obtained particle size distribution (D50 ) was designated as (D2).

[0074] [Hexagonal boron nitride powder impurity element concentration (mass%)] The concentrations of impurity elements (calcium, magnesium, sodium, aluminum, lithium, strontium, iron, sulfur, nickel, chromium, manganese, silicon, phosphorus, titanium, barium, and cobalt) in the sample hexagonal boron nitride powder were measured using a Rigaku ZSX Primus2 (product name).

[0075] Example 1 195 g of boron oxide with a residue on a 425 μm sieve of 2.1% by weight, 99 g of carbon black, and 55.2 g of calcium carbonate were mixed using a Spartan mixer. The (B / C) element ratio of the mixture was 0.68. The oxygen-containing boron compound, the carbon source, and the B 2 O 3 The content ratio of the oxygen-containing calcium compound in terms of CaO was 10.5 parts by mass relative to 100 parts by mass of the total mass converted into C. 1500 g of the mixture was subjected to nitriding treatment in a graphite Tammann furnace by holding the mixture at 1500° C. for 6 hours and at 1940° C. for 4 hours in a nitrogen gas atmosphere.

[0076] Next, the by-product-containing boron nitride was crushed and placed in a container, and hydrochloric acid (7 mass% HCl) was added in an amount 5 times the amount of the by-product-containing boron nitride, and the mixture was stirred for 24 hours at a rotation speed of 350 rpm by a three-one motor. After the acid washing, the acid was filtered, and the boron nitride obtained by filtration was dispersed in pure water in the same amount as the acid used, and filtered again. This operation was repeated until the aqueous solution after filtration became neutral, and then the mixture was vacuum dried at 200°C for 12 hours.

[0077] The powder obtained after drying was sieved through a sieve with an opening of 45 μm to obtain a white hexagonal boron nitride powder containing specific hexagonal boron nitride agglomerated particles. From the SEM observation image at a magnification of 10,000 times, it was confirmed that the major axis of the obtained hexagonal boron nitride powder was 5 to 10 μm, the major axis / minor axis was 1.0 to 1.3, the circularity was in the range of 0.3 to 0.8, and the maximum diameter of the primary particles that could be confirmed on the surface of the agglomerated particles was 4 μm or less. In addition, the presence ratio of the specific hexagonal boron nitride agglomerated particles calculated from the area ratio of the SEM observation image at a magnification of 500 times was 53%. In addition, the specific major axis, major axis / minor axis, circularity, and maximum diameter of the primary particles for one particle near the average particle size of the obtained specific hexagonal boron nitride agglomerated particles are shown in Table 2. Furthermore, the content of impurity elements in the specific hexagonal boron nitride agglomerated particles specified from the measurements of the obtained hexagonal boron nitride powder, the pore volume median diameter D1 (μm), and the pore volume (cm) of pores with a pore diameter of 3 μm or less 3 The average particle size distribution (μm / g) is also shown in Table 1. The impurity element concentration was 40 ppm. The oxygen concentration was 0.2%, and the carbon concentration was 0.01%.

[0078] Moreover, an SEM image of the representative specific hexagonal boron nitride agglomerated particles obtained in Example 1 is shown in FIG.

[0079] [Mixed hexagonal boron nitride powder and resin composition] 100 parts by mass of the boron nitride powder containing the specific hexagonal boron nitride agglomerated particles produced in this manner was mixed with 5 parts by mass of commercially available hexagonal boron nitride powder consisting of single particles of hexagonal boron nitride (wet particle size distribution D2=10 μm, average aspect ratio 10, impurity element concentration 40 ppm, oxygen concentration 0.2%, carbon concentration 0.01%) to obtain a mixed hexagonal boron nitride powder. The pore volume median diameter D1 (μm) and pore volume (cm) of pores with a pore diameter of 3 μm or less were measured for the obtained mixed hexagonal boron nitride powder. 3 / g) and the particle size D2 (μm) at 50% cumulative volume frequency in the wet particle size distribution are shown in Table 2.

[0080] The mixed hexagonal boron nitride powder was filled into epoxy resin to prepare a resin composition, and the thermal conductivity was evaluated. The epoxy resin was prepared by mixing 100 parts by mass (JER828 manufactured by Mitsubishi Chemical Corporation), 5 parts by mass of a curing agent (imidazole-based curing agent, Curesol 2E4MZ manufactured by Shikoku Kasei Co., Ltd.), and 210 parts by mass of methyl ethyl ketone as a solvent. Next, the varnish-like mixture and the hexagonal boron nitride powder were mixed in a rotation-revolution mixer (MAZERUSTAR manufactured by Kurashiki Boseki Co., Ltd.) so that the base resin was 35% by volume and the hexagonal boron nitride powder was 65% by volume, to obtain a resin composition.

[0081] The above resin composition was coated on a PET film to a thickness of about 250 to 300 μm using an automatic coater PI-1210 manufactured by Tester Sangyo Co., Ltd., dried, and cured under reduced pressure at a temperature of 200°C, a pressure of 5 MPa, and a retention time of 30 minutes to produce a sheet with a thickness of 220 μm. The sheet was analyzed using a temperature wave thermal analyzer to calculate the thermal conductivity. In addition, the dielectric strength was measured using a withstand voltage tester (manufactured by Tama Densoku Co., Ltd.). The results are also shown in Table 2.

[0082] Example 2 The residue on the 425μm sieve of boron oxide was 2.8% by weight, the (B / C) element ratio was 0.73, and the boron-containing oxygen compound was a carbon source. 2 O 3 The same procedure as in Example 1 was followed, except that the content ratio of the oxygen-containing calcium compound in terms of CaO was 8.2 parts by mass relative to 100 parts by mass of the total mass converted into C. The conditions and measured values ​​are shown in Table 1. The impurity element concentration was 20 ppm. The oxygen concentration was 0.2%, and the carbon concentration was 0.01%.

[0083] [Mixed hexagonal boron nitride powder and resin composition] Using the boron nitride powder containing the specific hexagonal boron nitride agglomerated particles thus produced, a mixed hexagonal boron nitride powder was prepared in the same manner as in Example 1, which was then mixed with a resin to prepare a resin composition, and the thermal conductivity and dielectric strength were measured. The results are shown in Table 2.

[0084] Example 3 The residue on the 425μm sieve of boron oxide is 1.0wt%, the (B / C) element ratio is 0.66, oxygen-containing boron compound, carbon source, B 2 O 3 The same procedure as in Example 1 was followed, except that the content ratio of the oxygen-containing calcium compound in terms of CaO was 7 parts by mass relative to 100 parts by mass of the total mass in terms of C. The conditions and measured values ​​are shown in Table 1. The impurity element concentration was 20 ppm. The oxygen concentration was 0.2%, and the carbon concentration was 0.01%.

[0085] [Mixed hexagonal boron nitride powder and resin composition] Using the boron nitride powder containing the specific hexagonal boron nitride agglomerated particles thus produced, a mixed hexagonal boron nitride powder was prepared in the same manner as in Example 1, which was then mixed with a resin to prepare a resin composition, and the thermal conductivity and dielectric strength were measured. The results are shown in Table 2.

[0086] Example 4 The same procedure was followed as in Example 1, except that the boron oxide residue on a 425 μm sieve was 0.1% by weight and the residue on a 300 μm sieve was 15.0% by weight. The conditions and measured values ​​are shown in Table 1. The impurity element concentration was 20 ppm. The oxygen concentration was 0.2%, and the carbon concentration was 0.01%.

[0087] [Mixed hexagonal boron nitride powder and resin composition] Using the boron nitride powder containing the specific hexagonal boron nitride agglomerated particles thus produced, a mixed hexagonal boron nitride powder was prepared in the same manner as in Example 1, which was then mixed with a resin to prepare a resin composition, and the thermal conductivity and dielectric strength were measured. The results are shown in Table 2.

[0088] Example 5 The residue on the 425 μm sieve of boron oxide is 0.5 wt%, the (B / C) element ratio is 0.70, and the oxygen-containing boron compound and carbon source are B 2 O 3The same procedure was followed as in Example 1, except that the content ratio of the oxygen-containing calcium compound in terms of CaO relative to 100 parts by mass of the total mass converted into C was 8 parts by mass. The measured values ​​are shown in Table 1. The impurity element concentration was 20 ppm. The oxygen concentration was 0.2%, and the carbon concentration was 0.01%.

[0089] Example 6 100 parts by mass of the boron nitride powder containing specific hexagonal boron nitride agglomerated particles produced in Example 1 was mixed with 15 parts by mass of commercially available hexagonal boron nitride single particle hexagonal boron nitride powder (wet particle size distribution D2 = 10 μm, average aspect ratio 10, impurity element concentration 40 ppm, oxygen concentration 0.2%, carbon concentration 0.01%) to prepare a mixed hexagonal boron nitride powder, which was further mixed with a resin in the same manner as in Example 1 to prepare a resin composition, and the thermal conductivity and dielectric strength were measured. The results are also shown in Table 2.

[0090] [Table 1]

[0091] [Table 2]

[0092] As described above, the thermal conductivity of the sheets filled with the hexagonal boron nitride powder produced in Examples 1 to 6 was 9.0 W / m K or more, indicating high thermal conductivity. In addition, the sheets had a high dielectric strength of 80 kV / mm or more, suggesting that there was little large void volume in the resin composition that could cause a decrease in dielectric strength.

[0093] For comparison, instead of the specific hexagonal boron nitride agglomerated particles of Example 1, agglomerated particles having a primary particle diameter of 8 μm were used. 50 A mixed hexagonal boron nitride powder was prepared in the same manner as in Example 1 using commercially available hexagonal boron nitride powder with a particle size of 25 μm. A resin composition was prepared using this and various tests were performed. The thermal conductivity was low, at 8.8 W / m K, and the dielectric strength was low, at 65 kV / mm.

Claims

1. Hexagonal boron nitride agglomerated particles are agglomerated particles of hexagonal boron nitride primary particles, characterized in that the long axis is 5 to 10 μm, the long axis / short axis ratio is 1.0 to 1.3, and the circularity is in the range of 0.3 to 0.8, and the maximum diameter of the primary particles that can be confirmed on the surface of the agglomerated particles in an SEM image at a magnification of 10,000 times is 4 μm or less.

2. 2. The hexagonal boron nitride agglomerated particles according to claim 1, having a content of metal impurities of 500 ppm or less.

3. The present invention relates to a method for producing a hexagonal boron nitride agglomerated particle of claim 1 or 2, and a hexagonal boron nitride single particle, the content of the hexagonal boron nitride agglomerated particles being 5% or more, and the particle size at a cumulative volume frequency of 50% in a particle size distribution measured by a wet laser diffraction particle size distribution method (D 50 ) is 5 to 150 μm.

4. 4. The hexagonal boron nitride powder according to claim 3, wherein the volume-based median diameter of the pores measured by mercury intrusion porosimetry is 3.0 μm or less.

5. A resin composition comprising the hexagonal boron nitride powder according to claim 3 or 4.

6. A resin sheet comprising the resin composition according to claim 5.

7. 7. The resin sheet according to claim 6, having a dielectric strength of 80 kV / mm or more.

Citation Information

Patent Citations

  • Primary particle aggregate of hexagonal boron nitride, resin composition and application of the same

    JP2017165609A

  • Hexagonal boron nitride powder and method for producing the same

    JP2017222522A

  • Hexagonal boron nitride powder and manufacturing method therefor

    JP2019218254A

  • Process for producing boron nitride agglomerates

    JP2019521064A

  • Boron nitride powder and resin composition

    WO2020158758A1