Water-based polyurethane dispersions and their preparation

Glycol ether ketones replace NMP in polyurethane dispersion synthesis, addressing regulatory concerns and maintaining film quality and stability in polyurethane dispersions.

JP7588584B2Active Publication Date: 2024-11-22DOW GLOBAL TECHNOLOGIES LLC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021532134
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-12-06
Filing Date
2019-11-19
Publication Date
2024-11-22
Estimated Expiration
2039-11-19

AI Technical Summary

Technical Problem

The use of N-methyl-2-pyrrolidone (NMP) as a solvent in polyurethane dispersion synthesis is regulated due to reproductive toxicity concerns, and alternative solvents are needed to maintain film quality without interfering with prepolymer formation.

Method used

The use of glycol ether ketones as solvents in the prepolymer process for polyurethane dispersions, which remain stable during dispersion and can act as coalescing aids, replacing NMP.

Benefits of technology

Glycol ether ketones provide a non-toxic alternative that maintains film quality and stability, ensuring effective dispersion and coalescence in polyurethane films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588584000011
    Figure 0007588584000011
  • Figure 0007588584000001
    Figure 0007588584000001
  • Figure 0007588584000002
    Figure 0007588584000002
Patent Text Reader

Abstract

The prepolymer containing acid groups is produced by a process comprising the steps of contacting (i) a diisocyanate, (ii) a polyol containing acid groups, and (iii) a polyol without acid groups, wherein the contacting is carried out under reactive conditions in a solvent consisting essentially of (A) a first component consisting essentially of at least one glycol ether ketone, and (B) optionally a second component consisting essentially of at least one aprotic glycol ether. The prepolymer is useful for preparing water-based polyurethane dispersions.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] SUMMARY OF THE DISCLOSURE Embodiments of the present invention relate to water-based polyurethane dispersions (PUDs), processes for making prepolymers for PUDs, and processes for making PUDs. [Background technology]

[0002] Water-based polyurethane dispersions (PUDs) are versatile products that are often used in various coating and adhesive formulations, either by themselves or in combination with other types of polymers. There are two different techniques for the commercial production of polyurethane dispersions: the acetone process and the prepolymer process. The prepolymer process is more widely used because acetone is a flammable solvent. The prepolymer process for PUD preparation is a two-step process. In step 1, polyurethane / polyurea is synthesized in the presence of an aprotic solvent, which helps to solubilize reactants such as isocyanates, diols, and dimethylolpropionic acid (DMPA) and reduce the viscosity of the reaction mixture. In step 2, this prepolymer is dispersed in water with the help of surface-active moieties. Quaternary ammonium salts, incorporated into the polyurethane structure by neutralizing DMPA with tertiary amines, provide sufficient ionicity that helps disperse the polymer in aqueous media. N-methyl-2-pyrrolidone (NMP) is one of the most widely used aprotic solvents for PUD synthesis. NMP is a good solvent for the synthesis of prepolymers, aids in the dispersion process, and ultimately acts as a coalescing aid when the PUD is applied as a film on the substrate. Additional information on PUD preparation with NMP can be found in the web publication “Polyurethane Dispersions”, CJ Hauthaway and Sons Corp. of Lynn, MA, and elsewhere in the technical literature. Although NMP is an excellent solvent for PUD synthesis, it has recently been classified as a potential reproductive toxicant under the Registration, Evaluation, Authorization, and Restriction of Chemicals (REACH), raising safety and regulatory concerns in the European Union and influencing regulations at a global level. This has accelerated the active search for suitable replacements.

[0003] Alkyl ketones such as acetone, methyl isobutyl ketone (MIBK), and methyl amyl ketone (MAK) can be used as solvents for prepolymer synthesis. For example, “Waterborne Polyurethane Coatings for Wood Floors” by Gertzmann et al., a web publication from Bayer Materials Science, Pittsburgh, PA, describes the acetone process for PUDs. However, due to their high volatility and poor performance as coalescing aids, alkyl ketones are usually removed from the prepolymer before the dispersion step that produces the PUD. For this reason, to obtain a suitable film from the PUD, it is necessary to add a coalescing aid such as dipropylene glycol mono n-butyl ether (e.g., DOWANOL™ DPnB) or other known coalescing aids used in coating formulations (see, for example, Hauthaway's publications). Although excellent coalescing aids, monoglycol ethers cannot be used for prepolymer synthesis because they have hydroxyl groups that react with isocyanates and interfere with the formation of the prepolymer.

[0004] An ideal solvent for PUD synthesis should be compatible with water-based PUDs with good affinity for polyols containing acid groups, such as, for example, DMPA. Summary of the Invention

[0005] The present invention relates to a process for making prepolymers containing acid groups, a process for making water-based PUDs, blends that can be used as solvents in making PUDs, and PUDs. The present invention utilizes glycol ether ketones as solvents for the preparation of PUDs. Such glycol ether ketones have been discovered to advantageously encompass properties desirable for the complete preparation of PUDs in that they are aprotic, are good solvents for prepolymer synthesis, can remain in the prepolymer during the dispersion step without compromising the stability of the final PUD, or have no volatility concerns and / or can function as coalescing aids for polyurethane films cast from the PUDs.

[0006] In some embodiments, the present invention provides a method for the preparation of a (i) a diisocyanate; (ii) a polyol containing an acid group; and (iii) a polyol having no acid groups, The contacting step comprises: (A) a first component comprising at least one glycol ether ketone; (B) optionally, a second component consisting of at least one aprotic glycol ether.

[0007] In some embodiments, the present invention provides a method for the preparation of a (1) (i) a diisocyanate; (ii) a polyol containing an acid group; and (iii) forming a prepolymer having acid groups by contacting a polyol having no acid groups with The contacting step comprises under reaction conditions: (A) a first component comprising at least one glycol ether ketone; (B) optionally a second component consisting of at least one aprotic glycol ether; (2) neutralizing any residual diisocyanate with the acid groups of the prepolymer and a base; (3) dispersing the neutralized prepolymer in water and, optionally, increasing the molecular weight with a chain extender. In one embodiment, the acid group of the polyol containing an acid group is a carboxylic acid group. In one embodiment, the polyol containing an acid group is 2,2-dimethylolpropionic acid. In one embodiment, an optional aprotic glycol ether is present. In one embodiment, the base is an amine.

[0008] In various embodiments of the process of the present invention, the glycol ether ketone has the following structure: [ka] wherein R1 is a straight or branched alkyl group having 1 to 8 carbon atoms, a benzyl group, or a phenyl group, R2 and R3 can be independently hydrogen, CH3, or CH2CH3, R4 is CH3 or CH2CH3, and n is 0, 1, or 2, except that when R3 is CH3 or CH2CH3, then R2 is hydrogen, and when R2 is CH3 or CH2CH3, then R3 is hydrogen, In some embodiments, the glycol ether ketone is 1-n-butoxy-2-propanone, 1-(2-methoxy-1-methylethoxy)-2-propanone, or 1-(2-n-propoxy-1-methylethoxy)-2-propanone.

[0009] In some embodiments, the present invention relates to a blend that may be used, for example, in the various processes disclosed herein, the blend comprising a glycol ether ketone and an aprotic glycol ether.

[0010] In some embodiments, the present invention relates to a polyurethane dispersion comprising (i) a prepolymer comprising neutralized acid groups, (ii) a glycol ether ketone, and (iii) water. In some embodiments, the dispersion further comprises an aprotic glycol ether. In some embodiments, the neutralized acid groups are carboxyl groups neutralized with an amine.

[0011] These and other embodiments are discussed in more detail in the detailed description. [Brief description of the drawings]

[0012] [Figure 1] A simplified synthesis protocol for water-based PUD is shown. PU polymer is produced by reacting diisocyanate with polyol containing acid group and polyol without acid group. 2,2-dimethylolpropionic acid (DMPA) is a polyol (specifically, diol) and is used to incorporate carboxylic acid functional groups into the PU prepolymer. In a second step, the carboxylic acid functional groups are neutralized with a tertiary amine, and in a third step, the neutralized PU polymer is dispersed in water and reacted with a diamine to increase the molecular weight and obtain a PUD. In step 1, a polar solvent is used to dissolve DMPA during the prepolymer synthesis. In commercial practice, NMP is the most widely used solvent for this purpose. In the present invention, the polar solvent is a system containing glycol ether ketone and, optionally, an aprotic glycol ether. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] definition For purposes of United States patent practice, the contents of any referenced patent, patent application, or publication are incorporated by reference in their entirety (or the equivalent United States version thereof is so incorporated by reference), particularly with respect to the disclosure of definitions (to the extent not inconsistent with any definitions specifically provided in this disclosure) and general knowledge in the art.

[0014] Unless stated to the contrary, implicit from the context, or customary in the art, all parts and percentages are by weight and all testing methods are current as of the filing date of this disclosure.

[0015] Numerical ranges disclosed herein include all values ​​from the lower limit to the upper limit, inclusive. For ranges containing explicit numerical values ​​(e.g., 1 or 2, or 3 to 5, or 6, or 7), any subrange between any two explicit numerical values ​​is included (e.g., 1 to 2, 2 to 6, 5 to 7, 3 to 7, 5 to 6, etc.).

[0016] The terms "comprising," "including," "having," and their derivatives are not intended to exclude the presence of any additional components, steps, or procedures, whether or not they are specifically disclosed. For the avoidance of any doubt, all compositions claimed through the use of the word "comprising" may include any additional additives, adjuvants, or compounds, whether polymeric or not, unless stated to the contrary. In contrast, the term "consisting essentially of" excludes from the scope of any succeeding citation any other component, step, or procedure, except those that are not essential to operability. The term "consisting of" excludes any component, step, or procedure not specifically described or listed. The term "or" refers to the recited members individually and in any combination, unless otherwise stated. The use of the singular includes the use of the plural, and vice versa.

[0017] "Prepolymer" and like terms refer to compounds made from the reaction of a diisocyanate with a polyol. A prepolymer is formed by combining an excess of a diisocyanate with a polyol. As shown in the following illustration, one of the isocyanate groups (NCO) of the diisocyanate reacts with one of the hydroxyl groups (OH) of the polyol, and the other end of the polyol reacts with another diisocyanate. The resulting prepolymer has an isocyanate group on both ends. A prepolymer is a diisocyanate itself, and it reacts like a diisocyanate, but with some important differences. Compared to the original diisocyanate, a prepolymer has a higher molecular weight, a higher viscosity, a lower isocyanate weight content (% NCO), and a lower vapor pressure. [ka] The prepolymers used in the practice of this invention contain one or more units derived from a polyol containing an acid group, such as, for example, DMPA, to introduce carboxylic acid functionality into the prepolymer.

[0018] "Acid group," "acid functional group," and like terms mean a substituent on a monomer, oligomer, or polymer that donates a proton or hydrogen ion in aqueous solution.

[0019] "Reaction conditions" and similar terms generally refer to temperature, pressure, reactant concentration, catalyst concentration, cocatalyst concentration, monomer conversion, product and by-product (or solids) content of the reaction mixture (or mass), and / or other conditions that affect the properties of the resulting product. Reaction conditions for forming prepolymers from diisocyanates and polyols are well known in the art, and they typically include temperatures between 40°C and 150°C, atmospheric pressure, a nitrogen atmosphere, and the absence of water.

[0020] "Solvent" and like terms refer to a substance that can dissolve another substance (i.e., a solute) to form an essentially uniformly dispersed mixture (i.e., a solution) at the molecular or ionic size level.

[0021] "Aprotic" and similar terms refer to solvents that cannot donate a proton, such as glycol ethers. Protic solvents are those that have a hydrogen atom attached to an oxygen (as in a hydroxyl group) or nitrogen (as in an amine group). In general, any solvent that contains a labile H+ is a protic solvent. Representative protic solvents include DOWANOL™ DPM (dipropylene glycol methyl ether), DOWANOL™ TPM (tripropylene glycol methyl ether), DOWANOL™ DPnP (dipropylene glycol n-propyl ether), DOWANOL™ DPnB (dipropylene glycol n-butyl ether), and DOWANOL™ TPnB (tripropylene glycol n-propyl ether). Molecules of such solvents readily donate a proton (H+) to the reagent. Glycol ethers used in the practice of the present invention, such as PROGLYDE™ DMM (dipropylene glycol dimethyl ether), do not contain a labile H+. Commercially available aprotic solvents that can be used in the practice of the present invention may contain small amounts of residual protic compounds from the manufacturing process that produces the aprotic solvent. "Small amounts" typically means 1% or less by weight, or 0.5% or less by weight, or 0.1% or less by weight, or 0.05% or less by weight, or 0.01% or less by weight of protic compounds in the aprotic solvent, based on the combined weight of the aprotic solvent and the protic compounds.

[0022] Diisocyanates The diisocyanate may be an aromatic, aliphatic, or cycloaliphatic diisocyanate, or a combination of two or more of these compounds. A non-limiting example of a diisocyanate (OCN-R-NCO) derived building block is represented by the following formula (I): [ka] where R is an alkylene, cycloalkylene, or arylene group. Representative examples of these diisocyanates can be found in U.S. Patents 4,012,445, 4,385,133, 4,522,975, and 5,167,899.

[0023] Non-limiting examples of suitable diisocyanates include 4,4'-diisocyanato-diphenylmethane, p-phenylene diisocyanate, 1,3-bis(isocyanatomethyl)-cyclohexane, 1,4-diisocyanato-cyclohexane, hexamethylene diisocyanate, 1,5-naphthalene diisocyanate-3,3'-dimethyl-4,4'-biphenyl diisocyanate, 4,4'-diisocyanatodicyclohexyl-methane, 2,4-toluene diisocyanate, and 4,4'-diisocyanato-diphenylmethane.

[0024] Polyol The polyols used in the practice of the invention, including both with and without acid groups, have molecular weights (number average) ranging from 200 to 10,000 g / mole. Non-limiting examples of suitable polyols that do not contain acid groups include polyether diols (yielding "polyether polyurethanes"); polyester diols (yielding "polyester polyurethanes"); hydroxy-terminated polycarbonates (yielding "polycarbonate polyurethanes"); hydroxy-terminated polybutadienes; hydroxy-terminated polybutadiene-acrylonitrile copolymers; hydroxy-terminated copolymers of dialkyl siloxanes with alkylene oxides, e.g., ethylene oxide, propylene oxide; natural oil diols, and any combination thereof. In one embodiment, a single polyol is used. In one embodiment, a combination of two or more polyols is used. In one embodiment, one or more of the aforementioned polyols may be mixed with the amine-terminated polyether and / or amino-terminated polybutadiene-acrylonitrile copolymer, depending on the reaction rate and the desired polymer structure. Triols and other polyols having three or more hydroxy groups may also be used, such as, for example, glycerol, trimethylolpropane, etc. Further examples of polyols useful in the practice of the present invention can be found in U.S. Patent No. 4,012,445.

[0025] In an embodiment of the present invention, the total hydroxyl group equivalent of the polyol compound (including the acid group-containing polyol) is preferably 120 to 1,500. When the number of hydroxyl equivalents is within this range, the aqueous resin dispersion containing the obtained polyurethane resin can be easily produced, and a coating film excellent in terms of hardness can be easily obtained. From the viewpoints of the storage stability of the obtained aqueous polyurethane resin dispersion, the hardness, drying properties, and thickening properties of the coating film obtained by coating, the number of hydroxyl group equivalents is preferably 150 to 1000, or 200 to 700, or 300 to 600.

[0026] The hydroxyl equivalent weight of a polyol can be calculated by dividing the molecular weight of each polyol by the number of hydroxyl groups in the polyol (excluding phenolic hydroxyl groups).

[0027] In order to introduce acid functional groups into the prepolymer, at least a portion of the polyol reacted with the diisocyanate contains an acid group, for example, a carboxyl group. The acid group-containing polyol contains two or more hydroxyl groups (excluding phenolic hydroxyl groups) and one or more acid groups in one molecule. Examples of acid groups include carboxyl groups, sulfonic acid groups, phosphoric acid groups, and phenolic hydroxyl groups. The acid group-containing polyol is preferably one having two hydroxyl groups and one carboxyl group in one molecule. The acid group-containing polyol may be used alone or in combination with two or more other polyols containing acid groups.

[0028] The polyol containing an acid group is not particularly limited, and examples thereof include, but are not limited to, dimethylolalkanoic acids, such as 2,2-dimethylolpropionic acid (DMPA) and 2,2-dimethylolbutanoic acid, N,N-bishydroxyethylglycine, N,N-bishydroxyethylalanine, 3,4-dihydroxy-butanesulfonic acid, and 3,6-dihydroxy-2-toluenesulfonic acid. In particular, from the viewpoint of availability, dimethylolalkanoic acids containing two methylol groups and having 4 to 12 carbon atoms are preferred. Among the dimethylolalkanoic acids, 2,2-dimethylolpropionic acid is preferred.

[0029] Chain extender Chain extenders are not required in the practice of the present invention, but may be used if desired. When used, they can be aliphatic straight or branched chain diamines or polyols that are multifunctional, typically difunctional, and have at least 2 but no more than 10 carbon atoms in the chain. Illustrative of such polyols are diols, ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, and the like, 1,4-cyclohexanedimethanol, hydroquinone bis-(hydroxyethyl)ether, cyclohexylenediol (1,4-, 1,3-, and 1,2-isomers), isopropylidenebis(cyclohexanol), diethylene glycol, dipropylene glycol, ethanolamine, N-methyl-diethanolamine, and the like, and mixtures of any of the above. An example of a diamine is propylenediamine.

[0030] The prepolymer may contain, for example, 2 to 25, preferably 3 to 20, and more preferably 4 to 18 weight percent (wt %) of the chain extender component.

[0031] catalyst In some embodiments, the reaction between diisocyanate and polyol is promoted by using a catalyst. Examples of catalysts include, but are not limited to, salts of organic or inorganic acids and metals, such as tin-based catalysts (e.g., trimethyltin laurate, dibutyltin dilaurate, etc.), or lead-based catalysts (e.g., lead octoate, etc.), and organometallic derivatives, amine-type catalysts (e.g., triethylamine, N-ethylmorpholine, triethylenediamine, etc.), and diazobicycloundecene-type catalysts. In some embodiments, tin-based catalysts are preferred.

[0032] Solvent System The solvent system of the present invention has a high affinity for solubility to polyols containing acid groups, such as, for example, DMPA. The solvent system of the present invention is useful in the preparation of polyurethane prepolymers and PUDs.

[0033] The solvent system of the present invention consists essentially of or consists of a first component and an optional second component. The first component consists essentially of or consists of at least one glycol ether ketone. Glycol ether ketones that can be used in embodiments of the present invention have the following structure: [ka] wherein R1 is a linear or branched alkyl group having 1 to 8 carbon atoms, a benzyl group, or a phenyl group; R2 and R3 can be independently hydrogen, CH3 or CH2CH3; R4 is CH3 or CH2CH3, except that when R3 is CH3 or CH2CH3, R2 is hydrogen; and when R2 is CH3 or CH2CH3, R3 is hydrogen; and n is 0, 1, or 2. In some embodiments, the glycol ether ketone is 1-n-butoxy-2-propanone, 1-(2-methoxy-1-methylethoxy)-2-propanone, or 1-(2-n-propoxy-1-methylethoxy)-2-propanone. The solvent system of the present invention may include two or more glycol ether ketones. When the first component consists essentially of or consists of two or more glycol ether ketones, the first component is a blend that may or may not be phase separated.

[0034] The optional second component essentially consists of or consists of aprotic glycol ethers, such as esterified (preferably acetylated) or etherified compounds based on ethylene glycol, propylene glycol, or other alkyl, such as butyl, glycol alkyl ethers. Diethers of diethylene glycol, dipropylene glycol, and tripropylene glycol may also be used (PROGLYDE™ DMM is a diether of dipropylene glycol). In one embodiment, the optional second component essentially consists of or consists of two or more aprotic glycol ethers. When the second component essentially consists of or consists of two or more aprotic glycol ethers, the second component is a blend that may or may not be phase separated.

[0035] Representative aprotic glycol ethers include, but are not limited to, dipropylene glycol dimethyl ether and tripropylene glycol dimethyl ether, propylene glycol methyl ether acetate, propylene glycol diacetate, diethylene glycol n-butyl ether acetate, dipropylene glycol methyl ether acetate, and ethylene glycol butyl ether benzoate. Acetate is particularly undesirable due to its limited water solubility and potential for hydrolysis once the final PUD is made, so acetate, if used at all, is typically used in combination with a water-soluble aprotic solvent such as PROGLYDE™ DMM or N,N-DMPA. Protic solvents such as ethylene glycol monobutyl ether, ethylene glycol monopropyl ether, diethylene glycol monoethyl ether, propylene glycol methyl ether, dipropylene glycol monomethyl ether, and tripropylene glycol monomethyl ether may be present in the solvent systems of this invention only as residuals of the manufacturing process in which the aprotic components in the solvent system are made, and only in small amounts, e.g., 1% by weight or less based on the combined weight of the aprotic and protic compounds in the solvent system. Protic solvents are not preferred because, like water, they react quickly with isocyanates.

[0036] Commercially available aprotic glycol ethers that can be used in the practice of this invention include, but are not limited to, DOWANOL™ PMA (propylene glycol methyl ether acetate), DOWANOL™ DPMA (dipropylene glycol methyl ether acetate), DOWANOL™ PGDA (propylene glycol diacetate), butyl CELLOSOLVE™ acetate (ethylene glycol n-butyl ether acetate), butyl CARBITOL™ acetate (diethylene glycol n-butyl ether acetate), ethylene glycol butyl ether benzoate, and PROGLYDE™ DMM (dipropylene glycol dimethyl ether) (all available from The Dow Chemical Company). Another aprotic glycol ether that can be used in some embodiments is tripropylene glycol dimethyl ether.

[0037] The solvent can be a binary blend of two glycol ether ketones or a binary blend of (1) one or more glycol ether ketones (e.g., 1-n-butoxy-2-propanone, 1-(2-methoxy-1-methylethoxy)-2-propanone, or 1-(2-n-propoxy-1-methylethoxy)-2-propanone) and (2) one or more aprotic glycol ethers (e.g., PROGLYDE™ DMM dipropylene glycol dimethyl ether, tripropylene glycol dimethyl ether, etc.).

[0038] In one embodiment, the solvent system consists of, or consists essentially of, 10-100 wt%, or 20-80 wt%, or 30-70 wt%, or 40-60 wt% of a first component and 0-90 wt%, or 20-80 wt%, or 30-70 wt%, or 40-60 wt% of a second component, in weight percent (wt%) based on the weight of the solvent system.

[0039] In one embodiment, the solvent system consists of, or consists essentially of, 30-100%, or 40-90%, or 50-80% by weight of at least one of 1-n-butoxy-2-propanone, 1-(2-methoxy-1-methylethoxy)-2-propanone, or 1-(2-n-propoxy-1-methylethoxy)-2-propanone, and 0-70%, or 10-60%, or 20-50% by weight of an aprotic glycol ether, in weight percent (wt %) based on the weight of the solvent system. In one embodiment, the aprotic glycol ether is dipropylene glycol dimethyl ether.

[0040] In embodiments where the first and / or second components consist of two or more substances, for example where the first component consists essentially of two or more glycol ether ketones and / or the second component consists essentially of two or more aprotic glycol ethers, the amount of each substance in a particular component may vary widely and advantageously. The amount of each individual substance in a component may vary from 0 to 100% by weight, or from 1 to 99% by weight, or from 10 to 90% by weight, or from 20 to 80% by weight, or from 30 to 70% by weight, or from 40 to 60% by weight, or from 50% by weight, based on the weight of the component.

[0041] Optional materials that may be included in the solvent system, while not essential to the operability of the solvent system of this invention, include, but are not limited to, antioxidants, colorants, moisture scavengers, stabilizers, fillers, diluents (e.g., aromatic hydrocarbons), and the like. These materials do not have any significant effect on the effectiveness of the solvent system to provide a reaction medium for the preparation of the prepolymer. These optional materials are used in known amounts, e.g., 0.10 to 5, or 4, or 3, or 2, or 1 weight percent based on the weight of the solvent system, and they are used in known manner.

[0042] Preparation of solvent system The solvent system of this invention, consisting essentially of or consisting of two or more compounds, e.g., glycol ether ketone and aprotic glycol ether, is prepared using known equipment and known techniques. The individual components of the solvent system are commercially available, are liquid at ambient conditions (23°C and atmospheric pressure), and can be easily mixed together using conventional mixing equipment and standard mixing protocols. The components can be added to each other in any order, including simultaneously.

[0043] Use of solvent systems The solvent systems of the present invention are eco-solvents, i.e., they do not have or have at reduced levels the toxicological problems associated with NMP. These solvent systems are used in the same manner as NMP and other polar solvents as a medium for the preparation of prepolymers. Thus, one application of the solvent systems of the present invention, including glycol ether ketones, is the preparation of polyurethane dispersions, as further described herein.

[0044] Polyurethane Dispersion The process for producing aqueous (water-based) polyurethane dispersions (PUDs) is a three-step process that includes (1) preparing the prepolymer described above, (2) neutralizing the acid functional groups of the prepolymer, and (3) dispersing the prepolymer in water and optionally increasing the molecular weight. Virtually any base can be used as the neutralizing agent. Examples include, but are not limited to, trimethylamine, triethylamine, triisopropylamine, tributylamine, triethanolamine, N-methyldiethanolamine, N-ethyldiethanolamine, N-phenyldiethanolamine, dimethylethanolamine, diethylethanolamine, N-methylmorpholine, organic amines such as pyridine, inorganic alkali salts such as sodium hydroxide and potassium hydroxide, and ammonia. For neutralizing carboxyl groups, organic amines are preferred, and tertiary amines, especially triethylamine, are more preferred. Such tertiary amines can preserve residual isocyanates in the prepolymer for subsequent reaction with chain extenders in the dispersion step.

[0045] The step of dispersing the polyurethane prepolymer in the aqueous medium may be carried out using conventional equipment and techniques. For example, the prepolymer may be added to an agitated water blender and mixed until a substantially homogenous blend is obtained. Alternatively, water may be added to the agitated prepolymer blender. Mixing is typically carried out at ambient conditions (23° C. and atmospheric pressure). Various additives, such as stabilizers, antioxidants, surfactants, etc., may be added to the dispersion in known amounts and using known methods. The amount of prepolymer in the dispersion may vary widely, but typically the prepolymer comprises 5 to 60, or 15 to 50 weight percent of the dispersion.

[0046] In some embodiments, after dispersing the neutralized prepolymer in water, a chain extender can be added to increase the molecular weight of the polyurethane. The chain extender can be used to increase the molecular weight using techniques known to those skilled in the art. Examples of chain extenders that can be used are listed above. As mentioned above, the prepolymer can contain, for example, 2 to 25, preferably 3 to 20, and more preferably 4 to 18 weight percent (wt%) of the chain extender component.

[0047] In some embodiments, polyurethane dispersions produced according to embodiments of the present invention include 1-15 wt % glycol ether ketone used as a solvent.

[0048] The following examples are non-limiting illustrations of the present invention. EXAMPLES

[0049] Synthesis of glycol ether ketone Oxidation of glycol ethers bearing secondary OH groups by any of a variety of methods known to those skilled in the art produces glycol ether ketones. The glycol ether ketones used in some embodiments of the present invention are prepared by two different procedures using commercially available trichloroisocyanuric acid as the oxidizing agent. Examples illustrating the preparation of 1-pentoxy-2-propanone ("PnPent ketone") and 1-(2-methoxy-1-methylethoxy)-2-propanone ("DPM ketone") follow.

[0050] Preparation of 1-pentoxy-2-propanone (PnPent Ketone) The Erlenmeyer flask is equipped with a magnetic stir bar and a thermocouple wire. The flask is charged with 1-pentoxy-2-propanol (160 g, 968.34 mmol), dichloromethane (485 mL), and TEMPO catalyst (2,2,6,6-tetramethylpiperidine-1-oxyl, 1.52 g, 9.7 mmol). The bright orange solution is cooled to 5 °C with an ice bath. Trichloroisocyanuric acid (237.43 g, 1021.64 mmol) is added in portions with a spatula to control the temperature. The resulting mixture is stirred for 1 h, then the ice bath is removed and the mixture is stirred at room temperature for an additional 2 h. The mixture is filtered and the filtrate is cooled to 5 °C with an ice bath. A saturated solution of aqueous sodium carbonate (200 mL) is added. The mixture is transferred to a separatory funnel and the liquid phases are separated. Transfer the organic phase to an Erlenmeyer flask and add 200 mL of a saturated solution of sodium carbonate and 20 mL of a saturated aqueous solution of sodium sulfite. Stir the mixture overnight at room temperature. Transfer the mixture to a separatory funnel and separate the liquid phases. Wash the organic phase twice with 600 mL of brine, dry over anhydrous magnesium sulfate, filter, and concentrate on a rotary evaporator to obtain 147.78 g of crude product. The single-necked round-bottom flask containing the crude product is equipped with a magnetic stir bar, a 1-foot Oldershaw column, and a distillation head capable of reflux digestion. Vacuum distill the crude product to obtain various fractions weighing a total of 101.13 g. Use the product, which is 98-99% pure by gas chromatography, to prepare polyurethane dispersions (PUDs) as described below.

[0051] Preparation of 1-(2-methoxy-1-methylethoxy)-2-propanone (DPM ketone) The synthesis employs the 2-octanol oxidation procedure reported by Hiegel et al. in Synthetic Communications, 22:11, pp. 1589-1595. A 5 L three-neck flask containing an integrated thermocouple well is fixed to the grid of a fume hood. An IKA Eurostar Power control Visc variable speed electric motor is fixed to the grid above the flask. A glass stirring shaft with a Teflon paddle is fitted with a Teflon sheathed glass bearing and the shaft is attached to the motor by inserting it into a short piece of stiff rubber tubing inserted into a short steel rod fixed in the chuck of the motor. The flask is fitted with a water-cooled 12-inch Allen condenser topped with a nitrogen bubbler. A lab jack is placed under the flask and an ice-water bath is placed on the lab jack. The lab jack is raised so that the flask is half-immersed in the ice bath. A thermocouple is placed in the thermocouple well, to which a small amount of glycerin has been added beforehand. The thermocouple is connected to a digital temperature controller. The flask is swept with nitrogen for approximately 10 minutes, then 897.06 g of 1-(2-methoxy-1-methylethoxy)-2-propanol (DOWANOL™ DPM, 6.05 mol), 848.6 g (10.7 mol) of anhydrous pyridine, and 1567 g of acetone are added in succession through the open neck while maintaining the nitrogen sweep. A glass stopper is placed on the neck and the nitrogen flow is reduced to create a nitrogen blanket. The reaction mixture is stirred at 250 rpm and cooled to 15° C. in an ice bath. Trichloroisocyanuric acid (738.75 g, 3.2 mol) is added in 50-80 g portions over 6 hours by momentarily removing the stopper and placing a solid addition funnel on the neck to facilitate the addition. The reaction temperature is maintained in the range of 15-25° C. by the ice bath throughout the reaction. Once the addition is complete, the reaction mixture is left stirring at room temperature overnight.

[0052] A small sample of the reaction mixture is removed with a disposable pipette, filtered through a 0.45 micron syringe filter, and analyzed on a gas chromatogram equipped with a 30mx0.32mmx1.0 micron Agilent J&W DB-1701 capillary column and a thermal conductivity (TCD) detector. The ratio of DPM ketone:DOWANOL™ DPM is determined to be 96.5%:3.5% based on the GC area. The reaction mixture is filtered through #4 filter paper and the filter cake is washed with acetone. Most of the acetone and some of the pyridine are removed on a rotary evaporator at 35°C and 135mmHg. The crude product weighed 1682.7g and contained 26.7% acetone, 14.0% pyridine, 1.8% DOWANOL™ DPM, 50.5% DPM ketone and minor components.

[0053] The crude product is then combined in a 5 L round-bottom boiling flask with product from other DPM Ketone batches prepared by the same procedure, and the combined product is purified by fractional distillation using a 1 ft x 1 in. i.d. silver-lined, vacuum-jacketed glass column packed with 0.25 in. ceramic saddles equipped with a water-cooled, temperature-controlled magnetic reflux splitter, a water-cooled receiver trap, and valves for nitrogen and vacuum operation. Acetone and pyridine are collected at a distillate temperature of 350-400 mmHg and 38 °C. The pressure is then reduced in stages while various intermediate fractions are collected. DPM Ketone, boiling at 32 °C and 1.6 mmHg, is isolated in 97.8% purity with only 0.8% residual glycol ethers. This product is subsequently used for the preparation of PUD, as described below.

[0054] Description of the equipment for preparing polyurethane dispersions (PUD) Polymerization Reactor The polyurethane prepolymer is prepared in a 300 mL jacketed glass vessel from Chemglass Life Sciences (part number CG-1929-10) with a 100 mm Schott O-ring flange and a lower Teflon screw plug valve, with the glass outlet set at a 45 degree angle and terminating in a 14 / 20 male joint. The inlet and outlet jacket connections are attached using tubing (rated at the temperature and materials used in the process) to a thermostatically controlled Cole Palmer water bath filled with 50% by volume propylene glycol in water. The reactor is equipped with a glass lid with three 24 / 40 female joints in a row. A glass bearing with a Teflon sheath is fitted with a glass stirring shaft and placed in the center joint. The stirring shaft is attached to an overhead digital stirrer motor from IKA (model Eurostar20). A water-cooled Allene condenser with an adapter connected to a nitrogen bubbler is placed in the second glass joint. A nitrogen adapter connected via Tygon® tubing to a low pressure Dwyer flowmeter is placed in the third glass joint. This nitrogen connection is used to purge the reactor before charging the reactants and to establish an initial nitrogen blanket. The adapter is replaced with a glass funnel when adding reactants and a glass stopper during the reaction. The reactor lid is also equipped with a 14 / 20 female joint with a stopper for sampling and a 14 / 20 screw joint with a glass thermocouple well. A thermocouple connected to a digital meter is placed in the thermocouple well to measure the internal reactor temperature. A 9-inch piece of Tygon tubing cut at an angle is attached to the drain and secured with a clamp.

[0055] Dispersion Reactor The polyurethane dispersion is prepared in a 3000 mL three-neck round-bottom flask equipped with a built-in thermocouple well, a Teflon-sheathed glass bearing with a glass stirring shaft, and a glass stopper. The stirring shaft is attached to an overhead Heidolph RZR-2000 digital stirring motor. The flask is secured to a grate in the hood and placed on a cork ring. Tygon tubing connected to the outlet of the polymerization reactor was inserted into the remaining neck of the flask. A thermocouple is inserted into the thermocouple well to measure the temperature rise during the addition of the prepolymer to the water in the flask.

[0056] Polymerization and Dispersion Procedure The details of the PUD preparation scheme are shown in Figure 1 and described below. The amounts of the various reactants are adjusted to obtain a 300 g batch of polyurethane prepolymer for subsequent dispersion in 400 mL of water. The following procedure reflects the target amounts of reagents in a typical preparation. The equipment used in the procedure is as described above.

[0057] Preparation of Polyurethane Before starting the reaction, the reactor is thoroughly flushed with nitrogen. The jacket temperature is set to 80°C and the water to the condenser is turned on. Terathane 1000 diol (60.17 g, 0.1203 OH equiv.) and Terathane 2000 diol (84.25 g, 0.0843 OH equiv.) are weighed into a plastic beaker and added to the vessel with the nitrogen adapter temporarily replaced with a glass funnel. The stirring motor is turned on to 150 rpm and the addition time is recorded. After 3 hours, the jacket temperature is reduced to 60°C and the diol is stirred overnight under a nitrogen sweep to remove residual moisture. The next day, the nitrogen adapter is replaced with a glass stopper and a nitrogen blanket established through the nitrogen adapter on top of the condenser. 2,2-bis-(hydroxymethyl)propionic acid (DMPA) is weighed into a weigh boat (16.85 g, 0.2512 OH equiv., 0.1256 COOH equiv.). Weigh the solvent desired for the process into a beaker (31.3 g). Turn off the stirrer, remove the stopper, put the glass funnel in place, and add both components to the reactor (the solvent is added last to wash the DMPA into the reactor). Remove the funnel, replace the stopper, and turn the stirrer back on. The isocyanate (4,4'-methylenebis-(cyclohexyl isocyanate, 95.48 g, 0.7277 NCO equivalents) is weighed into a disposable plastic beaker on a balance placed in the hood. The stopper is momentarily removed, stirring is stopped, and the isocyanate is slowly added to the reactor through the glass funnel. The stirrer is turned on and set to 200 rpm, and the bath temperature is increased to 80 °C. The reaction is monitored for approximately 10-15 minutes for any exotherm. Then, the bath temperature is increased to 95 °C. Once the internal pot temperature reaches 90 °C, a timer is set for 4 hours. Once the time has elapsed, stirring is discontinued and approximately 1.00 g of the reaction mixture is removed with a disposable glass pipette and weighed into a 250 mL Erlenmeyer flask and mixed with ASTM D6244. Test for %NCO using D2572. Based on the amounts of reactants used, a residual NCO content of 4% is expected at the end of the reaction. While the reaction is cooling, weigh out the triethylamine (TEA) required to neutralize the carboxyl content into a syringe on a balance placed in the hood (11.96 g, 0.1194 base equivalents).Once the pot temperature reaches 70°C, stop the stirring, momentarily remove the stopper, add the TEA, set the stirring to 250 rpm, and set the timer for 15 minutes. While the time is elapsed, the dispersion flask is prepared.

[0058] After the time has elapsed, the reactor drain valve is opened and the polyurethane is allowed to drain into a 3000 mL dispersion flask containing 400 mL of deionized water stirring at 400 rpm. This transfer took approximately 20-30 minutes, depending on the viscosity of the polymer. Once all the polymer has been transferred, the stopper of the dispersion flask is replaced with a previously prepared addition funnel equipped with a pressure equalization arm and filled with 19.31 g of propylene diamine (PDA) aqueous solution containing 8.31 g of PDA (0.2242 NH2 equivalents). The temperature in the dispersion flask is monitored along with the time taken for the addition. Once all the PDA solution has been added, a timer is set for 20 minutes while the PUD continues to stir at 400 rpm. The stirrer is turned off and the PUD is allowed to sit in the flask overnight. The next day, the PUD is filtered (using a paint filter) into a labeled bottle. The PUD is then characterized by its pH, viscosity, solids content, and minimum film formation temperature (MFFT) testing. Samples of the PUDs are removed onto phosphate-treated steel panels and the resulting films are tested for thickness, cross-hatch adhesion, Konig hardness, direct and indirect impact resistance, and gloss. The analytical procedures used to measure these properties are described in the Analytical Procedures section below.

[0059] Comparison of polyurethane dispersion (PUD) properties PUDs are prepared as above using 1-n-butoxy-2-propanone (PnB ketone), 1-butoxy-2-butanone (BnB ketone), 1-(2-methoxy-1-methylethoxy)-2-propanone (DPM ketone), 1-(2-n-propoxy-1-methylethoxy)-2-propanone (DPnP ketone), and 1-n-pentoxy-2-propanone (PnPent ketone). PUDs are prepared as above using NMP and PROGLYDE™ DMM for comparison (not an example of the present invention). PUD properties were measured and are summarized in Table 1. Although the viscosities differed slightly, all PUDs prepared with glycol ether ketones showed the same coalescence efficiency as those prepared with NMP and PROGLYDE™ DMM, as shown by the results of the MFFT evaluation. Film properties obtained from the various PUDs are summarized in Table 2. The PUDs prepared with glycol ether ketone produced films with excellent adhesion and impact resistance, desirable hardness values ​​above 50 seconds, and gloss similar to that obtained with the controls (NMP and PROGLYDE™ DMM). [Table 1] [Table 2]

[0060] Analytical procedures Moisture Percentage Measurement The water content of all solvents used is measured according to ASTM E203 using a Mettler V30 Karl Fischer water titrator attached to a Mettler Toledo GA 42 printer and a Mettler Toledo AE160 analytical balance. Fill a 1 cc syringe with a 21Gx1 / 2 inch needle with the solvent, place it on the analytical balance and tare. Add the sample (0.8775-2.5131 g) to the titration cup and begin the titration. An Aquastar® water standard containing 1.00 wt% water is used to ensure the equipment is working properly. High water content can react with isocyanates and adversely affect the formation of polyurethanes. If the water content is high (above 0.06 wt%), molecular sieves are added to the solvent and the solvent is allowed to stand for several days before use.

[0061] Percent solids (% solids by weight) Weight percent solids are measured according to ASTM D2369. Samples are prepared in triplicate by weighing 0.5 g of material (recording the exact weight to four decimal points) into tared and labeled disposable aluminum pans. The pans are placed on a tray to act as a secondary container, covered with a section of steel mesh, and placed in a Blue M oven at 110°C for 1 hour. (The mesh is used to prevent the pan from blowing away in the oven). After the time is up, the pans are removed from the oven, cooled, and reweighed. The solids content of each sample is calculated using the following formula, and the triplicate results are averaged:

number

[0062] Percent Isocyanate (%NCO) Percent NCO of polyurethane prepolymers is determined according to ASTM D2572. In this analysis, the unreacted isocyanate in the polyurethane is reacted with excess dibutylamine in toluene and the %NCO is calculated by back titrating the unreacted amine with 0.1N HCl. A blank is performed by taking an oven-dried 250mL Erlenmeyer flask containing a 1-inch Teflon stir bar, cooling it under a stream of nitrogen, and adding 25mL of anhydrous toluene. A stopper is placed briefly on the flask before adding 25mL of 0.1N dibutylamine in toluene via a TD (Delivery) pipette. The flask is stoppered, secured in place on a stir plate, and stirred at low speed for 15 minutes. 100mL of isopropyl alcohol is then added to the flask using a graduated cylinder, followed by 6 drops of bromophenol blue indicator solution (prepared as described below). The flask is stoppered, the solution is stirred for 1 minute, and titrated with 0.1N HCl to a pale yellow endpoint. When titrating polymer samples, an oven-dried Erlenmeyer flask containing a 1-inch Teflon stir bar is removed from the oven, cooled under nitrogen, stoppered, and placed on a balance. The sample, removed from the reactor with a disposable glass pipette, is added to the flask by momentarily removing the stopper, taking care not to stick the sample to the flask walls. The weight of the sample is recorded, the flask is placed on a stir plate, the stopper is momentarily lifted, and 25 mL of dry toluene is added. If the sample has not dissolved upon gentle stirring, a heat gun is used to warm the flask to facilitate dissolution of the sample. A 25 mL aliquot of 0.1 N dibutylamine solution (prepared as described below) is added to the sample and the same titration procedure used for the blank is followed. %NCO is calculated using the following formula: %NCO={[(BV)xNx0.0420] / W}x100 where B = mL of HCl solution for blank titration, V = mL of HCl solution for sample titration, N = normality of HCl solution (0.10 N), 0.0420 = milliequivalents of NCO groups, and W = sample weight (g).

[0063] A 0.1 N solution of bromophenol blue indicator is prepared by mixing 0.1013 g of water-insoluble bromophenol blue (acid form) with 1.5 mL of 0.1 N NaOH solution in a volumetric flask and diluting to 100 mL with deionized water.

[0064] A 0.1 N solution of dibutylamine is prepared by adding 6.46 g of dibutylamine to a 500 mL volumetric flask and diluting to the mark with anhydrous toluene. The molecular weight of dibutylamine is 129.24 g / mol.

[0065] pH The pH of the PUDs is measured using a calibrated Metro Toledo T70 titrator connected to a computer and printer. The pH meter probe is rinsed with deionized water, wiped with a Chem-Wipe, and inserted into the sample. The pH shortcut button is pressed and the probe is held stationary in the sample and allowed to equilibrate for approximately 30 seconds before recording the pH value.

[0066] viscosity PUD viscosity is measured at 25°C using a Brookfield Programmable DV-II+ viscometer attached to a Brinkmann MGW Lauda RM6 circulating bath filled with a 50:50 water-propylene glycol solution. A 0.5 mL sample of PUD is placed in the center of the sample cup using a disposable syringe. Measurements are taken with a CP-40 spindle.

[0067] Minimum Film Formation Temperature Test (MFFT(°F) MFFT testing is performed in accordance with ASTM D2354. The MFFT plate is set to the appropriate temperature (typical range is 31-53°F) and allowed to stabilize. Once the temperature is stable, six 1 inch wide x 24 inch long pieces of 3M Scotch Tape are placed on the MFFT plate. Care is taken to ensure that there is no condensation on the plate and that the tapes are securely fastened in place. A circular 5 mil drawdown bar is centered over each tape on the right hand side of the plate and a disposable pipette is used to dispense the PUD sample onto the drawdown bar. Even pressure is applied to draw the sample down onto the tape. A plexiglass plate with calibration lines corresponding to specific heated locations on the plate is set in position over the sample to be tested and an air line is attached to the plexiglass plate. Air pressure is set to 20 psig and a timer is set for 4 hours. One sample per PUD is run. MFFT is indicated by defects (i.e., cracks) at specific locations (temperatures) on the film.

[0068] Films prepared from the PUDs are tested according to the following method.

[0069] Drawdown and curing process A 10 mil wet film of the PUD is drawn down onto 4"x12"x.032" iron-phosphorus unpolished panels. The coated panels are placed on a tray and then placed in a vented 60°C oven for 30 minutes. The tray of panels is removed from the oven and the panels are placed on a laboratory rack at constant temperature (72°F) and constant humidity (42%). The panels are left on the rack for 7 days before analysis.

[0070] Thickness The thickness in mils of the cured PUD film is measured using a PosiTector 6000 thickness gauge. The probe is first calibrated using an untreated panel. The probe is placed flat on the coated panel and the measurements are recorded. A total of three measurements are taken on each panel tested, with the probe placed in various locations on the coated surface. The average thickness is calculated.

[0071] Glossiness Gloss is measured according to ASTM D523. Measurements are taken using a micro Tri-Gloss (20° / 60° / 85°) gloss meter. For each reading, the instrument is moved to a different location on the substrate. Measurements are taken three times and the average is reported. Crosshatch Adhesion (CH Adhesion)

[0072] The crosshatch adhesion test is performed according to ASTM Method D3359, Method B. The adhesion test is used to determine if the clearcoat has properly adhered to the surface of the panel. The test is performed by placing the panel on a solid counter and using a cutting tool to scratch the coated panel in one direction, then scratching the already scratched area in a perpendicular direction (so the pattern looks like a checkerboard). Any flakes or dust are lightly brushed off. ASTM tape is placed over the checkerboard area and the tab left on one end. After pressing the tape firmly onto the area, in a smooth, steady motion, the tape is quickly pulled off at 90 degrees with one hand while the other hand presses the panel against a flat surface. The crosscut area is evaluated for adhesion by comparing it to the example in Figure 1 of the ASTM method.

[0073] Konig pendulum hardness (average Konig) Hardness testing is performed in accordance with ASTM D4366 using a BYK Gardner pendulum hardness tester. The coated panel is placed on the lifting table and lifted into position using the handle. The displacement arm is used to pull the pendulum back behind the pin while the wire release button is held down. The start button on the front of the unit is pressed and then the wire release button is released. The instrument begins counting oscillations and gives an audible indication when the pendulum has stopped. The number of oscillations is recorded in seconds, the panel is moved to a new location and the testing process repeated. Each sample is tested in triplicate and the average value reported.

[0074] Direct / indirect impact resistance (direct and indirect impact) Direct impact testing is performed according to ASTM Method D2794 using a BYK Gardner heavy duty impact tester PF-1120 equipped with a 4 lb impact punch. The punch is lifted with one hand and the coated panel (coated side up) is placed between the punch and the retaining cup. The punch is slowly lowered onto the test panel. The weight is raised to its maximum height with one hand while the panel is held firmly with the opposite hand. The weight is released. After impact, the punch is lifted and the panel is inspected for damage such as starburst cracks or delamination. If damage occurs, the process is repeated at another location and the weight height is lowered until no damage is observed. Results are recorded in pounds, inches. The same process continues for indirect impact testing, except the panel is placed coated side down towards the retaining cup. The present invention includes the following aspects. Section 1. 1. A process for producing a prepolymer containing acid groups, said process comprising: (i) a diisocyanate; (ii) a polyol containing an acid group; and (iii) contacting a polyol having no acid groups with The contacting step comprises under reaction conditions: (A) a first component comprising at least one glycol ether ketone; (B) optionally a second component consisting of at least one aprotic glycol ether. Section 2. A three-step process for producing a water-based polyurethane dispersion (PUD), the process comprising: (1) (i) a diisocyanate; (ii) a polyol containing an acid group; and (iii) forming a prepolymer having acid groups by contacting a polyol having no acid groups with The contacting comprises under reaction conditions: (A) a first component comprising at least one glycol ether ketone; (B) optionally a second component consisting of at least one aprotic glycol ether; (2) neutralizing the acid groups and any residual diisocyanate of the prepolymer with a base; (3) dispersing the neutralized prepolymer in water and, optionally, increasing the molecular weight with a chain extender. Section 3. The glycol ether ketone has the following structure: [ka] The process according to item 1 or 2, wherein R1 is a linear or branched alkyl group having 1 to 8 carbon atoms, a benzyl group, or a phenyl group; R2 and R3 can be independently hydrogen, CH3, or CH2CH3; R4 is CH3 or CH2CH3; and n is 0, 1, or 2, except that when R3 is CH3 or CH2CH3, R2 is hydrogen, and when R2 is CH3 or CH2CH3, R3 is hydrogen. Section 4. The process according to any one of items 1 to 3, wherein the glycol ether ketone is 1-n-butoxy-2-propanone, 1-(2-methoxy-1-methylethoxy)-2-propanone, or 1-(2-n-propoxy-1-methylethoxy)-2-propanone. Section 5. 5. The process according to any one of items 1 to 4, wherein the acid group is a carboxyl group. Section 6. 5. The process according to any one of items 1 to 4, wherein the polyol containing an acid group is 2,2-dimethylolpropionic acid. Section 7. 7. The process of any one of paragraphs 1 to 6, wherein the optional second component is present and is at least one of dipropylene glycol dimethyl ether and tripropylene glycol dimethyl ether. Section 8. 8. The process according to any one of items 1 to 7, wherein a metal salt catalyst is used in the contacting step. Section 9. 9. The process of claim 8, wherein the metal salt catalyst is an organotin salt catalyst. Section 10. A blend comprising: (1) a glycol ether ketone; and (2) an aprotic glycol ether. Section 11. The glycol ether ketone has the following structure: [ka] Item 11. The blend of item 10, wherein R1 is a linear or branched alkyl group having 1 to 8 carbon atoms, a benzyl group, or a phenyl group; R2 and R3 may be independently hydrogen, CH3, or CH2CH3; R4 is CH3 or CH2CH3, except that when R3 is CH3 or CH2CH3, R2 is hydrogen, and when R2 is CH3 or CH2CH3, R3 is hydrogen; and n is 0, 1, or 2. Section 12. 11. The blend of claim 10, wherein the glycol ether ketone is 1-n-butoxy-2-propanone, 1-(2-methoxy-1-methylethoxy)-2-propanone, or 1-(2-n-propoxy-1-methylethoxy)-2-propanone. Section 13. Item 11. The blend of item 10, wherein the aprotic glycol ether is at least one of dipropylene glycol dimethyl ether and tripropylene glycol dimethyl ether. Section 14. A polyurethane dispersion (PUD) comprising: (i) a prepolymer containing neutralized acid groups; (ii) a glycol ether ketone; and (iii) water. Section 15. 15. The PUD of claim 14, further comprising an aprotic glycol ether.

Claims

1. 1. A process for producing a prepolymer containing acid groups, said process comprising: (i) a diisocyanate; (ii) a polyol containing an acid group; and (iii) contacting a polyol having no acid groups with The contacting step comprises under reaction conditions: (A) a first component consisting of at least one compound of structure (I): (B) optionally a second component consisting of at least one aprotic glycol ether; [Formula 1] In the above structure (I), R 1 is a linear or branched alkyl group having 4 to 8 carbon atoms, a benzyl group, or a phenyl group; R 2 and R 3 are independently hydrogen, CH 3 or CH 2 CH 3 (where R 3 CH 3 or CH 2 CH 3 If R 2 is not hydrogen, R 2 CH 3 or CH 2 CH 3 If R 3 is not hydrogen), R 4 But, CH 3 or CH 2 CH 3 and n is 0, 1 or 2.

2. 2. The process of claim 1, wherein the compound of structure (I) is 1-n-butoxy-2-propanone (PnB ketone), 1-butoxy-2-butanone (BnB ketone), or 1-n-pentoxy-2-propanone (PnPent ketone).

3. 3. The process according to claim 1 or 2, wherein the acid group is a carboxyl group.

4. The process of claim 1 or 2, wherein the polyol containing acid groups is 2,2-dimethylolpropionic acid.

5. 5. The process of any of claims 1 to 4, wherein the optional second component, when present, is at least one of dipropylene glycol dimethyl ether and tripropylene glycol dimethyl ether.

6. The process of any of claims 1 to 5, wherein a metal salt catalyst is used in the contacting step.

Citation Information

Patent Citations

  • Urethane polymer* polymer dispersion and useful semiester in it

    JP1981008346A

  • Solvent system containing methoxyacetone and water

    JP1994025067A

  • Curing agent for epoxy resin, curing catalyst and solvent solution for curing inhibitor

    JP1995138455A

  • Metallic-luster color ink

    JP1997048940A