Silica-Encapsulated Pigments for Nanometallography.

A method for printing metallic layers on substrates using a donor surface with selective particle transfer and continuous replenishment addresses waste and cost issues, maintaining high gloss and durability through a metal oxide and heteropolysiloxane treatment.

JP7588727B2Active Publication Date: 2024-11-22ECKART GMBH & CO KG
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023541791
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-01-11
Filing Date
2021-12-22
Publication Date
2024-11-22
Estimated Expiration
2041-12-22

AI Technical Summary

Technical Problem

Existing methods for printing metallic layers on substrates, such as foil stamping and foil fusing, result in significant waste due to unrecovered foil and are costly because metal foils are used only once, with the transferred metal layers often having lower gloss and deteriorating over time.

Method used

A method involving a donor surface coated with discrete metal particles, where the affinity of the particles for the substrate is higher than for the donor surface, allowing selective transfer and continuous replenishment of particles, using a metal matrix with a surface treatment of metal oxide and heteropolysiloxane or terminal functional groups to maintain high gloss and prevent degradation.

Benefits of technology

The method achieves high gloss and stable metallic layers without waste, ensuring long-term durability and efficient use of metal particles by selective transfer and continuous replenishment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588727000001
    Figure 0007588727000001
  • Figure 0007588727000002
    Figure 0007588727000002
Patent Text Reader

Abstract

A method is provided that does not exhibit various disadvantages of conventional methods for printing substrates. [Solution] A method for printing on the surface of a substrate, the method comprising: (a) coating a donor surface with discrete particles; (b) treating the surface of the substrate so that the affinity of the particles for at least selected areas of the surface of the substrate is greater than the affinity of the particles for the donor surface; and (c) contacting the surface of the substrate with the donor surface so that the particles transfer from the donor surface only to the treated selected areas of the surface of the substrate, thereby exposing the areas of the donor surface to which the particles have been transferred to corresponding areas on the substrate, wherein at least 50% by weight of the particles are metal pigments having a metal substrate and a surface treatment of the metal substrate, the surface treatment of the metal substrate comprising at least one coating layer having a metal oxide and surrounding the metal substrate, and a surface modification of the metal oxide layer having at least one heteropolysiloxane or compound having at least two terminal functional groups that are the same or different from each other and separated by a spacer, at least one terminal functional group being capable of chemically bonding to the metal oxide layer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for printing on a substrate, and in particular to a method by which a layer having a metallic appearance can be applied to a substrate. [Background technology]

[0002] Various systems are known in the art for printing layers with a metallic appearance on substrates, such as paper or plastic films. These systems belong to two major categories: foil stamping or foil fusing. One of the main disadvantages of these methods is the large amount of foil that is wasted in these methods, because the foil areas that are not transferred onto the substrate to form the desired image cannot be recovered for use in the same method. Because metal foils are expensive, these methods are relatively costly, because the foil can be used only once and only a small portion of the metal is effectively transferred to the substrate. Summary of the Invention [Problem to be solved by the invention]

[0003] In WO2016 / 189515A9, a new process is disclosed, which allows to print a layer with a metallic appearance on a substrate in a much more cost-effective manner, without any waste of metal or metallic foil. In this process, separate metal particles are transferred onto the substrate through a donor roll, and the metal particles on the donor roll are replenished in a repeating process. Although this process does not have all the disadvantages of the foil stamping or foil melting process, it has been found that the metal layer obtained via this process is not as high gloss and / or shows deterioration over time. [Means for solving the problem]

[0004] Surprisingly, a method has been found which does not exhibit the various disadvantages of the above mentioned processes, in particular a method according to the invention is provided for printing a layer having a metallic appearance on a substrate, this layer having a high gloss level which does not exhibit any degradation over time.

[0005] The method according to the invention relates to a method of printing on a surface of a substrate, the method comprising: a. providing a donor surface; b. passing the donor surface through a coating station, from which the donor surface emerges coated with discrete particles; and c. Repeatedly carrying out the following steps: i. treating a surface of the substrate such that the affinity of the particles for at least selected regions of the surface of the substrate is greater than the affinity of the particles for the donor surface; ii. contacting a surface of the substrate with a donor surface such that particles are transferred from the donor surface to only the treated selected areas of the surface of the substrate, thereby exposing areas of the donor surface through which the particles are transferred to corresponding areas of the substrate; and iii. thus forming a plurality of discrete particles adhered to the treated surface of the substrate; iv. Returning the donor surface to the coating station to make the monolayer of particles continuous, thereby allowing for subsequent printing of images on the surface of the substrate; wherein at least 50% by weight of the particles are metal pigments comprising a metal substrate and a surface treatment of the metal substrate, the surface treatment of the metal substrate comprising at least one coating layer surrounding the metal substrate and containing a metal oxide, and a surface modification of the coating layer, the surface modification of the coating layer comprising at least one heteropolysiloxane or compound having at least two terminal functional groups which are the same or different from each other and separated by a spacer; At least one terminal functional group is capable of chemically bonding to a coating layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0006] The method may further comprise a cleaning step during which particles remaining on the donor surface after contact with the substrate are removed from the donor surface, so that the donor surface is substantially free of particles before the next pass through the cleaning station. Such a cleaning step may be performed between each print cycle or may be performed intermittently, for example during particle exchange between print jobs. A print cycle corresponds to a time interval between subsequent passes of a reference point on the donor surface through a coating station, such passes being caused by the donor surface being movable relative to the coating station.

[0007] The particle-coated donor surface is used in a manner similar to the foils used in foil imaging, however, unlike foil imaging, damage to the continuity of the particle layer on the donor surface due to each print can be repaired by simply recoating the exposed areas of the donor surface where the previously applied layer was stripped by movement of the substrate to selected areas.

[0008] The reason that the particle layer on the donor surface can be repaired after each print is because the particles are selected to adhere to the donor surface stronger than they adhere to each other, resulting in the applied layer being essentially a monolayer of distinct particles.

[0009] Preferably, in step b, the donor surface leaves the coating station coated with a monolayer of particles. In the present disclosure, the term "monolayer" is used to describe a layer of particles on the donor surface, where at least 60% of the particles are in direct contact with the donor surface, in some embodiments, 70-100% of the particles are in direct contact with the donor surface, and in further embodiments, 85-100% of the particles are in direct contact with the donor surface. While some overlap may occur between particles in contact with such a surface, the layer may be only one particle deep over most of the area of ​​the surface. A monolayer in the present disclosure is formed from particles that are in sufficient contact with the donor surface, and thus is typically a single particle thick. Direct contact means that the particles remain attached to the donor surface at the exit of the coating station, for example after excess extraction, polishing, or any other similar process.

[0010] In order to obtain a mirror-like high gloss area on (a selected part of) the substrate, the selected surface (selected surface) must be sufficiently covered with particles, meaning that at least 70% of the selected surface is covered with particles, or at least 80%, or at least 90%, or at least 95% of the selected surface is covered with particles. The percentage of the area of ​​a particular target surface covered by particles can be evaluated by a number of methods known to those skilled in the art, for example by determining the optical density, optionally combined with determining the calibrated curvature of known covered points, by measuring the transmitted light if the substrate is sufficiently transparent, or by measuring the reflected light based on the reflectivity of the particles.

[0011] A preferred method for determining the percentage of the area of ​​a target surface covered by particles is as follows: A square sample with 1 cm sides is cut from the surface to be evaluated (e.g., cut from a donor surface or a printed substrate). The sample is analyzed by a microscope (laser confocal microscope (Olympus™, LEXT OLS30ISU) or optical microscope (Olympus™ BX61 U-LH100-3)) at up to 100x magnification (resulting in a field of view of at least about 128.9 μm×128.6 μm). At least three representative images are acquired in reflectance mode. The acquired images are analyzed using imageJ, a public domain Java image processing program developed by the National Institute of Health (NIH), USA). Images are displayed in 8-bit grayscale, and the program is allowed to suggest a reflectance threshold that distinguishes between reflective particles (relatively bright pixels) and possible gaps between adjacent or nearby particles (such voids appear as relatively dark pixels). A skilled operator can adjust the suggested thresholds as necessary, but typically will confirm them. The image analysis program then proceeds to measure the amount of pixels representing particles and the amount of pixels representing uncoated areas of interparticle voids, from which the area percentage of coverage can be readily calculated. Measurements made on different image portions of the same sample are averaged. If the sample is printed on a transparent substrate (e.g., a translucent plastic foil), a similar analysis can be performed in transmission mode, with particles appearing as relatively dark pixels and voids appearing as relatively light pixels. Results obtained by such methods, or by substantially similar analytical techniques known to those skilled in the art, are referred to as optical surface coverage and can be expressed as a percentage or ratio.

[0012] If printing is to be done on the entire surface of the substrate, a receiving layer (which may for example be adhesive) may be applied by a roller during step I to the substrate before it is pressed against the donor surface.

[0013] Most preferably, a receiving layer and / or an adhesive layer is applied onto the substrate in step i.

[0014] In particular, on the other hand, if printing is to be performed only on selected areas (selected areas) of the substrate, the adhesive layer or the receptive layer can be applied by any conventional printing method, for example by means of a die or printing plate, or by jetting the receptive layer onto the surface of the substrate. In other embodiments, the receptive layer is applied to the substrate surface by an indirect printing method, for example offset printing, screen printing, flexographic printing, or gravure printing.

[0015] As a further alternative, the entire surface of the substrate can be coated with an activatable receiving layer, which can be selectively made "tacky" by appropriate activation means. Whether selectively applied or selectively activated, the receiving layer in such cases constitutes at least a portion of the image printed on the substrate.

[0016] The term "tacky" is used in this disclosure only to indicate that the substrate surface or any selected area thereof has sufficient affinity for the particles to separate the particles from the donor surface and / or to hold the particles on the substrate when the donor surface and substrate are pressed against each other at a printing station, but does not necessarily have to be sticky to the touch. To allow printing of patterns in selected areas of the substrate, the affinity of the optionally activated receptor layer for the particles must be greater than the affinity of the uncovered substrate for the particles. In the context of this disclosure, the substrate is sometimes referred to as "uncovered" when it does not have a receptor layer or does not have a properly activated receptor layer. For most purposes, the uncovered substrate must have substantially no affinity for the particles, but some residual affinity (e.g., even if not visually detectable) may be tolerated or even desired for certain printing effects to allow selective affinity of the receptor layer.

[0017] The receiving layer may be activated, for example, by exposure to radiation (e.g., UV, IR, and near IR) before being pressed against the donor surface. Other means of receiving layer activation include temperature, pressure, moisture (e.g., moisture for rewettable adhesives), and even ultrasound, and such means may be combined to treat the receiving layer surface of the substrate, thereby rendering a compatible receiving layer tacky.

[0018] The nature of the receiving layer applied to the surface of the substrate may differ from substrate to substrate, inter alia, with respect to the mode of application and / or the selected activation means, but such formulations are known to those skilled in the art and do not need to be detailed further for understanding the printing method and system of the present invention. In brief, any thermoplastic, thermosetting, or hot melt polymer that is compatible with the intended substrate and exhibits sufficient adhesion, relative affinity for the envisaged particles, optionally after activation, may be used to implement the present disclosure. Preferably, the receiving layer is selected so as not to interfere with the desired printing effect (e.g., clear, transparent, and / or colorless).

[0019] Desirable characteristics of a suitable adhesive relate to the relatively short period of time required to activate the receiving layer, i.e., to selectively change the receiving layer from a non-tacky state to a tacky state, increasing the affinity of selected areas of the substrate so that they adhere sufficiently to the particles, thereby separating them from the donor surface. A fast activation time allows the receiving layer to be used in high speed printing. Adhesives suitable for the practice of the present disclosure are preferably capable of activation in a period of time no longer than the time it takes for the substrate to travel from the activation station to the printing station.

[0020] In some embodiments, activation of the receiving layer may occur substantially instantaneously upon printing. In other embodiments, an activation station or activation step may precede printing, in which case the receiving layer may be activated within a period of less than 10 seconds, or even less than 1 second, particularly less than about 0.1 seconds, or even less than 0.01 seconds. This period is referred to in this disclosure as the "activation time" of the receiving layer.

[0021] As mentioned above, a suitable receiving layer must have sufficient affinity with the particles for a monolayer according to the present disclosure to be formed. This affinity, which can alternatively be viewed as an intimate contact between the two, must be sufficient to hold the particles on the surface of the receiving layer and may result from the relative physical and / or chemical properties of the layer and the particles. For example, the receiving layer may have a hardness that is high enough to provide a satisfactory print quality, but low enough to allow adhesion of the particles to the layer. Such an optimal range may be viewed as allowing the receiving layer to be "locally deformable" on the scale of the particles, so that sufficient contact is formed. Such affinity or contact may additionally be augmented by chemical bonding. For example, the material forming the receiving layer may be selected so that it has suitable functional groups to hold the particles by reversible bonding (bonds supporting non-covalent electrostatic interactions, hydrogen bonds, and van der Waals interactions) or by covalent bonding. Similarly, the receiving layer must be suitable for the intended print substrate, and all these considerations are known to those skilled in the art.

[0022] The receiving layer may have a wide range of thicknesses, depending for example on the print substrate and / or on the desired print effect. A relatively thick receiving layer may be provided for an "embossed" embodiment, where the decoration is raised above the surface of the surrounding substrate. A relatively thin receiving layer may follow the contours of the surface of the print substrate, for example allowing a matte embodiment for a rough substrate. For gloss embodiments, the thickness of the receiving layer is typically selected to hide the substrate roughness, thus providing a flat surface. For example, for very smooth substrates, for example plastic films, the receiving layer may have a thickness of only a few tens of nanometers, for example for polyester films (e.g. polyethylene terephthalate (PET) foils) with a surface roughness of 50 nm, a thickness of about 100 nm. Smoother PET films allow the use of even thinner receiving layers. Substrates with a relatively rough surface in the micron or tens of microns range are advantageous for receiving layers with thicknesses in the same or similar size ranges when a gloss effect, and therefore some flattening / masking of the substrate roughness, is desired. Thus, depending on the substrate and / or the desired effect, the receptive layer may have a thickness of at least 10 nm, or at least 50 nm, or at least 100 nm, or at least 500 nm, or at least 1000 nm. For effects that can be recognized by tactile and / or visual detection, the receptive layer may even have a thickness of at least 1.2 micrometers (μm), at least 1.5 μm, at least 2 μm, at least 3 μm, at least 5 μm, at least 10 μm, at least 20 μm, at least 30 μm, at least 50 μm, or at least 100 μm. Although some effects and / or substrates (e.g., cardboard, carton, textiles, leather, etc.) may require a receptive layer having a thickness in the millimeter range, the receptive layer thickness is typically no more than 800 micrometers (μm), and is up to 600 μm, up to 500 μm, up to 300 μm, up to 250 μm, up to 200 μm, or up to 150 μm.

[0023] After printing has been performed, i.e. after the particles have been transferred from the donor surface to the tacky areas (i.e. the receiving layer) of the treated substrate surface upon pressing, the substrate may be further treated, for example by application of heat and / or pressure, to fix or polish the printed image, and / or may be coated with a varnish (e.g. a colorless or colored, transparent, semi-transparent or opaque overcoat), to protect the print surface, and / or may be overprinted with a different color ink (e.g. forming a foreground image). Some post-transfer steps (e.g. further pressure) may be performed on the entire surface of the printed substrate, while other steps may be applied only to selected parts. For example, a varnish may be selectively applied to parts of the image, for example to selected areas coated with particles, and optionally further to impart color effects.

[0024] Any device suitable for performing such a post-transfer step can be referred to as a post-transfer device (e.g., a coating device, a polishing device, a pressing device, a heating device, a curing device, etc.). The post-transfer device can additionally include any finishing device conventionally used in printing systems (e.g., a laminating device, a cutting device, a trimming device, a punching device, an embossing device, a perforating device, a creasing device, a bonding device, a folding device, etc.). The post-transfer device can be any suitable conventional equipment, the integration of which in the present printing system will be apparent to one skilled in the art without further detailed description.

[0025] In the method according to the invention, the particles contain at least 50% flaky metal substrate, preferably 75% of the particles have flaky metal substrate, more preferably at least 85%, and most preferably 95-100% of the particles contain flaky metal substrate.

[0026] In one embodiment of the method according to the invention, the metal substrate is a flaky metal substrate. In a further embodiment, the flaky metal substrate has an average thickness (h50 value) in the range of 10-500 nm, more preferably 20-300 nm, most preferably 30-100 nm.

[0027] In general, the thickness of metal or metallic particles can be determined by scanning electron microscopy (SEM). For this purpose, the particles are incorporated in a two-component clear coat (Autoclear Plus HS from Sikkens) at a concentration of about 10% by weight with a sleeve brush, applied to a film by a spiral applicator (wet film thickness 26 μm) and dried. After a drying time of 24 h, cross sections of the drawdowns of these applicators were made. The cross sections were analyzed by SEM (Zeiss supra35) using a SE (secondary electron) detector. For the value analysis of platelet particles, the particles must be well oriented in a plane parallel to the substrate, so that systematic errors in the tilt angle caused by poorly oriented flakes are minimized.

[0028] Here, a sufficient number of particles must be measured so that a representative average value is provided. Conventionally, about 100 particles are measured. The h50 value is the median value of the particle thickness distribution measured in this way. This h50 value can be used as a measure of the average thickness.

[0029] In one of the embodiments of the method according to the invention, the flaky metallic substrate has an aspect ratio in the range of 1500:1 to 10:1, preferably 1000:1 to 50:1, more preferably 800:1 to 100:1, the aspect ratio being defined as the ratio between the average pigment diameter (D50 value) and the average pigment thickness (h50 value).

[0030] Pigment sizes are typically indicated using D values, which represent the quantiles of the volume-average particle size distribution in frequency representation. Here, this number indicates the percentage of particles smaller than a certain size contained in the volume-average particle size distribution. For example, the D50 value indicates a size larger than 50% of the particles. These measurements are performed by laser granulometry, for example with a particle size analyzer manufactured by Sympatec (model: Helos / BR). The measurements are performed according to data from the manufacturer.

[0031] In one embodiment of the method according to the invention, the flaky metallic substrate is selected from flaky substrates of aluminum, copper, zinc, gold bronze, chromium, titanium, zirconium, tin, iron and steel, or pigments of alloys of these metals. In a preferred embodiment, the flaky metallic substrate is aluminum, gold bronze or copper, and in a most preferred embodiment, the flaky metallic substrate is aluminum.

[0032] Even if the coating contains a metal oxide, the metal substrate may contain up to 30% by weight of an oxide of the same metal, thus an aluminium substrate may contain up to 30% by weight of aluminium oxide.

[0033] The metal substrate may be produced by milling or by PVD (Physical Vapor Deposition) method. More preferred is a flake metal substrate produced by PVD method, and most preferred is such flake metal substrate is an aluminum pigment.

[0034] In one embodiment of the method according to the invention, the metal oxide of the coating layer is selected from the group consisting of silicon oxide, aluminum oxide, boron oxide, zirconium oxide, cerium oxide, iron oxide, titanium oxide, chromium oxide, tin oxide, zinc oxide, molybdenum oxide, vanadium oxide, and mixtures thereof. Such oxides stabilize the surface of the metal substrate against corrosion processes and contribute to a relatively high gloss level of the substrate treated by the method according to the invention, which is more stable over time.

[0035] More preferred metal oxides of the coating layer are silicon oxide, molybdenum oxide, aluminum oxide, and mixtures thereof. Most preferred are silicon oxide or molybdenum oxide. Another embodiment of the coating layer is molybdenum oxide, on which another metal oxide containing silicon oxide is coated.

[0036] In the present invention, the term "metal oxide" is used with respect to a particular metal to include any of the metal oxides, any of the metal hydroxides, any of the metal oxide hydrates, and mixtures thereof.

[0037] According to the invention, the metal oxide of the coating layer is based on a metal different from the metal substrate itself. Some metal substrates form native oxides under ambient atmospheric conditions. However, these native metal oxides do not provide the metal substrate with sufficient corrosion stability or mechanical rigidity. The most prominent example is aluminum, which forms a coating (covering layer) of aluminum oxide / hydroxide several nanometers thick when in contact with oxygen and / or moisture.

[0038] For the avoidance of doubt, such layers of native oxide that form on metal substrates under ambient atmospheric conditions are not considered to be surface treatments of metal substrates according to the present invention.

[0039] In one embodiment, the substrate is an aluminum substrate coated with silicon oxide or molybdenum oxide as a first coating layer and silicon oxide as a second coating layer.

[0040] In a further embodiment, the coating layer contains a metal oxide, preferably a silicon oxide, more preferably a silicon dioxide, in an amount of at least 60 wt.-%, further preferably at least 70 wt.-%, further preferably at least 80 wt.-%, further preferably at least 95 wt.-%, based on the total weight of the metal oxide- or silicon oxide-containing coating, respectively.

[0041] In another embodiment, up to 100% by weight of the remaining compounds in the metal oxide coating layer contain or consist of a further metal oxide different from silicon oxide, resulting in a mixed metal oxide layer surrounding the flaky metal substrate.

[0042] In another embodiment, up to 100% by weight of the remaining compounds in the metal oxide coating layer comprise or consist of organic materials, thus forming a hybrid metal oxide / organic coating layer.

[0043] In a particular embodiment, the organic material contains or consists of an organic oligomer and / or polymer. That is, the metal oxide coating may be formed as a hybrid layer of a metal oxide coating and an organic oligomer and / or an organic polymer, which preferably interpenetrate each other. Such a type of hybrid coating can be formed by simultaneous formation of a metal oxide coating, preferably by sol-gel synthesis, and formation of a polymer or oligomer. The hybrid layer is thus preferably an essentially homogeneous layer, in which the metal oxide coating and the one or more organic oligomers and / or the one or more organic polymers are essentially homogeneously distributed within the coating. Metal effect pigments coated with such a hybrid layer are disclosed in EP1812519B1 or WO2016 / 120015A1. Such a hybrid layer improves the mechanical properties of the coating layer.

[0044] According to another embodiment of the present invention, the metal oxide hybrid coating layer contains 70-95 wt. %, preferably 80-90 wt. %, of silicon oxide, preferably silicon dioxide, and 5-30 wt. %, preferably 10-20 wt. %, of organic oligomers and / or organic polymers, each based on the total weight of the metal oxide coating layer.

[0045] One or more organofunctional silanes are preferred for use as organic network formers in such hybrid layers. The one or more organofunctional silanes can be bonded to the silicon oxide network following hydrolysis of the hydrolyzable groups (hydrolyzable groups). Upon hydrolysis, the hydrolyzable groups are usually replaced by OH groups, which then form covalent bonds with the OH groups in the inorganic silica network by condensation. The hydrolyzable groups are preferably halogen, hydroxyl, or alkoxy having 1 to 10 carbon atoms, preferably 1 to 2 carbon atoms, which may be linear or branched in the carbon chain, and mixtures thereof.

[0046] Suitable organofunctional silanes are, for example, numerous representatives manufactured by Evonik and sold under the trade name "Dynasylan". For example, 3-methacryloxypropyltrimethoxysilane (Dynasylan MEMO) can be used to form (meth)acrylates or polyesters, vinyltriethoxysilane or vinyltrimethoxysilane (Dynasylan VTMO or VTEO) can be used to form vinyl polymers, 3-mercaptopropyltriethoxysilane or 3-mercaptopropyltrimethoxysilane (Dynasylan MTMO or 3201) can be used for copolymerization in rubber polymers, aminopropyltrimethoxysilane (Dynasylan AMMO) or N2-aminoethyl-3-aminopropyltrimethoxysilane (Dynasylan DAMO) can be used to form β-hydroxylamines, or 3-glycidoxypropyltrimethoxysilane (Dynasylan GLYMO) can be used to form urethane networks or polyether networks.

[0047] Other examples of silanes with vinyl or (meth)acrylate functionality are: isocyanatotriethoxysilane, 3-isocyanatopropoxyltriethoxysilane, vinylethyldichlorosilane, vinylmethyldichlorosilane, vinylmethyldiacetoxysilane, vinylmethyldiethoxysilane, vinyltriacetoxysilane, vinyltrichlorosilane, phenylvinyldiethoxysilane, phenylallyldiethoxysilane, phenylallyldichlorosilane, 3-methacryloxypropyltriethoxysilane, methacryl ... propyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, 2-methacryloxyethyltri-ethoxysilane, 2-methacryloxyethyltri-methoxysilane, 2-acryloxyethyltriethoxysilane, 2-acryloxyethyltrimethoxysilane, 3-methacryloxypropyltris(methoxy-ethoxy)silane, 3-methacryloxypropyltris(butoxyethoxy)silane, 3-methacryloxypropyltris(propoxy)silane, or 3-methacryloxypropyltris(butoxy)silane.

[0048] In a preferred development of the invention, the silicon oxide, preferably silicon dioxide, and the organic network of oligomers and / or polymers are both present as interpenetrating networks.

[0049] For the purposes of the present invention, "organic oligomer" in the hybrid layer is understood to mean the term commonly used in polymer chemistry, i.e. a bond from 2 to 20 monomer units (Hans-Georg Elias, "Makromolekule", 4th edition, 1981, Huethig & Wepf Verlag Basel). A polymer is a bond from more than 20 monomer units.

[0050] The average chain length of the organic moiety can be varied by varying the ratio of monomer concentration to the concentration of the organic network former. The average chain length of the organic moiety is from 2 to 10,000 monomer units, preferably from 3 to 5,000 monomer units, more preferably from 4 to 500 monomer units, and even more preferably from 5 to 30 monomer units. Furthermore, in other embodiments, for use as the organic component, the organic polymer has an average chain length of from 21 to 15,000 monomer units, more preferably from 50 to 5,000 monomer units, and most preferably from 100 to 1,000 monomer units.

[0051] In another embodiment of the present invention, the metal oxide-containing coating layer consists of a mixed layer of a metal oxide coating, preferably silicon oxide, more preferably silicon dioxide, and an organofunctional silane, the organofunctional silane having a functional group that is not polymerized or oligomerized. Such organofunctional silanes are called network modifiers.

[0052] Preferably, the network modifier is an organofunctional silane having the formula:

[0053] [ka]

[0054] In the formula, z is an integer from 1 to 3, R is an unsubstituted, unbranched or branched alkyl chain with 1 to 24 C atoms, or an aryl group with 6 to 18 C atoms, or an arylalkyl group with 7 to 25 C atoms, or a mixture thereof, and X is a halogen group and / or preferably an alkoxy group. Preferred are alkylsilanes with an alkyl chain in the range of 1 to 18 C atoms, or arylsilanes with a phenyl group. R may be cyclically bonded to Si, in which case z is typically 2. X is most preferably ethoxy or methoxy.

[0055] Mixtures of organofunctional silanes with different z values ​​may be used. Preferred examples of such network-modified organofunctional silanes are alkyl or aryl silanes. Examples of such silanes are butyltrimethoxysilane, butyltriethoxysilane, octyltrimethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, decyltrimethoxysilane, hexadecyltrimethoxysilane, hexadecyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, and mixtures thereof.

[0056] In one embodiment of the method according to the invention, the metal substrate comprises a second coating layer of a compound having at least two terminal functional groups, which may be the same or different from each other and separated by a spacer. At least one functional group is found to bond to the metal substrate having a first coating layer of a metal oxide. At least one other functional group faces outwardly towards the treated surface of the substrate.

[0057] Surface modification of coated flaky metal substrates Then, the surface of the flaky particles treated with the coating layer containing the metal oxide and optional further coating layer is further modified by a surface modification which is at least one heteropolysiloxane or a compound having at least two terminal functional groups which are the same or different from each other and spaced apart, at least one terminal functional group can be chemically bonded to the coating layer containing the metal oxide. In most preferred embodiments, the surface modification is bonded to the top surface of the metal oxide.

[0058] This surface modification makes it possible to modify and control the surface of the metal oxide, for example with regard to hydrophilic and hydrophobic surface properties, so that an optimal balance can be found with regard to the respective affinity of the coated particles, and in particular with regard to the affinity of the coated flake metallic effect pigments to the donor and to the substrate surface.

[0059] As terminal functional groups, alkoxysilyl groups (e.g. methoxy and ethoxy silanes), halosilanes (e.g. chlorosilanes) or the groups of phosphates or phosphites and acids of phosphites can be considered. The groups mentioned are linked to a second, lacquer-compatible group by means of a relatively long or relatively short spacer. The spacer can be a non-reactive alkyl chain, a siloxane, a polyether, a thioether or a urethane or a group of the general formula (C,Si) n H m (N, O, S) x , n=1 to 50, m=2 to 100 and x=0 to 50. The lacquer compatible groups preferably include acrylates, methacrylates, vinyl compounds, amino or cyano groups, isocyanates, epoxy groups, carboxy groups or hydroxy groups.

[0060] In certain embodiments, especially upon calcination or curing of the metal particles adhered to the substrate, these groups may chemically react with a reaction layer located between the substrate and the flake metal pigment in a crosslinking reaction according to known chemical reaction mechanisms.

[0061] The particles used in the method according to the invention are produced by first coating a metal substrate with a metal oxide, preferably by sol-gel synthesis. Here, flake-shaped metal effect pigments are dispersed in a solvent, which is preferably an alcoholic solvent, for example ethanol or isopropanol. A precursor of the metal oxide, for example tetraethoxysilane, and water are added, and the sol-gel synthesis is catalyzed by the addition of a base or an acid. Two-component catalysis may also be used, for example by first adding an acid and then a base, as described in WO2011 / 095341A1.

[0062] In a particular embodiment, the organic acid used as the acid catalyst is selected from formic acid, acetic acid, propionic acid, oxalic acid, malonic acid, maleic acid, succinic acid, anhydrides of these acids, and mixtures thereof. It is particularly preferred to use formic acid, acetic acid, or oxalic acid, and mixtures thereof. In a particular embodiment of the present invention, the amine catalyst is selected from dimethylethanolamine (DMEA), monoethanolamine, diethanolamine, triethanolamine, ethylenediamine (EDA), tert-butylamine, monomethylamine, dimethylamine, trimethylamine, monoethylamine, diethylamine, triethylamine, ammonia, pyridine, pyridine derivatives, aniline, aniline derivatives, chlorine, chlorine derivatives, urea, urea derivatives, hydrazine derivatives, and mixtures thereof.

[0063] As basic amine catalysts for the sol-gel reaction it is particularly preferred to use ethylenediamine, monoethylamine, diethylamine, monoethylamine, dimethylamine, trimethylamine, triethylamine, ammonia or mixtures thereof.

[0064] After the flake-shaped metal effect pigments have been coated with the metal oxide, the surface of the metal oxide is coated with a surface modifier. This step may be carried out in the same vessel in which the metal oxide was formed or in a different step. For example, the first coated flake-shaped particles are stirred and heated in an organic solvent, mixed with a solution of a base in water or another solvent, the surface modifier is added, the reaction mixture is cooled after a reaction time of 15 minutes to 24 hours, and the effect pigment is separated by suction removal. The resulting filter cake may be dried in vacuum at about 60-130°C. With some surface modifiers, it is not necessary to heat the mixture, and for these materials simple mixing may be sufficient.

[0065] Silane-based surface modifiers are described, for example, in DE 4011044 C2. Phosphoric acid-based surface modifiers are available, inter alia, as, for example, Lubrizol® 2061 and LUBRIZOL® 2063 (Langer & Co).

[0066] The surface modifiers can also be produced directly on the coated particles by chemical reaction from suitable starting materials. In this case, the coated particles are also stirred and heated in an organic solvent. Optionally, they are then mixed with a solution of a base, for example an organic amine, which can act as a kind of catalyst for the modification reaction. Essentially the same catalysts can be used as those used for the formation of the metal oxide. After a reaction time of about 1 to 6 hours, the suspension is cooled and subjected to suction removal of the flake-shaped effect pigments. The filter cake thus obtained can be dried in a vacuum at 60 to 130° C. The reaction can also be carried out in a solvent in which the coated particles are subsequently formed and used as a paste. In this case, a drying step becomes unnecessary.

[0067] Particular examples of surface modifiers which may be mentioned are, for example, crosslinkable organofunctional silanes, which, after the hydrolysis operation, are fixed with their reactive Si-OH units on the oxidized surface of the effect pigment. The potentially crosslinkable organic groups can subsequently react with reactive agents of the treated parts of the print substrate. Examples of suitable crosslinkable organofunctional silanes are: Vinyltrimethoxysilane, aminopropyltriethoxysilane, N-ethylamino-N-propyldimethoxysilane, isocyanatopropyltriethoxysilane, mercaptopropyltrimethoxysilane, vinyltriethoxysilane, vinylethyldichlorosilane, vinylmethyldiacetoxysilane, vinylmethoxydichlorosilane, vinylmethyldiethoxysilane, vinyltriacetoxysilane, vinyltrichlorosilane, phenylvinyldiethoxysilane, phenylallyldichlorosilane, 3-isocyanatopropoxyltriethoxysilane, methacryloxypropenyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 2-glycidyloxypropyltrimethoxysilane, 1,2-epoxy-4-(ethyltriethoxysilyl)-cyclohexane, 3-acryloxypropyltrimethoxysilane silane, 2-methacryloxyethyl trimethoxysilane, 2-acryloxyethyl trimethoxysilane, 3-methacryloxypropyl triethoxysilane, -acryloxypropyl trimethoxysilane, 2-methacryloxyethyl triethoxysilane, 2-acryloxyethyl tri-ethoxysilane, 3-methacryloxypropyl tris(methoxyethoxy)silane, 3-methacryloxypropyl tristbutoxyethoxysilane, 3-methacryloxypropyl tris(propoxy)silane, 3-methacryloxypropyl tris(butoxy)silane, 3-acryloxypropyl tris(methoxyethoxy)silane, 3-acryloxypropyl tris(butoxyethoxy)silane, -acryloxypropyl tris(propoxy)silane, 3-acryloxypropyl tris(butoxy)silane. 3-methacryloxypropyl trimethoxysilane is particularly preferred.

[0068] These and other silanes are commercially available, for example, from ABCR, D-76151 Karlsruhe, from Evonik, Essen, Germany under the trade name "Dynasylan", or from Sovento Chemie, D-40468 Düsseldorf. Vinylphosphonic acid or vinylphosphonic acid diethyl ester can also be listed here as a binder (Evonik, Essen, Germany).

[0069] The surface of the initially coated particles can also be modified with a layer having side-by-side one or more of the above-mentioned hydrophobic alkylsilanes (e.g. those described in EP 0 634 459 A2) and at least one other reactive species. Depending on the specific requirements imposed on the pigment, the proportion of the surface modifiers described in the present disclosure in the layer can essentially be 10% to 100%. However, it is particularly preferred if the proportion of reactive species, preferably reactive silane species, is 10, 30, 50, 75 or 100% by weight, based on the total amount of surface modifiers. Such different ratios of reactive species, for example to hydrophobic alkylsilanes, provide for a gradual change in the effective binding strength either to the surface of the donor substrate or to the surface of the treated part of the printing substrate.

[0070] In one embodiment of the method of the present invention, the metal substrate or coated metal substrate comprises a surface modification of a heteropolysiloxane, the heteropolysiloxane being prepared from a composition comprising at least one aminosilane component and at least one alkylsilane component.

[0071] The heteropolysiloxane may be a precondensed heteropolysiloxane, which is prepared by mixing an aminoalkylalkoxysilane with an alkyltrialkoxysilane and / or a dialkyldialkoxysilane, mixing the mixture with water, adjusting the pH of the reaction mixture to a value between 1 and 8, and removing the alcohol present and / or generated during the reaction. These precondensed heteropolysiloxanes are essentially free of organic solvents. The aminoalkylalkoxysilanes, alkyltrialkoxysilanes, and dialkyldialkoxysilanes that can be used to prepare the precondensed heteropolysiloxanes may be water-soluble or water-insoluble. Preferred heteropolysiloxanes can be obtained from Evonik Industries AG, 45128 Essen, Germany, and are available under the trade names Dynasylan Hydrosil 2627, Dynasylan Hydrosil 2776, Dynasylan Hydrosil 2909, Dynasylan 1146, and Dynasylan Hydrosil 2907. Particularly preferred water-based heteropolysiloxanes are Dynasylan Hydrosil 2627, Dynasylan Hydrosil 2776, Dynasylan Hydrosil 2907, and Dynasylan Hydrosil 2909. According to a preferred variant of the invention, the precondensed heteropolysiloxane is selected from the group consisting of Dynasylan Hydrosil 2627, Dynasylan Hydrosil 2776, Dynasylan Hydrosil 2909, Dynasylan 1146, Dynasylan Hydrosil 2907, and mixtures thereof.

[0072] The heteropolysiloxane preferably has an average molecular weight of at least 500 g / mol, particularly preferably at least 750 g / mol, most particularly preferably at least 1000 g / mol. The average molecular weight can be determined, for example, by NMR spectroscopy, e.g. 29 By Si-NMR, 1The molecular weight can be determined by combining with H-NMR. Descriptions of such methods can be found in, for example, "Organofunctional alkoxysilanes in dilute aqueous solution: New accounts on the dynamic structural mutability", Journal of Organometallic 5 Chemistry, 625 (2001), 208-216, and other publications.

[0073] Heteropolysiloxanes can be applied in various ways. It has been found that the addition of polysiloxanes, preferably in dissolved or dispersed form, to the suspension containing the metallic pigment to be coated is particularly advantageous. For example, the reaction product obtained from a previous coating step can be used together with a metal oxide, in particular a silicon oxide, to provide the suspension containing the metallic substrate to be coated.

[0074] The structure of the precondensed heteropolysiloxane of the present invention can be linear, ladder, cyclic, crosslinked, or a mixture thereof.Furthermore, in a further embodiment, it is preferred that the heteropolysiloxane is composed of at least 87% by weight, preferably at least 93% by weight, more preferably at least 97% by weight, based on the total weight of the heteropolysiloxane, of silane monomer components, and the silane monomer components are selected from the group consisting of aminosilane, alkylsilane, vinylsilane, arylsilane, and mixtures thereof.In particular, it is preferred that the heteropolysiloxane is composed of aminosilane and alkylsilane components in the above amounts.

[0075] Silane monomers are used, for example, in the form of alkoxides. The alkoxides are cleaved to initiate oligomerization or polymerization, and as a result of the condensation process, the silane monomers are converted into the corresponding heteropolysiloxanes or crosslinked. Preferably, in the present invention, methoxides and ethoxides are used as alkoxides. Unless otherwise stated, the weight percent of silane monomer components in heteropolysiloxanes in the sense of the present invention is based on the weight of silane monomers without components that are cleaved by condensation to heteropolysiloxanes, such as alkoxy groups. The preparation of such polysiloxanes is described in the literature. For example, corresponding preparation methods can be found in US 5,808,125A, US 5,679,147, and US 5,629,400. It has been found that aminosilanes with one or two amino groups per Si are particularly advantageous for forming the heteropolysiloxanes of the present invention. In a further embodiment, at least 92 wt. %, preferably at least 97 wt. %, of the aminosilane components contained in the heteropolysiloxane are selected from aminosilanes having one or two amino groups, each in wt. % based on the total weight of the aminosilane components contained in the heteropolysiloxane.

[0076] For example, (H2N(CH2)3Si(OCH3)3), ((3-aminopropyl 1)(trimethoxy)silane, AMMO), (H2N(CH2)3Si(OC2H5)3((3-aminopropyl / (triethoxysilane, AMEO), (H2N(CH2)2NH(CH2)3Si(OCH3)3, ((N-2-aminoethyl)-3-aminopropyl)(trimethoxysilane), (DAMO)), (H2N(CH2)2NH(CH2)3)Si( 0C2H5), ((N-(2-aminoethyl 1-3-aminopropyl)(triethoxy)silane), and mixtures thereof have been found to be advantageous. In a further embodiment, the aminosilane component contained in the heteropolysiloxane is at least 92% by weight, preferably at least 97% by weight, selected from the above group and mixtures thereof, each amount being based on the total weight of the aminosilane components contained in the heteropolysiloxane.

[0077] In a further embodiment, it is preferred that the heteropolysiloxane used according to the present invention contains only a small amount of epoxysilane or does not contain epoxysilane at all.The corresponding heteropolysiloxane in conventional wet coating system typically shows relatively good adhesion.In particular, in a further embodiment, it is preferred that the heteropolysiloxane contains 10wt% or less, preferably 6wt% or less, more preferably 4wt% or less, even more preferably a trace amount or less of epoxysilane component, each amount being based on the total amount of heteropolysiloxane.

[0078] It has been found that only small amounts of heteropolysiloxane are typically sufficient.In a further embodiment, the surface modification containing at least one, preferably only one, heteropolysiloxane has an average thickness of 20 nm or less, more preferably 10 nm or less.In particular, it is preferred that at least one, preferably only one, heteropolysiloxane is essentially present in the form of a monolayer.It has been found to be particularly advantageous when at least one heteropolysiloxane is applied to a surrounding coating layer containing silicon oxide.The application of the coating layer essentially composed of at least one metal oxide is preferably carried out by a sol-gel process.

[0079] The heteropolysiloxane used according to one embodiment of the present invention can be prepared, for example, by condensation of alkylsilane and aminosilane.However, those skilled in the art will recognize that the same heteropolysiloxane can also be prepared by other methods, for example, by reaction of at least one alkylsilane, at least one halogen alkylsilane, and at least one amine.Such heteropolysiloxane can also be considered formally as the condensation product of the corresponding alkylsilane and aminosilane, and is included in the present invention.Those skilled in the art can choose from various retrosynthetic routes based on the knowledge of the present invention and known expertise.

[0080] In a further embodiment, it is also preferred that 1 wt.% or less of the silane monomer component is a fluorinated silane, based on the total weight of the heteropolysiloxane. The fluorinated silane component is preferably contained in only trace amounts in the applied heteropolysiloxane layer, or more preferably, is absent from this layer.

[0081] In the context of the present invention, the term "aminosilane" indicates that the silane concerned has at least one amino group. This amino group does not necessarily have to be directly bonded to the silicon atom of the silyl group. Examples of suitable aminosilanes can be found, for example, in US 9,624,378 B2.

[0082] Examples of commercially available aluminum pigments that can be used in the process of the present invention are Hydrolan™ type products, Hydroshine™ type products, and Aquashine type products, all from ECKART, or Emeral™ (all from Toyo Aluminum Co., Japan), or Silbercote™ (all formerly Silberline Manufacturing Co.).

[0083] Donor Surface The donor surface of the printing method in a preferred embodiment is a hydrophobic surface, typically made of an elastomer that may be adapted to have the properties as described in this disclosure, and is generally prepared from a silicone-based material. Poly(dimethyl-siloxane) polymers are based on silicone and have been found to be suitable. In one embodiment, a liquid curable composition was formed by combining three silicone-based polymers: a vinyl-terminated polydimethylsiloxane 5000 cSt (DMS V35, Gelest™, CAS, No. 68083-19-2) in an amount of about 44.8 wt. % of the total composition; a vinyl-functional polydimethylsiloxane having terminal and pendant vinyl groups (Polymer XP RV5000, Evonik™ Hanse, CAS No. 68083-18-1) in an amount of about 19.2 wt. %; and a branched vinyl-functional polydimethylsiloxane (VQM Resin-146, Gelest™, CAS No. 68584-83-8) in an amount of about 25.6 wt. %. To the mixture of vinyl-functional polydimethylsiloxanes, the following was added: a platinum catalyst, for example platinum divinyltetramethyldisiloxane complex (SIP6831.2, Gelest™, CAS No. 68487-92-2) in an amount of about 0.1% by weight, an inhibitor to better control the curing conditions, Evonik™ Hanse's Inhibitor 600, in an amount of about 2.6% by weight, and finally a reactive crosslinker, for example methylhydrosiloxane dimethylsiloxane copolymer (HMS301, Gelest™, CAS No. 68037-59-2) in an amount of about 7.7% by weight, which initiates the addition cure. This addition curable composition is then applied immediately thereafter using a smooth leveling knife onto a donor surface support (for example, an epoxy sleeve that can be attached to the drum 10), which is optionally treated (for example, by corona or with a primer material) to improve the adhesion of the donor surface material to the support. The applied fluid is cured at 100-120° C. for 2 hours in a ventilated oven, thereby forming a donor surface.

[0084] This hydrophobicity allows the particles to be exposed to selective peeling without tearing by an adhesive film that forms on the receiving layer-bearing substrate, thereby providing a clean transfer to the substrate.

[0085] The donor surface must be hydrophobic, i.e., the wetting angle of the particles with the aqueous carrier must be greater than 90°. The wetting angle is determined by the meniscus at the liquid / air / solid interface. The wetting angle or equilibrium contact angle Θ is the angle between the receding (minimum) contact angle Θ and the surface ... r and the advancing (maximum) contact angle Θ A and can be calculated from these and evaluated at a given temperature and pressure related to the operating conditions of the process. It is conventionally measured at ambient temperature (about 23° C.) and pressure (about 100 kPa) from a drop of liquid having a volume of 5 μl, where the liquid-vapor interface meets the solid polymer surface, using a goniometer or drop shape analyzer. Contact angle measurements can be performed, for example, using a contact angle analyzer-Kruss™, "Easy Drop" FM40Mk2, using dilution water as the standard liquid.

[0086] This hydrophobicity may be an inherent property of the polymer forming the donor surface, or may be promoted by the addition of hydrophobic additives into the polymer composition. Additives that may promote the hydrophobicity of the polymer composition may be, for example, oils (e.g., synthetic, natural, vegetable, or mineral oils), waxes, plasticizers, and silicone additives. Such hydrophobic additives may be compatible with any polymeric material, so long as their respective chemical nature or amount does not interfere with the proper formation of the donor surface and, for example, does not interfere with the proper curing of the polymeric material.

[0087] The roughness or finish of the donor surface will be reproduced on the printed metallic surface. Thus, if a mirror finish or high gloss appearance is required, the donor surface needs to be smoother than if a matte or satin appearance is desired. These visual effects can also result from roughness of the printing substrate and / or the receiving layer.

[0088] The donor surface may be the outer surface of a drum, but this is not essential, since it may alternatively be the surface of an endless transport member, which has the form of a belt guided over guide rollers and is maintained under suitable tension at least during its passage through the coating device. Additional structures may allow the donor surface and the coating station to move relative to each other. For example, the donor surface may form a movable plane that can repeatedly pass under a static coating station, or it may form a static plane, the coating station repeatedly moving from one end of this plane to the other, thereby covering the donor surface entirely with particles. It is envisaged that both the donor surface and the coating station may move relative to each other and relative to a stationary point in space, thus reducing the time it would take to achieve an overall coating of the donor surface with particles provided by the coating station. All such donor surface configurations can be said to be movable (e.g., rotationally, circularly, endlessly, repeatedly, etc.) relative to the coating station, such that such passing donor surfaces can be coated with particles (or replenished with particles in exposed areas).

[0089] The donor surface may additionally accommodate practical or specific considerations arising from the particular configuration of the printing system. For example, it may be sufficiently flexible to be mounted onto a drum, may be sufficiently abrasion resistant, may be inert to the particles and / or fluids used, and / or may be resistant to any operating conditions of interest (e.g., pressure, heat, tension, etc.). Satisfying any of such characteristics tends to advantageously increase the useful life of the donor surface.

[0090] The donor surface, whether formed as a sleeve over a drum or as a belt over a guide roller, may have a body opposite the particle-receiving outer layer, which together with the donor surface may be referred to as a transfer member. The body may have different layers, each of which provides one or more desired selected properties to the overall transfer member, such as mechanical resistance, thermal conductivity, compressibility (e.g., to improve "macroscopic" contact between the donor surface and the print cylinder), conformability (e.g., to improve "microscopic" contact between the donor surface and the print substrate on the print cylinder), and any other property readily understood by those skilled in the art of print transfer members.

[0091] A further aspect of the invention is directed to the use of particles, at least 50% by weight of which are flaky metal pigments, comprising a flaky metallic substrate and a surface treatment of the metallic substrate, the surface treatment of the metallic substrate comprising at least one coating layer surrounding the metallic substrate comprising a metal oxide, the surface modification layer of the coating comprising at least one heteropolysiloxane or compound having at least two terminal functional groups which are the same or different from each other and separated by a spacer, at least one terminal functional group being capable of chemically bonding to the coating layer, 1. A method of printing on a surface of a substrate, the method comprising: (a.) providing a donor surface; (b.) passing a donor surface through a coating station, the donor surface emerging from the coating station coated with discrete particles; and (c.) Repeatedly performing the following steps: (i.) treating a surface of a substrate to cause at least selected regions of the surface of the substrate to have a greater affinity for the particles than the affinity of the particles for the donor surface; (ii.) contacting a surface of the substrate with a donor surface such that particles are transferred from the donor surface to only the treated selected areas of the surface of the substrate, thereby exposing areas of the donor surface to which particles have been transferred to corresponding areas on the substrate; and (iii.) thus forming a plurality of separate particles adhered to the treated surface of the substrate; (iv.) Returning the donor surface to the coating station, thereby making the monolayer of particles continuous, thus allowing subsequent printing of images onto the surface of the substrate.

[0092] All aspects mentioned above in the description relating to the method of printing according to the invention apply equally to the use of the particles in the method of printing on the surface of a substrate as outlined in the previous paragraph. EXAMPLES

[0093] [Table 1]

[0094] Example 1 35.49 pbw of AF1 and 43.09 pbw of isopropanol were mixed thoroughly until a dispersion was obtained. 0.02 pbw of peroxomolybdic acid solution (obtained by mixing 1 pbw of molybdic acid with 3 pbw of 30% hydrogen peroxide solution) was added and mixing was continued. The dispersion was then heated to 80°C and 3.71 pbw of TEOS, 5.20 pbw of water, and 0.56 pbw of acetic acid were added. The mixture was stirred for a period of time while maintaining the temperature at 80°C.

[0095] While stirring at 80° C., 0.28 pbw of ethylenediamine and 3.55 pbw of isopropanol were added at intervals for a total of 0.84 pbw of ethylenediamine. Then, with the mixture stirred and held at 80° C., 0.35 pbw of SD2 and 0.09 pbw of SD3 were added. Stirring at 80° C. was continued for several hours. The mixture was then cooled and some of the solvent was removed to obtain a paste of encapsulated aluminum particles.

[0096] Example 2 13.23 pbw of AF2, 67.53 pbw of isopropanol, 4.31 pbw of water, and 0.07 pbw of Disperbyk118 were mixed thoroughly until a dispersion was obtained. 5.03 pbw of TEOS was added, and the dispersion was heated to 80°C while mixing. While stirring at 80°C, 0.13 pbw of ethylenediamine, 3.32 pbw of isopropanol, and 0.21 pbw of water were added at intervals, for a total of 0.39 pbw of ethylenediamine. Then, 0.25 pbw of SD4 and 0.25 pbw of SD5 were added while stirring the mixture and maintaining it at 80°C. Stirring at 80°C was continued for a period of time. The mixture was then cooled and some of the solvent was removed to obtain a paste of encapsulated aluminum pigment.

[0097] Example 3 As in Example 1, except that 0.50 pbw of SD1 was used as the surface modification instead of silanes SD2 and SD3.

[0098] Example 4 The aluminum particle pastes obtained in each of Examples 1 to 3 were dispersed in water and applied to a substrate using the method described in WO2016 / 189515.

[0099] As Comparative Example 1, a paste of aluminum flakes (aluminum powder 6150, supplied by Quanzhou Manfong Metal Powder Co., Ltd., China) was dispersed in water and applied to a substrate using the method described in WO2016 / 189515.

[0100] In Comparative Example 2, a paste of aluminum flakes AF2 (Silvershine S1100, Eckart) coated with fatty acid was used.

[0101] As Comparative Example 3, the aluminum paste of Comparative Example 2 was coated with SiO2 according to the procedure of Example 1. However, silanes SD2 and SD3 were not added, so the aluminum flakes were coated with SiO2 only.

[0102] The gloss, gloss retention, and corrosion stability of the samples thus prepared were measured. By gloss retention, it is meant that the gloss is measured after repeated printing procedures over a period of time, for example, 1 day, 2 days, and finally 30 days after printing.

[0103] The samples prepared with aluminum particles of Examples 1-3 all showed high initial gloss levels, good gloss retention and good corrosion stability. In particular, the coated metallic effect pigments according to Examples 1 and 3 showed an average gloss of about 800 gloss units measured at 20° using the Byk-microTRI gloss. The substrates printed in Comparative Examples 1 and 2 showed high initial gloss levels, but poor gloss retention, since the samples showed corrosion within 2 days after application.

[0104] In contrast to the other examples according to the invention and Comparative Examples 1 and 2, the effect pigment of Comparative Example 3 was not transferred (transferred) in sufficient amounts to the donor surface and therefore the printing results of the substrate were not satisfactory. The present disclosure includes the following aspects: <Aspect 1> 1. A method of printing on a surface of a substrate, comprising: This method is a. providing a donor surface; b. passing the donor surface through a coating station, the donor surface exiting the coating station coated with discrete particles; and c. Repeat the following steps: (i.) treating a surface of a substrate such that the affinity of the particles for at least selected regions of the surface of the substrate is greater than the affinity of the particles for the donor surface; (ii.) contacting the surface of the substrate with the donor surface such that particles are transferred from the donor surface only to the selected treated areas of the surface of the substrate, thereby exposing areas of the donor surface from which particles have been transferred to corresponding areas on the substrate; and (iii.) thus forming a plurality of discrete particles adhered to the treated surface of the substrate; (iv.) returning the donor surface to the coating station to make the monolayer of particles continuous, thereby allowing subsequent printing of images onto the surface of a substrate; Including, At least 50% by weight of the discrete particles are metal pigments comprising a flake-shaped metal substrate and a surface treatment of the metal substrate, the surface treatment of the metal substrate comprising at least one coating layer containing a metal oxide and surrounding the metal substrate, and a surface modification of the coating layer, the surface modification comprising at least one heteropolysiloxane or a compound having at least two terminal functional groups, which are the same or different from each other and separated by a spacer, and at least one terminal functional group is capable of chemically bonding to the coating layer. method. <Aspect 2> 2. The method of embodiment 1, wherein the surface modification is attached to the top surface of the metal oxide. <Aspect 3> 3. The method of any one of the preceding claims, wherein in step b, the donor surface leaves the coating station coated with a monolayer of discrete particles. <Aspect 4> The method according to any one of aspects 1 to 3, wherein the flaky metal substrate has an average thickness (h50 value) in the range of 10 to 500 nm. <Aspect 5> 5. The method according to any one of the preceding claims, wherein the flaky metal substrate has an aspect ratio in the range of 1500:1 to 10:1, the aspect ratio being defined as the ratio between the average pigment diameter (D50 value) and the average pigment thickness (h50 value). <Aspect 6> 6. The method of any one of the preceding claims, wherein the flaky metal substrate is selected from flaky substrates or pigments of aluminum, copper, zinc, gold bronze, chromium, titanium, zirconium, tin, iron, and steel, or alloys of these metals. <Aspect 7> The method according to any one of the preceding aspects, wherein the flaky metal substrate is formed by a PVD method, and is preferably an aluminum pigment. <Aspect 8> The method of any one of the preceding aspects, wherein the first coating layer surrounding the metal substrate contains a metal oxide in an amount of at least 60% by weight, based on the weight of the first coating. <Aspect 9> 9. The method of any one of aspects 1-8, wherein the metal oxide of the first coating layer is selected from the group consisting of silicon oxide, aluminum oxide, boron oxide, zirconium oxide, cerium oxide, iron oxide, titanium oxide, chromium oxide, tin oxide, zinc oxide, molybdenum oxide, vanadium oxide, and oxide hydrates and hydroxides thereof, and mixtures thereof. <Aspect 10> The method of any one of the preceding aspects, wherein the heteropolysiloxane is prepared from multiple components including at least one aminosilane component and at least one alkylsilane component. <Aspect 11> The method of any one of aspects 1 to 9, wherein the surface modification layer comprises a compound having at least two terminal functional groups that are different from each other and separated by a spacer. <Aspect 12> The method according to any one of the preceding aspects, wherein a receiving layer and / or an adhesive layer is applied onto the substrate in step i. <Aspect 13> The method of any one of the preceding aspects, wherein the donor surface is a hydrophobic surface, preferably formed by an elastomer prepared from a poly(dimethylsiloxane) polymer. <Aspect 14> A use of particles comprising: At least 50% by weight of the particles are flaky metal pigments comprising a flaky metal substrate and a surface treatment of the metal substrate, the surface treatment of the metal substrate comprising at least one coating layer containing a metal oxide and surrounding the metal substrate, and a surface modification layer of the coating layer, the surface modification layer comprising at least one heteropolysiloxane or a compound having at least two terminal functional groups which are the same or different from each other and separated by a spacer, at least one terminal functional group being capable of chemically bonding to the coating layer; 1. A method of printing on a surface of a substrate, comprising: a. providing a donor surface; b. passing the donor surface through a coating station, the donor surface exiting the coating station coated with discrete particles; and c. Repeat the following steps: (i.) treating a surface of a substrate such that the affinity of the particles for at least selected regions of the surface of the substrate is greater than the affinity of the particles for the donor surface; (ii.) contacting the surface of the substrate with the donor surface such that particles are transferred from the donor surface only to the selected areas of the surface of the substrate that have been treated, thereby exposing areas of the donor surface from which particles have been transferred to corresponding areas on the substrate; and (iii.) thus forming a plurality of discrete particles adhered to the treated surface of the substrate; (iv.) returning the donor surface to the coating station to make the monolayer of particles continuous, thereby allowing subsequent printing of images onto the surface of a substrate; Including, use. <Aspect 15> Use of particles according to embodiment 14 in a printing method according to any one of embodiments 2 to 13.

Claims

1. 1. A method of printing on a surface of a substrate, comprising: The method comprises the following steps a, b and c: a. providing a donor surface; b. passing the donor surface through a coating station, the donor surface exiting the coating station coated with discrete particles; and c. Repeatedly carrying out the following steps (i) to (iii): (i.) treating a surface of a substrate such that the affinity of the particles for at least selected regions of the surface of the substrate is greater than the affinity of the particles for the donor surface; (ii.) contacting the surface of the substrate with the donor surface such that particles are transferred from the donor surface only to the selected treated areas of the surface of the substrate, exposing areas of the donor surface to which particles have been transferred to corresponding areas on the substrate as a result of said transfer of particles, and forming a plurality of discrete particles adhered to the treated surface of the substrate as a result of said transfer of particles; (iii) returning the donor surface to the coating station to replenish the particles, thereby enabling printing of a subsequent image onto the surface of the substrate; Including, At least 50% by weight of the discrete particles are metal pigments comprising a flake-shaped metal substrate and a surface treatment of the metal substrate, the surface treatment of the metal substrate comprising at least one coating layer containing a metal oxide and surrounding the metal substrate, and a surface modification of the coating layer, the surface modification comprising at least one heteropolysiloxane or a compound having at least two terminal functional groups, which are the same or different from each other and separated by a spacer, and at least one terminal functional group is capable of chemically bonding to the coating layer. method.

2. The method of claim 1 , wherein the surface modification is attached to a top surface of a metal oxide.

3. 3. The method of claim 1 or 2, wherein in step b, the donor surface leaves the coating station coated with a monolayer of discrete particles.

4. The method according to any one of claims 1 to 3, wherein the flaky metal substrate has an average thickness (h50 value) in the range of 10 to 500 nm.

5. 5. The method according to any one of claims 1 to 4, wherein the flaky metal substrate has an aspect ratio in the range of 1500:1 to 10:1, the aspect ratio being defined as the ratio between the average pigment diameter (D50 value) and the average pigment thickness (h50 value).

6. 6. The method according to any one of claims 1 to 5, wherein the flaked metal substrate is selected from flaked substrates or pigments of aluminium, copper, zinc, gold bronze, chromium, titanium, zirconium, tin, iron and steel or alloys of these metals.

7. The method according to any one of claims 1 to 6, wherein the flaky metal substrate is formed by a PVD method.

8. A method according to any one of claims 1 to 7, wherein the at least one coating layer includes a first coating layer surrounding the metal substrate, the first coating layer containing a metal oxide in an amount of at least 60 weight percent based on the weight of the first coating layer.

9. 9. The method according to any one of claims 1 to 8, wherein the metal oxide contained in the at least one coating layer surrounding the metal substrate is selected from the group consisting of silicon oxide, aluminum oxide, boron oxide, zirconium oxide, cerium oxide, iron oxide, titanium oxide, chromium oxide, tin oxide, zinc oxide, molybdenum oxide, vanadium oxide, and oxide hydrates and hydroxides thereof, and mixtures thereof.

10. The method of any one of claims 1 to 9, wherein the heteropolysiloxane is prepared from multiple components including at least one aminosilane component and at least one alkylsilane component.

11. The method of claim 1, wherein the surface modification of the coating layer comprises a compound having at least two terminal functional groups that are different from each other and separated by a spacer.

12. The method according to any one of the preceding claims, wherein a receiving layer and / or an adhesive layer is applied onto the substrate in step i.

13. The method of any one of claims 1 to 12, wherein the donor surface is a hydrophobic surface.

14. A use of particles comprising: At least 50% by weight of the particles are flaky metal pigments comprising a flaky metal substrate and a surface treatment of the metal substrate, the surface treatment of the metal substrate comprising at least one coating layer containing a metal oxide and surrounding the metal substrate, and a surface modification layer of the coating layer, the surface modification layer comprising at least one heteropolysiloxane or a compound having at least two terminal functional groups which are the same or different from each other and separated by a spacer, at least one terminal functional group being capable of chemically bonding to the coating layer; A method of printing on a surface of a substrate, the method comprising the steps of: a. providing a donor surface; b. passing the donor surface through a coating station, the donor surface exiting the coating station coated with discrete particles; and c. Repeatedly carrying out the following steps (i) to (iii): (i.) treating a surface of a substrate such that the affinity of the particles for at least selected regions of the surface of the substrate is greater than the affinity of the particles for the donor surface; (ii.) contacting the surface of the substrate with the donor surface such that particles are transferred from the donor surface only to the selected treated areas of the surface of the substrate, exposing areas of the donor surface to which particles have been transferred to corresponding areas on the substrate as a result of said particle transfer, and forming a plurality of discrete particles adhered to the treated surface of the substrate as a result of said particle transfer; (iii.) returning the donor surface to the coating station to replenish the particles, thereby enabling printing of a subsequent image onto the surface of the substrate; Including, use.

15. Use of particles according to claim 14 in a printing method according to any one of claims 2 to 13.

Citation Information

Patent Citations

  • Silver ink with good metal printing effect and printing process using silver ink

    CN104403407A

  • Printing method for producing UV-curable and printable foil coating on printable substrate to produce printed product utilized as e.g. packaging medium, involves drying metal particle-containing paint and / or printing ink after time delay

    DE102010017429A1

  • Method for producing surfactant-free aqueous suspensions based on nanostructured hydrophobic particles and their use

    JP2005532895A

  • pvd metal effect pigment powder

    JP2017533982A

  • Printing System and Method

    JP2018517596A