Circuit board manufacturing method

The described method for manufacturing circuit boards with semiconductor elements addresses the challenge of larger circuit sizes by using resin-filled cutouts and eliminating drilling, ensuring thermal stability and efficient production.

JP7589576B2Active Publication Date: 2024-11-26SUMITOMO BAKELITE CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021021483
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-15
Publication Date
2024-11-26
Estimated Expiration
2041-02-15

AI Technical Summary

Technical Problem

The existing methods for manufacturing power modules with semiconductor elements on metal circuit boards face challenges in managing the increase in circuit size due to thicker copper plates, which are necessary for higher current applications, leading to wider insulation widths and larger circuits.

Method used

A method involving a circuit forming step with a base circuit metal plate, resin coating, heat dissipation member bonding, mounting, and sealing steps to create a circuit board with a resin-filled cutout portion, eliminating the need for drilling and etching, thereby controlling circuit size and improving manufacturing efficiency.

Benefits of technology

This approach effectively suppresses the increase in circuit board size while maintaining thermal stability and insulation reliability, simplifying the manufacturing process and reducing material waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589576000001
    Figure 0007589576000001
  • Figure 0007589576000002
    Figure 0007589576000002
Patent Text Reader

Abstract

To provide a technique of suppressing enlargement of a circuit board where a semiconductor element is mounted.SOLUTION: A manufacturing method for a power module 100 includes: a resin covering step (S2) of filling a blank part 33 of a circuit pattern part 32 of a base circuit Cu plate 30 with first resin 6 and covering the circuit pattern part 32 with the first resin 6, thereby generating a resin covered Cu circuit 30A; a metal circuit generating step (S3) of removing a metal plate base part 31 and the first resin 6 (resin covered part 61) covering the circuit pattern part 32 of the resin covered Cu circuit 30A, thereby generating a Cu circuit 3 with the black part 33 of the circuit pattern (circuit pattern part 32) filled with the first resin 6; and a heat radiation member bonding step (S4) of press-bonding the Cu circuit 3 and a Cu heat sink 5 through a heat radiation sheet 4, thereby generating a heat radiation base substrate 30B.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a circuit board, for example, a method for manufacturing a circuit board on which a semiconductor element or the like is mounted. [Background technology]

[0002] The market for power modules in which power semiconductor elements are mounted on a metal circuit board for heat transfer is expanding. Various technologies have been proposed to realize high heat dissipation in such power modules. For example, a laminate for a finned heat sink integrated circuit board is known, which includes a finned heat sink and a substrate that contain a highly thermally conductive filler and a crystalline polymer and are integrally molded, an insulating layer that is formed on the substrate and contains an insulating thermally conductive filler and a crystalline polymer, and a metal layer that is formed on the insulating layer, in which the content of the highly thermally conductive filler in the finned heat sink and the substrate is 15 to 65 vol%, and the content of the thermally conductive filler in the insulating layer is 15 to 65 vol% (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2012-28421 A Summary of the Invention [Problem to be solved by the invention]

[0004] In the general manufacturing method for power modules, which have power semiconductor elements mounted on a metal circuit board for heat transfer, the copper plate that will become the circuit is first bonded to an insulating layer and a copper plate that will become the base, and then the copper plate is machined (generally drilled) and etched. In order to accommodate the increasing currents that have become common in recent years, there is an increasing demand for thicker copper for the circuits on insulating boards. When machining copper plates, the thicker the plate, the wider the insulation width becomes, which is an issue due to the effect of the drill shape, and this results in the circuit itself becoming larger, so a new technology was required.

[0005] The present invention has been made in view of the above circumstances, and has an object to provide a technique for preventing an increase in size of a circuit board on which a semiconductor element is mounted. [Means for solving the problem]

[0006] According to the present invention, a circuit forming process for producing a base circuit metal plate by providing a circuit pattern on one surface of a metal plate and using the other surface as a base surface on which no circuit pattern is provided; a resin coating step of filling a first resin into the cutout portion of the circuit pattern of the base circuit metal plate and covering the circuit pattern with the first resin to form a resin-coated metal circuit; a metal circuit forming step of removing the first resin covering the circuit pattern of the resin-coated metal circuit and the base surface to form a metal circuit in a state where the first resin is filled in a cut-out portion of the circuit pattern; a heat dissipation member bonding process for forming a heat dissipation base substrate by press-bonding the metal circuit and the heat dissipation member via a heat dissipation sheet; a mounting step of attaching a semiconductor element and a circuit element to the metal circuit; a sealing step of sealing the semiconductor element and the circuit element with a second resin; A method for manufacturing a circuit board is provided, comprising: Effect of the Invention

[0007] According to the present invention, it is possible to provide a technique for preventing an increase in size of a circuit board on which a semiconductor element is mounted. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a power module according to an embodiment. [Diagram 2] FIG. 2 is a flowchart showing a manufacturing process of a power module according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. The drawings are for illustrative purposes only. The shapes and dimensional ratios of the components in the drawings do not necessarily correspond to the actual products.

[0010] <Outline of Power Module 100> A power module 100 according to this embodiment will be described. FIG. 1 is a cross-sectional view that shows a schematic diagram of the power module 100 according to the embodiment of the present invention. For ease of explanation, the explanation may be given assuming that the positional relationship (upper and lower relationships, etc.) of each component of the power module 100 is as shown in each drawing. However, the positional relationship in this explanation is unrelated to the positional relationship during use or manufacture of the power module 100.

[0011] The power module 100 includes a power semiconductor chip 1, lead wires 7 that support and fix the power semiconductor chip 1 and electrically connect it to external wiring, a Cu circuit 3 provided on one surface (the lower surface in the drawing) of the power semiconductor chip 1, and a resin sealing portion 8 that seals the power semiconductor chip 1 and the lead wires 7. Furthermore, the power module 100 includes a Cu heat sink 5 provided on the lower surface of the Cu circuit 3, and a heat dissipation sheet 4 provided as a bonding layer between the Cu circuit 3 and the Cu heat sink 5. A specific description will be given below.

[0012] <Power semiconductor chip 1> The power semiconductor chip 1 is, for example, an insulated gate bipolar transistor (IGBT) and a diode. An electrode pattern (not shown) is formed on the upper surface of the power semiconductor chip 1, and a conductive pattern (not shown) is formed on the lower surface of the power semiconductor chip 1. The lower surface of the power semiconductor chip 1 is bonded to a Cu circuit 3 via a sintering layer 2, which is a bonding layer. The electrode pattern on the upper surface of the power semiconductor chip 1 is electrically connected to a lead wire 7.

[0013] <Lead wire 7> The lead wire 7 supports and fixes the power semiconductor chip 1 and makes an electrical connection with the external wiring, and is a component made of a thin plate of a metal material such as copper or iron by pressing, etching, or the like.

[0014] <Cu circuit 3> The Cu circuit 3 is a metal circuit board composed of a metal material (copper in this case) having conductivity. The power semiconductor chip 1 is provided on a circuit pattern formed on one surface (the upper surface in the drawing) of the Cu circuit 3 via the sintering layer 2. A Cu heat sink 5 is provided on the other surface (the lower surface in the drawing) of the Cu circuit 3 with a heat dissipation sheet 4 interposed therebetween.

[0015] Specifically, the Cu circuit 3 is a circuit board obtained by patterning thick copper (rolled copper). For example, thick copper (rolled copper) can be preferably used as the metal material constituting the Cu circuit 3. Thereby, the Cu circuit 3 has a relatively small resistance value. Note that at least a part of the Cu circuit 3 may be covered with a solder resist layer.

[0016] The Cu circuit 3 has a cutout portion 33 that constitutes the circuit pattern. The cutout portion 33 is filled with the first resin 6. The portion filled with the first resin 6 is referred to as a resin filling portion 62. The first resin 6 will be described later. Also, although the manufacturing method of the Cu circuit 3 will be described later with reference to FIG. 2, the Cu circuit 3 is obtained through a process of grinding or polishing the surface.

[0017] The thickness of the Cu circuit 3 is 0.5 mm or more and 2 mm or less. The lower limit is preferably 0.6 mm or more, more preferably 0.7 mm or more. The upper limit is preferably 1.7 mm or less, more preferably 1.5 mm or less. By setting the lower limit of the thickness of the Cu circuit 3 within the above range, heat generation of the Cu circuit 3 can be suppressed even in applications that require high current. Also, by setting the upper limit within the above range, circuit processability can be improved, and the thickness reduction of the entire product can be achieved.

[0018] The flatness of the upper surface (the surface on the power semiconductor chip 1 side) and the lower surface (the surface on the heat dissipation sheet 4 side) of the Cu circuit 3 is 0.01 mm or more and 0.15 mm or less. There is no particular restriction on the lower limit, and it may be within a practical range. The upper limit is preferably 0.13 mm or less, and more preferably 0.1 mm or less. The flatness is specified in JIS0621-1984, and there are two types of measurement methods, contact type (dial gauge, etc.) and non-contact type (coordinate measuring machine, etc.), either of which may be used. In addition, the flatness of the upper surface and the lower surface of the Cu circuit 3 may be different as long as it is within the above range. By setting the flatness within this range, the power semiconductor chip 1 and the lead wires 7 can be suitably bonded on the upper surface via the sintering layer 2. Also, the bonding to the heat dissipation sheet 4 on the lower surface can be satisfactorily performed.

[0019] <Components of the first resin 6 (resin filled portion 62)> The encapsulating resin composition constituting the first resin 6 is a cured product of a thermosetting composition (C) containing a thermosetting resin (A) and an inorganic filler (B). The thermosetting composition (C) contains a curing accelerator (D).

[0020] [Cure accelerator (D)] The curing accelerator (D) of the present embodiment has high activity, which allows low-temperature curing to be achieved, but if used as is without any special measures, the reaction will proceed during storage, resulting in reduced shelf life. Examples of the curing accelerator (D) include phosphorus atom-containing compounds such as organic phosphines, tetra-substituted phosphonium compounds, phosphobetaine compounds, adducts of phosphine compounds and quinone compounds, or adducts of phosphonium compounds and silane compounds; amidine compounds such as 1,8-diazabicyclo(5,4,0)undecene-7 and imidazole; and nitrogen atom-containing compounds such as tertiary amines such as benzyldimethylamine, amidinium salts, or ammonium salts. Among them, the curing accelerator (D) is preferably an imidazole-based curing accelerator or a phosphorus-based curing accelerator. As the imidazole-based curing accelerator, it is more preferable to include, for example, an imidazole compound of an amidine-based compound. Examples of the imidazole compound include, but are not limited to, 2-methylimidazole, 2-phenylimidazole, imidazole-2-carbaldehyde, 5-azabenzimidazole, and 4-azabenzimidazole. Among them, 2-methylimidazole is preferably used.

[0021] The content of the curing accelerator (D) in the encapsulating resin composition is not particularly limited, but is preferably, for example, from 0.1 mass % to 5 mass % and more preferably from 0.2 mass % to 4 mass % relative to the entire encapsulating resin composition. By setting the content of the curing accelerator (D) to the above lower limit or more, the encapsulating resin composition can be appropriately cured. On the other hand, by setting the content of the curing accelerator (D) to the above upper limit or less, the molten state can be prolonged, and the low viscosity state can be prolonged, making it easier to realize low-temperature encapsulation.

[0022] [Thermosetting resin (A)] Examples of the thermosetting resin (A) include phenolic resin, epoxy resin, unsaturated polyester resin, melamine resin, and polyurethane. These may be used alone or in combination of two or more. Among them, it is preferable to include at least one of phenolic resin and epoxy resin, and it is more preferable to include epoxy resin.

[0023] As the epoxy resin, any monomer, oligomer, or polymer having two or more epoxy groups in one molecule can be used, and the molecular weight and molecular structure thereof are not particularly limited. Specific examples of epoxy resins include crystalline epoxy resins such as biphenyl-type epoxy resins, bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, and tetramethylbisphenol F-type epoxy resins, stilbene-type epoxy resins, and hydroquinone-type epoxy resins; novolac-type epoxy resins such as cresol novolac-type epoxy resins, phenol novolac-type epoxy resins, and naphthol novolac-type epoxy resins; aralkyl-type epoxy resins such as phenylene-skeleton-containing phenol aralkyl-type epoxy resins, biphenylene-skeleton-containing phenol aralkyl-type epoxy resins, phenylene-skeleton-containing naphthol aralkyl-type epoxy resins, and alkoxynaphthalene-skeleton-containing phenol aralkyl-type epoxy resins; trifunctional epoxy resins such as triphenol methane-type epoxy resins and alkyl-modified triphenol methane-type epoxy resins; modified phenol-type epoxy resins such as dicyclopentadiene-modified phenol-type epoxy resins and terpene-modified phenol-type epoxy resins; and heterocyclic-containing epoxy resins such as triazine-nucleus-containing epoxy resins. These may be used alone or in combination of two or more. Among these, from the viewpoint of improving the balance between the reliability and moldability of the aluminum electrolytic capacitor, it is more preferable to use at least one of an aralkyl type epoxy resin and a naphthyl ether type epoxy resin.

[0024] The ICI viscosity of the thermosetting resin (A) at 150°C is suitably set depending on the content of the inorganic filler (B), and for example, the upper limit is preferably 60 poise or less, more preferably 50 poise or less, and further preferably 40 poise or less, which improves the fluidity of the encapsulating resin composition and makes it easier to realize low-temperature encapsulation. On the other hand, the lower limit of the ICI viscosity of the thermosetting resin (A) at 150° C. is not particularly limited, but may be, for example, 0.01 poise or more, where 1 poise is 0.1 Pa·s.

[0025] The content of the thermosetting resin (A) is not particularly limited, but is preferably from 1 mass % to 50 mass % inclusive, more preferably from 2 mass % to 30 mass % inclusive, and even more preferably from 5 mass % to 20 mass % inclusive, based on the entire encapsulating resin composition. By setting the content of the thermosetting resin (A) to the above lower limit or more, the flowability and moldability of the encapsulating resin composition can be more effectively improved, while by setting the content of the thermosetting resin (A) to the above upper limit or less, the reliability of the aluminum electrolytic capacitor can be more effectively improved.

[0026] [Inorganic filler (B)] Examples of the inorganic filler (B) include silica, alumina, kaolin, talc, clay, mica, rock wool, wollastonite, glass powder, glass flakes, glass beads, glass fiber, silicon carbide, silicon nitride, aluminum nitride, carbon black, graphite, titanium dioxide, calcium carbonate, calcium sulfate, barium carbonate, magnesium carbonate, magnesium sulfate, barium sulfate, cellulose, aramid, wood, etc. These may be used alone or in combination of two or more.

[0027] Examples of the silica include crystalline silica (fractured crystalline silica), fused silica (fractured amorphous silica, spherical amorphous silica), and liquid sealing silica (spherical amorphous silica for liquid sealing). Among them, fused spherical silica is preferable from the viewpoint of easily realizing low-temperature and low-pressure sealing.

[0028] The average particle size of the inorganic filler (B) is not particularly limited, but is typically 1 to 100 μm, preferably 1 to 50 μm, and more preferably 1 to 20 μm. It is believed that an appropriate average particle size can provide effects such as more uniform coating of the shell containing the molten mixture in the granulation step described below. In addition, when the finally obtained core-shell particles are used as a semiconductor encapsulant, the filling ability around the semiconductor element in the mold cavity can be improved. The volumetric particle size distribution of the inorganic filler (B) can be measured by a commercially available laser type particle size distribution analyzer (for example, SALD-7000, manufactured by Shimadzu Corporation).

[0029] The content of the inorganic filler (B) is not particularly limited, but is, for example, preferably 50% by mass or more and 95% by mass or less, more preferably 60% by mass or more and 95% by mass or less, and even more preferably 65% ​​by mass or more and 85% by mass or less, based on the entire encapsulating resin composition. By setting the content of the inorganic filler (B) to the above lower limit or more, the reliability of the aluminum electrolytic capacitor encapsulated with the encapsulating resin composition can be effectively improved. Also, by setting the content of the inorganic filler (B) to the above upper limit or less, the flowability of the encapsulating resin composition can be improved, and the moldability can be more effectively improved.

[0030] The encapsulating resin composition of the present embodiment may contain the following components in addition to those described above. [Hardening agent (C)] The encapsulating resin composition may contain a curing agent (C). The curing agent (C) is not particularly limited as long as it reacts with the thermosetting resin (A) to cure it, but examples of the curing agent include linear aliphatic diamines having 2 to 20 carbon atoms, such as ethylenediamine, trimethylenediamine, tetramethylenediamine, and hexamethylenediamine, as well as amines such as metaphenylenediamine, paraphenylenediamine, paraxylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylpropane, 4,4'-diaminodiphenylether, 4,4'-diaminodiphenylsulfone, 4,4'-diaminodicyclohexane, bis(4-aminophenyl)phenylmethane, 1,5-diaminonaphthalene, metaxylenediamine, paraxylenediamine, 1,1-bis(4-aminophenyl)cyclohexane, and dicyanodiamide; resole-type phenolic resins, such as aniline-modified resole resins and dimethyl ether resole resins; phenol novolac resins, cresol, and the like. Examples of the organic acids include novolac-type phenolic resins such as phenol novolac resins, tert-butylphenol novolac resins, and nonylphenol novolac resins; phenol aralkyl resins such as phenylene skeleton-containing phenol aralkyl resins and biphenylene skeleton-containing phenol aralkyl resins; phenolic resins having a condensed polycyclic structure such as a naphthalene skeleton or an anthracene skeleton; polyoxystyrenes such as polyparaoxystyrene; alicyclic acid anhydrides such as hexahydrophthalic anhydride (HHPA) and methyltetrahydrophthalic anhydride (MTHPA), and aromatic acid anhydrides such as trimellitic anhydride (TMA), pyromellitic anhydride (PMDA), and benzophenonetetracarboxylic acid (BTDA); polymercaptan compounds such as polysulfides, thioesters, and thioethers; isocyanate compounds such as isocyanate prepolymers and blocked isocyanates; and organic acids such as carboxylic acid-containing polyester resins. These may be used alone or in combination of two or more. Among these, from the viewpoint of realizing low-temperature and low-pressure encapsulation with the encapsulating resin composition, it is more preferable to use at least one of a novolac type phenol resin and a phenol aralkyl resin.

[0031] The content of the curing agent (C) in the encapsulating resin composition is not particularly limited, but is preferably, for example, from 1 mass % to 12 mass % and more preferably from 3 mass % to 10 mass % with respect to the entire encapsulating resin composition. By setting the content of the curing agent (C) to be equal to or more than the above lower limit, the encapsulating resin composition can be appropriately cured, whereas by setting the content of the curing agent (C) to be equal to or less than the above upper limit, appropriate fluidity can be maintained, making it easier to realize low-temperature and low-pressure encapsulation.

[0032] [Coupling agent (E)] The encapsulating resin composition may contain, for example, a coupling agent (E). As the coupling agent (E), known coupling agents such as various silane-based compounds, such as epoxysilane, mercaptosilane, aminosilane, alkylsilane, ureidosilane, and vinylsilane, titanium-based compounds, aluminum chelates, and aluminum / zirconium-based compounds may be used. More specifically, vinyltrichlorosilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltris(β-methoxyethoxy)silane, γ-methacryloxypropyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-methacryloxypropylmethyldiethoxysilane, γ-methacryloxypropyltriethoxysilane, vinyltriacetoxysilane, γ-mercaptopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-anilinopropyltrimethoxysilane, γ-anilinopropylmethyldimethoxysilane, γ-[bis(β-hydroxyethyl)]aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl) - silane coupling agents such as gamma-aminopropyltriethoxysilane, N-beta-(aminoethyl)-gamma-aminopropylmethyldimethoxysilane, N-phenyl-gamma-aminopropyltrimethoxysilane, gamma-(beta-aminoethyl)aminopropyldimethoxymethylsilane, N-(trimethoxysilylpropyl)ethylenediamine, N-(dimethoxymethylsilylisopropyl)ethylenediamine, methyltrimethoxysilane, dimethyldimethoxysilane, methyltriethoxysilane, N-beta-(N-vinylbenzylaminoethyl)-gamma-aminopropyltrimethoxysilane, gamma-chloropropyltrimethoxysilane, hexamethyldisilane, vinyltrimethoxysilane, gamma-mercaptopropylmethyldimethoxysilane, 3-isocyanatopropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, and hydrolyzate of 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine;Examples of titanate-based coupling agents include isopropyl triisostearoyl titanate, isopropyl tris(dioctyl pyrophosphate) titanate, isopropyl tri(N-aminoethyl-aminoethyl) titanate, tetraoctyl bis(ditridecyl phosphite) titanate, tetra(2,2-diallyloxymethyl-1-butyl)bis(ditridecyl)phosphite titanate, bis(dioctyl pyrophosphate)oxyacetate titanate, bis(dioctyl pyrophosphate)ethylene titanate, isopropyl trioctanoyl titanate, isopropyl dimethacryl isostearoyl titanate, isopropyl tridodecylbenzenesulfonyl titanate, isopropyl isostearoyl diacryl titanate, isopropyl tri(dioctyl phosphate) titanate, isopropyl tricumyl phenyl titanate, and tetraisopropyl bis(dioctyl phosphite) titanate. These may be used alone or in combination of two or more.

[0033] The content of the coupling agent (E) in the encapsulating resin composition is not particularly limited, but is preferably 0.05% by mass or more and 3% by mass or less, and more preferably 0.1% by mass or more and 2% by mass or less, based on the entire encapsulating resin composition. By making the content of the coupling agent (E) equal to or more than the lower limit, the dispersibility of the inorganic filler (B) in the encapsulating resin composition can be improved. In addition, by making the content of the coupling agent (E) equal to or less than the upper limit, the flowability of the encapsulating resin composition can be improved, and the moldability can be improved.

[0034] Furthermore, in addition to the above components, the encapsulating resin composition of the present embodiment may contain various additives, such as a colorant such as carbon black; a release agent such as natural wax, synthetic wax, higher fatty acid or metal salts thereof, paraffin, or polyethylene oxide; an ion scavenger such as hydrotalcite; a stress reducing agent such as silicone oil or silicone rubber; a flame retardant such as aluminum hydroxide; and an antioxidant.

[0035] As described above, the first resin 6 (resin filled portion 62) filled in the Cu circuit 3 undergoes a process of grinding or polishing the surface. At that time, it is preferable that the filler contained in the first resin 6 (resin filled portion 62) does not easily fall off. This is because it is undesirable for the resin surface to be uneven in the subsequent press bonding process. Therefore, the first resin 6 is preferably a material that has high interfacial adhesion strength between the filler and the thermosetting resin (A) and from which the filler does not easily fall off.

[0036] <Linear expansion coefficient of first resin 6> The linear expansion coefficient of the first resin 6 (resin filling portion 62) is 10 ppm / K or more and 20 ppm / K or less. The lower limit is preferably 12 ppm / K or more, and more preferably 15 ppm / K or more. The upper limit is preferably 18 ppm / K or less, and more preferably 16 ppm / K or less. By setting the linear expansion coefficient of the first resin 6 (resin filling portion 62) in such a range, it is possible to make it close to the linear expansion coefficient (approximately 17 ppm / K) of copper, which is the material of the Cu circuit 3. In other words, even when heat from the power semiconductor chip 1 acts, the interface between the first resin 6 of the resin filling portion 62 and the copper surface of the cutout portion 33 can be stabilized, and peeling or the like can be suppressed.

[0037] <Heat dissipation sheet 4> The heat dissipation sheet 4 is disposed between the Cu circuit 3 and the Cu heat sink 5. The heat of the power semiconductor chip 1 is transferred to the Cu circuit 3, and further transferred to the Cu heat sink 5, which is heat dissipation means, via the heat dissipation sheet 4, and dissipated to the outside. This allows the heat generated from the power semiconductor chip 1, which is a heat generating body (particularly the heat generated from the lower surface side of the power semiconductor chip 1), to be effectively dissipated to the outside of the power module 100 while maintaining the insulation of the power module 100. This makes it possible to improve the insulation reliability of the semiconductor device.

[0038] The planar shape of the heat dissipation sheet 4 is not particularly limited, and can be appropriately selected according to the shape of the Cu circuit 3 and the Cu heat sink 5, and can be, for example, rectangular. The film thickness of the heat dissipation sheet 4 is, for example, 50 μm or more and 250 μm or less. This allows the heat of the Cu circuit 3 to be more effectively transferred to the Cu heat sink 5 while improving the mechanical strength and heat resistance. Furthermore, the heat dissipation sheet 4 has an excellent balance between the heat dissipation property and the insulation property. The thermal conductivity of the heat dissipation sheet 4 is, for example, 5 W / mK or more and 25 W / mK or less. The lower limit is preferably 10 W / mK (175° C.) or more, and more preferably 15 W / mK (175° C.) or more. The upper limit is not particularly limited, but the above-mentioned 25 W / mK or less can be used as a general value.

[0039] [Material of heat dissipation sheet 4] The heat dissipation sheet 4 is, for example, a resin sheet, and is formed using a resin composition for sheets. The resin composition for sheets will be described below. In this embodiment, the resin composition for sheets preferably contains a thermosetting resin (A), a filler (B), and a curing agent (C), etc. When the resin composition contains a thermosetting resin, the resin sheet is a B-staged version of the thermosetting resin (A).

[0040] [Thermosetting resin (A)] Examples of the thermosetting resin (A) include epoxy resins, cyanate resins, polyimide resins, benzoxazine resins, unsaturated polyester resins, phenolic resins, melamine resins, silicone resins, bismaleimide resins, phenoxy resins, and acrylic resins. As the thermosetting resin (A), one of these may be used alone, or two or more of them may be used in combination. Among these, from the viewpoint of high insulating properties, the thermosetting resin (A) is preferably an epoxy resin, a phenol resin, or a phenoxy resin.

[0041] Examples of epoxy resins include bisphenol type epoxy resins such as bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol E type epoxy resin, bisphenol S type epoxy resin, bisphenol M type epoxy resin (4,4'-(1,3-phenylenediisopridiene) bisphenol type epoxy resin), bisphenol P type epoxy resin (4,4'-(1,4-phenylenediisopridiene) bisphenol type epoxy resin), and bisphenol Z type epoxy resin (4,4'-cyclohexydiene bisphenol type epoxy resin); phenol novolac type epoxy resin, cresol novolac type epoxy resin, trisphenol group methane type novolac type epoxy resin, tetraphenol group ethene type epoxy resin, and the like. Examples of the epoxy resins include novolac-type epoxy resins such as aryl alkylene-type epoxy resins, novolac-type epoxy resins having a condensed ring aromatic hydrocarbon structure, biphenyl-type epoxy resins, aryl alkylene-type epoxy resins such as xylylene-type epoxy resins and biphenyl aralkyl-type epoxy resins, naphthylene ether-type epoxy resins, naphthol-type epoxy resins, naphthalene diol-type epoxy resins, bifunctional to tetrafunctional epoxy-type naphthalene resins, binaphthyl-type epoxy resins, and naphthalene aralkyl-type epoxy resins, anthracene-type epoxy resins, phenoxy-type epoxy resins, dicyclopentadiene-type epoxy resins, norbornene-type epoxy resins, adamantane-type epoxy resins, and fluorene-type epoxy resins. One of these may be used alone, or two or more may be used in combination.

[0042] Among the epoxy resins, from the viewpoint of further improving heat resistance and insulation reliability, it is preferable to use one or more types selected from the group consisting of bisphenol type epoxy resins, novolac type epoxy resins, biphenyl type epoxy resins, aryl alkylene type epoxy resins, naphthalene type epoxy resins, anthracene type epoxy resins, and dicyclopentadiene type epoxy resins.

[0043] Examples of the phenol resin include novolac-type phenol resins such as phenol novolac resin, cresol novolac resin, and bisphenol A novolac resin, and resol-type phenol resins, etc. One of these may be used alone, or two or more of them may be used in combination. Among the phenolic resins, phenolic novolac resins are preferred.

[0044] The content of the thermosetting resin (A) is preferably 1% by mass or more, more preferably 5% by mass or more, based on the total amount of the sheet resin composition, while the content is preferably 30% by mass or less, more preferably 20% by mass or less, based on the total amount of the sheet resin composition. When the content of the thermosetting resin (A) is equal to or more than the above lower limit, the handleability of the sheet resin composition is improved, the resin sheet can be easily formed, and the strength of the resin sheet is improved. When the content of the thermosetting resin (A) is equal to or less than the above upper limit, the linear expansion coefficient and elastic modulus of the resin sheet are further improved, and the thermal conductivity is further improved.

[0045] [Filler (B)] The filler (B) in this embodiment is used from the viewpoints of improving the thermal conductivity of the resin sheet and obtaining strength.

[0046] The filler (B) is preferably a thermally conductive filler. More specifically, from the viewpoint of achieving a balance between thermal conductivity and electrical insulation, examples of the filler (B) include silica, alumina, boron nitride, aluminum nitride, and silicon carbide. These may be used alone or in combination of two or more. Among these, the filler (B) is preferably alumina or boron nitride.

[0047] The content of the filler (B) is preferably 90% by mass or less, more preferably 80% by mass or less, based on the total amount of the sheet resin composition, while from the viewpoint of thermal conductivity, the content is preferably 40% by mass or more, more preferably 50% by mass or more, based on the total amount of the sheet resin composition.

[0048] [Hardening agent (C)] When an epoxy resin or a phenol resin is used as the thermosetting resin (A), the sheet resin composition preferably further contains a curing agent (C).

[0049] As the curing agent (C), one or more types selected from the curing catalyst (C-1) and the phenol-based curing agent (C-2) can be used. Examples of the curing catalyst (C-1) include organic metal salts such as zinc naphthenate, cobalt naphthenate, tin octylate, cobalt octylate, bisacetylacetonate cobalt (II), and trisacetylacetonate cobalt (III); tertiary amines such as triethylamine, tributylamine, and 1,4-diazabicyclo[2.2.2]octane; imidazoles such as 2-phenyl-4-methylimidazole, 2-ethyl-4-methylimidazole, 2,4-diethylimidazole, 2-phenyl-4-methyl-5-hydroxyimidazole, and 2-phenyl-4,5-dihydroxymethylimidazole; triphenylphosphine, tri-p-tolylphosphine, tetraphenylphosphonium tetraphenylborate, triphenylphosphine triphenylborane, and 1,2-bis-(diphenylphosphine)-2-phenylphosphine; Examples of the curing catalyst (C-1) include organic phosphorus compounds such as phenol, bisphenol A, nonylphenol, and other phenolic compounds; organic acids such as acetic acid, benzoic acid, salicylic acid, p-toluenesulfonic acid, and other organic acids, or mixtures thereof. As the curing catalyst (C-1), one of these, including its derivatives, can be used alone, or two or more of these, including its derivatives, can be used in combination. The content of the curing catalyst (C-1) is not particularly limited, but is preferably from 0.001% by mass to 1% by mass based on the total amount of the resin composition for a sheet.

[0050] Examples of the phenol-based curing agent (C-2) include novolac-type phenolic resins such as phenol novolac resin, cresol novolac resin, trisphenolmethane-type novolac resin, naphthol novolac resin, and aminotriazine novolac resin; modified phenolic resins such as terpene-modified phenolic resin and dicyclopentadiene-modified phenolic resin; aralkyl-type resins such as phenol aralkyl resins having a phenylene skeleton and / or biphenylene skeleton and naphthol aralkyl resins having a phenylene skeleton and / or biphenylene skeleton; bisphenol compounds such as bisphenol A and bisphenol F; and resol-type phenolic resins, and these may be used alone or in combination of two or more. Among these, from the viewpoints of increasing the glass transition temperature and decreasing the linear expansion coefficient, the phenol-based curing agent (C-2) is preferably a novolac-type phenol resin or a resol-type phenol resin.

[0051] The content of the phenol-based curing agent (C-2) is not particularly limited, but is preferably 1% by mass or more, more preferably 5% by mass or more, based on the total amount of the sheet resin composition. On the other hand, the content is preferably 30% by mass or less, more preferably 15% by mass or less, based on the total amount of the sheet resin composition.

[0052] [Coupling agent (D)] The sheet resin composition may contain a coupling agent (D). The coupling agent (D) can improve the wettability at the interface between the thermosetting resin (A) and the filler (B).

[0053] The coupling agent (D) is not particularly limited, but it is preferable to use, for example, one or more coupling agents selected from an epoxy silane coupling agent, a cationic silane coupling agent, an amino silane coupling agent, a titanate-based coupling agent, and a silicone oil-type coupling agent. The content of the coupling agent (D) is not particularly limited, but is preferably 0.05% by mass or more, more preferably 0.1% by mass or more, based on 100% by mass of the filler (B), while the content is preferably 3% by mass or less, more preferably 2% by mass or less, based on 100% by mass of the filler (B).

[0054] [Phenoxy resin (E)] Furthermore, the resin composition for the sheet may contain a phenoxy resin (E). By containing the phenoxy resin (E), the bending resistance of the resin sheet (i.e., the heat dissipation sheet 4) can be improved. Furthermore, by including the phenoxy resin (E), it is possible to reduce the elastic modulus of the resin sheet, and the stress relaxation force of the resin sheet can be improved.

[0055] In addition, when the phenoxy resin (E) is contained, the viscosity increases, and the flowability decreases, and the occurrence of voids and the like can be suppressed. In addition, when the resin sheet is used in close contact with a metal member, the adhesion between the metal and the cured product of the sheet resin composition can be improved. These synergistic effects can further increase the insulation reliability of the semiconductor device.

[0056] Examples of the phenoxy resin (E) include phenoxy resins having a bisphenol skeleton, phenoxy resins having a naphthalene skeleton, phenoxy resins having an anthracene skeleton, and phenoxy resins having a biphenyl skeleton, etc. Phenoxy resins having a structure having a plurality of these skeletons can also be used.

[0057] The content of the phenoxy resin (E) is preferably, for example, 3% by mass or more and 10% by mass or less with respect to the total amount of the sheet resin composition.

[0058] [Other ingredients] The sheet resin composition may further contain an antioxidant, a leveling agent, etc., within the range not impairing the effects of the present invention.

[0059] <Cuヒートシンク5> The Cu heat sink 5 is a type of heat dissipation member also called a Cu base plate, and has a copper plate-shaped heat sink base 51 and a heat sink fin portion 52 (heat dissipation fins) extending integrally in a plurality of fin shapes from the lower surface of the heat sink base 51. Note that a plurality of pin-shaped heat dissipation pins may be provided instead of the heat dissipation fins. In addition to the Cu heat sink 5, for example, an aluminum heat sink may be used as the heat dissipation member. Also, as long as it has a function of acquiring heat generated by the power semiconductor chip 1 via the Cu circuit 3 and dissipating it elsewhere, it is not limited to a general heat dissipation member, and may be a part of another configuration (for example, a housing). Even in this case, the heat dissipation sheet 4 can be used.

[0060] <Sintering layer 2> The sintering layer 2 is a bonding layer formed by sintering a sintering paste containing metal particles. As the sintering paste, any one of Ag sintering paste containing silver particles, AL sintering paste containing aluminum particles, and Cu sintering paste containing copper particles can be used.

[0061] The above-mentioned sintering paste is provided between the power semiconductor chip 1 and the Cu circuit 3, and then laminated, and the power semiconductor chip 1 and the Cu circuit 3 are bonded by the sintering layer 2 through a sintering process. In addition, the Cu circuit 3 and the lead wire 7 are bonded by the sintering layer 2. In the sintering layer 2, a sintering network (metallic bond bus) is formed by metal particles, and high thermal conductivity and low electrical resistance are realized. From the viewpoint of improving the bonding property by the sintering layer 2, the Cu circuit 3 and the lead wire 7 may be subjected to a surface treatment of plating with a metal contained in the sintering paste. Specifically, in this embodiment, the surfaces of the Cu circuit 3 and the lead wire 7 may be subjected to Ag plating or Cu plating.

[0062] <Resin sealing part 8> The second resin used in the resin sealing portion 8 is, for example, a mold resin, and integrally seals components such as the power semiconductor chip 1, the lead wires 7, and the Cu circuit 3 that stacks them inside. In addition to the mold resin, silicone gel or the like may be used as a sealing material used in the resin sealing portion 8. The following describes the structure of integral sealing with the mold resin. In this sealing, a part of the lead wires 7 is sealed, and the other part that is not sealed is connected to an external device.

[0063] <Components of the second resin (resin sealing portion 8)> The molding resin (second resin) of the resin sealing portion 8 can be made of the same material as that exemplified as the first resin 6 filled in the resin filling portion 62 described above. In this case, the same material may be used, or different materials may be used. As for the first resin 6, as described above, it may be necessary to prevent the filler from falling off during the polishing process, etc., and a material corresponding to this may be preferable.

[0064] The linear expansion coefficient of the second resin is 10 ppm / K or more and 20 ppm / K or less, similar to that of the first resin 6. The lower limit is preferably 12 ppm / K or more, and more preferably 15 ppm / K or more. The upper limit is preferably 18 ppm / K or less, and more preferably 16 ppm / K or less.

[0065] <Manufacturing Method of Power Module 100> A method for manufacturing the power module 100 having the above configuration will be described with reference to the flowchart of FIG.

[0066] [Circuit formation process (S1)] In the circuit formation process (S1), a cut-out portion 33 is provided on one side of a copper plate (the upper side in the figure) to form a circuit pattern portion 32, and the other side (the lower side in the figure) is a metal plate base portion 31 on which no circuit pattern is provided, thereby producing a base circuit Cu plate 30. The circuit pattern portion 32 is formed, for example, by applying a resist to a copper plate of a predetermined thickness corresponding to the metal plate base portion 31 to form a circuit pattern, and then plating the circuit pattern portion 32. Thereafter, the resist is removed to form the base circuit Cu plate 30. The thickness of the circuit pattern portion 32 is set taking into consideration the final thickness of the Cu circuit 3 and an allowance for removal required for polishing or the like in the subsequent metal circuit forming step (S3).

[0067] [Resin coating process (S2)] In the resin coating process (S2), a first resin 6 is filled into the cut-out portion 33 of the circuit pattern portion 32 of the base circuit Cu plate 30 to form a resin filled portion 62, and a resin coating portion 61 is provided that covers the circuit pattern portion 32 with the first resin 6, thereby generating a resin-coated Cu circuit 30A.

[0068] [Metal circuit generation process (S3)] In the metal circuit generating step (S3), the first resin 6 (resin coated portion 61) covering the circuit pattern portion 32 of the resin-coated Cu circuit 30A and the metal plate base portion 31 are removed to generate a Cu circuit 3 in a state where the first resin 6 is filled in the cut-out portion 33 of the circuit pattern portion 32 (i.e., the Cu circuit 3 has a resin filled portion 62). Grinding or polishing can be used as a method for removing the resin coated portion 61 and the metal plate base portion 31, and either one or both of these methods may be used. In addition, with the resin coated portion 61 and the metal plate base portion 31 removed, the flatness of the surface of the Cu circuit 3 is 0.01 mm or more and 0.15 mm or less. In addition, the thickness of the Cu circuit 3 is 0.5 mm or more and 2 mm or less.

[0069] [Heat dissipation member joining process (S4)] In the heat dissipation member bonding step (S4), the Cu circuit 3 and the Cu heat sink 50 are press-bonded together via the heat dissipation sheet 4 to produce the heat dissipating base substrate 30B.

[0070] [Mounting process (S5)] In the mounting process (S5), the power semiconductor chip 1 and other circuit elements (e.g., lead wires 7) are attached to the Cu circuit 3 of the heat dissipating base substrate 30B. Specifically, the above-mentioned sintering paste is provided between the power semiconductor chip 1 and the Cu circuit 3 and laminated, and the power semiconductor chip 1 and the Cu circuit 3, and further the Cu circuit 3 and the lead wires 7 are bonded by the sintering layer 2 through a sintering process.

[0071] [Sealing process (S6)] In the sealing step (S6), a resin sealing portion 8 is provided on the upper surface of the heat dissipating base substrate 30B on which the power semiconductor chip 1 and the lead wires 7 are mounted, using a sintering layer 2. That is, the power semiconductor chip 1 and the lead wires 7 are covered and sealed with a second resin, thereby completing the power module 100.

[0072] As described above, the embodiment has the following effects. That is, the power module 100 is manufactured by a manufacturing method in which the Cu circuit 3 is created in advance and attached to the Cu heat sink 5. In addition, the cut-out portion 33 of the circuit pattern portion 32 of the Cu circuit 3 is a resin-filled portion 62 filled with the first resin 6. When forming the circuit pattern portion 32, mechanical processing with a drill is not used as in the conventional method, so that the manufacturing time can be shortened, and there is no concern that the insulation width becomes narrower due to the constraints of the drill shape when the copper thickness becomes thick, resulting in an increase in the size of the circuit. In addition, when the Cu heat sink 5 is provided with a heat sink fin portion 52 (or a heat dissipation pin), in the past, it was not possible to run the Cu heat sink 5 through a manufacturing line such as etching, and the manufacturing process tended to become complicated, but in this embodiment, etching processing is not necessary, so there is no such concern. In addition, the burden of disposal of the etching solution can be eliminated.

[0073] The features of this embodiment are summarized as follows. (1) The method for manufacturing the power module 100 of the present embodiment includes the following steps: A circuit formation process (S1) for producing a base circuit Cu plate 30 in which a circuit pattern portion 32 is provided on one side of a copper plate and a metal plate base portion 31 on the other side on which no circuit pattern is provided is provided; a resin coating step (S2) of filling a first resin 6 into a cutout portion 33 of a circuit pattern portion 32 of a base circuit Cu plate 30 and covering the circuit pattern portion 32 with the first resin 6 to form a resin-coated Cu circuit 30A; a metal circuit forming step (S3) of removing the first resin 6 (resin coating portion 61) covering the circuit pattern portion 32 of the resin-coated Cu circuit 30A and the metal plate base portion 31 to form a Cu circuit 3 in a state in which the first resin 6 is filled in the cutout portion 33 of the circuit pattern (circuit pattern portion 32); a heat dissipation member bonding step (S4) of press-bonding the Cu circuit 3 and the Cu heat sink 5 via the heat dissipation sheet 4 to generate a heat dissipation base substrate 30B; a mounting process (S5) for mounting the power semiconductor chip 1 and circuit elements (such as lead wires 7) on the Cu circuit 3; a sealing step (S6) of sealing the power semiconductor chip 1 and the circuit elements with a resin sealing portion 8; has. The power module 100 is manufactured by a manufacturing method in which the Cu circuit 3 is created in advance and then attached to the Cu heat sink 5, and therefore the manufacturing process can be simplified. (2) In the metal circuit forming process (S3), the resin coating 61 and the metal plate base 31 covering one surface of the heat dissipating base substrate 30B are removed by grinding. This makes it possible to shorten the manufacturing process and achieve a highly accurate flatness. (3) In the metal circuit forming step (S3), the flatness of one of the ground surfaces is 0.01 mm or more and 0.15 mm or less. (4) The linear expansion coefficient of the first resin 6 and the second resin (resin sealing portion 8) is 10 ppm / K or more and 20 ppm / K or less. By setting the linear expansion coefficient in this range, thermal stability can be achieved at the interface between the resin and the metal (Cu circuit 3) in contact with the resin. (5) The first resin 6 and the second resin may be made of different materials. (6) The first resin 6 and the second resin may be made of the same material. (7) The thickness of the Cu circuit 3 formed in the metal circuit forming step (S3) is 0.5 mm or more and 2 mm or less. (8) The thermal conductivity of the heat dissipation sheet 4 is 5 W / mK or more and 25 W / mK or less. (9) The Cu heat sink 5 includes a heat sink fin portion 52 or a heat dissipation pin. Since etching is not required, the manufacturing process can be simplified even for the power module 100 having the heat sink fin portion 52 or a heat dissipation pin.

[0074] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. [Explanation of symbols]

[0075] 1. Power semiconductor chip 2 Sintering layer 3 Cu circuit 4. Heat dissipation sheet 5 Cu Heatsink 6. First Resin 7 Lead Wire 8 Resin sealing part 30 Base circuit Cu board 30A Resin-coated Cu circuit 30B Heat dissipation base board 31 Metal plate base 32 Circuit pattern section 33 Punching part 51 Heat sink base 52 Heat sink fin section 61 Resin-coated part 62 Resin filling section 100 Power Module

Claims

1. a circuit forming process for producing a base circuit metal plate by providing a circuit pattern on one surface of a metal plate and using the other surface as a base surface on which no circuit pattern is provided; a resin coating step of filling a first resin into the cutout portion of the circuit pattern of the base circuit metal plate and covering the circuit pattern with the first resin to form a resin-coated metal circuit; a metal circuit forming step of removing the first resin covering the circuit pattern of the resin-coated metal circuit and the base surface to form a metal circuit in a state where the first resin is filled in a cut-out portion of the circuit pattern; a heat dissipation member bonding process for forming a heat dissipation base substrate by press-bonding the metal circuit and the heat dissipation member via a heat dissipation sheet; a mounting step of attaching a semiconductor element and a circuit element to the metal circuit; a sealing step of sealing the semiconductor element and the circuit element with a second resin; The method for manufacturing a circuit board comprising the steps of:

2. The method for manufacturing a circuit board according to claim 1 , wherein the metal circuit forming step removes the first resin covering the one surface and the base surface by grinding.

3. 3. The method for manufacturing a circuit board according to claim 2, wherein in the metal circuit forming step, the flatness of the ground one surface is 0.01 mm or more and 0.15 mm or less.

4. 4. The method for manufacturing a circuit board according to claim 1, wherein the first resin and the second resin have a linear expansion coefficient of 10 ppm / K or more and 20 ppm / K or less.

5. The method for manufacturing a circuit board according to claim 1 , wherein the first resin and the second resin are made of different materials.

6. The method for manufacturing a circuit board according to claim 1 , wherein the first resin and the second resin are made of the same material.

7. The method for manufacturing a circuit board according to claim 1 , wherein the thickness of the metal circuit formed in the metal circuit forming step is 0.5 mm or more and 2 mm or less.

8. The method for manufacturing a circuit board according to claim 1 , wherein the thermal conductivity of the heat dissipation sheet is 5 W / mK or more and 25 W / mK or less.

9. The method for manufacturing a circuit board according to claim 1 , wherein the heat dissipation member comprises a heat dissipation fin or a heat dissipation pin.

Citation Information

Patent Citations

  • Laminate sheet for circuit board integrating heat sink with fin, circuit board integrating heat sink with fin and method of manufacturing laminate sheet for circuit board integrating heat sink with fin

    JP2012028421A

  • Power module and manufacturing method therefor

    JP2015165545A

  • Power semiconductor device and method of manufacturing the same, and insulation substrate part

    JP2016096263A

  • Electric power semiconductor device and method for producing same

    WO2013099545A1