Pressure-sensitive adhesive sheet, its manufacturing method, and laminate manufacturing method

The adhesive sheet with an acrylic adhesive polymer and thermal initiator improves followability and solvent resistance by forming crosslinks post-bonding, addressing the challenges of adhering to irregular surfaces and maintaining adhesion at high temperatures.

JP7589604B2Active Publication Date: 2024-11-26TOAGOSEI CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021043786
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-17
Publication Date
2024-11-26
Estimated Expiration
2041-03-17

AI Technical Summary

Technical Problem

Adhesive sheets with crosslinked adhesive layers struggle to follow the uneven shape of adherends with large surface irregularities and fail to maintain adhesion in harsh environments, particularly at high temperatures, while also lacking sufficient solvent resistance.

Method used

The adhesive sheet incorporates an acrylic adhesive polymer with a low gel fraction and a thermal polymerization initiator, allowing crosslinking to occur after bonding to the adherend, forming a crosslinked structure that enhances followability and adhesion, even on irregular surfaces, and provides solvent resistance.

Benefits of technology

The adhesive sheet achieves excellent followability to irregularities, high temperature adhesiveness, and solvent resistance by minimizing crosslinking agents and using a specific component to form crosslinks post-bonding, resulting in improved adhesive performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589604000001
    Figure 0007589604000001
  • Figure 0007589604000002
    Figure 0007589604000002
  • Figure 0007589604000003
    Figure 0007589604000003
Patent Text Reader

Abstract

To provide an adhesive sheet having excellent unevenness followability, solvent resistance and high-temperature adhesion.SOLUTION: An adhesive sheet has an adhesive layer. The adhesive layer has an acrylic adhesive polymer (A) and a thermal-polymerization initiator. The acrylic adhesive polymer (A) has a (meth)acrylic acid alkoxyalkyl ester-derived constitutional unit. The gel fraction based on the acrylic adhesive polymer (A) of the adhesive layer is less than 20%. After heat treatment, the gel fraction based on the acrylic adhesive polymer (A) of the adhesive layer is 20% or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pressure-sensitive adhesive sheet, a method for producing the same, and a method for producing a laminate. [Background technology]

[0002] It is known that crosslinking of pressure-sensitive adhesives improves their cohesive strength at room temperature and at high temperatures, and improves their solvent resistance and oil resistance. Generally, crosslinking of pressure-sensitive adhesives is performed by incorporating a crosslinking agent such as an isocyanate-based curing agent into the pressure-sensitive adhesive layer and crosslinking the adhesive by heat, or by polymerizing a polyfunctional monomer by ultraviolet light (see, for example, Patent Document 1 and Patent Document 2).

[0003] Patent Document 1 discloses the production of an adhesive sheet using an acrylic resin composition containing a polymer having 40 to 99 mass% of structural units derived from (meth)acrylic acid alkoxyalkyl ester relative to all monomer units and a crosslinking agent. Patent Document 2 discloses the formation of an adhesive layer using a composition containing a thermally crosslinkable adhesive having a weight average molecular weight of less than 300,000 and a thermal crosslinking agent. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2018 / 235217 [Patent Document 2] JP 2017-197604 A Summary of the Invention [Problem to be solved by the invention]

[0005] When a pressure-sensitive adhesive sheet is attached to a fiber fabric or a decorative sheet is attached to an article, the adherend may have large surface irregularities. However, as in Patent Documents 1 and 2, pressure-sensitive adhesive sheets having a crosslinked pressure-sensitive adhesive layer cannot conform to the uneven shape of an adherend having a large surface irregularity, and are prone to peeling under harsh environments such as high temperatures, and there is concern that they may have poor adhesion (particularly, unevenness-conforming ability and high-temperature adhesion). In addition, one of the properties required for the pressure-sensitive adhesive layer is high solvent resistance.

[0006] The present invention has been made in view of the above circumstances, and a main object of the present invention is to provide a pressure-sensitive adhesive sheet that is excellent in unevenness-following ability, solvent resistance, and high-temperature adhesion. [Means for solving the problem]

[0007] The present inventors have conducted extensive research to solve the above problems, and have focused on reducing the amount of crosslinking agent as much as possible or forming crosslinks without using a crosslinking agent. Based on this focus, they have found that the pressure-sensitive adhesive sheet can have good conformability to uneven surfaces, solvent resistance, and high-temperature adhesion by incorporating a specific component into the pressure-sensitive adhesive layer, and have completed the present invention. Specifically, the present invention provides the following means.

[0008] [1] A pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer, the pressure-sensitive adhesive layer comprising an acrylic adhesive polymer (A) and a thermal polymerization initiator, the acrylic adhesive polymer (A) having a structural unit derived from an alkoxyalkyl ester of (meth)acrylic acid, the pressure-sensitive adhesive layer having a gel fraction based on the acrylic adhesive polymer (A) of less than 20%, and the pressure-sensitive adhesive layer having a gel fraction based on the acrylic adhesive polymer (A) after heat treatment of 20% or more.

[0009] [2] The pressure-sensitive adhesive sheet according to [1] above, wherein the content of structural units derived from an alkoxyalkyl (meth)acrylate in the acrylic pressure-sensitive adhesive polymer (A) is 20 mass% or more based on all structural units derived from monomers constituting the acrylic pressure-sensitive adhesive polymer (A). [3] The pressure-sensitive adhesive sheet according to the above [1] or [2], wherein the glass transition temperature of the acrylic pressure-sensitive adhesive polymer (A) is -80°C to 10°C.

[0010] [4] A method for producing a pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer, comprising: irradiating with active energy rays a layer made of a pressure-sensitive adhesive composition containing an acrylic adhesive polymer syrup, a photopolymerization initiator, and a thermal polymerization initiator, to form the pressure-sensitive adhesive layer containing an acrylic adhesive polymer (A) and a thermal polymerization initiator, wherein the acrylic adhesive polymer syrup contains a (meth)acrylic acid alkoxyalkyl ester, the pressure-sensitive adhesive layer has a gel fraction based on the acrylic adhesive polymer (A) of less than 20 mass%, and the pressure-sensitive adhesive layer after heat treatment has a gel fraction based on the acrylic adhesive polymer (A) of 20% or more. [5] A method for producing a laminate, comprising the steps of laminating the pressure-sensitive adhesive sheet according to any one of [1] to [3] above to an adherend, and then carrying out a heat treatment to cure the pressure-sensitive adhesive layer. Effect of the Invention

[0011] According to the present invention, a pressure-sensitive adhesive sheet having excellent conformability to irregularities, solvent resistance, and high-temperature adhesion can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will be described in detail below. In this specification, "(meth)acrylic" means acrylic and / or methacrylic. "(meth)acrylate" means acrylate and / or methacrylate.

[0013] <Adhesive sheet> The pressure-sensitive adhesive sheet of the present invention (hereinafter also referred to as "the pressure-sensitive adhesive sheet") is a sheet having a pressure-sensitive adhesive layer containing an acrylic pressure-sensitive adhesive polymer (A) and a thermal polymerization initiator. The pressure-sensitive adhesive sheet is a thermally reactive pressure-sensitive adhesive sheet that is used by laminating the pressure-sensitive adhesive layer and an adherend together, and then applying heat to the laminate to cure the pressure-sensitive adhesive layer.

[0014] Here, in the present adhesive sheet, a crosslinking reaction proceeds by performing a heat treatment after laminating the adhesive layer and the adherend. This forms a crosslinked structure, resulting in excellent adhesive performance and solvent resistance. The mechanism is presumed to be as follows. When the adhesive layer and the adherend are laminated and then heated, radicals are generated by the thermal polymerization initiator in the adhesive layer, and hydrogen is extracted from the side chain portion of the acrylic acid alkoxyalkyl ester constituting the acrylic adhesive polymer (A), and a peroxy radical is generated by bonding with oxygen (see the scheme below). After that, a hydrogen abstraction reaction occurs again, and the generated radicals are coupled with each other to form a crosslinked structure. Therefore, according to the present adhesive sheet, even if the adhesive layer does not contain a crosslinking agent or a compound having a reactive unsaturated bond (specifically, a monomer or a polyfunctional (meth)acrylic compound), a crosslinked structure can be formed by laminating the adhesive layer and the adherend and performing a heat treatment. Furthermore, when the adhesive layer of this pressure-sensitive adhesive sheet is attached to an adherend, the crosslinked structure has not yet been formed, so the adhesive layer is flexible and can be attached to an adherend with large surface irregularities by following the irregularities of the surface. This is presumably why an adhesive sheet with good irregularity-following properties can be obtained.

[0015] [ka]

[0016] Next, the acrylic adhesive polymer (A) and the thermal polymerization initiator contained in the adhesive layer of the present adhesive sheet will be described.

[0017] <Acrylic adhesive polymer (A)> The acrylic adhesive polymer (A) is a polymer mainly composed of structural units derived from (meth)acrylic monomers, and has adhesive properties. In this specification, the acrylic adhesive polymer (A) is "mainly composed of" (meth)acrylic monomers, and the ratio of structural units derived from (meth)acrylic monomers to all structural units derived from monomers constituting the acrylic adhesive polymer (A) (hereinafter also referred to as "total monomer units") is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, and even more preferably 80% by mass or more.

[0018] The acrylic adhesive polymer (A) has a structural unit derived from an alkoxyalkyl ester of (meth)acrylic acid. The alkoxyalkyl ester of (meth)acrylic acid constituting the acrylic adhesive polymer (A) preferably has an alkoxyalkyl group having 2 to 12 carbon atoms. Specific examples thereof include methoxymethyl (meth)acrylate, ethoxymethyl (meth)acrylate, methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, n-propoxyethyl (meth)acrylate, n-butoxyethyl (meth)acrylate, methoxypropyl (meth)acrylate, ethoxypropyl (meth)acrylate, n-propoxypropyl (meth)acrylate, n-butoxypropyl (meth)acrylate, methoxybutyl (meth)acrylate, ethoxybutyl (meth)acrylate, n-propoxybutyl (meth)acrylate, and n-butoxybutyl (meth)acrylate.

[0019] From the viewpoint of versatility, the (meth)acrylic acid alkoxyalkyl ester constituting the acrylic adhesive polymer (A) is preferably a (meth)acrylic acid alkoxyalkyl ester having an alkoxyalkyl group having 2 to 8 carbon atoms, and more preferably at least one selected from the group consisting of methoxymethyl (meth)acrylate, methoxyethyl (meth)acrylate, and ethoxyethyl (meth)acrylate. The (meth)acrylic acid alkoxyalkyl ester constituting the acrylic adhesive polymer (A) may be one type or two or more types.

[0020] In the acrylic adhesive polymer (A), the ratio of the structural unit derived from the (meth)acrylic acid alkoxyalkyl ester is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, and even more preferably 40% by mass or more, based on the total monomer units of the acrylic adhesive polymer (A), from the viewpoint of forming a crosslinked structure by utilizing the reaction caused by the coexistence of the (meth)acrylic acid alkoxyalkyl ester and oxygen radicals, and improving the adhesiveness, solvent resistance, and step followability of the adhesive sheet. In the acrylic adhesive polymer (A), the upper limit of the ratio of the structural unit derived from the (meth)acrylic acid alkoxyalkyl ester is not particularly limited, but from the viewpoint of improving the adhesive performance, it is preferably 99% by mass or less, more preferably 95% by mass or less, based on the total monomer units of the acrylic adhesive polymer (A).

[0021] The monomer constituting the acrylic adhesive polymer (A) may be only a (meth)acrylic acid alkoxyalkyl ester, but may also contain a monomer different from the (meth)acrylic acid alkoxyalkyl ester (hereinafter also referred to as "other monomer").

[0022] From the viewpoint of achieving excellent adhesive performance, it is preferable that the acrylic adhesive polymer (A) has, as another monomer, a structural unit derived from at least one selected from the group consisting of (meth)acrylic acid alkyl esters and (meth)acrylic acid hydroxyalkyl esters.

[0023] Specific examples of alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, and dodecyl (meth)acrylate.

[0024] From the viewpoint of increasing the elastic modulus and improving the heat resistance of the acrylic adhesive polymer (A), among these, (meth)acrylic acid alkyl esters in which the alkyl moiety has 1 to 8 carbon atoms are preferred, and (meth)acrylic acid alkyl esters in which the alkyl moiety has 1 to 4 carbon atoms are more preferred.

[0025] Specific examples of hydroxyalkyl (meth)acrylates include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate.

[0026] In the acrylic adhesive polymer (A), the ratio of the structural unit derived from the (meth)acrylic acid alkyl ester is preferably 3% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more, based on the total monomer units of the acrylic adhesive polymer (A) from the viewpoint of improving adhesive performance. In the acrylic adhesive polymer (A), the upper limit of the ratio of the structural unit derived from the (meth)acrylic acid alkyl ester is not particularly limited, but from the viewpoint of sufficiently performing crosslinking formation by the (meth)acrylic acid alkoxyalkyl ester, it is preferably 90% by mass or less, more preferably 80% by mass or less, based on the total monomer units of the acrylic adhesive polymer (A).

[0027] In the acrylic adhesive polymer (A), the ratio of the structural unit derived from the (meth)acrylic acid hydroxyalkyl ester is preferably 0.5% by mass or more, more preferably 1% by mass or more, and even more preferably 2% by mass or more, based on the total monomer units of the acrylic adhesive polymer (A), from the viewpoint of improving the cohesive strength of the adhesive layer and enhancing adhesive performance. The upper limit of the ratio of the structural unit derived from the (meth)acrylic acid hydroxyalkyl ester in the acrylic adhesive polymer (A) is preferably 10% by mass or less, more preferably 7% by mass or less, based on the total monomer units of the acrylic adhesive polymer (A), from the viewpoint of sufficiently performing crosslinking formation by the (meth)acrylic acid alkoxyalkyl ester.

[0028] In addition to the above, the acrylic adhesive polymer (A) may also use a monomer that is copolymerizable with the above monomer, as long as the adhesive performance is not impaired. Examples of such other monomers include alicyclic ester compounds of (meth)acrylic acid, aromatic ester compounds of (meth)acrylic acid, polyalkylene glycol mono(meth)acrylate compounds, aromatic vinyl compounds, imide group-containing vinyl compounds, amino group-containing unsaturated compounds, amide group-containing unsaturated compounds, and nitrile group-containing unsaturated compounds.

[0029] Specific examples of these include alicyclic ester compounds of (meth)acrylic acid, such as cyclohexyl (meth)acrylate, methylcyclohexyl (meth)acrylate, tert-butylcyclohexyl (meth)acrylate, cyclododecyl (meth)acrylate, isobornyl (meth)acrylate, 1-adamantyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentanyl (meth)acrylate.

[0030] Examples of the aromatic ester compound of (meth)acrylic acid include phenyl (meth)acrylate, benzyl (meth)acrylate, phenoxymethyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, and 3-phenoxypropyl (meth)acrylate.

[0031] Examples of the polyalkylene glycol mono(meth)acrylate compound include polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, polyethylene glycol-polypropylene glycol mono(meth)acrylate, polyethylene glycol-polytetraethylene glycol mono(meth)acrylate, methoxypolyethylene glycol mono(meth)acrylate, lauroxypolyethylene glycol mono(meth)acrylate, stearoxypolyethylene glycol mono(meth)acrylate, octoxypolyethylene glycol-polypropylene glycol mono(meth)acrylate, phenoxypolyethylene glycol mono(meth)acrylate, phenoxypolyethylene glycol-polypropylene glycol mono(meth)acrylate, nonylphenoxypolyethylene glycol mono(meth)acrylate, nonylphenoxypolypropylene glycol mono(meth)acrylate, and nonylphenoxypolyethylene glycol-polypropylene glycol mono(meth)acrylate.

[0032] Examples of aromatic vinyl compounds include styrene-based compounds such as styrene, α-methylstyrene, β-methylstyrene, vinylxylene, o-methylstyrene, m-methylstyrene, p-methylstyrene, o-ethylstyrene, m-ethylstyrene, p-ethylstyrene, pn-butylstyrene, p-isobutylstyrene, pt-butylstyrene, o-methoxystyrene, m-methoxystyrene, p-methoxystyrene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, p-hydroxystyrene, m-hydroxystyrene, o-hydroxystyrene, p-isopropenylphenol, m-isopropenylphenol, o-isopropenylphenol, o-vinylbenzoic acid, m-vinylbenzoic acid, p-vinylbenzoic acid, and divinylbenzene; vinylnaphthalene, and the like.

[0033] Examples of the imide group-containing vinyl compound include maleimide compounds such as maleimide and N-substituted maleimide compounds; itaconimide compounds such as N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-cyclohexylitaconimide, and N-laurylitaconimide; N-methylcitraconimide, N-ethylcitraconimide, N-butylcitraconimide, N-octylcitraconimide, N-2-ethylhexylcitraconimide, and N-cyclohexylitaconimide; Examples of the imide group-containing vinyl compound include citraconimide compounds such as cyclohexylcitraconimide and N-laurylcitraconimide; and (meth)acrylimide compounds such as N-(2-(meth)acryloyloxyethyl)succinimide, N-(2-(meth)acryloyloxyethyl)maleimide, N-(2-(meth)acryloyloxyethyl)phthalimide, N-(4-(meth)acryloyloxybutyl)succinimide, N-(4-(meth)acryloyloxybutyl)maleimide, and N-(4-(meth)acryloyloxybutyl)phthalimide. Of these, maleimide compounds are preferably used as the imide group-containing vinyl compound.

[0034] Examples of the amino group-containing unsaturated compound include dimethylaminomethyl (meth)acrylate, diethylaminomethyl (meth)acrylate, 2-dimethylaminoethyl (meth)acrylate, 2-diethylaminoethyl (meth)acrylate, 2-(di-n-propylamino)ethyl (meth)acrylate, 2-dimethylaminopropyl (meth)acrylate, 2-diethylaminopropyl (meth)acrylate, 2-(di-n-propylamino)propyl (meth)acrylate, 3-dimethylaminopropyl (meth)acrylate, 3-diethylaminopropyl (meth)acrylate, and 3-(di-n-propylamino)propyl (meth)acrylate.

[0035] Examples of the amide group-containing unsaturated compound include (meth)acrylamide, (meth)acrylamide derivatives, and N-vinylamide monomers. Specific examples of the (meth)acrylamide derivatives include tert-butyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N,N-dimethylaminopropyl(meth)acrylamide, and (meth)acryloylmorpholine. Specific examples of the N-vinylamide monomers include N-vinylacetamide, N-vinylformamide, and N-vinylisobutylamide.

[0036] Examples of the nitrile group-containing unsaturated compound include cyanomethyl (meth)acrylate, 1-cyanoethyl (meth)acrylate, 2-cyanoethyl (meth)acrylate, 1-cyanopropyl (meth)acrylate, 2-cyanopropyl (meth)acrylate, 3-cyanopropyl (meth)acrylate, 4-cyanobutyl (meth)acrylate, 6-cyanohexyl (meth)acrylate, 2-ethyl-6-cyanohexyl (meth)acrylate, 8-cyanooctyl (meth)acrylate, (meth)acrylonitrile, α-ethylacrylonitrile, α-isopropylacrylonitrile, α-chloroacrylonitrile, and α-fluoroacrylonitrile.

[0037] The proportion of the other monomer constituting the acrylic adhesive polymer (A) can be appropriately selected within a range that does not impair the effects of the present invention. As the other monomer, one type may be used alone, or two or more types may be used in combination.

[0038] (Method for producing acrylic adhesive polymer (A)) The acrylic adhesive polymer (A) is not particularly limited in the manufacturing method, and can be obtained by a known manufacturing method. For example, the acrylic adhesive polymer (A) can be obtained by polymerizing the above-mentioned monomers by adopting a known radical polymerization method such as solution polymerization, suspension polymerization, emulsion polymerization, or bulk polymerization.

[0039] In the case of the solution polymerization method, the production method may be such that an organic solvent and monomers are charged into a reactor, a polymerization initiator is added, and the mixture is heated to 50 to 300° C. to polymerize.

[0040] The method of feeding each raw material including the monomer may be a batch-type initial lump-sum feeding in which all raw materials are fed at once, a semi-continuous feeding in which at least a portion of the raw materials are continuously fed into the reactor, or a continuous polymerization method in which all raw materials are continuously fed and at the same time the produced resin is continuously withdrawn from the reactor.

[0041] Examples of organic solvents used in the solution polymerization method include cyclic ethers such as tetrahydrofuran and dioxane, aromatic hydrocarbon compounds such as benzene, toluene and xylene, esters such as ethyl acetate and butyl acetate, ketones such as acetone, methyl ethyl ketone and cyclohexanone, and alcohols such as methyl orthoformate, methyl orthoacetate, methanol, ethanol and isopropanol. As the organic solvent, one or more of these can be used. The amount of the organic solvent used is, for example, 1 to 50 mass% of the total amount of the monomers used in the polymerization relative to the total amount of the organic solvent and the monomers.

[0042] The polymerization initiator may be a known radical polymerization initiator such as an azo compound, an organic peroxide, or an inorganic peroxide, and is not particularly limited. Among these, an azo compound is preferred because it is easy to handle and does not easily cause side reactions during radical polymerization. An azo compound is preferred. In addition, a redox type polymerization initiator consisting of a known oxidizing agent and a known reducing agent may be used as the polymerization initiator. Furthermore, a known chain transfer agent may be used in combination with the polymerization initiator.

[0043] Specific examples of the polymerization initiator include azo compounds such as 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 4,4'-azobis(4-cyanovaleric acid), 2-(tert-butylazo)-2-cyanopropane, 2,2'-azobis(2,4,4-trimethylpentane), 2,2'-azobis(2-methylpropane), and dimethyl 2,2'-azobis(2-methylpropionate).

[0044] Examples of organic peroxides include cyclohexanone peroxide, 3,3,5-trimethylcyclohexanone peroxide, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, diisopropylbenzene peroxide, and 2,5-dimethyl-2,5-di(benzoylperoxy)hexane.

[0045] Examples of inorganic peroxides include potassium persulfate and sodium persulfate. Examples of redox type polymerization initiators include those using sodium sulfite, sodium thiosulfate, sodium formaldehyde sulfoxylate, ascorbic acid, ferrous sulfate, etc. as a reducing agent and potassium peroxodisulfate, hydrogen peroxide, tert-butyl hydroperoxide, etc. as an oxidizing agent. In producing the acrylic adhesive polymer (A), the amount of the polymerization initiator used is, for example, 0.01 to 20 parts by mass relative to 100 parts by mass of the total monomers used in the polymerization.

[0046] The glass transition temperature (Tg) of the acrylic adhesive polymer (A) is preferably in the range of -80°C or more and 10°C or less. If the Tg of the acrylic adhesive polymer (A) is -80°C or more, it is preferable in that the cohesive force of the adhesive layer can be sufficiently increased and sufficient adhesiveness can be ensured. From this viewpoint, the Tg of the acrylic adhesive polymer (A) is more preferably -60°C or more, even more preferably -50°C or more, and even more preferably -45°C or more.

[0047] On the other hand, if the Tg of the acrylic adhesive polymer (A) is 10°C or less, it is preferable because the adhesiveness under low temperature conditions can be sufficiently ensured, the adhesive sheet has good conformability to the adherend, and an adhesive sheet with high durability under high temperature or high temperature and high humidity can be obtained. The upper limit of the Tg of the acrylic adhesive polymer (A) is more preferably 5°C or less, even more preferably 0°C or less, even more preferably -5°C or less, and particularly preferably -10°C or less. The range of the Tg of the acrylic adhesive polymer (A) is more preferably -60°C or more and 5°C or less, even more preferably -50°C or more and 0°C or less.

[0048] In this specification, the Tg of a polymer is a value determined from the intersection point between the baseline of a heat flux curve obtained using a differential scanning calorimeter (DSC) and the tangent point at the inflection point. Details of the measurement conditions are as described in the examples below. The Tg of a polymer can be arbitrarily selected by changing the type and composition of the constituent monomers.

[0049] (Molecular weight characteristics of acrylic adhesive polymer (A)) The Mw of the acrylic adhesive polymer (A) is preferably 100,000 or more from the viewpoint of exerting sufficient cohesive force and good adhesiveness. When the Mw of the acrylic adhesive polymer (A) is 100,000 or more, sufficient adhesiveness and solvent resistance can be ensured. The Mw of the acrylic adhesive polymer (A) is more preferably 120,000 or more, even more preferably 150,000 or more, and even more preferably 200,000 or more.

[0050] The upper limit of Mw of the acrylic adhesive polymer (A) is not particularly limited, but from the viewpoint of ensuring good coating and handling properties when forming an adhesive sheet and further ensuring ease of production, it is preferably 3,000,000 or less, more preferably 2,000,000 or less, and even more preferably 1,500,000 or less. The range of Mw of the acrylic adhesive polymer (A) is preferably 100,000 or more and 3,000,000 or less, more preferably 150,000 or more and 2,000,000 or less, and even more preferably 200,000 or more and 1,500,000 or less. In this specification, the molecular weight of the polymer is a polystyrene-equivalent value measured by gel permeation chromatography (GPC).

[0051] The molecular weight distribution (Mw / Mn) of the acrylic adhesive polymer (A), which is expressed by the ratio of Mw to Mn, is preferably 10.0 or less, more preferably 9.0 or less, from the viewpoint of easily obtaining good adhesion and suppressing the increase in viscosity of the adhesive composition. The lower limit of Mw / Mn of the acrylic adhesive polymer (A) is not particularly limited, and can be 1.0 or more.

[0052] <Thermal polymerization initiator> The adhesive layer of the present pressure-sensitive adhesive sheet contains a thermal polymerization initiator. The thermal polymerization initiator is a compound that generates radicals when heat is applied. As the thermal polymerization initiator, a known thermal-start radical polymerization initiator can be used. Among them, organic peroxides and azo compounds are preferable as the thermal polymerization initiator contained in the adhesive layer of the present pressure-sensitive adhesive sheet.

[0053] Specific examples of organic peroxides include 1,1-bis(t-butylperoxy)2-methylcyclohexane, 1,1-bis(t-hexylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(t-hexylperoxy)cyclohexane, 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(t-butylperoxy)cyclohexane, 2,2-bis(4,4-di-butylperoxycyclohexyl)propane, 1,1 -Bis(t-butylperoxy)cyclododecane, t-hexylperoxyisopropyl monocarbonate, t-butylperoxymaleic acid, t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxylaurate, 2,5-dimethyl-2,5-di(m-toluoylperoxy)hexane, t-butylperoxyisopropyl monocarbonate, t-butylperoxy-2-ethylhexyl monocarbonate, t-hexylperoxybenzoate peroxide, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, t-butyl peroxyacetate, 2,2-bis(t-butylperoxy)butane, t-butyl peroxybenzoate, n-butyl-4,4-bis(t-butylperoxy)valerate, di-t-butylperoxyisophthalate, α,α'-bis(t-butylperoxy)diisopropylbenzene, dicumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, Examples of the hydroperoxide include t-butylcumyl peroxide, di-t-butyl peroxide, p-menthane hydroperoxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, diisopropylbenzene hydroperoxide, t-butyltrimethylsilyl peroxide, 1,1,3,3-tetramethylbutyl hydroperoxide, cumene hydroperoxide, t-hexyl hydroperoxide, and t-butyl hydroperoxide.

[0054] Specific examples of azo compounds include 1,1'-azobis(cyclohexane-1-carbonitrile), 2-(carbamoylazo)isobutyronitrile, 2-phenylazo-4-methoxy-2,4-dimethylvaleronitrile, azodi-t-octane, azodi-t-butane, etc. As the thermal polymerization initiator, one type may be used alone, or two or more types may be used in combination. When an organic peroxide is used, it is also possible to use it in combination with a reducing agent to cause a redox reaction.

[0055] The content of the thermal polymerization initiator in the adhesive layer is preferably 0.05 parts by mass or more relative to 100 parts by mass of the acrylic adhesive polymer (A). When the content of the thermal polymerization initiator is 0.05 parts by mass or more, it is preferable that a crosslinked structure can be formed using an acrylic acid alkoxyalkyl ester by the radicals generated in the adhesive layer by the heat treatment. From this viewpoint, the amount of the thermal polymerization initiator contained in the adhesive layer is more preferably 0.08 parts by mass or more, and even more preferably 0.1 parts by mass or more, relative to 100 parts by mass of the acrylic adhesive polymer (A). In addition, from the viewpoint of suppressing the deterioration of adhesive properties due to the excessive formation of a crosslinked structure after the heat treatment, the amount of the thermal polymerization initiator contained in the adhesive layer is preferably 15 parts by mass or less, more preferably 10 parts by mass or less, and even more preferably 5 parts by mass or less, relative to 100 parts by mass of the acrylic adhesive polymer (A). The content of the thermal polymerization initiator referred to here is the amount of the thermal polymerization initiator in the adhesive layer before the adhesive sheet is subjected to a heat treatment and cured.

[0056] <Manufacturing of adhesive sheets> The pressure-sensitive adhesive sheet can be produced by applying the pressure-sensitive adhesive composition to a substrate such as a separator to form a pressure-sensitive adhesive layer. There are no particular limitations on the form of the pressure-sensitive adhesive composition, but an active energy ray-curable pressure-sensitive adhesive composition containing an acrylic pressure-sensitive adhesive polymer syrup (hereinafter also referred to as "polymer syrup (Ac)"), a photopolymerization initiator, and a thermal polymerization initiator can be preferably used.

[0057] Polymer syrup (Ac) The active energy ray curable adhesive composition is a so-called syrup type adhesive composition that is cured by active energy rays such as ultraviolet rays and electron beams. The polymer syrup (Ac) contained in the active energy ray curable adhesive composition (hereinafter also simply referred to as "the adhesive composition") is a component that can obtain the acrylic adhesive polymer (A) that constitutes the adhesive layer by irradiation with active energy rays. The polymer syrup (Ac) contains a polymer component that constitutes a part of the acrylic adhesive polymer (A) contained in the adhesive layer, and a (meth)acrylic monomer component that constitutes the remainder. Specific embodiments of the polymer syrup (Ac) include, for example, the following embodiments (1) to (3).

[0058] (1) A mixture of a polymer component and a (meth)acrylic monomer component obtained by partially polymerizing all of the monomers constituting the acrylic adhesive polymer (A). (2) A mixture of a polymer component and a monomer component obtained by adding a (meth)acrylic monomer component of the same or different type as the monomer constituting the acrylic adhesive polymer (A) to the mixture (1) above. (3) A mixture of a polymer component and a (meth)acrylic monomer component, which is obtained by first obtaining a polymer component by a known polymerization method, and then mixing this polymer component with a desired (meth)acrylic monomer component.

[0059] The mixture of the polymer component and the (meth)acrylic monomer component exemplified in the above (1) to (3) can generally take the form of a solution in which the polymer component is dissolved in the (meth)acrylic monomer component. That is, the mixture of the polymer component and the (meth)acrylic monomer component is liquid before irradiation with active energy rays, while polymerization proceeds upon irradiation with active energy rays to produce the acrylic adhesive polymer (A).

[0060] The polymer component in the polymer syrup (Ac) (i.e., the monomer constituting the acrylic adhesive polymer (A)) and the (meth)acrylic monomer component (i.e., the (meth)acrylate compound) may be the same type, or at least a part of them may be different types. From the viewpoint of increasing the compatibility between the acrylic adhesive polymer (A) and the (meth)acrylate compound and increasing the transparency of the adhesive layer, it is preferable that the (meth)acrylate compound in the polymer syrup (Ac) is at least a part of the same as the monomer constituting the acrylic adhesive polymer (A), more preferably the same type as the monomer constituting the acrylic adhesive polymer (A), and even more preferably the same composition as the monomer constituting the acrylic adhesive polymer (A). That is, the (meth)acrylate compound contained in the present adhesive composition is preferably the same type as the monomer constituting the acrylic adhesive polymer (A), and more preferably the same composition.

[0061] In the polymer syrup (Ac), the ratio of the (meth)acrylic monomer component to the polymer component is not particularly limited as long as the viscosity required for forming a coating film and handling can be obtained. The ratio of the (meth)acrylic monomer component is, for example, 10 parts by mass or more, preferably 20 parts by mass or more, and more preferably 30 parts by mass or more, relative to 100 parts by mass of the total of the polymer component and the (meth)acrylic monomer component. The upper limit of the ratio is, for example, 99 parts by mass or less, preferably 97 parts by mass or less, and more preferably 95 parts by mass or less, relative to 100 parts by mass of the total of the polymer component and the (meth)acrylic monomer component.

[0062] The weight average molecular weight (Mw) of the polymer component in the polymer syrup (Ac) is preferably 100,000 or more, more preferably 120,000 or more, even more preferably 150,000 or more, and even more preferably 200,000 or more, from the viewpoint of exhibiting good adhesiveness and sufficient cohesive strength. The upper limit of Mw of the polymer component in the polymer syrup (Ac) is preferably 3,000,000 or less, more preferably 2,000,000 or less, and even more preferably 1,500,000 or less, from the viewpoint of ease of production. The range of Mw is preferably 100,000 or more and 3,000,000 or less, more preferably 150,000 or more and 2,000,000 or less, and even more preferably 200,000 or more and 1,500,000 or less.

[0063] The molecular weight distribution (Mw / Mn) of the polymer component in the polymer syrup (Ac), which is expressed by the ratio of Mw to Mn, is preferably 10.0 or less, more preferably 9.5 or less, and even more preferably 9.0 or less, in that good adhesiveness is easily obtained. The lower limit of Mw / Mn of the polymer syrup (Ac) is not particularly limited, and can be 1.0 or more.

[0064] Photopolymerization initiator The photopolymerization initiator contained in the pressure-sensitive adhesive composition may be a known photoinitiator such as a photoinitiator. Specific examples of the photopolymerization initiator include benzoin and its alkyl ethers, acetophenones, anthraquinones, thioxanthones, ketals, benzophenones and xanthones, acylphosphine oxides, α-diketones, and α-hydroxyketones. In addition, in order to improve the sensitivity to the active energy rays irradiated to obtain the acrylic pressure-sensitive adhesive polymer (A) by polymerizing the polymer syrup (Ac), a benzoic acid-based or amine-based photosensitizer may be used in combination as necessary.

[0065] The content of the photopolymerization initiator in the pressure-sensitive adhesive composition can be, for example, 0.01 parts by mass or more and 10 parts by mass or less with respect to 100 parts by mass of the polymer syrup (Ac). From the viewpoint of sufficiently proceeding with the polymerization reaction by irradiation with active energy rays, the content of the photopolymerization initiator is preferably 0.03 parts by mass or more, more preferably 0.05 parts by mass or more with respect to 100 parts by mass of the polymer syrup (Ac). In addition, the upper limit is preferably 3 parts by mass or less, more preferably 1 part by mass or less, and even more preferably 0.5 parts by mass or less, in order to prevent the gel fraction of the pressure-sensitive adhesive layer from becoming too high. The content of the photopolymerization initiator is preferably 0.03 parts by mass or more and 5 parts by mass or less, more preferably 0.05 parts by mass or more and 1 part by mass or less with respect to 100 parts by mass of the polymer syrup (Ac).

[0066] Thermal polymerization initiator The content of the thermal polymerization initiator in the present adhesive composition is preferably 0.05 parts by mass or more relative to 100 parts by mass of the acrylic adhesive polymer (A). When the content of the thermal polymerization initiator is 0.05 parts by mass or more, it is preferable that a sufficient amount of radicals can be generated in the adhesive layer, and the crosslinking structure using the acrylic acid alkoxyalkyl ester can be sufficiently formed. From this viewpoint, the content of the thermal polymerization initiator in the present adhesive composition is more preferably 0.08 parts by mass or more, and even more preferably 0.1 parts by mass or more, relative to 100 parts by mass of the acrylic adhesive polymer (A). In addition, from the viewpoint of suppressing the deterioration of adhesive performance due to excessive crosslinking density, the content of the thermal polymerization initiator in the present adhesive composition is preferably 15 parts by mass or less, more preferably 10 parts by mass or less, and even more preferably 5 parts by mass or less, relative to 100 parts by mass of the acrylic adhesive polymer (A).

[0067] Other Ingredients The pressure-sensitive adhesive composition may further contain components other than the polymer syrup (Ac), the photopolymerization initiator, and the thermal polymerization initiator (hereinafter, also referred to as "other components"), as long as the effects of the present invention are not impaired. Examples of other components include crosslinkers, tackifiers, plasticizers, antioxidants, UV absorbers, anti-aging agents, flame retardants, antifungal agents, silane coupling agents, fillers, colorants, etc. The content of each of these components can be appropriately set depending on the various compounds, as long as the effects of the present invention are not impaired.

[0068] The pressure-sensitive adhesive composition may contain a solvent such as an organic solvent as another component, but is preferably used as a solvent-free type that does not contain any solvent. A solvent-free curable pressure-sensitive adhesive composition is preferable because it allows the pressure-sensitive adhesive layer to be easily thickened.

[0069] When a crosslinking agent is blended into the pressure-sensitive adhesive composition, examples of the crosslinking agent (curing agent) include an epoxy compound having two or more epoxy groups, an isocyanate compound having two or more isocyanate groups, an aziridine compound having two or more aziridinyl groups, an oxazoline compound having an oxazoline group, a metal chelate compound, a butylated melamine compound, a polyfunctional (meth)acrylic compound, etc. However, from the viewpoint of improving the step-following ability of the pressure-sensitive adhesive sheet, it is preferable that the pressure-sensitive adhesive composition does not contain a crosslinking agent, or even if a crosslinking agent is blended, the amount is a very small amount.

[0070] Specifically, the content of the crosslinking agent in the present pressure-sensitive adhesive composition is preferably 0 to 0.5 parts by mass, and more preferably 0 to 0.3 parts by mass, per 100 parts by mass of the acrylic pressure-sensitive adhesive polymer (A), from the viewpoint of improving the step-following ability of the present pressure-sensitive adhesive sheet.

[0071] <Formation of adhesive layer> When a pressure-sensitive adhesive layer is produced using the present pressure-sensitive adhesive composition, the method is not particularly limited. For example, the pressure-sensitive adhesive layer can be produced by applying the present pressure-sensitive adhesive composition to a separator or the like, and then irradiating the pressure-sensitive adhesive composition with active energy rays to cure the pressure-sensitive adhesive composition.

[0072] The separator may be a resin film made of various resin materials, such as polyester resins such as polyethylene terephthalate, polyethersulfone resins, acetate resins, polycarbonate resins, and polyolefin resins.

[0073] The coating method can be appropriately set depending on the purpose, and examples thereof include various coating methods such as a bar coater, an applicator, a doctor blade, a dip coater, a roll coater, a spin coater, a flow coater, a knife coater, a comma coater, a reverse coater, a die coater, a lip coater, a gravure coater, a microgravure coater, and an ink jet. The coating amount of the present pressure-sensitive adhesive composition can be appropriately selected depending on the application, etc., so that the thickness of the pressure-sensitive adhesive layer after irradiation with active energy rays is within a desired range.

[0074] Examples of the active energy rays irradiated to the pressure-sensitive adhesive composition include ultraviolet rays, visible light, and electron beams. Of these, ultraviolet rays or electron beams are preferred. The active energy rays may be irradiated to only one side of the substrate coated with the pressure-sensitive adhesive composition, or may be irradiated to both sides. The irradiation energy can be appropriately set depending on the type of active energy rays and the formulation of the composition.

[0075] For example, when ultraviolet rays are used as the active energy rays, the wavelength is, for example, 250 to 400 nm. Examples of ultraviolet ray irradiation devices include high-pressure mercury lamps, metal halide lamps, ultraviolet electrodeless lamps, and ultraviolet light-emitting diodes (UV-LEDs). The integrated light amount is 500 mJ / cm. 2 More than 1,000 mJ / cm is preferable. 2 More preferably, 1,500 mJ / cm 2The upper limit of the accumulated light amount is preferably 100,000 mJ / cm from the viewpoint of minimizing the influence on each component in the pressure-sensitive adhesive composition and from the viewpoint of reducing energy. 2 Less than 50,000 mJ / cm is preferable. 2 The following is more preferred:

[0076] The illuminance and irradiation time of the ultraviolet light can be appropriately set so that the integrated light amount is the desired amount. For example, the illuminance is 0.5 mW / cm 2 More than 1.0mW / cm is preferable. 2 More preferably, 2.0 mW / cm 2 More preferably, the upper limit of the illuminance is 100 mW / cm 2 Less than 80mW / cm is preferable. 2 Less than 50 mW / cm is more preferable. 2 The following is even more preferred:

[0077] When an electron beam is used as the active energy beam, the electron beam irradiation device is not particularly limited, but examples thereof include Cockcroft-Walton type, Van de Graaff type, and resonant transformer type devices. The absorbed dose of the electron beam is preferably 1 to 200 kGy, more preferably 10 to 100 kGy. The acceleration voltage of the electron beam may be appropriately set within a range of 80 to 300 kV depending on the film thickness of the substrate. The oxygen concentration of the electron beam irradiation atmosphere is preferably 500 ppm or less, more preferably 300 ppm or less.

[0078] One embodiment of the present pressure-sensitive adhesive sheet thus obtained is a so-called substrate-less embodiment in which the pressure-sensitive adhesive layer is sandwiched between two separators having different peel strengths. The present pressure-sensitive adhesive sheet may also have a structure in which a substrate is disposed on one side of the pressure-sensitive adhesive layer and a separator is disposed on the other side. There is no particular restriction on the shape of the pressure-sensitive adhesive sheet, and it can be appropriately set according to the mode of use. The pressure-sensitive adhesive sheet may be, for example, in the form of a sheet, in the form of a roll, or cut into strips. It may also have any shape according to the bonding location.

[0079] <Gel fraction (before curing)> The pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet has a gel fraction based on the acrylic adhesive polymer (A) of less than 20%. By making the gel fraction of the pressure-sensitive adhesive layer less than 20%, a pressure-sensitive adhesive sheet exhibiting good step conformability can be obtained. The gel fraction referred to here is the gel fraction before the pressure-sensitive adhesive layer is cured (i.e., before the pressure-sensitive adhesive sheet is subjected to a heat treatment). From the viewpoint of making the pressure-sensitive adhesive sheet excellent in step conformability, the gel fraction of the pressure-sensitive adhesive layer is preferably 15% or less, more preferably 10% or less, even more preferably 7% or less, even more preferably 5% or less, and even more preferably 2% or less. In this specification, the gel fraction of the pressure-sensitive adhesive layer is the ratio of the mass W2 of the pressure-sensitive adhesive layer remaining after immersion in a solvent to the initial mass W1 of the pressure-sensitive adhesive layer. Details are as described in the measurement method of the examples described later.

[0080] <Method of manufacturing laminate> The pressure-sensitive adhesive sheet is attached to an adherend and then heat-treated to harden the pressure-sensitive adhesive layer, thereby improving the adhesion to the adherend. For example, to bond a first adherend and a second adherend with the pressure-sensitive adhesive sheet, the first adherend and the second adherend are first arranged to sandwich the pressure-sensitive adhesive layer, forming a laminate consisting of the first adherend / pressure-sensitive adhesive layer / second adherend. Heat is then applied to this laminate to harden the pressure-sensitive adhesive layer (hardening step). This makes it possible to obtain a laminate in which the first adherend and the second adherend are bonded with high adhesive strength via the adhesive layer.

[0081] In the heat treatment after laminating the pressure-sensitive adhesive sheet and the adherend, the heating temperature is preferably 80° C. or higher, more preferably 100° C. or higher, even more preferably 120° C. or higher, and even more preferably 130° C. or higher, from the viewpoint of sufficiently improving the cohesive strength and solvent resistance by forming a crosslinked structure. The upper limit of the heating temperature is preferably 250° C. or lower, more preferably 200° C. or lower, and even more preferably 180° C. or lower, from the viewpoint of suppressing the influence of heat. The heating time is preferably 0.1 to 60 minutes, and more preferably 0.1 to 30 minutes.

[0082] <Gel fraction (after curing)> The adhesive layer of the present adhesive sheet is cured by applying heat, thereby improving the cohesive strength, and improving the solvent resistance and oil resistance. After the adhesive layer is cured by applying heat, the gel fraction of the adhesive layer based on the acrylic adhesive polymer (A) is 20% or more. If the gel fraction of the adhesive layer based on the acrylic adhesive polymer (A) after heat treatment is less than 20%, the adhesive performance is insufficient and the solvent resistance tends to be poor. From the viewpoint of improving the cohesive strength and improving the adhesive performance as well as improving the solvent resistance, the gel fraction of the adhesive layer after curing is more preferably 30% or more, even more preferably 50% or more, even more preferably 60% or more, and even more preferably 65% ​​or more. The gel fraction based on the acrylic adhesive polymer (A) of the adhesive layer after heat treatment here is the gel fraction when the adhesive layer is heated under heating conditions that decompose the thermal polymerization initiator, and the specific heating conditions can be, for example, the heat treatment conditions described in the examples below. The gel fraction of the pressure-sensitive adhesive layer after curing can be adjusted by, for example, the content of structural units derived from an alkoxyalkyl (meth)acrylate in the acrylic pressure-sensitive adhesive polymer (A).

[0083] The thus obtained pressure-sensitive adhesive sheet can be used as a pressure-sensitive adhesive in a wide range of applications, such as clothing (including clothing accessories), sports goods (such as sportswear, sports shoes, sports gloves, bat and racket grips, etc.), medical supplies (such as supports and corsets), automobile interior and exterior products, outdoor products, handicrafts, toys, daily necessities, household goods, furniture, and the like.

[0084] For example, when the pressure-sensitive adhesive sheet is used as an adhesive for bonding fiber fabrics together, the fiber fabric to which it is applied is not particularly limited, and examples thereof include synthetic fibers such as polyester, polyamide, and acrylic fibers; regenerated fibers such as rayon and cupra; semi-synthetic fibers such as acetate; and natural fibers such as cotton, hemp, and wool. In addition, the textile products manufactured using the pressure-sensitive adhesive sheet are also not particularly limited, and the sheet can be used as an adhesive for manufacturing a wide range of clothing items such as everyday Western and Japanese clothing, ethnic clothing, underwear (e.g., seamless lingerie products and innerwear products), jackets, tops, bottoms, outdoor goods, work clothes, uniforms, formal wear, swimsuits, sportswear, socks, hats, shoes, etc., as well as for handicrafts.

[0085] In addition, when the pressure-sensitive adhesive sheet is used as an adhesive for attaching a decorative film to a molded body, the molded body to which the decorative film is attached is not particularly limited, and may be any product to which the decorative film can be attached, such as a resin product, a metal product, a ceramic product, a glass product, etc. Specific examples of the adhesive include various home appliances such as household appliances, kitchen appliances, health appliances, seasonal appliances, etc.; interior and exterior components of housing facilities such as toilets, bathrooms, doors, and walls; automobile interior and exterior parts such as bumpers, dashboards, doors, roofs, and bonnets; various miscellaneous goods such as household goods and daily miscellaneous goods; electronic parts; nursing care and medical supplies; interior and exterior parts of ships and aircraft, etc. EXAMPLES

[0086] The present invention will be specifically described below with reference to examples. However, the present invention is not limited to these examples. In the following, "parts" and "%" mean "parts by mass" and "% by mass", respectively, unless otherwise specified. The analysis methods for the polymers used in the examples and comparative examples are as follows.

[0087] <Molecular weight measurement> Using a gel permeation chromatograph (model name "HLC-8320", manufactured by Tosoh Corporation), the number average molecular weight (Mn) and weight average molecular weight (Mw) were obtained in terms of polystyrene under the following conditions. The molecular weight distribution (Mw / Mn) was calculated from the obtained values. Measurement conditions Column: Tosoh TSKgel SuperMultiporeHZ-M x 4 Column temperature: 40℃ Eluent: Tetrahydrofuran Detector: RI Flow rate: 600μL / min

[0088] <Measurement of glass transition temperature (Tg)> The glass transition temperature (Tg) of the polymer was determined from the intersection of the baseline of the heat flux curve obtained using a differential scanning calorimeter and the tangent at the inflection point. The heat flux curve was obtained by cooling about 10 mg of the sample to -50°C, holding it for 5 minutes, and then heating it to 300°C at 10°C / min, followed by cooling it to -50°C, holding it for 5 minutes, and then heating it to 350°C at 10°C / min. Measuring equipment: SII NanoTechnology DSC6220 Measurement atmosphere: Nitrogen atmosphere

[0089] <Calculation of monomer composition of polymer> The monomer composition of the resulting polymer was calculated from the charged amounts and the consumed amounts of monomers measured by gas chromatography (GC).

[0090] 1. Synthesis of acrylic adhesive polymer (A) [Synthesis Example 1] Polymer A-1 used in Examples 1 to 6 In a 3-liter four-neck flask, 2-methoxyethyl acrylate (hereinafter also referred to as "MEA") (421 parts by mass), 2-hydroxyethyl acrylate (hereinafter also referred to as "HEA") (21 parts by mass), n-butyl acrylate (hereinafter also referred to as "BA") (78 parts by mass), and ethyl acetate (770 parts by mass) were charged. The mixture was thoroughly degassed by bubbling nitrogen gas, the internal temperature of the mixture was raised to 75°C, and 2,2'-azobis(2,4-dimethylvaleronitrile) (manufactured by Wako Pure Chemical Industries, Ltd., hereinafter also referred to as "V-65") (0.35 parts by mass) was charged to initiate polymerization. After 5 hours, ethyl acetate was added so that the solid content became 30% by mass, and an ethyl acetate solution of polymer A-1 was obtained. The obtained polymer A-1 was composed of 80 mass % of MEA, 15 mass % of BA, and 5 mass % of HEA, and had Mn of 92,000, Mw / Mn of 8.7, and Tg of -35°C.

[0091] [Synthesis Example 2] Polymer A-2 used in Examples 2 to 7 and Comparative Examples 1 and 3 In a 3-liter four-neck flask, MEA (336 parts by mass), HEA (30 parts by mass), BA (144 parts by mass), methyl acrylate (hereinafter also referred to as "MA") (90 parts by mass), and ethyl acetate (890 parts by mass) were charged. This mixture was thoroughly degassed by bubbling nitrogen gas, the internal temperature of the mixture was raised to 75°C, V-65 (0.12 parts by mass) was charged, and polymerization was carried out for 5 hours. Ethyl acetate was added so that the solid content concentration was 30%, and an ethyl acetate solution of polymer A-2 was obtained. The obtained polymer A-2 consisted of MEA 52% by mass, MA 21% by mass, BA 22% by mass, and HEA 5% by mass, and had Mn 155,000, Mw / Mn 6.1, and Tg = -27°C.

[0092] [Synthesis Example 3] Polymer A-3 used in Example 8 MEA (104 parts by mass), HEA (21 parts by mass), BA (309 parts by mass), and ethyl acetate (770 parts by mass) were charged into a 3-liter four-neck flask. The mixture was thoroughly degassed by bubbling nitrogen gas, the internal temperature of the mixture was raised to 75°C, and V-65 (0.35 parts by mass) was charged to initiate polymerization. After 5 hours, ethyl acetate was added so that the solid content was 30% by mass, and an ethyl acetate solution of polymer A-3 was obtained. The obtained polymer A-3 consisted of 20% by mass of MEA, 75% by mass of BA, and 5% by mass of HEA, and had Mn of 92,000, Mw / Mn of 8.1, and Tg of -40°C.

[0093] [Synthesis Example 4] Polymer A-4 used in Example 9 In a 3-liter four-neck flask, 2-ethoxyethyl acrylate (hereinafter also referred to as "EEA") (420 parts by mass), HEA (21 parts by mass), BA (78 parts by mass), and ethyl acetate (770 parts by mass) were charged. This mixture was thoroughly degassed by bubbling nitrogen gas, the internal temperature of the mixture was raised to 75°C, and V-65 (0.35 parts by mass) was charged to start polymerization. After 5 hours, ethyl acetate was added so that the solid content was 30% by mass, and an ethyl acetate solution of polymer A-4 was obtained. The obtained polymer A-4 consisted of 80% by mass of EEA, 15% by mass of BA, and 5% by mass of HEA, and had Mn of 89,000, Mw / Mn of 8.7, and Tg of -56°C.

[0094] [Synthesis Example 5] Polymer A-5 used in Example 10 MEA (182 parts by mass), HEA (21 parts by mass), MA (312 parts by mass), and ethyl acetate (770 parts by mass) were charged into a 3-liter four-neck flask. The mixture was thoroughly degassed by bubbling nitrogen gas, the internal temperature of the mixture was raised to 75°C, and V-65 (0.35 parts by mass) was charged to initiate polymerization. After 5 hours, ethyl acetate was added so that the solid content was 30% by mass, and an ethyl acetate solution of polymer A-5 was obtained. The obtained polymer A-5 consisted of 60% by mass of MA and 35% by mass of MEA, and had Mn 90,000, Mw / Mn 8.4, and Tg = -10°C.

[0095] [Synthesis Example 6] Polymer A-6 used in Comparative Example 2 HEA (24 parts by mass), BA (506 parts by mass), and ethyl acetate (974 parts by mass) were charged into a 3-liter four-neck flask. The mixture was thoroughly degassed by bubbling nitrogen gas, the internal temperature of the mixture was raised to 75°C, and V-65 (0.25 parts by mass) was charged to initiate polymerization. After 5 hours, ethyl acetate was added so that the solid content became 30% by mass, and an ethyl acetate solution of polymer A-6 was obtained. The obtained polymer A-6 was composed of BA 95% by mass and HEA 5% by mass, and had Mn 87,000, Mw / Mn 5.4, and Tg = -41°C.

[0096] [Table 1]

[0097] The abbreviations in Table 1 represent the following names (same for Table 2). MEA: 2-Methoxyethyl acrylate EEA: 2-ethoxyethyl acrylate MA: Methyl acrylate BA: n-butyl acrylate HEA: 2-hydroxyethyl acrylate

[0098] 2. Preparation of Acrylic Syrup [Formulation Example 1] Preparation of Syrup Ac-1 used in Example 1 MEA (68.0 parts by mass), BA (12.7 parts by mass), and HEA (4.3 parts by mass) were added to the isolated polymer A-1 (15 parts by mass) and stirred until homogenous to obtain syrup Ac-1. The composition of syrup Ac-1 is shown in Table 2.

[0099] [Formulation Example 2] Preparation of Syrup Ac-2 used in Examples 2 to 7 and Comparative Examples 1 and 3 To the isolated polymer A-2 (15 parts by mass), MEA (44.2 parts by mass), MA (17.8 parts by mass), BA (18.7 parts by mass), and HEA (4.3 parts by mass) were added and stirred until homogenous, to obtain syrup Ac-2. The composition of syrup Ac-2 is shown in Table 2.

[0100] [Formulation Example 3] Preparation of Syrup Ac-3 used in Example 8 MEA (17.0 parts by mass), BA (63.7 parts by mass), and HEA (4.3 parts by mass) were added to the isolated polymer A-3 (15 parts by mass) and stirred until homogenous to obtain syrup Ac-3. The composition of syrup Ac-3 is shown in Table 2.

[0101] [Formulation Example 4] Preparation of Syrup Ac-4 used in Example 9 To the isolated polymer A-4 (15 parts by mass), EEA (68.0 parts by mass), BA (12.7 parts by mass), and HEA (4.3 parts by mass) were added and stirred until homogenous to obtain syrup Ac-4. The composition of syrup Ac-4 is shown in Table 2.

[0102] [Formulation Example 5] Preparation of Syrup Ac-5 used in Example 10 To the isolated polymer A-5 (15 parts by mass), MEA (29.7 parts by mass), MA (51.0 parts by mass), and HEA (4.3 parts by mass) were added and stirred until homogenous, to obtain syrup Ac-5. The composition of syrup Ac-5 is shown in Table 2.

[0103] [Formulation example 6] BA (80.7 parts by mass) and HEA (4.3 parts by mass) were added to the isolated polymer A-6 (15 parts by mass) and stirred until homogenous to obtain syrup Ac-6. The composition of syrup Ac-6 is shown in Table 2.

[0104] [Table 2]

[0105] 3. Preparation of adhesive composition and production of adhesive sheet [Example 1] The syrup Ac-1 obtained in Formulation Example 1 (100 parts by mass), 1-hydroxycyclohexyl phenyl ketone (manufactured by BASF, product name "Omnirad 184") (0.2 parts by mass) as a photopolymerization initiator, and t-butylperoxy-2-ethylhexyl monocarbonate (manufactured by NOF Corporation, product name "Perbutyl E") (0.1 parts by mass) as a thermal polymerization initiator were mixed to obtain a pressure-sensitive adhesive composition. This adhesive composition was applied onto a 50 μm thick polyethylene terephthalate (hereinafter referred to as "PET") separator. Next, a 38 μm thick PET separator with a different peel strength from the above separator was attached, and the adhesive composition was irradiated with a UV-LED surface irradiation device (model: HLDL-470X370U65PSCSP) manufactured by CCS Inc. at an illuminance of 3.0 mW / cm. 2 The adhesive composition was irradiated with UV light for 15 minutes to polymerize the monomers in the adhesive composition, and a double-sided separator-attached adhesive sheet sample was obtained. The polymer obtained at this time is called acrylic adhesive polymer (A). The thickness of the adhesive layer after UV curing was 100 μm. The obtained adhesive sheet sample was used to carry out various evaluations by the methods described below. The evaluation results are shown in Table 3.

[0106] <Evaluation method> Gel fraction measurement (before heat treatment) 0.2 g of adhesive was taken from the adhesive layer of the adhesive sheet sample, and the initial mass of the adhesive was weighed. The adhesive was immersed in 50 g of ethyl acetate and left at room temperature for 16 hours. Then, it was filtered through a 200 mesh wire net, and the residue remaining on the mesh was dried at 80°C for 3 hours and weighed. From the initial mass and the mass of the residue, the gel fraction based on the acrylic adhesive polymer (A) was calculated by the following formula. Gel fraction (%)=(mass of residue) / [(initial mass)×(solid content of acrylic adhesive polymer (A)) / (solid content of entire adhesive composition)]×100

[0107] Gel fraction measurement (after heat treatment) The pressure-sensitive adhesive sheet samples were heat-treated under the following heat treatment conditions, and the gel fraction of the heat-treated pressure-sensitive adhesive sheet samples was measured in the same manner as above. (Heat treatment conditions) The laminate after pressure bonding was subjected to a heat treatment at 150° C. for 10 minutes using a blower dryer (SPHH202 manufactured by Espec).

[0108] -Unevenness tracking evaluation Two sheets of polyester fabric were attached to each other using the adhesive sheet sample cut to a width of 10 mm, to obtain a laminate in the order polyester fabric / adhesive sheet sample / polyester fabric. The obtained laminate was subjected to a heat press treatment (conditions: 130°C, 3 kg / cm 2 When the laminate was peeled off by hand after being pressed together by pressure (for 10 seconds), those that broke inside the adhesive while peeling off were judged as having good conformability to the unevenness of the fabric, and were judged as "O", whereas those that peeled off at the fabric interface were judged as having insufficient conformability to the unevenness of the fabric, and were judged as "X".

[0109] Solvent resistance evaluation The laminate was manufactured in the same manner as in the unevenness-following evaluation, and then heat-treated at 150°C. It was placed in a 250mL glass bottle, to which 200mL of perchloroethylene was added and stirred with a MIX rotor for 1 hour. The test piece was then dried at 130°C for 5 minutes and evaluated for peeling of the adhesive. Those that showed no peeling were rated as "○", and those that showed peeling were rated as "×".

[0110] High temperature peel test A laminate was produced in the same manner as in the evaluation of the conformability to irregularities described above, and then heat-treated at 150°C to form a test piece. Using a tensile tester INSTRON 5566A (manufactured by Instron Japan), the T-type peel strength was measured under conditions of a measurement temperature of 80°C, a test piece width of 10 mm, and a peel speed of 300 mm / min, and this was taken as the high-temperature peel strength.

[0111] [Example 2] A pressure-sensitive adhesive composition was produced by the same procedure as in Example 1, except that syrup Ac-2 obtained in Formulation Example 2 was used instead of syrup Ac-1, and the amount of the thermal polymerization initiator "Perbutyl E" added was 0.1 parts by mass, and various evaluations were performed in the same manner as in Example 1. [Example 3] A pressure-sensitive adhesive composition was produced by the same procedure as in Example 1, except that syrup Ac-2 obtained in Formulation Example 2 was used instead of syrup Ac-1, and various evaluations were performed in the same manner as in Example 1. [Example 4] A pressure-sensitive adhesive composition was produced by the same procedure as in Example 1, except that syrup Ac-2 obtained in Formulation Example 2 was used instead of syrup Ac-1, and the amount of the thermal polymerization initiator "Perbutyl E" added was 0.6 parts by mass, and various evaluations were performed in the same manner as in Example 1.

[0112] [Example 5] A pressure-sensitive adhesive composition was produced by the same operation as in Example 1, except that syrup Ac-2 obtained in Formulation Example 2 was used instead of syrup Ac-1, and 0.01 parts by mass of a multifunctional acrylate, "Anilox M-309" (manufactured by Toagosei Co., Ltd.), was added, and various evaluations were performed in the same manner as in Example 1. [Example 6] An adhesive composition was produced by the same operations as in Example 1, except that syrup Ac-2 obtained in Formulation Example 2 was used instead of syrup Ac-1, and 0.3 parts by mass of t-hexylperoxyisopropyl monocarbonate (manufactured by NOF Corporation, product name "Perhexyl I"), a thermal polymerization initiator having a lower hydrogen abstraction ability than "Perbutyl E", was added instead of "Perbutyl E". Various evaluations were performed in the same manner as in Example 1. [Example 7] A pressure-sensitive adhesive composition was produced by the same procedure as in Example 1, except that syrup Ac-2 obtained in Formulation Example 2 was used instead of syrup Ac-1, and 0.6 parts by mass of "Perhexyl I" was added instead of "Perbutyl E", and various evaluations were performed in the same manner as in Example 1.

[0113] [Example 8] A pressure-sensitive adhesive composition was produced by the same procedure as in Example 1, except that syrup Ac-3 obtained in Formulation Example 3 was used instead of syrup Ac-1, and various evaluations were performed in the same manner as in Example 1. [Example 9] A pressure-sensitive adhesive composition was produced by the same procedure as in Example 1, except that syrup Ac-4 obtained in Formulation Example 4 was used instead of syrup Ac-1, and various evaluations were performed in the same manner as in Example 1. [Example 10] A pressure-sensitive adhesive composition was produced by the same procedure as in Example 1, except that syrup Ac-5 obtained in Formulation Example 5 was used instead of syrup Ac-1, and various evaluations were performed in the same manner as in Example 1.

[0114] [Comparative Example 1] A pressure-sensitive adhesive composition was produced in the same manner as in Example 1, except that syrup Ac-2 obtained in Formulation Example 2 was used instead of syrup Ac-1, and the thermal polymerization initiator "Perbutyl E" was not added, and various evaluations were performed in the same manner as in Example 1. [Comparative Example 2] A pressure-sensitive adhesive composition was produced in the same manner as in Example 1, except that syrup Ac-6 obtained in Formulation Example 6 was used instead of syrup Ac-1, and various evaluations were carried out in the same manner as in Example 1. [Comparative Example 3] An adhesive composition was produced in the same manner as in Example 1, except that syrup Ac-2 obtained in Formulation Example 2 was used instead of syrup Ac-1, and 1.0 part by mass of an isocyanate-based curing agent, "Takenate D-110N" (ethyl acetate solution with a solid content of 75%) manufactured by Mitsui Chemicals, was added in terms of solid content. In addition, an adhesive sheet sample with a double-sided separator was obtained using the obtained adhesive composition in the same manner as in Example 1. The adhesive sheet sample was aged at room temperature for one week to promote the reaction of the isocyanate-based curing agent. Various evaluations were performed using the obtained adhesive sheet sample in the same manner as in Example 1.

[0115] Table 3 shows the components and evaluation results of the pressure-sensitive adhesive compositions of Examples 1 to 10 and Comparative Examples 1 to 4. [Table 3]

[0116] The abbreviations in Table 3 represent the following names. M-309: Multifunctional acrylate, product name "Anilox M-309", manufactured by Toagosei Co., Ltd. D-110: Isocyanate-based hardener, product name "Takenate D-110N", manufactured by Mitsui Chemicals Omnirad184: Photopolymerization initiator, product name "Omnirad 184", manufactured by BASF Perbutyl E: Thermal polymerization initiator, product name "Perbutyl E", manufactured by NOF Corporation Perhexyl I: Thermal polymerization initiator, trade name "Perhexyl I", manufactured by NOF Corporation The amounts of the polyfunctional acrylate, the crosslinking agent, the photopolymerization initiator, and the thermal polymerization initiator are based on 100 parts by mass of the polymer syrup.

[0117] As shown in Table 3, all of the pressure-sensitive adhesive sheets of Examples 1 to 10, which were produced using a pressure-sensitive adhesive composition containing a polymer syrup producing an acrylic pressure-sensitive adhesive polymer (A) having (meth)acrylic acid alkoxyalkyl ester units and a thermal polymerization initiator, had good conformability, solvent resistance, and high-temperature adhesion. In particular, Examples 1 to 7 and 9, which showed a large difference in gel fraction before and after heating after bonding the adherend (polyester fabric) and the pressure-sensitive adhesive sheet, were rated as "○" for both conformability and solvent resistance, and also showed a high high-temperature peel strength of 1.5 N / 10 mm.

[0118] In contrast, Comparative Example 1, in which no thermal polymerization initiator was added to the adhesive composition, and Comparative Example 2, in which the adhesive layer contained a polymer having no (meth)acrylic acid alkoxyalkyl ester unit as the acrylic adhesive polymer, were rated as "x" for solvent resistance and had low high-temperature peel strength. Comparative Example 3, in which a crosslinking agent was added to the adhesive composition, had a high gel fraction of 78.3% for the adhesive sheet before it was attached to the adherend (i.e., before it was cured), and in this case, the unevenness-following ability and solvent resistance were rated as "x" and the high-temperature peel strength was also low.

Claims

1. A pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer, The pressure-sensitive adhesive layer contains an acrylic pressure-sensitive adhesive polymer (A) and a thermal polymerization initiator, The acrylic adhesive polymer (A) has a structural unit derived from an alkoxyalkyl (meth)acrylate, the pressure-sensitive adhesive layer has a gel fraction based on the acrylic pressure-sensitive adhesive polymer (A) of less than 20%, A pressure-sensitive adhesive sheet, wherein the pressure-sensitive adhesive layer has a gel fraction based on the acrylic pressure-sensitive adhesive polymer (A) of 20% or more after heat treatment.

2. The pressure-sensitive adhesive sheet according to claim 1, wherein the content of structural units derived from an alkoxyalkyl ester of (meth)acrylic acid in the acrylic pressure-sensitive adhesive polymer (A) is 20 mass% or more based on all structural units derived from monomers constituting the acrylic pressure-sensitive adhesive polymer (A).

3. The pressure-sensitive adhesive sheet according to claim 1 or 2, wherein the acrylic pressure-sensitive adhesive polymer (A) has a glass transition temperature of -80°C to 10°C.

4. A method for producing a pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer, comprising: The method includes a step of forming a pressure-sensitive adhesive layer containing an acrylic adhesive polymer (A) and a thermal polymerization initiator by irradiating an active energy ray onto a layer of a pressure-sensitive adhesive composition containing an acrylic adhesive polymer syrup, a photopolymerization initiator, and a thermal polymerization initiator, The acrylic adhesive polymer syrup contains an alkoxyalkyl (meth)acrylic acid ester, the pressure-sensitive adhesive layer has a gel fraction based on the acrylic pressure-sensitive adhesive polymer (A) of less than 20 mass%, the pressure-sensitive adhesive layer has a gel fraction based on the acrylic pressure-sensitive adhesive polymer (A) after heat treatment of 20% or more; A method for producing a pressure-sensitive adhesive sheet.

5. A method for producing a laminate, comprising a step of laminating the pressure-sensitive adhesive sheet according to any one of claims 1 to 3 to an adherend, and then carrying out a heat treatment to cure the pressure-sensitive adhesive layer.

Citation Information

Patent Citations

  • Method of treating workpiece

    JP2008021871A

  • Adhesive composition and adhesive, as well as adhesive for optical member, and optical member with adhesive layer obtained using the same

    JP2010121118A

  • Followable adhesive film for applied to uneven surface of decorative material and method for producing the same

    JP2017197604A

  • Adhesive sheet, adhesive sheet with peel-off sheet, laminate, and laminate manufacturing method

    JP2020033417A

  • Acrylic resin composition, adhesive agent composition, base for adhesive sheet, and adhesive sheet

    WO2018235217A1