Laminated Sheet
The laminated sheet addresses moldability issues in electromagnetic shielding by alternating layers with specific compositional differences, achieving high return loss and elongation at break, ensuring effective electromagnetic wave absorption and reduced defects during shaping.
Patent Information
- Application Number
- JP2021056861
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-30
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-03-30
AI Technical Summary
Existing electromagnetic shielding materials lack moldability, particularly when used in applications requiring shaping to match design specifications, such as building materials and electronic device housings, due to high concentrations of conductive or magnetic materials and poor processing characteristics.
A laminated sheet composed of alternately laminated layers with different compositions, ensuring a return loss of at least 5.0 dB and elongation at break between 1% and 2000% at 90°C, achieved by alternating layers with specific differences in elastic modulus, surface potential, atomic composition, or observable interfaces, and incorporating conductive, dielectric, or magnetic particles to enhance electromagnetic wave absorption and reflection.
The laminated sheet maintains excellent electromagnetic wave absorption performance while offering improved moldability, reducing stress and defects during stretching, and ensuring consistent shielding across various frequency bands.
Smart Images

Figure 0007589621000002 
Figure 0007589621000003 
Figure 0007589621000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate sheet having excellent electromagnetic wave shielding properties. [Background technology]
[0002] With the advancement of communication technology, electromagnetic waves of various frequency bands are used and fly around in the atmosphere, such as meter waves in the hundreds of MHz to several GHz bands mainly used in mobile phones and wireless communications, centimeter waves in the several GHz to several tens of GHz bands mainly used in mobile communications such as 4G and 5G and wireless LAN (Wi-fi) communications, and millimeter waves in the several tens of GHz to several hundreds of GHz bands mainly used in automobile collision prevention radar. Electromagnetic waves of appropriate frequency bands are selected according to the amount of information, the distance to be transmitted, and the purpose, but since electromagnetic waves of similar frequency bands are used in various devices and applications, there is an increasing need for electromagnetic wave shielding materials that block electromagnetic waves to prevent various radio interference (device malfunctions, communication failures, information leaks, and effects on the human body, which is sensitive to electromagnetic waves). In particular, in recent years, the development of communication technologies that use electromagnetic waves in the GHz frequency band has accelerated in order to realize high-speed and large-capacity communication, and electromagnetic wave shielding materials that can block electromagnetic waves in the relevant frequency bands are required.
[0003] Electromagnetic waves are waves composed of two components, an electric field and a magnetic field, which propagate through space while vibrating against each other. Electromagnetic shielding materials that block electromagnetic waves are materials that reflect electromagnetic waves on the surface / inside of the material, or absorb electromagnetic waves inside the material, thereby losing or attenuating electromagnetic wave energy, and the effect can be enhanced by combining reflection and absorption. For example, the effect of surface reflection of electromagnetic waves can be enhanced by the difference in electrical resistance (impedance) between the air interface and the electromagnetic shielding material interface, and generally, electromagnetic shielding properties over a wide range of frequency bands can be achieved by coating and laminating a material with a very low resistance value, such as metal (e.g., copper), on the surface of the substrate (Patent Document 1). In general, when shielding electromagnetic waves by reflecting them, it is necessary to install a shielding material at a position that separates the source of the electromagnetic waves from the object to be protected, so this is not suitable for protecting the radar itself from the electromagnetic waves emitted by the radar, for example.
[0004] On the other hand, electromagnetic wave shielding by absorption involves dissipating electromagnetic wave energy by incorporating conductive and / or magnetic materials into the substrate and absorbing the electromagnetic waves that enter the substrate as induced current, and the absorption performance is realized by incorporating carbon materials, ferrite, metal materials including various 3d transition elements such as iron, etc. into dielectric polymers such as rubber (Patent Documents 2 to 4). As for magnetic materials, a technology has been disclosed in which flexibility is imparted by dispersing them in acrylic rubber or silicone rubber (Patent Document 5). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Special Publication No. 2011-502285 [Patent Document 2] JP 2012-94764 A [Patent Document 3] JP 2000-243615 A [Patent Document 4] JP 2004-39703 A [Patent Document 5] JP 2019-75571 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, the techniques shown in Patent Documents 2 to 4 have poor moldability because they contain a high concentration of conductive material and / or magnetic material or the solvent is removed during production. Moldability is preferable in many applications requiring electromagnetic wave shielding materials, and in particular, when electromagnetic wave absorbing performance is used in building materials, electronic device housings, and the interior and exterior of transportation, it is required to be able to mold into a shape that matches the design. Patent Document 5 succeeds in imparting flexibility by using rubber as a binder, but this is insufficient to make it conform to deep shapes. The present invention aims to solve the above problems and provide a laminated sheet that combines electromagnetic wave shielding properties and moldability. [Means for solving the problem]
[0007] In order to solve the above problems, the present invention has the following configuration: That is, it is a laminate sheet including an alternating laminate unit in which two different types of layers (layers A and B) are alternately laminated in a total of five or more layers, and characterized in that, when the return loss of an electromagnetic wave is measured for each frequency and plotted with the return loss on the vertical axis and the frequency on the horizontal axis, the return loss at the peak top of the peak with the largest return loss is 5.0 dB or more, and the elongation at break at 90°C is more than 1% and not more than 2000%. Effect of the Invention
[0008] By laminating two types of layers, the present invention can reduce the stress during stretching and increase the elongation at break, thereby providing a laminate sheet with excellent formability while maintaining its electromagnetic wave absorption performance. [Brief description of the drawings]
[0009] [Figure 1]1 is a diagram showing the peak top of the peak with the largest return loss when plotted with the vertical axis representing the return loss and the horizontal axis representing the frequency. [Diagram 2] 1 is a diagram showing the peak top of the peak with the largest return loss when plotted with the vertical axis representing the return loss and the horizontal axis representing the frequency. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The laminate sheet of the present invention will be described in detail below. The laminate sheet of the present invention includes an alternating laminate unit in which two different layers (layers A and B) are alternately laminated for a total of five or more layers, and is characterized in that, when the return loss of an electromagnetic wave is measured for each frequency and plotted with the return loss on the vertical axis and the frequency on the horizontal axis, the return loss at the peak top of the peak with the largest return loss is 5.0 dB or more, and the elongation at break at 90°C is more than 1% and not more than 2000%.
[0011] The laminated sheet of the present invention is characterized by including an alternating laminate unit in which two different types of layers (layers A and B) are alternately laminated for a total of five or more layers. Here, "different from each other" refers to the fact that at least one of the resin and particles constituting each layer has a different composition, which can be confirmed by the following method.
[0012] Specifically, the compositions of the layers can be considered to be different in any of the following cases (1) to (5). (1): The elastic modulus of the film cross section is evaluated by dynamic viscoelasticity measurement (AFM-DMA) using an atomic force microscope, and the ratio of the average elastic modulus of the two layers is 1.1 or more. (2): The surface potential is evaluated using an electric force microscope (EFM), and the ratio of the average surface potential of the two layers is 1.1 or more. (3): The concentration of each atom is evaluated using energy dispersive X-ray spectroscopy (SEM-EDX), and the ratio of the mole fraction (or weight fraction) of each atom in the two layers is 1.1 or more. (4) The two layers can be peeled off, and the density, glass transition temperature, melting point, decomposition temperature, and ash content after decomposition are evaluated between the two layers, and at least one of the values differs by 3 degrees or more or 10% or more. (5) The cross section is observed at the desired magnification (500 to 20,000 times) using a transmission electron microscope (TEM) or a scanning electron microscope (SEM) and the interface can be confirmed. The fact that the interface can be confirmed here means that the brightness between adjacent layers is different. Specifically, first, the brightness is measured at 1000 points for each layer. Next, the average brightness for each layer and the standard deviation of the brightness for each layer are calculated. Then, if the difference between the average brightness of two adjacent layers is greater than either of the standard deviations of the brightness of each of the two layers, the brightness is determined to be different. In addition, which of the two types of layers is to be layer A and layer B can be determined by determining the layer with a higher surface potential by EFM as layer B. In addition, when conductive particles, dielectric particles, or magnetic particles are added to layer B to adjust the dielectric constant, it is preferable to make layer A the outermost layer from the viewpoint of film forming properties and prevention of particle falling off.
[0013] By laminating five or more different layers alternately, the layer with excellent formability acts as a support layer, improving the elongation at break, and defects such as tears and holes during molding can be suppressed. In addition, a thermally crystallized film becomes brittle, but in the present invention, the layers are made thin, suppressing thermal crystallization, and therefore defects such as cracks during molding can also be suppressed. Furthermore, while a large deformation is applied to the resin during molding, it is desirable that the resin is resistant to impacts and scratches (small deformations) after molding. According to the present invention, the interface layer between each layer maintains its shape against small deformations, but small fractures and slippage are caused at the interface against large deformations, so that the multi-layering provides good formability and allows the film to sufficiently follow recesses that are relatively difficult to mold. From the above viewpoint, the number of layers in the alternating laminate unit is preferably 11 or more, more preferably 51 or more, and particularly preferably 201 or more. There is no particular limit to the upper limit of the number of layers in the alternating unit, but from the viewpoint of film formation stability, the maximum number is about 2000 layers.
[0014] The laminated sheet of the present invention is required to have a return loss of 5.0 dB or more at the peak top of the peak with the largest return loss when the return loss of the electromagnetic wave is measured for each frequency in the measurement method described below and plotted with the return loss on the vertical axis and the frequency on the horizontal axis. The return loss is a value that represents the amount of loss of the electromagnetic wave while traveling back and forth in the laminated sheet when the intensity of the electromagnetic wave reflected by the laminated sheet is measured for an electromagnetic wave of a specific frequency that is incident on the laminated sheet and returned, and is expressed in decibels (dB). Specifically, using the coaxial waveguide method or the free space method, an electromagnetic wave is irradiated onto a laminated sheet combined with a metal reflector plate made of aluminum or the like on the back side, and the intensity of the electromagnetic wave reflected by the metal plate and traveling back and forth in the laminated sheet is measured and calculated. The return loss is measured by sweeping the frequency, and a return loss spectrum is plotted with the return loss on the vertical axis and the frequency on the horizontal axis. In some cases, multiple peaks are obtained, but the return loss peak with the largest peak intensity (attenuation) is the one that is the most important. The peak top referred to here refers to the position where the sign (slope) of the tangent to the reflectance attenuation spectrum changes from positive to negative or from negative to positive.
[0015] The return loss at the peak top of the peak with the largest return loss will be described with reference to Figs. 1 and 2. Figs. 1 and 2 are diagrams showing the peak top of the peak with the largest return loss when plotted with the return loss on the vertical axis and the frequency on the horizontal axis. In each diagram, the reference numeral 1 indicates the peak with the largest return loss, and the reference numeral 2 indicates the return loss at the peak top of the peak with the largest return loss. In the case of a single peak top without a slope of the baseline as shown in Fig. 1, the peak has the largest return loss, and the difference between the peak top of the peak and the baseline is the return loss at the peak top of the peak with the largest return loss. Even in the case of a single peak with a slope of the baseline as shown in Fig. 2, the return loss at the peak top of the peak with the largest return loss can be determined in the same manner as in Fig. 1, except that the baseline becomes a straight line with a slope. In addition, when a spectrum with multiple peak tops including a shoulder peak is obtained, the peak with the largest return loss can be identified from the multiple peaks, and the return loss at the peak top of the peak with the largest return loss can be determined in the same manner.
[0016] The return loss at the peak top of the peak with the largest return loss shown in this way must be 5.0 dB or more. Hereinafter, the "return loss at the peak top of the peak with the largest return loss" may be referred to as the "maximum return loss". A maximum return loss of less than 5.0 dB means that the electromagnetic wave transmittance is substantially higher than 30%. Therefore, a laminated sheet with a maximum return loss of less than 5.0 dB cannot be said to have sufficient electromagnetic wave shielding properties. From the viewpoint of electromagnetic wave shielding properties, the maximum return loss in the laminated sheet of the present invention is preferably 15.0 dB or more, more preferably 20.0 dB or more, and even more preferably 30.0 dB or more. When the maximum return loss is about 30.0 dB, it means that 99.9% of the electromagnetic wave of the frequency of the peak top that is incident is shielded, assuming that 100% of the electromagnetic wave in the frequency band around the peak is transmitted, and it can be said that the sheet has very high electromagnetic wave shielding properties in the frequency band. The upper limit is not particularly limited, but it is preferably 100 dB or less.
[0017] Methods for achieving a maximum return loss of 5.0 dB or more include, for example, a method using a fluorine-based high-dielectric constant resin such as polyvinylidene fluoride, or a conductive resin such as polythiophene or polyacetylene, etc. Also included are methods using a resin containing conductive particles such as carbon black, graphite, carbon fiber, carbon nanotubes, gold, silver, copper, etc., dielectric materials such as titanium oxide, mica, or metal titanate, or magnetic particles such as ferrite, carbonyl iron, or flat metal particles.
[0018] In addition, it is preferable that the frequency bandwidth where the return loss exceeds 5.0 dB at the peak of the largest return loss is as wide as possible while showing a steep and high electromagnetic wave shielding property, because this reduces the fluctuation of the frequency bandwidth that can be shielded due to the uneven thickness of the laminated sheet. Specifically, the frequency bandwidth where the return loss is 5.0 dB or more at the peak of the largest return loss is preferably 1.0 GHz or more, more preferably 3.0 GHz or more, and even more preferably 5.0 GHz or more. The upper limit is preferably 20.0 GHz or less.
[0019] As a method for making the frequency bandwidth where the return loss exceeds 5.0 dB at the peak with the largest return loss 1.0 GHz or more or the above-mentioned preferable range, for example, there is a method of matching the reflected waves from each layer by making it a multi-layer structure. If reflection occurs only at the laminated sheet surface and the reflector, there is only one matching wavelength, but by making it a multi-layer structure, the matching wavelength differs slightly for each layer, so it is possible to absorb electromagnetic waves over a wide band.
[0020] From the viewpoint of improving moldability, the laminated sheet of the present invention needs to have a breaking elongation at 90°C of more than 1% and not more than 2000%. The breaking elongation at 90°C is preferably 50% or more, more preferably 100% or more, even more preferably 200% or more, and particularly preferably 400% or more. By setting the breaking elongation within this range, defects such as tears and holes during molding can be suppressed. Methods for setting the breaking elongation within this range include, for example, multi-layering, using a resin with good moldability, and moderate stretching.
[0021] The elongation at break at 90 ° C. can be determined by the following procedure. First, according to the method described in JIS K-7161 (2014) and JIS K-7127 (1999), a sample with a measurement length of 5 cm × film width of 1 cm is measured at a temperature of 90 ° C. and a pulling speed of 300 mm / min in the longitudinal direction at break. Next, the measurement direction is similarly set to the width direction, and the elongation at break in the width direction is measured, and the average value of both is taken as the elongation at break at 90 ° C. The longitudinal direction refers to the direction in which the sheet runs in the manufacturing process (the winding direction in the case of a roll), and the width direction refers to the direction perpendicular to the longitudinal direction in the sheet plane. Note that, although multiple measurement methods specifying the longitudinal direction are described in this specification, when a sample with an unspecified longitudinal direction is used, the elongation at break is measured every 30 ° from any direction of the sample, and the direction with the smallest elongation at break is taken as the longitudinal direction.
[0022] In the laminated sheet of the present invention, the difference (ΔTcg) between the crystallization temperature Tc and the glass transition temperature Tg is preferably 50°C or more and 200°C or less, or the crystallization temperature Tc cannot be observed. In the case where the crystallization temperature Tc can be observed, ΔTcg is more preferably 70°C or more, and even more preferably 90°C or more. If the sheet does not soften during molding, molding is difficult and insufficient conformity to the molded object member is likely to occur, but if it crystallizes, it becomes brittle and defects are likely to occur. Therefore, molding must be performed at a temperature between the glass transition temperature and the crystallization temperature, but by setting ΔTcg in this range, the moldable temperature is widened, making it easy to obtain good moldability (including conformity), and the range of molded objects is also widened. In addition, even if the crystallization temperature is not observed, good moldability can be obtained because embrittlement due to crystallization does not occur. Methods for setting ΔTcg in the above range include multilayering, copolymerization and mixing of amorphous components, and copolymerization and mixing of low Tg resins.
[0023] Tg is determined based on the method described in JIS K-7121 (1987) using a differential scanning calorimetry chart obtained by heating a laminated sheet from 25°C to 290°C at a heating rate of 20°C / min, holding the sheet in that state for 5 minutes, and then quenching the sheet to 25°C or less. Tc can be determined by identifying the peak top temperature of the crystallization peak in a differential scanning calorimetry chart obtained during cooling when the sheet is heated from 25°C to 290°C at a heating rate of 20°C / min after the measurement of Tg (1st run) is completed, and the sheet is cooled from 290°C to 25°C at a cooling rate of 20°C / min. ΔTcg can be calculated by determining the difference between Tg and Tc.
[0024] The laminated sheet of the present invention preferably has a stress of 10.0 MPa or less at 100% elongation in a tensile test at 90 ° C., more preferably 5.0 MPa or less. Usually, in a film mainly composed of a thermoplastic resin, the polymer of the thermoplastic resin is oriented during stretching, so that the stress at 100% elongation is higher than the stress at the start of molding. By suppressing the stress at 100% elongation within the above range, molding is possible with a small force, and a sheet with excellent conformity to the molding member is obtained. In addition, the lower limit of the stress at 100% elongation in a tensile test at 90 ° C. is preferably 3.0 MPa, in order to prevent sagging due to too low stress. The stress at 100% elongation can be measured by a tensile test similar to that used to measure the elongation at break at 90 ° C., and the average value of the obtained values can be used.
[0025] An example of a method for adjusting the stress at 100% elongation in a tensile test at 90° C. to 10.0 MPa or less or to the above-mentioned preferred range is to adjust the stretch ratio of the laminated sheet. The higher the stretch ratio, the higher the stress can be.
[0026] From the viewpoint of reducing the decrease in return loss due to molding, the laminate sheet of the present invention preferably exhibits a change in peak-top return loss before and after stretching to a thickness of 5 / 6 of the original thickness of 5 dB or less, more preferably 4 dB or less, and even more preferably 3 dB or less. By adopting such an embodiment, the laminate sheet can ensure electromagnetic wave shielding properties even if the thickness of the laminate sheet becomes thinner as the laminate sheet is stretched by molding.
[0027] In order to make the change in the return loss at the peak top before and after stretching to 5 / 6 the thickness 5 dB or less or within the above-mentioned preferable range, the laminated sheet may be multi-layered. More specifically, the change in the return loss at the peak top can be suppressed by increasing the number of alternate laminations of two types of layers with different electrical conductivity.
[0028] In a sheet using electromagnetic wave absorbing particles such as magnetic material, the amount of magnetic material that the electromagnetic waves come into contact with when passing through the sheet is usually reduced as the thickness decreases, so the attenuation amount is greatly reduced. Therefore, there is a drawback that the electromagnetic wave shielding performance is reduced after molding. By configuring the laminated sheet to have two types of layers with different electrical conductivity laminated alternately, the dielectric is appropriately dispersed, and even if the thickness is reduced by stretching, the dielectric constant is improved due to the arrangement of the particles, so that the reduction in attenuation amount due to the reduction in thickness can be compensated for. However, if the above-mentioned multilayering is performed, a magnetic material may be used in combination within a range that does not impair the effect of the present invention. In addition, when multilayering and magnetic particles are used in combination, there is also the advantage that the arrangement of the magnetic particles is promoted by the layer containing the magnetic particles becoming thinner.
[0029] From the above viewpoint, the number of layers of the alternating laminate unit in the laminate sheet of the present invention is preferably 51 layers or more, and particularly preferably 201 layers or more. Furthermore, it is preferable that the laminate sheet contains a polymer, since it is expected to improve the dielectric constant due to the orientation of the polymer chain. Examples of the polymer include polyester, polyacrylate, polycarbonate, polyamide, polyimide, polyurethane, etc. Among them, it is preferable that the polymer has an aromatic ring in the molecule from the viewpoint of contributing to the improvement of the dielectric constant.
[0030] In the laminated sheet of the present invention, the change in peak top return loss before and after stretching to 2 / 3 of the thickness is preferably 10 dB or less, more preferably 7 dB or less, and even more preferably 5 dB or less. During molding, some parts are locally stretched at a high ratio, but by designing the return loss to be small even in the parts where the thickness is thin, various radio interference can be suppressed throughout the laminated sheet. Methods for keeping the return loss change within the above range include, for example, the use of a dielectric, the use of a polymer, and multi-layering, and the details are the same as the method for keeping the change in peak top return loss before and after stretching to 5 / 6 of the thickness to 5 dB or less or within the above preferred range.
[0031] When the laminated sheet of the present invention is stretched to a thickness of 5 / 6, the maximum change in the peak top return loss is preferably 5 dB or less, more preferably 2 dB or less, when the return loss for linearly polarized waves is measured. A detailed method for measuring the return loss for linearly polarized waves will be described later. By keeping the change in the return loss for linearly polarized waves within the above range, various radio interferences associated with communications and sensors using linearly polarized waves can be prevented even after molding. The method for measuring the return loss for linearly polarized waves will be described later.
[0032] In order to set the maximum change in the peak top return loss within the range when the return loss for linearly polarized waves is measured before and after the thickness is stretched to 5 / 6, in addition to the above-mentioned methods for suppressing the change in return loss (use of dielectric, use of polymer, multilayering, etc.), it is effective to increase the anisotropy of the particles. For example, there is a method of using particles with anisotropic dielectric constant such as titanium oxide or barium titanate, and a method of using particles with anisotropic shape such as carbon nanotubes, which are cylindrical carbon such as single-walled nanotubes, multi-walled nanotubes, and cup-stacked nanotubes, flat carbon such as graphite, graphite, and graphene, cylindrical graphite, carbon microcoils, fullerenes, carbon fibers (long fibers, short fibers), needle-shaped titanium oxide, and plate-shaped titanium oxide. In addition, as particles with small anisotropy but contributing to electromagnetic wave absorption, there are carbon black (spherical carbon) such as acetylene black, channel black, lamp black, thermal black, ketjen black, and furnace black, and spherical graphite, and it is also preferable to use these.
[0033] In the laminate sheet of the present invention, when the return loss for linearly polarized waves is measured before and after stretching to 2 / 3 of its thickness, the maximum change in the peak-top return loss is preferably 10 dB or less, more preferably 7 dB or less, and even more preferably 5 dB or less. By adopting such an embodiment, although some parts are locally stretched at a high ratio during molding, even the parts with a reduced thickness can sufficiently absorb linearly polarized waves, and various types of radio interference can be prevented.
[0034] As described above, methods for keeping the maximum change in peak-top return loss within the above range when measuring the return loss for linearly polarized waves before and after stretching to 2 / 3 of the thickness include, for example, the use of dielectrics, the use of polymers, multilayering, and the use of anisotropic particles.
[0035] In the laminated sheet of the present invention, the value (Aλ / d) obtained by dividing the return loss (dB) of the peak top by the thickness (μm) and multiplying it by the wavelength (mm) of the peak top is preferably 0.10 dB·mm / μm or more and 2.00 dB·mm / μm or less, more preferably 1.00 dB or less, even more preferably 0.50 dB or less, and particularly preferably 0.35 dB or less. Usually, the thinner the sheet is designed, the higher the frequency of electromagnetic waves it can absorb, but it is more likely to have the disadvantage that the attenuation fluctuates with a small change in thickness. On the other hand, if the sheet is thick, the attenuation is stable, but it is difficult to absorb electromagnetic waves of high frequencies. As a result of intensive research into a sheet that can stably absorb electromagnetic waves in the centimeter to millimeter wave band, it was found that a good attenuation can be stably obtained if Aλ / d is within the above range. The peak top referred to here refers to the peak top of the peak with the largest return loss when the return loss of the electromagnetic wave is measured for each frequency and plotted with the vertical axis as the return loss and the horizontal axis as the frequency. The thickness can be measured by a known dial gauge.
[0036] Methods for setting Aλ / d within the above range include adjusting the particle concentration in the sheet to set the dielectric constant of the sheet within an appropriate range, and adjusting the thickness during production. More specifically, Aλ / d can be reduced by increasing the particle concentration or increasing the thickness.
[0037] The laminated sheet of the present invention preferably has a Young's modulus (Ys) of 1.0 GPa or more and 10 GPa or less by a static viscoelasticity test, and a ratio (Ys / Yd) of the Young's modulus (Yd) by a dynamic viscoelasticity test of 0.5 or more. In the static viscoelasticity test, strength and ease of deformation against large deformation over a long period of time are evaluated, and a lower value is preferable when molding the laminated sheet according to the application. Therefore, it is preferable that Ys is 6.0 GPa or less. On the other hand, in the dynamic viscoelasticity test, strength and ease of deformation against momentary minute deformation are evaluated, and a higher value is preferable from the viewpoint of increasing the strength of the molded body. The Young's moduli measured in each test are generally proportional, but by setting Ys / Yd within the above range, good molding followability can be obtained while maintaining the strength after molding. From the above viewpoint, Ys / Yd is more preferably 2.0 or more.
[0038] The Young's modulus (Ys) in the static viscoelasticity test refers to the average value of the Young's modulus in the longitudinal direction and the width direction when pulled at room temperature of 23°C, 5 cm between chucks, and a pulling speed of 300 mm / min. The Young's modulus (Yd) in the dynamic viscoelasticity test can be determined by the following procedure. First, for a sample with a measurement length of 2 cm and a film width of 1 cm, the average storage modulus (Young's modulus) in the longitudinal direction is measured under the conditions of a temperature range of room temperature of 20°C to 30°C, a displacement of 10 μm, a vibration frequency of 10 Hz, and a temperature rise rate of 1°C / min. Next, the average storage modulus (Young's modulus) in the width direction is measured in the same manner, and the average value of both is taken as Yd.
[0039] A method for controlling Ys and Yd to satisfy the above requirements is, for example, extrusion film formation in a state where crystallization of the resin is suppressed by multilayering. By suppressing crystallization of the resin, Yd is suppressed, and by extruding each layer in a thin state, the molecular chains are oriented by shear, improving Ys. It is also possible to increase Ys by using a polymer with a rigid molecular chain or by stretching the polymer.
[0040] In the laminate sheet of the present invention, it is preferable to use a compound in which two or more resins are mixed in at least one layer from the viewpoint of improving moldability. It is preferable that the resin used is a thermoplastic resin, since this is particularly favorable from the viewpoint of the processability and film-forming property of the sheet.Examples of thermoplastic resins include polyolefin resins such as polyethylene, polypropylene, poly(1-butene), poly(4-methylpentene), polyisobutylene, polyisoprene, polybutadiene, polyvinylcyclohexane, polystyrene, poly(α-methylstyrene), poly(p-methylstyrene), polynorbornene, and polycyclopentene; polyamide resins such as nylon 6, nylon 11, nylon 12, and nylon 66; copolymer resins of vinyl monomers such as ethylene / propylene copolymer, ethylene / vinylcyclohexane copolymer, ethylene / vinylcyclohexene copolymer, ethylene / alkylacrylate copolymer, ethylene / acrylic methacrylate copolymer, ethylene / norbornene copolymer, ethylene / vinyl acetate copolymer, propylene / butadiene copolymer, isobutylene / isoprene copolymer, and vinyl chloride / vinyl acetate copolymer; acrylic resins such as polyacrylate, polymethacrylate, polymethyl methacrylate, polyacrylamide, and polyacrylonitrile; Polyester resins such as polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate, and polyethylene-2,6-naphthalate; polyether resins such as polyethylene oxide, polypropylene oxide, and polyacrylene glycol; cellulose ester resins such as diacetyl cellulose, triacetyl cellulose, propionyl cellulose, butyryl cellulose, acetylpropionyl cellulose, and nitrocellulose; biodegradable polymers such as polylactic acid and polybutyl succinate; and other polymers such as polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, polyvinyl butyral, polyacetal, polyglycolic acid, polycarbonate, polyketone, polyether sulfone, polyether ether ketone, modified polyphenylene ether, polyphenylene sulfide, polyetherimide, polyimide, polysiloxane, tetrafluoroethylene resin, trifluoroethylene resin, trichloroethylene resin, tetrafluoroethylene-hexafluoropropylene copolymer, and polyvinylidene fluoride can be used.
[0041] From the viewpoint of improving moldability, the laminated sheet of the present invention preferably contains at least one unit selected from the group consisting of cycloalkane units, chain alkane units having 5 or more carbon atoms, and polyethylene glycol units having a molecular weight of 20,000 or less in the resin component at 1 mol% to 99 mol%. As described above, from the viewpoint of suppressing the decrease in attenuation during molding, it is preferable to have an aromatic ring in the molecular chain, but from the viewpoint of moldability, it is not preferable because the packing between aromatic rings becomes strong. Therefore, by adding a molecular chain having a chain structure, it is possible to suppress the packing between aromatic rings and improve moldability. From the above viewpoint, it is more preferable that the resin component contains at least two units selected from the group consisting of cycloalkane units, chain alkane units having 5 or more carbon atoms, and polyethylene glycol units having a molecular weight of 20,000 or less in an amount of 1 mol% to 40 mol%. The number of carbon atoms in the chain alkane units is more preferably 7 or more, and particularly preferably 9 or more.
[0042] In addition, from the viewpoint of improving moldability, it is preferable to contain 1% by mass or more and 100% by mass or less of polyester in which at least one of a cycloalkane unit and a chain alkane unit having 5 or more carbon atoms is copolymerized. Here, 1% by mass or more and 100% by mass or less means 1% by mass or more and 100% by mass or less based on all components constituting the laminated sheet. By including it as a copolymerization component rather than a mixture, the molecular chain starts to move from the copolymerization part when heated, which may enhance the effect of reducing stress during molding. The number of carbon atoms in the chain alkane unit is more preferably 7 or more, and particularly preferably 9 or more.
[0043] In order to obtain the desired electromagnetic wave shielding properties, the prepared alternating laminate units can be bonded together with the same alternating laminate units or with alternating laminate units having different thicknesses or compositions via an adhesive sheet, pressure-sensitive adhesive sheet, double-sided tape, etc.
[0044] Furthermore, layers with different dielectric constants can be laminated on the outermost surface of the alternating laminate unit for the purpose of increasing electromagnetic wave transparency or causing electromagnetic wave reflection, etc. In this case, a coating layer containing a material exhibiting suitable electrical conductivity / magnetic properties may be applied, or different resin layers / mesh layers may be laminated via an adhesive sheet, etc., and resin / metal layers can also be laminated by sputtering (such as planar or rotary magnetron sputtering), evaporation (such as electron beam evaporation), chemical vapor deposition, metalorganic chemical vapor deposition, plasma enhanced / assisted / activated chemical vapor deposition, ion sputtering, etc., which are used as film metal coating techniques.
[0045] Hereinafter, the method for producing a laminate sheet of the present invention will be described with reference to specific examples, but the present invention is not limited to the following embodiments.
[0046] First, a laminated sheet in which rubber or a thermoplastic elastomer is used as a base polymer of a substrate will be described as an example. First, a predetermined amount of desired particles is mixed with the base polymer, and the particles are kneaded and mixed with a known device such as a kneader, a Banbury mixer, a mill mixer, a roll mill, a jet mill, or a ball mill to obtain a particle-containing base polymer mixture. The base polymer alone or the prepared particle-containing base polymer is rolled or melt extruded by a batch press to form a sheet of a desired thickness. Then, the prepared sheets corresponding to the A layer and the B layer are alternately stacked in a total of 5 layers or more, and pressed or laminated to obtain a laminated sheet. The fusion temperature at this time depends on the type of resin used, but is preferably 150°C to 400°C, more preferably 250°C to 380°C.
[0047] Next, a manufacturing method of a laminated sheet in which a thermoplastic resin exhibiting flexibility, which is a preferred resin in the present invention, is used, in which only layer B contains particles and layer A does not contain particles, will be described as an example. First, the thermoplastic resin prepared in the form of pellets and a predetermined amount of particles are kneaded in a twin-screw extruder and extruded into a gut shape, which is cooled in a water tank and cut with a chip cutter to form a particle-containing master pellet. At this time, the particles may be dry-blended with the resin and then metered and fed from a hopper, or side-fed into the molten resin using a side feeder from any position of the extruder. The feeding method is not limited to the above, and can be appropriately selected according to the specific gravity and shape of the particles used.
[0048] The thermoplastic resin compositions constituting the layers A and B are then dried in hot air or under vacuum, and fed to separate extruders, where they are heated and melted to a temperature equal to or higher than the melting point of the thermoplastic resin. The extrusion rate is then made uniform using a gear pump or the like, and the thermoplastic resin composition is discharged, and foreign matter, modified thermoplastic resin, and the like are removed using a filter or the like.
[0049] Next, these thermoplastic resin compositions are laminated in a multi-layer lamination device capable of laminating the desired number of layers, molded into a desired shape with a die, and discharged into a sheet. The sheet-like material discharged from the die is extruded onto a cooling body such as a casting drum, and cooled and solidified to become a cast sheet. At this time, since the cast sheet itself exhibits electrical conductivity, it is preferable to use a method in which air is blown out from a slit-shaped, spot-shaped, or planar device to bring the cast sheet into contact with a cooling body such as a casting drum and rapidly solidify it, or a method in which the cast sheet is brought into contact with a cooling body with a nip roll and rapidly solidify it.
[0050] As the multi-layer lamination device, a multi-manifold die, a feed block, a static mixer, etc. can be used, but in particular, in order to efficiently obtain the multi-layer laminate of the present invention, it is preferable to use a feed block having a fine slit. When such a feed block is used, the device does not become extremely large, so that the amount of foreign matter generated due to thermal deterioration is small, and high-precision lamination is possible even when the number of layers is extremely large. In addition, the lamination accuracy in the width direction is also significantly improved compared to the conventional technology. Furthermore, this device has the advantages that the thickness of each layer can be adjusted by the shape (length, width) of the slit, making it easy to achieve any layer thickness, and that the effect of the resin flow during the lamination process makes it easy to orient the particles in the direction of the laminated sheet surface.
[0051] When a laminate sheet is produced using a slit-type feedblock, the thickness and distribution of each layer can be adjusted by adjusting the pressure balance by changing the length and width of the slit. The length of the slit refers to the length of the comb teeth that form the flow path for alternately flowing layers A and B inside the slit plate. In addition, a method of forming a laminate in the feedblock and then stacking the layers through a static mixer to double the number of layers can also be used to increase the number of layers.
[0052] The cast sheet obtained can be biaxially stretched in the longitudinal direction and the transverse direction as necessary. When biaxial stretching is performed, the stretching may be performed sequentially or simultaneously. In addition, re-stretching may be performed in the longitudinal direction and / or the transverse direction as necessary.
[0053] First, sequential biaxial stretching in which the sheet is stretched in the longitudinal direction and then in the transverse direction will be described. Here, stretching in the longitudinal direction refers to uniaxial stretching for giving the sheet a molecular orientation in the longitudinal direction, and is usually performed by the difference in peripheral speed of the rolls. This stretching may be performed in one stage, or in multiple stages using a plurality of pairs of rolls. The stretching ratio varies depending on the type of resin, but is usually preferably 1.1 to 7.0 times, and particularly preferably 1.5 to 4.0 times. In addition, it is preferable to set the stretching temperature within the range of the glass transition temperature to the glass transition temperature + 100 ° C. and below the melting point for all the resins constituting the sheet. The uniaxially stretched laminated sheet obtained in this manner can be subjected to surface treatment such as corona treatment, frame treatment, and plasma treatment as necessary, and then a primer layer can be formed to improve adhesion with the film to be laminated on the upper side. In the in-line coating process, the primer layer may be applied to one side, or to both sides simultaneously or one side at a time.
[0054] The stretching in the width direction means stretching for giving the sheet a width direction orientation, and is usually performed by conveying the sheet while holding both ends with clips using a tenter. The stretching ratio varies depending on the type of resin, but is usually preferably 1.1 to 7.0 times, and particularly preferably 1.5 to 5.0 times. The stretching process can suppress the variation in attenuation and suppress the decrease in electromagnetic wave attenuation after molding. In addition, the stretching temperature is preferably within the range of glass transition temperature to glass transition temperature + 120 ° C for all resins constituting the sheet. The laminated sheet thus biaxially stretched is subjected to heat treatment at a temperature higher than the stretching temperature and lower than the melting point in a tenter, and is uniformly cooled slowly, cooled to room temperature, and wound up. In addition, if necessary, a relaxation treatment or the like may be used in the longitudinal direction and / or width direction when slowly cooling from the heat treatment in order to impart a low orientation angle and thermal dimensional stability to the sheet.
[0055] Next, the case of simultaneous biaxial stretching will be described. In the case of simultaneous biaxial stretching, the obtained cast sheet may be subjected to surface treatment such as corona treatment, frame treatment, plasma treatment, etc., as necessary, and then functions such as easy slip, easy adhesion, and antistatic properties may be imparted by in-line coating. In the in-line coating process, the coating layer may be applied to one side of the sheet, or may be applied to both sides simultaneously or one side at a time.
[0056] Next, the cast sheet is introduced into a simultaneous biaxial tenter, and conveyed while both ends of the sheet are held by clips, and stretched simultaneously and / or stepwise in the longitudinal and transverse directions. The simultaneous biaxial stretching machine (tenter) may be of the pantograph type, screw type, drive motor type, linear motor type, etc., but the drive motor type or linear motor type, which can change the stretching ratio at any time and can perform relaxation treatment at any location, is preferred. The stretching ratio varies depending on the type of resin, but is usually preferably 2.0 to 50 times in terms of area ratio, and more preferably 4.0 to 20 times. The stretching speed may be the same or different speeds in the longitudinal and transverse directions. The stretching temperature is preferably within the range of the glass transition temperature to glass transition temperature + 120°C for all resins constituting the alternating laminate unit.
[0057] In order to impart planarity and dimensional stability to the sheet thus simultaneously biaxially stretched, it is preferable to subsequently perform heat treatment in a tenter at a temperature equal to or higher than the stretching temperature and equal to or lower than the melting point of all the resins constituting the sheet. During this heat treatment, in order to suppress the distribution of the main orientation axis in the width direction, it is preferable to perform a relaxation treatment in the longitudinal direction immediately before and / or immediately after entering the heat treatment zone. After being heat treated in this manner, the sheet is uniformly cooled slowly, cooled to room temperature, and wound up. If necessary, a relaxation treatment in the longitudinal direction and / or width direction may be performed when slowly cooling from the heat treatment. A relaxation treatment in the longitudinal direction may also be performed immediately before and / or immediately after entering the heat treatment zone.
[0058] Furthermore, the laminate sheet of the present invention can be combined with an electromagnetic wave reflecting layer capable of shielding a wide frequency band to provide a laminate sheet that more strongly shields only some specific frequencies. On the other hand, a new layer exhibiting a low complex dielectric constant for lowering the reflection of electromagnetic waves on the surface can be provided on the outermost surface of the laminate sheet to provide a laminate sheet with a higher electromagnetic wave absorption effect. In addition to the latter, it is also preferable that the layer exhibiting a high complex dielectric constant of the laminate sheet exhibits a layer thickness distribution in which the layer thickness decreases continuously from the surface to the inside of the sheet. Since the concentration of the electromagnetic wave suppressing material added to the layer exhibiting a high complex dielectric constant is constant in this laminate sheet, the thickness of the layer exhibiting a high complex dielectric constant is continuously reduced from the surface layer to the inner layer, so that the electromagnetic wave suppressing material is more densely connected in the inner layer, and the complex dielectric constant gradually increases. This allows the electromagnetic waves to be taken into the interior of the laminate sheet without being carelessly reflected, thereby enhancing the effect of electromagnetic wave absorption.
[0059] Next, the electronic device, transportation, and building material of the present invention will be specifically described. The electronic device of the present invention is either an electrical product or a communication device equipped with the laminated sheet of the present invention. As a preferred embodiment of the present invention, the laminated sheet or the electromagnetic wave shielding body described above can be used for the purpose of preventing false images caused by electromagnetic waves used in 4G / 5G communication, wireless LAN, collision prevention (ITS) radar, etc., reducing unnecessary electromagnetic wave radiation from electronic devices, semiconductors, and circuits installed inside the housing of a computer, mobile phone, radio, measuring device, medical device, vehicle bumper, etc., and preventing device malfunction due to radiation from external or adjacent devices. In addition, the laminated sheet of the present invention can be used with any electrical product or communication device that uses frequencies in the GHz band, not limited to the above.
[0060] Further, preferred embodiments of the present invention include vehicles, aircraft, ships, and other means of transportation having the laminated sheet of the present invention, walls of structures such as buildings, tunnels, guardrails, highways, bridges, and steel towers, transportation facilities such as telegraphs and telephones, and transport means such as drones and unmanned vehicles. The laminated sheet of the present invention can be applied to structures such as floors, ceilings, walls, windows, and columns directly through an adhesive or via other sheets, shielding plates, panels, etc. The characteristics of the laminated sheet can also be preferably used in a method of molding the laminated sheet together with a support material into building materials for local 5G. In addition, the laminated sheet can also be used as a wall material or window material for a shielded room to prevent the influence of electromagnetic jamming noise from the outside. EXAMPLES
[0061] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. Each item was evaluated by the following methods.
[0062] (Methods for measuring characteristics and evaluating effects) The methods for measuring the characteristics and evaluating the effects of the present invention are as follows.
[0063] (1) Thickness Measurements were taken using a dial gauge (Mitutoyo 2019S-10) and a dial gauge stand (Mitutoyo 7002-10). Measurements were taken at n5 and the average value was used as the thickness.
[0064] (2) Return loss (unpolarized) The measurement unit was changed as follows according to the measurement frequency band, and measurements were performed.
[0065] (2-1) 1GHz~40GHz frequency band The attenuation of the sample was measured using a vector network analyzer (E8361A) manufactured by Agilent Technologies. A donut-shaped coaxial waveguide with an outer diameter of φ7 mm and an inner diameter of φ3.04 mm was used for the 0.5 GHz to 18 GHz frequency band, a rectangular waveguide with a rectangular shape of 4.32 mm × 10.67 mm was used for the 18 to 26.5 GHz frequency band, and a rectangular waveguide with an internal shape of 3.56 mm × 7.11 mm was used for the 26.5 to 40 GHz frequency band. The attenuation in the longitudinal direction was measured when the electric field direction in the waveguide was parallel to the longitudinal direction of the sample, and the attenuation in the width direction was measured when the electric field direction in the waveguide was parallel to the width direction. The measurement interval was set so that 200 points could be measured for each frequency band. A 3 mm aluminum metal plate was placed on the back of the sample, so that the incident electromagnetic wave was totally reflected when there was no electromagnetic wave absorption by the sample. The difference in S11, which represents the intensity ratio of the reflected electromagnetic wave to the incident electromagnetic wave, between the case with and without the sample was taken as the attenuation, and the average of the attenuation in the longitudinal direction and the width direction was taken as the return loss. In addition, the average of the frequencies that showed the maximum return loss in the longitudinal direction and the width direction before the stretching process was taken as the absorption frequency.
[0066] (2-2) 40~110GHz frequency band A measurement sample was prepared by attaching an aluminum metal plate to the back of a 150 mm square sample. Using a lens antenna type oblique incidence type electromagnetic wave absorber (electromagnetic wave absorbing material) return loss measurement device LAF-26.5B manufactured by Keycom Co., Ltd., electromagnetic waves were irradiated at an oblique incidence of 15° in accordance with JIS R 1679 (2007), and the return loss was measured for each frequency band of 33 to 50 GHz (WR-22), 50 to 75 GHz (WR-15), and 75 to 110 GHz (WR-10). The attenuation in the longitudinal direction was measured when the sample was placed parallel to the electric field direction, and the attenuation in the width direction was measured when the sample was placed parallel to the width direction. Note that this measurement method also measures values from 33 to 40 GHz, but the return loss in the frequency band from 33 GHz to less than 40 GHz was measured using the measurement data in (2-1). Next, the return loss and absorption frequency were calculated in the same manner as in (2-1).
[0067] (3) Return loss for linearly polarized waves As in (2), the return loss was measured from the stretching direction at 0° to 150° at 30° intervals. From the return loss spectrum at each angle obtained, the return loss at the peak top at each angle was calculated. The return loss at the peak top at the angle with the largest attenuation was taken as the return loss for linearly polarized waves.
[0068] (4) Stretching The samples were cut to a size of 100 mm x 100 mm and stretched to a stretch ratio of 1.3 to 2.5 times at a preheating and stretching temperature of 100°C for 1 minute and a stretching speed of 5% / sec using a film stretcher (Bruckner, KARO-IV) to obtain stretched samples of the specified thickness.
[0069] (5) Young's modulus (Ys) from static viscoelasticity test The sample was cut into a size of 1 cm x 20 cm along the longitudinal or transverse direction, and the Young's modulus was measured using an automatic film strength and elongation measuring device "Tensilon" (registered trademark) AMF / RTA-100 manufactured by Orientec Co., Ltd., at room temperature of 23°C, 5 cm between chucks, and a pulling speed of 300 mm / min. The measurement was performed according to the method described in JIS K-7161 (2014) and JIS K-7127 (1999). The measurement was performed five times in each of the longitudinal and transverse directions of each sample, and the average value was used as the Young's modulus (Ys).
[0070] (6)ΔTcg The samples were measured in accordance with JIS K-7121 (1987) and JIS K-7122 (1987) using a high-sensitivity differential scanning calorimeter "DSC6220" manufactured by Seiko Instruments Inc. as a measuring device and Muse standard analysis "Standard Analysis Ver9.0" for data analysis, as described below.
[0071] (6-1) Tg (1st Run) 5 mg of sample was weighed into a sample pan and heated from 25° C. to 290° C. at a heating rate of 20° C. / min, held at that state for 5 minutes, and then rapidly cooled to below 25° C. In the obtained differential scanning calorimetry chart, the glass transition temperature (Tg) was determined based on the method described in JIS K-7121 (2012) (determined from the point where a straight line equidistant in the vertical direction from the extended straight line of each baseline intersects with the curve of the step-like change in the glass transition).
[0072] (6-2)Tc Immediately after the first run measurement was completed, the temperature was raised from 25°C to 290°C at a heating rate of 20°C / min, and the state was maintained for 5 minutes, after which the temperature was lowered from 290°C to 25°C at a heating rate of 20°C / min. The crystallization temperature (Tc) was determined as the temperature at the top of the crystallization peak in the differential scanning calorimetry chart obtained during the temperature drop.
[0073] (6-3)ΔTcg The difference between the Tg and the Tc was defined as ΔTcg.
[0074] (7) Young's modulus (Yd) determined by dynamic viscoelasticity testing The sample was cut out from the center of the width direction to 7 cm x 1 cm in the longitudinal or transverse direction, and placed on a sample holder so that the measurement length was 2 cm. Using a Seiko Instruments Inc. DMS6100, the average storage modulus (Young's modulus) was measured in tension mode under the conditions of a temperature range of room temperature 20°C to 30°C, a displacement of 10 μm, a vibration frequency of 10 Hz, and a heating rate of 1°C / min. The measurement was performed according to the method described in JIS K-7244 (1998). Measurements were performed five times in each of the longitudinal and transverse directions of the sample, and the average value of the storage modulus (Young's modulus) was taken as Yd.
[0075] (8) Tensile stress / elongation at break The measurement was carried out in the same manner as in (5) except that the measurement was carried out at 90° C. The stress at 100% elongation was taken as the tensile stress, and the elongation at break was taken as the elongation at break.
[0076] (9) Electromagnetic wave absorption performance Considering the performance required for actual use in electromagnetic wave absorption applications, the electromagnetic wave absorption performance was evaluated based on the return loss before stretching according to the following criteria. Note that an evaluation result of B indicates practical performance, and an evaluation result of A indicates excellent absorption performance. A:20dB<return loss B:13dB<return loss≦20dB C: Return loss ≦13dB (10) Change in electromagnetic wave absorption performance The evaluation was based on the following criteria: Here, 5 / 6 stretching means stretching in one direction so that the thickness becomes 5 / 6, and 2 / 3 stretching is to be interpreted similarly. A: Satisfies "change in return loss is 5 dB or less after 5 / 6 extension" and "change in return loss is 10 dB or less after 2 / 3 extension." B: Either "change in return loss is 5 dB or less after 5 / 6 extension" or "change in return loss is 10 dB or less after 2 / 3 extension" is not satisfied. C: Neither of the conditions "change in return loss is 5 dB or less after 5 / 6 extension" nor "change in return loss is 10 dB or less after 2 / 3 extension" is satisfied.
[0077] (11) Presence or absence of polarization absorption properties If the difference between the return loss of linearly polarized waves and the return loss of non-polarized waves is 3 dB or more after 5 / 6 extension and 5 dB or more after 2 / 3 extension, it is determined that the polarized wave absorption characteristics are present. The return loss of linearly polarized waves and the return loss of non-polarized waves were measured using the methods (2) and (3) above.
[0078] (12) Formability (forming test) Molding was performed under the following conditions using a vacuum molding machine (Seiko Sangyo Co., Ltd. 300X). Heating was performed using an infrared heater, and the temperature was determined by attaching a thermo label to the sample. Molding tests were performed three times for each sample. The appearance after molding was visually checked and the following evaluations were performed. Heating time: 30 seconds Heating temperature: 110℃ Vacuum pump pressure: 0.17MPa Moulded shape: box shape, 5cm wide, 7.5cm long and 2cm deep.
[0079] (12-1) Tracking Ability A: All samples are in good contact with the edges and vertices and are wrinkle-free. B: One or two samples have air pockets around the edges or wrinkles near the vertices. C: All three times, there was space left on the edges or air remained near the vertices, causing wrinkles.
[0080] (12-2) Disadvantages A: None of the samples were torn, and there were no areas that were extremely thin or bent. B: One or two samples have tears near the edges or are extremely thin and warped. C: All three times there are tears near the edges or the paper has become extremely thin and warped.
[0081] (Ingredients used) Resin 1: Polyethylene terephthalate with an intrinsic viscosity (IV) of 0.78 Resin 2: Polybutylene terephthalate with IV 0.6 Resin 3: Resin 2 (50 parts by mass), dodecadione acid copolymerized polybutylene terephthalate (20 parts by mass), and polyethylene glycol having a molecular weight of 12,000 (10 parts by weight) are mixed in a twin-screw extruder and extruded into a gut shape, which is then cooled in a water tank and cut with a chip cutter. Resin 4: Resin 3 (60 parts by mass) and polycyclohexane terephthalate (30 parts by mass) were mixed in a twin-screw extruder and extruded into a gut shape, which was then cooled in a water tank and cut with a chip cutter. CB1: Ketjenblack particles with DBP oil absorption of 350 mL / 100 g and bulk density of 100 g / L Fe1: Carbonyl iron particles with Fe content of 97%, specific gravity of 1.49 g / mL, and average particle size (D50) of 3.5 μm CNT1: Multi-walled carbon nanotube particles with an average diameter of 10 nm and an average length of 1.5 μm Ti1: specific surface area 4m 2 / g, barium titanate particles with an average diameter of 0.3 μm.
[0082] (Examples 1 to 12, Examples 14 to 17, Comparative Examples 1 to 3) First, the resin for layer B was mixed and extruded in a twin-screw extruder in the form of a gut, cooled in a water tank, and cut with a chip cutter to obtain master pellets. The prepared resin for layer A and resin for layer B were each fed in pellet form into two twin-screw extruders, and both were melted at 270°C and mixed. The mixing conditions were a screw rotation speed of 0.7 relative to the discharge rate. Next, the mixture was joined in a multi-manifold type feed block with the number of layers shown in Table 1, and cast from a T-die into a cooled roll, forming a laminated sheet with 3 to 201 layers alternately stacked in the thickness direction with a layering ratio of 1.0. The evaluation results of each obtained laminated sheet are shown in Table 1. The thickness was adjusted by changing the discharge rate or line speed.
[0083] (Example 13) The composition of each layer is as shown in Table 1, and a laminate sheet was prepared in the same manner as described in the section "Examples 1 to 12, Examples 14 to 17, and Comparative Examples 1 to 3", and then the laminate sheet was heated to 95° C. with a heating roll and stretched to 1.5 times in the longitudinal direction, and then stretched to 1.5 times in a tenter at 100° C. The evaluation results of the obtained laminate sheet are shown in Table 1.
[0084] [Table 1] [Industrial Applicability]
[0085] According to the present invention, it is possible to provide a laminate sheet having excellent moldability while maintaining electromagnetic wave absorbing performance. Since the laminate sheet of the present invention has the above-mentioned excellent properties, it can be suitably used in electronic devices, transportation means, building materials, etc. [Explanation of symbols]
[0086] 1: Peak with the largest return loss 2: Return loss at the peak top with the largest return loss
Claims
1. A laminated sheet comprising an alternating laminate unit in which two different types of layers (layers A and B) are alternately laminated to form a total of five or more layers, and characterized in that, when the return loss of an electromagnetic wave is measured for each frequency and plotted with the return loss on the vertical axis and the frequency on the horizontal axis, the return loss at the peak top of the peak with the largest return loss is 5.0 dB or more, and the elongation at break at 90°C is more than 1% and not more than 2000%.
2. 2. The laminate sheet according to claim 1, wherein the difference (ΔTcg) between the crystallization temperature Tc and the glass transition temperature Tg is 50° C. or more and 200° C. or less, or the crystallization temperature Tc is not observable.
3. 3. The laminate sheet according to claim 1, wherein the stress at 100% elongation in a tensile test at 90°C is 10.0 MPa or less.
4. 4. The laminate sheet according to claim 1, wherein the change in peak top return loss before and after stretching to 5 / 6 of the thickness is 5 dB or less.
5. 5. The laminate sheet according to claim 1, wherein the change in peak top return loss before and after stretching to reduce the thickness to ⅔ is 10 dB or less.
6. 4. The laminate sheet according to claim 1, wherein the maximum change in peak top return loss is 5 dB or less when the return loss for linearly polarized waves is measured before and after the laminate sheet is stretched to a thickness of 5 / 6.
7. The laminate sheet according to any one of claims 1 to 3 or 6, wherein when the return loss for linearly polarized waves is measured before and after the laminate sheet is stretched to a thickness of 2 / 3, the maximum change in the return loss at the peak top is 10 dB or less.
8. The laminate sheet according to any one of claims 1 to 7, characterized in that the value obtained by dividing the reflection loss (dB) at the peak top by the thickness (µm) and multiplying the result by the wavelength (mm) at the peak top is 0.10 dB mm / µm or more and 2.00 dB mm / µm or less.
9. The laminate sheet according to any one of claims 1 to 8, wherein the Young's modulus (Ys) measured by a static viscoelasticity test is 1.0 GPa or more and 10 GPa or less, and the ratio (Ys / Yd) of the Young's modulus (Yd) measured by a dynamic viscoelasticity test is 0.5 or more.
10. The laminate sheet according to any one of claims 1 to 9, wherein the resin component contains at least one unit selected from the group consisting of a cycloalkane unit, a chain alkane unit having 5 or more carbon atoms, and a polyethylene glycol unit having a molecular weight of 20,000 or less in an amount of 1 mol% to 99 mol%.
11. 11. The laminate sheet according to claim 1, comprising 1% by mass or more and 100% by mass or less of a polyester in which at least one of a cycloalkane unit and a chain alkane unit having 5 or more carbon atoms is copolymerized.
12. A building material comprising the laminate sheet or a molded product of the laminate sheet according to any one of claims 1 to 11.
13. An electronic device comprising the laminate sheet or a molded product of the laminate sheet according to any one of claims 1 to 11.
14. A transportation system comprising the laminate sheet or a molded product of the laminate sheet according to any one of claims 1 to 11.
Citation Information
Patent Citations
Composite magnetic body and manufacture thereof
JP2000243615A
Electromagnetic wave absorption sheet and its manufacturing metod
JP2004039703A
Electromagnetic wave and sound wave absorber
JP2005109123A
Hard coat multilayered sheet, building window glass using it and flat panel display
JP2005254472A
Magnetic material sheet
JP2008004624A
Cited By
Electromagnetic wave absorption sheet
JP2025026546A