Fluorine-containing polymer, film, method for producing film, and organic photoelectron device
A fluoropolymer with controlled thermal properties addresses the instability in vapor deposition of fluororesins, ensuring stable and high-quality films for organic electroluminescent devices by maintaining consistent deposition conditions and film quality.
Patent Information
- Application Number
- JP2022503657
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-02-26
- Filing Date
- 2021-02-24
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-02-24
AI Technical Summary
The use of fluororesins in organic electroluminescent devices (EL devices) during vapor deposition leads to thermal decomposition, causing pressure increases in the vacuum chamber and instability in deposition conditions, which affects the quality and stability of the resulting films.
A fluoropolymer with specific properties, including a melting point of 200°C or higher, a thermogravimetric reduction rate below 400°C under controlled heating, and a narrow molecular weight distribution, is developed for stable vapor deposition, allowing for the formation of high-quality films.
The fluoropolymer ensures stable vapor deposition conditions, resulting in films with high heat resistance, transparency, and consistent quality, enhancing the performance of organic optoelectronic devices.
Smart Images

Figure 0007589734000005 
Figure 0007589734000006 
Figure 0007589734000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a fluorine-containing polymer, a film, a method for producing the film, and an organic optoelectronic device. [Background technology]
[0002] Conventionally, organic photoelectron elements (organic electroluminescence elements, hereinafter referred to as organic EL elements) have been known as self-luminous elements. The basic structure of an organic EL element is that multiple layers, such as a light-emitting layer, an electron transport layer, and a hole transport layer, are laminated between a pair of electrodes.
[0003] Fluororesins are often used as materials for the layers that make up organic electroluminescence devices, and are used for various purposes, such as as a low refractive index material for lowering the refractive index of layers and as a buffer for electrodes. For example, an organic EL element having an anode buffer layer made of a fluororesin is known (see Patent Document 1). In the organic EL element described in Patent Document 1, the anode buffer layer is formed by vapor deposition of the fluororesin. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Chinese Patent No. 100557852 Summary of the Invention [Problem to be solved by the invention]
[0005] In the examples of Patent Document 1, it is described that a fluororesin is evaporated under reduced pressure in a vacuum chamber. -3 The pressure in the chamber, which was 1 to 3 × 10 Pa, increased to 1 to 3 × 10 Pa at the end of film formation. -2The pressure inside the chamber is thought to increase as the fluororesin used is thermally decomposed under the deposition conditions, and the resulting low-molecular-weight decomposition products are vaporized. As described in Patent Document 1, it is expected that it will be difficult to ensure the desired deposition conditions if a fluororesin that decomposes thermally during deposition is used. Therefore, even if an organic EL element is obtained, there is a risk that the quality will be unstable, and improvements have been required.
[0006] The present invention has been made in view of the above circumstances, and has an object to provide a fluorine-containing polymer suitable for vapor deposition. Another object is to provide a film containing such a fluorine-containing polymer as a material. Another object is to provide a method for producing such a film, which allows such a film to be easily produced. Another object is to provide an organic optoelectronic device having such a film in its structure. [Means for solving the problem]
[0007] In order to solve the above problems, the present invention includes the following aspects. [1] A fluorine-containing polymer that satisfies the following (1) to (3): (1) The melting point is 200°C or higher. (2) 1×10 -3 (3) When heated at a rate of 2°C / min under a pressure of 1×10 Pa, the thermal weight loss rate reaches substantially 100% at 400°C or less. -3 When the temperature is increased at a rate of 2°C / min under a pressure of 10 Pa, the temperature range from the temperature at which the thermal weight loss rate becomes 10% to the temperature at which it becomes 90% is within 100°C. [2] Storage modulus at 25°C is 1×10 7 The change in storage modulus when cooled at a rate of 2°C / min is 1×10 6 The fluorine-containing polymer according to [1], wherein the temperature at which the temperature becomes less than Pa is 120° C. or higher. [3] The fluorine-containing polymer according to [1] or [2], which has a unit derived from a fluoroolefin. [4] The fluorine-containing polymer according to [3], which has at least a unit derived from tetrafluoroethylene. [5] The fluorine-containing polymer according to [3] or [4], which has a unit derived from a perfluoroalkyl vinyl ether. [6] The fluorine-containing polymer according to [5], wherein the perfluoroalkyl vinyl ether is perfluoropropyl vinyl ether.
[0008] [7] A film comprising the fluorine-containing polymer according to any one of [1] to [6] above and an organic semiconductor. [8] The film according to [7], wherein the proportion of the fluorine-containing polymer to the total of the fluorine-containing polymer and the organic semiconductor is 20 to 80% by volume. [9] The film according to [7] or [8], further comprising a dopant.
[10] The film according to any one of [1] to [9], which is a co-deposited film of the fluorine-containing polymer and the organic semiconductor.
[11] A method for producing a film, comprising a step of co-depositing the fluorine-containing polymer according to any one of the above [1] to [6] and an organic semiconductor.
[12] The method for producing a film according to
[11] , wherein a dopant is also co-deposited in the co-deposition step.
[0009]
[13] An organic optoelectronic device comprising the film according to any one of [7] to
[10] above.
[14] The organic optoelectronic device according to
[13] , comprising: a substrate; an anode provided on the substrate; a cathode facing the anode; an active layer disposed between the anode and the cathode; a hole transport layer disposed between the active layer and the anode; and a hole injection layer disposed between the hole transport layer and the anode, wherein at least one of the hole transport layer and the hole injection layer is the film.
[15] The organic optoelectronic device according to
[13] or
[14] , comprising: a substrate; an anode provided on the substrate; a cathode facing the anode; an active layer disposed between the anode and the cathode; an electron transport layer disposed between the active layer and the cathode; and an electron injection layer disposed between the electron transport layer and the cathode, wherein at least one of the electron transport layer and the electron injection layer is the film. Effect of the Invention
[0010] According to the present invention, it is possible to provide a fluorine-containing polymer suitable for vapor deposition. It is also possible to provide a film containing such a fluorine-containing polymer as a material. It is also possible to provide a method for producing such a film, which allows such a film to be easily produced. Furthermore, it is also possible to provide an organic photoelectron device having such a film in its structure. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic diagram illustrating the requirements (2) and (3) for the fluorine-containing polymer. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing the membrane of the first embodiment. [Diagram 3] FIG. 3 is a schematic diagram showing the steps for producing the membrane 10. [Figure 4] FIG. 4 is a schematic diagram showing the steps for producing the membrane 10. [Diagram 5] FIG. 5 is a schematic diagram showing the steps for producing the membrane 10. [Figure 6] FIG. 6 is a cross-sectional view showing an organic optoelectronic device (organic EL device) 100 according to a second embodiment of the present invention. [Figure 7] FIG. 7 is an explanatory diagram of an organic EL element 200 according to a third embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] In this specification, the term "unit" constituting a polymer means a portion derived from one monomer molecule (i.e., a monomer unit) that exists in the polymer and constitutes the polymer. Hereinafter, a unit derived from an individual monomer may be referred to by the name of the monomer followed by "unit."
[0013] As used herein, the "main chain" of a polymer refers to a carbon atom chain formed by addition polymerization of a monomer having a carbon-carbon unsaturated double bond, and composed of carbon atoms that constituted the carbon-carbon unsaturated double bond in the monomer.
[0014] In the present specification, the term "aliphatic ring" refers not only to a carbon ring structure whose ring skeleton is composed only of carbon atoms, but also to a heterocyclic ring structure whose ring skeleton contains an atom other than carbon atoms (heteroatom). Examples of the heteroatom include an oxygen atom, a nitrogen atom, and a sulfur atom.
[0015] [First embodiment] The fluoropolymer, membrane, and membrane production method according to the first embodiment of the present invention will be described below with reference to Figures 1 to 5. In all the following figures, the dimensions and ratios of the components are appropriately changed to make the figures easier to see.
[0016] (Fluorine-containing polymer) The fluoropolymer of the present embodiment satisfies the following requirements (1) to (3). Requirement (1) The melting point is 200°C or higher. Requirement (2) 1×10 -3 When the temperature is increased at a rate of 2°C / min under a pressure of 10 Pa, the thermal weight loss rate reaches substantially 100% at 400°C or lower. Requirement (3) 1×10 -3 When the temperature is increased at a rate of 2°C / min under a pressure of 10 Pa, the temperature range from the temperature at which the thermal weight loss rate becomes 10% to the temperature at which it becomes 90% is within 100°C.
[0017] A fluoropolymer satisfying the above requirements (1) to (3) has physical properties suitable for vapor deposition and can be suitably used to form a vapor-deposited film. The following explains each in order.
[0018] (Fluorine-containing polymer structure) The fluoropolymer of this embodiment is not particularly limited in terms of the units, so long as it is a polymer having high crystallinity and a melting point within a desired range.
[0019] The fluorine-containing polymer is preferably a polymer having units derived from a fluoroolefin, more specifically, the fluorine-containing polymer preferably has at least units derived from tetrafluoroethylene (TFE) (i.e., TFE units).
[0020] It is generally known that a fluoropolymer can have high crystallinity when it contains a high proportion of TFE units or units derived from chlorotrifluoroethylene (CTFE) (i.e., CTFE units). Therefore, the fluoropolymer of the present embodiment also preferably contains a high proportion of TFE units or CTFE units.
[0021] The ratio of TFE units and CTFE units to the entire fluoropolymer is preferably 50 mol% or more, more preferably 70 mol% or more, and even more preferably 90 mol% or more. When the fluoropolymer contains both TFE units and CTFE units, the sum of the ratio of TFE units and the ratio of CTFE units is preferably the above content or more. The upper limit of the content is 100 mol %.
[0022] The fluoropolymer of this embodiment may be a homopolymer of TFE or CTFE, or a copolymer of two or more monomers selected from the group consisting of TFE or CTFE and other monomers. The other monomer is not particularly limited as long as it is copolymerizable with TFE or CTFE. The other monomer may be a hydrocarbon monomer or a fluorine-containing monomer.
[0023] Examples of the hydrocarbon monomer as the other monomer include ethylene, propylene, styrene, and other hydrocarbon monomers. When a hydrocarbon-based monomer is used as the other monomer, the ratio of units derived from the other monomer to all units of the fluorine-containing polymer is preferably 50 mol % or less, more preferably 30 mol % or less, and even more preferably 10 mol % or less.
[0024] The other monomer is preferably a fluorine-containing monomer, since the refractive index of the resulting fluorine-containing polymer is relatively small. As the fluorine-containing monomer, a perfluoro compound is preferable. The fluorine-containing monomer as the other monomer may be a monomer which becomes a unit having an aliphatic ring structure in the main chain by polymerization, but is preferably not a monomer which brings about an aliphatic ring structure in the main chain of such a fluorine-containing polymer. A fluorine-containing polymer which does not have an aliphatic ring structure in the main chain has higher crystallinity than a fluorine-containing polymer which has an aliphatic ring structure in the main chain, and the melting point of the fluorine-containing polymer is easily controlled within a desired range. Examples of monomers which become units having an aliphatic ring structure in the main chain by polymerization include perfluorocyclic monoenes and perfluorodienes which can be cyclically polymerized, which will be described later. Examples of fluorine-containing monomers other than perfluoro compounds include trifluoroethylene (TrFE), vinylidene fluoride (VdF), 1,2-difluoroethylene, and 1-fluoroethylene.
[0025] Among the fluorine-containing monomers, examples of the perfluoro compound include the following perfluoroolefins, perfluoroalkyl vinyl ethers, perfluoro cyclic monoenes, and perfluorodienes capable of cyclopolymerization. Perfluoroolefin: Hexafluoropropene (HFP), etc. Perfluoroalkyl vinyl ether: perfluoromethyl vinyl ether (PMVE), perfluoroethyl vinyl ether (PEVE), perfluoropropyl vinyl ether (PPVE), etc. Perfluorocyclic monoenes: perfluoro(4-methoxy-1,3-dioxole), perfluoro(2,2-dimethyl-1,3-dioxole), perfluoro(4-methyl-2-methylene-1,3-dioxolane), etc. Cyclopolymerizable perfluorodienes: perfluoro(3-butenyl vinyl ether), etc.
[0026] Among them, the fluorine-containing polymer preferably has a perfluoroalkyl vinyl ether unit, and more preferably has a PPVE unit. The melting point of a fluoropolymer changes when the content of the PPVE unit changes. Specifically, when the content of the PPVE unit in the fluoropolymer increases, the melting point of the fluoropolymer tends to decrease.
[0027] The content of the PPVE unit in the fluoropolymer is preferably less than 14 mol %, more preferably 10 mol % or less. The content of the PPVE unit in the fluoropolymer is not particularly limited to an upper limit, but it is preferably more than 0 mol %, more preferably 1 mol % or more. The upper limit and the lower limit of the content of the PPVE unit in the fluoropolymer can be arbitrarily combined. For example, the content is preferably from 1 to 12 mol%.
[0028] The above-mentioned monomers are usually polymerized by radical polymerization using a radical polymerization initiator. In this case, the fluorine-containing polymer at the end of the polymerization is considered to have a structure at the end of the molecular chain (main chain) in which a fragment of the radical polymerization initiator used in the polymerization is added. In addition, when a chain transfer agent is used in the polymerization, the structure at the end of the molecular chain (main chain) may have a structure in which a fragment of the chain transfer agent is added. The above-mentioned terminal structure of the fluoropolymer may be converted to another structure. For example, by heat-treating the above-mentioned fluoropolymer at the end of the polymerization at 300° C. or more, the terminal structure of the main chain becomes —C(═O)—F, and the fluoropolymer becomes an acid fluoride.
[0029] By treating the acid fluoride with methanol, the structure of the terminal of the main chain becomes a methyl ester group. The methyl ester group can be converted from the highly reactive acid fluoride by a simple methanol treatment. Therefore, it is preferable because the stability of the obtained fluorine-containing polymer can be easily improved.
[0030] Furthermore, by subjecting the acid fluoride to a fluorination treatment, the structure of the terminal of the main chain becomes a trifluoromethyl group. As an example of the fluorination treatment, the treatment method described in paragraph 0040 of JP-A-11-152310 can be mentioned. The trifluoromethyl group is preferred because it has high heat resistance and the heat resistance of the obtained fluorine-containing polymer is easily improved. Furthermore, it is preferable that the fluorine-containing polymer has a terminal structure of the main chain which is a methyl ester group or a trifluoromethyl group, since the intermolecular interaction at the terminal of the main chain is small and the vapor deposition is facilitated. The above-mentioned structure of the main chain terminal can be confirmed by infrared spectroscopy.
[0031] (Requirement (1)) The fluoropolymer of the present embodiment is preferably crystalline. When the fluoropolymer has crystallinity, the melting point is likely to be 200° C. or higher. The melting point of the fluoropolymer of the present embodiment is preferably 215° C. or higher, more preferably 225° C. or higher, and even more preferably 240° C. or higher. Further, the melting point of the fluoropolymer of this embodiment is not particularly limited in its upper limit, but is preferably 350° C. or lower, more preferably 320° C. or lower, and even more preferably 300° C. or lower. The upper and lower limits of the melting point of the fluoropolymer can be combined in any desired manner. For example, the melting point of the fluoropolymer may be 200 to 350°C, 215 to 320°C, or 225 to 300°C.
[0032] In this embodiment, the melting point is a value measured using a differential scanning calorimeter (for example, DSC 204 F1 Phoenix manufactured by NETZSCH). 9 mg of the fluoropolymer is placed in a sample container, and the heat capacity is measured when the temperature is raised from -70°C to 350 at a rate of 10°C per minute, and the melting point is determined from the obtained melting peak.
[0033] (Requirement (2)) In this embodiment, the thermal weight loss rate is a value measured using a vacuum differential thermobalance (VPE-9000, manufactured by Advance Riko Co., Ltd.). -3 The weight loss rate (%) of the fluoropolymer relative to its initial weight (50 mg) is measured when the temperature is raised from room temperature to 500° C. at a rate of 2° C. per minute under a vacuum of 100 Pa.
[0034] The term "substantially" in requirement (2) means that in the above-mentioned method for measuring the rate of thermal weight loss, the thermal weight loss in the temperature range above 400°C is below the lower detection limit, and no thermal weight loss can be confirmed.
[0035] It can be said that the lower the temperature at which the above requirement (2) is satisfied, the lower the molecular weight (degree of polymerization) of the fluoropolymer of this embodiment. If an attempt is made to deposit a fluoropolymer that does not satisfy the above requirement (2) by heating it in a temperature range exceeding 400°C, the fluoropolymer may be thermally decomposed. In that case, the product of thermal decomposition may increase the internal pressure of the vacuum chamber used for deposition. If the internal pressure of the vacuum chamber increases in this way, the deposition conditions may become unstable, and the quality of the deposited film may become unstable. In addition, the partially pyrolyzed fluoropolymer may be mixed into the deposited film, damaging the quality of the deposited film.
[0036] On the other hand, when the fluoropolymer satisfying the above requirement (2) is used as a material for deposition under vacuum, it can be suitably deposited by heating at a temperature lower than 400° C. This allows deposition treatment under stable deposition conditions without the risk of the above-mentioned thermal decomposition.
[0037] The heat resistance of the fluoropolymer can be evaluated as follows, taking into consideration the change in the internal pressure of the vacuum chamber.
[0038] [Method for evaluating chamber pressure changes during deposition] 0.1 g of fluoropolymer was charged into the vacuum deposition machine, and the pressure in the chamber was increased to 10 -4 After reducing the pressure to below Pa, a fluorine-containing polymer is deposited to a thickness of 200 nm at a deposition rate of 0.1 nm / sec. During this process, the pressure inside the chamber is monitored and the maximum pressure during deposition is measured. A fluoropolymer having a chamber pressure increase rate calculated by the following formula of 2 times or less can be suitably deposited. Chamber pressure increase rate during deposition = Maximum pressure during deposition / Initial pressure before deposition
[0039] Fluorine-containing polymers with a rate of increase exceeding 2 times are prone to thermal decomposition and are therefore judged to be unsuitable for use in vapor deposition. Furthermore, when the fluoropolymer is thermally decomposed to such an extent that the chamber pressure increases by a factor of more than 10, the products produced by the thermal decomposition may cause the quality of the vapor-deposited film to be unstable.
[0040] The fluorine-containing polymer of this embodiment is 1×10 -3 It is preferable that the thermal weight loss rate when heated at a rate of 2° C. / min under a pressure of 100 Pa reaches substantially 100% at 350° C. or lower.
[0041] (Requirement (3)) The fluorine-containing polymer of this embodiment is 1×10 -3 When the temperature is increased at a rate of 2°C / min under a pressure of 10 Pa, the temperature range from the temperature at which the thermal weight loss rate becomes 10% to the temperature at which it becomes 90% is within 100°C.
[0042] It can be said that the narrower the temperature range in which the fluoropolymer of this embodiment satisfies the above requirement (3), the narrower the molecular weight distribution. If an attempt is made to produce a vapor-deposited film using a fluoropolymer that does not satisfy the above requirement (3), there will be a large difference between the molecular weight of the fluoropolymer deposited at the beginning of vapor deposition and the molecular weight of the fluoropolymer deposited at the end of vapor deposition, and the molecular weight of the fluoropolymer will vary in the thickness direction of the same vapor-deposited film, which may result in unstable physical properties of the vapor-deposited film. Furthermore, when vapor-deposited films are continuously produced under the same conditions, if a fluoropolymer not satisfying the above requirement (3) is used, the quality of the vapor-deposited films produced may vary from lot to lot. Thus, if a fluorine-containing polymer not satisfying the requirement (3) is used, the deposition conditions become unstable, and there is a risk that the quality of the deposited film will not be stable.
[0043] On the other hand, in the case of a fluoropolymer satisfying the above requirement (3), the difference between the molecular weight of the fluoropolymer deposited at the beginning of deposition and that of the fluoropolymer deposited at the end of deposition is small, and the change in the molecular weight of the fluoropolymer in the thickness direction of the deposited film is small. Therefore, the physical properties of the obtained deposited film tend to be stable. Furthermore, when vapor-deposited films are continuously produced under the same conditions, the variation in quality between lots of the vapor-deposited films produced can be suppressed. For these reasons, when a fluorine-containing polymer satisfying the requirement (3) is used, the quality of the vapor-deposited film tends to be stable.
[0044] The fluorine-containing polymer of this embodiment is 1×10 -3 When the temperature is increased at a rate of 2° C. / min under a pressure of 10 Pa, the temperature range from the temperature at which the thermal weight loss rate becomes 10% to the temperature at which it becomes 90% is preferably within 70° C.
[0045] Fig. 1 is a schematic diagram illustrating requirements (2) and (3), and is a graph showing the relationship between the measurement temperature and the thermal weight loss rate. The horizontal axis of Fig. 1 is the measurement temperature (unit: °C), and the vertical axis is the thermal weight loss rate (unit: %). In Fig. 1, the behavior of a fluoropolymer that satisfies requirements (2) and (3) is indicated by the symbol P, and the behavior of a fluoropolymer that does not satisfy requirements (2) and (3) is indicated by the symbol Px.
[0046] In FIG. 1, the graph P showing the behavior of the fluoropolymer of the present embodiment is a graph showing the behavior of the fluoropolymer at a temperature lower than 400° C. (T d100 ) the thermal weight loss rate reaches 100%. In contrast, in graph Px showing the behavior of a fluoropolymer not satisfying requirements (2) and (3), the thermal weight loss rate does not reach 100% at 400°C. In addition, in FIG. 1, a graph P showing the behavior of the fluoropolymer of the present embodiment is shown as T d90 -T d10 The value W is 100°C or less. As can be seen from FIG. 1, the fluoropolymer of the present embodiment is d10 and temperature T d90 It can be seen that a steep thermal weight loss occurs between
[0047] (Molecular weight fraction) A fluoropolymer satisfying the above requirements (2) and (3) can be obtained by molecular weight fractionation of a polymer. In the following description, the polymer to be subjected to molecular weight fractionation may be referred to as a "raw polymer." Examples of the molecular weight fractionation method include a method in which the molecular weight is fractionated by sublimation purification or supercritical extraction to prepare a polymer that satisfies the requirements (2) and (3).
[0048] (sublimation purification) Sublimation purification is a technique in which the target compound is separated and recovered as a solid by utilizing the precipitation temperature difference of compounds contained in the gaseous target compound after heating the target compound (raw polymer) under reduced pressure to sublimate or evaporate a part or all of the target compound. This type of sublimation purification can be performed using a sublimation purification device that has a feed section for feeding the target compound and a collection section for separating the target compound in the gaseous state according to its precipitation temperature and collecting it as a solid, and that can maintain a high degree of vacuum. The structure of the sublimation purification apparatus is not particularly limited, but for example, a so-called Mill-type sublimation purification apparatus consisting of a glass cooling tube, a flask-shaped glass container surrounding the cooling tube, and a vacuum exhaust device for reducing the pressure inside the glass container can be used. Also, as the sublimation purification apparatus, a glass tube-type sublimation purification apparatus including a cylindrical glass sublimation tube, a heating device for accommodating the sublimation tube inside and heating the sublimation tube, and a high vacuum exhaust device for reducing the pressure inside the sublimation tube can be used. Hereinafter, the sublimation purification of a fluoropolymer and the method of molecular weight fractionation by sublimation purification will be described taking a glass tube type sublimation purification apparatus as an example.
[0049] In the sublimation purification of fluoropolymers, the raw polymer is charged into the sublimation tube, and the pressure is reduced to, for example, 1×10 -3 After increasing the degree of vacuum in the sublimation tube to below 1 Pa, the feed section is heated using a heating device, which causes the fluorine-containing polymer contained in the raw polymer to sublimate or evaporate. In the sublimation tube, the region on the side of the feed section that is exhausted by the high vacuum exhaust device corresponds to the "collection section." The collection section is set at a temperature lower than the heating temperature of the feed section. The fluoropolymer sublimated or evaporated from the raw material polymer in the feed section precipitates and solidifies on the wall surface of the collection section, and is collected.
[0050] The collection temperature of the collection section corresponds to the temperature at which the fluoropolymer sublimes from a gas to a solid (precipitates), and corresponds to the molecular weight of the fluoropolymer. By providing a plurality of collection sections with different collection temperatures in the sublimation tube, the raw polymer can be fractionated into fluoropolymers with different molecular weights. Specifically, for example, when the feed section is heated to A°C and the collection section is heated to B°C and C°C from the side closer to the feed section (A>B>C), the collection section set at B°C collects a fluoropolymer in a molecular weight range that is in a gaseous state at A°C and a solid state at B°C. Similarly, the collection section set at C° C. collects a fluoropolymer in a molecular weight range which is gaseous at B° C. and solid at C° C. That is, the collection section set at C° C. collects, among the fluoropolymers contained in the raw material polymer, a fluoropolymer in the collection temperature range B° C.-C° C. which is gaseous at B° C. and solid at C° C.
[0051] The above-mentioned requirement (3) can be satisfied by controlling the collection temperature range as described above, for example, by collecting in a collection section having a collection temperature range of 100° C. The collected fluoropolymer is checked to see whether it satisfies requirement (3), and if it does not, the temperature conditions of the collection section are controlled to narrow the collection temperature range. In the collection section, the lower the set temperature of the fluoropolymer collected, the lower the concentration of fluoropolymers collected. -3 The temperature at which the thermal weight loss rate under a pressure of 100 Pa reaches 100% is low, that is, the molecular weight of the fluoropolymer is small.
[0052] The collection temperature range is preferably 100° C. or less, more preferably 70° C. or less, and even more preferably 40° C. or less. The smaller the collection temperature range, the less the fluctuation in the deposition conditions becomes, and the more easily a homogeneous phase-separated structure is formed in the film thickness direction.
[0053] As long as the molecular weight fractionated fluoropolymer satisfies the requirements (2) and (3), a plurality of fluoropolymers having different collection temperature ranges may be mixed.
[0054] (Supercritical extraction) Supercritical extraction is a technique for obtaining an extract by utilizing the high solubility and diffusivity of a supercritical fluid. For example, supercritical CO2 is used as the supercritical fluid, and a relatively low molecular weight fluorine-containing polymer is dissolved in the supercritical CO2 to obtain an extract. Furthermore, by using a fluorine-containing solvent as an additive (entrainer) for the supercritical fluid, the solubility of the fluorine-containing polymer in the supercritical fluid can be increased.
[0055] The fluorine-containing solvent used as the entrainer is not particularly limited. For example, the fluorinophilic parameter P F A fluorine-containing solvent having a fluorinophilic parameter P of 1 or more is preferred. F ) 30 μL of the fluorine-containing solvent is dropped into a two-phase system of 3 g of toluene and 3 g of perfluoromethylcyclohexane, mixed thoroughly, and allowed to stand overnight, and then the fluorine-containing solvent contained in the toluene and the fluorine-containing solvent contained in the perfluoromethylcyclohexane are measured by gas chromatography. The concentration (unit: mL / L) of the fluorine-containing solvent in the toluene is expressed as M P The concentration of the fluorine-containing solvent in the perfluoromethylcyclohexane (unit: mL / L) is M F When the above formula is used, the fluorine-philic parameter P is calculated by the following formula (A). F Let us assume that. P F =M F / M P …(A)
[0056] Examples of the fluorine-containing solvent used as an entrainer include the following compounds. 1,1,1,2,2,3,3,4,4,5,5,6,6-Tridecafluorohexane (AC-2000, manufactured by AGC) (P F =12) 1,1,1,2,2,3,3,4,4,5,5,6,6-Tridecafluorooctane (AC-6000, manufactured by AGC) (P F =5.6) Cytop CT-SOLV100E (AGC) (P F =8.2) Cytop CT-SOLV180 (AGC) (P F =∞) HFE7300 (manufactured by 3M) (P F =8.2) 1,1,1,2,2,3,4,5,5,5-Decafluoropentane (Vertre XF, manufactured by Chemours) (P F =3.7) 1H,1H,2H,2H-Perfluorooctanol (P F =1.1) 1,1,2,2-Tetrafluoroethyl-2,2,2-trifluoroethyl ether (AE-3000, manufactured by AGC) (P F =0.6) HCFC-225ca / HCFC-225cb(45 / 55)(P F =0.3) Perfluorobenzene (P F =0.3) Hexafluoro-2-propanol (P F =0.24) 1H,1H,7H-Perfluoroheptanol (P F =0.23) 1H,1H,5H-Perfluoropentanol (P F =0.1)
[0057] The extraction process can be carried out, for example, using supercritical CO2 under conditions of an extraction pressure of 7.4 MPa or higher and an extraction temperature of 31°C or higher. The extraction pressure is preferably 30 MPa or more, more preferably 50 MPa or more, and even more preferably 70 MPa or more. There is no particular limit to the upper limit of the extraction pressure, but it is preferably 100 MPa or less. The upper and lower limits of the extraction pressure can be combined in any way. The extraction temperature is preferably 40° C. or higher, and more preferably 80° C. or higher. The extraction temperature is preferably 300° C. or lower, more preferably 200° C. or lower, and even more preferably 100° C. or lower. The upper and lower limit values of the extraction temperature can be combined in any manner. Within the above range, the desired molecular weight fractionation of the fluoropolymer can be carried out efficiently.
[0058] (Other requirements) The fluoropolymer of the present embodiment preferably satisfies the following requirements (4) and (5). Requirement (4) Storage modulus at 25°C is 1 x 10 7 Pa or more. Requirement (5) When the fluoropolymer is cooled at a rate of 2°C / min, the storage modulus is 1×106 The temperature at which the pressure drops below 1 Pa is 120° C. or higher. When the fluoropolymer satisfies the above requirements (4) and (5), the heat resistance of the fluoropolymer is increased.
[0059] A fluoropolymer satisfying the above requirements (4) and (5) can be obtained, for example, by changing the content of PPVE units in the fluoropolymer. As the content of PPVE units increases, the storage modulus tends to decrease.
[0060] In this embodiment, the storage modulus is a value measured using a dynamic viscoelasticity measuring device (e.g., MCR502, manufactured by Anton Paar) and a heating furnace for viscoelasticity measuring devices (e.g., CTD450, manufactured by Anton Paar). Specifically, a sample (fluoropolymer) is heated to above its melting point, and then cooled at 2°C / min in a constant temperature reduction mode. Using the above measuring device, the storage modulus (G') is measured under conditions of a strain of 0.01% and a frequency of 1 Hz.
[0061] 2 is a schematic cross-sectional view showing the film of this embodiment. The film 10 shown in FIG. 2 is a co-deposition film of an organic semiconductor and a fluorine-containing polymer, and is formed on a substrate 50. In the film 10, the organic semiconductor and the fluorine-containing polymer are phase-separated, and the film 10 includes domains 51b of the organic semiconductor and domains 52b of the fluorine-containing polymer described above. The domains 51b and 52b are continuous in the film thickness direction. The size D of the domain 52b in the surface direction of the film 10 is, for example, about 10 nm to 20 nm. In the following description, the above-mentioned phase-separated structure of the film 10 may be referred to as a nano-domain structure.
[0062] As described above, the fluorine-containing polymer used in the present embodiment has a melting point of 200° C. or higher and is highly crystalline. Usually, when a film is formed using a material with high crystallinity, a film with high heat resistance is obtained. On the other hand, a film formed using a material with high crystallinity is likely to have high haze and low transparency because the crystallized portion scatters visible light. For this reason, it has been difficult to apply a film formed using a material with high crystallinity to an optoelectronic device or the like that requires transparency.
[0063] However, the film 10 has a nano-domain structure that is sufficiently small for visible light. Even if a part of the fluoropolymer contained in such a film 10 crystallizes, the size of the crystallized part is within the nano-domain structure. Therefore, the film 10 is less likely to scatter visible light and exhibits high transparency. Furthermore, the film 10 has high heat resistance due to the high crystallinity of the fluoropolymer, and therefore the film 10 can retain its nano-domain structure and maintain high transparency even when exposed to high temperatures.
[0064] The haze and heat resistance of the film 10 can be measured by the following method. [Preparation of samples for haze measurement] On a glass substrate, α-NPD and a fluoropolymer are co-deposited to form a 100 nm thick co-deposited film to obtain a sample for haze measurement. The total deposition rate of the two materials is 0.2 nm / sec. The deposition rate is adjusted to obtain the desired volume ratio of α-NPD to the fluoropolymer in the co-deposited film.
[0065] [Haze measurement] The haze is measured using a haze meter (Hazeguard K50-290, manufactured by Toyo Seiki Seisakusho). After measuring the initial haze of the haze measurement sample, heat the sample on a hot plate heated to 100°C for 1 hour. After returning the sample to room temperature, measure the haze again. Furthermore, heat the sample on a hot plate heated to 120°C for 1 hour, and measure the haze in the same manner.
[0066] The obtained haze is evaluated as follows. ○: Less than 0.2, △: 0.2 or more and less than 0.5 ×: 0.5 or more
[0067] The ratio of the fluorine-containing polymer to the total of the fluorine-containing polymer and the organic semiconductor constituting the film 10 is equal to the volume of the domains 52b to the entire film 10. The ratio of the domains 52b to the entire film 10 is preferably 20 to 80% by volume. When the ratio of the fluorine-containing polymer is 20% by volume or more, the film has a sufficiently low refractive index compared to an organic semiconductor film not having a fluorine-containing polymer. When the ratio of the fluorine-containing polymer is 80% by volume or less, the conductivity of the film 10 can be sufficiently ensured.
[0068] The refractive index of the film 10 can be measured by the following method using a sample prepared by the following method. [Preparation of samples for refractive index measurement] α-NPD and a fluoropolymer are co-deposited on a silicon substrate to form a 100 nm co-deposited film to obtain a sample for refractive index measurement. The total deposition rate of the two materials is 0.2 nm / sec. The deposition rate is adjusted to obtain the desired volume ratio of α-NPD and the fluoropolymer in the co-deposited film. [Refractive index measurement] Using a multi-angle spectroscopic ellipsometry (e.g., M-2000U manufactured by J.A. Woollam Co.), measurements are taken at a film on a silicon substrate, changing the angle of incidence of light in increments of 5 degrees in the range of 45 to 75 degrees. At each angle, the ellipsometry parameters Ψ and Δ are measured at approximately 1.6 nm intervals in the wavelength range of 450 to 800 nm. Using the measurement data, a fitting analysis is performed on the dielectric function of the organic semiconductor using the Cauchy model to obtain the refractive index of the evaporated film for light with a wavelength of 600 nm.
[0069] Any known organic semiconductor can be used, and an appropriate material can be selected depending on the function of the device including the film 10 of this embodiment. For example, examples of organic semiconductors include a hole injection material constituting a hole injection layer of an organic EL element, an electron injection material constituting an electron injection layer, a hole transport material constituting a hole transport layer, an electron transport material constituting an electron transport layer, and a host material or guest material constituting a light emitting layer.
[0070] Suitable examples of hole injection materials include aromatic amine derivatives, such as, but not limited to, α-NPD, TAPC, PDA, TPD, and m-MTDATA. [ka]
[0071] Examples of hole injection materials other than those mentioned above include the following semiconductor materials, organometallic complex materials, arylamine materials, polymer semiconductor materials, etc. In addition, the following are commercially available products. Semiconductor materials: metal oxides such as molybdenum oxide and tungsten oxide, and metal fluorides such as aluminum fluoride and magnesium fluoride Organometallic complex materials: copper phthalocyanine, etc. Arylamine materials: N,N'-diphenyl-N,N'-bis-[4-(phenyl-m-tolyl-amino)-phenyl]-biphenyl-4,4'-diamine (DNTPD), N,N'-di(1-naphthyl)-N,N'-diphenylbenzidine (NPB), 4,4',4"-tris(N,N-diphenylamino)triphenylamine (TDATA), dipyrazino[2,3-f:2',3'-h]quinoxaline-2,3,6,7,10,11-hexacarbonitrile (HAT-CN), 9,9',9"-triphenyl-9H,9'H,9"H-3,3':6',3"-tert-carbazole (Tris-PCz), 4,4',4"-tris(N,N-2-naphthylphenylamino)triphenylamine (2-TNATA), etc. Polymer semiconductor materials: polyaniline / dodecylbenzenesulfonic acid (PANI / DBSA), poly(3,4-ethylenedioxythiophene) / poly(4-styrenesulfonate) (PEDOT / PSS), polyaniline camphorsulfonic acid (PANI / CSA), or polyaniline / poly(4-styrenesulfonate) (PANI / PSS), etc. Commercially available products: N-(diphenyl-4-yl)-9,9-dimethyl-N-(4-(9-phenyl-9H-carbazoyl-3-yl)phenyl)-9H-fluoren-2-amine (hereinafter referred to as "HT211"), HTM081 (manufactured by Merck), HTM163 (manufactured by Merck), HTM222 (manufactured by Merck), NHT-5 (manufactured by NoValed), NHT-18 (manufactured by NoValed), NHT-49 (manufactured by NoValed), NHT-51 (manufactured by NoValed), NDP-2 (manufactured by NoValed), NDP-9 (manufactured by NoValed), etc.
[0072] The hole injection materials exemplified above are commercially available. These hole injection materials may be commercially available or may be synthetic products. The hole injection materials may be used alone or in combination of two or more.
[0073] Known materials can be used as the electron injection material. Specific examples include inorganic compounds such as LiF, Cs2CO3, and CsF, as well as the following Alq3, PBD, TAZ, BND, OXD-7, and 8-hydroxyquinolinolato-lithium (Liq), but are not limited thereto. In addition, commercially available products such as NDN-1 (manufactured by NoValed) and NDN-26 (manufactured by NoValed) can be used.
[0074] [ka]
[0075] Examples of the material for the hole transport layer (hole transport material) include, but are not limited to, the hole injection materials described above. For example, arylamine materials such as 4,4',4"-tri(9-carbazoyl)triphenylamine (TCTA), 2,2',7,7'-tetrakis(N,N-diphenylamino)-2,7-diamino-9,9'-spirobifluorene (Spiro-TAD), and 2,2',7,7'-tetrakis(N,N-di-p-methoxyphenylamino)-9,9'-spirobifluorene (Spiro-MeOTAD), other than those listed as the hole injection materials, can be used as the hole transport material.
[0076] Examples of hole transport materials other than those listed as the hole injection materials include triazole derivatives, oxadiazole derivatives, imidazole derivatives, pyrazoline derivatives, pyrazolone derivatives, phenylenediamine derivatives, arylamine derivatives, amino-substituted chalcone derivatives, oxazole derivatives, styrylanthracene derivatives, fluorenone derivatives, hydrazone derivatives, stilbene derivatives, silazane derivatives, etc. Among these, it is preferable to use porphyrin compounds, aromatic tertiary amine compounds and styrylamine compounds, in particular aromatic tertiary amine compounds. These hole transport materials may be commercially available products or synthetic products. The hole transport materials may be used alone or in combination of two or more kinds.
[0077] As the material of the electron transport layer (electron transport material), a known material can be used. For example, the electron transport material includes the above-mentioned electron injection material, but is not limited thereto. Examples of the electron transport material other than the above-mentioned electron injection material include 2,2',2''-(1,3,5-benzinetriyl)-tris(1-phenyl-1-H-benzimidazole) (TPBi), 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP), 2-(4-tert-butylphenyl)-5-(4-biphenylyl)-1,3,4-oxadiazole (t-Bu-PBD), and a silole derivative having a silole ring.
[0078] These electron transport materials may be commercially available products or synthetic products. The above electron transport materials may be used alone or in combination of two or more kinds.
[0079] The light-emitting layer may be formed from any of known materials, such as fluorescent materials, thermally activated delayed fluorescence (TADF) materials, and phosphorescent materials.
[0080] For example, materials for forming the light-emitting layer include, but are not limited to, light-emitting guest materials such as (E)-2-(2-(4-(dimethylamino)styryl)-6-methyl-4H-pyran-4-ylidene)malononitrile (DCM), 4-(dicyanomethylene)-2-methyl-6-julolidyl-9-enyl-4H-pyran (DCM2), Rubrene, Coumarin6, Ir(ppy)3, and (ppy)2Ir(acac); phosphorescent host materials such as 4,4'-bis(9H-carbazol-9-yl)biphenyl (CBP) and 3,3'-di(9H-carbazol-9-yl)-1,1'-biphenyl (mCBP); fluorescent host materials such as ADN and Alq3; and polymer materials such as polyphenylenevinylene (PPV) and MEH-PPV.
[0081] The material for forming the light-emitting layer may be used alone or in combination of two or more kinds. The material for forming the light-emitting layer is appropriately selected depending on the desired emission wavelength.
[0082] The organic semiconductor that is the material for forming the film 10 preferably has a molecular weight of 300 to 1000. The molecular weight of the organic semiconductor is more preferably 400 or more. Moreover, the molecular weight of the organic semiconductor is more preferably 900 or less. If the molecular weight of the organic semiconductor is 300 or more, the glass transition temperature (Tg) of the organic semiconductor is high, and the heat resistance of the organic semiconductor film is improved. If the molecular weight is 1000 or less, the vapor pressure of the organic semiconductor is high, and it is possible to deposit the organic semiconductor at a temperature below the thermal decomposition temperature. The upper limit and lower limit of the molecular weight of the organic semiconductor can be combined in any desired manner. That is, the molecular weight of the organic semiconductor may be 300-900, 400-1000, or 400-900. The molecular weight of the organic semiconductor can be determined by measurement using Time-of-Flight Secondary Ion Mass Spectrometry (TOF-SIMS).
[0083] The film 10 may further contain a dopant. Any known dopant can be used, and an appropriate material can be selected depending on the function of the device including the film 10 of the present embodiment. By containing a dopant, the film 10 can have an increased electrical conductivity. For example, dopants used as hole injection materials include TCNQ, F4-TCNQ, PPDN, TCNNQ, F6-TCNNQ, HAT-CN, HATNA, HATNA-Cl6, HATNA-F6, C 60 F 36 , F 16 Examples of the dopants include organic dopants such as CuPc, NDP-2 (manufactured by Novaled), and NDP-9 (manufactured by Novaled), and inorganic dopants such as MoO3, V2O5, WO3, ReO3, and CuI. Examples of dopants used as electron injection materials include 8-hydroxyquinolinolato-lithium (Liq), NDN-1 (manufactured by Novaled), and NDN-26 (manufactured by Novaled).
[0084] 3 to 5 are schematic diagrams showing the steps of producing the film 10 described above. First, as shown in Fig. 3, a substrate 50 on which a film 10 is to be formed is prepared. Such a substrate 50 is placed in a chamber 500 of a vacuum deposition apparatus, and an organic semiconductor 51a and a fluorine-containing polymer 52a are supplied from an organic semiconductor deposition source (crucible) 51 and a fluorine-containing polymer deposition source (crucible) 52, respectively, for co-deposition. Note that, although Fig. 3 shows that the organic semiconductor and the fluorine-containing polymer are deposited from separate deposition sources, they may be deposited from the same deposition source.
[0085] As the organic semiconductor 51a and the fluorine-containing polymer 52a, the organic semiconductor and the fluorine-containing polymer constituting the film 10 described above can be used, respectively. During co-deposition, deposition conditions are set so that the ratio of the fluorine-containing polymer to the total of the fluorine-containing polymer and the organic semiconductor in the co-deposition film formed on the substrate 50 is 20 to 80% by volume.
[0086] It is preferable that the organic semiconductor 51a does not decompose when heated during deposition. Whether the organic semiconductor does not decompose when heated during deposition can be determined by determining the weight loss rate of the organic semiconductor used by the following method.
[0087] (Judgment method) The measurement is performed using a vacuum differential thermobalance (Advance Riko Co., Ltd.: VPE-9000). 50 mg of the organic semiconductor is placed in a cell with an inner diameter of 7 mm, and the temperature is measured at 1 × 10 -3 Pa~1×10 -4 The weight loss rate (%) of the organic semiconductor was measured when the temperature was increased to 500°C at a rate of 2°C per minute under a vacuum of 100 Pa. The temperature at which the weight loss rate reached 50% (T d50 ) is required. Next, the weight loss rate of the organic semiconductor was measured by using a thermogravimetric differential thermal analyzer (Hitachi High-Tech Science Corporation: STA7200) when the temperature was raised to 450°C at a rate of 10°C per minute under a nitrogen flow. d50 The weight loss rate is calculated.
[0088] T d50 If the weight loss rate at normal pressure is 1% or less, then the weight loss rate at reduced pressure T d50 It is concluded that the weight loss in the organic semiconductor is due to sublimation, not thermal decomposition. Such an organic semiconductor does not decompose when heated during deposition, i.e., it is a material suitable for deposition. On the other hand, T d50 If the weight loss rate at normal pressure exceeds 1%, d50 The weight loss in the organic semiconductor is considered to be due to thermal decomposition. Since such an organic semiconductor decomposes when heated during deposition, it can be considered to be unsuitable for deposition.
[0089] As shown in FIG. 4, when an organic semiconductor and a fluorine-containing polymer are co-deposited, it is believed that the organic semiconductor and the fluorine-containing polymer undergo phase separation on the substrate, forming domains 51b of the organic semiconductor and domains 52b of the fluorine-containing polymer. The size (diameter) of the domains 52b of the fluorine-containing polymer is considered to fall within a certain numerical range with little variation depending on the relationship between the surface energy of the substrate 50 on which co-deposition is performed and the surface energy of the fluorine-containing polymer. That is, when the fluorine-containing polymer used is easy to spread on the surface of the substrate 50, the domains 52b are considered to be easy to spread widely, and when the fluorine-containing polymer is difficult to spread on the surface of the substrate 50, the diameter of the domains 52b is considered to be easy to become small.
[0090] 5, when the co-evaporation is continued, the organic semiconductor 51a sublimated from the deposition source 51 is energetically more stable than the domain 52b, and therefore is thought to deposit in the organic semiconductor domain 51b. Similarly, the fluorine-containing polymer 52a sublimated from the deposition source 52 is energetically more stable than the domain 51b, and therefore is thought to deposit in the fluorine-containing polymer domain 52b. As a result, domains 51b of the organic semiconductor that are continuous in the thickness direction of the co-deposited film and domains 52b of the fluorine-containing polymer that are continuous in the thickness direction of the co-deposited film are formed. When the co-deposited film is viewed from the normal direction of the substrate 50, the diameter of the domains 52b does not change significantly in the thickness direction of the co-deposited film and reflects the size of the initial domains 52b formed on the surface of the substrate 50. In this case, by using the above-mentioned fluorine-containing polymer, the molecular weight of the fluorine-containing polymer constituting the domain 52b is narrow, and the difference in physical properties between the initial stage and the final stage of deposition is small, so that the quality of the obtained film 10 is likely to be stable.
[0091] The membrane 10 is produced as described above. Here, when the film 10 is heated, the domains 52b become more likely to move due to heating, and adjacent domains 52b may coalesce with each other, resulting in the collapse of the nano-domain structure of the film 10. In contrast, when the fluorine-containing polymer used satisfies the above-mentioned requirements (4) and (5), the domains 52b are less likely to coalesce, resulting in a film 10 that is more likely to maintain the nano-domain structure.
[0092] According to the fluoropolymer having the above-mentioned constitution, it is possible to provide a fluoropolymer which has high heat resistance and is suitable for vapor deposition. Furthermore, the film having the above-mentioned structure has a low refractive index, high transparency, high heat resistance, and stable quality. Moreover, according to the method for producing a film having the above-mentioned configuration, such a film can be easily produced. In this embodiment, the film 10 is formed by co-evaporating the fluorine-containing polymer of this embodiment and the organic semiconductor, but the present invention is not limited to this. The film containing the fluorine-containing polymer of this embodiment and the organic semiconductor may be produced by a wet process such as coating.
[0093] [Second embodiment] 6 is a cross-sectional schematic diagram showing an organic optoelectronic device (organic EL device) 100 according to a second embodiment of the present invention. The organic EL device 100 has a structure in which a substrate 110, an anode 111, a hole injection layer 112, a hole transport layer 113, an emitting layer 114, an electron transport layer 115, an electron injection layer 116, and a cathode 117 are laminated in this order. The organic EL device 100 of this embodiment employs a top emission system in which light L generated in the emitting layer 114 is emitted to the outside via the cathode 117.
[0094] (substrate) The substrate 110 may or may not have optical transparency. The substrate 110 may be made of inorganic materials such as glass, quartz glass, silicon nitride, etc., or organic polymers (resins) such as polyimide resin, acrylic resin, polycarbonate resin, etc. Furthermore, as long as the insulating properties of the surface are ensured, a metal material may also be used as the substrate 110. The substrate 110 also includes various wirings and driving elements (not shown) that are electrically connected to the organic EL elements.
[0095] (anode) The anode 111 is formed on the substrate 110, and supplies holes to the hole transport layer 113. In addition, the anode 111 has light reflectivity that reflects light emitted from the light emitting layer 114.
[0096] The anode 111 can be made of a conductive metal oxide such as ITO (Indium Tin Oxide) or IZO (Indium Zinc Oxide). In order to impart light reflectivity to the anode 111, a reflective film made of a metal material is provided on the substrate 110 side of the anode 111. In other words, the anode 111 has a laminated structure of a layer made of a conductive metal oxide and the reflective film. The anode 111 may be made of silver.
[0097] The thickness of the anode 111 is not particularly limited, but is preferably 30 to 300 nm, and is, for example, 100 nm.
[0098] (Hole injection layer) The hole injection layer 112 is formed between the anode 111 and the hole transport layer 113. The hole injection layer 112 has a function of facilitating the injection of holes from the anode 111 to the hole transport layer 113. Note that the hole injection layer 112 does not necessarily have to be formed. The hole injection layer 112 can be formed using the hole injection materials described above. The thickness of the hole injection layer 112 is not particularly limited, but is preferably 1 to 100 nm, and is, for example, 5 nm.
[0099] (Hole transport layer) The hole transport layer 113 is formed on the hole injection layer 112. The hole transport layer 113 has a function of efficiently transporting holes injected from the anode 111 toward the light emitting layer 114. The hole transport layer 113 can be formed using the hole transport material described above. The hole transport layer 113 may be a single layer or may be a laminate of multiple layers of a hole transport material. When the hole transport layer 113 is a laminate of multiple layers of a hole transport material, the hole transport materials constituting each layer may be the same or different from each other.
[0100] The hole transport layer 113 has an absorption coefficient of 5000 cm in the wavelength range of 450 to 800 nm. -1 Preferably, it is less than 1000 cm -1 It is more preferable that the absorption band is equal to or less than 100 nm, and it is particularly preferable that the absorption band is not present in the above wavelength range. The absorption coefficient of each layer constituting the hole transport layer 113 is 5000 cm -1 When the light passes through a hole transport layer having a thickness of 100 nm once, 5% of the light is absorbed, assuming that the total amount of light before passing through is 100%. Inside the organic EL element, multiple interference of light causes accumulation of loss due to absorption of light when passing through the hole transport layer 113. Therefore, light absorption when passing through the hole transport layer is a factor that greatly reduces the light extraction efficiency. It is extremely important to use a hole transport layer with sufficiently low light absorption so as not to impair the luminous efficiency of the organic EL element. By not impairing the luminous efficiency of the organic EL element, the energy utilization efficiency is increased, and heat generation due to light absorption is suppressed, resulting in a longer element life.
[0101] The thickness of the hole transport layer 113 is not particularly limited, but is preferably 10 to 250 nm, and more preferably 20 to 150 nm.
[0102] (Light Emitting Layer) The light-emitting layer 114 is formed on the hole transport layer 113. In the light-emitting layer 114, holes injected from the anode 111 and electrons injected from the cathode 117 recombine to emit photons and emit light. The emission wavelength at that time is determined by the material from which the light-emitting layer 114 is formed. The light-emitting layer 114 corresponds to the "active layer" in the present invention. The light-emitting layer 114 can be formed using the above-mentioned materials for forming the light-emitting layer. The materials for forming the light-emitting layer may be used alone or in combination of two or more kinds, and are appropriately selected according to the desired emission wavelength. The thickness of the light-emitting layer 114 is not particularly limited, but is preferably 10 to 30 nm. The thickness of the light-emitting layer 114 is, for example, 15 nm.
[0103] (electron transport layer) The electron transport layer 115 is formed on the light emitting layer 114. The electron transport layer 115 has a function of efficiently transporting electrons injected from the cathode 117 toward the light emitting layer 114. The electron transport layer 115 can be formed using the electron transport materials described above. The thickness of the electron transport layer 115 is not particularly limited, but is preferably 30 to 80 nm, and is, for example, 60 nm.
[0104] (electron injection layer) The electron injection layer 116 is provided between the cathode 117 and the electron transport layer 115. The electron injection layer 116 has a function of facilitating the injection of electrons from the cathode 117 to the electron transport layer 115. The electron injection layer 116 can be formed from the above-mentioned electron injection materials. The electron injection layer 116 does not necessarily have to be formed. The thickness of the electron injection layer 116 is not particularly limited, but is preferably 0.5 to 2 nm, and is, for example, 1 nm.
[0105] (cathode) The cathode 117 is formed on the electron injection layer 116. The cathode 117 has a function of injecting electrons into the electron injection layer 116. A known material can be used to form the cathode 117. For example, a MgAg electrode or an Al electrode can be used as the material to form the cathode 117. A buffer layer such as LiF may be formed on the surface of the cathode 117. The cathode 117 is a semi-transparent film formed thin enough as a whole to reflect a part of the light emitted from the light-emitting layer 114 and transmit the rest. The thickness of the cathode 117 is not particularly limited, but is preferably 5 to 30 nm, and is, for example, 5 nm.
[0106] (Microcavity structure) In the organic EL element 100 of this embodiment, the anode 111 and the cathode 117 form an optical resonance structure (microcavity) that resonates light between the anode 111 and the cathode 117. Between the anode 111 and the cathode 117, light generated in the light-emitting layer 114 is repeatedly reflected, and light with a wavelength that matches the optical path length between the anode 111 and the cathode 117 resonates and is amplified. On the other hand, light with a wavelength that does not match the optical path length between the anode 111 and the cathode 117 is attenuated. The "optical path length" here is calculated using the wavelength of the desired light emitted outside the element and the refractive index of each layer at the wavelength of the desired light.
[0107] The optical path length between the anode 111 and the cathode 117 is set to, for example, an integer multiple of the central wavelength of the light L generated in the light-emitting layer 114. In this case, the light L emitted from the light-emitting layer 114 is amplified as it approaches the central wavelength and is attenuated as it deviates from the central wavelength, before being emitted to the outside of the organic EL element 100. In this way, the light L emitted from the organic EL element 100 has a narrow half-width of the emission spectrum and improved color purity.
[0108] The microcavity structure utilizes the resonance caused by the fixed-end reflection between the cathode and anode at both ends. Therefore, the desired microcavity structure can be formed when the optical path length from the light-emitting position to the anode is an integral multiple of 1 / 4 of the wavelength λ of the desired light to be emitted outside the element, and the optical path length from the light-emitting position to the cathode is an integral multiple of 1 / 4 of the wavelength λ of the desired light to be emitted outside the element.
[0109] The organic EL device 100 of this embodiment contains the above-mentioned fluorine-containing polymer in any one or more of the above-mentioned layers. The organic EL device 100 of this embodiment preferably contains the above-mentioned fluorine-containing polymer in at least one of the hole injection layer 112 and the hole transport layer 113. When the hole transport layer 113 is a laminate of layers of hole transport materials, at least one of the layers contains the above-mentioned fluorine-containing polymer. In addition, the organic EL device 100 of this embodiment preferably contains the above-mentioned fluorine-containing polymer in at least one of the electron transport layer 115 and the electron injection layer 116. When the electron transport layer 115 is a laminate of layers of electron transport materials, at least one of the layers contains the above-mentioned fluorine-containing polymer. In addition, in the organic EL device 100 of this embodiment, at least one of the hole injection layer 112 and the hole transport layer 113, and at least one of the electron transport layer 115 and the electron injection layer 116 preferably contain the above-mentioned fluorine-containing polymer.
[0110] Each layer containing the above-mentioned fluorine-containing polymer has a lower refractive index than a layer not containing the above-mentioned fluorine-containing polymer. Therefore, the organic EL element 100 of the present embodiment has improved light extraction efficiency and improved external quantum efficiency. As a result, the organic EL element 100 of the present embodiment can obtain the same amount of light emission as a conventional organic EL element with less input power compared to a conventional organic EL element not containing the above-mentioned fluorine-containing polymer. Moreover, each layer containing the above-mentioned fluorine-containing polymer has high heat resistance, so that the organic EL device 100 of this embodiment has high reliability.
[0111] The heat resistance of the organic EL element 100 can be evaluated by the following method. <Heat resistance rating 1> [Preparation of element 1 for conductivity evaluation] A glass substrate is used on which a 2 mm-wide strip of ITO (indium tin oxide) is formed. The substrate is ultrasonically cleaned using a neutral detergent, acetone, and isopropanol, and further cleaned by boiling in isopropanol, after which any deposits on the surface of the ITO film are removed by ozone treatment. After cleaning, the substrate was placed in a vacuum deposition machine and subjected to a pressure of 10 -4After reducing the pressure to below Pa, molybdenum trioxide is evaporated onto the substrate. The evaporation rate is 0.1 nm / sec, and a film of 5 nm is formed to produce a hole injection layer.
[0112] Next, α-NPD and a fluorine-containing polymer are co-deposited on the hole injection layer. The total deposition rate of the two materials is 0.2 nm / sec, and a film of 100 nm is formed to prepare a charge transport layer. The deposition rate is adjusted to obtain the desired volume ratio of α-NPD to the fluorine-containing polymer in the charge transport layer.
[0113] Next, aluminum is evaporated onto the charge transport layer in a strip shape with a width of 2 mm. The strip-shaped aluminum film is perpendicular to the ITO film when viewed from the vertical direction of the substrate. This results in a device with an area of 4 mm. 2 An element 1 for evaluating electrical conductivity (=ITO film 2 mm × aluminum film 2 mm) is obtained.
[0114] [Heat resistance evaluation of element 1] Using a source meter (Agilent Technologies: B1500A), a voltage was applied to the ITO of element 1 as the anode and the aluminum as the cathode, and the voltage was changed while measuring the current flowing through the element for each voltage. The current density (J) (unit: mA / cm) versus electric field (E) (unit: MV / cm) was calculated. 2 ) is required. The electric field (E) is the voltage value divided by 100 nm, which is the thickness of the charge transport layer, and the current density (J) is the current value divided by 4 mm 2 This is the value divided by .
[0115] Next, in an N2 atmosphere, the element 1 is heated on a hot plate at 80°C for 60 minutes. After returning the element 1 to room temperature, the current flowing through the element is measured again, and the relationship between the electric field (E) (unit: MV / cm) and the current density (J) (unit: mA / cm 2 ) is required. Next, the same element 1 is heated on a hot plate at 90°C for 60 minutes in a N2 atmosphere. After returning the element 1 to room temperature, the current flowing through the element is measured again, and the relationship between the electric field (E) (unit: MV / cm) and the current density (J) (unit: mA / cm 2 ) is required.
[0116] From the obtained results, the heat resistance of the element 1 is evaluated as follows. ×: After heating to 80℃, the current density of 0.4MV / cm is less than 90% of the initial value △: After heating to 90℃, the current density at 0.4MV / cm is less than 90% of the initial value. 〇: After heating to 90℃, the current density of 0.4MV / cm is 90% or more of the initial value
[0117] <Heat resistance rating 2> [Preparation of element 2 for conductivity evaluation] Element 2 for evaluating electrical conductivity is prepared in the same manner as in [Preparation of element 1 for evaluating electrical conductivity], except that HAT-CN is used instead of molybdenum trioxide and HT211 is used instead of α-NPD.
[0118] [Heat resistance evaluation of element 2] The same procedure as in [Evaluation of heat resistance of element 1] was repeated except that the heating temperatures were 100°C, 110°C, 120°C, and 130°C, and the heating times were 15 minutes each. The electric field (E) (unit: MV / cm) versus current density (J) (unit: mA / cm 2 ) is required. From the obtained results, the heat resistance of the element 2 is evaluated as follows. ×: After heating to 100℃, the current density of 0.4MV / cm is less than 90% of the initial value △: After heating to 110℃, the current density at 0.4MV / cm is less than 90% of the initial value. ○: After heating to 120℃, the current density at 0.4MV / cm is less than 90% of the initial value 〇〇: After heating to 130℃, the current density at 0.4MV / cm is less than 90% of the initial value XXX: After heating to 130℃, the current density of 0.4MV / cm is 90% or more of the initial value
[0119] In addition, the above-mentioned fluorine-containing polymer may be introduced into each layer as a co-deposited film co-deposited with the organic semiconductor constituting each layer during production. Specifically, for example, when the above-mentioned fluorine-containing polymer is to be contained in both the hole injection layer 112 and the hole transport layer 113, a co-deposited film (first film) may be formed by co-depositing a hole injection material and a fluorine-containing polymer, and then a co-deposited film (second film) may be formed by co-depositing a hole transport material and a fluorine-containing polymer.
[0120] According to the organic EL device 100 having the above-mentioned configuration, since at least one of the hole injection layer 112 and the hole transport layer 113 contains the above-mentioned fluorine-containing polymer, the external quantum efficiency is improved, resulting in an organic EL device with low power consumption.
[0121] [Third embodiment] FIG. 7 is an explanatory diagram of an organic EL element 200 according to a third embodiment of the present invention, and corresponds to FIG. The organic EL element 200 has a structure in which a substrate 210, an anode 211, a hole injection layer 112, a hole transport layer 113, an emitting layer 114, an electron transport layer 115, an electron injection layer 116, and a cathode 217 are laminated in this order. The organic EL element 200 of this embodiment employs a bottom emission system in which light L generated in the emitting layer 114 is emitted to the outside through the anode 211 and the substrate 210.
[0122] The substrate 210 is optically transparent. Materials that can be used to form the substrate 210 include inorganic materials such as glass, quartz glass, and silicon nitride, and organic polymers (resins) such as polyimide resin, acrylic resin, and polycarbonate resin. Also, composite materials formed by laminating or mixing the above materials can be used as long as they are optically transparent.
[0123] The anode 211 is formed on the substrate 210, and supplies holes to the hole transport layer 113. The anode 211 can be formed from a light-transmitting conductive metal oxide such as ITO or IZO.
[0124] The cathode 217 is formed on the electron injection layer 116. The cathode 217 has a function of injecting electrons into the electron injection layer 116. The cathode 217 also has a function of reflecting light L isotropically emitted from the light emitting layer 114 and directing the light toward the anode 211. The cathode 217 may be formed from a material such as MgAg, Ag, or Al. A buffer layer such as LiF may be formed on the surface of the cathode 217. The thickness of the cathode 217 is not particularly limited, but is preferably 30 to 300 nm, and is, for example, 100 nm.
[0125] In the organic EL element 200 having such a configuration, it is preferable that the above-mentioned fluorine-containing polymer is contained in any one or more of the above-mentioned layers, as in the organic EL element 100 shown in the second embodiment. In more detail, it is preferable that the organic EL element 200 contains the above-mentioned fluorine-containing polymer in at least one of the hole injection layer 112 and the hole transport layer 113. In addition, it is preferable that at least one of the electron transport layer 115 and the electron injection layer 116 of the organic EL device 200 contains the above-mentioned fluorine-containing polymer. Furthermore, in the organic EL device 200, at least one of the hole injection layer 112 and the hole transport layer 113, and at least one of the electron transport layer 115 and the electron injection layer 116 preferably contain the above-mentioned fluorine-containing polymer. This allows the organic EL element 200 to have improved light extraction efficiency compared to conventional organic EL elements that do not contain a fluorine-containing polymer.
[0126] The organic EL element 200 having the above-mentioned configuration also has improved external quantum efficiency and reduced power consumption because each layer contains the above-mentioned fluorine-containing polymer. Moreover, each layer containing the above-mentioned fluorine-containing polymer has high heat resistance, so that the organic EL element 200 of this embodiment has high reliability. The heat resistance of the organic EL element 200 can be evaluated in the same manner as the heat resistance of the organic EL element 100 described above. Other functional layers may be disposed between the layers of the organic EL element 100 or the organic EL element 200. For example, a hole blocking layer or an electron blocking layer may be disposed between the light-emitting layer and the charge transport layer, or an adjustment layer for forming the above-mentioned microcavity structure may be disposed.
[0127] Furthermore, a wavelength conversion layer including quantum dots may be disposed in the light emission direction in the organic EL element 100 or the organic EL element 200. By including such a wavelength conversion layer, an organic EL element with improved color purity of emitted light is obtained. In the organic EL element 100 or the organic EL element 200, quantum dots may be used as a material for forming the light-emitting layer 114. Quantum dots are nanoscale semiconductor crystals with unique optical properties that follow quantum mechanics. Quantum dots are usually single crystal particles with diameters of 2 to 10 nm. The band gap of quantum dots changes depending on the crystal size (=particle size), so the band gap can be adjusted by adjusting the particle size, thereby obtaining the desired emission wavelength.
[0128] As the quantum dots, colloidal quantum dots that can be dispersed in a solution can be used, and such colloidal quantum dots can be formed into a film by using a general wet coating technique. The type of quantum dots is not particularly limited, and perovskite quantum dots, carbon-based quantum dots, alloy-type quantum dots, core-shell type quantum dots, and core-type quantum dots can be used.
[0129] In addition, in the above-mentioned embodiment, an organic EL element has been described as an example of an organic optoelectronic element, but the organic optoelectronic element to which the film containing the fluorine-containing polymer of the present invention is applied is not limited to an organic EL element. The organic optoelectronic device of the present invention may be, for example, an organic semiconductor laser. A known configuration can be adopted for the organic semiconductor laser. By adopting the above-mentioned film containing the fluorine-containing polymer as any film made of an organic semiconductor constituting the organic semiconductor laser, an organic semiconductor laser with improved external quantum efficiency can be obtained. The organic optoelectronic device of the present invention may be, for example, a light receiving element such as a photosensor or a solar cell. The photosensor and the solar cell may have a known configuration. By employing the above-mentioned film containing a fluorine-containing polymer as either the film made of an organic semiconductor constituting the photosensor or the solar cell, it is possible to obtain a photosensor with improved detection performance and a solar cell with improved power generation efficiency.
[0130] Although the preferred embodiment of the present invention has been described above with reference to the accompanying drawings, the present invention is not limited to the above embodiment. The shapes and combinations of the components shown in the above embodiment are merely examples, and various modifications can be made based on design requirements, etc., without departing from the spirit of the present invention. EXAMPLES
[0131] The present invention will be described below with reference to examples, but the present invention is not limited to these examples.
[0132] <Evaluation method> In this embodiment, evaluation was performed by the following methods.
[0133] [Measurement of thermal weight loss rate of fluoropolymer under vacuum] The measurement was performed using a vacuum differential thermobalance (Advance Riko Co., Ltd.: VPE-9000). 50 mg of fluoropolymer was placed in a cell with an inner diameter of 7 mm, and the temperature was measured at 1 × 10 -3 The weight loss rate (%) of the fluoropolymer relative to the initial weight (50 mg) was measured when the temperature was raised from room temperature to 500° C. at a rate of 2° C. per minute under a vacuum of 100 Pa. The temperature at which the weight loss rate reaches 100% (T d100 ), the temperature at which the weight loss rate becomes 10% (T d10 ) and the temperature at which the weight loss rate reaches 90% (T d90 ) was sought.
[0134] [Melt point measurement] Measurement was performed using a differential scanning calorimeter (NETZSCH: DSC 204 F1 Phoenix). 9 mg of the fluoropolymer was placed in a sample container, and the heat capacity was measured when the temperature was raised from -70°C to 350 at a rate of 10°C per minute, and the melting point was calculated from the obtained melting peak.
[0135] [Measurement of storage modulus] In this embodiment, the storage modulus is a value measured using a dynamic viscoelasticity measuring device (MCR502, manufactured by Anton Paar) and a heating furnace for viscoelasticity measuring device (CTD450, manufactured by Anton Paar). Specifically, a sample (fluoropolymer) was heated to above its melting point, and then cooled at 2°C / min in a constant temperature-lowering mode. Using the above-mentioned measuring device, the storage modulus (G') was measured under conditions of a strain of 0.01% and a frequency of 1 Hz, and the G' and G' at 25°C were 1×10 6 The temperature at which the pressure drops below 1 Pa was determined.
[0136] <Synthesis of Fluorine-Containing Polymer> The fluorine-containing polymers used for the evaluation were synthesized as follows. [Synthesis Example 1] A jacketed polymerization tank (made of stainless steel) having an internal volume of 1.351 L was degassed, and 701 g of 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether (AE-3000, manufactured by AGC Corporation), 57 g of perfluoropropyl vinyl ether (PPVE), 108 g of tetrafluoroethylene (TFE), and 35.7 g of methanol were weighed and charged into the polymerization tank.
[0137] The temperature of the polymerization tank was maintained at 60° C., and 18.9 mL of a 0.53 mass % solution of t-butyl peroxypivalate (PBPV) (solvent: AE-3000) was charged to initiate polymerization. During the polymerization, the polymerization pressure decreased with the progress of the polymerization, so TFE was continuously introduced into the polymerization tank so that the polymerization pressure was kept almost constant. The polymerization pressure was maintained at 1.04±0.04 MPaG (gauge pressure). Note that "gauge pressure" is a relative pressure with atmospheric pressure being 0 MPaG, and refers to the difference from absolute pressure with a vacuum being zero.
[0138] The polymerization was terminated when the amount of TFE introduced reached 121 g, to obtain a fluoropolymer having a composition of PPVE units:TFE units=2:98 (mol %).
[0139] The resulting polymer was then heated in an oven at 330° C., immersed in methanol and heated in an oven at 75° C. for 40 hours to substitute the terminal groups with methyl ester groups, thereby obtaining a fluorine-containing polymer A.
[0140] 44 g of the obtained fluoropolymer A was charged into the raw material charging section of the above-mentioned glass tube type sublimation purification apparatus, and the inside of the collection section was heated to 3.0×10 -3 The pressure was reduced to 100 Pa. Then, the raw material supply section was gradually heated to 330° C. to sublimate the fluoropolymer A. In the sublimation purification apparatus, the collection section was heated at set temperatures of 310° C., 280° C., and 250° C. from the side closer to the supply section. Of this, the substance precipitated in the collection section set at a temperature of 280° C. was recovered to obtain 4 g of purified fluoropolymer A1.
[0141] [Synthesis Example 2] A fluoropolymer was obtained in the same manner as in Synthesis Example 1 except that 649 g of AE-3000, 152 g of PPVE, 109 g of TFE, 15.5 g of methanol, and 18.9 mL of a 0.79 mass % solution of PBPV (solvent: AE-3000) were used. The composition of the obtained fluoropolymer was PPVE units:TFE units=4:96 (mol %). Next, the terminal groups of the fluoropolymer were substituted with methyl ester groups under the same conditions as in Synthesis Example 1 to obtain fluoropolymer B.
[0142] Fluoropolymer B was sublimated in the same manner as in Synthesis Example 1, except that 20 g of fluoropolymer B was used. The substance precipitated in a collector set at a temperature of 250° C. was recovered to obtain 2 g of purified fluoropolymer B1.
[0143] Furthermore, 20 g of the obtained fluoropolymer B was placed in a pressure vessel of a supercritical extraction apparatus and subjected to supercritical extraction with carbon dioxide. After 0.2 g was extracted at an extraction temperature of 40°C, extraction pressure of 30 MPa, and carbon dioxide flow rate of 30 ml / min (condition 1), the extraction temperature was increased to 80°C and extraction pressure to 60 MPa, and AC-2000 (AGC) was used as an entrainer at a ratio of 10 volume% to carbon dioxide (condition 2), to obtain 1.4 g of extract. The extract obtained under the conditions 2 was designated as fluoropolymer B2.
[0144] [Synthesis Example 3] The fluoropolymer produced in the same manner as in Synthesis Example 2 was heated in an oven at 330°C, and then treated by the method described in paragraph
[0040] of JP-A-11-152310 to substitute the terminal groups of the fluoropolymer with -CF3 groups using fluorine gas, thereby obtaining a fluoropolymer C. The fluoropolymer C was sublimated in the same manner as in Synthesis Example 1, except that the raw material charging section was gradually heated to 360° C. The substances precipitated in the collection sections set at temperatures of 250° C. and 280° C. were recovered to obtain 6 g of purified fluoropolymer C1.
[0145] [Synthesis Example 4] A stainless steel autoclave with an internal volume of 1006 mL was charged with 57.9 g of PPVE, 767 g of AC2000 (AGC), 4.13 g of methanol, and 1.24 g of azobisisobutyronitrile (AIBN), and the contents were frozen and degassed with liquid nitrogen. After the autoclave was heated to 70°C, 48.4 g of TFE was introduced into the autoclave to initiate the polymerization reaction. As the polymerization proceeded, the pressure inside the autoclave decreased, so TFE was continuously fed and polymerization was continued while maintaining the temperature and pressure of the autoclave constant. Five hours after the start of polymerization, the autoclave was cooled to terminate the polymerization reaction, and the gas in the system was discharged to obtain a reaction solution.
[0146] The reaction solution was mixed with 800 g of methanol to precipitate the polymer dissolved in the reaction solution, and then the layers were separated to recover the lower layer in which the polymer was dispersed. The resulting polymer dispersion was dried with hot air at 80° C. for 16 hours, and then vacuum dried at 100° C. for 16 hours to obtain 19 g of a fluorine-containing polymer. The composition of the obtained fluoropolymer was PPVE units:TFE units=6:94 (mol %).
[0147] Next, the terminal groups of the fluoropolymer were substituted with methyl ester groups in the same manner as in Synthesis Example 1 to obtain fluoropolymer D. Fluorine-containing polymer D was sublimated in the same manner as in Synthesis Example 1. The substances precipitated in the collection sections set at temperatures of 250° C. and 280° C. were recovered to obtain 5 g of purified fluorine-containing polymer D1.
[0148] [Synthesis Example 5] A fluorine-containing polymer was obtained in the same manner as in Synthesis Example 4 except that 69.4 g of PPVE, 4.18 g of methanol and 1.26 g of AIBN were used. The composition of the obtained fluoropolymer was PPVE units:TFE units=8:92 (mol %).
[0149] Next, the terminal groups of the fluoropolymer were substituted with -CF3 groups under the same conditions as in Synthesis Example 3 to obtain a fluoropolymer E. The fluoropolymer E was sublimated in the same manner as in Synthesis Example 2 to obtain 4 g of a purified fluoropolymer E1.
[0150] [Synthesis Example 6] A fluorine-containing polymer was obtained in the same manner as in Synthesis Example 4 except that 78.9 g of PPVE, 4.23 g of methanol and 1.27 g of AIBN were used. The composition of the obtained fluoropolymer was PPVE units:TFE units=9:91 (mol %).
[0151] Next, the terminal groups of the fluoropolymer were substituted with methyl ester groups in the same manner as in Synthesis Example 1 to obtain fluoropolymer F. The fluoropolymer F was sublimated in the same manner as in Synthesis Example 1 to obtain 4 g of purified fluoropolymer F1.
[0152] [Synthesis Example 7] A fluorine-containing polymer was obtained in the same manner as in Synthesis Example 4 except that 85.9 g of PPVE, 4.27 g of methanol and 1.28 g of AIBN were used. The composition of the obtained fluoropolymer was PPVE units:TFE units=10:90 (mol %).
[0153] Next, the terminal groups of the fluoropolymer were substituted with -CF3 groups under the same conditions as in Synthesis Example 3 to obtain a fluoropolymer G. Fluoropolymer G was sublimated in the same manner as in Synthesis Example 3. Substances precipitated in collection sections set at temperatures of 250° C., 280° C. and 310° C. were recovered to obtain 6 g of purified fluoropolymer G1.
[0154] [Synthesis Example 8] A fluoropolymer was obtained in the same manner as in Synthesis example 4 except that 152.9 g of PPVE, 2.40 g of methanol, 1.15 g of AIBN and 56.3 g of TFE were used. The composition of the obtained fluoropolymer was PPVE units:TFE units=14:86 (mol %).
[0155] The obtained fluoropolymer was then heated in an oven at 330°C, immersed in methanol, and heated in an oven at 75°C for 40 hours to replace the terminal groups with methyl ester groups, thereby obtaining fluoropolymer H. The fluoropolymer H was sublimated in the same manner as in Synthesis Example 1 to obtain 4 g of purified fluoropolymer H1.
[0156] [Synthesis Example 9] 30 g of perfluoro(3-butenyl vinyl ether), 30 g of AC2000 (AGC), 0.5 g of methanol, and 0.44 g of diisopropyl peroxydicarbonate (IPP) were weighed and charged into a 50 ml glass reactor. After the inside of the reactor was replaced with high-purity nitrogen gas, the reactor was heated to 40° C. and polymerization was carried out for 24 hours. The resulting solution was desolvated under conditions of 666 Pa (absolute pressure) and 50° C. to obtain 28 g of a polymer.
[0157] The resulting polymer was then heated in an oven at 300° C., immersed in methanol, and heated in an oven at 75° C. for 20 hours to substitute the terminal groups with methyl ester groups, thereby obtaining a fluorine-containing polymer I. The fluoropolymer I was purified by sublimation in the same manner as in Synthesis Example 4 to obtain 4 g of purified fluoropolymer I1.
[0158] [Synthesis Example 10] A jacketed polymerization tank (made of stainless steel) with an internal volume of 1.351 L was degassed, and 331 g of R113 (1,1,2-trichloro-1,2,2-trifluoroethane, manufactured by AGC), 1.1 g of methanol, and 765 g of hexafluoropropene (HFP) were charged into the polymerization tank. Furthermore, TFE was charged into the polymerization tank to a temperature of 50° C. and a pressure of 1.34 MPaG. Next, 54.7 ml of a 1.5% by mass solution of bis(perfluorobutyryl)peroxide (solvent: R113) was charged to initiate polymerization.
[0159] As the polymerization proceeded, the pressure in the polymerization vessel decreased, so TFE was continuously charged to keep the polymerization pressure almost constant, which was maintained at 1.34 MPaG. A 1.5 mass% solution of bis(perfluorobutyryl)peroxide (solvent: R113) was intermittently charged into the polymerization tank, and the polymerization was terminated when 86 g of TFE was consumed, to obtain a fluorocopolymer J. The amount of TFE consumed was determined from the mass loss of the TFE gas cylinder.
[0160] The composition of the obtained fluoropolymer J was HFP units:TFE units=8:92 (mol %). The fluoropolymer J was sublimated in the same manner as in Synthesis Example 4 to obtain 4 g of purified fluoropolymer J1.
[0161] In addition, the following material, which is a copolymer of TFE and perfluoroalkyl vinyl ether (PFA), was used as a commercially available fluorine-containing polymer. Fluon PFA: AGC Fluon PFA P-63
[0162] The physical properties of the synthesized fluoropolymer were measured by the above-mentioned method. The measured physical properties are shown in Table 1. [Table 1]
[0163] As shown in Table 1, the fluororesins A1 to G1 and J1 satisfy the requirements (1) to (3) shown in the above-mentioned embodiment, but the fluoropolymers B, H and Fluon PFA do not satisfy the requirements (2) and (3), and the fluoropolymers I1, H1 and H do not satisfy the requirement (1). Since the fluoropolymer I1 is amorphous and has no crystallinity, the melting point was not detected.
[0164] The fluorine-containing polymers shown in Table 1 were used and the following evaluations 1 to 5 were carried out. <Evaluation 1: Change in chamber pressure during deposition> [Method for evaluating chamber pressure changes during deposition] 0.1 g of fluoropolymer was charged into the vacuum deposition machine, and the pressure in the chamber was increased to 10 -4 After reducing the pressure to below 1 Pa, a fluoropolymer film was formed at a deposition rate of 0.1 nm / sec to a thickness of 200 nm. The pressure in the chamber was monitored during this process, and the maximum pressure during deposition was measured. The measured value was used to calculate the pressure increase rate according to the following formula. Chamber pressure increase rate during deposition = Maximum pressure during deposition / Initial pressure before deposition Fluorine-containing polymers whose chamber pressure increase rate was 2 times or less were evaluated as "good," and fluorine-containing polymers whose chamber pressure increase rate was more than 2 times were evaluated as "poor."
[0165] <Evaluation 2: Refractive index> [Preparation of samples for refractive index measurement] On a silicon substrate, α-NPD, an organic semiconductor, and a fluoropolymer were co-deposited to form a 100 nm co-deposited film, to obtain a sample for refractive index measurement. The total deposition rate of the two materials was 0.2 nm / sec. The deposition rate was adjusted to obtain the desired volume ratio of α-NPD and the fluoropolymer in the co-deposited film.
[0166] [Refractive index measurement] Using a multi-angle spectroscopic ellipsometry (M-2000U manufactured by J.A. Woollam), measurements were performed on a film on a silicon substrate, changing the angle of incidence of light in increments of 5 degrees from 45 to 75 degrees. At each angle, the ellipsometry parameters Ψ and Δ were measured at approximately 1.6 nm intervals in the wavelength range of 450 to 800 nm. Using the above measurement data, a fitting analysis was performed on the dielectric function of the organic semiconductor using the Cauchy model to obtain the refractive index of the evaporated film for light with a wavelength of 600 nm.
[0167] <Rating 3: Haze> [Preparation of samples for haze measurement] On a glass substrate, α-NPD and a fluoropolymer were co-deposited to form a 100 nm co-deposited film, to obtain a sample for haze measurement. The total deposition rate of the two materials was 0.2 nm / sec. The deposition rate was adjusted to obtain a desired volume ratio of α-NPD and the fluoropolymer in the co-deposited film.
[0168] [Haze measurement] The haze was measured using a haze meter (Hazeguard K50-290, manufactured by Toyo Seiki Seisakusho). After measuring the initial haze of the haze measurement sample, the sample was heated on a hot plate heated to 100°C for 1 hour. After the sample was returned to room temperature, the haze was measured again. The sample was further heated on a hot plate heated to 120°C for 1 hour, and the haze was measured in the same manner.
[0169] The resulting haze was evaluated as follows. ○: Less than 0.2 △: 0.2 or more and less than 0.5 ×: 0.5 or more
[0170] <Rating 4: Heat resistance 1> [Preparation of element 1 for conductivity evaluation] A glass substrate on which an ITO (indium tin oxide) film was formed in a 2 mm wide band was used. The substrate was ultrasonically cleaned using a neutral detergent, acetone, and isopropanol, and further cleaned by boiling in isopropanol, and then treated with ozone to remove any deposits on the surface of the ITO film. After cleaning, the substrate was placed in a vacuum deposition machine and subjected to a pressure of 10 -4 After reducing the pressure to below Pa, molybdenum trioxide was evaporated onto the substrate. The evaporation rate was 0.1 nm / sec, and a film of 5 nm was formed to prepare a hole injection layer.
[0171] Next, α-NPD and a fluorine-containing polymer were co-deposited on the hole injection layer. The total deposition rate of the two materials was 0.2 nm / sec, and a film of 100 nm was formed to prepare a charge transport layer. The deposition rate was adjusted to obtain the desired volume ratio of α-NPD to the fluorine-containing polymer in the charge transport layer. Next, aluminum was evaporated onto the charge transport layer in a strip shape with a width of 2 mm. The strip-shaped aluminum film was perpendicular to the ITO film when viewed from the vertical direction of the substrate. This resulted in a device with an area of 4 mm. 2 An element 1 for evaluating electrical conductivity (=ITO film 2 mm × aluminum film 2 mm) was obtained.
[0172] [Heat resistance evaluation of element 1] Using a source meter (Agilent Technologies: B1500A), a voltage was applied to the ITO of element 1 as the anode and the aluminum as the cathode, and the voltage was changed while measuring the current flowing through the element for each voltage. The current density (J) (unit: mA / cm) versus electric field (E) (unit: MV / cm) was calculated. 2 ) was sought.
[0173] Next, the element 1 was heated on a hot plate at 80°C for 60 minutes in a N2 atmosphere. After returning the element 1 to room temperature, the current flowing through the element was measured again, and the relationship between the electric field (E) (unit: MV / cm) and the current density (J) (unit: mA / cm 2 ) was sought.
[0174] Next, the same element 1 was heated on a hot plate at 90°C for 60 minutes in a N2 atmosphere. After returning the element 1 to room temperature, the current flowing through the element was measured again, and the relationship between the electric field (E) (unit: MV / cm) and the current density (J) (unit: mA / cm 2 ) was sought.
[0175] From the obtained results, the heat resistance of the element 1 was evaluated as follows. ×: After heating to 80℃, the current density of 0.4MV / cm is less than 90% of the initial value △: After heating to 90℃, the current density at 0.4MV / cm is less than 90% of the initial value. 〇: After heating to 90℃, the current density of 0.4MV / cm is 90% or more of the initial value
[0176] <Rating 5: Heat resistance 2> [Preparation of element 2 for conductivity evaluation] Element 2 for evaluating electrical conductivity was prepared in the same manner as in [Preparation of element 1 for evaluating electrical conductivity], except that HAT-CN was used instead of molybdenum trioxide and HT211 was used instead of α-NPD.
[0177] [Heat resistance evaluation of element 2] The same procedure as in [Evaluation of heat resistance of element 1] was repeated except that the heating temperatures were 100°C, 110°C, 120°C, and 130°C, and the heating times were 15 minutes each. The electric field (E) (unit: MV / cm) versus current density (J) (unit: mA / cm 2 ) was sought.
[0178] From the obtained results, the heat resistance of the element 2 was evaluated as follows. ×: After heating to 100℃, the current density of 0.4MV / cm is less than 90% of the initial value △: After heating to 110℃, the current density at 0.4MV / cm is less than 90% of the initial value. ○: After heating to 120℃, the current density at 0.4MV / cm is less than 90% of the initial value 〇〇: After heating to 130℃, the current density at 0.4MV / cm is less than 90% of the initial value XXX: After heating to 130℃, the current density of 0.4MV / cm is 90% or more of the initial value
[0179] In the following Examples 1 to 18, specific evaluation details of the fluorine-containing polymer will be described.
[0180] [Example 1] The above-mentioned evaluations 1 to 3 and 5 were carried out using the fluoropolymer A1. In preparing the samples for evaluations 2, 3, and 5, the deposition rate in the co-deposition of the organic semiconductor and the fluorine-containing polymer was adjusted so that the volume ratio of the organic semiconductor to the fluorine-containing polymer was 50:50.
[0181] [Example 2] In preparing the sample, the deposition rate was adjusted and the volume ratio of the organic semiconductor to the fluorine-containing polymer was set to 80:20, and the evaluation was carried out in the same manner as in Example 1.
[0182] [Example 3] The sample was prepared by adjusting the deposition rate and setting the volume ratio of the organic semiconductor to the fluorine-containing polymer to 20:80, and the evaluation was carried out in the same manner as in Example 1.
[0183] [Example 4] The fluoropolymer B1 was used and the above-mentioned evaluations 1 to 5 were carried out. In preparing the samples for evaluations 2 to 5, the deposition rate in the co-deposition of the organic semiconductor and the fluorine-containing polymer was adjusted so that the volume ratio of the organic semiconductor to the fluorine-containing polymer was 50:50.
[0184] [Example 5] Evaluation was carried out in the same manner as in Example 1, except that B2 was used as the fluoropolymer. [Example 6] Evaluation was carried out in the same manner as in Example 1, except that C1 was used as the fluoropolymer. [Example 7] Evaluation was carried out in the same manner as in Example 4, except that D1 was used as the fluoropolymer. [Example 8] Evaluation was carried out in the same manner as in Example 1, except that E1 was used as the fluoropolymer. [Example 9] Evaluation was carried out in the same manner as in Example 1, except that F1 was used as the fluoropolymer.
[0185] [Example 10] Evaluation was carried out in the same manner as in Example 1, except that G1 was used as the fluoropolymer. [Example 11] Evaluation was carried out in the same manner as in Example 1, except that J1 was used as the fluoropolymer. [Example 12] Evaluation was carried out in the same manner as in Example 4, except that H1 was used as the fluoropolymer. [Example 13] Evaluation was carried out in the same manner as in Example 1, except that B was used as the fluoropolymer. [Example 14] Evaluation was carried out in the same manner as in Example 1, except that H was used as the fluoropolymer.
[0186] [Example 15] Evaluations 1 to 4 were carried out using the fluoropolymer I1. In preparing the samples for evaluations 2 to 4, the deposition rate in the co-deposition of the organic semiconductor and the fluorine-containing polymer was adjusted so that the volume ratio of the organic semiconductor to the fluorine-containing polymer was 50:50.
[0187] [Example 16] Fluon PFA, a commercially available fluorine-containing polymer, was used to evaluate Evaluation 1: Change in chamber pressure during deposition. Since the temperature rise in the chamber during deposition was extremely large in Evaluation 1, other evaluations requiring co-deposition were not performed.
[0188] [Example 17] As an example in which a fluorine-containing polymer was not used, a sample in which a single film of α-NPD was formed at a deposition rate of 0.1 nm / sec was used, and the above-mentioned evaluations 2 to 4 were carried out.
[0189] [Example 18] As an example of a sample not using a fluorine-containing polymer, evaluation 5 was carried out using a sample in which a single film of HT211 was formed at a deposition rate of 0.1 nm / sec.
[0190] Among the above Examples 1 to 18, Examples 1 to 11 correspond to the working examples, and Examples 12 to 18 correspond to the comparative examples. The results are shown in Table 2.
[0191] [Table 2]
[0192] As a result of the evaluation, it was found that in Examples 1 to 11, there was no increase in the pressure inside the chamber during deposition, and stable deposition was possible. It was also found that in Examples 1 to 11, an increase in haze was suppressed even when heated. Moreover, it was found that the elements 1 and 2 of Examples 1 to 11 were excellent in heat resistance. In contrast, in Examples 13, 14, and 16, an increase in the pressure inside the chamber during deposition was observed, and it was found that there was a risk of the deposition state becoming unstable. It was also found that the haze increased with heating in Examples 12, 14, 15, and 17. In Example 17, it is believed that the α-NPD melted by heating, and then crystallization proceeded, resulting in the generation of scattering sources. In Examples 12, 14, and 15, it is believed that the nanodomain structure of the co-evaporated film changed with heating, resulting in the generation of scattering sources inside the co-evaporated film. In addition, in Examples 12, 14, and 15, it was found that the heat resistance of elements 1 and 2 was low. From the above results, it was confirmed that the present invention is useful. The entire contents of the specification, claims, abstract and drawings of Japanese Patent Application No. 2020-030460, filed on February 26, 2020, are hereby incorporated by reference as the disclosure of the specification of the present invention. [Explanation of symbols]
[0193] 10...film, 50...substrate, 51, 52...evaporation source, 51a...organic semiconductor, 51b...(organic semiconductor) domain, 52a...fluorine-containing polymer, 52b...(fluorine-containing polymer) domain, 100, 200...organic EL element (organic photoelectron element), 110, 210...substrate, 111...anode, 112...hole injection layer, 113...hole transport layer, 114...light-emitting layer, 115...electron transport layer, 116...electron injection layer, 117, 217...cathode, 500...chamber
Claims
1. A fluorine-containing polymer that satisfies the following (1) to (3): (1) The melting point is 200°C or higher. (2) 1 x 10 -3 The thermal weight loss rate when the temperature is increased at a rate of 2° C. / min under a pressure of 100 Pa reaches substantially 100% at 400° C. or less. (3) 1 x 10 -3 When the temperature is increased at a rate of 2°C / min under a pressure of 10 Pa, the temperature range from the temperature at which the thermal weight loss rate becomes 10% to the temperature at which it becomes 90% is within 100°C.
2. Storage modulus at 25°C is 1 x 10 7 Pa or more, The change in storage modulus when the temperature is lowered at a rate of 2°C / min is 1 x 10 6 The fluoropolymer according to claim 1, wherein the temperature at which the viscosity becomes less than Pa is 120°C or higher.
3. The fluorine-containing polymer according to claim 1 or 2, which has units derived from a fluoroolefin.
4. The fluorine-containing polymer according to claim 3, which has at least a unit derived from tetrafluoroethylene.
5. The fluorine-containing polymer according to claim 3 or 4, which has a unit derived from a perfluoroalkyl vinyl ether.
6. The fluorine-containing polymer according to claim 5, wherein the perfluoroalkyl vinyl ether is perfluoropropyl vinyl ether.
7. A film comprising the fluorine-containing polymer according to any one of claims 1 to 6 and an organic semiconductor.
8. 8. The film according to claim 7, wherein the ratio of said fluorine-containing polymer to the total of said fluorine-containing polymer and said organic semiconductor is 20 to 80% by volume.
9. The film of claim 7 or 8, further comprising a dopant.
10. The film according to any one of claims 7 to 9, which is a co-deposited film of the fluorine-containing polymer and the organic semiconductor.
11. A method for producing a film, comprising a step of co-depositing the fluorine-containing polymer according to any one of claims 1 to 6 and an organic semiconductor.
12. The method for producing a film according to claim 11 , wherein a dopant is also co-deposited in the co-deposition step.
13. An organic optoelectronic device comprising the film according to any one of claims 7 to 10.
14. A substrate; an anode provided on the substrate; a cathode facing the anode; an active layer disposed between the anode and the cathode; a hole transport layer disposed between the active layer and the anode; a hole injection layer disposed between the hole transport layer and the anode; 14. The organic optoelectronic device of claim 13, wherein at least one of the hole transport layer and the hole injection layer is the film.
15. A substrate; an anode provided on the substrate; a cathode facing the anode; an active layer disposed between the anode and the cathode; an electron transport layer disposed between the active layer and the cathode; an electron injection layer disposed between the electron transport layer and the cathode; 15. The organic optoelectronic device according to claim 13, wherein at least one of the electron transport layer and the electron injection layer is the film.
Citation Information
Patent Citations
Organic EL device
CN100557852C
Water-repelling glass
JP1996239242A
Production of water repellent coating film
JP1997025559A
Thin film of oriented molecule
JP1999001593A
Non-aqueous polymerization of fluoromonomers