Manufacturing method of thick steel plate

Hot rolling thick steel plates with controlled temperature differences and rolling ratios effectively reduces void defects, enhancing internal quality and productivity while minimizing fracture risks.

JP7589785B2Active Publication Date: 2024-11-26JFE STEEL CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023194593
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-11-19
Filing Date
2023-11-15
Publication Date
2024-11-26
Estimated Expiration
2042-09-22

AI Technical Summary

Technical Problem

Thick steel plates face high risks of fractures such as ductile, brittle, and fatigue fractures due to void defects near the thickness center, and existing manufacturing methods are inefficient and costly, requiring expensive equipment.

Method used

A method involving hot rolling with specific temperature conditions (700°C at the center and a 100°C temperature difference between the surface and center) and a rolling reduction ratio of over 30% to reduce void defects to 0.5% or less, using a composition with controlled impurities.

Benefits of technology

Manufactures thick steel plates with excellent internal properties at low cost and high productivity without special equipment, reducing fracture risks and maintaining quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589785000001
    Figure 0007589785000001
  • Figure 0007589785000002
    Figure 0007589785000002
Patent Text Reader

Abstract

To provide a thick steel sheet which can be produced at low cost without requiring a special facility and has excellent inner quality characteristics.SOLUTION: A thick steel sheet has a predetermined component composition. The area ratio of void defects at the center position of the sheet thickness is 0.5% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a steel plate and a method for producing the same. [Background technology]

[0002] In recent years, structures have become larger in size in the fields of ships, line pipes, buildings, bridges, marine structures, wind power generators, construction and industrial machinery, pressure vessels, etc. Accordingly, the thickness of the steel plates used in the above fields has also increased.

[0003] As a technique relating to such a thick steel plate (hereinafter also referred to as thick steel plate) and a manufacturing method thereof, for example, Patent Document 1 discloses the following: "A hot forging method for steel material in which an axisymmetrical steel material is forged and stretched with an upper metal plate and a lower metal plate spread apart, the method being characterized by including a step of forming the cross-sectional shape of the steel material perpendicular to the forging direction into a rectangle or a substantially rectangle with a ratio of the long side length to the short side length of at least 1.4 between the start of forging and the end of forging." has been disclosed.

[0004] In Patent Document 2, "A slab forging method in which a slab is continuously pressed in the width direction and then in the thickness direction using an asymmetric anvil in which the widths of the upper and lower anvils are different. The above-mentioned width direction reduction is performed from one end of the slab in the longitudinal direction, and in this case, the amount of deviation of the end positions of the upper and lower anvils at the other end side of the slab in the longitudinal direction is ΔL, and the contact length of the upper and lower anvils that has the shorter contact length with the slab is B, the ratio ΔL / B of these is limited to 0.20 or less. has been disclosed.

[0005] In Patent Document 3, "A hot forging method for a slab, which comprises continuously applying reduction in the width direction and then the thickness direction to a slab produced by continuous casting using asymmetric anvils, The above-mentioned widthwise reduction of the slab is performed in two stages, with the slab being turned over between the first and second stages, and at least two reductions are performed in each stage. When reducing the slab in the width direction in each stage, an anvil having a width of 400 to 1200 mm is used as the short side anvil and anvil having a width of 800 to 1500 mm is used as the long side anvil. The reduction position of the short side anvil is shifted in the reduction phase so that the deviation (ΔL) between the slab feed allowance boundary at the first slab reduction and the center of the anvil contact length (B) at the next reduction satisfies ΔL≦0.20B. The reduction ratio in each of the width direction slab reductions is 4% or more, and The total reduction rate in the thickness direction of the slab shall be 10% or more. A method for hot forging a slab, comprising the steps of: has been disclosed.

[0006] Patent Document 4 states: In the manufacturing method of extra-thick steel plates, a slab cast by the continuous casting method is rolled to width in the rough rolling process, and then rolled to the product thickness in the finish rolling process, The method for producing an extra thick steel plate having excellent internal properties is characterized in that the finishing rolling step is performed by multiple passes at a rolling speed of 200 to 350 mm / sec. has been disclosed.

[0007] Patent Document 5 describes a slab "Immediately after cutting a continuous cast strand of aluminum killed steel with an aluminum content of 0.07% by weight or less into a predetermined length, the hot cast strand is hot charged into a blooming soaking furnace, soaked at a temperature of 1050 to 1150°C, and rolled into a slab such that the value of the shape ratio R according to the following formula is 0.5 or more. Next, the slab is subjected to a dehydrogenation treatment to reduce the diffusible hydrogen contained in the center of the slab to 1.2 ppm or less. The slab is then reheated to 950-1050°C and rolled into a plate with a required thickness of 50 mm or more. After the end of the rolling of the plate, accelerated cooling is performed from a temperature of Ar3 or a temperature not lower than 40°C therein to 500-350°C at a heat extraction rate of 15°C or more per minute. This is a method for producing high toughness thick steel plate with excellent internal quality by continuous casting, characterized by the sequential joining of the above. has been disclosed. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Japanese Patent Application Publication No. 58-167045 [Patent Document 2] Patent No. 6137080 [Patent Document 3] Patent No. 6156321 [Patent Document 4] Special Publication No. 6-69569 [Patent Document 5] Japanese Patent Application Publication No. 59-74220 Summary of the Invention [Problem to be solved by the invention]

[0009] However, due to the thickness of the steel plate, there is a high risk of fracture, such as ductile fracture, brittle fracture, and fatigue fracture. Therefore, there is a demand for a steel plate having excellent internal properties that reduces the risk of such fracture. However, the steel plate manufactured by the techniques of Patent Documents 1 to 5 may not be able to sufficiently reduce the risk of such fracture, and may not be able to obtain excellent internal properties.

[0010] In addition, the techniques of Patent Documents 1 to 3 involve hot forging of slabs. However, the manufacturing efficiency of hot forging is much lower than that of hot rolling. Therefore, there are problems in that the production capacity is low and the manufacturing cost is high.

[0011] The techniques of Patent Documents 4 and 5 apply hot rolling to slabs instead of hot forging, but require a large reduction in shape ratio. However, in order to apply a large reduction in shape ratio when the slab is still thick, it is necessary to increase the reduction amount per pass. This poses the problem of the need to introduce expensive rolling equipment with high load capacity and torque limits.

[0012] The present invention has been developed in view of the above-mentioned current situation, and has an object to provide a steel plate having excellent internal properties that can be manufactured at low cost (in other words, with high productivity) without requiring special equipment. Another object of the present invention is to provide a method for manufacturing the above-mentioned steel plate. [Means for solving the problem]

[0013] The present inventors have conducted extensive research to solve the above problems and have come to the following findings. Slabs, which are used to roll or forge thick steel plates, are generally manufactured by continuous casting or ingot casting. Therefore, the final solidification position is usually near the center of the slab's thickness. When molten steel solidifies, volume shrinkage occurs. Therefore, void defects inevitably occur near the center of the slab's thickness. These void defects become the starting point of fractures such as ductile fracture, brittle fracture, and fatigue fracture, and the more void defects there are, the higher the frequency of fractures. In order to reduce the occurrence of void defects near the center of the slab's thickness, it is effective to increase the amount of strain introduced near that position during hot rolling. However, the distribution of strain in the thickness direction introduced into the slab by hot rolling is greatest near the surface of the slab that is in contact with the rolling rolls, and becomes smaller the closer to the center of the thickness. Therefore, the amount of strain is smallest at the center of the slab's thickness, and the ability to compress void defects is also the lowest.

[0014] Therefore, the present inventors have conducted various studies in order to increase the amount of strain in the vicinity of the center position of the thickness of a slab during hot rolling without using special equipment. As a result, the present inventors have made the following discoveries. By applying a rolling process that sets the temperature difference between the surface and the center of thickness at a certain level, the deformation resistance near the surface of the slab is increased relative to the center of thickness, reducing the amount of strain applied near the surface of the slab. This reduction in strain near the surface of the slab has the effect of increasing the amount of strain applied near the center of thickness. In addition, by reducing the slab while maintaining the temperature at the center of the plate thickness at a certain level or higher, specifically at 700°C or higher, void defects can be closed by rolling strain and the slab can be compressed by metal bonding more effectively.

[0015] Based on the above findings, the inventors further conducted research and discovered that the occurrence of void defects near the center position of the slab's thickness can be significantly reduced by increasing the reduction ratio in rolling passes that satisfy the following (a) and (b): (a) Temperature at the center of the slab: 700°C or higher (b) Temperature difference between the surface of the slab and the center of the plate thickness: 100°C or more

[0016] Furthermore, the present inventors have further investigated and obtained the following findings. By keeping the area ratio of void defects at the center of thickness of thick steel plate to 0.5% or less, excellent internal quality characteristics can be obtained with a sufficiently reduced risk of fracture. In order to keep the area ratio of void defects at the center of thickness of a steel plate to 0.5% or less, it is effective to set the total reduction rate in the hot rolling process in the rolling passes that satisfy the above (a) and (b) to more than 30%. The present invention was completed based on the above findings and through further investigation.

[0017] That is, the gist and configuration of the present invention are as follows.

[0018] [1] In mass percent, C: 0.03 to 0.18%, Si: 0.03 to 0.70%, Mn: 0.30-2.50%, P: 0.030% or less, S: 0.0200% or less, Al: 0.001 to 0.100%, O: 0.0100% or less and N: 0.0100% or less and the balance being Fe and unavoidable impurities, A thick steel plate having an area ratio of void defects at the center of the plate thickness of 0.5% or less.

[0019] [2] The composition further comprises, in mass%, Cu: 2.00% or less, Ni: 2.50% or less, Cr: 1.50% or less, Mo: 1.00% or less Nb: 0.100% or less, Ti: 0.100% or less, V: 0.30% or less, B: 0.0100% or less, W: 0.50% or less, Ca: 0.0200% or less, Mg: 0.0200% or less and REM: 0.0500% or less The steel plate according to [1] above, comprising one or more selected from the group consisting of:

[0020] [3] A method for producing a steel plate according to the above [1] or [2], A preparation step of preparing a slab having the component composition described in [1] or [2] above; A hot rolling process for hot rolling the slab; The hot rolling step has a total rolling reduction of more than 30% in rolling passes that satisfy the following (a) and (b): (a) Temperature at the center of the slab: 700°C or higher (b) Temperature difference between the surface of the slab and the center of the plate thickness: 100°C or more Effect of the Invention

[0021] According to the present invention, it is possible to obtain a thick steel plate having excellent internal properties, which can be produced at low cost without requiring special equipment. The steel plate of the present invention is not particularly limited in its application, and can be used in a wide range of fields in which steel plates are generally used, such as ships, line pipes, buildings, bridges, marine structures, wind turbines, construction and industrial machinery, and pressure vessels. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The steel plate of the present invention will be described based on the following embodiments. First, the composition of the steel plate according to one embodiment of the present invention will be described. Note that the unit of the content of elements in the composition is "mass%", and hereinafter, unless otherwise specified, it will be simply indicated as "%".

[0023] C: 0.03 to 0.18% C is an element that can most inexpensively improve the strength of steel. C also contributes to strengthening the austenite grain boundaries. If the C content is less than 0.03%, the grain boundary strength of austenite decreases, and hot cracking of the slab occurs. This significantly reduces manufacturability. Furthermore, sufficient strength cannot be obtained. On the other hand, if the C content exceeds 0.18%, weldability decreases. Furthermore, toughness also decreases. Therefore, the C content is set to 0.03 to 0.18%. The C content is preferably 0.05% or more. Furthermore, the C content is preferably 0.17% or less.

[0024] Silicon: 0.03 to 0.70% Silicon is an element effective for deoxidization. If the silicon content is less than 0.03%, sufficient effect cannot be obtained. However, if the silicon content exceeds 0.70%, weldability decreases. Therefore, the silicon content is set to 0.03 to 0.70%. The silicon content is preferably 0.04% or more. The silicon content is preferably 0.60% or less.

[0025] Mn: 0.30-2.50% Mn is an element that improves the hardenability and strength of steel at low cost. From the viewpoint of obtaining such effects, the Mn content is set to 0.30% or more. On the other hand, if the Mn content exceeds 2.50%, the weldability decreases. Therefore, the Mn content is set to 0.30 to 2.50%. The Mn content is preferably 0.50% or more. Also, the Mn content is preferably 2.20% or less.

[0026] P:0.030% or less P is an element that has a large effect of embrittling grain boundaries. Therefore, if a large amount of P is contained, the toughness of the steel decreases. Therefore, the P content is set to 0.030% or less. The P content is preferably 0.025% or less. On the other hand, since the less P, the better, the lower limit of the P content is not particularly limited and may be 0%. However, P is an element that is inevitably contained in steel as an impurity, and excessively low P content leads to increased refining time and increased costs. Therefore, the P content is preferably 0.001% or more.

[0027] S: 0.0200% or less S reduces the toughness of steel. Therefore, the S content is set to 0.0200% or less. The S content is preferably 0.0100% or less. On the other hand, since the less S, the better, the lower limit of the S content is not particularly limited and may be 0%. However, S is an element that is inevitably contained in steel as an impurity, and excessive reduction in S content leads to increased refining time and increased costs. Therefore, the S content is preferably 0.0001% or more.

[0028] Al: 0.001 to 0.100% Al is an element effective for deoxidization. Also, Al is an element that has the effect of forming nitrides and reducing the austenite grain size. In order to obtain such an effect, the Al content is set to 0.001% or more. On the other hand, if the Al content exceeds 0.100%, the cleanliness of the steel decreases. As a result, the ductility and toughness decrease. Therefore, the Al content is set to 0.001 to 0.100%. The Al content is preferably 0.005% or more. Also, the Al content is preferably 0.080% or less.

[0029] O: 0.0100% or less O is an element that reduces ductility and toughness. Therefore, the O content is set to 0.0100% or less. On the other hand, since the less O, the better, the lower limit of the O content is not particularly limited and may be 0%. However, O is an element that is inevitably contained in steel as an impurity, and excessive reduction of O content leads to an increase in refining time and an increase in costs. Therefore, the O content is preferably 0.0005% or more.

[0030] N: 0.0100% or less N is an element that reduces ductility and toughness. Therefore, the N content is set to 0.0100% or less. On the other hand, since the less N, the better, the lower limit of the N content is not particularly limited and may be 0%. However, since N is an element that is inevitably contained in steel as an impurity, industrially it may be more than 0%. However, excessive reduction in N content leads to an increase in refining time and an increase in costs. Therefore, the N content is preferably 0.0005% or more.

[0031] The basic component composition of the thick steel plate according to one embodiment of the present invention has been described above. However, from the viewpoint of further improving the strength and weldability (such as the toughness and weldability of the welded portion), one or more of the following optional added elements may be appropriately contained. Cu: 2.00% or less, Ni: 2.50% or less, Cr: 1.50% or less, Mo: 1.00% or less Nb: 0.100% or less, Ti: 0.100% or less, V: 0.30% or less, B: 0.0100% or less, W: 0.50% or less, Ca: 0.0200% or less, Mg: 0.0200% or less and REM: 0.0500% or less

[0032] Cu:2.00% or less Cu is an element that improves the strength of steel without significantly deteriorating toughness. However, if the Cu content exceeds 2.00%, hot cracking due to the Cu-enriched layer formed just below the scale becomes a problem. Therefore, when Cu is contained, the Cu content is preferably 2.00% or less. The Cu content is more preferably 0.01% or more. The Cu content is more preferably 1.50% or less.

[0033] Ni: 2.50% or less Ni is an element that improves the hardenability of steel. Ni is also an element that has the effect of improving toughness. However, if the Ni content exceeds 2.50%, an increase in manufacturing costs becomes a problem. Therefore, when Ni is contained, the Ni content is preferably 2.50% or less. The Ni content is more preferably 0.01% or more. The Ni content is more preferably 2.00% or less.

[0034] Cr:1.50% or less Cr is an element that improves the hardenability of steel, thereby improving the strength of the steel. However, if the Cr content exceeds 1.50%, the weldability decreases. Therefore, when Cr is contained, the Cr content is preferably 1.50% or less. The Cr content is more preferably 0.01% or more. The Cr content is more preferably 1.20% or less.

[0035] Mo: 1.00% or less Mo is an element that improves the hardenability of steel, thereby improving the strength of the steel. However, if the Mo content exceeds 1.00%, the weldability decreases. Therefore, when Mo is contained, the Mo content is preferably 1.00% or less. The Mo content is more preferably 0.01% or more. The Mo content is more preferably 0.80% or less.

[0036] Nb: 0.100% or less Nb is an element that suppresses recrystallization when strain is applied to the austenite structure by solid solution Nb and finely precipitated NbC. Nb is also an element that has the effect of raising the temperature of the non-recrystallization temperature range. However, if the Nb content exceeds 0.100%, the weldability decreases. Therefore, when Nb is contained, the Nb content is preferably 0.100% or less. The Nb content is more preferably 0.001% or more, and further preferably 0.005% or more. The Nb content is more preferably 0.075% or less, and further preferably 0.050% or less.

[0037] Ti:0.100% or less Ti is an element that has the effect of pinning the movement of grain boundaries by precipitating as TiN and suppressing grain growth. However, if the Ti content exceeds 0.100%, the cleanliness of the steel decreases. As a result, the ductility and toughness decrease. Therefore, when Ti is contained, the Ti content is preferably 0.100% or less. The Ti content is more preferably 0.001% or more. The Ti content is more preferably 0.080% or less.

[0038] V: 0.30% or less V is an element that improves the hardenability of steel and generates carbonitrides to improve the strength of steel. However, if the V content exceeds 0.30%, the weldability decreases. Therefore, when V is contained, the V content is preferably 0.30% or less. The V content is more preferably 0.01% or more. The V content is more preferably 0.25% or less.

[0039] B: 0.0100% or less B is an element that improves the hardenability of steel, thereby improving the strength of the steel. However, if the B content exceeds 0.0100%, the weldability decreases. Therefore, when B is contained, the B content is preferably 0.0100% or less. The B content is more preferably 0.0001% or more. Moreover, the B content is more preferably 0.0070% or less.

[0040] W: 0.50% or less W is an element that improves the hardenability of steel, thereby improving the strength of the steel. However, if the W content exceeds 0.50%, the weldability decreases. Therefore, when W is contained, the W content is preferably 0.50% or less. The W content is more preferably 0.01% or more. The W content is more preferably 0.40% or less.

[0041] Ca:0.0200% or less Ca is an element that improves weldability by forming oxysulfides that are highly stable at high temperatures. However, if the Ca content exceeds 0.0200%, the cleanliness of the steel decreases, and the toughness of the steel decreases. Therefore, when Ca is contained, the Ca content is preferably 0.0200% or less. The Ca content is more preferably 0.0001% or more. The Ca content is more preferably 0.0180% or less.

[0042] Mg: 0.0200% or less Mg is an element that improves weldability by forming oxysulfides that are highly stable at high temperatures. However, if the Mg content exceeds 0.0200%, the effect of adding Mg becomes saturated and an effect commensurate with the content cannot be expected, which is economically disadvantageous. Therefore, when Mg is added, the Mg content is preferably 0.0200% or less. The Mg content is more preferably 0.0001% or more. The Mg content is more preferably 0.0180% or less.

[0043] REM: 0.0500% or less REM (rare earth metal) is an element that improves weldability by forming oxysulfides that are highly stable at high temperatures. However, if the REM content exceeds 0.0500%, the effect of adding REM becomes saturated and an effect commensurate with the content cannot be expected, which is economically disadvantageous. Therefore, when REM is contained, the REM content is preferably 0.0500% or less. The REM content is more preferably 0.0001% or more. The REM content is more preferably 0.0450% or less.

[0044] The balance other than the above elements in the composition of the steel plate according to one embodiment of the present invention is Fe and inevitable impurities. Note that, when the content of any of the above-mentioned optional added elements is less than the respective preferable lower limit, the element is treated as an inevitable impurity.

[0045] In addition, in a thick steel plate according to one embodiment of the present invention, it is extremely important that the area ratio of void defects at the center position of the plate thickness is 0.5% or less.

[0046] Area ratio of void defects at the center of plate thickness: 0.5% or less Void defects inside a thick steel plate are the starting point of fractures such as ductile fracture, brittle fracture, and fatigue fracture. In particular, if a large number of void defects remain at the center of the thickness of the thick steel plate, specifically, if the area ratio of void defects at the center of the thickness exceeds 0.5%, the frequency of such fractures increases, and a thick steel plate with excellent internal properties cannot be obtained. Therefore, the area ratio of void defects at the center of the thickness is set to 0.5% or less. The area ratio of void defects at the center of the thickness is preferably 0.3% or less. The lower limit of the area ratio of void defects at the center of the thickness is not particularly limited, and may be 0%.

[0047] Here, the area ratio of void defects at the center of the plate thickness is measured according to the procedure described in the Examples below. In addition, excellent internal quality properties means that the reduction ratio in the plate thickness direction of the thick steel plate measured by a tensile test conforming to ASTM A370 (2010) is 35% or more. The detailed test conditions are as described in the procedure described in the [Plate thickness direction tensile test] in the Examples below.

[0048] The thickness of the thick steel plate according to one embodiment of the present invention is preferably 30 to 240 mm. The thickness of the thick steel plate according to one embodiment of the present invention is more preferably 50 mm or more, and further preferably 101 mm or more. The thickness of the thick steel plate according to one embodiment of the present invention is more preferably 230 mm or less.

[0049] Next, a method for manufacturing a steel plate according to one embodiment of the present invention will be described. A method for manufacturing a steel plate according to one embodiment of the present invention includes the steps of: A preparation step of preparing a slab (steel material) having the above-mentioned composition; A hot rolling process for hot rolling the slab; The total reduction rate in the hot rolling passes that satisfy the following (a) and (b) is more than 30%. (a) Temperature at the center of the slab: 700°C or higher (b) Temperature difference between the surface of the slab and the center of the plate thickness: 100°C or more This makes it possible to suitably manufacture the steel plate according to the embodiment of the present invention described above. Each step will now be described.

[0050] The surface temperature of the slab can be measured, for example, by a radiation thermometer. The temperature at the center of the thickness of the slab can be measured, for example, by attaching a thermocouple to the center of the thickness of the slab, or by calculating the temperature distribution in the cross section of the slab by heat transfer analysis and correcting the result by the surface temperature of the slab. Hereinafter, unless otherwise specified, the temperatures of the slab and steel plate refer to the surface temperature. For convenience, the material being rolled during the hot rolling process will be referred to as a slab rather than a steel plate (hot-rolled steel plate or thick steel plate).

[0051] [Preparation process] In the preparation step, a slab having the above-mentioned composition is prepared. The preparation method is not limited. For example, molten steel is produced by a known melting method such as a converter, an electric furnace, or a vacuum melting furnace. Optionally, secondary refining such as ladle refining may be performed. Then, the produced molten steel is turned into a slab by, for example, a continuous casting method or an ingot casting method, to prepare a slab having the above-mentioned composition. Note that each condition may be in accordance with a conventional method.

[0052] [Hot rolling process] Next, the slab prepared in the preparation step is heated as necessary and hot-rolled to form a thick steel plate (hot-rolled steel plate). At this time, it is extremely important that the following conditions are satisfied.

[0053] Total reduction in rolling passes that satisfy (a) and (b) (hereinafter also referred to as rolling passes under specified conditions): More than 30% (a) Temperature at the center of the slab: 700°C or higher (b) Temperature difference between the surface of the slab and the center of the plate thickness: 100°C or more In order to close the void defects present near the center of the thickness of the slab and bond the slab by metal bonding, it is effective to apply strain when the temperature at the center of the thickness of the slab is 700°C or higher. In order to increase the amount of strain applied near the center of the thickness of the slab, it is necessary to perform rolling in a state where the temperature difference between the surface of the slab and the center of the thickness of the slab is 100°C or higher. From the viewpoint of ensuring the amount of strain required for closing and bonding the void defects present near the center of the thickness of the slab, the total reduction rate in the rolling passes under the specified conditions is more than 30%. The total reduction rate in the rolling passes under the specified conditions is preferably 40% or more. The upper limit of the total reduction rate in the rolling passes under the specified conditions is not particularly limited, but it is preferable that the total reduction rate in the rolling passes under the specified conditions is 65% or less.

[0054] The total reduction rate in rolling passes under predetermined conditions is calculated by the following formula (1). r t =100×{(t i1 -t f1 ) / t i1 +(t i2 -t f2 ) / t i2 +(t i3 -t f3 ) / t i3 +···+(t iN -t fN ) / t iN} ···(1) Where: r t is the total reduction rate (%) in a rolling pass under given conditions tiN is the slab thickness (mm) at the start of rolling in the Nth rolling pass among the rolling passes under the specified conditions, t fN is the slab thickness (mm) at the end of the Nth rolling pass among the rolling passes under the specified conditions, N is the number of rolling passes under the specified conditions.

[0055] Whether or not the temperature conditions specified in (a) and (b) above are satisfied is determined based on the surface temperature of the slab and the temperature at the center of the plate thickness at the start of the rolling pass.

[0056] The method for adjusting the temperature difference between the surface of the slab and the center of the thickness is not particularly limited. For example, the temperature difference between the surface of the slab and the center of the thickness can be adjusted to the above range by forcibly cooling the surface of the slab with air or water.

[0057] Conditions other than those mentioned above are not limited and may be those according to conventional methods. For example, the slab heating temperature is preferably 950 to 1300°C. The total number of rolling passes in hot rolling is preferably 5 to 60 passes. N (the number of rolling passes under predetermined conditions) is preferably 5 to 50 passes. The hot rolling reduction ratio (=[slab thickness (mm) at the start of hot rolling (start of first rolling pass)] / [steel sheet thickness (mm) obtained after the end of hot rolling (end of final rolling pass)]) is preferably 1.6 to 16. The finish rolling end temperature (exit temperature of the final pass) is preferably 650 to 1000°C.

[0058] After the hot rolling process, an optional cooling treatment may be performed. In addition, an optional heat treatment such as quenching, annealing, tempering, etc. The cooling treatment conditions and heat treatment conditions are not particularly limited and may be in accordance with the usual methods. EXAMPLES

[0059] Molten steel having the composition shown in Table 1 was melted, and slabs with a thickness of 260 to 600 mm were prepared by continuous casting, ingot casting, etc. Note that blanks in the element columns in Table 1 indicate that the element was not intentionally added, and include not only cases where the element was not contained (0%), but also cases where the element was unavoidably contained.

[0060] Next, the prepared slab was hot-rolled under the conditions shown in Table 2 to obtain a thick steel plate having a thickness (mm) shown in Table 2. The reduction ratio of the hot rolling was in the range of 2.5 to 3.5, and N (the number of rolling passes under the specified conditions) was 5 to 37 passes. The surface temperature of the slab was measured using a radiation thermometer, and the temperature at the center of the thickness of the slab was measured using a thermocouple. The temperature difference between the surface of the slab and the center of the thickness was adjusted by forcibly cooling the surface of the slab with air or water. Conditions other than those mentioned above were in accordance with conventional methods.

[0061] For each of the thick steel plates thus obtained, the area ratio of void defects at the center position of the plate thickness was measured in the following manner. The measurement results are shown in Table 2.

[0062] [Measurement of area ratio of void defects at the center of plate thickness] From each of the obtained thick steel plates, a sample was taken from the center position in the longitudinal direction (rolling direction) of the thick steel plate, covering the entire width of the thick steel plate, so that the cross section of the thick steel plate in the width direction (direction perpendicular to rolling) at the center position of the plate thickness of the thick steel plate was the evaluation surface. Next, each obtained sample was mirror-polished with an alumina buff finish. Next, the evaluation area of ​​each sample was set to the plate thickness direction: plate thickness center position ±3 mm × width direction: full plate width, and the area ratio of void defects in the evaluation area was measured by image analysis. The measured value was then taken as the area ratio of void defects at the center position of the plate thickness.

[0063] Further, for each of the obtained steel plates, a tensile test in the plate thickness direction was carried out as described below to evaluate the internal quality properties. The evaluation results are shown in Table 2.

[0064] [Tensile test in the thickness direction] A tensile test piece was taken from each of the obtained thick steel plates at the center position in the longitudinal direction (rolling direction) of the thick steel plate so that the longitudinal direction of the tensile test piece was parallel to the plate thickness direction of the thick steel plate. Here, the tensile test piece was taken so that the longitudinal center position of the tensile test piece was the plate thickness center position (plate thickness 1 / 2 position) of the thick steel plate. In addition, the tensile test piece was taken over the entire plate width with a sampling pitch of 100 mm in the plate width direction. The shape of the tensile test piece was ASTM A770 (2007) Type 3 shape. Next, a tensile test based on ASTM A370 (2010) was performed using each of the taken tensile test pieces to measure the reduction ratio. Then, the minimum value of the reduction ratios measured for each tensile test piece taken over the entire plate width of the thick steel plate was taken as the reduction ratio of the thick steel plate. Then, when the value was 35% or more, it was evaluated that excellent internal quality properties were obtained.

[0065] [Table 1]

[0066] [Table 2]

[0067] As shown in Table 2, all of the steel plates according to the present invention had excellent internal properties. In addition, all of the steel plates according to the present invention could be manufactured using ordinary hot rolling equipment, and could be manufactured at low cost (with high productivity) without requiring special equipment.

[0068] On the other hand, none of the comparative steel plates had sufficient internal properties.

Claims

1. In mass percent, C: 0.03-0.18%, Si: 0.03-0.70%, Mn: 0.30-2.50%, P: 0.030% or less, S: 0.0200% or less, Al: 0.001-0.100%, O: 0.0100% or less and N: 0.0100% or less and the balance being Fe and unavoidable impurities, A method for manufacturing a thick steel plate, in which the area ratio of void defects at the center position of the plate thickness is 0.5% or less, A preparation step of preparing a slab having the composition; A hot rolling process for hot rolling the slab; The hot rolling step has a total rolling reduction of more than 30% in rolling passes that satisfy the following (a) and (b): (a) Temperature at the center of the slab thickness: 700° C. or higher (b) Temperature difference between the surface of the slab and the center of the plate thickness: 100°C or more

2. The composition further comprises, in mass%, Cu: 2.00% or less, Ni: 2.50% or less, Cr: 1.50% or less, Mo: 1.00% or less, Nb: 0.100% or less, Ti: 0.100% or less, V: 0.30% or less, B: 0.0100% or less, W: 0.50% or less, Ca: 0.0200% or less, Mg: 0.0200% or less; REM: 0.0500% or less The method for producing a steel plate according to claim 1, further comprising one or more selected from the group consisting of:

Citation Information

Patent Citations

  • Hot forging of steel material

    JP1983167045A

  • Production of thick steel plate having high toughness and good internal quality by continuous casting

    JP1984074220A

  • Method for seasoning fried bean curd

    JP1986037080A

  • Liquid crystal shutter device

    JP1986056321A

  • Optical wavelength conversion apparatus

    JP1994069569A