Noise Suppression Sheet
A noise suppression sheet with magnetic powder particles and a binder, designed to handle multiple frequency bands, addresses the complexity of existing designs by providing effective noise suppression across a wide range of frequencies.
Patent Information
- Application Number
- JP2021011394
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-27
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-01-27
AI Technical Summary
Existing noise suppression sheets for small mobile terminals require multiple sheets to handle different frequency bands, complicating the manufacturing process and necessitating trial-and-error design methods.
A noise suppression sheet comprising flat magnetic powder particles with a reflux magnetic domain structure or magnetic vortex structure, along with a binder, where the magnetic powder particles have specific saturation magnetization, diameter, and thickness ratios, allowing for a method to design a single sheet that suppresses noise across multiple frequency bands.
The designed noise suppression sheet effectively suppresses noise in two distinct frequency bands, enabling efficient noise management without the need for multiple sheets and simplifying the design process.
Smart Images

Figure 0007589915000020 
Figure 0007589915000021 
Figure 0007589915000022
Abstract
Description
[Technical field]
[0001] The present invention relates to a noise suppression sheet and a method for designing the same. [Background technology]
[0002] In small mobile terminals such as smartphones, electromagnetic waves are emitted from noise sources such as internal ICs, causing electromagnetic interference with the antenna that transmits and receives carriers.Noise suppression sheets are used as a countermeasure against noise related to such electronic interference.
[0003] Patent Document 1 discloses this type of noise suppression sheet 900. The noise suppression sheet 900 in Patent Document 1 includes a sheet-shaped composite magnetic body. Here, the composite magnetic body includes a binder and soft magnetic powder dispersed in the binder. The noise suppression sheet 900 is capable of suppressing noise in a high-frequency band exceeding 3 GHz.
[0004] On the other hand, Non-Patent Document 1 discloses that the magnetic domain structure of a disk-shaped magnetic material made of polycrystalline Co produced by a thin-film manufacturing method has a magnetic vortex structure. In addition, Non-Patent Document 2 discloses the results of a theoretical analysis of the vibration mode of the magnetic vortex of a disk made of a soft magnetic permalloy-based material. However, the magnetic domain structure of the flat magnetic powder particles obtained by forging has not yet been clarified.
[0005] In addition, Non-Patent Documents 3 and 4 disclose a transformer-coupled magnetic permeability measuring device (TC-Perm) that can measure the high-frequency magnetic permeability of a single magnetic powder particle with a diameter of about 10 μm with a high signal-to-noise ratio. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2019-153623 A [Non-patent literature]
[0007] [Non-Patent Document 1] Y. Acremann et al.,Science,290,p492 (2000) [Non-Patent Document 2] K.Yu.Guslienko et al.,Journal of Applied Physics,2002,51,p8037 [Non-Patent Document 3] S.Tamaru et al.,Journal of Magnetism and Magnetic Materials,2020,501,p166434 [Non-Patent Document 4] Shingo Tamaru et al., "Magne", Magnetics Society of Japan, April 1, 2020, Vol. 15, No. 2, p. 134 Summary of the Invention [Problem to be solved by the invention]
[0008] Generally, noise frequencies that interfere with communication of small mobile terminals span a variety of frequency bands. However, the noise suppression sheet of Patent Document 1 only deals with noise in the high frequency band. Therefore, in order to suppress noise across multiple frequency bands, multiple noise suppression sheets corresponding to each of the noise frequency bands are required, which makes the manufacturing process complicated. In light of this situation, there is a demand for a noise suppression sheet that can deal with multiple noises in different frequency bands with just one sheet.
[0009] Furthermore, the current design of noise suppression sheets requires a process of trial and error, in which a prototype noise suppression sheet is subjected to radio wave absorption tests in the desired frequency band, and the materials, etc. are redesigned based on the test results. As a result, there is a demand for a method of designing a noise suppression sheet that enables a noise suppression sheet to be easily designed that can suppress noise in the desired frequency band based on the physical properties of the material that constitutes the noise suppression sheet.
[0010] Therefore, an object of the present invention is to provide a noise suppression sheet that can deal with a plurality of noises in different frequency bands with a single sheet, and to provide a method for designing a noise suppression sheet that enables a noise suppression sheet that can suppress noise in a desired frequency band to be easily designed. [Means for solving the problem]
[0011] The applicant has measured the frequency characteristics of the complex relative permeability of a noise suppression sheet containing magnetic powder particles over a wide range and has found that the imaginary component μ r The applicant found that "P" has peaks in two different frequency bands. The applicant also found that this phenomenon is due to the magnetic domain structure of the magnetic powder particles being a closure domain structure or a magnetic vortex structure. The applicant completed the present invention based on these findings.
[0012] That is, the present invention provides a first noise suppression sheet comprising: A noise suppression sheet comprising flat magnetic powder particles and a binder that binds the magnetic powder particles, The magnetic powder particles have a closure domain structure or a magnetic vortex structure as a magnetic domain structure, The saturation magnetization of the magnetic powder particles is μM S is 0.9T or more, The diameter D of the magnetic powder particles is 7500 μm or less, When the thickness of the magnetic powder particles is t, 1≦D / t≦1500 is satisfied, When the frequency of the noise that is shielded by the noise suppression sheet is f, the electrical resistivity of the magnetic powder particles is ρ, and the magnetic permeability of the magnetic powder particles is μ, the thickness t of the magnetic powder particles satisfies the relationship with the skin depth s shown in the following mathematical formula 1:
number
[0013] The present invention also provides a second noise suppression sheet comprising the first noise suppression sheet, The saturation magnetization is μM S is 2.0T or more, The diameter D of the magnetic powder particles is 20 μm or less, The condition 1≦D / t≦4 is satisfied. A noise suppression sheet is provided.
[0014] The present invention also provides a third noise suppression sheet, which is the first or second noise suppression sheet, The diameter D of the magnetic powder particles is expressed as the exchange stiffness constant A (J / m) and the anisotropy constant K (J / m 3 ) then the following formula 2 is satisfied.
number
[0015] The present invention also provides a method for designing a noise suppression sheet capable of suppressing noise in a desired frequency band, comprising the steps of: 1) A saturation magnetization of μM that can suppress noise in the desired frequency band S A material selection step of selecting a material having 2) an initial value setting step of setting initial values for a diameter D and a thickness t of the disk shape, assuming that the shape of the flat magnetic powder particles made of the selected material is a disk shape; 3) an aspect ratio calculation step of calculating an aspect ratio k from the diameter D and thickness t set in 2) using the following formula 3;
number
number
number
[0016] The noise suppression sheet of the present invention comprises flat magnetic powder particles and a binder that binds the magnetic powder particles, and the magnetic powder particles have a closure domain structure or a magnetic vortex structure as a magnetic domain structure. As a result, in the noise suppression sheet of the present invention, the imaginary component μ r '' produces peaks in two different frequency bands, making it possible for one filter to deal with multiple noises in different frequency bands.
[0017] Furthermore, the method for designing a noise suppression sheet of the present invention includes a demagnetizing field coefficient calculation step of calculating a demagnetizing field coefficient Nρ in the radial direction of the disk shape using the aspect ratio k calculated in the aspect ratio calculation step, using Equation 4; and a saturation magnetization μM of the material selected in the material selection step. S Using the demagnetizing factor Nρ calculated in the demagnetizing factor calculation step, the resonance frequency f HF,calc and a resonance frequency calculation step of calculating the resonance frequency using Equation 5. This makes it possible to easily design a noise suppression sheet that contains magnetic powder particles that have a closure domain structure or a magnetic vortex structure as a magnetic domain structure. In other words, according to the method for designing a noise suppression sheet of the present invention, it is possible to easily design a noise suppression sheet that is capable of suppressing noise in a desired frequency band. [Brief description of the drawings]
[0018] [Figure 1] 1 is a diagram showing a noise suppression sheet according to an embodiment of the present invention. [Diagram 2] 2 is a frequency characteristic graph showing the complex relative permeability of the noise suppression sheet of FIG. [Diagram 3] 2 is a frequency characteristic graph showing the complex magnetic susceptibility of a single magnetic powder particle contained in the noise suppression sheet of FIG. 1. [Figure 4] This is an image of the surface of the noise suppression sheet in Figure 1 observed with a magnetic force microscope (MFM). In the figure, domain walls are indicated by dotted lines, magnetic moments are indicated by arrows, and closure domain structures or magnetic vortex structures are indicated by circles. [Diagram 5] 2 is a diagram showing a schematic diagram of a magnetic domain structure in a magnetic powder particle contained in the noise suppression sheet of FIG. 1. [Figure 6] 4 is a flowchart illustrating a method for designing a noise suppression sheet according to an embodiment of the present invention. [Figure 7] 7 is a graph for explaining a method of designing the noise suppression sheet of FIG. 6. [Figure 8] 7 is another graph illustrating the design method of the noise suppression sheet of FIG. 6. [Figure 9] 7 is another graph illustrating the design method of the noise suppression sheet of FIG. 6. [Figure 10] 7 is another graph illustrating the design method of the noise suppression sheet of FIG. 6. [Figure 11] 7 is another graph illustrating the design method of the noise suppression sheet of FIG. 6. [Figure 12] 7 is another graph illustrating the design method of the noise suppression sheet of FIG. 6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] (Noise suppression sheet) Referring to FIG. 1, a noise suppression sheet 100 according to the embodiment of the present invention includes flat magnetic powder particles 200 and a binder 300 that binds the magnetic powder particles 200 together.
[0020] (Magnetic powder particles) The magnetic powder particles 200 of the present embodiment can be appropriately selected from known magnetic powder particles used in noise suppression sheets. The magnetic powder particles 200 are obtained by flattening (forging) magnetic particles obtained by a method such as atomization using a flattening device such as a ball mill. As the raw material of the magnetic powder particles 200, it is preferable to use soft magnetic powder, and it is more preferable to use Fe-based alloy soft magnetic powder containing Fe (iron) as the main component. Examples of Fe-based alloy soft magnetic powder include Fe, Fe-Al alloy powder, Fe-Co-V alloy powder, carbonyl iron powder, Fe-Si alloy powder, Fe-Ni alloy powder, Fe-Si-Cr alloy powder, Fe-Si-Al alloy powder, Fe-based alloy amorphous powder containing at least Fe-Si-B, and Fe-based alloy nanocrystalline powder containing at least Fe-BP-Cu. Here, the Fe-based alloy amorphous powder refers to an amorphous powder that does not have a crystalline structure among Fe-based alloy soft magnetic powders. The Fe-based alloy nanocrystalline powder refers to a material obtained by subjecting the Fe-based alloy amorphous powder to a heat treatment to precipitate fine α-Fe crystals in the amorphous phase. The Fe-based alloy nanocrystalline powder provides high saturation magnetic flux density (Bs) and low loss, and excellent magnetic properties, due to the high magnetization of α-Fe, reduced crystal magnetic anisotropy due to the fineness of the powder, and reduced magnetostriction due to the mixed phase of the positive magnetostriction of the amorphous phase and the negative magnetostriction of the α-Fe phase. In the present invention, one type of the above-mentioned various magnetic powder particles can be used alone, or two or more types can be used in combination.
[0021] The flat magnetic powder particles 200 are aligned and oriented parallel to the main surface of the noise suppression sheet 100. That is, the diameter D of the magnetic powder particle 200 is the size of the magnetic powder particle 200 in a direction perpendicular to the thickness direction of the noise suppression sheet 100, and the thickness t of the magnetic powder particle 200 is the size of the magnetic powder particle 200 in a direction parallel to the thickness direction of the noise suppression sheet 100. The diameter direction of the magnetic powder particle 200 is parallel to the direction in which the magnetic field component of the electromagnetic wave is applied, and the thickness direction of the magnetic powder particle 200 is perpendicular to the magnetic field component of the electromagnetic wave.
[0022] 5, magnetic powder particles 200 of this embodiment have a closure domain structure or a magnetic vortex structure as their magnetic domain structure. Moreover, magnetic powder particles 200 preferably have a magnetic vortex structure as their magnetic domain structure. Specifically, magnetic powder particles 200 have, as their magnetic domain structure, a magnetic vortex core 450 and a magnetic moment 400 around magnetic vortex core 450. As a result, with reference to FIG. 2, in noise suppression sheet 100 of this embodiment, the imaginary component μ r '' is the low frequency band f LF and high frequency band f HF 2 and 5, the peaks are generated in the low frequency band f LF The imaginary component μ of the complex relative permeability in r The peak of '' is presumed to be due to the inherent vibration of the magnetic vortex core 450 of the magnetic powder particle 200. HF The imaginary component μ of the complex relative permeability in r The peaks at '' are presumed to be due to the simultaneous excitation of the precession of the magnetic moments 400 of the magnetic powder particles 200.
[0023] The saturation magnetization of the magnetic powder particles 200 of this embodiment is μM S is 0.9 T or more. In addition, the saturation magnetization of the magnetic powder particles 200 is S is preferably 2.0 T or more. Here, μ0 represents the magnetic permeability (H / m) of a vacuum. The magnetic powder particles 200 have a saturation magnetization μ0M of 2.0 T or more.S In the case where the magnetic powder particle 200 has a diameter D and a thickness t, the imaginary component μ r '''s high frequency band f HF The carrier frequency of the fifth generation mobile communication system (5G) includes a frequency band of 28 GHz, but the saturation magnetization of the magnetic powder particles 200 is 20 μM. S When the noise suppression sheet 100 having a noise suppression coefficient of 2.0 T or more is used in a small mobile terminal such as a smartphone, the noise suppression effect can be achieved even at the carrier frequency of this fifth generation communication system.
[0024] The diameter D of the magnetic powder particle 200 in this embodiment is 7500 μm or less. The diameter D of the magnetic powder particle 200 is preferably 20 μm or less. The diameter D of the magnetic powder particle 200 is expressed by the exchange stiffness constant A (J / m) and the anisotropy constant K (J / m 3 ), the following formula 6 must be satisfied.
number
[0025] The thickness t of the magnetic powder particle 200 in this embodiment satisfies 1≦D / t≦1500. In addition, the thickness t of the magnetic powder particle 200 preferably satisfies 1≦D / t≦4.
[0026] In the noise suppression sheet 100 of the present embodiment, if the frequency of the noise to be shielded is f, the electrical resistivity of the magnetic powder particles 200 is ρ, and the magnetic permeability of the magnetic powder particles 200 is μ, then the thickness t of the magnetic powder particles 200 satisfies the relationship with the skin depth s shown in the following Equation 7.
number
[0027] That is, the thickness t of the magnetic powder particle 200 satisfies the following formula 8.
number
[0028] The method for producing the noise suppression sheet 100 of the present embodiment is not particularly limited, but it can be produced, for example, by the following method. First, a slurry made by mixing flat magnetic powder particles, a binder, and a solvent is formed into a sheet shape by a doctor blade method or the like to obtain a green body. The green body formed into a sheet shape is then heated to remove the solvent and fix the sheet shape to obtain the noise suppression sheet 100. Here, a crosslinking reaction may be caused by heating, and the sheet shape may be fixed as a crosslinked product. The above heating step may also be performed by hot press molding.
[0029] The noise suppression sheet 100 of the present embodiment thus obtained has high magnetic permeability and excellent noise suppression effect, and therefore, taking advantage of such characteristics, the noise suppression sheet 100 of the present embodiment can be suitably used for countermeasures against unwanted radiation, countermeasures against internal interference, improvement of RFID communication quality, countermeasures against ESD, countermeasures against SAR, etc.
[0030] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these descriptions.
[0031] <Example> The magnetic powder particles 200 were obtained by flattening (forging) Fe particles obtained by atomization using a flattening device such as a ball mill. The obtained magnetic powder particles 200 had a diameter D of 147 μm and a thickness t of 0.4 μm. Acrylic rubber was used as the binder. The obtained flat magnetic powder particles 100, a binder, and a solvent (toluene) were mixed to form a slurry, which was then molded into a sheet to obtain a molded body. The molded body was then heated to remove the solvent, and the sheet shape was fixed to produce a noise suppression sheet 100 with a length of 3 mm, a width of 35 mm, and a thickness of 0.05 mm. The frequency characteristics of the complex relative permeability of the produced noise suppression sheet 100 were measured using a complex permittivity measuring instrument PMM-9G1 (manufactured by Ryowa Electronics). In addition, the surface of the produced noise suppression sheet 100 was observed using a magnetic force microscope (MFM). Furthermore, for the magnetic powder particles 200 made from the noise suppression sheet 100, a frequency spectrum of the complex magnetic susceptibility of a single magnetic powder particle 200 was measured using a transformer-coupled magnetic permeability measuring device (TC-Perm) described in Non-Patent Documents 3 and 4. Specifically, a jig consisting of two short-circuit terminated planar waveguides (CPW1, 2) was first stacked while being insulated with Kapton tape to form a weakly coupled transformer. Then, the magnetic powder particle 200 was inserted between the signal lines of the planar waveguides (CPW1, 2). The planar waveguides (CPW1, 2) were connected to ports 1 and 2 of a vector network analyzer (VNA), respectively, and the transmission coefficient S of the jig in the measurement magnetic field and the saturation magnetic field was measured by the vector network analyzer (VNA). 21 The transmission coefficient S of the jig in the measured magnetic field and the saturated magnetic field obtained by this 21 Difference ΔS 21 Then, data processing for calibration was performed, thereby obtaining the complex magnetic susceptibility χ of the magnetic powder particle 200 in the measured magnetic field.
[0032] 2 is a graph showing the frequency characteristics of the complex relative permeability of the produced noise suppression sheet 100. As a result, the produced noise suppression sheet 100 has an imaginary component μ r '' are two different frequency bands (f LF ,f HF ) of the complex permeability of the produced noise suppression sheet 100. r '' is the low frequency band f LF There is a peak at about 150 MHz, and a peak at the high frequency band f HF It can be seen that another peak occurs near 3 GHz as a bimodal type μ r "It can be seen that it has a spectrum.
[0033] 3 is a graph showing the frequency characteristics of the complex magnetic susceptibility of the magnetic powder particle 200. As a result, the magnetic powder particle 200 has an imaginary component χ″ of the complex magnetic susceptibility in two different frequency bands (f LF ,f HF ) It can be seen that the imaginary component χ″ of the complex magnetic susceptibility of the magnetic powder particle 200 has a peak in the low frequency band f LF There is a peak at around 200 MHz, and a peak in the high frequency band f HF As a result, it can be seen that another peak occurs around 3 GHz as a result of the bimodal type μ r The spectrum is of 200 μm of a single magnetic powder particle. r "The spectrum was found to reflect the
[0034] In Non-Patent Document 2, the imaginary component μ of the complex relative permeability of a disk-shaped magnetic body is r '' peak frequency f in the low frequency band LF It has been concluded that this arises from resonance due to the orbital motion of the magnetic vortex core, and it has been disclosed that it can be described by the following Equation 9, where the gyromagnetic ratio is γ, the model parameter of the vortex magnetization distribution is ξ, and the static initial susceptibility is χ(0).
number
[0035] Here, when ξ=2 / 3 and χ(0) are substituted into the above formula 9 for the magnetic susceptibility χ' measured for a single magnetic powder particle 200, f LF,calc is calculated, but this calculated f LF,calc is the measured peak frequency f corresponding to the value of magnetic susceptibility χ' measured in a single magnetic powder particle 200. LF This confirmed that the noise suppression sheet 100 has a low frequency band f LF The imaginary component μ of the complex relative permeability in r It was found that the peak of '' can be explained by Equation 9. Therefore, the low frequency band f LF The imaginary component μ of the complex relative permeability in r It was speculated that the peak at '' was due to the inherent vibration of the magnetic vortex core of the magnetic powder particles 200.
[0036] In Non-Patent Document 1, a disk-shaped magnetic material made of C0 is HF The imaginary component μ of the complex relative permeability in r The peak of '' is concluded to be the simultaneous excitation of the precession of the magnetic moment in the magnetic vortex, and the saturation magnetization of the magnetic material is increased by μ0M S It is disclosed that if the demagnetizing field coefficient in the radial direction of the disk is Nρ, it can be expressed by the following equation 10.
number
[0037] Here, γ,M S ,N ρ Substituting the value of (data not shown) into the above formula 10 gives f HF,calc is calculated, but this calculated f HF,calc is the peak frequency f measured in a single magnetic powder particle 200 HF This confirmed that the noise suppression sheet 100 has a high frequency band f HF The imaginary component μ of the complex relative permeability inr It was found that the peak of '' can be explained by Equation 10. Therefore, the high frequency band f HF The imaginary component μ of the complex relative permeability in r It was speculated that the peaks at '' are due to the simultaneous excitation of precession of magnetic moments within the magnetic vortex of the magnetic powder particles 200.
[0038] 4 is a magnetic force microscope (MFM) image obtained by observing the surface of the produced noise suppression sheet 100 with an MFM. As a result, a group of magnetic moments 400 and domain walls 500 were observed in the magnetic powder particles 200 of the produced noise suppression sheet 100. In other words, it was confirmed that the magnetic powder particles 200 of the produced noise suppression sheet 100 have a plurality of closure domain structures 600 or magnetic vortex structures 600 as a magnetic domain structure.
[0039] (Noise suppression sheet design method) As described above, the applicant has developed a bimodal type μ r ''The spectrum is 200 μm for a single magnetic powder particle. r It was found that the spectrum of the noise suppression sheet 100 can be designed by designing the physical properties, etc., of a single magnetic powder particle 200. The design method for a noise suppression sheet of the present invention is based on this finding.
[0040] 6, the design method for the noise suppression sheet 100 according to this embodiment is a method for designing the noise suppression sheet 100 capable of suppressing noise in a desired frequency band. Specifically, the design method for the noise suppression sheet 100 according to this embodiment includes a material selection step, an initial value setting step, an aspect ratio calculation step, a demagnetizing field coefficient calculation step, a resonance frequency calculation step, a changing step, and a specifying step. The contents of each step are described in detail below.
[0041] First, the saturation magnetization μM that can suppress noise in the desired frequency band SIn this step, a material having a saturation magnetization of μM that can be used in a frequency band for suppressing noise is selected. S A material having the following properties is selected.
[0042] After the material selection step is performed, an initial value setting step is performed in which the shape of the flat magnetic powder particle 200 made of the selected material is assumed to be a disk shape, and initial values are set for the diameter D and thickness t of the disk shape. More specifically, after the material selection step is performed, an initial value setting step is performed in which the shape of the flat magnetic powder particle 200 made of the selected material and obtained by forging is assumed to be a disk shape, and initial values are set for the diameter D and thickness t of the disk shape.
[0043] After the initial value setting step is performed, an aspect ratio calculation step is performed in which an aspect ratio k is calculated from the diameter D and thickness t set in the initial value setting step using the following Equation 11.
number
[0044] After the aspect ratio calculation step is performed, a demagnetizing field coefficient calculation step is performed in which the demagnetizing field coefficient Nρ in the radial direction of the disk shape is calculated by the following Equation 12 using the aspect ratio k calculated in the aspect ratio calculation step.
number
[0045] After the demagnetization coefficient calculation step is performed, the saturation magnetization μM of the material selected in the material selection step is S Using the demagnetizing factor Nρ calculated in the demagnetizing factor calculation step, the resonance frequency f HF,calc A resonance frequency calculation step is performed to calculate the resonance frequency using the following formula 13.
number
[0046] After the resonant frequency calculation step is performed, the resonant frequency f HF,calc is not included in the desired frequency band, a modification step is performed to modify the diameter D and thickness t of the disk shape.
[0047] After the change step is performed, the resonant frequency f HF,calc is included in the desired frequency band, a specifying step is performed to specify the diameter D and thickness t of the disk shape by sequentially repeating the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonant frequency calculation step, and the changing step. In this way, the noise suppression sheet 100 capable of suppressing noise in the desired frequency band is designed.
[0048] In the design method for the noise suppression sheet 100 according to this embodiment, it is assumed that the flat magnetic powder particles 200 contained in the noise suppression sheet 100 are arranged with their orientation aligned parallel to the main surface of the noise suppression sheet 100. That is, the diameter D of the disk shape is the size of the disk shape in a direction perpendicular to the thickness direction of the noise suppression sheet 100, and the thickness t of the disk shape is the size of the disk shape in a direction parallel to the thickness direction of the noise suppression sheet 100. In addition, the diameter direction of the disk shape is parallel to the direction in which the magnetic field component of the electromagnetic wave is applied, and the thickness direction of the disk shape is perpendicular to the magnetic field component of the electromagnetic wave.
[0049] The present invention will be described in detail below by way of specific examples, but the present invention is not limited to the following examples.
[0050] Figure 7 shows the saturation magnetization in the material selection step. SThe diameter D and the resonant frequency f of the disk shape that satisfies the above formula 13 are calculated by selecting permendur (Fe-49%Co-2%V) with a magnetic field strength of 2.35 T as the material of the magnetic powder particles 200, and setting the thickness t of the disk shape to 0.1 μm, 0.5 μm, 1 μm, 4 μm, and 5 μm in the initial value setting step. HF,calc This shows the relationship between the frequency band in which noise is to be suppressed and the thickness t of the disk shape, 0.1 μm, and 0.2 μm≦D≦0.5 μm, 28 GHz≦f HF,calc Therefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0051] Similarly, referring to FIG. 7, when the desired frequency band is 28 GHz and the thickness t of the disk shape is 0.5 μm, 28 GHz≦f HF,calc Therefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0052] Also, referring to FIG. 7, when the desired frequency band is 28 GHz and the thickness t of the disk shape is 1 μm, 28 GHz≦f HF Therefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0053] Furthermore, referring to FIG. 7, when the desired frequency band is 28 GHz and the thickness t of the disk shape is 4 μm, 28 GHz≦f HF,calcTherefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0054] In addition, referring to FIG. 7, when the desired frequency band is 28 GHz and the thickness t of the disk shape is 5 μm, 28 GHz≦f HF,calc Therefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0055] In this way, the desired frequency band for suppressing noise is set to 28 GHz, and the saturation magnetization is set to 0.1 μM in the material selection step. S When permendur (Fe-49%Co-2%V) having a magnetic field strength of 2.35 T is selected as the material of the magnetic powder particles 200, the diameter D and thickness t of the disk shape are specified. Note that, in the above example, the process of specifying the diameter D and thickness t of the disk shape when the desired frequency band for suppressing noise is set to 28 GHz is shown, but even when the desired frequency band for suppressing noise is set to a frequency band other than 28 GHz, the diameter D and thickness t of the disk shape are similarly specified.
[0056] Figure 8 shows the saturation magnetization in the material selection step. S When Fe having a magnetic powder particle 200 material with a magnetic field strength of 2.15 T is selected as the material of the magnetic powder particle 200, and the thickness t of the disk shape is set to 0.1 μm, 0.5 μm, 1 μm, 4 μm, and 5 μm in the initial value setting step, the diameter D of the disk shape that satisfies the above formula 13 and the resonant frequency f HF,calc This shows the relationship between the frequency band in which noise is to be suppressed and the thickness t of the disk shape, 0.1 μm, and 0.2 μm≦D≦0.3 μm, 28 GHz≦f HF,calcTherefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0057] Similarly, referring to FIG. 8, when the desired frequency band is 28 GHz and the thickness t of the disk shape is 0.5 μm, 28 GHz≦f HF,calc Therefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0058] Also, referring to FIG. 8, when the desired frequency band is 28 GHz and the thickness t of the disk shape is 1 μm, 28 GHz≦f HF,calc Therefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0059] Furthermore, referring to FIG. 8, when the desired frequency band is 28 GHz and the thickness t of the disk shape is 4 μm, 28 GHz≦f HF,calc Therefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0060] In addition, referring to FIG. 8, when the desired frequency band is 28 GHz and the thickness t of the disk shape is 5 μm, 28 GHz≦f HF,calcTherefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0061] In this way, the desired frequency band for suppressing noise is set to 28 GHz, and the saturation magnetization is set to 0.1 μM in the material selection step. S Even when Fe, which has a magnetic field strength of 2.15 T, is selected as the material of the magnetic powder particles 200, the diameter D and thickness t of the disk shape are specified. Note that, in the above example, the process of specifying the diameter D and thickness t of the disk shape when the desired frequency band for suppressing noise is set to 28 GHz is shown, but even when the desired frequency band for suppressing noise is set to a frequency band other than 28 GHz, the diameter D and thickness t of the disk shape are similarly specified.
[0062] Figure 9 shows the saturation magnetization in the material selection step. S The diameter D and the resonant frequency f of the disk shape that satisfies the above formula 13 are calculated by selecting silicon steel (Fe-3% Si) with a resonant frequency of 2.0 T as the material of the magnetic powder particles 200, and setting the thickness t of the disk shape to 0.1 μm, 0.5 μm, 1 μm, 4 μm, and 5 μm in the initial value setting step. HF,calc This shows the relationship between the frequency band in which noise is to be suppressed and the thickness t of the disk shape, 0.1 μm, and 0.2 μm≦D≦0.4 μm, 25 GHz≦f HF,calc Therefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0063] Similarly, referring to FIG. 9, when the desired frequency band is 25 GHz and the thickness t of the disk shape is 0.5 μm, 25 GHz≦f HF,calcTherefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0064] Also, referring to FIG. 9, when the desired frequency band is 25 GHz and the thickness t of the disk shape is 1 μm, 25 GHz≦f HF,calc Therefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0065] Furthermore, referring to FIG. 9, when the desired frequency band is 25 GHz and the thickness t of the disk shape is 4 μm, 25 GHz≦f HF,calc Therefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0066] In addition, referring to FIG. 9, when the desired frequency band is 25 GHz and the thickness t of the disk shape is 5 μm, 25 GHz≦f HF,calc Therefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0067] In this way, if the desired frequency band for suppressing noise is set to 25 GHz, and the saturation magnetization is set to 0.1 μM in the material selection step, SEven when silicon steel (Fe-3%Si) having a resistance of 2.0T is selected as the material of the magnetic powder particles 200, the diameter D and thickness t of the disk shape are specified. Note that, in the above example, the process of specifying the diameter D and thickness t of the disk shape when the desired frequency band for suppressing noise is set to 25 GHz is shown, but even when the desired frequency band for suppressing noise is set to a frequency band other than 25 GHz, the diameter D and thickness t of the disk shape are similarly specified.
[0068] Figure 10 shows the saturation magnetization in the material selection step. S When Fe-3.5%Al having a magnetic powder particle 200 material with a magnetic field strength of 1.5 T is selected as the material of the magnetic powder particle 200, and the thickness t of the disk shape is set to 0.1 μm, 0.5 μm, 1 μm, 4 μm, and 5 μm in the initial value setting step, the diameter D of the disk shape that satisfies the above formula 13 and the resonant frequency f HF,calc This shows the relationship between the frequency band in which noise is to be suppressed and the thickness t of the disk shape, 0.1 μm, and 0.2 μm≦D≦0.3 μm, 20 GHz≦f HF,calc Therefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0069] Similarly, referring to FIG. 10, when the desired frequency band is 20 GHz and the thickness t of the disk shape is 0.5 μm, 20 GHz≦f HF,calc Therefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0070] Also, referring to FIG. 10, when the desired frequency band is 20 GHz and the thickness t of the disk shape is 1 μm, 20 GHz≦fHF,calc Therefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0071] Furthermore, referring to FIG. 10, when the desired frequency band is 20 GHz and the thickness t of the disk shape is 4 μm, 20 GHz≦f HF,calc Therefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0072] In addition, referring to FIG. 10, when the desired frequency band is 20 GHz and the thickness t of the disk shape is 5 μm, 20 GHz≦f HF,calc Therefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0073] In this way, if the desired frequency band for suppressing noise is set to 20 GHz, and the saturation magnetization is set to 0.1 μM in the material selection step, S Even when Fe-3.5%Al, which has a resistance of 1.5 T, is selected as the material of the magnetic powder particles 200, the diameter D and thickness t of the disk shape are specified. Note that, in the above example, the process of specifying the diameter D and thickness t of the disk shape when the desired frequency band for suppressing noise is set to 20 GHz is shown, but even when the desired frequency band for suppressing noise is set to a frequency band other than 20 GHz, the diameter D and thickness t of the disk shape are similarly specified.
[0074] Figure 11 shows the saturation magnetization μM in the material selection step. SSendust (registered trademark), which has a resonant frequency of 0.9T, is selected as the material of the magnetic powder particles 200, and the thickness t of the disk shape is set to 0.1 μm, 0.5 μm, 1 μm, 4 μm, and 5 μm in the initial value setting step. The diameter D and the resonant frequency f of the disk shape that satisfies the above formula 13 are calculated as follows: HF,calc This shows the relationship between the frequency band in which noise is to be suppressed and the thickness t of the disk shape, 0.1 μm, and 12 GHz ≦ f HF,calc Therefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0075] Similarly, referring to FIG. 11, when the desired frequency band is 12 GHz and the thickness t of the disk shape is 0.5 μm, 12 GHz≦f HF,calc Therefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0076] Also, referring to FIG. 11, when the desired frequency band is 12 GHz and the thickness t of the disk shape is 1 μm, 12 GHz≦f HF,calc Therefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0077] Furthermore, referring to FIG. 11, when the desired frequency band is 12 GHz and the thickness t of the disk shape is 4 μm, 12 GHz≦f HF,calcTherefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0078] In addition, referring to FIG. 11, when the desired frequency band is 12 GHz and the thickness t of the disk shape is 5 μm, 12 GHz≦f HF,calc Therefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0079] In this way, if the desired frequency band for suppressing noise is set to 12 GHz, and the saturation magnetization is set to 0.1 μM in the material selection step, S Even when Sendust (registered trademark), which has a coefficient of resistance of 0.9 T, is selected as the material of the magnetic powder particles 200, the diameter D and thickness t of the disk shape are specified. Note that, in the above example, the process of specifying the diameter D and thickness t of the disk shape when the desired frequency band for suppressing noise is set to 12 GHz is shown, but even when the desired frequency band for suppressing noise is set to a frequency band other than 12 GHz, the diameter D and thickness t of the disk shape are similarly specified.
[0080] Figure 12 shows the saturation magnetization μM in the material selection step. S Mu-metal (Fe-77Ni-2Cr-5Cu) with a magnetic powder particle 200 material having a magnetic field strength of 0.5 T is selected as the material of the magnetic powder particle 200, and the thickness t of the disk shape is set to 0.1 μm, 0.5 μm, 1 μm, 4 μm, and 5 μm in the initial value setting step. The diameter D and resonant frequency f of the disk shape that satisfies the above formula 13 are calculated as follows: HF,calc This shows the relationship between the frequency band in which noise is to be suppressed and the thickness t of the disk shape, 0.1 μm, and 0.2 μm≦D≦0.5 μm, 6 GHz≦f HF,calcTherefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0081] Similarly, referring to FIG. 12, when the desired frequency band is 6 GHz and the thickness t of the disk shape is 0.5 μm, 6 GHz≦f HF,calc Therefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0082] Also, referring to FIG. 12, when the desired frequency band is 6 GHz and the thickness t of the disk shape is 1 μm, 6 GHz≦f HF,calc Therefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0083] Furthermore, referring to FIG. 12, when the desired frequency band is 6 GHz and the thickness t of the disk shape is 4 μm, 6 GHz≦f HF,calc Therefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0084] In addition, referring to FIG. 12, when the desired frequency band is 6 GHz and the thickness t of the disk shape is 5 μm, 6 GHz≦f HF,calcTherefore, if the initial value of the diameter D is not within the above range, the aspect ratio calculation step, the demagnetizing field coefficient calculation step, the resonance frequency calculation step, and the change step are repeated in sequence while changing the value of the diameter D until it is within the above range.
[0085] In this way, the desired frequency band for suppressing noise is set to 6 GHz, and the saturation magnetization is set to 0.1 μM in the material selection step. S Even when mu-metal (Fe-77Ni-2Cr-5Cu) having a resistance of 0.5 T is selected as the material of the magnetic powder particles 200, the diameter D and thickness t of the disk shape are specified. Note that, in the above example, the process of specifying the diameter D and thickness t of the disk shape when the desired frequency band for suppressing noise is set to 6 GHz is shown, but even when the desired frequency band for suppressing noise is set to a frequency band other than 6 GHz, the diameter D and thickness t of the disk shape are similarly specified.
[0086] Although the present invention has been specifically described above with reference to the embodiment, the present invention is not limited to this and various modifications and changes are possible. [Explanation of symbols]
[0087] 100 Noise suppression sheet 200 magnetic powder particles 300 Binder 400 magnetic moments 450 Magnetic Vortex Core 500 domain wall 600 Closure domain structure 600 Magnetic Vortex Structure
Claims
1. A noise suppression sheet comprising flat magnetic powder particles and a binder that binds the magnetic powder particles, The magnetic powder particles have a closure domain structure or a magnetic vortex structure as a magnetic domain structure, The saturation magnetization μ of the magnetic powder particles 0 M S is 2.0T or more, The diameter D of the magnetic powder particles is 20 μm or less, When the thickness of the magnetic powder particle is t, the relationship 1≦D / t≦4 is satisfied, When the frequency of the noise that is shielded by the noise suppression sheet is f, the electrical resistivity of the magnetic powder particles is ρ, and the magnetic permeability of the magnetic powder particles is μ, the thickness t of the magnetic powder particles satisfies the relationship with the skin depth s shown in the following mathematical formula 1: [0010] Noise suppression sheet.
2. A noise suppression sheet comprising flat magnetic powder particles and a binder that binds the magnetic powder particles, The magnetic powder particles have a closure domain structure or a magnetic vortex structure as a magnetic domain structure, The saturation magnetization μ 0 M s of the magnetic powder particles is 0.9 T or more; The diameter D of the magnetic powder particles is 7500 μm or less, When the thickness of the magnetic powder particle is t, the relationship 1≦D / t≦1500 is satisfied, When the frequency of noise that is shielded by the noise suppression sheet is f, the electrical resistivity of the magnetic powder particles is ρ, and the magnetic permeability of the magnetic powder particles is μ, the thickness t of the magnetic powder particles satisfies the relationship with the skin depth s shown in the following mathematical formula 1, [0010] The diameter D of the magnetic powder particle is expressed by the exchange stiffness constant A (J / m) and the anisotropy constant K (J / m 3 ) then the following formula 2 is satisfied. [0025] Noise suppression sheet.
3. The noise suppression sheet according to claim 2, The saturation magnetization μ 0 M S is 2.0T or more, The diameter D of the magnetic powder particles is 20 μm or less, The relationship 1≦D / t≦4 is satisfied. Noise suppression sheet.
4. A method for designing a noise suppression sheet capable of suppressing noise in a desired frequency band, comprising the steps of: 1) Saturation magnetization μ that enables noise suppression in the desired frequency band 0 M S A material selection step of selecting a material having 2) an initial value setting step of setting initial values for a diameter D and a thickness t of the disk shape, assuming that the shape of the flat magnetic powder particles made of the selected material is a disk shape; 3) an aspect ratio calculation step of calculating an aspect ratio k from the diameter D and thickness t set in 2) using the following formula 3; [0030] 4) a demagnetizing field coefficient calculation step of calculating a demagnetizing field coefficient Nρ in a radial direction of the disk shape using the aspect ratio k calculated in 3) above, using the following formula 4; [0045] 5) Saturation magnetization μ of the material selected in 1) above 0 M S Using the demagnetizing factor Nρ calculated in 4), the resonance frequency f HF,calc A resonance frequency calculation step of calculating the resonance frequency by the following formula 5: [0050] 6) The resonance frequency f calculated in 5) above HF,calc a modification step of modifying the diameter D and thickness t of the disk shape if the desired frequency band is not included in the desired frequency band; 7) The resonance frequency f HF,calc A step of repeating steps 3) to 6) to specify a diameter D and a thickness t of the disk shape until the desired frequency band is reached. A method for designing a noise suppression sheet comprising:
Citation Information
Patent Citations
Method for manufacturing electromagnetic interference suppressor
JP2007173859A
Insulative coated powder for magnetic member
JP2015050361A
Flat powder and magnetic sheet used in high frequency
JP2018070929A
Uniaxially magnetically anisotropic bulk magnetic material and manufacturing method thereof
JP2019075403A
Noise suppression sheet
JP2019153623A