Semiconductor wafer processing solution containing hypochlorite ions

A cleaning solution with hypochlorite ions and alkylammonium ions effectively removes ruthenium and tungsten from semiconductor wafers, addressing slow etching and contamination issues, enhancing device yield and stability.

JP7590504B2Active Publication Date: 2024-11-26TOKUYAMA CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023111596
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-10-24
Filing Date
2023-07-06
Publication Date
2024-11-26
Estimated Expiration
2039-01-15

AI Technical Summary

Technical Problem

Conventional cleaning liquids for semiconductor wafers are ineffective in completely removing noble metals like ruthenium and tungsten, leading to cross-contamination and reduced yield due to slow etching rates and the presence of alkali metal ions, which can cause short circuits in electronic devices.

Method used

A cleaning solution containing hypochlorite ions with a pH between 7 and 12, stabilized by alkylammonium ions, and controlled concentrations of alkali and alkaline earth metal ions to enhance the etching rate and storage stability, effectively removing ruthenium and tungsten without damaging the wafer.

Benefits of technology

The solution achieves etching rates of 5 nm/min or more for ruthenium and 50 nm/min or more for tungsten, reduces residual metal ions on the wafer surface, and improves semiconductor device yield by minimizing contamination and ensuring long-term storage stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590504000006
    Figure 0007590504000006
  • Figure 0007590504000001
    Figure 0007590504000001
  • Figure 0007590504000002
    Figure 0007590504000002
Patent Text Reader

Abstract

To provide a process liquid and cleaning method, capable of removing ruthenium and / or tungsten adhering to an end face part and a rear face part of a semiconductor wafer.SOLUTION: The process liquid is a process liquid which is used to clean a semiconductor wafer and includes (A) a hypochlorite ion and (C) a solvent and has a pH of over 7 and under 12.0 at 25°C. The method for cleaning a semiconductor wafer removes ruthenium and tungsten from a semiconductor wafer with ruthenium or tungsten by bringing the process liquid into contact with the semiconductor wafer to clean the semiconductor wafer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel processing liquid used in the manufacturing process of semiconductor devices for cleaning the end faces and back faces of semiconductor wafers. [Background technology]

[0002] In recent years, design rules for semiconductor elements have become finer, and the requirements for impurity management in the semiconductor element manufacturing process have become stricter. The impurities generated in the manufacturing process of semiconductor elements differ for each manufacturing process. For this reason, it is important to identify the source of contamination for each manufacturing process and to manage the concentration of the impurities that are the source of contamination. In particular, since impurities such as metals and metal oxides remain in the manufacturing equipment, it is important not to carry the metals or metal oxides into the next process.

[0003] In recent years, large-diameter semiconductor wafers exceeding 300 mm have been used to improve the manufacturing efficiency of semiconductor elements. In large-diameter semiconductor wafers, the area of ​​the end face and back face where electronic devices are not fabricated is larger than that of small-diameter semiconductor wafers. Therefore, in the process of forming metal wiring and the process of forming barrier metal, metal wiring material and barrier metal material (hereinafter, sometimes collectively referred to as "metal material, etc.") are likely to adhere not only to the element formation portion on the surface of the semiconductor wafer where the semiconductor element is formed, but also to the end face and back face. As a result, as the diameter of the semiconductor wafer increases, the amount of excess metal material, etc. adhering to the end face and back face of the wafer increases.

[0004] Excess metal materials adhering to the edge or back surface of a semiconductor wafer contaminate the inside of the manufacturing equipment as metal or metal oxide particles during the oxygen ashing process or plasma dry etching process, which are processes that follow the formation of metal wiring and barrier metal. The particles may then adhere to and contaminate other wafers that are carried into the manufacturing equipment. This type of contamination is called cross-contamination. To prevent cross-contamination, metal materials adhering to the edge or back surface of a wafer must be removed before the wafer is carried into the next process.

[0005] Among these metal materials, precious metals such as platinum and ruthenium, and tungsten are often used in the element formation process. It is known that these metals are difficult to oxidize and dissolve in the subsequent etching and cleaning processes, and are difficult to remove, and continue to exist as impurities. Therefore, it is preferable to remove these precious metals and tungsten from the semiconductor wafer in preference to other metal materials. In particular, ruthenium is often used as a wiring material for semiconductor elements with design rules of 10 nm or less because it can reduce the resistance value more than when copper is used as a wiring material, so it is desired to remove it quickly from unnecessary parts. In addition, tungsten or tungsten alloys are often used as materials for gate electrodes, wiring, via holes, etc., but since they are formed by CVD or sputtering, they adhere to places other than the desired places. For this reason, like ruthenium, it is desired to remove tungsten quickly from unnecessary parts.

[0006] Generally, a method has been proposed for removing such precious metals and tungsten by oxidizing them with a strong oxidizing agent and forming compounds that dissolve in water. For example, Patent Document 1 proposes a cleaning method for removing precious metals by oxidizing ruthenium by adding a strong acid such as nitric acid to cerium (IV) ammonium nitrate as a cleaning solution.

[0007] Patent Document 2 discloses a method for treating ruthenium adhering to the end face of a semiconductor wafer, which involves cleaning with an oxidizing liquid having an oxidation-reduction potential 300 mV or more higher than the standard hydrogen electrode potential. Specifically, the liquid is an aqueous solution of sodium hypochlorite or ammonium hypochlorite having a pH of 12 or more.

[0008] Furthermore, in Patent Document 3, an aqueous solution of sodium hypochlorite or an aqueous solution of orthoperiodic acid is used as a method for etching a ruthenium film. In this method, ruthenium is etched while supplying benzotriazole to prevent corrosion of copper wiring.

[0009] In addition to removing precious metals, Example 5 of Patent Document 4 proposes a cleaning solution of pH 7 containing hypochlorous acid as a cleaning solution that can effectively remove contaminants such as particles on a substrate while preventing the corrosion and dissolution of device materials such as wiring, insulating films, and capacitive films, and preventing the occurrence of watermarks, without deteriorating the properties of the materials, in cleaning device substrates (semiconductor wafers).

[0010] Patent Document 5 proposes a cleaning composition using tetramethylammonium hypochlorite as an oxidizing agent for cleaning photoresist or residues from microelectronic substrates.

[0011] In addition, many types of cleaning solutions are known for the purpose of etching tungsten. For example, Patent Document 6 proposes a cleaning solution consisting of hydrogen peroxide, an organic acid salt, and water. [Prior art documents] [Patent documents]

[0012] [Patent Document 1] Patent Publication No. 2001-234373 [Patent Document 2] Patent Publication No. 2002-161381 [Patent Document 3] Patent Publication No. 2009-081247 [Patent Document 4] Patent Publication No. 2003-119494 [Patent Document 5] Patent Publication No. 2005-227749 [Patent Document 6] Patent No. 5523325 Summary of the Invention [Problem to be solved by the invention]

[0013] However, according to the investigations of the present inventors, it has been found that there is room for improvement in the above-mentioned conventional cleaning solutions in the following respects.

[0014] For example, in the method described in Patent Document 1, ruthenium attached to the edge or back surface of the semiconductor wafer is turned into ruthenium oxide and peeled off, but it was found that the peeled ruthenium oxide does not completely dissolve in the cleaning solution. Therefore, the peeled ruthenium oxide remains in the manufacturing equipment and may cause cross-contamination. In addition, there are cases where ruthenium oxide cannot be completely peeled off from the substrate, resulting in insufficient cleaning of the semiconductor wafer and leaving room for improvement.

[0015] In addition, it was found that the sodium hypochlorite aqueous solution with a pH of 12 or more described in Patent Document 2 has insufficient oxidizing power for ruthenium, and the etching rate of ruthenium is slow. The etching rate of ruthenium has a large effect on productivity, especially in the case of increasing the diameter of semiconductor wafers and improving throughput, so there is room for improvement in the hypochlorous acid aqueous solution of Patent Document 2. In addition, since sodium hypochlorite is used, the amount of sodium ions contained in the cleaning solution increases. As a result, sodium ions tend to adhere to semiconductor elements, which tends to reduce the yield of semiconductor elements.

[0016] In addition, the cleaning solution described in Patent Document 3 proposes a method of etching a ruthenium film with a sodium hypochlorite aqueous solution. It describes that hydrofluoric acid cleaning is performed to remove sodium resulting from the cleaning solution after etching. Hydrofluoric acid cleaning may also etch semiconductor wafers and silicon oxide films, which may reduce the yield of semiconductor elements.

[0017] In addition, in Example 5 of Patent Document 4, a cleaning solution containing hypochlorous acid and having a pH of 7 is proposed, but this cleaning solution is used for cleaning substrates having metal films or metal oxide films, and is intended to prevent the occurrence of watermarks, and is not intended to remove precious metals in particular. Therefore, even if the edge or back surface of a semiconductor wafer is cleaned with a cleaning solution having a pH of 7 to which 500 ppm of hypochlorous acid is added and the oxidation-reduction potential is adjusted to 612 mV, it is difficult to dissolve ruthenium, and it is also difficult to remove it, so further improvement is required. In addition, in this cleaning solution, ammonia is used as a pH adjuster to adjust the pH of the cleaning solution, but ammonia is highly volatile, and there is room for improvement in terms of the stability of the cleaning solution. Moreover, hypochlorite ions react with ammonia to partially generate highly explosive trichloramine, so that it is difficult to handle the cleaning solution after pH adjustment.

[0018] In the cleaning solution described in Patent Document 5, a cleaning solution containing tetramethylammonium hypochlorite as an oxidizing agent is proposed. According to the study by the present inventors, the pH of the cleaning solution exceeds 12. For example, the formulation A described as formulation A in Patent Document 5, which contains 17.6% by mass of TMAOCl, 6.6% by mass of TMACl, 0.43% by mass of TMAH, 85.3% by mass of water, and 0.05% by mass of Zonyl FSH, has a pH of 12.7. However, this cleaning solution is a cleaning solution used for cleaning photoresist and residues, and the metal coating of copper or aluminum containing ruthenium is not the object to be cleaned but is the object to be protected. Therefore, since the cleaning solution described in Patent Document 5 is not a cleaning solution intended to remove precious metals, there is room for improvement in that precious metals cannot be removed even if the cleaning solution described in Patent Document 5 is used.

[0019] The cleaning solution described in Patent Document 6 contains hydrogen peroxide and an organic acid salt, and is currently the mainstream etching solution for tungsten. This cleaning solution has a great advantage in that it causes little damage to silicon substrates. However, its etching rate for tungsten is insufficient, and from the viewpoint of improving throughput, a cleaning solution that has a faster etching rate for tungsten and does not cause damage to substrates is desired.

[0020] Therefore, an object of the present invention is to provide a processing liquid that can easily remove (clean) excess metal materials and the like adhering to the end faces or back faces of semiconductor wafers, and that is particularly effective in removing precious metals such as ruthenium and tungsten.

[0021] Another object of the present invention is to provide an improved treatment liquid that achieves the above-mentioned object, reduces alkali metal ions and alkaline earth metal ions, and improves the yield of semiconductor devices. Another object of the present invention is to provide a treatment liquid that is excellent in storage stability in addition to the above. [Means for solving the problem]

[0022] The present inventors have conducted extensive research to solve the above problems. They have investigated the use of hypochlorite ions, which are an oxidizing agent for precious metals and tungsten. Since the treatment solution containing hypochlorite ions is not sufficient in removing precious metals, etc., they have investigated various conditions and found that by setting the pH range to an appropriate range, cleaning properties and storage stability are significantly improved.

[0023] Furthermore, they have found that by using alkylammonium ion as the counter cation of hypochlorite ion, hypochlorite ion can be stabilized, storage stability can be improved, and the adverse effects caused by alkali metal ion and alkaline earth metal ion can be reduced.In addition, they have found that even when using alkali metal ion and alkaline earth metal ion as the counter cation of hypochlorite ion, by setting them in a specific concentration range, the adverse effects caused by alkali metal ion and alkaline earth metal ion can be reduced without impairing storage stability.

[0024] That is, the present invention relates to a processing liquid for cleaning semiconductor wafers, (1) The treatment liquid according to the first embodiment is (A) hypochlorite ion, and (C) Solvent and having a pH of more than 7 and less than 12.0 at 25°C. According to the treatment solution of the present invention, ruthenium or tungsten is oxidized by hypochlorite ions or chlorine. For example, in the case of ruthenium, ruthenium oxide ions (RuO 4 - ) and is believed to be removed from the system.

[0025] The treatment liquid preferably further contains (B1) an alkyl ammonium ion as an alkaline component. That is, (2) the treatment liquid according to the second embodiment is (A) hypochlorite ion, (B1) an alkyl ammonium ion, and (C) Solvent and having a pH of more than 7 and less than 12.0 at 25°C.

[0026] The mechanism by which the treatment liquid according to the second embodiment etches precious metals, for example, ruthenium, is considered to be as follows: In other words, in the presence of the alkylammonium ions, activated hypochlorite ions come into contact with ruthenium, and the ruthenium is oxidized, ionized, and removed (see formula 1). 2Ru+7ClO - +2OH - ⇔ 2RuO 4 - +7Cl - +H 2 O (Formula 1)

[0027] The treatment liquid preferably further contains, as an alkaline component, a specific amount of (B2) at least one type of metal ion selected from alkali metal ions and alkaline earth metal ions. That is, (3) the treatment liquid according to the third embodiment is (A) hypochlorite ion, (B2) at least one metal ion selected from an alkali metal ion and an alkaline earth metal ion, and (C) Solvent The treatment liquid has a concentration of the (B2) metal ions of 1 ppm or more and 20,000 ppm or less by mass, and a pH of more than 7 and less than 12.0 at 25°C.

[0028] It is believed that in the third embodiment, ruthenium is oxidized, ionized, and removed in the same manner as in the second embodiment. Through investigations, the present inventors have found that the above-mentioned reaction proceeds significantly when the alkali metal ions and / or alkaline earth metal ions are present in a specific amount, i.e., when the concentration is 1 ppm or more and 20,000 ppm or less by mass. The present invention can also take the following aspects.

[0029] (4) The treatment liquid according to any one of (1) to 3, wherein the concentration of the (A) hypochlorite ions is 0.05 to 20.0 mass %. (5) The treatment liquid according to (2), wherein the (B1) alkyl ammonium ion is a quaternary alkyl ammonium ion. (6) The treatment liquid according to (3), wherein the (B2) metal ion is a sodium ion. (7) A method for cleaning a semiconductor wafer, comprising contacting the semiconductor wafer with the treatment liquid according to any one of (1) to (6) above. (8) The method for cleaning a semiconductor wafer according to (7), wherein the semiconductor wafer has at least one metal selected from the group consisting of ruthenium and tungsten on its surface, and the metal is removed. (9) A method for producing the treatment liquid according to (2) above, comprising the steps of: (a) providing an alkylammonium-loaded ion exchange resin; and (b) contacting the alkylammonium-loaded ion exchange resin with an aqueous solution containing hypochlorite ions. A method for producing a treatment liquid comprising the steps of: (10) A method for producing the treatment liquid according to (9) above, comprising the steps of: A method for producing a treatment liquid, comprising the step (c) of adjusting the pH after the step (b).

[0030] The treatment liquid obtained by this method is a treatment liquid in which alkali metal ions and alkaline earth metal ions derived from salts that form hypochlorite are reduced.For example, when sodium hypochlorite is used, the treatment liquid is a treatment liquid in which sodium ions (alkali metal ions) contained in the treatment liquid are reduced.As a result, if the treatment liquid obtained by this method is used, problems caused by alkali metal ions and alkaline earth metal ions, such as adhesion of alkali metals to semiconductor wafers, are eliminated, and the yield rate when manufacturing semiconductor elements can be improved. Effect of the Invention

[0031] When the treatment solution of the present invention is used to clean a semiconductor wafer having a surface containing a metal component containing at least one metal selected from the group consisting of ruthenium and tungsten (hereinafter sometimes abbreviated as "Ru / W"), the semiconductor wafer can be cleaned with an etching rate of ruthenium of 5 nm / min or more, preferably 10 nm / min or more, if the cleaning conditions are properly adjusted. Also, the semiconductor wafer can be cleaned with an etching rate of tungsten of 50 nm / min or more, preferably 100 nm / min or more. In addition, in the treatment liquid according to the second embodiment, the concentration of cations (alkali metal ions or alkaline earth metal ions) remaining on the surface of the semiconductor wafer after cleaning can be increased to 1.5×10 15 atoms / cm 2 Less than 6.2 x 10 14 atoms / cm 2 It can also be less than.

[0032] Furthermore, the treatment solution according to the second embodiment has an effect of excellent long-term storage stability by controlling the concentration of alkylammonium ions in a specific range in addition to the pH. Since alkali metals and alkaline earth metals remaining in manufacturing equipment and on semiconductor wafers cause short circuits in electronic devices and lead to a decrease in the yield of semiconductor elements, it is desirable to reduce the amount of alkali metals and alkaline earth metals remaining after cleaning.

[0033] In addition, in the treatment liquid according to the third embodiment, the concentration of alkali metal ions and / or alkaline earth metal ions is set to 1 ppm or more and 20,000 ppm or less by mass, thereby reducing sodium ions remaining after cleaning and exhibiting excellent long-term storage stability. In addition, sodium ions remaining in the manufacturing equipment and on the semiconductor wafer can be reduced. As a result, sodium ions, which were thought to be a cause of short circuits in electronic devices, can be reduced, improving the yield of semiconductor elements.

[0034] Furthermore, the treatment solution of the present invention can effectively remove Si, which is the main material of semiconductor wafers, and Si-containing coatings (e.g., SiO 2 , Si 3 N 4 It can efficiently etch only the metals (Ru / W) that need to be removed without excessively etching other materials (SiC, SiOC, SiC, etc.). [Brief description of the drawings]

[0035] [Figure 1]1 is a schematic cross-sectional view showing an example of an end surface of a semiconductor wafer to which the treatment liquid of the present invention can be suitably applied; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0036] (Processing solution) The treatment liquid of the present invention can remove precious metals and tungsten adhering to the end face and back face of the semiconductor wafer without damaging the semiconductor wafer. Therefore, the treatment liquid of the present invention can be suitably used for cleaning the semiconductor wafer having precious metals and tungsten remaining on the surface. However, the object to be cleaned is not limited to this, and it is needless to say that the treatment liquid can also be used for cleaning the semiconductor wafer having no precious metals or tungsten on the surface.

[0037] Metals to which the treatment solution of the present invention is applied, particularly Ru / W, are attached not only to the front surface of a semiconductor wafer but also to its end face and back surface by CVD and sputtering methods mainly used in semiconductor device processes (see FIG. 1). As shown in FIG. 1, at least one metal 2 selected from the group consisting of ruthenium and tungsten is attached to the end face 3 and back surface 4 of this semiconductor wafer 1. This tendency becomes prominent when using a large-diameter semiconductor wafer having a diameter of more than 300 mm. In the present invention, when a semiconductor wafer has Ru / W on its front surface, this includes Ru / W present not only outside the semiconductor device formation region on the front surface of the semiconductor wafer but also on the end face and back surface.

[0038] For example, Ru / W is used as a material for metal wiring or barrier metal, and is therefore formed into a film on the silicon that constitutes a semiconductor wafer, or on silicon oxide that is laminated on silicon.

[0039] The treatment liquid of the present invention is not particularly limited, but can be suitably used for cleaning the above-mentioned semiconductor wafer. The treatment liquid contains (A) hypochlorite ions and (C) a solvent, and preferably contains (B1) alkylammonium ions or (B2) at least one metal ion selected from alkali metal ions and alkaline earth metal ions. The following will explain the treatment liquid step by step.

[0040] (A) Hypochlorite ion The hypochlorite ion used in the present invention can be generated by dissolving hypochlorite in a suitable solvent such as water. The salt in the hypochlorite is preferably an alkali metal and / or an alkaline earth metal. Among them, sodium is most preferable in consideration of cleaning effect.

[0041] In the treatment liquid of the present invention, the concentration of hypochlorite ions is preferably in the range of 0.05 to 20% by mass. Within the above range, Ru / W can be sufficiently dissolved and cleaned. If the concentration of hypochlorite ions exceeds 20% by mass, the decomposition reaction of hypochlorite ions tends to occur easily. On the other hand, if the concentration is less than 0.05% by mass, the etching rate tends to be slow and the cleaning ability tends to decrease. Therefore, the range of hypochlorite ions is preferably 0.1 to 15% by mass, more preferably 0.3 to 10% by mass, even more preferably 0.5 to 6% by mass, and particularly preferably 0.5 to 4% by mass.

[0042] In addition, in the present invention, in order to suppress the decomposition reaction of hypochlorite ion in the treatment liquid and suppress the decrease in the concentration of hypochlorite ion, the pH of the treatment liquid is preferably more than 7 and less than 12. When the pH of the treatment liquid is 7 or less, the decomposition reaction of hypochlorite ion is easily generated, and the concentration of hypochlorite ion tends to be easily decreased. Hereinafter, the effect of suppressing the decomposition reaction of hypochlorite ion in the treatment liquid and suppressing the decrease in the concentration of hypochlorite ion may be referred to as "storage stability".

[0043] Furthermore, in consideration of the storage stability of the treatment liquid, the concentration of hypochlorite ions is preferably in the range of 0.05 to 6 mass%. This range ensures high storage stability. If the concentration of hypochlorite ions exceeds 6 mass%, the decomposition reaction of hypochlorite ions tends to occur easily. Therefore, in consideration of the etching rate of Ru / W, cleaning properties, and the storage stability of the treatment liquid itself, the concentration of hypochlorite ions is more preferably in the range of 0.1 to 6 mass%, further preferably 0.3 to 6 mass%, and particularly preferably 0.5 to 4 mass%.

[0044] Therefore, in order to achieve a good combination of the etching rate of Ru / W, cleaning properties, and storage stability of the treatment liquid itself, a treatment liquid having a hypochlorite ion concentration range of 0.05 to 6 mass % and a pH of more than 7 and less than 12 is particularly preferred. Within the above ranges, the hypochlorite ion concentration is unlikely to decrease during storage, and the treatment liquid can exhibit sufficient cleaning properties for Ru / W even after storage for 15 days in a dark place at 20°C.

[0045] The concentration of hypochlorite ion can be calculated when producing the treatment liquid, or can be confirmed by directly analyzing the treatment liquid.The concentration of hypochlorite ion described in the following examples is obtained by measuring the effective chlorine concentration of the treatment liquid.Specifically, referring to the Ministry of Health, Labor and Welfare Notification No. 318 (last revised on March 11, 2005), potassium iodide and acetic acid are added to the solution containing hypochlorite ion, and the liberated iodine is subjected to oxidation-reduction titration with sodium thiosulfate aqueous solution to calculate the effective chlorine concentration.

[0046] (C) Solvent In the treatment liquid of the present invention, the remainder other than (A), (B1), (B2) and other additives described in detail below is a solvent, and after adjusting (A), (B1), (B2) and other additives, the remainder is adjusted with a solvent so that the total amount is 100 mass %.

[0047] Water is most preferably used as the solvent. The water contained in the treatment solution of the present invention is preferably water from which metal ions, organic impurities, particles, etc. have been removed by distillation, ion exchange treatment, filter treatment, various adsorption treatments, etc., and is particularly preferably pure water or ultrapure water. In this case, the concentration of water is the remainder excluding various chemicals.

[0048] In addition, an organic solvent may be used as long as hypochlorite ions are present in a stable manner. Examples of the organic solvent include acetonitrile and sulfolane.

[0049] In addition, water and an organic solvent may be used in combination as a solvent. By using water and an organic solvent in combination, oxidation of Ru / W proceeds relatively slowly, so that oxidation of wiring and the like in the circuit formation portion can be suppressed and excess Ru / W adhering to the end face and back face of the semiconductor wafer can be efficiently removed. When using water and an organic solvent in combination, the mass ratio of water to the organic solvent (water / organic solvent) may be about 60 / 40 to 99.9 / 0.1.

[0050] The treatment liquid of the present invention particularly preferably contains an alkaline component, which may be (B1) an alkyl ammonium ion (second embodiment) or a predetermined amount of (B2) at least one metal ion selected from alkali metal ions and alkaline earth metal ions (third embodiment).

[0051] (B1) Alkyl ammonium ion The alkylammonium ions used in the second embodiment are contained in the treatment liquid to improve the storage stability of the treatment liquid and to adjust the pH.

[0052] The alkyl ammonium ion is not particularly limited, and may be any of primary alkyl ammonium ions, secondary alkyl ammonium ions, tertiary alkyl ammonium ions, and quaternary alkyl ammonium ions, or a mixture thereof. Among them, quaternary alkyl ammonium ions are preferred in order to facilitate the production of the treatment liquid itself and to further enhance the cleaning effect of the treatment liquid.

[0053] The number of carbon atoms in the alkyl ammonium ion is not particularly limited. Among them, in order to facilitate the production of the treatment liquid itself and to further improve the cleaning effect of the treatment liquid, an alkyl group having 1 to 10 carbon atoms is preferred, and an alkyl group having 1 to 5 carbon atoms is more preferred.

[0054] Therefore, the alkyl ammonium ion is preferably a quaternary alkyl ammonium ion having 1 to 10 carbon atoms, and more preferably having 1 to 5 carbon atoms. Specific examples of the ions include a tetramethyl ammonium ion, a tetraethyl ammonium ion, and a tetrabutyl ammonium ion. The above alkyl ammonium ions do not affect the cleaning properties of the treatment liquid, and can enhance the storage stability of the treatment liquid.

[0055] The concentration of the alkylammonium ion is preferably in the range of 0.1 to 30% by mass. When the concentration of the alkylammonium ion satisfies this range, the pH fluctuation of the treatment liquid can be reduced even if Ru / W is oxidized, dissolved, or removed. As a result, etching can be performed stably, and the long-term storage stability is also excellent. In order to further exert this effect, the concentration of the alkylammonium ion is more preferably 0.15 to 20% by mass, further preferably 0.3 to 15% by mass, and particularly preferably 0.5 to 8% by mass.

[0056] The treatment liquid according to the second embodiment may contain alkali metal ions, alkaline earth metal ions, such as sodium ions and calcium ions, which are inevitably mixed in the treatment liquid in order to adjust the pH or in the manufacturing process of the treatment liquid. However, these alkali metal ions and alkaline earth metal ions may have adverse effects on semiconductor wafers (adverse effects such as a decrease in the yield of semiconductor wafers), so it is preferable that the mixing ratio of these ions is small, and in fact it is better that they are not included as much as possible. Specifically, the content is preferably 1 mass % or less, more preferably 0.7 mass % or less, even more preferably 0.3 mass % or less, particularly preferably 10 ppm or less, and most preferably 500 ppb or less.

[0057] Alkylammonium ions exist as counter cations for hypochlorite ions, stabilizing the hypochlorite ions. Also, unlike alkali metal ions and alkaline earth metal ions, they do not have any adverse effects on semiconductor wafers (such as a decrease in the yield of semiconductor wafers), and contribute to improving the quality of semiconductor wafers after cleaning.

[0058] (B2) At least one metal ion selected from alkali metal ions and alkaline earth metal ions In consideration of the productivity of the treatment liquid itself, the alkali metal ions and / or alkaline earth metal ions (hereinafter, sometimes simply referred to as "metal ions") used in the third embodiment are preferably (A) counter ions of hypochlorite ions, which are brought into the treatment liquid as salts for generating hypochlorite ions. Therefore, the type is determined by the raw material used. For example, when sodium hypochlorite is used to adjust hypochlorite ions, sodium ions will be present in the treatment liquid. However, it is also possible to prepare a solution containing hypochlorite ions that does not contain the metal ions, and add metal ions to it.

[0059] Incidentally, the at least one metal ion selected from alkali metal ions and alkaline earth metal ions may naturally be only alkali metal ions, only alkaline earth metal ions, or both. In the case where both are contained, the concentrations described below in detail are based on the total amount of both.

[0060] In the third embodiment, the concentration of metal ions must be 1 ppm or more and 20000 ppm or less by mass. If it is within the above range, even if ruthenium is oxidized, dissolved, or removed, the pH of the treatment liquid does not change, and etching can be performed stably. Furthermore, if it is within the above range, it is possible to make a treatment liquid excellent in long-term storage stability.

[0061] That is, when the concentration of metal ions is less than 1 ppm by mass, the ratio of ions that are paired with hypochlorite ions decreases, and the decomposition of hypochlorite ions is promoted. On the other hand, when the concentration of metal ions is more than 20,000 ppm by mass, hypochlorite ions can be stably present because there are many metal ions that are paired with hypochlorite ions, but the surface of the semiconductor wafer after cleaning is contaminated with metal ions. This causes a decrease in the yield of semiconductor elements. In the treatment liquid according to the third embodiment, by adjusting the blending amount, it is possible to obtain a concentration of 1×10 15 atoms / cm 2 As a result, it can be used suitably as a cleaning solution for the back surface and edge surfaces of semiconductor wafers.

[0062] Considering the storage stability of the treatment liquid and the cleaning effect, the metal ion concentration is 1 ppm to 20,000 ppm, more preferably 10 ppm to 15,000 ppm, even more preferably 200 ppm to 13,000 ppm, and still more preferably 1,000 ppm to 10,000 ppm. If it is within the above range, the pH of the treatment liquid does not change even if Ru / W is removed (cleaned), and stable treatment can be performed.

[0063] In addition, when the metal ions contained in the treatment solution as counter ions of hypochlorite ions are too much and need to be reduced, the following method can be adopted to prepare the solution so as to satisfy the requirements of the present invention.Specifically, the method of dissolving sodium hypochlorite in water, contacting it with cation exchange resin, and replacing sodium ions with hydrogen ions can be adopted.When the reduction of metal ions is insufficient, the above-mentioned operation of contacting it with cation exchange resin can be repeated to reduce the metal ions.

[0064] In order to adjust the pH of the treatment liquid according to the third embodiment and improve its storage stability, amines, preferably organic amines, can also be blended. The organic amine is not particularly limited as long as it is an amine that becomes an ammonium ion, an alkyl ammonium ion, or the like. Among them, an organic amine that becomes a quaternary alkyl ammonium ion is preferable. The carbon number of the quaternary alkyl ammonium ion is also not particularly limited, but it is preferably an alkyl group having 1 to 10 carbon atoms, and particularly preferably an alkyl group having 1 to 5 carbon atoms, specifically, a tetramethyl ammonium ion, a tetraethyl ammonium ion, or a tetrabutyl ammonium ion. In addition, in the third embodiment, when amines are blended, it is preferable to blend an amount that satisfies the pH range of the treatment liquid from more than 7 to 10.0 or less. However, these amines are not essential components. The treatment liquid according to the third embodiment contains a specific amount of metal ions, so that it exhibits excellent effects even if amines are not included. The metal ions can be directly produced from an aqueous hypochlorite solution by adjusting the production conditions. Therefore, in consideration of the ease of production of the treatment liquid, it is preferable that only a specific amount of metal ions is included.

[0065] (Other additives) The processing solution of the present invention may contain additives that have been conventionally used in processing solutions for semiconductors, if desired, within the scope of not impairing the object of the present invention. For example, additives such as acids, metal corrosion inhibitors, fluorine compounds, oxidizing agents, reducing agents, chelating agents, surfactants, and antifoaming agents may be added.

[0066] (pH of treatment solution) The treatment liquid of the present invention contains the (A) hypochlorite ion and the (C) solvent, preferably contains the (B1) alkylammonium ion or contains a predetermined amount of the (B2) metal ion, and contains other additives as necessary. If the (A) hypochlorite ion concentration (0.05 to 20 mass%), the (B1) alkylammonium ion concentration (0.1 to 30 mass%), or the (B2) metal ion concentration (1 ppm or more and 20,000 ppm or less) is suitable, the pH of the treatment liquid can be easily adjusted to more than 7 and less than 12. Since the pH of the treatment liquid of the present invention is more than 7 and less than 12 depending on the amount of each component, even if Ru / W is oxidized, dissolved, or removed, the pH of the treatment liquid does not change and it can be removed stably. Furthermore, within the above range, it is possible to obtain a treatment liquid with excellent long-term storage stability. If the pH of the treatment liquid is 12 or more, the etching rate of Ru / W is significantly reduced.

[0067] In addition, when the pH of the treatment liquid is 7 or less, the decomposition reaction of the hypochlorite ions contained in the treatment liquid tends to occur easily. Therefore, in consideration of the stable use of the treatment liquid and the storage stability of the treatment liquid itself, the pH of the treatment liquid is more preferably 8 or more and less than 12, and even more preferably 8 or more and less than 11.

[0068] The method for producing the treatment liquid of the present invention is not particularly limited. The treatment liquid according to the first embodiment can be produced in accordance with the method for producing the treatment liquid according to the second or third embodiment. The method for producing the treatment liquid according to the second and third embodiments will be described below using water as a solvent as an example. (Method for producing treatment liquid according to the second embodiment) The treatment liquid according to the second embodiment can be produced by preparing an ion exchange resin to which alkylammonium has been added, and contacting the ion exchange resin with an aqueous solution containing hypochlorite ions.

[0069] Each step will be described in detail below. (a) preparing an ion exchange resin having an alkyl ammonium salt attached thereto; An aqueous solution containing alkylammonium ions or alkylammonium halide ions, specifically an aqueous solution of alkylammonium hydroxide, is brought into contact with an ion exchange resin to prepare an ion exchange resin to which alkylammonium has been added.

[0070] The alkyl ammonium added to the ion exchange resin is not particularly limited, and may be any of primary alkyl ammonium, secondary alkyl ammonium, tertiary alkyl ammonium, and quaternary alkyl ammonium, or a mixture thereof. However, as described above, the alkyl ammonium ion contained in the treatment liquid is preferably a quaternary alkyl ammonium ion. Therefore, the alkyl ammonium is preferably a quaternary alkyl ammonium. The carbon number of the quaternary alkyl ammonium is also preferably 1 to 10, and more preferably 1 to 5, like the quaternary alkyl ammonium ion. An example of a specific compound is tetramethylammonium hydroxide. Therefore, in this embodiment, it is preferable to prepare an ion exchange resin to which alkyl ammonium is added by contacting an aqueous solution of tetramethylammonium hydroxide with the ion exchange resin.

[0071] The ion exchange resin to be used is not particularly limited as long as it is a known cation exchange resin. For example, hydrogen type ion exchange resin and sodium type ion exchange resin can be used. However, in the case of sodium type ion exchange resin, sodium is contained in the obtained treatment liquid, so hydrogen type ion exchange resin is preferred. In addition, weakly acidic or strongly acidic ion exchange resins can be used as hydrogen type ion exchange resins.

[0072] (b) contacting the alkylammonium-loaded ion exchange resin with an aqueous solution containing hypochlorite ions. After preparing the ion exchange resin to which alkylammonium has been added, the treatment liquid of this embodiment can be produced by contacting the ion exchange resin with an aqueous solution containing hypochlorite ions.

[0073] The aqueous solution containing hypochlorite ions can be prepared by dissolving hypochlorite in water. Examples of hypochlorite include calcium hypochlorite and sodium hypochlorite, and sodium hypochlorite is preferred in terms of good storage stability and handling.

[0074] The prepared aqueous solution containing hypochlorite ions is brought into contact with the ion exchange resin to which alkylammonium has been added, thereby producing a treatment liquid containing hypochlorite ions and alkylammonium ions.

[0075] In this embodiment, the ion exchange step (b) may be repeated. By repeating the ion exchange step, it is possible to reduce the amount of cations, such as sodium and calcium, that serve as counterions of hypochlorous acid contained in the aqueous solution containing hypochlorite ions. As described above, alkali metal ions such as sodium and calcium and alkaline earth metal ions contained in the treatment liquid cause a decrease in the yield of semiconductor elements. Therefore, as described above, the total amount of alkali metal ions and alkaline earth metal ions contained in the treatment liquid is 1 mass% or less, preferably 0.7 mass% or less, more preferably 0.3 mass% or less, even more preferably 10 ppm or less, and particularly preferably 1 ppm or less. In addition, when the treatment liquid of the present invention is applied to a manufacturing process in which the design rule of semiconductor elements is 10 nm or less, alkali metal ions and alkaline earth metal ions at a level of 10 ppm affect the yield of semiconductor elements, so that it is preferably 500 ppb or less. By repeating the (b) step, the total amount of alkali metal ions and alkaline earth metal ions contained in the treatment liquid can be reduced to the greatest extent possible.

[0076] Other additives that are added as necessary may be mixed into the solution (treatment liquid) obtained after the step (b).

[0077] The method for producing the treatment liquid according to the second embodiment has been described above. However, the treatment liquid of the present invention may be produced, for example, by contacting an aqueous solution containing hypochlorite ions with an ion exchange resin and mixing an aqueous solution containing hypochlorite ions in which alkali metal ions and alkaline earth metal ions have been reduced with an aqueous solution containing alkylammonium ions. Alternatively, the treatment liquid of the present invention may be produced by contacting an aqueous solution containing hypochlorite ions in which cations have been reduced with an ion exchange resin to which alkylammonium has been added.

[0078] However, in the manufacturing process of the aqueous solution containing hypochlorite ions, which is obtained by reducing alkali metal ions and alkaline earth metal ions from the aqueous solution containing hypochlorite ions, if the pH of the aqueous solution becomes acidic, the decomposition reaction of hypochlorite ions will start, and storage stability will decrease.Therefore, the manufacturing method of first preparing an ion exchange resin to which alkyl ammonium is added, and contacting the aqueous solution containing hypochlorite ions with this ion exchange resin can stably manufacture the treatment solution of the present invention without decomposing hypochlorite ions in the manufacturing process.

[0079] (c) pH adjustment process In the production of the treatment liquid according to the second embodiment, a step (c) of adjusting the pH can be included after the step (b). The pH of the treatment liquid can be adjusted by passing the treatment liquid obtained in the step (b) through a hydrogen-type cation exchange resin or by adding an acid such as hydrochloric acid to lower the pH of the treatment liquid (adjusting to the acidic side). The pH of the treatment liquid can be increased (adjusting to the alkaline side) by passing the treatment liquid obtained in the step (b) through a hydroxide-type anion exchange resin or by adding an alkylammonium hydroxide solution such as a tetramethylammonium hydroxide solution.

[0080] (Method for producing treatment liquid according to the third embodiment) The treatment liquid according to the third embodiment can be produced by preparing an aqueous solution of hypochlorite and reducing metal ions, which are counter ions of hypochlorite ions, from the solution.

[0081] As a method for reducing the amount of metal ions, a method may be adopted in which an ion exchange resin is brought into contact with hypochlorite to replace the metal ions with hydrogen ions.

[0082] Specifically, first, sodium hypochlorite is dissolved in water to prepare an aqueous solution containing hypochlorite ions, and this solution is brought into contact with a cation exchange resin. The metal ions contained in the aqueous solution containing hypochlorite ions are adsorbed by the ion exchange resin to adjust the metal ion concentration (1 ppm or more and 20000 ppm or less), thereby producing the treatment liquid according to the third embodiment.

[0083] The ion exchange resin can be any cation exchange resin, such as a strong acid ion exchange resin or a weak acid ion exchange resin, without any particular limitation. When the weak acid ion exchange resin is brought into contact with an aqueous solution of sodium hypochlorite, the ion exchange resin swells less and does not generate chlorine, so that the weak acid ion exchange resin is more preferable in terms of excellent handling.

[0084] The method for contacting the cation exchange resin with the aqueous sodium hypochlorite solution is not particularly limited, and any known method may be used. Specifically, the method includes contacting the aqueous sodium hypochlorite solution by passing the aqueous sodium hypochlorite solution through a column containing the cation exchange resin.

[0085] In addition, if necessary, the ion exchange resin may be regenerated. The regeneration method of the ion exchange resin is not particularly limited, and any known method may be adopted. Specifically, the method is to pass hydrochloric acid or sulfuric acid through a column containing a cation exchange resin after passing an aqueous solution of sodium hypochlorite through the column. After the above steps, a step (c) of adjusting the pH of the treatment liquid may be included, as in the second embodiment.

[0086] (Storage method) The method of storing the treatment solution of the present invention is not particularly limited, but since the decomposition of hypochlorite ion increases with increasing temperature, it is preferable to store the treatment solution at 20°C or less. In addition, since hypochlorite ion is also decomposed by ultraviolet light, it is preferable to store the treatment solution in a dark place. By applying such storage conditions, the storage stability of the treatment solution can be further improved.

[0087] (Method of cleaning semiconductor wafers) The cleaning conditions when using the treatment liquid of the present invention are a temperature range of 10 to 80° C., preferably 20 to 70° C., which may be appropriately selected according to the cleaning conditions of the cleaning device used.

[0088] Furthermore, the etching rate of Ru / W varies depending on the cleaning temperature. Therefore, in order to improve the cleaning ability of Ru / W, the cleaning temperature should be selected to be 50 to 70°C within the above temperature range. If the temperature is in the range of 50 to 70°C, the etching rate can be increased and processing can be performed with good operability using a simple device. For example, it is known that the cleaning ability differs between single-wafer cleaning and batch cleaning even when the same cleaning conditions are selected. Therefore, if the cleaning ability of Ru / W is insufficient depending on the type of cleaning device, the cleaning conditions should be appropriately selected, such as by setting the cleaning temperature higher.

[0089] The time for using the treatment liquid of the present invention is in the range of 0.1 to 120 minutes, preferably 0.5 to 60 minutes, and may be appropriately selected depending on the etching conditions and the semiconductor element to be used. As a rinse liquid after using the treatment liquid of the present invention, an organic solvent such as alcohol can be used, but simply rinsing with deionized water is sufficient.

[0090] As described above, the treatment solution of the present invention can efficiently etch Ru / W. For ruthenium, the etching rate can be 5 nm / min or more, preferably 10 nm / min or more. For tungsten, the etching rate can be 50 nm / min or more, preferably 100 nm / min or more. Furthermore, the amount of metal (e.g., sodium) remaining on the cleaned surface of the semiconductor wafer after cleaning is 1.0×10 15 atoms / cm 2 Less than 6.2 x 10 14 atoms / cm 2 The amount of Ru / W adhering to the edge or back surface of a semiconductor wafer can be reduced to a level below 100 nm. In addition, by adjusting the conditions, the etching rate (removal rate) of Ru / W after cleaning can be made sufficiently high, and metal residues can be further reduced. As is clear from this, the treatment liquid of the present invention can be suitably used in a method for manufacturing a semiconductor device that includes a step of removing Ru / W adhering to the edge or back surface of a semiconductor wafer. EXAMPLES

[0091] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0092] (pH measurement method) The pH of 30 mL of the treatment solution prepared in the examples and comparative examples was measured using a tabletop pH meter (LAQUA F-73, manufactured by Horiba, Ltd.) The pH measurement was carried out after the treatment solution was adjusted and stabilized at 25°C.

[0093] (Calculation method for available chlorine concentration and hypochlorite ion concentration) After preparing the treatment solution of the examples and comparative examples, 0.5 mL of the treatment solution, 2 g of potassium iodide (Wako Pure Chemical Industries, special grade reagent), 8 mL of 10% acetic acid, and 10 mL of ultrapure water were added to a 100 mL Erlenmeyer flask and stirred until the solids were dissolved to obtain a brown solution. The prepared brown solution was subjected to oxidation-reduction titration using 0.02 M sodium thiosulfate solution (Wako Pure Chemical Industries, volumetric analysis) until the color of the solution changed from brown to very light yellow, and then a starch solution was added to obtain a light purple solution. 0.02 M sodium thiosulfate solution was further added to this solution, and the effective chlorine concentration was calculated from the point where the solution became colorless and transparent as the end point. The hypochlorite ion concentration was also calculated from the obtained effective chlorine concentration. For example, if the effective chlorine concentration is 1%, the hypochlorite ion concentration is 0.73%.

[0094] (How to calculate sodium ion concentration) After preparing the treatment solutions of the Examples and Comparative Examples, the Na concentration was analyzed using a high-frequency inductively coupled plasma emission spectrometry (iCAP6500DuO, manufactured by Thermo Scientific).

[0095] (Calculation method for alkylammonium ion concentration) The alkylammonium ion concentrations in the treatment solutions of the Examples and Comparative Examples were calculated from the pH, hypochlorite ion concentration, and sodium ion concentration.

[0096] (Calculation method for Ru / W etching rate) An oxide film was formed on a silicon wafer using a batch-type thermal oxidation furnace, and a ruthenium or tungsten film was formed on top of it to a thickness of 120 nm (±10%) using the sputtering method. The sheet resistance was measured using a four-point probe resistance meter (Loresta-GP, manufactured by Mitsubishi Chemical Analytech Co., Ltd.) and converted into film thickness.

[0097] 30 ml of the treatment solution adjusted to the composition of the examples and comparative examples was prepared in a fluororesin container with a lid (AsOne, PFA container 94.0 mL), and each sample piece with a thickness of 10 × 20 mm was immersed in the treatment solution for 1 minute at 23 ° C., and the etching rate at 23 ° C. was calculated by dividing the change in film thickness before and after treatment by the immersion time. Similarly, a fluororesin container with a lid in which 30 mL of treatment solution was prepared was immersed in a water bath (Isotemp general-purpose hooded water bath, ThermoFisher Scientific) heated to 65 ° C. for 1 hour, and then each sample piece with a thickness of 10 × 20 mm was immersed in the treatment solution for 1 minute at 65 ° C., and the etching rate was calculated by dividing the change in film thickness before and after treatment by the immersion time, which was evaluated as the etching rate in the present invention.

[0098] In addition, after the ruthenium film was completely etched away, the silicon wafer surface was observed under a microscope at 20,000x magnification. If any foreign matter was observed, it was rated as poor (B), and if no foreign matter was found, it was rated as excellent (A). The origin and composition of this foreign matter are not necessarily clear, but it is believed that some component dissolved in the processing solution reattached to the wafer surface. Note that if the Ru etching rate is extremely slow, it takes time to remove the Ru film, so foreign matter is not evaluated.

[0099] (Method for evaluating the sodium concentration remaining on the cleaned surface of a wafer) Each sample piece cut to 10×20 mm was immersed in 30 mL of the treatment solution of the Examples and Comparative Examples for 1 minute. Then, 4 rinse solutions were prepared in advance, each of which had 30 mL of ultrapure water placed in a fluororesin container. Each sample piece was immersed in the treatment solution for 1 minute while being shaken, and washed four times in total. The Na concentration in the fourth rinse solution was analyzed using high-frequency inductively coupled plasma optical emission spectroscopy (iCAP6500DuO, Thermo Scientific). The residual Na concentration was 1.0×10 15 atoms / cm 2 If the amount exceeds 6.2×10, it may remain on the surface of the semiconductor element and significantly reduce the yield of the semiconductor device. 14atoms / cm 2 The results of this measurement serve as an index showing the tendency of sodium contained in the treatment liquid to remain on the wafer when the semiconductor wafer is cleaned using the treatment liquid. 15 atoms / cm 2 Even if the residual Na concentration exceeds this value, it is possible to reduce the residual Na concentration by performing repeated washing. The evaluation was based on the following criteria. A: 6.2×10 14 atoms / cm 2 less than B: 6.2×10 14 atoms / cm 2 Above 1.0×10 15 atoms / cm 2 Less than C: 1.0 x 10 15 atoms / cm 2 End

[0100] (Evaluation method for storage stability) 30 mL of the treatment solution of the Examples and Comparative Examples was placed in a fluororesin container and stored in a dark place at 20°C for 15 days. After 15 days of storage, the effective chlorine concentration of the treatment solution was measured and converted into hypochlorite ion concentration. The hypochlorite ion concentration immediately after production and after 15 days of storage were compared, and a ratio (immediately after production / after 15 days) of 0.5 to 1.0 was evaluated as excellent (A), and a ratio of less than 0.5 was evaluated as poor (B).

[0101] Example 1 (Production of processing solution) <Pretreatment of ion exchange resin: Hydrogen type ion exchange resin> 200 mL of strong acid ion exchange resin (Amberlite IR-120BNa, Organo Corporation) was placed in a glass column with an inner diameter of approximately 45 mm (AsOne Corporation, Biocolumn CF-50TK). Then, 1 L of 1N hydrochloric acid (Wako Pure Chemical Industries, Ltd., for volumetric analysis) was passed through the ion exchange resin column to exchange it into the hydrogen form, and 1 L of ultrapure water was passed through the column to wash the ion exchange resin.

[0102] <(a) Process> Furthermore, 1 L of 10% tetramethylammonium hydroxide solution was passed through 209 mL of 2 meq / mL-R ion exchange resin that had been exchanged into the hydrogen form, and the ion exchange resin was ion-exchanged from the hydrogen form to the tetramethylammonium (TMA) form. After the ion exchange, 1 L of ultrapure water was passed through the ion exchange resin to wash it.

[0103] <(b) Process> 69 g of sodium hypochlorite pentahydrate (Wako Pure Chemical Industries, Ltd., special grade reagent) was placed in a 2 L fluororesin container, and then 931 g of ultrapure water was added to prepare a 3.11 mass % aqueous sodium hypochlorite solution. 1 L of the prepared aqueous sodium hypochlorite solution was passed through a tetramethylammonium-type ion exchange resin to obtain a treatment solution with the composition shown in Table 2.

[0104] <Evaluation> The pH, available chlorine concentration, and hypochlorite ion concentration of the resulting treatment solution were evaluated, as well as the alkylammonium ion concentration, sodium ion concentration, ruthenium etching rate, tungsten etching rate, residual foreign matter, "sodium concentration remaining on the cleaned surface of the wafer," and storage stability. The results are shown in Table 3.

[0105] Example 2 The same procedure as in Example 1 was carried out except that the amount of ion exchange resin in step (a) was 282 mL and the concentration of the aqueous sodium hypochlorite solution in step (b) was 4.20 mass %, to obtain a treatment solution having the composition shown in Table 2. The evaluation results are shown in Table 3.

[0106] Example 3 The same procedure as in Example 1 was carried out except that the amount of ion exchange resin in step (a) was 141 mL and the concentration of the aqueous sodium hypochlorite solution in step (b) was 2.10 mass %, to obtain a treatment solution having the composition shown in Table 2. The evaluation results are shown in Table 3.

[0107] Example 4 The same operation as in Example 1 was carried out to obtain a treated liquid, and then, as a pH adjustment step (c), the treated liquid was passed through a glass column packed with 50 mL of 2 meq / mL-R cation exchange resin exchanged to a hydrogen form to obtain a treated liquid having the composition shown in Table 2. The evaluation results are shown in Table 3.

[0108] Example 5 A treatment liquid was obtained by carrying out the same operation as in Example 1, and then, as a pH adjustment step (c), a 25% tetramethylammonium hydroxide (TMAH) solution was added to the treatment liquid until the pH reached 11.5, thereby obtaining a treatment liquid having the composition shown in Table 2. The evaluation results are shown in Table 3.

[0109] Example 6 The same procedure as in Example 1 was carried out except that the amount of ion exchange resin in step (a) was 31 mL and the concentration of the aqueous sodium hypochlorite solution in step (b) was 0.46 mass %, to obtain a treatment solution having the composition shown in Table 2. The evaluation results are shown in Table 3.

[0110] Example 7 The same procedure as in Example 1 was carried out except that the amount of ion exchange resin in step (a) was 564 mL, the amount of 10% tetramethylammonium hydroxide solution passed was 2 L, and the concentration of the aqueous sodium hypochlorite solution in step (b) was 8.39 mass %, to obtain a treatment solution having the composition shown in Table 2. The evaluation results are shown in Table 3.

[0111] Example 8 The same operation as in Example 1 was carried out except that the amount of ion exchange resin in step (a) was 705 mL, the amount of 10% tetramethylammonium hydroxide solution passed was 2 L, and the concentration of the sodium hypochlorite aqueous solution in step (b) was 10.49 mass %, to obtain a treatment solution having the composition shown in Table 2. The evaluation results are shown in Table 3.

[0112] Example 9 Sodium hypochlorite pentahydrate (Wako Pure Chemical Industries, Ltd., special grade reagent) was dissolved in water so that the hypochlorite ion concentration was 2.15% by mass, to obtain a treatment solution having the composition shown in Table 2. The evaluation results are shown in Table 3.

[0113] Comparative Example 1 The same operation as in Example 1 was carried out to obtain a treated liquid, and then, as a pH adjustment step (c), the treated liquid was passed through a glass column packed with 203 mL of 2 meq / mL-R cation exchange resin exchanged to a hydrogen type to obtain a treated liquid having the composition shown in Table 2. The evaluation results are shown in Table 3.

[0114] Comparative Example 2 The same operation as in Example 1 was carried out to obtain a treated liquid, and then, as a pH adjustment step (c), the treated liquid was passed through a glass column packed with 208 mL of 2 meq / mL-R cation exchange resin exchanged to a hydrogen type to obtain a treated liquid having the composition shown in Table 2. The evaluation results are shown in Table 3.

[0115] Comparative Example 3 The same operation as in Example 1 was carried out to obtain a treated liquid, and then, as a pH adjustment step (c), the treated liquid was passed through a glass column packed with 209 mL of 2 meq / mL-R cation exchange resin exchanged to a hydrogen type to obtain a treated liquid having the composition shown in Table 2. The evaluation results are shown in Table 3.

[0116] Comparative Example 4 A treatment liquid was obtained by carrying out the same operation as in Example 1, and then, as a pH adjustment step (c), a 25% tetramethylammonium hydroxide solution was added to the treatment liquid until the pH reached 13.0, thereby obtaining a treatment liquid having the composition shown in Table 2. The evaluation results are shown in Table 3.

[0117] Table 1 shows the main conditions in the manufacturing process of the above-mentioned Examples and Comparative Examples, Table 2 shows the compositions of each treatment liquid, and Table 3 shows the evaluation results.

[0118] [Table 1]

[0119] [Table 2]

[0120] [Table 3]

[0121] As shown in Table 3, it was confirmed that the treatment solution of this embodiment has a high etching rate for ruthenium and tungsten, is effective in removing these metals, and leaves no residual foreign matter. The treatment solutions of Examples 5 and 6 have a low etching rate at 23°C, but by increasing the etching temperature, the etching rate is improved, and it was confirmed that they can be used without any problems in practice. The treatment solution of Example 9 contains a lot of Na ions, so there is a large amount of Na remaining after cleaning, but this residual Na can be sufficiently reduced by repeated cleaning. In addition, the treatment solution of this embodiment also has excellent storage stability. Furthermore, the treatment solution of this embodiment has been confirmed to have a high etching rate for Si, which is the main material of semiconductor wafers, and for the Si-containing coating (SiO 2 , Si 3 N 4 The etching rate for both materials was less than 0.1 nm / min, confirming that the target materials, ruthenium and tungsten, could be efficiently etched.

[0122] The treatment solutions of Comparative Examples 1, 2, and 3 have a low pH and a slow etching rate. In addition, foreign matter remains after etching, and the storage stability is low.

[0123] In Comparative Example 4, since the pH was higher than 12, it was found that even when the treatment was performed at 23° C. and 65° C., the etching speed was not sufficient to etch ruthenium adhering to the edge and back surfaces of the semiconductor wafer.

[0124] Example 10 Acetonitrile was added to the treatment liquid obtained in Example 2 to obtain a treatment liquid having the composition shown in Table 4. The pH of this treatment liquid and the etching rate of the Ru coating at 23° C. were evaluated. The results are shown in Table 4.

[0125] Example 11 Sulfolane was added to the treatment liquid obtained in Example 2 to obtain a treatment liquid having the composition shown in Table 4. The pH of this treatment liquid and the etching rate at 23° C. for a Ru coating were evaluated. The results are shown in Table 4.

[0126] [Table 4]

[0127] The treatment solutions of Examples 10 and 11 have the same composition as Example 2, except that water and an organic solvent are used in combination as the solvent. The Ru etching rate changed depending on the type of organic solvent. It was found that the Ru etching rate decreased with both acetonitrile and sulfolane.

[0128] Example 12 (Production of processing solution) <Pretreatment of ion exchange resin: Hydrogen type ion exchange resin> As a weakly acidic ion exchange resin, acrylic Diaion (Mitsubishi Chemical Corporation, WK40L) was packed in a column, and an aqueous solution of sodium hypochlorite adjusted to a predetermined hypochlorite ion concentration was passed through the column to obtain the treatment solution shown in Table 5. Specifically, in the case of the treatment solution shown in Example 12, an ion exchange resin having an ion exchange capacity equivalent to 1.3 mmol / L of Na ions was packed in a column, and a 3% aqueous solution of sodium hypochlorite was passed through the column to obtain the treatment solution shown in Table 5.

[0129] In addition, by checking the pH of the treated liquid after passing through, it was possible to check whether the ion exchange had progressed sufficiently, and if it had not, passing through the column was repeated until the specified pH was reached to obtain a treated liquid with the desired Na reduction. The contact area between the ion exchange resin and the aqueous sodium hypochlorite solution was adjusted according to the concentration of sodium to be reduced, and the treated liquid shown in Table 5 was obtained.

[0130] <Evaluation> The pH, hypochlorite ion concentration, sodium ion concentration, ruthenium etching rate at 23°C, residual foreign matter, "sodium concentration remaining on the cleaned surface of the wafer," and storage stability of the resulting treatment solution were evaluated. The results are shown in Table 5. A ruthenium etching rate of 10 nm / min or more was rated as excellent (A), and a rate of 5 nm / min or more but less than 10 nm / min was rated as good (B).

[0131] Example 13 The same procedure was carried out as in Example 12, except that an ion exchange resin having an ion exchange capacity equivalent to 1.2 mmol / L of Na ions was packed in the column, to obtain a treatment solution having the composition shown in Table 5. The results are shown in Table 5.

[0132] Example 14 The same procedure as in Example 12 was carried out except that an ion exchange resin having an ion exchange capacity equivalent to 6.5 mmol / L of Na ions was packed in a column and a 2% aqueous solution of sodium hypochlorite was passed through the column, to obtain a treatment solution having the composition shown in Table 5. The results are shown in Table 5.

[0133] Example 15 The same procedure as in Example 12 was carried out except that an ion exchange resin having an ion exchange capacity equivalent to 1.6 mmol / L of Na ions was packed in a column and a 4% aqueous solution of sodium hypochlorite was passed through the column, to obtain a treatment solution having the composition shown in Table 5. The results are shown in Table 5.

[0134] Comparative Example 5 The same procedure was carried out as in Example 12, except that an ion exchange resin having an ion exchange capacity equivalent to 290 mmol / L of Na ions was packed in the column, to obtain a treatment solution having the composition shown in Table 5. The results are shown in Table 5.

[0135] Comparative Example 6 The same procedure was carried out as in Example 12, except that an ion exchange resin having an ion exchange capacity equivalent to 287 mmol / L of Na ions was packed in the column, to obtain a treatment solution having the composition shown in Table 5. The results are shown in Table 5.

[0136] Comparative Example 7 The same procedure as in Example 12 was carried out except that the treatment solution was contacted with the ion exchange resin until the sodium ion concentration contained in the treatment solution became 10 ppb or less, to obtain a treatment solution having the composition shown in Table 5. The results are shown in Table 5.

[0137] Example 16 The same procedure as in Example 12 was carried out except that an ion exchange resin having an ion exchange capacity equivalent to 3.4 mmol / L of Na ions was packed in a column and an 8% aqueous solution of sodium hypochlorite was passed through the column, to obtain a treatment solution having the composition shown in Table 5. The results are shown in Table 5.

[0138] [Table 5]

[0139] As shown in Table 5, the treatment solutions of Examples 12 to 15 have a high etching rate for ruthenium, are capable of performing treatment with little residual sodium after washing, and also have excellent storage stability.

[0140] Residual foreign matter was found in the treatment solutions of Comparative Examples 5 and 6. In Comparative Example 7, the pH was as low as 3.0 and the amount of counter ions to hypochlorite ions was small, resulting in poor storage stability.

[0141] It was confirmed that the etching rate of ruthenium was good in Example 16 and that it could be used without any problems in practice. The treatment solution in Example 16 contains a large amount of Na ions, so there is a large amount of Na remaining after cleaning, but this residual Na can be sufficiently reduced by repeated cleaning. [Explanation of symbols]

[0142] 1. Semiconductor wafer 2 Ruthenium and / or Tungsten 3 End section 4 Back part

Claims

1. A treatment solution for cleaning a semiconductor wafer having at least one metal selected from the group consisting of ruthenium and tungsten on a surface thereof, and removing the metal, comprising: (A) hypochlorite ion, (B1) an alkyl ammonium ion, and (C) Solvent and wherein the concentration of the (B1) alkylammonium ion is 0.1 to 8.33 mass % (excluding those containing a bromine-containing compound).

2. The treatment liquid according to claim 1 , wherein the solvent (C) comprises an organic solvent.

3. A method for producing the treatment liquid according to claim 1 or 2, comprising the steps of: (a) providing an alkylammonium loaded ion exchange resin; and (b) contacting the ion exchange resin having the alkylammonium added thereto with an aqueous solution containing hypochlorite ions.

Citation Information

Patent Citations

  • Jet engine designed to drive compressor by its steam turbine

    JP1980023325A

  • Novel ester of alginic acid

    JP1988033401A

  • Removing solution for ruthenium series metal and using method therefor

    JP2001234373A

  • Method for etching ruthenium film

    JP2002161381A

  • Washing composition, and washing method and washing device using the same

    JP2003119494A