Hydrogel composition, method for producing same, and hydrogel

A hydrogel composition combining modified HA and PEGDA addresses the instability and mechanical weaknesses of HA-based hydrogels, offering enhanced mechanical properties and biocompatibility for diverse applications.

JP7590787B2Active Publication Date: 2024-11-27WIN COAT CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023034515
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-11-18
Filing Date
2023-03-07
Publication Date
2024-11-27
Estimated Expiration
2043-03-07

AI Technical Summary

Technical Problem

Hydrogels made from hyaluronic acid (HA) face challenges such as instability in water, mechanical weakness, and difficulty in shaping due to high viscosity, limiting their practical applications, especially in the biomedical field.

Method used

A hydrogel composition is developed using modified HA and poly(ethylene glycol) diacrylate (PEGDA) with controlled ratios and molecular weights to prevent precipitation and enhance mechanical properties, swelling ability, and biocompatibility.

Benefits of technology

The resulting hydrogel exhibits improved mechanical strength, rapid water absorption, and biocompatibility, making it suitable for various applications including the biomedical field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590787000009
    Figure 0007590787000009
  • Figure 0007590787000010
    Figure 0007590787000010
  • Figure 0007590787000001
    Figure 0007590787000001
Patent Text Reader

Abstract

To provide a hydrogel composition that produces a hydrogel material having good compatibility of raw materials, simultaneously offering good mechanical properties, good swellability and good biocompatibility.SOLUTION: Provided is a hydrogel composition, which comprises a modified hyaluronic acid (HA), poly(ethyleneglycol) diacrylate (PEGDA) and water, wherein, based on the total weight of the hydrogel composition, the content of the modified HA is 1 wt.% to 7 wt.% and the content of PEGDA is 43 wt.% to 49 wt.%; the modified HA is obtained by modifying HA with methacrylic anhydride; and the average molecular weight of PEGDA is 1 kDa to 10 kDa.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to compositions, methods of making the same, and materials, and in particular to hydrogel compositions, methods of making the same, and Hydrogels Regarding. [Background technology]

[0002] Hydrogel, also called aquagel, is a gel with water as a dispersion medium, and has high hydrophilicity and a crosslinked structure of a three-dimensional network. This crosslinked structure allows hydrogel to absorb and swell quickly in water, and to retain a large amount of water without losing this swelling state. The amount of water retained by hydrogel is closely related to the degree of crosslinking, and the higher the degree of crosslinking, the less water the hydrogel retains. As a material with high water adsorption and high water retention, hydrogel has a wide range of applications. For example, hydrogel can be applied to daily necessities such as diapers, sanitary products, or facial masks; can be applied in industrial fields such as wastewater treatment or air filtration; and can be applied in biomedical fields such as burn dressings, drug delivery carriers, or grafts.

[0003] Generally, water-soluble or hydrophilic polymers can form hydrogels through chemical or physical crosslinking reactions. According to the difference in the source of the polymer, hydrogels are classified into natural polymer hydrogels and synthetic polymer hydrogels. Natural polymer hydrogels are formed from natural polymers (e.g., polysaccharides such as starch, cellulose or hyaluronic acid (HA), and polypeptides such as collagen or polylysine), while synthetic polymer hydrogels are formed from synthetic polymers (e.g., alcohols and acrylic acid and its derivatives such as polyacrylic acid or polyacrylamide). In particular, due to the advantages of abundant raw material sources and excellent biocompatibility, the application of natural polymer hydrogels in the biomedical field has become the focus of research in industry and academia.

[0004] HA has excellent hydrophilicity and water retention, and is widely present in cartilage tissue, body fluids, and epithelial tissue, which gives it excellent biocompatibility. Therefore, HA is very suitable as a raw material for natural polymer hydrogels. However, due to the high viscosity of HA, it is difficult to inject and uniformly fill HA into a mold, and therefore it cannot be molded into a specific shape to meet various requirements. In addition, HA has the property of quickly dissolving in water, so the polymers formed by HA are difficult to be molded into a specific shape to meet various requirements. Hydrogels is unstable, easily dissolved and its mechanical properties do not meet real requirements, which limits its applicability in the biological field.

[0005] To address the above-mentioned shortcomings of HA, poly(ethylene glycol) diacrylate (PEGDA) was mixed with HA, and then Hydrogels Specifically, the photocrosslinking properties of PEGDA are used to form a crosslinked structure with a three-dimensional network, which Hydrogels can act as the main structure of the HA, limiting the aqueous solubility of HA, thereby Hydrogels However, in order to meet the requirements for mechanical properties in practical applications, it is necessary to adopt PEGDA with a relatively high average molecular weight, such as about 6 kilodaltons (kDa), as a raw material. In this case, the presence of PEGDA with a high average molecular weight and HA will cause an excluded volume effect, which will reduce the compatibility between PEGDA and HA, and even make HA more susceptible to precipitation, thereby Hydrogels This significantly limits follow-up use.

[0006] Therefore, PEGDA and HA were adopted as raw materials, which not only have good compatibility between PEGDA and HA to prevent HA precipitation, but also have improved mechanical properties to meet the requirements in practical applications. Hydrogels Further research and development is needed. Summary of the Invention [Problem to be solved by the invention]

[0007] In view of the above problems in the above prior art, the object of the present invention is to provide a hydrogel composition comprising PEGDA and HA, in which the raw materials, i.e., PEGDA and HA, have excellent compatibility to prevent the precipitation of HA, which is Hydrogels At the same time, the hydrogel compositions of the present invention are useful for follow-up applications in the formation of Hydrogels has improved mechanical properties, such as a Young's modulus of over 450 MPa, which can meet the requirements in practical applications, resulting in increased applicability.

[0008] Another object of the present invention is to provide a hydrogel composition, Hydrogels has good swelling ability, ie, quick water adsorption and retention properties.

[0009] Yet another object of the present invention is to provide a hydrogel composition, Hydrogels Since it has good biocompatibility, Hydrogels can be applied to the biomedical field. [Means for solving the problem]

[0010] In order to achieve the above object, the present invention provides a hydrogel composition, comprising modified HA, PEGDA, and water; based on the total weight of the hydrogel composition, the content of modified HA is 1 weight percent (wt%) to 7 wt%, and the content of PEGDA is 43 wt% to 49 wt%; the modified HA is obtained by modifying HA with methacrylic anhydride; and the average molecular weight of the PEGDA is 1 kDa to 10 kDa.

[0011] By adopting methacrylic anhydride modified HA and PEGDA with high average molecular weight as raw materials, and controlling the content of modified HA and PEGD within a specific range, the hydrogel composition of the present invention does not cause HA precipitation. That is, the above two raw materials have good compatibility, and the hydrogel composition can be further Hydrogels At the same time, the hydrogel composition of the present invention can form Hydrogels has the advantages of improved mechanical properties, good swelling ability, and good biocompatibility.

[0012] According to the present invention, HA refers to a disaccharide polymer, which contains N-acetylglucosamine and D-glucuronic acid linked by a β-1-3 glycosidic bond. The molecular formula of HA is (C 14 H 21 NO 11 ) n and the repeating unit of HA is represented by the following formula (a):

[0013] [ka] Formula (a)

[0014] According to the present invention, the above statement "the modified HA is obtained by modifying HA with methacrylic anhydride" indicates that after methacrylic anhydride reacts with HA, the methacrylate groups are linked to the hydroxyl groups of HA.

[0015] In some embodiments of the present invention, when HA is modified with methacrylic anhydride to obtain modified HA, the ratio of the number of moles of the methacrylic anhydride to the number of moles of the repeating units of HA may be 1 to 10. In some embodiments of the present invention, the ratio of the number of moles of the methacrylic anhydride to the number of moles of the repeating units of HA may be 1 to 4. In some embodiments of the present invention, the ratio of the number of moles of the methacrylic anhydride to the number of moles of the repeating units of HA may be 1 to 3. In some embodiments of the present invention, the ratio of the number of moles of the methacrylic anhydride to the number of moles of the repeating units of HA may be 2 to 3.

[0016] In some embodiments of the present invention, the ratio of methacrylate groups in the modified HA may be 20% to 55%. In some embodiments of the present invention, the ratio of methacrylate groups in the modified HA may be 20% to 50%. In some embodiments of the present invention, the ratio of methacrylate groups in the modified HA may be 20% to 40%. Specifically, the above "ratio of methacrylate groups in the modified HA" is: 1 H-nuclear magnetic resonance ( 1 The "ratio of methacrylate groups in modified HA" is obtained by dividing the total integral value of the measured hydrogen atoms of the methacrylate groups (chemical shift δ is about 5.56 and 6.06; the number of hydrogen atoms is 2) by the total integral value of the measured hydrogen atoms of the main chain of HA (chemical shift δ is about 3.0-4.5; the number of hydrogen atoms is 10).

[0017] In some embodiments of the present invention, the content of modified HA may be 2.5% to 7% by weight based on the total weight of the hydrogel composition. In some embodiments of the present invention, the content of modified HA may be 2.5% to 5% by weight based on the total weight of the hydrogel composition. In some embodiments of the present invention, the content of modified HA may be 4% to 6% by weight based on the total weight of the hydrogel composition.

[0018] In some embodiments of the present invention, the PEGDA content may be 43 wt% to 47.5 wt%, based on the total weight of the hydrogel composition. In some embodiments of the present invention, the PEGDA content may be 45 wt% to 47.5 wt%, based on the total weight of the hydrogel composition. In some embodiments of the present invention, the PEGDA content may be 44 wt% to 46 wt%, based on the total weight of the hydrogel composition.

[0019] In some embodiments of the present invention, the water content may be 40% to 60% by weight, based on the total weight of the hydrogel composition.In some embodiments of the present invention, the water content may be 44% to 56% by weight, based on the total weight of the hydrogel composition.

[0020] In some embodiments of the present invention, based on the total weight of the hydrogel composition, the content of modified HA may be 2.5 wt% to 5 wt%, the content of PEGDA may be 45 wt% to 47.5 wt%, and the ratio of the number of moles of the methacrylic anhydride to the number of moles of the repeating units of HA may be 1 to 3.

[0021] In some embodiments of the present invention, based on the total weight of the hydrogel composition, the content of modified HA may be 4 wt% to 6 wt%, the content of PEGDA may be 44 wt% to 46 wt%, and the ratio of the number of moles of the methacrylic anhydride to the number of moles of the repeating units of HA may be 1 to 3.

[0022] In some embodiments of the present invention, based on the total weight of the hydrogel composition, the content of modified HA may be 4 wt% to 6 wt%, the content of PEGDA may be 44 wt% to 46 wt%, and the ratio of the number of moles of the methacrylic anhydride to the number of moles of the repeating units of HA may be 2 to 3.

[0023] In some embodiments of the present invention, the average molecular weight of PEGDA may be from 4 kDa to 8 kDa.In some embodiments of the present invention, the average molecular weight of PEGDA may be from 5 kDa to 7 kDa.

[0024] In some embodiments of the invention, the average molecular weight of HA may be between 1 kDa and 200 kDa.

[0025] In some embodiments of the invention, the average molecular weight of HA may be between 1 kDa and 100 kDa.

[0026] Preferably, the hydrogel composition may further comprise a photoinitiator. The photoinitiator may be a compound that exhibits monomer polymerization, crosslinking, and hardening after exposure to light. For example, the photoinitiator may be, but is not limited to, lithium phenyl-2,4,6-trimethylbenzoylphosphinate (LAP), 2,4,6-trimethylbenzoyldiphenylphosphine oxide (also known as Irgacure TPO), 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone (also known as Irgacure 2959), or eosin Y. More preferably, the photoinitiator may be LAP.

[0027] In some embodiments of the present invention, the content of the photoinitiator may be 0.2% to 0.8% by weight based on the total weight of the hydrogel composition. In some embodiments of the present invention, the content of the photoinitiator may be 0.4% to 0.6% by weight based on the total weight of the hydrogel composition.

[0028] Furthermore, the present invention also provides a method for preparing a hydrogel composition, the method comprising: step (a): modifying HA with methacrylic anhydride to obtain modified HA; and step (b): mixing the modified HA, PEGDA, and water to obtain a hydrogel composition, in which, based on the total weight of the hydrogel composition, the content of the modified HA is 1 wt%-7 wt%, the content of the PEGDA is 43 wt%-49 wt%, and the average molecular weight of the PEGDA is 1 kDa-10 kDa.

[0029] By modifying HA with methacrylic anhydride to obtain modified HA in advance, and then mixing the modified HA with PEGDA having a high average molecular weight as raw materials, and controlling the contents of modified HA and PEGD within a certain range, the prepared hydrogel composition does not cause HA precipitation, that is, the raw materials have good compatibility, and the hydrogel composition can be further Hydrogels and at the same time, Hydrogels has the advantages of improved mechanical properties, good swelling ability, and good biocompatibility.

[0030] In some embodiments of the invention, in step (a), the ratio of the number of moles of the methacrylic anhydride to the number of moles of the repeating units of HA may be from 1 to 10; in some embodiments of the invention, the ratio of the number of moles of the methacrylic anhydride to the number of moles of the repeating units of HA may be from 1 to 4; in some embodiments of the invention, the ratio of the number of moles of the methacrylic anhydride to the number of moles of the repeating units of HA may be from 1 to 3; in some embodiments of the invention, the ratio of the number of moles of the methacrylic anhydride to the number of moles of the repeating units of HA may be from 2 to 3.

[0031] Preferably, in step (a), when HA is modified with methacrylic anhydride, the reaction time may be 20 hours to 30 hours, and the reaction temperature may be 0° C. to 8° C. More preferably, in step (a), when HA is modified with methacrylic anhydride, the reaction time may be 20 hours to 30 hours, and the reaction temperature may be 0° C. to 5° C.

[0032] Further, the present invention relates to a hydrogel composition formed from the hydrogel composition of the present invention. Hydrogels The present invention also provides Hydrogels has the advantages of improved mechanical properties, good swelling ability, and good biocompatibility, resulting in Hydrogels can be widely applied in various fields, especially in the biomedical field.

[0033] Preferably, Hydrogels has a Young's modulus of greater than 450 MPa. More preferably, Hydrogels has a Young's modulus of greater than 450 MPa and less than or equal to 700 MPa. Even more preferably, Hydrogels has a Young's modulus of 480 MPa or more and 700 MPa or less.

[0034] Preferably, Hydrogels The ultimate tensile strength (UTS) is greater than 13 MPa. More preferably, Hydrogels The ultimate tensile strength of is greater than 13 MPa and not more than 18 MPa. Even more preferably, Hydrogels The ultimate tensile strength of is 15 MPa or more and 18 MPa or less. Even more preferably, Hydrogels The ultimate tensile strength is 17 MPa or more and 18 MPa or less.

[0035] In this specification, a range expressed as "lower end value to upper end value" means that the range is equal to or greater than the lower end value and equal to or less than the upper end value, unless otherwise specified. For example, "the content is 1% by weight to 7% by weight" means that the content is "1% by weight or more and 7% by weight or less."

[0036] Other objects, advantages and novel features of the present disclosure will become more apparent from the following detailed description when taken in conjunction with the accompanying drawings. [Brief description of the drawings]

[0037] [Figure 1] 1H-NMR results of the modified HA of Preparation Example 4. [Diagram 2] 1 shows the results of a cell viability test of the hydrogel of Example 3A. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0038] Hereinafter, several preparation methods of the embodiment will be illustrated to describe the implementation of the present invention. Those skilled in the art can easily realize the advantages and effects of the present invention according to the contents of this specification. Various modifications and variations can be made to implement or apply the present invention without departing from the spirit and scope of the present invention.

[0039] Reagent Description 1. HA: purchased from Kewpie Corporation; average molecular weight is approximately 7 kDa 2. PEGDA: purchased from Sigma-Aldrich; average molecular weight approximately 6 kDa 3. Methacrylic anhydride: purchased from Sigma-Aldrich 4.LAP: purchased from Sigma-Aldrich 5. N,N-Dimethylacetamide (DMAC): purchased from Duksan Pure Chemicals Co., Ltd.

[0040] Preparation Examples 1 to 4 (PE1 to PE4): Modified HA 0.5 moles of HA and about 10 milliliters (mL) of deionized water were placed in a two-necked round-bottom flask, and then the flask was placed in a 4°C environment overnight to completely dissolve the HA in the deionized water. Next, about 6.7 mL of DMAC was added to the two-necked round-bottom flask. Then, depending on the difference in the ratio between the moles of methacrylic anhydride and the moles of the repeating units of HA listed in Table 1 below, an appropriate amount of methacrylic anhydride was added to the two-necked round-bottom flask, and then the solution was mixed uniformly. Next, 0.5 molar (M) NaOH was added to the mixed solution for titration, and the pH value of the mixed solution was controlled within the range of about 8 to 9 for 4 hours. Then, the mixed solution was placed in a 4°C environment, and the reaction was continuously stirred for about 20 hours.

[0041] After the reaction was completed, an appropriate amount of sodium chloride was added to the solution to make its concentration 0.5M. The solution was then mixed with ethanol in a volume ratio of 1:9 to produce a precipitate. The precipitate was then rinsed with ethanol to remove unreacted materials, and the precipitate was dissolved in deionized water to obtain a crude product. The crude product was then purified by dialysis in deionized water for 3 days, and then freeze-dried to obtain the modified HA of Preparation Examples 1-4.

[0042] [Table 1]

[0043] Furthermore, to confirm that the methacrylate group is contained in the modified HA of PE1 to PE4, the modified HA of PE4 was used as an example for explanation. 1 The denatured HA of PE4 was analyzed using a H-NMR spectrometer (manufacturer: Varian, Inc.; model: VNMRS 700MHz). 1The results of H-NMR are shown in Figure 1. The d-solvent used was DO. According to Figure 1, the obvious chemical shift peaks at about 1.86 ppm (i.e., labeled b in Figure 1), as well as 5.56 ppm and 6.06 ppm (i.e., labeled f in Figure 1) could prove that the methacrylate group was indeed linked to the structure of HA, and the chemical structure of the modified HA was expressed as the following formula (b): Furthermore, by calculating the ratio between the total integral value of the hydrogen molecules of the methacrylate group and the total integral value of the hydrogen atoms of the main chain of HA, the result was obtained that the ratio of the methacrylate group in the modified HA of PE4 was about 54.1%.

[0044] [ka] Formula (b)

[0045] Examples 1 to 5 (E1 to E5): Hydrogel Compositions According to the compositions and contents listed in Table 2 below, appropriate amounts of modified HA of PE1 to PE4, PEGDA and deionized water were prepared and then mixed uniformly to obtain the hydrogel compositions of Examples 1 to 5.

[0046] Comparative Example 1 (CE1): PEGDA solution According to Table 2 below, appropriate amounts of PEGDA and deionized water were uniformly mixed to obtain the PEGDA solution of Comparative Example 1. Based on the total weight of the PEGDA solution, the content of PEGDA was 50 wt%, and the rest was deionized water.

[0047] Comparative example 2 (CE2): HA / PEGDA solution According to Table 2 below, appropriate amounts of HA (unmodified HA), PEGDA and deionized water were uniformly mixed to obtain the HA / PEGDA solution of Comparative Example 2. Based on the total weight of the HA / PEGDA solution, the content of HA was 5 wt%, the content of PEGDA was 45 wt%, and the remainder was deionized water.

[0048] Comparative Examples 3 and 4 (CE3 and CE4): Hydrogel Compositions According to the composition and content listed in Table 2 below, appropriate amounts of PE2 modified HA, PEGDA and deionized water were prepared and then mixed uniformly to obtain the hydrogel compositions of Comparative Examples 3 and 4. The main difference between the hydrogel compositions of Comparative Examples 3 and 4 and the hydrogel compositions of Examples 1-5 was the different contents of modified HA and PEGDA.

[0049] [Table 2]

[0050] Analysis 1: Evaluation of raw material compatibility The hydrogel compositions E2 to E5 and the HA / PEGDA solution CE2 were used in this analysis. Specifically, the same amounts of the hydrogel compositions E2 to E5 and the HA / PEGDA solution CE2 were used and placed in different containers under the same conditions.

[0051] Next, the transparency of each group was observed with the naked eye, and obvious precipitation, i.e., HA precipitation, was observed in the HA / PEGDA solution of CE2. In other words, the HA / PEGDA solution of CE2 clearly had poor compatibility with the raw materials. On the other hand, no obvious precipitation was observed in the hydrogel compositions of E2 to E5. This indicates that all of the hydrogel compositions of E2 to E5 had good compatibility with the raw materials. Furthermore, the hydrogel composition of E5 had the best transparency, and therefore the best compatibility with the raw materials.

[0052] As a result, unlike the problem in the prior art that direct mixing of HA with PEGDA would result in HA precipitation, the hydrogel composition of the present invention employs HA modified with methacrylic anhydride and then mixed with PEGDA, thereby enhancing the compatibility of the raw materials and solving the problem of HA precipitation in PEGDA.

[0053] Examples 1A to 5A (E1A to E5A): Hydrogels Examples 1A to 5A adopt the hydrogel compositions of E1 to E5, respectively, and then add an appropriate amount of LAP as a photoinitiator so that the content reaches about 0.5 wt%. Then, each group of hydrogel compositions is placed into a mold and exposed to ultraviolet light (the light source is an LED with a wavelength of 390 nanometers (nm), and the light output is about 5 watts) for about 30 seconds to cause the hydrogel composition to undergo crosslinking reaction and subsequent curing, and the hydrogel compositions of Examples 1A to 5A are obtained. Hydrogels obtained.

[0054] Comparative examples 1A~4A (CE1A~CE4A): Hydrogels The manufacturing process of Comparative Examples 1A to 4A was almost the same as that of E1A to E5A. The main difference was that Comparative Examples 1A to 4A adopted a PEGDA solution of CE1, a HA / PEGDA solution of CE2, and a hydrogel composition of CE3 and CE4, respectively. The subsequent manufacturing process was the same as that of E1A to E5A, and Comparative Examples 1A to 4A Hydrogels obtained.

[0055] Analysis 2: Evaluation of mechanical properties E1A~E5A and CE1A~CE4A Hydrogels Specifically, E1A to E5A and CE1A to CE4A were used in this analysis. Hydrogels The samples were cut into samples with a length of about 30 millimeters (mm), a width of about 3 mm, and a height of about 0.5 mm. Each sample was then placed on an ElectroForce® 3200 Series III mechanical property tester, and the following conditions were selected for testing: a load cell of 225 Newtons (N) and an extension speed of 0.08 millimeters per minute (mm / min). The Young's modulus and ultimate tensile strength results for each group were then obtained and listed in Table 3 below. Young's modulus was obtained by calculating the slope of the linear elastic portion of the stress-strain curve. It indicates how difficult an object is to deform after a force is applied. In simple terms, the higher the Young's modulus, the more difficult the object is to deform after a force is applied. The ultimate tensile strength was the force measured when the object was stretched to break.

[0056] [Table 3]

[0057] According to the results in Table 3 above, E1A to E5A Hydrogels The Young's modulus of the CE1A prepared from the PEGDA solution was more than 450 MPa. Hydrogels , or CE2A formed from HA / PEGDA solution. Hydrogels Compared to E1A~E5A Hydrogels The Young's modulus of the HA was obviously high. That is, the present invention adopts HA modified with methacrylic anhydride and then mixed with PEGDA to obtain a HA-modified ... Hydrogels Since it forms Hydrogels actually has better mechanical strength.

[0058] Further comparison with the results of CE3A and CE4A shows that Hydrogels also employed HA modified with methacrylic anhydride and then mixed with PEGDA, but the CE3A Hydrogels For CE4A, the content of modified HA was 10 wt% and the content of PEGDA was 40 wt%; Hydrogels The modified HA content was 15 wt% and the PEGDA content was 35 wt%. That is, the raw material contents of CE3A and CE4A did not meet the specific ranges claimed in the present invention. Therefore, the content of CE3A was 15 wt% and the content of PEGDA was 35 wt%. Hydrogels The Young's modulus of CE4A is only 378.79 MPa, Hydrogels The Young's modulus of E1A to E5A is only 74.39 MPa. Hydrogels The Young's modulus was clearly worse than that of

[0059] Furthermore, the ultimate tensile strength results for E1A to E5A Hydrogels All of them are over 13MPa, and E1A to E5A Hydrogels had ultimate tensile strengths approaching or even exceeding those of CE1A. Furthermore, E1A-E5A had ultimate tensile strengths approaching or even exceeding those of CE2A-CE4A. Hydrogels had a clearly higher ultimate tensile strength.

[0060] Therefore, the present invention employs HA modified with methacrylic anhydride and PEGDA as raw materials, and further controls the content of the above raw materials within a specific range. Hydrogels actually had better Young's modulus results and close or better ultimate tensile strength results. Hydrogels indeed had improved mechanical properties.

[0061] Analysis 3: Evaluation of swelling capacity E1A~E5A Hydrogels were used in this analysis. Specifically, Hydrogels The samples were cut into cylindrical samples with a diameter of about 15 mm and a thickness of about 0.5 mm. The samples were then immersed in 5 mL of deionized water, and the weights of the samples were measured when the samples were immersed in deionized water for 30 seconds, 3 minutes, 5 minutes, 10 minutes, 15 minutes, 20 minutes, 30 minutes, and 60 minutes. The weights of the samples measured at different immersion times were then compared with the weights of the samples before immersion in water to obtain the swelling ratios of each group after immersion in water for different times, which were then used to calculate the swelling ratios of each group. Hydrogels The swelling ability of the different groups was evaluated after immersion in water for different times. The swelling ratio results for different groups after immersion in water for different times are listed in Table 4 below. The swelling ratio was obtained by the following formula: [(sample weight after immersion in water-sample weight before immersion in water) / sample weight before immersion in water x 100%]

[0062] [Table 4]

[0063] According to the results shown in Table 4 above, E1A to E5A Hydrogels All of E1A to E5A had swelling rates of over 200% after about 5 minutes of water immersion. In addition, when immersed in water for a longer period (about 10 minutes to 60 minutes), Hydrogels The swelling ratio of E1A to E5A was still more than 200%, and the swelling ratio was almost constant. Hydrogels It has been shown that the cellulose acylate has the characteristics of rapid water adsorption and long-term water retention. Hydrogels indeed had good swelling ability.

[0064] Analysis 4: Biocompatibility assessment E3A Hydrogels was employed in this analysis, and PrestoBlue reagent was used to test cell viability and evaluate biocompatibility. Hydrogels was immersed in deionized water to allow its swelling rate to reach a fixed value, and then cut into a cylindrical specimen with a diameter of about 6 mm and a thickness of about 0.5 mm. Next, for sterilization, the specimen was immersed in 30% ethanol and then placed under ultraviolet light. After that, the specimen was taken out and washed with phosphate buffer, and then placed in a 96-well cell culture dish, after which 200 microliters (μL) of Ham's F12 medium was added. At the same time, HIG-82 cells (cells isolated from the synovial membrane of the knee joint of rabbits) were transfected at a density of about 5 × 10 4 The cells were placed in another 96-well cell culture dish at a cell concentration of 1000 cells / mL and then cultured for one day at about 37°C in an environment of about 5% CO2. The samples immersed in Ham's F12 medium were then removed and added to the 96-well cell culture dish in which HIG-82 cells had been cultured, and then cultured for one day.

[0065] After the above culture was completed, Ham's F12 medium was removed from the 96-well cell culture dish, and then 100 μL of PrestoBlue solution (PrestoBlue reagent mixed with Ham's F12 at a volume ratio of 1:9) was added, and then cultured at about 37° C. in an environment of about 5% CO2 for 1.5 hours. Then, the PrestoBlue solution was taken out and analyzed by an enzyme-linked immunosorbent assay (ELISA) reader (manufacturer: Molecular Devices; model: SpectraMax M2) to measure the absorbance at wavelengths of 570 nm and 600 nm, and calculate the reduction rate of PrestoBlue. The higher the reduction rate of PrestoBlue, the higher the cell viability and the better the biocompatibility of the sample. The results of E3A are shown in FIG. 2; here, HIG-82 cells without any treatment were set as the control group, and each group was the result of five repeated experiments. The reduction rate of PrestoBlue was obtained by the following formula: In the formula, the test group represents the above group treated with the sample, and the control group and negative group represent groups that underwent the same experimental steps as above but did not contain HIG-82 cells.

[0066] TIFF0007590787000007.tif15150 TIFF0007590787000008.tif22150C RED : Concentration of reduced PrestoBlue (red) C OX : Concentration of oxidized PrestoBlue (blue) ε OX λ 570 : Molar absorption coefficient of oxidized PrestoBlue at a wavelength of 570 nm ε OX λ 600 : Molar absorption coefficient of oxidized PrestoBlue at a wavelength of 600 nm ε RED λ 570 : Molar absorption coefficient of reduced PrestoBlue at a wavelength of 570 nm ε RED λ 600 : Molar absorption coefficient of reduced PrestoBlue at a wavelength of 600 nm A: Absorbance of the test group (containing medium, sample, cells and PrestoBlue reagent) A': Absorbance of the negative control (containing medium, sample, and PrestoBlue reagent)

[0067] As shown in Figure 2, the reduction rate of PrestoBlue in the E3A and control groups was almost the same. This indicates that the cell viability of the E3A and control groups was almost the same. Hydrogels did not release any substances that were toxic, infectious, or stimulated the cells to become inflamed and cause cell death. Hydrogels indeed had good biocompatibility.

[0068] In summary, the present invention uses modified HA and PEGDA with a high average molecular weight as raw materials, and by controlling the content of the raw materials, a hydrogel composition with excellent compatibility with the raw materials can be obtained. Hydrogels After forming Hydrogels has good mechanical properties, good swelling ability and good biocompatibility at the same time, so that Hydrogelscan be applied in many fields, especially in the biomedical field, and thus has high development potential and value.

[0069] Although numerous features and advantages of the present invention have been described hereinbefore, together with details of the structure and characteristics of the invention, this disclosure is merely illustrative, and changes may be made in details, particularly in matters of shape, size and arrangement of parts, within the scope of the principles of the invention to the full extent indicated by the broad general meaning of the terms in which the appended claims are expressed.

Claims

1. A hydrogel composition comprising modified hyaluronic acid, poly(ethylene glycol) diacrylate, and water, the content of the modified hyaluronic acid being 1% to 7% by weight, the content of the poly(ethylene glycol) diacrylate being 43% to 49% by weight, based on the total weight of the hydrogel composition, the modified hyaluronic acid being obtained by modifying hyaluronic acid with methacrylic anhydride, and the average molecular weight of the poly(ethylene glycol) diacrylate being 1 kDa to 10 kDa.

2. 2. The hydrogel composition according to claim 1, characterized in that the ratio of the number of moles of methacrylic anhydride to the number of moles of repeating units of hyaluronic acid is 1-10.

3. 2. The hydrogel composition of claim 1, wherein the poly(ethylene glycol) diacrylate has an average molecular weight of 4 kDa to 8 kDa.

4. 2. The hydrogel composition according to claim 1, wherein the average molecular weight of the hyaluronic acid is from 1 kDa to 200 kDa.

5. The hydrogel composition according to any one of claims 1 to 4, further comprising a photoinitiator.

6. 1. A method for making a hydrogel composition, comprising: Step (a): modifying hyaluronic acid with methacrylic anhydride to obtain modified hyaluronic acid; Step (b): mixing the modified hyaluronic acid, poly(ethylene glycol) diacrylate, and water to obtain the hydrogel composition. Including, The method according to claim 1, wherein the content of the modified hyaluronic acid is 1% to 7% by weight, the content of the poly(ethylene glycol) diacrylate is 43% to 49% by weight, and the average molecular weight of the poly(ethylene glycol) diacrylate is 1 kDa to 10 kDa, based on the total weight of the hydrogel composition.

7. The method according to claim 6, wherein the ratio of the number of moles of methacrylic anhydride to the number of moles of the repeating units of hyaluronic acid is 1 to 10.

8. The method according to claim 6, characterized in that in step (a), when hyaluronic acid is modified with methacrylic anhydride, the reaction time is 20 hours to 30 hours, and the reaction temperature is 0°C to 8°C.

9. A hydrogel, characterized in that it is formed from a hydrogel composition described in any one of claims 1 to 4.

10. 10. The hydrogel of claim 9, wherein the hydrogel has a Young's modulus greater than 450 MPa.

Citation Information

Patent Citations

  • Composite material as well as preparation method and application thereof

    CN111743784A

  • Bone marrow mesenchymal stem cell / degradable hydrogel composite material as well as preparation method and application thereof

    CN114146226A

  • Degradable embolism microsphere and preparation method thereof

    CN115245591A

  • Composite hydrogel based on biological ionic liquid polymerization and preparation method thereof

    CN116173290A

  • Production, raw materials, products and uses of photocrosslinkable hydrogel materials