Active energy ray-curable composition and coating member
A curable composition with specific components and ratios forms a scratch-resistant, adherent coating film that mimics glass glaze, addressing the issues of low hardness and poor adhesion in existing top coats, without requiring high-temperature firing.
Patent Information
- Application Number
- JP2021107347
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-06-29
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2041-06-29
AI Technical Summary
Existing top coats formed from a coating composition with a (meth)acrylate, hydrophobic nanosilica, and glass filler have low hardness, are easily scratched, and may peel off from the base material due to poor adhesion, especially on materials like ceramics and electronic device casings.
A curable composition comprising urethane (meth)acrylate, (meth)acrylate compounds, polyfunctional thiol, polysiloxane, and hydrophobic silica, with specific component ratios, is cured with active energy rays to form a coating film that mimics glass glaze in texture, is resistant to scratches, and exhibits excellent adhesion.
The coating film achieves high hardness, resistance to scratches, and strong adhesion to various substrates, including ceramics and electronic device casings, while reducing the need for high-temperature firing processes.
Smart Images

Figure 0007590933000003 
Figure 0007590933000001 
Figure 0007590933000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an active energy ray-curable composition and a coating member. [Background technology]
[0002] For example, glass glaze is sometimes baked onto the parts of consumer goods that are visible to the user, such as the exterior materials of ceramics and home appliances, and the housings of electronic devices, for various purposes, such as improving stain resistance, improving scratch resistance, and creating a sense of luxury. However, firing of glass glaze requires heating at high temperatures, which poses problems such as a large amount of energy consumption in the firing process and a long firing time.
[0003] In response to such problems, a technique has been proposed for forming a coating film on the surface of a substrate using a coating agent mainly composed of an organic resin. For example, Patent Document 1 describes an active energy ray-curable coating composition for topcoat, which contains (A) a (meth)acrylate having an isocyanurate skeleton, (B) a polyfunctional (meth)acrylate other than (A), hydrophobic nanosilica (C), glass filler (D), and photopolymerization initiator (E), and is characterized in that the average particle size of (D) is 5 to 18 μm. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2020-152741 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the topcoat obtained by curing the coating composition of Patent Document 1 has a problem in that it has low hardness and is easily scratched. In addition, the topcoat of Patent Document 1 may have poor adhesion to some substrates, and may easily peel off from the substrate.
[0006] The present invention has been made in view of the above background, and aims to provide an active energy ray-curable composition capable of forming a coating film having a texture similar to that of glass glaze, which is resistant to scratches and has excellent adhesion to a substrate, and a coating member formed using the active energy ray-curable composition. [Means for solving the problem]
[0007] One aspect of the present invention is a composition comprising a component A consisting of a urethane (meth)acrylate; Component B consisting of a (meth)acrylate compound; A component C consisting of a multifunctional thiol; Component D consisting of polysiloxane; and an E component consisting of silica, The component A contains a urethane (meth)acrylate having three or more (meth)acryloyl groups in one molecule, The component B contains a (meth)acrylate compound having three or more (meth)acryloyl groups in one molecule, The component C contains a multifunctional thiol having 2 to 4 thiol groups in one molecule, The component D contains polysilsesquioxane, The component E contains hydrophobic silica having a hydrophobicity of 20% or more as measured by a methanol titration method, With respect to 100 parts by mass in total of the contents of the A component to the E component, the content of the A component is 30 parts by mass or more, the content of the B component is 0 parts by mass or more and 45 parts by mass or less, the total content of the A component and the B component is 60 parts by mass or more and 94 parts by mass or less, the content of the C component is 0.5 parts by mass or more and 30 parts by mass or less, and the content of the D component is 0.5 parts by mass or more. 1 part by mass or less the total content of the C component and the D component is 5 parts by mass or more, and the content of the E component is 0.5 parts by mass or more and 10 parts by mass or less.
[0008] Another aspect of the present invention is a substrate, A coating member having a coating film provided on the substrate, The coating film is a coating member made of a cured product of the active energy ray-curable composition of the above embodiment. Effect of the Invention
[0009] The active energy ray curable composition (hereinafter referred to as "curable composition") contains component A consisting of urethane (meth)acrylate, component B consisting of a (meth)acrylate compound, component C consisting of a multifunctional thiol, component D consisting of a polysiloxane, and component E consisting of silica, and the contents of these components are within the above-mentioned specific ranges. By curing components A to E of the curable composition with active energy rays, it is possible to form a coating film that has a texture similar to that of glass glaze, is resistant to scratches, and has excellent adhesion to the substrate.
[0010] In addition, a coating film made of a cured product of the curable composition is formed on the surface of the coating member. Therefore, the coating member has a texture similar to that of glass glaze. In addition, since the coating film is formed on the surface of the coating member, the surface of the coating member is less likely to be scratched. Furthermore, the coating film has excellent adhesion to the substrate.
[0011] As described above, according to the above-described aspect, it is possible to provide a curable composition capable of forming a coating film having a texture similar to that of glass glaze, which is resistant to scratches and has excellent adhesion to a substrate, and a coating member formed using the curable composition. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a cross-sectional view of a coating member in Example 1. As shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] (Active energy ray-curable composition) The function of each component contained in the curable composition and the reasons for limiting the content thereof will be described in detail below.
[0014] [Component A] The curable composition contains, as an essential component, component A consisting of urethane (meth)acrylate. The curable composition may contain one type of urethane (meth)acrylate, or may contain two or more types of urethane (meth)acrylate. The urethane (meth)acrylate is polymerized by active energy rays together with the (meth)acrylate compound, which is component B, to form the basic skeleton of the coating film.
[0015] The content of the A component in the curable composition may be 30 parts by mass or more relative to 100 parts by mass of the total content of the A component to the E component, and the total content of the A component and the B component may be in the range of 60 parts by mass or more and 94 parts by mass or less relative to 100 parts by mass of the total content of the A component to the E component. That is, for example, when the B component is not contained in the curable composition, the content of the A component may be in the range of 60 parts by mass or more and 94 parts by mass or less relative to 100 parts by mass of the total content of the A component to the E component. On the other hand, when the B component is blended in the curable composition, a part of the A component can be replaced with the B component. For example, when the B component is contained in the curable composition, the content of the A component may be set to 30 parts by mass or more relative to 100 parts by mass of the total content of the A component to the E component, and the total content of the A component and the B component may be set to 60 parts by mass or more and 94 parts by mass or less.
[0016] The hardness of the coating film can be improved by making the content of the A component in the curable composition 30 parts by mass or more relative to 100 parts by mass of the total content of the A component to the E component. If the content of the A component is less than 30 parts by mass relative to 100 parts by mass of the total content of the A component to the E component, the hardness of the coating film may be reduced. From the viewpoint of further increasing the hardness of the coating film, the content of the A component is preferably 32 parts by mass or more, more preferably 35 parts by mass or more relative to 100 parts by mass of the total content of the A component to the E component.
[0017] In addition, the curable composition can be easily cured by making the total content of the A component and the B component in the curable composition 60 parts by mass or more relative to 100 parts by mass of the total content of the A component to the E component. If the total content of the A component and the B component is less than 60 parts by mass relative to 100 parts by mass of the total content of the A component to the E component, the curability of the curable composition may be deteriorated. From the viewpoint of more reliably avoiding deterioration in the curability of the coating film, the total content of the A component and the B component is preferably 64 parts by mass or more, more preferably 65 parts by mass or more, relative to 100 parts by mass of the total content of the A component to the E component.
[0018] On the other hand, if the total content of the A component and the B component is too high, the proportion of other components in the curable composition will be low, which may lead to deterioration of the adhesion and antifouling properties of the coating film. By making the total content of the A component and the B component 94 parts by mass or less, preferably 87.5 parts by mass or less, and more preferably 82 parts by mass or less, relative to 100 parts by mass of the total content of the A component to the E component, a coating film with excellent adhesion and antifouling properties can be easily obtained.
[0019] When the curable composition contains the B component, the content of the A component is preferably 30 parts by mass or more and 63 parts by mass or less, more preferably 32 parts by mass or more and 52 parts by mass or less, and even more preferably 35 parts by mass or more and 45 parts by mass or less, relative to 100 parts by mass of the total of the A components to the E components. In this case, the amount of organic solvent in the curable composition can be reduced, or the curable composition can be prepared without adding any organic solvent. By using such a curable composition, a coating film can be easily formed even on a substrate made of a material that is easily dissolved in an organic solvent, such as plastic.
[0020] The urethane (meth)acrylate used as component A has a structural unit derived from an isocyanate and a structural unit derived from a (meth)acrylate compound in its molecular structure. In the molecular structure of the urethane (meth)acrylate, these structural units are bonded to each other via urethane bonds.
[0021] Examples of structural units derived from isocyanates in urethane (meth)acrylates include structural units derived from aromatic diisocyanates such as toluene diisocyanate (TDI) and diphenylmethane diisocyanate (MDI), structural units derived from aliphatic diisocyanates such as hexamethylene diisocyanate (HDI) and isophorone diisocyanate (IPDI), structural units derived from diisocyanate polymers such as biuret polyisocyanates and isocyanurate polyisocyanates, structural units derived from adduct polyisocyanates, and structural units derived from urethane prepolymers obtained by reacting polyisocyanates with polyols.
[0022] Examples of the structural unit derived from a (meth)acrylate compound in the urethane (meth)acrylate include a structural unit derived from acrylic acid, a structural unit derived from a monofunctional acrylic acid ester such as methyl acrylate, butyl acrylate, or isobutyl acrylate, 1,3-butylene glycol diacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, diethylene glycol diacrylate, trimethylolpropane triacrylate, ethoxylated trimethylolpropane triacrylate, propoxylated trimethylolpropane triacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, and dipentaerythritol pentaacrylate. structural units derived from polyfunctional acrylates such as acrylate, structural units derived from methacrylic acid, structural units derived from monofunctional methacrylates such as methyl methacrylate and butyl methacrylate, structural units derived from polyfunctional methacrylates such as 1,3-butylene glycol dimethacrylate, 1,4-butanediol dimethacrylate, 1,6-hexanediol dimethacrylate, diethylene glycol dimethacrylate, trimethylolpropane trimethacrylate, pentaerythritol trimethacrylate, pentaerythritol tetramethacrylate, and pentaerythritol pentamethacrylate, and structural units derived from oligomers of the above-mentioned (meth)acrylate monomers.
[0023] In addition, as component A, commercially available urethane (meth)acrylates such as "UV-1700B" manufactured by Mitsubishi Chemical Corporation, "CN9006NS" manufactured by Sartomer, and "UA-306H" and "UA-306T" manufactured by Kyoei Chemical Co., Ltd. can also be used.
[0024] The curable composition preferably contains a urethane (meth)acrylate having three or more (meth)acryloyl groups in one molecule as component A. Examples of such urethane (meth)acrylate include "CN9006NS" manufactured by Sartomer Corporation and urethane prepolymers obtained by condensing pentaerythritol triacrylate and diisocyanate (for example, "UA-306H" and "UA-306T" manufactured by Kyoei Chemical Co., Ltd.).
[0025] By using a multifunctional urethane (meth)acrylate with three or more (meth)acryloyl groups in one molecule as component A, it is possible to easily form a network-like structure in the coating film in which components A are bonded to each other or to other components, which results in a coating film that is harder and more resistant to scratches.
[0026] [B component] The curable composition may contain, as an optional component, a component B consisting of a (meth)acrylate compound. The curable composition may contain one type of (meth)acrylate compound, or may contain two or more types of (meth)acrylate compounds. The (meth)acrylate compound, like the urethane (meth)acrylate that is the component A, is polymerized by active energy rays and incorporated into the basic skeleton of the coating film. Therefore, in the curable composition, a part of the component A can be replaced with the component B.
[0027] The content of component B is 0 to 45 parts by mass relative to 100 parts by mass of the total content of components A to E, and the total of the content of components A and B is 60 to 94 parts by mass relative to 100 parts by mass of the total content of components A to E. If the content of component B is excessively high, the curability of the coating film may be deteriorated. By setting the content of component B to preferably 45 parts by mass or less, more preferably 43 parts by mass or less, and even more preferably 40 parts by mass or less relative to 100 parts by mass of the total content of components A to E, deterioration of the curability can be more reliably avoided.
[0028] As the (meth)acrylate compound, a (meth)acrylate monomer, an oligomer of a (meth)acrylate monomer, or the like can be used. As the (meth)acrylate monomer, for example, acrylic acid and methacrylic acid can be used. As the (meth)acrylate monomer, a polyfunctional (meth)acrylate compound such as triethylene glycol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, pentaerythritol penta(meth)acrylate, or ethoxylated trimethylolpropane triacrylate can also be used.
[0029] As the oligomer of the (meth)acrylate monomer, for example, the dimer or trimer of the above-mentioned (meth)acrylate monomer can be used. These (meth)acrylate compounds may be used alone, or two or more kinds of (meth)acrylate compounds may be used in combination.
[0030] The curable composition preferably contains a (meth)acrylate compound having three or more (meth)acryloyl groups in one molecule as component B. Examples of such (meth)acrylate compounds include "SR444", "SR295", "SR399NS" and "SR454NS" manufactured by Sartomer Corporation.
[0031] By using a polyfunctional (meth)acrylate compound with three or more (meth)acryloyl groups in one molecule as component B, it is possible to easily form a structure in the coating film in which components B are bonded to each other or to other components in a network shape, which results in a coating film with increased hardness and greater resistance to scratches.
[0032] In addition, the curable composition preferably contains a (meth)acrylate monomer as component B. Since the (meth)acrylate monomer has a lower viscosity than component A, the amount of organic solvent added for viscosity adjustment can be reduced by adding the (meth)acrylate monomer to the curable composition, or the curable composition can be prepared without adding any organic solvent. By using such a curable composition, a coating film can be easily formed even on a substrate made of a material that is easily affected by organic solvents, such as plastics.
[0033] In addition, in a curable composition containing a small amount of organic solvent or a curable composition containing no organic solvent, the amount of organic solvent volatilized from the curable composition applied to a substrate can be reduced or the volatilization of the organic solvent can be prevented. Such a curable composition is also effective in reducing the environmental load.
[0034] From the viewpoint of more reliably obtaining these effects, the content of component B is preferably 30 parts by mass or more per 100 parts by mass of the total content of components A to E.
[0035] [C component] The curable composition contains, as an essential component, a component C consisting of a polyfunctional thiol. The curable composition may contain one type of polyfunctional thiol, or may contain two or more types of polyfunctional thiol. The polyfunctional thiol has the effect of improving the reaction rate of the double bond contained in the component A, etc., when the curable composition is cured. In addition, when the curable composition is cured, if the curable composition is irradiated with active energy rays, peroxide radicals may be generated in the curable composition. However, in the reaction between the polyfunctional thiol and the double bond (the so-called ene-thiol reaction), the thiol group in the polyfunctional thiol can be reacted with the peroxide radical to form a thiyl radical. This can suppress the occurrence of effect inhibition caused by the peroxide radical.
[0036] The content of the C component in the curable composition may be in the range of 0.5 parts by mass or more and 30 parts by mass or less per 100 parts by mass of the total content of the A component to the E component, and the total content of the C component and the D component may be in the range of 5 parts by mass or more per 100 parts by mass of the total content of the A component to the E component. By setting the content of the C component in the curable composition within the above-mentioned specific range, the curability of the curable composition is improved. In addition, in this case, the shrinkage of the coating film during the curing process can be suppressed. Furthermore, such a curable composition can increase the crosslink density of the coating film and form a stronger coating film.
[0037] From the viewpoint of more reliably obtaining the above-mentioned action and effect, the content of component C in the curable composition is preferably 10 parts by mass or more, and more preferably 15 parts by mass or more, per 100 parts by mass of the total content of components A to E. If the content of component C is less than 0.5 parts by mass per 100 parts by mass of the total content of components A to E, the effect of component C in improving curability becomes insufficient, which may lead to deterioration in the curability and impact resistance of the curable composition.
[0038] Furthermore, if the total content of component C and content of component D is less than 5 parts by mass per 100 parts by mass of the total content of components A to E, the hardness of the coating film may decrease.
[0039] On the other hand, if the content of component C is excessively high, the hardness of the coating film may decrease. By setting the content of component C to 30 parts by mass or less, preferably 25 parts by mass or less, per 100 parts by mass of the total content of components A to E, such a problem can be easily avoided.
[0040] The polyfunctional thiol used as component C has two or more thiol groups (-SH) in one molecule. Examples of the polyfunctional thiol include bifunctional thiols such as 1,4-bis(3-mercaptobutyryloxy)butane, trifunctional thiols such as 1,3,5-tris[2-(3-mercaptobutyryloxy)ethyl]-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, and tetrafunctional thiols such as pentaerythritol tetrakis(3-mercaptobutyrate).
[0041] The curable composition preferably contains a polyfunctional thiol having 2 to 4 thiol groups in one molecule as component C. Examples of such polyfunctional thiols include "Karenz MT BD1", "Karenz MT PE1" and "Karenz MT NR1" manufactured by Showa Denko K.K. Incidentally, "Karenz MT" is a registered trademark of Showa Denko K.K.
[0042] By using a polyfunctional thiol having 2 to 4 thiol groups in one molecule as the C component, the amount of sulfur atoms contained in the coating film can be increased, and the refractive index of the coating film can be increased. As a result, the texture of the coating film can be made closer to glass glaze. In addition, by increasing the number of thiol groups in the polyfunctional thiol, hydrogen bonds are easily formed between the thiol groups and the hydroxyl groups. As a result, the adhesion between the coating film and a substrate having a hydroxyl group, such as ceramics, can be further improved. From the viewpoint of further enhancing these effects, it is more preferable that the curable composition contains a polyfunctional thiol having 3 to 4 thiol groups in one molecule as the C component.
[0043] [D component] The curable composition contains at least one type of polysiloxane as component D. Polysiloxane has excellent affinity with the organic components in the coating film, and has the effect of improving the adhesion between the coating film and the substrate. In addition, since polysiloxane also has excellent affinity with the inorganic components in the coating film, the combination of polysiloxane and silica (component E) can suppress the aggregation of silica in the curable composition and suppress the increase in viscosity of the curable composition. In addition, the combination of polysiloxane and silica can disperse silica in the coating film and strengthen the structure of the coating film.
[0044] The content of component D in the curable composition may be in the range of 0.5 to 5 parts by mass per 100 parts by mass of the total content of components A to E, and the total content of component C and component D may be in the range of 5 parts by mass or more per 100 parts by mass of the total content of components A to E. By setting the content of component D in the curable composition within the above specific range, it is possible to improve the adhesion between the curable composition and a substrate.
[0045] From the viewpoint of more reliably obtaining the above-mentioned action and effect, the content of component D in the curable composition is preferably 1 part by mass or more per 100 parts by mass of the total content of components A to E. If the content of component D is less than 0.5 parts by mass per 100 parts by mass of the total content of components A to E, this may lead to a deterioration in adhesion between the curable composition and the substrate.
[0046] On the other hand, if the content of component D is excessively high, the curing reaction of the curable composition is likely to be hindered by component D, which may lead to a decrease in the hardness of the coating film. By setting the content of component D to 5 parts by mass or less, preferably 4 parts by mass or less, and more preferably 3 parts by mass or less, per 100 parts by mass of the total content of components A to E, such problems can be easily avoided.
[0047] The polysiloxane used as component D may be a compound having a main chain formed by repeating siloxane bonds (-O-Si-). The curable composition may contain one type of polysiloxane, or may contain two or more types of polysiloxane. Examples of polysiloxane include linear polysiloxane, branched polysiloxane, cyclic polysiloxane, polysilsesquioxane, etc.
[0048] It is preferable that component D contains polysilsesquioxane. By using polysilsesquioxane as component D, the adhesion between the coating film and the substrate can be further improved and the structure of the coating film can be further strengthened. From the same viewpoint, it is more preferable that component D is made of polysilsesquioxane.
[0049] Polysilsesquioxane is a condensate obtained by hydrolysis of a silane compound containing a trifunctional silane. Examples of silane compounds used in the synthesis of polysilsesquioxane include phenyltriethoxysilane, trimethoxy(1-phenylethyl)silane, trimethoxy(2-phenylethyl)silane, (1E,4E)-1-(4-hydroxy-3,5-dimethoxyphenyl)-5-(3,4,5-trimethoxyphenyl)-1,4-pentadiene-3-one, trimethoxy(4-vinylphenyl)silane, trimethoxy(4-methoxyphenyl)silane, phenyltrimethoxysilane, silanes having a phenyl group such as benzyltriethoxysilane, methyltriethoxysilane, dodecyltrimethoxysilane, octadecyltriethoxysilane, n-octyltriethoxysilane, cyclohexyldimethoxymethylsilane, cyclohexyltrimethoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, ethyltrimethoxy ... methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltri Examples of the silane compounds include silanes having an alkyl group such as butyltriethoxysilane, ethyltriethoxysilane, decyltrimethoxysilane, decyltriethoxysilane, hexadecyltrimethoxysilane, hexadecyltriethoxysilane, propyltrimethoxysilane, propyltriethoxysilane, cyclopentyltrimethoxysilane, butyltriethoxysilane, isooctyltriethoxysilane, and isobutyltriethoxysilane; silanes having an unsaturated bond such as trimethoxy(4-vinylphenyl)silane, vinyltrimethoxysilane, 3-(trimethoxysilyl)propyl acrylate, 3-(triethoxysilyl)propyl methacrylate, allyltriethoxysilane, and allyltrimethoxysilane; and silanes having a mercapto group such as (3-mercaptopropyl)triethoxysilane (MPTES) and (3-mercaptopropyl)trimethoxysilane. These silane compounds may be used alone, or two or more types of silane compounds may be used in combination.
[0050] [E component] The curable composition contains at least one type of silica as component E. Since silica has a high affinity with polysiloxane (component D), the use of silica in combination with polysiloxane can suppress the aggregation of silica in the curable composition. As a result, the increase in viscosity of the curable composition can be suppressed, and the structure of the coating film can be strengthened and the abrasion resistance can be improved.
[0051] The content of component E in the curable composition is from 0.5 to 10 parts by mass, based on 100 parts by mass of the total content of components A to E. By setting the content of component E in the curable composition within the above-mentioned specific range, the structure of the coating film can be strengthened, and impact resistance and abrasion resistance can be improved.
[0052] From the viewpoint of more reliably obtaining the above-mentioned action and effect, the content of component E in the curable composition is preferably 1.5 parts by mass or more, and more preferably 2 parts by mass or more, per 100 parts by mass of the total content of components A to E. If the content of component E is less than 0.5 parts by mass per 100 parts by mass of the total content of components A to E, the impact resistance and abrasion resistance of the coating film may be deteriorated.
[0053] On the other hand, if the content of component E is excessively high, the toughness of the coating film may decrease, and the coating film may be easily cracked when subjected to impact. By setting the content of component E to 10 parts by mass or less, preferably 5 parts by mass or less, and more preferably 3 parts by mass or less, relative to 100 parts by mass of the total content of components A to E, such problems can be easily avoided.
[0054] The silica used as component E may be hydrophilic silica or hydrophobic silica. From the viewpoint of improving the antifouling property of the coating film, component E is preferably hydrophobic silica having a hydrophobicity of 20% or more by methanol titration method. By using hydrophobic silica as component E, the affinity between the coating film and dirt can be reduced. As a result, dirt can be easily removed from the coating film.
[0055] Specifically, the method for calculating the hydrophobicity by the methanol titration method is as follows. First, silica is dropped onto a methanol aqueous solution whose methanol concentration is known, and the silica floats on the liquid surface. From this state, methanol is dropped into the methanol aqueous solution, and the methanol concentration in the methanol aqueous solution is gradually increased. The methanol concentration in the methanol aqueous solution at the time when the silica settles from the liquid surface of the methanol aqueous solution is taken as the hydrophobicity. In other words, the hydrophobicity by the methanol titration method is a value expressed as a percentage (unit: %) of the ratio of the volume of methanol (unit: mL) in the methanol aqueous solution to the total volume (unit: mL) of the methanol aqueous solution at the time when the silica settles.
[0056] The hydrophobic silica having such characteristics can be obtained by, for example, carrying out surface treatment on silica particles using a surface treatment agent having a hydrophobic functional group.The silica particles to be surface-treated can be spherical silica particles or amorphous silica particles.For example, the surface treatment agent can be a silane coupling agent having a hydrophobic functional group such as methyltrimethoxysilane, hexamethyldisilazane, or phenyltrimethoxysilane.
[0057] As the hydrophobic silica, for example, commercially available products such as "QSG-30" manufactured by Shin-Etsu Chemical Co., Ltd., "MSP-011" manufactured by Teika Corporation, "AEROSIL NAX50" manufactured by Nippon Aerosil Co., Ltd., and "YA050C-SP3" manufactured by Admatechs Co., Ltd. can also be used. "AEROSIL" is a registered trademark of Evonik Operations GmbH.
[0058] The average primary particle size of silica is preferably more than 15 nm and less than 100 nm. In this case, the tear strength of the coating film can be further improved, and the abrasion resistance can be further improved. From the viewpoint of further enhancing such effects, the average primary particle size of silica is preferably 20 nm or more and 90 nm or less, and more preferably 25 nm or more and 80 nm or less. The average primary particle size of silica is a value calculated by a laser diffraction / scattering method.
[0059] [Active energy ray polymerization initiator] The curable composition is configured to be cured by irradiation with active energy rays. For example, the curable composition may contain an active energy ray polymerization initiator (hereinafter referred to as "polymerization initiator") configured to initiate a polymerization reaction by irradiation with active energy rays.
[0060] The polymerization initiator may be configured to generate radicals when irradiated with active energy rays such as light rays or electron beams. The energy required for generating radicals is not particularly limited. For example, the polymerization initiator may be configured to generate radicals by visible light, or may be configured to generate radicals by ultraviolet light.
[0061] The content of the polymerization initiator in the curable composition can be appropriately set, for example, within the range of 0.2 parts by mass or more and 8 parts by mass or less relative to 100 parts by mass of the total content of components A to E. By setting the content of the polymerization initiator in the curable composition within the specific range, the curable composition can be sufficiently cured, and a coating film having desired properties can be easily formed.
[0062] If the content of the polymerization initiator is too low, the amount of radicals generated from the polymerization initiator is insufficient, and the curing of the coating film is likely to be insufficient, whereas if the content of the polymerization initiator is too high, the properties of the coating film may be deteriorated.
[0063] As the polymerization initiator, for example, a photoradical polymerization initiator such as an acetophenone-based photoradical polymerization initiator, a benzophenone-based photoradical polymerization initiator, a phosphine oxide-based photoradical polymerization initiator, etc. As the photoradical polymerization initiator, for example, carbonyl compounds such as acetophenone, 2,2-diethoxyacetophenone, p-dimethylacetophenone, p-dimethylaminopropiophenone, benzophenone, 2-chlorobenzophenone, benzoin, benzoin methyl ether, benzoin ethyl ether, and benzoin isopropyl ether, and sulfur compounds such as thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, and tetramethylthiuram disulfide can be used.
[0064] In addition, as the photoradical polymerization initiator, commercially available products such as "Omnirad1173", "Omnirad184", "Omnirad369", "Omnirad500", "Omnirad651", "Omnirad754", "Omnirad819", "Omnirad907", "Omnirad1300", "Omnirad1800", "Omnirad1870", "Omnirad2959", "Omnirad4265", and "OmniradTPO H" manufactured by IGM Resins BV can also be used. Note that "Omnirad" is a registered trademark of IGM Group BV.
[0065] [Other ingredients] The curable composition may contain, if necessary, an organic solvent for adjusting the viscosity of the curable composition in addition to the above-mentioned components A to E. The curable composition may also contain additives such as a leveling agent, an ultraviolet absorber, an antioxidant, a colorant, an antifoaming agent, a thickener, a suspending agent, an antistatic agent, an antifogging agent, a non-slip agent, an antibacterial agent, and organic fine particles.
[0066] The curable composition may contain a filler for improving the properties of the coating film. By blending a filler in the curable composition, the physical properties of the coating film, such as scratch resistance, thermal conductivity, electrical conductivity, and refraction, can be improved depending on the material of the filler. Examples of the filler include zirconium compounds, glass powder with an average particle size of 0.5 μm to 5 μm, silica powder with an average particle size of 0.5 μm to 5 μm, alumina, carbon, and silver powder.
[0067] (Coating material) The curable composition is applied onto a substrate, and then cured to obtain a coating member. The coating member thus obtained comprises a substrate and and a coating film provided on the substrate. The coating film is composed of a cured product of the curable composition.
[0068] The material of the substrate in the coating member is not particularly limited. For example, the substrate may be made of an inorganic material such as metal or ceramic, or an organic material such as plastic. The shape of the substrate may be appropriately determined depending on the desired application.
[0069] The coating film may be provided on the entire surface of the substrate, or may be provided on a part of the surface of the substrate. The thickness of the coating film may be appropriately set, for example, within the range of 1 μm to 500 μm. The thickness of the coating film is preferably 3 μm to 150 μm, and more preferably 5 μm to 100 μm.
[0070] (Method of manufacturing coating member) In preparing the coating member, the curable composition may be applied to the surface of a substrate, and then the curable composition on the substrate may be cured. The method of applying the curable composition is not particularly limited, and the curable composition may be applied using various devices such as a bar coater, a die coater, a dip coater, a spray coater, a gravure printer, and a flexographic printer.
[0071] When the curable composition contains an organic solvent, the organic solvent may be volatilized from the curable composition applied onto the substrate, as necessary, during the period from the completion of application of the curable composition to the curing of the curable composition.
[0072] When curing the curable composition on the substrate, the curable composition may be irradiated with active energy rays. The energy of the active energy rays may be appropriately set according to the composition of the curable composition. For example, when a photoradical polymerization initiator is contained in the active energy rays, the curable composition may be irradiated with light rays corresponding to the absorption wavelength of the photoradical polymerization initiator. More specifically, when the absorption wavelength of the photoradical polymerization initiator is in the ultraviolet region, an ultraviolet lamp such as a low-pressure mercury lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a xenon lamp, a metal halide lamp, or an ultraviolet light-emitting diode may be used as the light source. In this case, the exposure dose of the curable composition may be, for example, 100 mJ / cm. 2 More than 900mJ / cm 2 The light irradiation time may be appropriately set within the following ranges: The light irradiation time may be appropriately set depending on the type of light source, the distance between the light source and the coating surface, the output of the light source, the desired exposure amount, and the like.
[0073] In the method for producing a coating member, it is preferable to subject the substrate to a surface treatment for improving adhesion to the coating film before applying the curable composition to the substrate surface. Examples of such surface treatment include plasma treatment. EXAMPLES
[0074] Example 1 An example of the curable composition and the coating member will be described with reference to Fig. 1. The curable composition of this example contains an A component made of urethane (meth)acrylate, a B component made of a (meth)acrylate compound, a C component made of a multifunctional thiol, a D component made of polysiloxane, and an E component made of silica. With respect to 100 parts by mass of the total content of the A component to the E component, the content of the A component is 30 parts by mass or more, the content of the B component is 0 parts by mass or more and 45 parts by mass or less, the total content of the A component and the B component is 60 parts by mass or more and 94 parts by mass or less, the content of the C component is 0.5 parts by mass or more and 30 parts by mass or less, the content of the D component is 0.5 parts by mass or more and 5 parts by mass or less, the total content of the C component and the D component is 5 parts by mass or more, and the content of the E component is 0.5 parts by mass or more and 10 parts by mass or less.
[0075] Moreover, by applying the curable composition of this example to a substrate 2 shown in FIG. 1 and then curing the curable composition by irradiating it with active energy rays, it is possible to obtain a coating member 1 having the substrate 2 and a coating film 3 formed on the substrate 2, which is made of a cured product of the curable composition.
[0076] In this example, curable compositions (test agents S1 to S3) containing components A to E and a polymerization initiator in the mass ratios shown in Table 1 were prepared, and the properties of these test agents were evaluated. The content of each component shown in Table 1 is the mass ratio when the total content of components A to E is 100 parts by mass. Specifically, components A to E and polymerization initiators used in this example are as follows:
[0077] Component A: Urethane acrylate (Mitsubishi Chemical Corporation "UV1700B") B component: Ethoxylated (3) trimethylolpropane triacrylate (SR454NS, manufactured by Sartomer) · Component C: Pentaerythritol tetrakis(3-mercaptobutyrate) ("Karenz MT PE1" manufactured by Showa Denko K.K.)
[0078] Component D: Polysilsesquioxane (condensation product of phenyltriethoxysilane (PhTES), (3-mercaptopropyl)triethoxysilane (MPTES) and 3-(trimethoxysilyl)propyl acrylate (ATEP))
[0079] The method for synthesizing polysilsesquioxane used in this example is as follows. First, 24.5 mmol of PhTES, 187.0 mmol of MPTES, 31.1 mmol of ATEP, 1.3 mol of H2O, 0.2 mol of ethanol, and 4.2 mmol of acetic acid are mixed. This mixture is heated at a temperature of 70°C for 3 hours to obtain a sol of polysilsesquioxane. Next, the sol of polysilsesquioxane is heated at a temperature of 70°C for 10 minutes in a vacuum to remove the solvent. In this way, polysilsesquioxane can be obtained. The polysilsesquioxane obtained in this manner is a viscous liquid.
[0080] E component: Hydrophobic silica surface-treated with methyltrimethoxysilane and hexamethyldisilazane ("QSG-30" manufactured by Shin-Etsu Chemical Co., Ltd., average primary particle size 30 nm, spherical, degree of hydrophobicity by methanol titration method: 67%) Polymerization initiator: Photoradical polymerization initiator (2-hydroxy-2-methyl-1-phenylpropanone, "Omnirad1173" manufactured by IGM Resins BV)
[0081] Test agents R1 to R9 shown in Table 1 are test agents for comparison with test agents S1 to S3. Test agents R1 to R9 have the same configuration as test agents S1 to S3, except that the mass ratios of the respective components are the values shown in Table 1.
[0082] In this example, the test agents shown in Table 1 were used to evaluate the hardness of the coating film, its adhesion to the substrate, and its impact resistance.
[0083] [Coating film hardness] The hardness of the coating film was evaluated based on the scratch hardness measured by the pencil method specified in JIS K5600-5-4:1999. First, an acrylic plate with a thickness of 1.0 mm was used as the substrate, and the test agent was applied to the substrate to a thickness of 15 μm. Next, the test agent was exposed to an exposure dose of 300 mJ / cm2. 2 The test agent was cured by irradiating it with ultraviolet light so that the cured agent became
[0084] Using the test pieces obtained above, the scratch hardness of the coating film was evaluated by the pencil method specified in JIS K5600-5-4: 1999. The scratch hardness of the coating film made of the cured product of each test agent was as shown in Table 1.
[0085] [Adhesion to substrate] The adhesion to the substrate was evaluated based on the adhesion by the cross-cut method specified in JIS K5600-5-6:1999. The substrate was an acrylic plate having a thickness of 1.0 mm, a glass plate having a thickness of 2.5 mm, an aluminum plate having a thickness of 0.5 mm, or an alumina plate having a thickness of 0.5 mm, and the test agent was applied to the substrate to a thickness of 15 μm. The test agent was then exposed to an exposure dose of 300 mJ / cm2. 2 The test agent was cured by irradiating it with ultraviolet light so that the cured agent became
[0086] Using the test pieces obtained above, the adhesion of the coating film was evaluated by the cross-cut method specified in JIS K5600-5-6: 1999. The adhesion of the coating film to each substrate was as shown in Table 1.
[0087] The meanings of the symbols showing the degree of adhesion shown in Table 1 are as follows: 0: The edges of the cut are completely smooth and there are no peeling marks on any of the grids. 1: There is a small amount of peeling of the coating at the intersection of the cuts. The percentage of the cross-cut area where the coating is peeling does not clearly exceed 5%. 2: The coating is delaminated along the edges of cuts and / or at cross-cuts. The percentage of delaminated coating in the cross-cut area is clearly greater than 5% but not greater than 15%. 3: The coating has been severely or completely removed along the edges of the cuts and / or has been partially or completely removed in various areas of the mesh. The percentage of the cross-cut area where the coating has been removed is clearly greater than 15% but not more than 35%. 4: The coating has partially or completely peeled off significantly along the edges of the cuts and / or has partially or completely peeled off in several sections. The percentage of peeled off coating in the cross-cut area does not clearly exceed 35%. 5: Cannot be classified into any of categories 1 to 4.
[0088] [Impact resistance] An acrylic plate having a thickness of 1.0 mm was used as a substrate, and the test agent was applied to the substrate to a thickness of 150 μm. The test agent was then exposed to an exposure dose of 300 mJ / cm 2 The test agent was cured by irradiating it with ultraviolet light so that the cured agent became
[0089] A steel ball weighing 130g was dropped from a height of 300mm onto the coating film of the test piece obtained in the above manner, to apply an impact to the coating film. The coating film was then visually observed and evaluated for the presence or absence of cracks or scratches. In the "Impact Resistance" column of Table 1, if there were no cracks or scratches on the coating film after the impact, the symbol "A" was entered, if there were scratches, the symbol "B", and if there were cracks, the symbol "C".
[0090] [Table 1]
[0091] As shown in Table 1, test agents S1 to S3 contain components A to E, and the contents of these components are within the specific ranges. Therefore, the coating films obtained by curing test agents S1 to S3 have a texture similar to that of glass glaze. Furthermore, the coating films obtained by curing these test agents have high hardness and are resistant to scratches. Furthermore, the coating films have high adhesion to various substrates.
[0092] On the other hand, Test Agent R1 has low curability of the curable composition because it does not contain Component C. Therefore, the coating film obtained by curing Test Agent R1 has inferior impact resistance compared to the coating films obtained by curing Test Agents S1 to S3.
[0093] Test agent R2 does not contain component D, so component E tends to aggregate. Therefore, the coating film obtained by curing test agent R2 has poorer adhesion to substrates made of inorganic materials such as glass, aluminum, and alumina than the coating films obtained by curing test agents S1 to S3.
[0094] Test agent R3 does not contain both components C and D. Therefore, the coating film obtained by curing test agent R3 has lower hardness and is inferior in adhesion to the substrate and impact resistance compared to the coating films obtained by curing test agents S1 to S3.
[0095] Test agent R4 does not contain component C, and contains a larger amount of component D than test agent S1, so the curability of the curable composition is low. Therefore, the coating film obtained by curing test agent R4 has a lower hardness than the coating film obtained by curing test agent S1, and the adhesion to the substrate is also deteriorated.
[0096] Test agent R5 does not contain component D, and contains a higher amount of component E than test agent S2, which makes it easier for component E to aggregate. Therefore, the impact resistance of the coating film obtained by curing test agent R5 was worse than that of the coating film obtained by curing test agent S2 due to the aggregation of component E.
[0097] Test agent R6 does not contain component E, so the coating film structure tends to be insufficiently strengthened compared to test agents S1 to S3. Therefore, the coating film obtained by curing test agent R6 has lower impact resistance and is more susceptible to scratches than the coating films obtained by curing test agents S1 to S6.
[0098] The amount of component C contained in test agent R7 is greater than the specific range, and therefore the hardness of the coating film obtained by curing test agent R7 is lower than the hardness of the coating films obtained by curing test agents S1 to S3.
[0099] Test agent R8 has a content of component D that is greater than the specific range, and therefore has lower curability than test agents S1 to S3. Therefore, the hardness of the coating film obtained by curing test agent R8 is lower than the hardness of the coating film obtained by curing test agents S1 to S3.
[0100] Since the content of component E in test agent R9 is higher than the specific range, component E is more likely to aggregate than in test agents S1 to S3, and therefore the coating film obtained by curing test agent R9 is inferior in impact resistance to the coating films obtained by curing test agents S1 to S3.
[0101] Example 2 In this example, an example of a curable composition containing an organic solvent will be described. As shown in Table 2, the curable compositions of this example (Test Agents S4 to S6) contain Component A, Components C to E, a polymerization initiator, and an organic solvent in the mass ratios shown in Table 2. On the other hand, the curable compositions of this example do not contain Component B. The components A, C to E, and the polymerization initiator used in this example are the same as the compounds used in Example 1. Specifically, the organic solvent used in this example is 1-methoxy-2-propanol.
[0102] Test agents R10 to R12 shown in Table 2 are test agents for comparison with test agents S4 to S6. Test agents R10 to R12 have the same configuration as test agents S4 to S6, except that the mass ratios of the respective components are the values shown in Table 2.
[0103] In this example, the hardness, adhesion to the substrate, and impact resistance of the coating film were evaluated using the test agents shown in Table 2. The method for evaluating these properties was the same as that described in Example 1, except that when forming a coating film on a substrate, the organic solvent was evaporated from the curable composition between the application of the curable composition on the substrate and the irradiation of ultraviolet rays. Table 2 shows the hardness, adhesion to the substrate, and impact resistance of the coating film obtained using each test agent.
[0104] [Table 2]
[0105] As shown in Table 2, test agents S4 to S6 contain the essential components A and C to E, and the contents of these components are within the specific ranges. Therefore, the coating films obtained by curing test agents S4 to S6 have a texture similar to that of glass glaze. Furthermore, the coating films obtained by curing these test agents have high hardness and are resistant to scratches. Furthermore, the coating films have high adhesion to various substrates.
[0106] On the other hand, Test Agent R10 has low curability of the curable composition because it does not contain Component C. Therefore, the coating film obtained by curing Test Agent R10 has poor impact resistance compared to the coating films obtained by curing Test Agents S4 to S6.
[0107] Test agent R11 does not contain component D, so component E tends to aggregate. Therefore, the coating film obtained by curing test agent R11 has poorer adhesion to substrates made of inorganic materials such as glass, aluminum, and alumina than the coating films obtained by curing test agents S4 to S6.
[0108] Test agent R12 does not contain both components C and D. Therefore, the coating film obtained by curing test agent R12 is less hard than the coating films obtained by curing test agents S4 to S6, and is inferior in adhesion to the substrate and impact resistance.
[0109] Specific embodiments of the active energy ray-curable composition and coating member according to the present invention have been described above based on Example 1 and Example 2. However, the specific embodiments of the active energy ray-curable composition and coating member according to the present invention are not limited to those in the Examples, and the configurations can be appropriately changed within the scope of the present invention. [Explanation of symbols]
[0110] 1 Coating materials 2 Base material 3. Coating film
Claims
1. Component A consisting of urethane (meth)acrylate; Component B consisting of a (meth)acrylate compound; A component C consisting of a multifunctional thiol; Component D consisting of polysiloxane; and an E component consisting of silica, The component A contains a urethane (meth)acrylate having three or more (meth)acryloyl groups in one molecule, The component B contains a (meth)acrylate compound having three or more (meth)acryloyl groups in one molecule, The component C contains a polyfunctional thiol having 2 to 4 thiol groups in one molecule, The component D includes polysilsesquioxane, The component E contains hydrophobic silica having a hydrophobicity of 20% or more as measured by a methanol titration method, an active energy ray-curable composition, wherein, relative to 100 parts by mass in total of the contents of the A component to the E component, the content of the A component is 30 parts by mass or more, the content of the B component is 0 parts by mass or more and 45 parts by mass or less, the sum of the contents of the A component and the B component is 60 parts by mass or more and 94 parts by mass or less, the content of the C component is 0.5 parts by mass or more and 30 parts by mass or less, the content of the D component is 0.5 parts by mass or more and 1 part by mass or less, the sum of the contents of the C component and the D component is 5 parts by mass or more, and the content of the E component is 0.5 parts by mass or more and 10 parts by mass or less.
2. 2. The active energy ray-curable composition according to claim 1, wherein the content of the A component is 30 parts by mass or more and 63 parts by mass or less, and the content of the B component is 30 parts by mass or more and 45 parts by mass or less, relative to 100 parts by mass in total of the contents of the A component to the E component.
3. A substrate; A coating member having a coating film provided on the substrate, A coating member, wherein the coating film is made of a cured product of the active energy ray-curable composition according to claim 1 or 2.
Citation Information
Patent Citations
Photocurable resin composition and its cured product
JP2002097217A
UV curable coating composition and use thereof
JP2007517935A
Radiation-sensitive composition for colored layer formation, color filter and color liquid crystal display element
JP2008242078A
Active energy ray curing type coating agent composition
JP2014105263A
Coating composition nd hard coat film using the same
JP2015086372A