Method for producing hollow fiber carbon membrane
The method of spinning hollow fibers onto a polygonal bobbin for drying and subsequent treatments enhances manufacturing capacity and formability, resulting in high-permeability hollow fiber carbon membrane modules.
Patent Information
- Application Number
- JP2020191861
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-18
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2040-11-18
Smart Images

Figure 0007591383000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a hollow fiber carbon membrane. [Background technology]
[0002] Conventionally, various organic and inorganic membranes have been considered for use as separation membranes for gases and the like. Organic membranes made of polysulfone, cellulose acetate, and the like have the advantages of good moldability and low cost, but have low solvent resistance and heat resistance. On the other hand, inorganic membranes have the advantages of excellent solvent resistance and heat resistance, but are difficult to mold and expensive. Therefore, hollow fiber carbon membranes, which have the advantages of excellent moldability, solvent resistance, and heat resistance, as well as low cost, have been attracting attention in recent years.
[0003] Patent Document 1 (JP Patent Publication No. 4-011933) discloses a method for producing a hollow fiber carbon membrane made of polyimide, and Patent Document 2 (JP Patent Publication No. 2009-034614) discloses a method for producing a hollow fiber carbon membrane made of a polyphenylene oxide derivative. More specifically, Patent Document 2 discloses a method for producing a hollow fiber carbon membrane by the following spinning process, drying process, infusible treatment process, and carbonization treatment process. (1) Spinning process Using a hollow fiber spinning nozzle with a double-tube structure, an organic solvent solution (film-forming solution) containing a polyphenylene oxide derivative polymer and a core liquid such as an inorganic salt aqueous solution or water are simultaneously extruded by the wet spinning method or the dry-wet spinning method to spin a hollow fiber (Figure 2). (2) Drying process The hollow fibers of the polyphenylene oxide derivative polymer obtained in the spinning process are dried. (3) Infusibility treatment process The dried hollow fiber material is subjected to an infusibility treatment under heat treatment conditions of 150 to 300° C. for 0.5 to 4 hours. (4) Carbonization process 10 -4The infusible hollow fiber material is heated at 450 to 850° C. for 0.5 to 4 hours under reduced pressure below atmospheric pressure or in an inert gas atmosphere in which air has been replaced with helium gas, argon gas, nitrogen gas or the like.
[0004] In the drying step, the core liquid remaining in the hollow portion of the hollow fiber is removed. Drying methods for efficiently removing the core liquid have been studied. Patent Document 3 (JP 2012-081375 A) discloses a method in which hollow fiber is cut to a predetermined length, each hollow fiber is hung vertically to remove the core liquid remaining in the hollow portion of the hollow fiber, and then moisture is evaporated from the polymer portion of the hollow fiber to dry it.
[0005] Furthermore, Patent Document 4 (JP 2013-000713 A) discloses a method for producing a hollow fiber carbon membrane in which a spun hollow fiber is wound around a bobbin, one end of the wound hollow fiber is left open, and air is pumped into the hollow portion of the hollow fiber from the other end to remove the core liquid remaining in the hollow portion of the hollow fiber. This production method makes it possible to perform infusible treatment and carbonization treatment while the hollow fiber is wound around a bobbin without cutting a hollow fiber longer than 100 m, thereby improving the production capacity of hollow fiber carbon membranes and also reducing manpower. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 4-011933 [Patent Document 2] JP 2009-034614 A [Patent Document 3] JP 2012-081375 A [Patent Document 4] JP 2013-000713 A Summary of the Invention [Problem to be solved by the invention]
[0007] There has been a demand for further shortening the time required for producing hollow fiber carbon membranes and improving the production capacity of hollow fiber carbon membranes. There has also been a demand for hollow fiber carbon membranes that have a linear shape and excellent formability. The present invention has been made in consideration of the above circumstances, and provides a method for producing a hollow fiber carbon membrane, which improves the production capacity of hollow fiber carbon membranes and also provides hollow fiber carbon membranes with improved formability. [Means for solving the problem]
[0008] The various aspects of the present invention are as follows. [1] A step of spinning a hollow fiber containing carbon; a step of winding the spun hollow fiber around a bobbin having a polygonal outer periphery; drying the hollow fiber material wound around the bobbin while rotating the bobbin; a step of subjecting the dried hollow fiber-like material to an infusible treatment; a step of subjecting the hollow fiber-like material that has been subjected to the infusible treatment to a carbonization treatment; A method for producing a hollow fiber carbon membrane comprising the steps of: [2] The method for producing a hollow fiber carbon membrane according to the above [1], wherein the polygon is a quadrilateral. [3] The method for producing a hollow fiber carbon membrane according to the above [1] or [2], wherein in the step of spinning the hollow fiber-like material, a membrane-forming dope is extruded from an outer tube of a double-tube nozzle, and a core liquid is extruded from an inner tube of the double-tube nozzle, thereby spinning a hollow fiber-like material. Effect of the Invention
[0009] It is possible to provide a method for producing a hollow fiber carbon membrane, which improves the production capacity of the hollow fiber carbon membrane and also gives a hollow fiber carbon membrane with improved formability. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a diagram illustrating a drying step in a method for producing a hollow fiber carbon membrane according to one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The method for producing a hollow fiber carbon membrane of the present invention includes a step of spinning a hollow fiber-like material containing carbon, a step of winding the spun hollow fiber-like material around a bobbin having a polygonal outer periphery, a step of drying the hollow fiber-like material wound around the bobbin while rotating the bobbin, a step of performing an infusible treatment on the dried hollow fiber-like material, and a step of carbonizing the infusible hollow fiber-like material. The term "hollow fiber-like material" refers to a filamentous molded product made of a carbon material obtained in an intermediate step of producing a hollow fiber carbon membrane, and the term "hollow fiber carbon membrane" refers to a filamentous molded product made of a carbon material finally obtained by the production method of the present invention. In the method for producing a hollow fiber carbon membrane of the present invention, first, a hollow fiber-like material containing carbon is spun by a wet spinning method or a dry-wet spinning method. In the step of spinning a hollow fiber-like material, a membrane forming solution is extruded from the outer tube of a double-tube nozzle, and a core liquid is extruded from the inner tube of the double-tube nozzle, thereby spinning the hollow fiber-like material. The double-tube nozzle has a structure having an inner tube and an outer tube provided on the outer periphery of the inner tube at a distance so as to cover the inner tube, and is capable of simultaneously extruding different materials from the inner tube and the outer tube. The spun hollow filament may be held in a wound form on the outer periphery of a cylindrical bobbin. Next, the spun hollow filament is wound on the outer periphery of a bobbin having a polygonal outer periphery. Here, the "outer periphery of the bobbin" refers to the periphery of the side of the bobbin (cross section perpendicular to the bobbin's rotation axis) for holding the wound hollow filament, and when the bobbin is lattice-shaped, it has a shape formed by lattice points when the bobbin is viewed in a cross section perpendicular to its rotation axis. After this, the hollow filament wound on the bobbin is dried while rotating the bobbin. At this time, due to the rotation of the bobbin, the core liquid remaining inside the hollow fiber (typically composed mostly of water) can easily move inside the hollow fiber by gravity, permeate and penetrate the hollow fiber, and evaporate from the surface of the hollow fiber. Therefore, there is no need to perform additional treatment or steps to remove the core liquid from the hollow fiber, and the hollow fiber can be dried in a short time. As a result, the production capacity of hollow fiber carbon membranes can be improved. In addition, the hollow fiber wound around the bobbin is linear because it has a shape that follows the outer periphery of the bobbin (polygon).Therefore, it is possible to prevent the hollow fiber from bending when the hollow fiber is dried while wound around a cylindrical bobbin. The hollow fiber maintains its straight shape even after drying. After this, the hollow fiber carbon membrane wound around the bobbin is subjected to an infusible treatment and a carbonization treatment. Since the hollow fiber maintains its straight shape even after the infusible treatment and the carbonization treatment, the moldability of the hollow fiber carbon membrane finally obtained can be improved. For example, when the hollow fiber carbon membrane is packed into a hollow fiber carbon membrane module, the packing density of the hollow fiber carbon membrane can be increased, and a hollow fiber carbon membrane module with a high permeability can be obtained. The hollow fiber carbon membrane manufactured as described above can be used for separation treatment of various substances, and an example of the separation treatment is gas separation such as hydrogen separation.
[0012] Each step of the method for producing a hollow fiber carbon membrane according to one embodiment will be described in detail below. (1) Spinning process In the spinning step, a hollow fiber containing carbon is spun. The material of the hollow fiber is not particularly limited as long as it is a known material (polymer) for hollow fiber carbon membranes, but is preferably a polyphenylene oxide polymer, more preferably a derivative in which 1 to 4 hydrogen atoms constituting polyphenylene oxide or aromatic rings of polyphenylene oxide are directly substituted with halogen atoms, sulfone groups, carboxyl groups, lower alkyl groups, tri(lower alkyl)silyl groups, diarylphosphino groups, or derivatives in which these atoms or groups are substituted via -CH2-. In addition, the above-mentioned lower alkyl is more preferably an alkyl having 1 to 5 carbon atoms. The above-mentioned polymer is dissolved in any soluble organic solvent, such as methanol, ethanol, tetrahydrofuran, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, or a mixture thereof, preferably at a concentration of 20 to 40% by weight, more preferably 25 to 35% by weight, to prepare a membrane-forming solution. By using a wet spinning method or a dry-wet spinning method, a membrane-forming solution is extruded from the outer tube of a hollow fiber spinning nozzle having a double-tube ring structure into a coagulation bath, and a solvent of the membrane-forming solution and a core liquid that is insoluble in the polymer are simultaneously extruded from the inner tube of the hollow fiber spinning nozzle to spin a hollow fiber. At this time, a hollow fiber made of a carbon material having a predetermined membrane outer diameter can be obtained by appropriately adjusting the diameter of the outer tube of the hollow fiber spinning nozzle and the winding speed when winding the hollow fiber around a bobbin, which will be described later.
[0013] The solvent of the core liquid and the coagulation bath is preferably a solvent in which the material (polymer) of the hollow fiber is not dissolved. For example, when the polymer is a polyphenylene oxide-based polymer, water or an aqueous solution of an ammonium salt such as ammonium nitrate, ammonium chloride, or ammonium sulfate can be used as the solvent. The temperature of the core liquid and the coagulation bath is preferably -20 to 60°C, more preferably 0 to 30°C. Next, the hollow fiber spun as described above is wound on a cylindrical bobbin. The outer diameter of the bobbin is preferably 0.5 to 2.0 m, more preferably 0.7 to 1.2 m, and the winding speed of the hollow fiber around the bobbin is preferably 10 to 60 m / min, more preferably 20 to 40 m / min. The total length of the hollow fiber wound around the bobbin is preferably 100 to 8000 m, more preferably 2000 to 4000 m. The hollow fiber-like material wound around a cylindrical bobbin in this manner may be immediately subjected to a drying step, or may be stored in water for a certain period of time.
[0014] (2) Drying process Next, the hollow fiber-like material is further sent out from the cylindrical bobbin, and the spun hollow fiber-like material is wound around the outer periphery of the bobbin having a polygonal outer periphery. The shape of the outer periphery of the bobbin is not particularly limited as long as it is polygonal, and examples thereof include a triangle, a rectangle, a pentagon, a hexagon, and other n-sided shapes (n is an integer of 7 or more), but the shape of the outer periphery of the bobbin is preferably a rectangle because of the excellent winding performance of the bobbin and the linearity of the shape of the hollow fiber-like material after drying. In addition, the shape of the outer periphery of the bobbin may be either a regular polygon or a polygon with different interior angles, but a regular polygon is preferable because of the excellent linearity of the shape of the hollow fiber-like material.
[0015] FIG. 1 is a diagram showing an example of a bobbin having a rectangular outer periphery. The bobbin 2 in FIG. 1 has a lattice shape, and while rotating in the A direction, the hollow fiber-like material 1 can be wound around the outer periphery 4. The outer periphery 4 has a rectangular shape consisting of four lattice points originating from the corners 3 in a cross section perpendicular to the rotation axis of the bobbin 2. The hollow fiber-like material 1 wound around the bobbin 2 in this way is linear except for the corners 3 on the outer periphery of the bobbin 2. Therefore, as the bobbin 2 rotates, the core liquid (typically mostly composed of water) remaining inside the hollow fiber-like material 1 easily moves by gravity inside the hollow fiber-like material 1 and permeates and penetrates the hollow fiber-like material 1, and also evaporates from the surface of the hollow fiber-like material 1. Therefore, there is no need to perform an additional process or step to remove the core liquid from the hollow fiber-like material 1, and the hollow fiber-like material 1 can be dried efficiently and in a short time. As a result, the production capacity of hollow fiber carbon membranes can be improved. In addition, since the hollow fiber-like material 1 after drying maintains a straight shape along the outer circumferential shape of the bobbin 2, the formability of the hollow fiber carbon membrane can be improved.
[0016] When the hollow fiber material 1 is wound around the outer periphery of the bobbin 2 in FIG. 1, the length of the hollow fiber material 1 is preferably 2.5 to 5 m, more preferably 3 to 4 m. The winding speed of the hollow fiber material 1 around the bobbin 2 in FIG. 1 is preferably 2 to 20 m / min, more preferably 4 to 14 m / min. When the hollow fiber material 1 is wound around the outer periphery of the bobbin 2 in FIG. 1, one turn is defined as one turn, and the hollow fiber material 1 is preferably wound around the bobbin 2 by 400 to 1200 turns, more preferably 600 to 1000 turns. When the hollow fiber material 1 is wound around the bobbin 2 in FIG. 1, it is preferable to provide a coil-shaped groove so that the hollow fiber material 1 for one turn is held at an interval of preferably 0.5 to 5 mm, more preferably 1 to 2 mm. When the hollow fiber-like material 1 is wound around the bobbin 2, drying by ventilation may be performed in order to promote drying of the hollow fiber-like material 1. The ventilation speed at this time is preferably 5 to 100 cm / sec, and more preferably 30 to 80 cm / sec, in terms of linear velocity.
[0017] Next, after the hollow fiber material 1 has been wound around the bobbin 2, the bobbin 2 continues to rotate. The rotation time of the bobbin 2 with the hollow fiber material 1 wound around it is preferably 30 to 150 minutes, more preferably 60 to 90 minutes. The rotation speed of the bobbin 2 with the hollow fiber material 1 wound around it is not particularly limited, but it is preferably the same rotation speed as when the hollow fiber material 1 is wound around it, that is, 4 to 14 m / min.
[0018] (3) Infusibility treatment process Next, the hollow fiber-like material 1 after drying in a state wound around a bobbin 2 as shown in FIG. 1 is subjected to an infusible treatment. The conditions of the infusible treatment can be appropriately set depending on the type of material of the hollow fiber-like material 1 and the number of windings. The conditions of the infusible treatment step can be, for example, 150 to 300°C in the presence of air for 0.5 to 4 hours, and the hollow fiber-like material 1 can be heated at a temperature lower than the temperature of the carbonization treatment step described later. In this infusible treatment step, intermolecular crosslinking of the material constituting the hollow fiber-like material 1 occurs due to oxidation, improving the heat resistance of the hollow fiber-like material. Therefore, it is possible to effectively prevent the hollow fiber-like material from melting in the carbonization treatment step described later. In addition, this intermolecular crosslinking can improve not only the heat resistance but also the mechanical strength properties of the hollow fiber carbon membrane finally obtained. Thereafter, the hollow fiber-like material is cut to a predetermined length (for example, 0.2 to 1 m). At this time, the hollow fiber-like material after the infusible treatment step maintains the linear shape after drying.
[0019] (4) Carbonization process Next, the hollow fiber-like material in the cut state is placed in a container and heated under a reduced pressure of preferably 10 Pa or less, more preferably 4 to 10 Pa, or under an inert gas atmosphere in which the air is replaced with helium gas, argon gas, nitrogen gas, or the like without reducing the pressure, thereby carbonizing the infusible hollow fiber-like material. This ultimately produces a hollow fiber carbon membrane. The carbonization conditions can be appropriately set depending on the type of material of the hollow fiber-like material, the number of windings, etc., but conditions such as 450 to 850 ° C and 0.5 to 4 hours are preferable. This carbonization process can increase the carbon content of the hollow fiber carbon membrane. The hollow fiber carbon membrane obtained after the carbonization process maintains the linear shape after drying, and its moldability can be improved. For example, when the hollow fiber carbon membrane is packed into a hollow fiber carbon membrane module, the packing density of the hollow fiber carbon membrane can be increased, resulting in a hollow fiber carbon membrane module with a high permeability.
[0020] (Hollow fiber carbon membrane module) In one embodiment, a hollow fiber carbon membrane module can be provided having a case and a hollow fiber carbon membrane housed in the case. Since the hollow fiber carbon membrane is manufactured by the hollow fiber carbon membrane manufacturing method of the present invention, the hollow fiber carbon membrane in the hollow fiber carbon membrane module is linear, and the packing density of the hollow fiber carbon membrane in the case can be increased. As a result, a hollow fiber carbon membrane module with high permeation rate can be provided. EXAMPLES
[0021] Preferred examples of the present invention will be specifically described below based on examples and comparative examples, but the present invention is not limited to these examples.
[0022] Example 1 (1) Spinning process 50 g of sulfonated poly(2,6-dimethyl-1,4-phenylene oxide), a polyphenylene oxide-based polymer, was dissolved in 150 g of dimethylformamide to prepare a membrane-forming solution with a concentration of 25% by weight. The membrane-forming solution was extruded into water from the outer tube of a nozzle with a double-tube structure having an outer diameter of 0.5 mm and an inner diameter of 0.25 mm, and at the same time, a core solution of pure water was extruded into water from the inner tube, and a hollow fiber-like material was obtained by a dry-wet spinning method. After this, the hollow fiber-like material was wound around the outer circumference of a cylindrical bobbin with an outer circumference length of 1 m at a speed of 20 m / min. The total length of the hollow fiber-like material was 1000 m.
[0023] (2) Drying process The hollow fiber material wound around the outer circumference of the cylindrical bobbin was sent out and further wound around the outer circumference of a bobbin 2 having a rectangular outer circumference as shown in FIG. 1. The long side of the rectangle constituting the outer circumference of the bobbin 2 in FIG. 1 was 1.2 m, the short side was 0.4 m, and the length of one circumference was 3.2 m. The winding speed of the hollow fiber material around the bobbin 2 in FIG. 1 was 4 m / min, the interval between adjacent hollow fiber materials for one turn after winding was 1 mm, and the hollow fiber material was wound around the outer circumference of the bobbin 2 until 300 turns were reached. After the winding of the hollow fiber material around the bobbin 2 in FIG. 1 was completed, the bobbin 2 was rotated at the same speed for 60 minutes to dry the hollow fiber material. As a result, it was confirmed that the hollow fiber material could be dried in a short time, and the production capacity of the hollow fiber carbon membrane was improved by the method of the present invention. In addition, it was confirmed that the hollow fiber material after drying had a linear shape and had excellent moldability.
[0024] (3) Infusibility treatment process The bobbin 2 in FIG. 1 with the hollow fiber-like material wound thereon was placed in a heating device and subjected to a heat treatment at 290°C for 2 hours to perform an infusibility treatment. Then, 2,400 hollow fiber-like materials were cut out to a length of 0.5 m. The cut hollow fiber-like materials maintained their linear shape, and it was confirmed that they had excellent moldability.
[0025] (4) Carbonization process Of the cut hollow fibers, 2000 were heated in an inert gas atmosphere at 600°C for 1 hour to obtain hollow fiber carbon membranes. When the shape of the obtained hollow fiber carbon membrane was checked, it was found to maintain the straight shape after the infusible treatment and to have good moldability without bending or breaking. It was confirmed that a hollow fiber carbon membrane having such an excellent straight shape can increase the packing density of the hollow fiber carbon membrane during the production of a hollow fiber carbon membrane module, and can be used as a hollow fiber carbon membrane module with high permeability.
[0026] Comparative Example 1 A hollow fiber carbon membrane was produced in the same manner as in Example 1, except that the following drying step (a) was carried out instead of the drying step in Example 1. (a) Drying process The hollow fiber-like material after spinning, wound around the outer circumference of a cylindrical bobbin, was sent out, and the hollow fiber-like material was further wound around the cylindrical bobbin, and then the hollow fiber-like material was dried. More specifically, the length of one revolution of the cylindrical bobbin used in this (a) drying step was 3 m, the winding speed of the hollow fiber-like material was 4 m / min, and the interval between adjacent hollow fiber-like material turns was 1 mm, and the hollow fiber-like material was wound up to 300 turns. After the winding of the hollow fiber-like material around the outer circumference of the cylindrical bobbin was completed, the hollow fiber-like material was dried while rotating the bobbin at the same rotation speed as when it was wound. During this drying, the water in the hollow fiber-like material remained inside the hollow fiber-like material, so it took 180 minutes to dry the hollow fiber-like material. Therefore, in Comparative Example 1, it took a long time to dry the hollow fiber-like material compared to Example 1, and the production capacity of the hollow fiber carbon membrane was low. In addition, (a) the hollow fiber-like material after the drying step was subjected to the infusible treatment step and the carbonization treatment step in the same manner as in Example 1, and the shape of the hollow fiber-like material after each of the infusible treatment step and the carbonization treatment step was checked to find that it had a circular curvature and was not linear. Therefore, it was confirmed that the hollow fiber carbon membrane obtained in Comparative Example 1 had poor moldability and could not have a high packing density when producing a hollow fiber carbon membrane module. [Explanation of symbols]
[0027] 1...hollow fiber-like object, 2...bobbin, 3...corner portion, 4...outer periphery
Claims
1. A step of spinning a hollow fiber containing carbon; a step of winding the spun hollow fiber around a bobbin having a polygonal outer periphery; drying the hollow fiber material wound around the bobbin while rotating the bobbin; a step of subjecting the hollow fiber-like material after drying in a state wound around the bobbin to an infusible treatment; a step of subjecting the hollow fiber-like material that has been subjected to the infusible treatment to a carbonization treatment; A method for producing a hollow fiber carbon membrane comprising the steps of:
2. The method for producing a hollow fiber carbon membrane according to claim 1 , wherein the polygon is a quadrangle.
3. 3. The method for producing a hollow fiber carbon membrane according to claim 1, wherein in the step of spinning the hollow fiber-like material, a membrane-forming dope is extruded from an outer tube of a double-tube nozzle, and a core liquid is extruded from an inner tube of the double-tube nozzle, thereby spinning the hollow fiber-like material.
Citation Information
Patent Citations
Automatic yarn separating device for spandex filaments
CN111155182A
Hollow yarn type mass transfer apparatus and production thereof
JP1984028971A
Production of hollow yarn bundle
JP1989189305A
Asymmetric carbon hollow fiber membrane and its production
JP1992011933A
Hollow fiber carbon membrane and method for producing the same
JP2009034614A