Common mode choke coil and manufacturing method thereof

The magnetic core design with a magnetic adhesive and grooves addresses the complexity and inefficiency of conventional coils, achieving stable inductance and strong bonding in common mode choke coils.

JP7591700B2Active Publication Date: 2024-11-29PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020096538
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-03
Publication Date
2024-11-29
Estimated Expiration
2040-06-03

AI Technical Summary

Technical Problem

Conventional common mode choke coils require complex polishing processes to ensure high adhesive strength and reduce magnetic flux leakage, leading to low productivity and inconsistent inductance values.

Method used

A magnetic core design with flanges and a magnetic plate bonded via an adhesive containing magnetic powder, with grooves on the magnetic plate to store excess adhesive and cover the magnetic flux loop, ensuring stable inductance and high bonding strength.

Benefits of technology

The solution provides a common mode choke coil with stable inductance values, reduced magnetic flux leakage, and enhanced bonding strength without complex polishing, improving manufacturing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591700000002
    Figure 0007591700000002
  • Figure 0007591700000003
    Figure 0007591700000003
  • Figure 0007591700000004
    Figure 0007591700000004
Patent Text Reader

Abstract

To obtain a highly reliable common mode choke coil with high inductance, small variation, and high bonding strength between a magnetic plate and a magnetic core.SOLUTION: A common mode choke coil includes a magnetic core 10 having a winding core portion 11 and a pair of flange portions 12 and 13 provided at both ends of the winding core portion 11, external electrodes 14 formed on the collars 12 and 13, a pair of windings 15 wound around the winding core portion 11 and whose ends pulled out to the external electrode 14 and joined to each other, and a magnetic plate 16 bonded to the pair of flange portions 12 and 13 with a magnetic adhesive 17 containing a magnetic material. The magnetic plate 16 has a joint portion 16a to be joined to the flange portions 12 and 13 and a facing portion 16d facing the winding core portion 11. The magnetic adhesive 17 is formed on the entire surface of the joining portion 16a and the facing portion 16d of the magnetic plate 16.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a common mode choke coil including a magnetic core and a wire, and more particularly to a common mode choke coil suitable for use in a common mode filter that removes noise. [Background technology]

[0002] 2. Description of the Related Art Conventionally, it has been known to use a wire-wound common mode choke coil as a countermeasure against unwanted radiation noise in a power supply line or a countermeasure against common mode noise in a high frequency signal.

[0003] Such a common mode choke coil of the prior art is composed of a ferrite magnetic core with flanges formed on both sides of the winding core, a wire made of multiple insulating coated copper wires wound around the winding core of the magnetic core by bifilar winding or the like for several turns to several tens of turns, and a magnetic plate having approximately the same magnetic permeability as the magnetic core and having both flanges of the magnetic core bonded together with an adhesive. The magnetic core and the magnetic plate are obtained by mixing ferrite powder with a binder, press molding, and then sintering the mixture. Furthermore, multiple electrodes are formed on both flanges or on one of the flanges, and the winding start end and winding end end of the wire are conductively connected to these electrodes by soldering, thermocompression, or the like, respectively. In such a common mode choke coil, a desired impedance value is obtained by appropriately setting the number of turns of the wire wound around the winding core of the core.

[0004] As prior art document information related to the invention of this application, for example, Patent Document 1 is known. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2014-99587 A Summary of the Invention [Problem to be solved by the invention]

[0006] In the configuration of Patent Document 1, adhesive is placed in the gap between the drum core and the plate-like core, and this gap gradually narrows from the edge of the drum core flange toward the center, where the plate-like core and the flange are in direct contact with each other. The drum core and the magnetic plate are bonded to each other via the adhesive in the gap that gradually narrows toward the center.

[0007] Since the magnetic plate and the flange are in direct contact near the center of the flange, the effect of the magnetic gap is reduced, and since the minimum amount of adhesive is present at the flange edge, high adhesive strength can be obtained between the plate core and the drum core.

[0008] However, in order to achieve this configuration, it is necessary to polish the upper surfaces of both flanges of the drum core, as well as the surface of the plate-shaped core facing the flanges of the drum core. Such polishing requires complicated processes such as polishing, cleaning, and drying, resulting in very poor productivity.

[0009] Furthermore, when a signal of a specified frequency is input to the coil of the coil component, magnetic lines of force corresponding to the signal are generated inside, looping through the center core of the drum core, one flange of the drum core, the magnetic plate, the other flange of the drum core, and the center core of the drum core. If the gap between the magnetic plate and the flange of the drum core is about 2 μm, most of the magnetic lines of force do not leak even with an adhesive that does not contain magnetic powder, but as the gap becomes larger, the magnetic line leakage also increases. In addition, the magnetic line loop is generated by the magnetic plate of the flange of the drum core. Since the magnetic field also passes through the vicinity of the center corner of the opposing drum core flange, if there is no magnetic material covering the trajectory of this magnetic field line loop, leakage of the magnetic field lines will occur here as well, resulting in a decrease in the inductance value.

[0010] The present invention provides a common mode choke coil that can be manufactured without complicated processes, suppresses a decrease in the adhesive strength between the drum core and the plate core, and suppresses leakage of magnetic lines of force, thereby providing a consistent inductance value. [Means for solving the problem]

[0011] In order to address this issue, the present invention provides a common mode choke coil comprising a magnetic core having a winding core portion and a pair of flange portions provided at both ends of the winding core portion, an external electrode formed on the flange portion of the magnetic core, a pair of windings wound around the winding core portion of the magnetic core and each end being drawn out to the external electrodes and joined, and a magnetic plate joined to the flange portion of the magnetic core with an adhesive, wherein the magnetic plate has a joint portion joined to the flange portion of the magnetic core and an opposing portion opposing the winding core portion of the magnetic core, and the adhesive is formed on the entire surfaces of the joint portion and the opposing portion of the magnetic plate. Effect of the Invention

[0012] With the above structure, the adhesive is securely applied to the joint between the magnetic core and the magnetic plate, completely enveloping the corners of the flange of the magnetic core on the center core side and completely covering the loop locus of the magnetic field lines, so there is no drop in inductance value and a stable product with little variation can be obtained. Furthermore, the adhesive is continuously applied to the joint of the magnetic plate and the opposing part of the center core, so an extremely high joint strength between the magnetic core and the magnetic plate can be achieved.

[0013] In the present invention, grooves are provided in the opposing portions of the magnetic plate. The grooves are intended to accommodate excess adhesive when the magnetic plate with an adhesive layer formed thereon is attached across both flanges of the magnetic core. If excess adhesive were allowed to drip onto the windings and remain there, there would be a risk of damage to the winding coating depending on the environment to which it is exposed due to the difference in thermal expansion between the resin components of the winding coating and the resin components of the adhesive. The formation of these grooves makes it possible to prevent damage to the winding coating.

[0014] The adhesive of the present invention preferably contains magnetic powder, which increases the magnetic permeability of the adhesive and allows the magnetic field lines to pass through the loops reliably. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a side view of a common mode choke coil according to an embodiment of the present invention. [Diagram 2]1 is a side view of another common mode choke coil according to an embodiment of the present invention; [Diagram 3] FIG. 1 is a side view of a common mode choke coil according to a conventional embodiment; [Figure 4] 1 is a diagram for explaining a method of manufacturing a common mode choke coil according to an embodiment of the present invention; [Diagram 5] 1 is a diagram for explaining a method of manufacturing a common mode choke coil according to an embodiment of the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, a common mode choke coil according to an embodiment of the present invention will be described with reference to the drawings.

[0017] Fig. 1(A) is a side view of a common mode choke coil in one embodiment of the present invention, and Fig. 1(B) is an enlarged view of the area surrounded by the dashed line in Fig. 1(A). Fig. 2(A) is a side view of another common mode choke coil in one embodiment of the present invention, and similarly Fig. 2(B) is an enlarged view of the area surrounded by the dashed line in Fig. 2(A). The magnetic core 10 comprises a winding core portion 11 and flange portions 12 and 13 provided at both ends of this winding core portion 11, and a pair of insulatingly coated conductor wires are wound around this winding core portion 11. The conductors are wound around each other to form a winding 15. The ends of each conductor are electrically connected to external electrodes 14 provided on flanges 12 and 13.

[0018] A magnetic plate 16 is bonded to the upper portions of the pair of flanges 12 and 13 via a magnetic adhesive 17. The enlarged cross-sectional views of Figure 1(B) and Figure 2(B) show the detailed bonding structure between flange 12 and magnetic plate 16. On the surface of flange 12 facing magnetic plate 16, there are flange joint portion 12a, flange winding core side corner portion 12b, and flange outer corner portion 12c, and magnetic adhesive 17 is formed on these areas.

[0019] The magnetic plate 16 in Figure 1 (B) has a joint portion 16a that faces the flange joint portion 12a, an outer corner portion 16c of the magnetic plate, and an opposing portion 16d that faces the winding core portion 11, and a magnetic adhesive 17 is formed on these areas and is bonded to the flange joint portion 12a, the flange winding core side corner portion 12b, and the flange outer corner portion 12c.

[0020] Here, it is desirable to use a magnetic adhesive made of resin containing magnetic powder. If the adhesive does not contain magnetic powder, no magnetic flux leakage will occur if the gap between the magnetic plate and the flange is 2 μm or less, but if it is larger than that, leakage will occur and the inductance value will decrease. If the gap is large, 2 μm or more, the effects of magnetic flux leakage can be reduced by mixing magnetic powder into the adhesive.

[0021] In the present invention, the epoxy resin is mixed with magnetic powder in a weight ratio of 2:1. By using this, it is possible to keep the leakage of magnetic flux as low as possible even if the gap is 10 μm or more.

[0022] Next, a configuration in which a groove is provided in the magnetic plate will be described. In the magnetic plate 16 of FIG. 2(B), a groove 16e is formed in the facing portion 16d near the joint portion 16a. This groove 16e absorbs the overflow of the magnetic adhesive 17 toward the winding 15 side caused by the pressing force when the magnetic plate 16 and the magnetic core 10 are joined. This groove 16e makes it possible to reliably suppress the adhesion of the magnetic adhesive 17 to the winding 15. If the magnetic adhesive 17 adheres to the winding 15, stress is applied to the conductor coating resin in a thermal cycle due to the difference in thermal expansion between the conductor coating resin and the magnetic adhesive resin, which is highly likely to break the coating resin layer or affect the high-frequency characteristics. To avoid this, the magnetic plate 16 is provided with the groove 16e.

[0023] In this case, the width of the groove 16e may be 100 μm or more, and the depth may be 20 μm or more. Preferably, the width is 100 μm to 300 μm, and the depth is 20 μm to 50 μm. For example, if the groove width is 50 μm or less, the depth of the magnetic plate groove must be made deeper to ensure the volume to store the overflowing magnetic adhesive. If the depth is 50 μm or more, even if the storage volume can be secured, the groove cut will be at an acute angle, so that the overflowing magnetic adhesive will not easily enter the groove, and voids will easily occur. In addition, making deep cuts makes it easy to cause internal cracks in the magnetic plate itself, and furthermore, stress will concentrate at the tip of the cut, which may cause the entire magnetic plate to warp after firing. Therefore, the groove width is preferably 100 μm or more, and the depth is preferably 50 μm or less.

[0024] If the groove width is too wide, the volume for accommodating the leaked magnetic adhesive will also be large, and there will be areas where the magnetic adhesive is not filled, making it difficult to form a magnetic adhesive layer over the entire surface of the magnetic plate facing portion. As a result, magnetic flux will leak in the areas where the magnetic adhesive is missing, so a groove width that is too wide is not preferable. The desirable range is about 100 μm to 300 μm.

[0025] When a frequency signal is input from the external electrode 14 to the winding 15, a magnetic flux corresponding to the signal passes through the winding core 11, the flange 12, the magnetic adhesive 17, the magnetic plate 16, the magnetic adhesive 17, the flange 13, and the winding core 11. If the gap between magnetic plate 16 and flange 12 and flange 13 is 2 μm or less, most of the magnetic flux does not leak even if an adhesive that does not contain magnetic material is used, but as the gap becomes larger, the magnetic flux leakage also becomes larger.

[0026] Comparing the differences with Patent Document 1, Patent Document 1 uses an adhesive that does not contain fillers such as magnetic materials. It describes how the center of the flange is made flat and this part is in direct contact with the magnetic plate without the use of adhesive, forming a closed magnetic circuit and reducing magnetic resistance, thereby obtaining a large inductance. However, Patent Document 1 has a tapered part at the edge of the flange, and since this tapered part is not in contact with the magnetic plate, a magnetic gap is formed, which generates magnetic resistance and leads to a decrease in inductance due to magnetic flux leakage.

[0027] When applying the configuration of the present invention to Patent Document 1, it is essential to use an adhesive containing a magnetic material. If an adhesive containing no magnetic material were applied over the entire surface, it would result in a large drop in inductance. However, if a magnetic material is applied between the tapered and flat portions of the flange and the magnetic plate, no magnetic resistance occurs and high inductance can be maintained. Furthermore, the bonding area with the magnetic adhesive can be made large, so an extremely large joining force can be obtained.

[0028] The magnetic core 10 is formed by mixing ferrite powder with a binder, press-molding the mixture, and sintering the mixture. In order to improve the release of the ferrite powder from the press die, the corners of the magnetic core 10 must be chamfered. Therefore, the corners 12b and 13b on the flange winding core side and the outer corners 12c and 13c on the flange where the magnetic adhesive 17 is formed are also chamfered with a certain radius of curvature. The magnetic flux loop passes not only through the central region of the flange joints 12a and 13a, but also through the flange winding core side corners 12b and 13b. If no magnetic material is present in these areas, magnetic flux leakage will occur, resulting in a decrease in inductance.

[0029] Fig. 3(A) shows a conventional common mode choke coil, and Fig. 3(B) is an enlarged cross-sectional view of the joint between flange 12 and magnetic plate 16 via magnetic adhesive 17. In this enlarged cross-sectional view, flange winding core side corner 12b is not covered with magnetic adhesive. That is, magnetic flux leakage occurs in this portion, resulting in a decrease in inductance. In contrast, the common mode choke coil of the present invention completely covers the trajectory through which the magnetic flux passes with magnetic adhesive 17, so there is no decrease in inductance and it is possible to ensure stable variation characteristics.

[0030] Furthermore, since the bonding area between the flanges 12, 13 and the magnetic plate 16 via the magnetic adhesive 17 in the present disclosure is large, the bonding strength is stronger than that of conventional common mode choke coils.

[0031] Next, a method for manufacturing the common mode choke coil according to the embodiment of the present disclosure will be described.

[0032] The magnetic core 10 is made up of a winding core 11 and a pair of flanges 12 and 13 provided on both ends of the winding core, and is obtained by mixing ferrite powder with a binder, press-molding the mixture, and sintering the mixture. An integrated external electrode 14 that spans from the outer surface to the bottom surface of the flanges 12 and 13 is joined with a magnetic adhesive 17. A pair of insulatingly coated conducting wires are wound around the winding core 11, and are electrically connected to the external electrodes 14 by laser welding.

[0033] 4 is a schematic diagram showing the manufacturing method of the present invention after the above steps. FIG. 4 shows a method of manufacturing a common mode choke coil in which grooves 16e are formed in the magnetic plate 16 shown in FIG. 2. The ferrite green sheet 16 is made by dispersing a ferrite magnetic material in an organic solvent containing a binder to form a slurry, which is then molded into a sheet to obtain a ferrite green sheet. The thickness of the ferrite green sheet is about 30 μm, and 26 of these are stacked and pressed to obtain a laminate with a thickness of 0.7 mm as shown in Figure 4(A). The laminate is pressed against a stamper equipped with multiple semicircular arc-shaped protrusions, each about 20 μm high and 100 μm wide, to form grooves in the laminate, forming grooves in the ferrite green sheet laminate.

[0034] Next, this is cut to a specified size and then fired to obtain individual magnetic plates 16 with grooves formed therein. After this, barrel polishing is performed to chamfer the corners of the magnetic plate 16 and roughen the entire outer periphery. This prevents chipping of the magnetic plate 16 and the anchor effect strengthens the bond with the magnetic adhesive. The thickness of the magnetic plate 16 at this point is approximately 0.6 mm.

[0035] The magnetic plate 16 is arranged on a fixture (not shown), and the magnetic adhesive 17 is formed thereon by printing or the like, as shown in FIG. 4(B). The pattern of the magnetic adhesive 17 is not formed in the places corresponding to the grooves 16e of the magnetic plate 16. The thickness of the magnetic adhesive 17 at this time is approximately 30 μm. The thickness of the magnetic adhesive is not limited to this numerical value, but is determined by the flatness of the flange joint and the chamfer R of the corners on the flange winding core side. The thickness of 30 μm is determined from the chamfer R radius of the flange corners, which is approximately 20 μm, and the flatness of the flange joint, which is 5 to 10 μm.

[0036] When a frequency signal is input to external electrode 14, the magnetic flux loop also passes through the corner on the flange winding core side. If there is no magnetic material in this portion, magnetic flux leakage occurs, resulting in a decrease in inductance, but if a layer of adhesive thicker than corner R is formed so that at least the corner on the flange winding core side is not exposed, leakage of the magnetic flux loop that passes through the corner on the flange winding core side can be prevented, and high inductance can be ensured.

[0037] The specific thickness of the magnetic adhesive 17 is 10 to 50 μm, preferably 20 to 40 μm. Since the flatness of the flange joint is about 5 to 10 μm, in order to fill the gap between the flange joint and the magnetic plate joint with the magnetic adhesive, the magnetic adhesive needs to have a thickness equal to or greater than the flatness of the magnetic plate, and also needs to have a thickness equal to or greater than the chamfer radius of the flange corner on the winding core side.

[0038] Next, as shown in Fig. 4(C), while the surface on which the magnetic adhesive 17 is formed faces upward, the flange joints 12a, 13a of the magnetic core 10 on which winding and laser welding have been completed are faced downward and pressed against the surface on which the magnetic adhesive 17 is formed. By pressing in this manner, part of the magnetic adhesive 17 that overflows from the flange joints 12a, 13a enters the groove 16e of the magnetic plate 16, making it extremely unlikely that the magnetic adhesive 17 will adhere to the winding 15. In the present invention, the depth of the groove 16e is set to 20 µm and the width to 100 µm or more, but this is not limited thereto. Depending on the dimensions and flatness of the flange, the size of the groove needs to be changed as appropriate.

[0039] Thereafter, the magnetic core 10 and the magnetic plate 16 are fixed together by processing for one hour at a magnetic adhesive hardening temperature of 150° C., completing the common mode choke coil.

[0040] 5 shows a manufacturing method in which the magnetic core 10 is fixed to a hoop or the like and the flange joints 12a and 13a face upward. The method for forming the groove 16e in the ferrite sheet laminate is the same as the manufacturing method in FIG. 4, so a description thereof will be omitted.

[0041] A pattern of magnetic adhesive 17 is formed on a resin sheet 19 such as PET. In the printing method, a printed pattern corresponding to the individual magnetic plate pieces or a line-shaped pattern may be formed using a blade with grooves cut into it. The thickness of the magnetic adhesive 17 at this time is also about 30 μm. Next, the grooved portion 16e surface of the magnetic plate 16 is turned downward and pressed against the magnetic adhesive pattern, and the pattern of magnetic adhesive 17 is transferred onto the magnetic plate 16. Next, the magnetic core with the windings 15 attached thereto is fixed to a hoop or the like. The magnetic plate 16 on which the magnetic adhesive pattern is formed is pressed against the winding 15. This pressing causes some of the magnetic adhesive 17 that overflows from the flange joints 12a, 13a to enter the groove 16e of the magnetic plate 16, making it extremely unlikely for the adhesive to adhere to the winding 15. The magnetic core 10 and the magnetic plate 16 are then fixed together by processing at an adhesive curing temperature of 150°C for one hour, and the magnetic core 10 and the magnetic plate 16 are then separated from the hoop, completing the common mode choke coil.

[0042] Here, a conventional method for forming an adhesive is explained. In Patent Document 1, after forming an adhesive on the flange, a magnetic plate is pressed against the surface, and the adhesive is spread and fixed by utilizing the capillary phenomenon or the like. Although the method for applying the adhesive is not described, the common methods are forming the adhesive by a pin transfer method or a dispenser application method. If the adhesive application surface of the flange is polished to promote flattening, it is possible to fill the magnetic plate and the flange with adhesive without any gaps, but if it is not polished, problems such as insufficient adhesive filling are likely to occur.

[0043] The flatness of each plane of the magnetic core produced by powder molding of magnetic powder is poor. When the flatness of the flange joint that faces the magnetic plate is measured, it is recessed by about 5 to 10 μm in the direction parallel to the winding core direction of both the left and right flanges. In other words, the outer surface side of the flange joint is higher and the winding core side is lower. Even if adhesive is applied to the flange joint in this state by pin transfer or a dispenser and a magnetic plate is pressed against it, there are likely to be areas where the adhesive is not present. In addition, since the flange is lower toward the winding core side, the probability of the adhesive not being present is extremely high, and magnetic flux leakage occurs in these areas.

[0044] Therefore, as described in the manufacturing method of the present invention, by applying an adhesive containing a magnetic material to the entire surface of the joint and opposing parts of the magnetic plate, leakage of magnetic flux can be suppressed, so that inductance and other properties can be achieved as designed and variations in the inductance can be reduced. In addition, since the bonding area between the magnetic plate and the flange via the adhesive is large, a high adhesive strength can be achieved.

[0045] Next, a specific embodiment will be described.

[0046] Example 1: A magnetic core with a size of 3.2 mm x 2.5 mm, a flange width of 600 μm, and a magnetic permeability of 880 at 1 MHz, and a magnetic permeability of 800 at 1 MHz, and a 40 μm diameter Cu wire were wound 30 turns around the core of the magnetic core, and the magnetic core and the magnetic plate were joined via a magnetic adhesive made of 1 part by weight of epoxy resin and 2 parts by weight of Ni-Zn ferrite powder dispersed therein, to produce 10 common mode choke coils as shown in FIG. 1. The manufacturing method was according to the method in FIG. 4. The thickness of the magnetic adhesive between the magnetic plate and the flange after the common mode choke coil was produced was 10 μm.

[0047] Example 2: Similarly, a magnetic core with a size of 3.2 mm x 2.5 mm, a flange width of 600 μm, and a magnetic permeability of 880 at 1 MHz and a magnetic permeability of 800 at 1 MHz were wound with 30 turns of 40 μm diameter Cu wire around the core of the magnetic core, and the magnetic core and magnetic plate were joined together using a magnetic adhesive made of 1 part by weight of epoxy resin with 2 parts by weight of Ni-Zn ferrite powder dispersed therein, to produce 10 common mode choke coils as shown in FIG. 2. The manufacturing method was according to the method shown in FIG. 4. The thickness of the magnetic adhesive between the magnetic plate and the flange was 10 μm.

[0048] Comparative Example 1: A magnetic core with a size of 3.2 mm x 2.5 mm, a flange width of 600 μm, and a magnetic permeability of 880 at 1 MHz, and a Cu wire with a diameter of 40 μm were wound 30 turns around the core of the magnetic core, and the magnetic core and magnetic plate were joined via a magnetic adhesive made of 1 part by weight of epoxy resin and 2 parts by weight of Ni-Zn ferrite powder dispersed therein, to produce 10 common mode choke coils as shown in FIG. 3. The manufacturing method was a conventional method in which four dots of magnetic adhesive with a diameter of 450 μm and a height of 60 μm were applied by pin transfer. The thickness of the magnetic adhesive between the magnetic plate and the flange at this time was 10 μm.

[0049] The 1MHz inductance value and its variation of the above common mode choke coil, as well as the bonding strength between the magnetic plate and the magnetic core were measured with a push-pull gauge. Both flanges of the magnetic core were clamped in a vice and the magnetic plate was pushed in from the longitudinal direction with a push pin, and the strength at which the magnetic plate came off or the strength at which the magnetic plate and the magnetic core broke were measured. These results are shown in Table 1.

[0050] [Table 1]

[0051] The inductance was designed assuming 1MHz:95μH in the simulation, and in Example 1 and Example 2, the value was realized as designed, and the characteristic value variation was small. The comparative example was 10μH lower than the design value. This is because the magnetic adhesive was not able to cover the corners of the flange winding core side. Incidentally, when the magnetic adhesive was applied to the corners of the flange winding core side of Comparative Example 1 afterwards and the corners were completely covered with magnetic adhesive, the inductance value increased to 91μH. The reason why it still did not reach the design value of 95μH is because there was a part where the magnetic adhesive was not filled at the joint between the magnetic core and the flange. In addition, the adhesive strength between the magnetic plate and the magnetic core is clearly higher in Examples 1 and 2 than in the conventional comparative examples. Here, an example was given in which a magnetic adhesive was used, but if the magnetic material was not included, the average impedance would be reduced to 70μH even in Example 1. This is because the magnetic resistance of the joint between the magnetic plate and the flange became large. Using an adhesive containing a magnetic material is also advantageous in terms of characteristics.

[0052] In the above manufacturing method, a method of forming a groove in the magnetic plate using a stamper has been described, but if the flatness of the flange of the magnetic core is high on the outer surface and low on the winding core side, it is also possible to process the stamper into a concave shape and create a magnetic plate that matches the shape of the flange. This makes it possible to reduce the gap between the magnetic core and the magnetic plate, making it possible to achieve an inductance value with less variation. [Industrial Applicability]

[0053] INDUSTRIAL APPLICABILITY The common mode choke coil and its manufacturing method of the present invention can provide a highly reliable common mode choke coil having high inductance with small variation in inductance and high bonding strength between the magnetic plate and the magnetic core, making it industrially useful. [Explanation of symbols]

[0054] 10 Magnetic core 11 core part 12. Blade 12a Flange joint 12b Flange core side corner 12c Outside corner of flange 13. Tail 13a Flange joint 13b Flange core side corner 13c Outer corner of flange 14 External electrodes 15 reels 16 Magnetic Board 16a Joint 16c Magnetic plate outer corner 16d Opposite part 17 Magnetic adhesive 19 Resin シート

Claims

1. A common mode choke coil comprising: a magnetic core having a winding core and a pair of flanges provided at both ends of the winding core; an external electrode formed on the flange; a pair of windings wound around the winding core and having ends extended to and joined to the external electrodes; and a magnetic plate joined to the pair of flanges, the magnetic plate has a joining portion joined to the flange portion and an opposing portion opposing the winding core portion, A groove having a width of 100 μm to 300 μm and a depth of 20 μm to 50 μm is formed in the facing portion, A common mode choke coil in which a layer of magnetic adhesive is formed on the entire surfaces of the joint portion and the opposing portion, the layer of magnetic adhesive being a thermosetting adhesive layer containing resin and magnetic powder.

2. A method for manufacturing a common mode choke coil comprising a magnetic core having a winding core and a pair of flanges provided at both ends of the winding core, an external electrode formed on the flange, a pair of windings wound around the winding core and having ends extended to the external electrodes and joined thereto, and a magnetic plate joined to the pair of flanges, the method comprising the steps of: laminating and pressing a plurality of magnetic sheets to form a laminate; pressing the laminate with a parallel plate die having a protrusion on at least one side to form a laminate having a width of 100 μm to 300 μm and a depth of 20 μm; A method for manufacturing a common mode choke coil, comprising the steps of: providing a groove portion of 50 μm or less; cutting the laminate with the groove portion provided into individual pieces and firing the laminate to create a magnetic plate; arranging a plurality of the fired magnetic plates with the groove portion facing up, and forming a layer of magnetic adhesive by printing on the entire surface of the magnetic plate where the groove portion is formed and which faces the magnetic core; pressing the flange portion of the magnetic core onto the layer of magnetic adhesive, and then thermally curing the layer of magnetic adhesive, wherein the layer of magnetic adhesive is a thermosetting adhesive layer containing resin and magnetic powder.

3. A method for manufacturing a common mode choke coil comprising a magnetic core having a winding core and a pair of flanges provided at both ends of the winding core, an external electrode formed on the flange, a pair of windings wound around the winding core and having ends extended to the external electrodes and joined thereto, and a magnetic plate joined to the pair of flanges, the method comprising the steps of: laminating and pressing a plurality of magnetic sheets to form a laminate; pressing the laminate with a parallel plate die having a protrusion on at least one side to form a groove having a width of 100 μm to 300 μm and a depth of 20 μm to 50 μm; cutting the laminate with the grooves provided into individual pieces and firing the pieces to form a magnetic plate; A method for manufacturing a common mode choke coil, comprising the steps of: printing an adhesive; pressing the adhesive on the resin film against the surface on which the groove is formed, transferring the magnetic adhesive, and forming a layer of the magnetic adhesive over the entire surface on which the groove is formed; and pressing the surface on which the magnetic adhesive layer is formed against the flange portion of the magnetic core, and then thermally curing the surface, wherein the magnetic adhesive is a thermosetting adhesive containing resin and magnetic powder.

4. 4. The method for manufacturing a common mode choke coil according to claim 2, wherein the thickness of the magnetic adhesive applied to the portion of the magnetic plate facing the winding core portion is thicker than the corner R of the flange portion.

Citation Information

Patent Citations

  • Common mode choke and manufacturing method thereof

    CN102074332A

  • JP1976081918U

  • Inductor -

    JP1984171315U

  • Paste application method and paste application apparatus

    JP2001062362A

  • Method for manufacturing wound coil component and coil component

    JP2003086442A