Enhanced guided self-assembly in the presence of low Tg oligomers for pattern formation

Low Tg oligomeric materials in block copolymer compositions address defects in self-assembly processes, enabling high-quality pattern formation for integrated circuits beyond 50 nm thickness.

JP7592017B2Active Publication Date: 2024-11-29MERCK PATENT GMBH
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021541212
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-04
Filing Date
2020-01-15
Publication Date
2024-11-29
Estimated Expiration
2040-01-15

AI Technical Summary

Technical Problem

Self-assembly of block copolymers like PS-b-PMMA results in significant defects in contact hole and line/space multiplication processes when film thickness exceeds 50 nm, leading to misalignment, bridges, and line or cylinder collapse, hindering the production of high-yield integrated circuits.

Method used

Incorporation of low Tg oligomeric materials into block copolymer compositions to reduce defects, using specific oligorandom and oligodiblock copolymers with controlled molecular weights and glass transition temperatures, which are processed through spin casting and annealing to form defect-reduced patterns.

Benefits of technology

The method enables the formation of high-quality, defect-reduced patterns even at film thicknesses greater than 50 nm, improving the yield and reliability of integrated circuit fabrication.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007592017000045
    Figure 0007592017000045
  • Figure 0007592017000046
    Figure 0007592017000046
  • Figure 0007592017000047
    Figure 0007592017000047
Patent Text Reader

Abstract

The present invention relates to a composition comprising components a), b), and c). Component a) is a block copolymer or a blend of multiple block copolymers. Component c) is a low Tg additive selected from the group consisting of oligorandom oligorandom copolymer b-1), oligodiblock copolymer b-2), oligodiblock copolymer b-2), and a mixture of at least two thereof. Component c) is an organic solvent for spin-casting. The present invention also relates to the use of the composition in directed self-assembly. Furthermore, the present invention relates to the novel oligodiblock copolymer b-2), which is an oligodiblock copolymer of block Ab) and block Bb), wherein Block Ab) is a random copolymer of repeating units having structures (III) and (IV), and Block Bb) is a random copolymer of repeating units having structures (V) and (VI). TIFF2022517412000036.tif48170
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to block copolymers and block copolymer compositions, and novel methods of using the block copolymer compositions to align microdomains of self-assembling block copolymers (BCPs) to form self-assembled features useful for forming arrays of contact holes or lines and spaces, which compositions and methods are useful in the manufacture of electronic devices. [Background technology]

[0002] Self-assembly of block copolymers is a useful method for generating ever smaller patterned features for the manufacture of microelectronic devices, which can achieve nanoscale feature critical dimensions (CD). Self-assembly methods are desirable for extending the resolution capabilities of microlithography techniques for repeating features such as arrays of contact holes or posts. Conventional lithography methods may use ultraviolet (UV) light to expose through a mask to a photoresist layer coated on a substrate or laminate substrate. Positive or negative photoresists are useful, and they may also contain refractory elements such as silicon to allow dry development using conventional integrated circuit (IC) plasma processing techniques. In positive photoresists, UV radiation passing through a mask causes a photochemical reaction in the photoresist that renders the exposed areas removable with a developer solution or by conventional IC plasma processing. Conversely, in negative photoresists, UV radiation passing through a mask renders the exposed areas less removable with a developer solution or by conventional IC plasma processing. Integrated circuit features such as gates, vias or interconnects are then etched into the substrate or layered substrate, and the remaining photoresist is removed. Using conventional lithographic exposure processes, there is a limit to the feature size of integrated circuit features. Further reduction in pattern size is difficult to achieve using radiation exposure due to limitations related to aberrations, focus, proximity effects, minimum achievable exposure wavelength, and maximum achievable numerical aperture. Due to the need for large scale integration, device circuit dimensions and features have been continually reduced. In the past, the final resolution of features has depended on the wavelength of light used to expose the photoresist, which is itself limited. Guided self-assembly techniques such as graphoepitaxy and chemoepitaxy using block copolymer imaging with patterned regions on the substrate are highly desirable techniques used to improve resolution while reducing CD variation.These techniques can be used to augment conventional UV lithography techniques or to enable even higher resolution and CD control in approaches using EUV, e-beam, deep UV or immersion lithography. Directed self-assembly block copolymers contain blocks of etch-resistant copolymeric units and blocks of etch-prone copolymeric units that, when coated, aligned and etched on a substrate, provide areas of very dense patterns.

[0003] Therefore, for guided or unguided self-assembly of block copolymer films on patterned or unpatterned substrate regions, typically the self-assembly process of the block copolymer layer occurs during annealing of the film over a neutral layer. The neutral layer on the semiconductor substrate may be an unpatterned neutral layer, or in chemoepitaxy or graphoepitaxy, the neutral layer may include graphoepitaxy or chemoepitaxy guided features (formed via UV lithography techniques as described above). During annealing of the block copolymer film, the underlying neutral layer induces nanophase separation of the block copolymer domains. One example is the formation of phase-separated domains that are lamellae or cylinders perpendicular to the underlying neutral layer surface. These nanophase-separated block copolymer domains form pre-patterns (e.g., lines and spaces L / S) that can be transferred into the substrate via an etching process (e.g., plasma etching). In graphoepitaxy or chemoepitaxy, these guiding features induce both pattern tailoring and pattern multiplication. In the case of unpatterned neutral layers, this produces, for example, repeating arrays of L / S or CH. For example, in conventional block copolymers such as poly(styrene-b-methyl methacrylate) (P(Sb-MMA)), where both blocks have similar surface energies at the BCP-air interface, this can be achieved by coating and thermal annealing the block copolymer onto a layer of non-preferential or neutral material that has been grafted or crosslinked at the polymer-substrate interface.

[0004] In the graphoepitaxy-induced self-assembly method, block copolymers self-assemble around a substrate that has been pre-patterned using conventional lithography (ultraviolet, deep UV, e-beam, extreme ultraviolet (EUV) exposure sources) to form repeating topographical features such as line / space (L / S) or contact hole (CH) patterns. In one example of an L / S-induced self-assembly array, the block copolymers can form self-aligned lamellar regions that can form parallel line-space patterns of different pitches in the trenches between the pre-patterned lines, enhancing pattern resolution by dividing the spaces in the trenches between the topographical lines into finer patterns. For example, diblock or triblock copolymers that can microphase separate and contain carbon-rich blocks (e.g., containing styrene or some other elements such as Si, Ge, Ti) that are resistant to plasma etching and blocks that are highly plasma etchable or removable can provide high-resolution pattern definition. An example of a highly etchable block may include a monomer, such as methyl methacrylate, that is oxygen-rich and free of refractory elements and yet capable of forming a highly etchable block. The plasma etching gases used in the etching process that defines the self-assembled pattern are typically those used in processes used in the manufacture of integrated circuits (ICs). In this manner, much finer patterns can be created in typical IC substrates than could be defined by conventional lithographic techniques, thus achieving pattern multiplication. Similarly, using graphoepitaxy, where a suitable block copolymer aligns itself by directed self-assembly around an array of contact holes or posts defined by conventional lithography, features such as contact holes can also be created more densely by forming a denser array of regions of etchable and etch-resistant domains that, when etched, give a denser array of contact holes. As a result, graphoepitaxy has the potential to provide both pattern tuning and pattern multiplication.

[0005] In chemical epitaxy or pinned chemical epitaxy, the self-assembly of block copolymers is formed on a surface that has no or little topography (also called non-guiding topography) that guides the shape of regions of different chemical affinity but determines the guided self-assembly process. For example, the surface of a substrate can be patterned using conventional lithography (UV, deep UV, e-beam, EUV) to generate a line-and-space (L / S) pattern of surfaces of different chemical affinity in which exposed regions, where the surface chemistry has been modified by radiation, alternate with unexposed regions that show no chemical change. These regions do not provide topographical differences, but surface chemical differences or pinning that guide the self-assembly of the block copolymer segments. Specifically, guided self-assembly of block copolymers with block segments that contain etch-resistant repeat units (e.g., styrene repeat units) and fast-etching repeat units (e.g., methyl methacrylate repeat units) would allow precise placement of the etch-resistant and fast-etching block segments on the pattern. This technique allows for precise placement of these block copolymers and subsequent pattern transfer to a substrate after plasma or wet etching processing. Chemical epitaxy has the advantage that this can be fine-tuned by changing chemical differences, allowing for tuning of the pattern, helping to improve line edge roughness and CD control. Other types of patterns, such as repeating contact hole (CH) arrays, can also be patterned using chemo-epitaxy.

[0006] These neutral layers are layers on the substrate or surfaces of the treated substrate that have no affinity for any of the block segments of the block copolymers used for directed self-assembly. Neutral layers are useful in graphoepitaxy methods of directed self-assembly of block copolymers because they allow for proper placement or orientation of the block polymer segments for directed self-assembly resulting in proper placement of the etch-resistant and highly etchable block polymer segments relative to the substrate. For example, in a surface containing line-and-space features defined by conventional radiation lithography, the neutral layer allows for the orientation of the block segments such that they are oriented perpendicular to the surface of the substrate, which is an ideal orientation for both pattern tuning and pattern multiplication depending on the length of the block segments in the block copolymer relative to the length between the lines defined by conventional lithography. If the substrate interacts too strongly with one of the block segments, the segment will lie flat on its surface, maximizing the contact area between the segment and the substrate; such a surface would disrupt the desired vertical alignment that can be used to achieve either pattern tuning or pattern multiplication based on features generated by conventional lithography. Modification or pinning selected small regions of the substrate to cause them to interact strongly with one block of the block copolymer, while leaving the remainder of the substrate coated with a neutral layer, can be useful to align the domains of the block copolymer in a desired direction, and this is the basis for pinned chemo- or graphoepitaxy used for pattern multiplication. [Prior art documents] [Non-patent literature]

[0007] [Non-Patent Document 1] Macromolecules 2019,52,2987-2994 [Non-Patent Document 2] Macromol.Rapid Commun.2018,39,1800479 [Non-Patent Document 3] A.Deiter Shluter et al Synthesis of Polymers,2014,Volume 1,p315 [Non-Patent Document 4] Encyclopedia of Polymer Science and Technology,2014,Vol 7,p.625 [Non-Patent Document 5] JBKruger, et al, “VLSI Electronics, Microstructure Science” Chapter 5, Academic Press, p.91-136, 1984 [Non-Patent Document 6] “Etch considerations for directed self-assembly patterning using capacitively coupled plasma”Vinayak Rastogi et al,Journal of Vacuum Science & Technology A36,031301,2018 [Non-Patent Document 7] David Uhrig and Jimmy Mays, “Techniques in High-Vacuum Anionic Polymerization”, Journal of Polymer Science:Part A: Polymer Chemistry,Vol.43,6179-6222(2005) [Non-Patent Document 8] Makmrnol.Chem.191,2309-2318(1990) [Non-Patent Document 9] Adv. Polym. Sci. 86, 147 (1988) Summary of the Invention [Problem to be solved by the invention]

[0008] Self-assembly using polystyrene-b-polymethylmethacrylate (PS-b-PMMA) has been widely used as a next-generation patterning material in lithography, and the nanophase separation assembly process produces well-ordered arrays of domains, but this occurs with significant amounts of defect formation when the film thickness exceeds 50 nm. These defects are prominent in contact hole and line / space multiplication processes and need to be greatly reduced to improve device yields in any commercially viable IC fabrication using directed self-assembly. One of the causes of defects is insufficient diffusion of block segments that gives rise to defects such as misregistration, bridging, networking, and collapse of lines or cylinders. Therefore, there is a need for new materials and methods that can affect directed self-assembly even in the case of such thick films. [Means for solving the problem]

[0009] The present inventors have discovered a series of low Tg oligomeric materials that can be used as additives to form novel block copolymer compositions and that can induce self-assembly of block copolymer domains that contain greatly reduced numbers of these defects, even at film thicknesses greater than 50 nm. [Brief description of the drawings]

[0010] [Figure 1]Top-down SEM study of contact hole arrays of self-assembled films of block copolymers of styrene and methyl methacrylate with or without oligo(S-co-MMA) additive [Synthesis Example 5]: 50 nm thick (approximately 1Lo); film cast on a film of neutral layer. The neutral layer was formed by casting neutral formulation Example 1 (74% PS) on a silicon wafer and baking it at 240°C / 5 min, followed by washing with PGMEA for 30 s and baking at 110°C for 1 min. Films of Formulations 1-3 (Form.Ex.1-3) contained 1.5 wt% solids in PGMEA, and blends of P(Sb-MMA) and 0-20 wt% oligo(S-co-MMA) (listed in Table 1) in PGMEA were spin-coated at 1500 rpm on top of this neutral layer to form films (Lo=45.3 / FT 50 nm) which were then baked at 250°C for 5 min under nitrogen to induce self-assembly, and etched with oxygen plasma for 50 and 70 s. [Diagram 2] X-section SEM study of contact hole array of self-assembled film of block copolymer of styrene and methyl methacrylate with or without oligo(S-co-MMA) additive [Synthesis Example 5]: film thickness 50 nm (about 1Lo); film cast on neutral layer film. Neutral layer was formed by casting neutral formulation example 1 (74% PS) on silicon wafer and baking it at 240°C / 5 min, followed by washing with PGMEA for 30 s and baking at 110°C for 1 min. Films of Formulations 2 and 3 (Form. Ex. 2 and 3) (listed in Table 1) contained 1.5 wt% solids in PGMEA, and a blend of P(Sb-MMA) and 10-20 wt% oligo(S-co-MMA) (listed in Table 1) in PGMEA was spin-coated at 1500 rpm on top of this neutral layer to form a film (Lo=45.3 / FT50nm) which was then baked at 250°C for 5 minutes under nitrogen to induce self-assembly and etched with oxygen plasma for 50 seconds. [Diagram 3]Top-down SEM study of contact holes in self-assembled films of block copolymers of styrene and methyl methacrylate with or without oligo(S-co-p-OS)-bP(MMA-co-DEGMEMA) additive [Synthesis Example 8]: film thickness was 50 nm (about 1Lo); cast on the film of neutral layer. The neutral layer was formed by casting neutral formulation example 1 (74% PS) on a silicon wafer and baking it at 240°C / 5 min, followed by washing with PGMEA for 30 s and baking at 110°C for 1 min. Films of Formulations 1, 4, and 5 (Form.Ex.1, 4, and 5) contained 1.5 wt% solids in PGMEA and were spin-coated at 1500 rpm on top of the neutral layer with blends of P(Sb-MMA) and oligo(S-co-p-OS)-bP(MMA-co-DEGMEMA) (Synth.Ex.8) (listed in Table 1) at 0-20 wt% in PGMEA to form films (Lo=45.3 / FT50nm) which were then baked at 250°C for 5 min under nitrogen to induce self-assembly and etched with oxygen plasma for 50 and 70 s. [Figure 4] Top-down SEM study of lines and spaces of self-assembled films of block copolymers of styrene and methyl methacrylate with and without oligo(S-co-p-OS)-bP(MMA-co-DEGMEMA) additive [Synthesis Example 9]: 50 nm thick (approximately 1Lo); film cast on a neutral layer film. The neutral layer was formed by casting neutral formulation example 1 (74% PS) on a silicon wafer and baking it at 240°C / 5 min, followed by washing with PGMEA for 30 s and baking at 110°C for 1 min. Films of Formulations 6, 10, 11 and 12 (Form. Ex. 6, 10, 11 and 4) contained 1.5 wt% solids in PGMEA and were spin-coated at 1500 rpm on top of the neutral layer with blends of P(Sb-MMA) and oligo(S-co-p-OS)-bP(MMA-co-DEGMEMA) (Synth. Ex. 9) (listed in Table 3) at 0-20 wt% in PGMEA to form films (Lo=45.3 / FT50nm) which were then baked at 250°C for 5 min under nitrogen to induce self-assembly and then etched with oxygen plasma for 50 and 70 s. [Diagram 5]Top-down SEM study of L / S of self-assembled film of styrene and methyl methacrylate block copolymer with or without oligo(Sb-MMA) additive [Synthesis Example 8]: film thickness was 50 nm (about 1Lo); cast on neutral layer film after etching with oxygen plasma. The neutral layer was formed by casting neutral formulation Example 1 (74% PS) on silicon wafer and baking it at 240°C / 5 min, followed by washing with PGMEA for 30 s and baking at 110°C for 1 min. Films of Formulations 6 (0 wt%), 13 (10 wt%) and 14 (20 wt%) (Form. Ex. 6, 13 and 14) contained 1.5 wt% solids in PGMEA and P(Sb-MMA) as block copolymer (42K-47K) and oligo(Sb-MMA) (Synth. Ex. 7) (listed in Table 3) at 0-20 wt% in PGMEA were spin-coated at 1500 rpm on top of the neutral layer to form films (Lo=45.3 / FT50nm) which were then baked at 250°C for 5 minutes under nitrogen to induce self-assembly and then etched with oxygen plasma for 30 seconds. [Figure 6] Top-down SEM examination of the L / S of self-assembled films of triblock copolymer comparative formulation 4 without oligomer [Synthesis Example 4a (50K-88k-50k)], formulation example 15 containing 20 wt% oligomer [Synthesis Example 9] or 20 wt% oligomer [Synthesis Example 7a].

[0011] One aspect of the invention relates to a composition comprising components a), b) and c), wherein a) is a block copolymer component or a blend of at least two block copolymers, b) is a low Tg additive selected from the group consisting of oligorandom copolymers b-1), oligodiblock copolymers b-2), oligodiblock copolymers b-3), and mixtures thereof, wherein b-1), b-2) and b-3) are as follows, and c) is a spin casting solvent:

[0012] b-1) is an oligorandom copolymer of two repeating units having the structures (Ib) and (IIb), in which R 1b and R 3b are independently selected from H or C1-C4 alkyl; R 2b is H or C1-C8 alkyl, R 4b is a C1-C8 alkyl, and the mole % values ​​based on the total number of moles of repeating units of structures (Ib) and (IIb) are about 40 mole % to about 80 mole % for repeating units of structure (Ib) and about 20 mole % to about 60 mole % for repeating units of structure (IIb), and the individual values ​​of the mole % for repeating units of structures (Ib) and (IIb) are selected from their respective ranges such that the total number of moles of repeating units of structures (Ib) and (IIb) total 100 mole %; and further the oligorandom copolymer b-1) has a Tg of about 0° C. to about 80° C., and a Mn of about 1000 g / mol to about 8,000 g / mol, and a polydispersity of about 1.3 to about 1.8:

[0013] [ka] b-2) is an oligodiblock copolymer of block Ab) and block Bb) having Mn of about 1,000 to 35,000 and polydispersity of 1.0 to about 1.1, where block Ab) is a random copolymer of repeating units having structures (III) and (IV), and block Bb) is a random copolymer of repeating units having structures (V) and (VI), and R5, R7, R9, and R 11 are independently selected from H or C1-C4 alkyl, R6 is a C7-C10 straight chain alkyl, R8 is a C1-C4 alkyl, and R 10 is C1-C4 alkyl, R 12 and R 13 are independently selected from C2-C5 alkylene, and R 14 is a C1 to C4 alkyl, and said oligodiblock copolymer b-2) has a Tg having a value of about 0°C to about 95°C.

[0014] [ka] b-3) is an oligodiblock copolymer of a block Ac) containing a repeating unit having the structure (Ic) and a block Bc) containing a repeating unit having the structure (IIc), in which R 1c and R 3c are independently selected from H or C1-C4 alkyl; R 2c is H or C1-C8 alkyl, R 4c is a C1-C8 alkyl, and the mole % values ​​based on the total number of moles of repeating units of Structures (Ic) and (IIc) are from about 36 mole % to about 74 mole % for repeating units of Structure (Ic) and from about 26 mole % to about 64 mole % for repeating units of Structure (IIc), and the individual values ​​of the mole % for repeating units of Structures (Ic) and (IIc) are selected from their respective ranges such that the total number of moles of repeating units of Structures (Ic) and (IIc) total 100 mole %; and the oligodiblock copolymer b-2) has a Mn of about 1000 g / mol to about 30,000 g / mol and a polydispersity of about 1.0 to about 1.1 and a Tg of about 0° C. to about 115° C.:

[0015] [ka] Another aspect of the invention is a method for using the composition in a self-assembly process and then pattern-transferring the self-assembled pattern into a substrate.

[0016] Yet another aspect of the present invention is a novel oligodiblock copolymer b-2) having the above block Ab) and block Bb). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] It is to be understood that both the general description above and the detailed description below are exemplary and explanatory, and are not intended to restrict the invention as claimed. In this application, unless specifically stated otherwise, the use of the singular includes the plural, the singular means "at least one," and the use of "or" means "and / or." Furthermore, the use of the term "comprises" and other verb forms such as "comprises" is not limiting. Also, the use of terms such as "element" or "component" includes both elements and components that contain one unit, and elements or components that contain more than one unit, unless specifically stated otherwise. Unless otherwise indicated, the conjunction "and" as used herein is intended to be inclusive, and the conjunction "or" is not intended to be exclusive. For example, the phrase "or instead of" is intended to be exclusive. As used herein, the conjunction "and / or" refers to any combination of the aforementioned elements, including the use of a single element.

[0018] The term C1-C4 alkyl is a generic term for methyl and C2-C4 straight chain alkyl and C3-C4 branched alkyl moieties, such as methyl (-CH3), ethyl (-CH2-CH3), n-propyl (-CH2-CH2-CH3), isopropyl (-CH(CH3)2, n-butyl (-CH2-CH2-CH2-CH3), tert-butyl (-C(CH3)3), isobutyl (CH2-CH(CH3)2, 2-butyl (-CH(CH3)CH2-CH3). Similarly, the term "C1-C8" is a generic term for methyl, C2-C8 straight chain alkyl, C3-C8 branched alkyl, C4-C8 cycloalkyl (e.g., cyclopentyl, cyclohexyl, etc.) or C5-C8 alkylenecycloalkyl (e.g., -CH2-cyclohexyl, CH2-CH2-cyclopentyl, etc.).

[0019] The term "C2-C5 alkylene" is a general term for C2-C5 linear alkylene moieties (eg, ethylene, propylene, etc.) and C3-C5 branched alkylene moieties (eg, -CH(CH3)-, -CH(CH3)-CH2-, etc.).

[0020] Diblock and triblock copolymers of styrenic and acrylic moieties useful as components in the compositions according to the invention described herein can be prepared by various methods, such as anionic polymerization, atom transfer radical polymerization (ATRP), reversible addition-fragmentation chain transfer (RAFT) polymerization, living radical polymerization and similar methods (Macromolecules 2019, 52, 2987-2994 (Non-Patent Document 1); Macromol. Rapid Commun. 2018, 39, 1800479 (Non-Patent Document 2); A. Deiter Shluter et al Synthesis of Polymers, 2014, Volume 1, p315 (Non-Patent Document 3); Encyclopedia of Polymer Science and Technology, 2014, Vol 7, p. 625 (Non-Patent Document 4)).

[0021] The random copolymer poly(styrene-co-methyl methacrylate) is abbreviated as "P(S-co-MMA)" and the oligomeric form of this material is abbreviated as oligo(S-co-MMA). Similarly, the block copolymer poly(styrene-block-methyl methacrylate) is abbreviated as P(Sb-MMA) while the oligomer of this material is abbreviated as oligo(Sb-MMA). The oligomer oligo(styrene-co-p-octylstyrene)-block-(methyl methacrylate-co-di(ethylene glycol) methyl ether methacrylate) uses the same abbreviations to refer to the block copolymer elements, specifically oligo(S-co-p-OS)-bP(MMA-co-DEGMEMA) (S=styrene, p-OS=para-octylstyrene, MMA=methacrylate, DEGMEMA=di(ethylene glycol) methyl ether methacrylate) to refer to the repeat units in this block copolymer where the two blocks are random copolymers.

[0022] The designation "g / mole" is an abbreviation for grams per mole.

[0023] FOV is an abbreviation for field of view for the top-down scanning electron microscopes (SEMs) in SEM drawings 1, 3, 4 and 5 of this application, in this example the field of view is 2 μm. The cross-sectional electron microscope (X-SEM) shown in FIG. 2 has a magnification of 250K. Field of view. The term "CH" is an abbreviation for contact hole lithography geometry and the term "L / S" is an abbreviation for line and space lithography geometry.

[0024] In the following description, "Synth" is an abbreviation for "synthesis"; "Comp" is an abbreviation for "comparative"; and the term "Ex" is an abbreviation for "Example."

[0025] The terms oligomer, oligo, and oligomeric polymer as used herein to refer to low Tg additives refer to low molecular weight polymers having a molecular weight range specific to the additive type referred to herein.

[0026] As used herein, the term "acrylic" generally includes repeat units derived from acrylate derivatives, such as repeat units derived from acrylate derivatives having the following structure: where the Alkyl portion can be a C1-C8 alkyl and Xacryl is either H or a C1-C4 alkyl:

[0027] [ka] As used herein, the term "styrenic" generally includes repeat units derived from styrene derivatives, such as repeat units derived from styrene derivatives having the structure: where Xsty moiety is H or a C1-C4 alkyl and Rsty is H or a C1-C8 moiety:

[0028] [ka] One aspect of the invention relates to a composition according to the invention comprising components a), b) and c), wherein a) is a block copolymer component or a blend of at least two block copolymers, b) is a low Tg additive selected from the group consisting of oligorandom copolymers b-1), oligodiblock copolymers b-2), oligodiblock copolymers b-3) and mixtures thereof, wherein b-1), b-2) and b-3) are as follows, and c) is a spin casting solvent:

[0029] b-1) is an oligorandom copolymer of two repeating units having the structures (Ib) and (IIb), in which R 1b and R 3b are independently selected from H or C1-C4 alkyl; R 2b is H or C1-C8 alkyl, R 4b is C1-C8 alkyl, and the mole percent values ​​based on the total number of moles of repeating units of structures (Ib) and (IIb) are about 40 mole % to about 80 mole % for repeating units of structure (Ib) and about 20 mole % to about 60 mole % for repeating units of structure (IIb), and the individual values ​​of the mole percents of repeating units of structures (Ib) and (IIb) are selected from their respective ranges such that the total number of moles of repeating units of structures (Ib) and (IIb) totals 100 mole %; and further the oligorandom copolymer b-1) has a Tg of about 0°C to about 80°C, and a Mn of about 1000 g / mol to about 8,000 g / mol, and a polydispersity of about 1.3 to about 1.8.

[0030] [ka] b-2) is an oligodiblock copolymer of block Ab) and block Bb) having Mn of about 1,000 to 35,000 and polydispersity of 1.0 to about 1.1, where block Ab) is a random copolymer of repeating units having structures (III) and (IV), and block Bb) is a random copolymer of repeating units having structures (V) and (VI), and R5, R7, R9, and R 11 are independently selected from H or C1-C4 alkyl, R6 is a C7-C10 straight chain alkyl, R8 is a C1-C4 alkyl, and R 10 is C1-C4 alkyl, R 12 and R 13 are independently selected from C2-C5 alkylene, and R 14 is a C1 to C4 alkyl, and said oligodiblock copolymer b-2) has a Tg having a value of about 0°C to about 95°C.

[0031] [ka] b-3) is an oligodiblock copolymer of a block Ac) containing repeating units having the structure (Ic) and a structure Bc) containing repeating units having the structure (IIc), where R 1c and R 3c is independently selected from H or C1-C4 alkyl; R 2c is H or C1-C8 alkyl, R 4c is C1-C8 alkyl. The mole % values ​​based on the total number of moles of repeating units of structures (Ic) and (IIc) are about 36 mole % to about 74 mole % for repeating units of structure (Ic) and about 26 mole % to about 64 mole % for repeating units of structure (IIc), and the individual values ​​of the mole % for repeating units of structures (Ic) and (IIc) are selected from their respective ranges such that the total number of moles of repeating units of structures (Ic) and (IIc) total 100 mole %, and the oligodiblock copolymer b-2) has an Mn of about 1000 g / mol to about 30,000 g / mol, a polydispersity of about 1.0 to about 1.1, and a Tg of about 0°C to about 115°C.

[0032] [ka] Another aspect of the compositions of the present invention comprising components a), b) and c) described herein is that component a) is selected from a single triblock copolymer and a blend of at least two triblock copolymers, or a single diblock copolymer and a blend of at least two diblock copolymers.

[0033] Component a) is a triblock copolymer.

[0034] Another aspect of the composition according to the present invention comprising components a), b) and c) is an embodiment in which the component a) is an ABA triblock copolymer component selected from the group consisting of ABA triblock copolymer component a-1t), ABA triblock copolymer a-2t), and a blend of ABA triblock copolymer a-1t) and ABA triblock copolymer a-2t).

[0035] In the above embodiment, a-1t) is an ABA triblock copolymer comprising a middle B styrenic block segment of repeating units having a styrenic structure (I) and two terminal acrylic block A) segments of equal length having the structure (II), where R1 and R3 are independently selected from H and C1-C4 alkyl, R2 is H or C1-C8 alkyl, and R4 is C1-C8 alkyl. Further, in this embodiment, the mole percent values ​​based on the total number of moles of repeating units of structures (I) and (II) are about 40 mole percent to about 80 mole percent for repeating units of structure (I) and about 20 mole percent to about 60 mole percent for repeating units of structure (II), and the individual mole percent values ​​of repeating units of structures (I) and (II) are selected from their respective ranges such that the total number of moles of repeating units of structures (I) and (II) total 100 mole percent, and the triblock copolymer a-1t) has a polydispersity of about 1.0 to about 1.1, and an Mn of about 70,000 g / mol to about 350,000 g / mol. In one aspect of this embodiment, the moiety R2 is attached to the aromatic ring of the styrenic unit via a para bond.

[0036] [ka] In the above embodiment, a-2t) is an ABA type triblock copolymer comprising a middle B) block segment of repeating units having an acrylic structure (Ia) and two end block B) segments of equal length having a styrenic structure (IIa), where R 1a and R 3a is independently selected from H and C1-C4 alkyl; R 2a is H or C1-C8 alkyl, R 4ais a C1-C8 alkyl, and the mole percent values ​​based on the total number of moles of repeating units of structures (Ia) and (IIa) are from about 40 mole percent to about 80 mole percent for repeating units of structure (Ia) and from about 20 mole percent to about 60 mole percent for repeating units of structure (IIa), and the individual values ​​of the mole percent values ​​for repeating units of structures (Ia) and (IIa) are selected from their respective ranges such that the total number of moles of repeating units of structures (Ia) and (IIa) total 100 mole percent; and the triblock copolymer a-2t) has a polydispersity of from about 1.0 to about 1.1 and a Mn of from about 70,000 g / mol to about 350,000 g / mol. In one aspect of this embodiment, the moiety R 2a is attached to the aromatic ring of the styrenic unit via a para bond.

[0037] [ka] In another aspect of the composition according to the invention, component a) is an ABA triblock copolymer selected from a-1t), a-2t), or blends thereof in the repeat units of structures (I), (II), (Ia) and (IIa). In another aspect of this embodiment, R 1a , R2 and R 2a is H, and R, R 3a , R4, and R 4a is independently selected from C1-C4 alkyl. In yet another aspect of this embodiment, R 1a , R2 and R 2a is H, and R, R 3a , R4, and R 4a In yet another aspect of this embodiment, R, R 1a , R2 and R 2a is H, and R, R 3a , R4, and R 4a is methyl.

[0038] In another aspect of the composition according to the invention, where component a) is an ABA type triblock copolymer, it is a triblock copolymer selected from the triblock copolymer of structure (ABA-1), the triblock copolymer of structure (ABA-2), and a mixture of these two block copolymers. In this embodiment, mt, mta, nt, and nta are the number of repeat units, R 1s , R 1sa , R 2s , and R 2sa are independently hydrogen, C1-C8 alkyl, -N(R 3s )2, -OR 4s , and Si(R 5s )3, where R 3s , R 4s and R 5s is independently selected from C1-C4 alkyl. In one more specific aspect of this embodiment, R1, R 1a , R2, R 2a and R 1s and R 2s is H, and R, R 3a , R4, and R 4a is independently selected from C1-C4 alkyl. In another more specific aspect of this embodiment, R1, R 1a , R2, R 2a and R 1s and R 2s is H, and R, R 3a , R4, and R 4a is methyl.

[0039] [ka] Component a) is a diblock copolymer.

[0040] In another aspect of the composition according to the invention described herein, component a) is a diblock copolymer or a blend of at least two diblock copolymers. In one aspect of this embodiment, it is selected from the group consisting of diblock copolymer a-1), diblock copolymer a-2), and blends of a-1) and a-2) as described below:

[0041] a-1) is a diblock copolymer of block A) containing repeating units having structure (I) and structure B) containing repeating units having structure (II), where R1 and R3 are independently selected from H and C1-C4 alkyl, R2 is H or C1-C8 alkyl, and R4 is C1-C8 alkyl. Further, the mole percent values ​​based on the total number of moles of repeating units of structures (I) and (II) are about 40 mole % to about 80 mole % for repeating units of structure (I) and about 20 mole % to about 60 mole % for repeating units of structure (II). Further, the individual values ​​of the mole percent of repeating units of structures (I) and (II) are selected from their respective ranges such that the total number of moles of repeating units of structures (I) and (II) add up to 100 mole percent, and the diblock copolymer a-1) has a polydispersity of about 1.0 to about 1.1 and a Mn of about 50,000 g / mol to about 150,000 g / mol. In one aspect of this embodiment, the moiety R2 is attached to the aromatic ring of the styrenic moiety through a para bond.

[0042] [ka] R a-2) is a diblock copolymer of a block Aa) containing a repeating unit having the structure (Ia) and a block Ba) containing a repeating unit having the structure (IIa). 1a and R 3a is independently selected from H or C1-C4 alkyl; R 2a is H or C1-C8 alkyl, C 4ais a C1-C8 alkyl. The mole percent values ​​based on the total number of moles of repeating units of structures (Ia) and (IIa) are about 40 mole % to about 80 mole % for repeating units of structure (Ia) and about 20 mole % to about 60 mole % for repeating units of structure (IIa). Furthermore, the individual mole percent values ​​of repeating units of structure (Ia) and structure (IIa) are selected from their respective ranges such that the total number of moles of repeating units of structure (Ia) and structure (IIa) sum to 100 mole %. Furthermore, the diblock copolymer a-2) has a polydispersity of about 1.0 to about 1.1 and an Mn of about 30,000 g / mol to about 90,000 g / mol. In one aspect of this embodiment, the moiety R 2a is attached to the aromatic ring of the styrenic moiety through a para bond. In one more specific aspect of these diblock copolymer embodiments, R, R 1a , R2 and R 2a is H, and R, R 3a , R4, and R 4a are independently selected from C1-C4 alkyl. In one more specific aspect of these embodiments, R1, R 1a , R2 and R 2a is H, and R, R 3a , R4, and R 4a is methyl.

[0043] [ka] In another aspect of the composition according to the invention, the diblock copolymer components a-1) and a-2) are 1a , R2 and R 2a is H, and R, R 3a , R4, and R 4a are independently selected from C1 to C4 alkyl. In one more specific aspect of this embodiment, R1, R 1a , R2 and R 2a is H, and R, R 3a , R4 and R 4a are independently methyl.

[0044] In the compositions according to the invention, in which component a) is the diblock copolymer components a-1) and a-2), in each case, a spacer moiety is present between the two blocks, which is a moiety derived from a 1,1-diphenylethylene derivative. In this embodiment, a-1) and a-2) have the structures (IS) and (ISa), respectively, in which R 1s , R 1sa , R 2s , and R 2sa are independently hydrogen, C1-C8 alkyl, -N(R 3s )2, -OR 4s , and Si(R 5s )3, where R 3s , R 4s and R 5s is independently selected from C1-C4 alkyl. In another aspect of this embodiment, R 1s , R 2s , R 1sa , and R 2sa is hydrogen. In the block A) and block Aa) (also called styrene-based block) of the polymer blocks in the structures (IS) and (ISa), these block chains are in the secondary position (in other words, R or R 1a = hydrogen) or tertiary position (in other words, R2 or R 2a = C1-C4 alkyl) to these spacer moieties. Correspondingly, block B) and block Ba) of the polymer blocks are terminally linked to spacer moieties (IS) and (ISa), respectively, via primary positions (in other words, CH2 moieties) on the "acrylic" repeat units at the ends of these blocks.

[0045] [ka] In each of the above aspects of the composition according to the invention, where component a) comprises a diblock copolymer component a-1), this component has a polydispersity of from about 1.00 to about 1.03.In another aspect of this embodiment, component a-1) has an Mn of from about 93,000 g / mol to about 105,300 g / mol.

[0046] In another aspect of the composition according to the present invention, in the diblock copolymer component a-1) as component a), the mole percentage of the repeating units of structure (I) is about 60 mole percent to about 80 mole percent, and the mole percentage of the repeating units of structure (II) is about 20 mole percent to about 40 mole percent.

[0047] In another aspect of the embodiment in which component a) is a diblock copolymer, the repeating units of Structure (I) are about 60 mol % to about 75 mol %, and the repeating units of Structure (II) are about 25 mol % to about 40 mol %. In one aspect of the composition according to the present invention, in the diblock copolymer component a-1) as component a), the mol % of Structure (I) is about 40 mol % to about 60 mol %, and the repeating units of Structure (II) are about 40 mol % to about 60 mol %.

[0048] In each of the above aspects of the composition according to the invention, this is such that, with respect to component a), the diblock copolymer component a-2) has a polydispersity of from about 1.00 to about 1.03.

[0049] In the above aspects of the composition according to the invention, in which the diblock copolymer as component a) comprises component a-2), this component in each case has an Mn of from about 40,800 g / mol to about 61,200 g / mol.

[0050] In any of the above aspects of the composition according to the invention, this means that with respect to component a), the total mole % values ​​are from about 40 mole % to about 60 mole % for repeat units of structures (I) and (Ia), and from about 40 mole % to about 60 mole % for repeat units of structures (II) and (IIa), either in the single block copolymer a-1) or a-2) or in a blend of a-1) and a-2).

[0051] In any of the above aspects of the composition according to the invention, this means that with respect to component a), the total mole % values ​​are from about 60 mole % to about 75 mole % for repeat units of structures (I) and (Ia), and from about 25 mole % to about 40 mole % for repeat units of structures (II) and (IIa), either in the single block copolymer a-1) or a-2) or in a blend of a-1) and a-2).

[0052] In one aspect of the composition according to the invention above, component a) may be a blend of a-1) and a-2).

[0053] In one aspect of the composition according to the invention above, component a) is either a-1) or a-2).

[0054] In one aspect of the composition according to the invention above, when component a) is either a diblock copolymer a-1), a diblock copolymer a-2), or a blend of a-1) and a-2), the total mole % (based on the total number of moles of all repeat units) of repeat units of structures (I) and (Ia) present in component a) is from about 45 mole % to about 75 mole %, and correspondingly, the sum of the mole % of repeat units of structures (II) and (IIa) is from about 25 mole % to about 55 mole %.

[0055] In any of the above aspects of the composition according to the invention, the weight percent of component a), whether component a) comprises diblock copolymer(s) or triblock copolymer(s), is from about 0.5 weight percent to about 2.00 weight percent of the total weight of the entire composition.

[0056] component b) In any of the above aspects of the composition according to the invention comprising the oligodiblock copolymer components b-2) and b-3), respectively, they may have a spacer moiety between block Ab) and block Bb) or between block Ac) and block Bc), respectively, as shown in Structure (ISb) and Structure (ISc), respectively, where R 1sb , R 1sc , R 2sb , and R 2sc are independently hydrogen, C1-C8 alkyl, -N(R 3s )2, -OR 4s , Si(R 5s )3, where R 3s , R 4s and R 5s is independently selected from C1-C4 alkyl. In another aspect of this embodiment, R 1sb , R 2sb , R 1sc , and R 2sc is hydrogen.

[0057] In the polymer blocks Ab) and Ac) (also called styrenic blocks) in structures (ISb) and (ISc), these block chains are terminally linked to their spacer moieties via secondary positions (also called when R5 or R7=hydrogen) or tertiary positions (also called when R5 or R7=C1-C4 alkyl). Correspondingly, the polymer blocks Bb) and Bc) are terminally linked to the spacer moieties (ISb) and (ISc), respectively, via primary positions (also called CH2 moieties) on the "acrylic" repeat units at the ends of these blocks.

[0058] [ka] In any of the above aspects of the composition according to the invention comprising the oligorandom copolymer b-1), this may be 1b and R2b is H, and R 3b and R 4b is methyl.

[0059] In any of the above aspects of the composition according to the invention comprising the oligorandom copolymer b-1), this has a polydispersity of from about 1.3 to about 1.5.

[0060] In any of the above aspects of the composition according to the invention, this is such that with respect to component b), the oligorandom copolymer b-1) has a Mn of from about 1000 g / mol to about 5000 g / mol.

[0061] In any of the above aspects of the composition according to the invention, this is such that, with respect to component b), the oligorandom copolymer b-1) has a polydispersity of from about 1.3 to about 1.6.

[0062] In any of the above aspects of the composition according to the invention, this is where component b) comprises an oligorandom copolymer b-1), which component has a Tg of from about 50°C to about 90°C.

[0063] In one aspect of the composition according to the invention described above, component b) is an oligorandom copolymer b-1).

[0064] In the above aspect of the composition according to the invention, component b) comprises an oligodiblock copolymer b-2), where R5, R7 and R8 are H, R6 is n-octyl or n-nonyl, R9 and R 11 is methyl, R 10 is methyl or ethyl, R 12 and R 13 is independently ethylene or propylene, and R 14 is methyl or ethyl. In another aspect of this embodiment, the oligodiblock copolymer b-2) has R6 being n-octyl and R 10 is methyl and R 12 and R 13 is ethylene and R14 is methyl.

[0065] In any of the above compositions according to the present invention in which component b) is an oligodiblock copolymer b-2), in one aspect, the sum of the mole percents of repeat units (III) and (IV) based on the total number of moles of repeat units having structures (III), (IV), (V) and (VI) is in the range of about 40 mole percent to about 80 mole percent, and the sum of the mole percents of repeat units (V) and (VI) is in the range of about 20 mole percent to about 60 mole percent, further wherein the mole percent of repeat unit (III) is in the range of about 2 mole percent to about 80 mole percent, and the mole percent of repeat unit (VI) is in the range of about 1 mole percent to about 80 mole percent. In another aspect of this embodiment, the mole percent of repeat unit (III) is in the range of about 2 mole percent to about 64 mole percent. In another aspect of this embodiment, the mole percent of (VI) is in the range of about 2 mole percent to about 48 mole percent.

[0066] In all embodiments described herein for oligodiblock copolymer b-2), the individual values ​​of the mole percent of repeat units of structures (III), (IV), (V) and (VI) are selected from their respective ranges such that the total number of moles of repeat units of structures (III), (IV), (V) and (VI) add up to 100 mole percent.

[0067] In another aspect of the composition according to the invention, the oligodiblock copolymer b-2) has said mole % of repeating units of structure (IV) from about 25 mole % to about 50 mole %, and said mole % of repeating units of structure (V) from about 40 mole % to about 60 mole %.

[0068] In another aspect of the composition according to the present invention, the oligodiblock copolymer b-2) has a molar percentage of repeating units of structure (III) that is about 20% to about 30% of the molar percentage of repeating units of structure (IV), and a molar percentage of repeating units of structure (VI) that is about 12% to about 20% of the molar percentage of repeating units of structure (V).

[0069] In another aspect of the composition according to the present invention, when component a) is either diblock copolymer a-1), diblock copolymer a-2), or a blend of a-1) and a-2), as described above, the mol% composition of block Ab) and block Bb) with respect to oligodiblock copolymer b-2) varies depending on the phase morphology window of the diblock copolymer component a) as a whole. Specifically, as an example, when the total mol% of repeating units of structures (III) and (IV) in block Ab) is selected from about 40 mol% to about 80 mol%, the specific total value selected in this range corresponds to the total mol% value of repeating units of structures (I) and (Ia) present in component a) when component a) is either diblock copolymer a-1), diblock copolymer a-2), or a blend of a-1) and a-2). Correspondingly, in block Bb), when the sum of the mole percent of repeat units of structures (V) and (VI) is from about 25 mole percent to about 55 mole percent, the specific total value selected in this range corresponds to the total mole percent value of repeat units of structures (II) and (IIa) present in component a), when component a) is either a diblock copolymer a-1), a diblock copolymer a-2), or a blend of a-1) and a-2).

[0070] In the above aspect of the composition according to the invention, component b) comprises an oligodiblock copolymer b-2), which has a polydispersity of from about 1.03 to about 1.08.

[0071] In the above aspect of the composition according to the invention, component b) comprises an oligodiblock copolymer b-2), which has an Mn of about 15000 g / mol to about 32000 g / mol, for example about 15000 g / mol to about 30000 g / mol.

[0072] In the above aspect of the composition according to the invention, component b) comprises an oligodiblock copolymer b-2), which has a Tg of about 50°C to about 90°C.

[0073] In one aspect of the composition according to the invention described above, component b) is an oligodiblock copolymer b-2).

[0074] Any one of the compositions according to the invention, in which component b) comprises an oligodiblock copolymer b-3), is 1c and R 2c is H and R 3c and R 4c is independently selected from C1-C4 alkyl. In another aspect of this embodiment, R 1c and R 2c is H, and R 3c and R 4c is methyl.

[0075] In the above aspect of the composition according to the invention, component b) comprises an oligodiblock copolymer b-3), which has a Mn of from about 15,000 to about 30,000 g / mol.

[0076] In the above aspect of the composition according to the invention, component b) comprises an oligodiblock copolymer b-3), which has a polydispersity of from about 1.02 to about 1.08.

[0077] In the above aspect of the composition according to the invention, where component b) comprises an oligodiblock copolymer b-3), this is such that said mol % of repeating units of structure (Ic) is from about 40 mol % to about 70 mol %, and said mol % of repeating units of structure (IIc) is from about 40 mol % to about 70 mol %.

[0078] In the above aspect of the composition according to the invention, component b) comprises an oligodiblock copolymer b-3), which has a Tg of about 50°C to about 90°C.

[0079] In one embodiment of the composition according to the invention described above, component b) is a diblock copolymer b-3).

[0080] In one embodiment of the composition according to the present invention that may be suitable for L / S applications, in the diblock copolymer component a-1), the molar percentage value of the repeating units of structure (I) is about 40 mol % to about 60 mol %, and the molar percentage value of the repeating units of structure (II) is about 40 mol % to about 60 mol %.

[0081] In one embodiment of the composition according to the present invention that may be suitable for CH applications, in the diblock copolymer component a-1), the molar percentage value of the repeating unit of structure (I) is about 60 mol % to about 75 mol %, and the repeating unit of structure (II) is about 25 mol % to about 40 mol %.

[0082] In any of the above embodiments of component b), this component may be about 0.05% to about 0.5% by weight of the total weight of the composition, including the spin-casting solvent. In another aspect of this embodiment, this is about 0.08% to about 0.4% by weight. In another aspect of this embodiment, this is about 1% to about 0.4% by weight. In another aspect of this embodiment, this is about 0.15% to about 0.4% by weight. In yet another aspect of this embodiment, this is about 0.2% to about 0.3% by weight. In yet another aspect of this embodiment, component b) is b-1). In another aspect of this embodiment, component b) is b-2). In yet another aspect of this embodiment, component b) is b-3). In yet another aspect of this embodiment, component b) is a mixture of at least two components b) selected from the group consisting of b-1), b-2), and b-3).

[0083] Ingredient c) For the spin-casting organic solvent of component c), suitable solvents for dissolving the compositions according to the invention described above include glycol ether derivatives such as ethyl cellosolve, methyl cellosolve, propylene glycol monomethyl ether (PGME), diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, dipropylene glycol dimethyl ether, propylene glycol n-propyl ether, or diethylene glycol dimethyl ether; glycol ether ester derivatives such as ethyl cellosolve acetate, methyl cellosolve acetate, or propylene glycol monomethyl ether acetate (PGMEA); carboxylates such as ethyl acetate, n-butyl acetate, and amyl acetate; carboxylates of dibasic acids such as diethyl oxylate and dimethyl malonate; dicarboxylates of glycols such as ethylene glycol diacetate and propylene glycol diacetate. and hydroxycarboxylates such as methyl lactate, ethyl lactate (EL), ethyl glycolate, and ethyl 3-hydroxypropionate; ketone esters such as methyl pyruvate or ethyl pyruvate; alkoxycarboxylates such as methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, ethyl 2-hydroxy-2-methylpropionate, or methyl ethoxypropionate; ketone derivatives such as methyl ethyl ketone, acetylacetone, cyclopentanone, cyclohexanone, or 2-heptanone; ketone ether derivatives such as diacetone alcohol methyl ether; ketone alcohol derivatives such as acetol or diacetone alcohol; ketals or acetals such as 1,3 dioxalane and diethoxypropane; lactones such as butyrolactone; amide derivatives such as dimethylacetamide or dimethylformamide, anisole, and mixtures thereof.

[0084] Additionally, the compositions according to the present invention may further comprise additives selected from the group consisting of surfactants, inorganic-containing polymers; additives including small molecules, inorganic-containing molecules, surfactants, photoacid generators, thermal acid generators, quenchers, curing agents, crosslinkers, chain extenders, and the like; and combinations comprising at least one of the foregoing, wherein one or more of the additional components and / or additives assemble with the block copolymer to form a block copolymer assembly.

[0085] Methods of the Invention The compositions according to the invention described herein may be used to generate arrays of features in unguided self-assembly processes or may be used in guided (alternatively guided) self-assembly processes, such as graphoepitaxy or chemoepitaxy, to effect either pattern tuning or pattern multiplication of chemoepitaxy or graphoepitaxy guided features.

[0086] After self-assembly, these patterns can be transferred into the underlying substrate by using plasma. In general, anisotropic etching using oxygen-containing plasmas, such as those used to etch resists (e.g., JBKruger, et al, "VLSI Electronics, Microstructure Science" Chapter 5, Academic Press, p.91-136, 1984 (Non-Patent Document 5)), is most commonly used as a mask for etching semiconductor substrates using self-assembled films of block copolymers of methyl methacrylate and polystyrene (e.g., "Etch considerations for directed self-assembly patterning using capacitively coupled plasma" Vinayak Rastogi et al, Journal of Vacuum Science & Technology A36, 031301, 2018 (Non-Patent Document 6)). Because the novel compositions described herein contain such block copolymers, these general types of conditions can be used to transfer patterns of self-assembled films of the compositions according to the invention into substrates.

[0087] One aspect of the invention comprises the steps of: i) forming a coating of a neutral layer on a substrate; ii) coating any of the compositions according to the present invention onto the neutral layer to form a film; ii) baking the film in an inert gas atmosphere at a temperature selected from about 240° C. to about 260° C. to form a self-assembled film; and iii) etching the substrate with a plasma to pattern-transfer the self-assembled monolayer into the substrate; Includes.

[0088] Another aspect of the present invention is a method for forming a line and space array, comprising the steps of: ia) forming a coating of a neutral layer on a substrate; iia) coating said composition according to the invention suitable for L / S application onto said neutral layer to form a membrane; iiia) baking the film in an inert gas atmosphere at a temperature selected from about 240° C. to about 260° C. to form a self-assembled film; and iva) etching the substrate with a plasma to pattern the self-assembled monolayer into the substrate to form an L / S array; Includes.

[0089] Another aspect of the present invention is a method of forming a line and space (L / S) pattern via a grapho-epitaxy process, comprising: ia') forming a coating of a neutral layer on a substrate; iia') coating a photoresist on top of the neutral layer coating to form a photoresist film; iiia') patterning the photoresist to produce an L / S patterned photoresist; iva') coating said composition according to the invention suitable for L / S application onto said patterned photoresist to form a film in which the L / S pattern is filled with said composition according to the invention suitable for L / S application and is flush with the surface of the photoresist; (va') baking the film in an inert gas atmosphere at a temperature selected from about 240°C to about 260°C to form a self-assembled film; and via') etching the substrate with plasma to transfer the self-assembled monolayer into the substrate to form an L / S pattern; The method comprises:

[0090] Another aspect of the present invention is a method for forming a line and space (L / S) pattern via a chemo-epitaxy process, comprising: ia'') forming a coating of a neutral layer on a substrate; iia'') coating a photoresist on top of the neutral layer coating to form a photoresist film; iiia'') patterning the photoresist to generate an L / S patterned photoresist film; iva'') etching the underlying neutral layer using the patterned photoresist film as a mask; (va'') stripping the resist to form a patterned neutral layer that is a chemo-epitaxy pattern without significant topography; via'') coating said composition according to the present invention suitable for L / S application onto said patterned neutral layer to form a block copolymer film; viia') baking the block copolymer film in an inert gas atmosphere at a temperature selected from about 240°C to about 260°C to form a self-assembled film; and viiia'') etching the substrate with plasma to transfer the self-assembled monolayer into the substrate to form an L / S pattern; The method comprises:

[0091] Another aspect of the present invention is a method for forming a contact hole (CH) array, comprising the steps of: ib) forming a coating of a neutral layer on a substrate; iib) coating said composition suitable for CH application onto said neutral layer to form a membrane; iiib) baking the film in an inert gas atmosphere at a temperature selected from about 240° C. to about 260° C. to form a self-assembled film; and ivb) etching the substrate with a plasma to pattern the self-assembled monolayer into the substrate to form a CH array; The method comprises:

[0092] Another aspect of the present invention is a method for forming a contact hole (CH) pattern via a grapho-epitaxy process, comprising: ib') forming a coating of a neutral layer on a substrate; iib') coating a photoresist on top of the neutral layer coating to form a photoresist film; iiib') patterning the photoresist to produce a CH patterned photoresist; ivb') coating said composition according to the invention suitable for CH application onto said patterned photoresist to produce a film in which the L / S pattern is filled with said composition according to the invention suitable for L / S application and is flush with the surface of the photoresist; vib') baking the film in an inert gas atmosphere at a temperature selected from about 240°C to about 260°C to form a self-assembled film; and viib') etching the substrate with plasma to transfer the self-assembled monolayer into the substrate to form a CH pattern; The method comprises:

[0093] Another aspect of the invention is a method of forming lines and spaces via a chemo-epitaxy process comprising: ib'') forming a coating of a neutral layer on a substrate; iib'') coating a photoresist on top of the neutral layer coating to form a photoresist film; iiib'') patterning the photoresist to produce a CH patterned photoresist; ivb'') Etching the underlying neutral layer using the patterned photoresist as a mask; vb'') stripping the resist to form a patterned neutral layer that is a chemo-epitaxy pattern without significant topography; vib'') coating said composition according to the invention suitable for CH applications onto said patterned neutral layer to form a block copolymer film; viib'') baking the block copolymer film in an inert gas atmosphere at a temperature selected from about 240°C to about 260°C to form a self-assembled film; and viiib″) etching the substrate with plasma to transfer the self-assembled monolayer into the substrate to form a CH pattern; The method comprises:

[0094] In the method according to the invention, when the composition according to the invention is coated on a substrate to form a coating, it may be optionally heated in an additional step prior to the heating step to produce the self-assembled monolayer in order to remove the spin-casting solvent in a separate separate step. For this additional step, the film may be heated at a temperature in the range of about 100°C to about 150°C or at a temperature in the range of about 120°C to about 150°C.

[0095] Typical film thicknesses after heating range from about 25 nm to about 70 nm, or from about 40 nm to about 60 nm, or from about 45 nm to about 55 nm, or from about 45 nm to about 52 nm.

[0096] It is also expected that the novel compositions suitable for CH or L / S can be used in other chemo-epitaxy and grapho-epitaxy processes or in hybrid processes combining the two. For example, in chemo-epitaxy, the guide pinning feature can alternatively be a separate patterned organic pinning layer instead of just a region of the uncovered bare semiconductor substrate. For example, the patterned pinning layer can cover the neutral layer or can be underneath the patterned pinning layer.

[0097] The composition according to the present invention that may be used to form contact hole arrays includes a diblock copolymer component a) selected from the group consisting of diblock copolymer a-1), diblock copolymer a-2), and blends of a-1) and a-2), where the total mole percent of styrenic repeat units of structures (I) and (Ia) is about 60 mole percent to about 75 mole percent, and the total mole percent of acrylic repeat units of structures (II) and (IIa) is about 40 mole percent to about 60 mole percent, and where component b) may be selected from copolymer b-1), copolymer b-2), such as oligodiblock copolymer b-2), or copolymer b-3), and mixtures thereof. In one aspect of this embodiment, component b) is exclusively oligorandom copolymer b-1), in another it is exclusively copolymer b-2), and in yet another it is exclusively copolymer b-3).

[0098] The compositions according to the present invention that may be used for the formation of line and space (L / S) arrays are those in which component a) is a diblock copolymer component selected from the group consisting of diblock copolymer a-1), diblock copolymer a-2) and blends of a-1) and a-2), wherein the total mole % of the styrenic repeat units of structures (I) and (Ia) is from about 60 mole % to about 75 mole %, and further, the total mole % of the acrylic repeat units of structures (II) and (IIa) is from about 25 mole % to about 40 mole %, and component b) is a copolymer b-1), such as an oligorandom copolymer b-1), a copolymer b-2), such as an oligodiblock copolymer b-2), or a copolymer b-3), such as an oligodiblock copolymer b-3). In one aspect of this embodiment, component b) is exclusively oligorandom copolymer b-1), in another it is exclusively copolymer b-2), and in yet another it is exclusively copolymer b-3).

[0099] Compositions according to the invention that may be used for the formation of line and space (L / S) arrays are those in which component a) is selected from the group consisting of triblock copolymer components a-1t), triblock copolymers a-2t), and blends of a-1t) and a-2t), wherein the total mole percent of the styrenic repeat units of structures (I) and (Ia) is from about 60 mole percent to about 75 mole percent, and the total mole percent of the acrylic repeat units of structures (II) and (IIa) is from about 40 mole percent to about 60 mole percent, and component b) is a copolymer b-2) or a copolymer b-3), such as an oligodiblock copolymer b-3). In one aspect of this embodiment, component b) is only copolymer b-2), and in yet another it is only copolymer b-3).

[0100] The composition according to the present invention that may be used for the formation of contact hole arrays is one in which component a) is selected from the group consisting of triblock copolymer component a-1t), triblock copolymer a-2t), and blends of a-1t) and a-2t), wherein the total mole percent of styrenic repeat units of structures (I) and (Ia) is about 60 mole percent to about 75 mole percent, and further, the total mole percent of acrylic repeat units of structures (II) and (IIa) is about 25 mole percent to about 40 mole percent, and component b) is a copolymer b-2), such as an oligodiblock copolymer b-2), or a copolymer b-3), such as an oligodiblock copolymer b-3). In one aspect of this embodiment, component b) is only copolymer b-2), and in yet another it is only copolymer b-3).

[0101] Another aspect of the present invention is a method for forming a contact hole array, comprising the steps of: i) forming a coating of a neutral layer on a substrate; ii) coating a composition comprising said diblock copolymer suitable for forming a contact hole array onto said neutral layer to form a film; ii) baking the film in an inert gas atmosphere at a temperature selected from about 240° C. to about 260° C. to form a self-assembled film; and iii) etching the substrate with a plasma to pattern-transfer the self-assembled monolayer into the substrate; The method includes:

[0102] In one aspect of this embodiment, component b) is an oligorandom copolymer b-1), in another aspect, component b) is a copolymer b-2), and in yet another, component b) is a copolymer b-3).

[0103] Another aspect of the present invention is a method for forming an L / S array, comprising the steps of: ib) forming a coating of a neutral layer on a substrate; iiib) coating a composition comprising said diblock copolymer suitable for forming an L / S array onto said neutral layer to form a film; ivb) baking the film in an inert gas atmosphere at a temperature selected from about 240° C. to about 260° C. to form a self-assembled film; and vb) etching the substrate with a plasma to pattern the self-assembled monolayer into the substrate; The method includes:

[0104] In one aspect of this embodiment, component b) is an oligorandom copolymer b-1), in another aspect, component b) is a copolymer b-2), and in yet another, component b) is a copolymer b-3).

[0105] 1. A method for forming a line and space array comprising: ic) forming a coating of a neutral layer on the substrate; iiic) coating a composition comprising said triblock copolymer suitable for forming an L / S array onto said neutral layer to form a film; ivc) baking the film in an inert gas atmosphere at a temperature selected from about 240° C. to about 260° C. to form a self-assembled film; and vc) etching the substrate with a plasma to transfer the self-assembled monolayer into the substrate in a pattern; The method includes:

[0106] 1. A method of forming a contact hole array, comprising: ic) forming a coating of a neutral layer on the substrate; iiid) coating a composition comprising said triblock copolymer suitable for forming a contact hole array onto said neutral layer to form a film; ivd) baking the film in an inert gas atmosphere at a temperature selected from about 240° C. to about 260° C. to form a self-assembled film; and vd) etching the substrate with a plasma to pattern the self-assembled monolayer into the substrate; The method includes:

[0107] Oligodiblock copolymer according to the present invention Another aspect of the invention is a diblock copolymer according to the invention comprising a block Ab) and a block Bb) having a Mn of about 1,000 to 35,000 g / mol and a polydispersity of 1.0 to about 1.1. In this material according to the invention, block Ab) is a random copolymer of repeating units having structures (III) and (IV), and block Bb) is a random copolymer of repeating units having structures (V) and (VI). Furthermore, in this novel oligodiblock copolymer, R5, R7, R9 and R 11 are independently selected from H or C1-C4 alkyl, R6 is a C7-C10 straight chain alkyl, R8 is a C1-C4 alkyl, and R 10 is C1-C4 alkyl, R 12 and R 13 is independently selected from C2-C5 alkylene, and R 14 is C1-C4 alkyl; R5, R7, R9, and R 11 are independently selected from H or C1-C4 alkyl, R6 is a C7-C10 straight chain alkyl, R8 is a C1-C4 alkyl, and R 10is C1-C4 alkyl, R 12 and R 13 is independently selected from C2-C5 alkylene, and R 14 is a C1-C4 alkyl, and further, the oligodiblock copolymer according to the present invention has a Tg having a value of from about 0°C to about 95°C.

[0108] [ka] In one aspect of the oligodiblock copolymer according to the present invention, the mole percentages based on the total number of moles of repeat units of structures (III), (IV), (V) and (VI) are as follows: In the repeating unit of structure (IV), the mole percentage is about 10 mole percent to about 50 mole percent. In the repeating unit of structure (V), the mole percentage is about 20 mole percent to about 60 mole percent. The mole % of the repeating unit of structure (III) is about 10% to about 0% of the mole % of the repeating unit of structure (IV); For repeat units of Structure (VI), the mole % is from about 10% to about 40% of the mole % of repeat units of Structure (V), and the individual values ​​of the mole % of repeat units of Structures (III), (IV), (V) and (VI) are selected from their respective ranges such that the total number of moles of repeat units of Structures (III), (IV), (V) and (VI) add up to 100 mole %.

[0109] In another aspect of the oligodiblock copolymer according to the present invention, as shown in structure (ISb), it has a spacer moiety between block Ab) and block Bb), where R 1sb and R 2sb are independently hydrogen, C1-C8 alkyl, -N(R 3s )2, -OR 4s , Si(R 5s ) 3, where R 3s , R 4s and R 5s is independently selected from C1-C4 alkyl. In another aspect of this embodiment, R1sb and R 2sb is hydrogen.

[0110] [ka] In another aspect of the oligodiblock copolymer according to the present invention, R5, R7 and R8 are H, R6 is a C8-C9 linear alkyl, and R9 and R 11 is methyl and R 10 is methyl or ethyl, and R 12 and R 13 is independently ethylene or propylene, and R 14 In another aspect of this embodiment, R6 is n-octyl and R 10 is methyl and R 12 and R 13 is ethylene, and R 14 is methyl.

[0111] In another aspect of the above oligodiblock copolymer according to the present invention, it has a Mn of about 15,000 to about 25,000 g / mol.

[0112] In another aspect of the oligodiblock copolymer according to the present invention, the mol % of the repeating unit of structure (IV) is about 25 mol % to about 50 mol %, and the mol % of the repeating unit of structure (V) is about 40 mol % to about 60 mol %.

[0113] In another aspect of the oligodiblock copolymer according to the present invention described above, the sum of the mole percent of repeat units (III) and (IV) is in the range of about 40 mole percent to about 80 mole percent, and the sum of the mole percent of repeat units (V) and (VI) is in the range of about 20 mole percent to about 60 mole percent, based on the total number of moles of repeat units having structures (III), (IV), (V) and (VI), further wherein the mole percent of repeat unit (III) is in the range of about 2 mole percent to about 80 mole percent, and the mole percent of repeat unit (VI) is in the range of about 1 mole percent to about 80 mole percent, and further wherein the individual values ​​of the mole percent of repeat units of structures (III), (IV), (V) and (VI) are selected from their respective ranges such that the total number of moles of repeat units of structures (III), (IV), (V) and (VI) sum to 100 mole percent.

[0114] In another aspect of the above oligodiblock copolymer according to the present invention, the mole percentage of repeating unit (III) is from about 2 mole percent to about 64 mole percent.

[0115] In another aspect of the above oligodiblock copolymer according to the present invention, the mole percent of (VI) is from about 2 mole percent to about 48 mole percent.

[0116] In another aspect of the oligodiblock copolymer according to the present invention, the mole % of repeating units of structure (III) is about 20% to about 30% of the mole % of repeating units of structure (IV), and the mole % of repeating units of structure (VI) is about 12% to about 20% of the mole % of repeating units of structure (V).

[0117] In all embodiments described herein for the novel oligodiblock copolymers, the individual values ​​of the mole percent of repeat units of Structures (III), (IV), (V), and (VI) are selected from their respective ranges described herein such that the total number of moles of repeat units of Structures (III), (IV), (V), and (VI) add up to 100 mole percent.

[0118] In another aspect of the above oligodiblock copolymer according to the present invention, the oligodiblock copolymer has a polydispersity of about 1.03 to about 1.08.

[0119] In another aspect of the oligodiblock copolymer according to the present invention, the oligodiblock copolymer has an Mn of about 15,000 g / mol to about 32,000 g / mol.

[0120] In another aspect of the oligodiblock copolymer according to the present invention, the oligodiblock copolymer has a Tg of about 50°C to about 90°C.

[0121] A further aspect of the invention is the use of the composition according to the invention or the oligodiblock copolymer according to the invention for preparing a self-assembled film on a substrate. EXAMPLES

[0122] chemicals Unless otherwise indicated, all chemicals were purchased from Sigma Aldrich (3050 Spruce St., St. Louis, MO 63103). Chemicals used in anionic polymerization were purified as described in the literature (e.g., David Uhrig and Jimmy Mays, "Techniques in High-Vacuum Anionic Polymerization", Journal of Polymer Science: Part A: Polymer Chemistry, Vol. 43, 6179-6222 (2005)).

[0123] All synthesis experiments were carried out in a N2 atmosphere. Lithography experiments were carried out as described herein. The molecular weight of the copolymer was measured using gel permeation chromatography. 3 Å, 10 5 Å and 10 6Gel permeation chromatography equipped with an Åμ-ultrastyragel column.

[0124] Lithography experiments were performed using a TEL Clean ACT8 track. SEM images were taken using an Applied Materials NanoSEM 3D. Scanning electron micrographs are shown at either 1 FOV magnification or 2 FOV magnification (field of view (FOV) = 5 μm or ).

[0125] Etching experiments were performed using standard isotropic oxygen etching conditions for self-assembled film block copolymers of methyl methacrylate and styrene.

[0126] Unless otherwise stated, molecular weight measurements (also known as Mn polydispersity) are performed at 100 Å, 500 Å, 10 3 Å, 10 5 Å and 10 6 The analysis was carried out by gel permeation chromatography using an Åμ-Ultrastyragel column (PSS Inc., Germany) with THF solvent as the eluent. Polystyrene polymer standards were used for calibration.

[0127] DSC measurements of glass transition temperature were performed using a TA Instruments DSC Q1000 under nitrogen with a heating rate of 10° C. / min. The glass transition temperature (Tg) was measured in the first heating scan from 0 to 300° C. The midpoint of the endothermic transition was considered.

[0128] 1 1 H NMR was recorded using a Bruker Advanced III 400 MHz spectrometer.

[0129] Synthesis Example 1: Synthesis of PS-co-PMMA neutral layer material A 250 ml flask equipped with a temperature controller, heating jacket and magnetic stirrer was set up. 26.04 grams (0.25 moles) of styrene, 24.03 grams (0.24 moles) of methyl methacrylate, 1.42 grams (0.10 moles) of glycidyl methacrylate, 0.41 grams (0.0025 moles) of azobisisobutyronitrile (AIBN) initiator and 100 grams of anisole were added to the flask. The stirrer was turned on and set to about 400 rpm. The reaction solution was then degassed by vigorously bubbling nitrogen through the solution at room temperature for about 30 minutes. After the 30 minutes of degassing, the heating jacket was turned on and the temperature controller was set to 70° C. and the stirred reaction mixture was maintained at this temperature for 20 hours. After this time, the heating mantle was turned off and the reaction solution was allowed to cool to about 40° C. The reaction mixture was then poured into 1.5 L of isopropanol with mechanical stirring during the addition. During the addition, polymer precipitated. The precipitated polymer was collected by filtration. The collected polymer was dried in a vacuum oven at 40° C. About 36 grams of polymer was obtained. The dried polymer was dissolved in 300 grams of THF and then filtered through a 0.2 μm nylon filter. The filtered solution was then precipitated again in a stirred solution of 1.5 L of methanol, the precipitated polymer was collected and dried under vacuum at 40° C. as before. In this way, 26 grams (50% yield) of polymer was obtained after drying. The polymer had a Mw of about 36k and a polydispersity (PDI) of 1.5.

[0130] Synthesis Example 2: Synthesis of P(Sb-MMA)(78K-b-39K) Styrene and methyl methacrylate monomers were distilled into a calibrated ampoule in the presence of a dehydrating agent and stored under N2. The liquid was transferred into the reactor under N2 via the ampoule or using a stainless steel cannula. 700 mL of anhydrous tetrahydrofuran was added into a dry 1 L round-bottom reactor equipped with a side arm for connecting the ampoule, a magnetic stir bar, and a nitrogen / vacuum three-way septum adapter. The temperature of the reactor was lowered to -78°C using a dry ice-acetone bath. Then, after titrating the impurities, 0.2 mL (1.4 M solution) of sec-butyl lithium was added into the reactor. Then, 20 g (0.192 moles) of styrene was added into the reactor from the ampoule with rapid stirring. The reaction solution changed its color to yellow-orange, and the reaction was stirred for 30 minutes. Then, 0.06 g (0.0003 mol) of 1,1'-diphenylethylene (DPE) in 2.5 ml of anhydrous toluene was added to the reactor via the ampoule. The orange color of the reaction mixture changed to a dark brick red color, suggesting that the styryllithium active centers were converted to delocalized DPE-adducted carbanions. After 2 min of stirring, a small amount (2 mL) of the reaction mixture was taken for PS block molecular weight analysis. Methyl methacrylate (9.98 g, 0.0998 mol) was then added via the ampoule. The reaction was quenched after 30 min with 1 mL of degassed methanol. The block copolymer was recovered by precipitation into excess isopropanol (5 times the volume of the polymer solution) containing 10% water, filtered, and dried under vacuum at 55° C. for 12 h to give 28 g of P(Sb-MMA) (94% yield) consisting of 66 mol % polystyrene blocks and 34 mol % polymethyl methacrylate blocks.

[0131] 100Å, 500Å, 10 3 Å, 10 5 Å and 10 6 Gel permeation chromatography using an Åμ-Ultrastyragel column showed that the first P(SDPE) block had an Mn(GPC) of 64,622 g / mol and an Mw / Mn of 1.02 relative to a PS calibration standard. The diblock copolymer molecular weight obtained from GPC was Mn,PS-b-PMMA = 107,150 g / mol and Mw / Mn = 1.01.

[0132] Synthesis Example 3: Synthesis of P(Sb-MMA)(34K-17K) PS-PMMA(34-17K) was synthesized using the same procedure as described in Example 2. To achieve the desired Mn of the PS and PMMA blocks, 0.42 mL of a 1.4 M solution of sec-butyllithium was added while keeping the amounts of styrene and MMA the same as in Example 2.

[0133] 100Å, 500Å, 10 3 Å, 10 5 Å and 10 6 Gel permeation chromatography with an Åμ-Ultrastyragel column showed that the first P(SDPE) block had a Mn(GPC) of 34,872 g / mol and a Mw / Mn of 1.03 relative to a PS calibration standard. The diblock copolymer molecular weight obtained from GPC was M n,PS-b-PMMA = 49,240 g / mol and Mw / Mn = 1.02. 1 1 H NMR showed 66.1 mol % polystyrene blocks and 33.9 mol % polymethyl methacrylate blocks.

[0134] Synthesis Example 4 Synthesis of P(Sb-MMA)(45k-b-51k) P(Sb-MMA) (45K-b-51K) was synthesized using the same procedure described in Example 2. The amount of initiator and monomer were varied to achieve the desired Mn and composition of the PS and PMMA blocks. Briefly, 20 g (0.192 mol) of styrene was polymerized with 0.32 mL (1.4 M solution) of sec-butyllithium. Then, 0.095 g (0.0005 mol) of 1,1'-diphenylethylene (DPE) in 2.5 ml of anhydrous toluene was added into the reactor via an ampoule. The orange color of the reaction mixture changed to a dark brick red color, suggesting that the styryllithium active center was converted to a delocalized DPE-adducted carbanion. After stirring for 2 min, a small amount (2 mL) of the reaction mixture was taken for PS block molecular weight analysis. Then, methyl methacrylate (22.85 g, 0.23 mol) was added via an ampoule. The reaction was quenched after 30 min with 1 mL of degassed methanol, and the block copolymer was recovered by precipitation into excess isopropanol (5 times the polymer solution) containing 10% water, filtered, and dried under vacuum at 55° C. for 12 h to give 40 g of P(Sb-MMA) (94% yield) consisting of 46.9 mol % polystyrene blocks and 53.1 mol % polymethyl methacrylate blocks.

[0135] 100Å, 500Å, 10 3 Å, 10 5 Å and 10 6 Gel permeation chromatography with an Åμ-Ultrastyragel column showed that the first P(SDPE) block had a Mn(GPC) of 45,048 g / mol and a Mw / Mn of 1.04 relative to a PS calibration standard. The diblock copolymer molecular weight obtained from GPC was M n,PS-b-PMMA = 88,348 g / mol and Mw / Mn = 1.02.

[0136] Synthesis Example 4a: Synthesis of triblock copolymer MMA-S-MMA, 50k-88k-50k The triblock polymer MMA-S-MMA was prepared as a THF solution using the procedures described in the literature (Mammol. Chem. 191, 2309-2318 (1990) (Non-Patent Document 8) and Adv. Polym. Sci. 86, 147 (1988) (Non-Patent Document 9)) utilizing potassium naphthalene as initiator. To avoid the attack of the ester group of MMA by PS carbanion, 1,1-diphenylethylene (DPE) was introduced to reduce the nucleophilicity of the active site. The presence of a single DPE in the copolymer between the two blocks does not affect its properties at all. In order to carry out the polymerization of MMA under good conditions at low temperature (-70°C). The polymer prepared in this manner had Mw of PMMA(50A)-PS(88K)-PMMA(50K) with a polydispersity of 1.04 as measured by gel permeation chromatography GPC.

[0137] Synthesis Example 5: Synthesis of Statistical Copolymer of Styrene and Methyl Methacrylate (P(S-co-MMA)) Oligomers for Contact Hole Assembly Additives The reaction was carried out under nitrogen in a 250 ml flask equipped with a condenser, nitrogen inlet and magnetic stir bar. 18.23 grams (0.17 moles) of styrene, 7.5 grams (0.075 moles) of methyl methacrylate, 2 grams (0.012 moles, 5% based on total monomers) of azobisisobutyronitrile (AIBN) initiator, 0.7 grams (0.0075 moles) of 1-butanethiol, and 50 grams of anisole were charged to the flask. The reaction was then degassed three times by vacuum / nitrogen cycles using the freeze-drying method and finally backfilled with nitrogen. The reaction was then maintained at 85° C. under stirring in an oil batch for 15 hours. After this time, the reaction was allowed to cool to about 25° C. The reaction mixture was then diluted with 100 mL of tetrahydrofuran and slowly poured into 700 mL of isopropanol that was stirred with mechanical stirring during the addition. The precipitated polymer was collected by filtration. The collected polymer was dried in a vacuum oven at 40° C. The yield was 45% and the copolymer had a M n,GPC= 4,700 g / mol, M w,GPC = 6,500 g / mol and a polydispersity index (PDI) of 1.38. The copolymer had a Tg = 86 °C, and 1 1 H NMR confirmed that the copolymer had 63 mol % and 37 mol % polystyrene and polymethyl methacrylate, respectively.

[0138] Synthesis Example 6: Synthesis of Statistical Copolymer of Styrene and Methyl Methacrylate (P(S-co-MMA)) Oligomers for Line-and-Space Assembly Additives The reaction was carried out under nitrogen in a 250 ml flask equipped with a condenser, nitrogen inlet and magnetic stir bar. 13 grams (0.12 moles) of styrene, 13.7 grams (0.14 moles) of methyl methacrylate, 2 grams (0.012 moles, 5% based on total monomers) of azobisisobutyronitrile (AIBN) initiator, 0.7 grams (0.0075 moles) of 1-butanethiol, and 50 grams of anisole were charged to the flask. The reaction was then degassed three times by vacuum / nitrogen cycles using the freeze-drying method and finally backfilled with nitrogen. The reaction was then maintained at 85° C. under stirring in an oil batch for 15 hours. After this time, the reaction was allowed to cool to about 25° C. The reaction mixture was then diluted with 100 mL of tetrahydrofuran and slowly poured into 700 mL of isopropanol that was stirred with mechanical stirring during the addition. The precipitated polymer was collected by filtration. The collected polymer was dried in a vacuum oven at 40° C. The yield was 45% and the copolymer had a M n,GPC = 2,300 g / mol, M w,GPC = 4,300 g / mol and a polydispersity index (PDI) of 1.82. The copolymer had a Tg = 53°C, and 1 1 H NMR confirmed that the copolymer had 42 mol % and 58 mol % polystyrene and polymethyl methacrylate, respectively.

[0139] Comparative Synthesis Example 1: Synthesis of a high molecular weight statistical copolymer of styrene and methyl methacrylate (P(S-co-MMA)) for line-and-space assembly additive Following a procedure similar to that described in Synthesis Example 5, a high molecular weight copolymer of 11,529 Mn and 19,600 K (PDI-1.7) was also prepared for comparison purposes in the absence of 1-butanethiol, which had 45 mol % and 55 mol % polystyrene and polymethyl methacrylate, respectively, in the copolymer and exhibited a Tg of 108° C.

[0140] Synthesis Example 7: Synthesis of Oligoblock Copolymer of Styrene and Methyl Methacrylate for L / S Assembly Additive The required monomers were distilled into calibrated ampoules in the presence of a dehydrating agent and stored under N2. The liquids were transferred into the reactor under N2 via ampoules or using stainless steel cannulas. 400 mL of anhydrous tetrahydrofuran was added into a dry 1 L round bottom reactor equipped with a side arm for connecting the ampoules, a magnetic stir bar, and a nitrogen / vacuum three-way septum adapter. The temperature of the reactor was lowered to -78°C using a dry ice-acetone bath. 1.4 mL (0.00189 moles) of sec-butyllithium was then added into the reactor after titrating the impurities. Styrene (18.8 g) was then added into the reactor from the ampoule with rapid stirring. The reaction solution turned orange and the reaction was stirred for 10 minutes. 0.4 g of 1,1'-diphenylethylene (DPE) in 3 ml of anhydrous toluene was then added into the reactor via the ampoule. The orange color of the reaction mixture changed to a dark brick red color. This suggests that the styryllithium active center was converted to a delocalized DPE-adducted carbanion. After 2 min of stirring, a small amount (2 mL) of the reaction mixture was taken for PS block molecular weight analysis. Then, 19.4 grams of methyl methacrylate (MMA) distilled in the presence of a small amount of triethylaluminum (1M in toluene) was added via ampoule. The reaction was stopped after 15 min with 1 mL of degassed methanol. The block copolymer was recovered by precipitation into an excess of methanol (5 times the polymer solution) containing 10% water, filtered, and dried under vacuum at 55° C. for 12 h to give 37 g of P(Sb-MMA) (97% yield).

[0141] 100Å, 500Å, 10 3 Å, 10 5 Å and 10 6 Gel permeation chromatography (GPC) with an Åμ-Ultrastyragel column showed that the first PS block had an M of 10,400 g / mol against a PS calibration standard. n,PS The diblock copolymer molecular weight obtained from GPC was shown to have a Mw / Mn of 1.06. n,P(S-b-MMA) = 23,400 g / mol and Mw / Mn = 1.09.n,PS The molecular weight of the PMMA block was calculated based on the NMR intensities of -OCH3 protons and aromatic protons on the basis of the (GPC) block. n,PMMA (NMR) = 11,000 g / mol. This is the V f-PS = 0.51. This triblock copolymer was also measured by GPC.

[0142] Synthesis Example 7a: Synthesis of Oligoblock Copolymers of Styrene and Methyl Methacrylate for L / S Assembly Additives This oligoblock copolymer (Sb-MMA) (20K-23K) was synthesized in a similar manner to that described in Synthesis Example 7. The ratio of S-BuLi and monomer was adjusted to achieve the desired molecular weight. 3 Å, 10 5 Å and 10 6 Gel permeation chromatography with an Åμ-Ultrastyragel column was used to determine the M n,PS (GPC)=20,253 g / mol and Mw / Mn=1.02. The diblock copolymer molecular weight obtained from GPC was Mn,P(Sb-MMA)=41,098 g / mol and Mw / Mn=1.02. The volume fraction determined by NMR was Vf-PS=0.506.

[0143] Synthesis Example 8: Synthesis of oligo(styrene-co-p-octylstyrene)-b-(methyl methacrylate-co-di(ethylene glycol) methyl ether methacrylate) for contact hole additive All monomers were distilled in the presence of a dehydrating agent into calibrated ampoules and stored under N2. The liquid was transferred into the reactor under N2 via the ampoules or using stainless steel cannula. 400 mL of anhydrous tetrahydrofuran was added into a dry 1 L round bottom reactor equipped with a side arm for connecting the ampoules, a magnetic stir bar, and a nitrogen / vacuum three-way septum adapter. The temperature of the reactor was lowered to -78°C using a dry ice-acetone bath. Then, after titrating the impurities, 1.2 mL (0.0016 moles) of sec-butyllithium was added into the reactor. Then, a mixture of styrene (8.92 g, S) and p-octylstyrene (3 g, OS) was added into the reactor from the ampoules with rapid stirring. The reaction solution turned yellow-orange and the reaction was stirred for 10 minutes. Then, 0.35 g of 1,1'-diphenylethylene (DPE) in 2.5 ml of anhydrous toluene was added into the reactor via the ampoules. The orange color of the reaction mixture changed to a dark brick red color, suggesting that the styryllithium active center was converted to a delocalized DPE-adducted carbanion. After 2 min of stirring, a small amount (2 mL) of the reaction mixture was taken for PS block molecular weight analysis. A mixture of methyl methacrylate (4.82 g, MMA) and di(ethylene glycol) methyl ethyl methacrylate (1.6 g, DEGMEMA), distilled in the presence of small amounts of triethylaluminum (1 M in toluene) and CaH2, respectively, was then added via ampoule. The reaction was quenched after 15 min with 1 mL of degassed methanol. The block copolymer was recovered by precipitation into excess methanol (five times the volume of the polymer solution) containing 10% water, filtered, and dried under vacuum at 55° C. for 12 hours to give 17 g of oligo(S-co-p-OS)-bP(MMA-co-DEGMEMA) consisting of 25 mol % OS in the polystyrene block and 25 mol % DEGMEMA in the polymethyl methacrylate block (94% yield). 3 Å, 10 5 Å and 10 6Gel permeation chromatography equipped with an Åμ-Ultrastyragel column showed that the first P(S-co-OS) block had an Mn (GPC) of 13,000 g / mol and an Mw / Mn of 1.015 relative to a PS calibration standard. The diblock copolymer molecular weight obtained from GPC was M n,P(S-co-p-OS)-b-P(MMA-co-DEGMEMA) = 19,500 g / mol and Mw / Mn = 1.04. The theoretical feed ratio of the non-polar block to the polar block is V f-P(S-co-OS) = 0.70. This block copolymer exhibited a Tg of 79°C.

[0144] Synthesis Example 9: Synthesis of oligo(styrene-co-p-octylstyrene)-b-(methyl methacrylate-co-di(ethylene glycol) methyl ether methacrylate) (oligo(S-co-p-OS)-bP(MMA-co-DEGMEMA)) for L / S assembly additive All monomers were distilled in the presence of a dehydrating agent into calibrated ampoules and stored under N2. The liquid was transferred into the reactor under N2 via the ampoules or using a stainless steel cannula. 400 mL of anhydrous tetrahydrofuran was added into a dry 1 L round-bottom reactor equipped with a side arm for connecting the ampoules, a magnetic stir bar, and a nitrogen / vacuum three-way septum adapter. The temperature of the reactor was lowered to -78°C using a dry ice-acetone bath. Then, after titrating the impurities, 1.0 mL (0.0013 moles) of sec-butyl lithium was added into the reactor. A mixture of styrene (10.64 g, S) and p-octylstyrene (1.76 g, OS) was then added into the reactor from the ampoules with rapid stirring. The reaction solution turned yellow-orange and the reaction was stirred for 10 minutes. Then, 0.32 g of 1,1'-diphenylethylene (DPE) in 2.5 ml of anhydrous toluene was added into the reactor via an ampoule. The orange color of the reaction mixture changed to a dark brick red color, suggesting that the styryllithium active center was converted to a delocalized DPE-adducted carbanion. After 2 min of stirring, a small amount (2 mL) of the reaction mixture was taken for PS block molecular weight analysis. Then, a mixture of methyl methacrylate (13.75 ml, 12.87 g, MMA) and di(ethylene glycol) methyl ethyl methacrylate (2 g, DEGMEMA), each distilled in the presence of small amounts of triethylaluminum (1 M in toluene) and CaH2, was added via an ampoule. The reaction was stopped after 15 min with 1 mL of degassed methanol. The block copolymer was recovered by precipitation into excess methanol (five times the volume of the polymer solution) containing 10% water, filtered, and dried at 55°C under vacuum for 12 hours to give 17 g of oligo(S-co-p-OS)-bP(MMA-co-DEGMEMA) (94% yield) consisting of 15 mol% OS in the polystyrene block and 14 mol% DEGMEMA in the polymethyl methacrylate block. 3 Å, 10 5 Å and 10 6Gel permeation chromatography with an Åμ-Ultrastyragel column showed that the first P(S-co-OS) block had a Mn (GPC) of 10,800 g / mol and a Mw / Mn of 1.14 relative to a PS calibration standard. The diblock copolymer molecular weight obtained from GPC was M n,P(S-co-p-OS)-b-P(MMA-co-DEGMEMA) = 30,000 g / mol and Mw / Mn = 1.07. The theoretical feed ratio of the non-polar block to the polar block is V f-P(S-co-OS) = 0.50. This block copolymer exhibited a Tg of 90°C.

[0145] Formulation Examples 1-5 (Form.Ex.1-5) Table 1 relates to formulations of block copolymers of styrene and methyl methacrylate P(Sb-MMA) for use in forming contact hole (CH) arrays. Formulations 1-5 contain no additive (Form. Ex. 1), an oligomeric random copolymer of styrene and methyl methacrylate (Form. Ex. 2 and 3), or the oligomer (styrene-co-p-octylstyrene)-b-(methyl methacrylate-co-di(ethylene glycol) methyl ether methacrylate) [oligo(P(S-co-p-OS)-bP(MMA-co-DEGMEMA))] (Form. Ex. 4 and 5), respectively. These formulations were prepared by dissolving block copolymers P(Sb-MMA)(78k-39k) (Synthesis Example 2) and P(Sb-MMA)(34K-17K) (Synthesis Example 3) individually in propylene glycol methyl ether acetate (PGMEA) to give 2.0 wt% solutions. These solutions were then combined and diluted to 1.5 wt% with PGMEA. In formulation example 1, which did not contain any additive, the solution was then filtered using a PTFE membrane. In formulations 2-5, the additive oligo(S-co-MMA) (Forms. Ex. 2 and 3) or oligo(S-co-p-OS)-bP(MMA-co-DEGMEMA) (Forms. Ex. 4 and 5) was added as shown in Table 1 before filtering through the PTFE membrane.

[0146] Formulation Examples 6-9 and Comparative Formulations 1-3 Table 2 relates to formulations of block copolymers of styrene and methyl methacrylate P(Sb-MMA) for use in the formation of contact hole (CH) self-assembly. Formulations 6-9 contain, respectively, no additive (Form.Ex.6), or oligo(S-co-MMA) as an additive (Form.Ex.7, 8 and 9), or, for comparative formulations 1-3, a random high molecular weight copolymer of styrene and methyl methacrylate P(MMA-co-S) [Comp.Form.Ex.1, 2 and 3]. These formulations were prepared by dissolving block copolymers of styrene and methyl methacrylate P(Sb-MMA)(42K-47K) (Synthesis Example 4) in PGMEA to give a 2.0 wt% solution. The solutions were then combined and diluted to 1.5 wt% with PGMEA. For formulation example 6 without additive, the solution was then filtered using a PTFE membrane. In Formulation Examples 7-9 (Form. Ex. 7-9), oligo P(S-co-MMA) (Synthesis Example 9) or in Comparative Examples 1-3 (Comp. Ex. 1-9), a high molecular weight random copolymer of styrene and methyl methacrylate P(S-co-MMA) (Comparative Synthesis Example 1) (Comp. Synth. Ex. 1) was added as an additive as described in Table 2 before filtering through a PTFE membrane.

[0147] Mixture Examples 6, 10-14 Table 3 relates to formulations of block copolymers of styrene and methyl methacrylate P(Sb-MMA) for use in forming contact hole line and space (L / S) arrays. These formulations were prepared by dissolving block copolymers of styrene and methyl methacrylate P(Sb-MMA) (42K-47K) (Synthesis Example 4) in PGMEA to give 2.0 wt % solutions. These solutions were then combined and diluted to 1.5 wt % with PGMEA. For formulation example 6, which did not contain additives, the solution was then filtered using a PTFE membrane. In Formulation Examples 10-12 (Form. Ex. 10-12), oligo(S-co-p-OS)-bP(MMA-co-DEGMEMA) was added as an additive, and in Formulation Examples 13-14, an oligomeric block copolymer of styrene and methyl methacrylate (oligo(Sb-MMA)) was added as an additive, as shown in Table 3, before filtering through a PTFE membrane.

[0148] Formulation Examples 15, 16 and Comparative Formulation 4 Preparation of stock solutions A first stock solution (3.2 wt %) of the ABA triblock copolymer was prepared by dissolving 0.6 g of Synthesis Example 4a in 18 g of PGMEA and filtering the solution.

[0149] A second stock solution (3.2 wt %) of the oligomeric block copolymer of Synthesis Example 9 was prepared by dissolving 0.6 g of this material in 18 g of PGMEA and filtering the solution.

[0150] A third stock solution of the oligomeric block copolymer of Synthesis Example 7a was prepared by dissolving 0.83 g of this material in 25 g of PGMEA and filtering the solution.

[0151] Comparative Formulation Example 4 The first stock solution was used as Comparative Example 4, i.e., a solution of triblock copolymer only was used to establish the defect level observed during self-assembly of this triblock copolymer without the addition of any oligomeric additive component.

[0152] Mixture Example 15 This formulation was prepared by combining 4.6 g of the first stock solution containing Synthesis Example 4a with 0.92 g of the second stock solution, and was used to demonstrate the effect of the oligomeric block copolymer of component type 2-b) (Synthesis Example 9) on the defect levels observed during self-assembly of the triblock copolymer.

[0153] Mixture Example 16 This formulation was prepared by combining 5.4 g of the first stock solution containing Synthesis Example 4a with 1.08 g of the second stock solution, and was used to demonstrate the effect of the oligomeric block copolymer of component type 3-b) (Synthesis Example 4a) on the defect levels observed during self-assembly of the triblock copolymer.

[0154] Processing of Comparative Example 4, Formulation Example 15 and Formulation Example 16 These formulations were filtered through a 0.2 μm Teflon filter prior to coating. Coating was performed using a TEL ACT8 track onto 8 inch silicon wafers that had been pre-coated with a neutral layer (see below), followed by a soft bake at 110° C. for 1 minute and a hard bake at 250° C. for 1 hour.

[0155] neutral layer For all block copolymer formulations tested, silicon wafers were first coated with "Neutral Layer Formulation 1" as a neutral layer formulation, which was prepared by dissolving the polymer of Synthesis Example 1 in PGMEA to form a neutral layer formulation, which was used to coat the overcoated wafer as follows: The neutral layer was formed by casting Neutral Formulation Example 1 (74% PS) onto a silicon wafer and baking it at 240°C / 5 minutes, followed by rinsing with PGMEA for 30 seconds and baking at 110°C for 1 minute.

[0156] Self-assembled membrane processing Unless otherwise stated, the self-assembly formulations described herein were spin-coated at 1500 rpm on top of the neutral layer to form films with a thickness of approximately 50 nm, then baked at 250°C for 5 minutes under nitrogen to allow self-assembly. After self-assembly, the films were then etched using oxygen plasma for times between 0 and 70 seconds as indicated in the particular figures and tables. The oxygen etch was performed using a Nordson-March etcher with RF power = 50 (W), base pressure = 50 (mTorr), process pressure = 90 (mTorr), and O2 = 15 (sccm).

[0157] Self-assembly and etching results Results of CH formulation Formulations of P(Sb-MMA) polymer blends containing up to 30 wt. % oligomeric additives, as shown in the examples in Table 1, showed reduced defects observed after up to three oxygen plasma etches compared to reference samples without these additives.

[0158] Specifically, Figure 1 shows top-down SEM investigations (2 μm FOV) of the self-assembly and etching of poly(styrene-block-methyl methacrylate) CH block copolymer formulations [blends of P(Sb-MMA) (78K-b-39K) and (34K-b-17K)] listed in Table 1 when cast as films onto a neutral layer. These results are based on the results of 50 nm films (approximately 1 L) of these formulations when coated onto a neutral layer, annealed at 250°C to induce self-assembly, and etched. o The effect of adding 0-20 wt% of oligo(S-co-MMA) as an additive in SiO2 films was shown. The films were etched with oxygen plasma for either 50 or 70 seconds. In these etched self-assembled films, the number of defects observed is greatly reduced with increasing amounts of this oligomeric additive. In contrast, formulations without any of the additives showed a significantly higher number of defects.

[0159] Similarly, Figure 2 shows a cross-sectional SEM image (250x magnification) of a self-assembled film of this CH formulation after etching for 20 seconds, where the number of defects decreased as the loading of this additive increased from 10 to 20 wt %.

[0160] Figure 3 shows similar top-down SEM CH defects as examined above for Figure 1. However, in this example, the additive used was oligo(S-co-p-OS)-bP(MMA-co-DEGMEMA) (Synth.Ex.8) rather than oligo(S-co-MMA). Use of oligo(S-co-p-OS)-bP(MMA-co-DEGMEMA) was also observed with a large decrease in defect count observed as the additive amount was increased from 0 wt% to 20 wt% as shown in Figure 3.

[0161] Results of L / S formulation FIG. 4 shows top-down SEM L / S study of self-assembled films of block copolymer P(Sb-MMA) (45.4kb-51K) formulated without oligo(S-co-p-OS)-bP(MMA-co-DEGMEMA) or with 10, 20 or 30 wt % of this additive [Synth.Ex.9] when cast on a neutral layer. These formulations are formulations 6, 7, 8 and 9 in Table 3, respectively. After etching these self-assembled films with oxygen plasma for 30, 50 or 70 seconds, the samples without the additive showed numerous defects, whereas, in contrast, the samples with 10 or 20 wt % of this additive showed almost no defects even after etching for 70 seconds.

[0162] FIG. 5 shows top-down SEM L / S study of self-assembled films of block copolymer P(Sb-MMA) (45.4kb-51k) formulated without oligo(Sb-MMA) (alternatively 0 wt%) or with this additive (Synth.Ex.7) (10 wt% or 20 wt%), when cast on a neutral layer. These formulations are formulations 6 (0 wt%), 13 (10 wt%) and 14 (20 wt%) in Table 3, respectively. After etching these self-assembled films with oxygen plasma for 30 seconds, the sample without additive (0 wt%) showed numerous defects, whereas, in contrast, the samples with 10 wt% or 20 wt% of this additive showed no noticeable defects even after etching for 30 seconds.

[0163] Tables 4 and 5 summarize the defect results obtained after self-assembly and etching for the L / S formulations described in Table 2. Tables 4 and 5 contrast the defects obtained after self-assembly and oxygen plasma etching for films of formulations of block copolymer P(Sb-MMA) (45.4 kb-51 k) (Form.Ex.7, 8 and 9) cast onto neutral layers containing oligo(S-co-MMA) as a low Tg additive (Comp.Synth.Ex.6) compared to films cast from formulations containing the same loadings of the high Tg polymeric additive P(S-co-MMA) [Comp.Synth.Ex.1] (Form.Comp.1, 2 and 3), at loadings ranging from 10 wt% to 30 wt%. This is surprising because the oligo(S-co-MMA) [Synth.Ex.7] was 1 micron smaller than the formulation containing P(S-co-MMA) [Comp.Synth.Ex.1]. 2 It is shown that it gives significantly less number-average network assembly defect per unit area.

[0164] FIG. 6 shows top-down SEM L / S study of self-assembled films of block copolymer P(MMA-bSb-MMA) (50k-88k-50k) formulated without additive (alternatively 0 wt%), with this additive [Synth.Ex.9] (oligo(S-co-p-OS)-bP(MMA-co-DEGMEMA) (20 wt%), or with this additive [Synth.Ex.7a] (oligo(Sb-MMA) (20 wt%)) when cast on a neutral layer. The latter two formulations are formulations 15 (20 wt%) and 16 (20 wt%) in Table 3, respectively. These self-assembled films were etched with oxygen plasma for 30 seconds. The defect counts of these 3LoFT self-assembled films were determined using a Hitachi DSA. The results were obtained using the APPS software. The sample without additive (0 wt%) showed a large number of defects (101 defects), whereas in contrast, the samples with 20 wt% (oligo(S-co-p-OS)-bP(MMA-co-DEGMEMA) or 20 wt% oligo(Sb-MMA) showed defect levels of only 7 and 15, respectively.

[0165] [Table 1]

[0166] [Table 2]

[0167] [Table 3]

[0168] [Table 4]

[0169] [Table 5] While this application is directed to the invention set forth in the claims, the disclosure of this application also includes: 1. A composition comprising the following components a), b) and c): a) is a block copolymer component or a blend of at least two block copolymers; b) is Oligorandom copolymer b-1), Oligodiblock copolymer b-2), Oligodiblock copolymer b-3), and Mixtures of these A low Tg additive selected from the group consisting of: b-1) is an oligorandom copolymer of two repeating units having the structure (Ib) and the structure (IIb), where R 1b and R 3b is independently selected from H or C1-C4 alkyl; R 2b is H or C1-C8 alkyl, R 4b is C1-C8 alkyl, and The mole percentages based on the total number of moles of repeating units of Structures (Ib) and (IIb) are about 40 mole % to about 80 mole % for repeating units of Structure (Ib) and about 20 mole % to about 60 mole % for repeating units of Structure (IIb); and the individual values ​​of the mole percent of repeat units of Structures (Ib) and (IIb) are selected from their respective ranges such that the total number of moles of repeat units of Structures (Ib) and (IIb) add up to 100 mole percent; and further The oligorandom copolymer b-1) has a Tg of about 0° C. to about 80° C., and has an Mn of about 1000 g / mol to about 8,000 g / mol; and having a polydispersity of about 1.3 to about 1.8;

change

change

change

change

change

change

change

change

change

change

change

change

Claims

1. A composition comprising the following components a), b) and c): a) is a block copolymer component or a blend of at least two block copolymers; The component a) is an ABA triblock copolymer component selected from the group consisting of ABA triblock copolymer a-1t), ABA triblock copolymer a-2t), and a blend of ABA triblock copolymer a-1t) and ABA triblock copolymer a-2t), with the proviso that a-1t) is an ABA triblock copolymer comprising an intermediate B) styrenic block segment of repeating units having a styrenic structure (I) and two terminal acrylic block A) segments of equal length having the structure (II), where R 1 and R 3 are independently selected from H and C1-C4 alkyl, R 2 is H or C1-C8 alkyl, and R 4 is C1-C8 alkyl; and the mole percent, based on the total number of moles of repeat units of structures (I) and (II), is 40 mole percent to 80 mole percent for repeat units of structure (I) and 20 mole percent to 60 mole percent for repeat units of structure (II); and the individual values ​​of the mole percent of repeat units of Structures (I) and (II) are selected from their respective ranges such that the total number of moles of repeat units of Structures (I) and (II) add up to 100 mole percent; and the triblock copolymer a-1t) has a polydispersity of 1.0 to 1.1 and a Mn of 70,000 g / mol to 350,000 g / mol; 【Chemistry 1】 a-2t) is an ABA triblock copolymer comprising a middle B) block segment of repeating units having a styrenic structure (Ia) and two end block A) segments of equal length having an acrylic structure (IIa), where R 1a and R 3a are independently selected from H and C1-C4 alkyl, R 2a is H or C1-C8 alkyl, and R 4a is C1-C8 alkyl; the mole percent, based on the total number of moles of repeat units of structures (Ia) and (IIa), is 40 mole % to 80 mole % for repeat units of structure (Ia) and 20 mole % to 60 mole % for repeat units of structure (IIa); and the individual values ​​of the mole percent of repeat units of structures (Ia) and (IIa) are selected from their respective ranges such that the total number of moles of repeat units of structures (Ia) and (IIa) add up to 100 mole percent; and The triblock copolymer a-2t) has a polydispersity of 1.0 to 1.1 and a Mn of 70,000 g / mol to 350,000 g / mol; 【Chemistry 2】 or, said component a) being a diblock copolymer component selected from the group consisting of diblock copolymer a-1), diblock copolymer a-2), and blends of a-1) and a-2), a-1) is a diblock copolymer of block A) comprising styrenic repeat units having a styrenic structure (I) and block B) comprising repeat units having an acrylic structure (II), wherein R 1 and R 3 are independently selected from H and C1-C4 alkyl, R 2 is H or C1-C8 alkyl, and R 4 is C1-C8 alkyl, and the mole percentages based on the total number of moles of repeat units of structures (I) and (II) are 40 mole % to 80 mole % for repeat units of structure (I) and 20 mole % to 60 mole % for repeat units of structure (II); the individual values ​​of the mole percent of repeat units of Structures (I) and (II) are selected from their respective ranges such that the total number of moles of repeat units of Structures (I) and (II) add up to 100 mole percent; and said diblock copolymer a-1) having a polydispersity of 1.0 to 1.1 and a Mn of 93,000 g / mol to 150,000 g / mol; 【Chemistry 3】 a-2) is a diblock copolymer of a block A-a) comprising repeating units having a styrenic structure (Ia) and a block B-a) comprising repeating units having an acrylic structure (IIa), where R 1a and R 3a are independently selected from H or C1-C4 alkyl, R 2a is H or C1-C8 alkyl, and C 4a is C1-C8 alkyl; and the mole percent, based on the total number of moles of repeat units of structures (Ia) and (IIa), is 40 mole % to 80 mole % for repeat units of structure (Ia) and 20 mole % to 60 mole % for repeat units of structure (IIa); and the individual values ​​of the mole percent of repeat units of Structures (Ia) and (IIa) are selected from their respective ranges such that the total number of moles of repeat units of Structures (Ia) and (IIa) add up to 100 mole percent; and The diblock copolymer a-2) has a polydispersity of 1.0 to 1.1 and a Mn of 30,000 g / mol to 90,000 g / mol; 【Chemistry 4】 b) is Oligorandom copolymer b-1), Oligodiblock copolymer b-2), Oligodiblock copolymer b-3), and Mixtures of these A low Tg additive selected from the group consisting of: b-1) is an oligorandom copolymer of two repeat units having the structure (Ib) and the structure (IIb), where R 1b and R 3b is independently selected from H or C1-C4 alkyl; R 2b is H or C1-C8 alkyl, R 4b is a C1-C8 alkyl, and The mole percentages based on the total number of moles of repeat units of structures (Ib) and (IIb) are 40 mole % to 80 mole % for repeat units of structure (Ib) and 20 mole % to 60 mole % for repeat units of structure (IIb); and the individual values ​​of the mole percent of repeat units of Structures (Ib) and (IIb) are selected from their respective ranges such that the total number of moles of repeat units of Structures (Ib) and (IIb) add up to 100 mole percent; and further The oligorandom copolymer b-1) has a Tg of 0° C. to 90° C., and has an Mn of 1000 g / mol to 5,000 g / mol; and having a polydispersity of 1.3 to 1.8; 【Chemistry 5】 b-2) is an oligodiblock copolymer of block A-b) and block B-b) having a Mn of 1,000 to 35,000 and a polydispersity of 1.0 to 1.1, provided that Block Ab) is a random copolymer of repeating units having structures (III) and (IV) and block Bb) is a random copolymer of repeating units having structures (V) and (VI), and R 5 , R 7 , R 9 , and R 11 is independently selected from H or C1-C4 alkyl; R 6 is a C7-C10 linear alkyl group; R 8 is H or C1-C4 alkyl, R 10 is C1-C4 alkyl, R 12 and R 13 is independently selected from C2-C5 alkylene, and R 14 is a C1 to C4 alkyl, and the oligodiblock copolymer b-2) has a Tg having a value from 0° C. to 95° C., 【Chemistry 6】 b-3) is an oligodiblock copolymer of a block Ac) containing a repeating unit having the structure (Ic) and a block B-c) containing a repeating unit having the structure (IIc), where R 1c and R 3c is independently selected from H or C1-C4 alkyl; R 2c is H or C1-C8 alkyl, R 4c is a C1-C8 alkyl, and the mole % values ​​based on the total number of moles of repeat units of Structures (Ic) and (IIc) are 36 mole % to 74 mole % for repeat units of Structure (Ic) and 26 mole % to 64 mole % for repeat units of Structure (IIc), and the individual values ​​of the mole % for repeat units of Structures (Ic) and (IIc) are selected from their respective ranges such that the total number of moles of repeat units of Structures (Ic) and (IIc) add up to 100 mole %, and said oligodiblock copolymer b-3) has a Mn of 1000 g / mol to 30,000 g / mol, a polydispersity of 1.0 to 1.1, and a Tg of 0° C. to 115° C.; 【Chemistry 7】 c) is an organic solvent for spin casting; The glass transition temperature (Tg) was determined by DSC measurement using a heating rate of 10°C / min under nitrogen, taking the Tg in a first heating scan from 0 to 300°C as the midpoint of the endothermic transition; and Mn and polydispersity were measured at 100 Å, 500 Å, ... 3 Å, 10 5 Å and 10 6 Determined by gel permeation chromatography equipped with an Åμ-Ultrastyragel column, However, compositions containing the diblock copolymer a-2) in combination with the oligodiblock copolymer b-3) are excluded.

2. 10. The composition of claim 1, wherein component a) is selected from either a single triblock copolymer and a blend of at least two triblock copolymers, or a single diblock copolymer and a blend of at least two diblock copolymers.

3. The component a) is a triblock copolymer selected from a triblock copolymer of structure (ABA-1), a triblock copolymer of structure (ABA-2), and a mixture of these two block copolymers, where mt, mta, nt, and nta are the number of repeat units, R 1s , R 1sa , R 2s , and R 2sa are independently hydrogen, C1-C8 alkyl, -N(R 3s ) 2 , -OR 4s , and Si(R 5s ) 3 where R 3s , R 4s and R 5s The composition of claim 1 or 2, wherein is independently selected from C1 to C4 alkyl. 【Chemistry 8】

4. R 1 , R 1a , R 2 , R 2a And R 1s and R 2s is H and R 3、 R 3a、 R 4 , and R 4a The composition of claim 3 , wherein is methyl.

5. R 1 , R 1a , R 2 and R 2a is H, and R 3、 R 3a、 R 4 , and R 4a The composition of claim 1 or 2, wherein is methyl.

6. Diblock copolymers a-1) and a-2) have structures (IS) and (IS-a), respectively, where R 1s , R 1sa , R 2s , and R 2sa are independently hydrogen, C1-C8 alkyl, -N(R 3s ) 2 , -OR 4s , and Si(R 5s ) 3 where R 3s , R 4s and R 5s The composition of claim 1 or 2, wherein is independently selected from C1 to C4 alkyl. 【Chemistry 9】

7. R 1s , R 2s , R 1sa and R 2sa The composition of claim 6 , wherein is hydrogen.

8. The oligodiblock copolymers b-2) and b-3) have a spacer moiety between block A-b) and block B-b) or between block A-c) and block B-c) as shown in structure (I-S-b) and structure (I-S-c), respectively, with the proviso that R 1sb , R 1sc , R 2sb , and R 2sc are independently hydrogen, C1-C8 alkyl, -N(R 3s ) 2 , -OR 4s , Si(R 5s ) 3 where R 3s , R 4s and R 5s The composition of any one of claims 1 to 7, wherein is independently selected from C1 to C4 alkyl. 【Chemistry 10】

9. R 1sb , R 2sb , R 1sc and R 2sc The composition of claim 8 , wherein is hydrogen.

10. 8. The composition according to claim 1, wherein for component a), the diblock copolymer component a-1) has a polydispersity of 1.00 to 1.03 and / or a Mn of 93,000 g / mol to 105,300 g / mol.

11. For said diblock copolymer component a-1) of component a), the mole percentage of repeat units of structure (I) is 40 mole % to 60 mole %, and the mole percentage of repeat units of structure (II) is 40 mole % to 60 mole %, or The mole percent of the repeating unit of structure (I) is 60 mole percent to 75 mole percent, and the mole percent of the repeating unit of structure (II) is 25 mole percent to 40 mole percent; The composition according to any one of claims 1 to 7.

12. 8. The composition according to any one of claims 1 to 7, wherein for component a), the diblock copolymer component a-2) has a polydispersity of 1.00 to 1.03 and / or a Mn of 40,800 g / mol to 61,200 g / mol.

13. For component a), in either the single block copolymer a-1) or a-2) or in a blend of a-1) and a-2), the total mole % value of repeat units of structures (I) and (Ia) is from 40 mol % to 60 mol %, and the total mole % value of repeat units of structures (II) and (IIa) is from 40 mol % to 60 mol %, or For component a), in either the single block copolymer a-1) or a-2) or in a blend of a-1) and a-2), the total mole % value of repeat units of structures (I) and (Ia) is from 60 mol % to 75 mol %, and the total mole % value of repeat units of structures (II) and (IIa) is from 25 mol % to 40 mol %; The composition according to any one of claims 1 to 7.

14. A composition according to any one of claims 1 to 7, wherein component a) is from 0.5% to 2.0% by weight of the total composition.

15. The oligorandom copolymer b-1) as component b) is R 1b and R 2b is H, and R 3b and R 4b is methyl; and / or The oligodiblock copolymer b-2) is R 5 , R 7 and R 8 is H, and R 6 is n-octyl or n-nonyl, R 9 and R 11 is methyl, R 10 is methyl or ethyl, R 12 and R 13 is independently ethylene or propylene, and R 14 is methyl or ethyl; and / or The oligodiblock copolymer b-3) is R 1c and R 2c is H, and R 3c and R 4c is methyl; The composition according to any one of claims 1 to 7.

16. R 6 is n-octyl, R 10 is methyl, R 12 and R 13 is ethylene, and R 14 The composition of claim 15 , wherein is methyl.

17. 8. The composition according to claim 1, wherein for component b), the oligorandom copolymer b-1) has a polydispersity of 1.3 to 1.5 and / or a Tg of 50°C to 90°C.

18. Regarding the oligodiblock copolymer b-2) of component b), this is said mole percent of repeat units of structure (IV) is 25 mole percent to 50 mole percent; and said mole percent of repeat units of structure (V) is 40 mole percent to 60 mole percent; or the mole % of repeat units of structure (III) is 20% to 30% of the mole % of repeat units of structure (IV), and the mole % of repeat units of structure (VI) is 12% to 20% of the mole % of repeat units of structure (V); the individual values ​​of the mole percent of repeat units of structures (III), (IV), (V), and (VI) are selected from their respective ranges such that the total number of moles of repeat units of structures (III), (IV), (V), and (VI) add up to 100 mole percent; It is something like, The composition according to any one of claims 1 to 7.

19. 8. The composition according to claim 1, wherein for component b), the oligodiblock copolymer b-2) has a polydispersity of 1.03 to 1.08, and / or a Mn of 15000 g / mol to 32000 g / mol, and / or a Tg of 50°C to 90°C.

20. 8. The composition according to claim 1, wherein for component b), the oligodiblock copolymer b-3) has a Mn of 15,000 to 30,000 g / mol, and / or a polydispersity of 1.02 to 1.08, and / or a Tg of 50° C. to 90° C.

21. Component b) is an oligodiblock copolymer b-3), which is The composition of any one of claims 1 to 7, wherein the mole percent of repeating units of structure (Ic) is from 40 mole percent to 60 mole percent, and the mole percent of repeating units of structure (IIc) is from 40 mole percent to 60 mole percent.

22. 8. The composition of claim 1, wherein component a) is a diblock copolymer component selected from the group consisting of diblock copolymer a-1), diblock copolymer a-2) and blends of a-1) and a-2), or a triblock copolymer component selected from the group consisting of triblock copolymer a-1t), triblock copolymer a-2t) and blends of a-1t) and a-2t), the total mole % of styrenic repeat units of structures (I) and (Ia) is from 45 mole % to 75 mole %, the total mole % of acrylic repeat units of structures (II) and (IIa) is from 25 mole % to 55 mole %, and component b) is an oligorandom copolymer b-1), an oligodiblock copolymer b-2) or an oligodiblock copolymer b-3).

23. 8. The composition of claim 1, wherein component a) is a diblock copolymer component selected from the group consisting of diblock copolymer a-1), diblock copolymer a-2), and blends of a-1) and a-2), or a triblock copolymer component selected from the group consisting of triblock copolymer a-1t), triblock copolymer a-2t), and blends of a-1t) and a-2t), the total mole % of styrenic repeat units of structures (I) and (Ia) is from 60 mole % to 75 mole %, and further the total mole % of acrylic repeat units of structures (II) and (IIa) is from 25 mole % to 40 mole %, and component b) is an oligorandom copolymer b-1), an oligodiblock copolymer b-2), or an oligodiblock copolymer b-3).

24. Next steps: i) forming a coating of a neutral layer on a substrate; ii) coating the composition according to any one of claims 1 to 23 onto the neutral layer to form a film; ii) baking the film in an inert gas atmosphere at a temperature selected from 240° C. to 260° C. to form a self-assembled film; and iii) etching the substrate with a plasma to transfer the self-assembled monolayer into the substrate in a pattern; The method includes:

25. 1. A method for forming a line and space array comprising: ia) forming a coating of a neutral layer on a substrate; iia) coating the composition of claim 22 onto the neutral layer to form a film; iiia) baking the film in an inert gas atmosphere at a temperature selected from 240° C. to 260° C. to form a self-assembled film; and iva) etching the substrate with a plasma to transfer the self-assembled monolayer into the substrate in a pattern; The method comprising:

26. 1. A method of forming a contact hole array, comprising: ib) forming a coating of a neutral layer on the substrate; iib) coating the composition of claim 23 onto the neutral layer to form a film; iiib) baking the film in an inert gas atmosphere at a temperature selected from 240° C. to 260° C. to form a self-assembled film; and ivb) etching the substrate with a plasma to transfer the self-assembled monolayer into the substrate in a pattern; The method comprising:

27. The oligodiblock copolymer b-2) as defined in any one of claims 1 to 23.

28. 28. The oligodiblock copolymer of claim 27, wherein the mole % of the sum of the mole % of repeat units (III) and (IV) ranges from 40 mol % to 80 mol %, and the mole % of the sum of the mole % of repeat units (V) and (VI) ranges from 20 mol % to 60 mol %, based on the total number of moles of repeat units having structures (III), (IV), (V), and (VI), further wherein the mole % of repeat units (III) ranges from 2 mol % to 64 mol %, and the mole % of repeat units (VI) ranges from 1 mol % to 48 mol %, and further wherein the individual values ​​of the mole % of repeat units of structures (III), (IV), (V), and (VI) are selected from their respective ranges such that the total number of moles of repeat units of structures (III), (IV), (V), and (VI) add up to 100 mol %.

29. The polymerizable composition of claim 20, wherein the mol% of repeating units of structure (IV) is 25 mol% to 50 mol% and the mol% of repeating units of structure (V) is 40 mol% to 60 mol%; the individual values ​​of the mole percent of repeat units of structures (III), (IV), (V), and (VI) are selected from their respective ranges such that the total number of moles of repeat units of structures (III), (IV), (V), and (VI) add up to 100 mole percent; 28. The oligodiblock copolymer of claim 27.

30. Use of a composition according to any one of claims 1 to 23 or an oligodiblock copolymer according to any one of claims 27 to 29 for preparing a self-assembled monolayer on a substrate.

Citation Information

Patent Citations

  • Buffer for absorbing striking energy

    JP1981042731A

  • Relay device

    JP1982010546A

  • Thin polymer film, patterned substrate, patterned medium for magnetic recording and their manufacturing methods

    JP2008231233A

  • Polymer thin film, pattern medium, and method for producing them

    JP2010144120A

  • Method of producing polymer thin film having microstructure and pattern substrate

    JP2013129836A