Thermally conductive adhesive, cured product, and structure

The thermally conductive adhesive, featuring a polyol and polyisocyanate composition with surface-treated fillers, addresses issues of slow curing and poor adhesion in existing adhesives, providing rapid curing, strong aluminum adhesion, and long-term durability.

JP7593468B1Active Publication Date: 2024-12-03TOYO INK MFG CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2023219951
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-12-26
Publication Date
2024-12-03
Estimated Expiration
2043-12-26

AI Technical Summary

Technical Problem

Existing urethane-based thermally conductive adhesives face issues with slow urethanization reactions, poor adhesion to aluminum substrates, and insufficient mechanical properties due to high filler loading, leading to poor adhesion and long-term humidity resistance.

Method used

A thermally conductive adhesive comprising a polyol composition containing a polyol, a phosphoric acid compound, a dispersant, and a thermally conductive filler, and a polyisocyanate composition with a trifunctional or higher functional epoxy compound and a thermally conductive filler, which are surface-treated with silane coupling agents, to enhance mixing, dispersion stability, and rapid curing at room temperature.

Benefits of technology

The adhesive exhibits excellent thermal conductivity, quick curing at room temperature, strong adhesion to aluminum substrates, and long-term moist heat resistance, with improved dispersion stability and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593468000001
    Figure 0007593468000001
  • Figure 0007593468000002
    Figure 0007593468000002
  • Figure 0007593468000003
    Figure 0007593468000003
Patent Text Reader

Abstract

Provided are a thermally conductive adhesive which is easy to mix with a polyol composition and a polyisocyanate composition and which is excellent in dispersion stability, thermal conductivity, rapid room temperature curing property, adhesion to aluminum substrates, and long-term moisture and heat resistance, and a cured product and structure using the adhesive. [Solution] The above-mentioned problems are solved by a thermally conductive adhesive comprising: a polyol composition containing a polyol (A), a phosphoric acid compound (B), a dispersant (C), and a thermally conductive filler (D1); and a polyisocyanate composition containing a polyisocyanate (E), a tri- or higher functional epoxy compound (F), and a thermally conductive filler (D2).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermally conductive adhesive that exhibits good mixability between a polyol composition and a polyisocyanate composition, and that is excellent in dispersion stability, thermal conductivity, rapid room-temperature curing property, adhesion to aluminum substrates, and long-term moisture and heat resistance, as well as to a cured product and a structure using the adhesive. [Background technology]

[0002] In recent years, with the miniaturization and high integration of electronic components, excessive heat generation and the resulting malfunctions have become problems. In order to operate electronic components normally, there is a demand for components that efficiently dissipate the generated heat. In particular, when it is necessary to fix components that generate heat to a structure, a thermally conductive adhesive that has thermal conductivity imparted by blending a thermally conductive filler into the adhesive resin is useful. When materials are bonded using such a thermally conductive adhesive, there is a problem that the adhesive layer is subjected to high stress due to the difference in the expansion coefficient between the materials caused by temperature changes in the manufacturing process or the temperature environment in which the adhesive layer is used, and this promotes the destruction or deterioration of the adhesive layer. For this reason, urethane-based thermally conductive adhesives with excellent stress relaxation properties have been attracting attention.

[0003] On the other hand, from the viewpoint of productivity and energy saving, the performance of exhibiting sufficient initial adhesive strength under short curing conditions at room temperature (hereinafter referred to as room temperature fast curing) is required, but conventional urethane-based thermally conductive adhesives have the problem that the urethane reaction is slow. In addition, conventional urethane-based thermally conductive adhesives have the problem that sufficient adhesive strength cannot be obtained unless a primer is provided. Furthermore, to obtain high thermal conductivity, it is necessary to fill the adhesive resin with a high concentration of thermally conductive filler, but such heat-dissipating adhesives have the problem of adversely affecting the mechanical properties of the cured coating film and reducing the adhesive strength.

[0004] For example, Patent Document 1 discloses a urethane-based thermally conductive adhesive having excellent mechanical properties, which contains a polyol component that is blended in combination with different filler materials that exhibit different thermal conductivities, and a polyisocyanate component.

[0005] Patent Document 2 discloses a urethane-based thermally conductive adhesive that contains an isocyanate composition containing polyisocyanate and metal oxide particles having a predetermined average particle size that have been surface-treated with an alkoxysilane, and a polyol composition containing a specific thermally conductive filler, and that is described as having low viscosity when mixed and exhibiting high thermal conductivity when cured.

[0006] Patent Document 3 discloses a curable composition containing a polyol containing 50% by weight or more of a polyalkylene glycol having a chemical formula weight or number average molecular weight of 1,000 or less, a polyisocyanate, an inorganic filler, and a specific dispersant, and describes that the composition has excellent thermal conductivity and flexibility, can conform to the shape of a heating element and adhere closely to it, and has excellent heat dissipation efficiency. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Special Publication No. 2021-507067 [Patent Document 2] Special Publication No. 2023-538181 [Patent Document 3] International Publication No. 2021 / 261519 Summary of the Invention [Problem to be solved by the invention]

[0008] However, the adhesive described in Patent Document 1 does not contain a phosphoric acid compound or a dispersant in the polyol component, does not contain a filler or an epoxy compound in the polyisocyanate component, and has low adhesion to aluminum substrates and problems with long-term wet heat resistance when a primer is not provided. In addition, because the filler is contained only in the polyol component, there is a large difference in viscosity between the polyol component and the polyisocyanate component, which causes a problem of easy mixing failure. The adhesive described in Patent Document 2 contains spherical metal oxide particles having an average particle size of 20 μm or more, but does not use a dispersant and has the problem of poor dispersion stability. The composition described in Patent Document 3 has a problem in that the urethane-forming reaction is slow because the polyisocyanate component does not contain an epoxy compound, and therefore the rapid room-temperature curing property is insufficient.

[0009] Therefore, an object of the present invention is to provide a thermally conductive adhesive which allows easy mixing of a polyol composition and a polyisocyanate composition and which is excellent in dispersion stability, thermal conductivity, rapid room temperature curing properties, adhesion to aluminum substrates, and long-term moisture and heat resistance, as well as a cured product and structure using the adhesive. [Means for solving the problem]

[0010] As a result of extensive investigations, the present inventors have found that the above-mentioned problems can be solved. [1] The present disclosure relates to a thermally conductive adhesive comprising: a polyol composition comprising a polyol (A), a phosphoric acid compound (B), a dispersant (C), and a thermally conductive filler (D1); and a polyisocyanate composition comprising a polyisocyanate (E), a tri- or higher functional epoxy compound (F), and a thermally conductive filler (D2).

[0011] [2] The present disclosure relates to the thermally conductive adhesive according to [1], wherein the thermally conductive filler (D1) and the thermally conductive filler (D2) each independently contain at least one filler selected from the group consisting of metal oxides and metal nitrides.

[0012] [3] The present disclosure relates to the thermally conductive adhesive according to [1] or [2], wherein the thermally conductive filler (D1) and the thermally conductive filler (D2) are each independently surface-treated with a silane coupling agent.

[0013] [4] The present disclosure relates to a thermally conductive adhesive according to any one of [1] to [3], wherein the total amount of the thermally conductive filler (D1) and the thermally conductive filler (D2) is 60 mass% or more based on the mass of the thermally conductive adhesive.

[0014] [5] The present disclosure relates to the thermally conductive adhesive according to any one of [1] to [4], wherein the polyol (A) contains 50 mass % or more of a polyol (A1) having a number average molecular weight of 2,000 or less.

[0015] [6] The present disclosure relates to the thermally conductive adhesive according to any one of [1] to [5], wherein the content of the phosphoric acid compound (B) is 0.1 to 5 mass% based on the mass of the polyol (A).

[0016] [7] The present disclosure relates to the viscosity (V OH ) vs. the viscosity (V NCO ) ratio (V NCO / V OH ) is 0.1 to 10.

[0017] [8] The present disclosure relates to a cured product of the thermally conductive adhesive according to any one of [1] to [7].

[0018] [9] The present disclosure relates to a structure comprising an adhesive layer between a first substrate and a second substrate, the adhesive layer being the cured product according to [8]. Effect of the Invention

[0019] The present invention can provide a thermally conductive adhesive which is easy to mix with a polyol composition and a polyisocyanate composition and which has excellent dispersion stability, thermal conductivity, rapid room temperature curing properties, adhesion to aluminum substrates, and long-term moist heat resistance, as well as a cured product and structure using the adhesive. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The thermally conductive adhesive of the present invention comprises a polyol composition and a polyisocyanate composition, the polyol composition comprising a polyol (A), a phosphoric acid compound (B), a dispersant (C) and a thermally conductive filler (D1), and the polyol composition comprising a polyisocyanate (E), a tri- or higher functional epoxy compound (F) and a thermally conductive filler (D2). The above-mentioned composition suppresses settling of the filler and improves the mixability of the polyol composition and the polyisocyanate composition, and also provides excellent thermal conductivity, rapid room temperature curing properties, adhesion to aluminum substrates, and long-term resistance to moist heat. The present invention will be described in detail below. Other embodiments are also included in the scope of the present invention as long as they are consistent with the gist of the present invention. In this specification, a numerical range specified using "~" includes the numerical values ​​before and after "~" as the lower and upper limit values.

[0021] <<Polyol composition>> The polyol composition contains a polyol (A), a phosphoric acid compound (B), a dispersant (C) and a thermally conductive filler (D1).

[0022] <Polyol (A)> The polyol (A) is not particularly limited as long as it is a compound having two or more hydroxyl groups in the molecule. When the polyol (A) is a resin, the hydroxyl group may be present at any one of the terminal, side chain, or side group of the resin. Examples of such polyols (A) that can be used include polyester polyols, polyether polyols, polyurethane polyols, polyesteramide polyols, acrylic polyols, polycarbonate polyols, polycaprolactone polyols, polyvalerolactone polyols, polybutadiene polyols, polyolefin polyols, polyhydroxyalkanes, castor oil, and mixtures thereof. Examples of the polyol (A) that can be used include glycols such as ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-5-pentanediol, 1,6-hexanediol, neopentyl glycol, methylpentane glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, bishydroxyethoxybenzene, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, and triethylene glycol; polyalkylene glycols having a number average molecular weight of 200 to 3,000; trifunctional or tetrafunctional aliphatic alcohols such as glycerin, trimethylolpropane, and pentaerythritol; and polyols in which the above-mentioned glycols or polyols are added to the above-mentioned trifunctional or tetrafunctional aliphatic alcohols. Among these, polyether polyols, polyurethane polyols, acrylic polyols, polycarbonate polyols, and polybutadiene polyols are preferred from the viewpoint of long-term resistance to moist heat. These polyols (A) may be used alone or in combination of two or more kinds.

[0023] The polyol (A) preferably contains 50% by mass or more of the polyol (A1) having a number average molecular weight of 2,000 or less, based on the total mass of the polyol (A). This is preferable because the fluidity of the polyol composition is not impaired even when a thermally conductive filler is blended. It is more preferable that it is 60% by mass or more. It is also preferably 70% by mass or more, more preferably 80% by mass or more. The number average molecular weight of the polyol (A1) is preferably 1,000 or less, more preferably 500 or less. In this specification, the number average molecular weight is a value measured by GPC (gel permeation chromatography) and converted into a polystyrene standard.

[0024] The polyol (A) may have a primary hydroxyl group at the end. When the polyol (A) has a primary hydroxyl group at the end, the initial adhesive strength at room temperature, the foaming inhibition of the coating film, and the strength after curing are excellent. The polyol (A) may also be a polyol having a urethane bond in the molecule (hereinafter, urethane polyol). By containing such a urethane polyol, the adhesive is prevented from sagging when applied to a vertical surface, and the cured coating film has excellent extensibility. That is, the polyol (A) preferably contains a urethane polyol having a primary hydroxyl group at the end and a urethane bond in the molecule.

[0025] The method for producing the urethane polyol is not particularly limited, and for example, a reaction product of a polyol and a polyisocyanate can be suitably used. As the polyol, for example, the compounds exemplified in the above section on <Polyol (A)> can be used.

[0026] Examples of the polyisocyanate include aromatic, aliphatic, or alicyclic diisocyanates (hereinafter also referred to as polyisocyanate monomers); dimers, trimers, biurets, and allophanates derived from polyisocyanate monomers; and polyisocyanates having a 2,4,6-oxadiazinetrione ring obtained from carbon dioxide gas and the above polyisocyanate monomers. These may be used alone or in combination of two or more.

[0027] Examples of aromatic diisocyanates include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate, tolidine diisocyanate, xylylene diisocyanate, m-tetramethylxylene diisocyanate, p-tetramethylxylene diisocyanate, 3,3'-dimethyl-4,4'-biphenylene diisocyanate, 3,3'-dimethoxy-4,4'-biphenylene diisocyanate, 3,3'-dichloro-4,4'-biphenylene diisocyanate, and 1,5-tetrahydronaphthalene diisocyanate.

[0028] Examples of the aliphatic diisocyanate include trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, 1,2-propylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, dodecamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, lysine ester triisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate tetramethylene diisocyanate, pentamethylene diisocyanate, and trimethylhexamethylene diisocyanate.

[0029] Examples of alicyclic diisocyanates include isophorone diisocyanate, 1,3-cyclopentane diisocyanate, 1,3-cyclohexane diisocyanate, 1,4-cyclohexane diisocyanate, methyl-2,4-cyclohexane diisocyanate, methyl-2,6-cyclohexane diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), 1,4-bis(isocyanatemethyl)cyclohexane, hydrogenated xylylene diisocyanate, dimer acid diisocyanate, and norbornene diisocyanate.

[0030] The number average molecular weight of the urethane polyol is not particularly limited, but is preferably from 3000 to 100000. When the number average molecular weight is 3000 or more, the cured product has excellent extensibility, and when it is 100,000 or less, the adhesive strength when cured at room temperature is excellent.

[0031] The urethane polyol may further have a urea bond in the molecule. By having a urea bond in the molecule, heat resistance durability and adhesive strength are improved. For example, an example of a urethane polyol having such a urea bond is a compound obtained by reacting an isocyanate group of a urethane polymer having an isocyanate group at the end, which is a reaction product of a polyol and a polyisocyanate, with an amino group of a monoamine compound having a molecular weight of less than 200 and having a hydroxyl group in the molecule. A compound using such a low molecular weight monoamine can increase the cohesive force of the resin without becoming too high in molecular weight, and is preferable in terms of suppressing sagging of the adhesive and improving adhesive strength.

[0032] <Phosphate Compounds (B)> The polyol composition contains a phosphoric acid compound (B). The phosphoric acid compound (B) accelerates the curing of the adhesive, improves good initial strength at room temperature curing and adhesion to metals, and can exhibit excellent adhesion to aluminum without the use of a primer. The phosphoric acid compound (B) may be any compound having at least one free oxygen acid, and examples thereof include phosphoric acids such as hypophosphorous acid, phosphorous acid, orthophosphoric acid, and hypophosphoric acid; condensed phosphoric acids such as metaphosphoric acid, pyrophosphoric acid, tripolyphosphoric acid, polyphosphoric acid, and ultraphosphoric acid; and phosphonic acids. Also, a derivative of a phosphoric acid compound may be used as the phosphoric acid compound (B). Examples of such derivatives include phosphonic acid esters, which are partially esterified with alcohol in a state where at least one free oxygen acid in the above-mentioned phosphorus oxygen acid remains. Examples of the alcohol include aliphatic alcohols such as methanol, ethanol, ethylene glycol, and glycerin; and aromatic alcohols such as phenol, xylenol, hydroquinone, catechol, and phloroglucinol. The phosphoric acid compound (B) may be used alone or in combination of two or more kinds.

[0033] The amount of the phosphoric acid compound (B) is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, even more preferably 0.6% by mass or more, and even more preferably 0.7% by mass or more, based on the mass of the polyol (A) from the viewpoints of curing acceleration and adhesion to metal. Also, from the viewpoint of the pot life after blending, it is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 2% by mass or less. The amount of the phosphoric acid compound (B) may be, for example, 0.1 to 5% by mass, based on the mass of the polyol (A).

[0034] <Dispersant (C)> The polyol composition contains a dispersant (C). The dispersant (C) can be appropriately selected from those conventionally used as dispersants for fillers. The dispersant (C) can uniformly disperse the thermally conductive filler (D1) in the polyol composition, thereby achieving low viscosity and suppression of aggregation. As the dispersant (C), for example, anionic, cationic, nonionic, amphoteric or other surfactants can be used. An anionic dispersant is one in which the hydrophilic group is ionized to generate an anion when dissolved in water. Examples of an anionic dispersant include phosphate ester type, sulfate ester type, sulfonic acid type, and carboxylate type. Examples of a cationic dispersant are one in which the hydrophilic group is ionized to generate a cation when dissolved in water. Examples of a cationic dispersant are alkylamine salt type and alkylammonium salt type. Examples of a nonionic dispersant are one in which the hydrophilic group does not have ionic dissociation properties. Examples of a nonionic dispersant are polyoxyalkylene type and ester type. An amphoteric dispersant is one that has both the anionic and cationic groups. The dispersant (C) may be used alone or in combination of two or more types. Among surfactants, polymer surfactants (polymer dispersants) are preferred because they can be uniformly and finely dispersed, and polymer dispersants having acidic groups are more preferred. Examples of acidic groups include carboxy groups, phosphoric acid groups and their salts, and sulfonic acid groups and their salts. Commercially available polymer dispersants having an acidic group include, for example, DISPERBYK-103, DISPERBYK-111, DISPERBYK-118, AJISPER PN411, and AJISPER PA111.

[0035] The amount of the dispersant (C) is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, and even more preferably 0.5% by mass or more, based on the mass of the thermally conductive filler (D1) described below, from the viewpoint of dispersibility, and is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 2% by mass or less, from the viewpoint of adhesion.

[0036] <Thermal conductive filler (D1)> The polyol composition includes a thermally conductive filler (D1). Examples of the thermally conductive filler (D1) include particles of silicon dioxide, metal oxides such as alumina, magnesium oxide, titanium oxide, and silica, metal carbonates such as calcium carbonate and magnesium carbonate, metal hydroxides such as aluminum hydroxide, magnesium hydroxide, and calcium hydroxide, metal nitrides such as aluminum nitride, boron nitride, and silicon nitride, metal carbides such as silicon carbide and boron carbide, silver, copper, aluminum, and alloys containing these. Among these, from the viewpoints of electrical insulation and thermal conductivity, the thermally conductive filler (D1) preferably contains at least one filler selected from the group consisting of metal oxides and metal nitrides. The thermal conductivity of the thermally conductive filler (D1) is preferably 5 W / m·K or more, more preferably 10 W / m·K or more, and even more preferably 20 W / m·K or more.

[0037] The thermally conductive filler (D1) may be surface-treated with a silane coupling agent. By surface-treating with a silane coupling agent, the wettability to the resin is improved and the reaction with the functional group and moisture in the polyol composition is suppressed. This improves the handling property and the strength of the cured film of the adhesive. Examples of the silane coupling agent include trialkoxysilanes having a vinyl group, such as vinyltrimethoxysilane and vinyltriethoxysilane; trialkoxysilanes having an amino group, such as 3-aminopropyltriethoxysilane and N-(2-aminoethyl)3-aminopropyltrimethoxysilane; trialkoxysilanes having a glycidyl group, such as 3-glycidoxypropyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane and 3-glycidoxypropyltriethoxysilane; alkoxysilane compounds having an isocyanate group, such as 3-isocyanatepropyltrimethoxysilane and 3-isocyanatepropyltriethoxysilane; trialkoxysilanes having a mercapto group, such as 3-mercaptopropyltrimethoxysilane; methyltrimethoxysilane, methyltriethoxysilane, n-propyltrimethoxysilane, Trialkoxysilane compounds such as dimethyldimethoxysilane, dimethyldiethoxysilane, and dimethoxydiphenylsilane; alkoxysilane compounds having (meth)acrylic groups such as 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropyltripropoxysilane, 3-(meth)acryloxypropyltributoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, and 3-(meth)acryloxypropylmethyldiethoxysilane; and the like. These may be used alone or in combination of two or more.

[0038] The content of the thermally conductive filler (D1) is preferably 60% by mass or more, more preferably 80% by mass or more, based on the mass of the polyol composition, and is preferably 97% by mass or less, more preferably 93% by mass or less. The total amount of the thermally conductive filler (D1) and the thermally conductive filler (D2) described below is preferably 60% by mass or more, more preferably 80% by mass or more, based on the mass of the thermally conductive adhesive, and is preferably 97% by mass or less, more preferably 93% by mass or less. The thermally conductive filler (D1) and a thermally conductive filler (D2) described below may be the same or different.

[0039] <<Polyisocyanate composition>> The polyisocyanate curing agent contains a polyisocyanate (E), a tri- or higher functional epoxy compound (F), and a thermally conductive filler (D2).

[0040] <Polyisocyanate (E)> The polyisocyanate (E) may be any compound having two or more isocyanate groups in the molecule, and examples of the polyisocyanate (E) include aromatic, aliphatic, or alicyclic diisocyanates (hereinafter also referred to as polyisocyanate monomers); dimers, trimers, biurets, and allophanates derived from polyisocyanate monomers; and polyisocyanates having a 2,4,6-oxadiazinetrione ring obtained from carbon dioxide gas and the above polyisocyanate monomers. These may be used alone or in combination of two or more.

[0041] Examples of aromatic diisocyanates include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate, tolidine diisocyanate, xylylene diisocyanate, m-tetramethylxylene diisocyanate, p-tetramethylxylene diisocyanate, 3,3'-dimethyl-4,4'-biphenylene diisocyanate, 3,3'-dimethoxy-4,4'-biphenylene diisocyanate, 3,3'-dichloro-4,4'-biphenylene diisocyanate, and 1,5-tetrahydronaphthalene diisocyanate.

[0042] Examples of the aliphatic diisocyanate include trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, 1,2-propylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, dodecamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, lysine ester triisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate tetramethylene diisocyanate, pentamethylene diisocyanate, and trimethylhexamethylene diisocyanate.

[0043] Examples of alicyclic diisocyanates include isophorone diisocyanate, 1,3-cyclopentane diisocyanate, 1,3-cyclohexane diisocyanate, 1,4-cyclohexane diisocyanate, methyl-2,4-cyclohexane diisocyanate, methyl-2,6-cyclohexane diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), 1,4-bis(isocyanatemethyl)cyclohexane, hydrogenated xylylene diisocyanate, dimer acid diisocyanate, and norbornene diisocyanate.

[0044] The polyisocyanate (E) may be a polyisocyanate having a urethane bond, which is a reaction product of the above-mentioned polyisocyanate and polyol. By including such a polyisocyanate having a urethane bond, the cured film of the adhesive has excellent flexibility, which is preferable. As the polyol, for example, the compounds exemplified in the above-mentioned section of <Polyol (A)> can be used.

[0045] As the polyisocyanate for forming the polyisocyanate having the urethane bond, from the viewpoint of initial adhesive strength, preferably an aromatic diisocyanate, more preferably diphenylmethane diisocyanate, is suitably used. That is, as the polyisocyanate (E), from the viewpoint of flexibility of the cured film and initial adhesive strength, a reaction product of an aromatic diisocyanate and a polyol is preferred, more preferably a reaction product of diphenylmethane diisocyanate and a polyol. In the reaction, the ratio (NCO / OH) of the number of isocyanate groups of the diphenylmethane diisocyanate to the number of hydroxyl groups of the polyol may be 1 or more, preferably 1.5 or more. The polyisocyanate (E) may be used in combination with another polyisocyanate depending on the required physical properties and viscosity. For example, polymeric MDI (hereinafter also referred to as crude MDI) and liquid MDI (a mixture of 2,4'-diphenylmethane diisocyanate and 4,4'-diphenylmethane diisocyanate) can be suitably used as the polyisocyanate to be used in combination with the polyisocyanate having a urethane bond.

[0046] <Epoxy compounds (F) with 3 or more functional groups> The polyisocyanate curing agent contains an epoxy compound (F) having three or more functional groups. By containing a compound (F) having three or more epoxy groups in one molecule, the adhesive can maintain its adhesive strength after a moist heat resistance test. Examples of such epoxy compounds (F) include epoxy compounds derived from polyvinylphenol, polyisopropenylphenol, 1,1-bis-(4-hydroxyphenyl)-1-phenylethane, 1,1-bis-(4-hydroxyphenyl)-1,1-dimethylmethane, etc.; novolak-based resins derived from phenol novolak, brominated phenol novolak, cresol novolak, brominated cresol novolak, resorcin novolak, brominated resorcin novolak, etc.; polyhydric phenol-based epoxy resins derived from resorcin, hydroquinone, methylresorcin, etc.; aniline, p-aminophenol, m-aminophenol, p-amino amine-based epoxy resins derived from m-cresol, 4,4'-diaminodiphenylmethane, etc.; glycidyl ester-based compounds derived from aromatic carboxylic acids such as p-oxybenzoic acid, m-oxybenzoic acid, terephthalic acid, isophthalic acid, etc.; hydantoin-based epoxy resins derived from 5,5'-dimethylhydantoin, etc.; alicyclic epoxy polymers such as vinylcyclohexene oxide; polyglycidyl ethers of multifunctional polyols such as trimethylolpropane and sorbitol; and others, such as triglycidyl isocyanurate, 2,4,6-triglycidoxy-5-triazine, epoxidized polybutadiene, and epoxidized vegetable oil. Modified products of these, such as dimer acid-modified epoxy resins and urethane-modified epoxy resins, may also be used. These epoxy compounds (F) may be used alone or in combination of two or more.

[0047] From the viewpoint of solution stability of the polyisocyanate curing agent, the epoxy compound (F) is preferably an alicyclic epoxy polymer formed by adding oxygen to a double bond, such as epoxidized butadiene, epoxidized SEBS, epoxidized vegetable oil, or vinylcyclohexene oxide.

[0048] <Thermal conductive filler (D2)> The polyisocyanate curing agent contains a thermally conductive filler (D2). As the thermally conductive filler (D2), the description in the above section on <Thermal conductive filler (D1)> can be used. The content of the thermally conductive filler (D2) is preferably 60% by mass or more, more preferably 70% by mass or more, based on the mass of the polyisocyanate curing agent. It is also preferably 97% by mass or less, more preferably 93% by mass or less. The thermally conductive filler (D2) may be surface-treated with a silane coupling agent, similar to the thermally conductive filler (D1). The surface treatment with a silane coupling agent improves the wettability to the resin and suppresses the reaction with the functional group or moisture in the polyisocyanate composition. This improves the handling property and the strength of the cured film of the adhesive.

[0049] <<Adjustment of thermal conductive adhesive>> The thermally conductive adhesive of the present invention can be obtained by mixing at least a polyol composition and a polyisocyanate composition by a known method. The ratio of the number of hydroxyl groups in the polyol composition to the number of isocyanate groups in the polyisocyanate composition [NCO / OH] is preferably 0.9 to 1.3, more preferably 1.0 to 1.2. The adhesive of the present invention may be either a solvent-based or solventless type, but is preferably a solventless type in that it does not require a drying step in the curing process. However, the solventless type may contain a small amount of solvent, such as a solvent contained in an antifoaming agent or a diluting solvent used when adding a solid additive.

[0050] From the viewpoint of coatability, the viscosity of the polyol composition is preferably 1 Pa·s to 500 Pa·s, more preferably 10 Pa·s to 300 Pa·s, and the viscosity of the polyisocyanate composition is preferably 1 Pa·s to 500 Pa·s, more preferably 10 Pa·s to 300 Pa·s. In addition, the viscosity of the polyol composition (V OH ) vs. the viscosity (V NCO ) ratio (V NCO / V OH ) is preferably 0.1 to 10, more preferably 0.2 to 5, from the viewpoint of stability of adhesive strength. The viscosity is a value measured using a rheometer MCR302 (manufactured by Anton Paar) at a temperature of 25° C. and a shear rate of 10 / s.

[0051] <Additives> The adhesive of the present invention may further contain known additives such as epoxy compounds, reaction accelerators, silane coupling agents, leveling agents or defoamers, fillers, propellants, plasticizers, superplasticizers, wetting agents, flame retardants, viscosity modifiers, preservatives, stabilizers, and colorants. Such additives may be used alone or in combination of two or more.

[0052] Examples of the epoxy compound include epoxy compounds derived from polyvinylphenol, polyisopropenylphenol, 1,1-bis-(4-hydroxyphenyl)-1-phenylethane, 1,1-bis-(4-hydroxyphenyl)-1,1-dimethylmethane, and the like; novolak-based resins derived from phenol novolak, brominated phenol novolak, cresol novolak, brominated cresol novolak, resorcin novolak, brominated resorcin novolak, and the like; polyhydric phenol-based epoxy resins derived from resorcin, hydroquinone, methylresorcin, and the like; aniline, p-aminophenol, m-aminophenol, p-amino-m-chloride, and the like; Examples of the epoxy resins include amine-based epoxy resins derived from resol, 4,4'-diaminodiphenylmethane, etc.; glycidyl ester-based compounds derived from aromatic carboxylic acids such as p-oxybenzoic acid, m-oxybenzoic acid, terephthalic acid, and isophthalic acid; hydantoin-based epoxy resins derived from 5,5'-dimethylhydantoin, etc.; alicyclic epoxy polymers such as vinylcyclohexene oxide; polyglycidyl ethers of multifunctional polyols such as trimethylolpropane and sorbitol; and others, such as triglycidyl isocyanurate, 2,4,6-triglycidoxy-5-triazine, epoxidized polybutadiene, and epoxidized vegetable oil. In addition, examples of the epoxy resins modified by these include dimer acid-modified epoxy resins and urethane-modified epoxy resins. The amount of the epoxy compound blended is preferably 1 to 20 mass % based on the total mass of the polyol (A) from the viewpoints of adhesiveness and moist heat resistance.

[0053] Examples of the reaction accelerator include metal catalysts such as dibutyltin diacetate, dibutyltin dilaurate, dioctyltin dilaurate, dibutyltin dimaleate, etc. The amount of the reaction accelerator is preferably 0.005 to 1% by mass based on the total mass of the polyol (A).

[0054] Examples of the silane coupling agent include trialkoxysilanes having a vinyl group, such as vinyltrimethoxysilane and vinyltriethoxysilane; trialkoxysilanes having an amino group, such as 3-aminopropyltriethoxysilane and N-(2-aminoethyl)3-aminopropyltrimethoxysilane; trialkoxysilanes having a glycidyl group, such as 3-glycidoxypropyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane and 3-glycidoxypropyltriethoxysilane; trialkoxysilanes having an isocyanato group, such as 3-isocyanatepropyltriethoxysilane; and trialkoxysilanes having a mercapto group, such as 3-mercaptopropylmethyldimethoxysilane and 3-mercaptopropyltrimethoxysilane. The amount of the silane coupling agent added is preferably 0.05 to 10% by mass based on the total mass of the adhesive.

[0055] Examples of the leveling agent include polyether-modified polydimethylsiloxane, polyester-modified polydimethylsiloxane, aralkyl-modified polymethylalkylsiloxane, polyester-modified hydroxyl group-containing polydimethylsiloxane, polyetherester-modified hydroxyl group-containing polydimethylsiloxane, acrylic copolymers, methacrylic copolymers, polyether-modified polymethylalkylsiloxane, acrylic acid alkyl ester copolymers, methacrylic acid alkyl ester copolymers, and lecithin.

[0056] Examples of the defoaming agent include known ones such as silicone resin, silicone solution, copolymers of alkyl vinyl ether, alkyl acrylate, and alkyl methacrylate.

[0057] <<Laminated body, cured product>> The cured product of the present invention can be obtained by curing the thermally conductive adhesive of the present invention by a known method. The structure of the present invention is characterized in that it has an adhesive layer between a first substrate and a second substrate, and the adhesive layer is the above-mentioned cured product. The method for producing the structure is not particularly limited, and for example, the adhesive is applied to one surface of the first substrate, and then the second substrate is placed on the uncured adhesive surface, and a curing reaction is carried out at about 20 to 40°C to cure the adhesive, thereby obtaining a structure. The thickness of the adhesive layer after curing is preferably 0.1 μm to 300 mm.

[0058] <First base material, second base material> The adhesive of the present invention can be used for bonding between various kinds of substrates. Substrates that can be used as the preferred first and second substrates include, for example, metals such as aluminum, thermoplastic polymers such as polyethylene, polypropylene, polyurethane, polyacrylate, polycarbonate and their copolymers, thermosetting polymers such as vulcanized rubber, urea-formaldehyde foam, melamine resin, wood, carbon fiber reinforced plastic, glass fiber reinforced plastic and other fiber reinforced plastics. The first substrate and the second substrate may be the same substrate or different substrates.

[0059] The adhesive of the present invention exhibits good mixability between the polyol composition and the polyisocyanate composition, and is excellent in dispersion stability, thermal conductivity, rapid room temperature curing properties, adhesion to aluminum substrates, and long-term moist heat resistance. Structures using the adhesive are useful for cooling heat-generating components such as semiconductor elements, LED backlights, batteries, and electric circuits incorporating these. EXAMPLES

[0060] The present invention will be described in more detail below with reference to examples, but the following examples are not intended to limit the scope of the invention. In the examples, "parts" and "%" represent "parts by mass" and "% by mass" unless otherwise specified.

[0061] <Average molecular weight (Mn)> The number average molecular weight (Mn) and mass average molecular weight (Mw) of the resin were determined by gel permeation chromatography (GPC) using standard polystyrene as the conversion value. The measurements were performed using a GPC-8020 (Tosoh Corporation) as the GPC device, tetrahydrofuran as the eluent, and three TSKgel SuperHM-M (Tosoh Corporation) columns connected in series under the conditions of a flow rate of 0.6 ml / min, an injection volume of 10 μl, and a column temperature of 40°C.

[0062] The abbreviations for compounds used in this specification are shown below. <Polyol> P-400: Bifunctional polypropylene glycol, number average molecular weight 400, hydroxyl value 280mgKOH / g, manufactured by ADEKA Corporation P-1000: Bifunctional polypropylene glycol, number average molecular weight 1,000, hydroxyl value 112 mgKOH / g, manufactured by ADEKA Corporation P-2000: Bifunctional polypropylene glycol, number average molecular weight 2,000, hydroxyl value 56 mgKOH / g, manufactured by ADEKA Corporation T-400: Trifunctional polypropylene glycol, number average molecular weight 400, hydroxyl value 410 mgKOH / g, manufactured by Mitsui Chemicals T5650E: Bifunctional polycarbonate polyol, number average molecular weight 500, hydroxyl value 220 mgKOH / g, product name "Duranol T5650E", manufactured by Asahi Kasei Corporation T5651: Bifunctional polycarbonate polyol, number average molecular weight 1,000, hydroxyl value 110 mgKOH / g, product name "Duranol T5651", manufactured by Asahi Kasei Corporation ·TMP: Trimethylolpropane GI-1000: Polybutadiene polyol, number average molecular weight 1,400, hydroxyl value 69 mgKOH / g, manufactured by Nippon Soda Co., Ltd.

[0063] <Polyisocyanate> IPDI: Isophorone diisocyanate ·TDI: Tolylene diisocyanate ·4,4'-MDI: 4,4'-diphenylmethane diisocyanate Liquid MDI: Millionate MN, manufactured by Tosoh Corporation Crude MDI: PM-200, manufactured by Wanhua Chemical HDI-Nurate: Hexamethylene diisocyanate nurate, Basonat HI-100, manufactured by BASF

[0064] <Epoxy compounds> JP-100: Epoxidized polybutadiene, manufactured by Nippon Soda Co., Ltd. ED-505: Trimethylolpropane triglycidyl ether, manufactured by ADEKA jER-828: Bisphenol A type epoxy resin, manufactured by Mitsubishi Chemical Corporation

[0065] <Dispersant> BYK-111: Phosphate ester compound (corresponding to a polymer dispersant having an acidic group), product name "DISPERBYK-111", manufactured by BYK Japan, acid value 129 mg KOH / g, non-volatile content 95.0%.

[0066] <Thermal conductive filler> DAW-45: Alumina, average particle size 46μm, thermal conductivity 27W / mK, manufactured by Denka DAW-20: Alumina, average particle size 23μm, thermal conductivity 27W / mK, manufactured by Denka DAW-05: Alumina, average particle size 6μm, thermal conductivity 27W / mK, manufactured by Denka DAW-01: Alumina, average particle size 2μm, thermal conductivity 27W / mK, manufactured by Denka HFS-80: Aluminum nitride, average particle size 80μm, thermal conductivity 170W / mK, manufactured by Tokuyama Corporation SP-3: Boron nitride, average particle size 4μm, thermal conductivity 60W / mK, manufactured by Denka

[0067] <Filler> MS-KY: Talc, average particle size 21μm, manufactured by Nippon Talc Co., Ltd.

[0068] <Synthesis of polyol> (Polyol A1) In a reaction vessel equipped with a nitrogen gas inlet tube, a stirrer, a thermometer, and a reflux condenser, 100 parts of T5651 and 13.7 parts of tolylene diisocyanate were charged and stirred uniformly. The mixture was then reacted for 5 hours at 110°C under a nitrogen atmosphere to obtain a urethane-type polyol (a1) having a number average molecular weight of 5,000.

[0069] (Polyol A2) In a reaction vessel equipped with a nitrogen gas inlet tube, a stirrer, a thermometer, and a reflux condenser, 100 parts of T5651 and 30.5 parts of isophorone diisocyanate were charged and stirred uniformly, and then reacted for 5 hours at 90°C under a nitrogen atmosphere to obtain a urethane prepolymer. Next, the mixture was cooled to 80°C, 4.8 parts of ethanolamine were added, and the mixture was reacted for 2 hours at 75°C to obtain a polyurethane urea polyol (a2) having a number average molecular weight of 6,000.

[0070] (Polyol A3) A reaction vessel equipped with a nitrogen gas inlet tube, a stirrer, a thermometer, and a reflux condenser was charged with 100 parts of P-1000 and 13.9 parts of tolylene diisocyanate, and the mixture was reacted at 110°C for 5 hours under a nitrogen atmosphere to obtain a urethane-type polyol (a3) ​​having a number average molecular weight of 5,000.

[0071] [Table 1]

[0072] <Synthesis of polyisocyanate> (Polyisocyanate e1) A reaction vessel equipped with a nitrogen gas inlet tube, a stirrer, a thermometer, and a reflux condenser was charged with 25 parts of P-400 and 45 parts of 4,4'-diphenylmethane diisocyanate, and reacted at 90°C for 3 hours under a nitrogen atmosphere to carry out a urethane reaction. After that, it was cooled to 50°C, and 30 parts of crude MDI was added and stirred for 15 minutes to obtain polyisocyanate (e1).

[0073] (Polyisocyanate E2) In a reaction vessel equipped with a nitrogen gas inlet tube, a stirrer, a thermometer, and a reflux condenser, 12 parts of P-400, 12 parts of P-2000, and 1.6 parts of T-400 were charged and stirred uniformly, after which 32.4 parts of 4,4'-MDI was charged and reacted at 90°C for 3 hours under a nitrogen atmosphere to carry out a urethane reaction. After that, it was cooled to 50°C, and 30 parts of crude MDI and 12 parts of liquid MDI were added and stirred for 15 minutes to obtain polyisocyanate (e2).

[0074] (Polyisocyanate e3) A reaction vessel equipped with a nitrogen gas inlet tube, a stirrer, a thermometer, and a reflux condenser was charged with 35 parts of liquid MDI, and a mixture of 39.6 parts of GI-1000 and 0.4 parts of TMP was added little by little, stirred uniformly, and reacted at 90°C for 3 hours under a nitrogen atmosphere to carry out a urethane reaction. The mixture was then cooled to 50°C, and 25 parts of liquid MDI was added and stirred to obtain polyisocyanate (e3).

[0075] [Table 2]

[0076] <Adjustment of thermally conductive filler> (Thermal conductive filler d1) In a reaction vessel equipped with a stirrer and a thermometer, 60 parts of DAW-45, 25 parts of DAW-20, and 15 parts of DAW-01 were charged and stirred uniformly, after which 1 part of decyltrimethoxysilane was charged and stirred for 30 minutes at 60° C. After that, it was dried at 150° C. for 3 hours to obtain a thermally conductive filler (d1).

[0077] (Thermal conductive filler d2) 30 parts of DAW-45, 50 parts of DAW-20, and 20 parts of DAW-01 were charged into a reaction vessel equipped with a stirrer and a thermometer and stirred uniformly, after which 1 part of decyltrimethoxysilane was charged and stirred for 30 minutes at 60° C. After that, it was dried at 150° C. for 3 hours to obtain a thermally conductive filler (d2).

[0078] (Thermal conductive filler d3) 60 parts of HFS-80, 25 parts of DAW-05, and 15 parts of DAW-01 were charged into a reaction vessel equipped with a stirrer and a thermometer and stirred uniformly, after which 1 part of decyltrimethoxysilane was charged and stirred for 30 minutes at 60° C. Then, it was dried at 150° C. for 3 hours to obtain a thermally conductive filler (d3).

[0079] (Thermal conductive filler d4) In a reaction vessel equipped with a stirrer and a thermometer, 12 parts of DAW-45, 5 parts of DAW-05, 3 parts of DAW-01, and 40 parts of SP-3 were charged and stirred uniformly, and then 1 part of decyltrimethoxysilane was charged and stirred for 30 minutes at 60° C. After that, it was dried at 150° C. for 3 hours to obtain a thermally conductive filler (d4).

[0080] (Thermal conductive filler d5) 60 parts of HFS-80, 25 parts of DAW-20, and 15 parts of SP-3 were charged into a reaction vessel equipped with a stirrer and a thermometer and stirred uniformly, after which 1 part of decyltrimethoxysilane was charged and reacted and stirred for 30 minutes at 60°C. After that, it was dried at 150°C for 3 hours to obtain a thermally conductive filler (d5).

[0081] (Thermal conductive filler d6) A reaction vessel equipped with a stirrer and a thermometer was charged with 60 parts of DAW-45, 25 parts of DAW-20, and 15 parts of DAW-01, and the mixture was stirred uniformly to obtain a thermally conductive filler (d6).

[0082] [Table 3]

[0083] <Production of Dispersant> (Dispersant (c1)) In a reaction vessel equipped with a nitrogen gas inlet tube, a stirrer, a thermometer, and a reflux condenser, 62.6 parts of 1-dodecanol, 287.4 parts of ε-caprolactone, and 0.1 parts of monobutyltin (IV) oxide as a catalyst were charged, and the mixture was heated and stirred at 120°C for 4 hours under a nitrogen atmosphere. After confirming that 98% had reacted by measuring the solid content, 36.6 parts of pyromellitic dianhydride was charged into the reaction product and reacted at 100°C for 5 hours to obtain dispersant (c1), which is a polymer dispersant having an acidic group.

[0084] <Production of polyol composition> (Polyol composition 1) 10 parts of polyol (a1), 90 parts of T5650E, 1.00 part of polyphosphoric acid, 1.45 parts of dispersant (c1), and 580 parts of thermally conductive filler (d1) were mixed, stirred and degassed using a planetary centrifugal mixer (Awatori Rentaro, manufactured by Thinky Corporation), to obtain polyol composition 1.

[0085] (Polyol Compositions 2 to 23) Except for changing the blending ratio of each component to that shown in Table 4, the components were mixed in the same manner as in Polyol Composition 1, to obtain Polyol Compositions 2 to 23.

[0086] The viscosity of the obtained polyol composition was measured using a rheometer MCR302 (manufactured by Anton Paar) at a temperature of 25° C. and a shear rate of 10 / s. The results are shown in Table 4.

[0087] [Table 4]

[0088] <Production of polyisocyanate composition> (Polyisocyanate composition 1) 100 parts of polyisocyanate (e1), 10 parts of JP-100, and 625 parts of thermally conductive filler (d1) were added and stirred and degassed using a planetary centrifugal mixer (Awatori Rentaro, manufactured by Thinky Corporation), to obtain polyisocyanate composition 1.

[0089] (Polyisocyanate compositions 2 to 17) Except for changing the blending ratio of each component to that shown in Table 5, the components were mixed in the same manner as in Polyisocyanate Composition 1, to obtain Polyisocyanate Compositions 2 to 17.

[0090] The viscosity of the obtained polyisocyanate composition was measured under the same conditions as those for the polyol composition, and the results are shown in Table 5.

[0091] [Table 5]

[0092] <Adjustment of thermally conductive adhesive> [Examples 1 to 23, Comparative Examples 1 to 6] The polyol composition and the polyisocyanate composition were stored in a 40°C environment for one month and then returned to room temperature, and two types of adhesives were prepared by changing the stirring and mixing time. Specifically, the composition shown in Table 6 was thoroughly stirred and mixed at 50 rpm for 60 seconds until homogenous to prepare a thermally conductive adhesive (X). Similarly, the composition was stirred and mixed for a short period of time at 50 rpm for 10 seconds to prepare a thermally conductive adhesive (Y). In addition, since Polyol Composition 20 did not contain a dispersant, the filler precipitated, and the composition was not evaluated as an adhesive (Comparative Example 1).

[0093] <Evaluation of thermally conductive adhesives> The adhesives (X) and (Y) obtained were subjected to the following evaluations, and the results are shown in Table 6. [Thermal Conductivity] The obtained adhesive (X) was applied to the untreated surface of a CPP film to a thickness of 1 mm, and cured for 3 days in a 23°C environment to obtain a cured film. The obtained cured film was removed from the CPP film, and the thermal conductivity was measured using a TRIDENT (manufactured by C-THERM). Based on the thermal conductivity value, the following criteria were used for evaluation. A: 2.0W / m K or more (very good) B: 1.5W / m K or more, less than 2.0W / m K (good) C: 1.0W / m K or more, less than 1.5W / m K (usable) D: Less than 1.0W / m K (unusable)

[0094] [Room temperature rapid curing] The obtained adhesive (X) was applied to a first aluminum substrate (length 100 mm, width 25 mm, thickness 2 mm) to a width of 25 mm, length 10 mm, and thickness of 0.3 mm, and then laminated to the same second aluminum substrate and pressed to maintain a thickness of 0.3 mm, and curing was started in an environment of 23°C. Every 10 minutes after the start of curing, the shear adhesive strength was measured using a tensile tester at a tensile speed of 50 mm / min under conditions of 23°C. Evaluation was made according to the following criteria based on the time until the shear strength reached 0.4 MPa or more. A: Within 20 minutes (very good) B: More than 20 minutes, less than 30 minutes (good) C: More than 30 minutes, up to 60 minutes (usable) D: More than 60 minutes (unavailable)

[0095] [AL base material adhesion] Test pieces prepared using adhesive (X) in the same manner as in the above [Room temperature fast curing] were aged for 3 days in a 23°C environment, and then the shear adhesive strength was measured using a tensile tester at a tensile speed of 50 mm / min under conditions of 23°C. The shear adhesive strength was evaluated according to the following criteria. A: 10MPa or more (very good) B: 7MPa or more, less than 10MPa (good) C: 5MPa or more, less than 7MPa (usable) D: Less than 5MPa (unusable)

[0096] [Long-term humidity and heat resistance] Test pieces prepared using adhesive (X) in the same manner as in the above [Room temperature fast curing] were cured for 3 days in a 23°C environment, and then stored for 1000 hours in an 85°C and 85% relative humidity environment. The shear strength of the test pieces before and after storage was measured using a tensile tester at a tensile speed of 50 mm / min under conditions of 23°C. The ratio of the shear strength value after storage to the shear strength value before storage was calculated using the following formula, and evaluated according to the following criteria. Formula) Ratio (%) of shear strength after storage to shear strength before storage = [(shear strength value after storage) / (shear strength value before storage)] × 100 A: 85% or more (very good) B: 75% or more, less than 85% (good) C: 50% or more, less than 75% (usable) D: Less than 50% (unusable)

[0097] [Adhesive strength stability] Test pieces were prepared in the same manner as described above in [Adhesion to AL substrate], except that adhesive (Y), which has a shorter mixing time, was used instead of adhesive (X). After curing for 3 days in an environment at 23°C, the shear adhesive strength was measured using a tensile tester at a tensile speed of 50 mm / min at 23°C. The ratio of the shear strength value when adhesive (Y) was used to the shear strength value when adhesive (X) was used (= the shear strength value in the above-mentioned [Adhesion to AL substrate]) was calculated using the following formula and evaluated according to the following criteria. Formula) The ratio (%) of the shear strength value when adhesive (Y) is used to the shear strength value when adhesive (X) is used = [(Shear strength value when adhesive (Y) is used) / (Shear strength value when adhesive (X) is used)] x 100 A: 85% or more (very good) B: 75% or more, less than 85% (good) C: 50% or more, less than 75% (usable) D: Less than 50% (unusable)

[0098] [Table 6]

[0099] According to Table 6, a thermally conductive adhesive containing a polyol composition containing a polyol, a phosphoric acid compound, a dispersant, and a thermally conductive filler, and a polyisocyanate composition containing a polyisocyanate, a tri- or higher functional epoxy compound, and a thermally conductive filler, had excellent dispersion stability and was less susceptible to filler settling, had high thermal conductivity, and exhibited good initial adhesive strength at room temperature in a short time, and further had excellent adhesion to aluminum substrates, long-term moist heat resistance, and adhesive strength stability when mixed for a short time.

Claims

1. A polyol composition comprising a polyol (A), a phosphoric acid compound (B), a dispersant (C) and a thermally conductive filler (D1); A polyisocyanate composition comprising a polyisocyanate (E), a tri- or higher functional epoxy compound (F) and a thermally conductive filler (D2); A thermally conductive adhesive comprising:

2. The thermally conductive adhesive according to claim 1, wherein the thermally conductive filler (D1) and the thermally conductive filler (D2) each independently contain at least one filler selected from the group consisting of metal oxides and metal nitrides.

3. 2. The thermally conductive adhesive according to claim 1, wherein the thermally conductive filler (D1) and the thermally conductive filler (D2) are each independently surface-treated with a silane coupling agent.

4. The thermally conductive adhesive according to claim 1 , wherein the total amount of the thermally conductive filler (D1) and the thermally conductive filler (D2) is 60 mass% or more based on the mass of the thermally conductive adhesive.

5. The thermally conductive adhesive according to claim 1 , wherein the polyol (A) contains 50 mass% or more of a polyol (A1) having a number average molecular weight of 2,000 or less.

6. The thermally conductive adhesive according to claim 1, wherein the content of the phosphoric acid compound (B) is 0.1 to 5 mass % based on the mass of the polyol (A).

7. Viscosity of the polyol composition (V OH ) to the viscosity of the polyisocyanate composition (V NCO ) ratio (V NCO / V OH 2. The thermally conductive adhesive according to claim 1, wherein the molecular weight of the polymer is 0.1 to 10.

8. A cured product of the thermally conductive adhesive according to claim 1 .

9. A structure comprising an adhesive layer between a first substrate and a second substrate, the adhesive layer being the cured product according to claim 8.

Citation Information

Patent Citations

  • Environment-friendly type composite resin and adhesive and paint based on resin

    CN104910817A

  • Water-dispersible polyisocyanate composition, water- based curable composition and its application

    JP2002194237A

  • Aqueous curable composition, coating and adhesive containing the same

    JP2005200497A

  • Flame-retardant adhesive composition, coverlay, adhesive sheet, and flexible printed wiring board

    JP2009096940A

  • 2-component type thermal conductive resin composition, thermal conductive sheet, metal product and electronic equipment

    JP2019172935A